Cosmetic product
Porous cellulose particles in cosmetics address the issues of makeup fading and shine by enhancing oil and water absorption, maintaining skin smoothness and brightness, and reducing color unevenness, offering a natural alternative to petroleum-derived plastics.
Patent Information
- Application Number
- JP2023073546
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional cosmetics using spherical resin particles for matte and slip effects face issues with makeup fading and shine due to sebum adsorption, and lack effective moisturizing properties, while there is a growing demand for natural alternatives to petroleum-derived plastic particles.
Incorporation of porous cellulose particles with specific fine porous structures into cosmetics, characterized by a mode diameter of 1.0 μm to 300.0 μm, surface openings communicating with internal voids, and a pore area ratio of 5% to 95% as observed under a scanning electron microscope, which suppresses sebum-induced shine and enhances moisturizing power.
The use of porous cellulose particles in cosmetics effectively reduces makeup deterioration and shine, maintains a smooth skin feel, and improves moisturization by absorbing both oil and water, while minimizing color unevenness and maintaining lightness and saturation.
Smart Images

Figure 2024158389000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a cosmetic product containing porous cellulose particles. [Background technology]
[0002] Conventionally, spherical resin particles have been used in various fields such as matting agents, slip agents, and antiblocking agents due to their characteristics, and various spherical resin particles are also used in cosmetics. On the other hand, due to the recent problems of marine pollution caused by microplastics, the raw materials of the spherical resin particles incorporated in cosmetics are shifting from synthetic materials derived from petroleum to natural materials.
[0003] In light of this, interest in natural and organic cosmetics has been growing in recent years, and natural raw materials that can replace petroleum-derived plastic particles are in demand. Cellulose is known as such a natural raw material, and for example, cosmetics containing spherical resin beads whose main component is a cellulose derivative are known (Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6762407 Summary of the Invention [Problem to be solved by the invention]
[0005] However, it is not known that cosmetics containing porous cellulose particles have excellent moisturizing properties and suppress makeup breakdown and shine caused by sebum adsorption. The present invention aims to provide a cosmetic product that uses porous cellulose particles that can be used as an alternative to petroleum-derived plastic particles, and that can suppress makeup breakdown and shine caused by sebum adsorption. Another objective of the present invention is to provide a cosmetic product that uses porous cellulose particles and has excellent moisturizing power. [Means for solving the problem]
[0006] The present inventors have found that when cellulose particles having a specific fine porous structure are blended into cosmetics, it is possible to suppress makeup breakdown and shine caused by sebum adsorption, and obtain excellent moisturizing power.Furthermore, the present inventors have found that when the cellulose particles have a specific bulk density, the skin feels light when applied, the skin feels smooth even after sebum adsorption, and the uneven color caused by application to the skin is suppressed.
[0007] That is, the present invention is as follows. [1] A cosmetic comprising approximately spherical porous cellulose particles, The mode diameter of the porous cellulose particles is from 1.0 μm to 300.0 μm; the porous cellulose particles have openings on the particle surface, the openings communicating with voids inside the particles; A cosmetic product, characterized in that the ratio of the total projected area of the open pores to the projected area of the porous cellulose particles, as observed with a scanning electron microscope, is 5% to 95%. [2] The cosmetic product described in [1], wherein the average diameter of the openings is from 0.01 μm to 10.0 μm. [3] The cosmetic product described in [1] or [2], wherein the bulk density of the porous cellulose particles is 0.10 g / ml to 0.90 g / ml. [4] The surface area per projected area of the porous cellulose particles as observed by a scanning electron microscope. The number of the openings is 3 / μm. 2 From 80 pieces / μm 2 The cosmetic product according to any one of [1] to [3], [5] The cosmetic product according to any one of [1] to [4], which is a foundation, lipstick, eye shadow, eyeliner, lotion, serum, lotion, milky lotion, base makeup, massage cream, makeup cream, skin cream, skin care cosmetics, moisturizing cosmetics, whitening cosmetics, medicated cosmetics, sunscreen cosmetics, facial cleansing cream, or cleansing agent. [6] The cosmetic product according to any one of [1] to [5], wherein the porous cellulose particles are produced by a method including the steps of: (a) heating and dissolving cellulose acetate in a mixed solvent of a solvent in which cellulose acetate is soluble and a solvent in which cellulose acetate is insoluble to prepare a cellulose acetate solution; (b) dispersing the cellulose acetate solution in water containing an emulsion stabilizer to obtain a dispersion; and (c) cooling the dispersion to precipitate cellulose acetate particles, wherein the mixed solvent is an organic solvent that is not miscible with water. [7] The cosmetic product according to [6], wherein in step (a), the solvent in which the cellulose acetate is soluble is benzyl alcohol, ethyl acetate, cyclohexanone, or isophorone. [8] The cosmetic product according to [6] or [7], wherein in step (a), the solvent in which the cellulose acetate is insoluble is an alcohol, a glycol, an ether, or an ester. [9] The cosmetic product according to any one of [6] to [8], wherein in step (a), the volume ratio of the solvent in which cellulose acetate is soluble to the solvent in which cellulose acetate is insoluble in the mixed solvent is from 5:95 to 95:5.
[10] The cosmetic product according to any one of [6] to [9], wherein in step (a), the ratio of cellulose acetate in the mixed solvent is 0.1% by mass to 50% by mass.
[11] The cosmetic product according to any one of [6] to
[10] , wherein in step (a), the mixed solvent contains a third component which is a polymer, and the third component is polyethylene glycol or polypropylene glycol.
[12] The cosmetic product according to any one of [6] to
[10] , wherein in step (b), the emulsion stabilizer is sodium dodecylbenzenesulfonate, polyvinyl alcohol, carboxymethyl cellulose, hydroxyethyl cellulose, or a mixture thereof. Effect of the Invention
[0008] The present invention exhibits the effect that, by incorporating cellulose particles having a specific fine porous structure into cosmetics, makeup breakdown and shine caused by sebum adsorption can be suppressed, and excellent moisturizing power can be obtained.Furthermore, by making the cosmetics containing the cellulose particles have a specific bulk density, the cosmetics have the effect that they are light to apply on the skin, can maintain a smooth feeling even after sebum adsorption, and can suppress the occurrence of uneven coloring. [Brief description of the drawings]
[0009] [Figure 1] 1 shows SEM photographs of the appearance of the particles of Example 1. Photographs of multiple particles, a single particle, an enlarged view of a single particle, and a particle cross section are shown, respectively. [Diagram 2] 2 is a photograph of the appearance of the particles of Example 2 observed by SEM. A photograph of a single particle is shown. [Diagram 3] 3 is a photograph of the appearance of the particles of Example 3 observed by SEM. A photograph of a single particle is shown. [Figure 4] 4 is a photograph of the appearance of the particles of Example 4 observed by SEM. A photograph of a single particle is shown. [Diagram 5] 5 is a photograph of the appearance of the particles of Example 5 observed by SEM. A photograph of a single particle is shown. [Figure 6] 6 is a photograph of the appearance of the particles of Comparative Example 1 observed by SEM. Photographs of multiple particles, a single particle, an enlarged view of a single particle, and a particle cross section are shown, respectively. [Figure 7] 7 is a photograph of the appearance of the particles of Comparative Example 2 observed by SEM. Photographs of multiple particles, a single particle, an enlarged view of a single particle, and a particle cross section are shown, respectively. [Figure 8] 8 is a set of SEM photographs of the appearance of the particles of Comparative Example 3. Photographs of multiple particles, a single particle, an enlarged view of a single particle, and a particle cross section are shown, respectively. [Figure 9] 9 is a photograph of the appearance of the particles of Comparative Example 4 observed by SEM. Photographs of multiple particles, a single particle, an enlarged view of a single particle, and a particle cross section are shown, respectively. [Figure 10]10 is a photograph of the appearance of the particles of Comparative Example 5 observed by SEM. Photographs of multiple particles, a single particle, an enlarged view of a single particle, and a particle cross section are shown, respectively. [Figure 11] FIG. 11 is a graph showing L* (lightness) when a dry sample is applied onto an evaluation substrate. [Figure 12] FIG. 12 is a graph showing L* (lightness) when an oil-impregnated sample is applied onto an evaluation substrate. [Figure 13] FIG. 13 is a graph showing the ratio of L* (brightness) when the oil-impregnated sample is applied to the L* (brightness) when the dry sample is applied on the evaluation substrate. [Figure 14] FIG. 14 is a graph showing C* (chroma) when a dry sample is applied onto an evaluation substrate. [Figure 15] FIG. 15 is a graph showing C* (chroma) when an oil-impregnated sample is applied onto an evaluation substrate. [Figure 16] FIG. 16 is a graph showing the ratio of C* (chroma) when the oil-impregnated sample is applied to C* (chroma) when the dry sample is applied on the evaluation substrate. [Figure 17] FIG. 17 is a graph showing the glossiness when a dry sample is applied onto an evaluation substrate. [Figure 18] FIG. 18 is a graph showing the glossiness when an oil-impregnated sample is applied onto an evaluation substrate. [Figure 19] FIG. 19 is a graph showing the ratio of glossiness when the oil-impregnated sample is applied to that when the dry sample is applied on the evaluation substrate. [Figure 20] FIG. 20 is a graph showing the drying speed when a dry sample is applied onto an evaluation substrate. [Figure 21] FIG. 21 is a graph showing the drying speed when an oil-impregnated sample is applied onto an evaluation substrate. [Figure 22] FIG. 22 is a graph showing the bulk density of the dry samples. [Diagram 23] FIG. 23 is a graph showing the bulk density of oil-impregnated samples. [Figure 24] FIG. 24 is a graph showing the standard deviation of L* (lightness) when the dry sample is applied to a double-sided tape. [Diagram 25] FIG. 25 is a graph showing the standard deviation of C* (chroma) when the dry sample is applied to a double-sided tape. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The cosmetic of the present invention is a cosmetic comprising approximately spherical porous cellulose particles, characterized in that the mode diameter of the porous cellulose particles is 1.0 μm to 300.0 μm, the porous cellulose particles have openings on the particle surface, the openings are connected to voids inside the particles, and the ratio of the total projected area of the openings to the projected area of the porous cellulose particles, as observed with a scanning electron microscope, is 5% to 95%.
