Mixed composition
A mixed composition of a composite metal acid compound with titanium and a resin addresses the challenge of forming effective photocatalytic films by ensuring compatibility and adherence, enhancing performance and film properties.
Patent Information
- Application Number
- JP2023073362
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing titanium oxide-based photocatalysts face challenges in forming good films with particles that maintain photocatalytic performance after film formation.
A mixed composition containing a composite metal acid compound with titanium as the main component and a resin, ensuring compatibility and adherence to substrates, with specific molar ratios and additives like molybdenum and tantalum, along with a resin such as styrene, to enhance film-forming properties and photocatalytic performance.
The composition achieves excellent photocatalytic performance and film-forming properties on substrates, with improved adhesion and transparency, while maintaining antibacterial and antiviral properties.
Smart Images

Figure 2024158281000006 
Figure 2024158281000007 
Figure 2024158281000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a mixture composition. [Background technology]
[0002] Titanium dioxide (TiO 2 When exposed to light, electrons are excited, which then bind to other molecules and reduce them. After these electrons are excited, positively charged holes are created which steal electrons from molecules and oxidize them. Development is underway to use this material as a photocatalyst.
[0003] As an example of the development of photocatalytic applications, Patent Document 1 describes the addition of Mo (molybdenum) or MoO as a sintering aid to titanium oxide powder. 3 (Molybdenum oxide) doped photocatalysts are disclosed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2001-170496 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, there are concerns that the titanium oxide disclosed in Patent Document 1 cannot be used to form a good film in its particle form. There is also a demand for the particles to maintain their photocatalytic performance even after film formation.
[0006] In view of the above problems, the present invention provides a mixed composition having excellent photocatalytic performance and excellent film-forming properties on a substrate. [Means for solving the problem]
[0007] The mixed composition of the present invention, which has been made to solve the above problems, is characterized by containing a composite metal acid compound containing titanium as a main component, and a resin. The mixed composition of the present invention is preferable in that it contains a composite metal acid compound having titanium as a main component and a resin, and therefore the composite metal acid compound and the resin are uniformly compatible with each other and adhere to the substrate, thereby providing excellent photocatalytic performance and excellent film-forming properties on the substrate.
[0008] The complex metal acid compound containing titanium as its main component, which is contained in the mixed composition of the present invention, is a complex metal acid compound in which the molar ratio of titanium to the sum of titanium and elements M other than titanium is 0.5 or more.
[0009] Here, the titanium content in the mixed composition of the present invention is determined by diluting the mixed composition appropriately with dilute hydrochloric acid as necessary, and measuring the titanium oxide (TiO 2 The titanium in the mixture composition of the present invention is not necessarily TiO 2 The titanium content is expressed as TiO 2 The conversions shown are based on convention.
[0010] The content of element M other than titanium in the mixed composition of the present invention is calculated by diluting the mixed composition appropriately with dilute hydrochloric acid as necessary and measuring the weight fraction of element M in terms of oxide by ICP emission spectrometry. The element M other than titanium may be one or more elements selected from the group consisting of Fe, Nb, Ta, W, Mo, Si, Zn, Al, Y, La, Ce, Zr, Nd, Sm, Eu, Dy, and Hf.
[0011] Thus, the molar ratio of titanium to the sum of the content of titanium (Ti) and the content of element M other than titanium (M) calculated by ICP optical emission spectrometry, Ti / (Ti+M), is preferably 0.5 or more. Note that titanium and element M other than titanium referred to in this specification include their oxides unless otherwise specified.
[0012] That is, the composite metal acid compound mainly composed of titanium contained in the mixed composition of the present invention is a composite metal acid compound in which the molar ratio (Ti / (Ti+M)) of titanium to the sum of titanium and elements other than titanium M is 0.5 or more, and titanium, one or more elements M selected from the group consisting of Fe, Nb, Ta, W, Mo, Si, Zn, Al, Y, La, Ce, Zr, Nd, Sm, Eu, Dy, and Hf, and oxygen element are composited in the composition. Moreover, the composite metal acid compound mainly composed of titanium contained in the mixed composition of the present invention is more preferably a composite metal acid compound in which the molar ratio (Ti / (Ti+M)) is 0.5 or more, titanium, molybdenum as element M, and oxygen element are composited in the composition, and further preferably a composite metal acid compound in which the molar ratio (Ti / (Ti+M)) is 0.5 or more, titanium, molybdenum and tantalum as element M, and oxygen element are composited in the composition.
[0013] The resin contained in the mixed composition of the present invention is uniformly compatible with the composite metal acid compound containing titanium as a main component and functions to adhere to the substrate, thereby improving the film-forming property and adhesion to the substrate.
[0014] The resin contained in the mixed composition of the present invention may be one or more water-soluble homopolymers selected from the group consisting of acrylic polymers, urethane polymers, styrene polymers, olefin polymers, amide polymers, siloxane polymers, epoxy polymers, vinyl chloride polymers, and vinyl acetate polymers, and / or copolymers consisting of two or more of these polymers. In particular, the resin contained in the mixed composition of the present invention is preferably one that contains a styrene polymer.
[0015] In addition, if the resin contained in the mixed composition of the present invention contains a styrene-based resin, it is preferable in that the transparency of the coating film is improved when the mixed composition of the present invention is used to form a coating film on a substrate. The styrene-based resin is, for example, a resin that can be obtained by addition polymerization of a styrene-based monomer. The styrene-based monomer is, for example, styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, p-chlorostyrene, p-nitrostyrene, p-aminostyrene, p-carboxystyrene, p-phenylstyrene, 2,5-dichlorostyrene, pt-butylstyrene, etc.
[0016] Furthermore, the resin contained in the mixed composition of the present invention may be a nonionic, anionic, or cationic styrene resin, and more preferably an anionic or cationic styrene resin. The resin contained in the mixed composition of the present invention may be a mixture of anionic and cationic styrene resins.
[0017] In addition, the content of the resin contained in the mixed composition of the present invention is preferably 1% by mass or more and 80% by mass or less, since it is possible to suppress aggregation of fine composite metal acid compounds. Furthermore, the content of the resin contained in the mixed composition of the present invention is more preferably 3% by mass or more and 70% by mass or less, even more preferably 5% by mass or more and 60% by mass or less, particularly preferably 10% by mass or more and 50% by mass or less, and particularly preferably 20% by mass or more and 40% by mass or less.
[0018] Here, the content of the resin contained in the mixed composition of the present invention can be obtained, for example, as follows. The mixed composition of the present invention is dried at 100°C to 200°C under an air atmosphere, and the solid content of the obtained dried product is measured. Then, the dried product is baked at 500°C to 1000°C under an air atmosphere, and the resin component of the dried product is volatilized, and the solid content of the obtained baked product is measured. Then, the difference between the solid content of the dried product and the solid content of the baked product can be calculated as the content of the resin contained in the mixed composition of the present invention. Alternatively, it can be calculated by liquid chromatography (LC) or gel permeation chromatography (GPC).
[0019] The mixed composition of the present invention may be in not only a liquid or powder form, but also a gel form as long as it can be applied to a substrate.
[0020] In the mixed composition of the present invention, the composite metal acid compound further contains molybdenum and tantalum, and the titanium content is TiO 2 When expressed as 1 (mol) in converted value, the molybdenum content is expressed as the molar ratio MoO 3 Conversion value / TiO 2 The conversion value is 0.01-20, and the tantalum content is the molar ratio Ta 2 O 5 Conversion value / TiO 2 It is characterized by a conversion value of 0.01-0.5. The mixed composition of the present invention further contains molybdenum and tantalum, and the titanium content is TiO 2 When expressed as 1 (mol) in terms of the converted value, the molybdenum content is expressed as the molar ratio MoO 3 Conversion value / TiO 2 The conversion value is 0.01-20, and the tantalum content is in the molar ratio Ta 2 O 5 Conversion value / TiO 2 A conversion value of 0.01 to 0.5 is preferable in that the particles are white, have excellent photocatalytic performance, and are excellent in film-forming properties on a substrate.
[0021] Here, the titanium content in the mixed composition of the present invention was determined by ICP emission spectrometry (Agilent Technologies: AG-5110) as described above. 2 The titanium in the mixture composition of the present invention is not necessarily TiO 2 The titanium content is expressed as TiO 2 The conversions shown are based on convention.
[0022] The content of molybdenum in the mixed composition of the present invention was determined by ICP emission spectrometry in the same manner as the content of titanium described above. 3 The molybdenum in the mixed composition of the present invention is not necessarily expressed as MoO 3 The molybdenum content is expressed as MoO 3 The conversions shown are based on convention.
[0023] Furthermore, the content of tantalum in the mixed composition of the present invention is determined by ICP emission spectrometry in the same manner as the content of titanium described above. 2 O 5 The weight fraction of Ta in the mixed composition of the present invention is calculated by measuring the weight fraction of Ta in terms of Ta. 2 O 5 The tantalum content is not expressed as Ta 2 O 5 The conversions shown are based on convention.
[0024] As described above, the contents of titanium, molybdenum, and tantalum calculated by ICP emission spectrometry were calculated by dividing the titanium content by the TiO 2 When expressed as 1 (mol) in terms of the converted value, the molybdenum content is expressed as the molar ratio MoO 3 Conversion value / TiO 2 The conversion value is 0.01-20, and the tantalum content is in the molar ratio Ta 2 O 5 Conversion value / TiO 2The molar ratio MoO is preferably 0.01-0.5. 3 Conversion value / TiO 2 It is more preferable that the molar ratio Ta 2 O 5 Conversion value / TiO 2 More preferably, the molar ratio MoO is 0.1-0.5. 3 Conversion value / TiO 2 Conversion value and molar ratio Ta 2 O 5 Conversion value / TiO 2 In calculating the conversion value, titanium is treated as oxide TiO 2 is calculated as 1 mole, and molybdenum is oxide MoO 3 is calculated as 1 mole, and tantalum is oxide Ta 2 O 5 The molar ratios are calculated based on 1 mole of titanium, molybdenum, and tantalum, and are expressed as the molar ratios calculated based on the respective oxides. Note that titanium, molybdenum, and tantalum referred to in this specification include their oxides unless otherwise specified.
[0025] The mixed composition of the present invention is characterized by further containing a solvent. The mixed composition of the present invention may contain water or an organic solvent as a solvent. The mixed composition of the present invention has high dispersibility in water and good solubility in water, so water can be used as a solvent. Here, if the solvent is only water, it is preferable from the viewpoint of reducing environmental load. On the other hand, if the solvent contains an organic solvent, it is preferable from the viewpoint of quick drying. Furthermore, a mixed solvent of water and an organic solvent can be used. Examples of the organic solvent include alcohol-based solvents and ketone-based solvents, and one or more selected from methanol, ethanol, propanol, isopropyl alcohol, ethylene glycol, polypropylene glycol, glycerin, acetone, methyl ethyl ketone, etc. can be used. In addition, industrial ethanol, which is a mixed alcohol solvent mainly composed of ethanol, may be used as the organic solvent.
[0026] In addition, the content of the solvent contained in the mixed composition of the present invention is preferably 10% by mass or more and 99% by mass or less in terms of high transparency of the coating film. Furthermore, the content of the solvent contained in the mixed composition of the present invention is more preferably 15% by mass or more and 95% by mass or less, even more preferably 20% by mass or more and 90% by mass or less, particularly preferably 25% by mass or more and 85% by mass or less, and particularly preferably 30% by mass or more and 80% by mass or less.
[0027] The mixed composition of the present invention is characterized by further containing a curing agent. The mixed composition of the present invention further contains a curing agent, which improves the water resistance of the coating film and maintains the antibacterial and antiviral properties.
[0028] Here, examples of the curing agent include compounds having an aziridine ring, isocyanate curing agents, and epoxy curing agents. Specifically, examples of the compound having an aziridine ring include Chemitite PZ-33 manufactured by Nippon Shokubai Co., Ltd. and Chemitite DZ-22E manufactured by Nippon Shokubai Co., Ltd. In addition, examples of the isocyanate curing agent include polyvalent isocyanates such as isocyanates and diisocyanates. In addition, examples of the epoxy curing agent include organic nitrogen compounds such as amine compounds and azole compounds (e.g., 2-methylimidazole, 2-indecylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, etc.), dicyandiamide, amino resins, compounds having a phenol skeleton, polyvalent phenol compounds, phenol resins, and mercaptan compounds.
