Metal member-bonded body

The use of a silver ink composition with silver carboxylate, an amine compound, and formic acid forms a strong, conductive bond between metal members, overcoming the limitations of solder and conductive adhesives by achieving high bonding strength and temperature resistance.

JP2024159786AActive Publication Date: 2024-11-08TOPPAN HOLDINGS INC +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024135487
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-05-24
Filing Date
2024-08-14
Publication Date
2024-11-08
Estimated Expiration
2039-09-30

AI Technical Summary

Technical Problem

Conventional methods for joining metal members using solder or conductive adhesives face issues such as remelting at high temperatures, shifting of mounting positions, high electrical resistivity, and insufficient heat resistance, while silver ink compositions lack sufficient bonding strength.

Method used

A method involving a silver ink composition containing silver carboxylate, an amine compound, and formic acid is used to bond metal members by heating without solidification, followed by pressing and firing to form metallic silver, ensuring high bonding strength through a conductive joint.

Benefits of technology

The method achieves a die shear strength of 15 MPa or more, providing a strong and durable bond between metal members that withstands high temperatures without remelting, addressing the limitations of solder and conductive adhesives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159786000007
    Figure 2024159786000007
  • Figure 2024159786000008
    Figure 2024159786000008
  • Figure 2024159786000009
    Figure 2024159786000009
Patent Text Reader

Abstract

To provide a method for bonding metal members together with high strength via a conductive bonding part.SOLUTION: A metal member-bonded body is formed by bonding a first metal member and a second metal member via metallic silver, wherein: either or both of the first and second metal members are made of copper and form a composite with a non-metal member; when the first member is made of copper, the metal member-bonded body has, from the first member side to the metallic silver side, in this order, a layer whose main constituent element is silver and a layer whose main constituent elements are copper and oxygen; when the second member is made of copper, the metal member-bonded body has, from the second member side to the metallic silver side, in this order, a layer whose main constituent element is silver and a layer whose main constituent elements are copper and oxygen; and the non-metal member is a semiconductor wafer, a semiconductor chip, an organic insulating base material, an inorganic insulating base material, or an organic-inorganic composite insulating base material.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for joining metal members, a joined body of metal members, and a circuit board. [Background technology]

[0002] Conventionally, solder has been widely used to join metal members together, such as between electronic components and a substrate, or between circuits. However, because the melting point of solder is relatively low, there is a problem that when a module manufactured by solder mounting is further mounted on an electronic substrate, the solder remelts during reflow at a temperature of about 260°C, causing a shift in the mounting position. In addition, the operating temperature of a power semiconductor module can reach high temperatures of 200°C or more. Therefore, the same problem exists with power semiconductor modules manufactured by solder mounting.

[0003] One solution to the problems caused by remelting of solder is a conductive adhesive that contains metallic silver and a binder that is a resin component. However, because conductive adhesives contain binders, it is unavoidable that the electrical resistivity of joints made with conductive adhesives is high (usually 100 μΩ·cm or more), and there is also the problem that the heat resistance of these joints is insufficient.

[0004] Meanwhile, a silver ink composition containing silver β-ketocarboxylate has been disclosed as a material that exhibits excellent electrical conductivity when subjected to heat treatment (see Patent Document 1). This silver ink composition is a material that forms metallic silver from silver β-ketocarboxylate by heat treatment, and can form metallic silver with an extremely low volume resistivity of 10 μΩ·cm or less. Furthermore, the formed metallic silver does not remelt even if it is subsequently exposed to high temperatures such as 200°C or higher. Therefore, the above-mentioned problems caused by remelting of the solder can be solved. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2014-193991 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, because the silver ink composition does not contain a binder, when this silver ink composition is used to join metal components together, there is a problem in that it is difficult to increase the strength of the structure in which the metal components are joined together via metallic silver, i.e., the joining strength.

[0007] The present invention has been made in consideration of the above circumstances, and has an object to provide a method for joining metal members, which can join metal members with high strength via a conductive joint. [Means for solving the problem]

[0008] In order to solve the above-mentioned problems, the present invention provides a method for joining metal members, comprising the steps of: heating a silver ink composition adhering to the surface of either or both of a first metal member and a second metal member at a temperature of 60°C or higher without solidifying the silver ink composition to obtain a heated product of the silver ink composition; and baking the heated product while pressing the first member and the second member together with the heated product of the silver ink composition between them, thereby joining the first member and the second member with metallic silver, wherein the silver ink composition is a blend of a silver carboxylate having a group represented by the formula "-COOAg", an amine compound, and formic acid, and the silver ink composition is a material for forming metallic silver by baking it. In the method for joining metal components of the present invention, it is preferable that the silver ink composition before being heated at a temperature of 60°C or higher without solidifying contains metallic silver particles generated from the silver carboxylate, and that the crystallite diameter of the metallic silver particles is less than 20 nm. In the method for joining metal members of the present invention, the silver carboxylate is preferably a silver β-ketocarboxylate represented by the following general formula (1).

[0009] [ka] (In the formula, R represents an aliphatic hydrocarbon group having 1 to 20 carbon atoms, in which one or more hydrogen atoms may be substituted with a substituent, a phenyl group, a hydroxyl group, an amino group, or a group represented by the general formula "R 1 -CY 1 2-," "CY 1 3-," "R 1 -CHY 1 -," "R 2 O-," "R 5 R 4 N-", "(R 3 O)2CY 1 -" or "R 6 -C(=O)-CY 1 2-" is a group represented by; Y 1 are each independently a fluorine atom, a chlorine atom, a bromine atom, or a hydrogen atom; R 1 is an aliphatic hydrocarbon group having 1 to 19 carbon atoms or a phenyl group; R 2 is an aliphatic hydrocarbon group having 1 to 20 carbon atoms; R 3 is an aliphatic hydrocarbon group having 1 to 16 carbon atoms; R 4 and R 5 are each independently an aliphatic hydrocarbon group having 1 to 18 carbon atoms; R 6 is an aliphatic hydrocarbon group having 1 to 19 carbon atoms, a hydroxyl group, or a group represented by the formula "AgO-"; X 1 are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a phenyl group or a benzyl group in which one or more hydrogen atoms may be substituted with a substituent, a cyano group, an N-phthaloyl-3-aminopropyl group, a 2-ethoxyvinyl group, or a group represented by the general formula "R 7 O-," "R 7 S-", "R 7 -C(=O)-" or "R 7 -C(=O)-O-; R 7 is an aliphatic hydrocarbon group having 1 to 10 carbon atoms, a thienyl group, or a phenyl group or diphenyl group in which one or more hydrogen atoms may be substituted with a substituent.

[0010] The present invention also provides a joined body of metal members obtained by the method for joining metal members, wherein the joined body of metal members has a die shear strength of 15 MPa or more. The present invention also provides a circuit board comprising the above-mentioned metal member assembly on an organic substrate, the metal member being a metal electrode. The present invention also provides a joined metal member, the joined metal member being configured by joining a first metal member and a second metal member via metallic silver, one or both of the first and second members being made of copper, and when the first member is made of copper, the joined metal member has, between the first member and the metallic silver, a layer having silver as a main component element and a layer having copper and oxygen as main component elements, in this order, from the first member side toward the metallic silver side, and when the second member is made of copper, the joined metal member has, between the second member and the metallic silver, a layer having silver as a main component element and a layer having copper and oxygen as main component elements, in this order, from the second member side toward the metallic silver side, and the joined metal member has a die shear strength of 15 MPa or more. Effect of the Invention

[0011] According to the present invention, there is provided a method for joining metal members, which can join the metal members with high strength via a conductive joint. [Brief description of the drawings]

[0012] [Figure 1] 1 is a cross-sectional view for illustrating a schematic example of a method for joining metal members according to an embodiment of the present invention. [Diagram 2] 10 is a cross-sectional view for illustrating a schematic diagram of another example of a method for joining metal members according to one embodiment of the present invention. FIG. [Diagram 3] 11 is a cross-sectional view for illustrating a schematic diagram of yet another example of a method for joining metal members according to one embodiment of the present invention. FIG. [Figure 4] 11 is a cross-sectional view for illustrating a schematic diagram of yet another example of a method for joining metal members according to one embodiment of the present invention. FIG. [Diagram 5] 11 is a cross-sectional view for illustrating a schematic diagram of yet another example of a method for joining metal members according to one embodiment of the present invention. FIG. [Figure 6] 10 is a cross-sectional view for illustrating a schematic diagram of another example of the joining step in the method for joining metal members according to one embodiment of the present invention. FIG. [Figure 7] 10 is a cross-sectional view for illustrating a schematic diagram of yet another example of a joining step in the method for joining metal members according to one embodiment of the present invention. FIG. [Figure 8] 10 is a cross-sectional view for illustrating a schematic diagram of yet another example of a joining step in the method for joining metal members according to one embodiment of the present invention. FIG. [Figure 9] 1 shows imaging data obtained when a cross section of the metal member bonded body obtained in Example 1 was observed using a transmission electron microscope. [Figure 10] 1 shows imaging data obtained when a cross section of the joined metal members obtained in Example 1 was observed by energy dispersive X-ray spectroscopy, during detection of elemental silver. [Figure 11] 1 shows imaging data obtained when a cross section of the joined metal members obtained in Example 1 was observed by energy dispersive X-ray spectroscopy, at the time when copper element was detected. [Figure 12] 1 shows imaging data obtained when the cross section of the joined metal members obtained in Example 1 was observed by energy dispersive X-ray spectroscopy, at the time of detecting oxygen element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] <<Method of joining metal components>> A method for joining metal members according to one embodiment of the present invention is a method for joining metal members together, and includes the steps of: heating a silver ink composition attached to the surface of one or both of a first metal member (hereinafter sometimes simply referred to as "first member") and a second metal member (hereinafter sometimes simply referred to as "second member") at a temperature of 60° C. or higher without solidifying the silver ink composition to obtain a heated product of the silver ink composition (hereinafter sometimes referred to as a "pre-heating step"); and bonding the first member and the second member with metallic silver by baking the heated product while pressing the first member and the second member with the heated product of the silver ink composition interposed therebetween (hereinafter sometimes referred to as a "bonding step"). The silver ink composition is a combination of a silver carboxylate having a group represented by the formula "-COOAg" (hereinafter sometimes simply referred to as "silver carboxylate"), an amine compound, and formic acid, and the silver ink composition is a material for forming metallic silver by baking the heated product.

[0014] According to this embodiment, by performing the pre-heating step and the bonding step using a silver ink composition within the specific range described above, a metal member bonded body in which the first member and the second member are bonded with high bonding strength via metallic silver can be obtained. The method for joining metal members according to this embodiment will be described in detail below.

[0015] <Preheating process> In the pre-heating step, the silver ink composition adhering to the surface of either or both of the first member and the second member is heated at a temperature of 60°C or higher without solidifying, thereby obtaining a heated product of the silver ink composition. The silver ink composition used in this step is a material for forming metallic silver, and is a mixture of the silver carboxylate, an amine compound, and formic acid.

[0016] In this process, before the heating is started to obtain the heated product, i.e., before heating at a temperature of 60° C. or higher without solidifying, the silver ink composition typically contains particles of metallic silver generated from the silver carboxylate. This is because the formation of metallic silver from the silver carboxylate is promoted by the action of the formic acid.

[0017] In this embodiment, the crystallite size of the metallic silver particles is preferably less than 20 nm, more preferably 19 nm or less, and even more preferably 17 nm or less. When the crystallite size is less than (or equal to) the upper limit value, a joined metal member having higher joining strength can be obtained.

[0018] The lower limit of the crystallite size of the metallic silver particles is not particularly limited. For example, the crystallite size is preferably 3 nm or more, in order to facilitate preparation of a silver ink composition containing such metallic silver particles.

[0019] The crystallite size of the metallic silver particles can be appropriately adjusted within a range set by any combination of any of the above upper and lower limits. For example, in one embodiment, the crystallite size of the metallic silver particles may be any one of 3 nm or more and less than 20 nm, 3 to 19 nm, and 3 to 17 nm, although these are only examples of the crystallite size of the metallic silver particles.

[0020] The crystallite diameter of metallic silver particles can be obtained by a known method. For example, metallic silver particles are subjected to X-ray diffraction measurement, and the crystallite diameter can be calculated from the peak of the most intense crystal plane in the obtained X-ray diffraction profile by using Scherrer's formula "D=kλ / βcosθ (wherein D is crystallite diameter (nm); k is a constant (here, 0.9 is used); λ is the wavelength of X-ray (CuKα ray) 0.154 nm; β is peak half-width (rad); θ is 1 / 2 the angle of measurement angle)".

[0021] The first member is made of metal, and the metal that constitutes it may be either an elemental metal or an alloy. Preferred examples of the metal include copper, silver, gold, palladium, nickel, and alloys containing one or more selected from the group consisting of copper, silver, gold, palladium, and nickel. Among these, the metal is more preferably copper, silver, gold, palladium, or nickel, and even more preferably copper or silver.

[0022] In the preheating step, a metal member having a metal layer formed on its surface may be used as the member including the first member. The metal layer can be formed on the surface of the metal member by a known method such as vapor deposition or plating.

[0023] In such a metal member having a metal layer on its surface, the location to which the silver ink composition for forming a conductive joint described later is applied becomes the first member. For example, when the silver ink composition is applied only to the metal layer, the metal layer becomes the first member. When the silver ink composition is applied to both the metal member and the metal layer, both the metal member and the metal layer become the first member. When the silver ink composition is applied only to the metal member, the metal member becomes the first member.

[0024] A preferred example of such a metal member having a metal layer on its surface is a copper member having a silver layer on its surface, but this is just one example.

[0025] In the preheating step, a composite of a metal member and a non-metal member may be used as the member including the first member. Examples of the non-metallic member include a semiconductor wafer, a semiconductor chip, an organic insulating substrate, an inorganic insulating substrate, and an organic-inorganic composite insulating substrate, and these may be publicly known.

[0026] The semiconductor wafer or semiconductor chip may be, for example, a wafer or chip made of a semiconductor such as silicon, silicon carbide, or gallium nitride. Examples of the organic insulating substrate include a polytetrafluoroethylene (PTFE) substrate, a polyimide substrate, a liquid crystal polymer substrate, and a cycloolefin polymer substrate. The inorganic insulating substrate may be, for example, a ceramic substrate. The organic-inorganic composite insulating substrate is a substrate made of both organic and inorganic materials, and an example of such a substrate is a substrate made of glass epoxy resin.

[0027] Regardless of the type of non-metallic component, the composite can be produced, for example, by forming a metallic component at a desired location on the non-metallic component by vapor deposition, plating, sputtering, printing, or the like, or by joining the metallic component by brazing or bonding with an adhesive, or the like.

[0028] So far, the metal members have been mainly described as being provided on semiconductor wafers, semiconductor chips, organic insulating substrates, inorganic insulating substrates, or organic-inorganic composite insulating substrates, but metal members such as metal plates (e.g., heat sinks) that are not provided on these substrates are also suitable.

[0029] The shape of the first member is not particularly limited, and may be, for example, a sheet, plate, prism, pyramid, cylinder, cone, sphere, spheroid, rod, a shape that is a combination or fusion of two or more types selected from the group consisting of these nine types (i.e., sheet, plate, prism, pyramid, cylinder, cone, sphere, spheroid, and rod), or an amorphous shape.

