Method for measuring density of green compact
The use of water-repellent coatings for green compacts, applied via dipping and drying, addresses safety and efficiency issues in conventional density measurement methods, enabling rapid and accurate density calculations for improved productivity and quality control.
Patent Information
- Application Number
- JP2023074909
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Conventional methods for measuring the density of green compacts, particularly using paraffin as a sealing agent, pose safety risks due to high melting temperatures, risk of sample damage, and prolonged processing times, leading to inaccurate density measurements and reduced productivity.
A method involving water-repellent coating, such as fluororesin-containing fluorine-based solvent-based agents, applied via dipping and drying, followed by underwater gravimetry for density measurement, reduces processing temperatures and simplifies excess agent removal, allowing for rapid and accurate density calculations.
The method safely lowers processing temperatures, prevents sample damage, and significantly reduces measurement time, enabling precise and automatic density calculations, enhancing productivity and quality control in green compact production.
Smart Images

Figure 2024159122000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for measuring the density of a powder compact. [Background technology]
[0002] Magnetic materials, for example, materials obtained by compacting metal powder such as ferrite or rare earth magnets (hereinafter also referred to as "green bodies"), are used as magnetic materials in a variety of applications including motors.
[0003] For example, Patent Document 1 discloses a method for producing a rare earth permanent magnet, which comprises forming an oxide film containing 0.2% to 1.6% by weight of oxygen on the surface of rare earth-iron-nitrogen magnet powder, pre-compressing the magnet powder with the oxide film into a predetermined shape in a non-oxidizing atmosphere to obtain a preform with a relative density of 40% or more, and then compressing the preform at a temperature of 350°C to 500°C in a non-oxidizing atmosphere to obtain a magnet molding with a relative density of 85% or more. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2005-223263 A Summary of the Invention [Problem to be solved by the invention]
[0005] When such a green compact is used, for example, as a magnetic material, the density, which is one of the physical properties of the green compact, is an important factor that determines the magnitude of magnetization and coercive force of the magnetic material, and is therefore one index for quality control in the production of the green compact.
[0006] The density of conventional green compacts is measured based on, for example, JIS Z 2501:2000 "Sintered metal materials - Test method for density, oil content and open porosity." Green compacts are usually water-absorbent, so in Patent Document 1, for example, the relative density of a magnet is measured by treating a sample with paraffin.
[0007] However, the conventional method for measuring the density of green compacts, especially the method using paraffin as a sealing material, had the following problems. (1) From a safety perspective, the temperature required to melt paraffin is as high as about 80°C, so there is a risk of injury from contact with heated and melted paraffin. (2) From a quality perspective, there is a risk of paraffin being left behind or the sample (workpiece) peeling off and being damaged during immersion in paraffin and wiping off excess paraffin after immersion in paraffin to prevent volume change, which can easily cause errors in the accuracy of the density measurement results obtained. (3) From a productivity perspective, the time required from melting and immersing in paraffin to removing and drying the paraffin is long, about 60 minutes. In addition, in order to calculate the desired density, it is necessary to take into account the weight of the green compact treated with paraffin, and automatic calculations cannot be performed using a density measuring instrument.
[0008] Therefore, an object of the present invention is to provide a method for simply measuring the density of a powder compact. [Means for solving the problem]
[0009] The inventors have examined various means for solving the above-mentioned problems, and as a result have found that by applying a water-repellent coating to a powder compact when measuring its density, (1) from a safety perspective, the temperature required for the coating process can be reduced, (2) from a quality perspective, the removal of excess coating agent can be simplified to just drying, preventing peeling and damage to the sample, and (3) from a productivity perspective, since only the surface of the sample needs to be treated to be water-repellent, the coating process time can be shortened, and further, since the amount of coating agent remaining on the powder compact is small, it is not necessary to take the weight of the coating agent into account when calculating the desired density, and automatic calculations can be made using a density measuring instrument, thereby completing the present invention.