[0029] In particular, when the curing agent is a compound having an aziridine ring, it is preferred since it has good compatibility with the anionic styrene-based resin.
[0030] In addition, the content of the curing agent contained in the mixed composition of the present invention is preferably 0.1% by mass or more and 50% by mass or less, since it improves the water resistance of the coating film and maintains antibacterial and antiviral performance. Furthermore, the content of the curing agent contained in the mixed composition of the present invention is more preferably 0.5% by mass or more and 45% by mass or less, even more preferably 1% by mass or more and 40% by mass or less, particularly preferably 1.5% by mass or more and 35% by mass or less, and particularly preferably 2% by mass or more and 30% by mass or less.
[0031] The mixed composition of the present invention is also characterized in that the complex metal acid compound contained in the mixed composition of the present invention has an amorphous and / or anatase type crystal structure. The composite metal acid compound contained in the mixed composition of the present invention is preferably one having an amorphous crystal structure, which has a high porosity and excellent photocatalytic performance. Also, the composite metal acid compound of the present invention is preferably one having an anatase crystal structure, which has a change in the migration speed of photoexcited carriers to the surface, which strongly depends on the surface potential barrier, and is presumed to be due to the lifespan specific to the crystal surface of the photoexcited carriers, which has excellent photocatalytic performance.
[0032] In addition, when the composite metal acid compound according to the present invention contains a crystal structure in which rutile and anatase types are mixed, the anatase ratio, which indicates the ratio of the molar ratio of anatase type to the total molar ratio of each crystal structure calculated from the XRD peak described later, is preferably 15% or more, more preferably 30% or more, even more preferably 50% or more, particularly preferably 60% or more, more particularly preferably 70% or more, even more particularly preferably 80% or more, and even more particularly preferably 90% or more. The anatase ratio is most preferably 100%.
[0033] Here, the crystal structure of the complex metal acid compound according to the present invention is judged to be an anatase crystal structure if a sharp XRD peak is observed at 2θ=25°±1 in an X-ray diffraction pattern obtained by X-ray diffraction measurement performed under the X-ray diffraction measurement conditions described below, and to be a rutile crystal structure if a sharp XRD peak is observed at 2θ=27°±1 (excluding 2θ=26°). On the other hand, if neither a sharp XRD peak indicating an anatase crystal structure nor a sharp XRD peak indicating a rutile crystal structure is observed, but a broad XRD peak is observed around 2θ=20° to 30°, the complex metal acid compound according to the present invention is judged not to be a crystalline structure but to be amorphous.
[0034] Furthermore, in the composite metal acid compound of the present invention, the area ratio of the XRD peak indicating the rutile crystal structure to the XRD peak indicating the anatase crystal structure, i.e., the anatase rate (%), can be calculated by carrying out X-ray diffraction measurement in accordance with ASTM D 3720-90 and using the following formula (1).
[0035]
number
[0036] The area (Ir) of the XRD peak showing the rutile type crystal structure in formula (1) and the area (Ia) of the XRD peak showing the anatase type crystal structure indicate the areas of the parts protruding from the baseline in the corresponding diffraction lines of the X-ray diffraction spectrum, and the calculation method thereof may be a known method, for example, computer calculation, approximate triangulation, etc.
[0037] The weight of the rutile powder (Wr) is the measured weight of the rutile powder, and the weight of the anatase powder (Wa) is the measured weight of the anatase powder. Furthermore, "K" is a constant that is calculated by plotting the difference between the actual weight ratio and the X-ray intensity ratio at several points, and corrects this difference.
[0038] In addition, when an XRD peak showing an anatase crystal structure is observed but an XRD peak showing a rutile crystal structure is not observed, the anatase ratio is set to 100%. In addition, when an XRD peak showing a rutile crystal structure is observed but an XRD peak showing an anatase crystal structure is not observed, the anatase ratio is set to 0%. Furthermore, the composite metal acid compound according to the present invention may be one in which a material showing an anatase crystal structure and a material showing a rutile crystal structure are mixed to adjust the anatase ratio.
[0039] Furthermore, when the composite metal acid compound according to the present invention contains a crystal structure in which amorphous and anatase types are mixed, the total ratio of amorphous and anatase types, which indicates the ratio of the total molar ratio of amorphous and anatase types to the total molar ratio of each crystal structure calculated from the above-mentioned XRD peak, is preferably 15% or more, more preferably 30% or more, even more preferably 50% or more, particularly preferably 60% or more, more particularly preferably 70% or more, even more particularly preferably 80% or more, and even more particularly preferably 90% or more. The total ratio of amorphous and anatase types is most preferably 100%.
[0040] Here, the total rate of amorphous and anatase type refers to the anatase rate of the sample, which can change the amorphous crystal structure to anatase type by heating a sample taken from the complex metal acid compound in an air atmosphere at 400°C for 3 hours. Since the XRD peak indicating the amorphous crystal structure is broadened, it is impossible to calculate the exact intensity ratio. Therefore, the amorphous region can be identified by heating the sample to change the amorphous to anatase type. For example, in a complex metal acid compound with an anatase rate of 40% and an amorphous peak, if the complex metal acid compound is heated in an air atmosphere at 400°C for 3 hours, and the anatase rate of the complex metal acid compound heated for 3 hours is 60%, the total rate of amorphous and anatase type of the complex metal acid compound is 60%.
[0041] In addition, the mixed composition of the present invention includes a complex metal oxide compound, L * a * b * L in color space * It is characterized by a value of 80 or more. The complex metal acid compound contained in the mixed composition of the present invention is L * a * b * L in color space * A value of 80 or more is preferable in that the color appears closer to white.
[0042] Here, L * a * b * L measured using the color system * The value indicates the lightness. * The closer the value is to 100, the lighter the color is, closer to white. * The closer the value is to 0, the darker the color is, closer to black. * The values are measured using a color difference meter (Konica Minolta: CR-300) in accordance with JIS Z 8722:2009.
[0043] The mixed composition of the present invention is also characterized in that the composite metal acid compound contained in the mixed composition of the present invention has an average primary particle size, as determined by observation with an electron microscope, of 0.1 nm or more and 50 μm or less. In the mixed composition of the present invention, the particles of the composite metal acid compound contained in the mixed composition of the present invention preferably have an average primary particle diameter of 0.1 nm or more and 50 μm or less as determined by electron microscopy, because the particle diameter is reduced and the photocatalytic performance is improved. The average primary particle diameter is more preferably 1 nm or more, and even more preferably 20 nm or more. The average primary particle diameter is more preferably 30 μm or less, even more preferably 1 μm or less, and particularly preferably 100 nm or less.
[0044] Here, the average primary particle diameter of the composite metal acid compound particles according to the present invention, as determined by electron microscopy, can be determined, for example, by using a scanning electron microscope (SEM) at an acceleration voltage of 1 kV and a magnification of 2,500x to 200,000x, in accordance with "JIS H 7804:2005 Method for measuring particle diameter of metal catalysts using an electron microscope." The average primary particle diameter is calculated by measuring the major axis Ll and minor axis Ls of 100 randomly selected primary particles, calculating the calculated particle diameter d from the formula "d=(Ll+Ls) / 2," and taking the arithmetic average of these values as the average primary particle diameter of the composite metal acid compound particles according to the present invention. Furthermore, when the maximum primary particle diameter of the composite metal acid compound particles of the present invention is 5 nm or less, it is difficult to measure accurately using a scanning electron microscope (SEM), so it may be determined using a transmission electron microscope (TEM) from a TEM image at a magnification of 20,000x to 150,000,000x under conditions of an accelerating voltage of 100 kV.
[0045] In addition, the mixed composition of the present invention is such that the composite metal oxide compound contained in the mixed composition of the present invention has a molar ratio of MoO 3 Conversion value / TiO 2 The converted value is represented as X, and the molar ratio Ta 2 O 5 Conversion value / TiO 2 When the converted value is represented as Y, the relationship 0.05≦X / Y≦400 is satisfied. The composite metal oxide compound contained in the mixed composition of the present invention has the molar ratio MoO 3 Conversion value / TiO 2 The converted value is represented as X, and the molar ratio Ta 2 O 5 Conversion value / TiO 2 When the converted value is expressed as Y, it is preferable in terms of having excellent photocatalytic performance if 0.05≦X / Y≦400 is satisfied, it is more preferable if 0.05≦X / Y≦100 is satisfied, it is even more preferable if 0.05≦X / Y≦50 is satisfied, it is particularly preferable if 0.1≦X / Y≦25 is satisfied, it is even more particularly preferable if 0.25≦X / Y≦15 is satisfied, and it is even more particularly preferable if 1≦X / Y≦15 is satisfied.
[0046] Unless otherwise specified, the composite metal acid compound of the present invention also includes a mixture of titanium oxide particles, molybdenum oxide particles, and tantalum oxide particles, and a mixture of partial composite metal acid compound particles (whose constituent elements are expressed as, for example, Ti-Mo-O+TaO or Ti-Ta-O+MoO) and single metal acid compound particles.
[0047] The mixed composition film of the present invention is characterized by containing the above-mentioned mixed composition of the present invention. The mixed composition film of the present invention contains the above-mentioned mixed composition of the present invention. The mixed composition film of the present invention can be used as a photocatalyst in building materials and coating materials. The manufacturing method of the mixed composition film of the present invention will be described later.
[0048] Here, the crystal structure of the composite metal acid compound crystal particles in the mixed composition film produced from the mixed composition of the present invention is judged to be an anatase type crystal structure if a sharp XRD peak is observed at 2θ=25°±1 in the X-ray diffraction pattern obtained by X-ray diffraction measurement performed according to the following thin film X-ray diffraction measurement conditions, and is judged to be a rutile type crystal structure if a sharp XRD peak is observed at 2θ=27°±1 (excluding 2θ=26°).
[0049] =Thin film X-ray diffraction measurement conditions= Diffraction equipment: X-ray diffraction equipment SmartLab (manufactured by Rigaku Corporation) Tube voltage / current: 40kV, 30mA Measurement range: 20~80(degrees) Measurement step: 0.04deg Measurement speed: 5deg / min ·Measurement method: General purpose / medium resolution PB / PSA (thin film method) *PB=Parallel Beam, PSA=Parallel Slit Analyzer X-ray analysis software: PDXL2 Version 2.9.1.0
[0050] Furthermore, the anatase ratio (%) of the composite metal acid compound crystal particles in the mixed composition film of the present invention can be calculated from the above formula (1) by carrying out X-ray diffraction measurement in accordance with ASTM D 3720-90.
[0051] The mixed composition and mixed composition film of the present invention are characterized in that the titanium or titanic acid, e.g., Mo-Ta-O+TiO, that is not combined with the molybdenum or molybdic acid and / or tantalum or tantalic acid remains. 2 The composition may contain, as an additive, oxide powders of Nb, W, Si, Zr, Zn, Al, Y, V, Fe, La-based (La, Ce, Nd, Eu, Gd, Dy, Yb), etc., within a range that does not impair the action and effect of the composition. The content of the additives described above is preferably less than 0.5% by mass, more preferably less than 0.1% by mass, and even more preferably less than 0.01% by mass, when the mixed composition of the present invention is taken as 100% by mass.
[0052] Furthermore, the mixed composition and the mixed composition film of the present invention may contain components (referred to as "other components") other than the components derived from titanium or titanic acid, molybdenum or molybdic acid, tantalum or tantalic acid, and the components derived from the dispersion, within a range that does not impair the action and effect of the mixed composition. Examples of the other components include Nb, W, Si, Zr, Zn, Al, Y, V, Fe, and La-based (La, Ce, Nd, Eu, Gd, Dy, Yb). However, the other components are not limited to these. The content of the above-mentioned other components is preferably less than 5% by mass, more preferably less than 4% by mass, and even more preferably less than 3% by mass, when the mixed composition of the present invention is taken as 100% by mass. It is assumed that the mixed composition and the mixed composition film of the present invention contain unavoidable impurities, which are not intended. The total content of unavoidable impurities is preferably less than 1 mass%, more preferably less than 0.1 mass%, and even more preferably less than 0.01 mass%, when the mixed composition of the present invention is 100 mass%.
