Flux-cored wire

A flux-cored wire with controlled austenite and ferrite phases addresses the strength and toughness issues of stainless steel wires for liquefied natural gas tanks, ensuring effective welding and low-temperature performance.

JP2024160398APending Publication Date: 2024-11-13KOBE STEEL LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024144196
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-13

AI Technical Summary

Technical Problem

Storage tanks for liquefied natural gas require toughness in a lower temperature range than those for liquefied ethylene gas, and existing stainless steel flux-cored wires do not provide sufficient strength and are prone to hot cracking, necessitating a flux-cored wire with improved welding workability and low-temperature toughness.

Method used

A flux-cored wire composition is specified within a predetermined range to control the ratio of austenite and ferrite phases, achieving single-phase ferrite solidification and precipitating fine Widmanstätten austenite, with specific elemental ratios to enhance tensile strength and low-temperature toughness.

Benefits of technology

The flux-cored wire achieves good welding workability with a weld metal exhibiting excellent tensile strength and low-temperature toughness, maintaining a balance between mechanical properties and weld quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160398000001_ABST
    Figure 2024160398000001_ABST
Patent Text Reader

Abstract

To provide a flux-cored wire which has excellent welding workability during gas-shielded arc welding and can give a welded metal having excellent toughness at low temperatures and tensile strength.SOLUTION: This flux-cored wire for gas-shielded arc welding has a sheath filled with a flux, with its chemical components adequately controlled, and θ of 10.0 or more to 30.0 or less calculated by the mathematical formula (I). (I): θ=4.1×α-3.2×γ-32.3, where α=0.02×[Si]+[Cr]+1.20×[Mo]+0.3×[Ti]+0.30 and γ=24×[C]+28×[N]+0.25×[Mn]+0.5×[Cu]+1.10×[Ni], when [Si], [Cr], [Mo], [Ti], [C], [N], [Mn], [Cu], and [Ni] denote the content (mass%) of Si, Cr, Mo, Ti, C, N, Mn, Cu and Ni respectively relative to the total mass of the wire.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a flux-cored wire. [Background technology]

[0002] Generally, gas is liquefied at low temperatures and stored in tanks to increase the efficiency of transportation and storage, so the structural components of storage tanks are required to have low-temperature toughness in the liquefaction temperature range of the stored gas. 5% Ni steel plates, which have good tensile strength and low-temperature toughness, are used as structural members for storage tanks for liquefied ethylene gas, etc. Ni-based alloy welding materials are often used as welding materials for 5% Ni steel plates, but stainless steel welding materials, which are less expensive than Ni-based alloys, are also used.

[0003] Here, Patent Document 1 discloses a stainless steel flux-cored wire for 5% Ni steel plate. This flux-cored wire aims to improve low-temperature toughness by adjusting the composition of the weld metal so as to have a fully austenitic structure. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 6719217 Summary of the Invention [Problem to be solved by the invention]

[0005] On the other hand, storage tanks for liquefied natural gas require toughness properties at even lower temperatures than tanks for liquefied ethylene gas, so 9% Ni steel plate, which has better low-temperature toughness and higher strength than 5% Ni steel plate, is used.

[0006] As with 5% Ni steel plate, Ni-based alloy welding materials are generally used for 9% Ni steel plate, but if stainless steel welding materials can be used, costs can be reduced. However, the stainless steel flux-cored wire described in Patent Document 1 cannot be used for 9% Ni steel plates because it may not have sufficient strength. In addition, in order to prevent hot cracking, it is preferable that the wire contains a certain amount of ferrite phase rather than a complete austenite structure. Furthermore, good welding workability is also required for the flux-cored wire during arc welding.

[0007] The present invention has been made in view of the above-mentioned circumstances, and has an object to provide a flux-cored wire which has good welding workability during gas-shielded arc welding and can provide a weld metal excellent in tensile strength and low-temperature toughness. [Means for solving the problem]

[0008] As a result of intensive research to solve the above problems, the inventors have found that by specifying the components of the flux-cored wire within a predetermined range, the ratio of austenite and ferrite phases in the weld metal can be controlled, the solidification form is F mode, which is a ferrite single-phase solidification, and fine Widmanstätten austenite is precipitated, thereby improving tensile strength and low-temperature toughness. The present invention was made based on these findings.

