OPTICAL ISOLATOR FOR WAVELENGTH BAND OF 780-820 nm
A composite oxide with a high Verdet constant and a hollow magnet configuration addresses the size limitations of conventional optical isolators, achieving miniaturization and improved performance in semiconductor lasers by optimizing the Faraday rotator's dimensions.
Patent Information
- Application Number
- JP2023072646
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-26
AI Technical Summary
Conventional optical isolators used in the 780-820 nm wavelength band are too large for modern semiconductor lasers, limiting their integration due to the size of the Faraday rotator materials, which require large magnets for sufficient magnetic flux density.
A composite oxide with a Verdet constant of 0.80 min/(Oe cm) or more, combined with a hollow magnet, is used to create a compact optical isolator by optimizing the Faraday rotator's length and magnetic flux density, allowing for miniaturization.
The solution achieves a high Faraday effect with reduced magnetic field requirements, enabling further miniaturization and improved spatial integration of optical isolators within semiconductor laser devices, reducing absorption and insertion losses.
Smart Images

Figure 2024157950000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical isolator for use in the 780-820 nm wavelength band. [Background technology]
[0002] Semiconductor lasers are the main industrial lasers used for optical recording, medical, and optical measurement. Traditionally, small semiconductor lasers with a wavelength of 780 nm have been used for optical recording on CDs, 800 nm pulse semiconductor lasers for bioimaging using two-photon fluorescence microscopy or second harmonic generation microscopy to visualize biomolecules, and semiconductor lasers with an infrared wavelength range of 780-800 nm have been used for laser length measuring instruments with positioning accuracy of a few nanometers to a few picometers.
[0003] A representative example of this type of semiconductor laser is the Fabry-Perot laser (Fabry-Perot laser diode). The principle of laser oscillation is to use a resonator with two reflective surfaces formed by cleaving a crystal, etc., facing each other at both ends of the path through which light passes, and to emit a laser when stimulated emission becomes stronger than light absorption. The structure of these resonators is very simple, which has the advantage of allowing the laser package to be made smaller, but when the emitted laser light is incident on the coupling end face of an optical fiber, etc., some of it may be reflected and become return light. If this return light is guided into the resonator, it will interfere with the laser light that is originally output, causing the problem of unstable laser output.
[0004] Therefore, for stable operation of the semiconductor laser, it is essential to place an optical isolator between the light source and the workpiece, which has the function of transmitting forward light and blocking reverse light, in order to prevent reflected light from returning to the light emitting element, which is the light source, and to block light that is reflected back from the optical fiber to the light emitting element.
[0005] Incidentally, to function as an optical isolator, a Faraday rotation angle of about 45° is required. Specifically, the polarization plane of light incident on an optical isolator is rotated 45° by the Faraday rotator, and the light passes through the input and output polarizers, each of which has its angle adjusted. On the other hand, the polarization plane of the returning light is rotated 45° in the opposite direction by utilizing the non-reciprocity of the Faraday rotator, and the returning light becomes orthogonal to the input polarizer at 90°, and cannot be transmitted. Optical isolators utilize this phenomenon to transmit light in only one direction, and prevent light from being reflected back.
[0006] An optical isolator with such a function is composed of three main components: a Faraday rotator, a pair of polarizers arranged on the light input side and light output side of the Faraday rotator, and a magnet that applies a magnetic field in the light transmission direction (optical axis direction) of the Faraday rotator. In this optical isolator, when light enters the Faraday rotator, a phenomenon occurs in which the polarization plane rotates inside the Faraday rotator. This phenomenon is generally called the Faraday effect, and the angle by which the polarization plane rotates is called the Faraday rotation angle, and its magnitude θ is expressed by the following equation. θ=V×H×L Here, V is the Verdet constant, which is determined by the material of the Faraday rotator and the measurement wavelength, H is the magnetic flux density, and L is the length of the Faraday rotator (= sample length).
[0007] The factor that determines the size of an optical isolator is the size of the magnet that provides the magnetic flux density H. A larger magnet will have a larger magnetic flux density H, and using a smaller magnet to achieve miniaturization will reduce the magnetic flux density H. Therefore, for a Faraday rotator of the same length, it is necessary to develop a material with a larger Verdet constant.
[0008] Conventionally, the material of Faraday rotators used in the wavelength range of 780 nm to 820 nm has been terbium gallium garnet (TGG) (chemical formula: Tb3Ga5O 12) are known. The Verdet constant of TGG in the 780nm-820nm wavelength band is a small value of 0.25-0.29 min / (Oe·cm), and even the Verdet constant of the TGG single crystal actually used is about 0.27 min / (Oe·cm) at a wavelength of 800nm. With a Verdet constant of about 0.27 min / (Oe·cm), a larger magnet with an outer diameter of φ3.5cm and length of 2.0cm must be used to function as an optical isolator, which causes the problem of the optical isolator becoming larger, making it unsuitable as a material for a Faraday rotator. Note that 1 min represents 1 / 60 degrees.