[0011] The cosmetic product of the present invention contains roughly spherical porous cellulose particles. The roughly spherical shape refers to a shape like a sphere or an oval sphere, and in a photograph of the appearance of the roughly spherical body, the major axis (longest diameter) is preferably 3 times or less than the minor axis (shortest diameter), more preferably 2 times or less, and even more preferably 1.5 times or less. The porous cellulose particles are preferably close to a true sphere. The closer the shape is to a true sphere, the higher the slipperiness is, so the particles exhibit excellent extensibility suitable for cosmetics, and the application feeling when applied to the skin becomes light. In addition, the excellent extensibility makes it easier to apply the cosmetics evenly to the skin, and the occurrence of uneven coloring is also easily suppressed.
[0012] The mode diameter of the porous cellulose particles used in the present invention is 1.0 μm to 300.0 μm, preferably 1.0 μm to 200.0 μm, more preferably 1.0 μm to 100.0 μm, more preferably 1.0 μm to 50.0 μm, even more preferably 2.0 μm to 24.0 μm, even more preferably 4.0 μm to 16.0 μm, and most preferably 8.0 μm to 12.0 μm. The mode diameter of the porous cellulose particles can be selected according to the application of the cosmetic of the present invention. For example, the mode diameter of the porous cellulose particles is preferably 5.0 μm to 10.0 μm when the cosmetic of the present invention is a foundation, preferably 30.0 μm to 50.0 μm when it is a foundation or emulsion, preferably 80.0 μm to 120.0 μm when it is a massage cream, and preferably 180.0 μm to 220.0 μm when it is a face wash cream. The mode diameter referred to here was calculated by measuring the mode diameter using a particle size distribution measuring device: Laser Scattering Particle Size distribution Analyzer Partica LA-950 manufactured by HORIBA.
[0013] The porous cellulose particles used in the present invention have openings on the particle surface, and the openings communicate with the voids inside the particles. That is, the porous cellulose particles have a pore structure consisting of a three-dimensional network skeleton and its voids, and have a fine porous structure in which the pores communicate from the particle surface to the inside. This structure can be confirmed, for example, by observing the surface and cross section of the porous cellulose particles using a scanning electron microscope. The openings of the porous cellulose particles are open without being blocked on the particle surface. The porous cellulose particles have such a fine porous structure as described above, which improves oil absorption, thereby suppressing shine caused by sebum adsorption. In addition, it is possible to suppress the decrease in L* (lightness) and C* (chroma) caused by sebum adsorption, and to suppress makeup breakdown caused by sebum adsorption. Furthermore, since the particles are excellent not only in oil absorption but also in water absorption, they can suppress evaporation of water from the skin both before and after sebum adsorption, and can exhibit excellent moisturizing power. In addition, light is easily scattered near the surface of the porous cellulose particles, increasing L* (lightness) and C* (chroma), improving the covering power to hide wrinkles, dullness, pores, etc. Furthermore, the bulk density tends to be low, which improves spreadability when applied to the skin and makes it easier to suppress uneven coloring.
[0014] The phrase "the openings communicate with the voids inside the particle" includes not only a state in which the pores pass from the openings on the particle surface through the inside of the particle to a surface other than the particle surface (i.e., a state in which both ends of the pores communicate with the particle surface), but also a state in which the pores communicate from the particle surface to the inside but do not communicate from the inside to a surface other than the particle surface (i.e., a state in which only one end of the pores communicates with the particle surface). In addition, the pores communicating from the openings on the particle surface to the inside may be continuous with one or more other pores to form voids inside the particle.
[0015] The ratio of the total projected area of the openings to the projected area of the porous cellulose particles observed under a scanning electron microscope is 5% to 95%, preferably 10% to 80%, more preferably 15% to 60%, even more preferably 20% to 50%, and most preferably 32% to 38%. Within the above range, the oil absorption is improved, so that shine caused by sebum adsorption can be suppressed. In addition, the decrease in L* (lightness) and C* (chroma) caused by sebum adsorption can be suppressed, and makeup breakdown caused by sebum adsorption can be suppressed. Furthermore, since it is excellent not only in oil absorption but also in water absorption, it suppresses the evaporation of water from the skin both before and after sebum adsorption, and exhibits excellent moisturizing power. Furthermore, within the above range, light is easily scattered near the surface of the porous cellulose particles, so L* (lightness) and C* (chroma) are increased, and the covering power to hide wrinkles, dullness, pores, etc. is improved. Furthermore, since the bulk density is easily reduced, it spreads well when applied and color unevenness is easily suppressed.
[0016] The ratio of the total projected area of the openings to the projected area of the porous cellulose particles is, for example, as follows: It can be obtained by the following method. First, a scanning electron microscope is used to photograph the porous cellulose particles so that the particle diameter is 0.5 times or more the long side of the photograph (the horizontal side of the photograph). The short side of the photograph (the vertical side of the photograph) is taken as the Y axis, and the long side is taken as the X axis. The average of the diameters of the porous cellulose particles in the Y axis direction and the X axis direction is calculated, and this is taken as the representative diameter [Dp] (μm).
[0017] Next, the center of the particle is surrounded by a square whose side length is two-thirds of the representative diameter [Dp], and the area outside the surrounded area is removed, resulting in a photograph that shows only the inside of the surrounded area. The position of the square is the point where the center of the porous cellulose particle shown in the photograph overlaps with the center of the square. The area [Ap] of the area surrounded by the square is calculated using the formula Ap (μm 2 )=(Dp×2÷3) 2 Ask for more.
[0018] Next, the processed image is processed by Sakai Chemical Industry Co., Ltd.'s AI image analysis service DeepCle to obtain the total number of apertures and the average aperture area. In addition, the total projection area [Sp] of the apertures is calculated using the formula Sp(μm 2 ) = Total number of openings (pieces) × Average opening area (μm 2 ) more. Then, the ratio of the total projected area of the open pores to the projected area of the porous cellulose particles is calculated by the formula: Open pore area ratio (%)=Sp÷Ap×100.