[0030] The size of the first member is not particularly limited.

[0031] The shape and size of the first member can be appropriately selected depending on the application of the first member. For example, when the first member is plate-shaped or rod-shaped, the length of one side of the joining surface (first surface described later) of the first member may be any of 0.01 to 30 mm, 0.02 to 24 mm, and 0.03 to 18 mm, and the thickness of the first member may be any of 0.01 to 5 mm, 0.02 to 3 mm, and 0.03 to 1.5 mm. However, these are only examples of the shape and size of the first member. First members of these shapes and sizes are suitable, for example, as electrodes that constitute a circuit. When the shape of the first component is neither plate-like nor rod-like, the size of the first component can be adjusted, for example, so that the area of ​​the bonding surface is equivalent to the area of ​​the bonding surface calculated from the length of one side described above.

[0032] The second member is also made of metal. Examples of the metal constituting the second member include the same metals as those constituting the first member described above. The shape of the second member may be the same as that of the first member. The size of the second member may be similar to the size of the first member.

[0033] The second member can be used as a member including the second member in the same manner as the first member, and the member including the second member can be used in the same manner as the member including the first member described above.

[0034] The first member and the second member may be the same as each other or may be different from each other. For example, the first member and the second member to be joined in the joining step described below may be the same as each other or may be different from each other in terms of material, shape, and size.

[0035] In this embodiment, preferred examples of the first member and the second member include electrodes that form a circuit.

[0036] In the preheating step, either one or both of the first member and the second member are used with the silver ink composition attached to their surfaces. That is, in the preheating step, (A1) a combination of a first member having the silver ink composition attached to its surface and a second member having no silver ink composition attached to its surface (sometimes referred to as "combination (A1)" in this specification), (A2) a combination of a first member having no silver ink composition attached to its surface and a second member having the silver ink composition attached to its surface (sometimes referred to as "combination (A2)" in this specification), or (A3) a combination of a first member having the silver ink composition attached to its surface and a second member having the silver ink composition attached to its surface (sometimes referred to as "combination (A3)" in this specification) is used.

[0037] When combination (A3) is used, the silver ink composition adhered to the surface of the first member and the silver ink composition adhered to the surface of the second member may be the same as or different from each other.

[0038] The silver ink composition can be attached to the surface of the first member or the second member by a known method such as a printing method or a coating method.

[0039] Examples of the printing method include screen printing, flexographic printing, offset printing, dip printing, inkjet printing, dispenser printing, jet dispenser printing, gravure printing, gravure offset printing, and pad printing.

[0040] Examples of the coating method include a method using various coaters such as a spin coater, an air knife coater, a curtain coater, a die coater, a blade coater, a roll coater, a gate roll coater, a bar coater, a rod coater, and a gravure coater; a method using a wire bar; a method using a coating device such as a slot die; and a spray method.

[0041] It is preferable to perform a cleaning treatment to remove impurities from the portion of the surface of the first member or the second member to which the silver ink composition is to be applied before the silver ink composition is applied, thereby obtaining a metal member assembly having higher bonding strength.

[0042] The cleaning treatment can be carried out by a known method, and may be, for example, either a chemical treatment of the surface with a chemical agent or a physical treatment by surface processing. Examples of the chemical agent include acids such as nitric acid, phosphoric acid, sulfuric acid, and hydrochloric acid; and organic solvents such as acetone. Chemical treatment with an acid is useful for removing impurities in general. When an acid is used, it is preferable to further wash the acid-treated surface of the first member or the second member with water. Chemical treatment with an organic solvent is useful for removing impurities that are highly fat-soluble. The surface treatment may be, for example, a polishing treatment using an abrasive such as a file.

[0043] The reason for using the silver ink composition containing the silver carboxylate, the amine compound, and formic acid in the pre-heating step is that it has the following advantages. That is, among all silver ink compositions containing the silver carboxylate, the silver ink composition is advantageous in that the amount of the silver carboxylate is increased. In this case, since the silver ink composition has a high content of components derived from the silver carboxylate (e.g., silver carboxylate, metallic silver generated from the silver carboxylate, etc.) per unit amount, a larger amount of the heated object can be formed on the surfaces of the first member and the second member in a single application. Furthermore, since the silver ink composition has a high viscosity, it is easy to increase the amount of the silver ink composition attached to the surfaces of the first member and the second member. Therefore, in this respect as well, the silver ink composition can form a larger amount of the heated object on the surfaces of the first member and the second member in a single application. In this way, the silver ink composition is advantageous in that it can easily increase the amount of the heated product formed on the surfaces of the first member and the second member.

[0044] In addition, the first and second members to which the silver ink composition is applied are made of metal, and metal oxides are easily generated on their surfaces by oxidation. When such metal oxides are generated in a film or non-film form, not only does the resistivity of the metal member assembly increase, but the bonding strength of the metal member assembly also decreases. In contrast, the formic acid contained in the silver ink composition has a reducing effect, and the silver ink composition itself has good reducing properties, so the silver ink composition is advantageous in that it can reduce the amount of metal oxide on the surfaces of the first member and the second member.

[0045] In addition, the reducing action of the compound having a formyl group is more activated under basic conditions. The silver ink composition is basic due to the influence of the amine compound contained therein, and the reducing action of the formic acid having a formyl group is more activated. Therefore, the silver ink composition is advantageous in that the above-mentioned effect of using formic acid is more pronounced.

[0046] The amount of the silver ink composition attached to the surface of the first member or the second member is not particularly limited, and may be set appropriately taking into consideration the desired thickness of the conductive joint.

[0047] The thickness of the heated silver ink composition on the surface of the first member or the second member is preferably 100 μm or more, more preferably 200 μm or more, and even more preferably 250 μm or more. When the thickness of the heated product is equal to or greater than the lower limit, a joined body of metal members having higher joining strength can be obtained.

[0048] There is no particular upper limit to the thickness of the heated silver ink composition on the surface of the first member or the second member. In order to avoid an excessive thickness, the thickness of the heated product is preferably 1000 μm or less.

[0049] The thickness of the heated object can be appropriately adjusted within a range set by any combination of any of the lower limit values ​​and upper limit values ​​described above. For example, in one embodiment, the thickness of the heated object may be any one of 100 to 1000 μm, 200 to 1000 μm, and 250 to 1000 μm, however, these are only examples of the thickness of the heated object.

[0050] In the pre-heating step, the heated silver ink composition may have one layer or two or more layers. If it has two or more layers, the combination and ratio of the layers can be adjusted as desired depending on the purpose. When the heated product of the silver ink composition has two or more layers, the total thickness of the layers should be adjusted to the above-mentioned preferred thickness of the heated product.

[0051] For example, depending on the type of silver ink composition or the method of applying the silver ink composition, the amount of the silver ink composition applied may not be the desired amount by performing the operation of applying the silver ink composition only once. In such cases, it is necessary to repeat the operation of applying the silver ink composition two or more times. In such cases, the finally obtained heated product may have one layer or two or more layers. Also, for example, depending on the purpose, it may be necessary to form a conductive joint composed of two or more layers with different compositions. In that case, the operation of applying different types of silver ink compositions needs to be performed two or more times in total. In this case, the finally obtained heated product has two or more layers. In this embodiment, the heated object having two or more layers can be treated in the same manner as the heated object having one layer, regardless of the type.

[0052] In the above-described method, the operation of adhering the silver ink composition to either the first member or the second member is repeated two or more times. However, as explained above, even when a combination of a first member having a silver ink composition adhered to its surface and a second member having a silver ink composition adhered to its surface (i.e., the above-described combination (A3)) is used, a similar conductive joint composed of two or more layers can ultimately be formed.

[0053] In the pre-heating step, it is preferable to directly heat the portions of the first member to which the silver ink composition is attached and the second member to which the silver ink composition is attached, which further enhances the effect of suppressing unintended deterioration of the silver ink composition.

[0054] In the pre-heating step, the silver ink composition can be heated by a known method, such as heating in an electric furnace, heating with a thermal head of a thermal type, heating by far-infrared radiation, heating by spraying high-temperature gas, heating by high-frequency radiation, or dielectric heating.

[0055] In the pre-heating step, in any of the combinations (A1) to (A3), the silver ink composition adhering to the surface of the first member and the silver ink composition adhering to the surface of the second member are heated at a temperature of 60° C. or higher. However, at this time, the silver ink composition is not solidified by heating. The heated silver ink composition obtained in this step without solidifying maintains its fluidity.

[0056] In the pre-heating step, the temperature of the silver ink composition at the start of heating may be, for example, room temperature. In this specification, "room temperature" refers to a temperature that is neither particularly cooled nor heated, that is, an ordinary temperature, and examples thereof include temperatures of 15 to 25°C.

[0057] The heating temperature of the silver ink composition in the preheating step may be, for example, any one of 70° C. or more, 80° C. or more, and 90° C. or more.

[0058] The upper limit of the heating temperature of the silver ink composition in the preheating step is not particularly limited. For example, the heating temperature is preferably 120° C. or less in order to easily avoid solidification of the silver ink composition.

[0059] The heating temperature of the silver ink composition in the preheating step can be adjusted as appropriate within a range set by any combination of any of the lower limit values ​​and upper limit values ​​described above. For example, in one embodiment, the heating temperature may be any of 60 to 120° C., 70 to 120° C., 80 to 120° C., and 90 to 120° C. However, these are just examples of the heating temperature.

[0060] In the pre-heating step, the temperature rise rate during heating of the silver ink composition is not particularly limited, but is preferably 5 to 50° C. / min, more preferably 5 to 30° C. / min, and even more preferably 5 to 16° C. / min.

[0061] In the pre-heating step, the heating time of the silver ink composition is not particularly limited, but is preferably 1 minute to 12 hours, more preferably 2 minutes to 6 hours, and even more preferably 4 minutes to 1 hour.

[0062] The preheating step may be carried out under normal pressure, reduced pressure, or increased pressure. The preheating step may be carried out, for example, in either an air atmosphere or an inert gas atmosphere, such as nitrogen gas, argon gas, or helium gas. When the preheating step is performed under conditions that can suppress an oxidation reaction of the first member, the second member, the silver ink composition, and the heated product, the preheating step is preferably performed under reduced pressure or in an inert gas atmosphere. For example, the preheating step is preferably performed under an inert gas atmosphere in terms of a high effect of suppressing an oxidation reaction, and is preferably performed under reduced pressure in terms of low cost.

[0063] In the pre-heating step, the temperature of the silver ink composition may be consistently increased until the end of the pre-heating step (in other words, the temperature does not have to be kept constant or decreased), or a period during which the temperature is kept constant may be set, or a period during which the temperature is decreased may be set. In particular, from the viewpoint of obtaining a metal member bonded body having higher bonding strength, it is preferable to always increase or keep the temperature of the silver ink composition constant (in other words, not decrease it at all) from the start to the end of the preheating step, and for example, the temperature of the silver ink composition may be consistently increased from the start of the preheating step, and then the maximum temperature reached there may be maintained for a certain period of time until the end of the preheating step. In this case, the time for which the temperature of the silver ink composition is maintained for a certain period of time is preferably 0.5 to 10 minutes, more preferably 0.5 to 6 minutes, and even more preferably 0.5 to 3 minutes.

[0064] In the pre-heating step, bubbling is typically observed in the silver ink composition until a heated product of the silver ink composition is obtained. This is because the reaction of the components in the silver ink composition progresses, gas is generated, and this gas escapes. Typically, by the end of this step, this bubbling disappears and gas generation stops almost or completely. Because foaming of the silver ink composition occurs in this manner, the mass of the heated silver ink composition at the end of this process is smaller than the mass of the silver ink composition at the start of this process. In other words, a decrease in the mass of the silver ink composition is observed in this process.

[0065] In this embodiment, (B1) after completion of the preheating step, the first member and the second member may be brought into contact with each other via the heated object (the first member, the heated object, and the second member may be laminated) (this may be referred to herein as a "preheating method (B1)"), (B2) the first member and the second member may be brought into contact with each other via the silver ink composition (after the first member, the silver ink composition, and the second member are laminated) and then the preheating step may be performed (this may be referred to herein as a "preheating method (B2)"), or (B3) during the preheating step, the first member and the second member may be brought into contact with each other via the silver ink composition being heated (the first member, the silver ink composition being heated, and the second member may be laminated) (this may be referred to herein as a "preheating method (B3)"), and the timing of laminating (laminating) the first member and the second member may be selected arbitrarily.

[0066] Among these, in terms of obtaining a joined body of metal members having higher joining strength, it is preferable to adopt the preheating method (B1) or (B3), and it is more preferable to adopt the preheating method (B1).

[0067] When combination (A1) is selected in the pre-heating step, a second member is brought into contact with the silver ink composition adhered to the surface of the first member before heating, the silver ink composition being heated, or the silver ink composition after heating (i.e., the heated object). When combination (A2) is selected in the pre-heating step, the first member is brought into contact with the silver ink composition before heating, the silver ink composition during heating, or the silver ink composition after heating (i.e., the heated object) that is adhered to the surface of the second member. When combination (A3) is selected in the pre-heating step, the silver ink composition before heating, the silver ink composition during heating, or the silver ink composition after heating that is adhered to the surface of the first member (i.e., the heated object) is contacted with the silver ink composition before heating, the silver ink composition during heating, or the silver ink composition after heating that is adhered to the surface of the second member (i.e., the heated object). In either case, the silver ink composition attached to the first member or the second member forms a conductive joint that joins the first member and the second member in a later step.

[0068] In this embodiment, the bonding strength of the conductive bonding portion is significantly increased by forming the heated object in the preheating step. The reason for such an excellent effect is unclear, but it is speculated that the heated object obtained by heating the silver ink composition without solidifying it has fluidity, unlike the case where the silver ink composition is solidified, and the adhesion between the heated object and the first member and the adhesion between the heated object and the second member are improved. In addition, as described above, bubbling is typically observed in the silver ink composition until the heated object is obtained, but this bubbling disappears by the end of this step, and further, since the heated object is not solidified, the roughness of the surface of the heated object caused by bubbling is reduced, and the contact area between the heated object and the first member and the contact area between the heated object and the second member are increased.

[0069] The heated product obtained in the pre-heating step typically does not have the luster specific to metallic silver, and is, for example, dark green in color. This external appearance characteristic also indicates that the heated product is not mainly made of high-purity metallic silver.

[0070] <Joining process> After the pre-heating step, in the bonding step, the first member and the second member are pressed together with the heated material of the silver ink composition therebetween, and the heated material is fired, thereby bonding the first member and the second member with metallic silver. The silver ink composition is a material for forming metallic silver, and in this step, the silver ink composition is solidified by baking to finally form metallic silver, which bonds the first member and the second member.

[0071] In the joining process, the first member and the second member can be pressure-bonded to a composite body in which a first member, the heated object, and the second member are stacked in this order by applying either or both of pressure in a direction from the first member to the second member and pressure in a direction from the second member to the first member.

[0072] When pressure is applied to the composite in a direction from the first member to the second member, it is preferable to apply the pressure in this direction with the second member fixed. When pressure is applied to the composite in a direction from the second member to the first member, it is preferable to apply the pressure in this direction while the first member is fixed.

