Low-carbon emission molded product, mold thereof, and equipment containing low-carbon emission molded product
The low carbon emission molding process forms products at room temperature using a specialized ore material, addressing high carbon emissions in traditional casting by eliminating heating and enhancing efficiency and durability.
Patent Information
- Application Number
- JP2023140250
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2023-08-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional metal casting methods emit high levels of carbon dioxide due to the energy-intensive process of heating metals to a molten state, which is inconsistent with environmental protection trends.
A low carbon emission molding process that forms molded products at room temperature without heating, using a low carbon emission ore molding material composed of binders, aggregates, and additives, with embedded members and connections pre-placed in the mold before casting.
Reduces carbon dioxide emissions by eliminating the need for high-temperature melting, saves energy, and enhances production efficiency by allowing for pre-embedded components, resulting in stronger and more durable products with reduced processing steps.
Smart Images

Figure 2024159404000001_ABST
Abstract
Description
[Technical field]
[0001] The present application relates to a low carbon emission molded product and a mold therefor, and an apparatus including the low carbon emission molded product. [Background technology]
[0002] Generally, casting techniques used for industrial parts involve a lot of heating of metal, but in the current climate of environmental protection, such manufacturing methods emit large amounts of carbon dioxide, making them a product with a large carbon footprint.
[0003] Additionally, traditional metal casting often involves pouring molten metals into a mold, which can then be formed into a casting after they cool and solidify. However, those skilled in the art know that heating metals to a molten state requires the consumption of large amounts of energy, which increases carbon emissions.
[0004] To further explain, the production of metal materials, such as smelting, produces a large amount of carbon emissions, so that each stage in the production process of casting products generates a large amount of carbon emissions, which is largely inconsistent with the current trend of environmental protection. Summary of the Invention [Problem to be solved by the invention]
[0005] Therefore, there is a need for a low carbon emission molded product and its mold, as well as an equipment including the low carbon emission molded product, that solves the above-mentioned conventional problems. [Means for solving the problem]
[0006] In accordance with the above objectives, the present invention provides a low carbon emission molded article, comprising a molded article body, a plurality of embedded members, and a connecting portion. The molded article body is formed by casting and solidifying at room temperature. The embedded members are embedded in the molded article body. The connecting portion is provided on at least one surface of the molded article body.
[0007] Preferably, at least one groove is defined in at least one surface of the molding body.
[0008] Preferably, the plurality of embedded members include a plurality of fixing members provided on a bottom surface of the molding body, each of the plurality of fixing members having at least one first locking hole defined therein, and the at least one first fastening component fastens the fixing member to the ground through the first locking hole.
[0009] Preferably, the connection portion is made of metal and includes a first connection member, a second connection member, and a third connection member, the first connection member being provided at the center of the upper surface of the molded body, the second connection member being provided adjacent to the first connection member, and the third connection member being provided on a side surface of the molded body.
[0010] Preferably, the plurality of embedded members include at least one conduit having both openings located on at least one surface of the molding body.
[0011] Preferably, the plurality of embedded members include a plurality of second fastening components, each of which includes a fastening unit, a connecting unit and an embedding unit. The fastening unit is located on one side of the molding body and has a screw hole defined therein. The connecting unit is connected to the fastening unit, and the embedding unit is connected to the connecting unit, and the effective diameter of the connecting unit is smaller than the effective diameters of the fastening unit and the embedding unit.
[0012] Preferably the low carbon emission mouldings have a wall thickness of greater than 50mm.
[0013] Based on the above object, the present invention further provides a mold for manufacturing the above-mentioned low carbon emission molding, comprising a mold bottom, a plurality of mold sides and at least one support member, the plurality of mold sides being provided on the mold bottom, and upper edges of the at least two sides being supported by both ends of the at least one support member.
[0014] Preferably, the low carbon emission molded article mold of the present invention further includes at least one channel forming member connected to the at least one support member and suspended from the mold bottom.
[0015] Based on the above objective, the present invention further provides an equipment including a low-carbon emission molded product, the equipment including the low-carbon emission molded product and a processing device connected to the low-carbon emission molded product. Effect of the Invention
[0016] The present application provides a low-carbon emission molding, a mold thereof, and an equipment including the low-carbon emission molding. Since the manufacturing of the molding body does not require a high-temperature molten state, it has the effect of saving energy and reducing carbon dioxide emissions. In addition, since the manufacturing of the molding body does not require a high-temperature molten state, the embedding member can be placed in the mold first, which reduces the number of subsequent processing steps and improves manufacturing efficiency. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a first schematic diagram of a low carbon emission molded article according to an embodiment of the present application. [Diagram 2] FIG. 2 is a second schematic diagram of a low carbon emission molded article according to an embodiment of the present application. [Figure 3A] FIG. 2 is a first schematic diagram of a second conduit according to an embodiment of the present application. [Figure 3B] FIG. 2 is a second schematic diagram of a second conduit according to an embodiment of the present application. [Figure 4] FIG. 2 is a schematic diagram of a second fastening component according to an embodiment of the present application. [Diagram 5] FIG. 2 is a schematic diagram of a low carbon emission ore molding material according to an embodiment of the present application. [Figure 6] FIG. 2 is a first schematic diagram of a mold for a low carbon emission molded product according to an embodiment of the present application. [Figure 7A] FIG. 2 is a second schematic diagram of a mold for a low carbon emission molded product according to an embodiment of the present application. [Figure 7B] FIG. 4 is a third schematic diagram of a mold for a low carbon emission molded product according to an embodiment of the present application. [Figure 7C] FIG. 4 is a fourth schematic diagram of a mold for a low carbon emission molding according to an embodiment of the present application. [Figure 8A]FIG. 3 is a third schematic diagram of a low carbon emission molded article according to an embodiment of the present application. [Figure 8B] FIG. 4 is a fourth schematic diagram of a low carbon emission molded article according to an embodiment of the present application. [Figure 9] FIG. 1 is a schematic diagram of a system including low carbon emission molded articles according to an embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] In order to allow the examiner to understand the technical features, contents, advantages and effects that can be achieved by the present application, the embodiments are described in detail with accompanying drawings. In addition, the drawings used in the present application are for illustrating and assisting the description, and do not necessarily represent the actual proportions and precise configurations after the implementation of the present application, so the proportions and configuration relationships of the accompanying drawings should not be interpreted as limiting the scope of rights in the actual implementation of the present application.
