Cellulose-containing fine particle and method for producing the same, and cosmetic product

A simplified spray-drying process for cellulose fine particles with specific structural modifications addresses the complexity of existing methods, resulting in high-quality particles with enhanced properties for cosmetic applications.

JP2024157632APending Publication Date: 2024-11-08TOAGOSEI CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023072085
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing methods for manufacturing cellulose fine particles are complicated and require multiple steps, such as acid hydrolysis, alkaline oxidative decomposition, and steam explosion decomposition, making them inefficient and costly.

Method used

A simple method involving spray-drying cellulose under specific conditions to produce cellulose fine particles with a type I crystal structure, anion-modifying groups, and controlled viscosity average degree of polymerization, which includes oxidation with hypochlorous acid or its salts to introduce carboxy groups and avoid N-oxyl compounds.

Benefits of technology

The method allows for the production of cellulose fine particles with excellent properties, including shape retention, water absorption, and improved feel when incorporated into cosmetics, while reducing environmental impact and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157632000001_ABST
    Figure 2024157632000001_ABST
Patent Text Reader

Abstract

To provide cellulose fine particles and the like.SOLUTION: The present invention provides cellulose-containing fine particles, where the cellulose has a type I crystal structure, where the cellulose has a viscosity-average degree of polymerization of 30-500, where the cellulose has an anionically modified group, where the anionically modified group has a proton or a cation with a valence of 2 or higher.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to cellulose-containing microparticles, a method for producing the same, and cosmetics containing the microparticles. [Background technology]

[0002] Most microparticles used in cosmetics are made from synthetic resins. However, in order to reduce environmental impact and solve the problem of marine microplastics, there is a growing trend to use biodegradable biomass, and the development of cellulose microparticles in particular is progressing.

[0003] For example, Patent Document 1 discloses a method for producing spherical cellulose particles, which comprises subjecting a raw cellulose material to one or a combination of two or more of acid hydrolysis, alkaline oxidative decomposition, enzymatic decomposition, and steam explosion decomposition, adjusting the suspension concentration to 1.0 to 25% by deliquoring or adding liquid, wet-pulverizing the material in a vessel with forced stirring, and drying by a spray method.

[0004] Furthermore, Patent Document 2 discloses "a method for producing cellulose derivative particles, which comprises alkali-substituting spherical cellulose particles to form alkali-impregnated cellulose and wetting the particles, adding an acid anhydride of a polycarboxylic acid to the wet alkali-impregnated cellulose, and introducing carboxyl groups to the hydroxyl groups of the spherical cellulose particles via ester bonds." [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 2976116 [Patent Document 2] Patent No. 4022085 Summary of the Invention [Problem to be solved by the invention]

[0006] The production methods described in Patent Documents 1 and 2 are complicated, and therefore, there is a demand for a simpler method for producing cellulose microparticles.

[0007] An object of the present invention is to provide a simple method for producing cellulose microparticles, and cellulose microparticles having excellent properties obtained by the method. [Means for solving the problem]

[0008] As a result of extensive investigations, the present inventors have found that cellulose microparticles can be easily produced by spray-drying cellulose under specified conditions, and that the cellulose microparticles obtained by this method have excellent properties.

[0009] The present invention includes the following embodiments. [1] A microparticle comprising cellulose, The cellulose has a type I crystal structure, the cellulose has a viscosity-average degree of polymerization of 30 to 500, The cellulose has an anion-modified group, and the anion-modified group has a proton or a divalent or higher valent cation. Fine particles. [2] The microparticles according to [1], wherein the cellulose is an oxide of a cellulose-based raw material with hypochlorous acid or a salt thereof, and is substantially free of N-oxyl compounds. [3] The microparticles according to [1] or [2], wherein the cellulose is modified with a polycarboxylic acid. [4] the anion-modified group is a carboxy group, The fine particles according to any one of [1] to [3], wherein the cellulose is modified with a polycarboxylic acid and / or phosphoric acid. [5] The microparticles according to any one of [1] to [4], wherein the microparticles have an average particle size of 0.1 to 200 μm. [6] The microparticles according to any one of [1] to [5], wherein the microparticles have an average circularity of 0.5 to 1 when left to stand in pure water for 30 minutes. [7] The microparticles according to any one of [1] to [6], which have a water absorption capacity of 1 to 10 times when the microparticles are spray-dried at 170°C. [8] A cosmetic product comprising the microparticles according to any one of [1] to [7]. [9] The method for producing microparticles according to any one of [1] to [7], The method includes a step of spray-drying a cellulose dispersion to obtain microparticles containing the cellulose, wherein the cellulose contained in the dispersion has a type I crystal structure, the cellulose contained in the dispersion has a viscosity-average degree of polymerization of 30 to 500, The cellulose contained in the dispersion has an anion-modified group, and the anion-modified group has a proton or a divalent or higher valent cation. Manufacturing method.

[10] A method for producing cellulose-containing microparticles, comprising: The method includes a step of spray-drying a cellulose dispersion to obtain microparticles containing the cellulose, The cellulose is an oxidation product of a cellulose-based raw material with hypochlorous acid or a salt thereof, and is substantially free of N-oxyl compounds; At least one of the following conditions 1 to 3 is met: Condition 1: the pH of the dispersion is 1.5 to 5.8; Condition 2: The cellulose contained in the dispersion is modified with a polycarboxylic acid and / or phosphoric acid; Condition 3: the cellulose contained in the dispersion has a carboxy group, and the carboxy group has a proton or a divalent or higher valent cation; Manufacturing method that meets the above requirements.

[11] The method according to

[10] , wherein the cellulose contained in the dispersion has a type I crystal structure.

[12] The method according to

[10] or

[11] , wherein the cellulose contained in the dispersion has a viscosity-average degree of polymerization of 30 to 500.

[13] The method according to any one of

[10] to

[12] , wherein the cellulose contained in the dispersion contains cellulose that has not been defibrated.

[14] The method according to any one of

[10] to

[13] , wherein the cellulose contained in the microparticles includes nanocellulose.

[15] The method according to any one of

[10] to

[14] , wherein the amount of the cellulose contained in the dispersion is 0.1 to 30 mass % based on the mass of the dispersion. [Effects of the Invention]

[0010] According to the present invention, it is possible to provide a simple method for producing cellulose microparticles, and cellulose microparticles having excellent properties obtained by the method. [Brief explanation of the drawings]

[0011] [Figure 1] FIG. 1 shows a micrograph of the cellulose microparticles of Example 1. [Figure 2] FIG. 2 shows a micrograph of the cellulose microparticles of Example 2. [Figure 3] FIG. 3 shows a micrograph of the cellulose fine particles of Comparative Example 1. DETAILED DESCRIPTION OF THE INVENTION

[0012] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to these and various modifications are possible without departing from the gist of the present invention.

