Laminate having primer composition layer for desorption and laminate desorption method

The laminate structure with EVOH or alternative release primer layers addresses the issue of poor gas barrier properties and facilitates easy separation of layers for recycling, enhancing sustainability.

JP2024159220APending Publication Date: 2024-11-08SAKATA INX
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2023075067
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing laminates for packaging materials have insufficient gas barrier properties under high temperature and high humidity conditions, and there is a need for effective methods to separate and detach printed layers from resin base and sealant layers for recycling.

Method used

A laminate structure comprising a resin base material layer, a release primer layer, and a printing layer, where at least one release primer layer is made of ethylene vinyl alcohol (EVOH) or alternative compositions like polyethyleneimine, polybutadiene, or polyvinyl alcohol, with specific ethylene content and saponification degrees, allowing for easy separation using a desorption liquid.

Benefits of technology

The laminate achieves excellent gas barrier properties under high temperature and high humidity conditions, enabling easy separation and recycling of resin base and sealant layers, thus improving environmental sustainability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159220000001
    Figure 2024159220000001
  • Figure 2024159220000002
    Figure 2024159220000002
  • Figure 2024159220000003
    Figure 2024159220000003
Patent Text Reader

Abstract

To reliably bond a resin base material layer and a printed layer during use, ensure excellent barrier properties under high temperature and high humidity, simply separate and desorb the printed layer from the resin base material layer after use, and then easily separate and desorb the printed layer from a desorption liquid.SOLUTION: A laminate is constituted by laminating a resin base material layer, a primer layer for desorption, a printed layer, a primer layer for desorption and a sealant layer, wherein the primer composition for desorption forming at least one layer out of the two primer layers for desorption is a primer composition for desorption containing an ethylene vinyl alcohol-based resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate having a removal primer composition layer and a method for removing the laminate. [Background technology]

[0002] Packaging materials using various plastic films are used for food, confectionery, household goods, pet food, etc., from the viewpoints of design, economy, content protection, transportability, etc. Furthermore, gravure printing or flexographic printing is applied to many packaging materials with the intention of adding designs and messages that will appeal to consumers. In order to obtain these packaging materials, printing is performed by printing directly onto the surface of the base film of the packaging material, or by applying an adhesive or anchor agent to the printed surface printed on the surface of the base film of the packaging material as necessary and laminating the base film. In printing for lamination, a colored ink composition and a white ink composition are printed in that order on various substrate films such as polyester, nylon, and aluminum foil, and then a polyethylene film or polypropylene film for heat sealing is laminated on the printed layer of the white ink composition by dry lamination using an adhesive or extrusion lamination using an anchor coating agent (see Patent Document 1).

[0003] In recent years, packaging made from plastic film, plastic bottles, and other plastic products have been discarded and dumped into the ocean as garbage, causing environmental pollution. These plastic products break down in seawater and become submicron-sized fragments (microplastics), which float in the seawater. If marine organisms such as fish ingest this plastic, it will accumulate in their bodies. This could have an impact on the health of seabirds and humans who consume the marine organisms as food. As one of various efforts to reduce microplastics in order to improve such problems, a recycling method has been proposed in which the plastic substrate of a laminate is removed from a laminate in which a printing ink composition is laminated. As a method for removing the plastic substrate of a laminate, a removing ink composition (e.g., see Patent Document 2), a removing adhesive (e.g., see Patent Document 3), a removing anchor coating agent, etc. (e.g., see Patent Documents 4 to 6), and a removing liquid (e.g., see Patent Document 7) have been proposed.

[0004] However, these methods have the problem that the barrier properties are insufficient when used in a laminate printing ink composition. It has also been proposed to provide a resin layer containing polyvinyl alcohol (hereinafter sometimes referred to as PVA) as a release layer (see, for example, Patent Document 8). However, when a resin layer containing polyvinyl alcohol is provided as a release layer, there is a problem that the gas barrier properties are reduced under high temperature and high humidity conditions. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 5-97959 [Patent Document 2] Patent No. 6631964 [Patent Document 3] Patent No. 6642688 [Patent Document 4] Patent No. 6388131 [Patent Document 5] JP 2020-175620 A [Patent Document 6] Patent Publication No. 2023-50125 [Patent Document 7] Patent No. 6690806 [Patent Document 8] International Publication No. 2021 / 090690 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a film that has excellent gas barrier properties under high temperature and high humidity conditions, and that allows a printed layer and a resin substrate layer, and a printed layer and a sealant layer to be separated and detached after use. [Means for solving the problem]

[0007] The present inventors have found that the above problems can be solved by using the laminate and the method for removing the laminate described below, and have arrived at the present invention described below. 1. A laminate comprising a resin substrate layer, a detachable primer layer, a printed layer, a detachable primer layer, and a sealant layer, wherein at least one of the two detachable primer layers is formed from a detachable primer composition containing an ethylene-vinyl alcohol-based resin. 2. A laminate according to 1, wherein when one of the two detachable primer layers is a layer made of a detachable primer composition that does not contain an ethylene vinyl alcohol-based resin, the detachable primer composition that does not contain an ethylene vinyl alcohol-based resin is any one of A to B below. A. Desorption primer composition containing a polyethyleneimine compound B. Detachment primer composition containing a polybutadiene compound C. Detachment primer composition containing polyvinyl alcohol 3. The laminate according to 1 or 2, wherein the content of ethylene units in all monomers constituting the ethylene-vinyl alcohol resin is 1 to 35 mol %. 4. The laminate according to any one of 1 to 3, wherein the ethylene-vinyl alcohol resin has a degree of saponification of 90% or more. 5. The solid coating amount of the detachable primer layer formed from the detachable primer composition containing the ethylene vinyl alcohol resin is 0.1 to 2.0 g / m 2 5. The laminate according to any one of 1 to 4, wherein 6. A method for removing a resin substrate layer, comprising the steps of immersing the laminate according to any one of 1 to 5 in a removing liquid, and recovering the resin substrate layer and the printed layer. Effect of the Invention

[0008] According to the present invention, the resin substrate layer and the sealant layer constituting the laminate can be easily removed from the printed layer by using a release liquid. As a result, the printed layer and the other layers can be collected separately, and the resin substrate layer and the sealant layer can be reused. In addition, the laminate can have excellent barrier properties under high temperature and high humidity conditions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention is a laminate comprising a resin substrate layer, a detachable primer layer, a printing layer, a detachable primer layer, and a sealant layer, wherein at least one of the detachable primer layers is made of a detachable primer composition containing an ethylene-vinyl alcohol-based resin. The laminate of the present invention may be formed only from the above-mentioned resin substrate layer, detachable primer layer, printed layer, detachable primer layer and sealant layer, or an anchor coat layer or an adhesive layer may be formed between any of these layers. Furthermore, the laminate of the present invention may be formed by forming a detachable primer layer and a printed layer on the entire surface of the resin substrate layer on the side on which the detachable primer layer is formed, and further laminating a detachable primer layer and a sealant layer, or may be formed by forming a detachable primer layer and a printed layer on a portion of the surface of the resin substrate layer on which the detachable primer layer is formed, and further laminating a detachable primer layer and a sealant layer.

[0010] [Resin base layer] The resin substrate layer in the present invention may be one layer or multiple layers. It may be a resin film in which a resin is laminated on a paper substrate. In addition, a laminate having a thermoplastic resin layer and a polyethylene-based resin layer may or may not be used. As such a resin substrate layer, a resin substrate layer containing a known resin and capable of being printed on the surface, and a resin film for laminate printing can be adopted. As such a resin substrate layer, a resin film such as polyester such as polyethylene terephthalate (PET), polyolefin such as polyethylene (PE) and polypropylene (PP), polyamide such as nylon (NY), the above resin film having a metal layer such as aluminum, the above resin film having a transparent deposition layer, etc. can be adopted. Specifically, biaxially oriented polypropylene, polyester, oriented nylon, transparent deposition film, etc., which have water resistance, heat resistance, impact resistance, and excellent moisture resistance and gas barrier properties, are preferred. Furthermore, the resin substrate layer may be in a plate shape rather than a film shape.

[0011] The surface of the resin substrate layer on which the layer of the removable primer composition is to be formed may be subjected to a surface treatment in advance. As such a surface treatment, a surface treatment for improving the adhesion between the surface of the resin substrate layer and the layer of the removable primer composition can be selected, such as a plasma treatment, a corona discharge treatment, or the formation of an anchor coat layer or an adhesive layer.

