Adhesive composition and adhesive sheet

The adhesive composition, utilizing (meth)acrylic resin and olefin resin particles with controlled properties, addresses the challenge of maintaining adhesion and removability in saltwater conditions, preventing peeling and residue on containers.

JP2024158537APending Publication Date: 2024-11-08NIPPON CARBIDE KOGYO KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023073802
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing adhesive compositions used for labeling containers transported by sea face challenges in maintaining adhesion to adherends even when immersed in saltwater, leading to peeling and adhesive residue, which is exacerbated by exposure to sea spray and potential immersion in seawater.

Method used

An adhesive composition comprising (meth)acrylic resin particles, olefin resin particles, and a crosslinking agent, with specific ratios and properties to form an adhesive layer that maintains high adhesion and removability, even when exposed to saltwater, by controlling the storage modulus and glass transition temperature.

Benefits of technology

The adhesive composition forms a layer that resists peeling from adherends in saltwater environments and minimizes adhesive residue, ensuring effective label attachment and removal without damage to the container.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158537000001
    Figure 2024158537000001
  • Figure 2024158537000002
    Figure 2024158537000002
  • Figure 2024158537000003
    Figure 2024158537000003
Patent Text Reader

Abstract

To provide an adhesive composition and the like that enable the formation of an adhesive layer resistant to peeling from an adherend even when immersed in salt water, such as seawater, and exhibiting superior re-peelability.SOLUTION: An adhesive composition includes: (meth)acrylic resin particles that include (A) a constitutional unit derived from a (meth)alkyl acrylate monomer and (B) a constitutional unit derived from a monomer with a carboxy group, where the content of the constitutional unit (B) is in the range of 0.01 mass% or more and 2.0 mass% or less relative to all the constitutional units; olefinic resin particles; a crosslinker; and water. The adhesive composition enables the formation of an adhesive layer that exhibits a storage modulus of more than 1.0×106 Pa to 1.0×108 Pa or less at 30°C and 1 Hz.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a pressure-sensitive adhesive composition and a pressure-sensitive adhesive sheet. [Background technology]

[0002] In recent years, from the viewpoint of global environmental conservation, there has been a demand for the development of water-based adhesives that use water instead of solvent-based adhesives that use organic solvents. Water-based adhesives are also widely used as removable adhesives.

[0003] For example, Patent Document 1 discloses a removable aqueous pressure-sensitive adhesive composition in which monomer components mainly composed of (meth)acrylate are charged all at once into a sealed pressure reaction vessel in the presence of an aqueous medium and subjected to emulsion polymerization, the time required for the weight conversion of the monomer components to reach 95% is substantially within 180 minutes, and the removable aqueous pressure-sensitive adhesive composition comprises polymer particles [X] containing carbonyl groups and carboxy groups and having an acid value of 3 to 30, and a hydrazine derivative [Y] having at least two hydrazino groups in the molecule, and the coating formed from the aqueous pressure-sensitive adhesive composition has a glass transition temperature of -25°C or lower and a gel fraction of 80% by weight or higher. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-281548 A Summary of the Invention [Problem to be solved by the invention]

[0005] By the way, labels with various information may be attached to containers such as drums and containers used for marine transportation by ship. The labels attached to these containers may be splashed with sea spray. In addition, these containers may fall into the sea during transportation, and the labels attached to the containers may be immersed in seawater. The presence of salt water such as seawater may deteriorate the adhesive layer of the label, which may cause the label to peel off from the adherend. For this reason, it is required that the adhesive composition used for attaching the label to the containers to be transported by ship can form an adhesive layer that is difficult to peel off from the adherend even when immersed in salt water such as seawater. In addition, these containers are often reused, and the labels need to be replaced. However, when the adhesive layer deteriorates, a phenomenon called "glue residue" is likely to occur in which a part of the adhesive layer remains on the adherend when the label is peeled off. For this reason, adhesive compositions used for attaching labels to containers undergoing marine transport by ship are required to be able to form an adhesive layer that is unlikely to leave adhesive residue on the adherend when peeled from the adherend, even when immersed in salt water such as seawater, i.e., an adhesive layer that has excellent removability.

[0006] Regarding the above-mentioned points, Patent Document 1 does not focus on realizing the formation of a pressure-sensitive adhesive layer that is difficult to peel off from an adherend and has excellent removability even when immersed in salt water such as seawater.

[0007] The present disclosure has been made in consideration of the above-mentioned circumstances. An object of one embodiment of the present disclosure is to provide a pressure-sensitive adhesive composition capable of forming a pressure-sensitive adhesive layer that is difficult to peel off from an adherend and has excellent removability, even when immersed in salt water such as seawater. The problem that another embodiment of the present disclosure aims to solve is to provide an adhesive layer that is difficult to peel off from an adherend even when immersed in salt water such as seawater and has excellent removability, and an adhesive sheet comprising the adhesive layer. [Means for solving the problem]

[0008] Specific means for solving the problems include the following aspects. <1> (meth)acrylic resin particles containing a structural unit (A) derived from a (meth)acrylic acid alkyl ester monomer and a structural unit (B) derived from a monomer having a carboxy group, the content of the structural unit (B) being in the range of 0.01% by mass or more and 2.0% by mass or less with respect to all structural units, an olefin resin particle, a crosslinking agent, and water; When the pressure-sensitive adhesive layer is formed, the storage modulus of the pressure-sensitive adhesive layer at 30° C. and 1 Hz is 1.0×10 6 Pa exceeds 1.0 × 10 8 The pressure-sensitive adhesive composition has a range of Pa or less. <2> The pressure-sensitive adhesive layer has a storage modulus of 1.0×10 at 30° C. and 1 Hz. 6 Pa exceeds 1.0 × 10 7 Pa or less <1> The pressure-sensitive adhesive composition according to claim 1. <3> Further, the present invention includes tackifier resin particles. <1> or <2> The pressure-sensitive adhesive composition according to claim 1. <4> The (meth)acrylic resin particles have a glass transition temperature in the range of -40°C or higher and 0°C or lower. <1> ~ <3> 13. The pressure-sensitive adhesive composition according to claim 12 . <5> The (meth)acrylic resin particles have an average particle size in the range of 5 nm to 250 nm. <1> ~ <4> 13. The pressure-sensitive adhesive composition according to claim 12 . <6> The (meth)acrylic resin particles further contain a structural unit (C) derived from a reactive surfactant. <1> ~ <5> 13. The pressure-sensitive adhesive composition according to claim 12 . <7> <1> ~ <6> 13. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to any one of claims 1 to 22. Effect of the Invention

[0009] According to one embodiment of the present disclosure, there is provided a pressure-sensitive adhesive composition capable of forming a pressure-sensitive adhesive layer that is difficult to peel off from an adherend and has excellent removability even when immersed in salt water such as seawater. According to another embodiment of the present disclosure, there is provided a pressure-sensitive adhesive layer that is difficult to peel off from an adherend even when immersed in salt water such as seawater and has excellent removability, and a pressure-sensitive adhesive sheet including the pressure-sensitive adhesive layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The adhesive composition, adhesive layer, and adhesive sheet of the present disclosure will be described in detail below. The following description of the requirements may be based on a representative embodiment of the present disclosure, but the present disclosure is not limited to such an embodiment, and can be modified as appropriate within the scope of the purpose of the present disclosure.

[0011] In the present disclosure, a numerical range indicated using "to" means a range that includes the numerical values ​​before and after "to" as the lower limit and upper limit, respectively. In the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in the present disclosure. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.

[0012] In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments.

[0013] In the present disclosure, when the adhesive composition contains multiple substances corresponding to each component, the amount of each component in the adhesive composition means the total amount of the multiple substances present in the adhesive composition, unless otherwise specified.

[0014] In the present disclosure, "(meth)acrylic monomer" means a monomer having a (meth)acryloyl group. In the present disclosure, "(meth)acrylic resin" means a resin that contains structural units derived from (meth)acrylic monomers and in which the proportion of structural units derived from (meth)acrylic monomers is 50 mass% or more. "Monomer" in this disclosure does not include reactive surfactants.

[0015] In this disclosure, "(meth)acrylic" is a term that encompasses both "acrylic" and "methacrylic", "(meth)acrylate" is a term that encompasses both "acrylate" and "methacrylate", and "(meth)acryloyl" is a term that encompasses both "acryloyl" and "methacryloyl".

[0016] In this disclosure, "n-" means normal, "i-" means iso, "s-" means secondary, and "t-" means tertiary.

[0017] In the present disclosure, "mass %" and "weight %" are synonymous, and "parts by mass" and "parts by weight" are synonymous.

[0018] In the present disclosure, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.

[0019] In the present disclosure, the term "layer" includes cases where the layer is formed over the entire area when the area is observed, as well as cases where the layer is formed over only a part of the area. The same applies to the term "film." In this disclosure, the term "lamination" refers to stacking layers, and a "lamination" may be two or more layers bonded together, or two or more layers may be detachable.

[0020] [Adhesive composition] The pressure-sensitive adhesive composition of the present disclosure comprises (meth)acrylic resin particles comprising a structural unit (A) derived from a (meth)acrylic acid alkyl ester monomer and a structural unit (B) derived from a monomer having a carboxy group, the content of the structural unit (B) being in the range of 0.01% by mass or more and 2.0% by mass or less with respect to all structural units, olefin-based resin particles, a crosslinking agent, and water, and when a pressure-sensitive adhesive layer is formed, the pressure-sensitive adhesive layer has a storage modulus at 30° C. and 1 Hz of 1.0×10 6 Pa exceeds 1.0 × 10 8 The range is below Pa. In the present disclosure, "(meth)acrylic resin particles which contain a structural unit (A) derived from a (meth)acrylic acid alkyl ester monomer and a structural unit (B) derived from a monomer having a carboxy group, and in which the content of the structural unit (B) is in the range of 0.01 mass % or more and 2.0 mass % or less with respect to all structural units" is also referred to as "specific (meth)acrylic resin particles".

[0021] The pressure-sensitive adhesive composition of the present disclosure comprises selected components, specific (meth)acrylic resin particles comprising structural units (A) derived from a (meth)acrylic acid alkyl ester monomer and structural units (B) derived from a monomer having a carboxy group in a specific range of proportions, olefin resin particles, a crosslinking agent, and water, and is designed so that when a pressure-sensitive adhesive layer is formed, the storage modulus of the pressure-sensitive adhesive layer at 30°C and 1 Hz is within a specific range, thereby achieving the formation of a pressure-sensitive adhesive layer that is difficult to peel off from an adherend and has excellent removability, even when immersed in salt water such as seawater. The adhesive composition of the present disclosure contains specific (meth)acrylic resin particles, and therefore can form an adhesive layer having high adhesive strength to an adherend. In addition, in the present disclosure, the adhesive composition is designed so that the storage modulus of the adhesive layer formed at 30°C and 1 Hz is a specific value or more, thereby imparting an appropriate hardness to the adhesive layer. When the adhesive layer is appropriately hardened, salt water such as seawater is less likely to penetrate between the adhesive layer and the adherend, and it is considered that the decrease in adhesive strength due to deterioration of the adhesive layer is suppressed. Therefore, it is presumed that the adhesive composition of the present disclosure can form an adhesive layer that is difficult to peel off from the adherend even when immersed in salt water such as seawater. Since the adhesive composition of the present disclosure contains specific (meth)acrylic resin particles, olefin resin particles, and a crosslinking agent, the formed adhesive layer is given a moderately high cohesive strength by the reaction between the carboxyl group derived from the structural unit (B) in a specific range of ratio contained in the specific (meth)acrylic resin particles and the crosslinking agent, and by the presence of the olefin resin particles. When the cohesive strength of the adhesive layer is high, the phenomenon of glue residue is unlikely to occur. In the present disclosure, by designing the adhesive composition so that the adhesive layer formed has the above-mentioned storage modulus, deterioration of the adhesive layer due to salt water such as seawater entering between the adhesive layer and the adherend is suppressed, and the cohesive strength of the adhesive layer is thought to be well maintained. In addition, in the present disclosure, the adhesive composition is designed so that the storage modulus of the adhesive layer formed at 30°C and 1 Hz is a specific value or less, thereby imparting moderate softness to the adhesive layer. When the adhesive layer becomes moderately soft, the adhesion between the adhesive layer and the substrate is increased, so that the phenomenon of glue residue is unlikely to occur. Therefore, it is presumed that the pressure-sensitive adhesive composition of the present disclosure can form a pressure-sensitive adhesive layer that has excellent removability even when immersed in salt water such as seawater.

[0022] However, (meth)acrylic resin and olefin resin have a large difference in polarity, so that they tend to separate easily even if they are mixed together. For example, when a (meth)acrylic resin and an olefin resin are used in a solvent-based pressure-sensitive adhesive, the olefin resin may be localized at the interface of the pressure-sensitive adhesive layer, and the components may become biased in the pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer with the components biased is prone to cohesive failure when peeled off from the adherend, and tends to have poor removability. In contrast, the pressure-sensitive adhesive composition of the present disclosure is an aqueous pressure-sensitive adhesive containing water, and contains particulate (meth)acrylic resin and particulate olefin resin, so that the (meth)acrylic resin and the olefin resin are well dispersed. This is believed to suppress localization of the olefin resin at the interface of the pressure-sensitive adhesive layer. Therefore, it is presumed that the pressure-sensitive adhesive layer formed by the pressure-sensitive adhesive composition of the present disclosure is unlikely to suffer from a decrease in removability due to the inclusion of the (meth)acrylic resin and the olefin resin.

[0023] In addition, since the pressure-sensitive adhesive composition of the present disclosure contains (meth)acrylic resin particles and olefin-based resin particles, which have significantly different polarities, it is presumed that the pressure-sensitive adhesive layer formed can exhibit the effects of the present disclosure regardless of the polarities of the substrate and adherend.