[0013] <Definition> In this specification, the term "comprise" means that the invention may include elements other than those explicitly stated to be included.

[0014] As used herein, the term "consisting only of" means including only the elements explicitly stated to be included. In other words, the term does not include any elements other than those explicitly stated to be included.

[0015] As used herein, the term "essentially consisting of" means including the elements explicitly stated to be included, but excluding other essential elements. An "essential element" is an element that substantially affects the essential characteristics of the present invention. Therefore, elements that do not substantially affect the essential characteristics of the present invention may be included.

[0016] <Cellulose fine particles> One embodiment of the present invention relates to cellulose-containing microparticles (referred to as "cellulose microparticles"), in which the cellulose has a type I crystal structure and a viscosity-average degree of polymerization of 30 to 500, and the cellulose has an anion-modified group, and the anion-modified group has a proton or a divalent or higher cation.

[0017] The cellulose fine particles according to this embodiment can improve the feel of cosmetics, for example, by being blended in cosmetics.

[0018] The cellulose microparticles according to this embodiment may be in a dry state or a swollen state. In this specification, "dry state" means that the amount of liquid contained in the cellulose microparticles is less than 15% by mass. In this specification, "swollen state" means that the amount of liquid contained in the cellulose microparticles is 15% by mass or more. Usually, the liquid contained in the cellulose microparticles is water.

[0019] The cellulose microparticles according to this embodiment have excellent shape-retaining properties, and therefore can maintain a spherical shape when swollen even after repeated drying and swelling. Therefore, when the cellulose microparticles are incorporated into cosmetics, for example, they can improve the feel of the cosmetics.

[0020] [Hypochlorous acid oxidation] The cellulose contained in the cellulose fine particles according to this embodiment is preferably an oxide of a cellulose-based raw material with hypochlorous acid or a salt thereof (oxidized cellulose).

[0021] Examples of hypochlorous acid or salts thereof include hypochlorous acid water, sodium hypochlorite, potassium hypochlorite, calcium hypochlorite, and ammonium hypochlorite.

[0022] The amount of hypochlorous acid or its salt used is not particularly limited, but it is preferable to use it so that the available chlorine concentration in the reaction system is 6 to 43 mass %. The available chlorine concentration may be a low concentration of 6 to 14 mass %, or a high concentration of 14 to 43 mass %.

[0023] The available chlorine concentration of hypochlorous acid or its salts is defined as follows: Hypochlorous acid is a weak acid that exists as an aqueous solution, and hypochlorite is a compound in which the hydrogen of hypochlorous acid is replaced by another cation. For example, sodium hypochlorite, a hypochlorite, exists in a solvent (preferably in an aqueous solution), so the concentration is measured as the amount of available chlorine in the solution, not the concentration of sodium hypochlorite. Here, with regard to the available chlorine of sodium hypochlorite, the oxidizing power of the divalent oxygen atom generated by the decomposition of sodium hypochlorite is equivalent to two atomic equivalents of monovalent chlorine. Therefore, the combined chlorine atoms of sodium hypochlorite (NaClO) have the same oxidizing power as two atoms of uncombined chlorine (Cl2), and available chlorine = 2 × (chlorine in NaClO). The specific measurement procedure is as follows: First, the sample is precisely weighed, and water, potassium iodide, and acetic acid are added and left to stand. The liberated iodine is titrated with a sodium thiosulfate solution using a starch aqueous solution as an indicator to measure the available chlorine concentration.

[0024] The cellulosic raw material is not particularly limited as long as it is a material mainly composed of cellulose, and examples thereof include pulp, natural cellulose, and fine cellulose obtained by depolymerizing cellulose through mechanical treatment. As the cellulosic raw material, commercially available products such as crystalline cellulose made from pulp can be used as is. In addition, unused biomass containing a large amount of cellulose components, such as soybean pulp refuse or soybean hulls, can also be used as the raw material. The main component of plants is cellulose, and bundles of cellulose molecules are called cellulose microfibrils. The cellulose in cellulosic raw materials is also contained in the form of cellulose microfibrils.

[0025] [N-oxyl compounds] The cellulose contained in the cellulose microparticles according to the present embodiment is preferably substantially free of N-oxyl compounds. By being substantially free of N-oxyl compounds, the impact on the environment and human body is sufficiently reduced, resulting in high safety. Examples of N-oxyl compounds include 2,2,6,6-tetramethylpiperidine-1-oxyl (TEMPO).

[0026] As used herein, "substantially free of N-oxyl compounds" means that no N-oxyl compounds are used in the production of oxidized cellulose, that the oxidized cellulose contains no N-oxyl compounds at all, or that the content of N-oxyl compounds is 2.0 ppm by mass or less, and preferably 1.0 ppm by mass or less, relative to the total amount of oxidized cellulose. In addition, when the content of N-oxyl compounds is, as an increase from the cellulosic raw material, preferably 2.0 mass ppm or less, more preferably 1.0 mass ppm or less, it is also considered to be "substantially free of N-oxyl compounds."

[0027] The content of N-oxyl compounds can be measured by known means, such as a method using a trace total nitrogen analyzer (for example, TN-2100H manufactured by Nitto Seiko Analytech Co., Ltd.).

[0028] [Crystal structure] The cellulose contained in the cellulose microparticles according to this embodiment has a type I crystal structure. The type I crystal structure is the structure possessed by natural cellulose. For example, when natural cellulose is treated with alkali or dissolved in a solvent and then solidified, the type I crystal structure changes to a type II crystal structure. Therefore, when cellulose has a type I crystal structure, it means that the cellulose microparticles have been produced without undergoing a process such as alkali treatment or dissolution treatment.

[0029] [Crystallization] The crystallinity of the cellulose contained in the cellulose fine particles according to this embodiment is preferably 20 to 80%, more preferably 30 to 80%, even more preferably 40 to 75%, and particularly preferably 50 to 70%.

[0030] Crystallinity is measured by the solid phase for freeze-dried cellulose. 13 C-NMR measurement can be performed and the C4 peak can be calculated from the peak of the fourth carbon atom (C4) of cellulose. Specifically, the C4 peak appears in the range of about 80 to 95 ppm, with the peaks of the crystalline portion (higher ppm side, about 85 to 95 ppm) and the amorphous portion (lower ppm side) overlapping, so the area of ​​each peak can be divided by the vertical division method and the C4 peak can be determined from the following formula. A more specific measurement method is described in the Examples below. Crystallinity=SC / (SC+SA)×100 [In the formula, SC is the crystalline portion, and SA is the amorphous portion.]