[0012] [Removable primer layer] The detachable primer layer in the present invention is provided between the surface of the resin substrate layer and the printed layer, and / or between the printed layer and the sealant layer, and is a detachable primer layer for separating the resin substrate layer and the printed layer, and separating the printed layer and the sealant layer, and detaching the printed layer from the resin substrate layer when reusing the printed matter after use, thereby detaching the printed layer from the sealant layer. Therefore, the application and required properties are different from those of anchor coating agents used when simply forming an anchor coating layer on the printed surface formed on a substrate and laminating a resin film or the like thereon. The detachment primer composition containing an ethylene-vinyl alcohol resin for forming the detachment primer layer will be described below.

[0013] An example of the removable primer layer for obtaining the laminate of the present invention is one that is formed before printing on the resin substrate layer with a printing ink composition. Furthermore, before the print layer and the sealant layer are dry laminated and / or before the print layer and the sealant layer are extrusion laminated, a removable primer layer may be formed in advance using a removable primer composition. The detachment primer composition for forming the detachment primer layer disposed so as to be located between the resin substrate layer and the printed layer, and the detachment primer composition for forming the detachment primer layer disposed so as to be located between the printed layer and the sealant layer may be the same or different. The detachment primer composition containing an ethylene-vinyl alcohol resin for forming the detachment primer layer will be described below.

[0014] <Detachment primer composition containing ethylene vinyl alcohol resin> The laminate of the present invention has a layer made of a release primer composition containing an ethylene-vinyl alcohol-based resin. (Ethylene vinyl alcohol resin) Ethylene-vinyl alcohol-based resins are obtained by saponifying ethylene-vinyl acetate copolymers, and have the properties of excellent moisture barrier properties and high transparency. The ethylene-vinyl alcohol-based resin may contain copolymer units derived from ethylene and a vinyl alcohol structure as copolymer components, in addition to the copolymer units derived from vinyl acetate and its saponification product and the copolymer units derived from ethylene. The ethylene content is a value obtained by dividing the number of moles of ethylene by the total number of moles of all the copolymerization components, with ethylene constituting the ethylene-vinyl alcohol resin as one copolymerizable component and another component having an unsaturated double bond as the other copolymerization component. The ethylene content of the ethylene-vinyl alcohol resin is preferably 1 mol % or more, more preferably 4 mol % or more, and is preferably 35 mol % or less, more preferably 30 mol % or less. If the ethylene content is less than 1 mol %, the gas barrier properties at high temperature and high humidity tend to decrease, whereas if the ethylene content is more than 35 mol %, the viscosity tends to increase. The ethylene vinyl alcohol resin preferably has a degree of saponification of 95% or more, more preferably 96% or more. If the degree of saponification is less than 95%, the gas barrier property and oil resistance may decrease. The release primer composition can be obtained by adding an ethylene-vinyl alcohol-based resin to a mixed solvent of lower alcohols as required, and dissolving the resin with stirring.

[0015] The detachment primer composition may contain an inorganic layered compound within a range in which the adhesion to adjacent layers such as the surface of the resin substrate layer or the printed layer is not reduced, and / or the lamination suitability is not reduced. As the inorganic layered compound, inorganic layered compounds that swell and cleave in the dispersion medium can be used. For example, kaolinite group having a 1:1 structure of phyllosilicate, antigorite group belonging to the jamonite group, smectite group depending on the number of interlayer cations, vermiculite group which is a hydrous silicate mineral, mica group, etc. can be mentioned. Specific examples of inorganic layered compounds include kaolinite, dickite, nacrite, halloysite, antigorite, chrysotile, pyrophyllite, montmorillonite, beidellite, hectorite, saponite, sauconite, stevensite, tetrasilylic mica, sodium taeniolite, muscovite, margarite, talc, vermiculite, phlogopite, xanthophyllite, and chlorite, which may be natural or synthetic. In addition, scaly silica and the like can also be used. These may be used alone or in combination of two or more kinds. Among these, montmorillonite is preferred from the viewpoints of coatability and gas barrier properties when used in a barrier coating agent.

[0016] The dispersion medium contained in the detachment primer composition may be either an aqueous dispersion medium or an organic dispersion medium. The aqueous dispersion medium may be water alone, or may be a dispersion medium containing water and a water-miscible organic solvent such as an alcohol such as methanol, ethanol, or propanol, a polyhydric alcohol such as ethylene glycol or propylene glycol, an alkyl ether derivative thereof, an ester such as ethyl formate, methyl acetate, or ethyl acetate, or a ketone such as acetone. As the dispersion medium, from the viewpoint of maintaining an appropriate solid content, it is preferable to use a mixture containing 50 to 95 mass % of water and 5 to 50 mass % of at least one of ethyl alcohol, propyl alcohol, and butyl alcohol, which are lower alcohols having 2 to 4 carbon atoms. The amount of the removable primer layer is 0.1 to 2 g / m 2 The preferred range is 0.1 g / m2. 2 If it is less than 2 g / m, the releasing property tends to decrease. 2 If the amount is larger, the adhesiveness tends to decrease.

[0017] <Removal primer compositions other than detachment primer compositions containing ethylene vinyl alcohol-based resins> In the present invention, as the detachment primer composition, a layer made of a detachment primer composition other than the ethylene vinyl alcohol resin-containing detachment primer composition may be used for at most one layer. As such a detachment primer composition that does not contain an ethylene vinyl alcohol polymerization resin, a composition containing at least one selected from A. a detachment primer composition containing a polyethyleneimine-based compound, B. a detachment primer composition containing a polybutadiene-based compound, and C. a detachment primer composition containing polyvinyl alcohol can be used.

[0018] In addition, each of A. the detachment primer composition containing a polyethyleneimine compound, B. the detachment primer composition containing a polybutadiene compound, and C. the detachment primer composition containing polyvinyl alcohol may contain an inorganic layer compound that can be contained in the detachment primer composition containing the above-mentioned ethylene vinyl alcohol (EVOH) resin, if necessary. Furthermore, the type and composition of the dispersion medium used, and the concentrations of the polyethyleneimine compound, the polybutadiene compound, and the polyvinyl alcohol can be selected from the same range as that of the detachment primer composition containing the above-mentioned ethylene vinyl alcohol (EVOH) resin. In addition, the amount of the layer consisting of the detachment primer composition other than these detachment primer compositions containing an ethylene vinyl alcohol (EVOH) resin can also ... 2 The preferred range is 0.1 g / m2. 2 If it is less than 2 g / m, the releasing property tends to decrease. 2 If the amount is larger, the adhesiveness tends to decrease.

[0019] (A. Desorption primer composition containing a polyethyleneimine compound) The polyethyleneimine compounds used in the detachment primer composition containing a polyethyleneimine compound can be further divided into A-1 to A-3, which are: A-1. polyethyleneimine compound, A-2. mixture containing a polyethyleneimine compound and a glycidyl group-containing silane coupling agent and / or an isocyanate group-containing silane coupling agent, and A-3. siloxane-modified polyethyleneimine compound. These compounds A-1 to A-3 are different from each other and do not overlap. The polyethyleneimine compound A preferably has an amine value of 5.0 to 25.0 mmol / g.

[0020] (A-1. Polyethyleneimine Compounds) A-1. As the polyethyleneimine compound, the polyethyleneimine compound preferably has an amine value of 15.0 to 25.0 mmol / g, more preferably 16.0 mmol / g or more and 20.0 mmol / g or less. In addition, it is preferable that the polyethyleneimine-based compound has all of the amino groups in the molecule, from the primary amino group to the tertiary amino group.Moreover, it is preferable that the secondary amino group is contained more than the primary and tertiary amino groups, and more preferably, the number of secondary amino groups to the total number of all amino groups from the primary to the tertiary is 40% or more.The more within these ranges, the easier the removal can be performed. The detachment primer composition containing the polyethyleneimine compound can be obtained by adding a solvent to the polyethyleneimine compound and stirring the mixture. As the solvent, a mixture of water and one or more alcohols such as methanol, ethanol, and isopropyl alcohol can be used. It should be noted that A-1. polyethyleneimine compound does not include A-3. siloxane-modified polyethyleneimine compound, and A-3. siloxane-modified polyethyleneimine compound is a compound different from A-1. polyethyleneimine compound.

[0021] (A-2. Mixture containing a polyethyleneimine compound and one or more selected from a glycidyl group-containing silane coupling agent and / or an isocyanate group-containing silane coupling agent) In order to further improve lamination suitability compared to the case where the above A-1. polyethyleneimine compound is used, it is preferable to further contain a silane coupling agent containing a glycidyl group and / or an isocyanate group in the above polyethyleneimine compound. As the polyethyleneimine compound, the above A-1. Polyethyleneimine compound can be used, and this polyethyleneimine compound does not include A-3. Siloxane-modified polyethyleneimine compound.

