R-t-b based permanent magnet and manufacturing method thereof
By incorporating controlled carbon and zirconium distributions in R-T-B magnets, the magnet's microstructure is optimized to enhance magnetic properties, addressing the limitations of existing magnets with reduced heavy rare earth elements and shorter sintering times.
Patent Information
- Application Number
- JP2024025671
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-02-22
- Publication Date
- 2024-11-08
AI Technical Summary
Existing R-T-B rare earth permanent magnets suffer from inadequate residual magnetic flux density (Br), coercive force (HcJ), and squareness ratio (Hk/HcJ), particularly when heavy rare earth elements are used in high quantities or with insufficient sintering times.
The R-T-B permanent magnet incorporates specific compositions and microstructures, including carbon (C) and zirconium (Zr), with controlled concentrations and distributions, to enhance magnetic properties. The magnet consists of main phase particles and grain boundaries, where Zr concentration gradients and ZrC distribution ratios are optimized to improve Br, HcJ, and Hk/HcJ.
The optimized R-T-B magnet achieves improved magnetic properties with high Br, HcJ, and Hk/HcJ, even with reduced heavy rare earth element content and shorter sintering times, maintaining excellent magnetic performance.
Smart Images

Figure 2024159498000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to RTB based permanent magnets and methods for producing the same. [Background technology]
[0002] Patent Document 1 describes an invention related to an RTB rare earth permanent magnet. In the method of manufacturing an RTB rare earth permanent magnet described in Patent Document 1, 14 A low R alloy mainly composed of B phase and a high R alloy containing more R than the low R alloy are used. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2004 / 029997 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present disclosure is to obtain an RTB permanent magnet with improved residual magnetic flux density Br, coercive force HcJ, and squareness ratio Hk / HcJ. [Means for solving the problem]
[0005] An RTB permanent magnet according to a first aspect of the present disclosure is an RTB permanent magnet containing C and Zr, the RTB permanent magnet comprises main phase grains and grain boundaries, In the cross section of the RTB permanent magnet, The Zr concentration at the center of the main phase grain is [Zr1], and [Zr1] is 0 to 0.35 at%; The total area of ZrB2 contained in the grain boundaries is S(B), the total area of ZrC contained in the grain boundaries is S(C), and S(C) / (S(B)+S(C)) is 98.0% or more; The RTB permanent magnet is taken as 100% by mass. The Zr content is 0.60 mass% or more and 1.60 mass% or less, The content of B is more than 0 mass% and 0.85 mass% or less, The C content is greater than 0 mass% and is 0.260 mass% or less.
[0006] An RTB permanent magnet according to a second aspect of the present disclosure is an RTB permanent magnet containing C and Zr, the RTB permanent magnet comprises main phase grains and grain boundaries, In the cross section of the RTB permanent magnet, the Zr concentration at the center of the main phase particle is [Zr1] and the Zr concentration at the outer edge of the main phase particle is [Zr2], and the atomic ratio [Zr1] / [Zr2] is 0.70 or more and 1.20 or less, The total area of ZrB2 contained in the grain boundaries is S(B), the total area of ZrC contained in the grain boundaries is S(C), and S(C) / (S(B)+S(C)) is 98.0% or more; The RTB permanent magnet is taken as 100% by mass. The Zr content is 0.60 mass% or more and 1.60 mass% or less, The content of B is more than 0 mass% and 0.85 mass% or less, The C content is greater than 0 mass% and is 0.260 mass% or less.
[0007] The following description is common to the first and second aspects.
[0008] The total area ratio of ZrB2 in the RTB permanent magnet may be 0% or more and less than 0.01%.
[0009] The grain size of ZrB2 may be a maximum of 1.0 μm or less, and the grain size of ZrC may be a maximum of 1.0 μm or less.
[0010] The content of the heavy rare earth element may be 0% by mass or more and 0.80% by mass or less.
[0011] It may further contain Ga, The Ga content may be 0.40 mass % or more and 1.00 mass % or less.
[0012] It may further contain Al, The Al content may be more than 0 mass % and not more than 0.07 mass %.
[0013] The content of the rare earth element may be 29.00 mass % or more and 34.00 mass % or less.
[0014] The rare earth element content may be 30.00 mass % or more and 33.00 mass % or less, and the B content may be 0.70 mass % or more and 0.85 mass % or less.
[0015] A method for producing an RTB permanent magnet according to a third aspect of the present disclosure includes the steps of: providing a main phase alloy and a grain boundary phase alloy; mixing the main phase alloy with the grain boundary phase alloy; The content of C in the main phase alloy is 0.07% by mass or more and 0.180% by mass or less, The Zr content in the grain boundary phase alloy is 3.00% by mass or more and 7.00% by mass or less, The mixing ratio of the main phase alloy to the grain boundary phase alloy is 85:15 to 92:8 in terms of mass ratio.
[0016] In the main phase alloy, The content of rare earth elements is 30.00% by mass or more and 32.50% by mass or less, The Al content is 0 mass% or more and 0.10 mass% or less, The Ga content is 0.40 mass% or more and 1.20 mass% or less, Cu content is 0.10 mass% or more and 1.00 mass% or less, The Co content is 0.50 mass% or more and 3.00 mass% or less, The Zr content is 0.10 mass% or more and 0.80 mass% or less, The content of B may be 0.70% by mass or more and 1.00% by mass or less, In the grain boundary phase alloy, The content of rare earth elements is 30.00% by mass or more and 45.00% by mass or less, The Al content is 0 mass% or more and 1.00 mass% or less, The Ga content is 0 mass% or more and 8.00 mass% or less, Cu content is 0 mass% or more and 5.00 mass% or less, The Co content may be 0% by mass or more and 10.00% by mass or less.
[0017] The area ratio of the 6-13-1 phase in a cross section of the main phase alloy may be 0% or more and less than 2.0%.
[0018] The method may further include a step of sintering the green body, and the sintering time may be 2 hours or more and 8 hours or less.
[0019] In the RTB permanent magnet, The content of rare earth elements is 30.00 mass% or more and 33.00 mass% or less, The B content is 0.70 mass% or more and 0.88 mass% or less, The Al content is greater than 0 mass% and 0.07 mass% or less, The Ga content is 0.40 mass% or more and 1.00 mass% or less, The Zr content may be more than 0.10 mass % and not more than 1.60 mass %. [Brief description of the drawings]
[0020] [Figure 1] 1 is an elemental mapping image of sample No. 3. [Diagram 2] 1 is an elemental mapping image of sample No. 10. [Diagram 3] FIG. 2 is an enlarged view of a main part of FIG. [Figure 4] FIG. 3 is an enlarged view of a main part of FIG. 2. [Diagram 5] 1 is an SEM image of sample No. 3. [Figure 6] 1 is an SEM image of sample No. 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, the present disclosure will be described based on embodiments.
[0022] (First embodiment) RTB permanent magnets are R2T 14 The alloy has main phase grains including crystal grains having a B-type crystal structure, and further has grain boundaries formed by two or more adjacent main phase grains.
[0023] RTB permanent magnets and R2T 14 In the B-type crystal structure, R represents a rare earth element, T represents a transition metal element, and B represents boron.
[0024] RTB permanent magnets and R2T 14 The rare earth element contained as R in the B-type crystal structure may be Sc, Y, or a lanthanoid. The transition metal element contained as T does not include a rare earth element. The transition metal element contained as T may be an iron group element. The iron group element contained as T may be Fe alone, or a part of the Fe contained as T may be substituted with Co. A part of the boron contained as B may be substituted with carbon.
[0025] In this embodiment, the rare earth elements are classified into heavy rare earth elements and light rare earth elements. The heavy rare earth elements are Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. The light rare earth elements are rare earth elements other than the heavy rare earth elements. The iron group elements are Fe, Co, and Ni.
[0026] The RTB permanent magnet according to this embodiment contains carbon (C) and zirconium (Zr), and has the following microstructure and composition.
[0027] (fine structure) The RTB permanent magnet includes main phase grains and grain boundaries, In the cross section of an RTB permanent magnet, The Zr concentration at the center of the main phase grain is [Zr1], and [Zr1] is 0 to 0.35 at%. The total area of ZrB2 contained in the grain boundaries is S(B), and the total area of ZrC contained in the grain boundaries is S(C), and S(C) / (S(B)+S(C)) is 98.0% or more.
[0028] In an RTB permanent magnet, the Zr concentration in the center of the main phase grains is low, and in the Zr compounds contained in the grain boundaries, the ZrC content is high relative to the total content of ZrB2 and ZrC, so that the Br, HcJ, and Hk / HcJ of the RTB permanent magnet are all favorable. In particular, even when the heavy rare earth element content is relatively small, the B content is relatively small, and / or the sintering time is relatively short, an RTB permanent magnet with favorable Br, HcJ, and Hk / HcJ can be obtained.