[0031] [Carboxylic group amount] The amount of carboxy groups in the cellulose contained in the cellulose microparticles according to this embodiment is preferably 0.1 to 3.0 mmol / g, more preferably 0.2 to 2.0 mmol / g, even more preferably 0.3 to 1.5 mmol / g, particularly preferably 0.4 to 1.2 mmol / g, and most preferably 0.5 to 0.9 mmol / g. When the amount of carboxy groups is within the above range, the feel of the cellulose microparticles can be further improved, and when the cellulose microparticles are blended in cosmetics, for example, the feel of the cosmetics can be further improved. The amount of carboxy groups in the cellulose contained in the cellulose fine particles is substantially the same as the amount of carboxy groups in the cellulose contained in the dispersion liquid that is spray-dried to produce the cellulose fine particles, as described below.

[0032] The amount of carboxyl groups in cellulose can be measured by the method described in the Examples below. The amount of carboxyl groups can be adjusted by changing the reaction time, reaction temperature, pH of the reaction solution, etc. of the oxidation reaction of the cellulosic raw material.

[0033] The cellulose contained in the cellulose microparticles according to this embodiment preferably has a structure in which at least two of the hydroxyl groups of the glucopyranose ring constituting the cellulose are oxidized, more specifically, the cellulose preferably has a structure in which the hydroxyl groups at the second and third positions of the glucopyranose ring are oxidized and a dicarboxyl group is introduced. Furthermore, it is preferable that the hydroxyl group at the sixth position of the glucopyranose ring is not oxidized and remains as a hydroxyl group. Note that the position of the carboxyl group on the glucopyranose ring is determined by the solid 13 It can be analyzed by C-NMR spectroscopy.

[0034] Rayon has the same chemical structure as cellulose, and its oxide (rayon oxide) is water-soluble. 13By C-NMR measurement, a carbon peak attributable to the carboxy group is observed at 165 to 185 ppm. In one embodiment of the oxidation of a cellulosic raw material with hypochlorous acid or its salt, two signals appear in this chemical shift range. Furthermore, by solution two-dimensional NMR measurement, it can be determined that the carboxy groups are introduced at the 2- and 3-positions.

[0035] Solid oxide of cellulosic raw materials with hypochlorous acid or its salts 13 In C-NMR, when the amount of carboxyl groups introduced is large, two signals appear at 165 to 185 ppm, and when the amount of carboxyl groups introduced is small, a very broad signal may appear. As can be seen from the results for oxidized rayon, the signals of the carboxyl group carbons introduced at the 2nd and 3rd positions are close to each other, and this is difficult to achieve with low-resolution solid state spectroscopy. 13 In C-NMR, the separation of the two signals is insufficient. Therefore, when the amount of carboxyl group introduced is small, a broad signal is observed. 13 In the C-NMR spectrum, the introduction of carboxy groups at the 2nd and 3rd positions can be confirmed by evaluating the broadening of the peaks appearing at 165 to 185 ppm.

[0036] That is, solid 13 A baseline is drawn around the peak in the range of 165 ppm to 185 ppm in the C-NMR spectrum to determine the overall area value, and then the area value is vertically divided at the peak top to determine the ratio of the two peak area values ​​(large area value / small area value). If the ratio of the peak area values ​​is 1.2 or more, the peak can be said to be broad. The presence or absence of the broad peak can be determined by the ratio of the length L of the baseline in the range of 165 ppm to 185 ppm to the length L' of the perpendicular line from the peak top to the baseline. That is, if the ratio L' / L is 0.1 or more, it can be determined that a broad peak is present. The ratio L' / L may be 0.2 or more, 0.3 or more, 0.4 or more, or even 0.5 or more. There is no particular upper limit to the ratio L' / L, but it is usually 3.0 or less, and may be 2.0 or less, or 1.0 or less.

[0037] The structure of the glucopyranose ring can also be determined by analysis according to the method described in Sustainable Chem. Eng. 2020, 8, 48, 17800-17806.

[0038] [Viscosity average degree of polymerization] The cellulose contained in the cellulose microparticles according to this embodiment has a viscosity-average degree of polymerization of 30 to 500. The viscosity-average degree of polymerization is preferably 60 to 300, more preferably 70 to 150, and even more preferably 80 to 130. When the viscosity-average degree of polymerization is within the above range, the length of the nanofibers constituting the cellulose microparticles becomes relatively short, which is advantageous in that the cellulose microparticles tend to return to a spherical shape when swollen. The viscosity-average degree of polymerization of the cellulose contained in the cellulose fine particles is substantially the same as the viscosity-average degree of polymerization of the cellulose contained in the dispersion liquid that is spray-dried to produce the cellulose fine particles, as described below.

[0039] The viscosity-average degree of polymerization of cellulose can be adjusted by changing the reaction time, reaction temperature, pH of the reaction solution, defibration conditions, etc. of the oxidation reaction of the cellulosic raw material.

[0040] The viscosity-average degree of polymerization is the average degree of polymerization measured by a viscosity method, and can be measured by the method described in the examples.

[0041] [Nanocellulose] The cellulose contained in the cellulose fine particles according to this embodiment is preferably nanocellulose.

[0042] Nanocellulose is a general term for micronized cellulose, including micronized cellulose fibers and cellulose nanocrystals. Micronized cellulose fibers are also called cellulose nanofibers (CNF).

[0043] The cellulose preferably has an anion-modified group. The "anion-modified group" refers to a group that generates an anion. Examples of the anion-modified group include a carboxy group, a phosphate ester group, a phosphite ester group, a sulfate ester group, and a xanthate ester group, and the carboxy group is preferred. The anion-modified group may be in the form of a salt. The anion-modified group preferably has a proton or a divalent or higher cation. When the anion-modified group has a divalent or higher cation, the divalent or higher cation is preferably shared by a plurality of anion-modified groups. Examples of the divalent or higher cation include Mg 2+ , Ca 2+ , Ba 2+ , Al 3+ , Fe 2+ , Fe 3+ , Ti 4+ , Zr 4+ etc.

[0044] It is presumed that the formation of crosslinks between cellulose molecules through hydrogen bonds when the anion-modifying group has a proton, or through the cations when the anion-modifying group has a cation with a valence of two or more, contributes to the formation of cellulose microparticles, but the present invention is not limited by this presumption in any way.