[0019] Hereinafter, embodiments of the present application will be described with reference to the related drawings. For ease of understanding, the same elements in the following embodiments will be denoted by the same reference numerals.
[0020] 1 to 4, the low carbon emission molded product 10 of the present application includes a molded product body 101, a plurality of embedded members, and a connection part. The molded product body 101 of the present application is formed by casting and solidifying at room temperature. That is, the molding material of the molded product body 101 is poured into a mold at room temperature and solidified at room temperature, without undergoing any heating or temperature increase process. Therefore, the plurality of embedded members are not affected by high temperatures as in conventional castings such as cast iron. The room temperature may be 25°C or other temperatures such as -5°C to 50°C, preferably 15°C to 40°C, more preferably 20°C to 35°C. It should be noted that the molded product material of the present application can be cast at extremely low room temperatures such as below 0°C.
[0021] The molding body 101 of the present application is made of a low-carbon emission ore molding material, which can be solidified to form a molding without the high temperature of metal melting, and can be used for the base, lathe body, beam, machine column, shaft head, machine body, worktable, etc. of a machine tool or other equipment. That is, in one embodiment, the low-carbon emission ore molding material does not include a metal material.
[0022] 5, the molded body 101 can include a binder 51, an ore material, and an additive 54. Specifically, the ore material can include a first aggregate 52 and a second aggregate 53. In other words, the molded body 101 can be formed of a low carbon emission ore molded material including the binder 51, the first aggregate 52, and the second aggregate 53.
[0023] In other embodiments, the production of the low carbon emission ore molded material of the present application may not use the second aggregate 53, and may use only the ore-based first aggregate 52 as the main aggregate of the molded product.
[0024] In one embodiment, the binder 51 may include a silicate, an aluminate, or a ferroaluminate, where the silicate may be tricalcium silicate and dicalcium silicate, the aluminate may be tricalcium aluminate, and the ferroaluminate may be tetracalcium aluminate, but is not limited thereto.
[0025] In one embodiment, the binder 51 can include tricalcium silicate, dicalcium silicate, tricalcium aluminate, tetracalcium aluminoferrite, microsilica powder (quartz powder), and other materials that can enhance strength and durability. In a preferred embodiment, the tricalcium silicate, dicalcium silicate, tricalcium aluminate, and tetracalcium aluminoferrite can comprise about 50% by weight of the binder.
[0026] Furthermore, in a preferred embodiment, tricalcium silicate, dicalcium silicate, tricalcium aluminate, tetracalcium ferroaluminate, and microsilica powder (quartz powder) are all nanoscale powders, so they can form a dense structure. In a preferred embodiment, the microsilica powder is silicon dioxide powder, and in order to form a dense structure, its particle size is between 7 nm and 40 nm, for example, 10 nm to 20 nm. In other embodiments, the silicon dioxide powder may have other particle sizes, such as less than 300 nm.
[0027] In one embodiment, the components of the binder 51 further include calcium oxide. The particle size of the fine calcium oxide in the calcium oxide may be between 0.7 and 100 μm, preferably between 20 and 80 μm. The weight percentage of the fine calcium oxide accounts for 90% to 99% of the calcium oxide.
[0028] In one embodiment, the binder 51 includes cement, silicon dioxide, and calcium oxide. The cement includes normal cement and very fine cement. The particle size of the very fine cement is 2 to 20 μm, and the weight ratio of the normal cement to the very fine cement is 3:1 to 5:1.
[0029] In one embodiment, the silicon dioxide can have two forms, namely, gas phase silicon dioxide and precipitated silicon dioxide, and the weight percentage of both can be 1:1 to 1:50.
[0030] In one embodiment, the cement may include one or more of blast furnace slag, fly ash, silica powder, pozzolan, calcium carbonate, silicon dioxide, aluminum oxides (such as aluminum trioxide), iron oxides (such as ferric oxide), and gypsum.
[0031] To further explain, the low carbon emission ore molding material of the present application has good penetration resistance and water absorption performance, and its water absorption performance depends on factors such as aggregate mixing ratio, water to binder ratio, material components, etc. In the case of the low carbon emission ore molding material of the present application, the water absorption rate is very low, less than about 0.1%. This is because the fine aggregate and powder make the microstructure of the molding more dense. In addition, the low carbon emission ore molding material of the present application usually contains a high-efficiency water reducer and other additives to improve fluidity and workability, which helps to reduce the water absorption of the final molding. The molding formed by the low carbon emission ore molding material of the present application also has excellent penetration resistance and can maintain high penetration resistance under water pressure.
