Abrasive composition

The polishing composition with α,β-unsaturated monocarboxylic acid and aliphatic (meth)acrylate stabilizes particle dispersion and reduces pH fluctuations, addressing agglomeration issues in abrasive slurries for semiconductor manufacturing, enhancing polishing selectivity and substrate flatness.

JP2024158594AInactive Publication Date: 2024-11-08ARAKAWA CHEM IND LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023073919
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing abrasive slurries used in semiconductor manufacturing face issues with particle agglomeration due to pH fluctuations, leading to increased polishing scratches and reduced polishing selectivity.

Method used

A polishing composition comprising 30 to 85 mol% of α,β-unsaturated monocarboxylic acid and 10 to 60 mol% of aliphatic (meth)acrylate, with a pH of 3 to 9, is used to stabilize the dispersion of metal oxide particles and reduce pH fluctuations.

Benefits of technology

The composition provides high polishing selectivity and stability, minimizing scratches and ensuring a flat substrate surface by effectively suppressing particle agglomeration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158594000001
    Figure 2024158594000001
Patent Text Reader

Abstract

To provide an abrasive composition capable of producing an abrasive slurry, with suppressed pH fluctuations in the slurry to prevent the aggregation of metal oxide particles, and offering high polishing selectivity.SOLUTION: An abrasive composition comprises a polymer of reactive components comprising 30-85 mol% of an α,β-unsaturated monocarboxylic acid (a1) and 10-60 mol% of an aliphatic (meth)acrylate (a2) with a C1-6 alkyl group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing composition. [Background technology]

[0002] In the manufacturing process of semiconductor devices, polishing such as mechanical polishing (polishing) and chemical mechanical polishing (CMP) is carried out to increase the density and miniaturization of the devices. The abrasive slurry used in this process generally contains metal compound particles, a dispersant, and water.

[0003] Examples of the particles include metal oxides such as alumina particles, silica particles, cerium oxide particles, and iron oxide particles. Alumina particles have very hard particles dispersed therein compared to other particles, and have been used for polishing for a long time. Cerium oxide particles have a lower hardness than alumina particles and silica particles, and are less likely to scratch the polished surface, and are often used for CMP. Silicon oxide films, silicon nitride films, and the like are used alone or in combination as substrates.

[0004] As for dispersants, in the case of polishing liquids containing cerium oxide particles, those using polyacrylic acid or copolymers of acrylic acid and methyl acrylate, etc. are known (Patent Documents 1 and 2). However, when such dispersants are used, the particles may aggregate to form larger particles, which may increase polishing scratches on the polished surface.

[0005] In order to reduce polishing scratches, it is necessary to stably disperse particles to suppress aggregation, and to reduce the polishing rate ratio of the substrate after polishing so that the entire surface of the wafer becomes flat (hereinafter referred to as polishing selectivity). One way to suppress particle dispersion is to reduce the pH fluctuation of the abrasive slurry, and a technique for adding a water-soluble polymer or an organic acid is known as a means of solving this problem (Patent Documents 3 and 4), but even in these cases, particle aggregation may occur. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-154672 [Patent Document 2] JP 2000-017195 A [Patent Document 3] International Publication No. 2000 / 039843 [Patent Document 4] International Publication No. 2012 / 086781 Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a composition for an abrasive which reduces the fluctuation in pH of the slurry in order to suppress the aggregation of metal oxide particles, and gives an abrasive slurry having high polishing selectivity. [Means for solving the problem]

[0008] The present inventors have conducted research focusing on the composition and amount of monomers constituting a polymer, and have found a solution to the above-mentioned problems, thereby completing the present invention. That is, the present invention relates to the following abrasive composition.

[0009] 1. A composition for abrasives comprising a polymer of reaction components comprising 30 to 85 mol % of an α,β-unsaturated monocarboxylic acid (a1) and 10 to 60 mol % of an aliphatic (meth)acrylate (a2) having an alkyl group with 1 to 6 carbon atoms.

[0010] 2. The polishing composition according to the above item 1, which has a pH of 3 to 9. Effect of the Invention

[0011] According to the polishing composition of the present invention, the fluctuation of the pH of the slurry is reduced, and an abrasive slurry having high polishing selectivity is obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The polishing composition of the present invention contains a polymer (A) of reaction components including 35 to 85 mol % of an α,β-unsaturated monocarboxylic acid (a1) (hereinafter referred to as component (a1)) and 10 to 60 mol % of an aliphatic (meth)acrylate (a2) (hereinafter referred to as component (a2)) having an alkyl group with 1 to 6 carbon atoms.