[0022] Examples of silane coupling agents containing a glycidyl group include 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropylmethoxydimethoxysilane, 3-glycidyloxypropylmethoxydiethoxysilane, and 3-glycidyloxypropyltriethoxysilane.

[0023] Examples of silane coupling agents containing an isocyanate group include 3-isocyanatepropyltriethoxysilane, 3-isocyanatepropyltrimethoxysilane, 2-isocyanateethyltriethoxysilane, and 2-isocyanateethyltrimethoxysilane.

[0024] From the viewpoint of suitability for lamination after retort, it is preferable to mix the silane coupling agent containing a glycidyl group and the silane coupling agent containing an isocyanate group so that the ratio of (the number of glycidyl groups of the silane coupling agent + the number of isocyanate groups) to (the number of amino groups of the polyethyleneimine compound) ((the number of glycidyl groups of the silane coupling agent + the number of isocyanate groups of the silane coupling agent) / the total number of primary amino groups and secondary amino groups of the polyethyleneimine compound) is 0.20 to 2.50. It is more preferable that the ratio is 0.30 or more, more preferably 2.20 or less, and even more preferably 1.90 or less. The number of amino groups is the sum of the number of primary amino groups and the number of secondary amino groups. This ratio of (the number of glycidyl groups in the silane coupling agent + the number of isocyanate groups) to (the number of amino groups in the polyethyleneimine compound) ((the number of glycidyl groups in the silane coupling agent + the number of isocyanate groups) / (the total number of primary amino groups and secondary amino groups in the polyethyleneimine compound)) can be calculated using the following formula:

[0025] [(Amount of glycidyl-containing silane coupling agent applied (g / m 2 ) × average number of glycidyl groups in one molecule) / average molecular weight of glycidyl group-containing silane coupling agent (g / mmol)] + [(coating amount of isocyanate group-containing silane coupling agent (g / m2 ) × average number of isocyanate groups in one molecule) / average molecular weight of isocyanate group-containing silane coupling agent (g / mmol)], [(coating amount of polyethyleneimine compound (g / m 2 ) × amine value (mmol / g) × (average (number of primary amino groups + number of secondary amino groups) per molecule) / (average (number of primary amino groups + number of secondary amino groups + number of tertiary amino groups) per molecule).

[0026] In addition, when the detachment primer composition of the present invention selectively contains both A-1. polyethyleneimine compound and A-2. a mixture containing a polyethyleneimine compound and a glycidyl group-containing silane coupling agent and / or an isocyanate group-containing silane coupling agent, these overlap in that they contain a polyethyleneimine compound, and therefore, in effect, a mixture containing A-2. a polyethyleneimine compound and a glycidyl group-containing silane coupling agent and / or an isocyanate group-containing silane coupling agent has been selected. The detachment primer composition containing a mixture containing a polyethyleneimine compound and one or more selected from a glycidyl group-containing silane coupling agent and an isocyanate group-containing silane coupling agent can be obtained by adding a solvent to the polyethyleneimine compound, stirring, and then further adding a glycidyl group-containing silane coupling agent and / or an isocyanate group-containing silane coupling agent and stirring. As the solvent, a mixture of water and one or more alcohols such as methanol, ethanol, and isopropyl alcohol can be used.

[0027] (A-3. Siloxane-modified polyethyleneimine compounds) To improve lamination suitability, a siloxane-modified polyethyleneimine compound can be used. The amine value of the siloxane-modified polyethyleneimine compound is preferably 5.0 mmol / g or more and 15.0 mmol / g or less. A-3. The siloxane-modified polyethyleneimine compound is a compound having the formula: RZ-SiY3 and a silane coupling agent-modified polyethyleneimine compound obtained by reacting at least one amine-reactive hydrolyzable organosilane represented by the formula: [wherein R represents an amine-reactive group selected from the group consisting of an isocyanate group, an oxiranyl group, a glycidoxy group, an acryloxy group, a carbethoxy group, a carbomethoxy group, a vinylsulfonyl group, and an acrylamide group, Z represents a divalent organic group containing a carbon atom, and each Y independently represents a hydrolyzable group], and a component comprising the following compound can be used. This siloxane-modified polyethyleneimine compound has a structure in which the group R of the silane coupling agent reacts with the amino group of polyethyleneimine to bond the silane coupling agent to the polyethyleneimine. However, as described above, it is preferable that the siloxane-modified polyethyleneimine compound has a predetermined amine value.

[0028] A-3. The detachment primer composition containing the siloxane-modified polyethyleneimine compound can be obtained by adding a solvent to the siloxane-modified polyethyleneimine and stirring the mixture. As the solvent, a mixture of water and one or more alcohols such as methanol, ethanol, and isopropyl alcohol can be used. The molecular weights of the polyethyleneimine compounds in A-1 and A-2 and the siloxane-modified polyethyleneimine compound in A-3 that may be contained in the primer composition of the present invention are preferably each independently a number average molecular weight of 1,000 to 200,000 in terms of suitability for lamination, and each independently a mass average molecular weight of 4,000 to 800,000. It should be noted that A-3. siloxane-modified polyethyleneimine compound is not included in the above a. polyethyleneimine compound and A-2. polyethyleneimine compound, and is a compound different from the polyethyleneimine compound.

[0029] (B. Detachment primer composition containing a polybutadiene compound) The polybutadiene-based compound-containing detachment primer composition is preferably an aqueous composition. In order to make it aqueous and improve adhesion, a hydroxyl group-containing polybutadiene compound or a carboxyl group-containing polybutadiene compound in which a hydroxyl group or a carboxyl group is introduced into a polybutadiene compound is preferred. In order to exert detachment properties, it is preferable that the polybutadiene compound is not crosslinked. Specific examples include EL-451 (Toyo-Morton Co., Ltd.) and T-180E (Nippon Soda Co., Ltd.). The polybutadiene-based compound-containing detachment primer composition can be obtained by adding a solvent to the polybutadiene-based compound and stirring the mixture. The solvent can be a mixture of water and one or more alcohols such as methanol, ethanol, and isopropyl alcohol.

[0030] (C. Detachment primer composition containing polyvinyl alcohol) Polyvinyl alcohol is a water-soluble resin obtained by saponifying polyvinyl acetate. It is used as a water-soluble packaging material, adhesive, emulsifier, etc., and is the raw material for the synthetic fiber Vinylon. It is generally abbreviated to poval or PVA. Commercially available products include Kuraray's Poval, Elvanol, and Exeval, Mitsubishi Chemical's Gohsenol, and Nippon Vinyl Acetate & Poval. The degree of saponification of polyvinyl alcohol is determined by the ratio of vinyl groups in polyvinyl acetate replaced with hydroxyl groups, and the degree of saponification is preferably 90% or more. Examples of polyvinyl alcohol with a degree of saponification of 90% or more include, but are not limited to, the following commercially available products: Kuraray Co., Ltd. Poval "3-98, 5-98, 28-98, 60-98, 27-96", Kuraray Co., Ltd. Elvanol "71-30, 90-50, T-25, T-66", Kuraray Co., Ltd. Exeval "AQ-4104, HR-3010, RS-2117, RS-1717", Mitsubishi Chemical Co., Ltd. Gohsenol "N-300, NL-050 ... ,A-300,AL-06R", Japan Vinyl Acetate & Poval Co., Ltd.'s "JC-25, JC-33, JC-40, JF-02, JF-03, JF-04, JF-05, JF-10, JF-17, JF-17L, JF-22, JM-17, JM-17L, JM-23, JM-26, JM-33, JT-05, JT-13Y", etc. The polyvinyl alcohol-containing release primer composition can be obtained by adding a solvent to polyvinyl alcohol and stirring the mixture. The solvent can be a mixture of water and one or more alcohols such as methanol, ethanol, and isopropyl alcohol.

[0031] [Print layer] In the present invention, the printed layer printed with the printing ink composition may be a known printing ink composition for lamination, such as a gravure printing ink composition for lamination, an active energy ray-curable offset printing ink composition for lamination, or an active energy ray-curable inkjet composition for lamination. In the laminate of the present invention, the above-mentioned detachment primer layer is formed on both sides of the printing layer. In addition, when the detachment primer composition is provided between the resin substrate layer and the printing layer, an anchor coating agent layer may be formed on the surface of the resin substrate layer, and then a detachment primer composition layer may be formed on the layers, and a printing layer may be further formed on the layer. In these cases, the surface of the resin substrate layer and the printing layer are not in direct contact with each other. However, the resin substrate layer can be peeled off from the printing layer together with the anchor coating agent layer.