[0029] If [Zr1] is too large, HcJ and Hk / HcJ decrease. If S(C) / (S(B)+S(C)) is too small, Br and Hk / HcJ decrease. Furthermore, HcJ tends to decrease.
[0030] The Zr concentration at the outer edge of the main phase grains may be [Zr2], and [Zr2] may be 0 or more and 0.72 at % or less.
[0031] The total area ratio of ZrB2 in the cross section of the RTB permanent magnet may be 0% or more and less than 0.01%. When the total area ratio of ZrB2 is within the above range, Hk / HcJ tends to be good.
[0032] Of the Zr compounds contained in the cross section of the RTB permanent magnet, 99% or more by number may have a grain size of 1.0 μm or less. The total number of ZrB2 having a grain size of 1.0 μm or less and ZrC having a grain size of 1.0 μm or less relative to the total number of ZrB2 and ZrC may be 99% or more. The grain size of the Zr compounds may be a maximum of 1.0 μm or less. The grain size of ZrB2 may be a maximum of 1.0 μm or less, and the grain size of ZrC may be a maximum of 1.0 μm or less.
[0033] The method for measuring [Zr1] and [Zr2] of the main phase particles contained in an RTB permanent magnet will be described below.
[0034] First, element mapping is performed on the cross section of the RTB permanent magnet. There are no particular limitations on the device used for element mapping, and any device capable of performing appropriate element mapping may be used. Examples include EPMA and EDS. The magnification may be any magnification capable of appropriately measuring [Zr1] and [Zr2]. For example, the magnification may be 1500 times or more and 10000 times or less. By element mapping, for example, the image shown in Figure 1 can be obtained.
[0035] 1 is an example, sample No. 3, described later. The RTB permanent magnet 1 includes main phase grains 11 and grain boundaries 13. The grain boundaries 13 include R-containing portions 13a and Zr-containing portions 13b.
[0036] The R-containing portion 13a is a portion that contains a large amount of R-rich phase and / or 6-13-1 phase in the grain boundary 13. The R-rich phase is a phase that contains at least a large amount of R, and further contains more Co, Cu and / or Ga than the main phase grains 11. The 6-13-1 phase is a phase that contains a large amount of R, Fe, Co, Cu and Ga.
[0037] The Zr-containing portion 13b is a portion of the grain boundary 13 that contains a particularly large amount of Zr compounds.
[0038] Furthermore, grain boundary 13 may include a portion that is difficult to identify as being an R-containing portion 13a or a Zr-containing portion 13b because it contains a large amount of R, Co, Cu, Ga, and / or both Ga and Zr.
[0039] Then, the position and shape of the main phase particle 11 included in the obtained element mapping image are identified. At this time, the element mapping image may be enlarged as appropriate. For example, FIG. 3 is an enlarged image of part A in FIG. 1. Next, the center of the main phase particle 11, the entirety of which is included in the element mapping image, is identified. Specifically, the center of the main phase particle 11 is determined as a part in the element mapping image whose distance from the surface of the main phase particle 11 is 40% or more of the equivalent circle diameter of the main phase particle. In other words, the center is located in a part whose distance from the boundary between the main phase particle 11 and the grain boundary 13 is 40% or more of the equivalent circle diameter of the main phase particle. Then, the Zr concentration in the center of the main phase particle 11 is measured and defined as [Zr1]. The measurement targets of [Zr1] and [Zr2] are main phase particles 11 having a region that satisfies the definition of the center and a region that satisfies the definition of the outer edge portion described later.
[0040] When calculating [Zr1] in the RTB permanent magnet 1, the element mapping image is observed so that the number of main phase grains 11 that are entirely included and have a central portion is at least three or more. The number of main phase grains 11 that are entirely included and have a central portion may be five or more. Then, [Zr1] of each main phase grain 11 entirely included in the element mapping image may be measured and averaged to calculate [Zr1] in the RTB permanent magnet 1.
[0041] The method for measuring [Zr2] is the same as the method for measuring [Zr1], except that the measurement location of the Zr concentration is changed from the center of the main phase particle 11 to the outer edge of the main phase particle 11. Specifically, the outer edge of the main phase particle 11 is a portion that is 30% or less of the equivalent circle diameter of the main phase particle from the surface of the main phase particle 11 in the element mapping image. In other words, the outer edge is located at a position where the distance from the boundary between the main phase particle 11 and the grain boundary 13 is 30% or less of the equivalent circle diameter of the main phase particle. In order to avoid detecting grain boundary components when measuring [Zr2], a portion that is 15% to 30% of the equivalent circle diameter of the main phase particle from the surface of the main phase particle 11 may be measured.
[0042] The RTB permanent magnet 2 shown in Fig. 2 is sample No. 10, a comparative example described below. Fig. 4 is an enlarged image of portion B in Fig. 2. Figs. 2 and 4 show that the RTB permanent magnet 2 shown in Fig. 2 has a higher Zr concentration in the main phase particles 11 than the RTB permanent magnet 1 shown in Fig. 1. In particular, the Zr concentration is high in the center of the main phase particles 11, and the distribution of Zr concentration makes it appear that the main phase particles 11 are core-shell particles containing a shell with a low Zr concentration and a core with a high Zr concentration. In other words, the RTB permanent magnet 2 has low HcJ and Hk / HcJ because [Zr1] is too large.
[0043] Below, we will explain how to observe Zr compounds and how to distinguish between ZrB2 and ZrC. We will also explain how to measure S(C) / (S(B)+S(C)) and how to measure the grain size of Zr compounds.
[0044] First, a composition image is observed for a cross section of the RTB permanent magnet. There are no particular limitations on the device used to observe the composition image, and any device that can properly observe the composition image may be used. For example, an SEM may be used. The magnification may be any magnification that can properly observe the Zr compound. For example, it may be 2500 times or more and 20000 times or less.
[0045] Figure 5 is an SEM image obtained by observing the cross section of the RTB permanent magnet 1 at 10,000 times using an SEM. Figure 6 is an SEM image obtained by observing a different part of the cross section of the RTB permanent magnet 1 from that shown in Figure 5 at 20,000 times using an SEM. Figure 5 also shows a square with a side length of 1 μm for comparison. Figure 6 shows a square with a side length of 1 μm and a square with a side length of 0.5 μm for comparison.
[0046] 5 and 6 mainly show Zr-containing portion 13b, which is a grain boundary containing a large amount of Zr compounds, together with main phase grains 11. Zr-containing portion 13b contains a large number of Zr compounds 15. In Zr-containing portion 13b, Zr compounds 15 can be distinguished from other portions by the difference in contrast.
[0047] Whether the Zr compound 15 is ZrB2 or ZrC can be distinguished by the shape of the Zr compound 15 in the SEM image of the cross section of the RTB permanent magnet 1. Specifically, it can be distinguished by the aspect ratio (major axis / minor axis) of the Zr compound 15. Zr compounds with an aspect ratio of more than 5 can be determined to be ZrB2, and Zr compounds with an aspect ratio of 5 or less can be determined to be ZrC. All of the Zr compounds 15 shown in Figures 5 and 6 are ZrC.
[0048] The possibility cannot be completely denied that the SEM images contain ZrC with an aspect ratio greater than 5 and / or ZrB2 with an aspect ratio less than 5. However, the above possibility can be ignored in calculating the total area ratio of ZrB2 in the RTB permanent magnet and S(C) / (S(B)+S(C)).
[0049] ZrB2 has an AlB2-based hexagonal crystal structure. In the SEM image, it has a needle-like shape. Therefore, it appears to be a long, thin, roughly rectangular shape. ZrC has a face-centered cubic structure. In the SEM image, it has a granular shape. Therefore, it appears to be a roughly rectangular shape.
[0050] The size of the observation area by SEM is set to a size that includes at least 5 or more Zr compounds 15. The size of the observation area by SEM may be set to a size that includes 10 or more Zr compounds 15. Then, the total area S(B) of ZrB2 and the total area S(C) of ZrC are measured, and S(C) / (S(B)+S(C)) is calculated. The particle size of each Zr compound is the circle equivalent diameter of each Zr compound.
[0051] (composition) As described above, the RTB permanent magnet contains carbon (C) and zirconium (Zr).
[0052] Taking the RTB permanent magnet as 100 mass%, the Zr content is 0.60 mass% or more and 1.60 mass% or less. It may be 0.80 mass% or more and 1.20 mass% or less. The lower the Zr content, the more likely it is that abnormal grain growth of the main phase particles will occur, and when abnormal grain growth occurs, the more likely it is that HcJ and Hk / HcJ will decrease. The higher the Zr content, the more likely it is that ZrB2 compounds will be produced during the production of the RTB permanent magnet, and the more likely S(C) / (S(B)+S(C)) will decrease. And the more likely it is that HcJ and Hk / HcJ will decrease.
