The active energy ray-curable coating agent with specific monomers and cellulose compounds, combined with a primer layer, addresses permeability and resistance issues in decorative sheets, ensuring uniform coating and enhanced resistance on paper materials.
Patent Information
- Application Number
- JP2023073260
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing decorative sheets face issues with permeability, uneven coating, and poor cellophane tape and solvent resistance due to the use of volatile organic compounds and permeable paper base materials, leading to environmental concerns and performance inconsistencies.
An active energy ray-curable coating agent containing specific amounts of monofunctional (meth)acrylate monomers, urethane (meth)acrylate, and cellulose compounds, along with a primer layer using acrylic resin and inorganic fine particles, is applied to a paper base material to prevent penetration and enhance resistance.
The solution results in a solvent-free, environmentally friendly coating that maintains uniformity and provides excellent cellophane tape resistance and solvent resistance, even on permeable paper materials.
Smart Images

Figure 2024158234000001 
Figure 2024158234000002 
Figure 2024158234000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an active energy ray-curable coating agent and a decorative sheet. [Background technology]
[0002] Generally, "decorative sheets" are used as materials that can impart an appearance (design) similar to that of natural materials by being attached to the surface of plywood or the like for furniture, residential interiors, vehicle interior materials, etc. Such decorative sheets are required to have high durability, design, and a texture similar to that of real natural materials, so a coating layer is provided on the substrate in addition to a printing layer for design, achieving both high durability and texture. Furthermore, from the viewpoint of manufacturing efficiency, such decorative sheets often use a paper substrate as the substrate.
[0003] Most of the coating agents currently used are two-component curing paints that contain organic solvents. However, in recent years, from the perspective of environmental friendliness, active energy ray-curable solventless coating agents that do not contain volatile organic compounds have been attracting attention (e.g., Patent Documents 1 and 2). Patent Document 1 discloses a decorative sheet that uses a primer made of an oil-resistant resin that has a permeation suppression effect so that a surface protective layer made of an ionizing radiation curable resin composition does not permeate and remains on the surface to obtain a sufficient thickness. However, the primer used in Patent Document 1 contains a solvent, and the entire decorative sheet manufacturing process is not environmentally friendly. Furthermore, Patent Document 2 discloses a decorative sheet composed of multiple layers such as a water-based ink layer, an ionizing radiation curable monomer layer, etc. However, in Patent Document 2, the paper substrate used may sometimes be a highly permeable substrate, and the ionizing radiation curable monomer layer may permeate into the paper substrate, resulting in problems with cellophane tape resistance and solvent resistance.
[0004] Furthermore, when applying a coating agent to a printed paper substrate, the ease with which the coating agent penetrates varies depending on the darkness of the print, and as a result uneven penetration can lead to inconsistent thickness of the coating layer, which can result in non-uniform improvements in cellophane tape resistance and solvent resistance due to the coating. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-1453 A [Patent Document 2] JP 2007-8150 A Summary of the Invention [Problem to be solved by the invention]
[0006] The problem that the present invention aims to solve is to provide an active energy ray-curable coating agent for paper that is environmentally friendly as it does not contain volatile organic compounds, yet is difficult to penetrate even into highly permeable paper substrates, and can exhibit excellent cellophane tape resistance and solvent resistance, and a decorative sheet using the same. [Means for solving the problem]
[0007] The present inventors have found that an active energy ray-curable composition containing a specific amount of a specific active energy ray-curable compound and a specific amount of a cellulose-based compound solves the above problems.
[0008] That is, the present invention provides an active energy ray-curable coating agent for paper that contains an active energy ray-curable compound and satisfies the requirements (1) to (3). (1) The active energy ray-curable compound contains a monofunctional (meth)acrylate monomer in an amount of 1 to 30% by mass of the total amount of the active energy ray-curable compound. (2) As the active energy ray curable compound, urethane (meth)acrylate, which is a reaction product of dicyclohexylmethane 4,4'-diisocyanate and a hydroxyl group-containing (meth)acrylate, is contained in an amount of 4 to 30 mass % of the total amount of the active energy ray curable compound. (3) The active energy ray-curable compound contains a cellulose-based compound in an amount of 1 to 6% by mass based on the total mass of the active energy ray-curable compound.
[0009] The present invention also provides a decorative sheet comprising a paper substrate and a surface protective layer formed by curing an active energy ray-curable coating agent, the active energy ray-curable coating agent containing an active energy ray-curable compound, and satisfying (1) to (3). (1) The active energy ray-curable compound contains a monofunctional (meth)acrylate monomer in an amount of 1 to 30% by mass of the total amount of the active energy ray-curable compound. (2) As the active energy ray curable compound, urethane (meth)acrylate, which is a reaction product of dicyclohexylmethane 4,4'-diisocyanate and a hydroxyl group-containing (meth)acrylate, is contained in an amount of 4 to 30 mass % of the total amount of the active energy ray curable compound. (3) The active energy ray-curable compound contains a cellulose-based compound in an amount of 1 to 6% by mass based on the total mass of the active energy ray-curable compound.
[0010] Furthermore, the present invention provides a paper substrate having a primer layer in contact with the paper substrate, the primer layer in contact with the paper substrate having a Cobb water absorbency of 0 to 15 g / m 2 and the primer layer further satisfies (4) and (5). (4) Contains acrylic resin or acrylic styrene resin and inorganic fine particles. (5) The ratio of resin solids to inorganic particles in the primer layer is within the range of 1:1 to 5:1.
[0011] Furthermore, the present invention provides a decorative material comprising the decorative sheet. Effect of the Invention
[0012] The active energy ray-curable coating agent for paper of the present invention is solvent-free and environmentally friendly, and when applied, it does not easily penetrate into the paper substrate, and when made into a decorative sheet, it can achieve good cellophane tape resistance and solvent resistance.
[0013] Furthermore, the decorative sheet of the present invention can achieve good cellophane tape resistance and solvent resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] (Definition of words) In the present invention, "(meth)acrylate" refers to either or both of acrylate and methacrylate, and "(meth)acrylic acid" refers to either or both of acrylic acid and methacrylic acid.
[0015] (Active energy ray curable coating agent) The active energy ray-curable coating agent of the present invention contains an active energy ray-curable compound and satisfies the following (1) to (3). (1) The active energy ray-curable compound contains a monofunctional (meth)acrylate monomer in an amount of 1 to 30% by mass of the total amount of the active energy ray-curable compound. (2) As the active energy ray curable compound, urethane (meth)acrylate, which is a reaction product of dicyclohexylmethane 4,4'-diisocyanate and hydroxyl group-containing (meth)acrylate, is contained in an amount of 4 to 30 mass % of the total amount of the active energy ray curable compound. (3) The composition contains a cellulose-based compound in an amount of 1 to 6% by mass based on the total mass of the active energy ray-curable compound.
[0016] (Active energy ray curable compound) The active energy ray curable compound used in the present invention must contain, as the active energy ray curable compound, (1) a monofunctional (meth)acrylate monomer in an amount of 1 to 30 mass % of the total amount of the active energy ray curable compound, and (2) a urethane (meth)acrylate which is a reaction product of dicyclohexylmethane 4,4'-diisocyanate and a hydroxyl group-containing (meth)acrylate in an amount of 4 to 30 mass % of the total amount of the active energy ray curable compound.
[0017] As the monofunctional (meth)acrylate monomer, a known monofunctional (meth)acrylate monomer can be used, for example, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, hexadecyl (meth)acrylate, octadecyl (meth)acrylate, isoamyl (meth)acrylate, isodecyl (meth)acrylate, isostearyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, methoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate. , nonylphenoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, glycidyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, diethylaminoethyl (meth)acrylate, nonylphenoxyethyl tetrahydrofurfuryl (meth)acrylate, caprolactone-modified tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, ethoxyethoxyethanol acrylic acid polymer ester, 2-(2-phenoxyethoxy)ethyl acrylate, and the like. These may be used alone or in combination of two or more.
[0018] Of these, the above 2-(2-phenoxyethoxy)ethyl acrylate is preferred.
[0019] It is preferable that the active energy ray curable coating agent of the present invention contains a monofunctional (meth)acrylate monomer in an amount of 1 to 30% by mass of the total amount of the active energy ray curable compound, from the viewpoint of suitable covering property and curing property of the coated surface. It is also preferable that the monofunctional (meth)acrylate monomer is contained in an amount of 2 to 25% by mass, more preferably 5 to 20% by mass, of the total amount of the active energy ray curable compound. If the monofunctional (meth)acrylate monomer is contained in an amount of 1% by mass or more based on the total mass of the active energy ray curable compound, the viscosity increase tends to be suppressed and the covering property tends to be sufficiently maintained, and if it is contained in an amount of 30% by mass or less, the scratch resistance and solvent resistance tend to be maintained.