[0032] In one embodiment, as shown in FIG. 5, other materials that can increase strength and durability can be reinforcing fibers 55, steel fibers, plastic steel fibers, plastic fibers (polyethylene, polypropylene), etc. Its length can be between 3mm and 10mm, preferably 4-6mm. Also, in one embodiment, the weight percent of reinforcing fibers 55 in the binder is less than 1%. Note that since the low carbon emission ore molding material of the present application has a low thermal conductivity coefficient, even if plastic fibers or other reinforcing fibers 55 that are weak at high temperatures are added, the properties of the reinforcing fibers 55 are unlikely to be affected by high temperatures. Note that in other embodiments, other materials that can increase strength and durability, such as reinforcing fibers 55, can be omitted, such as using a binder 51 containing only mineral components.
[0033] Furthermore, in a preferred embodiment, tricalcium silicate, dicalcium silicate, tricalcium aluminate, tetracalcium ferroaluminate, and microsilica powder (quartz powder) are all nanoscale powders, i.e., the particle size of these powders is about 100 to 300 nm, so that a dense structure can be formed.
[0034] To explain further, in the formation of microsilica powder, due to the action of surface tension during the formation of phase transition, the microsilica powder is in the amorphous phase under the action of surface tension, and the surface is smooth. Part of the microsilica powder is an aggregate of many spherical particles attached. Microsilica powder has a very large surface area and is a highly active material. The fineness of the microsilica powder is less than 1000 nm, the average particle size is 100-300 nm, and the specific surface area is 20-28 m 2 / g. Its fineness and specific surface area are approximately 80 to 100 times that of cement and 50 to 70 times that of fly ash. Therefore, it is very suitable for bonding to other substrates.
[0035] In a preferred embodiment, most of the microsilica powder is silicon dioxide powder, and its particle size is between 7 nm and 40 nm, for example, 10 nm to 20 nm, to form a dense structure. In other embodiments, the silicon dioxide powder may have other particle sizes, such as less than 300 nm.
[0036] Furthermore, in a preferred embodiment, the microsilica powder may be composed of one or more of the following by weight: 75% to 98% silicon dioxide, 1.0±0.2% aluminum oxide, 0.9±0.3% iron trioxide, 0.7±0.1% magnesium oxide, 0.3±0.1% calcium oxide, and 1.3±0.2% Na2O. Also, its bulk density is about 320 to 700 kg / m 3 It is.
[0037] In one embodiment, when microsilica powder reacts with silicate, a hydration reaction occurs to produce hydrated calcium silicate and calcium hydroxide. The hydrated calcium silicate has the effect of adhering other materials. When microsilica powder, calcium hydroxide and water react, more calcium silicate gel polymer is produced, but the content of calcium hydroxide decreases, which can be shown by the following chemical reaction:
[0038] Calcium hydroxide + microsilica powder + water → calcium silicate hydrate Ca(OH)2 + SiO2 + H2O → CSH
[0039] The calcium silicate gel polymer strengthens the bonds between the various matrices within the molding, helping to reduce permeability, and since calcium hydroxide is reduced during the reaction, it can improve the durability of the entire structure.
[0040] As mentioned above, the microsilica powder has very small particles, so it can be used as a filler or gelling agent. The microsilica powder can be filled between the particles of each base material, especially between the aggregates, and the microsilica powder can be combined with calcium hydroxide, so that the structure of the molded product is denser, stronger, and less permeable.
[0041] To further explain, the low carbon discharge ore material of the present application has good penetration resistance and water absorption performance, and its water absorption performance depends on factors such as aggregate mixing ratio, water to binder ratio, material components, etc. The low carbon discharge ore material of the present application has a very low water absorption rate, which is less than about 0.1%. This is because the fine aggregate and powder make the microstructure of the moldings more dense. In addition, the low carbon discharge ore material of the present application usually contains a high-efficiency water reducer and other additives to improve fluidity and workability, which helps to reduce the water absorption of the final moldings. The moldings formed by the low carbon discharge ore material of the present application also have excellent penetration resistance and can maintain high penetration resistance under water pressure.
[0042] In one embodiment, the particle size of the first aggregate 52 is 15 mm or less, and the second particle size of the second aggregate is smaller than the first particle size of the first aggregate. Preferably, in one embodiment, the particle size of the first aggregate is between 5 mm and 12 mm, such as, but not limited to, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, or 12 mm, or any particle size within these ranges. In one embodiment, preferably, the particle size of the first aggregate 52 is between 5 mm and 10 mm.
[0043] To further explain, in one embodiment, the first aggregate may be an air-dried hard stone material, and the first aggregate may be one or more of gabbro, granite, basalt, andesite, conglomerate, sandstone, shale, diabase, pyroxene, and quartz, i.e., the first aggregate may be selected to be one or more hard stone materials.
[0044] In one embodiment, the first aggregate 52 can be naturally dried or formed into an air-dried state by other methods. In another embodiment, the first aggregate 52 is a dust-free, angular, hard stone material. That is, in the present application, the ore raw material can obtain the first aggregate 52 only by going through processes such as drying, crushing, dust removal, washing, and particle size sorting (the order can be adjusted according to actual needs and is not particularly limited). The shape of the first aggregate 52 is not particularly limited, so the process of processing the aggregate shape can be omitted.