[0053] With the RTB permanent magnet being 100% by mass, the C content is greater than 0% by mass and is 0.260% by mass or less. The C content may be 0.150% by mass or more, 0.160% by mass or more, 0.167% by mass or more, 0.175% by mass or more, 0.200% by mass or more, or 0.226% by mass or more. The C content may be 0.248% by mass or less. The lower the C content, the less likely ZrC compounds are to be formed during the manufacture of the RTB permanent magnet, and the more likely ZrB2 compounds are to be formed. Then, S(C) / (S(B)+S(C)) is more likely to decrease. Then, Br, HcJ, and Hk / HcJ are more likely to decrease. The higher the C content, the more likely HcJ is to decrease.
[0054] With the RTB permanent magnet taken as 100% by mass, the B content is 0.85% by mass or less. The B content may be 0.70% by mass or more and 0.83% by mass or less. The lower the B content, the more likely it is that sintering will be insufficient. As a result, Br and HcJ are more likely to decrease. The higher the B content, the more likely it is that HcJ is more likely to decrease.
[0055] The content of rare earth elements (hereinafter, sometimes referred to as TRE) is not particularly limited. For example, it may be 29.00 mass% or more and 34.00 mass% or less, or 30.00 mass% or more and 33.00 mass% or less. The smaller the TRE, the more likely HcJ is to decrease. The larger the TRE, the more likely abnormal grain growth is to occur, and the more likely Br is to decrease.
[0056] The RTB permanent magnet may contain, as rare earth elements, one or more selected from Nd, Pr, Dy, and Tb, or may contain, as rare earth elements, one or more selected from Nd and Pr. Note that, "the RTB permanent magnet contains, as rare earth elements, one or more selected from Nd, Pr, Dy, and Tb," means that the content of rare earth elements other than Nd, Pr, Dy, and Tb is 0.01 mass% or less in total. "the RTB permanent magnet contains, as rare earth elements, one or more selected from Nd and Pr," means that the content of rare earth elements other than Nd and Pr is 0.01 mass% or less in total.
[0057] The content of the heavy rare earth element is not particularly limited. For example, it may be 0% by mass or more and 0.80% by mass or less, 0% by mass or more and 0.50% by mass or less, or 0% by mass or more and 0.30% by mass or less. The higher the content of the heavy rare earth element, the easier it is for the Br to decrease and the raw material cost to increase.
[0058] There is no particular limit to the content of iron group elements, and no particular limit to the content of Co. From the viewpoint of improving magnetic properties and corrosion resistance, the content of Co may be 0.50 mass% or more and 3.00 mass% or less, or 0.80 mass% or more and 3.00 mass% or less. Ni may not be substantially contained. Specifically, the content of Ni may be 0 mass% or more and less than 0.01 mass%.
[0059] The RTB permanent magnet may further contain Ga, Al and / or Cu.
[0060] There is no particular limit to the Ga content. For example, it may be 0.40 mass % or more and 1.00 mass % or less. The lower the Ga content, the easier it is for HcJ to decrease. The higher the Ga content, the easier it is for Br to decrease.
[0061] There is no particular limitation on the Al content. For example, it may be more than 0 mass% and 0.07 mass% or less, or it may be 0.02 mass% or more and 0.07 mass% or less. The lower the Al content, the more likely HcJ is to decrease. The higher the Al content, the more likely Br is to decrease.
[0062] There is no particular limitation on the Cu content. For example, it may be 0 mass% or more and 1.00 mass% or less, or it may be 0.15 mass% or more and 1.00 mass% or less. The lower the Cu content, the more likely Br is to decrease. The higher the Cu content, the more likely HcJ is to decrease.
[0063] Regarding the R-T-B-based permanent magnet being 100 mass%, it means that the total content of all elements is 100 mass%. And the Fe content in the R-T-B-based permanent magnet may be the substantial remainder in the R-T-B-based permanent magnet. Specifically, the content of elements other than the above-described elements, that is, elements other than rare earth elements, Fe, Co, Ni, B, Al, Ga, Zr, Cu, and C may each be 0.20 mass% or less, and the total may be 1.00 mass% or less.
[0064] <Method for manufacturing R-T-B-based permanent magnet> Hereinafter, an example of a method for manufacturing an R-T-B-based permanent magnet according to the present embodiment will be described. The method for manufacturing an R-T-B-based permanent magnet according to the present embodiment may include the following steps.
[0065] (a) Alloy preparation step of preparing a main phase alloy and a grain boundary phase alloy (b) Crushing step of crushing the main phase alloy and the grain boundary phase alloy (c) Mixing step of mixing the main phase alloy and the grain boundary phase alloy (d) Forming step of forming the obtained alloy powder (e) Sintering step of sintering the formed body to obtain an R-T-B-based permanent magnet (f) Aging treatment step of aging the R-T-B-based permanent magnet (g) Cooling step of cooling the R-T-B-based permanent magnet (h) Processing step of processing the R-T-B-based permanent magnet (i) Surface treatment process for RTB permanent magnets
[0066] Depending on the type of RTB permanent magnet finally obtained, some of the above steps may be omitted as appropriate. For example, if the RTB permanent magnet is an RTB sintered magnet, the sintering step (e) is included, but if the RTB permanent magnet is a bonded magnet, steps such as the sintering step (e) are not included. Hot compacting and hot working may be performed instead of sintering. Furthermore, steps other than the above steps may be added as appropriate.
[0067] However, the method for producing an RTB permanent magnet according to this embodiment necessarily includes at least the alloy preparation step (a) and the mixing step (c).
[0068] [Alloy preparation process] First, a main phase alloy and a grain boundary phase alloy are prepared (alloy preparation step). The RTB permanent magnet having the above configuration is obtained by a two-alloy method using a main phase alloy and a grain boundary phase alloy. There is no particular difference in the manufacturing method between the main phase alloy and the grain boundary phase alloy. Below, a strip casting method will be described as an example of an alloy preparation method for the main phase alloy, but the alloy preparation method is not limited to the strip casting method. With regard to the alloy preparation method for the grain boundary phase alloy, the main phase alloy in the following description will be read as the grain boundary phase alloy.
[0069] First, raw metals corresponding to the composition of the main phase alloy are prepared and melted in a vacuum or in an inert gas atmosphere such as Ar gas. The melted raw metals are then cast to produce the main phase alloy.
[0070] There is no particular limit to the type of raw metal. For example, rare earth metals or rare earth alloys, pure iron, pure cobalt, ferroboron, and alloys and compounds thereof can be used. There is no particular limit to the casting method for casting the raw metal. For example, ingot casting, strip casting, book molding, centrifugal casting, etc. can be mentioned. If the obtained main phase alloy has solidification segregation, it may be subjected to homogenization treatment (solution treatment) as necessary.
[0071] The alloy preparation method may be performed by atomization, in which case the pulverization step described below may be omitted.
[0072] [Crushing process] A method for crushing the main phase alloy will be described below. Regarding a method for crushing the grain boundary phase alloy, the main phase alloy in the following description will be read as the grain boundary phase alloy.
[0073] After the main phase alloy is produced, it is pulverized (pulverization step). The pulverization step may be performed in two stages, a coarse pulverization step in which the alloy is pulverized to a particle size of several hundred μm to several mm, and a fine pulverization step in which the alloy is pulverized to a particle size of several μm, or may be performed in one stage only, the fine pulverization step.
[0074] (Coarse grinding process) The main phase alloy is coarsely pulverized until the particle size is about several hundred μm to several mm (coarse pulverization step). This produces a coarsely pulverized powder of the main phase alloy. The coarse pulverization may be performed, for example, by hydrogen absorption pulverization. The hydrogen absorption pulverization can be performed by absorbing hydrogen into the main phase alloy and then releasing hydrogen based on the difference in the amount of hydrogen absorption between different phases, thereby causing self-destructive pulverization. Releasing hydrogen based on the difference in the amount of hydrogen absorption between different phases is called dehydrogenation. There are no particular limitations on the conditions for dehydrogenation, but dehydrogenation is performed, for example, at 300 to 650°C in an argon flow or in a vacuum.
[0075] The method of coarse pulverization is not limited to the above-mentioned hydrogen absorption pulverization. For example, coarse pulverization may be performed in an inert gas atmosphere using a coarse pulverizer such as a stamp mill, a jaw crusher, or a Braun mill.
[0076] In order to obtain an RTB permanent magnet having high magnetic properties, the atmosphere in each process from the coarse pulverization process to the sintering process described later may be an atmosphere with a low oxygen concentration. The oxygen concentration is adjusted by controlling the atmosphere in each manufacturing process. If the oxygen concentration in each manufacturing process is high, the rare earth elements in the alloy powder obtained by pulverizing the main phase alloy will be oxidized to generate oxides of the rare earth elements. The oxides of the rare earth elements are not reduced during sintering, and are precipitated as they are in the form of oxides of the rare earth elements at the grain boundaries. The grain boundaries are the portions that exist between two or more main phase particles. As a result, the Br of the obtained RTB permanent magnet is reduced. Therefore, for example, each process (fine pulverization process, molding process) may be performed in an atmosphere with an oxygen concentration of 100 ppm or less.