[0009] The above object of the present invention is achieved by the following configuration [1] relating to a flux-cored wire.

[0010] [1] A flux-cored wire for gas-shielded arc welding, the outer sheath of which is filled with flux, For the total mass of wire, Fe: 40% by mass or more and 70% by mass or less, Cr: 15.0% by mass or more and 25.0% by mass or less, Ni: 5.0% by mass or more and 11.0% by mass or less, Si: 0.5% by mass or more and 3.0% by mass or less, Mn: 0.5% by mass or more and 5.0% by mass or less, Total content of Na and K: 0.05% by mass or more and 1.0% by mass or less, TiO2: 3.0% by mass or more and 9.0% by mass or less, ZrO2: more than 1.0 mass% and 4.0 mass% or less, Al2O3: 0.3 mass% or more and 2.0 mass% or less, C: less than 0.015% by mass, Ti: 1.0% by mass or less, Mo: 2.0% by mass or less, Cu: 0.5% by mass or less, Al: 0.9% by mass or less, N: 0.040% by mass or less, F: 0.30% by mass or less, A flux-cored wire, wherein θ calculated by the following formula (I) is 10.0 or more and 30.0 or less. θ=4.1×α-3.2×γ-32.3 (I) However, when the Si content with respect to the total mass of the wire is defined as [Si] in mass%, the Cr content with respect to the total mass of the wire is defined as [Cr] in mass%, the Mo content with respect to the total mass of the wire is defined as [Mo] in mass%, the Ti content with respect to the total mass of the wire is defined as [Ti] in mass%, the C content with respect to the total mass of the wire is defined as [C] in mass%, the N content with respect to the total mass of the wire is defined as [N] in mass%, the Mn content with respect to the total mass of the wire is defined as [Mn] in mass%, the Cu content with respect to the total mass of the wire is defined as [Cu] in mass%, and the Ni content with respect to the total mass of the wire is defined as [Ni] in mass%, α=0.02×[Si]+[Cr]+1.20×[Mo]+0.3×[Ti]+0.30 Let γ=24×[C]+28×[N]+0.25×[Mn]+0.5×[Cu]+1.10×[Ni].

[0011] In addition, one embodiment of the flux-cored wire is For the total mass of wire, The alloy is characterized by containing Bi in an amount of 0.001% by mass or more and 0.10% by mass or less. Effect of the Invention

[0012] According to the present invention, it is possible to provide a flux-cored wire which exhibits good welding workability during gas-shielded arc welding and can produce a weld metal excellent in tensile strength and low-temperature toughness. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a graph showing the relationship between tensile strength and θ in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the embodiments of the present invention will be described in detail. Note that the present invention is not limited to the embodiments described below, and can be modified and implemented as desired without departing from the gist of the present invention.

[0015] [Flux-cored wire] The flux-cored wire according to this embodiment (hereinafter, simply referred to as "wire") has a steel sheath filled with flux. In this embodiment, the outer diameter of the wire is not particularly limited, but is preferably, for example, 0.9 mm or more and 1.6 mm or less. In addition, the flux filling rate can be set to any value as long as the content of each element in the wire is within the range of the present invention, but from the viewpoint of wire drawability and wire feedability during wire production, it is preferable to set it to, for example, 10 mass % or more and 20 mass % or less with respect to the total mass of the wire. Furthermore, the wire is not limited in the form of the seam or the cross-sectional shape, for example, in the case where the outer sheath has a seam or the case where the outer sheath has no seam. The wire according to this embodiment can be used for gas-shielded arc welding, for example, with 100 vol. % CO2 gas as the shielding gas.

[0016] Hereinafter, the components contained in the flux-cored wire for gas-shielded arc welding according to the present embodiment will be described in detail with respect to the reasons for their addition and the reasons for limiting their numerical values.

[0017] <Fe: 40 mass% or more and 70 mass% or less> Fe is the main component of the wire according to this embodiment. The Fe content with respect to the total mass of the wire is 40 mass% or more, preferably 45 mass% or more, and more preferably 50 mass% or more. Also, the Fe content with respect to the total mass of the wire is 70 mass% or less, preferably 67.5 mass% or less, and more preferably 65 mass% or less.