[0013] The component (a1) is an α,β-unsaturated monocarboxylic acid that suppresses the aggregation of metal oxide particles. "Unsaturated" refers to having one or more carbon-carbon double bonds or carbon-carbon triple bonds in the molecule (hereinafter the same).

[0014] Examples of the (a1) component include acrylic acid (2-propenoic acid), methacrylic acid (2-methyl-2-propenoic acid), 3-butenoic acid, 4-pentenoic acid, 5-hexenoic acid, 2-methyl-2-hexenoic acid, 3-methyl-2-hexenoic acid, 4-methyl-3-hexenoic acid, 2-heptenoic acid, 3-heptenoic acid, 4-heptenoic acid, 5-heptenoic acid, 6-heptenoic acid, and anhydrides thereof. In addition, the (a1) component may be an alkali metal salt such as sodium or potassium; an ammonium salt such as ammonia; or an organic amine salt such as trimethylamine, triethylamine, trimethanolamine, or triethanolamine. These may be used alone or in combination of two or more. Among them, acrylic acid and methacrylic acid are preferred from the viewpoint of stably dispersing metal oxide particles in the abrasive slurry containing the generated polymer (A).

[0015] The amount of the (a1) component used is 30 to 85 mol % with the total reaction components being 100 mol %. The total reaction components refer to the components excluding the additives and solvents described below (hereinafter the same). If the amount of the (a1) component used is less than 30 mol %, the abrasive slurry becomes difficult to disperse, and the pH is likely to fluctuate during storage. If the amount used exceeds 85 mol %, the polishing selectivity is likely to deteriorate. From the same point of view, the amount of the (a1) component used is preferably 40 to 80 mol %, more preferably 45 to 75 mol %.

[0016] The component (a2) is an aliphatic (meth)acrylate having an alkyl group with a carbon number of 1 to 6, and is a component for suppressing aggregation of metal oxide particles. "(Meth)acrylate" refers to methacrylate or acrylate (hereinafter the same).

[0017] Examples of the (a2) component include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, n-hexyl (meth)acrylate, and isohexyl (meth)acrylate. These may be used alone or in combination of two or more. Among these, from the viewpoint of easily suppressing aggregation of metal oxide particles, aliphatic (meth)acrylates in which the alkyl group has 2 to 5 carbon atoms are preferred, and alkyl groups in which the carbon number is 3 to 4 are more preferred. More preferred examples of the (a2) component include n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, and t-butyl (meth)acrylate.

[0018] The amount of the (a2) component used is 10 to 60 mol % with the total reactive components being 100 mol %. If the amount of the (a2) component used is less than 10 mol %, the polishing selectivity is likely to be poor, and if it exceeds 60 mol %, the abrasive slurry becomes difficult to disperse, and the pH is likely to fluctuate during storage. From the same point of view, the amount of the (a2) component used is preferably 15 to 55 mol %, more preferably 20 to 50 mol %.

[0019] The reaction components may further include an unsaturated monomer (a3) ​​other than the components (a1) and (a2) (hereinafter referred to as the component (a3)). Examples of the component (a3) ​​include (meth)acrylamides, unsaturated monomers having a hydroxy group, unsaturated monomers having an amino group, α,β-unsaturated dicarboxylic acids, unsaturated monomers having a sulfonyl group, styrenes, mercaptans, alcohols, and aromatic compounds. These may be used alone or in combination of two or more. "(Meth)acrylic" refers to methacryl or acrylic (hereinafter the same).

[0020] Examples of (meth)acrylamides include (meth)acrylamide, N-alkyl(meth)acrylamides such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, and Nt-butyl(meth)acrylamide, N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, and N,N-diisopropyl(meth)acrylamide, and N,N-alkylenebis(meth)acrylamides such as N,N'-methylenebis(meth)acrylamide and N,N'-ethylenebis(meth)acrylamide, etc. These may be used alone or in combination of two or more.

[0021] Examples of unsaturated monomers having a hydroxy group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0022] Examples of unsaturated monomers having an amino group include polymerizable monomers having a primary amino group, polymerizable monomers having a secondary amino group, polymerizable monomers having a tertiary amino group, quaternary salts of these polymerizable monomers, etc. These may be used alone or in combination of two or more.

[0023] Examples of the polymerizable monomer having a primary amino group include vinylamine, allylamine, etc. These may be used alone or in combination of two or more kinds.

[0024] Examples of the polymerizable monomer having a secondary amino group include diallylamine, etc. These may be used alone or in combination of two or more kinds.