[0077] (Fine grinding process) After the main phase alloy is coarsely pulverized, the obtained coarsely pulverized powder of the main phase alloy is finely pulverized until the average particle size is about several μm (fine pulverization process). This produces finely pulverized powder of the main phase alloy. The coarsely pulverized powder can be further finely pulverized to produce finely pulverized powder. There is no particular restriction on the D50 of the particles contained in the finely pulverized powder. For example, D50 may be 2.0 μm or more and 4.5 μm or less, or 2.5 μm or more and 3.5 μm or less. The smaller the D50, the more likely the HcJ of the RTB permanent magnet according to this embodiment is to be improved. However, abnormal grain growth is more likely to occur in the sintering process, and the upper limit of the sintering temperature range is lowered. The larger the D50, the less likely the abnormal grain growth is to occur in the sintering process, and the upper limit of the sintering temperature range is higher. However, the HcJ of the RTB permanent magnet according to this embodiment is more likely to be reduced.
[0078] Fine pulverization is performed by further pulverizing the coarsely pulverized powder using a fine pulverizer such as a jet mill, ball mill, vibration mill, or wet attritor while appropriately adjusting conditions such as pulverization time. Jet mills are described below. A jet mill is a fine pulverizer that releases high-pressure inert gas (e.g., He gas, N2 gas, or Ar gas) from a narrow nozzle to generate a high-speed gas flow, and accelerates the coarsely pulverized powder of the main phase alloy by this high-speed gas flow, causing collisions between the coarsely pulverized powder of the main phase alloy and with the target or the wall of the container, thereby pulverizing the powder.
[0079] A grinding aid may be added when the coarsely pulverized powder of the main phase alloy is pulverized. There is no particular limitation on the type of grinding aid. For example, an organic lubricant or a solid lubricant may be used. Examples of organic lubricants include oleic acid amide, lauric acid amide, and zinc stearate. Examples of solid lubricants include graphite. By adding a grinding aid, it is possible to obtain a finely pulverized powder that is likely to be oriented when a magnetic field is applied in the molding process. Either the organic lubricant or the solid lubricant may be used alone, or both may be used in combination. This is because the degree of orientation may decrease, especially when only a solid lubricant is used.
[0080] [Mixing process] Next, the main phase alloy and the grain boundary phase alloy are mixed to obtain an alloy powder for molding (mixing step). There are no particular limitations on the mixing method.
[0081] [Molding process] The alloy powder for molding is molded into a desired shape (molding step). In the molding step, the alloy powder for molding is filled into a die placed in an electromagnet and pressurized to mold the alloy powder for molding into a molded body. At this time, by molding while applying a magnetic field, the alloy powder for molding can be molded with the crystal axes of the alloy powder for molding oriented in a specific direction. Since the obtained molded body is oriented in a specific direction, an RTB permanent magnet with stronger anisotropy can be obtained. In addition, a molding aid may be added. There is no particular limit to the type of molding aid. The same lubricant as the grinding aid may be used. In addition, the grinding aid may also serve as the molding aid.
[0082] The pressure during pressurization may be, for example, 30 MPa or more and 300 MPa or less. The magnetic field to be applied may be, for example, 1000 kA / m or more and 1600 kA / m or less. The magnetic field to be applied is not limited to a static magnetic field, and may be a pulsed magnetic field. In addition, a static magnetic field and a pulsed magnetic field may be used in combination.
[0083] As a compacting method, in addition to the dry compaction in which the alloy powder for compaction is directly compacted as described above, wet compaction in which a slurry in which the alloy powder for compaction is dispersed in a solvent such as oil is also applicable.
[0084] The shape of the compact obtained by compacting the alloy powder for molding is not particularly limited, and can be, for example, a rectangular parallelepiped, a flat plate, a column, a ring, or any other shape that corresponds to the shape of the desired RTB permanent magnet.
[0085] [Sintering process] The compact obtained by molding in a magnetic field and forming into the desired shape is sintered in a vacuum or inert gas atmosphere to obtain an RTB permanent magnet (sintering process). The holding temperature (sintering temperature) and holding time (sintering time) during sintering need to be adjusted depending on various conditions, such as the composition, the crushing method, the particle size and particle size distribution, etc. There is no particular limit to the sintering temperature, but it may be 1040°C or higher and 1100°C or lower. There is no particular limit to the sintering time, but it may be 1 hour or higher and 10 hours or lower, 2 hours or higher and 8 hours or lower, or 3 hours or higher and 6 hours or lower. The shorter the sintering time, the higher the production efficiency. However, [Zr1] and [Zr2] tend to become larger, and the magnetic properties, especially Hk / HcJ, tend to decrease. The longer the sintering time, the easier it is to improve the magnetic properties. However, the production efficiency decreases.
[0086] There is no particular limit to the atmosphere during sintering. For example, it may be an inert gas atmosphere, a vacuum atmosphere of less than 100 Pa, or a vacuum atmosphere of less than 10 Pa. There is no particular limit to the heating rate up to the sintering temperature. By sintering, the alloy powder undergoes liquid phase sintering, and the RTB permanent magnet according to the present embodiment is obtained. There is no particular limit to the cooling rate after sintering the compact to obtain a sintered body, but the sintered body may be quenched to improve production efficiency. It may be quenched at a rate of 30°C / min or more.
[0087] [Aging treatment process] After sintering the compact, the RTB permanent magnet is subjected to an ageing treatment (aging treatment step). After sintering, the RTB permanent magnet is subjected to an ageing treatment by, for example, holding the obtained RTB permanent magnet at a temperature lower than that during sintering. Below, a case where the aging treatment is divided into two stages, a first aging treatment and a second aging treatment, will be explained, but only one of the aging treatments may be performed, or three or more stages of aging treatment may be performed.
[0088] There is no particular limit to the holding temperature and holding time in each aging treatment. For example, the first aging treatment may be performed at a holding temperature of 800°C or more and 900°C or less for 30 minutes to 4 hours. The heating rate to the holding temperature may be 5°C / min to 50°C / min. The atmosphere during the first aging treatment may be an inert gas atmosphere (e.g., He gas, Ar gas) at atmospheric pressure or higher. The second aging treatment may be performed under the same conditions as the first aging treatment, except that the holding temperature may be 450°C or more and 550°C or less. The magnetic properties of the RTB permanent magnet can be improved by the aging treatment. The aging treatment process may be performed after the processing process described later.
[0089] [Cooling process] After the RTB permanent magnet is subjected to an aging treatment (first aging treatment or second aging treatment), the RTB permanent magnet is rapidly cooled in an inert gas atmosphere (cooling step). This makes it possible to obtain the RTB permanent magnet according to this embodiment. The cooling rate is not particularly limited. It may be 30°C / min or more.
[0090] [Processing process] The obtained RTB permanent magnet may be processed into a desired shape as necessary (processing step). Examples of processing methods include shaping such as cutting and grinding, and chamfering such as barrel polishing.
[0091] [Grain boundary diffusion process] A heavy rare earth element may be further diffused into the grain boundaries of the processed RTB permanent magnet (grain boundary diffusion step). There are no particular limitations on the method of grain boundary diffusion. For example, it may be carried out by attaching a compound containing a heavy rare earth element to the surface of the RTB permanent magnet by coating or vapor deposition, etc., and then carrying out a heat treatment. It may also be carried out by carrying out a heat treatment on the RTB permanent magnet in an atmosphere containing vapor of the heavy rare earth element. Grain boundary diffusion can further improve the HcJ of the RTB permanent magnet.
[0092] [Surface treatment process] The RTB permanent magnet obtained by the above steps may be subjected to surface treatment such as plating, resin coating, oxidation treatment, chemical conversion treatment, etc. (surface treatment step), which can further improve the corrosion resistance.
[0093] In the above-mentioned method for producing an RTB permanent magnet, it is important to appropriately control the composition of the main phase alloy, the microstructure of the main phase alloy, the composition of the grain boundary phase alloy, and the mixing ratio of the main phase alloy and the grain boundary phase alloy. The main phase alloy is the alloy that will ultimately become mainly the main phase particles 11, and the grain boundary phase alloy is the alloy that will ultimately become mainly the grain boundaries 13.