[0019] The average diameter of the pores of the porous cellulose particles of the present invention is preferably 0.01 μm to 10.0 μm, more preferably 0.04 μm to 0.50 μm, even more preferably 0.06 μm to 0.30 μm, and most preferably 0.12 μm to 0.18 μm. Within the above range, sebum moves to the pores of the particles by capillary action, improving the oil absorption of the porous cellulose particles, and therefore the shine caused by sebum adsorption can be further suppressed. In addition, the decrease in L* (lightness) and C* (chroma) caused by sebum adsorption can be further suppressed, making it easier to suppress makeup from breaking down due to sebum adsorption. Furthermore, since the water absorption is also improved, it becomes easier to suppress the evaporation of water from the skin both before and after sebum adsorption, and the moisturizing power can be improved.
[0020] The average diameter of the openings of the porous cellulose particles can be determined, for example, by the following method. The image processed in the calculation of the "ratio of the total projected area of the openings to the projected area of the porous cellulose particles" described above is processed by DeepCle, an AI image analysis service provided by Sakai Chemical Industry Co., Ltd., to determine the average maximum width and average diagonal width of the openings. The diagonal width is the distance from edge to edge of the openings on a straight line perpendicular to the center of the maximum width line segment. Then, the average diameter [Dav] of the openings is calculated from the formula Dav (μm)=(average maximum width of the openings (μm)+average diagonal width of the openings (μm))÷2.
[0021] The average diameter of the openings of the porous cellulose particles is preferably 0.5 times or less, more preferably 0.1 times or less, the mode diameter of the porous cellulose particles. When the average diameter of the openings and the mode diameter of the porous cellulose particles satisfy the above relationship, the openings do not become too large relative to the porous cellulose particles, and the porous cellulose particles tend to maintain a substantially spherical shape.
[0022] The bulk density of the porous cellulose particles is preferably 0.10 g / ml to 0.90 g / ml, more preferably 0.20 g / ml to 0.80 g / ml, and even more preferably 0.30 g / ml to 0.70 g / ml. Within the above range, a lighter feel can be obtained when incorporated into cosmetics, spreadability when applied to the skin can be improved, and color unevenness can be suppressed.
[0023] The bulk density of the cosmetic product of the present invention is preferably 0.20 g / ml to 0.90 g / ml, more preferably 0.30 g / ml to 0.80 g / ml, and even more preferably 0.40 g / ml to 0.70 g / ml. If the bulk density is within the above range, a lighter feel can be obtained, spreadability when applied to the skin can be improved, and color unevenness can be suppressed. The bulk density of the cosmetic product of the present invention can be adjusted by adjusting the bulk density of the porous cellulose particles or the content of the porous cellulose particles in the cosmetic product.
[0024] The bulk density of the cosmetic product and the porous cellulose particles of the present invention can be determined, for example, by the following method. The cosmetic product or porous cellulose particles of the present invention are filled into a graduated test tube, and the graduated test tube is manually tapped 300 times from a height of 3 cm on a rubber sheet on a table to confirm the volume, and then tapped a further 200 times to confirm that there is no decrease in volume.The filled volume is then read and the bulk specific gravity is calculated by dividing the weight (g) of the sample by the filled volume (ml) after tapping.
[0025] The number of openings per projected area of the porous cellulose particles observed under a scanning electron microscope is 3 / μm. 2 From 80 pieces / μm2 It is preferable that the number of particles is 5 / μm. 2 From 70 pieces / μm 2 More preferably, it is 7 particles / μm 2 From 60 pieces / μm 2 More preferably, the number of particles is 12 / μm. 2 From 20 pieces / μm 2 It is more preferable that the above range is satisfied. Since a large number of openings are present on the surface of the porous cellulose particles, the oil absorption is improved, and the shine caused by sebum adsorption can be further suppressed. In addition, the decrease in L* (lightness) and C* (chroma) caused by sebum adsorption can be further suppressed, and makeup breakdown caused by sebum adsorption can be easily suppressed. Furthermore, since not only the oil absorption but also the water absorption is improved, the evaporation of water from the skin can be suppressed both before and after sebum adsorption, and the moisturizing power can be improved.
[0026] The number of openings per projected area of a porous cellulose particle can be calculated, for example, by the formula: number of openings per projected area of a porous cellulose particle (holes / μm) based on the total number of openings and the value of Ap, which are measured and calculated in the calculation of the above-mentioned "ratio of the total projected area of openings to the projected area of a porous cellulose particle". 2 ) = Total number of openings (pieces) ÷ Ap (μm 2 ) can be obtained.
[0027] The main component of the porous cellulose particles is cellulose or cellulose acetate. The main component here means a component whose content in the porous cellulose particles is 50% by mass or more. The content of cellulose and / or cellulose acetate in the porous cellulose particles is preferably 60% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, even more preferably 80% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass. The cellulose acetate used in the present invention is not particularly limited as long as it can be generally defined as cellulose diacetate, but it is preferable that the acetylation degree is 45 to 57%.
[0028] The sphericity of the porous cellulose particles is preferably 0.60 or more, more preferably 0.70 or more, even more preferably 0.80 or more, and still more preferably 0.90 or more, while the upper limit is preferably 1.00 or less.
[0029] The sphericity can be measured and calculated, for example, according to the following procedure. First, an SEM image of a porous cellulose particle taken with a scanning electron microscope (SEM) is subjected to image analysis, and the circularity C of each porous cellulose particle is calculated according to the following formula (1). Then, the arithmetic mean value of the circularities C of 10 or more arbitrarily selected porous cellulose particles is taken as the sphericity. C = (4πS1) / (L 2 ) ···(1)
[0030] In the above formula (1), S1 represents the area (projected area) of the porous cellulose particle in the image, and L represents the length of the outer periphery of the porous cellulose particle in the image. The closer to 1, the more spherical the particle shape is.
[0031] The cosmetic product of the present invention is not particularly limited, and examples thereof include foundation, lipstick, eye shadow, eyeliner, skin lotion, beauty essence, lotion, milky lotion, base cosmetic, massage cream, makeup cream, skin cream, skin care cosmetic, moisturizing cosmetic, whitening cosmetic, medicated cosmetic, sunscreen cosmetic, face wash cream, cleansing agent, and the like.
[0032] The formulation of the cosmetic product of the present invention is not particularly limited, and examples thereof include capsule, powder, granule, solid, liquid, gel, foam, emulsion, cream, ointment, sheet, mousse, powder dispersion, multi-layer, and aerosol forms.
[0033] The content (blended amount) of the porous cellulose particles in the cosmetic product of the present invention is not particularly limited, but is preferably 0.01% by mass to 50% by mass, more preferably 0.1% by mass to 40% by mass, and even more preferably 1.0% by mass to 30% by mass.
[0034] The cosmetic product of the present invention may contain optional ingredients that are commonly used in cosmetics to the extent that the effects of the present invention are not impaired. Examples of such optional ingredients are listed below. The oily components include polar oils, volatile hydrocarbon oils, and the like. Polar oils include synthetic ester oils such as isopropyl myristate, cetyl octanoate, octyldodecyl myristate, isopropyl palmitate, butyl stearate, hexyl laurate, myristyl myristate, decyl oleate, hexyldecyl dimethyloctanoate, cetyl lactate, myristyl lactate, lanolin acetate, isocetyl stearate, isocetyl isostearate, cholesteryl 12-hydroxystearate, and ethylene glycol di-2-ethylhexylate. , dipentaerythritol fatty acid esters, N-alkyl glycol monoisostearate, neopentyl glycol dicaprate, diisostearyl malate, glycerin di-2-heptylundecanoate, trimethylolpropane tri-2-ethylhexylate, trimethylolpropane triisostearate, pentaneerythritol tetra-2-ethylhexylate, glycerin tri-2-ethylhexylate, and trimethylolpropane triisostearate. In addition, cetyl 2-ethylhexanoate, 2-ethylhexyl palmitate, glyceryl trimyristate, tri-2-heptylundecanoate glyceride, methyl castor oil fatty acid Ester, oleic acid oil, cetostearyl alcohol, acetoglyceride, 2-heptylundecyl palmitate, diisobutyl adipate, N-lauroyl-L-glutamine Acid-2-octyldodecyl ester, di-2-heptylundecyl adipate, ethyl laurate, di-2-ethylhexyl sebacate, 2-hexyldecyl myristate, palmitic acid 2 2-hexyldecyl adipate, diisopropyl sebacate, 2-ethylhexyl succinate, ethyl acetate, butyl acetate, amyl acetate, triethyl citrate, octyl methoxycinnamate, and the like. Further, examples of natural oils include avocado oil, camellia oil, turtle oil, macadamia nut oil, corn oil, mink oil, olive oil, rapeseed oil, egg yolk oil, sesame oil, persic oil, wheat germ oil, sasanqua oil, castor oil, linseed oil, safflower oil, cottonseed oil, perilla oil, soybean oil, peanut oil, tea seed oil, kaya oil, rice bran oil, Chinese tung oil, Japanese tung oil, jojoba oil, germ oil, triglycerin, glycerin trioctanoate, and glycerin triisopalmitate.