[0020] The active energy ray-curable coating agent of the present invention must contain urethane (meth)acrylate, which is a reaction product of dicyclohexylmethane 4,4'-diisocyanate and a hydroxyl group-containing (meth)acrylate, in an amount of 4 to 30 mass % of the total amount of active energy ray-curable compounds.
[0021] Examples of the hydroxyl group-containing (meth)acrylate that can be used include hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, 1,4-cyclohexanedimethanol monoacrylate, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, trimethylolpropane diacrylate, trimethylolpropane dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol hexaacrylate, dipentaerythritol hexamethacrylate, glycidyl acrylate, and glycidyl methacrylate.
[0022] From the viewpoint of favorable coating properties and curing properties of the coating surface, the content of the urethane (meth)acrylate must be 4 to 30 mass % of the total amount of the active energy ray-curable compound, and from the viewpoint of preventing uneven coating due to rapid absorption into the paper substrate, a range of 5 to 30 mass % is more preferable. When the content of the above urethane (meth)acrylate is 4% by mass or more of the total amount of the active energy ray-curable compound, sufficient printability tends to be obtained, and when it is 30% by mass or less, an increase in viscosity tends to be suppressed and coverage tends to be sufficiently maintained.
[0023] The active energy ray curable coating agent of the present invention may contain a difunctional (meth)methacrylate or a trifunctional or higher functional (meth)methacrylate as an active energy ray curable compound. By using a difunctional (meth)acrylate or a trifunctional (meth)methacrylate in addition to the monofunctional (meth)acrylate monomer, it is possible to obtain a higher strength than when only a monofunctional monomer is used while maintaining the appearance of the coating film.
[0024] Examples of the bifunctional (meth)acrylate include 1,4-butanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 2-methyl-1,8-octanediol di(meth)acrylate, 2-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene ... Examples of the di(meth)acrylate include dihydric alcohol di(meth)acrylates such as pyrene glycol di(meth)acrylate and tripropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, di(meth)acrylate of tris(2-hydroxyethyl)isocyanurate, di(meth)acrylates of diols obtained by adding 4 moles or more of ethylene oxide or propylene oxide to 1 mole of neopentyl glycol, and di(meth)acrylates of diols obtained by adding 2 moles of ethylene oxide or propylene oxide to 1 mole of bisphenol A.
[0025] The active energy ray-curable coating agent of the present invention preferably contains ethylene oxide-modified 1,6-hexanediol diacrylate, and more preferably contains the ethylene oxide-modified 1,6-hexanediol diacrylate in an amount of 10 mass% or more based on the total mass of the active energy ray-curable compound. If the content of the ethylene oxide-modified 1,6-hexanediol diacrylate is 10% by mass or more and 50% by mass or less based on the total mass of the active energy ray-curable compound, the viscosity increase is suppressed, the coating property is sufficiently maintained, and scratch resistance and solvent resistance tend to be maintained. In the ethylene oxide-modified 1,6-hexanediol diacrylate, the amount of alkylene oxide added in the modification is preferably 1 to 2 moles.
[0026] Examples of the trifunctional or higher (meth)methacrylate include poly(meth)acrylates of trivalent or higher polyhydric alcohols such as trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, and dipentaerythritol poly(meth)acrylate; triol tri(meth)acrylate obtained by adding 3 moles or more of ethylene oxide or propylene oxide to 1 mole of glycerin; di- or tri(meth)acrylate of triol obtained by adding 3 moles or more of ethylene oxide or propylene oxide to 1 mole of trimethylolpropane; and poly(meth)acrylates of polyoxyalkylene polyols such as di(meth)acrylate of diol obtained by adding 4 moles or more of ethylene oxide or propylene oxide to 1 mole of bisphenol A.
[0027] The active energy ray-curable coating agent of the present invention preferably contains ethylene oxide-modified trimethylolpropane triacrylate, and preferably contains the ethylene oxide-modified trimethylolpropane triacrylate in an amount of 10 mass % or more based on the total mass of the active energy ray-curable compound. When the content of the ethylene oxide-modified trimethylolpropane triacrylate is 10% by mass or more and 50% by mass or less based on the total mass of the active energy ray-curable compound, an increase in viscosity is suppressed, sufficient coating properties are maintained, and scratch resistance tends to be maintained. In the ethylene oxide modified trimethylolpropane triacrylate, the amount of alkylene oxide added in the modification is preferably from 1 to 3 moles, more preferably from 2 to 3 moles.
[0028] The total amount of the monofunctional (meth)acrylate and the di- or higher functional (meth)acrylate is preferably in the range of 60 to 90 mass %, more preferably 65 to 88 mass %, of the total amount of the active energy ray-curable compound. The total amount of the monofunctional (meth)acrylate and the di- or higher functional (meth)acrylate does not include the urethane (meth)acrylate, which is a reaction product of dicyclohexylmethane 4,4'-diisocyanate and a hydroxyl group-containing (meth)acrylate, and the (meth)acrylic oligomer described later.
[0029] The active energy ray curable coating agent of the present invention may further use a (meth)acrylic oligomer as an active energy ray curable compound, if necessary. Examples of the (meth)acrylic oligomer include urethane (meth)acrylates other than urethane (meth)acrylates, which are reaction products of dicyclohexylmethane 4,4'-diisocyanate and hydroxyl group-containing (meth)acrylates, acrylic (meth)acrylates, epoxy (meth)acrylates, amine-modified polyether acrylates, amine-modified epoxy acrylates, amine-modified aliphatic acrylates, amine-modified polyester acrylates, amine-modified acrylates such as amino (meth)acrylates, polyester (meth)acrylates, polyether (meth)acrylates, polyolefin (meth)acrylates, polystyrene (meth)acrylates, etc. Among these, urethane (meth)acrylates other than urethane (meth)acrylates which are reaction products of dicyclohexylmethane 4,4'-diisocyanate and hydroxyl group-containing (meth)acrylates, epoxy (meth)acrylates, and acrylic (meth)acrylates are preferred in that they have a viscosity suitable for application as a coating agent, low gloss, stain resistance, and scratch resistance.
[0030] The acrylic (meth)acrylate may be one obtained by a known method. For example, a method of blending and copolymerizing a carboxyl group-containing polymerizable monomer such as acrylic acid or methacrylic acid as a copolymerization component to obtain a copolymer having a carboxyl group or an amino group, and then reacting the carboxyl group or the amino group with a monomer having a glycidyl group and a (meth)acryloyl group such as glycidyl methacrylate; a method of blending and copolymerizing a hydroxyl group-containing monomer such as 2-hydroxyethyl methacrylate or 2-hydroxyethyl acrylate as a copolymerization component to obtain a copolymer having a hydroxyl group, and then reacting the hydroxyl group with an isocyanate group and a (meth)acryloyl group such as isocyanate ethyl methacrylate; a method of first blending a glycidyl group-containing polymerizable monomer such as glycidyl methacrylate as a copolymerization component and copolymerizing it to obtain a copolymer having a glycidyl group, and then reacting the glycidyl group with a carboxyl group-containing polymerizable monomer such as acrylic acid or methacrylic acid; a method of using thioglycolic acid as a chain transfer agent during polymerization to introduce a carboxyl group to the copolymer end, and reacting the carboxyl group with a monomer having a glycidyl group and a (meth)acryloyl group, such as glycidyl methacrylate; and a method of using a carboxyl group-containing azo initiator such as azobiscyanopentanoic acid as a polymerization initiator to introduce a carboxyl group to the copolymer, and reacting the carboxyl group with a monomer having a glycidyl group and a (meth)acryloyl group, such as glycidyl methacrylate.
[0031] Among these, the simplest and most preferred method is to copolymerize a carboxyl group-containing monomer such as acrylic acid or methacrylic acid, or an amino group-containing monomer such as dimethylaminoethyl methacrylate or dimethylaminopropylacrylamide, and then react the carboxyl group or amino group with a monomer having a glycidyl group and a (meth)acryloyl group, such as glycidyl methacrylate, or the like, as a copolymerization component, to obtain a copolymer having a glycidyl group, and then react the glycidyl group with a carboxyl group-containing polymerizable monomer such as acrylic acid or methacrylic acid.