[0010] That is, the gist of the present invention is as follows. (1) A method for measuring the density of a powder compact, comprising the steps of: subjecting a powder compact to a water-repellent coating treatment; and measuring the density of the water-repellent coated powder compact by underwater gravimetry. (2) The method according to (1), wherein the powder compact is a magnetic material. (3) The method according to (1) or (2), wherein the water-repellent coating treatment is carried out by a dipping method including a dipping step of dipping the powder compact in a water-repellent coating agent and a drying step of drying the removed powder compact. (4) The method according to (3), wherein the water-repellent coating agent is a fluororesin-containing fluorine-based solvent-based coating agent that contains a fluorine-based solvent and a fluorine resin. (5) The method according to (4), wherein the time for the immersion step is 0.1 seconds to 3.0 seconds, the temperature for the drying step is 30°C to 50°C, the time for the drying step is 180 seconds to 300 seconds, and the amount of the fluororesin in the water-repellent coated powder compact is 0.02 wt % to 0.2 wt % based on the total weight of the powder compact. Effect of the Invention
[0011] The present invention provides a simple method for measuring the density of a powder compact. [Brief description of the drawings]
[0012] [Figure 1] 1 is a graph showing the weight change versus immersion time in water for the powder compact (untreated), and the powder compacts of Comparative Example 1 and Example 1. [Diagram 2] 1 is a graph showing the relationship between the immersion time of a green compact in a fluororesin-containing fluorine-based solvent-based coating agent and the associated amount of the coating agent applied. [Diagram 3] 1 is a graph showing the relationship between the coating amount before drying and the coating amount after drying on a green compact. [Figure 4] 1 is a graph showing the relationship between drying time and coating amount in a powder compact. [Diagram 5]1 is a graph showing the relationship between drying time and coating amount in hot air drying when ferrite or magnet is used as the powder compact. [Figure 6] 1 is a graph showing the measurement results (N=3) of the density of the paraffin-treated powder compact of Comparative Example 2 and the water-repellent coating-treated powder compact of Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Preferred embodiments of the present invention will now be described in detail. In this specification, the features of the present invention will be described with reference to the drawings as appropriate. The method for measuring the density of a powder compact according to the present invention is not limited to the following embodiments, and can be embodied in various forms including modifications and improvements that can be made by those skilled in the art without departing from the gist of the present invention.
[0014] The present invention relates to a method for measuring the density of a powder compact, the method including the steps of subjecting a powder compact to a water-repellent coating treatment and measuring the density of the water-repellent coated powder compact by underwater gravimetry.
[0015] Here, the powder compact to be the object of density measurement is not limited. The powder compact means a material obtained by pressing a metal powder, for example, a magnetic material. The powder compact may be a powder compact obtained by pressing and sintering a metal powder, for example, a magnetic material. Examples of the powder compact include water-absorbent magnetic materials, such as ferrite, rare earth magnets, such as SmCo rare earth magnets, NdFeB rare earth magnets, and SmFeN rare earth magnets.
[0016] According to the present invention, the density of even a water-absorbent powder compact can be simply measured.
[0017] The water-repellent coating treatment is not limited, and may be, for example, a method of contacting the powder compact with a water-repellent coating agent.