[0045] Examples of methods for producing cellulose having a carboxy group as an anion-modifying group include oxidation of cellulose, mercerization and etherification of cellulose, and acid modification of cellulose.

[0046] Examples of methods for producing cellulose having a phosphate ester group as an anion-modified group include reacting cellulose with a compound having a phosphate group (for example, phosphoric acid, sodium dihydrogen phosphate, and disodium hydrogen phosphate).

[0047] An example of a method for producing cellulose having a phosphite ester group as an anion-modifying group is a reaction of cellulose with a phosphorus oxoacid (sodium hydrogen phosphate or sodium hydrogen phosphite) and urea.

[0048] An example of a method for producing cellulose having sulfate ester groups as anion-modified groups is a reaction of cellulose with a solution containing dimethyl sulfoxide, acetic anhydride, and sulfuric acid.

[0049] A method for producing cellulose having a xanthate ester group as an anion-modified group includes, for example, a reaction between alkali-treated cellulose and carbon disulfide.

[0050] Nanocellulose is a collection of individual fibers. When nanocellulose contains carboxylated nanocellulose, it is sufficient that it contains at least one carboxylated nanocellulose, and it is preferable that carboxylated nanocellulose is the main component. Here, carboxylated nanocellulose being the main component means that the proportion of carboxylated nanocellulose in the total amount of nanocellulose exceeds 50% by mass, preferably exceeds 70% by mass, and more preferably exceeds 80% by mass. The upper limit of the above proportion is 100% by mass, but it may also be 98% by mass or 95% by mass.

[0051] (average fiber length) The average fiber length of nanocellulose is preferably 50 to 700 nm, more preferably 50 to 500 nm, even more preferably 50 to 300 nm, still more preferably 60 to 300 nm, and particularly preferably 70 to 200 nm. When the average fiber length is within the above range, the cellulose microparticles have the characteristic of easily deforming into perfect spheres when swollen with water.

[0052] (average fiber width) The average fiber width of nanocellulose is preferably 1 to 200 nm, more preferably 1 to 15 nm, even more preferably 1 to 10 nm, and even more preferably 1 to 5 nm. When the average fiber width is within this range, the cellulose microparticles have the characteristic of easily deforming into perfect spheres when swollen with water.

[0053] The average fiber width and average fiber length of nanocellulose are calculated by mixing nanocellulose with water to a nanocellulose concentration of approximately 1 to 10 ppm, air-drying the resulting diluted cellulose aqueous dispersion on a mica substrate, observing the shape of the nanocellulose using a scanning probe microscope, randomly selecting any number of fibers from the obtained image, and calculating the cross-sectional height of the shape image = fiber width and the perimeter divided by 2 = fiber length. Image processing software can be used to calculate these average fiber widths and lengths. While the image processing conditions are arbitrary, differences in calculated values ​​may occur even for the same image depending on the conditions. The range of difference in values ​​depending on the conditions is preferably within ±100 nm for average fiber length. The range of difference in values ​​depending on the conditions is preferably within ±10 nm for average fiber width.

[0054] Specifically, the average fiber length and the average fiber width can be measured according to the following method. The shape of nanocellulose was observed in AC mode using the Oxford Asylum MFP-3D infinity scanning probe microscope. The average fiber length is calculated by binarizing the image obtained using the image processing software "ImageJ" and analyzing it. For 100 or more fibers, the average fiber length is calculated as fiber length = "perimeter" ÷ 2. The average fiber width is calculated using the software provided with the "MFP-3D infinity" for 50 or more fibers, with the number average fiber width calculated as the cross-sectional height of the shape image = fiber width.

[0055] (aspect ratio) The aspect ratio of nanocellulose (average fiber length / average fiber width) is preferably 20 to 200, more preferably 30 to 190, and even more preferably 40 to 180. When the aspect ratio is within this range, the cellulose microparticles have the characteristic of easily deforming into perfect spheres when swollen with water.

[0056] (zeta potential) The zeta potential of nanocellulose is preferably -30 mV or less, more preferably -90 mV or more and -30 mV or less, even more preferably -80 mV or more and -30 mV or less, even more preferably -70 mV or more and -30 mV or less, and particularly preferably -65 mV or more and -35 mV or less.

[0057] The zeta potential can be adjusted by changing the reaction time, reaction temperature, stirring conditions, etc. of the oxidation reaction of the cellulosic raw material.

[0058] The zeta potential is a value measured on a cellulose aqueous dispersion prepared by mixing nanocellulose with water to a nanocellulose concentration of 0.1% by mass at pH 8.0 and 20°C. Specifically, it can be measured by the following method. The nanocellulose dispersion is diluted with pure water to a nanocellulose concentration of 0.1%. After dilution, a 0.05 mol / L aqueous solution of sodium hydroxide is added to the aqueous nanocellulose dispersion to adjust the pH to 8.0, and the zeta potential is measured at 20°C using an Otsuka Electronics Zeta Potential Meter (ELSZ-1000).

[0059] (light transmittance) Nanocellulose dispersions in which nanocellulose is dispersed in a dispersion medium exhibit low light scattering by cellulose fibers and can exhibit high light transmittance. Specifically, the light transmittance of a mixture of nanocellulose and water to a solids concentration of 0.1% by mass is preferably 95% or higher, more preferably 96% or higher, even more preferably 97% or higher, and particularly preferably 99% or higher. The light transmittance is the value measured at a wavelength of 660 nm using a spectrophotometer.

[0060] The light transmittance can be adjusted by changing the reaction time, reaction temperature, stirring conditions, etc. of the oxidation reaction of the cellulosic raw material.

[0061] The light transmittance can be measured by the following method. An aqueous dispersion of nanocellulose with a solid content of 0.1% by mass is placed in a 10 mm thick quartz cell, and the light transmittance at a wavelength of 660 nm is measured using a spectrophotometer (JASCO V-550).

[0062] [Polycarboxylic acid modified / phosphoric acid] The cellulose contained in the cellulose microparticles according to this embodiment is preferably modified with a polycarboxylic acid and / or phosphoric acid. In particular, when the cellulose has a carboxy group as an anion-modifying group, the cellulose is preferably modified with a polycarboxylic acid and / or phosphoric acid. The cellulose being modified with a polycarboxylic acid and / or phosphoric acid means that the cellulose is bonded to a polycarboxylic acid and / or phosphoric acid. The bond is preferably a covalent bond, more preferably an ester bond. The ester bond is preferably composed of oxygen (O) derived from a hydroxyl group of the cellulose and a carbonyl group (CO) derived from a polycarboxylic acid and / or phosphoric acid.