[0018] <Cr: 15.0 mass% or more and 25.0 mass% or less> Cr is an important constituent element that determines the amount of ferrite in the weld metal, and is also an important element for the oxidation resistance of the weld metal, the stability of ferrite, and the suppression of embrittlement behavior due to thermal cycles. When the Cr content with respect to the total mass of the wire is less than 15.0 mass%, it becomes insufficient to obtain a weld metal with a high ferrite structure. Therefore, the Cr content with respect to the total mass of the wire is 15.0 mass% or more, preferably 15.5 mass% or more, and more preferably 16.0 mass% or more. On the other hand, when the Cr content with respect to the total mass of the wire exceeds 25.0 mass%, the tendency for embrittlement due to multiple thermal cycles during welding becomes significant. Therefore, the Cr content with respect to the total mass of the wire is 25.0 mass% or less, preferably 24.5 mass% or less, and more preferably 24.0 mass% or less.

[0019] <Ni: 5.0 mass% or more and 11.0 mass% or less> Ni, like Cr, is an important constituent element that determines the amount of ferrite in the weld metal, and is also an important element for the oxidation resistance of the weld metal, the stability of austenite, and the suppression of embrittlement behavior due to thermal cycles. When the Ni content with respect to the total mass of the wire is less than 5.0 mass%, it becomes insufficient to obtain a weld metal with a high austenite structure. Therefore, the Ni content with respect to the total mass of the wire is 5.0 mass% or more, preferably 5.5 mass% or more, and more preferably 6.0 mass% or more. On the other hand, when the Ni content exceeds 11.0% by mass with respect to the total mass of the wire, it becomes difficult to secure the amount of ferrite considered necessary in the present invention. Therefore, the Ni content with respect to the total mass of the wire is 11.0% by mass or less, preferably 10.8% by mass or less, and more preferably 10.6% by mass or less.

[0020] <Si: 0.5% by mass or more and 3.0% by mass or less> Si is an important element as a deoxidizer for the weld metal and is a component having an effect of improving the wettability of the weld bead. When the Si content with respect to the total mass of the wire is less than 0.5% by mass, it causes insufficient deoxidation, which may cause pore defects such as blowholes or may cause a decrease in the toughness of the weld metal. Therefore, the Si content with respect to the total mass of the wire is 0.5% by mass or more, preferably 0.6% by mass or more, and more preferably 0.8% by mass or more. On the other hand, although Si is a ferrite stabilizing element, if it is added excessively to the wire, the toughness decreases even with the same amount of ferrite. Therefore, the Si content with respect to the total mass of the wire is 3.0% by mass or less, preferably 2.5% by mass or less, and more preferably 2.0% by mass or less. In this embodiment, the Si content represents the total Si content derived from Si alone, Si compounds, and Si alloys contained in the wire.

[0021] <Mn: 0.5% by mass or more and 5.0% by mass or less> Mn is an important element as a deoxidizer for the weld metal. When the Mn content with respect to the total mass of the wire is less than 0.5% by mass, it causes insufficient deoxidation, which may cause pore defects such as blowholes or may cause a decrease in the toughness of the weld metal. Therefore, the Mn content with respect to the total mass of the wire is 0.5% by mass or more, preferably 1.0% by mass or more, and more preferably 1.5% by mass or more. On the one hand, if the Mn content exceeds 5.0% by mass with respect to the total mass of the wire, the slag detachability may decrease. Therefore, the Mn content with respect to the total mass of the wire should be 5.0% by mass or less, preferably 4.0% by mass or less, and more preferably 3.0% by mass or less.