[0032] <Gravure printing ink composition for lamination> Examples of gravure printing inks for lamination include gravure printing inks for reverse printing that contain a binder resin, a colorant, a solvent such as an organic solvent or an aqueous medium, and additives. As the binder resin, a (biomass) urethane resin, and if necessary, a vinyl chloride / vinyl acetate copolymer or a rosin-based resin are used. The colorant may be an organic or inorganic pigment or dye used in a general gravure ink. The organic pigment may be an azo pigment, a phthalocyanine pigment, an anthraquinone pigment, a perylene pigment, a perinone pigment, a quinacridone pigment, a thioindigo pigment, a dioxazine pigment, an isoindolinone pigment, a quinophthalone pigment, an azomethine azo pigment, a dictopyrrolopyrrole pigment, or an isoindoline pigment. The inorganic pigment may be carbon black, titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, chromium oxide, silica, red iron oxide, aluminum, or mica. The colorant may be a glittering pigment (Metashine; Nippon Sheet Glass Co., Ltd.) in which a metal or a metal oxide is coated on a glass flake or agglomerated flake as a base material. Examples of organic solvents include aromatic organic solvents, ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, ester-based solvents such as ethyl acetate, n-propyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate, and alcohol-based solvents such as n-propanol, isopropanol, n-butanol, and propylene glycol monomethyl ether, and in recent years, it is preferable to use ester-based solvents and alcohol-based solvents from an environmental perspective. Examples of aqueous solvents include solvents in which a water-soluble alcohol-based solvent is mixed with water as the main component. Examples of the additives include extender pigments, pigment dispersants, antifoaming agents, waxes, plasticizers, antiblocking agents, adhesion improvers, infrared absorbing agents, ultraviolet absorbing agents, fragrances, and flame retardants.

[0033] <Active energy ray curable inkjet printing ink composition for lamination> Examples of the active energy ray-curable inkjet printing ink composition for lamination include an active energy ray-curable inkjet printing ink composition for lamination containing a colorant, a photopolymerizable compound containing a hydroxyl group, a photopolymerizable compound containing an amine-modified oligomer, and, as necessary, a polymerization initiator, a sensitizer, a pigment dispersant, an additive, and the like. For example, an active energy ray-curable inkjet printing ink composition for lamination such as that described in WO 2023 / 276290 can be used.

[0034] <Active energy ray curable offset printing ink composition for lamination> The active energy ray-curable offset printing ink composition for lamination contains a color pigment, a photopolymerizable compound including a photopolymerizable compound containing a hydroxyl group, an oligomer, and, if necessary, an initiator, a pigment dispersant, and additives. For example, an active energy ray-curable offset printing ink composition for lamination as described in Japanese Patent No. 7110508 can be used.

[0035] [Sealant layer] The surface of the printed layer is laminated by various methods to form a sealant layer, thereby obtaining a laminate for packaging bags, etc. Examples of lamination methods that can be used include an extrusion lamination method in which a molten polymer is laminated on the surface of the laminate, with or without applying an anchor coating agent, and a dry lamination method in which an adhesive is applied to the surface of the laminate, and then a film-like polymer is attached.

[0036] The extrusion lamination method is a method in which, after forming an anchor coat layer by applying an anchor coat agent such as a titanium-based, urethane-based, imine-based, polybutadiene-based agent to the surface of a laminate including a layer of a printing ink composition as necessary, or without applying an anchor coat layer, a molten resin is laminated by a known extrusion laminator, and the molten resin can be laminated as an intermediate layer with other materials in a sandwich shape. In this case, it is not necessary to use a polyethyleneimine-based anchor coat agent. As the molten resin used in the above extrusion lamination method, there can be used conventionally used resins such as polyolefin resins such as low density polyethylene, polyethylene polypropylene, and ethylene-vinyl acetate copolymers.

[0037] The dry lamination method is a method in which an adhesive such as a urethane-based or isocyanate-based adhesive is applied to the surface of the layer made of the laminate printing ink composition, and a resin film is laminated on the obtained adhesive layer by a known dry lamination machine. Examples of the resin film used in this case include non-oriented polyethylene film, non-oriented propylene film, non-oriented propylene film having a metal deposition layer, polyester film, nylon film, etc. Furthermore, it is also possible to use films obtained by processing such as coating or kneading an anti-fogging agent, or surface coating or kneading a matting agent in advance. As the resin film, a film in which a barrier layer formed by depositing metal or coating a barrier resin on various printing plastic films can be used.

[0038] [Anchor coat layer] In the laminate of the present invention, an anchor coat layer can be provided between the resin substrate layer and the removable primer layer in order to improve adhesion. As the anchor coating agent for forming the anchor coating layer, urethane-based, isocyanate-based, polyethyleneimine-based, and other anchor coating agents can be used.

[0039] [Method for producing a laminate having a removable primer layer] A method for producing a laminate having a detachable primer layer includes, for example, applying an anchor coating agent to a resin substrate layer as necessary to form an anchor coating layer, then applying a detachable primer composition to form a detachable primer layer, and then printing or imprinting each of the above-mentioned printing ink compositions to form a printed layer, and 1. applying the detachable primer composition to the printed surface to form a detachable primer layer, applying an adhesive, and further adhering a film with a dry laminator to provide a sealant layer, or 2. applying the detachable primer composition to the printed surface to form a detachable primer layer, applying an anchor coating agent, and further laminating molten resin with an extrusion laminator to provide a sealant layer, thereby obtaining the laminate of the present invention.

[0040] [Method for removing laminate having a removal primer layer] The laminate having the detachable primer layer is separated into the substrate, the printed layer, and the sealant layer, and the printed layer is detached from the laminate having the detachable primer layer. For this purpose, the laminate is cut into small pieces by any means, and the pieces are immersed in an alkaline aqueous solution containing a basic compound such as sodium hydroxide or potassium hydroxide, which is a detachment liquid, and if necessary, agitated. The concentration of sodium hydroxide or potassium hydroxide at this time is preferably 0.5 to 15 mass%, more preferably 1.0 mass% or more, and even more preferably 1.5 mass% or more. In addition, when treating waste liquid after use, it is preferably 5.0 mass% or less, and even more preferably 3.0 mass% or less. The detachment liquid when detaching may be at room temperature of about 25°C, or may be heated to 25 to 90°C. The immersion time is preferably 1 minute to 12 hours, more preferably 1 hour or less, even more preferably 30 minutes or less, and most preferably 10 minutes or less. At the same time, it is preferable to treat the fragmented laminate with a sufficiently large amount of release liquid, that is, 100 to 1,000,000 times the mass of the laminate, in order to achieve smooth release. After the step of immersing in the release liquid, a step of recovering the resin substrate layer, the print layer, and the sealant layer is provided. If the resin substrate layer of the laminate is, for example, polyester, this release method allows the ink layer to be removed in the release liquid, and the separated polyester is washed with water and dried to obtain a recycled polyester substrate. The recycled polyester substrate can also be recycled into pellets using an extruder for reuse. EXAMPLES

[0041] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "%" means "% by mass" and "parts" means "parts by mass." A detachment primer layer made of a detachment primer composition that does not contain an ethylene vinyl alcohol-based resin, rather than a layer formed from the detachment primer composition containing the ethylene vinyl alcohol-based resin of the present invention, has inferior gas barrier properties at high temperatures and high humidity conditions to a detachment primer composition layer containing the ethylene vinyl alcohol-based resin of the present invention, when viewed alone. However, since the present invention is a composition comprising at least one layer formed from a detachment primer composition containing an ethylene vinyl alcohol-based resin, the gas barrier properties of the laminate as a whole at high temperatures and high humidity conditions are not reduced.

[0042] <Resin base layer> OPP: Biaxially oriented polypropylene film P-2161#25 (manufactured by Toyobo Co., Ltd.) PET: Polyethylene terephthalate film E-5102#12 (manufactured by Toyobo Co., Ltd.) NY: Nylon film ONY-15#12 (manufactured by Unitika) PE: 0.25 μm thick corona-treated L-LDPE film (linear low-density polyethylene, manufactured by Mitsui Chemicals Tohcello) <Anchor coating agent> Takelac A-3210 / Takelac A-3072 diluted with ethyl acetate to 7% solids

[0043] [Removal primer composition containing ethylene vinyl alcohol resin] <Removal primer composition 1> Five parts by mass of an ethylene-vinyl alcohol copolymer (product name: Soarnol V2504NB (ethylene content 25 mol%)) was added to 95 parts by mass of a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol, and dissolved by stirring at 80°C to obtain a release primer composition 1 with a solid content of 5% by mass.