[0032] Examples of monomer components constituting the above acrylic (meth)acrylate include monofunctional monomers such as ethyl (meth)acrylate, ethylhexyl (meth)acrylate, styrene, methylstyrene, and N-vinylpyrrolidone, as well as polyfunctional monomers such as trimethylolpropane (meth)acrylate, hexanediol (meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol (meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and neopentyl glycol (meth)acrylate.
[0033] The weight average molecular weight of the acrylic (meth)acrylate is preferably in the range of 10,000 to 100,000. If the weight average molecular weight of the acrylic (meth)acrylate is 10,000 or more, tackiness is unlikely to remain in the coating film, and it is easy to make the coating film tack-free only by the drying process, and if it is 100,000 or less, the viscosity of the active energy ray curable building material coating material does not become too high, and the problem of the coating amount not being sufficient due to excessive dilution during coating can be avoided. In addition, from the viewpoint of workability, it is more preferable that it is 10,000 to 50,000, and even more preferable that it is in the range of 10,000 to 30,000. The weight average molecular weight is determined by measurement using GPC in terms of polystyrene.
[0034] The content of the acrylic (meth)acrylate is preferably 0.1 to 20% by mass of the total amount of active energy ray curable compounds in the coating agent from the viewpoint of suitable coverage and curability of the coated surface, and more preferably 0.5 to 20% by mass from the viewpoint of preventing uneven coating caused by rapid penetration into the paper substrate. If the content of the acrylic (meth)acrylate is 0.1% by mass or more of the total amount of active energy ray curable compounds in the coating agent, sufficient printability tends to be obtained, and if it is 20% by mass or less, viscosity increase is suppressed and coverage tends to be sufficiently maintained.
[0035] Furthermore, the glass transition temperature (Tg) of the acrylic (meth)acrylate is preferably in the range of 40 to 130° C., and if it is 40° C. or higher, sufficient strength can be obtained after curing when made into a coating film, and if it is 130° C. or lower, the tendency that brittleness appears and processability decreases when made into a coating film can be suppressed. The hydroxyl value of the acrylic (meth)acrylate is preferably in the range of 5 to 300 mgKOH / g, and if it is 5 mgKOH / g or higher, the dispersion of the matting agent such as silica used in combination does not decrease and low gloss tends to be easily maintained, and if it is 300 mgKOH / g or lower, the tendency that contamination resistance decreases can be suppressed. The glass transition temperature (Tg) is measured using a differential scanning calorimeter by scanning in a nitrogen atmosphere using a cooling device in a temperature range of −80 to 450° C. at a temperature rise rate of 10° C. / min.
[0036] The molecular weight of the (meth)acrylic oligomer is preferably in the range of 150 to 100,000 in number average molecular weight, and more preferably in the range of 200 to 10,000 in number average molecular weight.
[0037] In addition, at least one (meth)acrylic oligomer selected from the group consisting of urethane (meth)acrylates other than urethane (meth)acrylates, which are reaction products of dicyclohexylmethane 4,4'-diisocyanate and hydroxyl group-containing (meth)acrylates, epoxy (meth)acrylates, and acrylic (meth)acrylates is preferably contained in an amount of 4 to 30% by mass based on the total mass of the active energy ray curable compound. By containing the (meth)acrylic oligomer in an amount of 4% by mass or more based on the total mass of the active energy ray curable compound, scratch resistance tends to be maintained, and by containing the (meth)acrylic oligomer in an amount of 30% by mass or less, viscosity suitable for application as a coating agent tends to be maintained.
[0038] In addition, the active energy ray curable compound is a general term for compounds that have the property of reacting with active energy rays (ultraviolet rays or electron beams), and compounds that do not have a reactive group are not included in the active energy ray curable compound. For example, cellulose-based compounds, non-reactive additives, photopolymerization initiators, etc. are not included in the active energy ray curable compound.
[0039] (Cellulose compounds) The active energy ray-curable coating agent of the present invention must contain (3) a cellulose-based compound in an amount of 1 to 6 mass % based on the total mass of the active energy ray-curable compound.
[0040] Examples of the cellulose-based compound include cellulose acetate-based resins such as cellulose acetate (diacetyl cellulose, triacetyl cellulose, etc.), cellulose acetate propionate, cellulose acetate butyrate, cellulose acetate propionate butyrate, and cellulose acetate phthalate, as well as nitrocellulose (also called nitrocellulose), hydroxyalkyl cellulose, and carboxyalkyl cellulose. These may be used alone or in combination. When using in combination, the total content of the cellulose-based compounds used in combination may be 1 to 6% by mass based on the total mass of the active energy ray-curable compound.
[0041] A cellulose acetate resin is a semi-synthetic polymer obtained by esterifying cellulose, a natural polymer, with acetate. Cellulose is a polymer with anhydroglucose as a repeating unit, and has three hydroxyl groups per repeating unit. Cellulose acetate resins with different properties can be obtained depending on the degree of esterification (substitution degree). The substitution degree is expressed as an index called the acetylation degree. The acetylation degree of triacetyl cellulose, in which all three hydroxyl groups are acetylated, is 62.5%. The acetylation degree of the cellulose acetate resin used in the present invention is preferably 40 to 70%, and more preferably 43 to 62%. The average polymerization degree is preferably about 100 to 400. Nitrocellulose (nitrocellulose) is preferably obtained by reacting native cellulose with nitric acid to replace three hydroxyl groups in the six-membered ring of the anhydrous glucopyranose group in the native cellulose with nitric acid groups to form a nitric acid ester. Nitrocellulose (nitrocellulose) preferably has a nitrogen content of 10-13% by mass and an average degree of polymerization of 30-500, more preferably a nitrogen content of 10-13% by mass and an average degree of polymerization of 45-290.
[0042] As the cellulose-based compound, among the above, cellulose acetate-based resin and nitrocellulose are preferred, cellulose acetate propionate, cellulose acetate butyrate, and nitrocellulose are more preferred, and cellulose acetate propionate and cellulose acetate butyrate are even more preferred. Among them, cellulose acetate propionate in which an acetyl group having 2 carbon atoms and a propionyl group having 3 carbon atoms are bonded to cellulose is particularly preferred. The molecular weight is preferably 5,000 to 200,000 in weight average molecular weight, more preferably 10,000 to 50,000. In addition, the glass transition temperature is preferably 120°C to 180°C.
[0043] The active energy ray curable coating agent of the present invention contains a cellulose-based compound in an amount of 1 to 6% by mass based on the total mass of the active energy ray curable compounds. The content of the cellulose-based compound in this range is preferable from the viewpoint of preventing penetration. In addition, the content of the cellulose-based compound in the total mass of the active energy ray curable compounds is preferably 2 to 6% by mass, more preferably 2 to 4% by mass, from the viewpoint of coating suitability.
[0044] (Photopolymerization initiator) The active energy ray curable composition of the present invention contains a photopolymerization initiator since curing is usually initiated by ultraviolet rays, but when an electron beam is used as the active energy ray, the composition does not need to contain the photopolymerization initiator. As the photopolymerization initiator, a known one can be used.
[0045] As the photopolymerization initiator, a radical polymerization type photopolymerization initiator is preferable, and an α-hydroxyalkyl ketone-based photopolymerization initiator is more preferable because the solution does not color when the active energy ray curable compound is dissolved and does not yellow over time. Examples of the α-hydroxyalkyl ketone-based photopolymerization initiator include 1-phenyl-2-hydroxy-2-methylpropan-1-one, 1-(4-i-propylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, and 1-hydroxycyclohexyl phenyl ketone. Phenyl glyoxolate-based photopolymerization initiators are also preferable. Examples of the phenyl glyoxolate-based photopolymerization initiator include methyl benzoyl formate. Among them, 1-hydroxycyclohexyl phenyl ketone is preferable.
[0046] As other radical polymerization type photopolymerization initiators, monoacylphosphine oxide photopolymerization initiators having an absorption wavelength in the long wavelength region of ultraviolet rays may be appropriately used in combination. Examples of monoacylphosphine oxide photopolymerization initiators include monoacylphosphine oxides such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2,6-dimethoxybenzoyl-diphenylphosphine oxide, 2,6-dichlorobenzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoyl-phenylphosphinic acid methyl ester, 2-methylbenzoyl-diphenylphosphine oxide, and pivaloylphenylphosphinic acid isopropyl ester. Among these, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide is more preferable because it has a UV absorption wavelength that matches the emission wavelength region of UV-LEDs having an emission wavelength of 385 nm or 395 nm, thereby obtaining suitable curing properties and causing less yellowing of the cured film.