[0022] <Total amount of Na and K: 0.05% by mass or more and 1.0% by mass or less> Na and K are components that have the effect of stabilizing the arc. By adding an appropriate amount into the wire, a good bead shape can be obtained. If the total amount of Na and K with respect to the total mass of the wire is less than 0.05% by mass, a good bead shape cannot be obtained. Therefore, the total amount of Na and K with respect to the total mass of the wire should be 0.05% by mass or more, preferably 0.10% by mass or more, and more preferably 0.50% by mass or more. On the one hand, if the total amount of Na and K with respect to the total mass of the wire exceeds 1.0% by mass, the low-temperature toughness decreases. Therefore, the total amount of Na and K with respect to the total mass of the wire should be 1.0% by mass or less, preferably 0.9% by mass or less, and more preferably 0.8% by mass or less. Note that both Na and K may be contained in the wire, or only one of them may be contained in the wire, as long as the total amount is 0.05% by mass or more and 1.0% by mass or less.

[0023] <TiO2: 3.0% by mass or more and 9.0% by mass or less> TiO2 is added into the wire as a slag former and is a component having the effect of forming a slag with good covering property. If the TiO2 content with respect to the total mass of the wire is less than 3.0% by mass, the covering property of the slag deteriorates. Therefore, the TiO2 content with respect to the total mass of the wire should be 3.0% by mass or more, preferably 5.0% by mass or more, and more preferably 7.0% by mass or more. On the other hand, when the TiO₂ content with respect to the total mass of the wire exceeds 9.0% by mass, the amount of slag generation becomes excessive, and slag entrainment is likely to occur in the welded part. Therefore, the TiO₂ content with respect to the total mass of the wire should be 9.0% by mass or less, preferably 8.5% by mass or less, and more preferably 8.0% by mass or less. In this embodiment, the TiO₂ content is the TiO₂ conversion value of the Ti compound.

[0024] <ZrO₂::more than 1.0% by mass and 4.0% by mass or less> ZrO₂ is a high melting point oxide and is a component that adjusts the viscosity and melting point of the slag. It has the effect of increasing the solidification temperature of the slag and improving the bead shape during welding. When the ZrO₂ content with respect to the total mass of the wire is 1.0% by mass or less, the bead shape deteriorates. Therefore, the ZrO₂ content with respect to the total mass of the wire should be more than 1.0% by mass, preferably 1.3% by mass or more, and more preferably 1.6% by mass or more. On the other hand, when the ZrO₂ content with respect to the total mass of the wire exceeds 4.0% by mass, the melting point of the molten slag may become too high, resulting in deterioration of the bead appearance and bead shape. Therefore, the ZrO₂ content with respect to the total mass of the wire should be 4.0% by mass or less, preferably 3.0% by mass or less, and more preferably 2.0% by mass or less. In this embodiment, the ZrO₂ content is defined as the ZrO₂ conversion value of all Zr contained in Zr metal, Zr alloy and Zr compound.

[0025] <Al₂O₃: 0.3% by mass or more and 2.0% by mass or less> Al₂O₃ is a component that has the effect of increasing the viscosity of the molten slag, improving the fluidity, and improving the bead appearance and bead shape. If the Al2O3 content relative to the total mass of the wire is less than 0.3% by mass, the bead appearance and bead shape cannot be maintained well, and in particular, the workability of vertical welding deteriorates. Therefore, the Al2O3 content relative to the total mass of the wire is 0.3% by mass or more, preferably 0.6% by mass or more, and more preferably 0.9% by mass or more. On the other hand, if the Al2O3 content relative to the total mass of the wire exceeds 2.0% by mass, the viscosity of the molten slag becomes too high and the bead shape becomes poor. Therefore, the Al2O3 content relative to the total mass of the wire is 2.0% by mass or less, preferably 1.5% by mass or less, and more preferably 1.0% by mass or less. In this embodiment, the Al2O3 content is the value in terms of Al2O3 of the Al compound.

[0026] <C: less than 0.015% by mass> By containing C in the wire, the carbon amount in the weld metal increases and the low-temperature toughness decreases. Therefore, it is preferable to reduce the C content relative to the total mass of the wire as much as possible. When the C content relative to the total mass of the wire is 0.015% by mass or more, the low-temperature toughness of the weld metal decreases and the amount of spatter generated during welding increases. Therefore, the C content relative to the total mass of the wire is less than 0.015% by mass, preferably 0.012% by mass or less, and more preferably 0.009% by mass or less.

