Optical plastic film, polarizing plate, and image display device
The optical plastic film addresses the trade-off in scratch resistance by optimizing indentation hardness ratios and slow axis direction, providing enhanced protection against both hard and soft materials and improving mechanical durability.
Patent Information
- Application Number
- JP2024138922
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-05-30
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-13
AI Technical Summary
Existing stretched plastic films with high elastic modulus exhibit good scratch resistance against hard objects but are easily damaged by soft objects, while those with low elastic modulus provide better resistance to soft objects but are susceptible to scratches from hard objects, creating a trade-off in scratch resistance.
The optical plastic film is designed with specific indentation hardness ratios (MD2/MD1 and TD2/TD1 greater than 1.01 and less than 1.30, and X1/X2 ≤ 1.30) and controlled variations in the direction of the slow axis to enhance scratch resistance against both hard and soft materials.
The film achieves improved scratch resistance against both hard and soft materials, reduces rainbow unevenness, and prevents bending or breaking after bending tests, suitable for image display devices.
Smart Images

Figure 2024160365000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical plastic film, a polarizing plate, and an image display device. [Background technology]
[0002] Various optical plastic films are often used in optical components of image display devices, etc. For example, in an image display device having a polarizing plate on a display element, a plastic film (polarizer protective film) is used to protect the polarizer constituting the polarizing plate.
[0003] Plastic films for image display devices, such as polarizer protective films, are preferably excellent in mechanical strength, and therefore stretched plastic films are preferably used as the plastic films for image display devices.
[0004] In addition, it is preferable that the stretched plastic film has excellent scratch resistance. For this reason, as in Patent Documents 1 and 2, stretched plastic films with a high elastic modulus have been proposed. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-8293 A (Claim 4) [Patent Document 2] Special Publication No. 2018-538572 (Claim 7) Summary of the Invention [Problem to be solved by the invention]
[0006] As described in Patent Documents 1 and 2, a stretched plastic film with a high elastic modulus can have good scratch resistance when scratched with a hard object such as a pencil or a touch panel pen. However, a stretched plastic film with a high elastic modulus is often scratched earlier than a stretched plastic film with a low elastic modulus when repeatedly rubbed with a soft object such as a cloth. On the other hand, stretched plastic films with a low elastic modulus have relatively good scratch resistance when repeatedly rubbed with a soft object such as cloth, but are immediately damaged when scratched with a hard object such as a pencil or a touch panel pen. As described above, there is a trade-off between improving the scratch resistance of a plastic film against both hard and soft objects.
[0007] An object of the present invention is to provide an optical plastic film, a polarizing plate, and an image display device that can have good scratch resistance against both hard and soft objects. [Means for solving the problem]
[0008] The present invention provides the following optical plastic film, polarizing plate, and image display device. [1] An optical plastic film having a first surface and a second surface located opposite to the first surface, and satisfying the following condition 1: <Condition 1> Regarding the indentation hardness of a cross section in the machine direction of a plastic film, the softer of the indentation hardness of the cross section on the first surface side and the indentation hardness of the cross section on the second surface side is defined as MD1, and the indentation hardness of the cross section at the center in the thickness direction is defined as MD2. Regarding the indentation hardness of a cross section in the width direction of a plastic film, the softer of the indentation hardness of the cross section on the first surface side and the indentation hardness of the cross section on the second surface side is defined as TD1, and the indentation hardness of the cross section at the center in the thickness direction is defined as TD2. Under these conditions, both MD2 / MD1 and TD2 / TD1 are greater than 1.01 and not greater than 1.30. [2] The optical plastic film according to [1] above, further satisfying the following condition 2: <Condition 2> When the larger of the product of MD1 and MD2 and the smaller of the product of TD1 and TD2 is defined as X1 and X2, respectively, X1 / X2 is 1.30 or less. [3] The optical plastic film according to [1] or [2] above, further satisfying the following condition 3: <Condition 3> A sample measuring 50 mm in the flow direction and 50 mm in the width direction is cut out from a plastic film. The slow axis directions are measured at a total of five locations, including four locations 10 mm from the four corners of the sample toward the center and one location at the center of the sample. When the angles formed by either the flow direction or the width direction of the sample and the direction of the slow axis at each measurement location are defined as D1, D2, D3, D4, and D5, respectively, the difference between the maximum value of D1 to D5 and the minimum value of D1 to D5 is 5.0 degrees or more. [4] The optical plastic film according to any one of [1] to [3] above, which further satisfies the following condition 4: <Condition 4> A sample measuring 50 mm in the machine direction and 50 mm in the width direction is cut out from a plastic film. The in-plane retardation is measured at a total of five locations, including four locations 10 mm from the four corners toward the center of the sample and the center of the sample. When the in-plane retardation at the five locations is defined as Re1, Re2, Re3, Re4, and Re5, the average of Re1 to Re5 is 500 nm or less. [5] The optical plastic film according to any one of [1] to [4] above, further satisfying the following condition 5: <Condition 5> A sample measuring 50 mm in the machine direction and 50 mm in the width direction is cut out from a plastic film. The thickness direction retardation is measured at a total of five locations, including four locations 10 mm from the four corners toward the center of the sample and the center of the sample. When the thickness direction retardation at the five locations is defined as Rth1, Rth2, Rth3, Rth4, and Rth5, the average of Rth1 to Rth5 is 2000 nm or more. [6] A polarizing plate having a polarizer, a transparent protective plate A arranged on one side of the polarizer, and a transparent protective plate B arranged on the other side of the polarizer, wherein at least one of the transparent protective plate A and the transparent protective plate B is the optical plastic film described in any one of [1] to [5] above. [7] An image display device having a display element and a plastic film arranged on the light exit surface side of the display element, wherein the plastic film is an optical plastic film according to any one of [1] to [5] above. [8] The image display device according to [7], further comprising a polarizer between the display element and the plastic film. Effect of the Invention
[0009] The optical plastic film, polarizing plate and image display device of the present invention can have good scratch resistance against both hard and soft objects. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a perspective view of a sample for measuring the cross-sectional hardness of a plastic film. [Diagram 2] 10 is a cross-sectional view illustrating measurement points of the cross-sectional hardness of the first surface side and the cross-sectional hardness of the second surface side under conditions 1 and 2. FIG. [Diagram 3] FIG. 11 is a plan view illustrating five measurement positions under conditions 3 to 6. [Figure 4] 1 is a cross-sectional view showing an embodiment of an image display device of the present invention. [Diagram 5] FIG. 4 is a cross-sectional view showing another embodiment of an image display device of the present invention. [Figure 6] FIG. 1 is a schematic diagram showing a continuous folding test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described. [Optical plastic film] The optical plastic film of the present invention has a first surface and a second surface located on the opposite side to the first surface, and satisfies the following condition 1. <Condition 1> Regarding the indentation hardness of a cross section in the machine direction of a plastic film, the softer of the indentation hardness of the cross section on the first surface side and the indentation hardness of the cross section on the second surface side is defined as MD1, and the indentation hardness of the cross section at the center in the thickness direction is defined as MD2. Regarding the indentation hardness of a cross section in the width direction of a plastic film, the softer of the indentation hardness of the cross section on the first surface side and the indentation hardness of the cross section on the second surface side is defined as TD1, and the indentation hardness of the cross section at the center in the thickness direction is defined as TD2. Under these conditions, both MD2 / MD1 and TD2 / TD1 are greater than 1.01 and not greater than 1.30.