[0035] Volatile hydrocarbon oils include isododecane, isohexadecane, and the like.
[0036] Examples of surfactants include anionic surfactants such as fatty acid soaps (sodium laurate, sodium palmitate, etc.), potassium lauryl sulfate, and alkyl sulfate triethanolamine ether; stearyl trimethylammonium chloride, benzalkonium chloride, and lauric acid. Cationic surfactants such as alkylamine oxide, betaine surfactants (alkyl betaines, amido betaines, sulfo betaines, etc.), imidazoline amphoteric surfactants (2-cocoyl-2-imidazolinium hydroxide-1-carboxyethyloxy disodium salt, etc.), Amphoteric surfactants such as silylmethyltaurine, sorbitan fatty acid esters (sorbitan monostearate, sorbitan sesquioleate, etc.), glycerin fatty acids (glycerin monostearate, etc.), propylene glycol fatty acid esters (propylene glycol monostearate, etc.), hydrogenated castor oil derivatives, glycerin alkyl ether, POE sorbita Polyoxyethylene fatty acid esters (POE sorbitan monooleate, polyoxyethylene monostearate sorbitan, etc.), POE sorbitol fatty acid esters (POE-sorbitol monolaurate etc.), POE glycerin fatty acid esters (POE-glycerin monoisostearate etc.), POE fatty acid esters (polyethylene glycol monooleate, POE distearate etc.), POE alkyl ethers (POE 2-octyldodecyl ether etc.), POE alkyl phenyl ethers (POE nonylphenyl ether etc.), Pluronic types, POE POP alkyl ether (POE · POP 2-decyl tetradecyl ether, etc.), Tetronics, POE castor oil, hardened Examples of such surfactants include castor oil derivatives (POE castor oil, POE hydrogenated castor oil, etc.), sucrose fatty acid esters, and non-ionic surfactants such as alkyl glucosides.
[0037] Examples of polyhydric alcohols include polyethylene glycol, glycerin, 1,3-butylene glycol, erythritol, sorbitol, xylitol, maltitol, propylene glycol, dipropylene glycol, diglycerin, isoprene glycol, 1,2-pentanediol, 2,4-hexylene glycol, 1,2-hexanediol, and 1,2-octanediol.
[0038] Examples of thickening agents include guar gum, quince seed, carrageenan, galactan, gum arabic, pectin, mannan, starch, xanthan gum, curdlan, methylcellulose, hydroxyethyl cellulose, carboxymethyl cellulose, methylhydroxypropyl cellulose, chondroitin sulfate, dermatan sulfate, glycogen, heparan sulfate, hyaluronic acid, sodium hyaluronate, tragacanth gum, keratan sulfate, chondroitin, mucoitin sulfate, hydroxyethyl guar gum, carboxymethyl guar gum, dextran, keratosulfuric acid, locust bean gum, succinoglucan, caronic acid, chitin, chitosan, carboxymethyl chitin, agar, polyvinyl alcohol, polyvinylpyrrolidone, carboxyvinyl polymer, alkyl-modified carboxyvinyl polymer, sodium polyacrylate, polyethylene glycol, and bentonite.
[0039] Examples of powders include powders such as mica, talc, kaolin, synthetic mica, calcium carbonate, magnesium carbonate, anhydrous silicic acid (silica), aluminum oxide, and barium sulfate, which may be surface-treated; inorganic pigments such as red iron oxide, yellow iron oxide, black iron oxide, cobalt oxide, ultramarine, iron blue, titanium oxide, and zinc oxide, which may be surface-treated; pearling agents such as titanium mica, fish phosphorus foil, and bismuth oxychloride, which may be surface-treated; Examples of suitable organic pigments include Red No. 202, Red No. 228, Red No. 226, Yellow No. 4, Blue No. 404, Yellow No. 5, Red No. 505, Red No. 230, Red No. 223, Orange No. 201, Red No. 213, Yellow No. 204, Yellow No. 203, Blue No. 1, Green No. 201, Purple No. 201, and Red No. 204, which may be compounded; and organic powders such as polyethylene powder, polymethyl methacrylate, nylon powder, and organopolysiloxane elastomers.
[0040] UV absorbers include para-aminobenzoic acid UV absorbers, anthranilic acid UV absorbers, salicylic acid UV absorbers, cinnamic acid UV absorbers, benzophenone UV absorbers, sugar UV absorbers, and 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazo. and ultraviolet absorbing agents such as 4-methoxy-4'-t-butyldibenzoylmethane.
[0041] Cosmetics also contain water, ethanol, fragrances, preservatives, pH adjusters, coloring agents, active ingredients, etc. It is possible to include components. Cosmetics can be manufactured by processing and blending the above-mentioned ingredients according to conventional methods.
[0042] The cosmetic product of the present invention can be blended with any ingredient normally used in cosmetics, and the blending may be a blend with a powder raw material, or the active ingredient used in the cosmetic product may be filled into the porous cellulose particles through the pores of the particles. When the active ingredient is filled into the particles, a sustained release effect of the active ingredient from the porous cellulose particles can be expected.
[0043] The porous cellulose particles are produced by a method comprising the steps of: (a) preparing a cellulose acetate solution by heating and dissolving cellulose acetate in a mixed solvent of a solvent in which cellulose acetate is soluble and a solvent in which cellulose acetate is insoluble; (b) dispersing the cellulose acetate solution in water containing an emulsion stabilizer to obtain a dispersion; and (c) cooling the dispersion to precipitate cellulose acetate particles, wherein the mixed solvent is an organic solvent that is immiscible with water.
[0044] Regarding the (a) step of producing porous cellulose particles, in step (a), cellulose acetate as a raw material is dissolved in a mixed solvent to prepare a cellulose acetate solution. Cellulose acetate is a semi-synthetic polymer obtained by acetic esterification of cellulose, which is a natural polymer. The cellulose acetate used in the present invention is not particularly limited as long as it can be generally defined as cellulose acetate, but it is preferable that the cellulose acetate has a degree of polymerization of 50 to 300 and an acetylation degree of 45 to 57%. By using cellulose acetate with a degree of polymerization of 50 to 300 and an acetylation degree of 45 to 57%, it can be dissolved in a wider variety of solvents.
[0045] In step (a), the ratio of cellulose acetate in the mixed solvent is preferably 0.1 to 50% by mass, more preferably 5 to 20% by mass. Within this range, a uniform solution is obtained, and porous particles having openings with a uniform diameter are easily obtained. In addition, precipitation due to phase separation is likely to occur when cooled, the strength is sufficient, and the approximately spherical particle shape is easily maintained. In addition, the lower the cellulose acetate concentration in the cellulose acetate solution, the smaller the particle size of the obtained porous particles, the larger the average diameter of the openings, the larger the ratio of the total projected area of the openings to the projected area of the porous cellulose particles, and the smaller the bulk density.
