Ink, method of manufacturing ink, printing method, and printing device
An ink formulation with specific components and heating process addresses image defects on non-penetrating media and coated papers, enhancing fixability, permeability, and stability.
Patent Information
- Application Number
- JP2024138515
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-01-31
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Inkjet recording methods face issues with image defects such as blurring and poor ink fixation on non-penetrating media and coated papers, leading to reduced image quality and stability.
Ink formulation containing water, an organic solvent, polyurethane resin particles, and a cyclic ester with a specific structure, heated to minimize crystal formation and improve fixability and liquid permeability.
The ink achieves high fixability, liquid permeability, and stability on non-penetrating media and coated papers, ensuring high image density and ejection stability.
Smart Images

Figure 2024159835000064 
Figure 2024159835000065 
Figure 2024159835000066
Abstract
Description
[Technical field]
[0001] The present invention relates to an ink, a method for producing an ink, a printing method, and a printing apparatus. [Background technology]
[0002] Inkjet recording methods have been rapidly spreading in recent years because they can easily record color images, have low running costs, etc. However, this method has a problem in that image defects such as character bleeding are likely to occur depending on the combination of ink and recording medium, resulting in a significant decrease in image quality. For example, non-permeable media used in signage and other media do not absorb ink, which can lead to issues such as severe bleeding and failure to fix images. Furthermore, when recording is performed on coated paper using a filler such as calcium carbonate or kaolin as a coating layer material, such as coated paper for commercial printing or publication printing, the image may bleed significantly or may not develop density.
[0003] Therefore, in order to improve drying and fixing properties, the ink composition is changing to use hydrophobic organic solvents, such as organic solvents with an SP value of 8.9 to 12.0 or organic solvents with high vapor pressure, and also to use more water-dispersible resin particles.
[0004] In addition, because non-permeable media for signage have poor ink fixation properties, it is necessary to select water-dispersible resin particle materials, and the amount of these particles added is increasing. In particular, to improve the fixation properties of ink to non-permeable media films, polyurethane resin particles synthesized from polyol raw materials containing aromatic rings are increasingly used as ink components. Although the above-mentioned changes in circumstances have improved image quality, they have caused problems in ink storage stability, ink permeability, and ink ejection stability.
[0005] Patent Document 1 discloses an invention relating to an aqueous inkjet ink that is excellent in drying property and print fixation property when printed on the surface of a hydrophobic resin medium, and also has excellent dispersion stability of the resin binder. Claim 1 specifies that the ink contains an amide solvent having a specific structure, an aqueous emulsion polymer, and a crosslinking agent for the polymer. Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide an ink that has both good fixability and good liquid permeability. [Means for solving the problem]
[0007] The above issues are as follows: <1> The above-mentioned problems are solved by the invention. <1> An ink containing water, an organic solvent, and polyurethane resin particles, the ink contains a cyclic ester having a structure represented by the following general formula (I), and after the ink is left to stand for one month in a room temperature environment (25±5°C), the content of crystals of the cyclic ester having a particle size of 1 μm or more is less than 4 ppm in the entire ink. [ka] Effect of the Invention
[0008] An object of the present invention is to provide an ink that has both good fixability and good liquid permeability. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a diagram showing an example of a printing apparatus according to the present invention. [Diagram 2] FIG. 2 is a diagram showing an example of a recording apparatus using the ink of the present invention. [Diagram 3] FIG. 3 is a perspective view of a main tank that contains the ink of the present invention. [Figure 4]FIG. 4 is an exploded perspective view showing an example of an ink ejection head used in the present invention. [Diagram 5] FIG. 5 is a cross-sectional explanatory diagram taken along the longitudinal direction of the liquid chamber of the ink ejection head. [Figure 6] FIG. 6 is a cross-sectional explanatory diagram taken along the short side direction of the liquid chamber of the ink ejection head. [Figure 7] FIG. 7 is a plan view illustrating a nozzle plate of the ink ejection head. [Figure 8] FIG. 8 is a cross-sectional explanatory view of the nozzle plate shown in FIG. [Figure 9] FIG. 9 is an enlarged cross-sectional explanatory view of one nozzle portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described below. <1> The present invention will be described in detail below. <1> The present invention relates to the following embodiment: <2> ~ <21> are also included, so these will also be explained. <1> An ink containing water, an organic solvent, and polyurethane resin particles, the ink contains a cyclic ester having a structure represented by the following general formula (I), and after the ink is left to stand for one month in a room temperature environment (25±5°C), the content of crystals of the cyclic ester having a particle size of 1 μm or more is less than 4 ppm in the entire ink. [ka] <2> The polyurethane resin contains a polyurethane resin having a structure represented by the general formula (I). <1> The ink described in <3> The ink contains a colorant. <1> or <2> The ink described in <4> The solid content of the polyurethane resin particles in the ink is 3% by mass or more, and the solid content ratio of the colorant to the polyurethane resin particles is 1.0:(2.0 to 11.0). <3> The ink described in <5> The above, wherein the colorant is a pigment. <3> or <4> The ink described in <6> The organic solvent contains a diol compound and an organic solvent having a solubility parameter (SP value) of 8.9 to 12.0. <1> ~ <5> 13. The ink according to any one of claims 1 to 12. <7> The ink has a pH of 8.5 or more. <1> ~ <6> 13. The ink according to any one of claims 1 to 12. <8> The ink contains a strongly basic compound. <7> The ink described in <9> The method according to any one of claims 1 to 4, wherein the strongly basic compound is sodium hydroxide or potassium hydroxide. <8> The ink described in <10> The ink further contains a polyether-modified siloxane compound as a surfactant. <1> ~ <9> 13. The ink according to any one of claims 1 to 12. <11> A method for producing an ink containing water, an organic solvent, and polyurethane resin particles, comprising the steps of: mixing water, an organic solvent, and polyurethane resin particles; and heating the mixture obtained by the above step at a temperature of 40° C. or higher but lower than 70° C. for 6 hours or longer. <1> ~ <10> 13. A method for producing the ink according to any one of claims 1 to 12. <12> The ink further contains a colorant, and the method comprises the steps of mixing water, an organic solvent, polyurethane resin particles, and the colorant, and heating the mixture obtained by the above steps at a temperature of 40° C. or higher but lower than 70° C. for 6 hours or more. <11> A method for producing the ink described above. <13> the above <1> ~ <10> 2. A printing method comprising a step of depositing the ink according to any one of claims 1 to 11 onto a substrate and printing. <14> the step of depositing the ink on a substrate and printing the ink is a step of ejecting the ink from an ink ejection head having a nozzle plate that ejects the ink, and depositing the ink on the substrate; The ink contains water, an organic solvent, polyurethane resin particles, and a cyclic ester having a structure represented by the following general formula (I), and after being left to stand for one month in a room temperature environment (25±5° C.), the content of crystals of the cyclic ester having a particle size of 1 μm or more is less than 4 ppm in the entire ink, and the receding contact angle with respect to the nozzle plate is 35° or more. <13> A printing method according to claim 1. [ka] <15> the above <1> ~ <10> 2. A printing device comprising an ink cartridge containing the ink according to claim 1, and a discharge means for discharging the ink. <16> The ink cartridge according to any one of the preceding claims, wherein a filter is provided between the ink flow path and the ink ejection means for ejecting the ink. <15> The printing device described in <17> The ink ejection means is an ink ejection head having a nozzle plate for ejecting the ink, and a receding contact angle of the ink with respect to the nozzle plate is 35° or more. <15> or <16> The printing device described in <18> The nozzle plate has an ink-repellent film, and the ink-repellent film of the nozzle plate contains a fluorine-containing acrylate ester polymer. <17> The printing device described in <19> The fluorine-containing acrylate ester polymer comprises a polymer obtained by polymerizing at least one of a compound represented by the following general formula (II) and a compound represented by the following general formula (III): <18> The printing device described in [ka] [ka] In the general formulas (II) and (III), X is any one of a hydrogen atom, a linear or branched alkyl group having 1 to 21 carbon atoms, a halogen atom, a CFX1X2 group (wherein X1 and X2 are each independently a hydrogen atom or a halogen atom), a cyano group, a linear or branched fluoroalkyl group having 1 to 21 carbon atoms, a substituted or unsubstituted benzyl group, and a substituted or unsubstituted phenyl group, R1 is an alkyl group having 1 to 18 carbon atoms, R2 is an alkylene group having 2 to 6 carbon atoms, R3 is an alkylene group having 2 to 6 carbon atoms, Y is an acid group, and Rf is a linear or branched fluoroalkyl group having 1 to 21 carbon atoms. m is 1 to 10, n is 2 to 90, p is 1 to 90, and q is 1 to 10. <20> The fluorine-containing acrylate ester polymer contains a polymer having at least one of a structural unit represented by the following general formula (IV) and a structural unit represented by the following general formula (V): <19> The printing device described in [ka] [ka] In the general formulas (IV) and (V), X is any one of a hydrogen atom, a linear or branched alkyl group having 1 to 21 carbon atoms, a halogen atom, a CFX1X2 group (wherein X1 and X2 are each independently a hydrogen atom or a halogen atom), a cyano group, a linear or branched fluoroalkyl group having 1 to 21 carbon atoms, a substituted or unsubstituted benzyl group, and a substituted or unsubstituted phenyl group, R1 is an alkyl group having 1 to 18 carbon atoms, R2 is an alkylene group having 2 to 6 carbon atoms, R3 is an alkylene group having 2 to 6 carbon atoms, Y is an acid group, and Rf is a linear or branched fluoroalkyl group having 1 to 21 carbon atoms. m is 1 to 10, n is 2 to 90, p is 1 to 90, and q is 1 to 10. <21> The ink-repellent film comprises a polymer having a fluorine-containing heterocyclic structure in its main chain. <18> ~ <20> 2. The printing apparatus according to claim 1 ,
[0011] (ink) The ink of the present invention is an ink containing water, an organic solvent, and polyurethane resin particles, the ink containing a cyclic ester having a structure represented by the following general formula (I), and after the ink is left to stand for one month in a room temperature environment (25±5°C), the content of crystals of the cyclic ester having a particle size of 1 μm or more is less than 4 ppm in the entire ink. [ka]
[0012] In particular, since non-permeable media for signage have poor ink fixation properties, it is necessary to select a water-dispersible resin particle material or increase the amount added. Furthermore, to improve the ink fixation properties to non-permeable media films, there are an increasing number of cases where polyurethane resin particles synthesized from a polyol raw material containing an aromatic ring and having the structure shown in general formula (I) below are used as an ink component. [ka]
[0013] However, the polyol raw material containing an aromatic ring having the structure represented by general formula (I) used as a raw material for polyurethane resin particles contains, as a by-product, a cyclic ester having the structure represented by general formula (I) which is difficult to dissolve in water and water-soluble solvents. Since this is contained in the high-viscosity polyol, it becomes polyurethane resin particles in a state where it cannot be removed. When ink is produced using the polyurethane resin particles and the ink is placed in an ink pack and left to stand at room temperature (25±5°C) for one month or more, the cyclic ester compound having the structure represented by general formula (I) is eluted from the polyurethane resin particles, and cyclic ester crystals having the structure represented by general formula (I) are precipitated in the ink. It was found that the precipitation of the cyclic ester crystals in the ink deteriorates the ink permeability and also makes the ejection unstable.
[0014] The cyclic ester having the structure represented by general formula (I) contained in the ink is thought to include raw materials used in the production of the polyurethane resin and by-products of the raw materials, and examples thereof include the cyclic ester represented by the following structural formula A. [ka] In the above structural formula (A), R represents an alkylene group, and is usually an alkylene group having 3 to 10 carbon atoms. It was found that raw materials and by-products that are not removed during the purification or ink manufacturing process end up being contained in the ink, and over time, the cyclic ester having the structure represented by general formula (I) crystallizes in the ink. The present inventors have found that the object of the present invention can be achieved by providing an ink in which the content of crystals of the cyclic ester having the structure represented by general formula (I) with a particle size of 1 μm or more is less than 4 ppm in the entire ink. Furthermore, according to the present invention, it is possible to provide an ink that has high fixation and drying properties even on non-permeable media for signage and commercial printing paper, has high image density, and has good liquid permeability, ejection stability, and excellent storage stability.
[0015] Cyclic esters having the structure represented by general formula (I) are usually insoluble in water. Even if no cyclic esters having the structure represented by general formula (I) are found in the water of the aqueous dispersion of urethane resin particles, when the aqueous dispersion of urethane resin particles is mixed with other components such as an organic solvent to produce an ink, crystals of the cyclic esters having the structure represented by general formula (I) may precipitate in the ink. It is presumed that the cyclic esters having the structure represented by general formula (I) contained in the urethane resin particles are dissolved and crystallized by mixing with the organic solvent.
[0016] It was found that when the ink was left to stand at room temperature (25±5°C) for one month or more, if the ink contained 4 ppm or more of cyclic ester crystals with a particle size of 1 μm or more, practical problems occurred in the liquid permeability, and ultimately ejection failure occurred. It was also confirmed that if the ink contained less than 4 ppm of cyclic ester crystals with a particle size of 1 μm or more, there was no practical problem. Here, "less than 4 ppm" in the entire ink means that the content of crystals relative to the mass of the entire ink is less than 0.0004% by mass. Moreover, stationary storage means storage without intentionally subjecting the product to vibration. Furthermore, the amount of precipitation of the cyclic ester crystals is reduced by heating an ink containing a cyclic ester compound having a structure represented by general formula (I) at a temperature of 40° C. or higher and lower than 70° C. for 6 hours or longer, and it has also been found that the cyclic ester crystals precipitated in the ink disappear.
[0017] However, the mechanism by which the amount of cyclic ester crystals precipitated is reduced and the mechanism by which the cyclic ester crystals disappear are not clear. In the case of heating at 40°C, the precipitation of the cyclic ester crystals is reduced by heating at 40°C for two weeks or more. In the case of heating at 68°C, the precipitation of the cyclic ester crystals is eliminated by heating at 68°C for six hours, and the cyclic ester crystals precipitated in the ink also disappear. The heating time is preferably from 2 weeks to 1 month when heating at 40°C, and preferably from 6 hours to 12 hours when heating at 68°C. Heating to temperatures below 40° C. has no effect at all in reducing the precipitation of cyclic ester crystals, while heating to temperatures above 70° C. can cause the ink properties to change and ink separation to occur. It is particularly preferable to store the ink at a temperature of 55°C to 65°C for 12 to 24 hours, as this is very effective and causes little damage to the ink.
[0018] In the present invention, the precipitated crystals are filtered using a filter paper with a particle retention capacity of 1 μm (e.g., Kiriyama funnel filter paper No. 5C), and the mass of the filter paper before filtration, the mass of the crystals retained after filtration, and the mass of the filter paper are weighed and the difference is calculated to quantify the crystals of the cyclic ester having the structure represented by general formula (I). Therefore, the crystals retained after filtration have a particle size of 1 μm or more, and the amount of crystals of the cyclic ester having the structure represented by general formula (I) with a particle size of 1 μm or more is less than 4 ppm of the entire ink.
[0019] Although the mechanism by which the cyclic ester crystals decrease and disappear is only speculation, it is believed that when the ink is heated in the presence of a pH adjuster (basic compound) contained in the ink, the cyclic ester compound is hydrolyzed, and a basic compound is added to the ring-opened carboxyl group, resulting in a water-soluble compound, which ultimately causes the cyclic ester crystals in the ink to decrease and disappear. Under the above circumstances, the image quality was improved, and the ink storage stability, liquid permeability and ejection stability were also improved.
[0020] The ink containing the cyclic ester having the structure represented by the general formula (I) can be confirmed by separating the crystals precipitated in the ink from the ink and analyzing them by GC-MS and LC-MS+C. 13 -NMR+H 1 -Qualitative analysis can be performed using NMR and FT-IR.
[0021] In order to ensure sufficient wetting of the ink on non-permeable media for signage and commercial printing paper, it is preferable to reduce the dynamic surface tension of the ink at a surface life of 15 msec as measured by the maximum bubble pressure method at 25°C to 34.0 mN / m or less, and to maintain the static surface tension of the ink at 25°C to 20.0 mN / m or more. Under the above circumstances, the image quality was improved, and the ink storage stability, liquid permeability and ejection stability were also improved.