[0012] <Measurements for Conditions 1 and 2> Condition 1 and Condition 2 specify the indentation hardness of a cross section of a plastic film in the machine direction and the indentation hardness of a cross section of a plastic film in the width direction. Regarding Condition 1 and Condition 2, in order to measure the cross-sectional hardness of a plastic film, it is first necessary to prepare a sample for measurement. The sample can be prepared, for example, by the following steps (A1) to (A2).
[0013] (A1) An optical plastic film is cut into two cut samples, each having a size of 2 mm in the machine direction and 10 mm in the width direction, and then the cut sample S is embedded in resin R as shown in Figure 1 to prepare two embedded samples. The embedding resin is preferably epoxy resin. The embedded sample can be obtained, for example, by placing the cut sample in a silicon embedding plate (silicon capsule), pouring in embedding resin, hardening the embedding resin (in the case of the epoxy resin manufactured by Struers, which is exemplified below, it is preferable to leave it at room temperature for 12 hours to harden), and then removing the cut sample and the embedding resin that encases it from the silicon embedding plate (silicon capsule). The silicon embedding plate (silicon capsule) can be, for example, manufactured by Dosaka EM. The embedding epoxy resin can be, for example, a mixture of Struers' product name "Epofix" and the same company's product name "Epofix Hardener" in a ratio of 10:1.2. The two cut samples are taken from adjacent areas (within an area of 50 mm x 50 mm). The size of the two cut samples is 2 mm ± 0.2 mm in the flow direction x 10 mm ± 1 mm in the width direction.
[0014] (A2) One embedded sample is cut vertically along the flow direction with a diamond knife to expose the cross section in the flow direction, thereby preparing a sample for measuring the indentation hardness of the cross section in the flow direction. The other embedded sample is cut vertically along the width direction with a diamond knife to expose the cross section in the width direction, thereby preparing a sample for measuring the indentation hardness of the cross section in the width direction. It is preferable to cut the embedded sample so as to pass through the center of the cut sample. An example of an apparatus for cutting an embedded sample is the product name "Ultramicrotome EM UC7" manufactured by Leica Microsystems.
[0015] Using the sample for measuring the indentation hardness of the cross section in the flow direction prepared as described above, the indentation hardness of the cross section on the first surface side, the indentation hardness of the cross section on the second surface side, and the indentation hardness of the cross section at the center in the thickness direction are measured, and MD1 and MD2 are calculated. Similarly, using the sample for measuring the indentation hardness of the cross section in the width direction prepared as described above, the indentation hardness of the cross section on the first surface side, the indentation hardness of the cross section on the second surface side, and the indentation hardness of the cross section at the center in the thickness direction are measured, and TD1 and TD2 are calculated. In this specification, the indentation hardness of the cross section on the first surface side in the machine direction and width direction, the indentation hardness of the cross section on the second surface side, and the indentation hardness of the cross section at the center in the thickness direction refer to the average values of five measured values.
[0016] The indentation hardness of the cross section is measured by pressing a Berkovich indenter (material: diamond triangular pyramid) perpendicularly into the cut surface of the above-mentioned sample. The indentation hardness of the cross section on the first surface side and the indentation hardness of the cross section on the second surface side are measured at positions 2.0 μm inside from the first surface and the second surface as shown in Figure 2 (positions (i) and (iii) in Figure 2 correspond to the measurement points). Note that Figure 2 corresponds to the xz cross section of Figure 1. Also, "d" in Figure 2 means the thickness direction of the cut sample of the plastic film. Also, "(ii)" in Figure 2 means the center position in the thickness direction of the cut sample of the plastic film.
[0017] The indentation hardness is preferably measured under the following conditions. <Measurement conditions> Indenter used: Berkovich indenter (model number: TI-0039, manufactured by HYSITRON) -Indentation condition: Displacement control method Maximum indentation depth: 200 nm Load application time: 20 seconds (speed: 10 nm / sec) Hold time: Hold for 5 seconds at maximum pressing depth Loading / unloading time: 20 seconds (speed: 10 nm / sec)
[0018] The indentation hardness can be calculated as follows. First, the indentation depth h (nm) corresponding to the indentation load F (N) is continuously measured, and a load-displacement curve is created. The load-displacement curve is analyzed to determine the maximum indentation load F max (N) is the projected area A of the contact area between the indenter and the plastic film. p (mm 2 ) is the indentation hardness H IT can be calculated (formula (1) below). H IT =F max / A p …(1) Here, A p is the projected contact area corrected for indenter tip curvature in the standard manner for the instrument.
[0019] It is preferable to carry out standardization before measuring the indentation hardness. The standardization can be performed, for example, by carrying out an indentation test using a standard sample with known indentation hardness and composite elastic modulus, and verifying that the indentation hardness and composite elastic modulus obtained from the test results are within the standard values. It is preferable to perform standardization each time the sample is changed. However, if the sample is the same, it is preferable in terms of work efficiency to perform multiple indentation hardness measurements consecutively. That is, it is preferable to perform the measurements as described in (1) below. In the following (1), the order of the measurement of the indentation hardness of the cross section in the machine direction and the measurement of the indentation hardness of the cross section in the width direction may be reversed. (1) After performing the standard alignment, for the sample for measuring the indentation hardness of the cross section in the flow direction, the indentation hardness of the cross section on the first surface side, the indentation hardness of the cross section on the second surface side, and the indentation hardness of the cross section at the center in the thickness direction are each measured five times, and MD1 and MD2 are calculated. The standard alignment is performed again, and for the sample for measuring the indentation hardness of the cross section in the width direction, the indentation hardness of the cross section on the first surface side, the indentation hardness of the cross section on the second surface side, and the indentation hardness of the cross section at the center in the thickness direction are each measured five times, and TD1 and TD2 are calculated.
[0020] In addition, when the measurement of the indentation hardness continues for a long period of time, it is preferable to perform standardization at least before 12 hours have elapsed. For example, even if standardization is not performed every time a sample is changed, it is preferable to perform standardization at least before 12 hours have elapsed.
[0021] In this specification, the atmosphere for various measurements such as Condition 1, Condition 2, and Conditions 3 to 6 described later is set to a temperature of 23° C.±5° C. and a humidity of 40% to 65% RH unless otherwise specified. Furthermore, the sample is exposed to the atmosphere for 30 minutes or more before the measurement.
[0022] <Machine direction and cross direction> Optical plastic films are available in the form of, for example, a sheet or a roll. In the case of a roll form, the machine direction of the roll and the width direction of the roll are easily identified. On the other hand, in the case of a sheet-like form, when the machine direction and the width direction can be easily confirmed as in the case of a uniaxially stretched film, the machine direction and the width direction can be determined according to the confirmation (in the case of a uniaxially stretched film, the direction of the slow axis is usually the width direction). If it is difficult to confirm the machine direction and cross direction of the sheet, the machine direction and cross direction may be determined as follows (1) and (2) below. (1) When the sheet is rectangular or square, the machine direction or width direction can be determined by the four sides that make up the rectangle or square. Sheet films are produced by punching out rolled film. In order to increase the yield of the sheet, it is necessary to punch out the sheet along the machine direction and width direction of the roll. Therefore, when the sheet is rectangular or square, it is common technical knowledge that the directions of the four sides that make up the rectangle or square coincide with the machine direction or width direction. (2) If the sheet has a shape other than a rectangle or square (e.g., an oval, a triangle, or a polygon other than a triangle), draw a rectangle or square that has the largest area that does not extend beyond the shape, and determine the machine direction or width direction based on the drawn rectangle or square in the same manner as in (1) above.
[0023] In the determination of (1) and (2) above, it is not possible to distinguish which of the two directions is the machine direction and which is the width direction. However, conditions 1 to 6 in this specification are parameters that are valid even if the machine direction and the width direction are reversed, so long as the two directions, that is, the machine direction and the width direction, can be distinguished. Therefore, it is sufficient to determine the machine direction and the width direction using the methods of (1) and (2) above.