[0045] In one embodiment, the second particle size of the second aggregate 53 may be less than 3 mm, such as 1 mm, 2 mm, 3 mm, or any particle size between 0 mm and 3 mm. Preferably, the second aggregate may be an air-dried, dust-free, angular sandy material. To further explain, in one embodiment, the second aggregate may be natural sand or artificial sand, and its main material may be silicon dioxide.
[0046] In other embodiments, the second aggregate may include other materials, for example, the second aggregate may include one or more of slag, sea sand, and coral sand, which may partially or completely replace the silicon dioxide based sandy material.
[0047] In one embodiment, the weight percentage of the first aggregate 52 and the second aggregate 53 in the low carbon emission ore molded material may be between 0-80%. Preferably, the low carbon emission ore molded material of the present application may have, in weight percentage, 35%-45% binder, 35%-45% first aggregate 52 and the second aggregate 53, 5%-12% water, and 2%-8% additive. To further explain, in a preferred embodiment, the weight percentage of the first aggregate 52 and the second aggregate 53 may be about 50%.
[0048] In one embodiment, the additive may include one or more of a cement modifier and a concrete shrinkage modifier, for example, the cement modifier may be a superplasticizer, and the concrete shrinkage modifier may be a magnesium oxide expanding agent, a superplasticizer, and the like.
[0049] A plurality of embedding members may be embedded in the molding body 101. In one embodiment, the plurality of embedding members may include a plurality of fixing members 102. Furthermore, in one embodiment, the melting temperature or temperature resistance of the embedding members is lower than the melting temperature of the metal, for example, less than 800°C, and in another embodiment, the melting temperature or temperature resistance of the embedding members is less than 250°C.
[0050] A plurality of fixing members 102 are provided on the bottom surface of the molded body 101, and at least one first locking hole 1021 is defined in each of the plurality of fixing members 102. At least one first fastening part 1022 can fasten the fixing members 102 to the ground through the first locking hole 1021, so that the molded body 101 can be firmly fixed to the ground.
[0051] In other embodiments, the fixing member 102 may be provided with a locking hole, a fixing hole, a fixing unit, etc., in order to firmly connect the fixing member 102 to the molded body 101. In addition, since the fixing member 102 is embedded in the molded body 101 before the molded body 101 solidifies, the subsequent processing steps can be reduced.
[0052] In addition, the plurality of embedded members may also include at least one conduit, and both openings of each of the at least one conduit may be located on at least one surface of the molding body 101, that is, the inlet and outlet of the conduit may be located on the same surface or different surfaces of the molding body 101. Furthermore, in one embodiment, the melting temperature of the conduit is lower than the melting temperature of the metal, for example, less than 800°C, and in another embodiment, the melting temperature of the conduit is less than 250°C.
[0053] In one embodiment, as shown in Fig. 2, the pipeline may include a first pipeline 106 and a second pipeline 107. The first pipeline 106 may be a plastic pipeline, a metal pipeline, or the like, and may be used to pass wiring such as electric wires and control lines. In the present invention, the pipeline may be embedded before the molding body 101 solidifies, so that a pipeline having a complex shape such as a spiral pipeline may be provided. In contrast, conventional casting requires a process of melting metal or casting material, so that it is difficult to embed the pipeline beforehand, and subsequent processing cannot be performed until the casting is cooled.
[0054] The second conduit 107 may be a metal pipe or other conduit made of a material that is thermally conductive and durable. The second conduit 107 may pass various fluids such as water, oil, coolant, etc., and may be used as a cooling conduit or other supply conduit.
[0055] Preferably, in one embodiment, when the second conduit 107 is used as a cooling conduit, it can also be arranged in a spiral shape within the molding body 101 in the manner shown in Figures 3A and 3B to achieve a better temperature reduction effect.
[0056] In one embodiment, the plurality of embedded members may include a plurality of second fastening parts 108. As shown in FIG. 4, each second fastening part 108 may include a fastening unit 1081, a connecting unit 1082 and an embedding unit 1083. The fastening unit 1081 may be located on one side of the molding body 101, and a screw hole may be defined in the fastening unit 1081 for fastening other parts. The connecting unit 1082 may be coupled to the fastening unit 1081, and the embedding unit 1083 may be coupled to the connecting unit 1082. In this embodiment, the effective diameter of the connecting unit 1082 may be smaller than the effective diameters of the fastening unit 1081 and the embedding unit 1083, so that the second fastening part 108 may be firmly positioned in the molding body 101 after the molding body 101 is solidified.
[0057] In one embodiment, the plurality of embedded members may further include at least one sensor 110, such as a temperature sensor, a pressure sensor, a vibration sensor, a speed sensor, etc. The molding material of the present application can be cast without adding additional energy (at least without adding thermal or mechanical stress), so that the sensor 110 can be placed in the mold first and then the molding material can be added. Therefore, the subsequent processing steps can be reduced, and the sensor 110 will not be damaged by heat.
[0058] To explain further, the connection part may be provided on at least one surface of the molded body 101. In one embodiment, the connection part may be made of metal in order to improve processing accuracy, and may be processed by, for example, numerical control (computer numerical control, CNC), but is not limited thereto, and a metal connection part has the advantage that it has high processing accuracy and is easy to arrange structural features such as screw holes, tenons, and grooves.