[0094] (Main phase alloy composition) The main phase alloy is 100% by mass, and the C content is at least 0.070% by mass or more and 0.180% by mass or less. The C content may be 0.080% by mass or more, 0.090% by mass or more, 0.100% by mass or more, or 0.120% by mass or more. The C content may be 0.160% by mass or less. The lower the C content of the main phase alloy, the less likely ZrC compounds are to be formed during the manufacture of the RTB permanent magnet, and the more likely ZrB2 compounds are to be formed. The S(C) / (S(B)+S(C)) of the resulting RTB permanent magnet is more likely to decrease. The Br, HcJ, and Hk / HcJ of the resulting RTB permanent magnet are more likely to decrease. Furthermore, the 6-13-1 phase described later is more likely to be included in the main phase alloy, and the α-Fe is more likely to be included in the resulting RTB permanent magnet. The higher the C content of the main phase alloy, the more likely HcJ of the resulting RTB permanent magnet is more likely to decrease.
[0095] There is no particular limit to the content of other components in the main phase alloy. For example, assuming the main phase alloy is 100 mass%, The content of rare earth elements is 30.00% by mass or more and 32.50% by mass or less, The Al content is 0 mass% or more and 0.10 mass% or less, The Ga content is 0.40 mass% or more and 1.20 mass% or less, Cu content is 0.10 mass% or more and 1.00 mass% or less, The Co content is 0.50 mass% or more and 3.00 mass% or less, The Zr content is 0.10 mass% or more and 0.80 mass% or less, The B content may be 0.70 mass % or more and 1.00 mass % or less.
[0096] The main phase alloy being 100% by mass means that the total content of all elements is 100% by mass. The content of Fe in the main phase alloy may be substantially the remainder of the main phase alloy. Specifically, the content of elements other than rare earth elements, Fe, Co, B, Al, Ga, Zr, Cu, and C may each be 0.20% by mass or less, and may be 1.00% by mass or less in total.
[0097] (Microstructure of main phase alloy) The main phase alloy may have a small content of the 6-13-1 phase. Specifically, in the cross section of the main phase alloy, La6Co 11 R6T is a compound with a Ga3 type crystal structure. 13 The content of the phase containing the M compound may be 0% or more and less than 2.0%, or 0% or more and 1.0% or less. In general, there is no particular limitation on the type of M. Examples of M include Ga, Al, Cu, Zn, In, P, Sb, Si, Ge, Sn, and Bi.
[0098] Generally, when preparing a main phase alloy containing Ga, the 6-13-1 phase is likely to form in the main phase alloy. However, when preparing a main phase alloy containing 0.070 mass% or more of C in addition to Ga, the R6T 13 The production of M compounds is inhibited.
[0099] When a main phase alloy containing Ga but not containing 0.070 mass% or more of C is prepared, the 6-13-1 phase is generated in the main phase alloy. 13 M compounds precipitate. R6T 13 When M compounds are precipitated, the R6T contained in the main phase alloy is precipitated when the main phase alloy is heated to a specific temperature range in any of the manufacturing processes of RTB permanent magnets. 13The M compound decomposes to produce α-Fe, which can lead to a decrease in the magnetic properties such as Hk / HcJ of the final RTB permanent magnet.
[0100] Below, we will explain how to observe the 6-13-1 phase and how to measure the area ratio of the 6-13-1 phase.
[0101] First, a composition image is observed for the cross section of the main phase alloy. There is no particular limitation on the device used for observing the composition image, and any device capable of properly observing the composition image may be used. For example, an SEM may be used. The magnification may be any magnification capable of properly observing the 6-13-1 phase. For example, the magnification may be 1000 times or more and 5000 times or less. In the composition image obtained by SEM, the main phase is the dark gray part, and the R-rich phase is the light gray part. The 6-13-1 phase is included in the R-rich phase, but is a dark gray part compared to the other parts of the R-rich phase.
[0102] (Composition of grain boundary phase alloy) With the grain boundary phase alloy being 100 mass%, the Zr content is at least 3.00 mass% to 7.00 mass%. The lower the Zr content of the grain boundary phase alloy, the more likely abnormal grain growth of the main phase particles will occur, and when abnormal grain growth occurs, the more likely HcJ and Hk / HcJ will decrease. The higher the Zr content of the grain boundary phase alloy, the more likely ZrB2 compounds will be formed during the production of RTB permanent magnets, and the more likely S(C) / (S(B)+S(C)) will decrease. And the more likely HcJ and Hk / HcJ will decrease. During the production of RTB permanent magnets, ZrC compounds are less likely to be formed and ZrB2 compounds are more likely to be formed.
[0103] There is no particular limit to the content of other components in the grain boundary phase alloy. For example, assuming the grain boundary phase alloy to be 100 mass%, The content of rare earth elements is 30.00% by mass or more and 45.00% by mass or less, The Al content is 0 mass% or more and 1.00 mass% or less, The Ga content is 0 mass% or more and 8.00 mass% or less, Cu content is 0 mass% or more and 5.00 mass% or less, The Co content may be 0% by mass or more and 10.00% by mass or less.
[0104] There is no particular limit to the C content in the grain boundary phase alloy. For example, the C content may be 0.100% by mass or less, 0.090% by mass or less, or 0.050% by mass or less, assuming that the grain boundary phase alloy is 100% by mass. If the C content in the grain boundary phase alloy is too high, the C content in the RTB permanent magnet increases, and the HcJ tends to decrease.
[0105] The grain boundary phase alloy being 100% by mass means that the total content of all elements is 100% by mass. The content of Fe in the grain boundary phase alloy may be substantially the remainder in the grain boundary phase alloy. Specifically, the content of elements other than rare earth elements, Fe, Co, Al, Ga, Zr, Cu, and C may be 0.20% by mass or less, respectively, and 1.00% by mass or less in total.
[0106] (Comparison between main phase alloy and grain boundary phase alloy) When comparing the main phase alloy and the grain boundary phase alloy, the main phase alloy may have a higher Ga content. The main phase alloy may have a higher Cu content. The grain boundary phase alloy may have a higher Co content. The grain boundary phase alloy may have a higher Zr content. The main phase alloy may have a higher B content. The main phase alloy may have a higher C content.
[0107] (Mixing ratio of main phase alloy to grain boundary phase alloy) The mixing ratio of the main phase alloy to the grain boundary phase alloy is 85:15 to 92:8 by mass. If the final RTB permanent magnet has a similar composition, but the amount of main phase alloy is too small, the Hk / HcJ of the final RTB permanent magnet is likely to decrease. If the final RTB permanent magnet has a similar composition, but the amount of main phase alloy is too large, the magnetic properties, particularly Hk / HcJ, are likely to decrease.
[0108] The RTB permanent magnet obtained in the above manner has good magnetic properties. That is, an RTB permanent magnet with excellent magnetic properties can be obtained with a relatively small amount of heavy rare earth element used, a relatively small content of B, and a relatively short sintering time.
[0109] It should be noted that the present disclosure is not limited to the above-described embodiments, and various modifications can be made within the scope of the present disclosure.
[0110] Second embodiment The second embodiment will be described below, but matters not specifically mentioned are the same as those in the first embodiment.
[0111] In the second embodiment, the microstructure of the RTB permanent magnet is different from that of the first embodiment.
[0112] The RTB permanent magnet includes main phase grains and grain boundaries, In the cross section of an RTB permanent magnet, the Zr concentration at the center of the main phase particle is [Zr1], the Zr concentration at the outer edge of the main phase particle is [Zr2], and the atomic ratio of [Zr1] / [Zr2] is 0.70 or more and 1.20 or less; The total area of ZrB2 contained in the grain boundaries is S(B), and the total area of ZrC contained in the grain boundaries is S(C), and S(C) / (S(B)+S(C)) is 98.0% or more.
[0113] In the RTB permanent magnet, the difference between the Zr concentration at the center of the main phase particle and the Zr concentration at the outer edge of the main phase particle is small. In other words, the Zr concentration in the main phase particle is generally uniform. Furthermore, in the Zr compound contained in the grain boundary, the content ratio of ZrC relative to the total content of ZrB2 and ZrC is high, so that the Br, HcJ, and Hk / HcJ of the RTB permanent magnet are all favorable. In particular, even when the content of heavy rare earth elements is relatively small, the content of B is relatively small, and / or the sintering time is relatively short, an RTB permanent magnet with favorable Br, HcJ, and Hk / HcJ can be obtained.
[0114] If [Zr1] / [Zr2] is too large, HcJ and Hk / HcJ decrease. If S(C) / (S(B)+S(C)) is too small, Br and Hk / HcJ decrease. Furthermore, HcJ is also likely to decrease.
[0115] [Zr1] may be 0 or more and 0.50 at % or less, and [Zr2] may be 0 or more and 0.72 at % or less.
[0116] The method for measuring [Zr1] and [Zr2] of the main phase particles contained in an RTB permanent magnet will be described below.
