Manufacturing method of composite material

The method of discharging a coating liquid with airgel particles, binder resin, and glass fibers onto a target object and removing the liquid medium effectively addresses cracking issues, producing a strong and uniform composite material suitable for various applications.

JP2024158903APending Publication Date: 2024-11-08RESONAC CORP

Patent Information

Application Number
JP2023074526
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing methods for forming composite materials with airgel particles, binder resin, and glass fibers often result in cracking during film formation due to uneven distribution and orientation of glass fibers, making it difficult to produce a uniform and crack-free composite material.

Method used

A method involving the discharge of a coating liquid containing airgel particles, binder resin, and glass fibers onto a target object using a sprayer or dispenser, followed by removing a portion of the liquid medium to form a composite material, with specific conditions such as a discharge port diameter of 1.5 mm or more, and inclusion of a water-soluble polymer with hydrophobic groups to improve dispersibility and uniformity.

Benefits of technology

The method enables the production of a composite material with fewer cracks and higher film strength, maintaining uniformity and thermal insulation properties, suitable for applications in cryogenic containers, space fields, architecture, automotive, home appliances, and industrial equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158903000001
    Figure 2024158903000001
  • Figure 2024158903000002
    Figure 2024158903000002
  • Figure 2024158903000003
    Figure 2024158903000003
Patent Text Reader

Abstract

To provide a manufacturing method of a composite material for easily manufacturing a composite material that contains aerogel particles, binder resin, and glass fiber, and has little cracking.SOLUTION: A manufacturing method of a composite material includes: a coated film formation step for obtaining a coated film by discharging a coating liquid containing aerogel particles, binder resin, glass fiber, and a liquid medium toward an object; and a removal step for obtaining a composite material by removing at least a part of the liquid medium from the coated film.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a composite material. [Background technology]

[0002] Aerogel is known as a material with excellent thermal insulation properties. In addition, a method has been proposed in which aerogel is processed into particles and used as a constituent material of a thermal insulation material (for example, Patent Documents 1 and 2). Patent Document 1 proposes using particulate aerogel as a filler between resin plates that constitute a thermal insulation window. Patent Document 2 shows a method of producing a thermal insulation material (molded body) by preparing an aqueous dispersion containing aerogel particles and organic fibers, and then evaporating the water to obtain an intermediate product, which is then press-molded. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-091943 A [Patent Document 2] JP 2014-035044 A Summary of the Invention [Problem to be solved by the invention]

[0004] Composite materials containing aerogel particles and binder resins are expected to expand their scope of application and range of uses by being made into coating liquids.

[0005] The present inventors have investigated the incorporation of additional materials into the composite material and have found that the incorporation of glass fibers realizes high film strength suitable for use as a thermal insulating material. However, according to the findings of the present inventors, when a composite material containing glass fibers is applied to form a coating liquid, cracks are likely to occur during film formation, making it difficult to form a uniform composite material.

[0006] Therefore, an object of the present invention is to provide a method for producing a composite material that contains aerogel particles, a binder resin, and glass fibers and that is capable of easily producing a composite material with few cracks. [Means for solving the problem]

[0007] The present invention relates to, for example, the following [1] to

[10] . [1] a coating film forming step of discharging a coating liquid containing aerogel particles, a binder resin, glass fibers, and a liquid medium toward an object to obtain a coating film; a removing step of removing at least a portion of the liquid medium from the coating film to obtain a composite material; A method for producing a composite material, comprising: [2] The manufacturing method according to [1], wherein the coating film forming step is a step of ejecting the coating liquid toward the object using an ejection device selected from the group consisting of a sprayer and a dispenser. [3] the discharge device has a discharge port for discharging the coating liquid, The manufacturing method described in [2], wherein the inner diameter of the discharge outlet is 1.5 mm or more. [4] The method according to any one of [1] to [3], wherein the coating liquid further contains a water-soluble polymer having a hydrophobic group. [5] The method according to [4], wherein the hydrophobic group is an alkyl group having 6 to 26 carbon atoms. [6] The method according to any one of [1] to [5], wherein the coating liquid contains emulsified particles containing the binder resin. [7] The method according to [6], wherein the emulsion particles further contain a nonionic emulsifier. [8] The method according to any one of [1] to [7], wherein at least a portion of the aerogel particles form aggregates. [9] an emulsion preparation step of preparing an emulsion including emulsified particles containing a binder resin and a first liquid medium; a dispersion preparation step of mixing aerogel particles, glass fibers, and a second liquid medium to obtain a dispersion containing the aerogel particles, the glass fibers, and the second liquid medium; a coating liquid preparation step of mixing the emulsion and the dispersion to obtain the coating liquid; The method for producing a semiconductor device according to any one of [1] to [8], further comprising:

[10] the dispersion preparation step is a step of mixing the aerogel particles, the glass fibers, and the second liquid medium to aggregate at least a portion of the aerogel particles; The method according to [9], wherein the coating liquid contains aggregates of the aerogel particles. Effect of the Invention

[0008] According to the present invention, there is provided a method for producing a composite material, which contains aerogel particles, a binder resin, and glass fibers and is capable of easily producing a composite material with few cracks. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Preferred embodiments of the present invention will be described in detail below. However, the present invention is not limited to the following embodiments. In this specification, a numerical range indicated using "~" indicates a range including the numerical values ​​before and after "~" as the minimum and maximum values, respectively. "A or B" may include either A or B, or may include both. Unless otherwise specified, the materials exemplified in this embodiment may be used alone or in combination of two or more.

[0010] The method for producing a composite material of the present embodiment includes a step of ejecting a coating liquid containing aerogel particles, a binder resin, glass fibers, and a liquid medium toward an object to obtain a coating film (coating film forming step), and a step of removing at least a portion of the liquid medium from the coating film to obtain a composite material (removal step).

[0011] According to the findings of the present inventors, when glass fibers are further blended into a composite material containing aerogel particles and a binder resin, a high film strength suitable for use as a heat insulating material is realized. However, when a coating liquid containing aerogel particles, a binder resin, glass fibers, and a liquid medium is applied to an object using a roller, a trowel, or the like, there is a problem that the coating film is prone to cracking when it dries.

[0012] In the manufacturing method of the present embodiment, a coating film is formed by discharging a coating liquid onto an object. By forming a coating film in this manner, it is possible to easily form a composite material that is less likely to crack when dried, has high film strength, and has few cracks.

[0013] The reason why such an effect is achieved is believed to be as follows. For example, when a roller is used, components other than the glass fibers in the coating liquid mainly penetrate into the roller and are applied, which is believed to reduce the glass fiber density in the coating film and promote the occurrence of cracks. Also, when a trowel is used, it is believed that the glass fibers are oriented in the coating direction, and this orientation promotes the occurrence of cracks. In contrast, in the manufacturing method of this embodiment, the coating film is formed by discharging the coating liquid onto the target object, so the glass fiber density does not decrease and the glass fibers are less likely to be oriented, which is believed to make it less likely for cracks to occur.

[0014] In this embodiment, the coating liquid may further contain a water-soluble polymer having a hydrophobic group, which improves the dispersibility of the aerogel particles, making it possible to prepare a coating liquid with a higher loading of aerogel particles and facilitating the production of a more uniform composite material.

[0015] In the present embodiment, the coating liquid may contain emulsified particles containing a binder resin. By dispersing the binder resin as emulsified particles, the dispersibility of the binder resin is improved, and a more uniform composite material can be easily formed.

[0016] In this embodiment, the aerogel particles in the coating liquid may be partially or entirely in the form of aggregates, which tends to reduce the contact interface between the aerogel particles and the resin component (binder resin) during the formation of the composite material, suppressing the penetration of the resin component into the pores of the aerogel particles and resulting in a composite material with higher thermal insulation properties.

[0017] The method for producing a composite material of the present embodiment may further include a step of preparing an emulsion containing emulsified particles containing a binder resin and a first liquid medium (emulsion preparation step), a step of mixing aerogel particles, glass fibers, and a second liquid medium to obtain a dispersion containing aerogel particles, a water-soluble polymer, and the second liquid medium (dispersion preparation step), and a step of mixing the emulsion and the dispersion to obtain a coating liquid (coating liquid preparation step).

[0018] The dispersion preparation step may be a step of mixing aerogel particles, glass fibers, and a second liquid medium to aggregate at least a portion of the aerogel particles.

[0019] Each step in the method for producing a composite material according to this embodiment will be described in detail below.

[0020] <Coating film formation process> In the coating film forming process, a coating liquid is discharged onto an object to form a layer of the coating liquid (coating film) on the object.

[0021] The object is not limited to an object to which the composite material is applied, and may be, for example, a resin member, a metal member, a building material, etc.

[0022] The coating liquid may be discharged, for example, by using a discharge device selected from the group consisting of a spray (e.g., air spray, etc.) and a dispenser. The discharge device may have a discharge port for discharging the coating liquid. The inner diameter of the discharge port may be, for example, 1.5 mm or more, 2.0 mm or more, 2.5 mm or more, or 3.0 mm or more. The inner diameter of the discharge port may be, for example, 10.0 mm or less, 7.0 mm or less, 6.0 mm or less, or 5.0 mm or less.

[0023] <Removal process> In the removing step, at least a part of the liquid medium is removed from the coating film formed in the coating film forming step, thereby forming a composite material.

[0024] The method for removing the liquid medium from the coating film is not particularly limited, and examples thereof include a heating treatment (eg, 40 to 150° C.), a reduced pressure treatment (eg, 10,000 Pa or less), or both of these treatments.

[0025] The thickness of the composite material is not particularly limited and may be, for example, 0.05 mm or more, 0.1 mm or more, 0.5 mm or more, or 1 mm or more, and may be, for example, 30 mm or less, 20 mm or less, 10 mm or less, or 5 mm or less.

[0026] The composite material has pores due to the aerogel particles. The pore volume of the composite material is set to 0.15 cm3 in order to obtain higher thermal insulation. 3 / g or more is preferable, and 0.20 cm 3 / g or more is more preferable, and 0.60 cm 3 / g or more is more preferable. The upper limit of the pore volume of the composite material is not particularly limited. The pore volume of the composite material is, for example, 5.0 cm 3 / g or less.

[0027] The thermal conductivity of the composite material is, for example, 0.05 W / (m·K) or less, preferably 0.04 W / (m·K) or less, and more preferably 0.035 W / (m·K) or less. There is no particular lower limit to the thermal conductivity of the composite material. The thermal conductivity of the composite material may be, for example, 0.01 W / (m·K) or more.

[0028] The composite material has excellent heat insulating properties derived from the aerogel. Therefore, the composite material can be suitably used as a heat insulating material in cryogenic containers, the space field, the architectural field such as piping and exterior walls, the automotive field such as car air conditioning units and engines, the home appliance field such as refrigerators and freezers, the semiconductor field, and industrial facilities such as piping and tanks. In addition to being used as a heat insulating material, the composite material can also be used as a water repellent, sound absorbing material, vibration silencing material, catalyst carrier material, etc.

[0029] <Production of coating fluid> In this embodiment, the coating liquid may be produced by mixing, for example, aerogel particles, a binder resin, glass fibers, and a liquid medium.

[0030] In this embodiment, the coating liquid may be produced by a production method including, for example, a preparation step of preparing aerogel particles, a binder resin, and a liquid medium, and a mixing step of mixing the aerogel particles, the binder resin, and the liquid medium prepared in the preparation step to aggregate the aerogel particles, thereby obtaining a coating liquid containing an aggregate of the aerogel particles, the binder resin, and the liquid medium.