[0009] Therefore, Patent Document 1 describes an oxide containing terbium oxide at a molar ratio of 50% or more as a material that can be used to miniaturize optical isolators. According to the description, when this oxide is used, the Verdet constant V at a wavelength of 800 nm is 0.62 min / (Oe cm) or more, and the magnetic flux density B (Oe) applied to the Faraday rotator is 0.5×10 4 It is said that it is possible to miniaturize an optical isolator used at the same wavelength when the following is true: Specifically, for an oxide with a molar ratio of 60%, a Faraday rotation angle of 45 degrees was obtained with a magnet with an inner diameter of φ0.4 cm, an outer diameter of φ3.5 cm, and a length of 2.0 cm, which gave a magnetic flux density of 3950 [Oe] (= 0.395 [T]) for a sample length of 1.1 cm. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2015-018145 A Summary of the Invention [Problem to be solved by the invention]
[0011] However, in recent years, in the fields of optical recording, medical, and measurement applications in which semiconductor lasers are used, the package size of semiconductor lasers used in the infrared wavelength band of 780-820 nm has also been reduced, and there is a demand for optical isolators equipped outside this package to be even more compact in the same wavelength band. Since the Faraday rotator described in Patent Document 1 has a Verdet constant of 0.62 min / (Oe·cm) at a wavelength of 800 nm, the magnet size must have an outer diameter of φ3.5 cm and a length of 2.0 cm for a sample length of 1.1 cm. With these dimensions, the optical isolator will be larger than the laser package size, and there will be limitations on the layout of both. Therefore, the realistic outer diameter of a mountable optical isolator is φ1.7 cm or less, which is less than half of φ3.5 cm, and a length of 2.0 cm or less would be more suitable.
[0012] Therefore, conventional terbium oxide material, with a Verdet constant of 0.62 min / (Oe·cm) at a wavelength of 800 nm, was not sufficient to meet this demand.
[0013] The present invention has been made in consideration of the above circumstances, and aims to provide an even smaller optical isolator by combining a Faraday rotator with a large Faraday effect and a magnet with a small outer diameter in the wavelength band of 780 to 820 nm. [Means for solving the problem]
[0014] In order to achieve the above object, an optical isolator for use in the 780-820 nm wavelength band of the present invention is an optical isolator that is made of a composite oxide containing an oxide represented by the following formula (A) as a main component, and that is made of a Faraday rotator having a Verdet constant of 0.80 min / (Oe cm) or more at a wavelength of 800 nm, and a hollow magnet that is disposed on the outer periphery of the Faraday rotator, The sample length L (cm) of the Faraday rotator is within the range of the following formula (1), and the magnetic flux density B (Oe) applied to the Faraday rotator is within the range of the following formula (2). (Tx R 1-x )2O3(A) Here, in the above formula (A), x is 0.8≦x≦1.0, and R includes at least one element selected from the group consisting of the lanthanoid elements other than scandium, yttrium, and Tb (terbium). 0.8≦L≦1.1 (1) B≦0.4×10 4 (2)
[0015] In such an optical isolator, the Verdet constant is large, resulting in a strong Faraday effect, which in turn requires a small magnetic field to obtain a given Faraday rotation angle, and the hollow magnet can be made smaller, thereby enabling the optical isolator to be made even more compact.
[0016] The oxide is preferably a ceramic.
[0017] With such oxides, a Faraday rotator with a large Verdet constant can be easily realized.
[0018] Moreover, it is preferable that the Faraday rotator has an insertion loss of 1 dB or less and an extinction ratio of 30 dB or more within the sample length L (cm).
[0019] Such a Faraday rotator can provide a high-performance optical isolator with low loss and high isolation.
[0020] Moreover, the hollow magnet is preferably made of a neodymium-iron-boron (NdFeB) magnet.
[0021] With such a hollow magnet, it is possible to reliably apply magnetic flux density B to the Faraday rotator even in a small size. Effect of the Invention
[0022] As described above, the optical isolator for the 780-820 nm wavelength band of the present invention has a large Verdet constant, which results in a strong Faraday effect, a smaller magnetic field is required to obtain a specified Faraday rotation angle, and the magnet can be made smaller, thereby achieving even greater miniaturization of the optical isolator. Furthermore, the degree of freedom in terms of spatial dimensions within a laser device incorporating an optical isolator can be increased. Furthermore, since the length can be made shorter than that of a conventional TGG Faraday rotator, the shortening of the length reduces the absorption loss and the insertion loss, which is an important characteristic of an optical isolator. [Brief description of the drawings]
[0023] [Figure 1] 1 is a schematic cross-sectional view showing a configuration example of an optical isolator according to the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing a configuration example of an optical isolator according to Comparative Example 1. FIG. [Diagram 3] FIG. 2 is a wavelength characteristic diagram of the transmittance of the Faraday rotator (without AR coating) used in Example 1 and Comparative Example 1. [Figure 4] 1 is a diagram showing the relationship between the sample length L (0.8 to 1.1 cm) of a Faraday rotator and the magnitude of the magnetic flux density T (104 Oe) at which the Faraday rotation angle is 45 degrees. [Diagram 5] FIG. 11 is a simulation diagram of magnetic flux density for calculating the magnet shape used in the first embodiment. [Figure 6] FIG. 11 is a simulation diagram of magnetic flux density for calculating the magnet shape used in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] As described above, there has been a demand for further miniaturization of optical isolators for the 780-820 nm wavelength band.