[0018] The water-repellent coating agent is not limited. Examples of the water-repellent coating agent include water-repellent coating agents that are liquid during the water-repellent coating process, such as fluororesins, such as polytetrafluoroethylene (PTFE), perfluoroalkoxyalkane (PFA), perfluoroethylenepropene copolymer (PEA), ethylenetetrafluoroethylene copolymer (ETFE), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), and ethylenechlorotrifluoroethylene copolymer (ECTFE), which are dissolved in a volatile solvent, such as a fluorine-based solvent (e.g., hydrofluoroether (HFE), hydrofluorocarbon (HFC)) or an organic solvent (toluene, isobutanol, heptane, etc.) (fluororesin-containing solvent-based coating agent). The fluororesin-containing solvent-based coating agent contains a fluororesin in an amount of usually 0.2% by weight to 30% by weight, preferably 1% by weight to 3% by weight, and a solvent, such as a fluorine-based solvent, in an amount of usually 70% by weight to 99.8% by weight, preferably 97% by weight to 99% by weight, based on the total weight of the coating agent. Examples of the water-repellent coating agent include products containing fluororesin, such as SF Coat SFE-DP02H and SNF-DP20H (manufactured by AGC Seimi Chemical Co., Ltd.), Optoace WP-100 series (manufactured by Daikin Industries, Ltd.), Fluorosurf FG-3030 series, FG-3020 series, and FG-3650 series (manufactured by Fluoro Technology Co., Ltd.), and SURECO CC Series (manufactured by AGC Corporation). For example, a suitable water-repellent coating agent can be selected as one that does not absorb water (does not change in weight) for the time required for density measurement by underwater gravimetric method, typically 5 seconds or less, preferably 30 seconds or less, when the water absorption is confirmed based on the weight change of the powder compact relative to the immersion time in water after the powder compact is treated with the water-repellent coating agent.
[0019] Examples of the method for contacting the powder compact with the water-repellent coating agent include a method in which the water-repellent coating agent is sprayed or dropped onto the powder compact, and optionally evenly coated on the powder compact and then dried, and a method in which the powder compact is immersed in the water-repellent coating agent, taken out, and then dried (immersion method). The immersion method is preferred for the water-repellent coating treatment because it can be easily carried out.
[0020] As described above, the immersion method includes a step of immersing the powder compact in a water-repellent coating agent (immersion step) and a step of drying the powder compact after removal (drying step).
[0021] The temperature in the immersion step is not limited, and is, for example, room temperature, for example, 5°C to 35°C, and preferably 20°C to 30°C, from the viewpoint of safety.
[0022] The time for the immersion step is not limited as long as the surface of the powder compact is coated with a water-repellent coating.
[0023] The time for the immersion step is, for example, when the water-repellent coating agent is a fluorine-based solvent-based coating agent containing a fluorine resin, the object may be immersed in the entire object and then immediately removed from the water-repellent coating agent, and therefore, the time for the immersion step is usually 0.1 seconds or more, preferably 0.5 seconds or more. Also, the longer the time for the immersion step, the greater the amount of water-repellent coating agent, particularly the fluorine resin, that is applied, so, for example, when the water-repellent coating agent is a fluorine-based solvent-based coating agent containing a fluorine resin, the time for the immersion step is usually 3.0 seconds or less, preferably 2.5 seconds or less, more preferably 2.0 seconds or less.
[0024] By setting the temperature and time of the immersion step within the above ranges, it is possible to safely coat the powder compact with an appropriate amount of the precursor of the water-repellent coating agent.
[0025] The temperature in the drying step is not limited as long as it is a temperature at which the solvent that may be contained in the water-repellent coating agent, such as a fluorine-based solvent, volatilizes. The temperature in the drying step is, for example, room temperature (natural drying) to 60°C (hot air drying), for example, 5°C to 60°C, and preferably 30°C to 50°C.
[0026] The time of the drying step is not limited as long as it is the time required for the solvent, for example, the fluorine-based solvent, that may be contained in the water-repellent coating agent to volatilize. Therefore, the time of the drying step may also depend on the water-repellent coating agent and the drying temperature. For example, when the water-repellent coating agent is a fluorine-based solvent-based coating agent containing a fluorine resin, the time is usually 300 seconds or more if the water-repellent coating agent is naturally dried at about 22°C, and usually 180 seconds or more if the water-repellent coating agent is hot air dried at about 40°C. The upper limit of the time of the drying step is not limited, and the drying step can be completed as long as the fluorine-based solvent that may be contained in the water-repellent coating agent volatilizes. The time of the drying step can also be determined as the time when the weight of the powder compact after the immersion step has almost stopped changing by plotting the weight of the powder compact after the immersion step against the time of the drying step.