[0022] The dynamic surface tension of the ink at a surface life of 15 msec according to the maximum bubble pressure method can be measured at 25° C. using, for example, a SITA DynoTester (manufactured by SITA). The static surface tension of the ink can be measured at 25° C. using, for example, an automatic surface tensiometer (DY-300, manufactured by Kyowa Interface Science Co., Ltd.). By optimizing the balance between the dynamic surface tension and the static surface tension in the ink and making the receding contact angle of the ink with respect to the nozzle plate 35° or more, the ink is less likely to wet the ink-repellent film of the nozzle plate of the ink ejection head, ejection stability can be ensured, and an extremely stable and ideal printing device is achieved in which no nozzles are missing during continuous ejection.
[0023] The receding contact angle of the ink with respect to the nozzle plate is 35° or more, preferably 35° or more and 80° or less, and more preferably 40° or more and 70° or less. If the receding contact angle is 35° or more, even if ink adheres to the inner wall surface of the ink chamber of the ink ejection head, the ink is easily repelled again. Note that the larger the receding contact angle, the more difficult it becomes to wet, so the upper limit of the receding contact angle is not particularly limited in terms of wettability, but it is preferable that it does not exceed 80° (80° or less) in consideration of wettability and permeability to the recording medium. The receding contact angle can be measured, for example, using an automatic contact angle measuring device_expansion / contraction method. The automatic contact angle measuring device may be, for example, a contact angle meter DMo-501 (manufactured by Kyowa Interface Science Co., Ltd.). The receding contact angle can be measured, for example, by using the nozzle plate used in the present invention, extruding 2 μL of ink from a syringe onto the outer surface of the nozzle plate, and using the above-mentioned device by the contraction method. The receding contact angle in the present invention means a value at a measurement temperature of 25° C.
[0024] The static surface tension B of the ink at 25° C. is preferably 20.0 mN / m or more and 30.0 mN / m or less. When the static surface tension is 20.0 mN / m or more and 30.0 mN / m or less, the ink can sufficiently increase the wettability of the ink to non-penetrable media for signage and commercial printing paper, thereby improving the effect of reducing cockling and curling, and achieving good penetration and drying even when printing on ordinary paper.
[0025] Next, the ink and the method for producing the ink will be described in detail. <Ink> -Organic solvents- The ink of the present invention preferably contains at least one organic solvent having a solubility parameter (SP value) of 8.9 to 12.0 (hereinafter referred to as "organic solvent X"). This improves wettability to recording media, and enables the ink components to penetrate into commercial printing paper such as coated paper with a coating layer that has poor ink absorption, thereby suppressing beading. In addition, the ink also becomes more easily wetted onto non-permeable media. As described later, the ink of the present invention preferably contains a diol as an organic solvent, but the diol compound may also serve as an organic solvent having a solubility parameter (SP value) of 8.9 to 12.0. This improves wettability to recording media, and the ink components can penetrate into commercial printing paper such as coated paper with a coating layer that has poor ink absorption, thereby suppressing beading. In addition, the ink also becomes more easily wetted on non-permeable media.
[0026] Organic solvents with an SP value of 8.9 or more are generally highly soluble in water and are less likely to separate, making them suitable for use in water-based inks such as those of the present invention. Organic solvents with an SP value of 12.0 or less have good drying properties and are less susceptible to beading. The SP value is a value defined by the regular solution theory introduced by Hildebrand, and serves as a measure of the solubility of a binary solution. The SP value in the present invention is a value calculated by the Fedors method. It is expressed as the square root of the cohesive energy density in the regular solution theory, and its unit is (J / cm 3 ) 0.5 This can be calculated using commonly available simple software.
[0027] The organic solvent X is preferably a water-soluble one, and is particularly preferably an amide compound of the following general formula (VI) or an oxetane compound of the following general formula (VII).
[0028] [ka] (In the formula, R represents an alkyl group having 1 to 6 carbon atoms.)
[0029] [ka] (In the formula, R1 represents an alkyl group having 1 to 2 carbon atoms.)
[0030] Examples of the amide compound represented by the general formula (VI) include the compounds represented by the following formulae (1) to (4). [ka]
[0031] Moreover, examples of the oxetane compound represented by the general formula (VII) include the compounds represented by the following formulae (5) to (6). [ka]
[0032] The content of the organic solvent X is preferably 3% by mass or more of the total ink, and more preferably 5 to 20% by mass. If the content is 5% by mass or more, the ink components penetrate into commercial printing paper, making it possible to suppress beading, and the ink components can easily wet non-penetrating media. If the content is 20% by mass or less, the ink viscosity does not increase, which does not deteriorate the ejection stability.
[0033] Furthermore, in the present invention, by incorporating a glycol ether compound (compound Z) that exhibits a vapor pressure of 50 mmHg or more in an environment of 100°C as an organic solvent, drying properties are improved, and high drying properties can be achieved even on commercial printing paper. In addition, even if the image area comes into contact with the transport roller immediately after hot air drying at 100°C, the image is not transferred, ensuring high-speed productivity. Compound Z is preferably one that dissolves in high-purity water. Examples include propylene glycol monopropyl ether (bp 150°C, vapor pressure 107mmHg), propylene glycol monoethyl ether (bp 133°C, vapor pressure 252mmHg), propylene glycol monomethyl ether (bp 120°C, vapor pressure 360mmHg), propylene glycol monobutyl ether (bp 170°C, vapor pressure 59mmHg), 3-methoxy-1-butanol (bp 161°C, vapor pressure 76mmHg), and 3-methoxy-3-methyl-1-butanol (bp 174°C, vapor pressure 50mmHg).
[0034] The content ratio (mass ratio) of the organic solvent X to the compound Z in the ink is preferably 1:1 to 8:1. More preferably, it is 3:1 to 5:1. When this ratio is 1:1 or more, that is, when the organic solvent X is more than the compound Z, the ink does not dry too well, and the inkjet head does not dry out, causing problems in ejection stability. When the ratio is 8:1 or less, the organic solvent X is not too much, and the ink improves drying on commercial printing paper, improving productivity. The total content of the organic solvents in the ink, including the organic solvent X and the compound Z, is preferably 5 to 30% by mass of the entire ink. If it is 5% by mass or more, the effect of suppressing beading on commercial printing paper is not reduced. Also, if it is 30% by mass or less, the ink viscosity does not increase significantly, causing problems in ejection stability.
[0035] In addition, for the sake of ejection stability and ink storage stability, it is preferable to contain polyhydric alcohols as an organic solvent. Specifically, diethylene glycol (bp 245°C), triethylene glycol (bp 285°C), tetraethylene glycol (bp 324 to 330°C), 1,3-butanediol (bp 203 to 204°C), glycerin (bp 290°C), diglycerin (bp 270°C / 20hPa), 1,2,3-butanetriol (bp 175°C / 33hPa), 1,2,4-butanetriol (bp 190 to 191°C / 24hPa), dipropylene glycol (bp 232°C), 1,5-pentanediol (bp 242°C), propylene glycol (bp 252°C), propylene glycol (bp 262°C), propylene glycol (bp 270°C / 20hPa), propylene glycol (bp 282°C), propylene glycol (bp 270°C / 20hPa ... Examples include propylene glycol (bp 187°C), 2-methyl-2,4-pentanediol (bp 197°C), ethylene glycol (bp 196 to 198°C), tripropylene glycol (bp 267°C), hexylene glycol (bp 197°C), polyethylene glycol (viscous liquid to solid), 1,6-hexanediol (bp 253 to 260°C), 1,2,6-hexanetriol (bp 178°C), trimethylolethane (solid, mp 199 to 201°C), and trimethylolpropane (solid, mp 61°C).
[0036] The organic solvent preferably contains at least one non-wetting polyol compound or glycol ether compound having 8 to 11 carbon atoms. The polyol compound preferably contains a diol compound. Here, non-wetting means that the solubility is between 0.2 and 5.0% by mass in water at 25°C. Among these compounds, 1,3-diol compounds represented by the following general formula (VIII) are preferred, and 2-ethyl-1,3-hexanediol [solubility: 4.2% (25°C)] and 2,2,4-trimethyl-1,3-pentanediol [solubility: 2.0% (25°C)] are particularly preferred. [ka] (In the above formula, R' is a methyl group or an ethyl group, R'' is a hydrogen or a methyl group, and R''' is an ethyl group or a propyl group.)
[0037] Other non-wetting polyol compounds include, for example, aliphatic diols such as 2-ethyl-2-methyl-1,3-propanediol, 3,3-dimethyl-1,2-butanediol, 2,2-diethyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, 2,4-dimethyl-2,4-pentanediol, 2,5-dimethyl-2,5-hexanediol, 5-hexene-1,2-diol, and the like. The content of the non-wetting polyol compound and glycol ether compound having 8 to 11 carbon atoms in the ink is preferably 0.5 to 4 mass%, more preferably 1 to 3 mass%. If it is 0.5 mass% or more, the ink can have a penetrating effect, and image quality can be improved. If it is 4 mass% or less, it can be sufficiently dissolved in the ink, and problems such as separation or high initial ink viscosity do not occur.
[0038] -Water dispersible resin particles- Water-dispersible resin particles that are excellent in film-forming properties (image forming properties) and also have solvent resistance, high water resistance, and high weather resistance are useful for recording images with high water resistance and high image density (high color development), and examples of such particles include condensation-based synthetic resins, addition-based synthetic resins, and natural polymer compounds. The present invention contains polyurethane resin particles. In addition, because non-permeable media for signage have poor ink fixation, it is necessary to select the material of the water-dispersible resin particles or increase the amount added. Furthermore, to improve the fixation to the film of non-permeable media, polyurethane resin particles synthesized from a polyol raw material containing an aromatic ring with the structure shown in general formula (I) are often used. [ka]
[0039] Examples of polyol raw materials containing an aromatic ring having the structure represented by the general formula (I) include terephthalic acid, isophthalic acid, etc. When terephthalic acid or isophthalic acid is used as a raw material, a cyclic ester compound is generated. When the above two types of raw materials are used, it has been confirmed by GC-MS that a cyclic ester containing a mixture of two types of phthalic acid is generated. In the present invention, the polyurethane resin particles preferably contain polyurethane resin particles having a structure represented by general formula (I) using a polyol raw material containing an aromatic ring having the structure represented by general formula (I) as a raw material for the polyurethane resin particles. The proportion of the aromatic ring-containing polyol raw material having the structure represented by the general formula (I) in the polyurethane resin particles having the structure represented by the general formula (I) is about half of the polyol, and is preferably about 10 to 30% in the polyurethane resin. When the proportion of the polyol raw material is within the above range, the polyurethane resin has excellent alcohol resistance. The content of the polyurethane resin particles having the structure represented by general formula (I) is preferably in the range of 2.0 to 20.0 mass % in terms of resin solid content, and more preferably 2.8 to 15.0 mass %.
[0040] Other examples of condensation synthetic resins include polyester resins, polyurethane resins, polyepoxy resins, polyamide resins, polyether resins, poly(meth)acrylic resins, acrylic-silicone resins, fluorine-based resins, etc. Examples of the addition synthetic resins include polyolefin resins, polystyrene-based resins, polyvinyl alcohol-based resins, polyvinyl ester-based resins, polyacrylic acid-based resins, unsaturated carboxylic acid-based resins, etc. Examples of the natural polymer compounds include celluloses, rosins, natural rubber, etc. Among these, polyurethane resin particles are preferred in consideration of the fixability of the ink. Two or more kinds of the water-dispersible resins may be used in combination.
[0041] As the water-dispersible resin, those which have hydrophilic groups and are self-dispersible, and those which do not have dispersibility but are provided with dispersibility by a surfactant or a resin having hydrophilic groups can be used. Among these, emulsions of resin particles obtained by emulsifying and suspension polymerizing ionomers of polyester resins or polyurethane resins or unsaturated monomers are optimal. In the case of emulsion polymerization of unsaturated monomers, a resin emulsion is obtained by reacting in water to which an unsaturated monomer, a polymerization initiator, a surfactant, a chain transfer agent, a chelating agent, a pH adjuster, etc. have been added. This makes it easy to obtain a water-dispersible resin, and it is easy to change the resin composition and create the desired properties.
[0042] Since the water-dispersible resin undergoes dispersion destruction or hydrolysis or other cleavage of molecular chains under strong alkaline or strong acidic conditions, the pH is preferably 4 to 12, and from the viewpoint of miscibility with the water-dispersible colorant in particular, a pH of 7 to 11 is more preferable, and a pH of 8 to 10.5 is even more preferable.
[0043] In addition, the water-dispersible resin has the function of fixing the water-dispersible colorant to the media, and has the function of forming a film at room temperature or higher to improve the fixation of the colorant. Therefore, the minimum film-forming temperature (MFT) of the water-dispersible resin is preferably 100°C or lower. In addition, if the glass transition temperature of the water-dispersible resin is -40°C or lower, the viscosity of the resin film increases and tack occurs in the printed matter, so the glass transition temperature is preferably -30°C or higher. The content of the water-dispersible resin in the ink is preferably from 0.5 to 20% by mass, and more preferably from 1 to 15% by mass, in terms of solid content. However, taking into full consideration the substrate fixation of the colorant to non-permeable media for signage and commercial printing paper, the ink contains polyurethane resin particles at a solid content of 3 mass% or more, and the solid content ratio of the colorant to the polyurethane resin particles is preferably 1.0: (2.0 to 12.0), and particularly preferably 1.0: (2.0 to 11.0). The content of the polyurethane resin particles is the total amount of polyurethane resin particles, which are the solid content contained in the ink.
[0044] -Coloring agent- The ink of the present invention may be a clear ink that does not contain a colorant, but may also be an ink that contains a colorant. The colorant is preferably a pigment. Colorants include surfactant-dispersed pigments in which a pigment is dispersed in a surfactant, resin-dispersed pigments in which a pigment is dispersed in a resin, resin-coated pigments in which the surface of a pigment is coated with a resin, and self-dispersed pigments in which a hydrophilic group is provided on the pigment surface, but water-dispersible pigments are preferred. Among these, the resin-coated pigments and self-dispersed pigments having at least one hydrophilic group on the pigment surface are preferred. Examples of such hydrophilic groups include -COOM, -SO3M, -PO3HM, -PO3M2, -CONM2, -SO3NM2, -NH-C6H4-COOM, -NH-C6H4-SO3M, -NH-C6H4-PO3HM, -NH-C6H4-PO3M2, -NH-C6H4-CONM2, and -NH-C6H4-SO3NM2. These hydrophilic groups can be introduced by known methods.
[0045] The counter ion M in the hydrophilic group is preferably a quaternary ammonium ion, specific examples of which include a tetramethylammonium ion, a tetraethylammonium ion, a tetrapropylammonium ion, a tetrabutylammonium ion, a tetrapentylammonium ion, a benzyltrimethylammonium ion, a benzyltriethylammonium ion, and a tetrahexylammonium ion, with the tetraethylammonium ion, tetrabutylammonium ion, and benzyltrimethylammonium ion being preferred, and the tetrabutylammonium ion being particularly preferred. Inks using the above pigments have particularly high storage stability over time and suppress an increase in viscosity when water evaporates. This is presumably because the pigment dispersion is kept stable due to the hydrophilic group containing the quaternary ammonium ion, even when the water evaporates from the water-rich ink and the ink becomes organic solvent-rich.
[0046] As a colorant other than the pigment having a hydrophilic group, a polymer emulsion containing a pigment in polymer fine particles is preferred. The pigment may be encapsulated in the polymer fine particles or adsorbed on the surface of the polymer fine particles. In this case, it is not necessary for all the pigment to be encapsulated or adsorbed, and a part of the pigment may be dispersed in the emulsion. Examples of polymers for polymer fine particles include vinyl polymers, polyester polymers, and polyurethane polymers, and vinyl polymers and polyester polymers are particularly preferred. Specific examples thereof include those disclosed in Japanese Patent Application Laid-Open Nos. 2000-53897 and 2001-139849.