[0025] As a result of intensive research by the inventors, it was found that in the wavelength band of 780 nm to 820 nm, in order to keep the magnet outer diameter to φ1.2 cm or less and the length to 2.0 cm or less, the Verdet constant must be 0.80 min / (Oe cm) or more. If the value is less than this, the magnitude of the specified magnetic field used will be 0.4 × 10 4 (Oe) or more, making it difficult to further miniaturize the optical isolator.
[0026] To this end, the inventors conducted further investigations and developed an oxide material containing 80% or more terbium oxide in molar ratio terms, which has a Verdet constant of 0.85 min / (Oe·cm) or more at a wavelength of 800 nm. They found that when this material is used in a Faraday rotator, its length can be shortened to 1.1 cm or less, and that it can be mounted within the above-mentioned magnet dimensions.
[0027] Furthermore, the inventors discovered that further miniaturization can be achieved by combining the above-mentioned oxide material, which has a large Faraday effect, with a hollow magnet, which has a large magnetic flux density, and thus completed the present invention.
[0028] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited thereto.
[0029] The optical isolator according to the present invention is used for laser light in the wavelength band of 780 to 820 nm. This laser includes a semiconductor laser. Note that the design of the optical isolator according to the present invention can be modified to use laser light in other wavelength bands.
[0030] Figure 1 is a schematic cross-sectional view showing an example of the configuration of an optical isolator. In Figure 1, an input polarizer 1, a Faraday rotator 2, and an output polarizer 3 are sequentially arranged on an optical axis 6 that runs from the input side on the left to the output side on the right. On the input side, the input polarizer 1 is fixed to a polarizer holder 4, and on the output side, the output polarizer 3 is fixed to a polarizer holder 4. The polarization directions of the input and output are adjusted and fixed to a metal holder 5.
[0031] The shape of the Faraday rotator 2 is not particularly limited and may be a triangular prism or a quadrangular prism, but a cylindrical shape is preferable, so the following description will be given taking a cylindrical Faraday rotator 2 as an example.
[0032] A hollow magnet 7 is disposed on the outer periphery of this Faraday rotator 2. When the Faraday rotator 2 is cylindrical, the hollow magnet 7 is preferably hollow cylindrical, and the central axis of the Faraday rotator 2 and the central axis of the hollow part of the hollow magnet 7 are preferably coaxial. Furthermore, the outer diameter of the Faraday rotator 2 and the inner diameter of the hollow part of the hollow magnet 7 are approximately the same, and it is preferable to perform alignment after assembling the optical isolator. With this arrangement, the Faraday rotator 2 is disposed at the center of the hollow magnet 7.
[0033] Next, since the optical isolator of the present invention has a Faraday rotator with a Verdet constant of 0.80 min / (Oe·cm) or more at a wavelength of 800 nm, this Faraday rotator will be described.
[0034] The Faraday rotator is made of an oxide material that contains 80% or more terbium oxide (molar ratio) with a Verdet constant of 0.85 min / (Oe·cm) or more at a wavelength of 800 nm. The specific material is mainly composed of an oxide represented by the following formula (A), and may also contain sintering aids. (T x R 1-x )2O3(A) Here, in formula (A), x is 0.8≦x≦1.0, and R includes at least one element selected from the group consisting of lanthanoid elements other than scandium, yttrium, and Tb (terbium).
[0035] When such oxide crystals are used as Faraday rotators for isolators, it is preferable to perform a mirror finish on the surface after cutting using an abrasive or the like. The abrasive is not particularly limited, but may be, for example, colloidal silica.
[0036] The Faraday rotator may be made of any material as long as it is made of the above-mentioned material, but may be made of ceramics, since ceramics can easily realize a Faraday rotator with a large Verdet constant. Hereinafter, this material will be referred to as "transparent ceramics."
[0037] [Manufacturing method of transparent ceramics] Transparent ceramics are produced using oxide powders in a desired mixing ratio. The method for producing transparent ceramics can be appropriately selected from conventionally known production methods and is not particularly limited. Examples of the method for producing transparent ceramics include a hot isostatic pressing method, a method combining a solid phase method and a press molding method, and a method of vacuum sintering using mold molding, and are described in Akio Ikesue, "From Optical Single Crystals to Optical Polycrystals," Applied Physics, Vol. 75, No. 5, pp. 579-583 (2006), Takahiro Yanagidani and Hideyoshi Yagi, "The Present State and Future of Ceramic Laser Materials," Laser Research, Vol. 36, No. 9, pp. 544-548 (2008), and the like.
[0038] Hereinafter, an example of a method for producing transparent ceramics using hot isostatic pressing (HIP) will be described as a method for producing transparent ceramics.