[0027] By setting the temperature and time in the drying step within the above ranges, it is possible to coat the green compact with an appropriate amount of water-repellent coating agent safely.
[0028] The amount and film thickness of the water-repellent coating agent applied to the powder compact by the water-repellent coating treatment are not limited as long as the surface of the powder compact exhibits water repellency. However, it is preferable to set the amount and film thickness so as not to affect the calculation of the density of the powder compact.
[0029] The amount and thickness of the water-repellent coating agent is, for example, a fluororesin-containing fluorine-based solvent-type coating agent, usually 0.01 g or less of fluorine resin, and usually 1 μm or less of film thickness, relative to 7.5 g of the powder compact to be measured for density. The lower limit of the amount and thickness of the water-repellent coating agent is not limited as long as the powder compact surface shows water repellency, but, for example, when the water-repellent coating agent is a fluorine-based solvent-type coating agent containing fluorine resin, usually 0.002 g of fluorine resin, and usually 0.2 μm. Therefore, the amount of the water-repellent coating agent is, for example, when the water-repellent coating agent is a fluorine-based solvent-type coating agent containing fluorine resin, usually 0.02 wt% to 0.2 wt%, preferably 0.10 wt% to 0.15 wt%, relative to the total weight of the powder compact, relative to the total weight of the powder compact.
[0030] By setting the amount of water-repellent coating agent and the film thickness within the above ranges, water repellency is provided to the powder compact, and the density can be automatically calculated without having to take the amount into account when calculating the density, without having a significant effect.
[0031] The density of the water-repellent coated green compact is then measured by underwater gravimetry.
[0032] The underwater gravimetric method is well known in the art and is not limited to a specific one, for example, a method based on JIS Z 2501:2000 "Sintered metal materials - Test method for density, oil content and open porosity."
[0033] The density calculation by the underwater gravimetry method is carried out by, for example, first measuring the weight in the air of a water-repellent coated compact, then measuring the weight in water, and calculating the density using the following formula: Density (g / cm 3 )=weight in air / (weight in air - weight in water) It can be calculated by:
[0034] The method for measuring the density of a powder compact of the present invention can be used for quality control of a powder compact in a method for producing the powder compact.
[0035] For example, in a process of compacting a magnetic material, the magnetic powder is compressed in a press to produce a compact, and the compact is visually inspected for chips and cracks, and then the compact is subjected to the water-repellent coating treatment described above. Then, the weight of the sample in air (weight of the sample in air) and the weight of the sample in water (weight of the sample in water) are measured to automatically calculate the density. Next, it is determined whether the obtained density is within the set range of the density of the compact, and if an appropriate density is obtained, the production of the compact is continued without changing the production conditions, and if it is outside the appropriate density range, an instruction is given to change the production conditions so that an appropriate density is obtained.
[0036] According to the present invention, the temperature required for density measurement can be reduced to approximately room temperature, and the time required for density measurement can be drastically shortened compared to conventional methods (approximately 60 minutes or more in the conventional method to 5 minutes or less in the present invention). Therefore, even if a defect occurs in the manufacturing conditions during the production of green compacts, for example in the sintering process or compression process, the defect can be detected safely, quickly, and accurately, thereby reducing the occurrence of defective products and improving productivity. EXAMPLES
[0037] Several examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples.
[0038] 1. Water absorption evaluation 1-1.Sample preparation Comparative Example 1 The powder compact was subjected to paraffin treatment as follows. (1) The green compact (diameter φ17 mm × total thickness 11.3 mm, weight 7.87 g, ferrite powder Z10FG) was immersed in paraffin that had been melted by heating at approximately 80°C for 40 minutes. (2) The powder compact immersed in (1) was kept in paraffin for about 20 minutes so that the paraffin could penetrate into the pores present in the powder compact. (3) The powder compact held in (2) was removed from the paraffin, excess paraffin adhering to the periphery of the powder compact was wiped off, and the powder compact was dried at 22°C for 5 minutes to obtain a paraffin-treated powder compact.