[0024] <Condition 1> Condition 1 stipulates that both MD2 / MD1 and TD2 / TD1 are greater than 1.01 and equal to or less than 1.30.
[0025] Both MD2 / MD1 and TD2 / TD1 exceeding 1.01 means that the indentation hardness of the cross section of the plastic film is greater on the inside than on the surface side. When the hardness of the surfaces of two different objects is comparable, the one with a harder inside can have better scratch resistance when the surface of the object is scratched with a hard object. Therefore, by making both MD2 / MD1 and TD2 / TD1 exceeding 1.01, scratch resistance against hard objects can be improved regardless of the scratch direction. On the other hand, when both MD2 / MD1 and TD2 / TD1 are 1.30 or less, it means that the indentation hardness of the cross section of the plastic film is not excessively higher inside than on the surface side. When the surface of the plastic film is scratched with a soft object, the softer the inside of the plastic film, the easier it is to release the stress at the time of scratching. Therefore, by making both MD2 / MD1 and TD2 / TD1 1.30 or less, scratch resistance against soft objects can be improved regardless of the direction of scratching.
[0026] In condition 1, MD2 / MD1 and TD2 / TD1 are each preferably greater than 1.01 and equal to or less than 1.20, more preferably equal to or greater than 1.02 and equal to or less than 1.15, and even more preferably equal to or greater than 1.02 and equal to or less than 1.10.
[0027] The absolute values of MD1, MD2, TD1 and TD2 are not particularly limited as long as they are within a range that imparts appropriate mechanical strength, and are usually 150 MPa to 350 MPa, preferably 170 MPa to 300 MPa, more preferably 200 MPa to 270 MPa, and further preferably 220 MPa to 250 MPa.
[0028] It is preferable that an embodiment of the optical plastic film of the present invention further satisfies the following condition 2. <Condition 2> When the larger of the product of MD1 and MD2 and the smaller of the product of TD1 and TD2 is defined as X1 and X2, respectively, X1 / X2 is 1.30 or less.
[0029] A small X1 / X2 ratio means that the anisotropy of hardness between the machine direction and the width direction is small. Therefore, by making X1 / X2 1.30 or less, it is possible to suppress the occurrence of scratches in a specific direction when an object (e.g., the tip of a pen) hits the plastic film (hereinafter, this performance may be referred to as "dent resistance"). In addition, by making X1 / X2 1.30 or less, it is possible to easily suppress the occurrence of bending tendencies or breakage after a bending test. X1 / X2 is more preferably 1.25 or less, and even more preferably 1.20 or less. The lower limit of X1 / X2 is about 1.03, and is preferably 1.05 or more, and more preferably 1.10 or more.
[0030] It is preferable that an embodiment of the optical plastic film of the present invention further satisfies the following condition 3. <Condition 3> A sample measuring 50 mm in the flow direction and 50 mm in the width direction is cut out from a plastic film. The slow axis directions are measured at a total of five locations, including four locations 10 mm from the four corners of the sample toward the center and one location at the center of the sample. When the angles formed by either the flow direction or the width direction of the sample and the direction of the slow axis at each measurement location are defined as D1, D2, D3, D4, and D5, respectively, the difference between the maximum value of D1 to D5 and the minimum value of D1 to D5 is 5.0 degrees or more.
[0031] Condition 3 specifies that the difference between the maximum value of D1 to D5 and the minimum value of D1 to D5 is 5.0 degrees or more. By making the difference 5.0 degrees or more, blackout at least within the sample area can be suppressed when viewed through polarized sunglasses. Conventional plastic films for optical use are designed so that the direction of the slow axis does not shift, but the plastic film that satisfies condition 3 differs in structure from conventional optical films in that the direction of the slow axis is deliberately shifted. Another feature of the plastic film that satisfies condition 3 is that it focuses on the variation in the slow axis in a relatively small area of 50 mm length x 50 mm width.
[0032] Moreover, satisfying condition 3 is preferable in that the plastic film can have good bending resistance. On the other hand, general-purpose oriented films with aligned slow axes break or have a strong bending tendency after bending tests. Specifically, general-purpose uniaxially stretched films break when bent along the slow axis, and have a strong bending tendency when bent in a direction perpendicular to the slow axis. Moreover, general-purpose biaxially stretched films have a strong bending tendency when bent in a direction perpendicular to the slow axis. A plastic film that satisfies condition 3 is preferable in that it is possible to prevent the film from retaining a bending habit or breaking after a bending test, regardless of the bending direction.
[0033] The difference between the maximum value of D1 to D5 and the minimum value of D1 to D5 is more preferably 6.0 degrees or more, even more preferably 8.0 degrees or more, and even more preferably 10.0 degrees or more. If the difference between the maximum value of D1 to D5 and the minimum value of D1 to D5 is too large, the orientation of the plastic film tends to be low and the mechanical strength tends to decrease. Therefore, the difference is preferably 20.0 degrees or less, more preferably 17.0 degrees or less, and even more preferably 15.0 degrees or less.
[0034] In one embodiment of the optical plastic film, D1 to D5 are preferably 5 degrees to 30 degrees or 60 to 85 degrees, more preferably 7 degrees to 25 degrees or 65 degrees to 83 degrees, and even more preferably 10 degrees to 23 degrees or 67 degrees to 80 degrees, respectively. By setting D1 to D5 to 5 degrees or more or 85 degrees or less, respectively, it is possible to easily prevent blackout when viewed through polarized sunglasses. Also, by setting D1 to D5 to 30 degrees or less or 60 degrees or more, respectively, it is possible to easily prevent a decrease in mechanical strength due to a decrease in the orientation of the plastic film.
[0035] It is preferable that an embodiment of the optical plastic film of the present invention further satisfies the following condition 4. <Condition 4> A sample measuring 50 mm in the machine direction and 50 mm in the width direction is cut out from a plastic film. The in-plane retardation is measured at a total of five locations, including four locations 10 mm from the four corners toward the center of the sample and the center of the sample. When the in-plane retardation at the five locations is defined as Re1, Re2, Re3, Re4, and Re5, the average of Re1 to Re5 is 600 nm or less.
[0036] Condition 4 specifies that the average of Re1 to Re5 is 600 nm or less. By setting the average of Re1 to Re5 to 600 nm or less, it becomes easier to suppress rainbow pattern unevenness (rainbow unevenness) at least within the sample area when viewed with the naked eye.
[0037] The average of Re1 to Re5 is more preferably 300 nm or less, even more preferably 250 nm or less, and even more preferably 200 nm or less. The lower limit of the average of Re1 to Re5 is not particularly limited, but is usually about 50 nm, and preferably 100 nm or more.
[0038] Each of Re1 to Re5 is preferably 600 nm or less, more preferably 300 nm or less, even more preferably 250 nm or less, and even more preferably 200 nm or less. The difference between the maximum value of Re1 to Re5 and the minimum value of Re1 to Re5 is preferably 200 nm or less, more preferably 150 nm or less, and further preferably 100 nm or less.
[0039] The optical plastic film of one embodiment of the present invention preferably satisfies the following condition 5. <Condition 5> A sample measuring 50 mm in the machine direction and 50 mm in the width direction is cut out from a plastic film. The thickness direction retardation is measured at a total of five locations, including four locations 10 mm from the four corners toward the center of the sample and the center of the sample. When the thickness direction retardation at the five locations is defined as Rth1, Rth2, Rth3, Rth4, and Rth5, the average of Rth1 to Rth5 is 2000 nm or more.