[0073] The pressure in the two directions described above may be applied by a known method. For example, when applying pressure in only one of the two directions mentioned above, the composite can be fixed on a horizontal plane with one of the surfaces of the first member and the second member facing vertically downward, and the other surface of the first member and the second member facing vertically upward and a weight can be placed on it, thereby applying pressure to the composite from only one direction. Here, a case has been described in which pressure is applied to either the first member or the second member by placing a weight on it, but pressure may be applied by other pressing means. Further, although the above description has been given of the case where the composite is arranged with the surfaces of the first and second components facing in the vertical direction, the composite may be arranged facing in other directions, including the horizontal direction, instead of the vertical direction.

[0074] In the joining step, the pressure when the first member and the second member are pressed together with the heated object therebetween (sometimes abbreviated as "pressure" in this specification) is not particularly limited, but is preferably 0.2 MPa or more, more preferably 0.4 MPa or more, and even more preferably 0.6 MPa or more. By setting the pressure to be equal to or greater than the lower limit, a metal member joined body having higher joining strength can be obtained.

[0075] In the bonding step, the upper limit of the pressure is not particularly limited, but in terms of facilitating bonding, the pressure is preferably 3 MPa or less.

[0076] In the bonding step, the pressure can be appropriately adjusted within a range set by any combination of any of the lower limit values ​​and upper limit values ​​described above. For example, in one embodiment, the compression pressure may be any one of 0.2 to 3 MPa, 0.4 to 3 MPa, and 0.6 to 3 MPa, although these are only examples of the compression pressure.

[0077] In the bonding step, the pressure may be constant from the start of bonding to the end of bonding, or may not be constant. When the compression pressure is not constant, the compression pressure may be consistently increased (in other words, the compression pressure may neither be changed nor decreased), or a period during which the compression pressure is not changed may be set, or a period during which the compression pressure is decreased may be set. Among these, it is preferable that the compression pressure is always increased or not changed (in other words, not decreased at all).

[0078] In the bonding step, the heated object is fired to form metallic silver. The baking of the heated object in the bonding step can be carried out by further heating the heated object. The heating at this time can be carried out in the same manner as the heating performed on the silver ink composition in the pre-heating step.

[0079] In the bonding step, the temperature at the start of firing the heated object may be lower than the temperature at the end of the preheating step, for example, room temperature, but is preferably equal to or higher than the temperature at the end of the preheating step.

[0080] The baking temperature of the heated object in the bonding step may be, for example, any one of 170° C. or higher, 220° C. or higher, and 270° C. or higher.

[0081] The upper limit of the baking temperature of the heated object in the bonding step is not particularly limited. For example, in terms of shortening the process time and avoiding excessively high temperatures, the baking temperature is preferably 350° C. or less, and more preferably 320° C. or less. The reason why the baking temperature can be set relatively low in this manner is that the silver ink composition uses ingredients within a relatively limited range.

[0082] The firing temperature of the heated object in the bonding step can be appropriately adjusted within a range set by any combination of any of the lower limit values ​​and any of the upper limit values ​​described above. For example, in one embodiment, the firing temperature may be any one of 170 to 350°C, 220 to 350°C, and 270 to 350°C. In one embodiment, the firing temperature may be any one of 170 to 320°C, 220 to 320°C, and 270 to 320°C. However, these are just examples of the firing temperatures.

[0083] In the bonding step, the heating rate during firing of the heated object is not particularly limited, but is preferably 5 to 50° C. / min, more preferably 5 to 45° C. / min, and even more preferably 5 to 40° C. / min.

[0084] In the bonding step, the baking time of the heated objects is not particularly limited, but is preferably 1 minute to 24 hours, more preferably 5 minutes to 12 hours, and further preferably 10 minutes to 2 hours.

[0085] In the bonding process, the firing temperature of the heated object may be consistently increased until the end of the process (in other words, it does not have to be kept constant or decreased), or a period of time during which the temperature is kept constant may be set, or a period of time during which the temperature is decreased may be set. In particular, it is preferable that the firing temperature of the heated object is always increased or kept constant (in other words, not lowered at all) from the start to the end of the bonding process, and for example, the firing temperature of the heated object may be consistently increased from the start of the bonding process, and then the maximum temperature reached there may be held for a certain period of time until the end of the bonding process. In this case, the time for holding the firing temperature of the heated object for a certain period of time is preferably 5 to 60 minutes, more preferably 10 to 50 minutes, and even more preferably 15 to 40 minutes.

[0086] The bonding step may be carried out under normal pressure, reduced pressure, or increased pressure. The bonding step may be performed in, for example, either an air atmosphere or an inert gas atmosphere, such as nitrogen gas, argon gas, or helium gas. When the bonding step is performed under conditions that can suppress the oxidation reaction of the first member, the second member, and the fired product (i.e., metallic silver), it is preferable to perform the bonding step under reduced pressure or in an inert gas atmosphere. For example, the bonding step is preferably performed under an inert gas atmosphere in terms of a high effect of suppressing the oxidation reaction, and is preferably performed under reduced pressure in terms of low cost.

[0087] The thickness of the conductive joint (in other words, metallic silver) formed by firing the heated material is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 25 μm or more. When the thickness of the conductive joint is equal to or more than the lower limit, the bonding strength of the metal member joint is increased. Furthermore, a conductive joint having a thickness of 20 μm or more is easier to form. In this specification, the "thickness of the conductive joint" means the "thickness of the conductive joint in the joining direction between the first member and the second member".

[0088] The upper limit of the thickness of the conductive joint is not particularly limited, but in order to avoid an excessive thickness, the thickness of the conductive joint is preferably 100 μm or less.

[0089] The thickness of the conductive joint can be appropriately adjusted within a range set by any combination of any of the lower limit values ​​and upper limit values ​​described above. For example, in one embodiment, the thickness of the conductive joint may be any one of 10 to 100 μm, 20 to 100 μm, and 25 to 100 μm, although these are only examples of the thickness of the conductive joint.

[0090] The thickness of the conductive joint is determined, for example, by the thickness of the heated object before firing. Typically, the thickness of the conductive joint can be preferably 4 to 16%, more preferably 6 to 14%, and even more preferably 8 to 12% of the thickness of the heated object before firing, although these are only examples of the relationship between the thickness of the conductive joint and the thickness of the heated object before firing.

[0091] In this embodiment, (C1) the firing of the heated product may be started after starting the compression of the first member and the second member (sometimes referred to in this specification as the "compression firing method (C1)"); (C2) the compression of the first member and the second member may be started after starting the firing of the heated product (sometimes referred to in this specification as the "compression firing method (C2)"); or (C3) the compression of the first member and the second member and the firing of the heated product may be started simultaneously (sometimes referred to in this specification as the "compression firing method (C3)"); and the timing of the start of the above-mentioned compression and firing can be selected arbitrarily.

[0092] Among these, in terms of obtaining a metal member joined body having higher joining strength, it is preferable to adopt the compression bonding and sintering method (C1) or (C3), and it is more preferable to adopt the compression bonding and sintering method (C1).

[0093] In the bonding process, the bonding strength of the conductive bonded portion is significantly increased by the pressure bonding between the first member and the second member with the heated object interposed therebetween. It is completely unexpected that the bonding strength is increased in such a manner in the conductive bonded portion that does not contain a resin component such as a binder, unlike the conventional case. The reason for such an excellent effect is not clear, but it is speculated that the laminated structure of the first member, the heated object being baked, and the second member is pressure bonded to each other in the thickness direction, so that the volume of the voids in the heated object being baked is reduced and the density is increased, and as a result, the strength of the baked object (conductive bonded portion) is improved.

[0094] The strength of the conductive joint of the metal member joint obtained in this embodiment can be evaluated, for example, by the measured value of die shear strength. The die shear strength can be measured in accordance with JIS C62137-1-2:2010 (horizontal shear strength test, IEC 62137-1-2:2007). That is, in a metal member assembly, one of the first member and the second member joined by the conductive joint is fixed, and a force is applied to the other member in a direction perpendicular to the stacking direction of the first member, the conductive joint, and the second member (in other words, a direction parallel to the stacking plane of these members), and the force applied when the stacked structure of these members (the first member, the conductive joint, and the second member) is broken is adopted as the die shear strength.

[0095] In this embodiment, the die shear strength of the joined metal members is preferably 15 MPa or more, and may be, for example, any one of 22.5 MPa or more, 27.5 MPa or more, and 32.5 MPa or more.

[0096] In the present embodiment, there is no particular upper limit to the die shear strength of the joined metal members. For example, in terms of ease of production of the joined metal members, the die shear strength is preferably 50 MPa or less.

[0097] The die shear strength can be appropriately adjusted within a range set by any combination of any of the above-mentioned lower limit values ​​and upper limit values. For example, in one embodiment, the die shear strength may be any one of 15 to 50 MPa, 22.5 to 50 MPa, 27.5 to 50 MPa, and 32.5 to 50 MPa, although these are just examples of the die shear strength.

[0098] <Other processes> The method for joining metal members of this embodiment may include other processes that do not fall under either the preheating process or the joining process, as long as the effects of the present invention are not impaired. The other steps are not particularly limited and can be arbitrarily selected depending on the purpose. The timing of performing the other steps can also be selected arbitrarily depending on the purpose, and may be, for example, before the preheating step, between the preheating step and the bonding step, or after the bonding step.

[0099] <Examples of joining methods for metal components> FIG. 1 is a cross-sectional view for illustrating a schematic example of a method for joining metal members according to an embodiment of the present invention. In addition, the figures used in the following explanation may show key parts enlarged for convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may not necessarily be the same as the actual ones.

[0100] FIG. 1 is a cross-sectional view for illustrating a method for joining metal members (sometimes referred to in this specification as "joining method (1-1)") when combination (A1) and preheating method (B1) are selected. That is, in the preheating step of the bonding method (1-1), a combination of a first member 11 having a silver ink composition 130 attached to its surface and a second member 12 having no silver ink composition attached to its surface is used, as shown in Fig. 1(a). The silver ink composition 130 is attached to one surface 11a of the first member 11 (sometimes referred to as the "first surface" in this specification).

[0101] In the pre-heating step of the bonding method (1-1), the silver ink composition 130 adhering to the first surface 11a of the first member 11 is heated at a temperature of 60°C or higher without solidifying it, thereby obtaining a heated product 130' of the silver ink composition 130, as shown in Figure 1(b).

[0102] Next, in the bonding step of the bonding method (1-1), as shown in Fig. 1(c), the heated object 130' of the silver ink composition is interposed between the first member 11 and the second member 12, and the heated object 130' is baked while the first member 11 and the second member 12 are pressure-bonded together. At this time, the force applied to pressure-bond the laminated structure of the first member 11, the heated object 130', and the second member 12 can be either or both of force P1 and force P2. At this time, the surface 12a of the second member 12 facing the first member 11 (sometimes referred to as the "first surface" in this specification) comes into contact with the heated object 130'.

[0103] By carrying out the pre-heating process and the joining process in this manner, a metal member joined body 1 is obtained in which a first member 11 and a second member 12 are joined via metallic silver (in other words, a conductive joining portion) 13, as shown in FIG. 1(d).

[0104] FIG. 2 is a cross-sectional view for illustrating a schematic diagram of another example of the method for joining metal members according to one embodiment of the present invention. In FIG. 2 and subsequent figures, the same components as those shown in the figures already described are given the same reference numerals as in the figures already described, and detailed description thereof will be omitted.

[0105] FIG. 2 is a cross-sectional view for illustrating a method for joining metal members (sometimes referred to as "joining method (2-1)" in this specification) when combination (A2) and preheating method (B1) are selected. That is, in the preheating step of the bonding method (2-1), a combination of a first member 11 having no silver ink composition attached to its surface and a second member 12 having a silver ink composition 130 attached to its surface is used, as shown in Fig. 2(a). The silver ink composition 130 is attached to a first surface 12a of the second member 12.

[0106] In the pre-heating step of the bonding method (2-1), the silver ink composition 130 adhering to the first surface 12a of the second member 12 is heated at a temperature of 60°C or higher without solidifying it, thereby obtaining a heated product 130' of the silver ink composition 130, as shown in Figure 2(b).

[0107] Next, in the bonding step of the bonding method (2-1), as shown in Fig. 2(c), the heated object 130' of the silver ink composition is placed between the first member 11 and the second member 12 and the heated object 130' is baked while the first member 11 and the second member 12 are pressure-bonded together with the heated object 130'. At this time, the surface of the first member 11 facing the second member 12, i.e., the first surface 11a, comes into contact with the heated object 130'. After forming a laminated structure of the first member 11, the heated object 130', and the second member 12, this process can be performed in the same manner as the bonding method (1-1) described with reference to Figure 1.

[0108] By carrying out the pre-heating process and the joining process in this manner, a metal member joined body 1 is obtained in which a first member 11 and a second member 12 are joined via metallic silver (in other words, a conductive joining portion) 13, as shown in FIG. 2(d).

[0109] FIG. 3 is a cross-sectional view for illustrating a schematic diagram of still another example of the method for joining metal members according to one embodiment of the present invention. FIG. 3 is a cross-sectional view for illustrating a method for joining metal members (sometimes referred to in this specification as "joining method (3-1)") when combination (A3) and preheating method (B1) are selected. That is, in the preheating step of the bonding method (3-1), as shown in Fig. 3(a), a combination of a first member 11 having a silver ink composition 130 attached to its surface and a second member 12 having a silver ink composition 130 attached to its surface is used. The silver ink composition 130 is attached to both the first surface 11a of the first member 11 and the first surface 12a of the second member 12. These silver ink compositions 130, 130 may be the same as or different from each other.

[0110] In the pre-heating step of the bonding method (3-1), the silver ink composition 130 adhering to the first surface 11a of the first member 11 and the silver ink composition 130 adhering to the first surface 12a of the second member 12 are both heated at a temperature of 60°C or higher without solidifying them, thereby obtaining heated products 130' of the silver ink compositions 130, as shown in Figure 3(b).

[0111] Next, in the bonding step of the bonding method (3-1), as shown in Fig. 3(c), the first member 11 and the second member 12 are pressed together with two layers of heated objects 130', 130' of silver ink composition therebetween, and the heated objects 130', 130' are baked. At this time, the heated object 130' on the first surface 11a of the first member 11 and the heated object 130' on the first surface 12a of the second member 12 come into contact with each other. In this process, after forming such a laminated structure of the first member 11, the two layers of the heated object 130', and the second member 12, the laminated structure is subjected to pressure bonding, and the laminated structure is then subjected to pressure bonding in the same manner as in the bonding method (1-1) described with reference to FIG.

[0112] By carrying out the pre-heating process and the bonding process in this manner, a metal member bonded body 2 is obtained in which the first member 11 and the second member 12 are bonded via two layers of metallic silver (layers) 13, in other words, conductive bonding portions 23, as shown in FIG. 3(d).

[0113] Here, for convenience, the conductive joint 23 in the metal member joint 2 is shown to be composed of two layers. In the joining method (3-1), when the silver ink composition 130 initially attached to the first member 11 and the silver ink composition 130 initially attached to the second member 12 are different in type from each other, the conductive joint 23 is composed of such two layers. On the other hand, when the silver ink composition 130 initially attached to the first member 11 and the silver ink composition 130 initially attached to the second member 12 are the same in type from each other, the conductive joint 23 may be composed of such two layers or may be a conductive joint of one layer (for example, a conductive joint similar to the conductive joint 13 shown in FIG. 1 and FIG. 2).