[0039] Example 1 The green compact was subjected to a water-repellent coating treatment as follows. (1) The powder compact (diameter φ17 mm × total thickness 11.3 mm, weight 7.82 g, ferrite powder Z10FG) was immersed in a fluorine-based solvent-based coating agent containing fluorine resin (Fluorosurf (registered trademark) FG-3650TH series (solid content concentration 2 wt%)) at 22°C. (2) The green compact immersed in (1) was immersed entirely in a fluororesin-containing fluorine-based solvent-based coating agent and held there for 1 second. (3) The green compact held in (2) was removed from the fluororesin-containing fluorine-based solvent-based coating agent and dried in a hot air dryer at 40°C for 180 seconds to obtain a green compact treated with a water-repellent coating.
[0040] 1-2.Evaluation The powder compact (untreated product, diameter φ17 mm × total thickness 11.2 mm, weight 7.84 g, ferrite powder Z10FG), the paraffin-treated powder compact of Comparative Example 1, and the water-repellent coating-treated powder compact of Example 1 were immersed in water, and the change in weight (weight in water) with respect to the immersion time was evaluated. The results are shown in Figure 1.
[0041] 1, it was confirmed that the untreated powder compact started absorbing water immediately after immersion in water, and that the amount of water absorbed increased over time in the paraffin-treated powder compact of Comparative Example 1. On the other hand, no weight increase over time was observed in the water-repellent coated powder compact of Example 1 during the 30 seconds observed. Therefore, it was found that the water-repellent coated powder compact of Example 1 did not undergo weight change during weight measurement in the underwater gravimetry, i.e., did not absorb water.
[0042] 2. Relationship between immersion time and application amount 2-1.Sample preparation
[0043] Example 2 The powder compact was subjected to a water-repellent coating treatment as follows. This experiment was carried out three times (N=3). (1) The weight of the green compact (diameter φ17 mm × total thickness 11.3 mm, weight 7.85 g, ferrite powder Z10FG) was measured and immersed in a fluorine-based solvent-based coating agent containing a fluorine resin (Fluorosurf (registered trademark) FG-3650TH series (solid content concentration 2 wt%)) at 22°C. (2) The green compact immersed in (1) was immersed entirely in a fluororesin-containing fluorine-based solvent-based coating agent and held there for 0.5 seconds. (3) The green compact held in (2) was removed from the fluororesin-containing fluorine-based solvent-based coating agent, and the weight of the removed green compact was measured.
[0044] Example 3 An experiment was carried out in the same manner as in Example 2, except that the retention time in the fluorine-based solvent-based coating agent containing a fluorine resin in (2) was changed from 0.5 seconds to 1.0 seconds.
[0045] Example 4 An experiment was carried out in the same manner as in Example 2, except that the retention time in the fluororesin-containing fluorine-based solvent-based coating agent (2) was changed from 0.5 seconds to 2.0 seconds.
[0046] 2-2.Evaluation Figure 2 shows the relationship between the immersion time of the green compact in the fluororesin-containing fluororesin-based solvent-based coating agent and the associated amount of fluororesin-containing fluororesin-based solvent-based coating agent applied. The amount of application was calculated by subtracting the weight of the green compact itself from the weight measured in (3). Figure 2 shows that extending the immersion time in the fluororesin-containing fluororesin-based solvent-based coating agent increases the amount of fluororesin-containing fluororesin-based solvent-based coating agent applied proportionally. Therefore, it was found that the desired amount of fluororesin-containing fluororesin-containing fluororesin-based solvent-based coating agent can be applied by adjusting the immersion time in the fluororesin-containing fluororesin-based solvent-based coating agent.