[0031] In the preparation step, components other than the aerogel particles, the binder resin, and the liquid medium (for example, components described in <Other Components> below) may be further prepared.

[0032] In the mixing step, the components prepared in the preparation step are mixed so that the aerogel particles are aggregated. The mixing method may be any method that can form an aggregate of the aerogel particles, and may be, for example, a method of stirring and mixing the components prepared in the preparation step.

[0033] The stirring speed affects the size of the aggregates. The higher the stirring speed, the greater the shear stress, which tends to reduce the size of the aggregates. Therefore, from the viewpoint of obtaining aggregates of a suitable size, as described below, it is desirable to mix at a low stirring speed.

[0034] The viscosity during mixing also affects the size of the aggregates. Even at the same stirring speed, the shear stress changes depending on the viscosity. If the viscosity is high, a larger shear stress is applied and the aggregates tend to be smaller in size. On the other hand, if the viscosity is low, the shear stress is small and the aggregates tend to be larger. Therefore, the desired aggregate size can be achieved by adjusting the stirring speed depending on the viscosity.

[0035] In addition, the amount of liquid medium used during mixing also affects the size of the aggregates. Even if the final composition is the same, the size of the aggregates differs between (A) method in which the entire amount of liquid medium is added from the beginning of mixing and (B) method in which a small amount of liquid medium is used in the beginning of mixing and then the liquid medium is added. The above method (B) has a higher initial viscosity than the above method (A). For this reason, the above method (B) tends to produce smaller aggregates than the above method (A). By using these methods appropriately according to conditions such as the composition and the mixing device (stirring device), aggregates of the desired size can be formed.

[0036] The average diameter of the aggregates may be, for example, 20 μm or more, or may be 30 μm or more. If the average diameter of the aggregates is large, the contact interface between the aerogel and the binder resin becomes smaller, and the penetration of the resin into the pores of the aerogel is further suppressed. The average diameter of the aggregates may be, for example, 300 μm or less, or may be 200 μm or less, or 150 μm or less. If the average diameter of the aggregates is small, the decrease in film strength caused by the continuation of relatively fragile aerogel is suppressed, and a stronger composite material is easily obtained.

[0037] The average diameter of the aggregates may be two or more times the average diameter of the aerogel particles, or may be three or more times the average diameter of the aerogel particles. If the average diameter of the aggregates is large, the contact interface between the aerogel and the binder resin becomes smaller, and the penetration of the resin into the pores of the aerogel is further suppressed. In addition, the average diameter of the aggregates may be 30 or less, 20 or less, or 15 or less times the average diameter of the aerogel particles. If the average diameter of the aggregates is small, the decrease in film strength caused by the continuation of relatively fragile aerogel is suppressed, and a stronger composite material is easily obtained.

[0038] In this specification, the average diameter of the aggregates indicates a value measured by the following method. [Method for measuring the average diameter of aggregates in coating liquid] Put about 20 g of the coating liquid into a 100 mL plastic cup, and gradually dilute it by adding 2 g of water at a time while stirring with a spatula. Place the diluted sample on a glass plate and take a micrograph of the sample using an optical microscope (OLYMPUS, model number: BX51). Analyze the obtained micrograph using the image editing software ImageJ to determine the diameter of multiple aggregates in the micrograph. The average of the obtained values ​​is taken as the average diameter of the aggregates.

[0039] In this specification, the average diameter of the aerogel particles is synonymous with the above-mentioned average particle size (D50) of the aerogel particles.

[0040] In this embodiment, when the diluted solution obtained by diluting the coating liquid is observed with an optical microscope, the area occupied by aerogel particles (including agglomerates) within the observation field of view is preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, and may even be 100%, of the area occupied by aerogel particles (including agglomerates) within the observation field of view.

[0041] In this specification, the diluted solution obtained by diluting the coating solution and the observation method of the diluted solution may be the same as the sample prepared in the above-mentioned [Method for measuring the average diameter of aggregates in the coating solution] and the observation method of the sample. In addition, the "area within the observation field of view" is determined by analyzing the micrograph using the image editing software ImageJ.

[0042] In this embodiment, the coating liquid may be produced by a production method including, for example, an emulsion preparation step of preparing an emulsion containing emulsified particles containing a binder resin and a first liquid medium, a dispersion preparation step of mixing aerogel particles, glass fibers, and a second liquid medium to obtain a dispersion containing aerogel particles, glass fibers, and the second liquid medium, and a coating liquid preparation step of mixing the emulsion and the dispersion to obtain the coating liquid.

[0043] The emulsion preparation step is a step of preparing an emulsion containing emulsified particles containing a binder resin and a first liquid medium.

[0044] The emulsion preparation step may be, for example, a step of obtaining an emulsion by emulsion polymerization of the monomer components described below in a first liquid medium in the presence of an emulsifier.

[0045] Examples of the first liquid medium include the same liquid medium as described below. The first liquid medium is preferably an aqueous solvent.

[0046] The emulsion polymerization may be carried out, for example, by a step (i) of mixing a monomer component and an emulsifier in a first liquid medium to obtain a monomer emulsion, and a step (ii) of mixing the monomer emulsion with a radical polymerization initiator to perform emulsion polymerization of the monomer component.

[0047] In step (i), the amount of the emulsifier may be, for example, 0.01 parts by mass or more, 0.1 parts by mass or more, 0.3 parts by mass or more, 0.5 parts by mass or more, 0.7 parts by mass or more, 0.9 parts by mass or more, or 1 part by mass or more, relative to 100 parts by mass of the monomer component. In addition, in step (i), the amount of the emulsifier may be, for example, 15 parts by mass or less, 12 parts by mass or less, 10 parts by mass or less, 8 parts by mass or less, or 6 parts by mass or less, relative to 100 parts by mass of the monomer component.

[0048] The radical polymerization initiator is not particularly limited as long as it is a polymerization initiator capable of initiating emulsion polymerization of the monomer components, and may be appropriately selected from known radical polymerization initiators.

[0049] Examples of the radical polymerization initiator include hydrogen peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, 4,4'-azobis(4-cyanovaleric acid), and 2,2'-azobis[N-(2-hydroxyethyl)-2-methylpropanamide].

[0050] In step (ii), the amount of the radical polymerization initiator may be, for example, 0.001 parts by mass or more, 0.01 parts by mass or more, 0.05 parts by mass or more, or 0.1 parts by mass or more, relative to 100 parts by mass of the monomer component. In addition, in step (ii), the amount of the radical polymerization initiator may be, for example, 5 parts by mass or less, 3 parts by mass or less, 2 parts by mass or less, or 1 part by mass or less, relative to 100 parts by mass of the monomer component.

[0051] In step (ii), a reducing agent may be used together with the radical polymerization initiator as necessary. This promotes the generation of radicals from the radical polymerization initiator. Examples of the reducing agent include reducing organic compounds such as ascorbic acid, tartaric acid, citric acid, and glucose, and reducing inorganic compounds such as thiourea dioxide and hydrazine.

[0052] In step (ii), after the emulsion polymerization is completed, neutralization may be performed with a neutralizing agent. The neutralizing agent is not particularly limited and may be a known neutralizing agent. Examples of the neutralizing agent include aqueous ammonia, morpholine, 2-amino-2-methyl-1-propanol, triethylamine, triethanolamine, sodium hydroxide, and potassium hydroxide. The amount of the neutralizing agent is not particularly limited and may be appropriately adjusted so that the pH of the resulting emulsion is 7 to 11 (preferably 8 to 10).

[0053] The emulsion obtained in step (ii) contains emulsified particles containing a binder resin. The average particle size of the emulsified particles in the emulsion may be, for example, 50 nm or more, 70 nm or more, 90 nm or more, or 100 nm. The average particle size of the emulsified particles in the emulsion may be, for example, 400 nm or less, 350 nm or less, or 300 nm or less.

[0054] In this specification, the average particle size of emulsified particles in an emulsion refers to a value measured by dynamic light scattering (DLS) using a MICROTRAC UPA150 (manufactured by Microtrac-Bell Corporation) at 23°C.

[0055] The minimum film-forming temperature (MFT) of the emulsion obtained in step (ii) may be, for example, 25°C or less, and from the viewpoint of further improving film-forming properties, it is preferably 20°C or less, and more preferably 15°C or less. In addition, from the viewpoint of further improving film-forming properties at low temperatures, the minimum film-forming temperature (MFT) of the emulsion is preferably 10°C or less, more preferably 8°C or less, and may be 6°C or less. The lower limit of the minimum film-forming temperature (MFT) of the emulsion is not particularly limited. In addition, in the case of a paint containing a water-based solvent, an MFT of 0°C or less cannot be measured.

[0056] The dispersion preparation step is a step of mixing aerogel particles, glass fibers, and a second liquid medium to obtain a dispersion containing aerogel particles, glass fibers, and the second liquid medium.

[0057] The dispersion preparation step may be a step of mixing aerogel particles, glass fibers, and a second liquid medium so that the aerogel particles are aggregated to obtain a dispersion containing aggregates of aerogel particles, glass fibers, and the second liquid medium.

[0058] Examples of the second liquid medium include the liquid medium described below. The second liquid medium is preferably an aqueous solvent.

[0059] The dispersion may further contain a water-soluble polymer having a hydrophobic group. That is, the dispersion preparation step may be a step of mixing aerogel particles, glass fibers, a water-soluble polymer having a hydrophobic group, and a second liquid medium to obtain a dispersion containing aerogel particles, glass fibers, a water-soluble polymer having a hydrophobic group, and the second liquid medium.

[0060] In the dispersion preparation step, the amount of the water-soluble polymer may be, for example, 0.1 parts by mass or more, 0.5 parts by mass or more, 1 part by mass or more, 2 parts by mass or more, or 3 parts by mass or more, relative to 100 parts by mass of the aerogel particles. In addition, in the dispersion preparation step, the amount of the water-soluble polymer may be, for example, 20 parts by mass or less, 15 parts by mass or less, or 10 parts by mass or less, relative to 100 parts by mass of the aerogel particles.

[0061] In the dispersion preparation step, the mixing method is not particularly limited, and may be, for example, mixing by stirring.

[0062] The size of the aggregates in the dispersion is not particularly limited, and may be appropriately adjusted so that the size of the aggregates in the coating liquid falls within a suitable range described below.

[0063] The coating liquid preparation step is a step in which an emulsion and a dispersion are mixed to obtain a coating liquid.

[0064] In the coating liquid preparation step, the mixing method is not particularly limited, and may be, for example, mixing by stirring. The mixing method in the coating liquid preparation step may be appropriately adjusted so that the size of the aerogel particle aggregates falls within the above-mentioned preferred range.

[0065] Each component used in the method for producing a composite material according to the present embodiment will be described in detail below.

[0066] <Binder resin> Examples of binder resins include epoxy resins, silicone resins, phenolic resins, urea resins, melamine resins, polyurethane resins, polyethylene resins, polypropylene resins, polystyrene resins, polyester resins, acrylic resins, polyvinyl chloride resins, polyvinyl acetate resins, polyamide resins, polyimide resins, and polyvinyl resins.

[0067] In a preferred embodiment, the binder resin may be, for example, a polymer of a monomer component having an ethylenically unsaturated bond. Such a binder resin has a structural unit (also called a monomer unit) derived from the monomer component. Examples of the monomer component include an acrylic compound having a (meth)acryloyl group, an aromatic vinyl compound, a heterocyclic vinyl compound, vinyl esters, monoolefins, conjugated diolefins, α,β-unsaturated carboxylic acid, vinyl cyanides, and the like. These may be used alone or in combination of two or more.