[0053] The method for producing the above-mentioned mixed composition of the present invention will be described below.
[0054] In the method for producing the mixed composition of the present invention, a composite metal acid compound containing titanium as a main component and a resin are mixed and stirred to produce the mixed composition of the present invention.
[0055] First, the composite metal acid compound mainly composed of titanium contained in the mixed composition of the present invention can be produced, for example, by mixing and stirring a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion prepared as described below.
[0056] Examples of a method for producing a composite metal acid compound mainly composed of titanium and contained in the mixed composition of the present invention include a method for producing a composite metal acid compound of a first embodiment using a titanic acid aqueous dispersion as a titanic acid dispersion, and a method for producing a composite metal acid compound of a second embodiment using a titanium alkoxide as a titanic acid dispersion.
[0057] The method for producing the double metal acid compound of the first embodiment will be described below.
[0058] One example of a method for producing the titanic acid dispersion liquid of the first embodiment includes a production method in which a titanium salt solution is mixed with ammonia water to produce a neutralization reaction liquid (hereinafter referred to as the "titanium neutralization process"), a titanium-containing precipitate produced in the neutralization reaction liquid is washed (hereinafter referred to as the "titanium washing process"), and the washed titanium-containing precipitate is mixed with a quaternary ammonium salt and water (hereinafter referred to as the "titanium dissolution process") to obtain the titanic acid dispersion liquid of the first embodiment.
[0059] The titanium salt solution may be any solution in which titanium is dissolved, and examples thereof include an aqueous solution of titanyl sulfate, an aqueous solution of titanyl chloride, and an aqueous solution of titanium fluoride.
[0060] Here, the titanyl sulfate aqueous solution is obtained by dissolving titanyl sulfate in hot water. The titanyl sulfate aqueous solution contains titanium as TiO 2 It is preferable to prepare the content so that it is 8 to 15 mass % in terms of conversion.
[0061] (Titanium neutralization process) In the titanium neutralization step, a titanium salt solution, for example, an aqueous titanyl sulfate solution, is mixed with and reacted with aqueous ammonia to produce a neutralized reaction solution. Here, it is preferable to carry out a so-called reverse neutralization, in which the aqueous titanyl sulfate solution is added to aqueous ammonia to cause the reaction.
[0062] The ammonia concentration of the aqueous ammonia solution used for reverse neutralization is preferably 10% by mass to 40% by mass. If the ammonia concentration is 25% by mass, titanium is less likely to remain undissolved, and titanium or titanium oxide can be completely dissolved in water. On the other hand, if the ammonia concentration is 30% by mass or less, it is preferable because it is close to a saturated aqueous ammonia solution.
[0063] From this viewpoint, the ammonia concentration of the aqueous ammonia solution is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and particularly preferably 20% by mass, while the ammonia concentration is preferably 30% by mass or less, more preferably 35% by mass or less, and even more preferably 40% by mass or less.
[0064] In the case of reverse neutralization, the amount of titanyl sulfate solution added to the ammonia water is NH 3 / TiO 2 The molar ratio of is preferably 1 to 200, more preferably 10 to 100. In addition, the titanyl sulfate aqueous solution to be added to the ammonia water is adjusted to NH 3 / SO 4 2- The molar ratio of NH is preferably 1 or more, more preferably 5 or more, and even more preferably 10 or more. On the other hand, from the viewpoint of cost reduction, 3 / SO 4 2- The molar ratio of is preferably 50 or less, more preferably 40 or less, and even more preferably 30 or less.
[0065] In the reverse neutralization, the time for adding the titanyl sulfate aqueous solution to the ammonia water is preferably within 1 minute, more preferably within 30 seconds, and even more preferably within 10 seconds. That is, rather than gradually adding the titanyl sulfate aqueous solution over a period of time, it is preferable to add it to the ammonia water in as short a time as possible, for example, all at once, and carry out the neutralization reaction. In addition, in the reverse neutralization, since the acidic titanyl sulfate aqueous solution is added to the alkaline ammonia water, the neutralization reaction can be carried out while maintaining a high pH.
[0066] (Titanium cleaning process) By washing the slurry of the titanium-containing precipitate in the neutralization reaction solution obtained by reverse neutralization, impurities are removed and a titanium-containing precipitate is obtained. The slurry of the titanium-containing precipitate obtained by reverse neutralization contains unnecessary components other than titanium or titanium oxide hydrates or ions and ammonia, such as sulfate compounds such as ammonium sulfate, as impurities, and it is preferable to remove these.
[0067] Any method of washing, for example, a method of removing sulfate compounds, may be used. For example, a method using a membrane such as reverse osmosis filtration, ultrafiltration, or microfiltration using ammonia water or pure water, as well as centrifugation and other known methods may be used. The titanium washing step may be performed at room temperature, and there is no particular need to adjust the temperature of each step.
[0068] (Titanium melting process) Then, the titanium-containing precipitate obtained by removing impurities in the titanium washing process can be mixed with a dispersion medium such as water and a quaternary ammonium salt, and stirred as necessary to promote the reaction, thereby producing the titanic acid dispersion of the first embodiment.
[0069] Examples of the quaternary ammonium salt include tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, methyltripropylammonium hydroxide, methyltributylammonium hydroxide, tetrapentylammonium hydroxide, tetrahexylammonium hydroxide, ethyltrimethylammonium hydroxide, dimethyldiethylammonium hydroxide, benzyltrimethylammonium hydroxide, hexadecyltrimethylammonium hydroxide, and (2-hydroxyethyl)trimethylammonium hydroxide.
[0070] As described above, the amount of quaternary ammonium salt added is preferably such that a quaternary ammonium salt containing 0.44 moles or more of quaternary ammonium compound is mixed per mole of titanium contained in the titanium-containing precipitate after washing, since a larger amount of quaternary ammonium compound can increase the solubility of titanium or titanic acid in water, in the dissolving step. On the other hand, if the amount of quaternary ammonium compound is too large, problems such as impeding film formation or inhibiting catalytic action may occur, so that in the titanium dissolving step described above, a quaternary ammonium salt containing 1.0 moles or less of quaternary ammonium compound is mixed per mole of titanium contained in the titanium-containing precipitate after washing.
[0071] The above-mentioned titanium neutralization step, titanium washing step, and titanium dissolving step may be carried out at room temperature, and there is no particular need to adjust the temperature of each step.
[0072] Next, a method for producing a molybdic acid dispersion will be described below.
[0073] An example of a method for producing a molybdic acid dispersion liquid includes a method of producing a neutralized reaction liquid by adding an acidic molybdenum aqueous solution to an ammonia aqueous solution (hereinafter referred to as a "molybdenum neutralization step"), washing a molybdenum-containing precipitate produced in the neutralized reaction liquid (hereinafter referred to as a "molybdenum washing step"), and adding an organic nitrogen compound to the washed molybdenum-containing precipitate (hereinafter referred to as a "molybdenum dissolving step") to obtain a molybdic acid dispersion liquid.
[0074] The acidic aqueous molybdenum solution refers to an aqueous molybdenum sulfate solution obtained by subjecting a solution in which molybdenum is dissolved in an acidic aqueous solution containing sulfuric acid to solvent extraction.
[0075] Here, the molybdenum sulfate aqueous solution is prepared by adding water (e.g., pure water) to convert molybdenum to MoO 3 It is preferable to adjust the molybdenum concentration to 1-100g / L in terms of molybdenum concentration. 3 When the molybdenum concentration is 1 g / L or more in terms of the molybdenum oxide compound hydrate, which is easily soluble in water, it is preferable, and when productivity is taken into consideration, it is more preferable that the molybdenum concentration is 10 g / L or more, and even more preferable that the molybdenum concentration is 20 g / L or more. 3 A molybdic acid compound hydrate having a converted concentration of 100 g / L or less is preferable because it will be a molybdic acid compound hydrate that is easily soluble in water, and in order to more reliably synthesize a molybdic acid compound hydrate that is easily soluble in water, a concentration of 90 g / L or less is more preferable, a concentration of 80 g / L or less is even more preferable, and a concentration of 70 g / L or less is particularly preferable. From the viewpoint of completely dissolving molybdenum or molybdenum oxide, the pH of the aqueous molybdenum sulfate solution is preferably 2 or less, and more preferably 1 or less.
[0076] (Molybdenum neutralization process) In the molybdenum neutralization step, when an aqueous molybdenum sulfate solution is added to an aqueous ammonia solution, in the so-called reverse neutralization method, it is preferable to add the aqueous molybdenum sulfate solution to a 10% by mass to 30% by mass aqueous ammonia solution, i.e., to obtain a slurry of a molybdic acid compound hydrate, that is, a slurry of a molybdenum-containing precipitate, by the reverse neutralization method.
[0077] The ammonia concentration of the aqueous ammonia solution used for reverse neutralization is preferably 10% by mass to 30% by mass. When the ammonia concentration is 10% by mass, molybdenum is less likely to remain undissolved, and molybdenum or molybdenum oxide can be completely dissolved in water. On the other hand, when the ammonia concentration is 30% by mass or less, it is preferable because it is close to a saturated aqueous ammonia solution.
[0078] From this viewpoint, the ammonia concentration of the aqueous ammonia solution is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 25% by mass, while the ammonia concentration is preferably 30% by mass or less, more preferably 29% by mass or less, and even more preferably 28% by mass or less.
[0079] In the reverse neutralization, the amount of molybdenum sulfate solution added to the ammonia water is NH 3 / MoO 3 The molar ratio of is preferably 0.1 to 300, more preferably 5 to 200. In addition, the molybdenum sulfate aqueous solution added to the ammonia water is preferably NH 3 / SO 4 2- The molar ratio of NH is preferably 3.0 or more, more preferably 10.0 or more, and even more preferably 20.0 or more. On the other hand, from the viewpoint of cost reduction, 3 / SO 4 2- The molar ratio of is preferably 200 or less, more preferably 150 or less, and even more preferably 100 or less.
[0080] In the reverse neutralization, the time for adding the molybdenum sulfate aqueous solution to the ammonia water is preferably within 1 minute, more preferably within 30 seconds, and even more preferably within 10 seconds. In other words, rather than gradually adding the molybdenum sulfate aqueous solution over a period of time, it is preferable to add it to the ammonia water in as short a time as possible, for example, all at once, and carry out the neutralization reaction. In addition, in the reverse neutralization, since the acidic molybdenum sulfate aqueous solution is added to the alkaline ammonia water, the neutralization reaction can be carried out while maintaining a high pH.
[0081] (Molybdenum cleaning process) In the molybdenum washing step, sulfur is removed from the slurry of the molybdenum-containing precipitate obtained by the reverse neutralization method to produce a molybdenum-containing precipitate from which the sulfur is removed. Since the slurry of the molybdenum-containing precipitate obtained by the reverse neutralization method contains, as impurities, sulfate ions that remain without reacting with molybdenum or molybdenum oxide, and sulfur components in the form of hydrogen sulfate ions, it is preferable to remove these.
[0082] Any method for removing sulfur may be used, and examples of the method include a method using a membrane such as reverse osmosis filtration, ultrafiltration, or microfiltration using ammonia water or pure water, centrifugation, and other known methods. When removing sulfur from the slurry of the molybdenum-containing precipitate, temperature control is not particularly required, and the removal may be performed at room temperature.
[0083] Specifically, the molybdenum-containing precipitate slurry obtained by the reverse neutralization method is decanted using a centrifuge, and washing is repeated until the conductivity of the molybdenum-containing precipitate slurry becomes 500 μS / cm or less, thereby obtaining a molybdenum-containing precipitate from which sulfur has been removed. The conductivity was measured by adjusting the liquid temperature of the molybdenum-containing precipitate slurry to 25° C., immersing the measuring part of a conductivity meter (ASCON2 manufactured by AS ONE CORPORATION) in the supernatant liquid of the precipitate slurry, and reading the conductivity value after it stabilized.
