Calcium phosphate
The production of acicular calcium phosphate particles with controlled aspect ratio and width direction length addresses the orientation issue, resulting in improved performance as a structural material filler.
Patent Information
- Application Number
- JP2023074979
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Existing calcium phosphate fillers lack sufficient orientation, which affects their performance as structural material additives.
Production of acicular calcium phosphate particles with a specific aspect ratio and width direction length through a double tube mixing process, involving the rapid mixing of phosphoric acid and calcium hydroxide solutions using a jet stream, followed by aging at controlled temperatures.
The resulting calcium phosphate exhibits enhanced orientation and bulk specific volume, making it suitable for use as a filler in various applications.
Smart Images

Figure 2024159161000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to calcium phosphates. [Background technology]
[0002] Since calcium phosphate has low surface activity, no hygroscopicity, biocompatibility, and high safety, its use as a filler for structural materials is being considered (for example, Patent Document 1). From the viewpoint of dimensional stability of resins, fillers for structural materials are desired to be particulate and have a high aspect ratio. Patent Document 1 discloses flaky calcium hydrogen phosphate with an average aspect ratio of 5 or more. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-29693 A Summary of the Invention [Problem to be solved by the invention]
[0004] For use as a filler, there has been a demand for further improvement of calcium phosphate so as to improve the orientation. An object of the present invention is to provide a calcium phosphate having excellent orientation. [Means for solving the problem]
[0005] The calcium phosphate according to one embodiment of the present disclosure relates to the following aspects.
[0006] [Aspect 1] The calcium phosphate contains acicular particles each having a length L in the longitudinal direction, a length T in the thickness direction, and a length D in the width direction. The acicular particles have an aspect ratio (L / T) of 80 or more and 150 or less. The acicular particles have a length D in the width direction of 0.5 μm or more and 2.0 μm or less.
[0007] [Aspect 2] The needle-shaped particle is the calcium phosphate according to aspect 1, having a flat end surface at one end in the longitudinal direction.
[0008] [Aspect 3] The acicular particles are calcium phosphate according to embodiment 1 or 2, produced by mixing an aqueous phosphoric acid solution with a suspension of calcium hydroxide using a jet stream.
[0009] [Aspect 4] The method for producing calcium phosphate according to any one of aspects 1 to 3, wherein the acicular particles are produced by mixing an aqueous phosphoric acid solution and a suspension of calcium hydroxide using a double-pipe mixer. The double-pipe mixer includes an outer pipe and an inner pipe disposed within the outer pipe. The suspension of calcium hydroxide is supplied to the outer pipe. The aqueous phosphoric acid solution is supplied to the inner pipe.
[0010] [Aspect 5] 2. The calcium phosphate according to embodiment 1, having a bulk specific volume of 5 mL / g or more and 15 mL / g or less.
[0011] [Aspect 6] The method for producing calcium phosphate includes a mixing step of mixing an aqueous phosphoric acid solution with a suspension of calcium hydroxide to obtain a slurry. In the mixing step, the aqueous phosphoric acid solution and the suspension are mixed by a jet stream.
[0012] [Aspect 7] In the method for producing calcium phosphate according to aspect 6, a double-pipe mixer is used in the mixing step. The double-pipe mixer includes an outer pipe and an inner pipe disposed within the outer pipe. The calcium hydroxide suspension is supplied to the outer pipe. The phosphoric acid aqueous solution is supplied to the inner pipe.
[0013] [Aspect 8] The method for producing calcium phosphate includes an aging step of aging the slurry at a temperature of 60° C. to 100° C. The aging step is a method for producing calcium phosphate according to embodiment 7, in which an aging tank is used. The aging tank is provided downstream of the double-pipe mixing section. The aging tank receives the slurry discharged from the double-pipe mixing section.