[0059] In one embodiment, the connection portion includes at least one connection member, and may include, for example, a first connection member 103, a second connection member 104, and a third connection member 105. The first connection member 103 may be provided at the center of the upper surface of the molded body 101, the second connection member 104 may be provided adjacent to the first connection member 103, and the third connection member 105 may be provided on a side surface of the molded body 101.
[0060] In one embodiment, the first connecting member 103 can be connected to a slide rail, the second connecting member 104 can be connected to a processing device, such as a cutter, a three-axis processing platform, a multi-axis processing platform, etc., and the third connecting member 105 can fasten a sheet metal part, and the sheet metal part can be used as an outer shell.
[0061] In one embodiment, in order to reduce the weight of the low carbon emission molded product 10 of the present application, at least one groove 1011 may be defined on at least one surface of the molded product body 101 through the design of the mold. Therefore, the overall structure can be further reduced in weight while ensuring the mechanical strength of the entire low carbon emission molded product 10.
[0062] Accordingly, in one embodiment, the present application further provides a mold for producing the above-mentioned low carbon emission molded product 10. The mold for the low carbon emission molded product 10 includes a mold bottom 21, a plurality of mold sides 22, and at least one support member 23. The plurality of mold sides 22 are provided on the mold bottom 21, and both ends of the at least one support member 23 support upper edges of the at least two mold sides 22.
[0063] In one embodiment, components such as embedded members and connectors are embedded in advance in the molded body 101, and spaces such as lock holes and grooves are further defined in the molded body 101, so that the wall thickness (wall thickness) of the molded body 101 is different, for example, between parts and parts, between parts and spaces filled by the molded body 101, between spaces and spaces filled by the molded body 101, between spaces or between parts and edges of the molded body 101, etc. In order to maintain the strength of the entire molded body 101, the minimum wall thickness (wall thickness) is 50 mm.
[0064] The low carbon emission molded product 10 of the present application does not need to be heated, so there is no need to limit the choice of materials as in the case of conventional molds. For example, conventional iron castings usually require sand molds to manufacture iron castings, and for example, large castings usually only produce one casting in a sand mold, which is not efficient. In addition, in general sand molds, although the sand can be recycled, a considerable amount of electricity is required to recycle the sand, and the chemicals mixed with the sand cannot be reused. The mold of the low carbon emission molded product 10 of the present application is made of materials such as wood, plastic steel, and metal, which are easy to modularize the mold bottom 21 and multiple mold side parts 22, so it can be reused, and the combination of the low carbon emission molded product 10 of the present application and its materials is excellent in energy saving and low carbon emission effects.
[0065] In one embodiment, as shown in Figures 6 and 7A, both ends of the support member 23 support the upper edges of at least two mold side portions 22, so that the support force for the mold can be further increased. Note that in the present application, the arrangement method and the number of the support members 23 are not limited. For example, the support member 23 can be provided between two adjacent mold side portions 22, or only one support member 23 can provide support for the mold.
[0066] In one embodiment, the mold for the low carbon emission molding 10 may further include at least one groove forming member 24 for forming the groove 1011, and the groove forming member 24 may be connected to at least one support member 23 and suspended from the mold bottom 21.
[0067] In one embodiment, the groove forming member 24 may be made of a soft material such as, but not limited to, a rubber material. In another embodiment, at least one protruding member 25 may be provided on the upper edge of the plurality of mold side portions 22, which provides a space for the first fastening component 1022 to fasten and also reduces the weight of the entire structure to some extent. In addition, the groove forming member 24, the protruding member 25 and the filling member may all be made of a material that does not require high temperature resistance.
[0068] Please note that the mold bottom 21 in this application corresponds to the top surface of the molding body 101 in this application. That is, during production, the embedding members and the connecting parts can be placed in the mold first, and then the low carbon emission ore molding material can be added from above the mold. In another embodiment, a mold top can be added as needed, and the mold top can be placed over the bottom surface of the molding body 101.
[0069] In one embodiment, as shown in FIG. 7B and FIG. 7C, the edge of the mold may be chamfered 26 or rounded 27, for example, the joint between the mold side 22 and the mold bottom 21 may be chamfered 26 or rounded 27, for example, demolding. In this case, the molding body 101 may also be chamfered 26 or rounded 27 at the corresponding position to avoid stress concentration. In one embodiment, a structural reinforcement 109 may be further provided to further strengthen the structural strength or seismic performance of the entire low carbon emission molding 10. As shown in FIG. 8A, the structural reinforcement 109 may be a steel pipe or other strong rod and column, and the structural reinforcement 109 may be pre-placed in the mold 20 of the low carbon emission molding, and then the low carbon emission ore molding material may be added to strengthen the structure of the molding body 101.
[0070] In addition, the structural reinforcement 109 is not limited. For example, when the structural reinforcement 109 is a square steel pipe, at least one steel pipe may be provided crossing the molded body 101. In addition, when structural reinforcement in each direction is required, the steel pipes may be arranged crosswise first and connected by welding or the like. Therefore, after the molded body 101 is solidified and molded, the resistance in each direction can be increased by these crossed steel pipes. The method of crossing the structural reinforcement 109 is not particularly limited, but generally, there are at least several types, such as a form in which the structural reinforcement 109 is arranged parallel to each other along the same direction on a plane, a form in which the structural reinforcement 109 is arranged crosswise along two directions perpendicular to each other on a plane, and a form in which the structural reinforcement 109 is arranged crosswise along three directions perpendicular to each other in the molded body 101.