[0114] So far, we have explained the method for joining metal members when preheating method (B1) is selected in the preheating step, but in the above-mentioned manufacturing method, preheating method (B2) or (B3) can also be selected.

[0115] FIG. 4 is a cross-sectional view for illustrating a schematic diagram of a method for joining metal members (sometimes referred to as "joining method (1-2)" in this specification) when combination (A1) and preheating method (B2) are selected. That is, in the pre-heating step of the bonding method (1-2), similarly to the bonding method (1-1), a combination of a first member 11 having a silver ink composition 130 adhered to its surface and a second member 12 having no silver ink composition adhered to its surface, as shown in FIG. 1(a), is used.

[0116] In the preheating step of the bonding method (1-2), the first member 11 and the second member 12 are then brought into contact with each other via the silver ink composition 130 adhering to the first surface 11a of the first member 11, as shown in Fig. 4(b). After the first member 11, the silver ink composition 130, and the second member 12 are thus stacked, the silver ink composition 130 is heated at a temperature of 60°C or higher without solidifying, thereby obtaining a heated product 130' of the silver ink composition 130, as shown in Fig. 4(c). As a result, a laminated structure of the first member 11, the heated product 130', and the second member 12 in the same state as that shown in Fig. 1(c) is obtained.

[0117] Next, in the bonding process of bonding method (1-2), as shown in FIG. 4(c), the first member 11 and the second member 12 are pressed together with a heated object 130' of a silver ink composition therebetween, while the heated object 130' is baked in the same manner as in bonding method (1-1).

[0118] By carrying out the pre-heating process and the joining process in this manner, a metal member joined body 1 is obtained in which a first member 11 and a second member 12 are joined via metallic silver (in other words, a conductive joining portion) 13, as shown in FIG. 4(d).

[0119] FIG. 5 is a cross-sectional view for illustrating a method for joining metal members when the combination (A1) and preheating method (B3) are selected (sometimes referred to in this specification as "joining method (1-3)"). That is, in the pre-heating step of the bonding method (1-3), similarly to the bonding method (1-1), a combination of a first member 11 having a silver ink composition 130 adhered to its surface and a second member 12 having no silver ink composition adhered to its surface, as shown in FIG. 5(a), is used.

[0120] In the pre-heating step of the bonding method (1-3), heating is started as shown in Fig. 5(b) so as not to solidify the silver ink composition 130 adhering to the first surface 11a of the first member 11 at a temperature of 60°C or higher. Here, the silver ink composition in the middle of the heating process before becoming the heated object 130' is denoted by reference symbol 1301.

[0121] Next, in the pre-heating step of the bonding method (1-3), the first member 11 and the second member 12 are brought into contact with each other through the heated silver ink composition 1301 during this step, as shown in Fig. 5(c) . The temperature of the heated silver ink composition 1301 when they are brought into contact in this manner may be less than 60°C or may be 60°C or higher.

[0122] Next, in the pre-heating step of the bonding method (1-3), the silver ink composition 1301 adhering to the first member 11 and the second member 12 during heating is further heated at a temperature of 60°C or higher without solidifying, to obtain a heated product 130' of the silver ink composition 130, as shown in Figure 5(d).

[0123] Next, in the bonding process of bonding method (1-3), as shown in FIG. 5(e), the first member 11 and the second member 12 are pressed together with a heated object 130' of a silver ink composition therebetween while the heated object 130' is baked in the same manner as in bonding method (1-1).

[0124] By carrying out the pre-heating process and the joining process in this manner, a metal member joined body 1 is obtained in which the first member 11 and the second member 12 are joined via metallic silver (in other words, a conductive joining portion) 13, as shown in FIG. 5(f).

[0125] So far, we have explained the method for joining metal members when the combination (A1) and the preheating methods (B1) to (B3) are selected, but it is also possible to select the combination (A2) or (A3) and the preheating methods (B1), (B2) or (B3).

[0126] 1 to 5, the timing of the start of compression bonding between the first and second members via the heated silver ink composition and the timing of the start of baking the heated material in the bonding step have not been specifically described. In this embodiment, the timing of these steps can be selected arbitrarily, as described above as the compression bonding and baking methods (C1) to (C3).

[0127] Hereinafter, the joining method (1-1) described with reference to FIG. 1 will be described in more detail as an example. FIG. 6 is a cross-sectional view for illustrating a schematic diagram of a joining step in a method for joining metal members (sometimes referred to in this specification as "joining method (1-1-1)") when the combination (A1), the preheating method (B1), and the compression firing method (C1) are selected.

[0128] In the bonding process of the bonding method (1-1-1), a laminated structure of a first member 11, the heated object 130', and a second member 12 is obtained, as shown in FIG. 6(a), similar to that shown in FIG. 1(c). Next, as shown in FIG. 6(b), pressure bonding of this laminated structure begins.

[0129] Next, in the bonding step of the bonding method (1-1-1), the baking of the heated object 130' is started as shown in Fig. 6(c). Here, the heated object in the middle of the baking process (including the start of baking) before becoming the conductive bonding part 13 is denoted by the reference symbol 1301'.

[0130] By performing the joining process in this manner, a metal member joined body 1 is obtained in which a first member 11 and a second member 12 are joined via a conductive joint 13, as shown in Figure 6(d), similar to that shown in Figure 1(d).

[0131] FIG. 7 is a cross-sectional view for illustrating a schematic diagram of a joining step in a method for joining metal members (sometimes referred to in this specification as "joining method (1-1-2)") when the combination (A1), the preheating method (B1), and the compression firing method (C2) are selected.

[0132] In the bonding step of the bonding method (1-1-2), a laminated structure of a first member 11, the heated object 130', and a second member 12 is obtained as shown in FIG. 7(a), similar to that shown in FIG. 1(c). 7(b), the firing of the heated object 130′ is started. Here, too, the heated object in the middle of the firing process (including the start of firing) before it becomes the conductive joint 13 is denoted by reference symbol 1301′.

[0133] Next, in the bonding step of the bonding method (1-1-2), as shown in FIG. 7(c), pressure bonding of a laminated structure of the first member 11, the heated object 1301′ in the middle of the firing stage, and the second member 12 is started.

[0134] By performing the joining process in this manner, a metal member joined body 1 is obtained in which a first member 11 and a second member 12 are joined via a conductive joint 13, as shown in Figure 7(d), similar to that shown in Figure 1(d).

[0135] FIG. 8 is a cross-sectional view for illustrating a schematic diagram of a joining process in a method for joining metal members (sometimes referred to in this specification as "joining method (1-1-3)") when the combination (A1), the preheating method (B1), and the pressure bonding and firing method (C3) are selected.

[0136] In the bonding step of the bonding method (1-1-3), a laminated structure of a first member 11, the heated object 130', and a second member 12 is obtained as shown in FIG. 8(a), similar to that shown in FIG. 1(c). Next, as shown in FIG. 8(b), the baking of the heated object 130′ and the compression bonding of the laminated structure are started simultaneously. Here, the force applied at the start of compression bonding of the laminated structure is represented by the symbol P 11and code P 21 and the heated object at the start of firing is indicated by reference symbol 1302'.

[0137] By performing the joining process in this manner, a metal member joined body 1 is obtained in which a first member 11 and a second member 12 are joined via a conductive joint 13, as shown in Figure 8(c), similar to that shown in Figure 1(d).

[0138] So far, we have explained the method of joining metal members when the combination (A1), the preheating method (B1), and the compression firing methods (C1) to (C3) are selected, but it is also possible to select the combination (A2) or (A3), the preheating method (B1), (B2) or (B3), and the compression firing method (C1), (C2) or (C3).

[0139] So far, the method of joining metal components of this embodiment has been described in terms of joining one first component and one second component with one piece of metallic silver (conductive joint). However, in the method of joining metal components of this embodiment, one first component and one second component may also be joined with two or more pieces of metallic silver (conductive joints). In the method for joining metal members of this embodiment, one first member and two or more second members may be joined with one metallic silver (conductive joint). In this case, the two or more second members may all be the same, all be different, or only partly different. In addition, in the method for joining metal members of this embodiment, one first member and two or more second members may be joined with two or more metallic silver (conductive joints). In this case, the number of second members and the number of metallic silver (conductive joints) may be the same or different. Furthermore, the two or more second members may all be the same, all be different, or only some may be different. The numbers of first members and second members exemplified here may be reversed. Next, the silver ink composition used in this embodiment will be described in detail.

[0140] <Silver ink composition> The silver ink composition contains the silver carboxylate, the amine compound, and formic acid. The silver ink composition preferably does not contain a resin component such as a binder, and it is more preferable that the silver carboxylate is uniformly dispersed during blending.

[0141] By using the silver carboxylate, metallic silver is generated from it, and a conductive joint containing metallic silver as a main component is formed. In this case, the conductive joint can have a sufficiently high ratio of metallic silver to the extent that the conductive joint can be considered to be composed only of metallic silver by preferably not using the resin component. In this case, for example, the ratio of the total mass of metallic silver in the conductive joint to the total mass of the conductive joint can be, for example, 97 mass% or more, 98 mass% or more, or 99 mass% or more. The upper limit of the ratio can be, for example, 100 mass%, 99.9 mass%, 99.8 mass%, 99.7 mass%, 99.6 mass%, 99.5 mass%, 99.4 mass%, 99.3 mass%, 99.2 mass%, or 99.1 mass%, but these are just examples.

[0142] [Silver carboxylate] The silver carboxylate is a silver salt of a carboxylic acid and has a group represented by the formula "-COOAg." The silver carboxylate is not particularly limited as long as it has a group represented by the formula "-COOAg". For example, the number of groups represented by the formula "-COOAg" in one molecule of silver carboxylate may be only one, or may be two or more. In addition, the position of the group represented by the formula "-COOAg" in the silver carboxylate is not particularly limited.

[0143] In the present embodiment, the silver carboxylate may be used alone or in combination of two or more kinds. When two or more kinds are used in combination, the combination and ratio thereof may be adjusted as desired.

[0144] The silver carboxylate is preferably one or more selected from the group consisting of silver β-ketocarboxylate represented by the following general formula (1) (hereinafter may be abbreviated as "silver β-ketocarboxylate (1)") and silver carboxylate represented by the following general formula (4) (hereinafter may be abbreviated as "silver carboxylate (4)"): In this specification, unless otherwise specified, the mere description of "silver carboxylate" does not only mean "silver β-ketocarboxylate (1)" and "silver carboxylate (4)", but also means "silver carboxylate having a group represented by the formula "-COOAg", which includes these.

[0145] [ka] (In the formula, R represents an aliphatic hydrocarbon group having 1 to 20 carbon atoms, in which one or more hydrogen atoms may be substituted with a substituent, a phenyl group, a hydroxyl group, an amino group, or a group represented by the general formula "R 1 -CY 1 2-," "CY 1 3-," "R 1 -CHY 1 -," "R 2 O-," "R 5 R 4 N-", "(R 3 O)2CY 1 -" or "R 6 -C(=O)-CY 1 2-" is a group represented by; Y 1 are each independently a fluorine atom, a chlorine atom, a bromine atom, or a hydrogen atom; R 1 is an aliphatic hydrocarbon group having 1 to 19 carbon atoms or a phenyl group; R 2 is an aliphatic hydrocarbon group having 1 to 20 carbon atoms; R 3 is an aliphatic hydrocarbon group having 1 to 16 carbon atoms; R 4 and R 5 are each independently an aliphatic hydrocarbon group having 1 to 18 carbon atoms; R 6 is an aliphatic hydrocarbon group having 1 to 19 carbon atoms, a hydroxyl group, or a group represented by the formula "AgO-"; X 1are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a phenyl group or a benzyl group in which one or more hydrogen atoms may be substituted with a substituent, a cyano group, an N-phthaloyl-3-aminopropyl group, a 2-ethoxyvinyl group, or a group represented by the general formula "R 7 O-," "R 7 S-", "R 7 -C(=O)-" or "R 7 -C(=O)-O-; R 7 is an aliphatic hydrocarbon group having 1 to 10 carbon atoms, a thienyl group, or a phenyl group or diphenyl group in which one or more hydrogen atoms may be substituted with a substituent.

[0146] [ka] (In the formula, R 8 is an aliphatic hydrocarbon group having 1 to 19 carbon atoms, a carboxy group, or a group represented by the formula "-C(=O)-OAg", and when the aliphatic hydrocarbon group has a methylene group, one or more of the methylene groups may be substituted with a carbonyl group.

[0147] (Silver β-ketocarboxylate (1)) Silver β-ketocarboxylate (1) is represented by the above general formula (1). In the formula, R represents an aliphatic hydrocarbon group having 1 to 20 carbon atoms, in which one or more hydrogen atoms may be substituted with a substituent, a phenyl group, a hydroxyl group, an amino group, or a group represented by the general formula "R 1 -CY 1 2-," "CY 1 3-," "R 1 -CHY 1 -," "R 2 O-," "R 5 R 4 N-", "(R 3 O)2CY 1 -" or "R 6 -C(=O)-CY 1 2-" is a group represented by the formula:

[0148] The aliphatic hydrocarbon group having 1 to 20 carbon atoms in R may be any of linear, branched, and cyclic (aliphatic cyclic groups), and when cyclic, may be either monocyclic or polycyclic. The aliphatic hydrocarbon group may be any of saturated aliphatic hydrocarbon groups and unsaturated aliphatic hydrocarbon groups. The number of carbon atoms in the aliphatic hydrocarbon group is preferably 1 to 10, and more preferably 1 to 6. Preferable examples of the aliphatic hydrocarbon group in R include alkyl groups, alkenyl groups, and alkynyl groups.

[0149] Examples of the linear or branched alkyl group for R include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a 1-methylbutyl group, a 2-methylbutyl group, an n-hexyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 4-methylpentyl group, a 1,1-dimethylbutyl group, a 2,2-dimethylbutyl group, a 3,3-dimethylbutyl group, a 2, 3-dimethylbutyl group, 1-ethylbutyl group, 2-ethylbutyl group, 3-ethylbutyl group, 1-ethyl-1-methylpropyl group, n-heptyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 4-methylhexyl group, 5-methylhexyl group, 1,1-dimethylpentyl group, 2,2-dimethylpentyl group, 2,3-dimethylpentyl group, 2,4-dimethylpentyl group, 3,3-dimethylpentyl group, 4,4-dimethylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3-ethylpentyl group, 4-ethylpentyl, 2,2,3-trimethylbutyl, 1-propylbutyl, n-octyl, isooctyl, 1-methylheptyl, 2-methylheptyl, 3-methylheptyl, 4-methylheptyl, 5-methylheptyl, 1-ethylhexyl, 2-ethylhexyl, 3-ethylhexyl, 4-ethylhexyl, 5-ethylhexyl, 1,1-dimethylhexyl, 2,2-dimethylhexyl, 3,3-dimethylhexyl, 4,4-dimethylhexyl, 5,5-dimethylhexyl, 1,2, 3-trimethylpentyl, 1,2,4-trimethylpentyl, 2,3,4-trimethylpentyl, 2,4,4-trimethylpentyl, 1,4,4-trimethylpentyl, 3,4,4-trimethylpentyl, 1,1,2-trimethylpentyl, 1,1,3-trimethylpentyl, 1,1,4-trimethylpentyl, 1,2,2-trimethylpentyl, 2,2,3-trimethylpentyl, 2,2,4-trimethylpentyl, 1,3,3-trimethylpentyl, 2,3,3-trimethylpentyl, 3,3,Examples of the alkyl group include a 4-trimethylpentyl group, a 1-propylpentyl group, a 2-propylpentyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, and an icosyl group. Examples of the cyclic alkyl group for R include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclononyl group, a cyclodecyl group, a norbornyl group, an isobornyl group, a 1-adamantyl group, a 2-adamantyl group, and a tricyclodecyl group.