[0039] (Preparation of raw powder) The powder material of the oxide represented by the formula (A) used as the starting material is preferably one with high purity, and preferably has a purity of 99.9% by weight or more, more preferably 99.99% by weight or more, and even more preferably 99.999% by weight or more. Note that the terbium oxide is not limited to Tb2O3, and Tb4O7 can also be used.
[0040] Transparent ceramics are produced using oxide powders with a desired blending ratio, but the shape and size of the powder particles used are not particularly limited. The preparation method of these raw material powders is also not particularly limited. Raw material powders produced by dry grinding, wet grinding, coprecipitation, alkoxide hydrolysis, sol-gel, hydrothermal synthesis, spray pyrolysis, and any other synthesis method can be suitably used. In this case, it is sufficient that the oxide powder material is contained as the main component, and other components may be intentionally contained as subcomponents.
[0041] Here, containing as a main component means containing 50% by mass or more of the composite oxide represented by the formula (A). The content of the composite oxide represented by the formula (A) is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 97% by mass or more, and particularly preferably 98% by mass or more.
[0042] Commonly-cited examples of other minor components (components other than the main component) include dopants and fluxes that are doped during single crystal growth, and sintering aids that are added during ceramic production.
[0043] Here, examples of the sintering aid include oxides of Group 4 elements such as titanium, zirconium, and hafnium, and oxides of Group 2 elements such as magnesium and calcium. In addition, oxides of Group 4 elements and oxides of Group 2 elements may be used simultaneously. These oxides have no absorption at wavelengths around 800 nm, and are suitable for the transparent ceramics of the present invention. A predetermined amount of sintering aid may be added, and it is preferable that the amount of the sintering aid is more than 0.01 parts by mass and not more than 5.0 parts by mass, more preferably more than 0.03 parts by mass and not more than 3.0 parts by mass, and even more preferably more than 0.05 parts by mass and not more than 2.0 parts by mass, relative to 100 parts by mass of the composite oxide.
[0044] On the other hand, elements other than those mentioned above have problems such as absorption at a wavelength of about 800 nm, being difficult to dissolve in rare earth oxides and therefore not reacting as a sintering aid but instead precipitating on their own, being too active and resulting in crystal grain sizes that are not in the optimal range, and gradually reacting with moisture over a long period of time, causing the ceramic to become hygroscopic and devitrifying, and therefore are unsuitable as sintering aids for producing the transparent ceramics of the present invention.
[0045] Next, the obtained raw powder material is weighed out in a desired molar ratio, and then at least one of a dispersant such as ammonium polyacrylate or ammonium polycarboxylate is added as necessary to make the particle size uniform, and a binder such as methyl cellulose, polyvinyl alcohol, or polyethylene glycol is added to obtain a desired molded body. Water, methyl alcohol, ethyl alcohol, or the like is further used as a solvent to make the mixture into a slurry, which is then subjected to general mixing and grinding using a ball mill or the like for several to several tens of hours. The obtained slurry is spray-dried to obtain a dried spherical body.
[0046] Alternatively, the materials may be mixed and pulverized in a ball mill or the like and then calcined, or the materials may be calcined and then pulverized. Specifically, the materials may be mixed and pulverized in a ball mill or the like and then spray-dried to produce a mixed powder, which may then be calcined.
[0047] The firing temperature and firing time are not particularly limited, but the firing temperature is preferably 600 to 1,600°C, more preferably 800 to 1,400°C, and even more preferably 800 to 1,100°C. The firing atmosphere is not particularly limited, and can be suitably used from among air, oxygen and oxygen-containing atmospheres, argon atmosphere, nitrogen gas atmosphere, and other inert atmospheres. The firing time is not particularly limited, and may be appropriately selected depending on the moisture content of the mixed powder and the firing temperature, but is preferably 1 to 20 hours, more preferably 5 to 15 hours. When firing is performed, it is preferable to further pulverize and mix the mixture for several to tens of hours using a ball mill or the like after firing.
[0048] In addition, in order to sharpen the distribution of the average particle size of the mixed powder and to obtain a high purity, the powder material may be dissolved, recrystallized, and pulverized, and then used as a raw material powder. Specifically, a raw material powder with a high purity (for example, 99.9 mass% or more) is prepared, and weighed so that the molar ratio of Tb2O3:R2O3 is desired. These raw material powders are dissolved in a nitric acid solution with a concentration of 1 mol / l, mixed with an ammonium sulfate solution with a concentration of 1 mol / l, and further added with ultrapure water to adjust the concentration. While stirring the resulting solution, an ammonium bicarbonate solution with a concentration of 0.5 mol / l is dropped at a constant dropping rate until the pH becomes 8, and the solution is left at room temperature for several days while stirring, and then filtered and washed with ultrapure water, and dried at 150°C for several days.
[0049] The obtained mixed powder is placed in an alumina crucible and calcined in an inert atmosphere such as a nitrogen atmosphere or an argon atmosphere at preferably 800 to 1,500° C., more preferably 1,000 to 1,400° C., and even more preferably 1,100 to 1,200° C. for preferably 0.5 to 10 hours, more preferably 1 to 7 hours, and even more preferably 2 to 4 hours. The inert atmosphere is used here to prevent the valence of terbium oxide from changing.