[0025] Examples of the polymerizable monomer having a tertiary amino group include (meth)acrylates having a tertiary amino group such as N,N-dimethylaminoethyl (meth)acrylate and N,N-diethylaminoethyl (meth)acrylate, and (meth)acrylamides having a tertiary amino group such as N,N-dimethylaminopropyl (meth)acrylamide and N,N-diethylaminopropyl (meth)acrylamide. These may be used alone or in combination of two or more.

[0026] The quaternary salt of these monomers means a product obtained by reacting the polymerizable monomer having a primary amino group, the polymerizable monomer having a secondary amino group, or the polymerizable monomer having a tertiary amino group with a quaternary agent, and the quaternary salt may be an inorganic acid salt such as a hydrochloride or a sulfate, or an organic acid salt such as an acetate. Examples of the quaternary agent include methyl chloride, benzyl chloride, dimethyl sulfate, epichlorohydrin, and the like. These may be used alone or in combination of two or more.

[0027] Examples of α,β-unsaturated dicarboxylic acids include itaconic acid, itaconic anhydride, fumaric acid, maleic acid, maleic anhydride, etc. In addition, the α,β-unsaturated dicarboxylic acids may also be used in the form of salts such as alkali metal salts (e.g., sodium, potassium, etc.); ammonium salts (e.g., ammonia, etc.); and organic amine salts (e.g., trimethylamine, triethylamine, trimethanolamine, triethanolamine, etc.). These may be used alone or in combination of two or more.

[0028] Examples of unsaturated monomers having a sulfonyl group include vinyl sulfonic acid, methallyl sulfonic acid, and p-styrene sulfonic acid. In addition, salts of alkali metals such as sodium and potassium, and salts of ammonium salts, etc., can also be used as unsaturated monomers having a sulfonyl group. These may be used alone or in combination of two or more.

[0029] Examples of styrenes include styrene, α-methylstyrene, β-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, dimethylstyrene, etc. These may be used alone or in combination of two or more.

[0030] Examples of mercaptans include 2-mercaptoethanol, n-dodecyl mercaptan, etc. These may be used alone or in combination of two or more kinds.

[0031] Examples of the alcohol include ethanol, isopropyl alcohol, n-pentyl alcohol, etc. These may be used alone or in combination of two or more kinds.

[0032] Examples of aromatic compounds include α-methylstyrene dimer, ethylbenzene, isopropylbenzene, cumene, etc. These may be used alone or in combination of two or more.

[0033] The amount of component (a3) ​​used is preferably 10 mol % or less, and more preferably 5 mol % or less, of the total reactive components being 100 mol %, in order to suppress aggregation of the metal oxide particles and facilitate stable dispersion of the particles.

[0034] In the production of the polymer (A) of the present invention, additives such as organic acids such as citric acid, succinic acid, oxalic acid, etc.; inorganic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, etc.; inorganic acid salts such as sodium sulfate, potassium sulfate, ammonium sulfate, etc.; inorganic bases such as sodium hydroxide, potassium hydroxide, calcium hydroxide, etc.; ammonia; amines such as trimethylamine, triethylamine, etc.; starches such as oxidized starch, starch phosphate, urea phosphate, etherified starch, crosslinked starch, APS-modified starch, enzyme-modified starch, cationic starch, amphoteric starch, etc.; polyvinyl alcohol, urea, antifoaming agents, antioxidants, preservatives, bactericides, etc. may be added. These may be used alone or in combination of two or more, and the timing of addition (before, during, or after production) can be freely selected.

[0035] The method for producing the polymer (A) includes adding the components (a1) and (a2), and optionally the component (a3) ​​and additives, and polymerizing them in the presence of a polymerization initiator, and the order of addition and the method of addition (simultaneous, divided, dropwise, or a combination thereof, etc.) are not particularly limited. The polymerization reaction may be carried out in an atmosphere of an inert gas such as nitrogen or argon, and the pressure may be freely selected from normal pressure, increased pressure, reduced pressure, etc. Furthermore, a solvent may be used in the polymerization.

[0036] As for the polymerization conditions, for example, the temperature is usually 30 to 100° C., and preferably 50 to 90° C., and the time is usually 1 to 20 hours, and preferably 2 to 10 hours.

[0037] Examples of the polymerization initiator include persulfates such as ammonium persulfate, potassium persulfate, and sodium persulfate; azo-based polymerization initiators such as 2,2'-azobis(2-amidinopropane) hydrochloride; and hydrogen peroxide. These may be used alone or in combination of two or more. The amount of the polymerization initiator used is preferably 0.01 to 20 parts by weight, more preferably 0.1 to 15 parts by weight, based on 100 parts by weight of the total reaction components.