[0024] <<Storage modulus>> The pressure-sensitive adhesive composition of the present disclosure, when a pressure-sensitive adhesive layer is formed, has a storage modulus of the pressure-sensitive adhesive layer at 30° C. and 1 Hz of 1.0×10 6 Pa exceeds 1.0 × 10 8 The range is below Pa. Storage modulus at 30℃ and 1Hz is 1.0×10 6 A pressure-sensitive adhesive layer having a hardness exceeding 1.1×10 Pa has an appropriate hardness, so that salt water is unlikely to penetrate between the pressure-sensitive adhesive layer and the adherend, and the pressure-sensitive adhesive layer is unlikely to be deteriorated by salt water, and therefore tends not to peel off from the adherend even when immersed in salt water such as seawater. From this viewpoint, the pressure-sensitive adhesive composition of the present disclosure has a pressure-sensitive adhesive layer having a storage modulus of 1.1×10 at 30° C. and 1 Hz of 1.1×10 6 Pa or more, and 1.2×10 6 It is more preferable that the pressure is 1 Pa or more. Storage modulus at 30℃ and 1Hz is 1.0×10 8 A pressure-sensitive adhesive layer having a storage modulus of 5.0×10 Pa or less at 30° C. and 1 Hz tends to have high adhesion to a substrate and therefore has excellent removability even when immersed in salt water such as seawater. From this perspective, the pressure-sensitive adhesive composition of the present disclosure has a pressure-sensitive adhesive layer having a storage modulus of 5.0×10 7 Pa or less, and 1.0×10 7 Pa or less, and more preferably 5.0×10 6 It is more preferable that the viscosity is 0.1 Pa or less. In one embodiment, the pressure-sensitive adhesive composition of the present disclosure has a storage modulus at 30° C. and 1 Hz of 1.0×10 6 Pa exceeds 5.0 × 10 7 Pa or less, and may be in the range of 1.0 x 10 6 Pa exceeds 1.0 × 10 7Pa or less, and may be in the range of 1.0 x 10 6 Pa exceeds 5.0 × 10 6 Pa or less, and may be in the range of 1.1 x 10 6 Pa or more 5.0×10 6 Pa or less, and may be in the range of 1.2 x 10 6 Pa or more 5.0×10 6 It may be in the range of Pa or less.

[0025] In the present disclosure, the storage modulus of the pressure-sensitive adhesive layer is a value measured by the following method. A dynamic viscoelasticity measuring device is used as the measuring device, and the viscoelasticity spectrum of a 400 μm thick adhesive layer is measured using a dynamic viscoelasticity measuring method in accordance with JIS K7244-1:1998 (temperature range: 25°C to 130°C, heating rate: 5°C / min, frequency: 1 Hz, cone used: 8 mmφ), to determine the storage modulus (G') at 30°C. As a dynamic viscoelasticity measuring device, for example, Anton Paar's Physica MCR301 (product name) can be suitably used, although the dynamic viscoelasticity measuring device is not limited thereto.

[0026] The storage modulus of the pressure-sensitive adhesive layer can be controlled to a desired value by adjusting, for example, the composition, amount, particle size and glass transition temperature of the (meth)acrylic resin particles, the composition, amount and particle size of the olefin resin particles, the quantitative ratio of the (meth)acrylic resin particles to the olefin resin particles, the type and amount of the crosslinking agent, and the presence or absence, and the type and amount of an additive, all of which are contained in the pressure-sensitive adhesive composition. For example, increasing the glass transition temperature of the specific (meth)acrylic resin particles, incorporating tackifier resin particles in the adhesive composition, increasing the content of crosslinking agent in the adhesive composition, or increasing the content of olefin-based resin particles in the adhesive composition increases the elastic modulus of the adhesive layer, whereas decreasing the glass transition temperature of the specific (meth)acrylic resin particles, decreasing the content of crosslinking agent in the adhesive composition, or decreasing the content of olefin-based resin particles decreases the elastic modulus of the adhesive layer.

[0027] [Specific (meth)acrylic resin particles] The pressure-sensitive adhesive composition of the present disclosure contains (meth)acrylic resin particles (i.e., specific (meth)acrylic resin particles) that contain a constituent unit (A) derived from a (meth)acrylic acid alkyl ester monomer and a constituent unit (B) derived from a monomer having a carboxy group, and the content of the constituent unit (B) is in the range of 0.01% by mass or more and 2.0% by mass or less based on the total constituent units. In the pressure-sensitive adhesive composition of the present disclosure, the specific (meth)acrylic resin particles are present in a state of being dispersed in a medium containing water. The pressure-sensitive adhesive composition of the present disclosure may contain only one type of specific (meth)acrylic resin particles, or may contain two or more types.

[0028] <Structural Unit (A) Derived from (Meth)acrylic Acid Alkyl Ester Monomer> The specific (meth)acrylic resin particles contain a structural unit (A) derived from a (meth)acrylic acid alkyl ester monomer. In the present disclosure, the "structural unit (A) derived from a (meth)acrylic acid alkyl ester monomer" is also simply referred to as the "structural unit (A)". In the present disclosure, the term "structural unit derived from a (meth)acrylic acid alkyl ester monomer" refers to a structural unit formed by addition polymerization of a (meth)acrylic acid alkyl ester monomer. In the present disclosure, the term "(meth)acrylic acid alkyl ester monomer" refers to a (meth)acrylic acid alkyl ester monomer that does not have a carboxy group. In other words, in the present disclosure, a "(meth)acrylic acid alkyl ester monomer having a carboxy group" is classified as a monomer having a carboxy group.

[0029] The type of the (meth)acrylic acid alkyl ester monomer is not particularly limited. The (meth)acrylic acid alkyl ester monomer may be an acrylic acid alkyl ester monomer or a methacrylic acid alkyl ester monomer. The alkyl group in the (meth)acrylic acid alkyl ester monomer may be unsubstituted or may have a substituent, but is preferably unsubstituted. The alkyl group contained in the (meth)acrylic acid alkyl ester monomer may be linear, branched, or cyclic. The alkyl group in the (meth)acrylic acid alkyl ester monomer preferably has 1 to 18 carbon atoms, more preferably 1 to 12 carbon atoms, and further preferably 1 to 8 carbon atoms.

[0030] Specific examples of the (meth)acrylic acid alkyl ester monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-octyl (meth)acrylate, i-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, i-nonyl (meth)acrylate, n-decyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate. The (meth)acrylic acid alkyl ester monomer preferably contains at least one selected from the group consisting of n-butyl acrylate, methyl methacrylate, and 2-ethylhexyl acrylate, and more preferably contains at least one selected from the group consisting of n-butyl acrylate, methyl methacrylate, and 2-ethylhexyl acrylate.

[0031] The specific (meth)acrylic resin particles may contain only one type of structural unit (A), or may contain two or more types.

[0032] The content of the structural unit (A) in the specific (meth)acrylic resin particles is not particularly limited, but for example, with respect to all structural units of the specific (meth)acrylic resin particles (however, in cases where the specific (meth)acrylic resin particles contain a structural unit (C) derived from a reactive surfactant, the structural unit (C) is excluded), it is preferably in the range of 50.0 mass% or more and 99.99 mass% or less, more preferably in the range of 60.0 mass% or more and 99.95 mass% or less, even more preferably in the range of 70.0 mass% or more and 99.95 mass% or less, and particularly preferably in the range of 80.0 mass% or more and 99.95 mass% or less. The content of the structural unit (A) in the specific (meth)acrylic resin particles being 50.0 mass% or more relative to all structural units of the specific (meth)acrylic resin particles (excluding structural unit (C) in cases where the specific (meth)acrylic resin particles contain structural unit (C) derived from a reactive surfactant), means that the structural unit (A) is contained as a main component of the structural units of the resin that forms the specific (meth)acrylic resin particles.

[0033] <Structural Unit (B) Derived from Monomer Having a Carboxy Group> The specific (meth)acrylic resin particles contain the structural unit (B) derived from a monomer having a carboxy group in a ratio of 0.01% by mass to 2.0% by mass relative to all structural units (however, in cases where the specific (meth)acrylic resin particles contain a structural unit (C) derived from a reactive surfactant, the structural unit (C) is excluded). In the present disclosure, the "structural unit (B) derived from a monomer having a carboxy group" is also simply referred to as the "structural unit (B)". In the present disclosure, a "structural unit derived from a monomer having a carboxy group" refers to a structural unit formed by addition polymerization of a monomer having a carboxy group.

[0034] The type of the monomer having a carboxy group is not particularly limited. An example of a monomer having a carboxy group is a monomer having at least one carboxy group and an ethylenically unsaturated group in one molecule. The ethylenically unsaturated group is not particularly limited, and examples thereof include a vinyl group, an allyl group, a vinylphenyl group, a (meth)acrylamide group, and a (meth)acryloyl group. The ethylenically unsaturated group is preferably a (meth)acryloyl group.

[0035] Specific examples of monomers having a carboxy group include (meth)acrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, glutaconic acid, citraconic acid, ω-carboxy-polycaprolactone mono(meth)acrylate [e.g., ω-carboxy-polycaprolactone (n≒2) monoacrylate], and succinic acid derivatives (e.g., 2-acryloyloxyethyl-succinic acid). As the monomer having a carboxy group, a (meth)acrylic monomer having a carboxy group is preferable, and (meth)acrylic acid is more preferable.

[0036] The specific (meth)acrylic resin particles may contain only one type of structural unit (B), or may contain two or more types.

[0037] The content of the structural unit (B) in the specific (meth)acrylic resin particles is in the range of 0.01% by mass or more and 2.0% by mass or less with respect to all structural units of the specific (meth)acrylic resin particles (however, in cases where the specific (meth)acrylic resin particles contain a structural unit (C) derived from a reactive surfactant, the structural unit (C) is excluded). The content of the structural unit (B) in the specific (meth)acrylic resin particles is 0.01% by mass or more relative to the total structural units of the specific (meth)acrylic resin particles [however, when the specific (meth)acrylic resin particles contain the structural unit (C) derived from a reactive surfactant, the structural unit (C) is excluded. ] means that the specific (meth)acrylic resin particles actively contain the structural unit (B). When the specific (meth)acrylic resin particles contain the structural unit (B), the pressure-sensitive adhesive layer formed by the reaction between the carboxy group and the crosslinking agent has increased cohesive force, so that it tends to be difficult to peel off from the adherend even when immersed in salt water such as seawater. From this viewpoint, the lower limit of the content of the structural unit (B) in the specific (meth)acrylic resin particles is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, relative to the total structural units of the specific (meth)acrylic resin particles [however, when the specific (meth)acrylic resin particles contain the structural unit (C) derived from a reactive surfactant, the structural unit (C) is excluded. ]. When the content of the structural unit (B) in the specific (meth)acrylic resin particles is 2.0% by mass or less based on the total structural units of the specific (meth)acrylic resin particles (excluding the structural unit (C) when the specific (meth)acrylic resin particles contain the structural unit (C) derived from a reactive surfactant). ), the pressure-sensitive adhesive layer formed does not have too high a cohesive force, so that the adhesion to the substrate is not impaired, and even when immersed in salt water such as seawater, the pressure-sensitive adhesive layer tends to have excellent removability. From this viewpoint, the upper limit of the content of the structural unit (B) in the specific (meth)acrylic resin particles is preferably 1.8% by mass or less, more preferably 1.5% by mass or less based on the total structural units of the specific (meth)acrylic resin particles (excluding the structural unit (C) when the specific (meth)acrylic resin particles contain the structural unit (C) derived from a reactive surfactant). In one embodiment, the content of the structural unit (B) in the specific (meth)acrylic resin particles may be in the range of 0.05% by mass or more and 2.0% by mass or less, 0.05% by mass or more and 1.8% by mass or less, 0.05% by mass or more and 1.5% by mass or less, or 0.1% by mass or more and 1.5% by mass or less, based on all structural units of the specific (meth)acrylic resin particles (however, in cases where the specific (meth)acrylic resin particles contain a structural unit (C) derived from a reactive surfactant, the structural unit (C) is excluded).

[0038] <Structural unit (C) derived from reactive surfactant> The specific (meth)acrylic resin particles preferably further contain a structural unit (C) derived from a reactive surfactant. In the present disclosure, the term "reactive surfactant" refers to a surfactant having an ethylenically unsaturated double bond. In addition, in the present disclosure, the term "structural unit derived from a reactive surfactant" refers to a structural unit formed by addition polymerization of a reactive surfactant.

[0039] When the specific (meth)acrylic resin particles contain the structural unit (C) derived from a reactive surfactant, the adhesive layer tends to be less likely to peel off from the adherend when immersed in salt water such as seawater, compared to when the adhesive composition contains a non-reactive surfactant. Also, when the specific (meth)acrylic resin particles contain the structural unit (C), the adhesive layer tends to have better removability when immersed in salt water such as seawater, compared to when the adhesive composition contains a non-reactive surfactant.

[0040] The type of reactive surfactant is not particularly limited. The reactive surfactant may be an anionic reactive surfactant, a nonionic reactive surfactant, or a cationic reactive surfactant. The reactive surfactant is preferably at least one selected from the group consisting of anionic reactive surfactants and nonionic reactive surfactants, and more preferably a combination of at least one selected from anionic reactive surfactants and at least one selected from nonionic reactive surfactants.

[0041] The reactive surfactant preferably has an oxyalkylene group. Specific examples of the oxyalkylene group include an oxyethylene group, an oxypropylene group, and an oxybutylene group. As the oxyalkylene group, for example, an oxyethylene group is preferred from the viewpoint of high reactivity with the monomer.

[0042] The average number of moles of oxyalkylene groups added is not particularly limited. The average number of moles of oxyalkylene groups added is, for example, preferably 5 to 50, more preferably 5 to 40, and even more preferably 10 to 30, from the viewpoint of dispersibility of the specific (meth)acrylic resin particles.

[0043] For example, when the specific (meth)acrylic resin particles contain two or more types of structural units (C), the reactive surfactant is preferably an anionic reactive surfactant having an average added mole number of 10 to 20 oxyethylene groups, and at least one reactive surfactant is preferably a nonionic reactive surfactant having an average added mole number of 20 to 30 oxyethylene groups.

[0044] The reactive surfactant having an ethylenically unsaturated double bond can be obtained by adding a group having an ethylenically unsaturated double bond to a surfactant. Specific examples of the group having an ethylenically unsaturated double bond include a (meth)acryloyl group, a vinyl group, an allyl group, an isopropenyl group, a 1-propenyl group, an allyloxy group, and a styryl group. As the group having an ethylenically unsaturated double bond, for example, a 1-propenyl group or an allyloxy group is preferable from the viewpoint of high reactivity with the monomer.