[0040] By satisfying condition 5, the degree of stretching of the optical plastic film can be brought close to uniform biaxiality, and the mechanical strength of the optical plastic film can be improved. In addition, by satisfying condition 5, blackouts when viewed from an oblique direction through polarized sunglasses can be easily suppressed. The average of Rth1 to Rth5 is more preferably 3000 nm or more, and further preferably 4000 nm or more. The upper limit of the average of Rth1 to Rth5 is about 10000 nm, preferably 8000 nm or less, and more preferably 7000 nm or less. Furthermore, each of Rth1 to Rth5 is preferably 2000 nm to 10000 nm, more preferably 3000 nm to 8000 nm, and further preferably 4000 nm to 7000 nm.
[0041] The difference between the maximum value of Rth1 to Rth5 and the minimum value of Rth1 to Rth5 is preferably 200 nm or less, more preferably 150 nm or less, and further preferably 100 nm or less.
[0042] It is preferable that the optical plastic film of one embodiment of the present invention further satisfies the following condition 6. <Condition 6> The average of Re1 / Rth1, Re2 / Rth2, Re3 / Rth3, Re4 / Rth4 and Re5 / Rth5 is 0.10 or less.
[0043] The ratio (Re / Rth) of the in-plane retardation (Re) to the retardation (Rth) in the thickness direction is small, which means that the degree of stretching of the optical plastic film approaches uniform biaxiality. Therefore, by making the ratio 0.10 or less, the mechanical strength of the optical plastic film can be improved. The ratio is more preferably 0.07 or less, and even more preferably 0.05 or less. The lower limit of the ratio is about 0.01.
[0044] Each of Re1 / Rth1, Re2 / Rth2, Re3 / Rth3, Re4 / Rth4 and Re5 / Rth5 is preferably 0.10 or less, more preferably 0.07 or less, and even more preferably 0.05 or less. The lower limit of these ratios is about 0.01.
[0045] <Measurement of conditions 3 to 6> The samples with dimensions of 50 mm length × 50 mm width used in conditions 3 to 6 are cut out from any position on the plastic film. The five measurement points in conditions 3 to 6 are one in the center and four points 10 mm from the four corners toward the center of the sample (five points indicated by black circles in Figure 3).
[0046] The in-plane retardation (Re) of condition 4 and the thickness direction retardation (Rth) of condition 5 are expressed by the following formulas (1) and (2) using the refractive index nx in the slow axis direction, which is the direction in which the refractive index at each measurement point is the largest, the refractive index ny in the fast axis direction, which is the direction perpendicular to the slow axis direction at each measurement point, the refractive index nz in the thickness direction of the plastic film, and the thickness T [nm] of the plastic film. In this specification, the in-plane retardation (Re) and the thickness direction retardation (Rth) mean values at a wavelength of 550 nm. In-plane phase difference (Re)=(nx-ny)×T[nm] (1) Retardation in the thickness direction (Rth) = ((nx + ny) / 2 - nz) × T [nm] (2)
[0047] The direction of the slow axis, the in-plane retardation (Re) and the retardation in the thickness direction (Rth) can be measured using, for example, a product called "RETS-100" manufactured by Otsuka Electronics Co., Ltd., or a product called "KOBRA-WR" or "PAM-UHR100" manufactured by Oji Scientific Instruments Co., Ltd. When measuring the in-plane retardation (Re) and the like using Otsuka Electronics' product name "RETS-100", it is preferable to prepare for the measurement according to the following procedures (A1) to (A4).
[0048] (A1) First, turn on the RETS-100 light source and leave it for 60 minutes or more to stabilize it. After that, select the rotating analyzer method and select θ mode (angle direction phase difference measurement and Rth calculation mode). By selecting this θ mode, the stage becomes a tilt rotation stage. (A2) Next, enter the following measurement conditions into the RETS-100. (Measurement conditions) Retardation measurement range: Rotating analyzer method Measurement spot diameter: φ5mm Tilt angle range: 0° Measurement wavelength range: 400nm~800nm - Average refractive index of plastic film (for example, N=1.617 for PET film) Thickness: Thickness measured separately using SEM or optical microscope (A3) Next, background data is obtained without placing a sample in the instrument, in a closed system, and every time the light source is turned on. (A4) After that, the sample is placed on the stage inside the device and measured.
[0049] In Condition 3, the reference direction for the angle with the slow axis direction (flow direction or width direction) may be either the flow direction or the width direction, so long as the same direction is used as the reference for all of D1 to D5.
[0050] When multiple samples measuring 50 mm in length x 50 mm in width can be taken from a sheet-like plastic film, it is preferable that the proportion of samples that satisfy the specified conditions among the multiple samples is 50% or more, more preferably 70% or more, even more preferably 90% or more, and even more preferably 100% or more. In addition, when multiple samples each having a size of 50 mm length x 50 mm width can be taken from a roll-shaped plastic film, it is preferable that the samples taken from a predetermined position in the width direction of the roll satisfy the predetermined conditions in the majority of the flow direction of the roll. By satisfying this constitution, a plastic film having a predetermined effect can be obtained by picking up a plastic film from a predetermined position in the width direction of the roll.
[0051] <Plastic film> The laminated structure of the plastic film may be a single-layer structure or a multi-layer structure, of which the single-layer structure is preferred. As described later, the plastic film is preferably a stretched plastic film with a small in-plane retardation in order to suppress rainbow unevenness while improving mechanical strength. In order to reduce the in-plane retardation of the stretched plastic film, it is important to finely control the stretching, such as making the stretching in the longitudinal direction and the transverse direction close to uniform. Regarding fine control of the stretching, it is difficult to control in the multilayer structure due to differences in the physical properties of each layer, but the single-layer structure is preferable because it is easy to control.
[0052] Examples of resin components constituting the plastic film include polyester, triacetyl cellulose (TAC), cellulose diacetate, cellulose acetate butyrate, polyamide, polyimide, polyethersulfone, polysulfone, polypropylene, polymethylpentene, polyvinyl chloride, polyvinyl acetal, polyether ketone, polymethyl methacrylate, polycarbonate, polyurethane, and amorphous olefin (Cyclo-Olefin-Polymer: COP). Among these, polyester is preferred because it is easy to improve the mechanical strength. In other words, it is preferable that the optical plastic film is a polyester film.
[0053] Examples of polyesters constituting the polyester film include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), etc. Among these, PET is preferred because it has low intrinsic birefringence and is easy to reduce the in-plane retardation.
[0054] The plastic film may contain additives such as ultraviolet absorbers, light stabilizers, antioxidants, antistatic agents, flame retardants, antigelling agents, and surfactants.
[0055] The thickness of the plastic film is preferably 15 μm to 60 μm, more preferably 20 μm to 55 μm, and even more preferably 30 μm to 50 μm. By making the thickness 15 μm or more, it is possible to easily improve the mechanical strength. Also, by making the thickness 60 μm or less, it is possible to easily reduce the in-plane retardation.
[0056] For optical plastic films, the haze according to JIS K7136:2000 is preferably 3.0% or less, more preferably 2.0% or less, and even more preferably 1.0% or less. Furthermore, the total light transmittance of optical plastic films according to JIS K7361-1:1997 is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more.
[0057] In order to improve the mechanical strength, the plastic film is preferably a stretched plastic film, more preferably a stretched polyester film, and more preferably the stretched polyester film has a single-layer structure of a polyester resin layer.