[0047] The above-mentioned photopolymerization initiators may be used alone or in combination of two or more. The total amount of the photopolymerization initiators is preferably in the range of 0.01 to 5.0% by mass of the total amount of the active energy ray curable composition. If it is 0.01% by mass or more, good curability can be obtained. In addition, in the active energy ray curable matte coating agent used in the conventional decorative sheet, the photopolymerization initiator is generally added in an amount of 5.0 to 10.0% by mass of the total amount of the solid content of the coating agent, but in the present invention, by making it 5.0% by mass or less, the fluidity as a coating agent is maintained, and processability and workability are maintained. In addition, by irradiating ultraviolet rays under atmospheric conditions, the coating film surface of the matte coating film tends to be in a semi-cured state, and the fine particles of the matte agent are efficiently aligned by surface orientation, making it easy to obtain a matte effect.
[0048] Furthermore, the curing speed can be increased by adding a tertiary amine compound selected from aliphatic amine derivatives and / or benzoic acid amine derivatives as a sensitizer. Tertiary amine compounds are known to increase reactivity and prevent reaction inhibition by oxygen. Suitable tertiary amine compounds include free alkylamines such as triethylamine, methyldiethanolamine, and triethanolamine, aromatic amines such as 2-ethylhexyl-4-dimethylaminobenzoate and ethyl-4-dimethylaminobenzoate, and active energy ray polymerizable compounds such as polymeric unsaturated amines (e.g., (meth)acrylated amines), which are preferred because of their low odor, low volatility, and ability to be incorporated into the polymer matrix by curing, thereby suppressing yellowing.
[0049] The tertiary amine compound can be used in an amount of preferably 0.1 to 10% by mass, and more preferably 0.3 to 3% by mass, based on the total amount of the active energy ray-curable coating agent.
[0050] (Matte agent) The active energy ray-curable coating agent of the present invention may contain a matting agent. The matting agent preferably has an average particle diameter of 1 to 10 μm, and known matting agents can be used, and organic and / or inorganic agents can be used alone or in combination without particular limitation. Specifically, inorganic particles such as silica, titanium oxide, alumina particles (aluminum oxide), calcium carbonate, barium sulfate, and glass, organic particles such as acrylic resin, urethane resin, polycarbonate resin, silicone resin, and polystyrene resin, silicone beads, etc. can be used. As those that can be expected to have a high matting effect, inorganic fine particles such as silica and aluminosilicate beads, organic fine particles such as acrylic resin beads and urethane resin beads, and silicone beads, etc. are preferred. The amount of the matting agent added is preferably 5 to 20% by mass, more preferably 10 to 18% by mass, based on the total mass of the active energy ray-curable compound. If the content is 5% by mass or more, a sufficient matting effect is obtained, and if it is 20% by mass or less, the viscosity and scratch resistance that can be applied as a coating agent tend to be maintained.
[0051] (silica) As the silica, known silica can be used, and silica having an average particle size in the range of 1 to 10 μm is preferable. In the present invention, the average particle size is a value measured by a laser diffraction method. Specifically, amorphous silica is more preferred as silica. Examples of the amorphous silica include diatomaceous earth and activated clay. Among the amorphous silica, dry silica, wet silica, silica gel, etc. can be used as synthetic amorphous silica. Among them, wet silica produced by neutralizing and decomposing an aqueous solution of sodium silicate with an acid or an alkali metal salt is preferred. The wet silica can also be surface-treated. The method of surface-treating the silica particles is not particularly limited and may be any known method. Examples include surface-treated silica with wax or a silane coupling agent. The wet silica may be used by mixing a plurality of surface-treated and non-surface-treated silicas.
[0052] The average particle size of the wet silica used as the matting agent is 1 to 10 μm, more preferably 1.5 to 8 μm. If the average particle size is 1 μm or more, the viscosity is less likely to increase and it is easy to obtain a viscosity suitable for coating. If the average particle size is 10 μm or less, the silica is easily oriented on the coating surface layer, resulting in a good matte finish.
[0053] The content of silica is preferably 5 to 20% by mass, more preferably 10 to 18% by mass, based on the total mass of the active energy ray-curable compound. If the content is 5% by mass or more, a sufficient matte effect can be obtained, and if the content is 20% by mass or less, it is preferable since it tends to be easy to maintain the viscosity and scratch resistance that can be applied as a coating agent.
[0054] (beads) When beads are used in the present invention, there is no particular limitation and known beads can be used. Specifically, acrylic resin beads, silicone beads, glass beads, aluminosilicate beads, etc. can be used. By adding beads to the silica as the matting agent, it is possible to improve the scratch resistance of the coating surface in addition to a moderate low gloss. Although beads as the matting agent are required in larger amounts than silica, another advantage is that it is easier to fine-tune the gloss level by changing the amount of beads added. Among them, acrylic resin beads are preferred.
[0055] The active energy ray-curable composition of the present invention is preferably used without a solvent from the viewpoint of recent environmental friendliness, but an organic solvent can also be added as necessary.
[0056] (Organic solvent) As the organic solvent, any solvent can be used as long as it dissolves the active energy ray-curable composition used. Examples of the solvent include aromatic hydrocarbons such as toluene and xylene; aliphatic or alicyclic hydrocarbons such as n-hexane, cyclohexane, methylcyclohexane, and ethylcyclohexane; esters such as ethyl acetate, butyl acetate, and propyl acetate; alcohols such as methanol, ethanol, isopropyl alcohol, and n-butanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; alkylene glycol monoalkyl ethers such as ethylene glycol monoethyl ether and propylene glycol monomethyl ether; and ether esters such as propylene glycol monomethyl ether acetate. However, when aiming for environmental friendliness, in order to thoroughly reduce the amount of organic solvents evaporated into the atmosphere, i.e., to reduce volatile organic compounds (VOCs), it is preferable not to contain the above organic solvents.
[0057] From the viewpoint of coatability, it is preferable that the active energy ray curable composition of the present invention is adjusted to a coatable viscosity. The viscosity is preferably adjusted to 100 to 10,000 mPa·s, more preferably 100 to 5,000 mPa·s, and even more preferably 100 to 2,000 mPa·s. The active energy ray curable compounds generally have low molecular weights, and if the viscosity can be adjusted without diluting with an organic solvent, there is no need to dilute with an organic solvent. On the other hand, when a polymerizable oligomer having a high molecular weight and high viscosity is used in combination, the viscosity can be adjusted by diluting with an organic solvent or heating.
[0058] (Additives) In addition, the active energy ray-curable composition used in the present invention may contain known polymerization inhibitors, leveling agents, thixotropy-imparting agents, waxes, drying agents, thickeners, anti-sagging agents, plasticizers, dispersants, anti-settling agents, defoamers, ultraviolet absorbers, light stabilizers, resins, and the like, as necessary.
[0059] (Production of active energy ray curable coating agents) The active energy ray-curable coating agent of the present invention can be produced by mixing, kneading, and dispersing an active energy ray-curable compound, a cellulose-based compound, and, if necessary, a photopolymerization initiator, a matting agent, and various other additives. The active energy ray-curable coating agent of the present invention can be prepared by appropriately adjusting the size of the grinding media of the dispersing machine, the packing rate of the grinding media, the dispersion treatment time, etc. As the dispersing machine, a commonly used machine, such as a roller mill, a ball mill, a pebble mill, an attritor, a sand mill, etc., can be used. When air bubbles or unexpectedly large particles are contained in the coating agent, it is preferable to remove them by filtration, etc. As the filter, a conventionally known filter can be used.
[0060] (Surface protective layer) The active energy ray curable coating agent of the present invention can be applied to a substrate by a known coating / printing method to form a surface protective layer. The surface protective layer may be formed directly on the substrate, or may be formed by sandwiching a primer layer on the substrate. Specific examples of coating / printing methods include roll coaters, gravure coaters, gravure offset coaters, flexo coaters, air doctor coaters, blade coaters, air knife coaters, squeeze coaters, impregnation coaters, transfer roll coaters, kiss coaters, curtain coaters, cast coaters, spray coaters, die coaters, offset printers, screen printers, and the like.