[0045] As the reactive surfactant, commercially available products can be used. Examples of commercially available anionic reactive surfactants include "Aqualon KH-05" (active ingredient: polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium [oxyalkylene group type: oxyethylene group, average number of moles added: 5], active ingredient concentration: 99% by mass), "Aqualon KH-10" (active ingredient: polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium [oxyalkylene group type: oxyethylene group, average number of moles added: 10], active ingredient concentration: 99% by mass), "Aqualon AR-10" (active ingredient: polyoxyethylene styrenated propenyl phenyl ether sulfate ammonium [oxyalkylene group type: oxyethylene group, average number of moles added: 10], active ingredient concentration: 99% by mass), and "Aqualon "HS-10" [active ingredient: polyoxyethylene nonylpropenyl phenyl ether sulfate ammonium [oxyalkylene group type: oxyethylene group, average number of moles added: 10], active ingredient concentration: 99% by mass], "Aqualon BC-10" [active ingredient: polyoxyethylene nonylpropenyl phenyl ether sulfate ammonium [oxyalkylene group type: oxyethylene group, average number of moles added: 10], active ingredient concentration: 99% by mass], "Aqualon AR-20" [active ingredient: polyoxyethylene styrenated propenyl phenyl ether sulfate ammonium [oxyalkylene group type: oxyethylene group, average number of moles added: 20], active ingredient concentration: 99% by mass], and "Aqualon BC-20" [active ingredient: polyoxyethylene nonylpropenyl phenyl ether sulfate ammonium [oxyalkylene group type: oxyethylene group, average number of moles added: 20], active ingredient concentration: 99% by mass], and "ADEKA REASOAP" manufactured by ADEKA CORPORATION SR-10" [Active ingredient: Polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ester ammonium [Type of oxyalkylene group: oxyethylene group, average number of moles added: 10], Active ingredient concentration: 100% by mass], "ADEKA REASOAPSR-20" [active ingredient: polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium [type of oxyalkylene group: oxyethylene group, average number of moles added: 20], active ingredient concentration: 100% by mass], and Adeka Reasoap SR-3025" [active ingredient: polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium [type of oxyalkylene group: oxyethylene group, average number of moles added: 30], active ingredient concentration: 25% by mass]. Examples of commercially available nonionic reactive surfactants include "ADEKA REASOAP ER-10" (active ingredient: polyoxyethylene-1-(allyloxymethyl) alkyl ether [type of oxyalkylene group: oxyethylene group, average number of moles added: 10], active ingredient concentration: 100% by mass), "ADEKA REASOAP ER-30" (active ingredient: polyoxyethylene-1-(allyloxymethyl) alkyl ether [type of oxyalkylene group: oxyethylene group, average number of moles added: 30], active ingredient concentration: 65% by mass), and "ADEKA REASOAP ER-40" (active ingredient: polyoxyethylene-1-(allyloxymethyl) alkyl ether [type of oxyalkylene group: oxyethylene group, average number of moles added: 40], active ingredient concentration: 60% by mass), all manufactured by ADEKA Corporation. The above "Aqualon" and "Adeka Reasop" are both registered trademarks.

[0046] When the specific (meth)acrylic resin particles contain the structural unit (C), they may contain only one type of structural unit (C), or may contain two or more types of structural unit (C).

[0047] When the specific (meth)acrylic resin particles contain the structural unit (C), the content of the structural unit (C) is not particularly limited. When the specific (meth)acrylic resin particles contain the structural unit (C), the lower limit of the content of the structural unit (C) is, for example, preferably 0.5 parts by mass or more and more preferably 1.0 parts by mass or more per 100 parts by mass of all structural units of the specific (meth)acrylic resin particles (excluding the structural unit (C)). When the content of the structural unit (C) in the specific (meth)acrylic resin particles is 0.5 parts by mass or more per 100 parts by mass of all structural units of the specific (meth)acrylic resin particles (excluding the structural unit (C)), the specific (meth)acrylic resin particles tend to be well produced by emulsion polymerization. When the specific (meth)acrylic resin particles contain the structural unit (C), the upper limit of the content of the structural unit (C) is, for example, preferably 2.5 parts by mass or less, and more preferably 2.0 parts by mass or less, per 100 parts by mass of all structural units of the specific (meth)acrylic resin particles (excluding the structural unit (C)). When the specific (meth)acrylic resin particles contain the structural unit (C), the structural unit (C) may be unevenly distributed on the surface of the adhesive layer. If the content of the structural unit (C) in the specific (meth)acrylic resin particles is 2.5 parts by mass or less relative to 100 parts by mass of the total structural units of the specific (meth)acrylic resin particles (excluding the structural unit (C)), the amount of the structural unit (C) present on the surface of the adhesive layer is not too large, and the tackiness is maintained at an appropriate level, so that the adhesive layer tends to exhibit higher adhesive strength to the adherend. When water adheres to the surface of the adhesive layer, the reactive surfactant dissolves in the water, which may cause the phenomenon of water penetrating into the adhesive layer. On the other hand, if the content of the structural unit (C) in the specific (meth)acrylic resin particles is 2.5 parts by mass or less relative to 100 parts by mass of the total structural units of the specific (meth)acrylic resin particles (excluding the structural unit (C)), the penetration of water into the adhesive layer caused by the dissolution of the reactive surfactant is suppressed, so that the adhesive layer tends to be less likely to peel off from the adherend when immersed in salt water such as seawater. When the specific (meth)acrylic resin particle contains the structural unit (C), in one embodiment, the content of the structural unit (C) may be in the range of 0.5 parts by mass or more and 2.5 parts by mass or less, or in the range of 0.5 parts by mass or more and 2.0 parts by mass or less, or in the range of 1.0 parts by mass or more and 2.0 parts by mass or less, relative to 100 parts by mass of all structural units of the specific (meth)acrylic resin particle (excluding the structural unit (C)).

[0048] <Constituent units derived from other monomers> The specific (meth)acrylic resin particles may contain a structural unit derived from a monomer (so-called other monomer) that does not fall into either the (meth)acrylic acid alkyl ester monomer or the monomer having a carboxy group. In the present disclosure, the term "structural units derived from other monomers" refers to structural units formed by addition polymerization of other monomers.

[0049] Examples of structural units derived from other monomers include structural units derived from (meth)acrylates having an aromatic ring, such as benzyl (meth)acrylate and phenoxyethyl (meth)acrylate; structural units derived from alkoxyalkyl (meth)acrylates, such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; structural units derived from vinyl cyanide, such as acrylonitrile and methacrylonitrile; structural units derived from aromatic monovinyls, such as styrene, α-methylstyrene, t-butylstyrene, p-chlorostyrene, chloromethylstyrene, and vinyltoluene; structural units derived from vinyl esters, such as vinyl formate, vinyl acetate, vinyl propionate, and vinyl versatate; and the like.

[0050] When the specific (meth)acrylic resin particles contain a structural unit derived from another monomer, the specific (meth)acrylic resin particles may contain only one type of structural unit derived from the other monomer, or may contain two or more types of structural units derived from the other monomer.

[0051] When the specific (meth)acrylic resin particles contain structural units derived from other monomers, the content of the structural units derived from other monomers can be appropriately set within a range that does not impair the effects of the pressure-sensitive adhesive composition of the present disclosure.

[0052] <<Glass transition temperature of specific (meth)acrylic resin particles>> The glass transition temperature (also referred to as "Tg") of the specific (meth)acrylic resin particles is not particularly limited. The lower limit of the glass transition temperature of the specific (meth)acrylic resin particles is, for example, preferably not less than −60° C., more preferably not less than −50° C., and even more preferably not less than −40° C. When the glass transition temperature of the specific (meth)acrylic resin particles is not less than −60° C., a pressure-sensitive adhesive layer having a high storage modulus tends to be easily formed. The upper limit of the glass transition temperature of the specific (meth)acrylic resin particles is, for example, preferably 10° C. or less, more preferably 5° C. or less, and even more preferably 0° C. or less. When the glass transition temperature of the specific (meth)acrylic resin particles is 10° C. or less, the adhesive layer becomes softer, and the adhesive layer has higher adhesion to the substrate, so that the adhesive layer tends to have better removability when immersed in salt water such as seawater. In addition, when the glass transition temperature of the specific (meth)acrylic resin particles is 10° C. or less, the adhesive layer has higher wettability to the adherend, so that the adhesive layer tends to show higher adhesive strength to the adherend. In one embodiment, the glass transition temperature of the specific (meth)acrylic resin particles may be in the range of -60°C or more and 10°C or less, in the range of -50°C or more and 5°C or less, or in the range of -40°C or more and 0°C or less.

[0053] The glass transition temperature of the specific (meth)acrylic resin particles is a value measured by the following method using a differential scanning calorimetry (DSC). A water dispersion of specific (meth)acrylic resin particles is applied onto the release paper using a 4 mil (101.6 μm) applicator. The applied water dispersion of specific (meth)acrylic resin particles is then dried (drying temperature: 105° C., drying time: 10 minutes) to obtain a dried product of specific (meth)acrylic resin particles. 10 mg of this dried product is packed into an aluminum sample pan (e.g., Tzero Pan (trade name) manufactured by TA Instrument Co., Ltd.) and sealed with an aluminum lid (e.g., Tzero Hermetic Lid (trade name) manufactured by TA Instrument Co., Ltd.), and then the glass transition temperature is measured using a differential scanning calorimeter under the following measurement conditions. In this measurement, the glass transition temperature is determined as the temperature at the intersection of a straight line extending the low-temperature side baseline to the high-temperature side in the obtained DSC curve and a tangent line drawn at a point where the gradient of the curve of the stepwise change part of the glass transition is maximum. As the differential scanning calorimeter, for example, a differential scanning calorimeter (product name: Discovery DSC 2500) manufactured by TA Instruments Japan Co., Ltd. can be used. However, the differential scanning calorimeter is not limited to this.

[0054] -Measurement conditions- Atmospheric conditions: under air Measurement temperature range: -90℃~100℃ Heating rate: 10℃ / min Standard: empty crucible

[0055] The glass transition temperature of the specific (meth)acrylic resin particles can be adjusted, for example, by changing the types and ratio of monomers that are raw materials for the specific (meth)acrylic resin particles.

[0056] <<Shape of specific (meth)acrylic resin particles>> The shape of the specific (meth)acrylic resin particles is not particularly limited. The specific (meth)acrylic resin particles are preferably spherical in shape. In the present disclosure, the term "spherical" includes not only a perfect sphere but also an approximately spherical shape.

[0057] <<Average particle size of specific (meth)acrylic resin particles>> The average particle size of the specific (meth)acrylic resin particles is not particularly limited. In this disclosure, "average particle size" refers to the average primary particle size. The average particle size of the specific (meth)acrylic resin particles is preferably larger than the average particle size of the olefin resin particles. When the average particle size of the specific (meth)acrylic resin particles is larger than that of the olefin resin particles, the adhesive strength of the formed pressure-sensitive adhesive layer to the adherend tends to be higher. The reason for this is considered to be as follows. When the average particle size of the specific (meth)acrylic resin particles is larger than that of the olefin resin particles, excessive exposure of the olefin resin particles on the surface of the formed pressure-sensitive adhesive layer is suppressed, and the wettability of the pressure-sensitive adhesive layer to the adherend is less likely to be impaired. Therefore, it is considered that the adhesive strength of the pressure-sensitive adhesive layer is more easily expressed when the pressure-sensitive adhesive layer is pressed against the adherend.

[0058] The average particle size of the specific (meth)acrylic resin particles is not particularly limited. The lower limit of the average particle size of the specific (meth)acrylic resin particles is, for example, preferably 5 nm or more, more preferably 10 nm or more, even more preferably 20 nm or more, and particularly preferably 30 nm or more, from the viewpoint of the production suitability of the specific (meth)acrylic resin particles. The upper limit of the average particle size of the specific (meth)acrylic resin particles is, for example, preferably 600 nm or less, more preferably 450 nm or less, further preferably 300 nm or less, and particularly preferably 250 nm or less. When the average particle size of the specific (meth)acrylic resin particles is 600 nm or less, the adhesive layer tends to be less likely to peel off from the adherend when immersed in salt water such as seawater. The reason for this is thought to be as follows. When the particle size of the specific (meth)acrylic resin particles is small, the specific (meth)acrylic resin particles are thought to be densely arranged during the drying process of the coating film of the adhesive composition. It is thought that the dense arrangement of the specific (meth)acrylic resin particles increases the smoothness of the surface of the adhesive layer formed, making it difficult for water to penetrate between the adhesive layer and the adherend. In one embodiment, the average particle diameter of the specific (meth)acrylic resin particles may be in the range of 5 nm or more and 600 nm or less, 5 nm or more and 450 nm or less, 5 nm or more and 300 nm or less, 5 nm or more and 250 nm or less, 10 nm or more and 450 nm or less, 20 nm or more and 300 nm or less, or 30 nm or more and 250 nm or less.

[0059] The average particle size of the specific (meth)acrylic resin particles can be adjusted, for example, by changing the concentration of the reactive surfactant in the polymerization reaction solution when the specific (meth)acrylic resin particles are produced. For example, the particle size of the specific (meth)acrylic resin particles becomes smaller when the concentration of the reactive surfactant in the polymerization reaction solution is high at the beginning of the production process, and becomes larger when the concentration of the reactive surfactant in the polymerization reaction solution is low at the beginning of the production process. The "early stage of the production process" here refers to the time when an emulsion of a mixture containing a monomer component and a reactive surfactant is prepared, for example, when the method [3] is adopted as the emulsion polymerization method for producing the specific (meth)acrylic resin particles described later. The particle size of the specific (meth)acrylic resin particles can also be adjusted, for example, by changing the dispersion conditions in the reaction field (eg, stirring speed) so that the dispersion state of the components contained in the polymerization reaction solution varies.