[0071] In another embodiment, as shown in Fig. 8B, the structural reinforcement 109 may be a reinforcing bar such as a deformed reinforcing bar. In practice, the deformed reinforcing bar may be placed in the low carbon emission molding die 20 first, and then the low carbon emission ore molding material may be added to strengthen the structure of the molding body 101. To further explain, in order to increase the resistance of the molding body 101 in each direction, the reinforcing bars may first be connected or wound together to form a cage-like structure.
[0072] Additionally, in other embodiments, the embodiments of Figures 8A and 8B can be used in combination, for example, the structural reinforcement 109 can be rebar, steel beams or steel pipes, and the rebar can surround the steel beams or steel pipes to form a stronger structure.
[0073] In one embodiment, when producing a low carbon emission molded article 10, crushing the ore feedstock to form a plurality of crushed ore feedstocks; sorting the plurality of crushed raw ore materials based on a first particle size to obtain a first aggregate 52; A process of removing dust and purifying the first aggregate 52; preparing a second aggregate 53; A process of removing dust and purifying the second aggregate 53; mixing a first aggregate 52, a second aggregate 53, a binder 51, an additive 54 and water to form a low carbon emission ore molding material; The low carbon emission molding 10 can be manufactured by a method including the steps of first placing the embedding members and the connecting parts into a mold at room temperature, and finally adding a low carbon emission ore molding material to the mold and allowing the low carbon emission ore molding material to solidify at room temperature to form the low carbon emission molding 10.
[0074] In the above manufacturing process, the second aggregate 53 may be omitted. Also, the embedding members and the connecting parts are placed in the mold first, that is, the embedding members and the connecting parts are embedded in the molded body 101 in advance.
[0075] To further explain, in one embodiment, the first connecting member 103, the second connecting member 104, the third connecting member 105, the second fastening part 108, the first pipeline 106, and the second pipeline 107 can be placed in the mold first, and then the low-carbon emission ore molding material can be added and the fixing member 102 and the groove 1011 can be provided. After that, after the low-carbon emission ore molding material has solidified, the mold and excess material 40 can be removed, and then the necessary processing can be performed to obtain the low-carbon emission molding 10.
[0076] In one embodiment, the low-carbon emission ore molding material does not include a resin material. To further explain, the low-carbon emission ore molding material of the present application does not contain a resin material such as an epoxy resin, and therefore can have better fluidity than molding materials containing at least a resin material. The low-carbon emission ore molding material of the present application has excellent fluidity and has the ability to fill every corner of a mold before solidifying. That is, the low-carbon emission ore molding material of the present application can be poured at room temperature (e.g., 20°C to 35°C), filled into a mold under natural flow, and then solidified to form a low-carbon emission ore molding. Therefore, the material can be smoothly and reliably filled into the mold without the need for a vibration device or other external means.
[0077] In one embodiment, the mold is provided with parts such as embedded members and connecting parts, and further has parts for defining spaces such as locking holes and grooves, so that the molded body 101 has different wall thicknesses (wall thicknesses), for example, gaps between parts filled by the molded body 101, gaps between parts and spaces filled by the molded body 101, gaps between spaces filled by the molded body 101, etc. In order to maintain the strength of the entire molded body 101, the minimum gap between each part in the mold and each part in the mold and the mold is 50 mm.
[0078] Further, in one embodiment, the minimum spacing between each part in the mold and the spacing between each part in the mold and the mold can be zero so that the two parts are connected, or the part (e.g., the connecting portion) can be placed in close contact with the mold so that the part (e.g., the connecting portion) is exposed to the molded body 101 after the molding material is poured.
[0079] Specifically, in order to provide sufficient strength to the molded body 101 and to allow the molding material to flow smoothly within the mold when poured, the minimum spacing within the mold is 50 mm, i.e., the minimum wall thickness (wall thickness) of the molded body 101 is approximately 50 mm.
[0080] More specifically, the low carbon emission molding 10 formed by the low carbon emission ore molding material of the present application, which includes or is composed of the above-mentioned material, has a thermal conductivity of 2 to 7 W·m -1 K -1 Thermal conductivity coefficient: 0.7-1.5 kJ kg -1 K -1 Specific heat capacity, 5-15×10 -6 / K linear thermal expansion coefficient, compressive strength over 125MPa, flexural strength over 15MPa, Young's modulus between 40000MPa, 2-3g cm -3 The density is between .
[0081] In addition, the low carbon emission molding 10 made of the low carbon emission ore molding material has high temperature resistance and can withstand high temperatures of 450°C or more while maintaining excellent mechanical and physical properties. Compared with moldings containing resin materials, such as materials containing epoxy resin, the heat resistance temperature of the present application is at least 200°C higher (generally, the maximum applicable temperature range of epoxy resin is about 150°C).