[0063] The polycarboxylic acid is not particularly limited as long as it is a compound having two or more carboxylic acid groups or an anhydride thereof, and examples of the polycarboxylic acid include a dicarboxylic acid and an anhydride thereof, and a tricarboxylic acid and an anhydride thereof. Examples of dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, phthalic acid, isophthalic acid, and terephthalic acid. Examples of tricarboxylic acids include citric acid, isocitric acid, aconitic acid, tricarballylic acid, hemimellitic acid, and trimellitic acid.

[0064] The (total) amount of polycarboxylic acid and / or phosphoric acid is preferably 2 to 30 mass %, more preferably 4 to 25 mass %, even more preferably 6 to 20 mass %, and particularly preferably 8 to 15 mass %, based on the mass of cellulose. When the amount of polycarboxylic acid and / or phosphoric acid is within the above range, the particle size, circularity, and shape retention of the cellulose microparticles are further improved.

[0065] It is presumed that the polycarboxylic acid and / or phosphoric acid exerts its function by forming crosslinks between cellulose molecules, but the present invention is not limited to this presumption.

[0066] [Average particle size] The cellulose microparticles according to this embodiment preferably have an average particle size of 0.1 to 200 μm. The average particle size is preferably 0.5 to 50 μm, more preferably 1 to 30 μm, even more preferably 2 to 15 μm, and particularly preferably 5 to 10 μm. When the average particle size is within this range, the feel of the cellulose microparticles can be further improved, and when the cellulose microparticles are blended into cosmetics, for example, the feel of the cosmetics can be further improved.

[0067] The average particle size can be determined by measuring the particle size (circle equivalent diameter) of each of 100 microparticles from an image of the cellulose microparticles obtained using a microscope and calculating the average value, as described in the Examples below.

[0068] [Average circularity] The cellulose microparticles according to this embodiment preferably have an average circularity of 0.5 to 1 when left to stand in pure water for 30 minutes. The average circularity is preferably 0.6 to 1, more preferably 0.7 to 1, even more preferably 0.8 to 1, and particularly preferably 0.9 to 1. When the average circularity is within the above range, the feel of the cellulose microparticles can be further improved, and when the cellulose microparticles are blended into cosmetics, for example, the feel of the cosmetics can be further improved.

[0069] The average circularity can be determined by measuring the circularity of 100 individual microparticles from an image of the cellulose microparticles taken using a microscope and calculating the average value. The circularity of each microparticle can be determined from the perimeter of a circle having an area equal to that of each microparticle (circular equivalent perimeter) and the actual perimeter of each microparticle (actually measured perimeter) according to the following formula. The closer the circularity is to 1, the closer the shape of the microparticle is to a perfect circle. Circularity = Equivalent perimeter / Actual perimeter The specific method is as described in the Examples below.

[0070] [Water absorption rate] The cellulose microparticles according to this embodiment preferably have a water absorption capacity of 1 to 10 times when spray-dried at 170°C. The water absorption capacity is preferably 1.5 to 7 times, and more preferably 2 to 5 times. When the water absorption capacity is within the above range, the feel of the cellulose microparticles can be further improved, and when the cellulose microparticles are blended into cosmetics, for example, the feel of the cosmetics can be further improved.

[0071] The water absorption capacity can be determined according to the following formula using the mass of 1.0 g of microparticles (dried microparticles) spray-dried at 170°C and the mass of the microparticles (swollen microparticles) obtained by leaving the dried microparticles in pure water for 30 minutes and then removing the unabsorbed water. Water absorption ratio = [mass of swollen particles - mass of dry particles] / mass of dry particles

[0072] [Application] The cellulose microparticles according to this embodiment can be used in a variety of applications, including, for example, cosmetics.

[0073] <Cosmetics> One embodiment of the present invention relates to a cosmetic product comprising the above-mentioned cellulose microparticles.

[0074] The amount of cellulose fine particles is preferably 0.1 to 40% by mass, more preferably 0.5 to 30% by mass, and even more preferably 1 to 25% by mass, based on the mass of the cosmetic product. When the amount of cellulose fine particles is within this range, the feel of the cosmetic product can be further improved.

[0075] Examples of cosmetics include foundation, emulsion, lipstick, beauty serum, moisturizing cream, eye shadow, etc.

[0076] <Method for producing cellulose microparticles (first production method)> One embodiment of the present invention is a method for producing microparticles comprising cellulose, comprising the steps of: The method includes a step of spray-drying a cellulose dispersion to obtain microparticles containing the cellulose, The cellulose is an oxidation product of a cellulose-based raw material with hypochlorous acid or a salt thereof, and is substantially free of N-oxyl compounds; At least one of the following conditions 1 to 3 is met: Condition 1: the pH of the dispersion is 1.5 to 5.8; Condition 2: The cellulose contained in the dispersion is modified with a polycarboxylic acid and / or phosphoric acid; Condition 3: the cellulose contained in the dispersion has a carboxy group, and the carboxy group has a proton or a divalent or higher cation; The term "having a proton or a divalent or higher cation" means "having -COOH or -COO - X [wherein X is a divalent or higher cation].

[0077] The production method according to this embodiment includes a step of spray-drying a cellulose dispersion to obtain fine particles containing the cellulose (referred to as a "spray-drying step"). The production method according to this embodiment may include an oxidation step and a modification step, which will be described later. The production method according to this embodiment preferably does not include a cellulose defibration treatment step prior to the spray drying step. By not including the defibration treatment step, cellulose microparticles can be produced easily and at low cost.

[0078] The production method according to this embodiment preferably consists essentially of an oxidation step and a spray-drying step, or consists essentially of an oxidation step, a modification step, and a spray-drying step. The production method according to this embodiment preferably comprises only an oxidation step and a spray-drying step, or comprises only an oxidation step, a modification step, and a spray-drying step.

[0079] [Oxidation process] The oxidation step is a step of oxidizing a cellulosic raw material. In the oxidation step, the cellulosic raw material is oxidized with hypochlorous acid or a salt thereof without using an N-oxyl compound. Details of the cellulosic raw material and hypochlorous acid or a salt thereof are as described in the above [Hypochlorous Acid Oxidation] section. Details of the N-oxyl compound are as described in the above [N-oxyl Compound] section. Specific methods for the oxidation step include, for example, the methods described in WO 2022 / 009979 and WO 2022 / 009980.

[0080] An example of an oxidation product of a cellulosic raw material with hypochlorous acid or a salt thereof is Aronfibro (registered trademark) manufactured by Toagosei Co., Ltd.