[0044] <Removal primer composition 2> 7 parts by mass of an ethylene-vinyl alcohol copolymer (product name: Soarnol V2504NB (ethylene content 25 mol%)) was added to 93 parts by mass of a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol, and dissolved by stirring at 80°C to obtain a release primer composition 2 with a solid content of 7% by mass.

[0045] <Removal primer composition 3> 10 parts by mass of an ethylene-vinyl alcohol copolymer (product name: Exeval HR-3010 (ethylene content 4.5 mol%)) was added to 90 parts by mass of purified water and dissolved by stirring at 95°C, and then diluted with a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol to obtain a release primer composition 3 with a solid content of 5% by mass.

[0046] <Removal primer composition 4> Five parts by mass of an ethylene-vinyl alcohol copolymer (product name: Soarnol DC3212 (ethylene content 32 mol%)) was added to 95 parts by mass of a mixed solvent containing 30% by mass of purified water and 70% by mass of isopropyl alcohol, and dissolved by stirring at 80°C to obtain a release primer composition 4 with a solid content of 5% by mass.

[0047] <Removal primer composition 5> Five parts by mass of montmorillonite (product name: Kunipia F, Kunimine Kogyo Co., Ltd.), an inorganic layered compound, was added to 95 parts by mass of purified water with stirring, and thoroughly dispersed at a pressure of 50 MPa using a high-pressure dispersion device to obtain an inorganic layered compound dispersion liquid with a solid content of 5% by mass. Next, while stirring 85 parts by mass of the primer composition for detachment 1 at high speed, 15 parts by mass of the inorganic layered compound dispersion was added, and then the mixture was subjected to dispersion treatment at a pressure of 50 MPa using a high-pressure dispersion device, filtered through a 255-mesh filter, to obtain a primer composition for detachment 5 with a solid content of 5% by mass (ethylene-vinyl alcohol copolymer resin / inorganic layered compound = 85 / 15 (solid content mass ratio)).

[0048] <Coating conditions for primer compositions for detachment 1 to 5> The primer compositions for detachment 1, 3, and 4 were applied using a bar coater so that the dry coating amount was 1.0 g / m 2 . The primer composition for detachment 5 was applied using a bar coater so that the dry coating amount was 0.5 g / m 2 . The primer composition for detachment 2 was applied using a bar coater so that the dry coating amount was 1.4 g / m 2 .

[0049] [Primer composition for detachment not containing ethylene-vinyl alcohol resin] <A-1. Primer composition for detachment containing polyethyleneimine-based compound> (Primer composition for detachment 1 containing polyethyleneimine-based compound) (a) Polyethyleneimine-based compound Epomin P-1000 (trade name Epomin P-1000 (Nippon Shokubai Co., Ltd., number average molecular weight 70,000, mass average molecular weight 350,000, amine value 18 mmol / g, amine ratio (primary:secondary:tertiary (%)) = 25 / 50 / 25)) was diluted with a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol so that the solid content concentration was 2% by mass to obtain a primer composition for detachment 1 containing a polyethyleneimine-based compound. The above number average molecular weight (Mn) was measured by the viscosity method, and the mass average molecular weight (Mw) was measured by the GPC method. Amine value: Measured by acid titration in a non-aqueous system. Amine ratio: Measured by NMR (13C).

[0050] <A-2. Desorption Primer Composition Containing Polyethyleneimine Compound and Glycidyl Group-containing Silane Coupling Agent> (Desorption Primer Composition 2 Containing Polyethyleneimine-based Compound) A mixture of a polyethyleneimine-based compound (trade name: Epomin P-1000, manufactured by Nippon Shokubai Co., Ltd.) and 3-glycidyloxypropyltrimethoxysilane (product name: Epomin P-1000 (manufactured by Nippon Shokubai Co., Ltd.)) / 3-glycidyloxypropyltrimethoxysilane (mass ratio) = 1 / 2 was diluted with a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol so that the solid content concentration was 2% by mass to obtain Desorption Primer Composition 2 Containing Polyethyleneimine-based Compound.

[0051] <A-3. Desorption Primer Composition Containing Siloxane-modified Polyethyleneimine Compound> (Desorption Primer Composition 3 Containing Polyethyleneimine-based Compound) Trimethoxysilylpropyl-modified polyethyleneimine (trade name: SSP-060, Gelest), molecular weight 1,500 - 1,800, amine value 10 mmol / g, the amine value was measured by acid titration in a non-aqueous system, and the amine ratio was measured by NMR (13C).) was diluted with a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol so that the solid content concentration was 2% by mass to obtain Desorption Primer Composition 3 Containing Polyethyleneimine-based Compound.

[0052] <B. Desorption Primer Composition Containing Polybutadiene-based Compound> A polybutadiene-based compound (trade name: Titabond T-180E, (solid content concentration 10% by mass), manufactured by Nippon Soda Co., Ltd.) was diluted with a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol so that the solid content concentration was 2% by mass to obtain a desorption primer composition containing a polybutadiene-based compound.

[0053] <C. Desorption Primer Composition Containing Polyvinyl Alcohol> Five parts by mass of Kuraray Co., Ltd.'s Poval 5-98 (a polyvinyl alcohol with a degree of saponification of 90% or more) was added to 95 parts by mass of a mixed solvent containing 50% by mass of purified water and 50% by mass of isopropyl alcohol and stirred to obtain a polyvinyl alcohol-containing detachment primer composition with a solids concentration of 5% by mass.

[0054] (Application conditions for the detachment primer composition not containing ethylene vinyl alcohol resin) The above-mentioned A. removal primer composition containing a polyethyleneimine compound and B. removal primer composition containing a polybutadiene compound were applied with a bar coater in a dry coating amount of 0.2 g / m 2 The coating was then dried to form a release primer layer. The above C. polyvinyl alcohol-containing detachment primer composition was applied with a bar coater in a dry coating amount of 1.0 g / m 2 The coating was then dried to form a release primer layer.

[0055] <Printing ink composition> ·Reverse printing ink composition As the printing ink composition for reverse printing, for example, Bellflora R Indigo 800MK (manufactured by Sakata Inx Corporation) can be used, but is not limited to this composition.

[0056] <Printing method using reverse printing ink composition> [If there is a detachment layer] On each of the four resin substrate layers, if necessary, apply an anchor coating agent with a bar coater at a dry coating amount of 0.1 g / m 2It was applied and dried so as to obtain an anchor coat layer. Next, on the coated surface to which the anchor coat agent was applied, each of the above-described primer compositions 1 to 5 for detachment and the primer compositions for detachment of Comparative Examples 1 and 2 (a total of 7 primer compositions for detachment) were applied and dried with a bar coater so as to have a predetermined coating amount, and a total of 28 samples in which each primer composition layer for detachment was formed were obtained. Then, a mixed solvent (ethyl acetate / propyl acetate / IPA (isopropyl alcohol) = 50 / 25 / 25) was added to the printing ink composition for back coating on each of the primer layers for detachment, and the diluted printing ink composition for back coating diluted to 16 seconds with a Rheological Society Zahn cup No. 3 was printed and dried using a bar coater to form a printed layer. [In the case of not having a release layer] To each of the above 4 resin base material layers, a mixed solvent (ethyl acetate / propyl acetate / IPA (isopropyl alcohol) = 50 / 25 / 25) was added to the printing ink composition for back coating, and the diluted printing ink composition for back coating diluted to 16 seconds with a Rheological Society Zahn cup No. 3 was printed and dried using a bar coater to form a printed layer.

[0057] <UV-Curable Inkjet Printing Ink Composition and Printing Method Thereby> As the UV-curable inkjet printing ink composition, for example, BSR06 (Sakata Inx) can be used, but it is not limited to this composition. [In the case of having a release layer] To each of the above 4 resin base material layers, an anchor coat agent was dry-coated with a bar coater so that the dry coating amount was 0.1 g / m 2 and applied and dried to obtain an anchor coat layer. Next, each of the above-described primer compositions 1 to 5 for detachment and the primer compositions for detachment of Comparative Examples 1 and 2 (a total of 7 primer compositions for detachment) were applied and dried with a bar coater so as to have a predetermined coating amount, and a total of 28 samples in which each primer composition layer for detachment was formed were obtained. Then, BSR06 was printed on each of the primer layers for detachment using a bar coater, and with a UV-LED light lamp manufactured by Foseon Technology, at a distance of 2 cm below the lamp and the coated surface of the ink, a UV integrated light amount of 180 mJ / cm 2It was completely cured to form a printed layer. [When there is no release layer] On each of the above four resin substrate layers, BSR06 was printed using a bar coater, and sufficiently irradiated with ultraviolet rays (UV) to be completely cured to form a printed layer.