[0150] Examples of the alkenyl group in R include groups in which one single bond (CC) between carbon atoms in the alkyl group in R is replaced with a double bond (C=C). Examples of such alkenyl groups include vinyl groups (ethenyl groups, -CH=CH2), allyl groups (2-propenyl groups, -CH2-CH=CH2), 1-propenyl groups (-CH=CH-CH3), isopropenyl groups (-C(CH3)=CH2), 1-butenyl groups (-CH=CH-CH2-CH3), 2-butenyl groups (-CH2-CH=CH-CH3), 3-butenyl groups (-CH2-CH2-CH=CH2), cyclohexenyl groups, and cyclopentenyl groups.

[0151] Examples of the alkynyl group in R include groups in which one single bond (CC) between carbon atoms in the alkyl group in R is replaced with a triple bond (C≡C). Examples of such alkynyl groups include an ethynyl group (-C≡CH) and a propargyl group (-CH2-C≡CH).

[0152] In the aliphatic hydrocarbon group having 1 to 20 carbon atoms in R, one or more hydrogen atoms may be substituted with a substituent. Preferred examples of the substituent include a fluorine atom, a chlorine atom, and a bromine atom. In addition, in the aliphatic hydrocarbon group, the number and position of the substituent are not particularly limited. When the number of the substituents is more than one, these multiple substituents may be the same or different from each other. That is, all the substituents may be the same, all the substituents may be different, or only some of the substituents may be different.

[0153] In the phenyl group in R, one or more hydrogen atoms may be substituted with a substituent. Preferred examples of the substituent include a saturated or unsaturated monovalent aliphatic hydrocarbon group having 1 to 16 carbon atoms, a monovalent group formed by bonding the aliphatic hydrocarbon group to an oxygen atom, a fluorine atom, a chlorine atom, a bromine atom, a hydroxyl group (-OH), a cyano group (-C≡N), and a phenoxy group (-O-C6H5). In the phenyl group having a substituent, the number and position of the substituent are not particularly limited. When the number of the substituents is more than one, the multiple substituents may be the same or different from each other. Examples of the aliphatic hydrocarbon group which is a substituent include the same aliphatic hydrocarbon groups as those for R, except that they have 1 to 16 carbon atoms.

[0154] Y in R 1 are each independently a fluorine atom, a chlorine atom, a bromine atom, or a hydrogen atom. 1 -CY 1 2-," "CY 1 3-" and "R 6 -C(=O)-CY 1 In "2-", each has multiple Y 1 may be the same or different from each other.

[0155] R in R 1 R is an aliphatic hydrocarbon group having 1 to 19 carbon atoms or a phenyl group (C6H5-). 1Examples of the aliphatic hydrocarbon group in include the same aliphatic hydrocarbon groups as those in R, except that they have 1 to 19 carbon atoms. R in R 2 is an aliphatic hydrocarbon group having 1 to 20 carbon atoms, and examples thereof include the same aliphatic hydrocarbon groups as those represented by R. R in R 3 R is an aliphatic hydrocarbon group having 1 to 16 carbon atoms. 3 Examples of the aliphatic hydrocarbon group in include the same aliphatic hydrocarbon groups as those in R, except that they have 1 to 16 carbon atoms. R in R 4 and R 5 are each independently an aliphatic hydrocarbon group having 1 to 18 carbon atoms. That is, R 4 and R 5 may be the same or different, R 4 and R 5 Examples of the aliphatic hydrocarbon group in include the same aliphatic hydrocarbon groups as those in R, except that they have 1 to 18 carbon atoms. R in R 6 R is an aliphatic hydrocarbon group having 1 to 19 carbon atoms, a hydroxyl group, or a group represented by the formula "AgO-". 6 Examples of the aliphatic hydrocarbon group in include the same aliphatic hydrocarbon groups as those in R, except that they have 1 to 19 carbon atoms.

[0156] Among the above, R is a linear or branched alkyl group, a group represented by the general formula "R 6 -C(=O)-CY 1 2-”, a hydroxyl group or a phenyl group. 6 is preferably a linear or branched alkyl group, a hydroxyl group, or a group represented by the formula "AgO-".

[0157] In the general formula (1), X 1are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, a phenyl group or a benzyl group (C6H5-CH2-) in which one or more hydrogen atoms may be substituted with a substituent, a cyano group, an N-phthaloyl-3-aminopropyl group, a 2-ethoxyvinyl group (C2H5-O-CH=CH-), or a group represented by the general formula "R 7 O-," "R 7 S-", "R 7 -C(=O)-" or "R 7 It is a group represented by "-C(=O)-O-". X 1 Examples of the aliphatic hydrocarbon group having 1 to 20 carbon atoms in the above group include the same aliphatic hydrocarbon groups in the above group.

[0158] X 1 Examples of the halogen atom in include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. X 1 In the phenyl group and benzyl group, one or more hydrogen atoms may be substituted with a substituent. Preferred examples of the substituent include halogen atoms (fluorine atom, chlorine atom, bromine atom, iodine atom), nitro group (-NO2), etc. In the phenyl group and benzyl group having a substituent, the number and position of the substituent are not particularly limited. When the number of the substituents is multiple, these multiple substituents may be the same or different from each other.

[0159] X 1 R in 7 R is an aliphatic hydrocarbon group having 1 to 10 carbon atoms, a thienyl group (C4H3S-), or a phenyl group or diphenyl group (biphenyl group, C6H5-C6H4-) in which one or more hydrogen atoms may be substituted with a substituent. 7 Examples of the aliphatic hydrocarbon group in R include the same aliphatic hydrocarbon groups as those in R, except that the number of carbon atoms is 1 to 10. 7The substituents of the phenyl and diphenyl groups in the above formula (I) include, for example, halogen atoms (fluorine, chlorine, bromine, and iodine atoms). In the phenyl and diphenyl groups having a substituent, the number and positions of the substituents are not particularly limited. When the number of the substituents is more than one, the multiple substituents may be the same or different from each other. R 7 When X is a thienyl group or a diphenyl group, 1 In the above, the bonding position to the adjacent group or atom (oxygen atom, sulfur atom, carbonyl group, carbonyloxy group) is not particularly limited. For example, the thienyl group may be either a 2-thienyl group or a 3-thienyl group.

[0160] In the general formula (1), two X 1 may be bonded as a single group to the carbon atom between the two carbonyl groups via a double bond. 1 Examples of the group include a group represented by the formula "=CH-C6H4-NO2".

[0161] X 1 Among the above, R is a hydrogen atom, a linear or branched alkyl group, a benzyl group, or a group represented by the general formula "R 7 It is preferable that at least one of X is a group represented by "-C(=O)-". 1 is preferably a hydrogen atom.

[0162] Silver β-ketocarboxylates (1) are silver 2-methylacetoacetate (CH3-C(=O)-CH(CH3)-C(=O)-OAg), silver acetoacetate (CH3-C(=O)-CH2-C(=O)-OAg), silver 2-ethylacetoacetate (CH3-C(=O)-CH(CH2CH3)-C(=O)-OAg), silver propionylacetate (CH3CH2-C(=O)-CH2-C(=O)-OAg), and isobutyric acid. Silver pivaloyl acetate ((CH3)3C-C(=O)-CH2-C(=O)-OAg), silver caproyl acetate (CH3(CH2)3CH2-C(=O)-CH2-C(=O)-OAg), silver 2-n-butylacetoacetate (CH3-C(=O)-CH(CH2CH2CH2CH3)-C(=O)-OAg), 2-benzyl Silver acetoacetate (CH3-C(=O)-CH(CH2C6H5)-C(=O)-OAg), silver benzoylacetate (C6H5-C(=O)-CH2-C(=O)-OAg), silver pivaloylacetoacetate ((CH3)3C-C(=O)-CH2-C(=O)-CH2-C(=O)-OAg), silver isobutyrylacetoacetate ((CH3)2CH-C(=O)-CH2-C(=O)-CH2-C(=O)-O Silver 2-acetylpivaloyl acetate ((CH3)3C-C(=O)-CH(-C(=O)-CH3)-C(=O)-OAg), 2-acetylisobutyryl silver acetate ((CH3)2CH-C(=O)-CH(-C(=O)-CH3)-C(=O)-OAg), or silver acetonedicarboxylate (AgO-C(=O)-CH2-C(=O)-CH2-C(=O)-OAg).

[0163] In a conductor (metallic silver) formed by drying a silver ink composition or subjecting it to a solidification treatment such as heating (baking) using silver β-ketocarboxylate (1), the concentration of remaining raw materials and impurities can be further reduced. In such a conductor, the fewer raw materials and impurities there are, the better the contact between the formed metallic silver particles becomes, making electrical conduction easier and lowering the resistivity.

[0164] As described below, silver β-ketocarboxylate (1) can decompose to form metallic silver at a low temperature of preferably 60 to 210° C., more preferably 60 to 200° C., even without using a reducing agent or the like known in the art. Furthermore, silver β-ketocarboxylate (1) decomposes to form metallic silver at an even lower temperature when used in combination with a reducing agent.

[0165] In the present invention, the silver β-ketocarboxylate (1) may be used alone or in combination of two or more kinds. When two or more kinds are used in combination, the combination and ratio thereof can be adjusted as desired.

[0166] (Silver carboxylate (4)) The silver carboxylate (4) is represented by the above general formula (4). In the formula, R 8 is an aliphatic hydrocarbon group having 1 to 19 carbon atoms, a carboxy group (-COOH), or a group represented by the formula "-C(=O)-OAg." R 8 The aliphatic hydrocarbon group in R may be the same as the aliphatic hydrocarbon group in R, except that the number of carbon atoms is 1 to 19. 8 The aliphatic hydrocarbon group in the above formula preferably has 1 to 15 carbon atoms, and more preferably has 1 to 10 carbon atoms.

[0167] R 8 When the aliphatic hydrocarbon group in has a methylene group (-CH2-), one or more of the methylene groups may be substituted with a carbonyl group. The number and position of the methylene groups that may be substituted with a carbonyl group are not particularly limited, and all of the methylene groups may be substituted with a carbonyl group. Here, the term "methylene group" includes not only a single group represented by the formula "-CH2-", but also one group represented by the formula "-CH2-" in an alkylene group in which multiple groups represented by the formula "-CH2-" are linked together.

[0168] The silver carboxylate (4) is preferably silver pyruvate (CH3-C(=O)-C(=O)-OAg), silver acetate (CH3-C(=O)-OAg), silver butyrate (CH3-(CH2)2-C(=O)-OAg), silver isobutyrate ((CH3)2CH-C(=O)-OAg), silver 2-ethylhexanoate (CH3-(CH2)3-CH(CH2CH3)-C(=O)-OAg), silver neodecanoate, silver oxalate (AgO-C(=O)-C(=O)-OAg), or silver malonate (AgO-C(=O)-CH2-C(=O)-OAg). Also preferred are those in which one of the two groups represented by the formula "-COOAg" in silver oxalate (AgO-C(=O)-C(=O)-OAg) and silver malonate (AgO-C(=O)-CH2-C(=O)-OAg) is a group represented by the formula "-COOH" (HO-C(=O)-C(=O)-OAg, HO-C(=O)-CH2-C(=O)-OAg).

[0169] When silver carboxylate (4) is used, the concentration of remaining raw materials and impurities can be further reduced in the conductor (metallic silver) formed by solidification treatment such as drying treatment and heating (baking) treatment of the silver ink composition, as in the case of using silver carboxylate (1). Furthermore, when silver carboxylate (4) is used in combination with a reducing agent, it decomposes at a lower temperature to form metallic silver.

[0170] In the present invention, the silver carboxylate (4) may be used alone or in combination of two or more kinds. When two or more kinds are used in combination, the combination and ratio thereof can be adjusted as desired.

[0171] The silver carboxylate is preferably a silver β-ketocarboxylate (1). Among these silver β-ketocarboxylates (1), silver 2-methylacetoacetate, silver acetoacetate, silver isobutyrylacetate, and silver pivaloylacetate have excellent compatibility with nitrogen-containing compounds (especially amine compounds) described below, and are particularly suitable for increasing the concentration of a silver ink composition.

[0172] The ratio of the total mass of silver derived from the silver carboxylate in the silver ink composition to the total mass of the silver ink composition is preferably 5% by mass or more, and more preferably 8% by mass or more. When the ratio is in this range, the formed conductive layer (silver layer) has better quality. The upper limit of the ratio is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 25% by mass in consideration of the handleability of the silver ink composition. In this specification, unless otherwise specified, "silver derived from a silver carboxylate" is synonymous with the silver in the silver carboxylate that was blended during the production of the silver ink composition, and is a concept that includes all of the silver that continues to constitute the silver carboxylate after blending, the silver in the decomposition products produced by decomposition of the silver carboxylate after blending, and the silver itself (metallic silver) produced by decomposition of the silver carboxylate after blending.

[0173] [Amine compounds] The amine compound preferably has 1 to 25 carbon atoms, and may be any of a primary amine, a secondary amine, and a tertiary amine. The amine compound may be any one of linear, branched, and cyclic. In this specification, the term "straight-chain amine compound" means "amine compound having a straight-chain main chain", the term "branched-chain amine compound" means "amine compound having a branched main chain", and the term "cyclic amine compound" means "amine compound having a cyclic main chain". The term "main chain" refers to a chain structure in which an amine moiety (e.g., an amino group (-NH2) of a primary amine) described later is directly bonded.

[0174] The amine compound may have one or more nitrogen atoms constituting the amine moiety (for example, nitrogen atoms constituting the amino group (-NH2) of a primary amine).

[0175] Examples of the primary amine include monoalkylamines, monoarylamines, mono(heteroaryl)amines, diamines, and the like, in which one or more hydrogen atoms may be substituted with a substituent.

[0176] The alkyl group constituting the monoalkylamine may be any one of linear, branched, and cyclic, and examples of such an alkyl group include the same as the alkyl group in R. The alkyl group is preferably a linear or branched alkyl group having 1 to 19 carbon atoms, or a cyclic alkyl group having 3 to 7 carbon atoms. Specific examples of preferred monoalkylamines include n-butylamine, n-hexylamine, n-octylamine, n-dodecylamine, n-octadecylamine, isobutylamine, sec-butylamine, tert-butylamine, 3-aminopentane, 3-methylbutylamine, 2-heptylamine (2-aminoheptane), 2-aminooctane, 2-ethylhexylamine, and 1,2-dimethyl-n-propylamine.