[0027] <Ti: 1.0% by mass or less> Ti is not an essential component in the wire of this embodiment, but since it is an element having a deoxidizing action, Ti can be contained in the wire as an optional component. When the Ti content relative to the total mass of the wire exceeds 1.0% by mass, due to the effect as a strong deoxidizer, the carbon in the weld metal increases and the toughness of the weld metal decreases. Therefore, the Ti content relative to the total mass of the wire is 1.0% by mass or less, preferably 0.8% by mass or less, and more preferably 0.6% by mass or less. Note that the lower limit of the Ti content with respect to the total mass of the wire is not particularly limited and may be 0% by mass, but may also be 0.001% by mass or more. Also, in the present embodiment, the Ti content is the total amount of Ti contained in Ti alone and Ti alloys.

[0028] <Mo: 2.0% by mass or less> Mo is not an essential component in the wire of the present embodiment, but Mo can be contained in the wire as an optional component for the purpose of improving the strength of the weld metal. When the Mo content with respect to the total mass of the wire exceeds 2.0% by mass, the low-temperature toughness decreases. Therefore, the Mo content with respect to the total mass of the wire is 2.0% by mass or less, preferably 1.8% by mass or less, and more preferably 1.6% by mass or less. Note that the lower limit of the Mo content with respect to the total mass of the wire is not particularly limited and may be 0% by mass, but may also be 0.001% by mass or more.

[0029] <Cu: 0.5% by mass or less> Cu is not an essential component in the wire of the present embodiment, but Cu can be contained in the wire as an optional component for the purpose of stabilizing the austenite structure. When the Cu content with respect to the total mass of the wire exceeds 0.5% by mass, the low-temperature toughness decreases. Therefore, the Cu content with respect to the total mass of the wire is 0.5% by mass or less, preferably 0.3% by mass or less, and more preferably 0.1% by mass or less. Note that the lower limit of the Cu content with respect to the total mass of the wire is not particularly limited and may be 0% by mass, but may also be 0.001% by mass or more.

[0030] <Al: 0.9% by mass or less> Al is not an essential component in the wire of the present embodiment, but since Al is an element having a deoxidizing action, Al can be contained in the wire as an optional component. When the Al content with respect to the total mass of the wire exceeds 0.9% by mass, the solidification structure of ferrite changes from columnar crystals to equiaxed crystals, and the shape of austenite formed thereafter changes from Widmanstätten structure to granular structure. As a result, the toughness decreases and the slag detachability deteriorates. Therefore, the Al content with respect to the total mass of the wire is 0.9% by mass or less, preferably 0.6% by mass or less, and more preferably 0.2% by mass or less. Note that the lower limit of the Al content with respect to the total mass of the wire is not particularly limited, and it may be 0% by mass, or may be 0.001% by mass or more. In this embodiment, the Al content is the total amount of Al contained in Al alone and Al alloys.

[0031] <N: 0.040% by mass or less> N is not an essential component in the wire of this embodiment, but since it is an element having an effect of improving the strength of the weld metal and reducing the surface tension to improve the bead conformity, N can be contained in the wire as an optional component. When the N content with respect to the total mass of the wire exceeds 0.040% by mass, the surface tension of the molten metal becomes too low, spatter increases, the bead shape deteriorates, and the slag detachability also deteriorates. Therefore, the N content with respect to the total mass of the wire is 0.040% by mass or less, preferably 0.030% by mass or less, and more preferably 0.020% by mass or less. Note that the lower limit of the N content with respect to the total mass of the wire is not particularly limited, and it may be 0% by mass, or may be 0.001% by mass or more.

[0032] <F: 0.30% by mass or less> F is not an essential component in the wire of this embodiment, but since it is an element having an effect of increasing the viscosity of the molten slag, improving the fluidity, and improving the bead appearance and bead shape, F can be contained in the wire as an optional component. If the F content exceeds 0.30% by mass relative to the total mass of the wire, there is a risk of increasing pore defects. Therefore, the F content relative to the total mass of the wire is set to 0.30% by mass or less, preferably 0.25% by mass or less, and more preferably 0.20% by mass or less. The lower limit of the F content relative to the total mass of the wire is not particularly limited, and may be 0 mass %, but may be 0.001 mass % or more.