[0047] In addition, a general organic pigment or a composite pigment in which inorganic pigment particles are coated with an organic pigment or carbon black can also be used. The composite pigment can be prepared by a method of precipitating an organic pigment in the presence of inorganic pigment particles, or a mechanochemical method of mechanically mixing and grinding an inorganic pigment and an organic pigment. Furthermore, if necessary, a layer of an organosilane compound generated from polysiloxane and alkylsilane can be provided between the inorganic pigment and the organic pigment to improve the adhesion between them. The mass ratio of the inorganic pigment particles to the organic pigment or carbon black coloring material is preferably 3:1 to 1:3, and more preferably 3:2 to 1:2. When the amount of the coloring material is within the above range, the color development and coloring power are not reduced, and the transparency and color tone are not deteriorated. As the composite pigment, silica / carbon black composite material, silica / phthalocyanine PB15:3 composite material, silica / disazo yellow composite material, silica / quinacridone PR122 composite material, and the like manufactured by Toda Kogyo Co., Ltd. are suitable because they have a small average primary particle size.
[0048] Here, when inorganic pigment particles with a primary particle diameter of 20 nm are covered with an equal amount of organic pigment, the primary particle diameter of this pigment will be about 25 nm. If an appropriate dispersant can be used to disperse this down to the primary particles, it will be possible to produce a very fine pigment dispersion ink with a dispersed particle diameter of 25 nm. In the above composite pigment, not only does the organic pigment on the surface contribute to the dispersion, but the properties of the inorganic pigment in the center also appear through a thin layer of organic pigment about 2.5 nm thick, so it is also important to select a pigment dispersant that can simultaneously stabilize the dispersion of both.
[0049] Examples of the inorganic pigment include titanium oxide, iron oxide, calcium carbonate, barium sulfate, aluminum hydroxide, barium yellow, cadmium red, chrome yellow, carbon black, etc. Among these, carbon black is particularly preferable, and examples thereof include channel black, furnace black, gas black, lamp black, etc., which are produced by known methods such as a contact method, a furnace method, and a thermal method.
[0050] Examples of the organic pigment include azo pigments, polycyclic pigments, dye chelates, nitro pigments, nitroso pigments, and aniline black. Among these, azo pigments and polycyclic pigments are preferred. Examples of the azo pigments include azo lakes, insoluble azo pigments, condensed azo pigments, and chelate azo pigments. Examples of the polycyclic pigments include phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, indigo pigments, thioindigo pigments, isoindolinone pigments, and quinophthalone pigments. Examples of the dye chelates include basic dye chelates and acid dye chelates.
[0051] Examples of the organic pigments include CI Pigment Yellow 1, 3, 12, 13, 14, 17, 24, 34, 35, 37, 42 (yellow iron oxide), 53, 55, 74, 81, 83, 95, 97, 98, 100, 101, 104, 408, 109, 110, 117, 120, 128, 139, 150, 151, 155, 153, 180, and 183. , 185, 213, CI Pigment Orange 5, 13, 16, 17, 36, 43, 51, CI Pigment Red 1, 2, 3, 5, 17, 22, 23, 31, 38, 48:2, 48:2 (Permanent Red 2B (Ca)), 48:3, 48:4, 49:1, 52:2, 53:1, 57:1 (Brilliant Carmine 6B), 60:1, 6 3:1, 63:2, 64:1, 81, 83, 88, 101 (Red oxide), 104, 105, 106, 108 (Cadmium red), 112, 114, 122 (Quinacridone magenta), 123, 146, 149, 166, 168, 170, 172, 177, 178, 179, 185, 190, 193, 209, 219, CI Pigment CI Pigment Green 1, 4, 7, 8, 10, 17, 18, 36, and others.
[0052] The BET specific surface area of the pigment used is preferably about 10 to about 1500 m 2 / g, more preferably about 20 to about 600 m 2 / g, more preferably about 50 to about 300 m 2 / g. If the desired specific surface area is not readily available, the pigment can be subjected to conventional size reduction or milling processes (e.g., ball milling, jet milling, sonication) to reduce the particle size of the pigment to a relatively small particle size. The median diameter (D50) of the water-dispersible colorant in the ink is preferably 10 to 200 nm. The content of the water-dispersible colorant in the ink is preferably 1 to 15 mass % in terms of solid content, and more preferably 1.5 to 10 mass %. If the content is 1 mass % or more, the color development and image density of the ink are improved, and if it is 15 mass % or less, the ink does not thicken and the ejection properties are not deteriorated, and it is also economically preferable. In the present invention, dyes may be used in combination for the purpose of adjusting the color tone, but they must be used within a range that does not deteriorate the weather resistance.
[0053] -Surfactants- In the present invention, it is preferable to use a polyether-modified siloxane compound as a surfactant. This makes the ink less likely to wet the ink-repellent layer of the head nozzle plate, prevents ejection failure due to ink adhesion to the nozzle, and improves ejection stability. In addition, the ink is less likely to adhere to the nozzle ink-repellent layer surface, which is particularly prone to problems, and makes the ink less likely to cause ejection failure. Among them, those represented by the following general formulas (IX) to (XII) are preferred, and in particular, those which do not impair dispersion stability depending on the type of water-dispersible colorant or the combination with an organic solvent, have low dynamic surface tension, and have high penetrability and leveling properties are preferred. These surfactants may be used alone or in combination of two or more.
[0054] [ka] (In the above formula, R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, m represents an integer of 0 to 23, n represents an integer of 1 to 10, a represents an integer of 1 to 23, and b represents an integer of 0 to 23.)
[0055] Examples of the compound represented by the above general formula (IX) include the compounds represented by the following formulae (7) to (14). [ka]
[0056] [ka]
[0057] [ka] (In the above formula, R2 and R3 represent a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, m represents an integer of 1 to 8, and c and d represent integers of 1 to 10.)
[0058] An example of the compound represented by the above general formula (X) is the compound represented by the following formula (15). [ka]
[0059] [ka] (In the above formula, R4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and e represents an integer of 1 to 8.)
[0060] An example of the compound represented by the above general formula (XI) is the compound represented by the following formula (16). [ka]
[0061] [ka] (In the above formula, R5 represents a polyether group of the following general formula (A), and f represents an integer of 1 to 8.)
[0062] [ka] (In the above formula, R6 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, g represents an integer of 0 to 23, and h represents an integer of 0 to 23, except for the case where g and h are both 0.)
[0063] Examples of the compound represented by the above general formula (XII) include the compounds represented by the following formulae (17) to (19). [ka]
[0064] Furthermore, commercially available polyether-modified siloxane compound surfactants that have the same effect as the above compounds include TORAY Dow Corning's 71ADDITIVE, 74ADDITIVE, 57ADDITIVE, 8029ADDITIVE, 8054ADDITIVE, 8211ADDITIVE, 8019ADDITIVE, 8526ADDITIVE, FZ-2123, and FZ-2191; Momentive Performance Materials' TSF4440, TSF4441, TSF4445, TSF4446, TSF4450, TSF4452, and TSF4460; and Nissin Chemical Industry's Silface. Examples of the antibacterial agents include SAG002, Silface SAG003, Silface SAG005, Silface SAG503A, Silface SAG008, Silface SJM003, TEGO_Wet_KL245, TEGO_Wet_250, TEGO_Wet_260, TEGO_Wet_265, TEGO_Wet_270, TEGO_Wet_280 manufactured by Evonik, and BYK-345, BYK-347, BYK-348, BYK-375, BYK-377 manufactured by BYK Japan.
[0065] If necessary, the polyether-modified siloxane compound surfactant may be used in combination with a fluorine-based surfactant, a silicone-based surfactant, or an acetylene glycol or acetylene alcohol-based surfactant. The content of the surfactant in the ink is preferably 0.001 to 5% by mass, and more preferably 0.5 to 3% by mass. If the content is 0.001% by mass or more, the effect of adding the surfactant can be obtained. However, when the amount exceeds 5 mass, the effect of addition becomes saturated, so there is no point in increasing the amount.
[0066] -Other ingredients- In addition to the above-mentioned components, the ink of the present invention may contain various known additives as necessary, such as a penetrating agent, a foam suppressant (defoamer), a pH adjuster, an antiseptic / fungal agent, a chelating agent, a rust inhibitor, an antioxidant, an ultraviolet absorber, an oxygen absorber, and a light stabilizer.
[0067] - Foam suppressor - A foam suppressor is added in small amounts to the ink to suppress foaming. Here, foaming refers to a liquid that turns into a thin film and encases air. The generation of this foam is related to the characteristics of the ink, such as the surface tension and viscosity. That is, liquids with high surface tension, such as water, are less likely to foam because of the force that tries to make the surface area of the liquid as small as possible. In contrast, inks with high viscosity and high permeability tend to foam easily because of their low surface tension, and the generated bubbles tend to be maintained due to the viscosity of the solution, making them difficult to eliminate.
[0068] Usually, foam suppressors destroy bubbles by locally lowering the surface tension of the foam film, or by dotting the foaming liquid surface with foam suppressors that are insoluble in the foaming liquid. When the ink contains a polyether-modified siloxane compound surfactant, which has a very strong effect of lowering surface tension, the foaming liquid surface tension cannot be locally lowered even with the use of a foam suppressor that uses the former mechanism. Therefore, the latter foam suppressor that is insoluble in the foaming liquid is used, but in this case, the stability of the ink is reduced by the foam suppressor that is insoluble in the solution. In contrast, the foam suppressor of the following general formula (XIII) is not as effective at lowering surface tension as the polyether-modified siloxane compound surfactant, but is highly compatible with said surfactant. For this reason, it is believed that the foam suppressor is efficiently incorporated into the foam film, and the difference in surface tension between the surfactant and the foam suppressor causes the surface of the foam film to become locally unbalanced, resulting in the destruction of the foam.
[0069] [ka] (In the above formula, R7 and R8 each independently represent an alkyl group having 3 to 6 carbon atoms; R9 and R 10each independently represents an alkyl group having 1 to 2 carbon atoms, and n represents an integer of 1 to 6.
[0070] Preferred examples of the compound represented by the general formula (XIII) include 2,4,7,9-tetramethyldecane-4,7-diol and 2,5,8,11-tetramethyldodecane-5,8-diol. 2,5,8,11-tetramethyldodecane-5,8-diol is particularly preferred due to its anti-foaming effect and high compatibility with ink. The content of the foam suppressor in the ink is preferably 0.01 to 10% by mass, and more preferably 0.1 to 5% by mass. If the content is 0.01% by mass, a foam suppression effect is obtained, and if the content is 10% by mass or less, the foam suppression effect does not plateau and there is no adverse effect on the ink properties such as viscosity and particle size.
[0071] -pH adjuster- There are no particular limitations on the pH adjuster, so long as it can adjust the pH to 7 to 11 without adversely affecting the ink being formulated, and it can be appropriately selected depending on the purpose. Examples of such an acid include alcohol amines, hydroxides of alkali metal elements, hydroxides of ammonium, phosphonium hydroxides, and carbonates of alkali metals. If the pH is outside the range of 7 to 11, the ink will dissolve a large amount of the inkjet head and ink supply unit, which can cause problems such as ink deterioration, leakage, and ejection failure. Examples of the alcohol amines include diethanolamine, triethanolamine, and 2-amino-2-ethyl-1,3 propanediol. Examples of the hydroxides of the alkali metal elements include lithium hydroxide, sodium hydroxide, and potassium hydroxide. Examples of the hydroxide of ammonium include ammonium hydroxide and quaternary ammonium hydroxide. The phosphonium hydroxide includes, for example, a quaternary phosphonium hydroxide. Examples of the alkali metal carbonate include lithium carbonate, sodium carbonate, and potassium carbonate. As the pH adjuster, it is preferable to use a strongly basic compound.
[0072] By including a strong basic compound in the ink, it is possible to suppress the precipitation of crystals of the cyclic ester having the structure represented by general formula (I). This improves the fixation of the ink and also increases the permeability of the ink. When ejecting the ink using the inkjet method, ejection failures can be avoided, enabling stable printing. It is presumed that the strong base compound acts on the cyclic ester compound having the structure represented by the general formula (I), causing hydrolysis, thereby obtaining the effect of suppressing crystal precipitation. The strong base compound is not particularly limited, but it is preferable to use sodium hydroxide or potassium hydroxide from the viewpoint of effectively suppressing crystallization. The content of the strong base compound contained in the ink is preferably 0.05% by mass or more and 0.24% by mass or less in order to effectively suppress crystallization. It is also preferable to use 2-amino-2-ethyl-1,3 propanediol as a pH adjuster.
[0073] -Preservative and fungicidal agent- Examples of antiseptic and antifungal agents include sodium dehydroacetate, sodium sorbate, sodium 2-pyridinethiol-1-oxide, sodium benzoate, and sodium pentachlorophenol.
[0074] -Chelating agents- Examples of the chelating agent include sodium ethylenediaminetetraacetate, sodium nitrilotriacetate, sodium hydroxyethylethylenediaminetriacetate, sodium diethylenetriaminepentaacetate, and sodium uramildiacetate.
[0075] -Rust inhibitor- Examples of the rust inhibitor include acid sulfite, sodium thiosulfate, ammonium thiodiglycolate, diisopropylammonium nitrite, pentaerythritol tetranitrate, and dicyclohexylammonium nitrite.
[0076] -Antioxidants- Examples of the antioxidant include phenol-based antioxidants (including hindered phenol-based antioxidants), amine-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants.
[0077] -Ultraviolet absorber- Examples of the ultraviolet absorbing agent include benzophenone-based ultraviolet absorbing agents, benzotriazole-based ultraviolet absorbing agents, salicylate-based ultraviolet absorbing agents, cyanoacrylate-based ultraviolet absorbing agents, and nickel complex salt-based ultraviolet absorbing agents.
[0078] -Ink manufacturing- The ink of the present invention can be produced by the steps of dispersing or dissolving water, an organic solvent, polyurethane resin particles, a colorant added as necessary, and other components in an aqueous medium, and further stirring and mixing as necessary, and heating the mixture obtained by the above step at a temperature of 40° C. or higher but lower than 70° C. for 6 hours or more. This stirring and mixing can be carried out by, for example, a sand mill, a homogenizer, a ball mill, a paint shaker, an ultrasonic disperser, etc., and the stirring and mixing can be carried out by a stirrer using a normal stirring blade, a magnetic stirrer, a high-speed disperser, etc.
[0079] -Ink properties- There are no particular limitations on the physical properties of the ink of the present invention and they can be appropriately selected depending on the purpose. However, if the static surface tension of the ink is 20 mN / m or more and the dynamic surface tension at a bubble lifetime of 15 msec as measured by the maximum bubble pressure method is 34 mN / m or less, then, although sufficient wettability to the recording medium can be ensured, the ink will be less likely to wet the water-repellent film of the nozzle plate optool of the inkjet head, and ejection stability can be ensured, resulting in an extremely stable ink, which is preferable. The viscosity of the ink at 25° C. is preferably 5 to 25 mPa·s, and more preferably 6 to 20 mPa·s. If the viscosity is 5 mPa·s or more, the effect of improving the print density and character quality can be obtained. Furthermore, if the viscosity is 25 mPa·s or less, the ink ejection properties can be ensured. The viscosity can be measured at 25° C. using, for example, a viscometer (RE-85L, manufactured by Toki Sangyo Co., Ltd.). To ensure the storage stability of the ink, the pH is preferably in the range of 8 to 11, and more preferably in the range of 8.5 to 11.
[0080] The ink of the present invention can be used well in printers equipped with any type of inkjet head, such as a so-called piezoelectric type inkjet head that uses a piezoelectric element as pressure generating means to pressurize the ink in the ink flow path, thereby deforming a diaphragm that forms the wall of the ink flow path, changing the internal volume of the ink flow path and ejecting ink droplets (see JP Patent Publication No. 2-51734), a so-called thermal type inkjet head that uses a heating resistor to heat the ink in the ink flow path and generate bubbles (see JP Patent Publication No. 61-59911), or an electrostatic type inkjet head that has a diaphragm that forms the wall of the ink flow path and an electrode opposed to each other, and deforms the diaphragm by electrostatic force generated between the diaphragm and the electrode, thereby changing the internal volume of the ink flow path and ejecting ink droplets (see JP Patent Publication No. 6-71882). The ink of the present invention may be used by being contained in a container such as an ink cartridge.
[0081] <Recording Media> There are no particular limitations on the recording medium on which recording can be performed using the ink of the present invention, and it can be appropriately selected depending on the purpose, and examples thereof include plain paper, glossy paper, special paper, cloth, film, OHP sheet, general-purpose printing paper, etc. However, the ink of the present invention is extremely excellent in that it can print well on non-permeable media for signage and commercial printing paper in the same way as on other papers. Printed matter having an image formed using the ink of the present invention has high image quality, is free of bleeding, and has excellent stability over time, and can be suitably used for various purposes such as documents on which various types of printing or images are recorded.