[0061] When the active energy ray-curable coating agent used contains an organic solvent, the surface protective layer formed by the above-mentioned formation method can be obtained by drying the solvent in a drying oven or the like and then curing with active energy rays to obtain a cured surface protective layer, but this is not necessary when no solvent is used. In addition, the active energy ray may be ultraviolet light or an electron beam.
[0062] When ultraviolet rays are used as the active energy rays to cure the active energy ray curable coating agent, the ultraviolet rays can be irradiated by a known method. For example, ultraviolet rays are irradiated from a light source such as a germicidal lamp, an ultraviolet fluorescent lamp, an ultraviolet light emitting diode (UV-LED), a carbon arc, a metal halide lamp, a xenon lamp, a chemical lamp, a low pressure mercury lamp, a high pressure mercury lamp for copying, a medium pressure or high pressure mercury lamp, an ultra-high pressure mercury lamp, an electrodeless lamp, a metal halide lamp, natural light, or the like. The cumulative amount of UV light in the curing process is 20 to 1000 mJ / cm 2 In order to maximize the effect of the present invention, it is preferable that the integrated light amount is within the range of 40 to 800 mJ / cm. 2 It is more preferable that the integrated amount of ultraviolet light is in the range of 20 mJ / cm. 2 If it is more than 1000mJ / cm, the curing efficiency is good. 2 If the temperature is within this range, damage to the substrate due to heat generation can be prevented.
[0063] In addition, when the active energy ray-curable coating agent contains a matting agent, the coating surface is semi-cured, which makes it easier to efficiently obtain a matting effect due to the surface orientation of the matting agent, and is preferable because it can obtain a matting effect similar to that of a solvent-based paint even without a solvent. In this case, after the above-mentioned curing step, a step of irradiating the active energy ray to completely cure the active energy ray-curable coating agent may be further included. The integrated light amount of ultraviolet light in this step is 20 to 1000 mJ / cm. 2 In order to maximize the effect of the present invention, it is preferable that the integrated light amount is within the range of 40 to 800 mJ / cm. 2 It is even more preferable that the range is:
[0064] When the active energy ray-curable coating agent of the present invention is cured using ultraviolet rays as the active energy rays, it is more preferable to irradiate the active energy ray with ultraviolet rays in an atmosphere having an oxygen concentration of less than 5%. Here, an atmosphere with an oxygen concentration of less than 5% means an atmosphere filled with an inert gas containing oxygen, and the oxygen concentration is less than 5%. As the inert gas, one or more of nitrogen gas, carbon dioxide gas, argon gas, etc. may be used. In addition, there is no problem if a small amount of other gases such as carbon dioxide contained in air is contained.
[0065] On the other hand, when the active energy ray curable coating agent of the present invention is cured using an electron beam as the active energy ray, an electron beam irradiation device is used. The irradiation dose is preferably about 10 to 230 kGy, more preferably about 10 to 100 kGy. In the case of electron beam irradiation, the atmosphere preferably has an oxygen concentration of 2% or less.
[0066] The thickness of the surface protective layer thus obtained is preferably in the range of 0.1 to 100 μm, and most preferably in the range of 0.5 to 50 μm. By keeping the thickness in this range, the effects of the present invention can be maximized.
[0067] (decorative sheet) The decorative sheet of the present invention comprises a paper substrate and a surface protective layer formed by curing an active energy ray-curable coating agent, the active energy ray-curable coating agent containing an active energy ray-curable compound and satisfying the following (1) to (3): (1) The active energy ray-curable compound contains a monofunctional (meth)acrylate monomer in an amount of 1 to 30% by mass of the total amount of the active energy ray-curable compound. (2) As the active energy ray curable compound, urethane (meth)acrylate, which is a reaction product of dicyclohexylmethane 4,4'-diisocyanate and hydroxyl group-containing (meth)acrylate, is contained in an amount of 4 to 30 mass % of the total amount of the active energy ray curable compound. (3) The composition contains a cellulose-based compound in an amount of 1 to 6% by mass based on the total mass of the active energy ray-curable compound.
[0068] The surface protective layer in the decorative sheet of the present invention is a surface protective layer made of the above-mentioned active energy ray-curable coating agent of the present invention, and the preferred raw materials and composition are also as described above.
[0069] (Paper base material) The paper substrate used in the present invention can be used without any particular limitation. Types of paper substrates for decorative sheets include, for example, thin paper, plain paper, reinforced paper, resin-impregnated paper, and other paper quality sheets, titanium paper, and the like, which are also referred to as base paper. In addition, base paper with a printed layer added to it is also treated as a paper substrate in the present invention. In other words, the paper substrate includes not only base paper such as plain paper, reinforced paper, and resin-impregnated paper, but also laminates in which a printed layer such as a solid ink layer or a pattern ink layer is laminated on the base paper.
[0070] (Printing layer) The paper substrate used in the present invention may have a printed layer on the base paper. The printed layer may be a single layer or multiple layers may be laminated. Furthermore, solid printing may be performed, or printing may be performed only on a part of the paper substrate. The printing layer can be printed on the base paper by a known coating / printing method, such as roll coating, gravure coating, spray coating, or gravure printing, offset printing, letterpress printing, screen printing, inkjet printing, or other printing methods. The pattern to be applied to the printed layer may be freely determined, and examples thereof include wood grain patterns, patterns imitating the surface of rocks such as marble patterns, fabric patterns imitating the grain of fabric or patterns on fabric, tile patterns, etc., flower patterns in which flowers or bunches of flowers are arranged at equal intervals, letters, etc. In order to make the pattern stand out, a solid printed layer such as a white background may be provided under the pattern printed layer.
[0071] As the ink constituting the printed layer, known inks can be used, and examples of the ink that can be used include oil-based inks, water-based inks, active energy ray-curable inks, etc. In addition, liquid printing inks such as flexographic printing inks and gravure printing inks, lithographic offset printing inks, inkjet inks, etc. may be selected according to the printing method.
[0072] The decorative sheet of the present invention further comprises a primer layer in contact with the paper substrate, and the primer layer in contact with the paper substrate has a Cobb water absorbency of 0 to 15 g / m 2 and it is preferable that the primer layer satisfies (4) and (5). (4) Contains acrylic resin or acrylic styrene resin and inorganic fine particles. (5) The ratio of resin solids to inorganic particles in the primer layer is within the range of 1:1 to 5:1.
[0073] (Primer layer) The primer layer of the present invention preferably contains (3) an acrylic resin or an acrylic styrene resin, and inorganic fine particles, and (4) the ratio of the resin solid content to the inorganic fine particles in the primer layer is in the range of 1:1 to 5:1.
[0074] (Acrylic resin or acrylic styrene resin) The primer layer of the present invention preferably contains an acrylic resin or an acrylic-styrene resin.
[0075] (Acrylic resin) Examples of the acrylic resin include, as monomers, unsaturated carboxylic acids such as (meth)acrylic acid and (anhydrous) maleic acid, (meth)acrylic acid esters having an aliphatic hydrocarbon group such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, myristyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, oleyl (meth)acrylate, and eicosyl (meth)acrylate, 2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl ... ) (meth)acrylic acid ester compounds having hydroxyalkyl groups such as 2-hydroxypropyl acrylate and 3-hydroxypropyl (meth)acrylate, (meth)acrylamide, acrylonitrile, olefin-based compounds, styrene, α-methylstyrene, vinyltoluene, dimethylstyrene, ethylstyrene, isopropylstyrene, t-butylstyrene, chlorostyrene, dichlorostyrene, bromostyrene, fluorostyrene, styrene, and other styrene-based monomers, benzyl (meth)acrylate-based monomers such as benzyl (meth)acrylate, and phenyl (meth)acrylate-based monomers such as phenyl (meth)acrylate. These acrylic resins may be used alone or in combination of two or more.
[0076] The acid value of the acrylic resin is preferably 10 to 500 mgKOH / g. The content of the acrylic resin in the primer layer is preferably 1 to 20% by mass in terms of acrylic resin solid content.
[0077] (Acrylic styrene resin) The acrylic styrene-based resin is a copolymer of styrenes, (meth)acrylic acid, and (meth)acrylic acid alkyl ester. Known monomers that can be used as comonomers in acrylic resins, such as acrylamide and acrylonitrile, can be used as long as they do not impair the effects of the acrylic styrene-based resin. The styrenes are those having a styrene skeleton, such as styrene, α-methylstyrene, p-chlorostyrene, and p-methylstyrene, and among them, styrene is preferred from the viewpoint of industrial use. As the (meth)acrylic acid and (meth)acrylic acid ester, those exemplified in the above acrylic resin can be used. The content of the acrylic styrene-based resin in the primer layer is preferably 1 to 10% by mass, and more preferably 2 to 5% by mass, calculated as the acrylic styrene-based resin solid content.