[0058] <EB Curing Type Offset Printing Ink Composition> As an EB (electron beam) curing type offset printing ink composition, the one prepared from the following EB (electron beam) curing type offset printing ink composition can be used, but it is not limited to this composition. (Preparation of EB Curing Type Offset Printing Ink Composition) 22.7 parts by mass of PB15:3, 40.0 parts by mass of polyester acrylate oligomer: CN704 (manufactured by Sartomer), 36.2 parts by mass of 6EO modified TMPTA (6EO modified trimethylolpropane triacrylate), 0.1 parts by mass of methylhydroquinone, 1.0 parts by mass of dimethyl silicone oil: TSF-451-5M (manufactured by Momentive) were blended and stirred and mixed to obtain an electron beam curing type printing ink composition. (Printing with EB (electron beam) Curing Type Offset Printing Ink Composition) [When there is a release layer] On each of the above four resin substrate layers, an anchor coat agent was dry-coated with a bar coater so that the dry coating amount was 0.1 g / m 2 to obtain an anchor coat layer. Next, each of the above primer compositions 1 to 5 for release and the primer compositions for release of Comparative Examples 1 and 2 (a total of 7 primer compositions for release) were coated and dried with a bar coater so as to have a predetermined coating amount to obtain a total of 28 samples in which each primer composition layer for release was formed. Next, the above EB curing type offset printing ink composition was transferred at 0.1 cc each onto each primer composition layer for release of those samples using a simple color development machine (RI tester, manufactured by Toyoei Seiko Co., Ltd.), and irradiated with an electron beam at a conveyor speed of 10 m / min using an electron beam curing device (EC90, manufactured by Iwasaki Electric Co., Ltd.) (acceleration voltage 90 kV, irradiation dose 30 kGy) to be completely cured to form each printed layer. [When there is no release layer] To each of the above four resin substrate layers, 0.1 cc was transferred using a simple color development machine (RI tester, manufactured by Toyoei Seiko Co., Ltd.), and an electron beam curing device (EC90, manufactured by Iwasaki Electric Co., Ltd.) (acceleration voltage 90 kV, irradiation dose 30 kGy) was used to irradiate the electron beam at a conveyor speed of 10 m / min to completely cure and form each printing layer.

[0059] <UV-curable offset printing ink composition> 50.0 parts by mass of rosin-modified maleic acid resin (Harima M-453, manufactured by Harima Chemicals Inc.), 41.0 parts by mass of trimethylolpropane (6EO) triacrylate, 2.0 parts by mass of dimethyl silicone oil (KF-96H-100,000 cs), 5.0 parts by mass of 2-methyl-1(4-methylthiophenyl)-2-morpholinopropan-1-one, and 4,4-bis(diethylamino)benzophenone were blended and stirred and mixed to obtain a UV-curable printing ink composition. (Printing with the UV-curable offset printing ink composition) [When there is a release layer] To each of the above four resin substrate layers, an anchor coat agent was dry-coated with a bar coater so that the dry coating amount was 0.1 g / m 2 to obtain an anchor coat layer. Next, each of the above release primer compositions 1 to 5 and the release primer compositions 1 and 2 of Comparative Examples 1 and 2 (a total of 7 release primer compositions) were coated and dried with a bar coater so as to have a predetermined coating amount to obtain a total of 28 samples in which each release primer composition layer was formed. Next, the above UV-curable offset printing ink composition was transferred onto each release primer composition layer of those samples, 0.1 cc each, using a simple color development machine (RI tester, manufactured by Toyoei Seiko Co., Ltd.), and with a UV-LED light lamp manufactured by Foseon Technology Co., Ltd., at a distance of 2 cm below the lamp and the coating surface of the ink, the UV integrated light amount was 180 mJ / cm 2 to completely cure and form a printing layer. [When there is no release layer] 0.1 cc of each of the four resin substrate layers was transferred onto each of the four types of resin substrate layers using a simple color development machine (RI Tester, manufactured by Toyoei Seiko Co., Ltd.), and the ink was then applied to a UV-LED lamp manufactured by Phoseon Technology Co., Ltd. at a distance of 2 cm from the lamp to the ink application surface, with a UV cumulative light quantity of 180 mJ / cm. 2 The resulting mixture was completely cured at 40° C. to form a printing layer.

[0060] <Sealant layer> (For dry lamination) Sealant Layer : RXC-22#60: Non-oriented propylene film (Mitsui Chemicals Tocello Co., Ltd.) :TUX TM : Linear low-density polyethylene (Mitsui Chemicals Tocello) glue: When the resin substrate layer was P-2161#25 (biaxially oriented polypropylene film (OPP)), the adhesive was Takelac A-969V / Takelac A-5 (solid content 30% by mass, manufactured by Mitsui Chemicals, Inc.). When the resin substrate layer was PET, NY, or PE, the adhesive was Takelac A-515 / Takelac A-50 (solid content 30% by mass, manufactured by Mitsui Chemicals, Inc.). (In the case of extrusion lamination) Sealant layer: Molten polyethylene Sumikasen L705 resin temperature 355°C (Sumitomo Chemical Co., Ltd.) Anchor coating agent: Takelac A-3210 / Takelac A-3072, solid content 7% by mass

[0061] The structure of the laminate will be explained below by dividing it into laminates (A) to (M). (A) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer / EVOH-containing removable primer layer / printing layer / EVOH-containing removable primer layer / adhesive layer / sealant layer (dry) (B) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer / EVOH-containing removable primer layer / printing layer / adhesive layer / EVOH-containing removable primer layer / sealant layer (dry) (C) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer / EVOH-containing removable primer layer / printing layer / EVOH-containing removable primer layer / anchor coat layer / sealant layer (extrusion) (D) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer / EVOH-containing removable primer layer / printing layer / removable primer layer other than EVOH-containing removable primer layer / adhesive layer / sealant layer (dry) (E) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer / EVOH-containing removable primer layer / printing layer / adhesive layer / removable primer layer other than EVOH-containing removable primer layer / sealant layer (dry) (F) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer / EVOH-containing removable primer layer / printing layer / removable primer layer other than EVOH-containing removable primer layer / anchor coat layer / sealant layer (extrusion) (G) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer as necessary / removable primer layer other than EVOH-containing removable primer layer / printing layer / EVOH-containing removable primer layer / adhesive layer / sealant layer (dry) (H) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer as necessary / removable primer layer other than EVOH-containing removable primer layer / printing layer / adhesive layer / EVOH-containing removable primer layer / sealant layer (dry) (I) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer as necessary / removable primer layer other than EVOH-containing removable primer layer / printing layer / EVOH-containing removable primer layer / anchor coat layer / sealant layer (extrusion) (J) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer as necessary / removable primer layer other than EVOH-containing removable primer layer / printing layer / removable primer layer other than EVOH-containing removable primer layer / adhesive layer / sealant layer (dry) (K) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer as necessary / removable primer layer other than EVOH-containing removable primer layer / printing layer / removable primer layer other than EVOH-containing removable primer layer / anchor coat layer / sealant layer (extrusion) (L) Resin substrate layer (OPP, PET, NY, PE) / printing layer / adhesive layer / sealant layer (dry) (M) Resin substrate layer (OPP, PET, NY, PE) / printing layer / anchor coat layer / sealant layer (extrusion)

[0062] <Formation of sealant layer by dry lamination> In the case of laminates (A), (D), (G) and (J) Each release primer composition was applied to each printed layer with a bar coater to a specified thickness and dried, and then each adhesive was applied with a bar coater. RXC-22#60: Non-oriented propylene film (Mitsui Chemicals Tocello Co., Ltd.), TUX TM Linear low density polyethylene (Mitsui Chemicals Tocello Co., Ltd.) was hand-pasted to obtain each laminate. In the case of laminates (B), (E), and (H) RXC-22#60: Non-oriented propylene film (Mitsui Chemicals Tocello), TUX TM Each release primer composition was applied to a linear low-density polyethylene (Mitsui Chemicals Tocello Co., Ltd.) with a bar coater to a specified thickness and dried to form each release layer. After each adhesive was applied thereon with a bar coater, each of the above printed layers was attached by hand to obtain each laminate. In the case of a laminate of L RXC-22#60: Non-oriented propylene film (Mitsui Chemicals Tocello Co., Ltd.), TUX TM A linear low density polyethylene (Mitsui Chemicals Tocello) and each printed layer were hand-pasted to obtain each laminate.