[0068] Examples of the acrylic compound include (meth)acrylic acid alkyl esters. The alkyl group of the (meth)acrylic acid alkyl ester may be linear, branched, or cyclic. The number of carbon atoms of the alkyl group of the (meth)acrylic acid alkyl ester may be, for example, 1 to 20, 1 to 18, 1 to 16, or 1 to 14. Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and isobornyl (meth)acrylate.

[0069] Examples of the acrylic compound include a polar group-containing acrylic compound having a (meth)acryloyl group and a polar group (a polar group other than a (meth)acryloyl group). Examples of the polar group include a hydroxy group, an amino group, a substituted amino group (e.g., a dialkylamino group, a hydroxyalkylamino group, etc.), an amide group, a substituted amide group (e.g., a dialkylamide group, a hydroxyalkylamide group, etc.), an epoxy group, a silyl group (e.g., a trialkoxysilyl group, etc.), a cyano group, an isocyanate group, a phosphate group, a carbonyl group, etc.

[0070] Examples of polar group-containing acrylic compounds include compounds in which a polar group is substituted on the alkyl group of (meth)acrylic acid alkyl ester. Examples of such compounds include hydroxyalkyl(meth)acrylates (e.g., hydroxyethyl(meth)acrylate, etc.), dialkylaminoalkyl(meth)acrylates (e.g., dimethylaminoethyl(meth)acrylate, etc.), glycidyl(meth)acrylates, trialkoxysilylalkyl(meth)acrylates, isocyanatoalkyl(meth)acrylates (e.g., 2-isocyanatoethyl(meth)acrylate, etc.), and 2-(meth)acryloyloxyethyl acid phosphate.

[0071] The polar group-containing acrylic compound also includes a compound in which a (meth)acryloyl group is bonded to a polar group, such as (meth)acrylic acid, (meth)acrylamide, n-methylol (meth)acrylamide, diacetone acrylamide, etc.

[0072] Examples of polar group-containing acrylic compounds also include diacetone (meth)acrylate, acetoacetoxyalkyl (meth)acrylate (for example, acetoacetoxyethyl (meth)acrylate), and the like.

[0073] Examples of the acrylic compound include acrolein and vinyl alkyl ketones (for example, vinyl methyl ketone).

[0074] Examples of aromatic vinyl compounds include styrene, α-methylstyrene, p-methylstyrene, and ethylvinylbenzene.

[0075] Examples of the heterocyclic vinyl compound include vinylpyrrolidone, vinylfuran, vinylthiophene, vinyloxazoline, and vinylpyrrole.

[0076] Examples of vinyl esters include vinyl acetate, vinyl alkanoate, and vinyl versatate.

[0077] Examples of monoolefins include ethylene, propylene, butylene, and isobutylene.

[0078] Conjugated diolefins include, for example, butadiene, isoprene, and chloroprene.

[0079] Examples of the α,β-unsaturated carboxylic acid include crotonic acid, itaconic acid, maleic acid, fumaric acid, and anhydrides thereof.

[0080] Examples of vinyl cyanides include acrylonitrile and methacrylonitrile.

[0081] As the monomer component, from the viewpoint of more significantly achieving the above-mentioned effects, a compound selected from the group consisting of an acrylic compound, an aromatic vinyl compound, a heterocyclic vinyl compound, and an α,β-unsaturated carboxylic acid is preferable.

[0082] From the viewpoint of achieving the above-mentioned effects more significantly, the monomer component preferably contains an acrylic compound. The content of the acrylic compound may be, for example, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, or 100% by mass based on the total amount of the monomer component.

[0083] From the viewpoint of more significantly achieving the above-mentioned effects, the acrylic compound preferably contains a (meth)acrylic acid alkyl ester. The content of the (meth)acrylic acid alkyl ester may be, for example, 50% by mass or more based on the total amount of the monomer components, and from the viewpoint of further improving the water resistance of the composite material, it may be 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more. In addition, the content of the (meth)acrylic acid alkyl ester may be, for example, 99% by mass or less, 97% by mass or less, or 95% by mass or less based on the total amount of the monomer components.

[0084] The acrylic compound may further include a polar group-containing acrylic compound. The content of the polar group-containing acrylic compound may be, for example, 1% by mass or more, 3% by mass or more, or 5% by mass or more based on the total amount of the monomer components. The content of the polar group-containing acrylic compound may be, for example, 30% by mass or less, 25% by mass or less, 20% by mass or less, 15% by mass or less, or 10% by mass or less based on the total amount of the monomer components.

[0085] The monomer component may, for example, be selected from the group consisting of methyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, hydroxyethyl (meth)acrylate, (meth)acrylic acid, and styrene.

[0086] The monomer component may be appropriately selected so that the glass transition temperature (Tg) of the binder resin falls within a suitable range described later. The glass transition temperature (Tg) of the binder resin can be measured by the method described in the examples described later.

[0087] The glass transition temperature (Tg) of the binder resin can be estimated by the weight ratio of each monomer unit constituting the binder resin and the Tg of the homopolymer of each monomer using the FOX formula. With reference to the values ​​estimated by the FOX formula, the monomer components may be appropriately selected so that the glass transition temperature (Tg) of the binder resin falls within a suitable range.

[0088] The glass transition temperature (Tg) of the binder resin may be, for example, 25° C. or lower, and from the viewpoint of further improving the film-forming property, it is preferably 20° C. or lower, and more preferably 15° C. or lower. From the viewpoint of further improving the film-forming property at low temperatures, the glass transition temperature (Tg) of the binder resin is preferably 10° C. or lower, and more preferably 8° C. or lower, and may be 6° C. or lower. There is no particular restriction on the lower limit of the glass transition temperature (Tg) of the binder resin, and it may be, for example, −40° C. or higher, or −20° C. or higher.

[0089] The binder resin can be produced, for example, by emulsion polymerization of monomer components in a liquid medium (preferably an aqueous solvent) in the presence of an emulsifier, which forms emulsion particles containing the binder resin and the emulsifier.

[0090] The emulsifier may be any emulsifier capable of emulsifying the binder resin, and may be a known emulsifier. Examples of the emulsifier include anionic emulsifiers and nonionic emulsifiers.

[0091] From the viewpoint of easily obtaining a coating liquid with low corrosiveness to metals, the emulsifier is preferably a nonionic emulsifier. By selecting a nonionic emulsifier, it is believed that corrosion of metals caused by ions contained in other emulsifiers (e.g., anionic emulsifiers) is suppressed.

[0092] The nonionic emulsifier may be any known nonionic emulsifier that can emulsify the binder resin. Examples of the nonionic emulsifier include polyoxyalkylene alkyl ether, polyoxyalkylene alkylphenol ether, polyoxyalkylene fatty acid ester, polyoxyalkylene sorbitan fatty acid ester, etc., and polyoxyalkylene alkyl ether is preferred, and polyoxyethylene alkyl ether is more preferred.

[0093] The HLB value of the emulsifier is preferably 13 or more, more preferably 14 or more, from the viewpoint of easier emulsification of the binder resin, and is preferably 15 or more, more preferably 16 or more, from the viewpoint of further improving the film-forming properties of the coating liquid. Moreover, the HLB value of the emulsifier is preferably 19 or less, from the viewpoint of preventing a decrease in the water resistance of the composite material.

[0094] The content of the emulsifier may be, for example, 0.01 parts by mass or more relative to 100 parts by mass of the binder resin, and from the viewpoint of delaying the surface drying of the coating film and improving the film-forming property and the core drying property, it may be 0.1 parts by mass or more, 0.3 parts by mass or more, 0.5 parts by mass or more, 0.7 parts by mass or more, 0.9 parts by mass or more, or 1 part by mass or more. In addition, the content of the emulsifier may be, for example, 15 parts by mass or less relative to 100 parts by mass of the binder resin, and from the viewpoint of further improving the water resistance of the composite material, it may be 12 parts by mass or less, 10 parts by mass or less, 8 parts by mass or less, or 6 parts by mass or less.

[0095] The average particle size of the emulsion particles may be, for example, 50 nm or more, 70 nm or more, 90 nm or more, or 100 nm or more, and may be, for example, 400 nm or less, 350 nm or less, or 300 nm or less.

[0096] The content of the binder resin in the coating liquid may be, for example, 30% by mass or more, 35% by mass or more, 40% by mass or more, or 45% by mass or more, based on the total amount of nonvolatile content in the coating liquid. The content of the binder resin in the coating liquid may be, for example, 80% by mass or less, 75% by mass or less, or 70% by mass or less, based on the total amount of nonvolatile content in the coating liquid.

[0097] The content of the binder resin in the coating liquid may be appropriately adjusted so that the content of the binder resin in the composite material falls within a suitable range described below.

[0098] The content of the binder resin in the composite material may be, for example, 1 vol% or more, 3 vol% or more, 5 vol% or more, or 10 vol% or more based on the total volume of the composite material. The content of the binder resin in the composite material may be, for example, 40 vol% or less, 30 vol% or less, 25 vol% or less, or 20 vol% or less based on the total volume of the composite material.

[0099] <Glass fiber> The glass fibers act as anchors between the aerogel particles, further improving the strength of the composite material.

[0100] The fiber diameter of the glass fiber may be, for example, 0.01 μm or more, and from the viewpoint of coating film strength, may be 0.1 μm or more, 1 μm or more, or 3 μm or more. The fiber diameter of the glass fiber may be, for example, 100 μm or less, and from the viewpoint of coating film smoothness, may be 50 μm or less, or 30 μm or less.

[0101] The fiber length of the glass fiber may be, for example, 0.1 mm or more, and from the viewpoint of coating strength, may be 1 mm or more, 1.5 mm or more, 2 mm or more, or 3 mm or more. The fiber diameter of the glass fiber may be, for example, 20 mm or less, and from the viewpoint of dispersibility and coating liquid dischargeability, may be 7 mm or less, or 5 mm or less.

[0102] The content of glass fibers in the coating liquid may be, for example, 0.5% by mass or more based on the total amount of non-volatile content in the coating liquid, and from the viewpoint of coating film strength, may be 2% by mass or more, 3% by mass or more, or 5% by mass or more. The content of glass fibers in the coating liquid may be, for example, 15% by mass or less based on the total amount of non-volatile content in the coating liquid, and from the viewpoint of dispersibility and coating liquid dischargeability, may be 12% by mass or less, or 10% by mass or less.

[0103] The content of the glass fiber in the coating liquid may be appropriately adjusted so that the contents of the binder resin and the emulsifier in the composite material are within the suitable ranges described below.

[0104] The glass fiber content in the composite material may be, for example, 0.1 volume % or more, 0.2 volume % or more, 0.3 volume % or more, or 0.4 volume % or more, based on the total volume of the composite material. The glass fiber content in the composite material may be, for example, 5 volume % or less, 3 volume % or less, or 2 volume % or less, based on the total volume of the composite material.

[0105] <Water-soluble polymer> The water-soluble polymer may have a hydrophobic group and is water-soluble.

[0106] Examples of the hydrophobic group include an alkyl group (preferably a long-chain alkyl group having 6 to 26 carbon atoms), an ester group, an alkoxy group, a halogen, etc. Among these, the hydrophobic group is preferably an alkyl group, more preferably a long-chain alkyl group having 6 to 26 carbon atoms, still more preferably a long-chain alkyl group having 8 to 26 carbon atoms, still more preferably a long-chain alkyl group having 10 to 26 carbon atoms, may be a long-chain alkyl group having 12 to 26 carbon atoms, or may be a long-chain alkyl group having 15 to 26 carbon atoms.