[0050] [Manufacturing process] The raw material powder is molded into a predetermined shape, degreased, sintered, and further processed by hot isostatic pressing (HIP) to produce a transparent composite oxide sintered body.
[0051] (molding) In the molding, a normal press molding process can be suitably used. That is, a very common press process in which the material is filled into a mold and pressed from a certain direction, or a CIP (Cold Isostatic Press) process in which the material is sealed and stored in a deformable waterproof container and pressed with hydrostatic pressure can be used. The applied pressure can be adjusted appropriately while checking the relative density of the resulting molded body, and is not particularly limited. In addition, other molding methods such as slip casting can also be suitably used in the molding process. In addition, the shape to be molded is not particularly limited, and can be selected appropriately depending on the device to be used, and for example, molding into a cylindrical shape is exemplified.
[0052] (Degreasing) In degreasing, a normal degreasing process can be suitably used. That is, a temperature-raising degreasing process using a heating furnace can be performed. The temperature at this time is preferably 200 to 600° C., more preferably 250 to 400° C. The atmosphere in which degreasing is performed is not particularly limited, and air, oxygen, argon gas atmosphere, etc. can be suitably used.
[0053] (Sintering) In the sintering, a general sintering process can be preferably used. That is, a heat sintering process such as a resistance heating method or an induction heating method can be preferably used. The atmosphere is not particularly limited, and various atmospheres such as air, inert gas, oxygen gas, hydrogen gas, and helium gas can be preferably used, but sintering under reduced pressure (vacuum) can be more preferably used.
[0054] The vacuum level during sintering was 1×10 -1 Pa or less, and 1×10 -2Pa or less is more preferable. Sintering conditions are preferably 1,300 to 1,800°C, more preferably 1,400 to 1,700°C, and even more preferably 1,400 to 1,600°C. Sintering time is preferably 1 to 50 hours, more preferably 2 to 25 hours, and even more preferably 5 to 20 hours. At this time, the heating rate is preferably 100 to 500°C / hr, more preferably 200 to 400°C / hr, and even more preferably 250 to 350°C / hr up to about 1,200°C, and at temperatures above that, the heating rate is preferably slowed down, and more preferably 20 to 100°C / hr.
[0055] (Processing by hot isostatic pressing (HIP)) In addition, after the above sintering, a post-process such as hot isostatic pressing (HIP) is carried out to further increase transparency. In particular, in the case of a transparent complex oxide sintered body that does not exhibit translucency even after the sintering process is completed, it is preferable to proceed to HIP treatment, since this makes it possible to eliminate bubbles in the sintered body and facilitates the attainment of translucency.
[0056] The treatment temperature is preferably higher than the sintering temperature, and is preferably 1,300°C or higher. In addition, the treatment temperature in the HIP treatment is preferably 1,800°C or lower, and more preferably 1,700°C or lower, because it becomes difficult to remove bubbles if grain growth occurs during the HIP treatment. The treatment pressure is preferably 196 MPa or lower, which is convenient and can be treated with a commercially available HIP device. The treatment time is not particularly limited, but is preferably 50 hours or lower, more preferably 25 hours or lower, and even more preferably 10 hours or lower. In addition, it is preferably 15 minutes or more, more preferably 30 minutes or more, and even more preferably 1 hour or more. In this case, an inert gas such as argon or Ar-O2 can be preferably used as the pressurized gas medium.
[0057] (processing) When the obtained transparent body is used for optical purposes, both end faces on the axis to be optically used are optically polished to a length L (cm), and the flatness at this time is preferably λ / 2 or less, and particularly preferably λ / 8 or less, when λ=633 nm. It is also possible to further reduce optical loss by forming an appropriate anti-reflection film on the optically polished surface.
[0058] In the present invention, the Verdet constant is not particularly limited as long as it is 0.80 min / (Oe·cm) or more, but the Verdet constant for 100% terbium oxide content is the upper limit. If the Verdet constant is less than 0.80 min / (Oe·cm), the size of the magnet required to set the Faraday rotation angle to 45° becomes large, making it difficult to miniaturize the optical isolator.
[0059] The Verdet constant can be measured according to a standard method, and is not particularly limited. Specifically, an oxide of a predetermined thickness is cut out, mirror-polished, and attached to a permanent magnet with a known magnetic flux density as a Faraday rotator, and the Verdet constant is measured at a wavelength of 800 nm in air at a measurement condition of 25±10°C.
[0060] Table 1 shows the (Tb x R 1-x )2O3 and the value of the Verdet constant at a wavelength of 800 nm are shown below.
[0061] [Table 1]
[0062] From Table 1, in the three composition examples, when x = 0.8 and 1.0, the Verdet constant is 0.85 to 1.05 min / (Oe·cm), and all of them satisfy 0.80 min / (Oe·cm) or more.