[0060] The average particle size of the specific (meth)acrylic resin particles is a value measured by the dynamic light scattering method described in "New Experimental Chemistry Lectures 4, Basic Technology 3, Light (II)" edited by the Chemical Society of Japan, pages 725 to 741 (published by Maruzen Co., Ltd. on July 20, 1976). The specific method is as follows. An aqueous dispersion of specific (meth)acrylic resin particles (hereinafter referred to as "aqueous dispersion X") is diluted with distilled water and thoroughly mixed, after which 5 mL is taken into a 10 mm square glass cell using a Pasteur pipette, and this is set in a dynamic light scattering photometer (e.g., Zetasizer 1000HS manufactured by Sysmex Corporation). The attenuation rate (Attenuator) is set to x8 (8 times), and the concentration of the diluted aqueous dispersion X is adjusted so that the count rate of the attenuation rate is 150 kCps to 200 kCps. The results of the measurement under conditions of a measurement temperature of 25°C ± 1°C and a light scattering angle of 90° are then processed by computer to determine the average particle size of the specific (meth)acrylic resin particles. The Z-average value is used as the average particle size. However, the dynamic light scattering photometer is not limited to the above.

[0061] <<Content of specific (meth)acrylic resin particles>> The content of the specific (meth)acrylic resin particles in the pressure-sensitive adhesive composition of the present disclosure is not particularly limited, but for example, is preferably in the range of 25 mass % or more and 80 mass % or less, more preferably in the range of 30 mass % or more and 75 mass % or less, and even more preferably in the range of 35 mass % or more and 70 mass % or less, relative to the total solid content in the pressure-sensitive adhesive composition.

[0062] In the present disclosure, the term "total solid content in the PSA composition" refers to the mass of the residue remaining after removing the solvent from the PSA composition. In the present disclosure, the term "solvent" refers to water and organic solvents.

[0063] [Olefin-based resin particles] The pressure-sensitive adhesive composition of the present disclosure contains olefin-based resin particles. When the pressure-sensitive adhesive composition of the present disclosure contains olefin-based resin particles in addition to the specific (meth)acrylic resin particles, the pressure-sensitive adhesive layer formed has increased cohesive strength and therefore tends to have excellent removability even when immersed in salt water such as seawater.

[0064] In the present disclosure, the term "olefin resin" refers to a resin that contains structural units derived from an olefin monomer and in which the proportion of structural units derived from the olefin monomer is 50 mass% or more. In addition, in the present disclosure, the term "olefin monomer" refers to a monomer having an olefin skeleton.

[0065] The olefin resin may be a homopolymer of one type of olefin monomer, a copolymer of two or more types of olefin monomers, or a copolymer of one or more types of olefin monomers and one or more types of monomers other than olefin monomers (excluding the case of (meth)acrylic resins).

[0066] Examples of olefin monomers include α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, and 4-methyl-1-hexene.

[0067] The olefin-based resin particles may be chlorinated olefin-based resin particles. However, it is preferable that the olefin-based resin particles are not chlorinated, and more specifically, that the olefin-based resin particles do not contain chlorine atoms, in that there are no concerns about the impact on the environment and health.

[0068] The olefin-based resin particles are preferably acid-modified olefin-based resin particles. When the olefin-based resin particles are acid-modified olefin-based resin particles, the adhesive strength of the formed pressure-sensitive adhesive layer to the adherend tends to be increased. Also, when the olefin-based resin particles are acid-modified olefin-based resin particles, the pressure-sensitive adhesive layer tends to be less likely to peel off from the adherend when immersed in salt water such as seawater. In the present disclosure, the term "acid-modified olefin resin particles" refers to particles of an olefin resin having an acidic group that can react with a crosslinking agent and that has been modified with an acidic group-containing compound such as an unsaturated carboxylic acid or an unsaturated carboxylic anhydride (e.g., maleic anhydride). The acid anhydride structure itself does not exhibit acidity, but, for example, it is hydrolyzed to open the ring and generate an acidic group, and therefore exhibits the same reactivity as an acidic group. Therefore, in the present disclosure, the acid anhydride structure is considered to be an acidic group.

[0069] The shape of the olefin resin particles is not particularly limited, but is preferably spherical. The average particle size of the olefin-based resin particles is not particularly limited, but from the viewpoint of the dispersion stability of the olefin-based resin particles, it is preferably in the range of 10 nm or more and 300 nm or less, more preferably in the range of 20 nm or more and 250 nm or less, and even more preferably in the range of 30 nm or more and 200 nm or less.

[0070] The average particle size of the olefin resin particles is a value measured by the same method as that for the average particle size of the specific (meth)acrylic resin particles described above.

[0071] As the olefin-based resin particles, commercially available products can be used. Examples of commercially available olefin-based resin particles include "Auroren AE-301," "Auroren AE-310," "Auroren AE-502," "Auroren AE-504," "Auroren AE-511," "Superclone E-415," and "Superclone E-480T" manufactured by Nippon Paper Industries Co., Ltd. The above "Auroren" and "Superclone" are both registered trademarks.

[0072] The pressure-sensitive adhesive composition of the present disclosure may contain only one type of olefin-based resin particles, or may contain two or more types.

[0073] The content of the olefin resin particles in the pressure-sensitive adhesive composition of the present disclosure is not particularly limited. The lower limit of the content of the olefin-based resin particles in the pressure-sensitive adhesive composition of the present disclosure is, for example, preferably 5 parts by mass or more, more preferably 8 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the specific (meth)acrylic resin particles. When the content of the olefin resin particles in the pressure-sensitive adhesive composition of the present disclosure is 5 parts by mass or more per 100 parts by mass of the specific (meth)acrylic resin particles, the cohesive strength of the pressure-sensitive adhesive layer is increased, and therefore the pressure-sensitive adhesive layer tends to have better removability when immersed in salt water such as seawater. The upper limit of the content of the olefin-based resin particles in the pressure-sensitive adhesive composition of the present disclosure is, for example, preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 50 parts by mass or less, relative to 100 parts by mass of the specific (meth)acrylic resin particles. When the content of the olefin resin particles in the pressure-sensitive adhesive composition of the present disclosure is 100 parts by mass or less per 100 parts by mass of the specific (meth)acrylic resin particles, the adhesive strength of the formed pressure-sensitive adhesive layer to an adherend tends to be increased. In one embodiment, the content of the olefin resin particles in the pressure-sensitive adhesive composition of the present disclosure may be in the range of 5 parts by mass or more and 100 parts by mass or less, 8 parts by mass or more and 80 parts by mass or less, or 10 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the specific (meth)acrylic resin particles.

[0074] [Crosslinking Agent] The pressure-sensitive adhesive composition of the present disclosure contains a crosslinking agent. When the pressure-sensitive adhesive composition of the present disclosure contains a crosslinking agent, it tends to be possible to form a pressure-sensitive adhesive layer that is difficult to peel off from the adherend even when immersed in salt water such as seawater. The reason for this is believed to be that the crosslinking agent reacts with the carboxyl group derived from the structural unit (B) of the specific (meth)acrylic resin particle, thereby increasing the cohesive force of the pressure-sensitive adhesive layer formed, making it difficult for salt, water, etc. in an ionized state to enter between the pressure-sensitive adhesive layer and the adherend.

[0075] The type of crosslinking agent is not particularly limited. Examples of the crosslinking agent include a carbodiimide-based crosslinking agent, an oxazoline-based crosslinking agent, a hydrazide-based crosslinking agent, an epoxy-based crosslinking agent, and an isocyanate-based crosslinking agent.

[0076] In the present disclosure, the term "carbodiimide-based crosslinking agent" refers to a compound having two or more carbodiimide groups or cyanamide groups that are in a tautomeric relationship therewith in one molecule, the term "oxazoline-based crosslinking agent" refers to a compound having two or more oxazoline groups in one molecule, the term "hydrazide-based crosslinking agent" refers to a compound having two or more hydrazide groups in one molecule, the term "epoxy-based crosslinking agent" refers to a compound having two or more epoxy groups in one molecule, and the term "isocyanate-based crosslinking agent" refers to a compound having two or more isocyanate groups in one molecule.

[0077] The crosslinking agent is preferably at least one selected from a carbodiimide-based crosslinking agent and an oxazoline-based crosslinking agent, and more preferably a carbodiimide-based crosslinking agent.

[0078] Specific examples of carbodiimide-based crosslinking agents include aromatic polycarbodiimides such as poly(4,4'-diphenylmethanecarbodiimide), poly(p-phenylenecarbodiimide), poly(m-phenylenecarbodiimide), poly(diisopropylphenylcarbodiimide), and poly(triisopropylphenylcarbodiimide), alicyclic polycarbodiimides such as poly(dicyclohexylmethanecarbodiimide), and aliphatic polycarbodiimides such as poly(diisopropylcarbodiimide). Commercially available examples of carbodiimide crosslinking agents include "Carbodilite V-02", "Carbodilite V-02-L2", "Carbodilite SV-02", "Carbodilite V-04", "Carbodilite V-10", "Carbodilite E-02", and "Carbodilite E-05" manufactured by Nisshinbo Chemical Inc. The above "Carbodilite" is a registered trademark.

[0079] The oxazoline group contained in the oxazoline-based crosslinking agent may be any one of a 2-oxazoline group, a 3-oxazoline group, and a 4-oxazoline group. Specific examples of oxazoline-based crosslinking agents include polymer compositions containing structural units derived from compounds such as 2-vinyl-2-oxazoline, 5-methyl-2-vinyl-2-oxazoline, 4,4-dimethyl-2-vinyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 4,4-dimethyl-2-isopropenyl-2-oxazoline, 4-acryloyloxymethyl-2,4-dimethyl-2-oxazoline, 4-methacryloyloxymethyl-2,4-dimethyl-2-oxazoline, 4-methacryloyloxymethyl-2-phenyl-4-methyl-2-oxazoline, 2-(4-vinylphenyl)-4,4-dimethyl-2-oxazoline, 4-ethyl-4-hydroxymethyl-2-isopropenyl-2-oxazoline, and 4-ethyl-4-carboethoxymethyl-2-isopropenyl-2-oxazoline. Examples of commercially available oxazoline-based crosslinking agents include "Epocross WS-300," "Epocross WS-500," and "Epocross WS-700" manufactured by Nippon Shokubai Co., Ltd. The above "Epocross" is a registered trademark.

[0080] The pressure-sensitive adhesive composition of the present disclosure may contain only one type of crosslinking agent, or may contain two or more types.

[0081] The content of the crosslinking agent in the pressure-sensitive adhesive composition of the present disclosure is not particularly limited. The lower limit of the content of the crosslinking agent in the pressure-sensitive adhesive composition of the present disclosure is, for example, preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 3 parts by mass or more, relative to 100 parts by mass of the specific (meth)acrylic resin particles. The upper limit of the content of the crosslinking agent in the pressure-sensitive adhesive composition of the present disclosure is, for example, preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of the specific (meth)acrylic resin particles. In one embodiment, the content of the crosslinking agent in the pressure-sensitive adhesive composition of the present disclosure may be in the range of 0.1 parts by mass or more and 15 parts by mass or less, 1 part by mass or more and 10 parts by mass or less, 3 parts by mass or more and 10 parts by mass or less, or 3 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the specific (meth)acrylic resin particles.

[0082] [Tackifying resin particles] The pressure-sensitive adhesive composition of the present disclosure preferably further contains tackifier resin particles. When the pressure-sensitive adhesive composition of the present disclosure contains tackifier resin particles, the adhesive strength of the formed pressure-sensitive adhesive layer to an adherend tends to be higher. Also, when the pressure-sensitive adhesive composition of the present disclosure contains tackifier resin particles, the pressure-sensitive adhesive layer tends to be less likely to peel off from the adherend when immersed in salt water such as seawater.

[0083] In the present disclosure, "tackifier resin particles" refers to particles of a resin that has the property of being able to impart tackiness when blended and has a molecular weight of less than 10,000 (preferably in the range of 500 or more and less than 10,000). "Tackiness" here refers to a sticky property. The "tackifier resin" is also called a tackifier. The "tackifier resin particles" in the present disclosure do not include those that correspond to specific (meth)acrylic resin particles and olefin resin particles.

[0084] The molecular weight of the tackifier resin particles is a value measured by gel permeation chromatography (GPC). Specifically, it is a weight average molecular weight measured by GPC under the following conditions in terms of standard polystyrene.

[0085] ~Conditions~ Measurement equipment: High-speed GPC [Model: HLC-8420 GPC, manufactured by Tosoh Corporation] Detector: Differential refractometer (RI) [installed in HLC-8420, manufactured by Tosoh Corporation] Column: TSKgel GMH XL Two Tosoh products are used. Column temperature: 40℃ Eluent: Tetrahydrofuran Sample solution injection volume: 100μL Flow rate: 0.8mL / min

[0086] However, when a commercially available product is used as the tackifier resin particles and the molecular weight is described in the catalog of the commercially available product, the molecular weight of the tackifier resin particles is taken from the value in the catalog of the commercially available product.

[0087] Examples of tackifier resins include resins having a rosin skeleton (so-called rosin-based resins), resins having a terpene skeleton (so-called terpene-based resins), and resins having a styrene skeleton (so-called styrene-based resins). The tackifier resin particles are preferably particles of a rosin-based resin.

[0088] Specific examples of rosin-based resins include rosin, esterified rosin (so-called rosin ester resin), hydrogenated rosin, and disproportionated rosin. As the rosin-based resin, a rosin ester resin is preferable.

[0089] The softening point of the tackifier resin particles is not particularly limited, but from the viewpoint of easy availability of commercial products, for example, it is preferably 160°C or lower, more preferably in the range of 60°C or higher and 160°C or lower, even more preferably in the range of 80°C or higher and 160°C or lower, and particularly preferably in the range of 100°C or higher and 160°C or lower.

[0090] The softening point of the tackifier resin particles is a value measured by a method (so-called ring and ball method) in accordance with JIS K 7234: 1986. However, when a commercially available product is used as the tackifier resin particles and the softening point is described in the catalog of the commercially available product, the softening point of the tackifier resin particles is the value in the catalog of the commercially available product.

[0091] The tackifier resin particles are preferably spherical in shape.

[0092] The average particle diameter of the tackifier resin particles is not particularly limited, but from the viewpoint of commercial availability, for example, it is preferably 100 nm or more, more preferably in the range of 100 nm or more and 600 nm or less, and even more preferably in the range of 200 nm or more and 500 nm or less.