[0107] Examples of the water-soluble polymer include modified carboxyl vinyl polymers, modified polyether urethane, cellulose-based resins, polyethylene oxide, polyvinyl alcohol, polyacrylates, polyvinylpyrrolidone, dextrin-based resins, chitin-based resins, and chitosan-based resins.

[0108] As the water-soluble polymer, a cellulose-based resin can be suitably used, such as methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, and modified products obtained by further modifying these (e.g., hydrophobizing them), etc.

[0109] The cellulose-based resin is preferably a cellulose-based resin having an alkyl group, more preferably a cellulose-based resin having a long-chain alkyl group having 6 to 26 carbon atoms. With such a cellulose-based resin, the effects of the present invention are more pronounced. The carbon number of the long-chain alkyl group is preferably 6 to 26, more preferably 8 to 26, even more preferably 10 to 26, still more preferably 12 to 26, and even more preferably 15 to 26.

[0110] In the cellulose-based resin, the content of the long-chain alkyl group having 6 to 26 carbon atoms is preferably 0.01 to 5 mass %, and more preferably 0.01 to 3 mass %, based on the total amount of the cellulose-based resin.

[0111] The cellulose-based resin is preferably, for example, a cellulose-based resin having a structural unit represented by the following formula (A-1). [ka]

[0112] In formula (A-1), R A is a hydrogen atom, an alkyl group, a hydroxyalkyl group, -R A1 -OR A2 A group represented by R A1 represents an alkanediyl group or a hydroxyalkanediyl group, R A2 represents an alkyl group.) or -(R A3 O) n A group represented by H (R A3 represents an alkanediyl group, and n represents an integer of 2 or more. A may be the same or different from each other. However, three R A At least one of the groups is an alkyl group or -R A1 -OR A2 It is a group represented by the following formula:

[0113] In formula (A-1), R A The alkyl group in R is preferably an alkyl group having 1 to 26 carbon atoms. AThe alkyl group in is more preferably a short-chain alkyl group having 1 to 3 carbon atoms, or a long-chain alkyl group having 6 to 26 carbon atoms. The long-chain alkyl group preferably has 8 to 26 carbon atoms, more preferably 10 to 26 carbon atoms, even more preferably 12 to 26 carbon atoms, and even more preferably 15 to 26 carbon atoms.

[0114] In formula (A-1), R A The hydroxyalkyl group in is preferably a hydroxyalkyl group having 1 to 26 carbon atoms, more preferably a hydroxyalkyl group having 1 to 10 carbon atoms, and further preferably a hydroxyalkyl group having 1 to 5 carbon atoms.

[0115] In formula (A-1), R A1 The alkanediyl group in R is preferably an alkanediyl group having 1 to 26 carbon atoms, more preferably an alkanediyl group having 1 to 10 carbon atoms, and further preferably an alkanediyl group having 1 to 5 carbon atoms. A1 The hydroxyalkanediyl group in the formula (I) is preferably a hydroxyalkanediyl group having 1 to 26 carbon atoms, more preferably a hydroxyalkanediyl group having 1 to 10 carbon atoms, and even more preferably a hydroxyalkanediyl group having 1 to 5 carbon atoms.

[0116] In formula (A-1), R A2 is preferably an alkyl group having 1 to 26 carbon atoms. A2 The alkyl group in is preferably a short-chain alkyl group having 1 to 3 carbon atoms or a long-chain alkyl group having 6 to 26 carbon atoms, and more preferably a long-chain alkyl group. The long-chain alkyl group preferably has 8 to 26 carbon atoms, more preferably 10 to 26 carbon atoms, even more preferably 12 to 26 carbon atoms, and even more preferably 15 to 26 carbon atoms.

[0117] In formula (A-1), R A3 As the alkanediyl group, an alkanediyl group having 2 to 3 carbon atoms is preferable, and an alkanediyl group having 3 carbon atoms is more preferable.

[0118] In formula (A-1), three R AAt least one of the R A At least one of them is -R A1 -OR A2 and R A2 is preferably a long chain alkyl group.

[0119] The content of the water-soluble polymer in the coating liquid may be, for example, 0.03% by mass or more based on the total amount of non-volatile content in the coating liquid, and from the viewpoint of further improving the dispersibility of the aerogel particles, it may be 0.05% by mass or more, 0.07% by mass or more, 0.09% by mass or more, 0.2% by mass or more, 0.4% by mass or more, 0.6% by mass or more, or 0.8% by mass or more. The content of the water-soluble polymer in the coating liquid may be, for example, 6% by mass or less based on the total amount of non-volatile content in the coating liquid, and from the viewpoint of further improving the water resistance of the composite material, it may be 5% by mass or less, 4% by mass or less, or 3% by mass or less.

[0120] The content of the water-soluble polymer in the coating liquid may be, for example, 0.1 parts by mass or more relative to 100 parts by mass of the aerogel particles, and from the viewpoint of further improving the dispersibility of the aerogel particles, it may be 0.5 parts by mass or more, 1 part by mass or more, 2 parts by mass or more, or 3 parts by mass or more. Moreover, from the viewpoint of further improving the water resistance of the composite material, the content of the water-soluble polymer in the coating liquid may be, for example, 20 parts by mass or less, 15 parts by mass or less, or 10 parts by mass or less relative to 100 parts by mass of the aerogel particles.

[0121] The content of the water-soluble polymer in the coating liquid may be appropriately adjusted so that the content of the water-soluble polymer in the composite material falls within a suitable range described below.

[0122] The content of the water-soluble polymer in the composite material may be, for example, 0.01 vol% or more, 0.05 vol% or more, 0.1 vol% or more, or 0.15 vol% or more, based on the total volume of the composite material. The content of the water-soluble polymer in the composite material may be, for example, 1.5 vol% or less, or 1 vol% or less, based on the total volume of the composite material.

[0123] <Aerogel> In this embodiment, the term "aerogel" refers to aerogel in a broad sense, namely, "gel comprised of a microporous solid in which the dispersed phase is a gas."

[0124] The aerogel of this embodiment is, for example, a silica aerogel mainly composed of silica. Examples of the silica aerogel include so-called organic-inorganic hybrid silica aerogels into which an organic group (such as a methyl group) or an organic chain is introduced.

[0125] The aerogel of the present embodiment may have the following aspects, for example. By employing each aspect, it is possible to obtain an aerogel having the heat insulating property, flame retardancy, heat resistance, and flexibility according to each aspect.

[0126] (First aspect) The aerogel according to the present embodiment may have a structure represented by the following general formula (1): The aerogel according to the present embodiment may have a structure represented by the following general formula (1a) as a structure including the structure represented by formula (1). [ka] [ka]

[0127] In formula (1) and formula (1a), R 1 and R 2 each independently represents an alkyl group or an aryl group; R 3 and R 4 Each of R independently represents an alkylene group. Examples of the aryl group include a phenyl group and a substituted phenyl group. Examples of the substituent of the substituted phenyl group include an alkyl group, a vinyl group, a mercapto group, an amino group, a nitro group, and a cyano group. p represents an integer of 1 to 50. In formula (1a), when two or more R1 may be the same or different, and similarly, two or more R 2 may be the same or different. In formula (1a), two R 3 may be the same or different, and similarly, two R 4 may be the same or different.

[0128] By introducing the structure represented by the above formula (1) or formula (1a) into the skeleton of an aerogel as an aerogel component, an aerogel having low thermal conductivity and flexibility can be obtained. 1 and R 2 Each of R independently represents an alkyl group having 1 to 6 carbon atoms, a phenyl group, etc., and the alkyl group may be a methyl group, etc. 3 and R 4 are each independently an alkylene group having 1 to 6 carbon atoms, and examples of the alkylene group include an ethylene group, a propylene group, etc. In formula (1a), p can be an integer of 2 to 30, and may be an integer of 5 to 20.

[0129] (Second Aspect) The aerogel of this embodiment has a ladder-type structure having struts and bridges, and the bridges can have a structure represented by the following general formula (2). By introducing such a ladder-type structure into the skeleton of the aerogel as an aerogel component, the heat resistance and mechanical strength can be improved. In this embodiment, the "ladder-type structure" refers to a structure having two struts and bridges connecting the struts (having a so-called "ladder" shape). In this embodiment, the skeleton of the aerogel may have a ladder-type structure, but the aerogel may also have a ladder-type structure partially. [ka]

[0130] In formula (2), R 5 and R6 Each independently represents an alkyl group or an aryl group, and b represents an integer of 1 to 50. Here, examples of the aryl group include a phenyl group and a substituted phenyl group. Examples of the substituent of the substituted phenyl group include an alkyl group, a vinyl group, a mercapto group, an amino group, a nitro group, and a cyano group. In addition, in the formula (2), when b is an integer of 2 or more, two or more R 5 may be the same or different, and similarly, two or more R 6 may be the same or different.

[0131] By introducing the above structure into the skeleton of an aerogel as an aerogel component, an aerogel having superior flexibility to, for example, an aerogel having a structure derived from a conventional ladder-type silsesquioxane can be obtained.

[0132] The structure that serves as the support portion and its chain length, as well as the spacing between the structures that serve as the bridging portions are not particularly limited. From the viewpoint of further improving heat resistance and mechanical strength, the ladder structure may have a ladder structure represented by the following general formula (3). [ka]

[0133] In formula (3), R 5 , R 6 , R 7 and R 8 each independently represents an alkyl group or an aryl group, a and c each independently represent an integer of 1 to 3000, and b represents an integer of 1 to 50. Here, examples of the aryl group include a phenyl group and a substituted phenyl group. Examples of the substituent of the substituted phenyl group include an alkyl group, a vinyl group, a mercapto group, an amino group, a nitro group, and a cyano group. In addition, when b is an integer of 2 or more in formula (3), two or more R 5 may be the same or different, and similarly, two or more R 6 In addition, in formula (3), when a is an integer of 2 or more, there are two or more R 7may be the same or different, and similarly, when c is an integer of 2 or more, two or more R 8 may be the same or different.

[0134] In order to obtain better flexibility, R 5 , R 6 , R 7 and R 8 (However, R 7 and R 8 (only in formula (3)) each independently includes an alkyl group having 1 to 6 carbon atoms, a phenyl group, etc., and the alkyl group includes a methyl group, etc. In formula (3), a and c each independently can be 6 to 2000, but may be 10 to 1000. In formulas (2) and (3), b can be 2 to 30, but may be 5 to 20.

[0135] (Third Aspect) The aerogel of this embodiment may be a dried product of a wet gel (obtained by drying a wet gel produced from a sol) which is a condensate of a sol containing at least one selected from the group consisting of a silicon compound having a hydrolyzable functional group or a condensable functional group, and a hydrolysis product of a silicon compound having a hydrolyzable functional group. The aerogel described above may also be obtained by drying a wet gel produced from a sol containing a silicon compound or the like in this way.

[0136] As the silicon compound having a hydrolyzable functional group or a condensable functional group, a polysiloxane compound can be used. That is, the sol can contain at least one compound selected from the group consisting of a polysiloxane compound having a hydrolyzable functional group or a condensable functional group, and a hydrolysis product of a polysiloxane compound having a hydrolyzable functional group (hereinafter, sometimes referred to as a "polysiloxane compound group").