[0046] In step (a), the solvent in which the cellulose acetate solution is soluble, i.e., the good solvent, is not particularly limited as long as it can dissolve cellulose acetate, but an organic solvent with low solubility in water is preferred. The good solvent here refers to a solvent in which the solute dissolves in the solvent alone and a transparent solution containing no solid matter is obtained. In particular, the good solvent here refers to a solvent that can provide a solution of preferably 1% by mass or more at a temperature below the boiling point of the solvent. The solvent may be used alone or in combination of two or more solvents. Specific examples include benzyl alcohol, ethyl acetate, cyclohexanone, isophorone, and mixtures thereof. Among these, benzyl alcohol is preferred in terms of providing openings.
[0047] In step (a), the solvent in which the cellulose acetate solution is insoluble, i.e., the poor solvent, can be alcohols, glycols, ethers, esters, and mixtures thereof. The poor solvent refers to a solvent that has no or low solubility for a solute compared to a good solvent, specifically, a solvent that cannot dissolve the solute alone at a temperature below the boiling point of the solvent and cannot obtain a transparent solution. In particular, the poor solvent refers to a solvent that cannot dissolve 1% by mass or more of the solute at a temperature below the boiling point of the solvent. Solvents with low solubility in water are preferred. In particular, alcohols are preferred. The alcohols are preferably lower alcohols, and more preferably 1-hexanol in terms of providing openings.
[0048] In step (a), the volume ratio of the solvent in which cellulose acetate is soluble, i.e., the good solvent, to the solvent in which cellulose acetate is insoluble, i.e., the poor solvent, in the mixed solvent is preferably 5:95 to 95:5. The higher the ratio of the poor solvent in the mixed solvent, the larger the average diameter of the openings tends to be.
[0049] In step (a), the mixed solvent is an organic solvent that is not miscible with water. If it becomes miscible with water, a dispersion cannot be obtained in step (b).
[0050] In step (a), a third component, which is a polymer, can be added to the mixed solvent. As the third component polymer, polyethylene glycol or polypropylene glycol is preferable, and polypropylene glycol is more preferable. When polyethylene glycol or polypropylene glycol is added as the third component, the ratio of the total projected area of the openings to the projected area of the porous cellulose particles tends to be large, and the bulk density tends to be small.
[0051] In step (a), when the third component is polypropylene glycol, its molecular weight is not particularly limited, but from the viewpoint of ease of handling during the production process and the average diameter of the openings of the porous particles, it is preferable that the average molecular weight (Mw) is 100 to 3000. Moreover, the higher the molecular weight of the polymer of the third component, the larger the average diameter of the openings tends to be.
[0052] In step (a), from the viewpoint of the average diameter of the openings in the porous particles, the concentration of the third component in the mixed solvent is preferably 0.1 to 10 mass %, and the higher the concentration of the third component, the larger the average diameter of the openings, the larger the ratio of the total projected area of the openings to the projected area of the porous cellulose particles, and the smaller the bulk density tends to be.
[0053] In the step (a), the heating temperature for dissolving by heating is preferably, for example, in the range of 50 to 130° C. In this temperature range, it is preferable that the cellulose acetate dissolves in the mixed solvent. The heating and dissolving time is not particularly limited, and may be, for example, 3 to 24 hours.
[0054] In the step (b) of producing porous cellulose particles, the cellulose acetate solution is dispersed in high-temperature water in which an emulsion stabilizer is dissolved. In this step, the volume ratio of the cellulose acetate solution to the high-temperature water is not particularly limited as long as a dispersion system in which the cellulose acetate solution is the dispersed phase and the high-temperature water is the continuous phase can be obtained. From the viewpoint of obtaining a stable dispersion system, the volume ratio of the cellulose acetate solution to the high-temperature water (dispersed phase / continuous phase) is preferably 1.0 or less. The temperature of the high-temperature water is preferably 50 to 100°C, more preferably 60 to 95°C.
[0055] In step (b), any known method can be used for the dispersion method. For example, there are a method using a mixer such as an agitator, a method using a homogenizer, a method using ultrasonic waves, and the like. In addition, there are a method of extruding a cellulose acetate solution from a fine nozzle using what is generally called a microreactor to obtain droplets, and a method of extruding a cellulose acetate solution or a mixture of a cellulose acetate solution, water, and an emulsion stabilizer from a uniform, fine-diameter porous membrane and applying shear. Among them, the method of dispersing using an agitator is preferred because it is a simple method.
[0056] In step (b), the emulsion stabilizer is not particularly limited as long as it has the effect of increasing the stability of the dispersion system and preventing particle aggregation. For example, natural polymers such as starch, pectin, alginic acid, alginates, and gelatin, natural polymer processed products such as methyl cellulose, carboxymethyl cellulose, and hydroxyethyl cellulose, synthetic polymers containing alcoholic OH such as polyvinyl alcohol and partially saponified polyvinyl acetate, sulfonated Examples of suitable surfactants include SO3H group-containing polymers such as styrene, COOH group-containing polymers such as acrylic acid esters, nitrogen-containing synthetic polymers such as polyvinylpyrrolidone, inorganic powders such as barium sulfate, talc, bentonite, and titanium oxide, anionic surfactants such as linear alkylbenzenesulfonate sodium, cationic surfactants such as alkyltrimethylammonium salts, amphoteric surfactants such as alkyldimethylamine oxide, nonionic surfactants such as fatty acid sorbitan esters, and mixtures thereof. In particular, from the viewpoint of stabilizing the dispersion system, sodium dodecylbenzenesulfonate, polyvinyl alcohol, carboxymethylcellulose, hydroxyethylcellulose, and mixtures thereof are preferred.
[0057] The amount of emulsion stabilizer used in step (b) is preferably 0.01% by mass or more in terms of concentration in high-temperature water from the viewpoint of stabilizing the dispersion system. In this concentration range, if the amount of emulsion stabilizer added is increased, the particle size of the resulting porous cellulose particles tends to be smaller. Conversely, if the amount of emulsion stabilizer added is small, the particle size of the resulting porous cellulose particles tends to be large.
[0058] In the step (c) of producing porous cellulose particles, the dispersion liquid obtained in the step (b) is cooled. By cooling, thermally induced phase separation occurs, and porous particles having open pores can be obtained.
[0059] In step (c), the temperature to which the dispersion is cooled is not particularly limited as long as the cellulose acetate is precipitated at that temperature. However, the cooling temperature is preferably 0° C. to 50° C. in order to allow sufficient precipitation of the porous cellulose particles.
[0060] The above-mentioned manufacturing method can obtain porous cellulose particles made from cellulose acetate. When the porous cellulose particles made from cellulose acetate are to be made hydrophilic, the cellulose acetate can be converted into cellulose by saponification in a solution of an alkali metal hydroxide compound such as sodium hydroxide. If the porous cellulose particles of the present invention are used as cellulose acetate, a small amount of acetic acid may be released from the cellulose acetate in the cosmetic product, resulting in the odor of acetic acid. Therefore, it is preferable to remove the acetic acid content in advance by saponification.
[0061] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples. EXAMPLES
[0062] <Example 1> Porous cellulose particles were produced by the following procedure. First, a dispersed phase was prepared by dissolving cellulose diacetate in the following manner. In a 1L three-neck flask, 303.6 g of benzyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) and 215.4 g of 1-hexanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) were charged, and 77.9 g of cellulose diacetate (manufactured by Daicel Corporation, product name: L-20) was gradually added and dispersed while stirring. The mixture was then heated to 120°C using a mantle heater to dissolve the cellulose diacetate. After dissolution, the liquid temperature in the three-neck flask was lowered from 120°C to 100°C to form a dispersed phase, which was then maintained at 100°C in preparation for the dropwise addition of the dispersed phase to the continuous phase described below.