[0063] <Formation of sealant layer by extrusion lamination> In the case of laminates (C), (F), (I), and (K) Each release primer composition was applied to each printed layer using a bar coater to a specified thickness and dried, after which an anchor coating agent was applied and polyethylene Sumikathene L705 (Sumitomo Chemical Co., Ltd.) was laminated using an extrusion laminator to obtain each laminate. In the case of M laminate An anchor coating agent was applied onto each printed layer, and polyethylene Sumikathene L705 (manufactured by Sumitomo Chemical Co., Ltd.) was further laminated thereon using an extrusion laminator to obtain each laminate.

[0064] <Evaluation of ink release properties> Each of the above laminates was cut into small pieces of about 15 mm MD×25 mm TD to obtain samples for ink release property testing. (Removal liquid consisting of an alkaline aqueous solution) 2.0 parts by mass of sodium hydroxide was added to 98.0 parts by mass of water, and the mixture was stirred and dissolved to obtain a release liquid consisting of an alkaline aqueous solution. (Mixing and separation with the desorption liquid) The release liquid consisting of the above alkaline aqueous solution was heated to 70°C, after which each of the above ink release test samples was placed in each and stirred for 30 minutes using a stainless steel stirring blade with a blade diameter of 25 mm. After stirring, the HDPE (high density polyethylene) container was removed from the hot water bath and allowed to stand at room temperature for 5 minutes. The release liquid and the various film pieces were separated using a stainless steel mesh with a mesh opening of approximately 2 mm. (rinse) After the detachment, each film was transferred to a 200cc HDPE container and 100g of water was added. The mixture was stirred for 5 minutes using a stainless steel stirring blade with a blade diameter of 25mm. After leaving the mixture to stand for 5 minutes, the film pieces were separated from the water using a stainless steel mesh. After drying the film pieces, the ink releasability from each film was visually evaluated. (Evaluation Criteria) ◯: The ink coating was completely peeled off from the film as coating pieces. ×: No peeling occurred.

[0065] <Tape adhesion (printed items immediately after printing and drying)> Adhesion was evaluated according to the following criteria based on the degree to which the printed film peeled off when cellophane tape was applied to the printed surface of each of the obtained prints and then quickly peeled off. (Evaluation Criteria) ◯: The area ratio of the printed coating that peeled off from the film was less than 5%. △: 5% or more and less than 30% of the area of ​​the printed coating peeled off from the film. ×: 30% or more of the area of ​​the printed coating peeled off from the film.

[0066] <Barrier properties> After each laminate was obtained, the oxygen transmission rate (OTR value) was measured using an oxygen transmission rate measuring device (Mocon, product name: OX-TRAN1 / 50) according to JIS K7126 method B. The measurement was performed at 25°C and in an atmosphere of 0% RH. (Evaluation Criteria) 〇: OTR value is 10 or less ×: OTR value is over 10

[0067] <Peel strength> After each laminate was obtained, it was cut to a width of 15 mm, and the T-peel strength was measured using a Yasuda Seiki Seisakusho peel tester. (Evaluation Criteria) When the resin substrate layer is OPP ○: Peel strength is 1.2N / 15mm or more △: Peel strength is 0.7N / 15mm or more and less than 1.2N / 15mm ×: Peel strength is less than 0.7N / 15mm When the resin substrate layer is PET, NY, or PE ○: Peel strength is 5N / 15mm or more △: Peel strength is 3N / 15mm or more and less than 5N / 15mm ×: Peel strength is less than 3N / 15mm

[0068] When a printing layer is formed using various reverse printing ink compositions (A) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer / EVOH-containing removable primer layer / printing layer / EVOH-containing removable primer layer / adhesive layer / sealant layer (dry) Laminates were obtained as shown in the following Table 1. For each of Laminates 1 to 5 in (A), four types of resin substrate layers, four types of printing layers, and two types of sealant layers were used to obtain a total of 32 types of laminates (4 × 4 × 2 = 32). The laminates were evaluated for ink releasability, barrier properties, adhesion and peel strength, and the evaluation results for each evaluation item were ◯ for all laminates.

[0069] [Table 1]

[0070] (B) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer / EVOH-containing removable primer layer / printing layer / adhesive layer / EVOH-containing removable primer layer / sealant layer (dry) Laminates were obtained as shown in the following Table 2. For each of Laminates 1 to 5 in (B), four types of resin substrate layers, four types of printing layers, and two types of sealant layers were used to obtain a total of 32 types of laminates (4 × 4 × 2 = 32). The laminates were evaluated for ink releasability, barrier properties, adhesion and peel strength, and the evaluation results for each evaluation item were ◯ for all laminates.

[0071] [Table 2]

[0072] (C) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer / EVOH-containing removable primer layer / printing layer / EVOH-containing removable primer layer / anchor coat layer / sealant layer (extrusion) Laminates were obtained as shown in the following Table 3. For each of Laminates 1 to 5 in (C), four types of resin substrate layers, four types of printing layers, and one type of sealant layer were used, resulting in a total of 16 types (4×4×1=16) of laminates. The ink releasability, barrier properties, adhesion and peel strength of these laminates were evaluated, and the evaluation results for each evaluation item for all laminates were ◯.

[0073] [Table 3]

[0074] (D) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer / EVOH-containing removable primer layer / printing layer / removable primer layer other than EVOH-containing removable primer layer / adhesive layer / sealant layer (dry) Laminates were obtained as shown in Table 4 below. In Laminates 1 to 5 of (D), the printed layer was a layer made of a printing ink composition for reverse printing, and four types of resin substrate layers and two types of sealant layers were used for each laminate, resulting in eight types of laminates for each of Laminates 1 to 5. In addition, in each of Laminates 1 to 5, only PET was used as the resin substrate layer and two types of sealant layers were used, and a total of three types of ink compositions, an EB-curable inkjet printing ink composition, an EB-curable offset printing ink composition, and a UV-curable offset printing ink composition, were printed on the resin substrate layers to obtain six types of laminates. Similarly, in laminates 6 to 9 of (D), the printed layer was a layer made of a printing ink composition for reverse printing, and four types of resin substrate layers and two types of sealant layers were used in each laminate, resulting in eight types of laminates for each of laminates 6 to 9. Also, in each of laminates 6 to 9, only PET was used as the resin substrate layer and two types of sealant layers were used, and six types of laminates were obtained by printing with three types of ink compositions, namely, an EB-curable inkjet printing ink composition, an EB-curable offset printing ink composition, and a UV-curable offset printing ink composition. The ink releasability, barrier properties, adhesion and peel strength of these laminates were evaluated, and the evaluation results for each evaluation item for all laminates were ◯.

[0075] [Table 4]

[0076] (E) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer / EVOH-containing removable primer layer / printing layer / adhesive layer / removable primer layer other than EVOH-containing removable primer layer / sealant layer (dry) Laminates were obtained as shown in Table 5 below. In each of Laminates 1 to 9 of (E), the printed layer was a layer made of a printing ink composition for reverse printing, and four types of resin substrate layers and two types of sealant layers were used for each laminate, resulting in eight types of laminates for each of Laminates 1 to 9. In addition, in each of Laminates 1 to 9, only PET was used as the resin substrate layer and two types of sealant layers were used, and a total of three types of ink compositions, an EB-curable inkjet printing ink composition, an EB-curable offset printing ink composition, and a UV-curable offset printing ink composition, were printed on the resin substrate layers to obtain six types of laminates. The laminates were evaluated for ink releasability, barrier properties, adhesion and peel strength, and the evaluation results for each evaluation item were ◯ for all laminates.

[0077] [Table 5]

[0078] (F) Resin substrate layer (OPP, PET, NY) / anchor coat layer / EVOH-containing removable primer layer / printing layer / removable primer layer other than EVOH-containing removable primer layer / adhesive layer / sealant layer (extrusion) Laminates were obtained as shown in Table 6 below. In each of Laminates 1 to 9 of (F), the printed layer was a layer made of a printing ink composition for reverse printing, and four types of resin substrate layers were used for each laminate, to obtain four types of laminates with different resin substrate layers in each of Laminates 1 to 9. In addition, in each of Laminates 1 to 9, only PET was used as the resin substrate layer, and a total of three ink compositions, namely, an EB-curable inkjet printing ink composition, an EB-curable offset printing ink composition, and a UV-curable offset printing ink composition, were printed on this to obtain three types of laminates. The ink releasability, barrier properties, adhesion and peel strength of these laminates were evaluated, and the evaluation results for each evaluation item for all laminates were ◯.