[0093] The average particle size of the tackifier resin particles is a value measured by the same method as that for measuring the average particle size of the specific (meth)acrylic resin particles.

[0094] As the tackifier resin particles, commercially available products can be used. Examples of commercially available tackifier resin particles include "YS Polystar U115", "YS Polystar U130", "YS Polystar T30", "YS Polystar T80", "YS Polystar T100", "YS Polystar T115", "YS Polystar T130", "YS Polystar TH130", "YS Polystar T145", "YS Polystar T160", "YS Polystar S145", "YS Polystar G125", "YS Polystar G150", "YS Polystar N125", "YS Polystar K125", "YS Polystar K140", "YS Resin CP", "YS Resin PX800", "YS Resin PX1000", "YS Resin PX1150", "YS Resin PX1250", "YS Resin TO85", "YS Resin TO105", "YS Resin TO115", and "YS Resin Examples of such a surfactant include "SUPERESTER A-100", "SUPERESTER E-720", "SUPERESTER E-788", "SUPERESTER E-865-NT", "SUPERESTER E-865-WR", "SUPERESTER E-900-NT", "SUPERESTER E-910-NT", "PINE CRYSTAL KE-359", "PINE CRYSTAL D-6011", "TAMANOL E-200-NT", "TAMANOL E-300-NT", "TAMANOL 803L", and "TAMANOL 901" manufactured by Arakawa Chemical Industries Co., Ltd., "HARIESTAR SK-130D" manufactured by Harima Chemical Industries Co., Ltd., and "SYLVALITE 9000" manufactured by Kraton. The above "YS Polystar," "YS Resin," "Nanolet," "Pine Crystal," "Tamanol," "Harriester," and "SYLVALITE" are all registered trademarks.

[0095] When the PSA composition of the present disclosure contains tackifier resin particles, it may contain only one type of tackifier resin particles, or may contain two or more types of tackifier resin particles.

[0096] When the pressure-sensitive adhesive composition of the present disclosure contains tackifier resin particles, the content of the tackifier resin particles is not particularly limited, but is, for example, preferably in the range of 10 parts by mass or more and 100 parts by mass or less, more preferably in the range of 20 parts by mass or more and 80 parts by mass or less, and even more preferably in the range of 30 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the specific (meth)acrylic resin particles.

[0097] 〔water〕 The pressure-sensitive adhesive composition of the present disclosure contains water. The water is not particularly limited, but from the viewpoint of having fewer impurities, for example, distilled water, ion-exchanged water, pure water, and the like are preferable.

[0098] The water content in the pressure-sensitive adhesive composition of the present disclosure is not particularly limited, but is, for example, preferably 40% by mass to 80% by mass, and more preferably 40% by mass to 70% by mass, relative to the total mass of the pressure-sensitive adhesive composition.

[0099] [Aqueous media other than water] The pressure-sensitive adhesive composition of the present disclosure may contain an aqueous medium other than water. Examples of aqueous media other than water include water-miscible organic solvents. Examples of water-miscible organic solvents include monohydric alcohol compounds such as methanol, ethanol, propanol, and isopropanol; polyhydric alcohol compounds such as glycerin, ethylene glycol, diethylene glycol, and propylene glycol; and glycol derivatives such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monobutyl ether, and dipropylene glycol monomethyl ether.

[0100] When the pressure-sensitive adhesive composition of the present disclosure contains an aqueous medium other than water, it may contain only one type of aqueous medium other than water, or may contain two or more types of aqueous medium other than water.

[0101] When the pressure-sensitive adhesive composition of the present disclosure contains an aqueous medium other than water, the content of the aqueous medium other than water can be appropriately set depending on the purpose, as long as the effects of the pressure-sensitive adhesive composition of the present disclosure are not impaired.

[0102] [Water-immiscible organic solvent] The pressure-sensitive adhesive composition of the present disclosure preferably does not contain a water-immiscible organic solvent or the content of the water-immiscible organic solvent is in the range of more than 0 mass% to not more than 5 mass% relative to the total mass of the pressure-sensitive adhesive composition, more preferably does not contain a water-immiscible organic solvent or the content of the water-immiscible organic solvent is in the range of more than 0 mass% to not more than 3 mass% relative to the total mass of the pressure-sensitive adhesive composition, even more preferably does not contain a water-immiscible organic solvent or the content of the water-immiscible organic solvent is in the range of more than 0 mass% to not more than 1 mass% relative to the total mass of the pressure-sensitive adhesive composition, and particularly preferably does not contain a water-immiscible organic solvent or the content of the water-immiscible organic solvent is in the range of more than 0 mass% to not more than 0.5 mass% relative to the total mass of the pressure-sensitive adhesive composition.

[0103] Examples of water-immiscible organic solvents include aromatic hydrocarbon compounds such as benzene, toluene, and xylene; ether compounds such as diethyl ether and diisopropyl ether; aliphatic hydrocarbon compounds such as hexane and heptane; halogenated hydrocarbon compounds such as dichloroethane and chloroform; ester compounds such as ethyl acetate and butyl acetate; alcohol compounds such as octanol; and ketone compounds such as methyl isobutyl ketone.

[0104] [Other ingredients] The pressure-sensitive adhesive composition of the present disclosure may contain components other than the components described above (so-called other components) as necessary, provided that the effects of the composition are not impaired. Examples of other components include specific (meth)acrylic resin particles, olefin resin particles, and resin particles other than tackifying resin particles, as well as various additives such as antioxidants, antistatic agents, conductivity imparting agents, pH adjusters, defoamers, wetting agents, thickeners, fillers, pigments, and plasticizers.

[0105] <<pH of adhesive composition>> The pH of the pressure-sensitive adhesive composition of the present disclosure is preferably 2 to 10, and more preferably 6 to 9, from the viewpoint of dispersibility of the specific (meth)acrylic resin particles and olefin resin particles in the pressure-sensitive adhesive composition. The method for measuring the pH of the pressure-sensitive adhesive composition of the present disclosure is not particularly limited. The pH of the pressure-sensitive adhesive composition of the present disclosure is measured using a pH meter in accordance with a method in accordance with JIS Z 8802:2011 at a liquid temperature of 25° C. The measurement device may be, for example, a pH meter (product name: F-51) manufactured by Horiba, Ltd. However, the measurement device is not limited thereto.

[0106] [Application] The application of the pressure-sensitive adhesive composition of the present disclosure is not particularly limited. The pressure-sensitive adhesive composition of the present disclosure has high adhesive strength to an adherend, is difficult to peel off from an adherend even when immersed in salt water such as seawater, and is capable of forming an adhesive layer with excellent removability. Therefore, the pressure-sensitive adhesive composition is suitable for applications such as attaching labels to cargo and its containers (e.g., drums and containers) that may be transported by sea by ship. Containers such as drums and containers are often reused, and labels need to be replaced. In general, synthetic paper containing olefin resin (e.g., Yupo Paper (registered trademark)) is used for labels used on cargo and its containers that are transported by sea so that the labels can withstand sea spray and the like. However, synthetic paper labels containing olefin resin have low polarity, and therefore tend to have low adhesion to acrylic adhesives and to easily leave adhesive residue on the adherend when peeled off from the adherend. In contrast, the adhesive composition of the present disclosure has excellent adhesion to substrates made of low polarity materials, and can form an adhesive layer that is unlikely to leave adhesive residue on the adherend when peeled off from the adherend, making it suitable for applications in which labels are attached to cargo and its containers that may be transported by sea by ship.

[0107] The pressure-sensitive adhesive composition of the present disclosure can be preferably used for both low-polarity and high-polarity materials. Specific examples of low polarity materials include resins such as polyolefins (eg, polyethylene (PE) and polypropylene (PP)) and polystyrene. Specific examples of highly polar materials include metals such as stainless steel (SUS), aluminum, and copper, resins such as acrylic resin and polycarbonate (PC), and glass.

[0108] [Method for producing pressure-sensitive adhesive composition] The method for producing the pressure-sensitive adhesive composition of the present disclosure is not particularly limited as long as the pressure-sensitive adhesive composition of the present disclosure can be produced. For example, the pressure-sensitive adhesive composition of the present disclosure is preferably produced by a method including a step of producing specific (meth)acrylic resin particles by emulsion polymerization.

[0109] Examples of emulsion polymerization methods for producing the specific (meth)acrylic resin particles include the following methods [1] to [3]. Hereinafter, the monomers forming the structural units of the specific (meth)acrylic resin particles [at least the (meth)acrylic acid alkyl ester monomer and the monomer having a carboxy group] are also referred to as "monomer components".

[0110] [1] A method in which a monomer component, a reactive surfactant and / or a non-reactive surfactant, and water are charged into a reactor equipped with a thermometer, a stirrer, a raw material inlet pipe, a reflux condenser, a nitrogen inlet pipe, etc., and the temperature is raised while stirring under a nitrogen stream, and then a polymerization initiator, a reducing agent, etc. are appropriately added to allow the emulsion polymerization reaction to proceed (the so-called lump-sum charging method). [2] A method in which at least a reactive surfactant and / or a non-reactive surfactant and water are charged into a reactor equipped with a thermometer, a stirrer, a raw material introduction tube, a reflux condenser, a nitrogen introduction tube, etc., and the temperature is raised while stirring under a nitrogen stream, and then a monomer component is dropped, and a polymerization initiator, a reducing agent, etc. are appropriately added to proceed with the emulsion polymerization reaction (the so-called monomer dropping method). [3] A reactive surfactant and / or a non-reactive surfactant and water are charged into a reactor equipped with a thermometer, a stirrer, a raw material introduction pipe, a reflux condenser, a nitrogen introduction pipe, etc., and the temperature is raised while stirring under a nitrogen stream, and then a polymerization initiator, a reducing agent, etc. are added as appropriate. Meanwhile, in a separate vessel, a monomer component is emulsified in advance using at least a reactive surfactant and / or a non-reactive surfactant and water to prepare an emulsion of a mixture containing the monomer component and the reactive surfactant and / or the non-reactive surfactant. Next, the emulsion of the mixture containing the monomer component and the reactive surfactant and / or the non-reactive surfactant is dropped into the reactor, and a polymerization initiator, a reducing agent, etc. are added as appropriate to proceed with the emulsion polymerization reaction (so-called emulsion monomer dropping method). Among these, as the emulsion polymerization method for producing the specific (meth)acrylic resin particles, the above-mentioned emulsion monomer dropping method [3] is preferred from the viewpoint of industrial productivity, for example.

[0111] The method for producing the pressure-sensitive adhesive composition of the present disclosure preferably includes a step of producing (meth)acrylic resin particles by emulsion polymerization of at least a (meth)acrylic acid alkyl ester monomer, a monomer having a carboxy group, and a reactive surfactant using a chain transfer agent. The use of a chain transfer agent inhibits entanglement of the monomer components forming the (meth)acrylic resin particles, thereby imparting flexibility to the pressure-sensitive adhesive layer that is formed, which makes it easier for the pressure-sensitive adhesive layer to wet and spread over the adherend when pressure-sensitive, and tends to further increase the adhesive strength of the pressure-sensitive adhesive layer to the adherend.

[0112] For example, when the emulsion monomer dropping method described above in [3] is adopted as the emulsion polymerization method for producing the specific (meth)acrylic resin particles, the following operations are carried out. Water and a reactive surfactant are charged into a reactor equipped with a thermometer, a stirrer, a raw material introduction tube, a reflux condenser, a nitrogen introduction tube, etc., and the temperature is raised while stirring under a nitrogen stream, and then a polymerization initiator, a reducing agent, etc. are appropriately added. Meanwhile, in a separate vessel, a monomer component is emulsified in advance using at least a reactive surfactant, a chain transfer agent, and water to prepare an emulsion of a mixture containing the monomer component and the reactive surfactant. Next, the emulsion of the mixture containing the monomer component and the reactive surfactant is dropped into the reactor, and a polymerization initiator, a reducing agent, etc. are appropriately added to proceed with the emulsion polymerization reaction.

[0113] The specific (meth)acrylic resin particles obtained by the above emulsion polymerization method are obtained in the state of a dispersion in which the particles are dispersed in a medium containing at least water.

[0114] The details of the (meth)acrylic acid alkyl ester monomer are as described above. The amount of the (meth)acrylic acid alkyl ester monomer used is not particularly limited, but for example, relative to 100 parts by mass of the total of the monomer components, is preferably in the range of 50.0 parts by mass or more and 99.99 parts by mass or less, more preferably in the range of 60.0 parts by mass or more and 99.95 parts by mass or less, even more preferably in the range of 70.0 parts by mass or more and 99.95 parts by mass or less, and particularly preferably in the range of 80.0 parts by mass or more and 99.95 parts by mass or less.

[0115] The details of the monomer having a carboxy group are as described above. The amount of the monomer having a carboxy group used is preferably in the range of 0.01 parts by mass or more and 2.0 parts by mass or less per 100 parts by mass of the total of the monomer components. The lower limit of the amount of the monomer having a carboxy group to be used is more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, based on 100 parts by mass of the total of the monomer components. The upper limit of the amount of the monomer having a carboxy group to be used is more preferably 1.8 parts by mass or less, and even more preferably 1.5 parts by mass or less, based on 100 parts by mass of the total of the monomer components.

[0116] In the method for producing a pressure-sensitive adhesive composition of the present disclosure, as the surfactant, only a reactive surfactant may be used, only a non-reactive surfactant may be used, or both a reactive surfactant and a non-reactive surfactant may be used.

[0117] The details of the reactive surfactant are as described above. In the method for producing a pressure-sensitive adhesive composition of the present disclosure, when a reactive surfactant is used, only one type of reactive surfactant may be used, or two or more types may be used. When a reactive surfactant is used in the method for producing a pressure-sensitive adhesive composition of the present disclosure, the amount of the reactive surfactant used is not particularly limited. When a reactive surfactant is used, the lower limit of the amount of the reactive surfactant used is, for example, preferably 0.5 parts by mass or more, and more preferably 1.0 part by mass or more, per 100 parts by mass of the total of the monomer components. When a reactive surfactant is used, the upper limit of the amount of the reactive surfactant used is, for example, preferably 2.5 parts by mass or less, and more preferably 2.0 parts by mass or less, per 100 parts by mass of the total of the monomer components.