[0082] In one embodiment, the thermal conductivity of the low carbon emission molding 10 formed by the first embodiment of the low carbon emission ore molding material is 2 to 5 W·m -1 K -1 For example, 3.0 W m -1 K -1 The specific heat capacity of the molded product is 0.8 to 2.0 kJ kg-1 K -1 For example, 1.2 kJ kg -1 K -1 The linear thermal expansion coefficient of the molded product is 8 to 15 × 10 -6 / K, for example 12×10 -6 / K, the compressive strength of the molding is greater than 125 MPa, the flexural strength of the molding is greater than 15 MPa, the Young's modulus of the molding is 45000 MPa, and the density of the molding is 1.8-3.3 g cm -3 For example, 2.5 g cm -3 the damping logarithmic damping factor may be 0.02-0.04, for example 0.03, and the damping ratio may be 0.4-0.6, for example 0.5.
[0083] In another embodiment, the thermal conductivity coefficient of a molding formed according to the second embodiment of the low carbon emission ore molding material is between 3 and 9 W m -1 K -1 For example, 6.0 W m -1 K -1 The specific heat capacity of the molded product is 0.5 to 1.6 kJ kg -1 K -1 For example, 0.85 kJ kg -1 K -1 The linear thermal expansion coefficient of the molded product is 5 to 15 × 10 -6 / K, for example, 7 x 10 -6 / K, the compressive strength of the molding is greater than 150 MPa, the flexural strength of the molding is greater than 20 MPa, the Young's modulus of the molding is 80000 MPa, and the density of the molding is 1.8-3.3 g cm -3 For example, 2.8 g cm -3 the damping logarithmic damping factor may be between 0.01 and 0.03, for example 0.021, and the damping ratio may be between 0.2 and 0.5, for example 0.33.
[0084] To explain further, the thermal conductivity of epoxy resin mineral moldings is 2.9 to 3.0 W m -1 K -1 The specific heat capacity of epoxy resin ore molding is 0.7~0.9kJ kg -1 K -1 The linear thermal expansion coefficient of epoxy resin ore molding is 15×10-6 / K, the compressive strength of the epoxy resin ore molding is 110-150MPa, the bending strength of the epoxy resin ore molding is 30-35MPa, the Young's modulus of the epoxy resin ore molding is 38000-45000MPa, and the density of the epoxy resin ore molding is 2.3-2.4g cm -3 It is.
[0085] To explain further, the thermal conductivity of ordinary concrete is 2W·m -1 K -1 , the specific heat capacity of ordinary concrete is 1 kJ kg -1 K -1 The coefficient of linear thermal expansion of ordinary concrete is 10~11×10 -6 / K, the compressive strength of ordinary concrete is 5-55MPa, the flexural strength of ordinary concrete is 0-5MPa, the Young's modulus of ordinary concrete is 22000-35000MPa, and the density of ordinary concrete is 2.3g cm -3 It is.
[0086] To explain further, the thermal conductivity of natural hard stone is 1.7 W m -1 K -1 , the specific heat capacity of natural hard stone is 0.85 kJ kg -1 K -1 The linear thermal expansion coefficient of natural hard stone is 5.5 to 7.5 × 10 -6 / K, the compressive strength of natural hard stone is 280-360MPa, the bending strength of natural hard stone is 13-35MPa, the Young's modulus of natural hard stone is 90000-120000MPa, and the density of natural hard stone is 2.9-3.0g cm -3 It is.
[0087] To explain further, the thermal conductivity of cast iron is 29 to 54 W·m -1 K -1 , the specific heat capacity of cast iron is 0.46~0.63kJ kg -1 K -1 , the linear thermal expansion coefficient of cast iron is 9.5~10.5×10 -6 / K, the bending strength of cast iron is 100-800MPa, the Young's modulus of cast iron is 80000-185000MPa, and the density of cast iron is 7.2-7.4g cm -3 ,The damping logarithmic decay rate is 0.003, and the damping ratio is 0.05.
[0088] To explain further, the thermal conductivity of S235 steel is 50 W m -1 K -1 , the specific heat capacity of S235 steel is 0.45 kJ kg -1 K -1 , the linear thermal expansion coefficient of S235 steel is 12×10 -6 / K, the bending strength of S235 steel is 340-470MPa, the Young's modulus of S235 steel is 210000MPa, and the density of S235 steel is 7.8g cm -3 , the damping logarithmic decay rate is 0.001, and the damping ratio is 0.02.
[0089] To explain further, the thermal conductivity of aluminum is 130 to 220 W·m -1 K -1 , the specific heat capacity of aluminum is 0.9 kJ kg -1 K -1 The linear thermal expansion coefficient of aluminum is 23 to 24 × 10 -6 / K, the bending strength of aluminum is 120-500MPa, the Young's modulus of aluminum is 70000MPa, and the density of aluminum is 2.7g cm -3 It is.
[0090] To explain further, the thermal conductivity of stainless steel is 15 W m -1 K -1 , the specific heat capacity of stainless steel is 0.5 kJ kg -1 K -1 , the linear thermal expansion coefficient of stainless steel is 10~16×10 -6 / K.
[0091] More specifically, the logarithmic damping factor of the aluminum alloy is 0.01 to 0.15, and the damping ratio is 0.01 to 0.05.
[0092] From the above, it can be seen that the vibration-damping performance of the moldings made from the low-carbon emission ore molding material of the present application is about 10 times that of cast iron (gray cast iron), has a lower thermal conductivity coefficient than cast iron, and has better heat resistance and Young's modulus than epoxy resin ore moldings, and a lower thermal expansion coefficient. In other words, the moldings made from the low-carbon emission ore molding material of the present application have the effects of heat resistance, low thermal conductivity, low expansion coefficient, high vibration-damping performance, etc.