[0084] The cleaning solution used to remove the sulfur content is preferably ammonia water. Specifically, ammonia water of 5.0 mass% or less is preferable, ammonia water of 4.0 mass% or less is more preferable, ammonia water of 3.0 mass% or less is even more preferable, and ammonia water of 2.5 mass% is particularly preferable. When the ammonia water is 5.0 mass% or less, ammonia and ammonium ions are appropriate for the sulfur content, and unnecessary cost increases can be avoided.
[0085] (Molybdenum melting process) In the molybdenum dissolving step, an organic nitrogen compound is added to a molybdenum-containing precipitate slurry obtained by dissolving the molybdenum-containing precipitate in a slurry state, thereby producing a molybdic acid dispersion liquid. The molybdenum-containing precipitate slurry is prepared by diluting the molybdenum-containing precipitate from which the sulfur content has been removed as described above with pure water or the like to produce a slurry state. The molybdenum concentration of the molybdenum-containing precipitate slurry from which the sulfur content has been removed is measured by taking a portion of the slurry, drying it at 110°C for 24 hours, and then calcining it at 1,000°C for 4 hours to obtain MoO 3 The MoO 3 The weight of the slurry is measured, and the molybdenum concentration of the slurry can be calculated from the weight.
[0086] Then, an organic nitrogen compound is mixed with the molybdenum-containing precipitate slurry from which the sulfur content has been removed, thereby obtaining a molybdic acid dispersion.
[0087] Specifically, the molybdenum concentration in the final mixture is MoO 3 The obtained molybdenum-containing precipitate slurry is added to an organic nitrogen compound so that the molybdenum concentration is 0.1 to 40 mass % in terms of molybdenum content, and then mixed with pure water. The mixture is stirred while maintaining the liquid temperature at room temperature (25°C) for 1 hour, thereby obtaining a molybdic acid dispersion.
[0088] The organic nitrogen compounds which are mixed with the molybdenum-containing precipitation slurry are preferably amines, especially aliphatic amines, and / or quaternary ammonium compounds.
[0089] Here, from the viewpoint of solubility, the aliphatic amine is preferably mixed so that the aliphatic amine concentration in the molybdenum-containing precipitation slurry is 40 mass% or less. From the same viewpoint, the aliphatic amine is preferably mixed so that the aliphatic amine concentration in the molybdenum-containing precipitation slurry is 0.1 mass% or more, more preferably 20 mass% or more. The aliphatic amine is more preferably methylamine or dimethylamine, and particularly preferably methylamine.
[0090] On the other hand, from the viewpoint of solubility, the quaternary ammonium compound is preferably mixed so that the concentration of the quaternary ammonium compound in the molybdenum-containing precipitation slurry is 40 mass% or less. From the same viewpoint, the quaternary ammonium compound is preferably mixed so that the concentration of the quaternary ammonium compound in the molybdenum-containing precipitation slurry is 0.1 mass% or more, and more preferably 20 mass% or more. The quaternary ammonium compound is more preferably tetramethylammonium hydroxide (TMAH) or tetraethylammonium hydroxide (TEAH).
[0091] The above-mentioned molybdenum neutralization step, molybdenum washing step, and molybdenum dissolving step may be carried out at room temperature, and there is no particular need to adjust the temperature of each step.
[0092] Furthermore, a method for producing the tantalic acid dispersion will be described below.
[0093] As an example of a method for producing a tantalic acid dispersion, a tantalum salt solution is added to an amine aqueous solution to produce a primary reaction solution (hereinafter referred to as a "tantalum primary neutralization step"), the primary reaction solution is added to an ammonia water to produce a secondary reaction solution (hereinafter referred to as a "tantalum secondary neutralization step"), the tantalum-containing precipitate produced in the secondary reaction solution is washed (hereinafter referred to as a "tantalum washing step"), and the washed tantalum-containing precipitate is mixed with an amine and water (hereinafter referred to as a "tantalum dispersion step") to obtain a tantalic acid dispersion. In addition, a tantalic acid compound described later can be used to mix a tantalic acid compound with an amine and water to obtain a tantalic acid dispersion.
[0094] The tantalum salt solution as the starting material may be any solution in which tantalum is dissolved, such as an aqueous solution of tantalum fluoride or tantalum chloride.
[0095] Tantalum fluoride aqueous solution is prepared by reacting tantalum, tantalum oxide, or tantalum hydroxide with hydrofluoric acid (HF), such as hydrofluoric acid aqueous solution, to produce tantalum fluoride (H 2 TaF 7 ) and dissolving it in water to prepare the product.
[0096] This tantalum fluoride aqueous solution is made by adding water (e.g., pure water) to the tantalum. 2 O 5 It is preferable to prepare the solution so that it contains 1-100 g / L in terms of tantalum content. In this case, if the tantalum concentration is 1 g / L or more, it will become a tantalic acid compound hydrate that is easily soluble in water, so the tantalum concentration of the tantalum fluoride aqueous solution is Ta 2 O 5 It is more preferable that the tantalum concentration is 1 g / L or more in terms of the concentration, and in terms of productivity, it is 10 g / L or more, and even more preferable that it is 20 g / L or more. On the other hand, if the tantalum concentration is 100 g / L or less, the tantalic acid compound hydrate that is easily soluble in water will be obtained, so in order to more reliably synthesize a tantalic acid compound hydrate that is easily soluble in water, it is more preferable that the tantalum concentration is 90 g / L or less, and even more preferable that it is 80 g / L or less, and even more preferable that it is 70 g / L or less.
[0097] The pH of the tantalum fluoride aqueous solution is preferably 2 or less, more preferably 1 or less, from the viewpoint of completely dissolving tantalum or tantalum oxide. On the other hand, the tantalum chloride aqueous solution contains tantalum chloride (TaCl 5 ) in a small amount of methanol and then adding water.
[0098] (Tantalum primary neutralization process) It is important to react the tantalum salt solution with the aqueous amine solution (primary neutralization) and then to carry out a treatment of reacting it with aqueous ammonia (secondary neutralization).
[0099] If the primary neutralization is performed only with the tantalum salt solution and the aqueous amine solution, and the secondary neutralization is not performed with aqueous ammonia, the precipitate will not be generated or the amount of precipitate generated will be small, and the yield of the present tantalic acid dispersion will be low. Furthermore, even if the precipitate is generated, if it is directly subjected to the washing step, it will become a tantalic acid compound hydrate that is partially insoluble, and a tantalic acid dispersion with high dispersibility cannot be obtained.
[0100] Furthermore, even if the order of the primary and secondary neutralization is reversed, and the tantalum salt solution is reacted with ammonia water and then with an aqueous amine solution, the tantalum or tantalic acid cannot be suitably dispersed in water in the subsequent dispersion step, much less converted into an aqueous solution.
[0101] In the primary tantalum neutralization step, it is preferable to carry out reverse neutralization, in which a tantalum salt solution such as a tantalum fluoride aqueous solution is added to an amine aqueous solution to cause a reaction. In normal neutralization, in which an amine aqueous solution is added to a tantalum salt solution such as a tantalum fluoride aqueous solution, the tantalum or tantalic acid cannot be suitably dispersed in water in the subsequent dispersion step, much less made into an aqueous solution. It is presumed that reverse neutralization makes the structure of the tantalum or tantalic acid more water-soluble.
[0102] Preferred examples of the amine in the aqueous amine solution used in the tantalum primary neutralization step include alkylamines.
[0103] The alkylamine preferably has 1-3 alkyl groups. When the alkylamine has 2-3 alkyl groups, the 3 alkyl groups may be the same or different. From the viewpoint of solubility, the alkyl group of the alkylamine preferably has 1-6 carbon atoms, more preferably 4 or less, even more preferably 3 or less, and even more preferably 2 or less.
[0104] Specific examples of the alkylamine include methylamine, dimethylamine, trimethylamine, ethylamine, methylethylamine, diethylamine, triethylamine, methyldiethylamine, dimethylethylamine, n-propylamine, di-n-propylamine, tri-n-propylamine, iso-propylamine, di-iso-propylamine, tri-iso-propylamine, n-butylamine, di-n-butylamine, tri-n-butylamine, iso-butylamine, di-iso-butylamine, tri-iso-butylamine, tert-butylamine, n-pentylamine, and n-hexylamine.
[0105] Among these, from the viewpoint of solubility, methylamine, dimethylamine, trimethylamine, ethylamine, methylethylamine, diethylamine, triethylamine, methyldiethylamine and dimethylethylamine are preferred, and among these, methylamine, dimethylamine and trimethylamine are more preferred.
[0106] In the primary neutralization of tantalum, from the viewpoint of enhancing dispersibility, the tantalum salt solution is preferably added to an aqueous amine solution containing an amine in an amount equal to or greater than the molar ratio of fluorine contained in the tantalum salt solution, i.e., 1 or more, and more preferably 1.2 or more, and even more preferably 1.4 or more.
[0107] On the other hand, from the viewpoint of increasing the amount of waste liquid, it is preferable to add the tantalum salt solution to an aqueous amine solution containing an amine in a molar ratio to the fluorine contained in the tantalum salt solution of 2 or less, and more preferably 1.8 or less, and even more preferably 1.6 or less.
[0108] In the primary tantalum neutralization step, when a tantalum salt solution such as a tantalum fluoride aqueous solution is added to an amine aqueous solution, it is preferable to carry out the neutralization reaction within 1 minute. That is, it is preferable to add the tantalum salt solution within 1 minute, for example, all at once, rather than gradually adding the tantalum salt solution over a period of time, to carry out the neutralization reaction. In this case, the addition time of the tantalum salt solution is preferably within 1 minute, more preferably within 30 seconds, and even more preferably within 10 seconds.
[0109] (Tantalum secondary neutralization process) In the secondary neutralization of tantalum, it is preferable to add the primary reaction solution obtained in the primary neutralization step of tantalum to ammonia water to obtain a secondary reaction solution. When the primary reaction solution is added to ammonia water, a precipitate (called a "tantalum-containing precipitate") is generated in the water.
[0110] In the secondary neutralization of tantalum, from the viewpoint of further improving the dispersibility of the present tantalic acid dispersion, it is preferable to carry out reverse neutralization in which the primary reaction liquid obtained in the primary neutralization step of tantalum is added to aqueous ammonia for reaction.
[0111] In this case, from the viewpoint of enhancing the dispersibility of the present tantalic acid dispersion, the ammonia concentration of the above-mentioned aqueous ammonia solution is preferably 10-30% by mass. Of these, it is more preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more. On the other hand, it is more preferably 29% by mass or less, and even more preferably 28% by mass or less.
[0112] In the secondary tantalum neutralization step, from the viewpoint of improving dispersibility in the subsequent tantalum dispersion step, it is further preferable to add the primary reaction liquid to an aqueous ammonia solution containing an ammonia having a molar ratio of 7.5 or more, particularly 8.0 or more, and particularly 8.5 or more, relative to the fluorine contained in the primary reaction liquid.
[0113] On the other hand, from the viewpoint of increasing the amount of waste liquid, it is preferable to add the primary reaction liquid to ammonia water containing an ammonia at a molar ratio of 10.0 or less to the fluorine contained in the primary reaction liquid, and more preferably to add the primary reaction liquid to ammonia water containing an ammonia at a ratio of 9.5 or less, and even more preferably 9.0 or less.
[0114] In the tantalum secondary neutralization step, when the primary reaction liquid is added to the ammonia water, it is preferable to carry out the neutralization reaction within 1 minute. That is, it is preferable to add the primary reaction liquid within 1 minute, for example, all at once, rather than gradually adding the primary reaction liquid over a period of time, to carry out the neutralization reaction. In this case, the addition time of the primary reaction liquid is preferably within 1 minute, more preferably within 30 seconds, and even more preferably within 10 seconds.
[0115] (Tantalum cleaning process) In the secondary reaction liquid obtained by the secondary neutralization of tantalum, particularly in the tantalum-containing precipitate, unnecessary components other than tantalum or tantalic acid hydrates or ions and amines, such as fluorine compounds such as ammonium fluoride, are present as impurities in the water, and therefore it is preferable to remove these unnecessary components.
[0116] Any method for washing, for example, a method for removing fluorine compounds, may be used. For example, a method using a membrane such as reverse osmosis filtration, ultrafiltration, or microfiltration using ammonia water or pure water, as well as centrifugation and other known methods may be used.