[0118] In this disclosure, "non-reactive surfactant" refers to a surfactant that does not have an ethylenically unsaturated double bond. The type of the non-reactive surfactant is not particularly limited. The non-reactive surfactant is preferably at least one selected from an anionic non-reactive surfactant and a non-ionic non-reactive surfactant, and more preferably a non-ionic non-reactive surfactant.

[0119] Examples of anionic non-reactive surfactants include polyoxyalkylene polycyclic phenyl ether sulfate salts, such as polyoxyethylene distyrenated phenyl ether ammonium sulfate, polyoxyalkylene polycyclic phenyl ether sulfate salts, such as polyoxyethylene distyrenated phenyl ether ammonium sulfate, polyoxyalkylene alkyl phenyl ether sulfate salts, such as polyoxyethylene nonyl phenyl ether sodium sulfate, polyoxyalkylene alkyl ether sulfate salts, such as polyoxyethylene lauryl ether sodium sulfate, polyoxyalkylene alkyl ether sulfate salts, polyoxyalkylene alkyl ether sulfate salts, and alkyl phosphate salts. Examples of nonionic nonreactive surfactants include polyoxyalkylene alkyl ethers such as polyoxyethylene oleyl ether and polyoxyethylene lauryl ether, and polyoxyalkylene styrenated phenyl ethers such as polyoxyethylene styrenated phenyl ether.

[0120] As the non-reactive surfactant, commercially available products can be used. Examples of commercially available anionic non-reactive surfactants include "Hitenol (registered trademark) NF-13" and "Hitenol (registered trademark) NF-17" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., and "Newcol (registered trademark) 707-SF" manufactured by Nippon Nyukazai Co., Ltd. An example of a commercially available nonionic nonreactive surfactant is "Noigen (registered trademark) DKS NL-600F" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.

[0121] In the method for producing a pressure-sensitive adhesive composition of the present disclosure, when a non-reactive surfactant is used, only one type of non-reactive surfactant may be used, or two or more types of non-reactive surfactants may be used.

[0122] When a non-reactive surfactant is used in the method for producing a pressure-sensitive adhesive composition of the present disclosure, the amount of the non-reactive surfactant used is not particularly limited. When a non-reactive surfactant is used, the lower limit of the amount of the non-reactive surfactant used is, for example, preferably 0.5 parts by mass or more, and more preferably 1.0 part by mass or more, per 100 parts by mass of the total of the monomer components. When a non-reactive surfactant is used, the upper limit of the amount of the non-reactive surfactant used is, for example, preferably 2.5 parts by mass or less, and more preferably 2.0 parts by mass or less, per 100 parts by mass of the total of the monomer components.

[0123] The total amount of the reactive surfactant and the non-reactive surfactant used is not particularly limited. The lower limit of the total amount of the reactive surfactant and the non-reactive surfactant used is, for example, preferably 0.5 parts by mass or more, and more preferably 1.0 part by mass or more, per 100 parts by mass of the total of the monomer components. The upper limit of the total amount of the reactive surfactant and the non-reactive surfactant used is, for example, preferably 2.5 parts by mass or less, and more preferably 2.0 parts by mass or less, per 100 parts by mass of the total of the monomer components.

[0124] The chain transfer agent is not particularly limited as long as it can be used in ordinary emulsion polymerization. Examples of the chain transfer agent include cyanoacetic acid, alkyl ester compounds of cyanoacetic acid having 1 to 8 carbon atoms, bromoacetic acid, alkyl ester compounds of bromoacetic acid having 1 to 8 carbon atoms, aromatic compounds such as α-methylstyrene, anthracene, phenanthrene, fluorene, and 9-phenylfluorene, aromatic nitro compounds such as p-nitroaniline, nitrobenzene, dinitrobenzene, p-nitrobenzoic acid, p-nitrophenol, and p-nitrotoluene, benzoquinone derivatives such as benzoquinone and 2,3,5,6-tetramethyl-p-benzoquinone, borane derivatives such as tributylborane, carbon tetrabromide, ... Examples of the halogenated hydrocarbon compounds include carbon chloride, 1,1,2,2-tetrabromoethane, tribromoethylene, trichloroethylene, bromotrichloromethane, tribromomethane, and 3-chloro-1-propene, aldehyde compounds such as chloral and furaldehyde, alkyl mercaptan compounds having 1 to 18 carbon atoms, aromatic mercaptan compounds such as thiophenol and toluene mercaptan, mercaptoacetic acid, alkyl ester compounds of mercaptoacetic acid having 1 to 10 carbon atoms, hydroxyalkyl mercaptan compounds having 1 to 12 carbon atoms, and terpene compounds such as pinene and terpinolene.

[0125] In the emulsion polymerization method for producing the specific (meth)acrylic resin particles, when a chain transfer agent is used, only one type of chain transfer agent may be used, or two or more types of chain transfer agents may be used.

[0126] The chain transfer agent is used in an amount conventionally used. The amount of the chain transfer agent used is preferably, for example, 0.01 to 0.05 parts by mass per 100 parts by mass of the total of the monomer components.

[0127] The polymerization initiator is not particularly limited as long as it can be used in ordinary emulsion polymerization. Examples of the polymerization initiator include persulfates, organic peroxides, and azo compounds. Specific examples of persulfates include ammonium persulfate, sodium persulfate, and potassium persulfate. Specific examples of organic peroxides include t-butyl hydroperoxide, benzoyl peroxide, lauroyl peroxide, caproyl peroxide, di-i-propyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, and t-butyl peroxypivalate. Specific examples of azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), and 2,2'-azobis(isobutyrate) dimethyl.

[0128] In the emulsion polymerization method for producing the specific (meth)acrylic resin particles, only one type of polymerization initiator may be used, or two or more types may be used.

[0129] The polymerization initiator is used in an amount usually used. The amount of the polymerization initiator used is preferably, for example, 0.2 parts by mass to 5.0 parts by mass per 100 parts by mass of the total of the monomer components.

[0130] The reducing agent is not particularly limited as long as it can be used in ordinary emulsion polymerization. Examples of reducing agents include sodium metabisulfite, sodium sulfite, sodium hydrogensulfite, sodium pyrosulfite (also called "sodium disulfite"), sodium hydroxymethanesulfinate, sodium pyrophosphate, thioglycolic acid, sodium thiosulfate, thiourea dioxide, L-ascorbic acid, tartaric acid, citric acid, and glucose.

[0131] In the emulsion polymerization method for producing the specific (meth)acrylic resin particles, only one type of reducing agent may be used, or two or more types of reducing agents may be used.

[0132] The reducing agent is used in an amount normally used. The amount of the reducing agent used is preferably, for example, 0.2 to 5.0 parts by mass per 100 parts by mass of the total of the monomer components.

[0133] The polymerization temperature is preferably, for example, 50°C to 90°C. The polymerization time is preferably, for example, 1 hour to 5 hours.

[0134] The method for producing a pressure-sensitive adhesive composition of the present disclosure preferably includes a step of adjusting the pH of the dispersion liquid containing the specific (meth)acrylic resin particles obtained above. The pH of the dispersion liquid containing the specific (meth)acrylic resin particles is preferably adjusted to 2 to 10, and more preferably 5 to 9, from the viewpoint of dispersibility of the specific (meth)acrylic resin particles in the pressure-sensitive adhesive composition. The method for adjusting the pH of the dispersion liquid containing the specific (meth)acrylic resin particles is not particularly limited, and examples thereof include a method using a pH adjuster. As the pH adjuster, for example, ammonia water can be suitably used.

[0135] The pH of the dispersion liquid containing the specific (meth)acrylic resin particles is measured using a pH meter in accordance with a method conforming to JIS Z 8802:2011 at a liquid temperature of 25° C. The measurement device may be, for example, a pH meter (product name: F-51) manufactured by Horiba, Ltd. However, the measurement device is not limited to this.

[0136] In the above, emulsion polymerization has been given as an example of a method for producing the specific (meth)acrylic resin particles. However, the method for producing the specific (meth)acrylic resin particles in the present disclosure is not limited to the above-mentioned emulsion polymerization, and for example, a seed polymerization method can also be used.

[0137] The method for producing the pressure-sensitive adhesive composition of the present disclosure preferably includes a step of mixing the dispersion containing the specific (meth)acrylic resin particles obtained above, olefin resin particles, and a crosslinking agent.

[0138] The details of the olefin-based resin particles are as described above. The amount of the olefin resin particles used is not particularly limited, but is preferably in the range of 5 parts by mass or more and 100 parts by mass or less per 100 parts by mass of the specific (meth)acrylic resin particles. The lower limit of the amount of the olefin-based resin particles used is more preferably 8 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the specific (meth)acrylic resin particles.The upper limit of the amount of the olefin-based resin particles used is more preferably 80 parts by mass or less, and even more preferably 50 parts by mass or less, relative to 100 parts by mass of the specific (meth)acrylic resin particles.

[0139] [Adhesive sheet] The pressure-sensitive adhesive sheet of the present disclosure includes a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition of the present disclosure. The pressure-sensitive adhesive sheet of the present disclosure has a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition of the present disclosure, and therefore has high adhesion to an adherend, is difficult to peel off from the adherend even when immersed in salt water such as seawater, and has excellent removability. Therefore, the pressure-sensitive adhesive sheet of the present disclosure is suitable as a label to be attached to cargo and its container (e.g., drums and containers) that may be transported by sea by ship.

[0140] The thickness of the pressure-sensitive adhesive layer provided in the pressure-sensitive adhesive sheet of the present disclosure is not particularly limited. The thickness of the pressure-sensitive adhesive layer is generally from 1 μm to 300 μm, preferably from 5 μm to 200 μm, and more preferably from 10 μm to 100 μm.

[0141] In the present disclosure, the "thickness of the pressure-sensitive adhesive layer" means the average thickness of the pressure-sensitive adhesive layer. The average thickness of the pressure-sensitive adhesive layer is a value determined by the following method. The thickness of the adhesive layer is measured at 10 randomly selected locations in the thickness direction using a thickness gauge. The arithmetic mean of the measured values ​​is calculated and this value is regarded as the average thickness of the adhesive layer.

[0142] The pressure-sensitive adhesive sheet of the present disclosure may be a substrate-free pressure-sensitive adhesive sheet that does not have a substrate, or a substrate-containing pressure-sensitive adhesive sheet that has a pressure-sensitive adhesive layer on one or both sides of a substrate. When the pressure-sensitive adhesive sheet of the present disclosure is a substrate-free type pressure-sensitive adhesive sheet that does not have a substrate, or when it is a substrate-containing type pressure-sensitive adhesive sheet that has a pressure-sensitive adhesive layer on one side of a substrate, the exposed surface of the pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet of the present disclosure may be protected by a release sheet. In general, the release sheet protects the surface of the pressure-sensitive adhesive layer until the pressure-sensitive adhesive sheet is put to practical use, and is peeled off at the time of use.

[0143] The release sheet is not particularly limited as long as it can be easily peeled off from the pressure-sensitive adhesive layer. Examples of release sheets include resin films, paper, synthetic paper, one or both sides of which have been surface-treated with a release agent (so-called easy-release treatment), and composite sheets obtained by laminating two or more of these. In the present disclosure, a release sheet in an embodiment in which one or both sides of a resin film have been surface-treated with a release treating agent (so-called easy-release treatment) is also referred to as a "release film". Examples of the release agent include silicone-based release agents (eg, silicone), wax-based release agents (eg, paraffin wax), and fluorine-based release agents (eg, fluorine-based resins). An example of the resin film is a polyester film, typically a polyethylene terephthalate (PET) film. Examples of the paper include fine paper and coated paper. The thickness of the release sheet is not particularly limited, and is generally 20 μm to 180 μm.

[0144] When the pressure-sensitive adhesive sheet of the present disclosure includes a substrate, the substrate is not particularly limited as long as a pressure-sensitive adhesive layer can be formed thereon. Examples of the substrate include films containing resins such as polyolefins (e.g., polyethylene (PE) and polypropylene (PP)), polyesters (e.g., polyethylene terephthalate (PET)), acetate resins (e.g., triacetyl cellulose), polyethersulfone, polycarbonate (PC), polyamide (PA), polyimide (PI), polyurethane, acrylic resins, polyvinyl chloride (PVC), acrylonitrile / butadiene / styrene resins (ABS resins), and fluororesins, paper (e.g., wood-free paper and coated paper), and synthetic paper (e.g., Yupo Paper (registered trademark)). Examples of the substrate include composite sheets in which two or more of these are laminated. The pressure-sensitive adhesive sheet of the present disclosure, even when provided with a substrate containing a low-polarity resin such as polyolefin, has excellent adhesion between the substrate and the pressure-sensitive adhesive layer, and even when immersed in salt water such as seawater and then peeled from the adherend, is less likely to leave adhesive residue on the adherend and tends to have excellent removability.

[0145] The surface of the substrate on which the adhesive layer is provided may be subjected to a surface treatment such as corona discharge treatment or plasma discharge treatment (so-called adhesion enhancing treatment) in order to improve adhesion between the substrate and the adhesive layer.

[0146] The substrate may contain various additives, such as plasticizers, colorants (eg, dyes and pigments), heat stabilizers, light stabilizers, antistatic agents, flame retardants, antioxidants, fillers, and the like. The substrate may be partially or entirely patterned.

[0147] The thickness of the substrate is not particularly limited, but is, for example, preferably 5 μm to 500 μm, more preferably 10 μm to 400 μm, further preferably 10 μm to 300 μm, and particularly preferably 10 μm to 200 μm.

[0148] "Substrate thickness" in this disclosure means the average thickness of the substrate. The average thickness of the substrate is a value determined by the following method. The thickness of the substrate is measured at 10 randomly selected locations in the thickness direction using a film thickness meter. The arithmetic mean of the measured values ​​is calculated and this value is regarded as the average thickness of the substrate.

[0149] [Method of producing adhesive sheet] The method for producing the pressure-sensitive adhesive sheet of the present disclosure is not particularly limited. The pressure-sensitive adhesive sheet of the present disclosure can be produced by known methods. The pressure-sensitive adhesive sheet of the present disclosure can be produced, for example, by the following method.