[0014] [Aspect 9] The method for producing calcium phosphate according to any one of aspects 6 to 8, wherein the calcium phosphate comprises needle-shaped particles each having a length L in the longitudinal direction, a length T in the thickness direction, and a length D in the width direction. The needle-shaped particles have an aspect ratio (L / T) of 80 or more and 150 or less. The length D in the width direction is 0.5 μm or more and 2.0 μm or less. Effect of the Invention
[0015] The calcium phosphate according to the present invention has excellent orientation. [Brief description of the drawings]
[0016] [Figure 1] 1 is a SEM photograph (1) of calcium phosphate according to the present embodiment. [Diagram 2] 1 is a SEM photograph (2) of calcium phosphate according to the embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic diagram showing a calcium phosphate manufacturing apparatus according to an embodiment of the present invention. [Figure 4] FIG. 2 is a schematic diagram showing a double-pipe mixer according to the present embodiment. [Diagram 5] 1 shows SEM photographs of samples according to an embodiment and a reference example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] [Calcium phosphate] Hereinafter, calcium phosphate according to one embodiment of the present invention will be described with reference to the drawings. Figure 1 is an SEM photograph (1) of calcium phosphate according to this embodiment, and Figure 2 is an SEM photograph (2) of calcium phosphate according to this embodiment.
[0018] 1 and 2, calcium phosphate contains a plurality of acicular particles 10 each having a length L in the longitudinal direction, a length T in the thickness direction, and a length D in the width direction. The acicular particles 10 may be agglomerated with other acicular particles 10 contained in the calcium phosphate and with irregular particles other than the acicular particles 10, or may exist alone without agglomerating with other particles.
[0019] Examples of calcium phosphate include calcium hydrogen phosphate, calcium hydrogen phosphate dihydrate, calcium dihydrogen phosphate, calcium dihydrogen phosphate monohydrate, tricalcium phosphate, octacalcium phosphate, hydroxyapatite, fluorapatite, chlorapatite, carbonate apatite, whitlockite, amorphous calcium phosphate, tetracalcium phosphate, and calcium pyrophosphate.
[0020] The aspect ratio (L / T) of the acicular particle 10 is 80 or more and 150 or less. The length L in the longitudinal direction is the length of the longest axis of the acicular particle 10 of interest. The length T in the thickness direction is the length of the shortest axis corresponding to the length L in the longitudinal direction of the acicular particle 10 of interest.
[0021] The acicular particle 10 has a widthwise length D of 0.5 μm or more and 2.0 μm or less. The widthwise length D is the length in the direction perpendicular to the longitudinal direction and thickness direction of the acicular particle 10 of interest. That is, the widthwise length D is the distance between both sides along the longitudinal axis of the acicular particle 10 of interest, with the surface including the longitudinal axis and the widthwise axis of the acicular particle 10 of interest being the front. In the front view, the widthwise length at one end of the longitudinal direction of the acicular particle 10 is not limited to the case where the widthwise length at the other end opposite to the one end is the same. The widthwise length of the acicular particle 10 may gradually increase or decrease from one end to the other end in the longitudinal direction. The widthwise length D of the acicular particle 10 is the maximum value from one end to the other end in the longitudinal direction. The widthwise length D of the acicular particle 10 is preferably 0.7 μm or more and 1.3 μm or less.
[0022] For example, as shown in Fig. 1, the longitudinal length L is specified as L1 to L5. The width direction length D is specified as D1 to D5. Furthermore, the thickness direction length T is specified by selecting an acicular particle 10 suitable for measuring the thickness direction, as shown in Fig. 2.
[0023] The acicular particles 10 according to this embodiment have an aspect ratio (L / T) of 80 to 150, and a widthwise length D of 0.5 μm to 2.0 μm, resulting in excellent orientation. The acicular particles 10 have a widthwise length D of 0.7 μm to 1.3 μm, resulting in even better orientation.
[0024] The acicular particle 10 preferably has a flat end face 12 at one end in the longitudinal direction of the acicular particle 10 of interest. The end face 12 is a surface that connects both sides that intersect in the width direction of the acicular particle 10 at one end in the longitudinal direction of the front of the acicular particle 10 of interest. The end face 12 is not limited to being parallel to the width direction, and may be inclined. The acicular particle 10 may have a flat end face at each of both ends in the longitudinal direction.