[0117] (Tantalum dispersion process) Next, a dispersion medium such as water is added to the tantalum-containing precipitate obtained by washing in the tantalum washing step, for example, the tantalum-containing precipitate obtained by removing fluorine, and an amine and / or a quaternary ammonium compound is added, and the mixture is stirred as necessary to promote the reaction, thereby producing a tantalic acid dispersion.
[0118] The type of amine to be added is the same as that which can be used in the primary neutralization. As described above, the amount of amine added is preferably adjusted as described above, since a larger amount of amine can increase the dispersibility or solubility of tantalum or tantalic acid in water, while an excessively large amount of amine can cause problems such as impeding film-forming properties or inhibiting catalytic action.
[0119] On the other hand, from the viewpoint of solubility, the quaternary ammonium compound is preferably mixed so that the concentration of the quaternary ammonium compound in the tantalum-containing precipitate is 40 mass% or less. From the same viewpoint, the quaternary ammonium compound is preferably mixed so that the concentration of the quaternary ammonium compound in the tantalum-containing precipitate is 0.1 mass% or more, and more preferably 20 mass% or more. The quaternary ammonium compound is more preferably tetramethylammonium hydroxide (TMAH) or tetraethylammonium hydroxide (TEAH).
[0120] The tantalum primary neutralization step, the tantalum secondary neutralization step, the tantalum washing step, and the tantalum dispersion step may be carried out at room temperature, and there is no particular need to forcibly adjust the temperature.
[0121] The titanic acid dispersion, molybdic acid dispersion, and tantalic acid dispersion containing quaternary ammonium obtained through the above-mentioned manufacturing steps were dissolved in water to obtain a titanium content of TiO 2 When the molybdenum content is expressed as 1, the molar ratio MoO 3 Conversion value / TiO 2 The molybdic acid dispersion was prepared so that the conversion value was 0.01-20, and the tantalum content was calculated as the molar ratio Ta 2 O 5 Conversion value / TiO 2 This is mixed with a tantalic acid dispersion liquid adjusted to have a conversion value of 0.01-0.5, and the liquid is stirred for 10 minutes at room temperature (25°C) to produce a composite metal mixture liquid.
[0122] In addition, the step of producing the composite metal mixture liquid in the first embodiment may involve mixing and stirring a titanic acid dispersion liquid and a tantalic acid dispersion liquid, and then adding and stirring a molybdic acid dispersion liquid to produce a mixture liquid.
[0123] When mixing the titanic acid dispersion liquid containing a quaternary ammonium compound, the molybdic acid dispersion liquid, and the tantalic acid dispersion liquid, the intermediate mixed liquid obtained by mixing the titanic acid dispersion liquid containing a quaternary ammonium compound and the tantalic acid dispersion liquid prepared as described above is stirred for 10 minutes at room temperature (25°C), and then the molybdic acid dispersion liquid prepared as described above is added to the intermediate mixed liquid and stirred for a further 10 minutes at room temperature (25°C), thereby obtaining the composite metal mixed liquid of the first embodiment.
[0124] Adding a tantalic acid dispersion to a titanic acid dispersion and then adding a molybdic acid dispersion is preferable in that after a portion of the titanium and tantalum are dissolved in solid solution, the remaining titanium and molybdenum are dissolved in solid solution, thereby reducing the particle size and making the mixture less likely to gel.
[0125] The composite metal mixture of the first embodiment thus obtained is placed in a static furnace and dried at atmospheric pressure for 6 hours at a heating temperature of about 110°C to remove moisture from the composite metal mixture of the first embodiment, thereby obtaining the dried powder of the first embodiment. The mixture of the first embodiment may also be placed in a vacuum drying furnace with an internal pressure of 0.01 MPa, heated to 110°C or higher, and vacuum dried for 6 hours. Here, a portion of the dried powder was sampled and subjected to X-ray diffraction measurement, and a broad XRD peak indicating amorphous was observed around 2θ=20° to 30°.
[0126] Next, the obtained dry powder is placed in a stationary furnace, heated at the following heating temperature, and calcined for 3 hours to obtain a calcined powder, i.e., a powdered composite metal acid compound of the first embodiment. Here, when the heating temperature is more than 400°C and not more than 900°C, the crystal structure of the composite metal acid compound crystal particles contained in the composite metal acid compound of the first embodiment is anatase type, which is preferable in terms of having excellent photocatalytic performance in the visible light region. Furthermore, when the heating temperature is 400°C or less, the composite metal acid compound of the first embodiment does not have a crystal structure and is amorphous. In this case, it is preferable in terms of being able to keep the heating temperature low and reducing the manufacturing cost. Furthermore, the calcination time is preferably 1 hour to 10 hours. When the calcination time is 1 hour to 10 hours, it is sufficient time for the growth of the composite metal acid compound crystal particles, and unnecessary costs can be reduced. Furthermore, the calcination time is more preferably 1.5 hours to 8 hours, and even more preferably 2 hours to 6 hours.
[0127] The calcined powder may be pulverized and used as the complex metal acid compound. Regardless of whether or not the calcined powder is pulverized, the undersieve (fine particle side) obtained by classifying the calcined powder using a sieve or the like may be used as the complex metal acid compound. The oversieve (coarse particle side) may be pulverized again and classified for use. It is also possible to combine pulverization and classification using a vibrating sieve into which iron balls coated with nylon or fluororesin are charged as pulverizing media. By combining classification and pulverization in this way, even if there are complex metal acid compound particles that are too large after roasting, they can be removed. Specifically, when classifying using a sieve, it is preferable to use one with an opening of 150 μm to 1,000 μm. If the opening is 150 μm to 1,000 μm, the proportion of oversieve particles will not be too high, so that re-pulverization will not be repeated, and complex metal acid compounds that need to be re-pulverized will not be classified as undersieve.
[0128] Next, a method for producing the complex metal acid compound of the second embodiment will be described below, with the same production method as the production method for the complex metal acid compound of the first embodiment being omitted.
[0129] The titanium alkoxide used as the titanic acid dispersion liquid of the second embodiment, for example, titanium tetraisopropoxide, the molybdic acid dispersion liquid, and the tantalic acid dispersion liquid are mixed together to obtain a titanium content of TiO 2 When the molybdenum content is expressed as 1, the molar ratio MoO 3 Conversion value / TiO 2 The molybdic acid dispersion was prepared so that the conversion value was 0.01-20, and the tantalum content was calculated as the molar ratio Ta 2 O 5 Conversion value / TiO 2 The composite metal mixture of the second embodiment is obtained by hydrothermal synthesis of the mixture prepared by mixing with a tantalic acid dispersion liquid adjusted to have a conversion value of 0.01-0.5 in an autoclave at a heating temperature of 25°C-400°C, a heating time of 1 hour-99 hours, and a pressurizing pressure of 0.1 MPa-40 MPa. The composite metal mixture of the second embodiment is a translucent sol (suspension solution).
[0130] Examples of titanium alkoxides used as the titanic acid dispersion liquid of the second embodiment include titanium i-propoxide, titanium n-butoxide, titanium 2-ethylhexoxide, titanium tert-butoxide, titanium stearyl alkoxide, and titanium tetraisopropoxide, in addition to titanium tetraisopropoxide.
[0131] The molybdic acid dispersion and the tantalic acid dispersion to be mixed with the titanium alkoxide preferably contain a relatively highly volatile amine instead of a quaternary ammonium compound. If the molybdic acid dispersion and the tantalic acid dispersion to be mixed with the titanium alkoxide contain a quaternary ammonium compound, molybdenum will dissolve during the above-mentioned hydrothermal synthesis, and the composition of the composite metal mixture of the second embodiment will change.
[0132] The heating temperature in the hydrothermal synthesis is preferably, for example, 180° C., the heating time is preferably 12 hours, and the applied pressure is preferably equal to or higher than the saturated water vapor pressure, and more preferably 1.05 MPa.
[0133] Furthermore, similarly to the method for producing a composite metal mixture liquid of the first embodiment, titanium alkoxide and a tantalic acid dispersion liquid are mixed and stirred, and then a molybdic acid dispersion liquid is added and stirred to produce a mixture liquid, after which hydrothermal synthesis is carried out. This is preferable in that after a portion of the titanium and tantalum are dissolved, the remaining titanium and molybdenum are dissolved, resulting in a small particle size and making it less likely to gel.
[0134] The composite metal mixture of the second embodiment thus obtained is centrifuged at a rotation speed of 300 rpm to 6,000 rpm for a rotation time of 1 minute to 99 minutes using a centrifuge (Hitachi, Ltd.: himac CT 6E), to precipitate a precipitate cake. The rotation speed of the centrifuge is preferably 4,000 rpm, and the rotation time is preferably 20 minutes.
[0135] The precipitated cake is then collected and placed in a static furnace, where it is dried at a heating temperature of 25°C to 600°C for a heating time of 1 minute to 24 hours, and the dried precipitate cake is pulverized to obtain a powdered composite metal acid compound of the second embodiment. A part of the composite metal acid compound of the second embodiment is sampled and subjected to X-ray diffraction measurement, and a sharp XRD peak indicating an anatase type is observed at 2θ=25°±1. When the precipitate cake is dried, the heating temperature is preferably 110°C, and the heating time is preferably 1 hour.
[0136] As with the composite metal mixture liquid of the first embodiment, the dried precipitate cake may be pulverized, placed in a stationary furnace, heated at a heating temperature of 600° C., and baked for 3 hours.
[0137] Then, the obtained composite metal acid compound of the first or second embodiment is mixed with a solvent such as water, an organic solvent, or a mixed solvent of water and an organic solvent, and a dispersant (e.g., a phosphate ester-based dispersant), and the composite metal acid compound of the first or second embodiment is crushed using a paint shaker or a bead mill.
[0138] When the composite metal acid compound of the first or second embodiment is crushed using a paint shaker or a bead mill, the addition of a dispersant improves dispersibility and facilitates crushing into fine powder, which is preferable in that the transparency of the coating film is increased as a result. Examples of the dispersant include a phosphate ester dispersant.
[0139] The amount of the dispersant added is preferably 0% by mass or more and 50% by mass or less based on the weight of the composite metal acid compound, since this improves dispersibility and facilitates crushing into fine powder, resulting in high transparency of the coating film.The amount of the dispersant added is more preferably 0.1% by mass or more and 40% by mass or less based on the weight of the composite metal acid compound, more preferably 0.2% by mass or more and 30% by mass or less, and particularly preferably 0.3% by mass or more and 30% by mass or less.
[0140] Thereafter, a resin (e.g., a styrene-based resin), a curing agent, and if necessary, water, an organic solvent, or a mixed solvent of water and an organic solvent are added, mixed, and stirred at 25°C for 10 minutes to obtain the mixed composition of the present invention. When the resin is an anionic styrene resin, the curing agent is preferably a compound having an aziridine ring, such as an aziridine-based crosslinking agent. The water, organic solvent, or mixed solvent of water and an organic solvent may be added in an amount necessary to adjust the mixed composition of the present invention to an arbitrary concentration.
[0141] Next, a method for producing the mixed composition film of the present invention will be described below.
[0142] The method for producing a mixed composition film of the present invention is to apply the mixed composition produced by the above-mentioned method for producing a mixed composition of the present invention onto a substrate and dry it to produce a mixed composition film. Note that the mixed composition of the present invention may be added with water, an organic solvent, or a mixed solvent of water and an organic solvent to a concentration that makes it easy to apply the mixed composition onto a substrate.
[0143] Specifically, the mixed composition obtained by the method for producing the mixed composition of the present invention is dropped onto a substrate using a syringe while being filtered, for example, with a filter having a pore size of 2 μm, as necessary, and then coated by spin coating (1,500 rpm, 30 seconds).Then, the substrate coated with the mixed composition of the present invention is placed in a static furnace and dried at room temperature (25° C.) for 3 hours to obtain a mixed composition film of the present invention.
[0144] Alternatively, the substrate coated with the mixture composition of the present invention may be placed in a static furnace, heated to 110° C., and dried for 6 hours, or heated to 600° C. and baked for 3 hours.