[0093] In other words, the low-carbon emission molding 10 formed from the low-carbon emission ore molding material of the present application has a low thermal conductivity coefficient and sufficient compressive strength, bending strength, and Young's modulus compared to other materials, particularly conventional materials such as cast iron and concrete, and is therefore suitable for equipment such as machine tools that require excellent insulation and vibration resistance.
[0094] In one embodiment, the molding formed by the low carbon emission ore molding material of the present application may have a width of about 3 meters, a height of about 2 to 4 meters, and a length of about 4 meters. At least the molding of this embodiment can have each function of each of the above embodiments.
[0095] In addition to the above advantages, the low carbon emission moldings 10 formed from the low carbon emission ore molding material of the present application have a lower density than cast iron and most metal materials, which significantly reduces the overall weight of the finished product, i.e., the low carbon emission moldings 10 of the present application not only have excellent mechanical properties, but also have the effect of reducing weight.
[0096] As shown in Fig. 9, the present application further provides a low-carbon emission molded product-containing equipment 30, which includes the low-carbon emission molded product 10 and a processing device 31. The processing device 31 can be connected to the low-carbon emission molded product 10. In one embodiment, the processing device 31 can be connected to a connection portion of the low-carbon emission molded product 10.
[0097] The processing device 31 may include one or more of a three-axis processing device, a five-axis processing device, a cutter, a linear slide rail, a lifting table, a heating device, a cooling device, and a conveying device. The molding body 101 may be a base, a lathe body, a beam, a machine column, a spindle head, a machine body, a worktable, etc. of a machine tool or other equipment.
[0098] As described above, the present application provides a low-carbon emission molding, a mold thereof, and an equipment including the low-carbon emission molding. Since the manufacturing of the molding body does not require a high-temperature molten state, it is possible to save energy and reduce carbon dioxide emissions. In addition, since the manufacturing of the molding body does not require a high-temperature molten state, the embedding member can be placed in the mold first, which reduces the number of subsequent processing steps and improves manufacturing efficiency.
[0099] The above description is merely illustrative and not limiting. Any equivalent modifications or variations made without departing from the spirit and scope of the present application should be included in the appended claims. [Explanation of symbols]
[0100] 10: Low carbon emission moldings 101: Molded product body 1011: Groove 102: Fixing member 1021: First lock hole 1022: First fastening part 103: First connecting member 104: Second connecting member 105: Third connecting member 106: 1st conduit 107:Second conduit 108: Second fastening part 1081: Fastening unit 1082: Connection unit 1083: Buried unit 109: Structural reinforcement 110: Sensor 20: Low carbon emission molded products 21: Bottom of mold 22: Mold side 23: Support member 24: Groove forming member 25: Protruding member 26: Chamfering 27: Roundness 30: Equipment 31: Processing equipment 40: Excess material 51: Binder 52: 1st aggregate 53:Second aggregate 54: Additives 55: Reinforced fiber
Claims
1. A molded body formed by casting and solidifying at room temperature; A plurality of embedded members embedded in the molded body; A connection portion provided on at least one surface of the molded body.
2. 10. The low carbon emission molded article of claim 1, wherein at least one groove is defined in at least one surface of the molded article body.
3. The low carbon emission molded product of claim 1, wherein the plurality of embedded members include a plurality of fixing members provided on the bottom surface of the molded product body, each of the plurality of fixing members having at least a first locking hole defined therein, and at least a first fastening part fastens the fixing member to the ground through the first locking hole.
4. The low carbon emission molded product of claim 1, wherein the connecting portion is made of metal and includes a first connecting member, a second connecting member and a third connecting member, the first connecting member being provided at the center of the upper surface of the molded body, the second connecting member being provided adjacent to the first connecting member, and the third connecting member being provided on a side surface of the molded body.
5. 2. The low carbon emission molded article of claim 1, wherein the plurality of embedded members includes at least one conduit having both openings located on at least one surface of the molded article body.
6. The low carbon emission molded product of claim 1, wherein the plurality of embedded members include a plurality of second fastening parts including a fastening unit, a connection unit and an embedding unit, the fastening unit is located on one surface of the molded product body, and a screw hole is defined, the connection unit is connected to the fastening unit, the embedding unit is connected to the connection unit, and the effective diameter of the connection unit is smaller than the effective diameters of the fastening unit and the embedding unit.
7. 2. The low carbon emission molding of claim 1, wherein the low carbon emission molding has a wall thickness of greater than 50 mm.
8. A mold bottom portion; A plurality of mold sides provided on the mold bottom; 2. The mold for producing low carbon emission molded articles of claim 1, further comprising: at least one support member having opposite ends supporting upper edges of the at least two mold sides.
9. 9. The mold of claim 8 further comprising at least one channel forming member connected to said at least one support member and suspended from said mold bottom.
10. The low carbon emission molded article according to claim 1; and a processing device coupled to the low carbon emission molded article.
Citation Information
Patent Citations
Cementitious inductrial instrument
JP1987119150A
Manufacture of transverse wall with precast concrete joint pipe to be used for special section of pipe utility conduit
JP1998146818A
Outer wall panel of building and its manufacture
JP2000127139A
Low environmental load type ultra high early strength concrete