[0082] Next, the ink ejection head will be described. <Ink ejection head> The ink ejection head includes a nozzle plate, and may further include other members as required.
[0083] -Nozzle plate- The nozzle plate includes a nozzle substrate and an ink-repellent film on the nozzle substrate.
[0084] -Nozzle board- The nozzle substrate is provided with nozzle holes, and the number, shape, size, material, structure, etc. of the nozzle holes are not particularly limited and can be appropriately selected depending on the purpose. The nozzle substrate has an ink ejection side surface from which ink is ejected from the nozzle holes, and a liquid chamber joining surface located on the opposite side to the ink ejection side surface. The ink-repellent film is formed on the surface of the nozzle substrate on the ink ejection side.
[0085] The planar shape of the nozzle substrate is not particularly limited and can be appropriately selected depending on the purpose, and examples of the planar shape include a rectangle, a square, a rhombus, a circle, an ellipse, etc. In addition, examples of the cross-sectional shape of the nozzle substrate include a flat plate shape, a plate shape, etc. The size of the nozzle substrate is not particularly limited and can be appropriately selected depending on the size of the nozzle plate.
[0086] The material of the nozzle substrate is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include stainless steel, Al, Bi, Cr, InSn, ITO, Nb, Nb2O5, NiCr, Si, SiO2, Sn, Ta2O5, Ti, W, ZAO (ZnO+Al2O3), and Zn. These may be used alone or in combination of two or more. Among these, stainless steel is preferred from the viewpoint of rust resistance.
[0087] The stainless steel is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include austenitic stainless steel, ferritic stainless steel, martensitic stainless steel, precipitation hardening stainless steel, etc. These may be used alone or in combination of two or more.
[0088] At least the surface of the nozzle substrate on the ink ejection side may be subjected to oxygen plasma treatment to introduce hydroxyl groups in order to improve adhesion between the ink repellent film and the nozzle substrate.
[0089] -Nozzle hole- The nozzle holes are not particularly limited in number, arrangement, interval, opening shape, opening size, cross-sectional shape of the opening, etc., and may be appropriately selected depending on the purpose. The arrangement of the nozzle holes is not particularly limited and may be appropriately selected depending on the purpose. For example, the nozzle holes may be arranged at equal intervals along the longitudinal direction of the nozzle substrate. The arrangement of the nozzle holes can be appropriately selected depending on the type of ink to be ejected, but one to multiple rows are preferable, and one to four rows are more preferable. The number of the nozzle holes per row is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 10 or more and 10,000 or less, and more preferably 50 or more and 500 or less. The interval (pitch) P, which is the shortest distance between the centers of adjacent nozzle holes, is not particularly limited and can be appropriately selected depending on the purpose, but is preferably, for example, 21 μm or more and 169 μm or less. The opening shape of the nozzle hole is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a circle, an ellipse, a rectangle, etc. Among these, a circle is preferable from the viewpoint of ejecting ink droplets.
[0090] -Ink-repellent film- The ink-repellent film preferably contains a fluorine-containing acrylate ester polymer or a polymer having a fluorine-containing heterocyclic structure in the main chain. By including the fluorine-containing acrylate ester polymer or the polymer having a fluorine-containing heterocyclic structure in the main chain, the ink-repellent film has a very small surface free energy, and is therefore preferable because it can maintain a state in which it is difficult to wet even with the ink having a low surface tension used in the present invention. However, when other materials are used as the ink-repellent film, the surface free energy becomes very small, and the ink having a low surface tension used in the present invention may become wet.
[0091] --Fluorine-containing acrylate ester polymer-- The fluorine-containing acrylate ester polymer preferably contains at least one of a compound represented by the following general formula (II) and a compound represented by the following general formula (III) as a monomer unit. [ka] [ka] In the general formulas (II) and (III), X is any one of a hydrogen atom, a linear or branched alkyl group having 1 to 21 carbon atoms, a halogen atom, a CFX1X2 group (wherein X1 and X2 are each independently a hydrogen atom or a halogen atom), a cyano group, a linear or branched fluoroalkyl group having 1 to 21 carbon atoms, a substituted or unsubstituted benzyl group, and a substituted or unsubstituted phenyl group, R1 is an alkyl group having 1 to 18 carbon atoms, R2 is an alkylene group having 2 to 6 carbon atoms, R3 is an alkylene group having 2 to 6 carbon atoms, Y is an acid group, and Rf is a linear or branched fluoroalkyl group having 1 to 21 carbon atoms. m is 1 to 10, n is 2 to 90, p is 1 to 90, and q is 1 to 10. Furthermore, a polymer obtained by polymerizing at least one of the compounds represented by the general formula (II) and the general formula (III) is a polymer having at least one of a structural unit represented by the general formula (IV) and a structural unit represented by the general formula (V).
[0092] The R1 preferably has 1 to 18 carbon atoms, more preferably 1 to 4 carbon atoms, and examples thereof include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, and an undecyl group. The R2 is an alkylene group having 2 to 6 carbon atoms, such as an ethylene group, a propylene group, a butylene group, etc. Among these, an ethylene group is preferable. The R3 is an alkylene group having 2 to 6 carbon atoms, such as an ethylene group, a propylene group, a butylene group, etc. Among these, an ethylene group is preferable. The Y is an acid group, and examples thereof include a sulfonic acid group, a succinic acid group, an acetic acid group, a phthalic acid group, a hydrogenated phthalic acid group, and a maleic acid group.
[0093] The Rf is a linear or branched fluoroalkyl group having 1 to 21 carbon atoms, preferably a perfluoroalkyl group, and more preferably Rf has 1 to 10 carbon atoms. Examples of Rf include -CF3, -CF2CF3, -CF2CF2CF3, -CF(CF3)2, -CF2CF2CF2CF3, -CF2CF(CF3)2, -C(CF3)3, -(CF2)4CF3, -(CF2)2CF(CF3)2, -CF2C(CF3)3, -CF(CF3)CF2CF2CF3, -(CF2)5CF3, -(CF2)3CF(CF3)2, -(CF2)4CF(CF3)2, -(CF2)7CF3, -(CF2)5CF(CF3)2, -(CF2)6CF(CF3)2, -(CF2)9CF3, and the like.
[0094] The above m is preferably an integer of 1 to 10, and more preferably an integer of 1 to 3. The above n is preferably an integer of 2 to 90, more preferably an integer of 3 to 50, and further preferably an integer of 4 to 30. The above p is preferably an integer of 1 to 90, and more preferably an integer of 1 to 30. The q is preferably an integer of 1 to 10, and more preferably an integer of 1 to 3.
[0095] As the fluorine-containing acrylate ester polymer, a suitably synthesized product or a commercially available product may be used. The fluorine-containing acrylate ester polymer represented by the general formula (III) (Rf is C6F 13 can be synthesized, for example, by the following reaction scheme:
[0096] [ka]
[0097] The fluorine-containing acrylate ester polymer represented by the general formula (III) (Rf is C6F 13 can be synthesized, for example, by the following reaction scheme:
[0098] [ka]
[0099] The fluorine content in the fluorine-containing acrylate ester polymer is preferably 10% by mass or more, more preferably 25% by mass or more, and even more preferably 50% by mass or more, from the viewpoint of ink repellency (contact angle). Examples of the commercially available products include krytoxFSL (manufactured by DuPont), krytoxFSH (manufactured by DuPont), FomblinZ (manufactured by Solvay Solexis), FLUOROLINKS10 (manufactured by Solvay Solexis), Optool DSX (manufactured by Daikin Industries, Ltd.), FLUOROLINKC10 (manufactured by Solvay Solexis), Moresco Phosphorol A20H (manufactured by Matsumura Oil Research Institute Co., Ltd.), Moresco Phosphorol ADOH (manufactured by Matsumura Oil Research Institute Co., Ltd.), Moresco Phosphorol DDOH (manufactured by Matsumura Oil Research Institute Co., Ltd.), Fluorosurf FG5010 (manufactured by Fluorotechnology Co., Ltd.), Fluorosurf FG5020 (manufactured by Fluorotechnology Co., Ltd.), Fluorosurf FG5060 (manufactured by Fluorotechnology Co., Ltd.), and Fluorosurf FG5070 (manufactured by Fluorotechnology Co., Ltd.).
[0100] The ink-repellent film is composed of a compound film containing the fluorine-containing acrylate ester polymer skeleton in its molecule. An inorganic oxide layer can be provided between the nozzle substrate and the ink-repellent film in order to improve adhesion by providing a large number of hydroxyl groups that serve as bonding points with the compound containing the fluorine-containing acrylate ester polymer skeleton in its molecule. Examples of materials for the inorganic oxide layer include SiO2 and TiO2. The average thickness of the inorganic oxide layer is preferably from 0.001 μm to 0.2 μm, and more preferably from 0.01 μm to 0.1 μm.
[0101] Examples of the compound containing a fluorine-containing acrylate ester polymer skeleton in the molecule include low molecular weight substances and resins. Examples of the compound containing a fluorine-containing acrylate ester polymer skeleton in the molecule include those disclosed in JP-B-3-43065, JP-A-6-210857, JP-A-10-32984, JP-A-2000-94567, JP-A-2002-145645, JP-A-2003-341070, JP-A-2007-106024, and JP-A-2007-125849. A particularly preferred example is modified perfluoropolyoxetane (Optool DSX, manufactured by Daikin Industries, Ltd.). The average thickness of the ink repellent film is preferably from 0.001 μm to 0.2 μm, and more preferably from 0.01 μm to 0.1 μm.
[0102] Examples of methods for forming an ink-repellent film from a compound containing a fluorine-containing acrylate ester polymer skeleton in the molecule include coating methods such as spin coating, roll coating, and dipping using a fluorine-based solvent, printing, and vacuum deposition. Examples of the fluorine-based solvent include Novec (manufactured by 3M Co.), Vertrel (manufactured by DuPont), and Galden (manufactured by Solvay Solexis).
[0103] --Polymer having a fluorine-containing heterocyclic structure in the main chain-- The polymer having a fluorine-containing heterocyclic structure in the main chain is preferably an amorphous fluorine-containing polymer having a heterocyclic structure, since the amorphous polymer has excellent film strength, adhesion to a substrate, film uniformity, etc., and can further exhibit the effects of the present invention. As the polymer having a fluorine-containing heterocyclic structure in the main chain, for example, the polymers described in U.S. Pat. No. 3,418,302, U.S. Pat. No. 3,978,030, JP-A-63-238111, JP-A-63-238115, JP-A-1-131214, JP-A-1-131215, etc. are preferably used. Among these, the following polymers having a heterocyclic structure are representative, however, the content of the present invention is not limited to these only.
[0104] [ka]
[0105] [ka] In the general formulae (i) and (ii), Rf1, Rf2, and Rf3 each represent a fluorine-containing alkyl group.
[0106] [ka]
[0107] [ka]
[0108] [ka]
[0109] [ka]
[0110] [ka]
[0111] [ka]
[0112] Furthermore, in order to improve adhesion to a substrate and to control the glass transition temperature (Tg) and solubility in a solvent, a structure represented by the following general formula (iii) may be introduced into the main chain, and these structures can be obtained by copolymerizing with comonomers represented by the following structural formulas (vii) to (ix).
[0113] [ka] In the general formula (iii), R4, R5, and R6 each represent a hydrogen atom, a fluorine atom, a chlorine atom, or Rf4, where Rf4 is a fluorine-containing alkyl group. X represents a hydrogen atom, a fluorine atom, a chlorine atom, Rf5, or Rf6, where Rf5 is a fluorine-containing organic substituent having a functional group such as an acid, an ester, an alcohol, an amine, or an amide at its terminal, and Rf6 is a fluorine-containing alkyl group or a fluorine-containing ether group.
[0114] [ka]
[0115] [ka]
[0116] [ka]
[0117] Examples of materials having the specific chemical structure as described above and suitable as ink repellent treatment agents include product names: Cytop CTX-105 (manufactured by Asahi Glass Co., Ltd.), Cytop CTX-805 (manufactured by Asahi Glass Co., Ltd.), product name: Teflon (registered trademark) AF1600, and product name: AF2400 (manufactured by DuPont).
[0118] Examples of methods for forming an ink-repellent film using a polymer having a fluorine-containing heterocyclic structure in the main chain include coating methods such as spin coating, roll coating, and dipping using a fluorine-based solvent, printing, and vacuum deposition. The fluorine-based solvent is not particularly limited as long as it can dissolve the polymer having a fluorine-containing heterocyclic structure in the main chain, and can be appropriately selected depending on the purpose. For example, fluorine-containing solvents such as perfluorobenzene, "Product name: Afluid" (product name: fluorine-based solvent manufactured by Asahi Glass Co., Ltd.), and "Fluorinert FC-75" (product name: liquid containing perfluoro(2-butyltetrahydrofuran) manufactured by 3M Corporation) are suitable. These may be used alone or in combination of two or more. Among these, in the case of a mixed solvent, hydrocarbons, chlorinated hydrocarbons, fluorochlorohydrocarbons, alcohols, or other organic solvents can also be used in combination. The solution concentration is preferably from 0.01% by mass to 50% by mass, and more preferably from 0.01% by mass to 20% by mass. The average thickness of the ink-repellent film is sufficient to achieve the above-mentioned object if it is 0.01 μm or more, but it is preferably 0.01 μm or more and 2 μm or less.
[0119] The heat treatment conditions (temperature) of the polymer having a fluorinated heterocyclic structure in the main chain are determined by the boiling point of the solvent, the glass transition temperature of the polymer, and the heat resistance temperature of the substrate. That is, a temperature higher than the boiling point of the solvent and the glass transition temperature of the polymer and lower than the heat resistance temperature of the substrate should be selected. The glass transition temperature of the polymer having a fluorine-containing heterocyclic structure in the main chain varies depending on the structure. For example, since the structures of the structural formulas (iv) to (vi) are mostly from 50° C. to 110° C., the heat treatment conditions are preferably a temperature of from 120° C. to 170° C. and a time of 30 minutes to 2 hours.
[0120] In addition, a copolymer having the structure of the above general formula (ii) and the structure of the following structural formula (x) in the main chain is sold by DuPont under the trade name "Teflon (registered trademark) AF."
[0121] [ka]
[0122] The Teflon (registered trademark) AF can have various glass transition temperatures by changing the copolymerization ratio. That is, as the ratio of the PDD [perfluoro(2,2-dimethyl-1,3-dioxole)] component increases, the glass transition temperature increases. Depending on the component ratio, it can range from 80°C to 330°C, and commercially available ones are 160°C (AF1600) and 240°C (AF2400). For example, the heat treatment temperature for the 160°C one is preferably 165°C to 180°C, taking into account the heat resistance temperature of the base material.
[0123] -Other materials- The other members are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other members include a pressure chamber and a stimulus generating means.
[0124] --Pressure chamber-- The pressurized chambers are arranged in individual correspondence with the multiple nozzle holes provided in the nozzle plate, and are multiple individual flow paths that communicate with the nozzle holes, and may also be referred to as ink flow paths, pressurized liquid chambers, pressure chambers, ejection chambers, liquid chambers, etc.
[0125] --Means for discharging ink-- The ink ejection head has means for generating a stimulus which is applied to the ink. The stimulus in the stimulus generating means is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include heat (temperature), pressure, vibration, light, etc. These may be used alone or in combination of two or more. Among these, heat and pressure are preferred. Examples of the stimulus generating means include a heating device, a pressure device, a piezoelectric element, a vibration generating device, an ultrasonic oscillator, a light, etc. Specific examples of the stimulus generating means include a piezoelectric actuator such as a piezoelectric element, a thermal actuator that utilizes a phase change caused by film boiling of ink using an electrothermal conversion element such as a heating resistor, a shape memory alloy actuator that uses a metal phase change caused by a temperature change, and an electrostatic actuator that uses an electrostatic force.
[0126] When the stimulus is "heat", thermal energy corresponding to a recording signal is applied to the ink in the ink ejection head using, for example, a thermal head, etc. The thermal energy generates bubbles in the ink, and the ink is ejected as droplets from the nozzle holes of the nozzle plate by the pressure of the bubbles. When the stimulus is "pressure," for example, a method is given in which the piezoelectric element is bonded to a position called the pressure chamber in the ink flow path in the ink ejection head by applying a voltage to the piezoelectric element, which is bent, thereby contracting the volume of the pressure chamber and ejecting the ink as droplets from the nozzle hole of the ink ejection head. Among these, the piezoelectric method in which a voltage is applied to a piezoelectric element to cause ink to fly is preferred.