[0078] Commercially available acrylic resins and acrylic styrene resins include, for example, the Hi-Loss-X series (X-436, JE-1056, PE-2273, QE-2128, NE-2260, ME-2039, X-1, RS-1193, VS-1259, TS-1318, YS-1274, VS-1047, RS-1191, etc.) (manufactured by Seiko PMC Corporation), the JONCRYL series (HPB-4110, HPB-1631, 67, 678, 611, 680, 682, 693, 690, 52J, 57J, 60J, 61J, 62J, 63J, DFC3030, DFC3040, DFC3050, PDX-7357, PDX-7326, PDX-7741, PDX-7356, PDX-7615, PDX-7789, PDX-7164, PDX-7430, HPD-96J, etc.) (manufactured by BASF), NEOCRYL series (A-1127, A-2902, XK-12, XK-190, etc.) (manufactured by Kusumoto Chemicals), ZAIXXEN A (manufactured by Sumitomo Seika Chemicals), etc., but are not limited thereto.
[0079] The glass transition temperature (Tg) of the acrylic resin or acrylic styrene resin is preferably 15 to 90° C., and more preferably 20 to 85° C. When Tg is within this range, the paper base material can have a low Cobb water absorbency, which makes it easier to suppress the penetration of the surface protective layer and makes it easier to achieve both cellophane tape resistance and solvent resistance.
[0080] (Other resins) The primer layer of the present invention may contain other resins besides the acrylic resin or the acrylic styrene resin. Examples of the other resins include urethane resins, epoxy resins, alkyd resins, amino acid resins, polyester resins, polyvinyl chloride resins, cellulose derivatives, casein, and the like. Among these, urethane resins are preferred.
[0081] (Inorganic fine particles) The primer layer of the present invention preferably contains inorganic fine particles. The inorganic fine particles are not particularly limited, and examples thereof include talc, silica, alumina, kaolin, clay, zirconia, mica, cordierite, boehmite (aluminum hydroxide), diaspore, glass, magnesium hydroxide, zirconium hydroxide, nickel hydroxide, boron hydroxide, hydrotalcite, calcium silicate, magnesium oxide, potassium titanate, barium titanate, magnesium titanate, calcium titanate, strontium titanate, iron oxide, red iron oxide, copper oxide, zinc oxide, tin oxide, titanium oxide, calcium oxide, chromium oxide, cerium oxide, antimony oxide, barium sulfate, barium carbonate, calcium carbonate, manganese dioxide, silicon carbide, silicon nitride, boron nitride, and aluminum nitride, but are not limited thereto. The inorganic fine particles may be used alone or in combination of two or more kinds.
[0082] The inorganic fine particles are preferably one or more selected from the group consisting of calcium carbonate, silica, alumina, mica, kaolin, clay, aluminum hydroxide, barium titanate, talc, boron nitride, and aluminum nitride, more preferably one or more selected from the group consisting of calcium carbonate, silica, alumina, aluminum hydroxide, talc, mica, and kaolin, and particularly preferably mica and kaolin.
[0083] The shape of the inorganic fine particles is not particularly limited, and may be, for example, spherical, true spherical, plate-like, or granular, and may be appropriately selected depending on the intended use. The surface treatment state of the inorganic fine particles is also not particularly limited, and may be, for example, surface-modified with saturated fatty acid or the like depending on the intended use.
[0084] The particle size of the inorganic fine particles is not particularly limited, but from the viewpoint of permeation prevention, the inorganic fine particles preferably have an aspect ratio, and more preferably have an average aspect ratio of 30 or more. When the inorganic fine particles have an aspect ratio, the inorganic fine particles in the primer layer are arranged parallel to the paper substrate, thereby exerting an excellent permeation prevention effect. In addition, when inorganic fine particles having a high aspect ratio of 30 or more are used, they tend to be oriented toward the paper substrate surface with respect to the thickness of the primer layer, so this is more preferable.
[0085] The ratio of the resin solid content to the inorganic fine particles in the primer layer is preferably in the range of 1:1 to 5:1. When the ratio of the inorganic fine particles is smaller than the resin solid content in the primer layer, the inorganic fine particles are less likely to dry up, so that the appearance defect of the primer layer is easily suppressed. In addition, when the ratio of the inorganic fine particles is larger, the penetration prevention effect tends to be larger, and the penetration of the active energy ray curable coating agent can be effectively suppressed.
[0086] (Additives) The primer layer may contain, as necessary, a leveling agent, a thixotropic agent, a wax, a drying agent, a thickener, an anti-sagging agent, a plasticizer, a dispersant, an anti-settling agent, an antifoaming agent, an ultraviolet absorbing agent, and the like.
[0087] (Cobb water absorbency of primer layer in contact with paper substrate) The Cobb water absorbency of the primer layer in contact with the paper substrate is 0 to 15 g / m 2 It is preferable that the thickness is 0 to 10 g / m 2 It is more preferable that the Cobb water absorption is 0 to 15 g / m 2 If so, the effect of preventing the low molecular weight monomer from penetrating into the paper base material becomes small, and the cellophane tape resistance and solvent resistance decrease. Cobb water absorbency is measured based on JISP 8140-1964. Specifically, distilled water (temperature 20±5°C) is used for the test in an atmosphere that matches the conditions of JISP 8111 (pretreatment of test paper). The procedure begins with placing a weighed test specimen (13 cm × 13 cm) on the mat on the base plate of the test specimen holder, and then attaching it to a metal ring (inner diameter 112.8±0.1 mm, area 100 cm). 2 ) and securely tighten the clamping device so that no water leaks out. Then, carefully pour about 50 mL of water into the metal ring. Start the second timer as soon as the test piece comes into contact with the water. Immediately after the contact time (60 seconds) is reached, lightly press the test piece with blotting paper to remove the water from the surface. Next, fold the test piece in half and weigh it again to determine the difference from the initial weight. The water absorption is calculated using the formula A = 100W for 1 m 2 Here, A is the Cobb water absorbency and W is the weight increase of the test piece (unit: g).
[0088] The thickness of the primer layer is preferably 1 to 100 μm, and more preferably 3 to 50 μm. Within this range, the permeation suppression effect is high, and the effects of the present invention can be effectively exhibited.
[0089] (Primer composition) The primer layer can be obtained by coating and drying the primer composition on a paper substrate. The primer composition preferably contains water. As the water, ion-exchanged water, distilled water, tap water, purified and sterilized industrial water, well water, etc. can be used, and ion-exchanged water and distilled water are preferably used. That is, the primer composition is preferably an aqueous primer composition, in other words, the primer layer is preferably a layer obtained by coating and drying an aqueous primer. The acrylic resin or acrylic styrene resin is preferably blended in the primer composition in the form of an emulsion or an aqueous solution. In addition, since the primer layer is formed by coating and drying the primer composition, the ratio of the resin solid content to the inorganic fine particles in the primer layer is the same as that in the primer composition.
[0090] As a method for applying the primer composition, a conventionally known method can be adopted, and for example, a roll coater, a gravure coater, a gravure offset coater, a flexo coater, an air doctor coater, a blade coater, an air knife coater, a squeeze coater, an impregnation coater, a transfer roll coater, a kiss coater, a curtain coater, a cast coater, a spray coater, a die coater, an offset printing machine, a screen printing machine, or the like can be appropriately adopted.
[0091] As the drying method, a conventionally known method can be used, such as hot air drying, heat roll drying, near infrared drying, etc.
[0092] (Decorative materials) A decorative material can be obtained by laminating the decorative sheet of the present invention to wood, plywood, fiberboard, etc. The decorative sheet of the present invention is resistant to damage caused by postings such as memos and tapes for positioning when processing the decorative material at the construction site, has excellent cellophane tape resistance, and can also exhibit solvent resistance, so it can be used for residential interior materials, furniture, home appliances, office supplies, toys, vehicle interior materials, etc., and is particularly suitable for use in residential interior materials, furniture, and home appliances. EXAMPLES
[0093] The present invention will be described in more detail below with reference to examples. In the examples, % means mass % and parts means mass parts. Blank spaces in the tables indicate that the components are not blended.