[0063] Furthermore, the length (sample length) L (cm) of the Faraday rotator of the present invention and the magnetic flux density B (Oe) of the mounted magnet satisfy the following formulas (1) and (2). 0.8≦L≦1.1 (1) B≦0.4×10 4 (2) If the length of the Faraday rotator is less than 0.8 cm, the magnetic flux density required to obtain a Faraday rotation angle of 45 degrees is 0.4 × 10 4 Oe, the magnet outer size becomes larger, making miniaturization difficult. Also, if the sample length of the Faraday rotator exceeds 1.1 cm, the applied magnetic flux density becomes extremely small, but conversely, the magnet becomes longer and the isolator length becomes longer, so it becomes difficult to further miniaturize the isolator.
[0064] The Faraday rotator of the present invention preferably has an insertion loss of 1 dB or less and an extinction ratio of 30 dB or more at a sample length L (cm) that satisfies the above formula. In addition, it is preferable that the sample length L is within the range that satisfies the above formula, since it is possible to fabricate an optical isolator that has optical characteristics of low loss and high isolation. The optical characteristics such as the insertion loss and the extinction ratio are measured in the atmosphere at a wavelength of 800 nm under measurement conditions of 25±10°C according to a standard method.
[0065] Furthermore, the Faraday rotator of the present invention preferably has a total light transmittance (total light transmittance) of 78% or more, more preferably 80% or more, at a wavelength of 800 nm and a sample length L cm in the range of 0.8≦L≦1.1. The higher the total transmittance, the more preferable it is, but the upper limit is not particularly limited and is 100% or less.
[0066] The total light transmittance was measured using a UV-Visible Spectrophotometer V-670 manufactured by JASCO Corporation. The light was made uniform by multiple reflections in an integrating sphere with a highly reflective material applied to the inner wall, and the light scattered by the turbidity of the sample was also measured based on the intensity of the captured light, and the total light transmittance was calculated based on the following formula. The wavelength in this case was 800 nm. Total light transmittance=I / Io×100 In the above formula, I is the transmitted light intensity (the intensity of light transmitted through a sample with a thickness of L cm), and Io is the incident light intensity. If the transmittance of the oxide obtained is not uniform and varies depending on the measurement point, the average transmittance of 10 arbitrary points is used as the transmittance of the oxide.
[0067] Next, we will explain the hollow magnet 7 used in the optical isolator of the present invention. It is preferable that the hollow magnet 7 is a permanent magnet that is as small as possible, and in order to obtain a large magnetic field strength, it is preferable to use a neodymium-iron-boron (NdFeB) magnet.
[0068] Generally, to provide a higher magnetic flux density, a demagnetizing magnet configuration using multiple magnets is required, including a second hollow magnet 8 and a third hollow magnet 9, as shown in Figure 2. In this case, a yoke structure made of carbon steel is required around the magnet, resulting in a larger external size.
[0069] Therefore, in order to miniaturize the optical isolator, it is preferable to use a single hollow magnet, and it is preferable that the hollow magnet 7 according to the present invention has the magnetic field polarity of the hollow magnet 7 oriented in the direction of the optical axis 6, is provided with a polarizer material on the outer periphery of the hollow magnet 7, and is provided with a stainless steel metal holder 5 that can be fixed by welding, as shown in Fig. 1. With such a configuration, the magnet shape can be made small and the magnetic flux density applied to the Faraday rotator 2 can be maximized.
[0070] In the basic design of the optical isolator of the present invention, it is important for miniaturization that the outer diameter and length of the hollow magnet 7 are reduced. To achieve this, it is important to combine a Faraday rotator 2 with a large Faraday effect with a hollow magnet 7 material (magnet) with a large magnetic flux density in order to achieve even greater miniaturization.
[0071] In addition, when a semiconductor laser is used in an optical isolator, optical damage to the Faraday rotator 2 caused by high-power light becomes a problem. This problem is determined by the transmittance of the Faraday rotator 2 and its length L. Therefore, in order to reduce this optical damage, it is advantageous for the Faraday rotator 2 to have a high transmittance and a short length L.
[0072] Furthermore, in the optical isolator of the present invention, it is preferable to provide two or more polarization-dependent glass polarizers on the optical axis, and this configuration makes it possible to provide a polarization-dependent optical isolator.
[0073] It is more preferable to provide two or more flat birefringent crystals and one or more 45-degree rotators on the optical axis 6, and this configuration can also be used to make a polarization-independent isolator. In this case, it is preferable that the optical axis of the flat birefringent crystal is in the direction of approximately 45° with respect to the optical axis 6 and that the thickness is 1.0 cm or more. For example, when a rutile single crystal (TiO2) is used, it is possible to accommodate a beam diameter of φ1.0 mm, which is 1 / 10 of the thickness, and when an α-BBO crystal (BaB2O4) is used, it is possible to accommodate a beam diameter of φ0.35 mm, which is approximately 1 / 30 of the thickness.
[0074] The embodiment of the present invention has been described above. EXAMPLES
[0075] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these.