[0063] Next, benzyl alcohol and 1-hexanol were added to pure water to prepare a continuous phase according to the following procedure. Put 1.8 L of pure water into a separatory funnel, and while stirring, add 122.8 g of benzyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) and 122.8 g of 1-hexanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent). The mixture was then left to stand to separate into an aqueous phase and an oil phase, and 1.8 L of the lower layer of solvent-saturated water was separated and transferred to a 5 L separable flask. The 5 L separable flask was immersed in a water bath, and four paddle blades were attached to the 5 L separable flask as stirring blades. The flask was heated to 60°C while stirring at a rotation speed of 250 rpm. While continuing to stir, 1.44 g of polyvinyl alcohol (JP-18E, manufactured by Japan Acetate & Poval Co., Ltd.) and 25.2 g of sodium carboxymethylcellulose (reagent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to the 5 L separable flask at 60°C and dissolved, and this was used as the continuous phase.
[0064] For the granulation operation, the stirring blade of the 5L separable flask was changed to an edge turbine blade. The mixture was stirred at 1,000 rpm and heated in a water bath until the continuous phase reached 80°C, and the dispersed phase prepared above was added dropwise. This caused the dispersed phase to disperse in the continuous phase in the form of oil droplets. After dispersion, the temperature of the water bath was lowered, and the contents of the 5 L separable flask were cooled to 30°C, and the oil droplets were removed. The dispersed phase was fixed to obtain a cellulose diacetate particle slurry. The cellulose diacetate particle slurry was taken from the 5 L separable flask and filtered. The cellulose diacetate particles were washed with pure water, then with methanol, and again with pure water to remove the residual solvent from within the cellulose diacetate particles.
[0065] For the saponification reaction, 100 g (water content 87%) of cellulose diacetate particles in a wet state after removing residual solvent was placed in a 500 ml separable flask, and 135 ml of methanol solution (45% by volume) was added and stirred. The liquid temperature in the separable flask was adjusted to 35°C, 36 g of 20% aqueous sodium hydroxide solution was added, and the mixture was stirred at 150 rpm at 35°C for 4 hours to promote the saponification reaction, and cellulose particles were obtained from the cellulose diacetate particles by the saponification reaction.
[0066] After the saponification reaction, dilute acetic acid was dropped into the cellulose particle slurry in the separable flask to neutralize it, and then the slurry was filtered in a vacuum bottle using filter paper (5B manufactured by Advantec Toyo Co., Ltd.). The filtered cellulose particles were washed with a large amount of pure water and filtered again to obtain wet cellulose particles. After drying the particles, they were passed through a sieve with a mesh size of 45 μm to remove particles with a large particle size, and the resulting particles were used as the porous cellulose particles of Example 1.
[0067] <Example 2> In order to prepare porous cellulose particles having an opening area different from that in Example 1, the following procedure was carried out. First, a dispersed phase was prepared by dissolving cellulose diacetate in the following manner. 242.8 g of benzyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) and 172.3 g of 1-hexanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) were charged into a 1 L three-neck flask, and 77.9 g of cellulose diacetate (manufactured by Daicel Corporation, product name: L-20) was gradually added and dispersed while stirring. The mixture was then heated to 120°C using a mantle heater to dissolve the cellulose diacetate. After dissolution, the liquid temperature in the three-neck flask was lowered from 120°C to 100°C to form a dispersed phase, which was then maintained at 100°C in preparation for the dropwise addition of the dispersed phase to the continuous phase described below.
[0068] Next, benzyl alcohol and 1-hexanol were added to pure water to prepare a continuous phase according to the following procedure. 1.92 L of pure water was charged into a separatory funnel, and 131.0 g of benzyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) and 93.0 g of 1-hexanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) were added and mixed while stirring. The mixture was then left to stand to separate into an aqueous phase and an oil phase, and 1.92 L of the lower solvent-saturated water was separated and separated into a 5 L separable flask. The 5 L separable flask was immersed in a water bath, and four paddle blades were attached as stirring blades to the 5 L separable flask, and the flask was heated to 60 °C while stirring at a rotation speed of 250 rpm. 1.54 g of polyvinyl alcohol (manufactured by Japan Acetate Poval Co., Ltd., JP-18E) and 26.9 g of sodium carboxymethylcellulose (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) were added to the 5 L separable flask at 60 °C while continuing to stir, and dissolved, and this was used as the continuous phase. Thereafter, granulation, washing, saponification and classification were carried out in the same manner as in Example 1 to obtain porous cellulose particles of Example 2.
[0069] <Example 3> In order to prepare porous cellulose particles having an open pore area different from that in Examples 1 and 2, the following procedure was carried out. In a 1L three-neck flask, 242.8 g of benzyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) and 172.3 g of 1-hexanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) were charged, and 93.5 g of cellulose diacetate (manufactured by Daicel Corporation, product name: L-20) was gradually added and dispersed while stirring. Then, the temperature was raised to 120°C using a mantle heater to dissolve the cellulose diacetate. After dissolution, the liquid temperature in the three-neck flask was lowered from 120°C to 100°C to make this a dispersed phase, and the temperature was kept at 100°C in preparation for the dropwise addition of the dispersed phase to the continuous phase described below. Then, the continuous phase was prepared, granulated, washed, saponified, and classified in the same manner as in Example 2 to obtain porous cellulose particles of Example 3.
[0070] <Example 4> In order to prepare porous cellulose particles having an open pore area different from those in Examples 1 to 3, the following procedure was carried out. In a 1L three-neck flask, 242.8 g of benzyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) and 172.3 g of 1-hexanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) were charged, and 109.1 g of cellulose diacetate (manufactured by Daicel Corporation, product name: L-20) was gradually added and dispersed while stirring. Then, the temperature was raised to 120°C using a mantle heater to dissolve the cellulose diacetate. After dissolution, the liquid temperature in the three-neck flask was lowered from 120°C to 100°C to make this a dispersed phase, and the temperature was kept at 100°C in preparation for the dropwise addition of the dispersed phase to the continuous phase described below. Then, the continuous phase was prepared, granulated, washed, saponified, and classified in the same manner as in Example 2 to obtain porous cellulose particles of Example 4.
[0071] <Example 5> In order to prepare porous cellulose particles having an open pore area different from those in Examples 1 to 4, the following procedure was carried out. First, a dispersed phase was prepared by dissolving cellulose diacetate in the following manner. In a 1L three-neck flask, 303.6 g of benzyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent) and 220.0 g of 2-ethylbutyl alcohol (manufactured by JNC Corporation, industrial) were charged, and 77.9 g of cellulose diacetate (manufactured by Daicel Corporation, product name: L-20) was gradually added and dispersed while stirring. The mixture was then heated to 120°C using a mantle heater to dissolve the cellulose diacetate. After dissolution, the liquid temperature in the three-neck flask was lowered from 120°C to 100°C to form a dispersed phase, which was then maintained at 100°C in preparation for the dropwise addition of the dispersed phase to the continuous phase described below.
[0072] Next, a continuous phase was prepared by adding benzyl alcohol and 2-ethylbutyl alcohol to pure water according to the following procedure. A separatory funnel was charged with 1.8 L of pure water, and 122.8 g of benzyl alcohol (Fujifilm Wako Pure Chemical Industries, reagent) and 89.0 g of 2-ethylbutyl alcohol (JNC Corporation, industrial use) were added and mixed while stirring. The mixture was then left to stand to separate into an aqueous phase and an oil phase, and 1.92 L of the lower layer of solvent-saturated water was separated and separated into a 5 L separable flask. The 5 L separable flask was immersed in a water bath, and four paddle blades were attached as stirring blades inside the 5 L separable flask. The mixture was stirred at a rotation speed of 250 rpm, and the inside of the flask was heated to 60°C. Stirring was continued. While keeping the temperature at 60°C, 1.44 g of polyvinyl alcohol (JP-18E, manufactured by Japan Vinyl Acetate & Poval Co., Ltd.) and 25.2 g of sodium carboxymethylcellulose (reagent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to a 5 L separable flask and dissolved, forming a continuous phase.
[0073] For the granulation operation, the stirring blade of the 5L separable flask was changed to an edge turbine blade. The mixture was stirred at 1,000 rpm and heated in a water bath until the continuous phase reached 80°C, and the dispersed phase prepared above was added dropwise. This caused the dispersed phase to disperse in the continuous phase in the form of oil droplets. The mixture of the dispersed phase and the continuous phase was then poured into ice water to immobilize the oil droplet-like dispersed phase, yielding a cellulose diacetate particle slurry. The cellulose diacetate particle slurry was taken from the 5 L separable flask and filtered. The cellulose diacetate particles were washed with pure water, then washed with methanol, and washed again with pure water to remove the residual solvent from the cellulose diacetate particles. Thereafter, washing and classification were performed in the same manner as in Example 1 to obtain the porous particles of Example 5.