[0145] In this specification, when "X to Y" (X and Y are any numbers) is expressed, unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably greater than X" or "preferably smaller than Y". In addition, when "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the meaning of "preferably greater than X" or "preferably less than Y". Effect of the Invention
[0146] The mixed composition of the present invention has excellent photocatalytic performance and is excellent in film-forming properties on a substrate. [Brief description of the drawings]
[0147] [Figure 1] 1 is a table showing physical property values of the mixed compositions according to Examples 1 to 7 and the double metal acid compound according to Comparative Example 1. [Diagram 2] 1 is a table showing the physical property values and measurement results of the double metal acid compounds according to Experimental Examples 1 to 18. BEST MODE FOR CARRYING OUT THEINVENTION
[0148] The mixed composition according to the embodiment of the present invention will be further described below with reference to the following examples, although the present invention is not limited to these examples.
[0149] Example 1 The mixed composition according to Example 1 was obtained as follows. First, industrial ethanol (manufactured by Japan Alcohol Sales Co., Ltd., product name: Solmix) and a phosphate ester-based dispersant as a dispersant were added to the composite metal acid compound described below, and the mixture was crushed using a paint shaker. At that time, the amount of the dispersant added was set to 5 mass% with respect to the weight of the composite metal acid compound. Next, when the mixed composition according to Example 1 was taken as 100 mass%, 0.7 mass% of the composite metal acid compound, 33.3 mass% of a cationic styrene resin (manufactured by Arakawa Chemical Industries Co., Ltd., product name: WC-M-1206) as a resin, and 66.0 mass% of industrial ethanol as a solvent were prepared, mixed, and stirred at room temperature (25°C) for 10 minutes to obtain a composition.
[0150] Here, the composite metal acid compound of Example 1 was obtained by mixing a titanic acid dispersion liquid, a molybdic acid dispersion liquid, and a tantalic acid dispersion liquid prepared as described below, stirring the resulting mixture at room temperature (25°C) for 10 minutes, placing the mixture in a static furnace, and drying it in the air at a heating temperature of about 110°C for 6 hours to remove the moisture from the mixture, and then drying the resulting dry powder in the air at a heating temperature of 600°C for 3 hours.
[0151] First, the titanic acid dispersion was obtained, for example, by the process described below.
[0152] 33.3 g of titanyl sulfate (Teika Co., Ltd., TiO 2 The titanyl sulfate aqueous solution (titanium concentration (TiO 2 The resulting solution had a pH of 1 or less (calculated as 11% by mass, sulfuric acid 17% by mass, pH 1 or less).
[0153] 100g of this titanyl sulfate aqueous solution was added to 2,200g of 25% by mass ammonia water (18.9 moles of ammonia per mole of sulfuric acid in the titanyl sulfate aqueous solution) over a period of less than 1 minute. After that, the mixture was stirred for 15 minutes to obtain a neutralized reaction liquid (pH 12). This neutralized reaction liquid was a slurry of titanium-containing material, in other words, a slurry of titanium-containing precipitate.
[0154] Next, the neutralized reaction solution was decanted using a centrifuge and washed until the sulfuric acid content of the supernatant was 100 mg / L or less, to obtain a titanium-containing precipitate from which sulfuric acid had been removed. At this time, ammonia water was used as the washing liquid.
[0155] A portion of this titanium-containing precipitate was calcined at 1,000°C for 4 hours to obtain TiO 2 The mass of TiO contained in the titanium-containing precipitate was calculated. 2 The concentration was calculated. 2 The concentration was 11.0% by mass.
[0156] Then, 45 g of this titanium-containing precipitate was mixed with 5 g of tetramethylammonium hydroxide pentahydrate (TMAH concentration: 50% by mass) (0.443 mol per mol of Ti in the titanium-containing precipitate) and the mixture was shaken for 24 hours with a paint shaker to obtain an aqueous titanic acid solution.
[0157] Next, the molybdic acid dispersion was obtained, for example, by the steps described below.
[0158] 100 g of molybdenum trioxide was dissolved in 200 g of a 55 mass% aqueous sulfuric acid solution, and ion-exchanged water was added to convert molybdenum to MoO 3 An aqueous solution of molybdenum sulfate containing 100 g / L of molybdenum was obtained. 200 mL of this aqueous solution of molybdenum sulfate was added to ammonia water (NH 3 (NH 3 / MoO 3 Molar ratio = 105.66, NH 3 / SO 4 2-The reaction solution was a slurry of a molybdic acid compound hydrate, in other words, a slurry of a molybdenum-containing precipitate.
[0159] The reaction solution was then decanted using a centrifuge and washed until the electrical conductivity reached 500 μS / cm or less to obtain a molybdenum-containing precipitate from which the sulfur content had been removed. In this case, aqueous ammonia was used as the washing liquid.
[0160] Furthermore, the molybdenum-containing precipitate from which the sulfur content had been removed was diluted with pure water to obtain a molybdenum-containing precipitate slurry from which the sulfur content had been removed. A portion of the molybdenum-containing precipitate slurry from which the sulfur content had been removed was dried at 110°C for 24 hours and then calcined at 1,000°C for 4 hours to obtain MoO 3 The weight of the molybdenum-containing precipitation slurry from which the sulfur content has been removed is calculated based on the weight of the molybdenum-containing precipitation slurry. 3 The concentration was calculated.
[0161] The sulfur-removed molybdenum-containing precipitate slurry was diluted with pure water and the molybdenum concentration of the final mixture was MoO 3 Methylamine was mixed with pure water at 2% by mass so that the converted concentration was 10% by mass, and the mixture was stirred and held at room temperature (25° C.) for 1 hour to obtain an aqueous molybdic acid solution.
[0162] Furthermore, the tantalic acid dispersion liquid was obtained, for example, by the process described below.
[0163] 137.9g of tantalum hydroxide (Ta 2 O 5 A tantalum fluoride aqueous solution (Ta 2 O 5 A concentration of 9.1% by weight was obtained.
[0164] 100 g of this tantalum fluoride aqueous solution was added to 100 mL of 50 mass % dimethylamine over a period of less than 1 minute. After that, the mixture was stirred for 15 minutes to obtain a primary reaction liquid (pH 11). This primary reaction liquid was dissolved in ammonia water (NH 3 The solution was added to 460 mL of tantalum oxide (concentration: 25% by mass) over a period of less than one minute to obtain a second reaction solution (pH 12). This second reaction solution was a slurry of a tantalic acid compound hydrate, in other words, a slurry of a tantalum-containing precipitate.
[0165] Next, this secondary reaction liquid was decanted using a centrifuge and washed until the amount of free fluorine in the supernatant was 100 mg / L or less, to obtain a tantalum-containing precipitate from which fluorine had been removed. At this time, ammonia water was used as the washing liquid.
[0166] A part of this tantalum-containing precipitate was calcined at 1,000°C for 4 hours to obtain Ta 2 O 5 The mass of the tantalum-containing precipitate was calculated based on the Ta content. 2 O 5 The concentration was calculated. 2 O 5 The concentration was 38% by mass.
[0167] 29.2 mL of pure water and 9 g of 50 mass % dimethylamine were added to 11.8 g of this tantalum-containing precipitate, and the liquid temperature was kept at room temperature (25° C.) and stirred for 24 hours to obtain a tantalic acid dispersion.
[0168] The above-mentioned titanic acid dispersion, molybdic acid dispersion, and tantalic acid dispersion were each prepared by dispersing the titanic acid dispersion in a TiO 2 In terms of 1 mol, the molybdic acid dispersion is MoO 3 The tantalic acid dispersion is converted to 0.75 mol of Ta 2 O 5The mixed solution prepared so as to have a concentration of 0.05 mol was stirred at room temperature (25° C.) for 10 minutes, and then the mixed solution was placed in a static furnace and dried in the air at a drying temperature of 110° C. for 6 hours to remove moisture from the mixed solution. The dried powder obtained was then calcined at a calcination temperature of 600° C. for 3 hours to obtain the complex metal acid compound of Example 1. The crystal structure of the complex metal acid compound of Example 1 was anatase type, and the anatase ratio was 100%.
[0169] Example 2 The mixed composition of Example 2 was obtained in the same manner as in Example 1, except that it was prepared so as to contain 0.3 mass% of a composite metal acid compound, 33.3 mass% of a cationic styrene resin as a resin, and 66.3 mass% of industrial ethanol as a solvent.
[0170] Example 3 The mixed composition of Example 3 was obtained in the same manner as in Example 1, except that it was prepared so as to contain 0.2 mass% of a composite metal acid compound, 33.3 mass% of a cationic styrene resin as a resin, and 66.5 mass% of industrial ethanol as a solvent.
[0171] Example 4 The mixed composition of Example 4 was obtained in the same manner as in Example 1, except that it was prepared so that it contained 0.3 mass% of a composite metal acid compound and 33.3 mass% of an anionic styrene resin (manufactured by Arakawa Chemical Industries, Ltd., product name: WC-M-1208) as the resin.
[0172] Example 5 The mixed composition of Example 5 was obtained in the same manner as in Example 1, except that it was prepared so as to contain 0.2 mass% of a composite metal acid compound, 33.3 mass% of anionic styrene resin as a resin, and 66.5 mass% of industrial ethanol as a solvent.
[0173] Example 6 The mixed composition of Example 6 was prepared in the same manner as in Example 1, except that it contained 0.2 mass% of a composite metal acid compound, 30.8 mass% of anionic styrene resin as a resin, and 61.4 mass% of industrial ethanol as a solvent, and further contained 7.7 mass% of an aziridine-based crosslinking agent (product name: Chemitite PZ-33, manufactured by Nippon Shokubai Co., Ltd.) as a curing agent.
[0174] Example 7 The mixed composition of Example 7 was obtained in the same manner as in Example 1, except that it was prepared so as to contain 1.3 mass% of a composite metal acid compound, 33.3 mass% of a cationic styrene resin as a resin, and 65.3 mass% of industrial ethanol as a solvent.
[0175] Comparative Example 1 Comparative Example 1 was prepared in the same manner as Example 1, except that no resin was included, and the composite metal acid compound was prepared at 2.0 mass% and 98.0 mass% industrial ethanol was used as the solvent. The composite metal acid compound of Comparative Example 1 was obtained in the same manner as Example 1.
[0176] The complex metal acid compounds used in the above-mentioned Examples 1 to 7 and Comparative Example 1 are the same complex metal acid compounds as the complex metal acid compound according to Experimental Example 5 described later, but they may be replaced with complex metal acid compounds according to other Experimental Examples described later other than the complex metal acid compound according to Experimental Example 5. Note that the titanic acid dispersion liquid, molybdic acid dispersion liquid, and tantalic acid dispersion liquid used in Experimental Examples 1 to 18 were prepared in the same manner as in Examples 1 to 7, and therefore detailed explanations will be omitted.
[0177] (Experimental Example 1) The composite metal acid compound according to Experimental Example 1 was prepared by dispersing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and dispersing the titanic acid dispersion with TiO 2 In terms of 1 mol, the molybdic acid dispersion is MoO 3 The tantalic acid dispersion is converted to 0.05 mol of Ta 2 O 5The mixed solution was stirred at room temperature (25°C) for 10 minutes to obtain 0.05 mol equivalent, and then the mixed solution was placed in a static furnace and dried in the air at a drying temperature of 110°C for 6 hours to remove moisture from the mixed solution. The dried powder obtained was further calcined at a calcination temperature of 600°C for 3 hours to obtain the complex metal acid compound of Experimental Example 1. The crystal structure of the complex metal acid compound of Experimental Example 1 was anatase type, and the anatase ratio was 100%.
[0178] (Experimental Example 2) The composite metal acid compound according to Experimental Example 2 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then dissolving the molybdic acid dispersion in MoO 3 A complex metal acid compound according to Experimental Example 2 was obtained in the same manner as in Experimental Example 1, except that the amount was adjusted to 0.01 mol in terms of conversion. In addition, the crystal structure of the complex metal acid compound according to Experimental Example 2 was anatase type, and the anatase ratio was 100%.
[0179] (Experimental Example 3) The composite metal acid compound according to Experimental Example 3 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then dissolving the molybdic acid dispersion in MoO 3 A complex metal acid compound according to Experimental Example 3 was obtained in the same manner as in Experimental Example 1, except that the amount was adjusted to 0.25 mol in terms of conversion. In addition, the crystal structure of the complex metal acid compound according to Experimental Example 3 was anatase type, and the anatase ratio was 100%.