[0094] (Preparation of active energy ray-curable coating agent) Example A-1 5.6 parts of urethane (meth)acrylate "Photomer 6184 (manufactured by IGM Resins B.V.)" which is a reaction product of dicyclohexylmethane 4,4'-diisocyanate and hydroxyl group-containing (meth)acrylate, 22.2 parts of 2-(2-phenoxyethoxy)ethyl acrylate "M-101A (manufactured by Toa Gosei Co., Ltd.)" which is a monofunctional acrylate, 22.2 parts of hexanediol ethylene oxide modified diacrylate "Miramer M202 (manufactured by MIWON Co., Ltd.)" which is a bifunctional acrylate, and 22.2 parts of trimethylolpropane ethylene oxide modified diacrylate "Miramer M202 (manufactured by MIWON Co., Ltd.)" which is a trifunctional acrylate. A total of 107.7 parts of a mixture consisting of 50 parts of ethylene oxide-modified triacrylate "M3130 (manufactured by MIWON)," 4.4 parts of 1-hydroxycyclohexylphenyl ketone "Omnirad184" (manufactured by BASF), 2.2 parts of cellulose ester resin "CAP-482-05 (manufactured by EASTMAN CHEMICAL)," and 1.2 parts of acrylic-modified polysiloxane "TEGORAD2700 (manufactured by Evonik Japan)" was stirred and mixed in a stirrer for 1 hour, and then stirred in a bead mill for 2 hours to produce the active energy ray-curable coating agent of Example A-1.
[0095] [Examples A-2 to A-14, Comparative Examples A-1 to A-6] The active energy ray-curable coating agents of Examples A-2 to A-14 and Comparative Examples A-1 to A-6 were prepared in the same manner as in Example A-1, according to the formulations shown in Tables 1 to 3. In Tables 1 to 3, the formulation amounts are shown in mass% (simply referred to as %). The abbreviations in the table are as follows: Photomer 6184: Urethane acrylate oligomer manufactured by IGM Resins BV Viscoat 190D: Ethoxyethoxyethanol acrylic acid polymer ester manufactured by Osaka Organic Chemical Industry Co., Ltd. Miramer M170: Ethoxydiethylene glycol acrylate (EOEOEA) manufactured by MIWON M-101A: 2-2-(phenoxyethoxy)ethyl acrylate manufactured by Toagosei Co., Ltd. M-113: 2-(4-nonylphenoxy)ethyl acrylate manufactured by Toagosei Co., Ltd. Miramer M202: 1,6-Hexanediol diacrylate modified with ethylene oxide, manufactured by MIWON Miramer M3130: Ethylene oxide modified trimethylolpropane triacrylate manufactured by MIWON Omnirad184: BASF photoinitiator 1-hydroxy-cyclohexyl-phenyl-ketone ·CAP-482-05: Cellulose acetate propionate manufactured by EASTMAN CHEMICAL CAB-381-01: Cellulose acetate butyrate manufactured by EASTMAN CHEMICAL ·CAB-381-05: Cellulose acetate butyrate manufactured by EASTMAN CHEMICAL Syloid 7000: W.R. Grace silica, average particle size 4μm TEGORAD2700: Acrylic modified polysiloxane manufactured by Evonik Japan
[0096] (Preparation of decorative sheet for evaluation) Basis weight 30g / m 2 The paper base material (Cobb water absorbency 6.2 g / m2) has a wood grain pattern layer made with acrylic ink on the surface of the reinforced paper (Tenma Tokushu Paper Co., Ltd.). 2 ) was used, and 5 g / m of each of the active energy ray-curable coating agents of Examples A-1 to A-14 and Comparative Examples A-1 to A-6 was applied using a bar coater. 3After coating, the coating was irradiated once with ultraviolet light using high-pressure mercury to cure. Using a UV irradiation device (GS Yuasa Corporation) equipped with an air-cooled high-pressure mercury lamp (output 120 W / cm1 lamp) and a belt conveyor, the coated material was placed on the conveyor and passed directly under the lamp (irradiation distance 11 cm) at a speed of 20 meters per minute to cure the active energy ray-curable coating agent, and decorative sheets for evaluation were produced using the active energy ray-curable coating agents of Examples A-1 to A-14 and Comparative Examples A-1 to A-6. The ultraviolet light irradiation dose was measured at 50 mJ / cm using an ultraviolet integrating light meter (industrial UV checker UVR-N1, manufactured by GS Yuasa Corporation). 2 It was confirmed that.
[0097] [Evaluation method] The method for evaluating the active energy ray-curable coating agent of the present invention will be described below.
[0098] [Evaluation item 1: Viscosity] The viscosity of the active energy ray-curable coating agent adjusted to 45°C was measured using a Zahn Cup No. 5 (manufactured by Rigo Co., Ltd., orifice diameter 5 mm) and evaluated on the following three-level scale. (Evaluation Criteria) 〇: 20 seconds or less △: Less than 20 to 60 seconds ×: More than 60 seconds
[0099] [Evaluation item 2: Penetration into paper] Two sheets of "Hibari" (manufactured by Nippon Paper Industries) were stacked and fixed in place, and 2g of active energy ray-curable coating agent was dropped onto them. After a certain amount of time had passed, the top sheet was removed, and the time it took for a mark of penetration to appear on the bottom sheet was measured. The measurement was carried out twice, and the average was used to evaluate the product on a four-point scale. A permeability rating of △ or higher was deemed suitable for practical use. (Evaluation Criteria) ◎: 120 seconds or more ○: 60 seconds or more but less than 120 seconds △: 30 seconds or more but less than 60 seconds ×: Less than 30 seconds
[0100] [Evaluation item 3: Cellophane tape resistance] The decorative sheets for evaluation that were produced were designed to simulate the use of tape to temporarily hold down notes and other notices or for alignment purposes when actually processing the sheets at the construction site. Cellophane tape was then applied to the hardened coating film on the surface of the decorative sheet and quickly peeled off 10 times. The appearance of the printed film was evaluated on a three-point scale. (Evaluation Criteria) ⊚: No peeling of the printed film was observed. ○: More than 50% of the printed film remains in terms of area ratio. △: Less than 50% of the printed film remained in terms of area ratio. ×: The base paper was torn within 10 times.
[0101] [Evaluation item 4: MEK rubbing resistance] For the purpose of solvent resistance evaluation, 400g / cm 2 A gauze moistened with MEK (methyl ethyl ketone) was attached to the tip of the weight, and a rubbing test was conducted on the surface of the decorative sheet. The appearance of the printed coating was visually checked, and the number of rubbings when 50% of the surface area had peeled off was evaluated on the following four-point scale. (Evaluation Criteria) ◎: 30 or more round trips ○: 15 or more round trips but less than 30 round trips △: 5 to 15 round trips ×: Less than 5 round trips
[0102] Tables 1 to 3 show the evaluation results of the decorative sheets using each active energy ray-curable coating agent.
[0103] [Table 1]
[0104] [Table 2]
[0105] [Table 3]
[0106] The active energy ray curable coating agents of the present invention, Examples A-1 to A-14, were able to exhibit excellent cellophane tape resistance and solvent resistance while being environmentally friendly and not containing volatile organic compounds. In addition, since the coating agent was difficult to penetrate into the paper, coating unevenness can be reduced even when the paper substrate does not have printing ink or the amount of printing ink applied is small and the paper substrate is easily penetrated. Furthermore, the coating agents had a good viscosity that allows coating.
[0107] (Preparation of Aqueous Primer Composition) Example B-1 An aqueous primer composition of Example B-1 was prepared by thoroughly stirring a total of 100 parts of 17.1 parts (in terms of solids) of an acrylic styrene emulsion resin "Hiros-X·X-436 (Seiko PMC Corporation, glass transition temperature 21°C)," 10.9 parts (in terms of solids) of an acrylic emulsion resin "Hiros-X·JE-1056 (Seiko PMC Corporation, glass transition temperature 82°C)," 28.6 parts of a kaolin clay "Polygloss 90 (Kamin LLC, average particle size 0.2 μm)," 28.6 parts of ion-exchanged water, and 14.8 parts of ethanol with a stirrer for 15 minutes.