[0074] (Measurement of mode diameter) The particle size distribution was measured and the mode diameter was determined for the porous cellulose particles of Examples 1 to 5. The following apparatus was used for the measurement. The measurement results are shown in Table 1. Equipment: Laser Scattering Particle Size distribution Analyzer Partica LA-960 (manufactured by HORIBA)
[0075] (Measurement of bulk density) The bulk density of the porous cellulose particles of Examples 2 to 4 was measured by the following procedure. 20 g of each sample of the porous cellulose particles of Examples 2 to 4 was filled into a 100 ml graduated test tube, and the graduated test tube was manually tapped 300 times from a height of 3 cm on a tabletop rubber sheet to confirm the bulk, and then tapped an additional 200 times to confirm that there was no decrease in bulk. Thereafter, the filling volume was read, and the bulk density was calculated by dividing the weight (20 g) of the sample by the filling volume (ml) after tapping. The results are shown in Table 1.
[0076] [Table 1]
[0077] (SEM observation) SEM observation was carried out using an ultra-high resolution field emission scanning electron microscope "SU8020" manufactured by Hitachi High-Technologies. The porous cellulose particles of Examples 1 to 5 and the particles of Comparative Examples 1 to 5 were freeze-dried as a pretreatment, and then Au-coated, and photographed. The product names of the particles of Comparative Examples 1 to 5 are shown in Table 2. The results of SEM observation are shown in Figures 1 to 10. Photographs of single porous cellulose particles were taken so that the diameter of the particle was 0.5 or more times the long side of the photograph (the horizontal side of the photograph). 1 to 5, it was confirmed that the porous cellulose particles of Examples 1 to 5 were approximately spherical and had open pores on the particle surface. It can be seen that the openings in the powder particles are connected to the pores inside the powder, whereas the particles of Comparative Examples 1 to 5 have no openings, as shown in Figures 6 to 10.
[0078] [Table 2]
[0079] (Measurement of the average diameter of the openings) Using the photographs of single particles taken in the SEM observation in Figs. 1 to 5, the average diameter of the openings in the porous cellulose particles of Examples 1 to 5 was determined by the following method. The short side of the photograph (the vertical side of the photograph) was taken as the Y-axis and the long side was taken as the X-axis, and the average of the diameters of the porous cellulose particles in the Y-axis direction and the X-axis direction was calculated, and this was designated as the representative diameter [Dp] (μm).
[0080] Next, the center of the particle was surrounded by a square whose side length was two-thirds of the representative diameter [Dp], and the outside of the surrounded area was deleted, resulting in a photograph that showed only the inside of the surrounded part of the particle. The position of the square was determined as the point where the center of the porous cellulose particle shown in the photograph overlapped with the center of the square. The area [Ap] of the part surrounded by the square was calculated using the formula Ap(μm 2 )=(Dp×2÷3) 2 I asked for more.
[0081] Next, the processed images were processed using DeepCle, an AI image analysis service from Sakai Chemical Industry Co., Ltd., to determine the total number of apertures, the average maximum width and average diagonal width of the apertures, and the average aperture area. The diagonal width is the distance from edge to edge of the opening on a line perpendicular to the center of the maximum width line segment. The average diameter [Dav] of the openings was calculated from the formula Dav (μm) = (average maximum width of the openings (μm) + average diagonal width of the openings (μm)) ÷ 2. The total projected area [Sp] of the openings was calculated from the formula Sp (μm 2 ) = Total number of openings (pieces) × Average opening area (μm 2 ) was obtained. Then, the ratio of the total horizontal projected area of the open pores to the horizontal projected area of the porous cellulose particles was calculated by the formula: Open pore area ratio (%)=Sp÷Ap×100.
[0082] (Calculation of the number of openings per projected area of porous cellulose particles) Based on the total number of openings and the value of Ap, the number of openings per projected area of the porous cellulose particle is calculated by the formula: Number of openings per projected area of the porous cellulose particle (holes / μm 2 ) = Total number of openings (pieces) ÷ Ap (μm2 ) was obtained.
[0083] The results of each measurement using photographs of single particles in Examples 1 to 5 are shown in Table 3. "Ratio of open pore area per unit area" refers to the ratio of the total open pore area to the projected area of the surface of a porous cellulose particle, and "number of open pores per unit area" refers to the number of open pores per projected area of the surface of a porous cellulose particle.
[0084] [Table 3]
[0085] <Evaluation method> 1. Preparation method of powder foundation for evaluation (dry sample) A commercially available foundation (manufactured by Lucky Trendy Co., Ltd., product name: Crayon Touch Me ST Powder Foundation Ocher) was pulverized in a mixer to obtain a powder foundation. This was used as a standard powder foundation without the addition of spherical particles. In addition, the particles of Example 1 or Comparative Examples 1 to 5 were mixed in a mortar to obtain 10% by mass of this powder foundation, thereby obtaining a uniform powder foundation for evaluation (dry sample).
[0086] 2. Method for preparing olive oil-impregnated powder foundation for evaluation (oil-impregnated sample) Olive oil (manufactured by Ajinomoto Co., Inc., product name: JOYL (J Oil) Ajinomoto Olive Oil) was mixed uniformly in a mortar to a concentration of 10% by mass for the standard powder foundation without the addition of spherical particles and each dry sample to prepare an olive oil-impregnated powder foundation for evaluation (oil-impregnated sample). This oil-impregnated sample was used as a model of the powder foundation with sebum adsorbed.
[0087] 3. How to prepare the evaluation board Artificial leather-coated rice cakes were prepared as substrates for evaluation of the dry and oil-impregnated samples. A rectangular piece of rice cake (manufactured by Sato Foods Co., Ltd., product name: Sato's rice cake, approximately 6.5 cm long x 4 cm wide x 1.6 cm high) was entirely wrapped in oil blotting paper (manufactured by Kyowa Shiko Co., Ltd., product name: Oil blotting paper tabletop box type 90 mm x 90 mm), and the surface to be used for evaluation (approximately The edges of the oil blotting paper were fixed with cellophane tape on the back side of a 6.5 cm long x 4 cm wide sheet of paper. The surface to be used for evaluation was then covered with black artificial leather (Idemitsu Technofine Co., Ltd., product name: Suplarre), and the edges of the black artificial leather were fixed with cellophane tape to the four side surfaces adjacent to the surface to be used as a substrate for evaluation.
[0088] 4. Method of applying dry and oil-impregnated samples to evaluation substrates For each dry sample and oil-impregnated sample, a urethane puff was used to apply 0.5 mg / cm 2 One type of sample (either a dry sample or an oil-impregnated sample) was applied to each evaluation substrate.
[0089] 5. How to measure lightness and chroma Using a color difference meter (Konica Minolta, product name: Color Reader CR-10), The L* (lightness) and C* (chroma) of the dry sample and the oil-impregnated sample coated on the substrate were measured, respectively.
[0090] 6. Gloss measurement method A gloss meter (Horiba Ltd., product name: Handy gloss meter IG-320) was used. The glossiness of the dry sample and the oil-impregnated sample applied to the evaluation substrate was measured.
[0091] 7. Measurement method of bulk density 3 g of the dry sample and oil-impregnated sample were filled into a 10 ml graduated test tube, and the graduated test tube was manually tapped 300 times from a height of 3 cm on a rubber sheet on a table to check the volume. Then, it was tapped a further 200 times to check that there was no decrease in volume. The filled volume was then read and the bulk specific gravity was calculated by dividing the weight of the sample (3 g) by the filled volume (ml) after tapping.