[0047] 3. Relationship between the amount of fluororesin-containing fluorine-based solvent-based coating agent applied and the amount of fluororesin applied 3-1.Sample preparation The coating amount (weight before drying) of a single fluororesin-containing fluorine-based solvent-based coating agent (Fluorosurf (registered trademark) FG-3650TH series (solid content concentration 2 wt%)) at 22°C was measured under seven conditions, and then it was dried for 30 to 300 seconds in a hot air dryer at 40°C, and the weight (weight after drying) was measured again, and the coating amount of the fluororesin-containing fluorine-based solvent-based coating agent (coating amount before drying) and the coating amount of the fluororesin (coating amount after drying) on the treated green compact were calculated.
[0048] 3-2.Evaluation Figure 3 shows the relationship between the coating amount before drying and the coating amount after drying in the compact. From Figure 3, it was found that there is a proportional relationship between the coating amount before drying and the coating amount after drying. Therefore, it was found that the coating amount of the fluororesin in the coating agent can be controlled by adjusting the immersion time in the fluororesin-containing fluorine-based solvent-based coating agent to adjust the coating amount of the coating agent.
[0049] 4. Examination of the drying process in the immersion method 4-1.Measurement The weight of the compact (diameter φ17 mm × total thickness 8.45 mm, weight 5.88 g, ferrite powder Z10FG) was measured and immersed in a fluororesin-containing fluorine-based solvent-based coating agent (Fluorosurf (registered trademark) FG-3650TH series (solid content concentration 2 wt%)) at 22°C to produce a compact with a coating amount of approximately 0.3 g of fluororesin-containing fluorine-based solvent-based coating agent. The change in the coating amount of the coating agent versus drying time when the compact was dried naturally (22°C) or by hot air drying (40°C) was measured. The coating amount was calculated by subtracting the weight of the compact itself from the weight after drying.
[0050] 4-2.Evaluation FIG. 4 shows the relationship between the drying time and the coating amount in the compact. From FIG. 4, it was found that the coating amount decreases over time in both natural drying and hot air drying, and becomes constant at 0.01 g or less after about 300 seconds in natural drying and about 180 seconds in hot air drying. In other words, it was found that both natural drying and hot air drying can be used in the drying process, but hot air drying is preferable from the viewpoint of shortening the time. In this experiment, it was found that when the immersion time in the fluororesin-containing fluorine-based solvent-based coating agent (solid content concentration 2 wt%) was adjusted to 0.5 to 2.0 seconds for a 5.88 g compact, and the coating amount of the fluororesin-containing fluorine-based solvent-based coating agent was adjusted to 0.25 to 0.35 g, it was found that the coating amount of 0.01 g of fluororesin can be achieved in about 300 seconds in natural drying and about 180 seconds in hot air drying.
[0051] Figure 5 shows the relationship between the drying time and the coating amount when drying with hot air when ferrite (diameter φ17mm × total thickness 8.45mm, weight 5.88g, ferrite powder Z10FG) or magnet material (diameter φ17mm × total thickness 4.9mm, weight 6.39g, SmFeN magnet powder Z12) is used as the green compact. Figure 5 shows that the drying process can be completed in a similar drying time even when ferrite or magnet is used as the green compact.