[0038] In addition, optionally, a reducing agent may be used in combination to facilitate the generation of radicals from the organic peroxide. Examples of the reducing agent include sulfites such as sodium sulfite, hydrogen sulfites such as sodium hydrogen sulfite, triethanolamine, cuprous sulfate, etc.

[0039] Examples of the solvent include water such as tap water, ion-exchanged water, industrial water, pure water, and ultrapure water; alcohols such as methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, sec-butyl alcohol, t-butyl alcohol, isobutyl alcohol, n-hexyl alcohol, n-octyl alcohol, ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, and diacetone alcohol; and ethers such as ethylene glycol monobutyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether. These may be used alone or in combination of two or more. Among these, water is preferred. In addition, when a solvent is used, it is preferable to adjust the polymerization concentration to 5 to 50% by weight.

[0040] To the obtained polymer (A), for example, antislip agents, preservatives, rust inhibitors, pH adjusters, defoamers (such as silicone-based defoamers), thickeners, fillers, antioxidants, pigments, dyes, etc. may be added.

[0041] The physical properties of the polymer (A) obtained by the above-mentioned production method include, for example, a pH of preferably 3 to 9, more preferably 4 to 8, and even more preferably 5 to 7. The pH here is a value measured with a commercially available pH meter calibrated with a standard substance. When the pH shows the above-mentioned value, the solubility of the polymer (A) in water is increased, and the generation of sediment during long-term storage of the abrasive slurry is easily suppressed.

[0042] The non-volatile content of the polymer (A) is preferably from 1 to 50% by weight, more preferably from 5 to 50% by weight.

[0043] The abrasive composition of the present invention can be mixed with metal compound particles and the above-mentioned solvent to prepare an abrasive slurry. Examples of the metal compound particles include silica particles, silicon carbide particles, boron nitride particles, alumina particles, alumina zirconia particles, zirconium oxide particles, cerium oxide particles, iron oxide particles, titanium oxide particles, chromium oxide particles, or mixtures thereof. In addition, when preparing the abrasive slurry, a dispersant other than the polymer (A) may be added.

[0044] As the dispersant other than the polymer (A), for example, a nonionic dispersant, a cationic dispersant, an anionic dispersant, etc. can be added. These may be used alone or in combination of two or more kinds.

[0045] The method for producing the abrasive slurry includes, for example, mixing the polymer (A), metal compound particles, a solvent, and, if necessary, a dispersant other than the polymer (A). The mixture may be heated or cooled during mixing.

[0046] The content of each component when preparing the abrasive slurry can be freely selected. The slurry concentration of the resulting abrasive slurry is preferably in the range of 0.5 to 20% by weight in terms of ease of handling the abrasive slurry.

[0047] The abrasive composition of the present invention and an abrasive slurry containing the same can be used for applications such as grinding wheel polishing, buff polishing, lapping polishing, and barrel polishing, and is preferably suitable for lapping polishing and is most suitable for CMP (chemical mechanical) polishing. EXAMPLES

[0048] The present invention will be described below with reference to examples, but the present invention is not limited thereto. In the examples and comparative examples, "%" is by weight unless otherwise specified.

[0049] Example 1 In a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, a nitrogen gas inlet tube, and two dropping funnels, 100.0 g of ion-exchanged water and 200.0 g of isopropyl alcohol were placed, and oxygen in the reaction system was removed with nitrogen gas, and then the reaction system was heated to 90°C. A monomer mixture of 133.0 g (80 mol%) of methacrylic acid (MAA) and 50.0 g (20 mol%) of isopropyl methacrylate (iPrMA) was placed in the dropping funnel (I), and an initiator aqueous solution of 12.0 g of ammonium persulfate (APS) and 100.0 g of ion-exchanged water was placed in the dropping funnel (II). Next, the monomer mixture and the initiator aqueous solution were dropped into the system from the dropping funnel over a period of 3 hours. After the dropping was completed, a solution in which 0.5 g of APS was dissolved in 5.0 g of ion-exchanged water was added, and the mixture was kept warm for 2 hours. After isopropyl alcohol was removed by distillation under reduced pressure, the pH was adjusted to 7 with a 25% aqueous ammonia solution to obtain a polymer (A-1) with a non-volatile content of 20%.