[0150] When the adhesive sheet of the present disclosure is a substrate-free type adhesive sheet, first, the adhesive composition of the present disclosure is applied to the easy-release treated surface of the release sheet to form a coating film on the release sheet.Then, the formed coating film is dried to form an adhesive film on the release sheet.Then, the exposed surface of the formed adhesive film is laminated and attached to the easy-release treated surface of a separately prepared release sheet, and then cured to produce the adhesive sheet of the present disclosure having a laminated structure of release sheet / adhesive layer / release sheet.

[0151] When the adhesive sheet of the present disclosure is a substrate-type adhesive sheet, first, the adhesive composition of the present disclosure is applied to the easy-adhesion-treated surface of the substrate to form a coating film on the substrate. Then, the formed coating film is dried to form an adhesive film on the substrate. Then, the exposed surface of the formed adhesive film is laminated on the easy-release-treated surface of the release sheet, and the laminate is cured to produce the adhesive sheet of the present disclosure having a laminated structure of substrate / adhesive layer / release sheet.

[0152] When the pressure-sensitive adhesive sheet of the present disclosure is a substrate-type pressure-sensitive adhesive sheet, another method may be, for example, the following method. The pressure-sensitive adhesive composition of the present disclosure is applied to the easy-release treated surface of a release sheet to form a coating film on the release sheet. The formed coating film is then dried to form an adhesive film on the release sheet. The exposed surface of the formed adhesive film is then laminated onto the easy-adhesion treated surface of the substrate, and cured to produce the pressure-sensitive adhesive sheet of the present disclosure having a laminated structure of substrate / adhesive layer / release sheet.

[0153] The method for applying the pressure-sensitive adhesive composition is not particularly limited. Examples of methods for applying the pressure-sensitive adhesive composition include known methods using a gravure roll coater, reverse roll coater, kiss roll coater, dip roll coater, knife coater, spray coater, bar coater, applicator, and the like. The amount of the adhesive composition to be applied is not particularly limited, and is appropriately set depending on, for example, the thickness of the adhesive layer to be formed.

[0154] The method for drying the coating film is not particularly limited. Examples of methods for drying the coating film include natural drying, heat drying, hot air drying, and vacuum drying. The drying temperature and drying time of the coating film are not particularly limited, and are appropriately set depending on the thickness of the coating film, the amount of water contained in the coating film, and the like. An example of the drying conditions is drying using a hot air circulation dryer at 70° C. to 120° C. for 30 to 180 seconds.

[0155] As a method for curing, for example, a method of leaving the product to stand for 2 to 7 days in an environment with an atmospheric temperature of 20° C. to 35° C. and a relative humidity of 45% to 55% can be mentioned. EXAMPLES

[0156] The pressure-sensitive adhesive composition, pressure-sensitive adhesive layer, and pressure-sensitive adhesive sheet of the present disclosure will be described in more detail below with reference to examples. The present disclosure is not limited to the following examples as long as they do not depart from the gist of the disclosure.

[0157] [Production of (meth)acrylic resin particles] [Manufacturing example A-3] A monomer mixture was prepared by mixing 79.0 parts by mass (316.0 g) of n-butyl acrylate (n-BA) [acrylic acid alkyl ester monomer], 20.0 parts by mass (80.0 g) of methyl methacrylate (MMA) [acrylic acid alkyl ester monomer], and 1.0 part by mass (4.0 g) of acrylic acid (AA) [monomer having a carboxy group]. To the prepared monomer mixture, 0.32 parts by mass [equivalent to active ingredient] (1.26 g) of AQUALON (registered trademark) AR-10 (trade name, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), 0.50 parts by mass [equivalent to active ingredient] (3.0 g) of ADEKA REASOAP (registered trademark) ER-30 (trade name, manufactured by ADEKA Corporation), 0.025 parts by mass (0.10 g) of n-dodecyl mercaptan (chain transfer agent), and 77.8 parts by mass (311.7 g) of ion-exchanged water were added and stirred, thereby preparing an emulsion X of a mixture containing the monomer components and the reactive surfactants. Next, 33.1 parts by mass (132.7 g) of ion-exchanged water and 0.18 parts by mass (effective ingredient equivalent) (0.72 g) of Aqualon (registered trademark) AR-10 (trade name, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), an anionic reactive surfactant, were charged into a reactor equipped with a thermometer, a stirrer, a successive dropping device, a reflux condenser and a nitrogen inlet tube, and nitrogen was sealed in, after which the internal temperature was raised to 80° C. While maintaining the internal temperature of the reactor at 80° C., 0.10 parts by mass (solid content equivalent) (10.1 g) of a 4% by mass concentration ammonium persulfate aqueous solution (polymerization initiator) and 0.10 parts by mass (solid content equivalent) (10.1 g) of a 4% by mass concentration sodium pyrosulfite aqueous solution (reducing agent) were added, and immediately, the emulsion X prepared above was continuously dropped for 3 hours to perform emulsion polymerization. In parallel with this operation, 0.56 parts by mass [solid content equivalent] (56.9 g) of 4% by mass concentration ammonium persulfate aqueous solution [polymerization initiator] and 0.56 parts by mass [solid content equivalent] (56.9 g) of 4% by mass concentration sodium pyrosulfite aqueous solution [reducing agent] were dropped into the reactor. After the dropwise addition, 0.07 parts by mass [active ingredient equivalent] (4.1 g) of 6.9% by mass concentration t-butyl hydroperoxide aqueous solution [polymerization initiator] and 0.07 parts by mass [active ingredient equivalent] (4.1 g) of 6.9% by mass concentration Techlite [trade name, active ingredient: thiourea dioxide, active ingredient concentration: 100% by mass, manufactured by ADEKA Corporation, reducing agent] were added to the obtained emulsion polymer, and the mixture was aged at 80°C for 2 hours and then cooled to room temperature. After cooling, ammonia water was added to adjust the pH to a range of 5 to 9. After adjusting the pH, ion-exchanged water was added to adjust the concentration, thereby obtaining an aqueous dispersion of (meth)acrylic resin particles A-3. The resulting aqueous dispersion of (meth)acrylic resin particles A-3 had a solid content concentration of 45.5% by mass and a pH of 8.2.

[0158] The term "solid content" used herein means the mass ratio of the (meth)acrylic resin particles A-3 to the aqueous dispersion of the (meth)acrylic resin particles A-3. The same applies to the aqueous dispersions of the (meth)acrylic resin particles A-1, A-2, and A-4 to A-17 produced below.

[0159] [Production Examples A-1, A-2, A-4 to A-6, A-10 to A-14 and A-16] In Production Examples A-1, A-2, A-4 to A-6, A-10 to A-14, and A-16, the composition of the (meth)acrylic resin particles was changed to the composition shown in Table 1, but the same operation as in Production Example A-3 was performed to obtain aqueous dispersions of (meth)acrylic resin particles A-1, A-2, A-4 to A-6, A-10 to A-14, and A-16. Each of the obtained aqueous dispersions of (meth)acrylic resin particles A-1, A-2, A-4 to A-6, A-10 to A-14, and A-16 had a solid content concentration of 45.5% by mass and a pH of 8.2.

[0160] [Production Examples A-7 and A-8] In Production Examples A-7 and A-8, the same operations as in Production Example A-3 were carried out except that the ratio between the amount of reactive surfactant used in preparing emulsion X and the amount of reactive surfactant charged in the reactor, the stirring speed, etc. were appropriately changed to obtain aqueous dispersions of (meth)acrylic resin particles A-7 and A-8. The resulting aqueous dispersions of (meth)acrylic resin particles A-7 and A-8 each had a solid content concentration of 45.5% by mass and a pH of 8.2.

[0161] [Manufacturing example A-9] In Production Example A-9, the composition of the (meth)acrylic resin particles was changed to the composition shown in Table 1, and a non-reactive surfactant shown in Table 1 was used. The same procedure as in Production Example A-3 was carried out to obtain an aqueous dispersion of (meth)acrylic resin particles A-9. The resulting aqueous dispersion of (meth)acrylic resin particles A-9 had a solid content concentration of 45.5% by mass and a pH of 8.2.

[0162] [Manufacturing example A-15] In Production Example A-15, the composition of the (meth)acrylic resin particles was changed to the composition shown in Table 1, and the ratio of the amount of the reactive surfactant used to prepare the emulsion X to the amount of the reactive surfactant charged in the reactor, the stirring speed, etc. were appropriately changed. The same operation as in Production Example A-3 was performed to obtain an aqueous dispersion of (meth)acrylic resin particles A-15. The resulting aqueous dispersion of (meth)acrylic resin particles A-15 had a solid content concentration of 45.5% by mass and a pH of 8.2.

[0163] [Manufacturing example A-17] In Production Example A-17, the same procedure as in Production Example A-3 was carried out except that a non-reactive surfactant was used instead of a reactive surfactant as shown in Table 1, to obtain an aqueous dispersion of (meth)acrylic resin particles A-17. The resulting aqueous dispersion of (meth)acrylic resin particles A-17 had a solid content concentration of 45.5% by mass and a pH of 8.2.

[0164] The pH of each of the aqueous dispersions of the (meth)acrylic resin particles A-1 to A-17 was measured at a liquid temperature of 25° C. using a pH meter (product name: F-51) manufactured by Horiba, Ltd., in accordance with a method in accordance with JIS Z 8802:2011.

[0165] Table 1 shows the composition (unit: parts by mass) of the (meth)acrylic resin particles A-1 to A-17, the glass transition temperature (Tg, unit: ° C.) of the (meth)acrylic resin particles A-1 to A-17, and the average particle size (unit: nm) of the (meth)acrylic resin particles A-1 to A-17. When a non-reactive surfactant was used in the production of the (meth)acrylic resin particles, the type and amount of the non-reactive surfactant used are also shown in Table 1.

[0166] The glass transition temperatures of the (meth)acrylic resin particles A-1 to A-17 were measured by the same method as that for the specific (meth)acrylic resin particles described above, using a Discovery DSC 2500 (trade name) manufactured by TA Instruments Japan, Inc.

[0167] The average particle size of the (meth)acrylic resin particles A-1 to A-17 was measured by the same method as the above-mentioned method for measuring the average particle size of the specific (meth)acrylic resin particles. The measurement device used was Zetasizer 1000HS (product name) manufactured by Sysmex Corporation.

[0168] Of the (meth)acrylic resin particles A-1 to A-17 obtained above, the (meth)acrylic resin particles A-2 to A-4 and A-6 to A-17 correspond to the specific (meth)acrylic resin particles in the present disclosure.

[0169] [Table 1]

[0170] Details of the monomer components and reactive surfactants listed in Table 1 are as follows. For convenience, in Table 1, components corresponding to "(meth)acrylic acid alkyl ester monomer" are classified as "(A)", components corresponding to "monomer having a carboxy group" are classified as "(B)", other monomer components are classified as "others", and components corresponding to "reactive surfactant" are classified as "(C)".

[0171] The amounts of reactive surfactant and non-reactive surfactant shown in Table 1 are all calculated as active ingredients.

[0172] <(Meth)acrylic acid alkyl ester monomer> "n-BA": n-butyl acrylate "2EHA": 2-Ethylhexyl acrylate "MMA": Methyl methacrylate <Monomers having a carboxy group> "AA": acrylic acid "MAA": methacrylic acid <Other monomers> "AN": acrylonitrile

[0173] <Reactive surfactant> -Anionic reactive surfactant- "AR-10" [Product name: Aqualon (registered trademark) AR-10, active ingredient: polyoxyethylene styrenated propenyl phenyl ether sulfate ammonium [type of oxyalkylene group: oxyethylene group, average number of moles added: 10], active ingredient concentration: 99% by mass, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.] -Nonionic reactive surfactant- "ER-30" [Product name: ADEKA REASOAP (registered trademark) ER-30, active ingredient: polyoxyethylene-1-(allyloxymethyl) alkyl ether [type of oxyalkylene group: oxyethylene group, average number of moles added: 30], active ingredient concentration: 65% by mass, manufactured by ADEKA Corporation] <Non-reactive surfactant> -Nonionic non-reactive surfactant- "NL-600F" [Product name: Noigen (registered trademark) DKS NL-600F, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.]

[0174] In Table 1, a "-" in the composition column means that the component in that column is not used.

[0175] [Preparation of Adhesive Composition] Example 1 The aqueous dispersion of the (meth)acrylic resin particles A-2 obtained above (100 parts by mass (solid content equivalent)), 10 parts by mass (solid content equivalent) of Auroren (registered trademark) AE-301 (trade name, acid-modified, non-chlorinated polyolefin particles, average particle size: 72 nm, manufactured by Nippon Paper Industries Co., Ltd.) as olefin resin particles, 40 parts by mass (solid content equivalent) of Super Ester E-865-NT (trade name, manufactured by Arakawa Chemical Industries Co., Ltd.) as tackifier resin particles, 0.25 parts by mass of ammonia water, 0.4 parts by mass (solid content equivalent) of CP-101 (trade name, manufactured by San Nopco Ltd.) as a defoaming agent, 0.2 parts by mass (solid content equivalent) of SN DEFOAMER 470 (trade name, manufactured by San Nopco Ltd.) as a defoaming agent, and ACTICIDE (registered trademark) BW-20 (trade name, manufactured by San Nopco Ltd.) as a preservative were mixed. A pressure-sensitive adhesive composition of Example 1 was prepared by mixing 0.04 parts by mass (solid content equivalent) of Nisshin Chemical Industry Co., Ltd.'s Surfynol (registered trademark) 440 (trade name, manufactured by Nisshin Chemical Industry Co., Ltd.) as a wetting agent, 1.5 parts by mass (solid content equivalent) of Nisshin Chemical Industry Co., Ltd.'s Surfynol (registered trademark) 440 as a wetting agent, and 1.7 parts by mass (solid content equivalent) of Nisshin Chemical Industry Co., Ltd.'s Nikazol (registered trademark) VT-253A (trade name, manufactured by Nippon Carbide Industries Co., Ltd.) as a thickening agent, and then adding 5 parts by mass (solid content equivalent) of Carbodilite (registered trademark) V-04 (trade name, carbodiimide crosslinking agent, manufactured by Nisshinbo Chemical Inc.) as a crosslinking agent and thoroughly mixing. The resulting pressure-sensitive adhesive composition of Example 1 had a water content of 57.5 mass % relative to the total mass of the pressure-sensitive adhesive composition, and a pH of 8.2.