[0052] 5. Density measurement evaluation 5-1.Sample preparation Comparative Example 2 The density of the green compact (magnet material) was measured three times (N=3) by paraffin treatment according to the procedure described below. (1) The weight of the green compact (diameter φ17 mm × total thickness 4.9 mm, weight 6.39 g, SmFeN magnet powder Z12) was measured. (2) The powder compact whose weight was measured in (1) was immersed in paraffin that had been melted by heating at approximately 80°C for 40 minutes. (3) The powder compact immersed in (2) was kept in paraffin for about 20 minutes so that the paraffin could penetrate into the pores present in the powder compact. (4) The green compact held in (3) was removed from the paraffin, excess paraffin adhering to the green compact was wiped off, and the green compact was dried at 22°C for 5 minutes. (5) The weight of the paraffin-treated green compact dried in (4) was measured. (6) The weight of the paraffin-treated green compact weighed in (5) was measured in water. (7) Density was calculated based on the following formula: Density (g / cm 3 ) = Weight in air measured in (1) / (Weight in air measured in (5) - Weight in water measured in (6))
[0053] Example 5 The density of the compact (magnetic material) was measured three times (N=3) after the water-repellent coating treatment according to the procedure described below. (1) The weight of the green compact (diameter φ17 mm × total thickness 4.65 mm, weight 5.80 g, SmFeN magnet powder Z12) was measured. (2) The powder compact whose weight was measured in (1) was immersed in a fluorine-based solvent-based coating agent containing a fluororesin (Fluorosurf (registered trademark) FG-3650TH series (solids concentration 2% by weight)) at 22°C. (3) The green compact immersed in (2) was immersed entirely in a fluororesin-containing fluorine-based solvent-based coating agent and held there for 1.0 second. (4) The green compact held in (3) was removed from the fluororesin-containing fluorine-based solvent-based coating agent and dried in a hot air dryer at 40°C for 180 seconds to obtain a green compact treated with a water-repellent coating. (5) The weight of the water-repellent coated green compact dried in (4) was measured. (6) The weight of the water-repellent coated green compacts measured in (5) was measured in water. (7) Density was calculated based on the following formula: Density (g / cm 3 ) = Weight in air measured in (1) / (Weight in air measured in (5) - Weight in water measured in (6))
[0054] 5-2.Evaluation Fig. 6 shows the measurement results (N=3) of the density of the paraffin-treated green compact of Comparative Example 2 and the water-repellent coating-treated green compact of Example 5. Fig. 6 shows the maximum, average, and minimum values for each experimental example.
[0055] As shown in FIG. 6, in the density measurement by paraffin treatment in Comparative Example 2, the obtained density result was the density of the green compact used calculated by the following calculation: Weight (6.39g) / Volume (3.14×1.7×1.7 / 4×0.49=1.11cm 3 )=density(5.75g / cm 3 ) On the other hand, in the density measurement using the water-repellent coating treatment in Example 5, the density result was found to be greater than the density of the green compact obtained by the following calculation: Weight (5.80g) / Volume (3.14×1.7×1.7 / 4×0.465=1.05cm 3 )=density(5.50g / cm 3 ) It was found that the error was small and there was almost no variation.
Claims
1. A method for measuring the density of a powder compact, comprising the steps of: subjecting a powder compact to a water-repellent coating treatment; and measuring the density of the water-repellent coated powder compact by underwater gravimetry.
2. The method of claim 1 , wherein the powder compact is a magnetic material.
3. 3. The method according to claim 1 or 2, wherein the water-repellent coating treatment is carried out by a dipping method including a dipping step of dipping the powder compact in a water-repellent coating agent and a drying step of drying the removed powder compact.
4. The method according to claim 3, wherein the water-repellent coating agent is a fluororesin-containing fluororesin-containing solvent-based coating agent containing a fluorine-based solvent and a fluorine resin.
5. 5. The method according to claim 4, wherein the immersion time is 0.1 seconds to 3.0 seconds, the drying time is 30° C. to 50° C., the drying time is 180 seconds to 300 seconds, and the amount of the fluororesin in the water-repellent coated green compact is 0.02 wt % to 0.2 wt % based on the total weight of the green compact.
Citation Information
Patent Citations
Method for testing volume density of porous material with complex shape
CN114813461A
Soft magnetic dust core
JP2013247214A
Magnetic material, magnetic core, and method for manufacturing the same
JP2017188680A
Powder magnetic core and manufacturing method thereof
JP2022094461A
Powder magnetic core and electromagnetic part
US20200143973A1