[0177] Examples of the aryl group constituting the monoarylamine include a phenyl group, a 1-naphthyl group, a 2-naphthyl group, etc. The aryl group preferably has 6 to 10 carbon atoms.

[0178] The heteroaryl group constituting the mono(heteroaryl)amine has a heteroatom as an atom constituting an aromatic ring skeleton, and examples of the heteroatom include a nitrogen atom, a sulfur atom, an oxygen atom, and a boron atom. The number of the heteroatoms constituting the aromatic ring skeleton is not particularly limited, and may be one or two or more. When there are two or more, these heteroatoms may be the same or different from each other. That is, these heteroatoms may all be the same, all be different, or only some may be different. The heteroaryl group may be either monocyclic or polycyclic, and the number of ring members (the number of atoms constituting the ring skeleton) is not particularly limited, but is preferably a 3- to 12-membered ring.

[0179] Examples of the heteroaryl group that is a monocyclic group having 1 to 4 nitrogen atoms include a pyrrolyl group, a pyrrolinyl group, an imidazolyl group, a pyrazolyl group, a pyridyl group, a pyrimidyl group, a pyrazinyl group, a pyridazinyl group, a triazolyl group, a tetrazolyl group, a pyrrolidinyl group, an imidazolidinyl group, a piperidinyl group, a pyrazolidinyl group, and a piperazinyl group. Such a heteroaryl group is preferably a 3- to 8-membered ring, and more preferably a 5- or 6-membered ring. The heteroaryl group is preferably a monocyclic group having one oxygen atom, and more preferably a 3- to 8-membered ring, and more preferably a 5- or 6-membered ring. Among the heteroaryl groups, examples of monocyclic groups having one sulfur atom include a thienyl group, and such heteroaryl groups are preferably 3- to 8-membered rings, and more preferably 5- or 6-membered rings. Examples of the heteroaryl group that is a monocyclic group having 1 to 2 oxygen atoms and 1 to 3 nitrogen atoms include an oxazolyl group, an isoxazolyl group, an oxadiazolyl group, and a morpholinyl group. Such a heteroaryl group is preferably a 3- to 8-membered ring, and more preferably a 5- or 6-membered ring. Examples of the monocyclic heteroaryl group having 1 to 2 sulfur atoms and 1 to 3 nitrogen atoms include a thiazolyl group, a thiadiazolyl group, and a thiazolidinyl group. Such a heteroaryl group is preferably a 3- to 8-membered ring, and more preferably a 5- or 6-membered ring. Examples of the heteroaryl group that is a polycyclic group having 1 to 5 nitrogen atoms include an indolyl group, an isoindolyl group, an indolizinyl group, a benzimidazolyl group, a quinolyl group, an isoquinolyl group, an indazolyl group, a benzotriazolyl group, a tetrazolopyridyl group, a tetrazolopyridazinyl group, and a dihydrotriazolopyridazinyl group. Such a heteroaryl group is preferably a 7- to 12-membered ring, and more preferably a 9- to 10-membered ring. Examples of the polycyclic heteroaryl group having 1 to 3 sulfur atoms include a dithianaphthalenyl group and a benzothiophenyl group. Such a heteroaryl group is preferably a 7- to 12-membered ring, and more preferably a 9- to 10-membered ring. Examples of the polycyclic heteroaryl group having 1 to 2 oxygen atoms and 1 to 3 nitrogen atoms include a benzoxazolyl group and a benzoxadiazolyl group. Such a heteroaryl group is preferably a 7- to 12-membered ring, and more preferably a 9- to 10-membered ring. Examples of the polycyclic heteroaryl group having 1 to 2 sulfur atoms and 1 to 3 nitrogen atoms include a benzothiazolyl group and a benzothiadiazolyl group. Such a heteroaryl group is preferably a 7- to 12-membered ring, and more preferably a 9- to 10-membered ring.

[0180] The diamine has only to have two amino groups, and the positional relationship of the two amino groups is not particularly limited.Preferred diamines include, for example, monoalkylamines, monoarylamines, or mono(heteroaryl)amines in which one hydrogen atom other than the hydrogen atom constituting the amino group (-NH2) is substituted with an amino group. The number of carbon atoms in the diamine is preferably 1 to 10. More preferable examples of the diamine include ethylenediamine, 1,3-diaminopropane, and 1,4-diaminobutane.

[0181] Examples of the secondary amine include dialkylamines, diarylamines, and di(heteroaryl)amines in which one or more hydrogen atoms may be substituted with a substituent.

[0182] The alkyl group constituting the dialkylamine is the same as the alkyl group constituting the monoalkylamine, and is preferably a linear or branched alkyl group having a carbon number of 1 to 9, or a cyclic alkyl group having a carbon number of 3 to 7. In addition, the two alkyl groups in one molecule of the dialkylamine may be the same or different. Specific examples of preferred dialkylamines include N-methyl-n-hexylamine, diisobutylamine, and di(2-ethylhexyl)amine.

[0183] The aryl group constituting the diarylamine is similar to the aryl group constituting the monoarylamine, and preferably has a carbon number of 6 to 10. Furthermore, the two aryl groups in one diarylamine molecule may be the same or different.

[0184] The heteroaryl group constituting the di(heteroaryl)amine is the same as the heteroaryl group constituting the mono(heteroaryl)amine, and is preferably a 6- to 12-membered ring. Furthermore, the two heteroaryl groups in one molecule of the di(heteroaryl)amine may be the same or different.

[0185] Examples of the tertiary amine include trialkylamines and dialkylmonoarylamines in which one or more hydrogen atoms may be substituted with a substituent.

[0186] The alkyl group constituting the trialkylamine is the same as the alkyl group constituting the monoalkylamine, and is preferably a linear or branched alkyl group having 1 to 19 carbon atoms, or a cyclic alkyl group having 3 to 7 carbon atoms. The three alkyl groups in one molecule of trialkylamine may be the same or different from each other. That is, the three alkyl groups may all be the same, all be different, or only some may be different. Specific examples of preferred trialkylamines include N,N-dimethyl-n-octadecylamine and N,N-dimethylcyclohexylamine.

[0187] The alkyl group constituting the dialkylmonoarylamine is the same as the alkyl group constituting the monoalkylamine, and is preferably a linear or branched alkyl group having a carbon number of 1 to 6, or a cyclic alkyl group having a carbon number of 3 to 7. In addition, the two alkyl groups in one molecule of the dialkylmonoarylamine may be the same or different. The aryl group constituting the dialkylmonoarylamine is the same as the aryl group constituting the monoarylamine, and preferably has 6 to 10 carbon atoms.

[0188] Although the chain-like amine compounds have been mainly described so far, the amine compounds may be heterocyclic compounds in which the nitrogen atom constituting the amine moiety is part of a ring skeleton structure (heterocyclic skeleton structure). That is, the amine compounds may be cyclic amines. In this case, the ring structure (the ring containing the nitrogen atom constituting the amine moiety) may be either monocyclic or polycyclic, and the number of ring members (the number of atoms constituting the ring skeleton) is not particularly limited, and may be either an aliphatic ring or an aromatic ring. Preferred cyclic amines include, for example, pyridine.

[0189] In the primary amine, secondary amine, and tertiary amine, the "hydrogen atom which may be substituted by a substituent" refers to a hydrogen atom other than the hydrogen atom bonded to the nitrogen atom constituting the amine moiety. The number of the substituents is not particularly limited, and may be one, two or more, and all of the hydrogen atoms may be substituted by a substituent. When the number of the substituents is more than one, these multiple substituents may be the same or different from each other. That is, the multiple substituents may all be the same, all be different, or only some may be different. The position of the substituent is also not particularly limited.

[0190] Examples of the substituent in the amine compound include an alkyl group, an aryl group, a halogen atom, a cyano group, a nitro group, a hydroxyl group, a trifluoromethyl group (-CF3), etc. Here, examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.

[0191] When the alkyl group constituting the monoalkylamine has a substituent, the alkyl group is preferably a linear or branched alkyl group having 1 to 9 carbon atoms and having an aryl group as a substituent, or a cyclic alkyl group having 3 to 7 carbon atoms and having an alkyl group having preferably 1 to 5 carbon atoms as a substituent. Specific examples of monoalkylamines having such a substituent include 2-phenylethylamine, benzylamine, and 2,3-dimethylcyclohexylamine. In addition, the aryl group and alkyl group as the substituent may further have one or more hydrogen atoms substituted with halogen atoms. Examples of monoalkylamines having a substituent substituted with such halogen atoms include 2-bromobenzylamine. Here, examples of the halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, etc.

[0192] When the aryl group constituting the monoarylamine has a substituent, the aryl group is preferably an aryl group having 6 to 10 carbon atoms and having a halogen atom as a substituent. Specific examples of monoarylamines having such a substituent include bromophenylamine. Here, examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0193] When the alkyl group constituting the dialkylamine has a substituent, the alkyl group is preferably a linear or branched alkyl group having 1 to 9 carbon atoms and having a hydroxyl group or an aryl group as a substituent. Specific examples of dialkylamines having such a substituent include diethanolamine and N-methylbenzylamine.

[0194] The amine compound is preferably n-propylamine, n-butylamine, n-hexylamine, n-octylamine, n-dodecylamine, n-octadecylamine, isobutylamine, sec-butylamine, tert-butylamine, 3-aminopentane, 3-methylbutylamine, 2-heptylamine, 2-aminooctane, 2-ethylhexylamine, 2-phenylethylamine, ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, N-methyl-n-hexylamine, diisobutylamine, N-methylbenzylamine, di(2-ethylhexyl)amine, 1,2-dimethyl-n-propylamine, N,N-dimethyl-n-octadecylamine, or N,N-dimethylcyclohexylamine. Among these amine compounds, 2-ethylhexylamine has excellent compatibility with the silver carboxylate and is particularly suitable for increasing the concentration of the silver ink composition, and further is particularly suitable for reducing the surface roughness of metallic silver.

[0195] In the present embodiment, the amine compound is preferably linear or branched.

[0196] In the present embodiment, the amine compounds may be used alone or in combination of two or more kinds. When two or more kinds are used in combination, the combination and ratio thereof can be adjusted as desired.

[0197] In the silver ink composition, the amount of the amine compound is preferably 0.3 to 15 mol, more preferably 0.3 to 12 mol, and particularly preferably 0.3 to 8 mol, per mol of the silver carboxylate, and may be, for example, any one of 0.3 to 5 mol, 0.3 to 3 mol, and 0.3 to 1.5 mol. When the amount of the amine compound is within such a range, the stability of the silver ink composition is further improved, and the quality of the metallic silver is further improved.

[0198] [Formic acid] In the silver ink composition, the amount of formic acid (HC(=O)-OH) is preferably 0.04 to 3.5 mol, more preferably 0.06 to 2.5 mol, per 1 mol of the silver carboxylate, and may be, for example, any one of 0.08 to 1.5 mol, or 0.1 to 1 mol. When the amount of formic acid is within such a range, the silver ink composition can form metallic silver more easily and more stably.

[0199] [Other ingredients] The silver ink composition may be one containing another component that does not fall into any of the categories of the silver carboxylate, the amine compound, and formic acid. The other components are not particularly limited and can be selected arbitrarily depending on the purpose. Examples of the other components include alcohol and solvents other than alcohol (sometimes simply referred to as "solvents" in this specification).

[0200] In the present embodiment, when the other components are used, the other components may be used alone or in combination of two or more kinds. When two or more kinds are used in combination, the combination and ratio thereof can be adjusted as desired.

[0201] (alcohol) The alcohol is preferably an acetylene alcohol represented by the following general formula (2) (hereinafter sometimes abbreviated as "acetylene alcohol (2)").

[0202] [ka] (In the formula, R' and R'' each independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or a phenyl group in which one or more hydrogen atoms may be substituted with a substituent.)

[0203] Acetylene alcohol (2) The acetylene alcohol (2) is represented by the above general formula (2). In the formula, R' and R'' each independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or a phenyl group in which one or more hydrogen atoms may be substituted with a substituent. The alkyl group having 1 to 20 carbon atoms in R' and R'' may be linear, branched, or cyclic, and when cyclic, may be monocyclic or polycyclic. Examples of the alkyl group in R' and R'' include the same as the alkyl group in R.

[0204] Examples of the substituent with which a hydrogen atom of the phenyl group in R' and R'' may be substituted include a saturated or unsaturated monovalent aliphatic hydrocarbon group having 1 to 16 carbon atoms, a monovalent group formed by bonding the aliphatic hydrocarbon group to an oxygen atom, a fluorine atom, a chlorine atom, a bromine atom, a hydroxyl group, a cyano group, a phenoxy group, and the like. These substituents are the same as the substituent with which a hydrogen atom of the phenyl group in R may be substituted. In the phenyl group having a substituent, the number and positions of the substituents are not particularly limited, and when the number of the substituents is multiple, these multiple substituents may be the same or different from each other.

[0205] R' and R'' are preferably a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, and more preferably a hydrogen atom or a linear or branched alkyl group having 1 to 10 carbon atoms.

[0206] Preferred acetylene alcohols (2) include, for example, 3,5-dimethyl-1-hexyn-3-ol, 3-methyl-1-butyn-3-ol, 3-methyl-1-pentyn-3-ol, 2-propyn-1-ol, 4-ethyl-1-octyn-3-ol, and 3-ethyl-1-heptyn-3-ol.

[0207] The alcohols may be used alone or in combination of two or more kinds. When two or more kinds are used in combination, the combination and ratio thereof can be adjusted arbitrarily.

[0208] (solvent) The solvent is not particularly limited as long as it is a solvent other than an alcohol (one that does not have a hydroxyl group). However, the solvent is preferably liquid at room temperature. Examples of the solvent include aromatic hydrocarbons such as toluene, o-xylene, m-xylene, and p-xylene; aliphatic hydrocarbons such as pentane, hexane, cyclohexane, heptane, octane, cyclooctane, nonane, decane, undecane, dodecane, tridecane, tetradecane, pentadecane, and decahydronaphthalene; halogenated hydrocarbons such as dichloromethane and chloroform; esters such as ethyl acetate, monomethyl glutarate, and dimethyl glutarate; ethers such as diethyl ether, tetrahydrofuran (THF), and 1,2-dimethoxyethane (dimethylcellosolve); ketones such as acetone, methyl ethyl ketone (MEK), and cyclohexanone; nitriles such as acetonitrile; and amides such as N,N-dimethylformamide (DMF) and N,N-dimethylacetamide.

[0209] The amount of the other components in the silver ink composition may be appropriately selected depending on the type of the other components.

[0210] For example, when acetylene alcohol (2) is used as the other component, the amount of acetylene alcohol (2) in the silver ink composition is preferably 0.01 to 0.7 mol, more preferably 0.02 to 0.5 mol, and particularly preferably 0.02 to 0.3 mol per 1 mol of silver β-ketocarboxylate (1). When the amount of acetylene alcohol (2) is within such a range, the stability of the silver ink composition is further improved.

[0211] For example, when the solvent is used as the other component, the amount of the solvent may be selected depending on the purpose, such as the viscosity of the silver ink composition, etc. However, typically, in the silver ink composition, the ratio of the amount of the solvent to the total amount of the components is preferably 30 mass % or less, more preferably 20 mass % or less, and particularly preferably 10 mass % or less.