[0058] The stretched plastic film can be obtained by stretching a resin layer containing components constituting the plastic film. The stretching method includes biaxial stretching such as sequential biaxial stretching and simultaneous biaxial stretching, and uniaxial stretching such as longitudinal uniaxial stretching. Among these, biaxial stretching is preferred because it is easy to reduce the in-plane retardation and to increase the mechanical strength. That is, the stretched plastic film is preferably a biaxially stretched plastic film. Among biaxially stretched plastic films, a biaxially stretched polyester film is preferred, and a biaxially stretched polyethylene terephthalate film is more preferred. In addition, from the viewpoint of easily satisfying condition 2, it is preferable that the stretching ratios in the machine direction and the width direction of the biaxially stretched plastic film are close to each other.
[0059] -Sequential biaxial stretching- In sequential biaxial stretching, the casting film is stretched in the machine direction, and then stretched in the width direction of the film. Stretching in the machine direction is usually performed by the difference in peripheral speed of the stretching rolls, and may be performed in one step, but may also be performed in multiple steps using multiple pairs of stretching rolls. From the viewpoint of suppressing excessive variation in optical properties such as in-plane retardation, it is preferable to place multiple nip rolls close to the stretching roll. The stretching ratio in the machine direction is usually 2 to 15 times, and from the viewpoint of suppressing excessive variation in optical properties such as in-plane retardation, it is preferably 2 to 7 times, more preferably 3 to 5 times, and even more preferably 3 to 4 times. From the viewpoint of suppressing excessive variation in optical properties such as in-plane retardation, the stretching temperature is preferably from the glass transition temperature of the resin to the glass transition temperature + 100° C. In the case of PET, the temperature is preferably 70 to 120° C., more preferably 80 to 110° C., and even more preferably 95 to 110° C. Regarding the stretching temperature, the average in-plane retardation tends to be small by shortening the stretching section at low temperature by heating the film quickly, whereas the average in-plane retardation tends to be large and the variation of the slow axis tends to be small by lengthening the stretching section at low temperature by heating the film slowly. It is preferable to use a heater that generates turbulent airflow when heating during stretching. Heating with turbulent airflow generates temperature differences in minute regions within the film plane, which in turn generates minute shifts in the orientation axis, making it easier to satisfy condition 3.
[0060] The film stretched in the machine direction may be imparted with properties such as easy slippage, easy adhesion, antistatic properties, etc., by in-line coating. Furthermore, before in-line coating, surface treatment such as corona treatment, frame treatment, plasma treatment, etc. may be performed as necessary. The coating film formed by in-line coating in this way is very thin, about 10 nm to 2000 nm thick (the coating film is stretched even thinner by stretching treatment). In this specification, such a thin layer is not counted as the number of layers constituting the plastic film.
[0061] The stretching in the width direction is usually performed by using a tenter method, in which the film is conveyed while both ends of the film are held by clips, and stretched in the width direction. The stretching ratio in the width direction is usually 2 to 15 times, and from the viewpoint of suppressing excessive variation in optical properties such as in-plane retardation, it is preferably 2 to 5 times, more preferably 3 to 5 times, and further preferably 3 to 4.5 times. It is also preferable to make the width stretching ratio higher than the longitudinal stretching ratio. The stretching temperature is preferably the glass transition temperature of the resin to glass transition temperature+120°C, and the temperature preferably increases from upstream to downstream. Specifically, when the transverse stretching section is divided into two, the difference between the upstream and downstream temperatures is preferably 20°C or more, more preferably 30°C or more, even more preferably 35°C or more, and even more preferably 40°C or more. In the case of PET, the first-stage stretching temperature is preferably 80 to 120°C, more preferably 90 to 110°C, and even more preferably 95 to 105°C.
[0062] The plastic film sequentially biaxially stretched as described above is preferably heat-treated in a tenter at a temperature equal to or higher than the stretching temperature but lower than the melting point in order to impart planarity and dimensional stability. Specifically, in the case of PET, heat setting is preferably performed in the range of 150 to 255°C, more preferably 200 to 250°C. In this case, by heat-setting at a temperature as high as possible lower than the melting point, the crystallinity inside the film is maintained while the crystallinity on the film surface is slightly reduced, making it easier to satisfy condition 1. In addition, from the viewpoint of suppressing excessive variation in optical properties such as in-plane retardation, it is preferable to perform heat treatment post-stretching of 1 to 10% in the first half of the heat treatment. After the plastic film is heat-treated, it is slowly cooled to room temperature and then wound up. If necessary, a relaxation treatment or the like may be performed during the heat treatment or the slow cooling. The relaxation rate during the heat treatment is preferably 0.5 to 5%, more preferably 0.5 to 3%, even more preferably 0.8 to 2.5%, and even more preferably 1 to 2%, from the viewpoint of suppressing excessive variation in optical properties such as in-plane retardation. The relaxation rate during the slow cooling is preferably 0.5 to 3%, more preferably 0.5 to 2%, even more preferably 0.5 to 1.5%, and even more preferably 0.5 to 1.0%, from the viewpoint of suppressing excessive variation in optical properties such as in-plane retardation. The temperature during the slow cooling is preferably 80 to 150°C, more preferably 90 to 130°C, even more preferably 100 to 130°C, and even more preferably 100 to 120°C, from the viewpoint of flatness.
[0063] -Simultaneous biaxial stretching- In the simultaneous biaxial stretching, the casting film is introduced into a simultaneous biaxial tenter, and the film is conveyed while both ends are held by clips, and stretched simultaneously and / or stepwise in the machine direction and width direction. The simultaneous biaxial stretching machine may be of the pantograph type, screw type, drive motor type, or linear motor type, but the drive motor type or linear motor type is preferred because it can change the stretch ratio at any time and can perform relaxation treatment at any location.
[0064] The magnification of the simultaneous biaxial stretching is usually 6 to 50 times as an area magnification, and from the viewpoint of suppressing excessive variation in optical properties such as in-plane retardation, it is preferably 8 to 30 times, more preferably 9 to 25 times, even more preferably 9 to 20 times, and still more preferably 10 to 15 times. In the case of simultaneous biaxial stretching, in order to suppress differences in in-plane orientation, it is preferable to make the stretching ratios in the machine direction and the width direction the same, and to make the stretching speeds approximately equal.
[0065] From the viewpoint of suppressing excessive variation in optical properties such as in-plane retardation, the stretching temperature in the simultaneous biaxial stretching is preferably from the glass transition temperature of the resin to the glass transition temperature + 120° C. In the case of PET, the temperature is preferably 80 to 160° C., more preferably 90 to 150° C., and even more preferably 100 to 140° C.
[0066] The simultaneously biaxially stretched film is preferably subsequently heat-treated in a heat-fixing chamber in a tenter at a temperature equal to or higher than the stretching temperature but lower than the melting point in order to impart flatness and dimensional stability to the film. The conditions for the heat treatment are the same as those for the heat treatment after the successive biaxial stretching.
[0067] <Bending resistance> It is preferable that the plastic film does not crack or break after 100,000 times (more preferably after 300,000 times) of the folding test shown in the examples. In addition, when the measurement sample is placed on a horizontal table after 100,000 times (more preferably after 300,000 times), the angle at which the end of the sample rises from the table is preferably 20 degrees or less, more preferably 15 degrees or less. The angle at which the end of the sample rises from the table is 15 degrees or less means that the sample is unlikely to develop a crease due to folding. In addition, a plastic film that shows the above-mentioned results (no cracks, breaks, or creases due to folding. The angle at which the end of the sample rises after the test is 20 degrees or less) in both the machine direction and the width direction of the plastic film is preferable.
[0068] <Thickness> From the viewpoint of mechanical strength, the optical plastic film is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 25 μm or more. From the viewpoint of reducing the in-plane retardation, the optical plastic film is preferably 100 μm or less, more preferably 75 μm or less, and even more preferably 50 μm or less. In addition, it is preferable to make the thickness 50 μm or less from the viewpoint of improving bending resistance.