[0127] Here, an example of an ink ejection head used in the present invention will be described with reference to Fig. 4 to Fig. 6. Fig. 4 is an exploded perspective view of the head, Fig. 5 is a cross-sectional view of the head taken along a direction perpendicular to the nozzle arrangement direction (longitudinal direction of the liquid chamber), and Fig. 6 is a cross-sectional view of the head taken along the nozzle arrangement direction (lateral direction of the liquid chamber).
[0128] The ink ejection head has a flow path plate (liquid chamber substrate, flow path member) 1, a vibration plate member 2 joined to the lower surface of the flow path plate 1, and a nozzle plate 3 which is a nozzle forming member joined to the upper surface of the flow path plate 1, and these form a plurality of liquid chambers (also called pressurized liquid chambers, pressure chambers, pressurized chambers, flow paths, etc.) 6 as individual flow paths in which a plurality of nozzle holes 4 which eject liquid droplets (ink droplets) are each connected via a nozzle communication passage 5, a fluid resistance section 7 which also serves as a supply path for supplying ink to the liquid chambers 6, and a communication section 8 which communicates with the liquid chambers 6 via the fluid resistance section 7, and ink is supplied to the communication section 8 from a common liquid chamber 10 formed in a frame member 17 via a supply port 19 formed in the vibration plate member 2.
[0129] Flow path plate 1 is formed by etching a silicone substrate to form openings such as communication passage 5, liquid chamber 6, and fluid resistance portion 7. Note that flow path plate 1 can also be formed by etching a SUS substrate using an acid etching solution or by machining such as punching (pressing).
[0130] The vibration plate member 2 has vibration regions (diaphragm portions) 2a that form the wall surfaces corresponding to the liquid chambers 6, and an island-shaped protrusion 2b is provided on the outer surface of the vibration region 2a (the surface opposite to the liquid chambers 6). The upper end surfaces (joining surfaces) of the piezoelectric element columns 12A, 12B of the laminated piezoelectric elements 12, 12, which act as driving elements (actuator means, pressure generating means) that generate energy to deform the vibration region 2a and eject droplets, are joined to the island-shaped protrusion 2b. The lower end surface of the laminated piezoelectric element 12 is joined to a base member 13.
[0131] Here, the piezoelectric element 12 is formed by alternately laminating piezoelectric material layers 21 such as PZT and internal electrodes 22a, 22b, and the internal electrodes 22a, 22b are each drawn out to the end face, i.e., the side face of the piezoelectric element 12 that is approximately perpendicular to the vibration plate member 2, and connected to end face electrodes (external electrodes) 23a, 23b formed on this side face, and displacement in the lamination direction occurs when a voltage is applied to the end face electrodes (external electrodes) 23a, 23b. This piezoelectric element 12 is formed by forming a required number of piezoelectric element columns 12A, 12B for one piezoelectric element member by groove processing using half-cut dicing.
[0132] It should be noted that the piezoelectric element columns 12A and 12B of the piezoelectric element 12 are the same, but the piezoelectric element column that is driven by applying a driving waveform is called the piezoelectric element column 12A, and the piezoelectric element column that is used simply as a support column without applying a driving waveform is called the piezoelectric element column 12B. In this case, either a bi-pitch configuration in which the driving piezoelectric element columns 12A and the support piezoelectric element columns 12B are used alternately, or a normal pitch configuration in which all the piezoelectric element columns are used as driving piezoelectric element columns 12A, can be adopted.
[0133] As a result, two rows of drive elements (rows of drive piezoelectric element columns 12A) are provided on the base member 13, in which a plurality of drive piezoelectric element columns 12A as drive elements are arranged side by side.
[0134] In addition, the ink in the liquid chamber 6 is pressurized by using displacement in the d33 direction (stacking direction of the piezoelectric material layers) as the piezoelectric direction of the laminated piezoelectric element 12, but it is also possible to use displacement in the d31 direction (plane direction of the piezoelectric material layers: direction perpendicular to the electric field) as the piezoelectric direction of the laminated piezoelectric element 12 to pressurize the ink in the pressurized liquid chamber 6.
[0135] Furthermore, the piezoelectric element material is not particularly limited, and electromechanical transducers such as ferroelectrics, such as BaTiO3, PbTiO3, (NaK)NbO3, etc., which are generally used as piezoelectric element materials, can also be used. Furthermore, although a laminated type piezoelectric element is used, a single-plate piezoelectric element can also be used. The single-plate piezoelectric element can be one that is machined, a thick film that is screen printed and sintered, or a thin film that is formed by sputtering, vapor deposition, or a sol-gel method. Furthermore, the laminated type piezoelectric elements 12 provided on one base member 13 can be in one row or a structure in which multiple rows are provided.
[0136] The external electrodes 23a of the driving piezoelectric element columns 12A of the piezoelectric elements 12 are directly connected to the FPC 15 as wiring means by a solder member in order to provide a driving signal, and a driving circuit (driver IC) 16 for selectively applying a driving waveform to each driving piezoelectric element column 12A of the piezoelectric elements 12 is mounted on the FPC 15. The external electrodes 23b of all the piezoelectric element columns 12A are electrically connected in common and are connected to the common wiring of the FPC 15 by the same solder member. Here, the output terminal portion of the FPC 15 that is joined to the piezoelectric elements 12 is solder-plated to enable solder bonding, but solder plating may be applied to the piezoelectric elements 12 side instead of the FPC 15. As for the bonding method, bonding using an anisotropic conductive film or wire bonding may be used in addition to solder bonding.
[0137] The nozzle plate 3 is constructed by forming an ink-repellent film 32 on the droplet ejection side (surface in the ejection direction: ejection surface, or the surface opposite the liquid chamber 6, nozzle formation surface) of a nozzle substrate 31 in which holes constituting nozzle holes 4 with diameters of 10 μm or more and 35 μm or less are formed corresponding to each liquid chamber 6.
[0138] A frame member 17 formed by injection molding of epoxy resin or polyphenylene sulfite is joined to the outer periphery of the piezoelectric actuator unit 100, which is composed of the piezoelectric element 12 on which the FPC 15 is mounted (connected) and the base member 13. The frame member 17 has the above-mentioned common liquid chamber 10 formed therein, and further has a supply port 19 for supplying ink from the outside to the common liquid chamber 10, which is further connected to an ink supply source such as a sub-tank or ink storage container (not shown).
[0139] In an ink ejection head configured in this manner, for example, by lowering the voltage applied to the driving piezoelectric element column 12A from the reference potential, the piezoelectric element column 12A contracts, the vibration area 2a of the vibration plate member 2 descends and the volume of the liquid chamber 6 expands, causing ink to flow into the liquid chamber 6, and then the voltage applied to the piezoelectric element column 12A is increased to extend the piezoelectric element column 12A in the stacking direction, and the vibration plate member 2 is deformed toward the nozzle hole 4 to contract the volume of the liquid chamber 6, whereby the ink in the liquid chamber 6 is pressurized and droplets of ink are ejected (sprayed) from the nozzle hole 4.
[0140] Then, by returning the voltage applied to the piezoelectric element columns 12A to the reference potential, the vibration plate member 2 is restored to its initial position, and the liquid chamber 6 expands to generate negative pressure, at which point ink fills the liquid chamber 6 from the common liquid chamber 10. Then, after the vibration of the meniscus surface of the nozzle hole 4 has attenuated and stabilized, the operation proceeds to eject the next droplet.
[0141] The method of driving the ink ejection head is not limited to the above example (pull-push shot), and pull shots, push shots, etc. can be performed depending on the driving waveform applied.
[0142] Next, details of the nozzle plate 3 according to the present invention will be described with reference to Fig. 7 to Fig. 9. Fig. 7 is an explanatory plan view of the nozzle plate 3, Fig. 8 is a cross-sectional view of the same, and Fig. 9 is an enlarged cross-sectional view of one nozzle portion. The nozzle plate 3 is formed by depositing a Ti layer 33 as an underlayer, a SiO2 film 34, and a perfluoropolyether film having alkoxysilane in its molecules (this film is called a "water-repellent film") 32 in this order on the ejection surface 31a of a nozzle substrate 31 made of, for example, a Ni metal plate, from the surface of the nozzle substrate 31. In the vicinity of the outlet of the inner wall surface 4a of the nozzle hole 4, a underlayer (Ti layer) 33 is deposited continuously from the ejection surface on the SiO2 film 35 formed on the liquid chamber surface 31b of the nozzle substrate 31, and the underlayer (Ti layer) 33 is exposed on the outermost surface.
[0143] The nozzle base material 31 may be made of a Ni metal plate or the like, but is not limited to this.
[0144] Here, the water-repellent layer 32 of the nozzle plate 3 is formed by deposition, and no deposited film for forming the water-repellent layer 32 is formed near the outlet of the inner wall surface of the nozzle hole 4. This allows stable droplet ejection without causing ejection defects or impairing liquid filling properties.
[0145] <Printing method and printing device> The printing method of the present invention is a printing method in which printing is performed by ejecting the ink of the present invention, and includes at least an ink ejection step, and further includes other steps appropriately selected as necessary, such as a stimulus generation step and a control step. The printing device of the present invention has at least an ink cartridge that contains the ink of the present invention and an ink ejection means that ejects the ink, and further has other means appropriately selected as necessary, such as a stimulus generating means and a control means. The printing method of the present invention can be suitably carried out by the printing apparatus of the present invention, the ink ejection step can be suitably carried out by the ink ejection means, and the other steps can be suitably carried out by the other means.
[0146] -Ink ejection process (an example of the printing process)- The ink ejection process is a process in which a stimulus (energy) is applied to the ink, and the ink is ejected onto a recording medium to perform printing. In this process, a known inkjet recording method can be applied as a method for ejecting the ink to print onto a recording medium. Examples of such a method include an inkjet recording method that uses a scanning head, and an inkjet recording method that uses a line-type head to perform image recording on a sheet of recording medium. There are no particular limitations on the driving method of the recording head, which is the ink ejection means, and it is possible to use an on-demand type head that uses a piezoelectric element actuator using PZT or the like, a method that uses thermal energy, an actuator that uses electrostatic force, etc., or recording can be performed using a continuous ejection type charge control type head.
[0147] In the printing method of the present invention, a heating and drying step can be provided after the ink ejection step, if necessary. For example, the recording medium can be dried using an infrared drying device, a microwave drying device, a roll heater, a drum heater, hot air, or the like.
[0148] An example of the above-mentioned printing device is shown in FIG. This diagram shows a case having an image forming process and a drying process, where 1 is a recording medium, 2 is an ink ejection section, 3 is a conveyor belt, 4 is a hot air drying device, 5 is an image forming section, 6 is a drying processing section, and 7 is a transfer roll.
[0149] <Recording device and recording method> The ink of the present invention can be suitably used in various recording devices using the ink jet recording method, such as printers, facsimile machines, copying machines, printer / fax / copier combination machines, and three-dimensional modeling devices. In the present invention, the recording apparatus and recording method refer to an apparatus capable of ejecting ink, various treatment liquids, etc. onto a recording medium, and a method of recording using the apparatus. The recording medium refers to an object onto which ink or various treatment liquids can be attached even temporarily. This recording device can include not only a head portion that ejects ink, but also means related to feeding, transporting, and discharging the recording medium, as well as other devices called pre-processing devices and post-processing devices. The recording apparatus and the recording method may have a heating means used in the heating step and a drying means used in the drying step. The heating means and the drying means include, for example, a means for heating and drying the printed surface and the back surface of the recording medium. The heating means and the drying means are not particularly limited, but for example, a hot air heater and an infrared heater can be used. Heating and drying can be performed before, during, or after printing. In addition, the recording device and recording method are not limited to those that visualize meaningful images such as characters and figures with ink. For example, those that form patterns such as geometric designs and those that create three-dimensional images are also included. Furthermore, unless otherwise specified, the recording apparatus includes both a serial type apparatus in which the ejection head moves and a line type apparatus in which the ejection head does not move. Furthermore, this recording device includes not only desktop types, but also wide-width recording devices capable of printing on A0-sized recording media, and continuous-feed printers that can use continuous paper wound into a roll as a recording medium. An example of a recording device will be described with reference to Figs. 2 and 3. Fig. 2 is a perspective view of the device. Fig. 3 is a perspective view of a main tank. An image forming device 400 as an example of a recording device is a serial type image forming device. A mechanism unit 420 is provided inside an exterior 401 of the image forming device 400. Each ink storage unit 411 of the main tanks 410 (410k, 410c, 410m, 410y) for each color of black (K), cyan (C), magenta (M), and yellow (Y) is formed of a packaging material such as an aluminum laminate film. The ink storage unit 411 is stored in a storage container case 414 made of plastic, for example. As a result, the main tanks 410 are used as ink cartridges of each color. On the other hand, a cartridge holder 404 is provided at the back side of the opening when the cover 401c of the apparatus body is opened. A main tank 410 is detachably attached to the cartridge holder 404. As a result, each ink outlet 413 of the main tank 410 communicates with an ejection head 434 for each color via a supply tube 436 for each color, and ink can be ejected from the ejection head 434 to a recording medium.
[0150] 3, a filter is preferably provided in the ink flow path from ink storage unit (ink cartridge) 411 to ejection head (ejection means for ejecting ink) 434. A filter may also be provided at ink outlet 413. The filter is preferably a filter capable of retaining particles of 10 μm or more, and by providing a filter, particles of 10 μm or more can be removed, making it possible to provide a printing device with excellent ejection stability. Since the filter is constantly in contact with ink, it is preferably made of stainless steel from the viewpoint of corrosion resistance, and among them, it is preferable to use austenitic stainless steel, more particularly SUS304, SUS316 or SUS316L, because of its excellent corrosion resistance. It is preferable that the composition contains any one of the above, and more preferably, the composition consists of any one of the above.
[0151] Filters with different filtering accuracy are commercially available, and for example, an Acro Last Chance filter manufactured by Nippon Pall Corporation can be used. The use of a filter with a filtering accuracy of 10 μm or less is preferable because it can remove solid matter present in the ink and improve the ejection stability. The use of a filter with a filtering accuracy of 6 μm or more and 10 μm or less is preferable because it allows the ink to be appropriately supplied to the ejection means. A specific example of the product is a 10 μm disposable filter, PALL ACRO25 LCF-12100, filtration accuracy: 10 μm, material: polypropylene.
[0152] By using an ink containing water, an organic solvent, polyurethane resin particles, and a cyclic ester having a structure represented by general formula (I), in which the content of crystals of the cyclic ester having the structure represented by general formula (I) having a particle size of 1 μm or more is less than 4 ppm in the entire ink after storing the ink at room temperature for one month (25±5°C), it has become possible to provide an ink, a printing method, and a printing device that have high fixing and drying properties even on non-permeable media for signage and commercial printing paper, high image density, good liquid permeability and ejection stability, and excellent storage stability. [ka]
[0153] By using a printing device in which a filter is provided between the ink flow path from the ink cartridge to the ejection means that ejects the ink, it is possible to remove crystals present in the ink, for example those with a particle size exceeding 10 μm, thereby obtaining favorable ejection stability.
[0154] In the manufacturing process of an ink containing at least water, an organic solvent, and polyurethane resin particles, a step of mixing water, an organic solvent, and polyurethane resin particles is followed by a step of heating the resulting mixture at 40°C or more and less than 70°C for 6 hours or more, so that the content of crystals of cyclic ester having a structure represented by general formula (I) in the ink with a particle size of 1 μm or more can be made less than 4 ppm in the entire ink. By lowering the content of cyclic ester having a structure represented by general formula (I) in the ink, an ink with high fixability and drying properties, high image density, good liquid permeability, good ejection stability, and excellent storage stability can be obtained. Regarding the crystals, even if large crystals with a particle size of more than 10 μm remain, it is considered that more suitable ejection stability can be obtained by removing the large crystals with a filter.