[0081] [Denaturation process] The modification step is a step of modifying cellulose with a polycarboxylic acid and / or phosphoric acid. In the modification step, cellulose oxidized with hypochlorous acid or its salt is reacted with a polycarboxylic acid and / or phosphoric acid to form a bond. Details of the bond type, the type and amount of polycarboxylic acid and / or phosphoric acid, etc. are as described above in the section [Modification with polycarboxylic acid / phosphoric acid].

[0082] [Spray drying process] The spray-drying step is a step of spray-drying a cellulose dispersion to obtain fine particles containing the cellulose. The spray-drying step satisfies at least one, preferably at least two, and more preferably all of the above "Condition 1" to "Condition 3."

[0083] By satisfying the above-mentioned "Condition 1" in the spray drying step, cellulose microparticles excellent in particle size, circularity, and shape retention can be produced. The pH of the dispersion in "Condition 1" is preferably 1.5 to 5.8, more preferably 2.0 to 5.0, and even more preferably 2.0 to 4.0. The pH of the dispersion can be adjusted by adding an acid or a base to the dispersion.

[0084] By satisfying the above-mentioned "Condition 2" in the spray-drying step, it is possible to produce cellulose microparticles that are excellent in particle size, circularity, and shape retention. Details of "Condition 2" are as described in the above section on [Modification step].

[0085] By satisfying the above-mentioned "Condition 3" in the spray-drying step, cellulose microparticles excellent in particle size, circularity, and shape retention can be produced. "Condition 3" can be satisfied, for example, by reacting cellulose with an acid or a compound containing a specific cation.

[0086] The dispersion medium contained in the dispersion liquid is not particularly limited, but is preferably a dispersion medium that does not dissolve cellulose, and from the viewpoint of safety, is more preferably water.

[0087] The cellulose contained in the dispersion preferably has a type I crystal structure. Details of the type I crystal structure are as described above in the section [Crystal Structure].

[0088] The cellulose contained in the dispersion preferably has a crystallinity of 20 to 80%. Details of the crystallinity are as described above in the column [Crystallinity].

[0089] The cellulose contained in the dispersion preferably has a carboxyl group amount of 0.1 to 3.0 mmol / g. Details of the carboxyl group amount are as described above in the [Carboxy group amount] section.

[0090] The cellulose contained in the dispersion preferably has a viscosity-average degree of polymerization of 30 to 500. Details of the viscosity-average degree of polymerization are as described above in the column [Viscosity-average degree of polymerization].

[0091] The amount of cellulose contained in the dispersion is preferably 0.1 to 30% by mass, more preferably 1.0 to 25% by mass, even more preferably 2.5 to 20% by mass, and particularly preferably 3.0 to 15% by mass, based on the mass of the dispersion. When the amount of cellulose contained in the dispersion is within the above range, the production efficiency of cellulose microparticles can be improved. On the other hand, if the concentration is too high, the viscosity increases, which may clog the nozzle of the spray drying. Cellulose oxidized with hypochlorous acid or a salt thereof is less likely to increase in viscosity when prepared as an aqueous dispersion, and therefore can be handled at a high concentration.

[0092] It is preferable that the cellulose contained in the dispersion has not been subjected to a defibration treatment. In other words, it is preferable that the cellulose has not been subjected to a defibration treatment step before the spray-drying step. In this specification, the "defibration treatment step" is an independent process aimed at defibrating cellulose into nanocellulose. Note that cellulose oxidized with hypochlorous acid or its salt is easily defibrated, so even if a defibration treatment step is not performed (for example, even if it is gently mixed with other components), some of the cellulose may be defibrated, but this does not constitute defibration treatment. In this specification, the term "defibration treatment" refers to a process in which most of the cellulose (for example, 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more) is defibrated into nanocellulose.

[0093] The cellulose contained in the cellulose fine particles is preferably defibrated into nanocellulose, the details of which are as described in the above section [Nanocellulose]. Cellulose oxidized with hypochlorous acid or its salts is easily defibrated, so when cellulose that has not been defibrated is spray-dried, the cellulose can be defibrated into nanocellulose during the process of forming cellulose microparticles.

[0094] The preferred average particle size, average circularity, and water absorption capacity of the cellulose fine particles are as described above in detail in the columns [Average particle size], [Average circularity], and [Water absorption capacity].

[0095] The spray drying may be carried out using a commercially available spray dryer, and the spray drying conditions may be adjusted appropriately depending on the composition of the dispersion to be prepared.

[0096] <Method for producing cellulose microparticles (second production method)> One embodiment of the present invention is a method for producing microparticles comprising cellulose, comprising the steps of: a step of spray-drying a cellulose dispersion to obtain fine particles containing the cellulose (spray-drying step), The cellulose contained in the dispersion has a type I crystal structure, the cellulose contained in the dispersion has a viscosity-average degree of polymerization of 30 to 500, The cellulose contained in the dispersion has an anion-modified group, and the anion-modified group has a proton or a divalent or higher valent cation. Regarding the manufacturing method.

[0097] The production method according to this embodiment may include the oxidation step and modification step described in the section <Production method of cellulose fine particles (first production method)> above. The production method according to this embodiment preferably does not include a cellulose defibration treatment step prior to the spray drying step. By not including the defibration treatment step, cellulose microparticles can be produced easily and at low cost.

[0098] The production method according to this embodiment preferably consists essentially of an oxidation step and a spray-drying step, or consists essentially of an oxidation step, a modification step, and a spray-drying step. The production method according to this embodiment preferably comprises only an oxidation step and a spray-drying step, or comprises only an oxidation step, a modification step, and a spray-drying step.

[0099] For details of the production method according to this embodiment, the contents described above in the section <Production method of cellulose microparticles (first production method)> can be cited. [Example]

[0100] The present invention will be described in more detail below using examples and comparative examples, but the technical scope of the present invention is not limited to these. Various values ​​in the examples may be used as preferred lower or upper limits in the embodiments of the present invention. Two values ​​of the same type in the examples may be appropriately combined to form a preferred numerical range.