[0180] (Experimental Example 4) The composite metal acid compound of Experimental Example 4 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then dissolving the molybdic acid dispersion in MoO 3 A complex metal acid compound according to Experimental Example 4 was obtained in the same manner as in Experimental Example 1, except that the amount was adjusted to 0.5 mol in terms of conversion. In addition, the crystal structure of the complex metal acid compound according to Experimental Example 4 was anatase type, and the anatase ratio was 100%.
[0181] (Experimental Example 5) The composite metal acid compound of Experimental Example 5 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then dissolving the molybdic acid dispersion in MoO 3 A complex metal acid compound according to Experimental Example 5 was obtained in the same manner as in Experimental Example 1, except that the amount was adjusted to 0.75 mol in terms of conversion. The complex metal acid compound according to Experimental Example 5 had an anatase crystal structure, and the anatase ratio was 100%.
[0182] (Experimental Example 6) The composite metal acid compound of Experimental Example 6 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then dissolving the molybdic acid dispersion in MoO 3 A complex metal acid compound according to Experimental Example 6 was obtained in the same manner as in Experimental Example 1, except that the amount was adjusted to 1 mol in terms of conversion. The complex metal acid compound according to Experimental Example 6 had an anatase crystal structure, and the anatase ratio was 100%.
[0183] (Experimental Example 7) The composite metal acid compound of Experimental Example 7 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then dissolving the molybdic acid dispersion in MoO 3 A complex metal acid compound according to Experimental Example 7 was obtained in the same manner as in Experimental Example 1, except that the total amount was adjusted to 5 mol. The complex metal acid compound according to Experimental Example 7 had an anatase crystal structure, and the anatase ratio was 100%.
[0184] (Experimental Example 8) The composite metal acid compound of Experimental Example 8 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then dissolving the molybdic acid dispersion in MoO 3 A complex metal acid compound according to Experimental Example 8 was obtained in the same manner as in Experimental Example 1, except that the amount was adjusted to 10 mol in terms of conversion. The complex metal acid compound according to Experimental Example 8 had an anatase crystal structure, and the anatase ratio was 100%.
[0185] (Experimental Example 9) The composite metal acid compound of Example 9 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then dissolving the molybdic acid dispersion in MoO 3 A complex metal acid compound according to Experimental Example 9 was obtained in the same manner as in Experimental Example 1, except that the total amount was adjusted to 20 mol. The complex metal acid compound according to Experimental Example 9 had an anatase crystal structure, and the anatase ratio was 100%.
[0186] (Experimental Example 10) The composite metal acid compound of Example 10 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then mixing the tantalic acid dispersion with Ta 2 O 5 A complex metal acid compound according to Experimental Example 10 was obtained in the same manner as in Experimental Example 1, except that the amount was adjusted to 0.01 mol in terms of conversion. The complex metal acid compound according to Experimental Example 10 had an anatase crystal structure, and the anatase ratio was 100%.
[0187] (Experimental Example 11) The composite metal acid compound of Example 11 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then mixing the tantalic acid dispersion with Ta 2 O 5 A complex metal acid compound according to Experimental Example 11 was obtained in the same manner as in Experimental Example 1, except that the amount was adjusted to 0.1 mol in terms of conversion. The complex metal acid compound according to Experimental Example 11 had an anatase crystal structure, and the anatase ratio was 100%.
[0188] (Experimental Example 12) The composite metal acid compound of Example 12 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then mixing the tantalic acid dispersion with Ta 2 O 5 A complex metal acid compound according to Experimental Example 12 was obtained in the same manner as in Experimental Example 1, except that the amount was adjusted to 0.25 mol in terms of conversion. In addition, the crystal structure of the complex metal acid compound according to Experimental Example 12 was anatase type, and the anatase ratio was 100%.
[0189] (Experimental Example 13) The composite metal acid compound of Example 13 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then mixing the tantalic acid dispersion with Ta 2 O 5 A complex metal acid compound according to Experimental Example 13 was obtained in the same manner as in Experimental Example 1, except that the amount was adjusted to 0.5 mol in terms of conversion. In addition, the crystal structure of the complex metal acid compound according to Experimental Example 13 was anatase type, and the anatase ratio was 100%.
[0190] (Experimental Example 14) The composite metal acid compound of Example 14 was prepared by mixing a titanic acid dispersion, a molybdic acid dispersion, and a tantalic acid dispersion, and then dissolving the molybdic acid dispersion in MoO 3 The tantalic acid dispersion is converted to 0.1 mol of Ta 2 O 5 A complex metal acid compound according to Experimental Example 14 was obtained in the same manner as in Experimental Example 1, except that the amount was adjusted to 0.1 mol in terms of conversion. The complex metal acid compound according to Experimental Example 14 had an anatase crystal structure, and the anatase ratio was 100%.
[0191] (Experimental Example 15) Rutile-type titanium oxide powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.: titanium oxide (IV), rutile type, the above-mentioned molybdic acid dispersion liquid and tantalic acid dispersion liquid were added to the titanium oxide amount of TiO 2 In terms of 1 mol, the molybdic acid dispersion is MoO 3 The tantalic acid dispersion is converted to 0.05 mol of Ta 2 O 5 The mixture was prepared so that the total amount was 0.05 mol, and was stirred at room temperature (25°C) for 10 minutes. The mixture was then placed in a static furnace and dried in the air at a drying temperature of 110°C for 6 hours to remove the moisture from the mixture. The dried powder obtained was then calcined at a calcination temperature of 600°C for 3 hours to obtain a rutile-type complex metal acid compound.
[0192] Then, the anatase-type complex metal acid compound according to Experimental Example 1 and the rutile-type complex metal acid compound having the same composition were collected so that the weight ratio was 81:19, and mixed at room temperature to obtain a two-type mixed powder, thereby obtaining the complex metal acid compound according to Experimental Example 15. The crystal structure of the complex metal acid compound according to Experimental Example 15 was a mixture of the anatase type and the rutile type, and the anatase ratio was 81%.
[0193] (Experimental Example 16) The anatase-type complex metal acid compound according to Experimental Example 1 and the rutile-type complex metal acid compound obtained in the same manner as in Experimental Example 15 were collected so that the weight ratio was 54:46, and mixed at room temperature to form a two-kind mixed powder, thereby obtaining the complex metal acid compound according to Experimental Example 16. The crystal structure of the complex metal acid compound according to Experimental Example 16 was a mixture of the anatase type and the rutile type, and the anatase ratio was 54%.
[0194] (Experimental Example 17) The anatase-type complex metal acid compound according to Experimental Example 1 and the rutile-type complex metal acid compound obtained in the same manner as in Experimental Example 15 were collected so that the weight ratio was 15:85, and mixed at room temperature to form a two-kind mixed powder, thereby obtaining the complex metal acid compound according to Experimental Example 17. The crystal structure of the complex metal acid compound according to Experimental Example 17 was a mixture of the anatase type and the rutile type, and the anatase ratio was 15%.
[0195] (Experimental Example 18) The dried powder obtained in the same manner as in Experimental Example 1 was not subsequently fired at a firing temperature of 600° C. for 3 hours to obtain a composite metal acid compound according to Experimental Example 18. The crystal structure of the composite metal acid compound according to Experimental Example 18 was amorphous, and the anatase ratio was 0%.
[0196] The following physical properties were measured for the mixed products according to Examples 1 to 7, the composite metal acid compounds according to Experimental Examples 1 to 18, and the composite metal acid compound according to Comparative Example 1. The methods for measuring the physical property values are as follows.
[0197] <Elemental analysis> If necessary, the sample was appropriately diluted with dilute hydrochloric acid and TiO was analyzed by inductively coupled plasma emission spectrometry (Agilent Technologies: AG-5110). 2 In addition to the converted Ti weight fraction, MoO 3 Mo weight fraction, Ta 2 O 5 The converted Ta weight fraction was measured.
[0198] <Powder crystal structure (XRD)> For the composite metal acid compounds of Experimental Examples 1 to 18, if a sharp XRD peak was observed at 2θ=25°±1 in the X-ray diffraction pattern obtained by powder X-ray diffraction measurement using CuKα radiation, it was determined that the compound had an anatase-type crystal structure, and if a sharp XRD peak was observed at 2θ=27°±1 (excluding 2θ=26°), it was determined that the compound had a rutile-type crystal structure.
[0199] = Powder X-ray diffraction measurement conditions = Diffraction equipment: MiniFlex2 (Rigaku Corporation) ·X-ray tube: Cu Tube voltage / current: 30kV, 15mA ·Slit: DS-SS; 1.25 degree, RS; 0.3mm Monochromator graphite Measurement interval: 0.01 degree Counting method: Constant counting method X-ray analysis software: PDXL2 Version 2.9.1.0
[0200] Furthermore, the anatase ratio (%) of the composite metal acid compounds according to Experimental Examples 1 to 18 was calculated using the above formula (1). When an XRD peak indicating an anatase crystal structure was observed but an XRD peak indicating a rutile crystal structure was not observed, the anatase ratio was determined to be 100%.
[0201] <Particle size measurement> The average primary particle size of the composite metal acid compounds according to Experimental Examples 1 to 18 was measured by analyzing SEM images taken with a field emission scanning electron microscope (FE-SEM) (S-4800 manufactured by Hitachi High-Tech Sciences Corporation).
[0202] Specifically, the average primary particle diameter of 100 particles randomly selected from the SEM images of the composite metal acid compounds according to Experimental Examples 1 to 18 was determined by measuring the long axis Ll and the short axis Ls of the primary particles for each of the 100 primary particles randomly selected for each of Experimental Examples 1 to 18 in accordance with "JIS H 7804:2005 Method for Measuring Particle Diameter of Metal Catalysts by Electron Microscope," calculating the calculated particle diameter d from the above formula "d=(Ll+Ls) / 2," and the arithmetic average value of these was used as the average primary particle diameter of the composite metal acid compounds according to Experimental Examples 1 to 18. If the average primary particle diameter was 100 nm or less, it was evaluated as "○○ (Very Good)," if the average primary particle diameter was more than 100 nm and less than 50 μm, it was evaluated as "○ (Good)," and if the average primary particle diameter was more than 50 μm, it was evaluated as "× (Bad)."
[0203] <Photocatalytic performance evaluation test (under visible light)> A sample solution was prepared by adding 10 g of methylene blue trihydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 300 mg of the complex metal acid compound according to Experimental Examples 1 to 18 to 100 g of pure water, and while stirring with a stirrer, a U4-100CL (manufactured by Nexfilm Co., Ltd.) was attached to the irradiation port of a Solar Simulator (manufactured by Minaga Electric Works, Ltd.) and irradiated with a Xe light (illuminance 87,600 lux) that cuts off ultraviolet rays of 400 nm or less for 60 minutes. Then, the absorbance reduction rate (%) before and after light irradiation at the methylene blue absorption peak of 665 nm was calculated by the following formula (2). If the calculated absorbance reduction rate (%) was 30% or more, it was evaluated as "○○ (Very Good)", if the absorbance reduction rate (%) was 10% or more and less than 30%, it was evaluated as "○ (Good)", and if the absorbance reduction rate (%) was less than 10%, it was evaluated as "× (Bad)".
[0204]
number
[0205] <Photocatalytic performance evaluation test (in the dark)> The sample solutions made from the complex metal acid compounds according to Experimental Examples 1 to 18 were prepared in the same manner as in the photocatalytic performance evaluation test (under visible light), and after stirring in a dark room for 60 minutes, the absorbance reduction rate (%) at the methylene blue absorption peak of 665 nm was evaluated before and after stirring. If the absorbance reduction rate (%) was 10% or more, it was evaluated as "○○ (Very Good)", if the absorbance reduction rate (%) was 5% or more and less than 10%, it was evaluated as "○ (Good)", and if the absorbance reduction rate (%) was less than 5%, it was evaluated as "× (Bad)".