[0155] The shape of the filter used in the present invention is not particularly limited, and any known filter can be used. Among them, it is preferable to use a sintered filter formed by laminating stainless steel fibers in a felt-like form and sintering them, or a twill weave filter formed by weaving stainless steel fibers in a twill weave, since this provides an inkjet recording device (ink supply unit) with longer-term ejection reliability.
[0156] In the present invention, the terms image formation, recording, printing, printing, etc. are all synonymous.
[0157] Recording medium, media, and printed material are all synonymous. EXAMPLES
[0158] The present invention will be described in more detail below with reference to Preparation Examples, Production Examples, Examples, and Comparative Examples, but the present invention is not limited to these Examples. In the Examples, "parts" and "%" are "parts by mass" and "% by mass" unless otherwise specified. Unless otherwise specified, the preparation and evaluation of inks were carried out at room temperature of 25° C. and humidity of 60%.
[0159] <Preparation of pigment dispersion> (Preparation Example 1) -Preparation of surface-modified black pigment dispersion- Cabot Corporation's Black Pearls (registered trademark) 1000 (BET specific surface area 343 m 2 100g of carbon black (100g / g, dibutyl phthalate absorption (DBPA) 105mL / 100g), 100 mmol of sulfanilic acid, and 1L of ion-exchanged high purity water were mixed at room temperature using a Silverson mixer (6000 rpm). Next, 100 mmol of nitric acid was added to the resulting slurry, and after 30 minutes, sodium nitrite (100 mmol) dissolved in 10mL of ion-exchanged high purity water was slowly added. The mixture was further heated to 60°C while stirring, and reacted for 1 hour to obtain a modified pigment in which sulfanilic acid was added to carbon black. Next, the pH was adjusted to 9 with a 10% tetrabutylammonium hydroxide solution (methanol solution), and after 30 minutes, a modified pigment dispersion was obtained. Next, this dispersion and ion-exchanged high purity water were used to perform ultrafiltration using a dialysis membrane, and further ultrasonic dispersion was performed to obtain a modified pigment dispersion containing 20% pigment solids. The surface treatment level of the pigment was 0.75 mmol / g, and the median diameter (D50) measured with a particle size distribution measuring device (Nanotrac UPA-EX150 manufactured by Nikkiso Co., Ltd.) was 120 nm.
[0160] (Preparation Example 2) -Preparation of surface-modified magenta pigment dispersion- 1 kg of pigment dispersion SMART Magenta 3122BA (Pigment Red 122 surface-treated dispersion, pigment solid content 14.5%) manufactured by SENSIENT was acidified with 0.1N HCl aqueous solution. Next, the pH was adjusted to 9 with 10% tetraethylammonium hydroxide aqueous solution, and after 30 minutes, a modified pigment dispersion was obtained. The modified pigment dispersion containing a pigment bonded to at least one aminobenzoic acid group or aminobenzoic acid tetraethylammonium salt and ion-exchanged high purity water were subjected to ultrafiltration with a dialysis membrane, and further ultrasonic dispersion was performed to obtain a modified pigment dispersion containing 20% pigment solid content. The median diameter (D50) measured with a particle size distribution measuring device (Nanorakku UPA-EX150 manufactured by Nikkiso Co., Ltd.) was 104 nm.
[0161] (Preparation Example 3) -Preparation of surface-modified cyan pigment dispersion- 1 kg of pigment dispersion SMART Cyan 3154BA (Pigment Blue 15:4 surface-treated dispersion, pigment solid content 14.5%) manufactured by SENSIENT was acidified with 0.1N HCl aqueous solution. Next, the pH was adjusted to 9 with 40% benzyltrimethylammonium hydroxide solution (methanol solution), and after 30 minutes, a modified pigment dispersion was obtained. The modified pigment dispersion containing a pigment bonded to at least one aminobenzoic acid group or aminobenzoic acid benzyltrimethylammonium salt and ion-exchanged high-purity water were subjected to ultrafiltration through a dialysis membrane, and further ultrasonic dispersion was performed to obtain a modified pigment dispersion containing 20% pigment solid content. The median diameter (D50) measured with a particle size distribution measuring device (Nanorakku UPA-EX150 manufactured by Nikkiso Co., Ltd.) was 116 nm.
[0162] (Preparation Example 4) -Preparation of surface-modified yellow pigment dispersion- 1 kg of pigment dispersion SMART Yellow 3074BA (Pigment Yellow 74 surface-treated dispersion, pigment solid content 14.5%) manufactured by SENSIENT was adjusted to pH 9 with 10% tetrabutylammonium hydroxide solution (methanol solution), and after 30 minutes, a modified pigment dispersion was obtained. The modified pigment dispersion containing a pigment bonded to at least one aminobenzoic acid group or aminobenzoic acid tetrabutylammonium salt and ion-exchanged high purity water were subjected to ultrafiltration through a dialysis membrane, and further ultrasonic dispersion was performed to obtain a modified pigment dispersion containing 20% pigment solid content. The median diameter (D50) measured with a particle size distribution measuring device (Nanorakku UPA-EX150 manufactured by Nikkiso Co., Ltd.) was 145 nm.
[0163] (Preparation Example 5) -Preparation of magenta pigment-containing polymer particle dispersion- <Preparation of polymer solution A> A 1 L flask equipped with a mechanical stirrer, a thermometer, a nitrogen gas inlet tube, a reflux condenser, and a dropping funnel was thoroughly purged with nitrogen gas, and then 11.2 g of styrene, 2.8 g of acrylic acid, 12.0 g of lauryl methacrylate, 4.0 g of polyethylene glycol methacrylate, 4.0 g of styrene macromer, and 0.4 g of mercaptoethanol were mixed and heated to 65°C. Next, a mixed solution of 100.8g of styrene, 25.2g of acrylic acid, 108.0g of lauryl methacrylate, 36.0g of polyethylene glycol methacrylate, 60.0g of hydroxylethyl methacrylate, 36.0g of styrene macromer, 3.6g of mercaptoethanol, 2.4g of azobismethylvaleronitrile, and 18g of methyl ethyl ketone was dropped into the flask over 2.5 hours. After the dropwise addition, a mixed solution of 0.8g of azobismethylvaleronitrile and 18g of methyl ethyl ketone was dropped into the flask over 0.5 hours. After aging at 65°C for 1 hour, 0.8g of azobismethylvaleronitrile was added and aged for another 1 hour. After the reaction was completed, 364g of methyl ethyl ketone was added to the flask, and 800g of polymer solution A with a concentration of 50% by mass was obtained.
[0164] <Preparation of pigment-containing polymer particle dispersion> 28 g of polymer solution A, 42 g of CI Pigment Red 122, 13.6 g of 1 mol / L potassium hydroxide aqueous solution, 20 g of methyl ethyl ketone, and 13.6 g of ion-exchanged water were thoroughly stirred and then kneaded using a roll mill. The obtained paste was put into 200 g of pure water, thoroughly stirred, and then methyl ethyl ketone and water were distilled off using an evaporator. In order to remove further coarse particles, this dispersion was pressure-filtered with a polyvinylidene fluoride membrane filter with an average pore size of 5.0 μm to obtain a magenta pigment-containing polymer microparticle dispersion containing 15% by mass of pigment and 20% by mass of solids. The median diameter (D50) of the polymer microparticles in the obtained magenta pigment-containing polymer microparticle dispersion was measured and found to be 127 nm. The median diameter (D50) was measured using a particle size distribution measuring device (Nanorakku UPA-EX150, manufactured by Nikkiso Co., Ltd.).
[0165] (Preparation Example 6) -Preparation of cyan pigment-containing polymer particle dispersion- A cyan pigment-containing polymer fine particle dispersion was prepared in the same manner as in Preparation Example 5, except that in Preparation Example 5, CI Pigment Red 122 was replaced with a phthalocyanine pigment (CI Pigment Blue 15:3). The median diameter (D50) of the polymer fine particles in the obtained cyan pigment-containing polymer fine particle dispersion was measured with a particle size distribution measuring device (Nanotrac UPA-EX150, manufactured by Nikkiso Co., Ltd.) and was 93 nm.
[0166] (Preparation Example 7) -Preparation of yellow pigment-containing polymer particle dispersion- A yellow pigment-containing polymer fine particle dispersion was prepared in the same manner as in Preparation Example 5, except that CI Pigment Red 122 used in Preparation Example 5 was changed to a bisazo yellow pigment (CI Pigment Yellow 155) as the pigment. The median diameter (D50) of the polymer fine particles in the obtained yellow pigment-containing polymer fine particle dispersion was measured with a particle size distribution measuring device (Nanotrac UPA-EX150, manufactured by Nikkiso Co., Ltd.) and was 76 nm.
[0167] (Preparation Example 8) -Preparation of polymer particle dispersion containing carbon black pigment- A carbon black pigment-containing polymer fine particle dispersion was prepared in the same manner as in Preparation Example 5, except that the CI Pigment Red 122 used in Preparation Example 5 was changed to carbon black (FW100, manufactured by Degussa) as the pigment. The median diameter (D50) of the polymer fine particles in the obtained carbon black pigment-containing polymer fine particle dispersion was 104 nm as measured with a particle size distribution measuring device (Nanotrac UPA-EX150, manufactured by Nikkiso Co., Ltd.).
[0168] <Example of resin particle preparation> <Preparation of Water-Dispersible Polyurethane Resin (A)> (Preparation of polyester polyol P-1) In a reaction vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, 830 parts of terephthalic acid, 830 parts of isophthalic acid, 374 parts of ethylene glycol, 598 parts of neopentyl glycol, and 0.5 parts of dibutyltin oxide were charged while introducing nitrogen gas, and a polycondensation reaction was carried out at 180 to 230°C for 15 hours at 230°C until the acid value became 1 or less, thereby obtaining a polyester polyol P-1 having a hydroxyl value of 74.5, an acid value of 0.2, and an average molecular weight of 1,500.
[0169] (Preparation of Hydrophobic Polyester Polyol Q-1) In a reaction vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, 1,660 parts of orthophthalic acid, 1,637 parts of diethylene glycol, and 0.5 parts of dibutyltin oxide were charged while introducing nitrogen gas, and a polycondensation reaction was carried out at 180 to 230°C for 15 hours at 230°C until the acid value became 1 or less, thereby obtaining polyester polyol Q-1 having an aromatic ring structure with a hydroxyl value of 190 and an acid value of 0.3.
[0170] (Preparation of Water-Dispersible Polyurethane Resin (A)) 1,000 parts of polyester polyol P-1 were dehydrated at 100°C under reduced pressure, and then cooled to 80°C. After that, 907 parts of methyl ethyl ketone was added and thoroughly stirred to dissolve, 80 parts of 2,2'-dimethylolpropionic acid was added, and then 281 parts of isophorone diisocyanate was added and reacted at 75°C for 8 hours to carry out a urethane-forming process. After confirming that the isocyanate value was 0.1% or less, the mixture was cooled to 50°C, and 340 parts of the polyester polyol Q-1 was added to obtain a homogeneous solution. Then, 60 parts of triethylamine was added to neutralize the solution, and 7,000 parts of water was added to make the solution water-soluble. Methyl ethyl ketone was removed from the resulting transparent reaction product at 40 to 60°C under reduced pressure, and water was then added to adjust the concentration to obtain a stable semi-transparent colloidal aqueous dispersion with a non-volatile content of 25%.
[0171] <Preparation of Water-Dispersible Polyurethane Resin (B)> 1,000 parts of the polyester polyol P-1 described above was dehydrated at 100°C under reduced pressure, and then cooled to 80°C. After that, 907 parts of methyl ethyl ketone was added and thoroughly stirred to dissolve, 80 parts of 2,2'-dimethylolpropionic acid was added, and then 281 parts of isophorone diisocyanate was added and reacted at 75°C for 8 hours to carry out a urethane-forming process. After it was confirmed that the isocyanate value was 0.1% or less, the mixture was cooled to 50° C., neutralized by adding 60 parts of triethylamine, and then dissolved in water by adding 7,000 parts of water. Methyl ethyl ketone was removed from the resulting transparent reaction product at 40 to 60°C under reduced pressure, and water was then added to adjust the concentration to obtain a stable semi-transparent colloidal aqueous dispersion with a non-volatile content of 25%.
[0172] <Preparation of Water-Dispersible Polyurethane Resin (C)> (Preparation of polyester polyol P-2) While introducing nitrogen gas into a reaction vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, 664 parts of terephthalic acid, 631 parts of isophthalic acid, 472 parts of 1,4-butanediol, 447 parts of neopentyl glycol, and 0.5 parts of dibutyltin oxide were charged and esterified at 180 to 230 ° C. for 5 hours, and then polycondensation reaction was carried out at 230 ° C. for 6 hours until the acid value became 1 or less. Then, the mixture was cooled to 120 ° C., and 321 parts of adipic acid and 268 parts of 2,2'-dimethylolpropionic acid were added, and the mixture was heated again to 170 ° C. and reacted at this temperature for 20 hours to obtain a polyester polyol P-2 containing a carboxyl group with an acid value of 46.5 and a hydroxyl value of 59.8.
[0173] (Preparation of Water-Dispersible Polyurethane Resin (C)) 1,000 parts of polyester polyol P-2 were dehydrated at 100°C under reduced pressure, then cooled to 80°C, 812 parts of methyl ethyl ketone were added and thoroughly stirred to dissolve, 20 parts of 1,4-butanediol were added, and then 198 parts of dicyclohexylmethane-4,4'-diisocyanate (hydrogenated MDI) was added and reacted at 75°C for 8 hours. After confirming that the isocyanate value was 0.1% or less, the mixture was cooled to 50° C., neutralized by adding 84 parts of triethylamine, and then dissolved in water by adding 7,000 parts of water. Methyl ethyl ketone was removed from the resulting transparent reaction product at 40 to 60°C under reduced pressure, and water was then added to adjust the concentration to obtain a stable semi-transparent colloidal aqueous dispersion with a non-volatile content of 25%.
[0174] <Preparation of Water-Dispersible Polyurethane Resin (D)> 1,000 parts of polyester polyol P-1 were dehydrated at 100°C under reduced pressure, and then cooled to 80°C. After that, 907 parts of methyl ethyl ketone was added and thoroughly stirred to dissolve, 80 parts of 2,2'-dimethylolpropionic acid was added, and then 281 parts of isophorone diisocyanate was added and reacted at 75°C for 8 hours to carry out a urethane-forming process. After it was confirmed that the isocyanate value was 0.1% or less, the mixture was cooled to 50° C., neutralized by adding 60 parts of triethylamine, and then dissolved in water by adding 7,000 parts of water. Methyl ethyl ketone was removed from the resulting transparent reaction product at 40 to 60°C under reduced pressure, and water was then added to adjust the concentration to obtain a stable semi-transparent colloidal aqueous dispersion with a non-volatile content of 25%.
[0175] <Preparation of Acrylic-Silicone Polymer Microparticles A> After thoroughly replacing the air in a 1L flask equipped with a mechanical stirrer, a thermometer, a nitrogen gas inlet tube, a reflux tube, and a dropping funnel with nitrogen gas, 8.0 g of Latemul S-180 (Kao Corporation, reactive anionic surfactant) was added to 350 g of ion-exchanged water and mixed, and the temperature was raised to 65 ° C. Next, 3.0 g of reaction initiator t-butyl peroxobenzoate and 1.0 g of sodium isoascorbate were added, and after 5 minutes, a mixture of 45 g of methyl methacrylate, 160 g of 2-ethylhexyl methacrylate, 5 g of acrylic acid, 45 g of butyl methacrylate, 30 g of cyclohexyl methacrylate, 15 g of vinyltriethoxysilane, 8.0 g of Latemul S-180, and 340 g of ion-exchanged water was added dropwise over 3 hours. Next, the mixture was heated and aged at 80 ° C for 2 hours, cooled to room temperature, and the pH was adjusted to 7 to 8 with sodium hydroxide. The ethanol was then removed using an evaporator, and the moisture content was adjusted to obtain 730 g of acrylic-silicone polymer microparticles with a solid content of 40%. The median diameter (D50) of the polymer microparticles in the dispersion was measured using a particle size distribution analyzer (Nanorakku UPA-EX150, manufactured by Nikkiso Co., Ltd.) and found to be 125 nm.