[0025] The calcium phosphate has a bulk specific volume of preferably 5 mL / g or more and 15 mL / g or less, more preferably 9 mL / g or more and 12 mL / g or less. The calcium phosphate has a large bulk specific volume by containing acicular particles 10 having an aspect ratio (L / T) of 80 or more and 150 or less, and a width direction length D of 0.5 μm or more and 2.0 μm or less. The bulk specific volume in this embodiment is a loose bulk specific volume. The packed bulk specific volume is about half of the above-mentioned loose bulk specific volume.
[0026] [Calcium phosphate manufacturing equipment] An example of a calcium phosphate manufacturing apparatus for manufacturing the above calcium phosphate will be described with reference to Fig. 3 and Fig. 4. Fig. 3 is a schematic diagram showing a calcium phosphate manufacturing apparatus according to this embodiment, and Fig. 4 is a schematic diagram showing a double-pipe mixer according to this embodiment. The manufacturing apparatus 14 includes a double-pipe mixer 16. The reaction apparatus 14 may further include an aging section 18.
[0027] The double-pipe mixing section 16 rapidly mixes the calcium hydroxide suspension and the phosphoric acid aqueous solution. The double-pipe mixing section 16 preferably mixes the calcium hydroxide suspension and the phosphoric acid aqueous solution by jet flow. The double-pipe mixing section 16 has an outer pipe 20 and an inner pipe 22. The inner pipe 22 is disposed within the outer pipe 20. The outer pipe 20 and the inner pipe 22 are preferably disposed coaxially.
[0028] The outer pipe 20 extends from upstream to downstream. An upstream end 20U of the outer pipe 20 is connected to an outer pipe side liquid feed pump (not shown). The calcium hydroxide suspension fed from the outer pipe side liquid feed pump flows from upstream to downstream in the outer pipe 20. A downstream end 20D of the outer pipe 20 is connected to the maturation section 18.
[0029] The inner pipe 22 extends from upstream to downstream. An upstream end 22U of the inner pipe 22 is connected to an inner pipe side liquid feed pump (not shown). The phosphoric acid aqueous solution fed from the inner pipe side liquid feed pump flows from upstream to downstream in the inner pipe 22. As shown in FIG. 4, the downstream end 22D of the inner pipe 22 may terminate upstream of the downstream end 20D of the outer pipe 20. That is, the double pipe mixer 16 may have a predetermined distance PL from the downstream end 22D of the inner pipe 22 to the downstream end 20D of the outer pipe 20 (FIG. 4).
[0030] The maturation section 18 has an aging tank 24 and a discharge pipe 25. The aging tank 24 has an inlet 26 and an outlet 28. The aging tank 24 receives the slurry discharged from the double-pipe mixing section 16 from the inlet 26. The aging tank 24 holds and matures the slurry in the aging tank 24 under conditions, for example, at a temperature of 60°C to 100°C for 2 minutes to 1 hour, and preferably at a temperature of 80°C to 100°C for 30 minutes to 1 hour. The discharge pipe 25 is connected to the outlet 28. The aging section 18 discharges the aged slurry from the aging tank 24 to the discharge pipe 25 through the outlet 28.
[0031] [Method of producing calcium phosphate] A method for producing calcium phosphate will be described using the above-mentioned production apparatus 14 as an example. Calcium phosphate can be produced by a mixing step. The method for producing calcium phosphate may further include an aging step. The steps will be described in order below. In the mixing step, an aqueous phosphoric acid solution and a suspension of calcium hydroxide are quickly mixed to obtain a slurry.
[0032] First, a mixture is mixed at a predetermined linear velocity V out The calcium hydroxide suspension is delivered at a linear velocity V out is the flow rate of the calcium hydroxide suspension flowing through the pipe divided by the cross-sectional area of the pipe. out The calcium hydroxide suspension is flowing at a predetermined linear velocity V from the inner pipe 22 of the double-pipe mixing section 16 so as to contact the calcium hydroxide suspension. in The phosphoric acid aqueous solution is delivered at a linear velocity of V inis the flow rate of the phosphoric acid aqueous solution flowing through the pipe divided by the cross-sectional area of the pipe. The volume mean diameter (MV) of calcium hydroxide contained in the calcium hydroxide suspension may be, for example, 6 to 10 μm. in and linear velocity V out may be the same or different.