[0076] <Example 1> In Example 1, an optical isolator for the 780-820 nm wavelength band was manufactured with the configuration shown in Fig. 1. For the input polarizer 1 and output polarizer 3, absorptive glass polarizers with high transparency / extinction ratio in the 780-820 nm wavelength band were used, and an anti-reflection film with a central wavelength of 800 nm was applied to their light transmitting surfaces. In order to prevent reflected light from the light transmitting surfaces from returning to the input light path, the polarizers were inserted into a metal holder 5 by adhesively fixing the four corners of the bottom surfaces of the polarizers onto a polarizer holder 4 tilted at an angle of 5 degrees.
[0077] The Faraday rotator 2 was positioned at the center of the hollow part of the hollow magnet 7 and was fixed at a position where the magnetic field distribution by the hollow magnet 7 was maximized. The input polarizer 1 and output polarizer 3, arranged in the order of the incident light path, had their optical axes adjusted to maximize the isolation characteristics in accordance with the polarization angle of 45 degrees rotated after passing through the Faraday rotator 2, and the outer periphery joints of the polarizer holder 4 and metal holder 5 were fixed by laser welding. The light transmitting surface of the Faraday rotator 2 is coated with an anti-reflection film (not shown) with a center wavelength of 800 nm.
[0078] As the material for the Faraday rotator 2, terbium / scandium oxide with a Verdet constant of 0.85 min / (Oe·cm) or more at a wavelength of 800 nm was used with reference to Table 1. The sample length L of the Faraday rotator 2 was set to 1.1 cm, and a hollow magnet 7 made of a neodymium-iron-boron (NdFeB) magnet was placed on the outer periphery of the Faraday rotator 2, with a SUS metal housing placed on the outside of that.
[0079] To further explain the details of the Faraday rotator 2 of Example 1, a terbium / scandium oxide ceramic containing 80% terbium oxide in terms of molar ratio was used as a specific material for the Faraday rotator 2. When the optical characteristics of this ceramic were measured at a wavelength of 800 nm, the insertion loss was 0.1 dB, the extinction ratio was 38 dB, and the Verdet constant was 0.85 min / (Oe·cm). The shape of the sample measured at this time was a cylinder with an outer diameter of φ2.3 cm and a length of 1.10 cm. Figure 3 shows the wavelength transmission characteristics of this Faraday rotator 2.
[0080] FIG. 4 shows the magnetic flux density Br (T=10 4 3 and 4 show the relationship between the elongation (Oe) and the sample length L (cm). Note that in Figs. 3 and 4, the material described in Patent Document 1 is shown as a reference example.
[0081] In the case of the Faraday rotator 2 of Example 1, the sample length L is 1.10 cm and the Verdet constant of the Faraday rotator 2 is 0.85 min / (Oe·cm). Therefore, when the magnetic flux density at which the Faraday rotation angle is 45 degrees in this case is calculated from the relationship in FIG. 4, it is found that the magnetic flux density is approximately 2900 [Oe] (=0.29 [T]).
[0082] In the present invention, the lower limit of the Verdet constant is 0.80 min / (Oe cm), and the material used for the Faraday rotator 2 in this case is terbium / scandium, terbium / yttrium, or terbium / lutetium oxide, which contains at least 80% terbium oxide in terms of molar ratio. Since the lower limit of the sample length L is 0.8 cm, the magnetic flux density of this oxide is calculated from the relationship in FIG. 4 to be 0.4×10 4 It can be seen that the value of [Oe] (=0.4 [T]) is the upper limit of Br. Therefore, in order to further reduce the size of the optical isolator, it is preferable that the magnetic flux density B (Oe) of the hollow magnet used in the present invention satisfies the following formula (2). B≦0.4×10 4 (2)
[0083] Next, the shape of the hollow magnet that satisfies the magnetic flux density of Example 1 will be described. The shape of this hollow magnet was determined by the following magnetic field analysis. That is, the finite element method (JMAG-Designer) was selected as the magnetic field analysis method, a neodymium-iron-boron (NdFeB) magnet manufactured by Shin-Etsu Chemical Co., Ltd. was selected as the magnet material, and SUS stainless steel was selected as the material for the metal holder 5. Also, Fig. 5 shows the simulation results of the magnetic flux density distribution obtained by setting the outer diameter of the hollow magnet to φ1.2 cm and the length (L') of the hollow magnet as a parameter.
[0084] According to the results of Fig. 5, it was found that the hollow magnet shape showing the magnetic flux density distribution when the sample length L of Example 1 is 1.10 cm has an inner diameter of φ0.3 cm, an outer diameter of φ1.2 cm, and a length of 2.0 cm. Here, Z [cm] in the figure indicates the distance from the center on the optical axis 6, and the sample length L [cm] is calculated as 2 x Z. In other words, in Fig. 5, the sample length L is 1.10 cm at the position where the horizontal axis Z is 0.55 cm.
[0085] When an optical isolator was assembled at a wavelength of 800 nm, an optical isolator with optical characteristics of an insertion loss of 0.5 dB and an isolation of 38 dB was fabricated.