[0176] (Examples 1 to 26 and Comparative Examples 1 to 21) <Pre-ink manufacturing example> (Pre-ink manufacturing example 1) In a container equipped with a stirrer, 7.50 parts of 3-methoxy-N,N-dimethylpropanamide represented by the above formula (1), 5.00 parts of propylene glycol monopropyl ether, 18.00 parts of propylene glycol, 2.00 parts of 2,2,4-trimethyl-1,3-pentanediol, and 0.50 parts of 2,4,7,9-tetramethyldecane-4,7-diol, and 1.00 parts of a polyether-modified siloxane compound represented by the above formula (8) were added and mixed and stirred for 30 minutes. Next, 0.05 parts of a preservative and antifungal agent (Proxel GXL manufactured by Avecia), 0.30 parts of 2-amino-2-ethyl-1,3-propanediol, 56.00 parts of the prepared water-dispersible polyurethane resin (A), 1.62 parts of a polyurethane dispersion "Takelac W-6110 manufactured by Mitsui Chemicals", and an amount of high purity water to make the total 100 parts were added and mixed and stirred for 60 minutes. Next, the resulting mixture was pressure filtered through a polyvinylidene fluoride membrane filter having an average pore size of 1.2 μm to remove coarse particles and dust, thereby obtaining pre-ink 1.
[0177] (Pre-ink manufacturing example 2) In a container equipped with a stirrer, 7.50 parts of 3-methoxy-N,N-dimethylpropanamide represented by the above formula (1), 5.00 parts of propylene glycol monopropyl ether, 22.00 parts of propylene glycol, 2.00 parts of 2-ethyl-1,3-hexanediol, and 0.50 parts of 2,4,7,9-tetramethyldecane-4,7-diol, and 1.50 parts of the polyether-modified siloxane compound represented by the above formula (8) were placed and mixed with stirring for 30 minutes. Next, 0.05 parts of an antiseptic and antifungal agent (Proxel GXL manufactured by Avecia), 0.30 parts of 2-amino-2-ethyl-1,3-propanediol, 24.00 parts of the prepared water-dispersible polyurethane resin (A), 1.62 parts of a polyurethane dispersion "Takelac W-6110 manufactured by Mitsui Chemicals, Inc.", 15.00 parts of the surface-modified black pigment dispersion of Preparation Example 1, and a total amount of 100 parts of highly purified water were added and mixed and stirred for 60 minutes. Next, the resulting mixture was pressure-filtered through a polyvinylidene fluoride membrane filter with an average pore size of 1.2 μm to remove coarse particles and dust, and pre-ink 2 was obtained.
[0178] (Pre-ink manufacturing examples 3 to 24) In the same manner as in Pre-ink Production Examples 1 and 2, the organic solvent, surfactant, and defoamer shown in each column of Pre-ink Production Examples 3 to 24 in Tables 1 to 3 below were mixed and stirred, then the antiseptic / antifungal agent, pH adjuster, and colorant (pigment dispersion) were mixed and stirred, and further the water-dispersible polyurethane resin and resin particles were mixed and stirred. The resulting mixture was pressure-filtered through a polyvinylidene fluoride membrane filter with an average pore size of 1.2 μm to remove coarse particles and dust, thereby obtaining Pre-inks 3 to 24.
[0179] [Table 1]
[0180] [Table 2]
[0181] [Table 3]
[0182] Details of the abbreviations in Tables 1 to 3 are as follows. Direct Blue 199 (water-soluble cyan dye): EKTA INTERNATIONAL Superflex 300: Polyurethane dispersion, solids 30.0%, Tg=-42℃, manufactured by Daiichi Kogyo Seiyaku Co., Ltd. Takelac W-6110: Polyurethane dispersion, solids 30.9%, Tg = -20°C, manufactured by Mitsui Chemicals Compound of formula (1): 3-methoxy-N,N-dimethylpropanamide Compound of formula (2): 3-n-butoxy-N,N-dimethylpropanamide Compound of formula (5): 3-ethyl-3-hydroxymethyloxetane Compound of formula (6): 3-methyl-3-hydroxymethyloxetane ·TEGO Wet270: Polyether modified siloxane compound (Evonik, 100% active ingredient) · Silface SAG503A: Polyether modified siloxane compound (Made by Nissin Chemical Industry Co., Ltd., 100% active ingredient) · Unidyne DSN403N: Polyoxyethylene perfluoroalkyl ether (Manufactured by Daikin Industries, 100% active ingredient) ·Proxel GXL:1,2-benzisothiazolin-3-one Main ingredient: Antiseptic and antifungal agent (Manufactured by Avecia, contains 20% dipropylene glycol)
[0183] The physical properties of each of the inks in Pre-ink Production Examples 1 to 24 were measured as follows. The results are shown in Table 4. <Viscosity> The viscosity was measured at 25°C using a viscometer (RE-85L, manufactured by Toki Sangyo Co., Ltd.). <ph> The measurement was performed at 25°C using a pH meter (HM-30R type, manufactured by TOA-DKK Corporation). <Static surface tension> The measurements were made at 25° C. using an automatic surface tensiometer (DY-300, manufactured by Kyowa Interface Science Co., Ltd.). <Dynamic surface tension> The dynamic surface tension of the ink of the present invention was measured at 25° C. using a SITA_DynoTester (manufactured by SITA) at a surface life of 15 msec according to the maximum bubble pressure method.
[0184] [Table 4]
[0185] <Ink manufacturing example> The pre-inks 1 to 24 were heated under the conditions shown in Table 5 to obtain inks 1 to 27. The physical properties of each ink were measured in the same manner as for the pre-inks. The results are shown in Table 5. [Table 5]
[0186] The pre-ink and the ink heated under each condition were filled into an ink pack, and the ink was left to stand at room temperature (25±5°C) for one month before being evaluated as described below. Images were formed using the ink, and the characteristics were evaluated. The results are shown in Table 6.
[0187] -Qualitative and quantitative analysis of crystals of cyclic ester having the structure represented by general formula (I) contained in ink- <Qualitative method, quantitative method> The amount of cyclic ester crystals having the structure represented by general formula (I) contained in the ink can be quantified simply by filtering each ink in the manufacturing examples using a filtering tool consisting of a Φ60mm Kiriyama funnel with Kiriyama funnel filter paper Φ60mm No.5C (particle retention capacity 1μm), thoroughly washing the crystals and filter paper retained after filtration with high purity water, and then drying the filter paper to the moisture content before filtration. The amount of cyclic ester crystals having the structure represented by general formula (I) can be quantified by weighing the mass of the filter paper before filtration and the mass of the crystals and filter paper retained after filtration and taking the difference. In order to improve the accuracy of quantification, 3000 g of ink was filtered and quantified. The crystals on the filter paper were all dissolved in tetrahydrofuran, and the remaining filter paper was dried and then weighed. The difference between the weighed filter paper mass and the filter paper mass before filtration was checked, but there was no difference. The solution dissolved in tetrahydrofuran was analyzed by LC-MS to check whether it contained any other components. The structure of the crystals precipitated in the ink and obtained by filtration was determined by GC-MS analysis and LC-MS analysis + C 13 -NMR+H 1 When qualitatively analyzed by -NMR+FT-IR, it was confirmed that all of the compounds were cyclic esters having the structure represented by the following structural formula (B). [ka]
[0188] -Ink ejection process (image formation process)- Under environmental conditions adjusted to 23±0.5°C and 50±5% RH, an inkjet recording device (IPSiO GXe-5500, Ricoh Co., Ltd.) was used to vary the drive voltage of the piezo element so that the amount of ink ejected was uniform. 2 ) was set so that the same amount of ink was adhered to the ink cartridge. In addition, in Example 18, Example 19, Comparative Example 18, and Comparative Example 19, a filter was installed between the ink storage section (ink cartridge) and the ink flow path to the ejection head (ejection means for ejecting ink). The filter used was an Acro Last Chance filter manufactured by Nippon Pall Corporation. 10μm disposable filter: PALL ACRO25 LCF-12100, filtration accuracy: 10μm, Material: Polypropylene
[0189] Next, the preparation of the nozzle plate to be attached to the inkjet head will be described. (Example 101) <Preparation of Nozzle Plate A> <<Synthesis of fluorine-containing acrylate ester polymer A>> -Synthesis of ethylene oxide chain-containing fluoromonomer (MPOERfA)- The reaction formula for the synthesis of an ethylene oxide chain-containing fluorine monomer is shown below. [ka] In the above reaction scheme, the average of n is 8 to 9.
[0190] Next, 52.13 g of one-terminated methoxy polyethylene glycol (average EO number: 8-9, Uniox M-400, NOF Corporation) and 0.94 g of boron trifluoride diethyl ether complex were charged into a four-neck flask. Under a nitrogen stream, 50 g of 3-perfluorohexyl-1,2-epoxypropane was added dropwise over 30-40 minutes at room temperature while taking care not to generate heat. After the addition was completed, the reaction was continued at room temperature for about 2 hours, and then it was confirmed by gas chromatography (GC) that the peak of 3-perfluorohexyl-1,2-epoxypropane had disappeared. 0.03 g of tertiary butyl catechol was added to the mixture and thoroughly stirred. Furthermore, 14.81 g of triethylamine was added, and 12.04 g of acrylic acid chloride was added dropwise over about 20 minutes while taking care not to generate heat. After the addition was completed, the reaction was continued at room temperature for about 2 hours, and then it was confirmed by GC that the peak of acrylic acid chloride had almost disappeared. The product was identified by IR, 1H-NMR and 19F-NMR spectra.
[0191] -Synthesis of fluorine-containing acrylate ester polymer A- In a 200 mL four-neck flask, 10% by mass of the synthesized MPOERfA monomer, 60% by mass of 2-(perfluorohexyl)ethyl acrylate, 20% by mass of polyethylene glycol monoacrylate (EO: 10 moles, NOF Corp., AE-400), 5% by mass of 2-hydroxyethyl acrylate, 2.5% by mass of acetoacetoxyethyl methacrylate, and 2.5% by mass of dimethylaminoethyl acrylate were charged with 60 g of isopropyl alcohol. Nitrogen was blown into the flask for 60 minutes to replace the air in the system with nitrogen. While continuing the nitrogen flow, the internal temperature was raised to 75°C to 80°C, and then 0.25 g of azobisisobutyronitrile was added and the polymerization reaction was carried out for 8 hours. When the polymerization solution was analyzed by gas chromatography (GC) and gel permeation chromatography, it was confirmed that the peak derived from the monomer almost disappeared and a peak derived from the copolymer was generated. In addition, the weight average molecular weight of the copolymer was 17,000 (polystyrene equivalent). Finally, 0.42 g of acetic acid was added to neutralize the solution, and the solution was diluted with water to give a 20% by mass solution of the fluorine-containing acrylate ester copolymer A.
[0192] -Making the nozzle plate- Next, a nozzle substrate made of stainless steel (SUS304) with a length of 34 mm, width of 16 mm, and average thickness of 20 μm was prepared. The nozzle substrate had four nozzle hole rows formed therein, each row having 320 nozzle holes with an average hole diameter of 25 μm and a pitch (the shortest distance between the centers of the nozzle holes) of 85 μm (300 dpi). A 20% by mass solution of the prepared fluorine-containing acrylate ester polymer A was applied by dipping onto the ink ejection side surface of the nozzle substrate, and dried to form an ink-repellent film with an average thickness of 50 nm. In this way, the nozzle plate A of the manufacturing example 101 was produced. At this time, the nozzle holes were masked with a water-soluble resin, and the back surface of the nozzle substrate was masked with tape, and after the ink-repellent film was formed, the masking was peeled off and removed. In addition, the ink-repellent film was formed by heating at 120°C for 1 hour.
[0193] (Example 102) <Preparation of Nozzle Plate B> <<Synthesis of fluorine-containing acrylate ester polymer B>> -Synthesis of Rf epoxy adduct (FAGMA) of 2-hydroxyethyl acrylate (HEA)- The reaction scheme for the synthesis of the Rf epoxy adduct of 2-hydroxyethyl acrylate is shown below. [ka]
[0194] 20g of 2-hydroxyethyl acrylate (HEA), 0.61g of boron trifluoride diethyl ether complex, and 0.026g of tertiary butyl catechol were charged into a four-neck flask. 64.83g of 3-perfluorohexyl-1,2-epoxypropane was added dropwise over 30 to 40 minutes at room temperature while taking care not to generate heat. After the addition was completed, the reaction was continued at room temperature for about 2 hours, and then gas chromatography (GC) confirmed that the peak of 3-perfluorohexyl-1,2-epoxypropane had disappeared. After the reaction was completed, the reactant was dissolved in 100g of 1,1-dichloro-1,2,2,3,3-pentafluoropropane (HCFC225), and 100g of water was added, followed by washing with a separatory funnel, separation, and then the organic layer was taken out. This washing and separation procedure was repeated once more, and the organic layer was taken out, followed by adding 5g of anhydrous magnesium sulfate, and drying overnight. HCFC225 was evaporated to obtain an Rf epoxy adduct of HEA (FAGMA). The product was identified by IR spectrum, 1H-NMR, and 19F-NMR spectrum. Analysis of the product showed that a mixed monomer was obtained, consisting of approximately 64% by mass of 1-mol adduct (n=1) of 3-perfluorohexyl-1,2-epoxypropane, approximately 27% by mass of 2-mol adduct (n=2), and approximately 9% by mass of 3-mol adduct.
[0195] -Synthesis of sulfonic acid-containing fluoromonomer- The reaction formula for the synthesis reaction of the sulfonic acid-containing fluoromonomer is shown below. [ka]
[0196] 30 g of the synthesized HEA Rf epoxy adduct (FAGMA), 30 g of dichloromethane, 7.8 g of triethylamine, and 0.024 g of hydroquinone monomethyl ether were charged into a four-neck flask. This mixed solution was cooled in an ice bath to 0 to 10°C. A dichloromethane solution of chlorosulfonic acid (7.48 g of chlorosulfonic acid + 15 g of dichloromethane) was gradually added dropwise to this over about 30 minutes, while paying attention to heat generation. After the dropwise addition was completed, the reaction was allowed to proceed at room temperature for 3 hours. 100 g of water was added to the reaction product, and washing and separation operations were repeated twice. The organic layer was taken out, 5 g of anhydrous magnesium sulfate was added, and the mixture was dried overnight. The product (sulfonic acid-containing fluorine monomer) was identified by IR spectrum, 1H-NMR, and 19F-NMR spectrum.
[0197] -Synthesis of fluorine-containing acrylate ester polymer B- A fluorine-containing acrylate ester polymer B was synthesized in the same manner as in Production Example 101, except that the monomer composition was changed to 60% by mass of 2-(perfluorohexyl)ethyl acrylate, 20% by mass of the sulfonic acid group-containing fluorine monomer, 17.5% by mass of polyethylene glycol monoacrylate (EO: 10 moles, NOF Corporation, AE-400), and 2.5% by mass of acetoacetoxyethyl methacrylate. The weight average molecular weight of the obtained copolymer was 17,000 (polystyrene equivalent). Finally, 0.42 g of acetic acid was added to neutralize, and the mixture was diluted with water to a 20% by mass solution of the fluorine-containing acrylate ester polymer B.
[0198] -Making the nozzle plate- A 20% by mass solution of the prepared fluorine-containing acrylate ester polymer B was applied by dipping to the ink ejection side surface of the same nozzle substrate as in Production Example 101, and dried to form an ink-repellent film with an average thickness of 30 nm. In this way, the nozzle plate B of the manufacturing example 102 was produced. At this time, the nozzle holes were masked with a water-soluble resin, and the back surface of the nozzle substrate was masked with tape, which was peeled off and removed after the ink-repellent film was formed. In addition, the ink-repellent film was formed by heating at 120°C for 1 hour.
[0199] (Example 103) <Preparation of nozzle plate C> A fluorine-containing acrylate ester polymer solution (Optool DSX, manufactured by Daikin Industries, Ltd.) was prepared. The fluorine-containing acrylate ester polymer solution (Optool DSX, manufactured by Daikin Industries, Ltd.) was applied by dipping to the ink ejection side surface of the same nozzle substrate as in Manufacturing Example 101, and then dried to form an ink-repellent film with an average thickness of 20 nm. In this way, the nozzle plate C of Manufacturing Example 103 was produced. At this time, the nozzle holes were masked with a water-soluble resin, and the back surface of the nozzle substrate was masked with tape, which was peeled off and removed after the ink-repellent film was formed. In addition, the ink-repellent film was formed by heating at 120°C for 1 hour.