[0033] The aqueous phosphoric acid solution and the suspension of calcium hydroxide come into contact with each other at the above-mentioned predetermined linear velocity and are mixed by the jet stream. The mixing of the aqueous phosphoric acid solution and the suspension of calcium hydroxide is completed through the mixing zone Z (FIG. 4).
[0034] The mixing section Z is a section where the phosphoric acid aqueous solution flowing out from the pipe and the calcium hydroxide suspension flowing out from the pipe join together and become a steady flow. As a result, a slurry containing acicular particles 10 is generated in the mixing section Z and further downstream from the mixing section Z.
[0035] The linear velocity V of the phosphoric acid solution flowing through the pipe in and the linear velocity V of the calcium hydroxide suspension flowing through the pipe. out Ratio to (V in / V out ) is preferably 10 or more and 20 or less. in and the linear velocity V of the calcium hydroxide suspension. out When the linear velocity ratio is within the above range, the suspension of calcium hydroxide and the aqueous phosphoric acid solution can be mixed rapidly.
[0036] In this embodiment, the calcium hydroxide suspension and the phosphoric acid aqueous solution pass through the mixing zone Z and become a steady flow, completing the mixing. That is, in order to rapidly mix the calcium hydroxide suspension and the phosphoric acid aqueous solution, it is preferable that the mixing zone Z is short. The linear velocity V of the phosphoric acid aqueous solution in and the linear velocity V of the calcium hydroxide suspension out Linear velocity ratio (V in / V out ) is larger, the shorter the mixing interval is.
[0037] When mixing a suspension of calcium hydroxide with an aqueous phosphoric acid solution, it is preferable that the dissipation energy ε represented by the following formula 1 is large.
[0038]
number
[0039] Q is the flow rate, ΔP is the pressure loss in the space of interest, V is the volume of the space of interest, ρ is the density, and τ is the residence time. The dissipated energy ε can be increased by narrowing the flow path through which the fluid flows or by increasing the flow rate to shorten the residence time. In addition, if a mixed fluid of a calcium hydroxide suspension and an aqueous phosphoric acid solution is made into a jet stream, ΔP will be larger. As a result, the dissipated energy ε can be increased.
[0040] In the maturation step, the slurry obtained in the mixing step is kept in the maturation section 18 at a temperature of 60° C. to 100° C. for 2 minutes to 1 hour, preferably at a temperature of 80° C. to 100° C. for 30 minutes to 1 hour, to mature the slurry. By passing through the maturation step, the slurry becomes calcium phosphate with high purity.
[0041] The manufacturing method may further include a washing step and a drying step. In the washing step, the slurry after the aging step is first suction filtered using filter paper to obtain a cake. Then, the obtained cake is washed with ion-exchanged water. By passing through the washing step, impurities can be removed and the purity can be further increased. In the drying step, the cake can be heated to obtain dried acicular particles.
[0042] [Action and Effects] Calcium phosphate contains needle-like particles 10 with an aspect ratio (L / T) of 80 to 150 and a width direction length D of 0.5 μm to 2.0 μm, and thus has better orientation than plate-like, foil-like, and palisade-like particles. Calcium phosphate has excellent orientation, and can be suitably used, for example, as a filler. Calcium phosphate can be used, for example, as a filler for paints, resins, and medicines.
[0043] The acicular particles 10 have a flat end surface 12 at one end in the longitudinal direction, and therefore are easier to maintain their particle shape compared to particles with pointed tips. The acicular particles 10 have an aspect ratio (L / T) of 80 to 150 and a width D of 0.5 μm to 2.0 μm, and therefore calcium phosphate having a bulk specific volume of 5 mL / g to 15 mL / g is obtained.
[0044] Calcium phosphate can be produced by a production method including a mixing step of mixing an aqueous phosphoric acid solution with a suspension of calcium hydroxide to obtain a slurry, and an aging step of aging the slurry at a temperature of 80° C. or higher. In the mixing step, the aqueous phosphoric acid solution and the suspension are mixed by a jet stream. By rapidly mixing the aqueous phosphoric acid solution with the suspension of calcium hydroxide by, for example, a jet stream, acicular particles 10 can be obtained.