[0212] For example, when a component that does not fall into either the acetylene alcohol (2) or the solvent is used as the other component, the ratio of the amount of the other component to the total amount of the components in the silver ink composition is preferably 10 mass % or less, and more preferably 5 mass % or less.

[0213] Even if the ratio of the blended amount of the other components to the total amount of the blended components is 0 by mass, that is, even if no other components are blended, the silver ink composition sufficiently exhibits its effects.

[0214] In the silver ink composition, all of the components may be dissolved, or some or all of the components may be in a dispersed state without being dissolved. However, it is preferable that all of the components are dissolved, and it is preferable that the undissolved components are uniformly dispersed.

[0215] <Method of manufacturing silver ink composition> The silver ink composition is obtained by blending the silver carboxylate, the amine compound, formic acid, and, if necessary, the other components. After blending the components, the resulting blend may be used as the silver ink composition as is, or a purified product obtained by subsequently carrying out a known purification operation, if necessary, may be used as the silver ink composition. In this embodiment, when blending the above components, the generation of impurities that reduce the conductivity of metallic silver can be suppressed. This tendency is particularly noticeable when silver β-ketocarboxylate (1) is used as the silver carboxylate. Therefore, metallic silver having sufficient conductivity can be obtained even if the silver ink composition is used without carrying out a purification operation.

[0216] The order of mixing the components is not particularly limited. A preferred example of a method for mixing the components is to add the silver carboxylate to the amine compound, and then add formic acid to the resulting mixture.

[0217] When the components are mixed, all the components may be added and then mixed, or some of the components may be added sequentially while being mixed, or all the components may be added sequentially while being mixed. The mixing method is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blade, etc.; a method of mixing using a mixer, a three-roll mill, a kneader, a bead mill, etc.; a method of mixing by adding ultrasound, etc. In the silver ink composition, when undissolved components are to be uniformly dispersed, it is preferable to employ a dispersion method using, for example, the above-mentioned three-roll mill, kneader, or bead mill.

[0218] The temperature during blending is not particularly limited as long as each blended component does not deteriorate, but is preferably −5 to 60° C. The temperature during blending may be appropriately adjusted depending on the types and amounts of the blended components so that the mixture obtained by blending has a viscosity that allows easy stirring. The blending time is not particularly limited as long as each blended component does not deteriorate, but is preferably 10 minutes to 36 hours.

[0219] <<Metal member assembly>> A joined metal member according to one embodiment of the present invention (a joined metal member of the first aspect) is a joined metal member obtained by the above-mentioned method for joining metal members, and the die shear strength of the joined metal member is 15 MPa or more. The metal member joined body of this embodiment and its die shear strength are as described above.

[0220] The conductive joint in the metal member assembly of the first embodiment (in other words, the metallic silver formed from the silver ink composition) may contain extremely small amounts of impurities derived from the blended components, such as decomposition products generated by decomposition of any of the blended components of the silver ink composition, namely, the silver carboxylate, the amine compound, formic acid, and the other components; compounds generated by reaction of any of the silver carboxylate, the amine compound, formic acid, and the other components with the decomposition products; and compounds generated by reaction of any of the silver carboxylate, the amine compound, formic acid, and the other components with each other. It can be confirmed that the composition of these impurities is clearly different from that of the metallic silver formed from another silver ink composition produced by blending essential components different from those of the silver ink composition. On the other hand, the baking temperature of the heated silver ink composition in the bonding step can be set to a relatively low temperature, because the silver ink composition contains the blended components (the silver carboxylate, the amine compound, and formic acid) within the above-mentioned limited ranges. That is, the impurities in the metallic silver in the first embodiment reflect the use of the silver ink composition, which has the advantage that metallic silver can be formed (ie, fired) at relatively low temperatures.

[0221] A metal member joined body according to one embodiment of the present invention (a metal member joined body of a second aspect) is constructed by joining a first metal member and a second metal member via metallic silver, and either one or both of the first and second members are made of copper. When the first member is made of copper, the metal member joined body has, between the first member and the metallic silver, a layer whose main constituent element is silver and a layer whose main constituent elements are copper and oxygen, in that order, from the first member side toward the metallic silver side. When the second member is made of copper, the metal member joined body has, between the second member and the metallic silver, a layer whose main constituent element is silver and a layer whose main constituent elements are copper and oxygen, in that order, from the second member side toward the metallic silver side. The die shear strength of the metal member joined body is 15 MPa or more. The joined metal members of the second embodiment can also be obtained by the above-mentioned method for joining metal members.

[0222] When the first member is made of copper, the metal member joint of the second embodiment has a layered structure in which a first member made of copper, a layer mainly composed of silver, a layer mainly composed of copper and oxygen, and metallic silver are present in this order. When the second member is made of copper, the metal member joint of the second embodiment has a layered structure in which a second member made of copper, a layer mainly composed of silver, a layer mainly composed of copper and oxygen, and metallic silver are present in this order. These layered structures are quite unexpected in that the silver and copper elements are arranged in alternating fashion.

[0223] In the layer containing copper and oxygen as the main constituent elements, oxygen may be present as a product of reaction with copper, such as copper oxide, or may be present alone without reacting with copper.

[0224] The above-mentioned "layer containing silver as a main constituent element" means a layer that contains silver as a constituent element to such an extent that the properties due to the inclusion of silver are clearly exhibited, and for example, includes a layer in which the ratio of the mass of silver element to the total mass of all elements in the target layer is 50 mass% or more. The above-mentioned "layer containing copper and oxygen as main constituent elements" means a layer containing copper and oxygen as constituent elements to such an extent that the properties due to the inclusion of copper and oxygen are clearly exhibited, and an example of the layer in question is a layer in which the ratio of the total mass of copper element and oxygen element to the total mass of all elements is 50 mass% or more.

[0225] Thus, in the second embodiment of the metal member joint, the first copper member and the metallic silver, or the second copper member and the metallic silver, are not simply in contact with each other, but have the above-described layered structure. Although it is not clear why this is the case, it is presumed to be as follows. That is, it is presumed that by using the silver ink composition having a composition within a specific range and performing the preheating step and the bonding step according to the manufacturing method of this embodiment, the first copper member or the second copper member reacts with the silver ink composition or a heated product thereof, resulting in either or both of the diffusion of metallic silver into the first copper member or the second copper member, and the diffusion of copper in the first copper member or the second copper member into metallic silver. Such diffusion may be related to the reducing action of formic acid, which is a compounding component of the silver ink composition. Therefore, regardless of whether the first component or the second component is made of copper, it is presumed that the silver in the layer containing silver as the main constituent element originates from the silver ink composition or a heated version of the silver ink composition. Furthermore, regardless of whether the first component or the second component is made of copper, it is presumed that the copper in the layer containing copper and oxygen as its main constituent elements originates from the first component or the second component, which is also made of copper.

[0226] The fact that the joined body of metal members of the second aspect has the above-mentioned layered structure is consistent with the fact that the joined body of metal members has a sufficiently large die shear strength.

[0227] The die shear strength of the joined metal members of the second aspect is 15 MPa or more, which is similar to the die shear strength of the joined metal members of the first aspect.

[0228] The laminated structure in the metal member joined body of the second embodiment can be confirmed, for example, by preparing a cross-section of the metal member joined body in a direction parallel to the joining direction of the first member, the metallic silver, and the second member, and observing the cross-section using a Transmission Electron Microscope (abbreviated as TEM) or by observing the cross-section using Energy Dispersive X-ray Spectroscopy (abbreviated as EDS or EDX).

[0229] The use of the metal member joined body of the present embodiment (first aspect, second aspect) is not particularly limited. As one example, the metal member joined body is useful as a joined body between electrodes in a circuit board. That is, preferred examples of the metal members constituting the metal member joined body, i.e., the first member and the second member, include metal electrodes.

[0230] <<Circuit board>> A circuit board according to one embodiment of the present invention includes the metal member assembly on an organic substrate, and the metal member serves as a metal electrode. As described above, the baking temperature of the heated silver ink composition in the bonding step can be set to a relatively low temperature because the silver ink composition contains ingredients within a relatively limited range. Therefore, even if an organic substrate containing an organic component such as a resin having a relatively low heat resistance is used as the constituent material of the substrate and the above-mentioned method for joining metal members is applied to the metal electrodes thereon, a circuit substrate free from quality problems can be manufactured. In contrast, such a circuit substrate cannot be manufactured if an extremely high heating temperature is required for joining the metal members.

[0231] The circuit board of the present embodiment can have the same configuration as known circuit boards, except that it includes the above-mentioned metal member assembled body having a die shear strength of 15 MPa or more, and can be manufactured by the same method as known circuit boards, except that it uses the above-mentioned metal member assembled body. EXAMPLES

[0232] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the following examples.

[0233] [Example 1] <<Manufacturing of metal component joints>> <Production of Silver Ink Composition> In a beaker, 2-ethylhexylamine (0.4 times the molar amount relative to silver 2-methylacetoacetate described below) was added with 2-methylacetoacetate (19.0 g) so that the liquid temperature was 50° C. or less, and the mixture was stirred for 15 minutes using a mechanical stirrer to obtain a liquid. Formic acid (0.7 times the molar amount relative to silver 2-methylacetoacetate) was added dropwise to this liquid over 30 minutes so that the temperature of the reaction liquid was 50° C. or less. After the addition of formic acid was completed, the reaction liquid was stirred at 25° C. for an additional 1.5 hours to obtain a silver ink composition.

[0234] The type and mixing ratio of each compound is shown in Table 1. In Table 1, "amine compound (molar ratio)" means the amount (number of moles) of amine compound per mole of silver carboxylate ([number of moles of amine compound] / [number of moles of silver carboxylate]). Similarly, "molar ratio of formic acid" means the amount (number of moles) of formic acid per mole of silver carboxylate ([number of moles of formic acid] / [number of moles of silver carboxylate]).

[0235] <Manufacturing of metal component joints> A copper plate measuring 12 mm×8 mm×0.8 mm and a copper chip measuring 4 mm×4 mm×0.8 mm were prepared as the first member or the second member. These (i.e., the copper plate and the copper chip) were polished with water-wetted waterproof abrasive paper (grain size 2000) (manufactured by Sankyo Rikagaku Co., Ltd.) to clean their surfaces. Next, a 0.3 mm thick metal mask having two parallel rectangular areas measuring 4 mm x 4 mm was placed on the cleaned copper plate, and the silver ink composition obtained above was solid printed on the copper plate covered with the mask by screen printing. As a result of the above, two parallelepiped printed layers of the silver ink composition measuring approximately 4 mm×4 mm×0.3 mm were formed on the surface of the copper plate.

[0236] Next, under normal pressure and in an atmospheric air atmosphere, the copper plate with the printed layer was heated from the side without the printed layer using a hot plate, and the temperature of the copper plate and the printed layer was raised to 100°C over a period of 5 minutes, and the temperature was further maintained at 100°C for 1 minute (preheating step). During this time, the printed layer (i.e., the silver ink composition) did not solidify and maintained its fluidity, and bubbling was observed after the temperature reached 100°C. This bubbling disappeared before the temperature of the copper plate and the printed layer had been maintained at 100°C for 1 minute. In this manner, a heated silver ink composition was obtained. The resulting heated product did not have the luster characteristic of metallic silver and was dark green in color.

[0237] A total of two such first laminates each having a heated silver ink composition on a copper plate were produced. Then, these two first laminates were arranged in parallel with their longitudinal directions aligned.

[0238] Next, immediately under normal pressure and in an air atmosphere, the copper chip was placed on the surface of the heated object of the silver ink composition (printed layer) in the first laminate, and a weight of 5 kg was placed on the surface of the copper chip. At this time, one copper chip was placed on one of the heated objects, and the positions of the outer periphery of the heated object and the copper chip were aligned when viewed from above. In addition, one weight was placed so as to straddle all four copper chips, and the position of the weight was adjusted so that pressure was applied evenly to these four copper chips by this one weight. In this way, a second laminate was prepared by aligning and laminating the heating object, copper chips, and weight on the surface of the copper plate. The second laminate was composed of two copper plates, four heating objects, four copper chips, and one weight. At this time, the pressure applied by the weight to one copper tip was 0.8 MPa.

[0239] Next, under normal pressure and in an air atmosphere, the temperature of the second laminate in this state was raised to 300°C over a period of 5 minutes, and the temperature was further maintained at 300°C for 30 minutes (bonding step). In other words, in this step, the copper plate and the copper chip were pressed together with the heated object interposed therebetween, and the heated object was fired, thereby bonding the copper plate and the copper chip with metallic silver. Next, the weight was removed to obtain two metal member joints in which the copper plate and the copper chip were joined with metallic silver. In these joints, the fired product of the heated material, i.e., the conductive joint made of metallic silver, was a rectangular parallelepiped with dimensions of approximately 4 mm × 4 mm × 0.03 mm. As described above, in this embodiment, the combination (A1), the preheating method (B1), and the compression-bonding and baking method (C1) were adopted.

[0240] <<Evaluation of silver ink composition>> <Measurement of Viscosity of Silver Ink Composition> The viscosity of the silver ink composition obtained above was measured at a shear rate of 1000 / s at 25° C. using a rheometer ("MCR301" manufactured by Anton Paar). The results are shown in Table 1.

[0241] <Calculation of crystallite size of metallic silver particles in silver ink composition> Using an X-ray diffraction device (Bruker AXS, D8 DISCOVER with GADDS), the silver ink composition obtained above was filled into the sample holder, and X-ray diffraction measurement was performed on the metallic silver particles in the silver ink composition under the following measurement conditions. Next, the crystallite size was calculated based on the Scherrer formula described above using the peak (2θ=38.1°) of the crystal plane with the strongest intensity in the obtained X-ray diffraction profile. The results are shown in Table 1. (Measurement conditions) ·Incidence side optical system X-ray source: CuK (wavelength 1.542Å) Output: 50kV, 100mA Monochromator: Multilayer mirror Beam size: 10mm(H)×1.0mm(W) ·Receiving side optical system Parallel Soller slit resolution: 0.12° Detector: Scintillation counter Camera distance: 15cm Scanning conditions Scanning method:-2 (Locked Coupled) Scanning speed: 3dig / min Increment: 0.02°

[0242] <<Evaluation of metal component joints>> <Measurement of die shear strength> The die shear strength of the two metal member joints obtained above was measured using a testing machine (Dage's "Bond Tester 4000") in accordance with JIS C62137-1-2:2010 (lateral shear strength test, IEC 62137-1-2:2007). This measurement was performed for every four copper chips, and the average of the four measurements was finally adopted as the die shear strength of the metal member bonded body. The results are shown in Table 2.

[0243] <Analysis of bonding state> Using a focused ion beam (FIB) device, one of the two metallic member joints obtained above was cut to expose a cross section. The cross section was observed using a transmission electron microscope (TEM), and the image data obtained at this time is shown in FIG. At this time, the cross section was further observed by energy dispersive X-ray spectroscopy (EDS, EDX). Of the acquired imaging data, imaging data when silver element was detected is shown in FIG. 10, imaging data when copper element was detected is shown in FIG. 11, and imaging data when oxygen element was detected is shown in FIG.