[0137] The functional group in the polysiloxane compound is not particularly limited, but may be a group that reacts with the same functional group or reacts with another functional group. Examples of hydrolyzable functional groups include alkoxy groups. Examples of condensable functional groups include hydroxyl groups, silanol groups, carboxyl groups, and phenolic hydroxyl groups. The hydroxyl group may be contained in a hydroxyl group-containing group such as a hydroxyalkyl group. The polysiloxane compound having a hydrolyzable functional group or a condensable functional group may further have a reactive group (a functional group that does not fall under the category of hydrolyzable functional group and condensable functional group) different from the hydrolyzable functional group and the condensable functional group. Examples of the reactive group include an epoxy group, a mercapto group, a glycidoxy group, a vinyl group, an acryloyl group, a methacryloyl group, and an amino group. The epoxy group may be contained in an epoxy group-containing group such as a glycidoxy group. The polysiloxane compound having these functional groups and reactive groups may be used alone or in a mixture of two or more types. Among these functional groups and reactive groups, for example, groups that improve the flexibility of the aerogel include alkoxy groups, silanol groups, hydroxyalkyl groups, etc., and among these, alkoxy groups and hydroxyalkyl groups can further improve the compatibility of the sol. In addition, from the viewpoint of improving the reactivity of the polysiloxane compound and reducing the thermal conductivity of the aerogel, the number of carbon atoms of the alkoxy group and hydroxyalkyl group can be 1 to 6, but from the viewpoint of further improving the flexibility of the aerogel, it may be 2 to 5 or 2 to 4.

[0138] (Fourth aspect) The aerogel according to the present embodiment may further contain silica particles in addition to the aerogel component in order to further increase toughness and to achieve even better heat insulation and flexibility. An aerogel containing an aerogel component and silica particles can also be called an aerogel composite. Although the aerogel composite is a composite of the aerogel component and the silica particles, it has a cluster structure that is characteristic of aerogel and is considered to have a three-dimensional fine porous structure.

[0139] The aerogel containing the aerogel component and silica particles can be said to be a dried product of a wet gel which is a condensation product of a sol containing at least one selected from the group consisting of a silicon compound having a hydrolyzable functional group or a condensable functional group, and a hydrolysis product of a silicon compound having a hydrolyzable functional group, and silica particles. Therefore, the description of the first to third aspects can be appropriately applied to the aerogel according to this embodiment.

[0140] The silica particles can be used without any particular limitation, and include amorphous silica particles. The amorphous silica particles can be fused silica particles, fumed silica particles, colloidal silica particles, etc. Among them, colloidal silica particles have high monodispersity and are easy to suppress aggregation in sol. The silica particles may be silica particles having a hollow structure, a porous structure, etc.

[0141] The shape of the silica particles is not particularly limited, and examples thereof include spherical, cocoon-shaped, and association-shaped. Among these, by using spherical particles as the silica particles, aggregation in the sol can be easily suppressed. The average primary particle diameter of the silica particles may be 1 nm or more, 5 nm or more, or 20 nm or more from the viewpoint of easily imparting appropriate strength and flexibility to the aerogel and easily obtaining an aerogel having excellent shrinkage resistance during drying. The average primary particle diameter of the silica particles may be 500 nm or less, 300 nm or less, or 100 nm or less from the viewpoint of easily suppressing the solid thermal conduction of the silica particles and easily obtaining an aerogel having excellent heat insulation. From these viewpoints, the average primary particle diameter of the silica particles may be 1 to 500 nm, 5 to 300 nm, or 20 to 100 nm.

[0142] In this embodiment, the average particle size of the aerogel components and the average primary particle size of the silica particles can be obtained by directly observing the aerogel using a scanning electron microscope (hereinafter abbreviated as "SEM"). The "diameter" here means the diameter when the cross section of the particle exposed on the cross section of the aerogel is regarded as a circle. In addition, the "diameter when the cross section is regarded as a circle" means the diameter of the perfect circle when the area of ​​the cross section is replaced with a perfect circle of the same area. In addition, when calculating the average particle size, the diameter of the circle is calculated for 100 particles and the average is taken.

[0143] The average particle size of silica particles can also be measured from the raw material. For example, the biaxial average primary particle size is calculated from the results of observing 20 arbitrary particles by SEM as follows. That is, taking colloidal silica particles dispersed in water with a normal solid content concentration of about 5 to 40% by mass as an example, a chip obtained by cutting a wafer with pattern wiring into 2 cm squares is immersed in a dispersion of colloidal silica particles for about 30 seconds, and then the chip is rinsed with pure water for about 30 seconds and dried by nitrogen blow. Thereafter, the chip is placed on a sample stage for SEM observation, an accelerating voltage of 10 kV is applied, and the silica particles are observed at a magnification of 100,000 times, and an image is taken. 20 silica particles are arbitrarily selected from the obtained image, and the average of the particle sizes of those particles is taken as the average particle size.

[0144] <Aerogel particles> The aerogel particles in this embodiment can be obtained, for example, by pulverizing a bulk aerogel as described later.

[0145] The average particle size (D50) of the aerogel particles (also referred to as the average diameter) can be 0.1 to 1000 μm, but may be 0.5 to 700 μm, 1 to 500 μm, 3 to 100 μm, or 5 to 50 μm. When the average particle size (D50) of the aerogel particles is large, it is easy to obtain aerogel particles with excellent dispersibility, handleability, etc. On the other hand, when the average particle size (D50) is small, it is easy to obtain aerogel particles with excellent dispersibility. The average particle size (D50) of the aerogel particles can be appropriately adjusted by the grinding method and grinding conditions, sieve, classification method, etc.

[0146] The average particle diameter (D50) of aerogel particles can be measured by a laser diffraction / scattering method. For example, aerogel particles are added to a solvent (ethanol) so that the content of the aerogel particles is 0.05-5% by mass, and the aerogel particles are dispersed by vibrating with a 50W ultrasonic homogenizer for 15-30 minutes. Then, about 10 mL of the dispersion is injected into a laser diffraction / scattering type particle size distribution measuring device, and the particle size is measured at 25°C, with a refractive index of 1.3 and an absorption of 0. Then, the particle diameter at an integrated value of 50% (volume basis) in this particle size distribution is taken as the average particle diameter D50. As a measuring device, for example, Microtrac MT3000 (manufactured by Nikkiso Co., Ltd., product name) can be used.

[0147] Commercially available aerogel particles may also be used, such as ENOVA MT1100 (manufactured by CABOT) and AeroVa (manufactured by JIOS AEROGEL CORPORATION).

[0148] In this embodiment, the amount of aerogel particles in the coating liquid is preferably such that the content of the aerogel particles in the composite material is 70 volume % or more, more preferably 72 volume % or more, and even more preferably 74 volume % or more, based on the total volume of the composite material. The amount of aerogel particles in the coating liquid may be such that the content of the aerogel particles in the composite material is, for example, 99 volume % or less, 98 volume % or less, or 97 volume % or less, based on the total volume of the composite material.

[0149] <Method of manufacturing aerogel particles> The method for producing the aerogel particles is not particularly limited, but for example, the aerogel particles can be produced by the following method.

[0150] The aerogel particles of this embodiment can be produced by a production method mainly including a sol production process, a wet gel production process in which the sol obtained in the sol production process is gelled and then aged to obtain a wet gel, a washing and solvent replacement process in which the wet gel obtained in the wet gel production process is washed and (if necessary) solvent-replaced, a drying process in which the washed and solvent-replaced wet gel is dried, and a crushing process in which the aerogel obtained by drying is crushed.

[0151] Alternatively, the composition may be produced by a production method mainly including a sol generation step, a wet gel generation step, a wet gel crushing step of crushing the wet gel obtained in the wet gel generation step, a washing and solvent replacement step, and a drying step.

[0152] The size of the obtained aerogel particles can be further uniformed by sieving, classification, etc. By adjusting the particle size, the dispersibility can be improved. In addition, "sol" means a state before the gelation reaction occurs, and in this embodiment, the silicon compound and, in some cases, silica particles are dissolved or dispersed in a solvent. In addition, the wet gel means a gel solid in a wet state that does not have fluidity even though it contains a liquid medium.

[0153] (Sol generation process) The sol generation process is a process in which a silicon compound and, optionally, silica particles (or a solvent containing silica particles) are mixed to carry out a hydrolysis reaction, and then a sol is generated. In this process, an acid catalyst may be further added to the solvent in order to promote the hydrolysis reaction. In addition, as shown in Japanese Patent No. 5250900, a surfactant, a thermally hydrolyzable compound, etc. may also be added to the solvent. Furthermore, for the purpose of suppressing heat radiation, etc., components such as carbon graphite, an aluminum compound, a magnesium compound, a silver compound, and a titanium compound may be added to the solvent.

[0154] As the solvent, for example, water or a mixture of water and alcohol can be used. Examples of alcohol include methanol, ethanol, n-propanol, 2-propanol, n-butanol, 2-butanol, and t-butanol. Among these, examples of alcohol that have low surface tension and low boiling point in terms of reducing the interfacial tension with the gel wall include methanol, ethanol, and 2-propanol. These may be used alone or in combination of two or more.

[0155] For example, when alcohol is used as the solvent, the amount of alcohol can be 4 to 8 mol per mole of the total amount of the silicon compounds and the polysiloxane compounds, but may also be 4 to 6.5, or may also be 4.5 to 6 mol. By making the amount of alcohol 4 mol or more, it becomes easier to obtain good compatibility, and by making it 8 mol or less, it becomes easier to suppress shrinkage of the gel.

[0156] Examples of the acid catalyst include inorganic acids such as hydrofluoric acid, hydrochloric acid, nitric acid, sulfuric acid, sulfurous acid, phosphoric acid, phosphorous acid, hypophosphorous acid, bromic acid, chloric acid, chlorous acid, hypochlorous acid, etc.; acid phosphates such as acid aluminum phosphate, acid magnesium phosphate, and acid zinc phosphate; and organic carboxylic acids such as acetic acid, formic acid, propionic acid, oxalic acid, malonic acid, succinic acid, citric acid, malic acid, adipic acid, and azelaic acid. Among these, an organic carboxylic acid can be mentioned as an acid catalyst that further improves the water resistance of the obtained aerogel. The organic carboxylic acid can be acetic acid, but it can also be formic acid, propionic acid, oxalic acid, malonic acid, etc. These can be used alone or in a mixture of two or more types.

[0157] By using an acid catalyst, the hydrolysis reaction of the silicon compound can be accelerated, and the sol can be obtained in a shorter time.

[0158] The amount of the acid catalyst added may be 0.001 to 0.1 part by mass per 100 parts by mass of the total amount of the polysiloxane compounds and the silicon compounds.

[0159] The surfactant may be a nonionic surfactant, an ionic surfactant, etc. These may be used alone or in combination of two or more kinds.

[0160] As the nonionic surfactant, for example, a compound containing a hydrophilic part such as polyoxyethylene and a hydrophobic part mainly composed of an alkyl group, a compound containing a hydrophilic part such as polyoxypropylene, etc. can be used. Examples of the compound containing a hydrophilic part such as polyoxyethylene and a hydrophobic part mainly composed of an alkyl group include polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene alkyl ether, etc. Examples of the compound containing a hydrophilic part such as polyoxypropylene include polyoxypropylene alkyl ether, block copolymers of polyoxyethylene and polyoxypropylene, etc.