[0069] <Application> As described above, the plastic film of the present invention can provide good scratch resistance when scratched with a hard object such as a pencil or a touch panel pen, and good scratch resistance when repeatedly rubbed with a soft object such as a cloth. Therefore, the optical plastic film of the present invention can be suitably used as a plastic film for an image display device, and can be suitably used as a plastic film for an image display device equipped with a touch panel. Furthermore, a plastic film of one embodiment of the present invention that satisfies condition 2 or 3 can be prevented from retaining a bending habit or breaking after a bending test, regardless of the bending direction, and can therefore be suitably used as a plastic film for curved image display devices and foldable image display devices. Examples of plastic films for image display devices include plastic films used as substrates for various functional films such as polarizer protective films, surface protective films, anti-reflection films, and conductive films constituting touch panels.
[0070] [Optical laminate] The optical plastic film of the present invention may be further formed with functional layers such as a protective layer, an antireflection layer, a hard coat layer, an antiglare layer, a retardation layer, an adhesive layer, a transparent conductive layer, an antistatic layer and an antifouling layer to form an optical laminate. The functional layer of the optical laminate preferably includes an antireflection layer. The antireflection layer is preferably disposed on the outermost surface of the plastic film on the side having the functional layer. By providing an antireflection layer as a functional layer of the optical laminate, rainbow unevenness can be easily suppressed.
[0071] Moreover, the functional layer more preferably includes a hard coat layer and an antireflection layer. When the functional layer includes a hard coat layer and an antireflection layer, it is preferable that the hard coat layer and the antireflection layer are disposed in this order on the optical plastic film. The hard coat layer and the antireflection layer may be general-purpose layers.
[0072] [Polarizing plate] The polarizing plate of the present invention has a polarizer, a transparent protective plate A arranged on one side of the polarizer, and a transparent protective plate B arranged on the other side of the polarizer, and at least one of the transparent protective plate A and the transparent protective plate B is the optical plastic film of the present invention described above.
[0073] The polarizing plate is used, for example, in combination with a λ / 4 retardation plate to provide anti-reflection properties. In this case, the λ / 4 retardation plate is disposed on the display element of the image display device, and the polarizing plate is disposed closer to the viewer than the λ / 4 retardation plate. When the polarizing plate is used for a liquid crystal display device, it is used to provide a liquid crystal shutter function. In this case, the liquid crystal display device is arranged in the order of a lower polarizing plate, a liquid crystal display element, and an upper polarizing plate, and the absorption axis of the polarizer of the lower polarizing plate is arranged perpendicular to the absorption axis of the polarizer of the upper polarizing plate. In this configuration, it is preferable to use the polarizing plate of the present invention as the upper polarizing plate.
[0074] <Transparent protection plate> The polarizing plate of the present invention uses the above-mentioned optical plastic film of the present invention as at least one of the transparent protective plate A and the transparent protective plate B. In a preferred embodiment, both the transparent protective plate A and the transparent protective plate B are the above-mentioned optical plastic film of the present invention.
[0075] When one of the transparent protective plate A and the transparent protective plate B is the above-mentioned optical plastic film of the present invention, the other transparent protective plate is not particularly limited, but is preferably an optically isotropic transparent protective plate. Optically isotropic refers to an in-plane retardation of 20 nm or less, preferably 10 nm or less, more preferably 5 nm or less. Examples of transparent substrates having optical isotropy include acrylic film and triacetyl cellulose (TAC) film. When one of the transparent protective plates A and B is the above-mentioned optical plastic film of the present invention, it is preferable to use the above-mentioned optical plastic film of the present invention as the transparent protective plate on the light exit side.
[0076] <Polarizer> Examples of polarizers include sheet-type polarizers such as polyvinyl alcohol films, polyvinyl formal films, polyvinyl acetal films, and saponified ethylene-vinyl acetate copolymer films dyed with iodine or the like and stretched, wire-grid-type polarizers made of a large number of metal wires arranged in parallel, coating-type polarizers coated with lyotropic liquid crystal or a dichroic guest-host material, and multilayer thin-film-type polarizers. These polarizers may be reflective polarizers that have the function of reflecting polarized components that are not transmitted.
[0077] The polarizer is preferably arranged so that its absorption axis is approximately parallel or approximately perpendicular to the flow direction or width direction of the optical plastic film. Approximately parallel means within 0 degrees ±5 degrees, preferably within 0 degrees ±3 degrees, more preferably within 0 degrees ±1 degree. Approximately perpendicular means within 90 degrees ±5 degrees, preferably within 90 degrees ±3 degrees, more preferably within 90 degrees ±1 degree.
[0078] [Image display device] The image display device of the present invention is an image display device having a display element and a plastic film arranged on the light emission surface side of the display element, wherein the plastic film is the optical plastic film of the present invention described above.
[0079] 4 and 5 are cross-sectional views showing an embodiment of an image display device 100 of the present invention. The image display device 100 in Figs. 4 and 5 has an optical plastic film 10 on the light exit surface side of the display element 20 (upper side in Figs. 4 and 5). Both image display devices 100 in Figs. 4 and 5 have a polarizer 31 between the display element 20 and the optical plastic film 10. In Figs. 4 and 5, a transparent protective plate A (32) and a transparent protective plate B (33) are laminated on both sides of the polarizer 31. In the image display device in Fig. 5, the optical plastic film 10 is used as the transparent protective plate A (32).
[0080] It should be noted that the image display device 100 is not limited to the form shown in Fig. 4 and Fig. 5. For example, while the components constituting the image display device 100 are arranged at a predetermined interval in Fig. 4 and Fig. 5, the components may be integrated together via an adhesive layer or the like. The image display device may also have components (other plastic films, functional layers, etc.) that are not shown.
[0081] <Display element> Examples of the display element include a liquid crystal display element, an EL display element (an organic EL display element, an inorganic EL display element), a plasma display element, and further include an LED display element such as a micro LED display element. When the display element of the display device is a liquid crystal display element, a backlight is required on the surface of the liquid crystal display element opposite to the resin sheet.
[0082] The image display device may be an image display device equipped with a touch panel function. Examples of touch panels include resistive, capacitive, electromagnetic induction, infrared, and ultrasonic touch panels. The touch panel function may be added to a display element, such as an in-cell touch panel liquid crystal display element, or may be a display element having a touch panel placed on it.
[0083] As described above, the optical plastic film of the present invention can suppress the occurrence of bending creases or breakage after a bending test, and therefore the image display device of the present invention is preferable in that it can exert a more remarkable effect when the image display device is a curved image display device or a foldable image display device. When the image display device is a curved image display device or a foldable image display device, the display element is preferably an organic EL display element.
[0084] <Plastic film> The image display device of the present invention has the above-mentioned optical plastic film of the present invention on the light emission surface side of the display element. The plastic film may be only one sheet or two or more sheets. Examples of the plastic film arranged on the light exit surface side of the display element include plastic films used as substrates for various functional films such as polarizer protective films, surface protective films, anti-reflection films, and conductive films that constitute touch panels.
[0085] <Other plastic films> The image display device of the present invention may contain other plastic films as long as the effects of the present invention are not impaired. As the other plastic films, those having optical isotropy are preferred. EXAMPLES
[0086] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.
[0087] 1. Measurement and Evaluation The atmosphere for the following measurements and evaluations is set to a temperature of 23° C.±5° C. and a humidity of 40 to 65% RH. Furthermore, before the measurements and evaluations, the samples are exposed to the above atmosphere for 30 minutes or more.