[0117] First, element mapping is performed on the cross section of the RTB permanent magnet. There are no particular limitations on the device used for element mapping, and any device capable of performing appropriate element mapping may be used. Examples include EPMA and EDS. The magnification may be any magnification capable of appropriately measuring [Zr1] and [Zr2]. For example, the magnification may be 1500 times or more and 10000 times or less. By element mapping, for example, the image shown in Figure 1 can be obtained.
[0118] 1 is an example, sample No. 3, described later. The RTB permanent magnet 1 includes main phase grains 11 and grain boundaries 13. The grain boundaries 13 include R-containing portions 13a and Zr-containing portions 13b.
[0119] The R-containing portion 13a is a portion that contains a large amount of R-rich phase and / or 6-13-1 phase in the grain boundary 13. The R-rich phase is a phase that contains at least a large amount of R, and further contains more Co, Cu and / or Ga than the main phase grains 11. The 6-13-1 phase is a phase that contains a large amount of R, Fe, Co, Cu and Ga.
[0120] The Zr-containing portion 13b is a portion of the grain boundary 13 that contains a particularly large amount of Zr compounds.
[0121] Furthermore, grain boundary 13 may include a portion that is difficult to identify as being an R-containing portion 13a or a Zr-containing portion 13b because it contains a large amount of R, Co, Cu, Ga, and / or both Ga and Zr.
[0122] Then, the position and shape of the main phase particle 11 included in the obtained element mapping image are identified. At this time, the element mapping image may be enlarged as appropriate. For example, FIG. 3 is an enlarged image of part A in FIG. 1. Next, the center of the main phase particle 11, the entirety of which is included in the element mapping image, is identified. Specifically, the center of the main phase particle 11 is determined as a part whose distance from the surface of the main phase particle 11 in the element mapping image is 40% or more of the equivalent circle diameter of the main phase particle. In other words, the center is located in a part whose distance from the boundary between the main phase particle 11 and the grain boundary 13 is 40% or more of the equivalent circle diameter of the main phase particle. Then, the Zr concentration in the center of the main phase particle 11 is measured and defined as [Zr1]. The measurement targets of [Zr1] and [Zr2] are main phase particles 11 having a region that satisfies the definition of the center and a region that satisfies the definition of the outer edge portion described later.
[0123] When calculating [Zr1] in the RTB permanent magnet 1, the element mapping image is observed so that the number of main phase grains 11 that are entirely included and have a central portion is at least three or more. The number of main phase grains 11 that are entirely included and have a central portion may be five or more. Then, [Zr1] of each main phase grain 11 entirely included in the element mapping image may be measured and averaged to calculate [Zr1] in the RTB permanent magnet 1.
[0124] The method for measuring [Zr2] is the same as the method for measuring [Zr1], except that the measurement location of the Zr concentration is changed from the center of the main phase particle 11 to the outer edge of the main phase particle 11. Specifically, the outer edge of the main phase particle 11 is a portion that is 30% or less of the equivalent circle diameter of the main phase particle from the surface of the main phase particle 11 in the element mapping image. In other words, the outer edge is located at a position where the distance from the boundary between the main phase particle 11 and the grain boundary 13 is 30% or less of the equivalent circle diameter of the main phase particle. In order to avoid detecting grain boundary components when measuring [Zr2], a portion that is 15% to 30% of the equivalent circle diameter of the main phase particle from the surface of the main phase particle 11 may be measured.
[0125] [Zr1] / [Zr2] of each main phase particle 11 is calculated by measuring and calculating [Zr1] and [Zr2] of each main phase particle 11. [Zr1] / [Zr2] in the RTB permanent magnet 1 is calculated by dividing [Zr1] in the RTB permanent magnet 1 calculated by the above method by [Zr2] in the RTB permanent magnet 1 calculated by the above method.
[0126] The RTB permanent magnet 2 shown in FIG. 2 is sample No. 10, a comparative example described below. FIG. 4 is an enlarged image of portion B in FIG. 2. As shown in FIGS. 2 and 4, the RTB permanent magnet 2 shown in FIG. 2 has a higher Zr concentration in the main phase particles 11 than the RTB permanent magnet 1 shown in FIG. 1. In particular, the Zr concentration is high in the center of the main phase particles 11, and the distribution of the Zr concentration makes it appear that the main phase particles 11 are core-shell particles containing a shell with a low Zr concentration and a core with a high Zr concentration. In other words, the RTB permanent magnet 2 has low HcJ and Hk / HcJ because [Zr1] / [Zr2] is too large. EXAMPLES
[0127] The present invention will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples.
[0128] (Experimental Example 1) (Alloy preparation process) In the alloy preparation step, a main phase alloy, a grain boundary phase alloy, and an alloy for the single alloy method were finally prepared, each having the composition shown in Tables 1 to 3. TRE means the content of rare earth elements. The content of elements other than Fe that are not shown in Tables 1 to 3 is all less than 0.01 mass%. That is, in each of the examples and comparative examples shown in Tables 1 to 3, Fe is the substantial balance.
[0129] The composition of the RTB permanent magnet finally obtained in Experimental Example 1 was substantially the same except for the Zr content and the C content.
[0130] First, raw metals containing predetermined elements were prepared. The raw metals were prepared by appropriately selecting, for example, simple substances of the elements shown in Tables 1 to 3, alloys containing the elements shown in Tables 1 to 3, and / or compounds containing the elements shown in Tables 1 to 3.
[0131] Next, these raw metals were weighed and strip-cast to prepare main phase alloys, grain boundary phase alloys, and single alloy alloys. The carbon content of each alloy was controlled by changing the ratio of pig iron used in the raw metals.
[0132] (Crushing process) In the pulverization process, each alloy obtained in the preparation process was pulverized to obtain alloy powder. The pulverization was carried out in two stages: coarse pulverization and fine pulverization. Coarse pulverization was carried out by hydrogen absorption pulverization. After hydrogen was absorbed into each alloy, dehydrogenation was carried out at 300 to 600°C in an argon flow or in a vacuum. Through the coarse pulverization, alloy powder with a particle size of several hundred μm to several mm was obtained.
[0133] Fine pulverization was carried out by adding oleic acid amide as a grinding aid to the alloy powder obtained by coarse pulverization, mixing, and then using a jet mill. The amount of grinding aid added was determined so that the composition of the final magnet would be as shown in Table 4. Nitrogen gas was used in the jet mill. Fine pulverization was carried out until the D50 of the alloy powder reached approximately 3.0 μm.
[0134] (Mixing process) For each sample except for sample number 10, alloy powders obtained by pulverizing the main phase alloys of the types shown in Table 4 and alloy powders obtained by pulverizing the grain boundary phase alloys of the types shown in Table 4 were mixed in the mixing ratios shown in Table 4 to obtain alloy powders for molding. For sample number 10, alloy α after fine pulverization as shown in Table 4 was used as the alloy powder for molding.
[0135] (molding process) In the compacting process, the alloy powder obtained in the pulverizing and mixing processes was compacted in a magnetic field to obtain a compact. The alloy powder was filled into a die placed in an electromagnet, and then pressed and compacted while applying a magnetic field from the electromagnet. The strength of the applied magnetic field was 1200 kA / m. The pressure during compacting was 40 MPa.
[0136] (Sintering process) In the sintering step, the obtained molded body was sintered to obtain a sintered body. The holding temperature during sintering (sintering temperature) was 1080°C. The holding time during sintering (sintering time) was the time shown in Table 4. The heating rate when raising the temperature to the holding temperature was 8.0°C / min, and the cooling rate when cooling from the holding temperature to room temperature was 50°C / min. The sintering atmosphere was a vacuum atmosphere or an inert gas atmosphere.
[0137] (Aging process) In the aging step, the obtained sintered body was subjected to aging treatment to obtain an RTB permanent magnet. The aging treatment was carried out in two stages, a first aging treatment and a second aging treatment.
[0138] In the first aging treatment, the heating rate was 8.0°C / min when heating to the holding temperature, the holding temperature was 900°C, the holding time was 1.0 hour, and the cooling rate was 50°C / min when cooling from the holding temperature to room temperature. The atmosphere during the first aging treatment was an Ar atmosphere.
[0139] In the second aging treatment, the heating rate was 8.0°C / min when heating to the holding temperature, the holding temperature was 500°C, the holding time was 1.5 hours, and the cooling rate was 50°C / min when cooling from the holding temperature to room temperature. The atmosphere during the second aging treatment was an Ar atmosphere.
[0140] It was confirmed by composition analysis using X-ray fluorescence spectrometry, inductively coupled plasma mass spectrometry (ICP method), and gas analysis that the composition of the RTB permanent magnet finally obtained in each of the examples and comparative examples was the composition shown in Table 4. In particular, the C content was measured by oxygen flow combustion-infrared absorption method. Also, the B content was measured by ICP method.