[0101] <Measurement of carboxyl group amount> To 60 ml of an oxidized cellulose aqueous dispersion, in which the oxidized cellulose concentration had been adjusted to 0.5% by mass, 0.1 M aqueous hydrochloric acid was added to adjust the pH to 2.5, and then 0.05 N aqueous sodium hydroxide solution was added dropwise, and the electrical conductivity was measured until the pH reached 11.0. The amount of carboxyl groups (mmol / g) was calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, in which the change in electrical conductivity was gradual. Amount of carboxyl group = a (ml) x 0.05 / mass of oxidized cellulose (g)

[0102] <Measurement of average degree of polymerization> Oxidized cellulose was added to a sodium borohydride solution adjusted to pH 10 and reduced at 25°C for 5 hours. The amount of sodium borohydride was 0.1 g per 1 g of oxidized cellulose fiber. After reduction, solid-liquid separation was performed by suction filtration, followed by washing with water. The resulting oxidized cellulose fiber was freeze-dried. 0.04 g of dried oxidized cellulose fiber was added to 10 ml of purified water and stirred for 2 minutes. 10 ml of 1 mol / L copper ethylenediamine solution was then added to dissolve the fiber. The flow times of the blank solution and the cellulose solution were then measured at 25°C using a capillary viscometer. The relative viscosity (ηr), specific viscosity (ηsp), and intrinsic viscosity (η) were calculated sequentially from the flow times of the blank solution (t0), the flow times of the cellulose solution (t), and the concentration of oxidized cellulose fiber (c [g / ml]) using the following equations. The degree of polymerization (DP) of the oxidized cellulose fiber was then calculated using the following viscometric equation. ηr=η / η0=t / t0 ηsp=ηr-1 [η]=ηsp / (100×c(1+0.28ηsp)) DP=175×[η]

[0103] [Crystallization degree] Crystallinity was measured by the solid-state method for freeze-dried cellulose. 13 C-NMR measurements were performed, and the degree of crystallinity was calculated from the peak of the fourth carbon (C4) of cellulose. Specifically, the C4 peak appears in the range of approximately 80 to 95 ppm, with peaks from the crystalline portion (higher ppm side, approximately 85 to 95 ppm) and the amorphous portion (lower ppm side) overlapping, and the area of ​​each peak was divided by the vertical division method (crystalline portion: SC, amorphous portion: SA). The degree of crystallinity was calculated using the following formula. Crystallinity=SC / (SC+SA)×100 solid 13 C-NMR measurements were performed under the following conditions. Equipment: JNM-ECA, JEOL Frequency: 15kHz Measurement method: CP / MAS method Wait time: 5 seconds Accumulation count: 10,000 times

[0104] [Example 1] (oxidation process) 500 g of sodium hypochlorite solution with a pH of 12.7 and an available chlorine concentration of 12.5% ​​by mass was placed in a jacketed glass vessel and stirred at 200 rpm using a mixer with three swept-back blades (Three-One Motor, BL600, manufactured by Shinto Scientific Co., Ltd.) while heating to 35°C. Then, 47 g of cellulosic raw material (KC Flock W-100GK, powdered pulp manufactured by Nippon Paper Industries Co., Ltd.) was added. The mixture was stirred at 35°C until the pH dropped to 10.5. Then, 25% by mass of sodium hydroxide solution was added to maintain the pH of the reaction system at 10.5. The mixture was stirred under the same conditions for a total of 520 minutes after the cellulosic raw material was added. After the reaction was completed, the remaining sodium hypochlorite was inactivated with aqueous hydrogen peroxide, and then hydrochloric acid was added to convert the carboxyl groups of the resulting oxidized cellulose from the salt form (-COO-Na) to the proton form (-COO-H). The proton-form oxidized cellulose aqueous dispersion was subjected to solid-liquid separation by pressure filtration at 0.2 MPa and washed with aqueous hydrochloric acid at pH 2.5 to obtain a proton-form oxidized cellulose aqueous dispersion at pH 2.5.

[0105] (spray drying process) Pure water was added to a proton-type oxidized cellulose aqueous dispersion at pH 2.5 to a solids concentration of 2.7% by mass, yielding a proton-type oxidized cellulose aqueous dispersion at pH 2.7. This oxidized cellulose aqueous dispersion was spray-dried using a spray dryer (Tokyo Rikakikai SD-1000, two-fluid nozzle) to obtain cellulose microparticles. The crystallinity of the cellulose contained in the cellulose microparticles was in the range of 20-80%. The spray drying conditions were as follows: Inlet temperature: 170℃ Outlet temperature: 85℃ Blower flow rate: 0.3m 3 / min Atomizer pressure: 6 x 10 kPa

[0106] (Properties of oxidized cellulose) The amount of carboxyl groups in the oxidized cellulose obtained in the oxidation step was measured using the method described above and found to be 0.78 mmol / g. Furthermore, when the nitrogen content derived from N-oxyl compounds in the oxidized cellulose was measured using a trace total nitrogen analyzer (TN-2100H manufactured by Nitto Seiko Analytech Co., Ltd.), the increase from the raw pulp was found to be less than 1 ppm. The crystallinity of the oxidized cellulose was 55%. The viscosity-average degree of polymerization of the oxidized cellulose was 110.

[0107] [Example 2] Sodium hydroxide was added to the proton-type oxidized cellulose aqueous dispersion at pH 2.5 obtained in the oxidation step of Example 1, converting the carboxyl groups of the oxidized cellulose from the proton-type (-COO-H) back to the salt-type (-COO-Na), thereby obtaining a salt-type oxidized cellulose aqueous dispersion at pH 7.4. Pure water was added to the salt-form oxidized cellulose aqueous dispersion to a solids concentration of 3.5% by mass, and 10 parts by mass of citric acid per 100 parts by mass of oxidized cellulose was added and stirred until uniform, yielding a modified oxidized cellulose aqueous dispersion with a pH of 3.7. This modified oxidized cellulose aqueous dispersion was spray-dried in the same manner as in Example 1 to obtain cellulose microparticles.

[0108] [Example 3] Cellulose microparticles were obtained in the same manner as in Example 2, except that the amount of citric acid in Example 2 was changed from "10 parts by mass" to "5 parts by mass." The pH of the modified oxidized cellulose aqueous dispersion to be spray-dried was 4.0.

[0109] [Comparative Example 1] Pure water was added to the aqueous dispersion of oxidized cellulose in the salt form (—COO—Na) with a pH of 7.4 obtained in Example 2 so that the solids concentration was 3.5% by mass, yielding an aqueous dispersion of oxidized cellulose in the salt form with a pH of 7.0. This aqueous dispersion of oxidized cellulose was spray-dried in the same manner as in Example 1, yielding cellulose microparticles.