[0050] Examples 2 to 4, Comparative Examples 1 to 2 The same procedure as in Example 1 was carried out except for changing the composition and molar ratio as shown in Table 1, to obtain aqueous solutions of polymers (A-2) to (A-4) and (B-1) to (B-2) having a pH of 7 and a non-volatile content of 20%, respectively.

[0051] The polymers (A-1) to (A-4) and (B-1) to (B-2) were used as they were as compositions for abrasive slurry.

[0052] <Preparation of abrasive slurry> After mixing 200.0 g of cerium oxide particles and 795.0 g of ion-exchanged water, 5.0 g of each abrasive slurry composition (non-volatile content: 20%) was added and ultrasonically dispersed (frequency: 400 kHz, time: 30 minutes) while stirring. Then, the mixture was classified and diluted with ion-exchanged water to prepare abrasive slurries with a non-volatile content of 5%.

[0053] <Polishing selectivity> Substrate (a) and substrate (b) described below were polished as blanket wafers under the following conditions, thoroughly washed with pure water, and then dried. Next, a film thickness measuring device (product name: "Lambda Ace VL-M8000LS", manufactured by Dai Nippon Screen Mfg. Co., Ltd.) was used to measure the film thickness difference before and after polishing on substrates (a) and (b), and the polishing speed was calculated based on the film thickness difference. The polishing speed ratio of the silicon nitride film to the silicon oxide film was calculated and evaluated according to the following criteria.

[0054] (substrate) (a) A 200 mm diameter substrate with a silicon oxide film (thickness: 1000 nm) formed on a silicon wafer by CVD. (b) A 200 mm diameter substrate with a silicon nitride film (thickness: 200 nm) formed on a silicon wafer by CVD.

[0055] (polishing conditions) Polishing equipment - Product name: "Mirra", manufactured by Applied Materials Polishing pad - Model number: "IC1010", manufactured by Rohm and Haas Processing load - 21kPa Abrasive slurry supply rate: 150mL / min Platen rotation speed: 90 rpm · Substrate rotation speed - 90 rpm ·Polishing time - 60 seconds

[0056] (Evaluation Criteria) ◎: The polishing rate ratio of silicon nitride film to silicon oxide film is less than 0.2% ○: The polishing rate ratio of the silicon nitride film to the silicon oxide film is 0.2% or more and less than 0.5%. △: The polishing rate ratio of the silicon nitride film to the silicon oxide film is 0.5% or more and less than 1%. ×: The polishing rate ratio of the silicon nitride film to the silicon oxide film is 1% or more.

[0057] (pH stability) The pH of each abrasive slurry was adjusted to 7 using a 10% aqueous acetic acid solution or a 10% aqueous ammonia solution. After standing at 50°C for 2 weeks, the pH of the abrasive slurry was measured using a commercially available pH meter (manufactured by Horiba, Ltd.), the absolute value of the change was read, and the results were evaluated according to the following criteria. The results are shown in Table 1 (same below).

[0058] (Evaluation Criteria) ⊚: The absolute value of the change was less than 0.1. ◯: The absolute value of the change range was 0.1 or more and less than 0.2. △: The absolute value of the change range was 0.2 or more and less than 0.3. ×: The absolute value of the change was 0.3 or more.

[0059] [Table 1]

[0060] The abbreviations shown in Table 1 represent the following monomers. ·MAA: Methacrylic acid i-PrMA: Isopropyl methacrylate IBMA: Isobutyl methacrylate

[0061] The results in Table 1 show that when an abrasive slurry was prepared and used with the abrasive composition of each Example, the polishing rate ratio of a silicon nitride film to a silicon oxide film was reduced, and the substrate became flat as a whole (i.e., excellent polishing selectivity), and the pH stability was also excellent even when stored for a long period of time at 50°C.

Claims

1. A composition for abrasives comprising a polymer of reaction components comprising 30 to 85 mol % of an α,β-unsaturated monocarboxylic acid (a1) and 10 to 60 mol % of an aliphatic (meth)acrylate (a2) having an alkyl group with 1 to 6 carbon atoms.

2. 2. The polishing composition according to claim 1, which has a pH of 3 to 9.

Citation Information

Patent Citations

  • Cerium oxide abrasive material and polishing method of substrate

    JP1998154672A

  • Cerium oxide abrasive, polishing of substrate and semiconductor device

    JP2000017195A

  • CMP abrasive, liquid additive for CMP abrasive and method for polishing substrate

    WO2000039843A1

  • Polishing liquid and method for polishing substrate using the polishing liquid

    WO2012086781A1