[0088] 1-1. In-plane retardation (Re), thickness retardation (Rth) and slow axis direction Samples of 50 mm in the machine direction × 50 mm in the width direction were cut out from the optical plastic films of the Examples and Comparative Examples produced or prepared in "2" below. The in-plane retardation, thickness direction retardation, and slow axis direction were measured for a total of five locations, 4 locations 10 mm from the four corners toward the center of the cut out sample, and the center of the sample. The average of Re1 to Re5 calculated from the measurement results is shown in Table 1. The measurement device used was "RETS-100 (measurement spot: diameter 5 mm)" manufactured by Otsuka Electronics Co., Ltd. The slow axis direction was measured in the range of 0 to 90 degrees, with the machine direction (MD) of the plastic film as the reference 0 degree.
[0089] 1-2. Cross-section indentation hardness Two cut samples were prepared by cutting the sample into pieces measuring 2 mm in the flow direction and 10 mm in the width direction from within the region of the sample cut out in 1-1 above, measuring 50 mm in the flow direction and 50 mm in the width direction, and then the cut samples were embedded in resin to prepare two embedded samples, as shown in Figure 1. The embedded samples were prepared according to the preferred methods exemplified in (A1) and (A2) of the main text of the specification. One embedded sample was cut vertically along the flow direction with a diamond knife, and a cross section in the flow direction was exposed to prepare sample A for measuring the indentation hardness of the cross section in the flow direction. The other embedded sample was cut vertically along the width direction with a diamond knife, and a cross section in the width direction was exposed to prepare sample B for measuring the indentation hardness of the cross section in the width direction. The device used to cut the embedded sample was Leica Microsystems' product name "Ultramicrotome EM UC7". The embedded sample was cut so as to pass through the center of the cut sample. The cutting was performed roughly at first (rough trimming), and finally, the cutting was performed precisely under the conditions of "SPEED: 1.00 mm / s" and "FEED: 70 nm" so that the cut surface passing through the center of the sample was approximately flat. After the precise trimming, it was confirmed with a microscope that there were no foreign objects or unevenness that would hinder the measurement on the cut surface. Next, using sample A, the indentation hardness of the cross section on the first surface side, the indentation hardness of the cross section on the second surface side, and the indentation hardness of the cross section at the center in the thickness direction were measured, and MD1 and MD2 were calculated. Similarly, using sample B, the indentation hardness of the cross section on the first surface side, the indentation hardness of the cross section on the second surface side, and the indentation hardness of the cross section at the center in the thickness direction were measured, and TD1 and TD2 were calculated. The results are shown in Table 1. As described in the specification, MD1, MD2, TD1, and TD2 mean the average values of five measured values. The indentation hardness of the cross section on the first surface side and the indentation hardness of the cross section on the second surface side were measured at positions 2.0 μm inward from the first surface and the second surface, as shown in FIG. The indentation hardness was measured by pressing a Berkovich indenter (material: diamond triangular pyramid) vertically into the cross section, using a measuring device, model number "TI950 TriboIndenter" manufactured by HYSITRON Corporation, and the application software (TriboScan Version 9.6.0.2) that came with the device, under the following conditions. In addition, in the above measurement, before measuring the indentation hardness of each sample, a standard sample (fused quartz (5-0098) manufactured by HYSITRON) with known indentation hardness and composite modulus was used to perform an indentation test, and standard alignment was performed to confirm that the indentation hardness and composite modulus obtained from the test results were within the standard values. That is, after performing the standard alignment, the indentation hardness of the cross section on the first surface side, the indentation hardness of the cross section on the second surface side, and the indentation hardness of the cross section at the center in the thickness direction were each measured five times for sample A. Then, after the measurement of sample A was completed, the standard alignment was performed again, and the indentation hardness of the cross section on the first surface side, the indentation hardness of the cross section on the second surface side, and the indentation hardness of the cross section at the center in the thickness direction were each measured five times for sample B. In Table 1, those that satisfy condition 1 (MD2 / MD1 and TD2 / TD1 are both greater than 1.01 and less than or equal to 1.30) are indicated as "Y", and those that do not are indicated as "N".
[0090] <Measurement conditions> Indenter used: Berkovich indenter (model number: TI-0039, manufactured by HYSITRON) -Indentation condition: Displacement control method Maximum indentation depth: 200 nm Load application time: 20 seconds (speed: 10 nm / sec) Hold time: Hold for 5 seconds at maximum pressing depth Loading / unloading time: 20 seconds (speed: 10 nm / sec)
[0091] 1-3. Scratch resistance 1 (resistance to scratches caused by hard objects) A test pencil having a hardness of F as specified by JIS S6006 was pressed against the surface of the optical plastic film of each of the examples and comparative examples, and a pencil hardness test (4.9N load) as specified by JIS K5600-5-4:1999 was performed. The test was performed in both the machine direction and the width direction. As a result, the plastic film whose surface was not scratched in either direction was rated as "A", and the plastic film whose surface was scratched in at least one direction was rated as "C".
[0092] 1-4. Scratch resistance 2 (scratch resistance against soft objects) A cotton No. 300 flannel cloth was pressed against the surface of the optical plastic film of each of the examples and comparative examples with a load of 500 g / cm. 2 After rubbing 1000 times with a brush, the film was visually inspected for scratches under fluorescent lighting. The test was performed in both the machine direction and the width direction. The test equipment used was a Gakushin abrasion tester (model number "AB-301" manufactured by Tester Sangyo Co., Ltd.). As a result, plastic films that did not have scratches on the surface in either direction were rated as "A," and plastic films that had scratches on the surface in at least one direction were rated as "C."
[0093] 1-5. Flexibility <Width direction> From the optical plastic films of the Examples and Comparative Examples, rectangular samples with short sides (width direction) of 30 mm and long sides (flow direction) of 100 mm were cut out. Both ends of the short side (30 mm) of the sample were fixed (a region 10 mm from the tip was fixed) to a durability tester (product name "DLDMLH-FS", manufactured by Yuasa System Equipment Co., Ltd.), and a continuous folding test was performed by folding the sample 180 degrees 100,000 times. The folding speed was 120 times per minute. A more detailed method of the folding test is shown below. After the folding test, the rectangular sample was placed on a horizontal table and the angle at which the end of the sample rose above the table was measured. The results are shown in Table 1. Samples that broke midway through the folding test were recorded as "broken." <Flow direction> From the optical plastic films of the Examples and Comparative Examples, rectangular samples with short sides (machine direction) of 30 mm and long sides (width direction) of 100 mm were cut out and evaluated in the same manner as above.
[0094] <Details of folding test> 6(A), in the continuous folding test, first, side portion 10C of plastic film 10 and side portion 10D opposite side portion 10C are fixed by fixing portions 60 arranged in parallel with each other. Fixing portions 60 are slidable in the horizontal direction. Next, as shown in Figure 6 (B), the fixing portions 60 are moved closer to each other to deform the plastic film 10 in a folding manner, and further, as shown in Figure 6 (C), the fixing portions 60 are moved to a position where the distance between the two opposing edges of the plastic film 10 fixed by the fixing portions 60 is 2 mm, and then the fixing portions 60 are moved in the opposite direction to eliminate the deformation of the plastic film 10. 6(A) to 6(C), the plastic film 10 can be folded 180 degrees by moving the fixing part 60. Moreover, by performing a continuous folding test so that the bent part 10E of the plastic film 10 does not protrude from the lower end of the fixing part 60 and controlling the distance between the fixing parts 60 at their closest point to 2 mm, the distance between the two opposing sides of the optical film 10 can be set to 2 mm.