[0110] Comparative Example 2 The same procedure as in Example 1 was carried out, except that oxidized cellulose obtained by TEMPO oxidation ("TEMPO-oxidized cellulose") was used. The viscosity-average degree of polymerization of the TEMPO-oxidized cellulose was 550. Because the viscosity-average degree of polymerization of TEMPO-oxidized cellulose is high, the viscosity of the TEMPO-oxidized cellulose dispersion was high, and the solids concentration had to be diluted to 0.1% for spray drying. Because the solids concentration was too low, the spray drying was insufficient, and even after drying, the amount of particles produced was so small that evaluation was not possible.

[0111] The oxidized cellulose used in Comparative Example 2 was produced according to the following method. 0.016 g of TEMPO and 0.1 g of sodium bromide were placed in a beaker, and purified water was added and stirred to form an aqueous solution, to which 1.0 g of powdered pulp (KC Flock W-100GK) from Nippon Paper Industries Co., Ltd. was added as a cellulosic raw material. The above aqueous solution was heated to 25 ° C in a thermostatic water bath while stirring with a stirrer, and then 0.1 mol / L sodium hydroxide was added and stirred to obtain an aqueous solution of pH 10.0. 2.58 g of an aqueous solution of sodium hypochlorite with an effective chlorine concentration of 13.2% by mass was added thereto, and while keeping the temperature at 25 ° C in the same thermostatic water bath, 0.1 mol / L sodium hydroxide was added to adjust the pH during the reaction to 10.0, and the solution was stirred with a stirrer for 120 minutes. After the reaction was completed, the product was subjected to solid-liquid separation by suction filtration using a PTFE membrane filter with 0.1 μm openings, yielding oxidized cellulose. The filtered product was washed with pure water and then the amount of carboxyl groups was measured. The amount of carboxyl groups was 1.55 mmol / g, and the amount of the filtered product was about 1.0 g. The nitrogen content derived from N-oxyl compounds in the oxidized cellulose was measured using a trace total nitrogen analyzer (manufactured by Nitto Seiko Analytech Co., Ltd., device name: TN-2100H), and the increase from the raw pulp was calculated to be 5 ppm.

[0112] <Evaluation of cellulose microparticles> Pure water was added to the cellulose microparticles, and the mixture was allowed to stand for 30 minutes. The average particle size, average circularity, and shape retention were then evaluated using the following methods. The results are shown in Table 1.

[0113] [Average particle size] An image of the cellulose microparticles was obtained using a microscope (Nikon Corporation ECLIPSE LV100ND). 100 cellulose microparticles were randomly selected from the image, and the particle diameter of each microparticle was measured. The average value was used as the average particle diameter. The particle diameter of each microparticle was measured as the diameter of a circle having an area equal to that of each microparticle (circle equivalent diameter).

[0114] [Average circularity] From the images of cellulose microparticles obtained in the above [Average particle size], 100 cellulose microparticles were randomly selected, and the circularity of each microparticle was measured using the measurement system of the microscope, and the average value was taken as the average circularity. The circularity of each microparticle was measured using the perimeter of a circle having an area equal to that of each microparticle (circular equivalent perimeter) and the actual perimeter of each microparticle (actual measured perimeter) according to the following formula. Circularity = Equivalent perimeter / Actual perimeter

[0115] [Shape retention performance] From the images of the cellulose microparticles obtained in the above [Average particle diameter], 100 cellulose microparticles were randomly selected, and the shape retention performance was evaluated according to the following evaluation criteria. (Evaluation criteria) A: 90% or more of the particles do not collapse due to swelling and maintain their shape. B: Less than 90% of the particles do not collapse due to swelling and maintain their shape.

[0116] [Table 1]

Claims

1. A microparticle comprising cellulose, The cellulose has a crystal structure of I type, The cellulose has a viscosity average degree of polymerization of 30 to 500, The cellulose has an anion-modified group, and the anion-modified group has a proton or a divalent or higher cation. Fine particles.

2. 2. The microparticle of claim 1, wherein the cellulose is an oxidation product of a cellulosic raw material with hypochlorous acid or a salt thereof, and is substantially free of N-oxyl compounds.

3. The microparticle according to claim 1 , wherein the cellulose is modified with a polycarboxylic acid.

4. The anion-modified group is a carboxy group, The microparticle according to claim 1 , wherein the cellulose is modified with a polycarboxylic acid and / or phosphoric acid.

5. The microparticles according to claim 1, wherein the microparticles have an average particle size of 0.1 to 200 μm.

6. 2. The microparticles according to claim 1, wherein the microparticles have an average circularity of 0.5 to 1 when the microparticles are allowed to stand in pure water for 30 minutes.

7. 2. The microparticles according to claim 1, wherein the microparticles have a water absorption capacity of 1 to 10 times when the microparticles are spray-dried at 170°C.

8. A cosmetic comprising the microparticles according to any one of claims 1 to 7.

9. A method for producing the microparticles according to claim 1, The method includes a step of spray-drying a cellulose dispersion to obtain fine particles containing the cellulose, the cellulose contained in the dispersion having an I-type crystal structure, the cellulose contained in the dispersion has a viscosity average degree of polymerization of 30 to 500; The cellulose contained in the dispersion has an anion-modified group, and the anion-modified group has a proton or a divalent or higher cation. Manufacturing method.

10. A method for producing a cellulose-containing microparticle, comprising the steps of: The method includes a step of spray-drying a cellulose dispersion to obtain microparticles containing the cellulose, The cellulose is an oxidation product of a cellulose-based raw material with hypochlorous acid or a salt thereof, and is substantially free of N-oxyl compounds; At least one of the following conditions 1 to 3: Condition 1: the pH of the dispersion is 1.5 to 5.8; Condition 2: The cellulose contained in the dispersion is modified with a polyvalent carboxylic acid and / or phosphoric acid. Condition 3: the cellulose contained in the dispersion has a carboxy group, and the carboxy group has a proton or a divalent or higher cation; A manufacturing method that satisfies the above requirements.

11. The method according to claim 10 , wherein the cellulose contained in the dispersion has a type I crystal structure.

12. The method according to claim 10, wherein the cellulose contained in the dispersion has a viscosity average degree of polymerization of 30 to 500.

13. The method according to claim 10 , wherein the cellulose contained in the dispersion liquid includes cellulose that has not been defibrated.

14. The method of claim 13 , wherein the cellulose contained in the microparticles comprises nanocellulose.

15. The method according to claim 10, wherein the amount of the cellulose contained in the dispersion is 0.1 to 30% by mass based on the mass of the dispersion.

Citation Information

Patent Citations

  • Method for producing spherical cellulose particles

    JP2976116B2

  • Cellulose derivative particles, method for producing the same, and cosmetics using the same

    JP4022085B2