[0079] [Table 6]

[0080] (G) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer as necessary / removable primer layer other than EVOH-containing removable primer layer / printing layer / EVOH-containing removable primer layer / adhesive layer / sealant layer (dry) Laminates were obtained as shown in Table 7 below. In each of Laminates 1 to 9 of (F), the printed layer was a layer made of a printing ink composition for reverse printing, and four types of resin substrate layers and two types of sealant layers were used for each laminate, resulting in eight types of laminates for each of Laminates 1 to 9. In each of Laminates 1 to 9, only PET was used as the resin substrate layer and two types of sealant layers were used, and a total of three types of ink compositions, an EB-curable inkjet printing ink composition, an EB-curable offset printing ink composition, and a UV-curable offset printing ink composition, were printed on the resin substrate layers to obtain six types of laminates. The ink releasability, barrier properties, adhesion and peel strength of these laminates were evaluated, and the evaluation results for each evaluation item for all laminates were ◯.

[0081] [Table 7]

[0082] (H) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer as necessary / removable primer layer other than EVOH-containing removable primer layer / printing layer / adhesive layer / EVOH-containing removable primer layer / sealant layer (dry) Laminates were obtained as shown in Table 8 below. In each of Laminates 1 to 9 of (H), the printed layer was a layer made of a printing ink composition for reverse printing, and four types of resin substrate layers and four types of sealant layers were used for each laminate, resulting in eight types of laminates for each of Laminates 1 to 9. In each of Laminates 1 to 9, only PET was used as the resin substrate layer and two types of sealant layers were used, and a total of three types of ink compositions, an EB-curable inkjet printing ink composition, an EB-curable offset printing ink composition, and a UV-curable offset printing ink composition, were printed on the resin substrate layers to obtain six types of laminates. The laminates were evaluated for ink releasability, barrier properties, printed layer adhesion and peel strength, and the evaluation results for each evaluation item for all laminates were ◯.

[0083] [Table 8]

[0084] (I) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer as necessary / removable primer layer other than EVOH-containing removable primer layer / printing layer / anchor coat layer / EVOH-containing removable primer layer / anchor coat layer / sealant layer (extrusion) Laminates were obtained as shown in Table 9 below. In each of laminates 1 to 9 in (I), the printed layer was a layer made of a printing ink composition for reverse printing, and four types of resin substrate layers were used for each laminate, to obtain four types of laminates with different resin substrate layers in each of laminates 1 to 9. In each of laminates 1 to 9, only PET was used as the resin substrate layer, and a total of three ink compositions, namely, an EB-curable inkjet printing ink composition, an EB-curable offset printing ink composition, and a UV-curable offset printing ink composition, were printed on this to obtain three types of laminates. The laminates were evaluated for ink releasability, barrier properties, printed layer adhesion and peel strength, and the evaluation results for each evaluation item for all laminates were ◯.

[0085] [Table 9]

[0086] (J) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer as necessary / removable primer layer other than EVOH-containing removable primer layer / printing layer / removable primer layer other than EVOH-containing removable primer layer / adhesive layer / sealant layer (dry) Laminates were obtained as shown in Table 10 below. In each of Laminates 1 to 5 of (J), the printed layer was a layer made of a printing ink composition for reverse printing, and four types of resin substrate layers and two types of sealant layers were used for each laminate, thereby obtaining eight types of laminates with different resin substrate layers for each of Laminates 1 to 5. In each of Laminates 1 to 5, only PET was used as the resin substrate layer and two types of sealant layers were used, and a total of three types of ink compositions, namely an EB-curable inkjet printing ink composition, an EB-curable offset printing ink composition, and a UV-curable offset printing ink composition, were printed on the resin substrate layers to obtain six types of laminates. The evaluation results for the ink releasability, adhesion, and peel strength of these laminates were ◯, but the barrier properties of Laminates 1 to 5 in (J) were ×.

[0087] [Table 10]

[0088] (K) Resin substrate layer (OPP, PET, NY, PE) / anchor coat layer as necessary / removable primer layer other than EVOH-containing removable primer layer / printing layer / removable primer layer other than EVOH-containing removable primer layer / anchor coat layer / sealant layer (extrusion) Laminates were obtained as shown in Table 11 below. In each of Laminates 1 to 5 of (K), the printed layer was a layer made of a printing ink composition for reverse printing, and four types of resin substrate layers were used for each laminate, to obtain four types of laminates with different resin substrate layers in each of Laminates 1 to 5. In each of Laminates 1 to 5, only PET was used as the resin substrate layer, and a total of three ink compositions, namely, an EB-curable inkjet printing ink composition, an EB-curable offset printing ink composition, and a UV-curable offset printing ink composition, were printed on this to obtain three types of laminates. The evaluation results for the ink releasability, adhesion, and peel strength of these laminates were ◯, but the barrier properties of Laminates 1 to 5 of (K) were ×.

[0089] [Table 11]

[0090] (L) Resin substrate layer (OPP, PET, NY, PE) / printing layer / adhesive layer / sealant layer (dry) Laminates were obtained as shown in Table 12 below. In Laminate 1 (L), the printed layer was a layer made of a printing ink composition for reverse printing, and four types of resin substrate layers were used for each laminate, to obtain four types of laminates with different resin substrate layers. In Laminate 1, only PET was used as the resin substrate layer, and three types of ink compositions, an EB-curable inkjet printing ink composition, an EB-curable offset printing ink composition, and a UV-curable offset printing ink composition, were printed on this to obtain three types of laminates. The laminates were evaluated as having excellent adhesiveness and peel strength, but were evaluated as poor in terms of releasability due to a release liquid and barrier properties.

[0091] [Table 12]

[0092] (M) Resin substrate layer (OPP, PET, NY, PE) / printing layer / anchor coat layer / sealant layer (extrusion) Laminates were obtained as shown in Table 13 below. In Laminate 1 (M), the printed layer was a layer made of a printing ink composition for reverse printing, and four types of resin substrate layers and two types of sealant layers were used for each laminate, to obtain eight types of laminates with different resin substrate layers. In addition, in Laminate 1, only PET was used as the resin substrate layer and two types of sealant layers were used, and a total of three ink compositions, an EB-curable inkjet printing ink composition, an EB-curable offset printing ink composition, and a UV-curable offset printing ink composition, were printed on the resin substrate layers to obtain six types of laminates. The laminates were evaluated as having excellent adhesiveness and peel strength, but were evaluated as poor in terms of releasability due to a release liquid and barrier properties.

[0093] [Table 13]

Claims

1. A laminate comprising a resin substrate layer, a detachable primer layer, a printed layer, a detachable primer layer, and a sealant layer, at least one of the two detachable primer layers being a layer formed from a detachable primer composition containing an ethylene-vinyl alcohol-based resin.

2. The laminate according to claim 1, wherein one of the two detachable primer layers is a layer made of a detachable primer composition that does not contain an ethylene vinyl alcohol-based resin, and the detachable primer composition that does not contain an ethylene vinyl alcohol-based resin is any one of the following A to B: A. Desorption primer composition containing a polyethyleneimine compound B. Detachment primer composition containing a polybutadiene compound C. Polyvinyl alcohol-containing release primer composition

3. 3. The laminate according to claim 1, wherein the content of ethylene units in all monomers constituting the ethylene-vinyl alcohol-based resin is 1 to 35 mol %.

4. 3. The laminate according to claim 1, wherein the ethylene-vinyl alcohol resin has a degree of saponification of 90% or more.

5. The solid content coating amount of the detachment primer layer formed from the detachment primer composition containing the ethylene vinyl alcohol resin is 0.1 to 2.0 g / m 2 3. The laminate according to claim 1 or 2,

6. A method for removing a resin substrate layer, comprising: a step of immersing the laminate according to claim 1 or 2 in a removing liquid; and a step of recovering the resin substrate layer and the printed layer.

Citation Information

Patent Citations

  • Label

    JP1999085034A

  • Double structured container

    JP2021151893A

  • Migration-preventing coating agent

    JP2023007353A

  • Primer composition for detachment and printed matter

    JP2023050125A

  • Composite film and method for producing the same

    JP2024121064A