[0244] [Example 2] <<Manufacturing of metal component joints>> <Production of Silver Ink Composition> A silver ink composition was prepared in the same manner as in Example 1.

[0245] <Manufacturing of metal component joints> Using the same copper plate and copper chip as in Example 1, and using the same method as in Example 1, two parallel rectangular printed layers of silver ink composition measuring approximately 4 mm x 4 mm x 0.3 mm were formed on the surface of the copper plate.

[0246] Next, under normal pressure and in an atmospheric air atmosphere, the copper chip was placed on the surface of the printed layer (silver ink composition) so that when viewed from above, the positions of the outer periphery of the printed layer and the copper chip were aligned. Next, under normal pressure and in an atmospheric air atmosphere, the copper plate with the printed layer was heated from the side without the printed layer using a hot plate, and the temperature of the copper plate, the printed layer, and the copper chip was raised to 100°C over a period of 5 minutes, and the temperature was further maintained at 100°C for 1 minute (preheating step). During this time, the printed layer (i.e., the silver ink composition) did not solidify and maintained its fluidity, and bubbling was observed after the temperature reached 100°C. This bubbling disappeared before the temperature of the copper plate and the printed layer had been maintained at 100°C for 1 minute. In this manner, a heated silver ink composition was obtained. The resulting heated product did not have the luster characteristic of metallic silver and was dark green in color.

[0247] Next, immediately under normal pressure and in an air atmosphere, weights with a mass of 5 kg were placed on the surfaces of the copper chips, one weight per copper chip, and the positions of the centers of the copper chips and the weights were aligned when viewed from above. As a result of the above, two laminates were formed in which the heating object, copper chip, and weight were aligned and laminated on the surface of the copper plate. At this time, the pressure applied by the weight to one copper tip was 0.8 MPa.

[0248] Next, the bonding process was carried out in the same manner as in Example 1, and the copper plate and the copper chip were pressed together with the heated object interposed therebetween while the heated object was fired, thereby bonding the copper plate and the copper chip with metallic silver. As a result, a metal member joint was obtained in which the copper plate and the copper chip were joined by metallic silver. In this joint, the fired product of the heated material, i.e., the joint made of metallic silver, had a rectangular shape with dimensions of approximately 4 mm × 4 mm × 0.03 mm. Furthermore, another identical metal member joined body was produced by the same method, so that a total of two metal member joined bodies were produced. As described above, in this embodiment, the combination (A1), the preheating method (B2), and the compression and baking method (C1) were adopted.

[0249] <<Evaluation of silver ink composition>> The viscosity of the silver ink composition was measured, and the crystallite size of the metallic silver particles in the silver ink composition was calculated in the same manner as in Example 1. The results are shown in Table 1.

[0250] <<Evaluation of metal component joints>> <Measurement of die shear strength> Except for using the two joined metal members obtained above, the die shear strength of the joined metal members was measured in the same manner as in Example 1. The results are shown in Table 2.

[0251] <<Production and evaluation of metal component joints>> [Example 3] A metal member joint was manufactured and evaluated in the same manner as in Example 1, except that in the joining process, instead of raising the temperature of the copper plate and the laminate to 300°C over 5 minutes and then holding the temperature at 300°C for 30 minutes, the temperature of the copper plate and the laminate was raised to 250°C over 5 minutes and then held at 250°C for 30 minutes. In the obtained metal member joint in Example 3, the fired product of the heated parts, i.e., the joint made of metallic silver, had a rectangular parallelepiped shape with dimensions of approximately 4 mm × 4 mm × 0.03 mm. The results are shown in Table 2.

[0252] [Example 4] A metal member joint was manufactured and evaluated in the same manner as in Example 1, except that in the joining process, instead of raising the temperature of the copper plate and the laminate to 300°C over 5 minutes and then holding the temperature at 300°C for 30 minutes, the temperature of the copper plate and the laminate was raised to 200°C over 5 minutes and then held at 200°C for 30 minutes. In the obtained metal member joint in Example 4, the fired product of the heated material, i.e., the joint made of metallic silver, had a rectangular parallelepiped shape with dimensions of approximately 4 mm × 4 mm × 0.03 mm. The results are shown in Table 2.

[0253] [Comparative Example 1] In the preheating step, after the temperature of the copper plate and the printed layer was raised to 100°C, the time for which the temperature was maintained at 100°C was changed from 1 minute to 5 minutes (hereinafter, this step may be referred to as the "comparative preheating step"), and after the preheating step, the heated material was fired without placing a weight of 5 kg on the surface of the copper chip (hereinafter, this step may be referred to as the "comparative joining step"). Except for this, a metal member joint was manufactured and evaluated in the same manner as in Example 1. That is, in Comparative Example 1, immediately after the comparative pre-heating step, the copper chip was placed on the surface of the heated silver ink composition (printed layer) to form two comparative laminates in which the heated object and the copper chip were aligned and laminated on the surface of the copper plate.The temperature of the copper plate and the comparative laminate in this state was then raised to 300°C over 5 minutes, and the temperature was maintained at 300°C for a further 30 minutes.Thereafter, an attempt was made to join the copper plate and the copper chip with metallic silver in the same manner as in Example 1. However, in Comparative Example 1, the copper plate and the copper chip could not be joined with metallic silver, and the intended joined metal member body could not be obtained. In Comparative Example 1, at the end of the comparative pre-heating step, the printed layer (i.e., the silver ink composition) had solidified and lost fluidity. This solidified material did not have the luster characteristic of metallic silver and was dark green in color. After the temperature of the printed layer reached 100°C, bubbling was observed. In the final product obtained, the fired product of the heated product, i.e., the part composed of metallic silver, was a rectangular parallelepiped with dimensions of approximately 4 mm x 4 mm x 0.03 mm. The results are shown in Table 2.

[0254] [Comparative Example 2] In the preheating step, after the temperature of the copper plate and the printed layer was raised to 100°C, the time for which the temperature was maintained at 100°C was changed from 1 minute to 5 minutes (i.e., a comparative preheating step was performed). A metal member joint was manufactured and evaluated in the same manner as in Example 1, except that. In Comparative Example 2, at the end of the comparative pre-heating step, the printed layer (i.e., the silver ink composition) had solidified and lost fluidity. This solidified material did not have the luster characteristic of metallic silver and was dark green in color. After the temperature of the printed layer reached 100°C, bubbling was observed. In the obtained metal member joint, the fired product of the heated material, i.e., the joint made of metallic silver, was a rectangular parallelepiped with dimensions of approximately 4 mm x 4 mm x 0.03 mm. The results are shown in Table 2.

[0255] [Table 1]

[0256] [Table 2]

[0257] As is clear from the above results, in Examples 1 to 4, by performing the preheating step and the joining step, the die shear strength of the metal member joined body was 17.5 MPa or more (17.5 to 35 MPa), and the joining strength was sufficiently high. In particular, from the results of Examples 1 and 2, it was confirmed that the joining strength was further increased by placing the copper chip after the preheating step (i.e., by adopting the preheating method (B1)).

[0258] In all of Examples 1 to 4, the silver ink composition did not solidify and maintained fluidity during the preheating step. This was evident from the fact that bubbling was observed in the silver ink composition. In Example 2, the main surface of the silver ink composition (printed layer) was covered with copper chips and not exposed during the preheating step, so bubbling of the silver ink composition could not be directly confirmed. However, slight fluctuations were observed in the copper chips, so it was indirectly confirmed that bubbling was occurring in the silver ink composition. Furthermore, in all of Examples 1 to 4, the bubbling of the silver ink composition had disappeared by the end of the preheating step, and it was presumed that the generation of gas from the silver ink composition had almost or completely ceased at this stage.

[0259] In contrast, no metal member bonded body was obtained in Comparative Example 1. This was because the silver ink composition had solidified at the end of the comparative pre-heating step, and the copper plate and the copper chip were not pressure-bonded when the heated object was fired in the comparative bonding step. In Comparative Example 1, after the temperature of the silver ink composition reached 100°C, bubbling was initially observed. However, before this bubbling disappeared, the silver ink composition solidified, and the surface of the heated silver ink composition was rougher than in Examples 1 to 4 due to the bubbling.

[0260] In Comparative Example 2, the die shear strength of the metal member bonded body was 3 MPa, which was a low bonding strength, because the silver ink composition had solidified at the end of the comparative pre-heating step. In Comparative Example 2, as in Comparative Example 1, bubbling was initially observed after the temperature of the silver ink composition reached 100°C. However, before this bubbling disappeared, the silver ink composition solidified, and the surface of the heated silver ink composition was rougher than in Examples 1 to 4 due to the bubbling. However, in Comparative Example 2, unlike Comparative Example 1, the copper plate and the copper chip were pressure-bonded when the heated object was fired in the bonding step, and therefore a metal member bonded body was obtained.

[0261] FIG. 9 shows TEM image data of the boundary between the copper chip and the metallic silver (conductive joint) and the area nearby. In FIG. 9, the area on the left side of the image is the copper chip, and the area on the right side of the image is the silver metal. In FIG. 9, the colorless portions including those indicated by the arrows are minute voids (sometimes referred to as "microvoids" in this specification and drawings). As is clear from FIG. 9, two regions that were distinguishable from other regions, namely, region 9-1 and region 9-2, were observed between the copper chip and metallic silver across the top and bottom of the image.

[0262] FIG. 10 shows image data of the same region as FIG. 9 when silver element was detected by EDS (EDS). In Fig. 10, as in Fig. 9, two distinct regions, namely, region 10-1 and region 10-2, were observed between the copper chip and the metallic silver across the top and bottom of the image. The shape of region 10-1 was similar to that of region 9-1, and the shape of region 10-2 was similar to that of region 9-2. The acquired imaging data shows that fluorescence is generated in the metallic silver region and region 10-1, and elemental silver is detected in these regions. On the other hand, the imaging data does not show that significant fluorescence is generated in other regions, including region 10-2, and elemental silver is not significantly detected in these regions.

[0263] FIG. 11 shows imaging data of the same region as FIG. 9 when copper element was detected by EDS (EDS). In Fig. 11, as in Fig. 9, two distinct regions, namely, region 11-1 and region 11-2, were observed between the copper chip and the metallic silver across the top and bottom of the image. The shape of region 11-1 was similar to that of region 9-1, and the shape of region 11-2 was similar to that of region 9-2. The acquired imaging data shows that fluorescence is generated in the copper chip region and region 11-2, and copper elements were detected in these regions. On the other hand, the imaging data does not show that significant fluorescence is generated in other regions, including region 11-1, and copper elements were not significantly detected in these regions.

[0264] FIG. 12 shows imaging data of the same region as FIG. 9 when oxygen elements are detected by EDS (EDS). In Fig. 12, unlike Fig. 9, one area, namely area 12-1, which was distinguishable from other areas, was observed between the copper chip and the metallic silver across the top and bottom of the image. The shape of area 12-1 was similar to that of area 9-2. The acquired imaging data showed that fluorescence was generated in the region 12-1, and oxygen element was detected in this region. On the other hand, the imaging data suggested that weak fluorescence was generated in other regions, but the fluorescence intensity was slight compared to the fluorescence intensity in the region 12-1, and the amount of oxygen element detected was minute.

[0265] From the above results, it was found that the regions 9-1, 10-1, and 11-1 indicate the same region, and this region is a layer containing silver as a main constituent element. Moreover, the regions 9-2, 10-2, 11-2, and 12-1 indicate the same region, and it was found that this region was a layer containing copper and oxygen as main constituent elements. That is, it was found that the above-obtained joined metal member had, between the copper chip and the metallic silver, a layer mainly composed of silver and a layer mainly composed of copper and oxygen, in this order from the copper chip side to the metallic silver side. Thus, the joined metal member had a layered structure in which the copper chip, the layer mainly composed of silver, the layer mainly composed of copper and oxygen, and the metallic silver were present in this order, with the silver elements and the copper elements being arranged alternately.

[0266] The above results were obtained by analyzing the boundary between the copper chip and the metallic silver (conductive joint) and the surrounding area. Similar results were also obtained from analysis of the opposite side of the metal component joint, i.e., the boundary between the copper plate and the metallic silver (conductive joint) and the surrounding area. That is, it was found that the joined metal member had, between the copper plate and the metallic silver, a layer mainly composed of silver and a layer mainly composed of copper and oxygen, in this order from the copper plate side to the metallic silver side. Thus, the joined metal member had a layered structure in which the copper plate, the layer mainly composed of silver, the layer mainly composed of copper and oxygen, and the metallic silver were present in this order, with the silver elements and the copper elements being arranged alternately.

[0267] In the layers on both the copper chip side and the copper plate side, whose main constituent elements are copper and oxygen, oxygen may exist as a product of reaction with copper, such as copper oxide, or it may exist alone without reacting with copper.

[0268] The fact that the joined metal member body has the above-mentioned layered structure is consistent with the fact that the joined metal member body has a sufficiently large die shear strength. [Industrial Applicability]

[0269] The present invention can be used to manufacture various devices including a metal member assembly, such as a circuit board. [Explanation of symbols]

[0270] DESCRIPTION OF SYMBOLS 1, 2...Metal member assembly, 11...First metal member, 11a...First surface of first metal member, 12...Second metal member, 12a...First surface of second metal member, 13, 23...Metallic silver (conductive joint), 130...Silver ink composition, 130'...Heated product of silver ink composition

Claims

1. A metal member joint, The metal member joint body is configured by joining a first metal member and a second metal member via metallic silver, Either one or both of the first member and the second member are made of copper; When the first member is made of copper, the metal member joint body includes, between the first member and the metallic silver, a layer containing silver as a main component and a layer containing copper and oxygen as main components, in this order from the first member side toward the metallic silver side, When the second member is made of copper, the metal member joint body includes, between the second member and the metallic silver, a layer containing silver as a main component and a layer containing copper and oxygen as main components, in this order from the second member side toward the metallic silver side, One or both of the first member and the second member form a composite body with a non-metallic member, A metal member bonded body, wherein the non-metallic member is a semiconductor wafer, a semiconductor chip, an organic insulating substrate, an inorganic insulating substrate, or an organic-inorganic composite insulating substrate.

2. The semiconductor wafer or semiconductor chip is a wafer or chip made of silicon, silicon carbide, or gallium nitride; the organic insulating substrate is a polytetrafluoroethylene substrate, a polyimide substrate, a liquid crystal polymer substrate, or a cycloolefin polymer substrate; the inorganic insulating substrate is a ceramic substrate, 2. The metal member joined body according to claim 1, wherein the organic-inorganic composite insulating substrate is a glass epoxy resin substrate.

Citation Information

Patent Citations

  • Conductive bonding material, method of bonding with the same, and semiconductor device bonded with the same

    JP2010257880A

  • Metal connection structure and method for producing the same

    JP2017101314A

  • Junction structure and production method thereof

    JP2018193604A

  • METHOD FOR MANUFACTURING CIRCUIT BOARD PLATE, ... METHOD FOR MANUFACTURING SEMICONDUCTOR MODULE, AND SEMICONDUCTOR MODULE

    JP2019512867A

  • Method for producing a substrate plate, substrate plate, method for producing a semiconductor module and semiconductor module

    WO2017140574A1