[0141] (evaluation) (6-13-1 phase area ratio in main phase alloy) The cross sections of each main phase alloy shown in Table 1 were observed at a magnification of 2000x using a SEM (Hitachi High-Tech SU5000) with an accelerating voltage of 3.0 kV, with the contrast and brightness adjusted so that the main phase, R-rich phase, and 6-13-1 phase could be distinguished. The area of each phase was then analyzed, and the area of the 6-13-1 phase was divided by the area of the observed cross section to calculate the area ratio of the 6-13-1 phase. The results are shown in Table 1. In Experimental Example 1, the 6-13-1 phase was not observed in any main phase alloy other than Alloy A.
[0142] ([Zr1], [Zr2]) For the cross section of each magnet shown in Table 4, elemental mapping was performed in a range of 51.2 μm × 51.2 μm using an EPMA (JXA-8500F manufactured by JEOL) under conditions of an acceleration voltage of 15 kV, a probe current of 100 nA, and an analysis step of 0.20 nm / step. The positions and shapes of the main phase particles included in the obtained elemental mapping image were identified. It was confirmed that the number of main phase particles that were entirely included in the elemental mapping image and included an area that satisfied the definition of the center and an area that satisfied the definition of the outer edge was 50 or more. Then, for each main phase particle that was entirely included in the elemental mapping image and included an area that satisfied the definition of the center and an area that satisfied the definition of the outer edge, a measurement point was set at a portion where the distance from the surface of each main phase particle was 40% or more of the circle equivalent diameter of the main phase particle, and the Zr concentration was measured. The Zr concentration at each measurement point was averaged to calculate [Zr1] for each magnet. Note that, for the calculation of [Zr1] for each magnet, the Zr concentration was measured at one point per main phase particle.
[0143] Furthermore, for each main phase particle that was entirely included in the element mapping image and that included an area that satisfied the definition of the center and an area that satisfied the definition of the outer edge, the Zr concentration was measured by setting measurement points at a portion of the main phase particle whose distance from the surface was 30% or less of the equivalent circle diameter of that main phase particle. [Zr2] for each magnet was calculated by averaging the Zr concentrations at each measurement point. Furthermore, [Zr1] / [Zr2] for each magnet was calculated. The results are shown in Table 5. Note that when calculating [Zr2] for each magnet, the Zr concentration was measured at one point per main phase particle.
[0144] (S(C) / (S(B)+S(C))) The cross section of each magnet shown in Table 4 was observed at three locations at a magnification of 1500x using an SEM. For all SEM images obtained, ZrB2 and / or ZrC contained in the grain boundary phase was identified. The total area of ZrB2 was designated as S(B). The total area of ZrC was designated as S(C). S(C) / (S(B)+S(C)) was then calculated. The results are shown in Table 5. The presence of ZrB2 was not confirmed in any sample other than Samples No. 1 and 9.
[0145] The maximum particle size of the Zr compound was determined as the circle equivalent diameter of the largest Zr compound among the Zr compounds included in the SEM image. The results are shown in Table 5. In all the examples and comparative examples, no Zr compounds other than ZrB2 and ZrC were observed.
[0146] (Magnetic properties) The magnetic properties of the RTB permanent magnets of the examples and comparative examples were measured using a BH tracer. Specifically, Br, HcJ and Hk / HcJ were measured. The results are shown in Table 5.
[0147] In Experimental Examples 1 to 3, Br was deemed to be good when Br was 1330 mT or more. HcJ was deemed to be good when HcJ was 1850 kA / m or more. Hk / HcJ was deemed to be good when Hk / HcJ was 95.0% or more.
[0148] [Table 1]
[0149] [Table 2]
[0150] [Table 3]
[0151] [Table 4]
[0152] [Table 5]
[0153] The RTB permanent magnets of each Example had good Br, HcJ and Hk / HcJ.
[0154] Sample No.1 had too little carbon in the main phase alloy, which resulted in too small S(C) / (S(B)+S(C)) and reduced Br, HcJ and Hk / HcJ.
[0155] Sample No. 5 had too much carbon in the main phase alloy, which resulted in the final RTB permanent magnet having too much carbon, resulting in a decrease in HcJ.
[0156] The amount of Zr in the grain boundary phase alloy of sample No. 6 was too small. As a result, HcJ and Hk / HcJ decreased. The decrease in HcJ and H / HcJ is believed to be due to abnormal grain growth of the main phase grains.
[0157] Sample No. 9 had too much Zr in the grain boundary phase alloy, which resulted in too small S(C) / (S(B)+S(C)), and reduced Br and Hk / HcJ.
[0158] Although the composition of sample No. 10 was the same as that of sample No. 3, the [Zr1] was too large and the [Zr1] / [Zr2] was too large in the single alloy sample No. 10. As a result, HcJ and Hk / HcJ were decreased.
[0159] (Experimental Example 2) Except for the change in sintering time, the conditions were the same as for sample No. 3. The results are shown in Table 6.
[0160] [Table 6]
[0161] Even when the sintering time was changed, each example in which [Zr1], [Zr1] / [Zr2], and S(C) / (S(B)+S(C)) were within the specified ranges had good Br, HcJ, and Hk / HcJ.
[0162] (Experimental Example 3) Samples Nos. 16 and 17 were prepared by varying the mixing ratio of the main phase alloy and the grain boundary phase alloy from sample No. 3, and by varying the compositions of the main phase alloy and the grain boundary phase alloy so that the composition of the final RTB permanent magnet would be approximately the same as that of sample No. 3. The results are shown in Tables 7 to 10.
[0163] [Table 7]
[0164] [Table 8]
[0165] [Table 9]
[0166] [Table 10]
[0167] Even when the mixing ratio was changed, each Example in which [Zr1], [Zr1] / [Zr2], and S(C) / (S(B)+S(C)) were within the specified ranges had good Br, HcJ, and Hk / HcJ.
[0168] (Experimental Example 4) Hereinafter, Experimental Example 4 will be described, but the methods for producing the samples are the same as those of Experimental Example 1 unless otherwise specified.
[0169] (Alloy preparation process) In the alloy preparation step, main phase alloys, grain boundary phase alloys, and single alloy method alloys were prepared, each having the composition shown in Tables 11 to 13. TRE means the content of rare earth elements. The content of elements other than Fe that are not shown in Tables 11 to 13 is all less than 0.01 mass%. That is, in each of the examples and comparative examples shown in Tables 11 to 13, Fe is the substantial balance.
[0170] The composition of the RTB permanent magnet finally obtained in Experimental Example 4 was substantially the same except for the Zr content and the C content.
[0171] First, raw metals containing predetermined elements were prepared. For example, the raw metals were appropriately selected and prepared from simple elements listed in Tables 11 to 13, alloys containing the elements listed in Tables 11 to 13, and / or compounds containing the elements listed in Tables 11 to 13.
[0172] (Mixing process) For each sample except for sample number 28, an alloy powder for molding was obtained by mixing an alloy powder obtained by pulverizing a main phase alloy of the type shown in Table 14 and an alloy powder obtained by pulverizing a grain boundary phase alloy of the type shown in Table 14 in the mixing ratio shown in Table 14. For sample number 28, the alloy β after fine pulverization as shown in Table 14 was used as the alloy powder for molding.
[0173] (evaluation) (6-13-1 phase area ratio in main phase alloy) The cross section of each main phase alloy shown in Table 11 was observed at a magnification of 10,000 times using a SEM. The SEM images were then visually observed to identify whether each part was the main phase, a grain boundary phase other than the 6-13-1 phase, or the 6-13-1 phase. The area ratio of the 6-13-1 phase was then calculated. The results are shown in Table 11. In Experimental Example 4, the 6-13-1 phase was not observed in any of the main phase alloys other than Alloy J.
[0174] ([Zr1], [Zr2]) For the cross section of each magnet shown in Table 14, elemental mapping was performed in an area of 51.2 μm × 51.2 μm using an EPMA. The position and shape of the main phase particles included in the obtained elemental mapping image were identified. It was confirmed that the number of main phase particles that were entirely included in the elemental mapping image and had a circle equivalent diameter of more than 2.5 μm was 50 or more. Then, the Zr concentration was measured in a portion of each main phase particle that was entirely included in the elemental mapping image and was greater than 1.0 μm deep from the surface. [Zr1] for each magnet was calculated by averaging the Zr concentrations in the portions of each main phase particle that were greater than 1.0 μm deep from the surface. Note that, in calculating [Zr1] for each magnet, the Zr concentration was measured at one location per main phase particle.
[0175] Furthermore, for main phase particles that were entirely included in the element mapping image and had an equivalent circle diameter greater than 2.5 μm, measurement points were set at a depth of 0.3 μm from the surface, and Zr concentration was measured. [Zr2] for each magnet was calculated by averaging the Zr concentrations at each measurement point. Furthermore, [Zr1] / [Zr2] for each magnet was calculated. The results are shown in Table 15. Note that when calculating [Zr2] for each magnet, the Zr concentration was measured at one point per main phase particle.