[0161] Examples of the ionic surfactant include cationic surfactant, anionic surfactant, amphoteric surfactant, etc. Examples of the cationic surfactant include cetyltrimethylammonium bromide, cetyltrimethylammonium chloride, etc. Examples of the anionic surfactant include sodium dodecylsulfonate, etc. Examples of the amphoteric surfactant include amino acid surfactant, betaine surfactant, amine oxide surfactant, etc. Examples of the amino acid surfactant include acyl glutamic acid, etc. Examples of the betaine surfactant include lauryl dimethyl amino acetate betaine, stearyl dimethyl amino acetate betaine, etc. Examples of the amine oxide surfactant include lauryl dimethyl amine oxide.

[0162] These surfactants are believed to act to reduce the difference in chemical affinity between the solvent in the reaction system and the growing siloxane polymer in the wet gel formation process described below, thereby suppressing phase separation.

[0163] The amount of the surfactant to be added depends on the type of surfactant or the type and amount of the silicon compound, but can be, for example, 1 to 100 parts by mass per 100 parts by mass of the total amount of the polysiloxane compounds and the silicon compounds, or 5 to 60 parts by mass.

[0164] It is believed that the thermally hydrolyzable compound generates a base catalyst by thermal hydrolysis, makes the reaction solution basic, and promotes the sol-gel reaction in the wet gel production step described below. Therefore, the thermally hydrolyzable compound is not particularly limited as long as it is a compound that can make the reaction solution basic after hydrolysis, and examples of the thermally hydrolyzable compound include urea; acid amides such as formamide, N-methylformamide, N,N-dimethylformamide, acetamide, N-methylacetamide, and N,N-dimethylacetamide; and cyclic nitrogen compounds such as hexamethylenetetramine. Among these, urea is particularly likely to achieve the above-mentioned promotion effect.

[0165] The amount of the thermohydrolyzable compound to be added is not particularly limited as long as it is an amount that can sufficiently promote the sol-gel reaction in the wet gel generation step described below. For example, when urea is used as the thermohydrolyzable compound, the amount of the compound to be added can be 1 to 200 parts by mass relative to 100 parts by mass of the total amount of the polysiloxane compound group and the silicon compound group. The amount of the compound to be added may be 2 to 150 parts by mass. By making the amount of the compound to be added 1 part by mass or more, it becomes easier to obtain good reactivity, and by making the amount of the compound to be added 200 parts by mass or less, it becomes easier to suppress the precipitation of crystals and the decrease in gel density.

[0166] The hydrolysis in the sol production step may be carried out for 10 minutes to 24 hours in a temperature environment of 20 to 60° C., or for 5 minutes to 8 hours in a temperature environment of 50 to 60° C., depending on the types and amounts of the silicon compound, silica particles, acid catalyst, surfactant, etc. in the mixed liquid. This allows the hydrolyzable functional groups in the silicon compound to be sufficiently hydrolyzed, and the hydrolysis product of the silicon compound can be obtained more reliably.

[0167] However, when a thermally hydrolyzable compound is added to the solvent, the temperature environment of the sol generation step may be adjusted to a temperature that suppresses hydrolysis of the thermally hydrolyzable compound and suppresses gelation of the sol. The temperature at this time may be any temperature as long as it can suppress hydrolysis of the thermally hydrolyzable compound. For example, when urea is used as the thermally hydrolyzable compound, the temperature environment of the sol generation step may be 0 to 40°C, but may also be 10 to 30°C.

[0168] (Wet gel production process) The wet gel forming step is a step of gelling the sol obtained in the sol forming step, followed by aging to obtain a wet gel. In this step, a base catalyst can be used to promote gelling.

[0169] Examples of the base catalyst include carbonates such as calcium carbonate, potassium carbonate, sodium carbonate, barium carbonate, magnesium carbonate, lithium carbonate, ammonium carbonate, copper (II) carbonate, iron (II) carbonate, and silver (I) carbonate; hydrogen carbonates such as calcium hydrogen carbonate, potassium hydrogen carbonate, sodium hydrogen carbonate, and ammonium hydrogen carbonate; alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, potassium hydroxide, and cesium hydroxide; ammonium compounds such as ammonium hydroxide, ammonium fluoride, ammonium chloride, and ammonium bromide; basic sodium phosphates such as sodium metaphosphate, sodium pyrophosphate, and sodium polyphosphate; allylamine, diallylamine, triallylamine, isopropylamine, diisopropylamine, ethylamine, diethylamine, Aliphatic amines such as amine, triethylamine, 2-ethylhexylamine, 3-ethoxypropylamine, diisobutylamine, 3-(diethylamino)propylamine, di-2-ethylhexylamine, 3-(dibutylamino)propylamine, tetramethylethylenediamine, t-butylamine, sec-butylamine, propylamine, 3-(methylamino)propylamine, 3-(dimethylamino)propylamine, 3-methoxyamine, dimethylethanolamine, methyldiethanolamine, diethanolamine, and triethanolamine; nitrogen-containing heterocyclic compounds such as morpholine, N-methylmorpholine, 2-methylmorpholine, piperazine and its derivatives, piperidine and its derivatives, and imidazole and its derivatives. Among these, ammonium hydroxide (aqueous ammonia) is highly volatile and does not easily remain in the aerogel particles after drying, so it is not likely to impair water resistance, and is also excellent in terms of economy. The above-mentioned base catalysts may be used alone or in a mixture of two or more types.

[0170] By using a base catalyst, the dehydration condensation reaction or the dealcoholization condensation reaction of the silicon compound and the silica particles in the sol can be promoted, and the gelation of the sol can be performed in a shorter time. This also makes it possible to obtain a wet gel with higher strength (rigidity). In particular, since ammonia is highly volatile and does not easily remain in the aerogel particles, the use of ammonia as a base catalyst makes it possible to obtain aerogel particles with better water resistance.

[0171] The amount of the base catalyst added can be 0.5 to 5 parts by mass, but may be 1 to 4 parts by mass, relative to 100 parts by mass of the total amount of the polysiloxane compounds and the silicon compounds. By making the amount 0.5 parts by mass or more, gelation can be performed in a shorter time, and by making the amount 5 parts by mass or less, the decrease in water resistance can be further suppressed.

[0172] The gelation of the sol in the wet gel generating step may be carried out in a sealed container so that the solvent and the base catalyst do not volatilize. The gelation temperature may be 30 to 90°C, but may be 40 to 80°C. By setting the gelation temperature at 30°C or higher, the gelation can be carried out in a shorter time, and a wet gel with higher strength (rigidity) can be obtained. Furthermore, by setting the gelation temperature at 90°C or lower, it becomes easier to suppress the volatilization of the solvent (especially alcohol), so that gelation can be carried out while suppressing volumetric shrinkage.

[0173] The aging in the wet gel production step may be performed in a sealed container so that the solvent and the base catalyst do not volatilize. The aging strengthens the bonds between the components that make up the wet gel, and as a result, a wet gel with sufficient strength (rigidity) to suppress shrinkage during drying can be obtained. The aging temperature can be 30 to 90°C, but may be 40 to 80°C. By setting the aging temperature at 30°C or higher, a wet gel with higher strength (rigidity) can be obtained, and by setting the aging temperature at 90°C or lower, it becomes easier to suppress the volatilization of the solvent (especially alcohol), so that gelation can be performed while suppressing volumetric shrinkage.

[0174] Since it is often difficult to determine the end time of the gelation of the sol, the gelation of the sol and the subsequent aging may be carried out continuously in a series of operations.

[0175] The gelation time and aging time can be appropriately set depending on the gelation temperature and aging temperature. When silica particles are contained in the sol, the gelation time can be particularly shortened compared to when silica particles are not contained. This is presumably because the silanol group or reactive group of the silicon compound in the sol forms a hydrogen bond or a chemical bond with the silanol group of the silica particles. The gelation time can be 10 to 120 minutes, but may be 20 to 90 minutes. By setting the gelation time to 10 minutes or more, a homogeneous wet gel can be easily obtained, and by setting it to 120 minutes or less, the washing and solvent replacement process to the drying process described later can be simplified. In addition, the total time of the gelation time and aging time as a whole process of gelation and aging can be 4 to 480 hours, but may be 6 to 120 hours. By setting the total of the gelation time and aging time to 4 hours or more, a wet gel with higher strength (rigidity) can be obtained, and by setting it to 480 hours or less, the effect of aging can be more easily maintained.

[0176] In order to reduce the density of the resulting aerogel particles or to increase the average pore size, the gelation temperature and aging temperature may be increased within the above ranges, or the total time of the gelation time and aging time may be increased within the above ranges. In addition, in order to increase the density of the resulting aerogel particles or to decrease the average pore size, the gelation temperature and aging temperature may be decreased within the above ranges, or the total time of the gelation time and aging time may be shortened within the above ranges.

[0177] (Wet gel crushing process) When the wet gel crushing step is performed, the wet gel obtained in the wet gel production step is crushed. The crushing can be performed, for example, by putting the wet gel in a Henshall mixer, or by performing the wet gel production step in a mixer and operating the mixer under appropriate conditions (rotation speed and time). More simply, the wet gel can be placed in a sealable container, or by performing the wet gel production step in a sealable container, and shaking for an appropriate time using a shaking device such as a shaker. If necessary, the particle size of the wet gel can also be adjusted using a jet mill, roller mill, bead mill, or the like.

[0178] (Washing and solvent replacement process) The washing and solvent replacement process includes a process (washing process) of washing the wet gel obtained by the wet gel production process or the wet gel crushing process, and a process (solvent replacement process) of replacing the washing liquid in the wet gel with a solvent suitable for drying conditions (drying process described later). The washing and solvent replacement process can be carried out in a form in which only the solvent replacement process is carried out without performing the process of washing the wet gel, but from the viewpoint of reducing impurities such as unreacted substances and by-products in the wet gel and enabling the production of aerogel particles with higher purity, the wet gel may be washed.

[0179] In the washing step, the wet gel obtained in the wet gel generating step or the wet gel crushing step is washed. The washing can be repeatedly performed using, for example, water or an organic solvent. In this case, the washing efficiency can be improved by heating.

[0180] As the organic solvent, various organic solvents such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, acetone, methyl ethyl ketone, 1,2-dimethoxyethane, acetonitrile, hexane, toluene, diethyl ether, chloroform, ethyl acetate, tetrahydrofuran, methylene chloride, N,N-dimethylformamide, dimethyl sulfoxide, acetic acid, formic acid, etc. The above organic solvents may be used alone or in combination of two or more.

[0181] In the solvent replacement step described below, a solvent with low surface tension can be used to suppress the shrinkage of the gel due to drying. However, a solvent with low surface tension generally has extremely low mutual solubility with water. Therefore, when a solvent with low surface tension is used in the solvent replacement step, the organic solvent used in the washing step can be a hydrophilic organic solvent having high mutual solubility with both water and a solvent with low surface tension. The hydrophilic organic solvent used in the washing step can play the role of preliminary replacement for the solvent replacement step. Among the above organic solvents, examples of hydrophilic organic solvents include methanol, ethanol, 2-propanol, acetone, methyl ethyl ketone, etc. In addition, methanol, ethanol, methyl ethyl ketone, etc. are excellent in terms of economy.

[0182] The amount of water or organic solvent used in the washing step can be an amount that can sufficiently replace the solvent in the wet gel and wash it. The amount can be 3 to 10 times the volume of the wet gel. Washing can be repeated until the water content in the wet gel after washing is 10 mass% or less relative to the mass of silica.