[0108] (Preparation of Aqueous Primer Composition) [Examples B-2 to B-17, Comparative Examples B-3 to B-5] The aqueous primer compositions of Examples B-2 to B-17 and Comparative Examples B-3 to B-5 were prepared in the same manner as in Example B-1 according to the formulations shown in Tables 4 to 7. In Tables 4 to 7, the formulation amounts are shown in mass% (simply expressed as %). The abbreviations in the table are as follows: ·X-436: Acrylic styrene emulsion resin Hi-Loss-X·X-436 manufactured by Seiko PMC Corporation, glass transition temperature 21℃ ·JE-1056: Acrylic emulsion resin Hi-Loss-X·JE-1056 manufactured by Seiko PMC Corporation, glass transition temperature 82℃ ·QE-2128: Acrylic emulsion resin Hi-Loss-X·QE-2128 manufactured by Seiko PMC Corporation, glass transition temperature 63℃ DFC3040: BASF acrylic styrene emulsion resin JONCRYL DFC3040, glass transition temperature 21℃ HPB-4110: BASF acrylic styrene emulsion resin JONCRYL HPB-4110, glass transition temperature 44℃ Polygloss 90: Kaolin clay manufactured by Kamin LLC, average particle size 0.2μm Micron White 5000A: Talc manufactured by Hayashi Kasei Co., Ltd., average particle size 4.1 μm Somasif MAE: Synthetic mica manufactured by Co-op Chemical Co., Ltd. (maximum average length of flat surface: 7.3 μm, average width of short surface: 0.38 μm) HM6040: Natural mica from Nhui Heng Hao Science and Technology Co., Ltd., maximum average length of flat surface 19μm, average width of short surface 0.53μm
[0109] (Preparation of primer layer and decorative sheet) Two types of paper substrates were used, each having a wood grain pattern layer formed on the base paper using acrylic ink, and the aqueous primer compositions of Examples B-1 to B-17 and Comparative Examples B-3 to B-5 were applied at 5 g / m2 using a bar coater. 3After coating, the coating was dried overnight at 40°C using a dryer to prepare a primer layer. In addition, paper substrates without a primer layer were prepared as Comparative Examples B-1 and B-2. The active energy ray curable coating agents of Examples A-6, Comparative Examples A-1, and Comparative Examples A-4 were coated on the substrates, and ultraviolet light was irradiated once using high pressure mercury to cure the coating film. Using a UV irradiation device (GS Yuasa Corporation) equipped with an air-cooled high pressure mercury lamp (output 120W / cm1 lamp) and a belt conveyor, the coated material was placed on the conveyor and passed directly under the lamp (irradiation distance 11 cm) at a speed of 20 meters per minute to cure the active energy ray curable coating agent and form a surface protective layer, and the decorative sheets of Examples B-1 to B-17 and Comparative Examples B-1 to B-5 were prepared. The types of coating agents used in the surface protective layer of each decorative sheet are listed in Tables 4 to 7. The UV exposure was measured at 50 mJ / cm using a UV integrating light meter (GS Yuasa Corporation's industrial UV checker UVR-N1). 2 It was confirmed that.
[0110] [Evaluation method] The evaluation methods for the decorative sheet and primer layer of the present invention are described below. The evaluation results are shown in Tables 4 to 7.
[0111] [Evaluation item 1: Cobb water absorbency] The aqueous primer compositions prepared in Examples B-1 to B-17 and Comparative Examples B-3 to B-5 were applied to each paper substrate under the same conditions as in the preparation of the decorative sheet to prepare a primer layer. The primer layers were measured for Cobb water absorption (60 seconds) [unit: g / m2] based on JISP 8140-1964. 2 ] was measured. Incidentally, the Cobb water absorbency of the paper substrate on which the wood grain pattern layer was formed using acrylic ink before the aqueous primer composition was applied was as follows. Wood grain pattern B: 27g / m 2 Wood grain pattern C: 17g / m 2
[0112] [Evaluation item 2: Uneven penetration] The coating agent was applied onto the primer layer in the same manner as in the method for producing the decorative sheet described above, and the state of the coating film was visually evaluated about 10 seconds later and rated into the following four levels. (Evaluation Criteria) ◎: Penetrates evenly and has no uneven application ○: Slight unevenness in the coating along the grain is visible. △: There are uneven areas of coating along the grain of the wood, but the coating is still usable. ×: Penetration into the paper substrate is rapid, and coating unevenness is noticeable.
[0113] [Evaluation item 3: Cellophane tape resistance] For the decorative sheets of Examples B-1 to B-17 and Comparative Examples B-1 to B-5, cellophane tape was applied to the surface protective layer of the prepared decorative sheet surface, simulating the use of tape to temporarily hold down notes and other notices or for alignment purposes when actually processing the sheets at the construction site, and the tape was quickly peeled off 10 times. The appearance of the printed film was evaluated on a four-point scale as follows: (Evaluation Criteria) ⊚: No peeling of the printed film was observed. ○: More than 50% of the printed film remains in terms of area ratio. △: Less than 50% of the printed film remained in terms of area ratio. ×: The base paper was torn within 10 times.
[0114] [Evaluation item 4: MEK rubbing resistance] For the purpose of solvent resistance evaluation, 400g / cm 2 A gauze moistened with MEK (methyl ethyl ketone) was attached to the tip of the weight, and a rubbing test was carried out on the surface of the decorative sheets of Examples B-1 to B-17 and Comparative Examples B-1 to B-5. The appearance of the printed coating was visually confirmed, and the number of rubbings when 50% of the area was peeled off was evaluated using the following four-point scale. (Evaluation Criteria) ◎: 30 or more round trips ○: 15 or more round trips but less than 30 round trips △: 5 to 15 round trips ×: Less than 5 round trips
[0115] [Table 4]
[0116] [Table 5]
[0117] [Table 6]
[0118] [Table 7]
[0119] The decorative sheets of Examples B-1 to B-17, which are the decorative sheets of the present invention, have printability with little uneven penetration even without using organic solvents, and also have cellophane tape resistance and solvent resistance. In particular, the Cobb water absorbency of the primer layer in contact with the paper substrate is 0 to 15 g / m 2 and the primer layer contains an acrylic resin or an acrylic styrene resin and inorganic fine particles, and the ratio of the resin solid content to the inorganic fine particles in the primer layer is in the range of 1:1 to 5:1. The primer layer had good printability without uneven penetration, and was very excellent in both cellophane tape resistance and solvent resistance. On the other hand, the decorative sheets of Comparative Examples B-1 to B-5 had uneven penetration and were poor in cellophane tape resistance and MEK rubbing resistance.
Claims
1. An active energy ray-curable coating agent for paper, which contains an active energy ray-curable compound and satisfies (1) to (3). (1) The active energy ray-curable compound contains a monofunctional (meth)acrylate monomer in an amount of 1 to 30% by mass of the total amount of the active energy ray-curable compound. (2) As the active energy ray curable compound, a urethane (meth)acrylate which is a reaction product of dicyclohexylmethane 4,4'-diisocyanate and a hydroxyl group-containing (meth)acrylate is contained in an amount of 4 to 30% by mass of the total amount of the active energy ray curable compound. (3) The composition contains a cellulose-based compound in an amount of 1 to 6% by mass based on the total mass of the active energy ray-curable compound.
2. A decorative sheet comprising a paper substrate and a surface protective layer formed by curing an active energy ray-curable coating agent, the active energy ray-curable coating agent containing an active energy ray-curable compound, and satisfying (1) to (3). (1) The active energy ray-curable compound contains a monofunctional (meth)acrylate monomer in an amount of 1 to 30% by mass of the total amount of the active energy ray-curable compound. (2) As the active energy ray curable compound, a urethane (meth)acrylate which is a reaction product of dicyclohexylmethane 4,4'-diisocyanate and a hydroxyl group-containing (meth)acrylate is contained in an amount of 4 to 30% by mass of the total amount of the active energy ray curable compound. (3) The composition contains a cellulose-based compound in an amount of 1 to 6% by mass based on the total mass of the active energy ray-curable compound.
3. A primer layer is provided in contact with the paper base material, and the primer layer in contact with the paper base material has a Cobb water absorbency of 0 to 15 g / m 2 3. The decorative sheet according to claim 2, wherein the primer layer satisfies (4) and (5). (4) Contains an acrylic resin or an acrylic-styrene resin and inorganic fine particles. (5) The ratio of resin solids to inorganic fine particles in the primer layer is in the range of 1:1 to 5:
1.
4. A decorative material comprising the decorative sheet according to claim 2 or 3.
Citation Information
Patent Citations
Decorative material
JP2001001453A
Decorative paper sheet
JP2007008150A