[0176] (S(C) / (S(B)+S(C))) The cross section of each magnet shown in Table 14 was observed at three locations at a magnification of 1500x using an SEM. For all SEM images obtained, ZrB2 and / or ZrC contained in the grain boundary phase was identified. The total area of ZrB2 was designated as S(B). The total area of ZrC was designated as S(C). S(C) / (S(B)+S(C)) was then calculated. The results are shown in Table 5. Note that the presence of ZrB2 was not confirmed in any sample other than Samples No. 19 and 27.
[0177] The maximum particle size of the Zr compound was determined as the circle equivalent diameter of the largest Zr compound among the Zr compounds included in the SEM image. The results are shown in Table 15.
[0178] (Magnetic properties) The magnetic properties of the RTB permanent magnets of the examples and comparative examples were measured using a BH tracer. Specifically, Br, HcJ and Hk / HcJ were measured. The results are shown in Table 15.
[0179] In Experimental Examples 4 to 6, Br was deemed to be good when Br was 1350 mT or more. HcJ was deemed to be good when HcJ was 1730 kA / m or more. Hk / HcJ was deemed to be good when Hk / HcJ was 95.0% or more.
[0180] [Table 11]
[0181] [Table 12]
[0182] [Table 13]
[0183] [Table 14]
[0184] [Table 15]
[0185] The RTB permanent magnets of each Example had good Br, HcJ and Hk / HcJ.
[0186] Sample No. 19 had too little carbon in the main phase alloy, which resulted in too small S(C) / (S(B)+S(C)) and reduced Br, HcJ and Hk / HcJ.
[0187] Sample No. 23 had too much carbon in the main phase alloy, which resulted in the final RTB permanent magnet having too much carbon, resulting in a decrease in HcJ.
[0188] The amount of Zr in the grain boundary phase alloy of sample No. 24 was too small. As a result, HcJ and Hk / HcJ decreased. The decrease in HcJ and H / HcJ is believed to be due to abnormal grain growth of the main phase grains.
[0189] Sample No. 27 had too much Zr in the grain boundary phase alloy, which resulted in too small S(C) / (S(B)+S(C)), and reduced Br and Hk / HcJ.
[0190] Although the composition of sample No. 21 was the same, sample No. 28, which was made by the single alloy method, had too large [Zr1] and too large [Zr1] / [Zr2]. As a result, HcJ and Hk / HcJ were decreased.
[0191] (Experimental Example 5) Except for the change in sintering time, the same conditions as those for sample No. 21 were used. The results are shown in Table 16.
[0192] [Table 16]
[0193] Even when the sintering time was changed, each example in which [Zr1], [Zr1] / [Zr2], and S(C) / (S(B)+S(C)) were within the specified ranges had good Br, HcJ, and Hk / HcJ.
[0194] (Experimental Example 6) Samples Nos. 34 and 35 were prepared by varying the mixing ratio of the main phase alloy and the grain boundary phase alloy from sample No. 21, and by varying the composition of the main phase alloy and the grain boundary phase alloy so that the composition of the final RTB permanent magnet would be approximately the same as that of sample No. 21. The results are shown in Tables 17 to 20.
[0195] [Table 17]
[0196] [Table 18]
[0197] [Table 19]
[0198] [Table 20]
[0199] Even when the mixing ratio was changed, each Example in which [Zr1], [Zr1] / [Zr2], and S(C) / (S(B)+S(C)) were within the specified ranges had good Br, HcJ, and Hk / HcJ. [Explanation of symbols]
[0200] 1, 2...RTB permanent magnet 11...Main phase particles 13...Grain boundary 13a...R-containing part 13b...Zr-containing part 15...Zr compound
Claims
1. An R-T-B system permanent magnet containing C and Zr, the R-T-B system permanent magnet includes main phase grains and grain boundaries, In the cross section of the R-T-B system permanent magnet, The Zr concentration at the center of the main phase grain is [Zr1], and [Zr1] is 0 to 0.35 at%; ZrB contained in the grain boundary 2 is defined as the total area of ZrC contained in the grain boundaries, S(C) / (S(B)+S(C)) is 98.0% or more; The R-T-B system permanent magnet is taken as 100 mass %, The Zr content is 0.60 mass% or more and 1.60 mass% or less, The content of B is more than 0 mass% and 0.85 mass% or less, An R-T-B system permanent magnet having a C content of more than 0 mass % and 0.260 mass % or less.
2. An R-T-B system permanent magnet containing C and Zr, the R-T-B system permanent magnet includes main phase grains and grain boundaries, In the cross section of the R-T-B system permanent magnet, the Zr concentration at the center of the main phase particle is [Zr1] and the Zr concentration at the outer edge of the main phase particle is [Zr2], and the atomic ratio [Zr1] / [Zr2] is 0.70 or more and 1.20 or less, ZrB contained in the grain boundary 2 is defined as the total area of ZrC contained in the grain boundaries, S(C) / (S(B)+S(C)) is 98.0% or more; The R-T-B system permanent magnet is taken as 100 mass %, The Zr content is 0.60 mass% or more and 1.60 mass% or less, The content of B is more than 0 mass% and 0.85 mass% or less, An R-T-B system permanent magnet having a C content of more than 0 mass % and not more than 0.260 mass %.
3. ZrB in the R-T-B system permanent magnet 2 The R-T-B system permanent magnet according to claim 1 or 2, wherein the total area ratio of is 0% or more and less than 0.01%.
4. ZrB 2 3. The RTB system permanent magnet according to claim 1, wherein the grain size of is a maximum of 1.0 μm or less, and the grain size of ZrC is a maximum of 1.0 μm or less.
5. 3. The R-T-B system permanent magnet according to claim 1, wherein the content of heavy rare earth elements is from 0% by mass to 0.80% by mass.
6. Further containing Ga, 3. The RTB system permanent magnet according to claim 1, wherein the Ga content is from 0.40 mass % to 1.00 mass %.
7. Further containing Al, 3. The R-T-B system permanent magnet according to claim 1, wherein the Al content is greater than 0 mass % and is 0.07 mass % or less.
8. 3. The RTB system permanent magnet according to claim 1, wherein the rare earth element content is 29.00% by mass or more and 34.00% by mass or less.
9. 3. The R-T-B system permanent magnet according to claim 1, wherein the rare earth element content is from 30.00 mass % to 33.00 mass %, and the B content is from 0.70 mass % to 0.85 mass %.
10. providing a main phase alloy and a grain boundary phase alloy; mixing the main phase alloy with the grain boundary phase alloy; The content of C in the main phase alloy is 0.070% by mass or more and 0.180% by mass or less, The Zr content in the grain boundary phase alloy is 3.00% by mass or more and 7.00% by mass or less, A method for producing an R-T-B system permanent magnet, in which the mixing ratio of the main phase alloy and the grain boundary phase alloy is 85:15 to 92:8 by mass ratio.
11. In the main phase alloy, The content of rare earth elements is 30.00% by mass or more and 32.50% by mass or less, The Al content is 0 mass% or more and 0.10 mass% or less, The Ga content is 0.40 mass% or more and 1.20 mass% or less, The Cu content is 0.10 mass% or more and 1.00 mass% or less, The Co content is 0.50 mass% or more and 3.00 mass% or less, The Zr content is 0.10 mass% or more and 0.80 mass% or less, The content of B is 0.70 mass% or more and 1.00 mass% or less, In the grain boundary phase alloy, The content of rare earth elements is 30.00% by mass or more and 45.00% by mass or less, The Al content is 0 mass% or more and 1.00 mass% or less, The Ga content is 0% by mass or more and 8.00% by mass or less, The Cu content is 0 mass% or more and 5.00 mass% or less, The method for producing an R-T-B system permanent magnet according to claim 10, wherein the Co content is from 0% to 10.00% by mass.
12. The method for producing an RTB system permanent magnet according to claim 10 or 11, wherein the area ratio of the 6-13-1 phase in a cross section of the main phase alloy is 0% or more and less than 2.0%.
13. The method for producing an RTB system permanent magnet according to claim 10 or 11, further comprising a step of sintering the compact, the sintering time being from 2 hours to 8 hours.
14. In the R-T-B system permanent magnet, The content of rare earth elements is 30.00% by mass or more and 33.00% by mass or less, The B content is 0.70 mass% or more and 0.88 mass% or less, The content of Al is greater than 0 mass% and not more than 0.07 mass%; The Ga content is 0.40 mass% or more and 1.00 mass% or less, The method for producing an R-T-B system permanent magnet according to claim 10 or 11, wherein the Zr content is greater than 0.10 mass % and not more than 1.60 mass %.
Citation Information
Patent Citations
R-t-b based rare earth element permanent magnet and magnet composition
WO2004029997A1