[0183] The temperature environment in the washing step can be a temperature equal to or lower than the boiling point of the solvent used in washing. For example, when methanol is used, the temperature can be raised to about 30 to 60°C.

[0184] In the solvent replacement step, the solvent of the washed wet gel is replaced with a predetermined replacement solvent in order to suppress the shrinkage of the aerogel in the drying step. In this case, the replacement efficiency can be improved by heating. Specifically, the replacement solvent may be a low surface tension solvent as described below when drying is performed at a temperature below the critical point of the solvent used for drying in the drying step under atmospheric pressure. On the other hand, when supercritical drying is performed, the replacement solvent may be, for example, ethanol, methanol, 2-propanol, dichlorodifluoromethane, carbon dioxide, or a mixture of two or more of these.

[0185] An example of a solvent with low surface tension is a solvent having a surface tension of 30 mN / m or less at 20° C. The surface tension may be 25 mN / m or less, or 20 mN / m or less. Examples of low surface tension solvents include aliphatic hydrocarbons such as pentane (15.5), hexane (18.4), heptane (20.2), octane (21.7), 2-methylpentane (17.4), 3-methylpentane (18.1), 2-methylhexane (19.3), cyclopentane (22.6), cyclohexane (25.2), and 1-pentene (16.0); aromatic hydrocarbons such as benzene (28.9), toluene (28.5), m-xylene (28.7), and p-xylene (28.3); and halides such as dichloromethane (27.9), chloroform (27.2), carbon tetrachloride (26.9), 1-chloropropane (21.8), and 2-chloropropane (18.1). halogenated hydrocarbons; ethers such as ethyl ether (17.1), propyl ether (20.5), isopropyl ether (17.7), butyl ethyl ether (20.8), 1,2-dimethoxyethane (24.6); ketones such as acetone (23.3), methyl ethyl ketone (24.6), methyl propyl ketone (25.1), diethyl ketone (25.3); esters such as methyl acetate (24.8), ethyl acetate (23.8), propyl acetate (24.3), isopropyl acetate (21.2), isobutyl acetate (23.7), ethyl butyrate (24.6) etc. (The value in parentheses indicates the surface tension at 20℃, in [mN / m]). Among these, aliphatic hydrocarbons (hexane, heptane, etc.) have low surface tension and are excellent in the working environment. Among these, hydrophilic organic solvents such as acetone, methyl ethyl ketone, and 1,2-dimethoxyethane can be used as the organic solvent in the washing step. Among these, solvents having a boiling point of 100° C. or less at normal pressure may be used in terms of ease of drying in the drying step described below. The above solvents may be used alone or in combination of two or more.

[0186] The amount of the solvent used in the solvent replacement step can be an amount that can sufficiently replace the solvent in the wet gel after washing, and can be 3 to 10 times the volume of the wet gel.

[0187] The temperature environment in the solvent replacement step can be a temperature equal to or lower than the boiling point of the solvent used for replacement. For example, when heptane is used, the temperature can be raised to about 30 to 60°C.

[0188] In addition, when silica particles are contained in the gel, the solvent replacement process is not essential. The mechanism is assumed to be as follows. That is, the silica particles function as a support for the three-dimensional mesh-like skeleton, thereby supporting the skeleton and suppressing the shrinkage of the gel in the drying process. Therefore, it is considered that the gel can be directly subjected to the drying process without replacing the solvent used for washing. In this way, by using silica particles, it is possible to simplify the washing and solvent replacement processes to the drying process.

[0189] (drying process) In the drying step, the wet gel washed and (if necessary) solvent-substituted as described above is dried. This allows an aerogel (aerogel block or aerogel particles) to be obtained. That is, an aerogel can be obtained by drying the wet gel produced from the sol.

[0190] The drying method is not particularly limited, and known methods such as normal pressure drying, supercritical drying, or freeze drying can be used. Among these, normal pressure drying or supercritical drying can be used from the viewpoint of ease of manufacturing low-density aerogel. Furthermore, normal pressure drying can be used from the viewpoint of low-cost production. In this embodiment, normal pressure means 0.1 MPa (atmospheric pressure).

[0191] The aerogel can be obtained by drying the wet gel that has been washed and (if necessary) solvent-substituted at atmospheric pressure at a temperature below the critical point of the solvent used for drying. The drying temperature varies depending on the type of substituted solvent (or the solvent used for washing if solvent substitution is not performed), but can be 20 to 150°C, taking into consideration that drying at a high temperature may accelerate the evaporation rate of the solvent and cause large cracks in the gel. The drying temperature may be 60 to 120°C. The drying time varies depending on the volume of the wet gel and the drying temperature, but can be 4 to 120 hours. It should be noted that drying at normal pressure also includes applying a pressure below the critical point to accelerate drying within a range that does not impair productivity.

[0192] The aerogel can also be obtained by subjecting a wet gel that has been washed and (if necessary) solvent-substituted to supercritical drying. Supercritical drying can be performed by a known method. Examples of the supercritical drying method include a method of removing the solvent at a temperature and pressure equal to or higher than the critical point of the solvent contained in the wet gel, or a method of supercritical drying includes a method of immersing the wet gel in liquefied carbon dioxide under conditions of, for example, 20 to 25°C and about 5 to 20 MPa to replace all or a part of the solvent contained in the wet gel with carbon dioxide having a lower critical point than the solvent, and then removing the carbon dioxide alone or a mixture of carbon dioxide and the solvent.

[0193] The aerogel obtained by such normal pressure drying or supercritical drying may be further dried at normal pressure at 105 to 200°C for about 0.5 to 2 hours. This makes it easier to obtain an aerogel with low density and small pores. The additional drying may be performed at normal pressure at 150 to 200°C.

[0194] (Crushing process) When the wet gel crushing step is not performed, the aerogel obtained by drying (aerogel block) is crushed to obtain aerogel particles. For example, this can be done by putting the aerogel into a jet mill, roller mill, bead mill, hammer mill, etc., and operating it at an appropriate rotation speed for an appropriate time.

[0195] <Liquid medium> As the liquid medium, an aqueous solvent containing water is preferable. The aqueous solvent may contain an organic solvent other than water. The organic solvent may be any one that is compatible with water, and examples thereof include alcohols such as methanol, ethanol, isopropanol, butanol, ethylene glycol, and propylene glycol; ethers such as diethyl ether, tetrahydrofuran, and 1,4-dioxane; ketones such as acetone and methyl ethyl ketone; carboxylic acids such as acetic acid and propionic acid; and nitrogen-containing compounds such as acetonitrile, dimethylformamide, and triethylamine.

[0196] In this embodiment, the content of the liquid medium in the coating liquid is not particularly limited and may be appropriately changed depending on the desired viscosity of the coating liquid, etc. For example, the content of the liquid medium may be an amount that causes the non-volatile content of the coating liquid to fall within a suitable range described below.

[0197] The non-volatile content of the coating liquid may be, for example, 10% by mass or more, preferably 15% by mass or more, and more preferably 20% by mass or more. The non-volatile content of the coating liquid may be, for example, 70% by mass or less, preferably 60% by mass or less, and more preferably 50% by mass or less.

[0198] <Other ingredients> In this embodiment, the coating liquid may further contain other components in addition to those described above.

[0199] The coating liquid of the present embodiment may further contain, for example, a thickener, a pigment, a leveling agent, etc. Examples of the thickener include fine particles of fumed silica, clay minerals, and the like.

[0200] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments. EXAMPLES

[0201] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0202] Example 1 (1) Emulsion production A reaction vessel equipped with a stirrer, a thermometer, a cooling tube, and a dropping funnel was charged with 160 parts by mass of ion-exchanged water and 1.2 parts by mass of a nonionic emulsifier (Emulgen 1150S-60, a 60% aqueous solution of polyoxyethylene alkyl ether, manufactured by Kao Corporation, HLB value: 18.5), stirred, and heated to 65°C, after which nitrogen was passed through the reaction vessel to remove dissolved oxygen.

[0203] Next, 274 parts by mass of butyl acrylate, 173.5 parts by mass of methyl methacrylate, 24 parts by mass of 2-hydroxyethyl methacrylate, 9 parts by mass of methacrylic acid, 215 parts by mass of ion-exchanged water, and 48.8 parts by mass of a nonionic emulsifier (Emulgen 1150S-60, a 60% aqueous solution of polyoxyethylene alkyl ether, manufactured by Kao Corporation, HLB value: 18.5) were mixed and emulsified in a homomixer to obtain a monomer emulsion.

[0204] 3% of this monomer emulsion was added to the reaction vessel under stirring, and 0.7 parts by mass of "Trigonox A-W70" (70% aqueous solution of tert-butyl hydroperoxide, manufactured by Kayaku Nouryon Co., Ltd.) and 0.23 parts by mass of ascorbic acid were added as a radical polymerization initiator, and reacted for 15 minutes. Next, the remaining 97% of the monomer emulsion, a solution in which 0.9 parts by mass of "Trigonox A-W70" was dissolved in 60 parts by mass of ion-exchanged water, and a solution in which 0.37 parts by mass of ascorbic acid was dissolved in 60 parts by mass of ion-exchanged water were each dropped into the reaction vessel over 4 hours to react. After the dropwise addition, the mixture was further stirred at 65°C for 1 hour, cooled to 40°C or less, and 2.9 parts by mass of ammonia water with a concentration of 26% was added as a neutralizing agent. As a result, an emulsion containing emulsified particles containing a binder resin and a nonionic emulsifier and water was obtained.

[0205] The properties of the emulsion were as follows: Non-volatile content: 49.5% by mass Viscosity at 23°C: 35mPa·s pH at 23°C: 8.6 ·Minimum film forming temperature (MFT): 5℃ - Glass transition temperature of binder resin: 9℃ - Average emulsion particle size: 210nm

[0206] [Measurement of non-volatile content of emulsion] 1 g of the emulsion was weighed out, placed on an aluminum dish with a diameter of 5 cm, and placed in a dryer. While circulating air in the dryer, the emulsion was dried at 1 atmosphere (1013 hPa) and a temperature of 105° C. for 1 hour, and the mass of the remaining components was measured. The mass ratio (mass%) of the above components remaining after drying relative to the mass (1 g) of the emulsion before drying was calculated, and this was taken as the non-volatile content concentration (mass%).

[0207] [Measurement of emulsion viscosity] The measurement was performed using a BL type viscometer at a temperature of 23° C. and a rotation speed of 60 rpm.

[0208] [Measurement of emulsion pH] The pH at 23° C. was measured using a pH meter (glass electrode type hydrogen ion concentration indicator HM-30G, manufactured by DKK-TOA Corporation).

[0209] [Measurement of average particle size of emulsion particles] The average particle size (d50) of the emulsion particles was measured by dynamic light scattering (DLS) using a MICROTRAC UPA150 (Microtrac Bell, Inc.) at 23°C.

[0210] [Measurement of minimum film formation temperature (MFT)] The emulsion was applied to the measurement surface of the thermal gradient MFT measuring instrument using a 0.3 mm applicator and dried in still air. The dried film was visually observed for poor film formation and cracks, and the MFT was measured.

[0211] [Glass transition temperature (Tg) of binder resin] The glass transition temperature (Tg) of the binder resin was determined by measuring the temperature dependence of the loss tangent using a rheometer (MCR-102, manufactured by Anton Paar). A parallel flat plate with a diameter of 12 mm was used, and the vibration mode was set at a frequency of 1 Hz and a strain of 2%. After a small amount of emulsion was dispensed onto the measurement plate, the plate was brought into contact with the plate and the temperature was raised from 30°C to 180°C at a rate of 10°C / min, removing the volatile matter in the emulsion and adhering the resin to the plate. The temperature was then lowered from 180°C to 0°C at a rate of 2°C / min, and the loss tangent was measured at intervals of 1 point / °C. The temperature at which the loss tangent was maximum was determined as the glass transition temperature.