[0045] In the manufacturing method of this embodiment, by using the double-pipe mixer 16, it is possible to more reliably generate a jet stream of a mixture of the phosphoric acid aqueous solution and the calcium hydroxide suspension.
[0046] The slurry obtained in the double-pipe mixer 16 can be continuously processed by receiving and maturing it in the maturation tank 24, so that calcium phosphate can be obtained more efficiently.
[0047] [Measurement method] (aspect ratio and width) The size of the needle-like particles is observed by a scanning electron microscope (SEM). The magnification of the SEM observation is, for example, 5,000 times to 20,000 times. In the captured image, for example, five needle-like particles are arbitrarily selected, and the longitudinal length L and the width direction length D are measured. In addition, the same number of needle-like particles (five in this case) suitable for measuring the thickness direction length T are arbitrarily selected, and the thickness direction length T is measured. The average value of the aspect ratio (L / T) is calculated from the total value of the measured longitudinal length L and the total value of the measured thickness direction length T. The average value is the aspect ratio (L / T) of the calcium phosphate. In addition, the average value calculated from the total value of the width direction length D is the width direction length D of the calcium phosphate.
[0048] (Bulk ratio) Gently place 5 g of calcium phosphate into a 50 mL measuring cylinder, level it evenly, and read the volume of the calcium phosphate. Calculate the mass of the calcium phosphate packed in by the volume, and use this value as the loose bulk specific volume.
[0049] [Variations] The present invention is not limited to the above embodiment, and can be appropriately modified within the scope of the present invention. For example, in the above embodiment, the needle-shaped particles have a flat end face at one end in the longitudinal direction, but the present invention is not limited to this. The needle-shaped particles may have an end face including a convex portion or a concave portion at one or both ends in the longitudinal direction.
[0050] Although the needle-shaped particles in the above embodiment are produced using a double-pipe mixer, the present invention is not limited to this. The needle-shaped particles may be produced using other methods as long as the calcium hydroxide suspension and the phosphoric acid aqueous solution can be mixed quickly, for example, by a jet stream. EXAMPLES
[0051] The present invention will be described in more detail below with reference to examples. However, these examples are merely illustrative and are not intended to limit the present invention in any way.
[0052] [sample] According to the above "Calcium phosphate manufacturing method", samples were produced using the double-pipe mixing section shown in "Calcium phosphate manufacturing apparatus". Details of each material are explained below.
[0053] Example 1 A 4.9 mol% aqueous solution of phosphoric acid whose temperature was adjusted to 80° C. and a 3.7 mol% suspension of calcium hydroxide whose temperature was adjusted to 80° C. were prepared. A double-pipe mixing section was prepared, with an outer pipe having an inner diameter of 8 mm, an inner pipe having an inner diameter of 1.8 mm, and the length of the PL part in Figure 4 being 80 mm.
[0054] Next, a constant volume pump was used to supply the phosphoric acid aqueous solution to the outer tube and the calcium hydroxide suspension to the inner tube. The solution was supplied to the double tube mixing section so that the phosphorus to calcium ratio during the reaction was 1:1. The supply rate of the phosphoric acid aqueous solution and the calcium hydroxide suspension was 180 ml / min. The reaction was continued under these conditions for 2 minutes, and 716 mL of slurry was obtained. The obtained slurry was suction filtered using filter paper to obtain a cake. The obtained cake was washed with 975 mL of ion-exchanged water. It was then dried overnight at 105°C to obtain calcium hydrogen phosphate of Example 1.
[0055] Example 2 The same procedure as in Example 1 was carried out except that the slurry obtained after the reaction was aged at 80° C. for 1 hour, to obtain calcium hydrogen phosphate of Example 2.
[0056] (Reference example 1) 100 mL of ion-exchanged water was placed in a batch reaction tank, and the temperature was adjusted to 80°C. While stirring the ion-exchanged water at 300 rpm, a 0.51 mol / L aqueous solution of phosphoric acid and a 0.51 mol / L solution of calcium chloride were mixed, and a 0.67 mol / L solution of sodium hydroxide was simultaneously poured in over about 1 minute to start the reaction. After the pouring was completed, the mixture was filtered, washed and dried in the same manner as in Example 1, and a sample of Reference Example 1 was obtained. (Reference example 2) After the addition was completed, the same procedure as in Reference Example 1 was carried out except that the obtained slurry was aged at 80° C. for 1 hour, to obtain a sample of Reference Example 2.