[0092] 8. How to measure color unevenness (σL*, σC*) Double-sided tape (3 cm x 3 cm) was attached to a transparent plastic plate, the dry sample was sprayed onto it, and excess dry sample was removed with a cosmetic brush to adjust the amount of applied dry sample to 5 mg, thereby obtaining a sample for measuring color unevenness. Furthermore, the sample for measuring color unevenness was divided into six parts, and L* (lightness) and C* (chroma) were measured at six points using a color difference meter (Konica Minolta, product name: Color Reader CR-10), and the standard deviations of L* and C* (σL*, σC*) were calculated.
[0093] 9. Method for measuring the moisturizing power of powder The dry sample and the oil-impregnated sample were applied at 0.3 mg / cm2 on the surface of the evaluation substrate prepared in the above section "3. Preparation of evaluation substrate". 2 The powder was applied with a makeup brush so that the moisture content was 100% and left to stand for 8 hours in an airflow circulation type thermostatic chamber (37°C) at 50% humidity, and the drying rate [mg / h] of the evaluation substrate was calculated to evaluate the moisture retention of the powder. One type of sample (dry sample or oil-impregnated sample) was applied to each evaluation substrate. The drying rate [mg / h] of the evaluation substrate was calculated by subtracting the weight of the evaluation substrate before standing from the weight after standing (i.e., the amount of water evaporated) [mg], and dividing this value by the standing time (8 hours).
[0094] <Evaluation Results> 1. Evaluation results of the physical properties of each powder foundation using the evaluation substrate The physical property evaluation results of each powder foundation are shown in Table 4 and FIGS.
[0095] [Table 4] In the table, "L*(+ / -)" indicates the difference in brightness compared to L* (brightness) when the dry sample is applied. "L*" represents the ratio of L* when the oil-impregnated sample is applied to the dry sample, and "C*(+ / -)" represents the ratio of C* (chroma) when the oil-impregnated sample is applied to the dry sample.
[0096] The relationship between the abbreviations in each table and figure and each particle is as follows: The blank represents a standard powder foundation containing no spherical particles. Cosmetic Example 1 is a powder foundation containing the particles of Example 1 at 10% by mass. Comparative cosmetic example 1 is a powder foundation containing 10 mass % of the particles of Comparative example 1. The comparative cosmetic product 2 is a powder foundation containing the particles of the comparative example 2 at 10 mass %. The comparative cosmetic product 3 is a powder foundation containing the particles of the comparative example 3 at 10 mass %. The cosmetic comparative example 4 is a powder foundation containing 10 mass % of the particles of Comparative Example 4. The comparative cosmetic product 5 is a powder foundation containing the particles of the comparative example 5 at 10 mass %.
[0097] 2. Evaluation of L* (lightness) of dry and oil-impregnated samples Compared to the dry samples other than Cosmetic Example 1, the dry sample of Cosmetic Example 1 was shown to have high L* (lightness) and bright color development (Table 4 and Figure 11). Furthermore, even when impregnated with oil, Cosmetic Example 1 showed little decrease in L* (lightness) (Table 4 and Figures 12-13). From these results, when actually applied to the skin, it is expected that the product will develop a bright color and there will be little change in brightness even after sebum absorption, and that it will have the effect of preventing makeup from coming off.
[0098] 3. Evaluation of C* (chroma) for dry and oil-impregnated samples 14 to 16, the dry sample of cosmetic example 1 has high C* (chroma), and the decrease in C* (chroma) after oil impregnation is very small. From these results, when actually applied to the skin, there is little change in chroma before and after sebum absorption, and it is expected that the effect of preventing makeup from coming off is expected.
[0099] 4. Evaluation of gloss of dry and oil-impregnated samples 17 to 19, the dry sample of cosmetic example 1 has low gloss, and the change in gloss after oil impregnation is very small. From these results, when actually applied to the skin, there is no change in gloss before and after sebum absorption, and it is expected to have an effect of suppressing the so-called shine of the skin caused by sebum.
[0100] 5. Evaluation of bulk density As shown in Table 5 and Figure 22, the bulk density of the dry sample of Cosmetic Example 1 is smaller than that of the dry samples other than Cosmetic Example 1, so that a light feel can be expected when actually applied to the skin. Also, as shown in Table 5 and Figure 23, Cosmetic Example 1 has a small bulk density even when impregnated with oil, so that a so-called dry feeling can be expected to be maintained even after absorbing sebum.
[0101] [Table 5]
[0102] 6. Evaluation of color unevenness (σL*, σC*) 24-25, the standard deviations of both brightness (L*) and chroma (C*) were smaller or comparable for the dry samples of Cosmetic Example 1 compared to those of the dry samples other than Cosmetic Example 1. These results suggest that the product is less likely to cause color unevenness when actually applied to the skin.
[0103] [Table 6] 7.Evaluation of the moisturizing power of powders 20-21, when the dry sample of cosmetic example 1 was applied, the drying speed of the evaluation substrate was slow, and the evaporation of water from the evaluation substrate was suppressed. The drying speed of the oil-impregnated sample was also slow, and the evaporation of water from the evaluation substrate was suppressed. When actually applied to the skin, a high moisturizing effect can be expected both before and after sebum absorption.
[0104] [Table 7]
Claims
1. A cosmetic product comprising substantially spherical porous cellulose particles, The mode diameter of the porous cellulose particles is 1.0 μm to 300.0 μm; the porous cellulose particles have openings on the particle surface, the openings communicating with voids inside the particles; A cosmetic product characterized in that the ratio of the total projected area of the openings to the projected area of the porous cellulose particles, as observed under a scanning electron microscope, is 5% to 95%.
2. The cosmetic product according to claim 1, wherein the average diameter of the openings is from 0.01 μm to 10.0 μm.
3. The cosmetic product according to claim 1 or 2, wherein the porous cellulose particles have a bulk density of 0.10 g / ml to 0.90 g / ml.
4. The number of the openings per projected area of the porous cellulose particles observed with a scanning electron microscope is 3 / μm 2 From 80 pieces / μm 2 The cosmetic product according to claim 1 or 2,
5. 3. The cosmetic product according to claim 1 or 2, which is a foundation, lipstick, eye shadow, eyeliner, skin lotion, beauty serum, lotion, milky lotion, base cosmetic, massage cream, makeup cream, skin cream, skin care cosmetic, moisturizing cosmetic, whitening cosmetic, medicated cosmetic, sunscreen cosmetic, face wash cream, or cleansing agent.
6. 3. The cosmetic product according to claim 1 or 2, wherein the porous cellulose particles are produced by a method comprising the steps of: (a) preparing a cellulose acetate solution by heating and dissolving cellulose acetate in a mixed solvent of a solvent in which cellulose acetate is soluble and a solvent in which cellulose acetate is insoluble; (b) dispersing the cellulose acetate solution in water containing an emulsion stabilizer to obtain a dispersion; and (c) cooling the dispersion to precipitate cellulose acetate particles, wherein the mixed solvent is an organic solvent that is not miscible with water.
7. 7. The cosmetic product according to claim 6, wherein in step (a), the solvent in which the cellulose acetate is soluble is benzyl alcohol, ethyl acetate, cyclohexanone, or isophorone.
8. 7. The cosmetic product according to claim 6, wherein in step (a), the solvent in which the cellulose acetate is insoluble is an alcohol, a glycol, an ether, or an ester.
9. 7. The cosmetic product according to claim 6, wherein in step (a), the volume ratio of the solvent in which the cellulose acetate is soluble to the solvent in which the cellulose acetate is insoluble in the mixed solvent is from 5:95 to 95:
5.
10. The cosmetic product according to claim 6, wherein in step (a), the ratio of cellulose acetate in the mixed solvent is from 0.1% by mass to 50% by mass.
11. The cosmetic product according to claim 6, wherein in step (a), the mixed solvent contains a third component which is a polymer, and the third component is polyethylene glycol or polypropylene glycol.
12. In step (b), the emulsion stabilizer is selected from the group consisting of sodium dodecylbenzenesulfonate, polyvinyl alcohol, carboxymethyl cellulose, hydroxyethyl cellulose, and the like. The cosmetic product according to claim 6, which is a mixture of these.
Citation Information
Patent Citations
Resin bead manufacturing method, resin beads, and products using resin beads