[0212] (2) Manufacturing of coating fluid In a 500 mL separable flask, 1 part by mass of Sangelose 90L (manufactured by Daido Chemical Industry Co., Ltd.) as a water-soluble polymer, 9 parts by mass of isopropyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., reagent), 179 parts by mass of hot water, and 4 parts by mass of glass fiber (manufactured by Nitto Boseki Co., Ltd., product name: CS 3J-891) were added, and the mixture was stirred at 200 rpm using a mechanical stirrer for 1 minute to obtain a dispersion. Next, while cooling the flask in an ice-water bath, the mixture was stirred at 200 rpm using a mechanical stirrer to dissolve Sangelose 90L, and a pregel, which is an aqueous solution of Sangelose 90L, was obtained. 188 parts by mass of the pregel and 21 parts by mass of aerogel particles (manufactured by CABOT, product name: ENOVA MT1100, particle diameter 2-24 μm, average particle size (D50) 10 μm) were added to a planetary mixer (manufactured by Primix, 2P-1 type) and stirred at 25 rpm for 10 minutes. Next, 86 parts by mass of the emulsion obtained in (1) were added and stirred at 25 rpm for 15 minutes to obtain a coating liquid. In addition, based on the total volume of solids in the coating liquid, the content of the aerogel particles was 84.9 vol %, the content of the water-soluble polymer was 0.3 vol %, and the content of the acrylic resin was 14.1 vol %. The average diameter of the aerogel particle aggregates in the resulting coating liquid was measured by the following method. The results are shown in Table 1.

[0213] <Measurement of the average diameter of aerogel particle aggregates> Approximately 20 g of the coating liquid was placed in a 100 mL polycup, and water was added in 2 g portions while stirring with a spatula, gradually diluting the mixture. The diluted sample was placed on a glass plate, and the aerogel particle aggregates in the coating liquid were observed using an optical microscope (OLYMPUS, model number: BX51) to obtain micrographs. The micrographs obtained were analyzed using the image editing software ImageJ to determine the average diameter of the aerogel particle aggregates.

[0214] <Crack evaluation> The coating liquid was applied to a stainless steel plate (100mm x 70mm x 0.8mm) with an air spray (Graco Corporation hopper gun, model 25D496) to a thickness of 2mm, and the coating liquid was left for 12 hours at room temperature of 23°C to remove the liquid medium, yielding a stainless steel plate with a 1mm thick composite material. The resulting composite material was evaluated for cracking, with A being the case where there were no cracks overall, B being the case where there were localized cracks, and C being the case where there were cracks overall.

[0215] <Evaluation of pore volume of composite materials> A composite material was prepared in the same manner as in the above <Crack evaluation>. 100 mg of the obtained composite material was sampled, and the pore volume was calculated using a high-sensitivity gas adsorption analyzer (Quantachrome, AutoSorb iQ).

[0216] <Evaluation of thermal conductivity of composite materials> A composite material was prepared in the same manner as in the above <Crack Evaluation>. This procedure was repeated to obtain a 3.0-m-thick composite material. The thermal conductivity of the obtained composite material was measured by a steady-state method using a thermal conductivity measuring device "HFM-446" (product name, manufactured by NETZSCH).

[0217] Example 2 A coating liquid was produced in the same manner as in Example 1. The obtained coating liquid was used to draw a line under conditions of 30 kPa and a speed of 20 mm / s using a dispenser (ML-808GX (dispenser) / SHOTMASTERΩx (motion unit) manufactured by Musashi Engineering Co., Ltd.) equipped with a tapered nozzle having an inner diameter of 1.6 mm, and the line was left at room temperature of 23° C. for 12 hours to remove the liquid medium from the coating liquid, thereby obtaining a stainless steel plate with a composite material line having a width of 1.6 mm and a maximum thickness of 0.8 mm. The obtained composite material was evaluated for cracking, with A being the case where there were no cracks overall, B being the case where there were cracks locally, and C being the case where there were cracks overall. The rest of the evaluation was performed in the same manner as in Example 1. The results are shown in Table 1.

[0218] Comparative Example 1 A coating liquid was produced in the same manner as in Example 1. 15 g of the obtained coating liquid was placed on a stainless steel plate, swept several times using a disposable spatula (made of PP, manufactured by AS ONE), and left for 12 hours at room temperature of 23°C to remove the liquid medium from the coating liquid, thereby obtaining a stainless steel plate with a composite material having a thickness of 1 mm. The obtained composite material was evaluated for cracking, with A being when there were no cracks overall, B being when there were localized cracks, and C being when there were cracks overall. The rest of the evaluation was performed in the same manner as in Example 1. The results are shown in Table 1.

[0219] Comparative Example 2 A coating liquid was produced in the same manner as in Example 1. The obtained coating liquid was applied to a stainless steel plate using a roller (for interior paint finishing, bristle length 5 mm) and left for 12 hours at room temperature of 23°C to remove the liquid medium from the coating liquid, thereby obtaining a stainless steel plate with a composite material having a thickness of 0.2 mm. The degree of cracking of the obtained composite material was evaluated as follows: A: no cracks overall, B: cracks locally present, and C: cracks overall. The rest of the evaluation was performed in the same manner as in Example 1. The results are shown in Table 1.

[0220] [Table 1]

[0221] Example 3 (1) Preparation of aerogel particles A As a silica particle-containing raw material, 100.0 parts by mass of PL-2L (manufactured by Fuso Chemical Co., Ltd., product name), 80.0 parts by mass of water, 0.5 parts by mass of acetic acid as an acid catalyst, 1.0 parts by mass of cetyltrimethylammonium bromide (manufactured by Wako Pure Chemical Industries, Ltd.) as a cationic surfactant, and 150.0 parts by mass of urea as a thermal hydrolysis product were mixed, and 60.0 parts by mass of methyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-13) as a silicon compound, 20.0 parts by mass of dimethyldimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: KMB-22), and 20.0 parts by mass of a bifunctional alkoxy-modified polysiloxane compound at both ends (hereinafter referred to as "polysiloxane compound A") were added thereto, and the mixture was reacted at 25 ° C. for 2 hours to obtain a sol. The obtained sol was gelled at 60 ° C., and then aged at 60 ° C. for 48 hours to obtain a wet gel. The above "polysiloxane compound A" was synthesized as follows. First, in a 1-liter three-neck flask equipped with a stirrer, a thermometer, and a Dimroth condenser, 100.0 parts by mass of dimethylpolysiloxane XC96-723 (product name, manufactured by Momentive Performance Materials Japan LLC) having silanol groups at both ends, 181.3 parts by mass of methyltrimethoxysilane, and 0.50 parts by mass of t-butylamine were mixed and reacted at 30°C for 5 hours. After that, this reaction liquid was heated at 140°C for 2 hours under a reduced pressure of 1.3 kPa to remove volatile matter, thereby obtaining a polysiloxane compound modified with alkoxy at both ends (polysiloxane compound A). The wet gel obtained was then transferred to a plastic bottle, sealed, and pulverized at 27,000 rpm for 10 minutes using an extreme mill (MX-1000XTS, manufactured by AS ONE Corporation) to obtain a particulate wet gel. The particulate wet gel obtained was immersed in 2500.0 parts by mass of methanol and washed at 25°C for 24 hours. This washing operation was performed a total of three times while replacing with fresh methanol. Next, the washed particulate wet gel was immersed in 2500.0 parts by mass of heptane, a low surface tension solvent, and solvent replacement was performed at 25°C for 24 hours. This solvent replacement operation was performed a total of three times while replacing with fresh heptane. The washed and solvent-replaced particulate wet gel was dried at 40°C for 96 hours under normal pressure, and then further dried at 150°C for 2 hours. Finally, it was sieved (manufactured by Tokyo Screen Co., Ltd., mesh size 45μm, wire diameter 32μm) to obtain aerogel particles A.

[0222] (2) Manufacturing of coating fluid A coating liquid was produced in the same manner as in Example 1, except that the aerogel particles were changed to aerogel particles A. The obtained coating liquid was evaluated in the same manner as in Example 1, and the results are shown in Table 2.

[0223] Example 4 A coating liquid was produced in the same manner as in Example 1, except that the aerogel particles were changed to aerogel particles A. The obtained coating liquid was evaluated in the same manner as in Example 1, except that cracks were evaluated in the same manner as in Example 2. The results are shown in Table 2.

[0224] Comparative Example 3 A coating liquid was produced in the same manner as in Example 1, except that the aerogel particles were changed to aerogel particles A. The obtained coating liquid was evaluated in the same manner as in Example 1, except that cracks were evaluated in the same manner as in Comparative Example 1. The results are shown in Table 2.

[0225] Comparative Example 4 A coating liquid was produced in the same manner as in Example 1, except that the aerogel particles were changed to aerogel particles A. The obtained coating liquid was evaluated in the same manner as in Example 1, except that cracks were evaluated in the same manner as in Comparative Example 2. The results are shown in Table 2.

[0226] [Table 2]

Claims

1. a coating film forming step of discharging a coating liquid containing aerogel particles, a binder resin, glass fibers, and a liquid medium toward an object to obtain a coating film; a removing step of removing at least a portion of the liquid medium from the coating film to obtain a composite material; A method for producing a composite material, comprising:

2. The method according to claim 1 , wherein the coating film forming step is a step of discharging the coating liquid toward the object by a discharging device selected from the group consisting of a sprayer and a dispenser.

3. the discharge device has a discharge port for discharging the coating liquid, The method according to claim 2 , wherein the inner diameter of the discharge port is 1.5 mm or more.

4. The method according to claim 1 , wherein the coating liquid further contains a water-soluble polymer having a hydrophobic group.

5. The method according to claim 4, wherein the hydrophobic group is an alkyl group having 6 to 26 carbon atoms.

6. The method according to claim 1 , wherein the coating liquid contains emulsified particles containing the binder resin.

7. The method according to claim 6 , wherein the emulsion particles further contain a nonionic emulsifier.

8. The method of claim 1 , wherein at least a portion of the aerogel particles form aggregates.

9. an emulsion preparation step of preparing an emulsion including emulsified particles containing a binder resin and a first liquid medium; a dispersion preparation step of mixing aerogel particles, glass fibers, and a second liquid medium to obtain a dispersion containing the aerogel particles, the glass fibers, and the second liquid medium; a coating liquid preparation step of mixing the emulsion and the dispersion to obtain the coating liquid; The method of claim 1 further comprising:

10. the dispersion preparation step is a step of mixing the aerogel particles, the glass fibers, and the second liquid medium to aggregate at least a portion of the aerogel particles; The method according to claim 9 , wherein the coating liquid contains aggregates of the aerogel particles.

Citation Information

Patent Citations

  • Coating liquid, production method for coating film, and coating film

    WO2019069492A1

  • Coating liquid, composite material, and coating film

    WO2020208759A1

  • Manufacturing method for coating liquid and manufacturing method for insulating material

    WO2021153764A1

  • Method for producing coating liquid and method for producing thermal insulation material

    WO2022190209A1

  • aerogel

    JP2012091943A

Cited By

  • Flame-retardant, heat-insulating and sound-insulating coating and preparation method thereof

    CN119463590A