[0176] [Examples 2 to 15] In Examples 2 to 15, the adhesive compositions of Examples 2 to 15 were prepared in the same manner as in Example 1, except that the formulations of the adhesive compositions were as shown in Table 2. The obtained pressure-sensitive adhesive compositions of Examples 2 to 15 all had a water content of 57.5 mass % relative to the total mass of the pressure-sensitive adhesive composition, and a pH of 8.2.

[0177] [Examples 16 to 26] In Examples 16 to 26, the adhesive compositions of Examples 16 to 26 were prepared in the same manner as in Example 1, except that the formulations of the adhesive compositions were as shown in Table 3. The resulting pressure-sensitive adhesive compositions of Examples 16 to 26 all had a water content of 57.5 mass % relative to the total mass of the pressure-sensitive adhesive composition, and a pH of 8.2.

[0178] [Comparative Examples 1 to 7] In Comparative Examples 1 to 7, the adhesive compositions were prepared in the same manner as in Example 1, except that the formulations of the adhesive compositions were as shown in Table 4. The resulting pressure-sensitive adhesive compositions of Comparative Examples 1 to 7 all had a water content of 57.5 mass % relative to the total mass of the pressure-sensitive adhesive composition, and a pH of 8.2.

[0179] The pH of each of the pressure-sensitive adhesive compositions of Examples 1 to 26 and Comparative Examples 1 to 7 was measured at a liquid temperature of 25° C. using a pH meter (product name: F-51) manufactured by Horiba, Ltd., in accordance with a method in accordance with JIS Z 8802:2011.

[0180] [Preparation of Adhesive Sheet X for Evaluation] The adhesive composition prepared above was applied to the easy-release treated surface of a release sheet (product name: SL-80KCM, manufactured by Sumika Kakoshi Co., Ltd.) in an amount of 30 g / m2 after drying. 2 The coating was applied with an applicator so that the coating film was formed. The coating film thus formed was then dried using a hot air circulation dryer under conditions of a drying temperature of 105°C and a drying time of 90 seconds, forming an adhesive film on the surface of the release sheet. Next, the exposed surface of the adhesive film formed on the surface of the release sheet was laminated on one side of Yupo paper (product name: Yupotac (registered trademark) base paper SGS110, thickness: 110 μm, manufactured by Yupo Corporation) as a substrate. Next, the laminate obtained by lamination was left to stand for 7 days (so-called curing period) in an environment with an atmospheric temperature of 23°C and 50% RH, to allow the adhesive film to cure. In this manner, an evaluation pressure-sensitive adhesive sheet X having a structure of release sheet / pressure-sensitive adhesive layer (thickness: 25 μm) / substrate (Yupo paper) was prepared.

[0181] [Measurement and Evaluation] 1.Storage modulus The adhesive composition prepared above was applied to the easy-release treated surface of a release sheet (product name: SL-80KCM, manufactured by Sumika Kakoshi Co., Ltd.) in an amount of 30 g / m2 after drying. 2 The coating film was formed by applying the adhesive using an applicator so that the thickness of the coating film was 105°C and the thickness of the coating film was 90 seconds using a hot air circulation dryer, and an adhesive film was formed on the surface of the release sheet. The adhesive films were then stacked to a thickness of 400 μm, and a laminate P having a release sheet / adhesive film / release sheet structure was obtained. The obtained laminate P was then left to stand in an environment with an atmospheric temperature of 23°C and 50% RH for 7 days (so-called curing period) to cure the adhesive film, thereby producing a laminate Q having a release sheet / adhesive layer (thickness: 400 μm) / release sheet structure. The laminate Q prepared above was cut out to fit a measuring jig PP8 (trade name, manufactured by Anton Paar). Then, two release sheets were peeled off from the cut out laminate Q to obtain an adhesive layer. Next, the viscoelasticity spectrum of the obtained adhesive layer was measured using a dynamic viscoelasticity measuring device manufactured by Anton Paar (trade name: Physica MCR301) by a dynamic viscoelasticity measuring method (temperature range: 25°C to 130°C, heating rate: 5°C / min, frequency: 1Hz, cone used: 8mmφ) in accordance with JIS K7244-1:1998, and the storage modulus (G') at 30°C was obtained. The results are shown in Tables 2 to 4.

[0182] 2. Adhesive strength The adhesive sheet X for evaluation prepared above was cut to a size of 25 mm × 100 mm to prepare an adhesive sheet piece X for evaluation. Next, the release sheet was peeled off from the prepared adhesive sheet piece X for evaluation (configuration: release sheet / adhesive layer / substrate). Hereinafter, the adhesive sheet piece X for evaluation from which the release sheet has been peeled off is referred to as "adhesive sheet piece X1 for evaluation." The surface of the adhesive layer exposed by peeling was placed on one side of SUS304 (stainless steel plate; simply referred to as "SUS") that had been polished with a cloth soaked in isopropanol (IPA), and then pressed by two reciprocating strokes of a 2 kg roller to prepare a test piece. The prepared test piece was left to stand for 30 minutes in an environment with an atmospheric temperature of 23°C and 50% RH. For the test piece after standing, the adhesive strength (unit: N / 25 mm) when the evaluation adhesive sheet piece X1 (configuration: adhesive layer / substrate) was peeled off from the SUS at 180° in the long side (100 mm) direction was measured using a single column type material testing machine (model number: STA-1225) manufactured by A&D Co., Ltd. as a measuring device under conditions of an atmospheric temperature of 23°C, 50% RH, and a peeling speed of 300 mm / min. Evaluation was then performed according to the following evaluation criteria. The measured values ​​and evaluation results are shown in Tables 2 to 4. In the following evaluation criteria, "A" and "B" are at levels that are not problematic in practical use, with "A" being the most preferable.

[0183] -Evaluation criteria- A: The adhesive strength was 10.0N / 25mm or more. B: The adhesive strength was 5.0 N / 25 mm or more and less than 10.0 N / 25 mm. C: The adhesive strength was 1.0 N / 25 mm or more and less than 5.0 N / 25 mm. D: The adhesive strength was less than 1.0 N / 25 mm.

[0184] 3.Durability against immersion in salt water (1) Peeling The adhesive sheet X for evaluation prepared above was cut to a size of 25 mm × 100 mm to prepare an adhesive sheet piece X for evaluation. Next, the release sheet was peeled off from the prepared adhesive sheet piece X for evaluation (configuration: release sheet / adhesive layer / substrate). Hereinafter, the adhesive sheet piece X for evaluation from which the release sheet has been peeled off is referred to as "adhesive sheet piece X1 for evaluation." The surface of the adhesive layer exposed by peeling was placed on one side of a SUS board that had been polished with a cloth soaked in isopropanol (IPA), and then pressed with a 2 kg roller back and forth twice to prepare a test piece. The test piece thus prepared was immersed in a 5% by mass aqueous sodium chloride solution at a liquid temperature of 50°C for one week, and then removed from the aqueous sodium chloride solution. The removed test piece was visually observed and evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 2 to 4. In the following evaluation criteria, "A" and "B" are at levels that are not problematic in practical use, with "A" being the most preferable.

[0185] -Evaluation criteria- A: The adhesive layer did not peel off at all from the SUS. B: Peeling of the adhesive layer from the SUS was confirmed, but the area of ​​the adhesive layer that had peeled off from the SUS was less than 50% of the adhesive area between the SUS and the adhesive layer before immersion in salt water. C: Peeling of the adhesive layer from the SUS was confirmed, and the area of ​​the adhesive layer that had peeled off from the SUS was 50% or more of the adhesive area between the SUS and the adhesive layer before immersion in salt water (excluding cases that fall under D). D: The adhesive layer was completely peeled off from the SUS.

[0186] (2)Removability In the above evaluation test for "(1) Peeling", the test pieces after confirming the presence or absence and the degree of peeling of the adhesive layer from the SUS were used to perform an evaluation test for removability. The evaluation adhesive sheet piece X1 (structure: adhesive layer / substrate) was peeled off from the SUS by hand in the long side (100 mm) direction. The SUS surface after peeling off the adhesive layer was visually observed and evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 2 to 4. In the following evaluation criteria, "A" and "B" are at levels that are not problematic in practical use, with "A" being the most preferable.

[0187] -Evaluation criteria- A: No adhesive residue was found at all. B: Adhesive residue was observed, but the area of ​​the adhesive residue was less than 50% of the adhesive area between the SUS and the adhesive layer before immersion in salt water. C: Adhesive residue was observed, and the area ratio of the adhesive residue was 50% or more of the adhesive area between the SUS and the adhesive layer before immersion in salt water.

[0188] [Table 2]

[0189] [Table 3]

[0190] [Table 4]

[0191] Details of the components listed in Tables 2 to 4 are as follows. <Olefin resin particles> "AE-301" [Product name: Auroren (registered trademark) AE-301, acid modification: yes, chlorination: no, average particle size: 72 nm, manufactured by Nippon Paper Industries Co., Ltd.] <Crosslinking agent> "V-04" [Product name: Carbodilite (registered trademark) V-04, carbodiimide crosslinking agent, manufactured by Nisshinbo Chemical Co., Ltd.] "WS-500" [Product name: Epocross (registered trademark) WS-500, oxazoline-based crosslinking agent, manufactured by Nippon Shokubai Co., Ltd.] <Tackifying resin particles> "E-865-NT" [Product name: Super Ester E-865-NT, rosin resin, softening point: 160°C, average particle size: 300 nm, solid content: 50% by mass, manufactured by Arakawa Chemical Industries, Ltd.] "E-865-WR" [Product name: Super Ester E-865-WR, rosin resin, softening point: 160°C, average particle size: 300 nm, solid content: 50% by mass, manufactured by Arakawa Chemical Industries, Ltd.] "E-900-NT" [Product name: Super Ester E-900-NT, rosin resin, softening point: 160°C, shape: particulate, average particle size: 300 nm, solid content: 50% by mass, manufactured by Arakawa Chemical Industries, Ltd.] "E-910-NT" [Product name: Super Ester E-910-NT, rosin resin, softening point: 160°C, average particle size: 300 nm, solid content: 50% by mass, manufactured by Arakawa Chemical Industries, Ltd.]

[0192] In Tables 3 and 4, "-" in the column of the composition of the adhesive composition means that the component in that column was not used. In Table 4, the "-" in the column for evaluation of removability indicates that the adhesive layer was completely peeled off from the SUS during the peel evaluation test, and therefore the removability evaluation test was not performed.

[0193] As shown in Tables 2 and 3, it was confirmed that the pressure-sensitive adhesive layers formed from the pressure-sensitive adhesive compositions of the Examples had high adhesive strength to adherends. It was also confirmed that the pressure-sensitive adhesive layers formed from the pressure-sensitive adhesive compositions of the Examples were difficult to peel off from adherends even when immersed in salt water, and had excellent removability.

[0194] On the other hand, as shown in Table 4, it was confirmed that the adhesive layer formed from the adhesive composition of Comparative Example 1, in which the (meth)acrylic resin particles do not contain the structural unit (B) derived from a monomer having a carboxy group, is easily peeled off from the adherend when immersed in salt water. It was confirmed that the adhesive layer formed from the adhesive composition of Comparative Example 2, which contains (meth)acrylic resin particles in which the content of structural units (B) derived from a monomer having a carboxy group exceeds 2.0 mass% relative to the total structural units, is prone to leaving adhesive residue on the substrate when peeled from the substrate when immersed in salt water. Storage modulus at 30℃ and 1Hz is 1.0×10 6 It was confirmed that the pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition of Comparative Example 3 and the pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition of Comparative Example 4, which have a compressive strength of 0.1 Pa or less, are easily peeled off from the adherend when immersed in salt water. Storage modulus at 30℃ and 1Hz is 1.0×10 8 It was confirmed that the adhesive layer formed from the adhesive composition of Comparative Example 5, which has a compressive strength exceeding 1 Pa, has low adhesive strength to the adherend. It was also confirmed that the adhesive layer formed from the adhesive composition of Comparative Example 5, when immersed in salt water, is likely to leave adhesive residue on the adherend when peeled from the adherend. It was confirmed that the adhesive layer formed from the adhesive composition of Comparative Example 6, which did not contain olefin-based resin particles, was prone to leaving adhesive residue on the substrate when peeled off from the substrate when immersed in salt water. It was confirmed that the pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition of Comparative Example 7, which did not contain a crosslinking agent, was easily peeled off from the adherend when immersed in salt water.

Claims

1. (Meth)acrylic resin particles containing a structural unit (A) derived from a (meth)acrylic acid alkyl ester monomer and a structural unit (B) derived from a monomer having a carboxy group, the content of the structural unit (B) being in the range of 0.01% by mass or more and 2.0% by mass or less with respect to all structural units; Olefin-based resin particles; A cross-linking agent; Water, Including, When the pressure-sensitive adhesive layer is formed, the storage modulus of the pressure-sensitive adhesive layer at 30° C. and 1 Hz is 1.0×10 6 Pa over 1.0 x 10 8 The pressure-sensitive adhesive composition has a viscosity in the range of 0.1 Pa or less.

2. The pressure-sensitive adhesive layer has a storage modulus of 1.0×10 at 30° C. and 1 Hz. 6 Pa over 1.0 x 10 7 The pressure-sensitive adhesive composition according to claim 1 , wherein the viscosity is in the range of 0.1 Pa or less.

3. The pressure-sensitive adhesive composition according to claim 1 , further comprising tackifier resin particles.

4. 2. The pressure-sensitive adhesive composition according to claim 1, wherein the (meth)acrylic resin particles have a glass transition temperature in the range of -40°C or higher and 0°C or lower.

5. The pressure-sensitive adhesive composition according to claim 1, wherein the (meth)acrylic resin particles have an average particle size in the range of 5 nm or more and 250 nm or less.

6. The pressure-sensitive adhesive composition according to claim 1 , wherein the (meth)acrylic resin particles further contain a structural unit (C) derived from a reactive surfactant.

7. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Repeelable aqueous pressure-sensitive adhesive composition and pressure-sensitive adhesive product