[0206] <L * measurement> The composite metal acid compounds according to Experimental Examples 1 to 18 were applied onto a PET film using a bar coater, and the coating film samples thus formed were measured using a colorimeter (Konica Minolta: CR-300) according to CIE1976(L) in accordance with JIS Z 8722:2009. * a * b * ) color space L * The value was also calculated. * If the value is 80 or more, it will be marked as "XX (Very Good)" and * If the value was 70 or more and less than 80, it was evaluated as "○ (Good)".
[0207] <Stability test over time> The mixed products according to Examples 1 to 7 and the complex metal acid compound according to Comparative Example 1 were left to stand at room temperature of 25°C for 30 days, and then visually observed for the presence or absence of white precipitation or gelation. Products in which no white precipitation or gelation was observed were evaluated as having temporal stability and were rated as "Good", whereas products in which even one white precipitation or gelation was observed were evaluated as not having temporal stability and were rated as "Bad". Here, gelation was judged to have occurred when the mixed products according to Examples 1 to 7 and the complex metal acid compound according to Comparative Example 1 were placed in a plastic container, and the container was turned upside down, and if the container did not fall quickly, it was judged to have gelled.
[0208] <Transmittance measurement> The mixed products according to Examples 1 to 7 were applied onto a PET film ("Lumirror (registered trademark)": #100-T60, manufactured by Toray Industries, Inc.) using a bar coater, and the transmittance of the mixed product films (film thickness: 20 μm) (samples) according to Examples 1 to 7 thus produced was measured with a spectrophotometer under the transmittance measurement conditions described below. In addition, the composite metal acid compound according to Comparative Example 1 was applied onto the PET film using a bar coater, but a film could not be formed, and the transmittance could not be measured, so Comparative Example 1 was deemed ineligible for evaluation.
[0209] =Transmittance measurement conditions= Measurement equipment: UV-Vis-NIR spectrophotometer UH4150 (manufactured by Hitachi High-Tech Science Corporation) Measurement mode: Wavelength scan Data mode: %T (transparent) Measurement wavelength range: 210~1000nm Scan speed: 600nm / min Sampling interval: 2nm
[0210] The transmittance at a wavelength of 350 nm was measured based on the transmittance measurement conditions.
[0211] <Tape peeling test> The mixed products according to Examples 1 to 7 were filtered through a filter with a pore size of 2 μm, and dropped onto a 50 mm×50 mm glass substrate that had been degreased and washed with acetone and then dried, using a syringe, and applied by spin coating (1,500 rpm, 15 seconds). The applied portion was then naturally dried to form a coating film (sample) on the glass substrate. Then, cellophane adhesive tape as specified in JIS Z 1522:2009 was attached to the coating film surface formed on the glass substrate. The cellophane adhesive tape was squeezed from above with a finger, and then quickly peeled off in a direction perpendicular to the coating film surface, and the presence or absence of peeling of the coating film on the glass substrate was observed. Those in which no peeling of the coating film was observed were evaluated as having excellent adhesion and were evaluated as “◯ (GOOD)”, and those in which peeling of the coating film was observed were evaluated as not having excellent adhesion and were evaluated as “× (BAD)”. The samples used in the tape peeling test were those that had been applied for one day. Moreover, when the composite metal acid compound of Comparative Example 1 was applied onto the glass substrate, the coating film formed was easily peeled off.
[0212] <Antiviral Test> The mixed products according to Examples 1 to 7 were subjected to an antiviral test in accordance with ISO21702. The mixed products according to Examples 1 to 7 were applied onto a substrate (PET film), and 150 μl of the test virus liquid was dropped onto the test piece on which the coating film was formed, covered with an adhesive film, and left in a dark place at 25°C ± 3°C in a moist environment as specified. In order to evaluate the presence or absence of antiviral properties of each test piece, an untreated test piece without a coating film was prepared. After being left to stand for a predetermined time, the test virus liquid was collected with 5 ml of PBS. The test virus was generated by diluting a preserved virus liquid containing bacteriophage QB as the main component with phosphate buffer solution (PBS) to an appropriate concentration (10 times or more).
[0213] The virus infectivity was measured from the collected test virus solution using the plaque method. Specifically, the host cells were cultured in a monolayer on a 6-well plate, and 0.1 mL of serially diluted test virus solution was inoculated into each well. The incubation temperature was 37°C, 5% CO 2After culturing for 1 hour under the above conditions to allow the virus to adsorb to the cells, the agar medium was poured into a 6-well plate and cultured for an additional 2 to 3 days. After culturing, the cells were fixed and stained, and the number of plaques formed was counted to calculate the virus infectivity.
[0214] The antiviral activity value (V) was calculated from the calculated virus infectivity value according to the following formula (3): B in the following formula (3) represents the virus infectivity value of the test piece, and C represents the virus infectivity value of the untreated test piece.
[0215]
number
[0216] If V was 2 or more, it was deemed to have antiviral properties and was evaluated as "○ (Good)", and if V was less than 2, it was deemed to have no antiviral properties and was evaluated as "× (Bad)". Furthermore, the composite metal acid compound according to Comparative Example 1 was applied onto the glass substrate, and the coating film formed peeled off, making it impossible to measure the virus activity value (V), and therefore Comparative Example 1 was deemed ineligible for evaluation.
[0217] <Antibacterial Test> The mixed products according to Examples 1 to 7 were subjected to antibacterial tests in accordance with JIS Z 2801. The mixed products according to Examples 1 to 7 were applied onto a substrate (PET film), and 150 μl of test bacteria liquid was dropped onto the test piece on which the coating film was formed, covered with an adhesive film, and left in a dark place at 25°C ± 3°C in a moist environment as specified. In order to evaluate the presence or absence of antibacterial properties of each test piece, a non-treated test piece without a coating film was prepared. After leaving the test piece for a predetermined time, a bacteria washout solution was added to each test piece, the bacteria were dispersed by shaking, and the number of live bacteria in the washout solution was measured by a pour plate culture method. The test bacteria were prepared by diluting a stock bacteria solution mainly composed of gram-negative bacteria (e.g., Escherichia coli) with phosphate buffer solution (PBS) to an appropriate concentration (10 times or more).
[0218] The antibacterial activity value (R) was calculated from the viable cell count recovered after inoculating each test piece with the test bacteria for 24 hours and the viable cell count recovered after inoculating an untreated test piece with the test bacteria for 24 hours, according to the following formula (4). In the following formula (4), T represents the viable cell count of the test piece, and U represents the viable cell count of the untreated test piece.
[0219]
number
[0220] If R was 2 or more, it was deemed to have antibacterial properties and was evaluated as "○ (Good)", and if R was less than 2, it was deemed to have no antibacterial properties and was evaluated as "× (Bad)". Furthermore, the composite metal acid compound according to Comparative Example 1 was applied onto the glass substrate, and the coating film formed peeled off, making it impossible to measure the antibacterial activity value (R), and therefore Comparative Example 1 was deemed ineligible for evaluation.
[0221] The physical property values of Examples 1 to 7 and Comparative Example 1 measured by the above-mentioned measuring methods are shown in Fig. 1, and the measurement results are shown in Table 1. The physical property values and measurement results of Examples 1 to 18 are shown in Fig. 2.
[0222] The content of the dispersant in FIG. 1 is a value in which the dispersant is 5 mass % relative to the weight of the complex metal acid compound in the mixed compositions of Examples 1 to 7 and the complex metal acid compound of Comparative Example 1.
[0223] [Table 1]
[0224] The mixed compositions according to Examples 1 to 7 contained a composite metal acid compound containing titanium as a main component and a resin, and therefore had excellent photocatalytic performance and excellent film-forming properties on a substrate.
[0225] In the mixed compositions according to Examples 1 to 7, the composite metal oxide compound contained in the mixed composition further contains molybdenum and tantalum, and the titanium content is TiO 2When expressed as 1 (mol) in converted value, the molybdenum content is expressed as the molar ratio MoO 3 Conversion value / TiO 2 The conversion value is 0.01-20, and the tantalum content is the molar ratio Ta 2 O 5 Conversion value / TiO 2 When the conversion value was 0.01 to 0.5, the photocatalytic performance was excellent and the film-forming property on the substrate was also excellent.
[0226] The mixed compositions according to Examples 1 to 7 were excellent in transparency when the resin contained in the mixed composition was a styrene-based resin.
[0227] Moreover, the mixed compositions according to Examples 1 to 7 did not gel even after being left to stand at room temperature of 25° C. for 30 days, and were therefore excellent in stability over time.
[0228] In addition, when the mixed compositions of Examples 1 to 7 were applied to the coating surface formed on a glass substrate with a cellophane adhesive tape and the cellophane adhesive tape was peeled off, no peeling of the coating on the glass substrate was observed, and the mixed compositions had excellent adhesion to the substrate.
[0229] Moreover, the mixed compositions according to Examples 1 to 7 were excellent in antiviral and antibacterial properties.
[0230] The inventions disclosed in this specification include, in addition to the configurations of each invention or embodiment, those that are specified by changing these partial configurations to other configurations disclosed in this specification, to the extent applicable, or those that are specified by adding other configurations disclosed in this specification to these configurations, or those that are specified as higher-level concepts by deleting these partial configurations to the extent that partial action and effects are obtained. [Industrial Applicability]
[0231] The mixed composition according to the present invention has excellent photocatalytic performance and excellent film-forming properties on a substrate, and is therefore suitable for use as a photocatalyst in building materials and coating materials. In addition, since the mixed composition according to the present invention has excellent photocatalytic performance, it can exhibit equivalent photocatalytic performance even in a smaller amount than before. This makes it possible to reduce the amount of the product itself and the associated waste, and to reduce energy costs in manufacturing and disposal. In this way, it leads to the achievement of sustainable management and efficient benefits of natural resources, as well as decarbonization (carbon neutrality). Furthermore, since the mixed composition according to the present invention has antiviral and antibacterial properties, it can reduce the risk of infectious diseases and ensure the healthy lives of all people of all ages and promote welfare.
Claims
1. A mixed composition comprising a composite metal acid compound containing titanium as a main component and a resin.
2. The complex metal acid compound further contains molybdenum and tantalum, When the titanium content is expressed as 1 (mol) in terms of TiO2, The molybdenum content is expressed by the molar ratio MoO 3 Conversion value / TiO 2 The converted value is 0.01-20, and the tantalum content is the molar ratio Ta 2 O 5 Conversion value / TiO 2 The mixture composition according to claim 1, characterized in that the converted value is 0.01 to 0.
5.
3. The mixture composition according to claim 1, further comprising a solvent.
4. The mixture composition of claim 1 further comprising a curing agent.
5. 2. The mixed composition according to claim 1, wherein the resin is a styrene-based resin.
6. 6. The mixed composition according to claim 5, wherein the styrene-based resin comprises a cationic or anionic styrene resin.
7. 5. The mixed composition according to claim 4, wherein the curing agent is a compound having an aziridine ring.
8. 8. The mixed composition according to claim 1, wherein the complex metal acid compound has an amorphous or / and anatase type crystal structure.
9. The complex metal acid compound is L * a * b * L in color system * 8. The mixed composition according to claim 1, wherein the value is 80 or more.
10. 8. The mixed composition according to claim 1, wherein the composite metal acid compound has an average primary particle size of 0.1 nm or more and 50 μm or less as determined by observation with an electron microscope.
11. The composite metal acid compound has a molar ratio of MoO 3 Conversion value / TiO 2 The mixed composition according to any one of claims 1 to 7, characterized in that the converted value is 0.01 to 5.
12. The complex metal acid compound has a molar ratio of Ta 2 O 5 Conversion value / TiO 2 The mixed composition according to any one of claims 1 to 7, characterized in that the converted value is 0.1 to 0.
5.
13. The composite metal acid compound has a molar ratio of MoO 3 Conversion value / TiO 2 The converted value is represented as X, and the molar ratio Ta 2 O 5 Conversion value / TiO 2 When the converted value is expressed as Y, 0.05≦X / Y≦400 The mixed composition according to any one of claims 1 to 7, characterized in that it satisfies the above.
14. The composite metal acid compound is such that X / Y is 0.05≦X / Y≦100 The mixture composition according to claim 13, characterized in that it satisfies the above.
15. A mixed composition film comprising the mixed composition according to any one of claims 1 to 7.
Citation Information
Patent Citations
Photocatalyst and method of producing the same
JP2001170496A