[0200] (Example 104) <Preparation of Nozzle Plate D> A silicone resin solution (SR 2441 RESIN, manufactured by Dow Corning Toray Co., Ltd.) was prepared. The silicone resin solution was applied by dipping to the ink ejection side of the same nozzle substrate as in Manufacturing Example 101, and dried to form an ink-repellent film with an average thickness of 100 nm. In this manner, nozzle plate D of Manufacturing Example 104 was produced. At this time, the nozzle holes were masked with water-soluble resin, and the back surface of the nozzle substrate was masked with tape, which was peeled off and removed after the ink-repellent film was formed. This was heated and cured at 150°C for 2 hours in air to form an ink-repellent film.
[0201] (Example 105) <Preparation of Nozzle Plate E> The ink repellent agent used was a solution prepared by diluting Cytop CTX-105 (product name, manufactured by Asahi Glass Co., Ltd.) to 0.2 mass % with a mixture of CT-solv.100 (manufactured by Asahi Glass Co., Ltd.) and CT-solv.180 (manufactured by Asahi Glass Co., Ltd.) in a volume ratio of 1:1. Silicone rubber was placed on a spinner, and 2 mL of this liquid was dropped onto the silicone rubber. After dropping, the silicone rubber was rotated on the spinner to produce a uniform film. The rotation speed was set as follows: 1st: 1,000 rpm, 5 seconds, 2nd: 3,000 rpm, 20 seconds. The same nozzle substrate surface as in Production Example 101 was pressed onto the silicone rubber to perform transfer. This was done three times with a pressing pressure of 2 kg / head. After the transfer, the head was placed in an oven at 150° C. for two and a half hours for heat treatment, thereby producing a nozzle plate E of Production Example 105.
[0202] (Example 106) <Preparation of Nozzle Plate F> The ink repellent agent used was a solution obtained by diluting AF1600 (Teflon (registered trademark) AF, manufactured by DuPont) with Fluorinert FC-75 (manufactured by 3M) to 0.5% by mass. In the same manner as in Production Example 105, silicone rubber was placed on a spinner, and 2 mL of this liquid was dropped onto the silicone rubber. After dropping, the silicone rubber was rotated on the spinner to produce a uniform film. The rotation speed was set as follows: 1st: 1,000 rpm, 5 seconds, 2nd: 3,000 rpm, 20 seconds. The same nozzle substrate surface as in Example 1 was pressed onto the silicone rubber to perform transfer. This was done three times with a pressing pressure of 2 kg / head. After the transfer was completed, the head was placed in a 165° C. oven for 2 hours and 30 minutes for heat treatment, thereby producing a nozzle plate F of Production Example 106.
[0203] -Ink ejection process (printing process)- Under environmental conditions adjusted to 23±0.5°C and 50±5% RH, an inkjet printing device (IPSiO GXe-5500, Ricoh Co., Ltd.) was used to vary the drive voltage of the piezo element so that the amount of ink ejected was uniform. 2 ) were set so that the same amount of ink was deposited on each.
[0204] <Image density> Using each ink, a chart containing 64-point JIS X 0208 (1997), 2223 general symbols, created using Microsoft Word 2000, was printed out on MyPaper (manufactured by Ricoh Co., Ltd.), the symbols were measured using a spectrodensitometer (X-Rite939, manufactured by X-Rite Co., Ltd.), and the image density of each color was evaluated according to the following criteria. The print mode used was the "plain paper - standard fast" mode in the driver attached to the printer, modified to "no color correction." JIS X 0208 (1997), 2223 is a symbol with an outer shape of a square, and the entire symbol is filled with ink. [Evaluation Criteria] A: Black: 1.25 or higher Yellow: 0.80 or higher Magenta: 1.00 or higher Cyan: 1.05 or higher B: Black: 1.20 or more, less than 1.25 Yellow: 0.75 or more, less than 0.80 Magenta: 0.95 or more, less than 1.00 Cyan: 1.00 or more, less than 1.05 C: Black: 1.15 or more, less than 1.20 Yellow: 0.70 or more, less than 0.75 Magenta: 0.90 or more, less than 0.95 Cyan: 0.95 or more, less than 1.00 D: Black: Less than 1.15 Yellow: Less than 0.70 Magenta: Less than 0.90 Cyan: Less than 0.95
[0205] <Ink storage stability> The storage stability was calculated from the viscosity measured using the viscometer before storage and after storage in a sealed container at 60° C. for 7 days according to the following formula, and evaluated based on the following criteria.
number
[0206] <Liquid permeability> A cellulose acetate membrane filter with a pore size of 0.8 μm (Advantec Toyo Co., Ltd., 28CP) was used to filter the sample at an air pressure of 1 kgf / cm. 2 The ink was filtered under pressure, and the ink permeability was evaluated from the slope (attenuation rate) of the linear approximation of the decrease in filtration speed versus the amount of filtered liquid and the maximum filtration speed. [Evaluation criteria] Liquid permeability Good_A <--------> D_Poor A: Decay rate is 1.5×10 -3 / sec and the maximum filtration rate is 1.0g / sec or more. B: Decay rate is 1.5×10 -3 / sec and maximum filtration rate is less than 1.0 g / sec. C: Decay rate is 1.5×10 -3 / sec or more 2.5×10 -3 / sec D: Decay rate is 2.5×10 -3 / sec or more
[0207] <Discharge stability-1> -Continuous discharge evaluation- Immediately after 1 L of individually adjusted ink was passed from the ink cartridge of an inkjet printing device (IPSiO GXe-5500, manufactured by Ricoh Co., Ltd.) through the ejection head of each color, a chart was created using Microsoft Word 2000, in which 80% of the area of an A4-sized sheet of paper was filled with a solid image, and 200 sheets were printed consecutively onto MyPaper (manufactured by Ricoh Co., Ltd.). After printing, a nozzle check chart was printed out and the ejection disturbance of each nozzle was evaluated according to the following criteria. The print mode used was the driver that came with the printer, with the plain paper user settings modified from "plain paper - standard fast" mode to "no color correction." [Evaluation Criteria] A: No disturbance in discharge B: Some irregular discharge C: Discharge is disturbed or there are areas where discharge is not performed D: Severely turbulent discharge or many nozzles not discharging
[0208] <Ejection stability-2> -Evaluation of ink repellency time of nozzle plate- In an environment adjusted to a temperature of 23°C ± 0.5°C and a relative humidity of 50% ± 5%, 50 g of each ink shown in Table 7 was placed in a 50 mL beaker, the nozzle plate was removed from the image forming apparatus (IPSiO GXe-5500, manufactured by Ricoh Co., Ltd.), the nozzle plate prepared above was clamped with tweezers, and immersed in the ink at a speed of 315 mm / min. The nozzle plate was then removed at the same speed. The ink repellency time (ink retraction time) from the ink-repellent film of the nozzle plate was measured and evaluated according to the following criteria. [Evaluation Criteria] A: Ink repellency time is less than 10 seconds B: Ink repellency time is 10 seconds or more and less than 30 seconds C: Ink repellency time is 30 seconds or more and less than 60 seconds D: Ink repellency time is 60 seconds or more If the ink repellency time is long, the nozzle plate becomes easily wetted with ink, and therefore nozzles are easily missing in a continuous ejection evaluation.
[0209] <Retreating contact angle> 2.0 μL of each ink shown in Tables 4 and 5 was extruded from a syringe equipped with a syringe needle having an inner diameter of 0.37 μm and 0.18 mm onto the nozzle plate surface prepared above in a 25°C environment, and the receding contact angle (°) at 25°C was measured using the shrinkage method with an automatic contact angle measuring device DMo-501 (manufactured by Kyowa Interface Science Co., Ltd.).
[0210] <Drying> Using the image forming apparatus shown in Figure 1, a chart with the same general symbols as for image density was printed on a sheet of paper with Oji Paper's OK top coat + U.S. basis weight 104.7 g / m 2 The image was printed on a paper sheet and dried by exposing it to hot air at 100°C for 10 seconds in the drying process. The dried image was then visually inspected to see whether the ink in the image area adhered to the transfer roll and evaluated according to the following criteria. [Evaluation Criteria] A: No transfer at all B: Slight transfer, no practical issues C: With transcription D: Severe transfer
[0211] <Alcohol resistance (fixability)> Using each ink, a chart containing 64-point JIS X 0208 (1997), 2223 general symbols was printed on PVC media NIJ-PVCM (Panassia Co., Ltd.) using Microsoft Word 2000. The print mode used was the "plain paper - standard fine" mode in the driver that came with the printer, modified to "no color correction." A cotton swab was soaked in 0.5 mL of ethanol and the solid image area printed above was rubbed back and forth 10 times, and the image was visually observed and evaluated according to the following criteria. [Evaluation Criteria] A: No change in the image area B: The image is legible but slightly damaged. C: Image is legible but damaged D: The image area has peeled off and the recording media area is visible.
[0212] [Table 6] [Explanation of symbols]
[0213] (About Figures 1 to 3) 1 Recording medium 2 Ink ejection section 3 Conveyor belt 4. Hot air drying device 5. Image forming section 6 Drying processing section 7 Transfer roll 400 Image forming device 401 Exterior of image forming device 401c Device body cover 404 Cartridge Holder 410 Main Tank 410k, 410c, 410m, 410y Main tanks for black (K), cyan (C), magenta (M), and yellow (Y) 411 Ink storage unit 413 Ink outlet 414 Storage container case 420 Mechanism Department 434 Discharge Head 436 Supply Tube (About Figures 4 to 9) 1 Flow path plate, liquid chamber substrate, flow path member 2. Diaphragm member 2a Vibration area (diaphragm part) 2b Island-shaped protrusion 3 Nozzle Plate 4 Nozzle Holes 5 Nozzle connection passage 6 Liquid chamber, pressurized liquid chamber, pressure chamber, pressurized chamber, flow path 7 Fluid resistance section 8 Communication section 10 Common liquid chamber 12 Piezoelectric elements, multi-layer piezoelectric elements 12A Piezoelectric element column, driving piezoelectric element column 12B Piezoelectric element column, Piezoelectric element column for support 13 Base material 15 FPC 16 Drive circuit (driver IC) 17 Frame members 19 Supply Inlet 21 Piezoelectric material layer 22a, 22b internal electrodes 23a, 23b End electrode (external electrode) 31 Nozzle base material 31a Discharge surface 32 Water-repellent film 33 Ti layer (base layer) 34 SiO2 film on the ejection surface 35 SiO2 film on the liquid chamber side 100 Piezoelectric actuator unit [Prior art documents] [Patent documents]
[0214] [Patent Document 1] JP2012-241135 Public Relations [Patent Document 2] JP 2012-207202 A [Patent Document 3] JP 2014-94998 A< / ph>
Claims
1. An ink containing water, an organic solvent, and polyurethane resin particles, the ink contains a cyclic ester having a structure represented by the following general formula (I), and after the ink is left to stand for one month in a room temperature environment (25±5°C), the content of crystals of the cyclic ester having a particle size of 1 μm or more is less than 4 ppm of the entire ink. [Case 1]
2. The ink according to claim 1 , wherein the polyurethane resin comprises a polyurethane resin having a structure represented by general formula (I).
3. The ink according to claim 1 or 2, further comprising a colorant.
4. 4. The ink according to claim 3, wherein the solid content of the polyurethane resin particles in the ink is 3% by mass or more, and the solid content ratio of the colorant to the polyurethane resin particles is 1.0:(2.0 to 11.0).
5. 5. An ink according to claim 3 or 4, wherein the colorant is a pigment.
6. 6. The ink according to claim 1, comprising, as the organic solvent, a diol compound and an organic solvent having a solubility parameter (SP value) of 8.9 to 12.
0.
7. The ink according to any one of claims 1 to 6, wherein the ink has a pH of 8.5 or higher.
8. 8. The ink according to claim 7, further comprising a strongly basic compound.
9. 9. The ink of claim 8, wherein the strongly basic compound is sodium hydroxide or potassium hydroxide.
10. 10. The ink according to claim 1, further comprising a polyether-modified siloxane compound as a surfactant.
11. 11. A method for producing an ink containing water, an organic solvent, and polyurethane resin particles, comprising: a step of mixing water, an organic solvent, and polyurethane resin particles; and a step of heating the mixture obtained in the above step at 40° C. or higher and lower than 70° C. for 6 hours or longer.
12. 12. The method for producing an ink according to claim 11, wherein the ink further contains a colorant, the method comprising the steps of: mixing water, an organic solvent, polyurethane resin particles, and the colorant; and heating the mixture obtained by the above steps at a temperature of 40° C. or higher and lower than 70° C. for 6 hours or longer.
13. A printing method comprising a step of depositing the ink according to any one of claims 1 to 10 onto a substrate and printing.
14. the step of depositing the ink on a substrate and printing the ink is a step of ejecting the ink from an ink ejection head having a nozzle plate that ejects the ink, and depositing the ink on the substrate; 14. The printing method according to claim 13, wherein the ink contains water, an organic solvent, polyurethane resin particles, and a cyclic ester having a structure represented by the following general formula (I), and after being left to stand for one month in a room temperature environment (25±5°C), the content of crystals of the cyclic ester having a particle size of 1 μm or more is less than 4 ppm of the entire ink, and the receding contact angle with respect to the nozzle plate is 35° or more. [Case 1]
15. A printing device comprising an ink cartridge containing the ink according to any one of claims 1 to 10, and a discharging means for discharging the ink.
16. 16. The printing apparatus according to claim 15, further comprising a filter in an ink flow path from the ink cartridge to the ink ejection means for ejecting ink.
17. 17. The printing apparatus according to claim 15, wherein the ejection means for ejecting the ink is an ink ejection head having a nozzle plate for ejecting the ink, and a receding contact angle of the ink with respect to the nozzle plate is 35[deg.] or more.
18. 18. The printing apparatus according to claim 17, wherein the nozzle plate has an ink-repellent film, the ink-repellent film of the nozzle plate containing a fluorine-containing acrylate ester polymer.
19. 19. The printing device according to claim 18, wherein the fluorine-containing acrylate ester polymer comprises a polymer obtained by polymerizing at least one of a compound represented by the following general formula (II) and a compound represented by the following general formula (III): [Case 2] [C3] In the general formulas (II) and (III), X is any one of a hydrogen atom, a linear or branched alkyl group having 1 to 21 carbon atoms, a halogen atom, a CFX1X2 group (wherein X1 and X2 are each independently a hydrogen atom or a halogen atom), a cyano group, a linear or branched fluoroalkyl group having 1 to 21 carbon atoms, a substituted or unsubstituted benzyl group, and a substituted or unsubstituted phenyl group; R 1 is an alkyl group having 1 to 18 carbon atoms; R 2 is an alkylene group having 2 to 6 carbon atoms, R 3 is an alkylene group having 2 to 6 carbon atoms, Y is an acid group, and Rf is a linear or branched fluoroalkyl group having 1 to 21 carbon atoms, m is 1 to 10, n is 2 to 90, p is 1 to 90, and q is 1 to 10.
20. 20. The printing device according to claim 19, wherein the fluorine-containing acrylate ester polymer contains a polymer having at least one of a structural unit represented by the following general formula (IV) and a structural unit represented by the following general formula (V): [C4] [C5] In the general formulas (IV) and (V), X is any one of a hydrogen atom, a linear or branched alkyl group having 1 to 21 carbon atoms, a halogen atom, a CFX1X2 group (wherein X1 and X2 are each independently a hydrogen atom or a halogen atom), a cyano group, a linear or branched fluoroalkyl group having 1 to 21 carbon atoms, a substituted or unsubstituted benzyl group, and a substituted or unsubstituted phenyl group; R 1 is an alkyl group having 1 to 18 carbon atoms; R 2 is an alkylene group having 2 to 6 carbon atoms, R 3 is an alkylene group having 2 to 6 carbon atoms, Y is an acid group, and Rf is a linear or branched fluoroalkyl group having 1 to 21 carbon atoms, m is 1 to 10, n is 2 to 90, p is 1 to 90, and q is 1 to 10.
21. 20. The printing device according to claim 17, wherein the ink repellent film contains a polymer having a fluorine-containing heterocyclic structure in its main chain.
Citation Information
Patent Citations
Inkjet ink, inkjet recording method, and inkjet recording device
JP2012207202A
Inkjet ink
JP2012241135A
Inkjet recording method
JP2014094998A