[0057] [Measurement results] The measurement results of the obtained acicular particles are shown in Table 1, and an SEM photograph is shown in FIG.
[0058] [Table 1] As shown in Table 1 and FIG. 5, it was confirmed that in Example 1, needle-like particles having an aspect ratio (L / T) of 80 or more and 150 or less, and a width direction length D of 1.4 μm to 1.6 μm or less were obtained. It was confirmed from the SEM observation photograph that the aspect ratio (L / T) and width direction length D of Example 2 were equivalent to those of Example 1. In contrast, as is clear from the SEM observation photograph, Reference Examples 1 and 2 were thin plate-like particles with a large width direction length. It was also confirmed that Examples 1 and 2 had a larger bulk specific volume than Reference Examples 1 and 2. [Explanation of symbols]
[0059] 10 Acicular particles 12 End face 14 Manufacturing equipment 16 Double tube mixing section 18. Aging Department 20 outer tube 20D Downstream end 20U upstream end 22 Inner tube 22D Downstream end 22U Upstream end 24 Aging tank 25 Discharge piping 26 Entrance 28 Exit
Claims
1. A calcium phosphate containing needle-shaped particles each having a length L in a longitudinal direction, a length T in a thickness direction, and a length D in a width direction, The acicular particles have an aspect ratio (L / T) of 80 or more and 150 or less, and a length D in the width direction of 0.5 μm or more and 2.0 μm or less. Calcium phosphate.
2. The calcium phosphate according to claim 1 , wherein the acicular particles have a flat end surface at one end in the longitudinal direction.
3. 2. The calcium phosphate of claim 1, wherein the acicular particles are produced by mixing an aqueous solution of phosphoric acid with a suspension of calcium hydroxide in a jet stream.
4. The acicular particles are produced by mixing an aqueous phosphoric acid solution and a suspension of calcium hydroxide using a double-pipe mixer; The double-pipe mixing section includes an outer pipe and an inner pipe disposed within the outer pipe, The method for producing calcium phosphate according to claim 1 , wherein the calcium hydroxide suspension is supplied to the outer tube, and the phosphoric acid aqueous solution is supplied to the inner tube.
5. 2. The calcium phosphate according to claim 1, having a bulk specific volume of 5 mL / g or more and 15 mL / g or less.
6. The method includes a mixing step of mixing an aqueous phosphoric acid solution with a suspension of calcium hydroxide to obtain a slurry, The method for producing calcium phosphate, wherein the mixing step includes mixing the aqueous phosphoric acid solution and the suspension by a jet stream.
7. The mixing step uses a double-pipe mixing section, The double-pipe mixing section includes an outer pipe and an inner pipe disposed within the outer pipe, The method for producing calcium phosphate according to claim 6, wherein the calcium hydroxide suspension is supplied to the outer tube, and the phosphoric acid aqueous solution is supplied to the inner tube.
8. The method further includes a maturation step of maturating the slurry at a temperature of 60° C. or more and 100° C. or less, The aging step uses an aging tank, 8. The method for producing calcium phosphate according to claim 7, wherein the maturation tank is provided downstream of the double-pipe mixing section and receives the slurry discharged from the double-pipe mixing section.
9. The calcium phosphate includes needle-shaped particles each having a length L in a longitudinal direction, a length T in a thickness direction, and a length D in a width direction, 7. The method for producing calcium phosphate according to claim 6, wherein the acicular particles have an aspect ratio (L / T) of 80 or more and 150 or less, and a length D in the width direction of 0.5 μm or more and 2.0 μm or less.
Citation Information
Patent Citations
Microfluidic chip based method for synthesizing needle-like hydroxyapatite nanoparticle
CN102745660A
Production of hydroxyapatite
JP1988170205A
Hydroxyapatite pigment and its production and cosmetic
JP2000143443A
Hydroxyapatite particle
JP2017171573A
Acicular hydroxyapatite particle and method for producing the same
JP2020111484A