[0095] 1-6.Rainbow unevenness The samples (samples prepared in 1-1) cut from the optical plastics of the Examples and Comparative Examples were placed on the viewing-side polarizing plate of the image display device having the following configuration so that the TD direction of the samples was parallel to the horizontal direction of the screen. The image display device was then turned on in a darkroom environment and observed from various angles with the naked eye to evaluate the presence or absence of rainbow unevenness according to the following criteria. A: No rainbow unevenness is visible. B: Rainbow unevenness is visible in a small area. C: Rainbow unevenness is visible in most areas. <Configuration of image display device> (1) Backlight light source: White LED or cold cathode fluorescent lamp (2) Light source side polarizing plate: TAC as protective film on both sides of polarizer made of PVA and iodine The film is arranged so that the absorption axis of the polarizer is perpendicular to the horizontal direction of the screen. (3) Image display cell: Liquid crystal cell (4) Viewing side polarizing plate: TAC as a polarizer protection film for a polarizer made of PVA and iodine A polarizing plate using film. The polarizer is arranged so that the absorption axis is perpendicular to the parallel direction of the screen. (5) Size: 10 inches diagonal
[0096] 1-7. Blackout The samples (samples prepared in 1-1) cut out from the optical plastics of the Examples and Comparative Examples were placed on the viewing-side polarizing plate of the image display device having the configuration shown in 1-6 so that the TD direction of the samples was parallel to the horizontal direction of the screen. Next, with the image display with the samples placed in portrait orientation, the image display devices prepared in the Examples and Comparative Examples were viewed from the front through polarized sunglasses that absorb S-polarized light, and blackout was evaluated according to the following criteria. A: The entire area does not black out. B: A small area is blacked out. C: Most of the area is blacked out.
[0097] 2. Preparation and Fabrication of Stretched Polyester Film [Example 1] 1 kg of PET (melting point 258°C, absorption center wavelength: 320 nm) and 0.1 kg of ultraviolet absorber (2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazinon-4-one) were melt-mixed at 280°C in a kneader to produce pellets containing the ultraviolet absorber. The pellets and PET with a melting point of 258°C were fed into a single-screw extruder and melt-kneaded at 280°C, extruded from a T-die, and cast onto a cast drum with a surface temperature controlled at 25°C to obtain a casting film. The amount of ultraviolet absorber in the casting film was 1 part by mass per 100 parts by mass of PET. The obtained casting film was heated with a group of rolls set at 95°C, and then stretched 3.3 times in the machine direction while being heated from both sides with a radiation heater so that the film temperature at a point 150 mm into the 400 mm stretching section (starting point is stretching roll A and ending point is stretching roll B; stretching rolls A and B each have two nip rolls) would be 103°C, and then cooled once. During heating with the radiation heater, air at 92°C and 4 m / s was blown toward the film from the opposite side of the film from the radiation heater, causing turbulence on both sides of the film and disrupting the temperature uniformity of the film. Next, both sides of this uniaxially stretched film were subjected to a corona discharge treatment in air to set the wetting tension of the base film to 55 mN / m, and the corona discharge-treated surfaces of both sides of the film were in-line coated with "a lubricity layer coating solution containing a polyester resin with a glass transition temperature of 18°C, a polyester resin with a glass transition temperature of 82°C, and silica particles with an average particle size of 100 nm" to form a lubricity layer. Next, the uniaxially stretched film was introduced into a tenter, preheated with hot air at 95°C, and then stretched 4.5 times in the film width direction at a temperature of 105°C in the first stage and 140°C in the second stage. Here, when the transverse stretching section was divided into two, the film was stretched in two stages so that the stretch amount of the film at the midpoint of the transverse stretching section (film width at the measurement point - film width before stretching) was 80% of the stretch amount at the end of the transverse stretching section. The transversely stretched film was heat-treated in the tenter stepwise from 180°C to 245°C with hot air, followed by 1% relaxation treatment in the width direction under the same temperature conditions, and further quenched to 100°C, followed by 1% relaxation treatment in the width direction, and then wound up to obtain an optical plastic film of Example 1 (biaxially stretched polyester film, thickness 40 μm).
[0098] [Example 2] An optical plastic film (biaxially oriented polyester film, thickness 40 μm) of Example 2 was obtained in the same manner as Example 1, except that the point where the film temperature reached 103°C was changed to a point 200 mm into the 400 mm stretching section.
[0099] [Example 3] An optical plastic film (biaxially oriented polyester film, thickness 50 μm) of Example 3 was obtained in the same manner as in Example 1, except that the thickness of the casting film of Example 1 was increased, the stretching ratio in the machine direction was changed from 3.3 times to 3.5 times, and the stretching ratio in the width direction was changed from 4.5 times to 5.0 times.
[0100] [Example 4] An optical plastic film (biaxially oriented polyester film, thickness 42 μm) of Example 4 was obtained in the same manner as in Example 1, except that the thickness of the casting film of Example 1 was increased, the stretching ratio in the machine direction was changed from 3.3 times to 3.5 times, and the stretching ratio in the width direction was changed from 4.5 times to 5.0 times.
[0101] [Comparative Example 1] As an optical plastic film of Comparative Example 1, a commercially available biaxially stretched polyester film (manufactured by Toyobo Co., Ltd., product name: Cosmoshine A4100, thickness: 50 μm) was prepared.
[0102] [Comparative Example 2] As the optical plastic film of Comparative Example 2, a biaxially stretched polyester film having a three-layer structure (three layers of crystalline polyester / non-crystalline polyester / crystalline polyester) according to Example 13 of JP-A No. 2018-59078 was prepared.
[0103] [Table 1]
[0104] From the results in Table 1, it can be confirmed that the optical plastic films of Examples 1 to 4, which satisfy Condition 1, can provide good scratch resistance against both hard and soft objects. It can also be confirmed that the optical plastic films of Examples 1 to 4 can suppress blackout by satisfying Condition 3, and furthermore, can suppress the remaining bending tendency or breakage after a bending test, regardless of the bending direction. It can also be confirmed that the optical plastic films of Examples 1 and 2 can suppress rainbow unevenness by satisfying Condition 4. [Explanation of symbols]
[0105] 10: Optical plastic film 20: Display element 30: Polarizing plate 31: Polarizer 32: Transparent protection plate A 33: Transparent protection plate B 50: Cabinet 100: Image display device S: Cut sample of plastic film R:Embedding resin d: Thickness direction of cut sample of plastic film
Claims
[Claim 1] An optical plastic film having a first surface and a second surface located opposite to the first surface, and satisfying the following condition 1: <Condition 1> Regarding the indentation hardness of the cross section in the machine direction of the plastic film, the softer of the indentation hardness of the cross section on the first surface side and the indentation hardness of the cross section on the second surface side is defined as MD1, and the indentation hardness of the cross section at the center in the thickness direction is defined as MD2. Regarding the indentation hardness of the cross section in the width direction of the plastic film, the softer of the indentation hardness of the cross section on the first surface side and the indentation hardness of the cross section on the second surface side is defined as TD1, and the indentation hardness of the cross section at the center in the thickness direction is defined as TD2. Under such a premise, both MD2 / MD1 and TD2 / TD1 are greater than 1.01 and less than 1.30.
Citation Information
Patent Citations
Cellulose acylate film and its manufacturing method, and optical retardation film, polarizing plate and liquid crystal display device obtained using the same
JP2007332367A
Hardcoating film and antireflection film
JP2009227906A
Phosphor element, light emitting device, and method of manufacturing phosphor element
JP2010283214A
Hard coating film and image display device using the same
JP2017156753A
Prism, particularly for optical data communication
US20150285965A1