[0086] <Comparative Example 1> In Comparative Example 1, an optical isolator was fabricated using a TGG single crystal (Verdet constant 0.27 min / (Oe·cm)) as a Faraday rotator. The magnetic flux density to be applied to this TGG single crystal was calculated in the range of sample lengths of 0.80 to 1.10 cm, and the results are shown in FIG. 4. In particular, it can be seen that the magnetic flux density required for Comparative Example 1 at a sample length of 1.1 cm, which is the same as in Example 1, is approximately 9,100 [Oe] (=0.91 [T]). Therefore, in order to calculate the hollow magnet shape in the same way as in Example 1, the outer diameter is set to φ2.5 cm, and the simulation result of the magnetic flux density distribution obtained by using the length (MT) of the hollow magnet 7 shown in FIG. 2 as a parameter is shown in FIG. 6.
[0087] 6, it was found that the hollow magnet shape that satisfies the magnetic flux density in Comparative Example 1 is an antimagnetic field configuration consisting of hollow magnet 7, second hollow magnet 8, and third hollow magnet 9, with an inner diameter of φ0.3 cm, an outer diameter of φ2.5 cm, and a total length of 6.5 cm including the length MT of hollow magnet 7 of 2.0 cm. Here, Z [cm] in the figure indicates the distance from the center on the optical axis 6, and the sample length L [cm] is calculated as 2×Z.
[0088] Comparing the above results between Example 1 and Comparative Example 1, it was confirmed that Example 1 could achieve a size reduction of 90% or more in comparison with the TGG optical isolator of Comparative Example 1, in terms of the volume ratio calculated from the outer diameter and length of both magnets.
[0089] In addition, since it is generally known that the Verdet constant has wavelength dependency and the constant decreases as the wavelength becomes longer, the Verdet constant was also evaluated at 820 nm, which is the upper limit wavelength in the 780-820 nm band. As a result, the Verdet constant was 0.26 min / (Oe·cm) for the TGG of Comparative Example 1, whereas it was 0.80 min / (Oe·cm) for Example 1, confirming that even at the long wavelength of 800 nm, the performance was more than three times that of the TGG of Comparative Example 1.
[0090] Therefore, it was confirmed that the optical isolator of this embodiment can be put into practical use as a sufficiently compact optical isolator having low loss and high isolation characteristics in the 780-820 nm band.
[0091] The present invention includes the following aspects. [1]: An optical isolator comprising a Faraday rotator made of a composite oxide containing an oxide represented by the following formula (A) as a main component and having a Verdet constant of 0.80 min / (Oe cm) or more at a wavelength of 800 nm, and a hollow magnet disposed on the outer periphery of the Faraday rotator, An optical isolator for the 780-820 nm wavelength band, characterized in that the sample length L (cm) of the Faraday rotator is within the range of the following formula (1), and the magnetic flux density B (Oe) applied to the Faraday rotator is within the range of the following formula (2). (T x R 1-x )2O3(A) Here, in the above formula (A), x is 0.8≦x≦1.0, and R includes at least one element selected from the group consisting of the lanthanoid elements other than scandium, yttrium, and Tb (terbium). 0.8≦L≦1.1 (1) B≦0.4×10 4 (2) [2]: The optical isolator according to the above [1], wherein the oxide is a ceramic. [3]: The optical isolator according to [1] or [2] above, wherein the Faraday rotator has an insertion loss of 1 dB or less and an extinction ratio of 30 dB or more over the sample length L (cm). [4]: The optical isolator according to any one of [1] to [3] above, wherein the hollow magnet is made of a neodymium-iron-boron (NdFeB) magnet.
[0092] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]
[0093] 1...incident polarizer, 2...Faraday rotator, 3...exit polarizer, 4...polarizer holder, 5...metal holder, 6...optical axis, 7...hollow magnet, 8...second hollow magnet, 9...third hollow magnet.
Claims
1. An optical isolator comprising a composite oxide containing an oxide represented by the following formula (A) as a main component, a Faraday rotator having a Verdet constant of 0.80 min / (Oe cm) or more at a wavelength of 800 nm, and a hollow magnet disposed on the outer periphery of the Faraday rotator, The sample length L (cm) of the Faraday rotator is within the range of the following formula (1), and the magnetic flux density B (Oe) applied to the Faraday rotator is within the range of the following formula (2). () x R 1-x ) 2 O 3 () Here, in the above formula (A), x satisfies 0.8≦x≦1.0, and R includes at least one element selected from the group consisting of lanthanoid elements other than scandium, yttrium, and Tb (terbium). 0.8≦L≦1.1 (1) B≦0.4×10 4 (2)
2. 2. The optical isolator according to claim 1, wherein the oxide is a ceramic.
3. 2. The optical isolator according to claim 1, wherein the Faraday rotator has an insertion loss of 1 dB or less and an extinction ratio of 30 dB or more in the sample length L (cm).
4. 4. The optical isolator according to claim 1, wherein the hollow magnet is made of a neodymium-iron-boron (NdFeB) magnet.
Citation Information
Patent Citations
Optoisolator with bandwidth of 1 mu m
CN103364972A
Optical isolator
JP2015018145A
Optical isolator
JP2015125375A
One micrometer band optical isolator
JP2016109743A
Optical isolator
JP2022170038A