[0033] <θ calculated by formula (I): 10.0 or more and 30.0 or less> In this embodiment, by appropriately controlling the content of each of the above elements and controlling θ calculated by the following formula (I) based on the amount of each alloy element contained in the wire, it is possible to maintain a predetermined ferrite amount in the weld metal and obtain desired strength and toughness. If θ calculated by formula (I) is less than 10.0, the amount of ferrite will be insufficient and the strength of the weld metal will be insufficient. Therefore, θ is set to 10.0 or more, preferably 12.0 or more, and more preferably 24.0 or more. On the other hand, if θ calculated by formula (I) exceeds 30.0, the amount of ferrite becomes excessive, the low-temperature toughness decreases, and the desired Charpy impact value cannot be obtained. Therefore, θ is set to 30.0 or less, and preferably 29.0 or less.

[0034] θ=4.1×α-3.2×γ-32.3 (I) However, when the Si content with respect to the total mass of the wire is defined as [Si] in mass%, the Cr content with respect to the total mass of the wire is defined as [Cr] in mass%, the Mo content with respect to the total mass of the wire is defined as [Mo] in mass%, the Ti content with respect to the total mass of the wire is defined as [Ti] in mass%, the C content with respect to the total mass of the wire is defined as [C] in mass%, the N content with respect to the total mass of the wire is defined as [N] in mass%, the Mn content with respect to the total mass of the wire is defined as [Mn] in mass%, the Cu content with respect to the total mass of the wire is defined as [Cu] in mass%, and the Ni content with respect to the total mass of the wire is defined as [Ni] in mass%, α=0.02×[Si]+[Cr]+1.20×[Mo]+0.3×[Ti]+0.30 Let γ = 24×[C] + 28×[N] + 0.25×[Mn] + 0.5×[Cu] + 1.10×[Ni].

[0035] <Bi: 0.001 mass% or more and 0.10 mass% or less> The wire according to this embodiment may further contain Bi. Bi is a component having the effect of improving slag detachability. However, if it is contained in the wire in excess, Bi segregates in the final solidification region of the weld metal, and the high-temperature crack resistance of the weld metal deteriorates. When Bi is contained in the wire, if the Bi content with respect to the total mass of the wire is 0.001 mass% or more, the effect of improving slag detachability can be obtained. Therefore, the Bi content with respect to the total mass of the wire is preferably 0.001 mass% or more, and more preferably 0.01 mass% or more. On the other hand, if the Bi content with respect to the total mass of the wire is 0.10 mass% or less, deterioration of the high-temperature crack resistance of the weld metal can be suppressed. Therefore, the Bi content with respect to the total mass of the wire is preferably 0.10 mass% or less, and more preferably 0.08 mass% or less. In this embodiment, the Bi content means the total amount of Bi contained in Bi alone, Bi alloys, and Bi compounds.

[0036] <Remainder> The wire according to this embodiment contains inevitable impurities in the range of 2.0% or less as the remainder of the components other than the above. Further, Co, V, W, etc. may be contained in the remainder of the wire in the range of 1.0% or less respectively.

[0037] The wire according to this embodiment preferably contains Fe, Cr, Ni, Si, Mn, Na and K, TiO2, ZrO2, Al2O3, C, Ti, Mo, Cu, Al, N, F in total by 90 mass% or more, more preferably 93 mass% or more, still more preferably 95 mass% or more, and particularly preferably 98 mass% or more.

Examples

[0038] The effects of the present invention will be specifically described below with reference to examples of the present invention and comparative examples, but the present invention is not limited thereto.

[0039] The chemical components of the wire were adjusted to various contents, and flux-cored wires for gas shielded arc welding with a diameter of 1.20 mm were fabricated.

[0040] <Evaluation of mechanical properties> Using the prepared flux-cored wire, gas-shielded arc welding was performed under the welding conditions for the evaluation test of mechanical properties shown in Table 1 below. In this example, a test plate with the symbol 1.3 specified in JIS Z3111 was used, and two layers of buttering were applied to the groove surface using the wire to be used, and then gas-shielded arc welding was performed to prepare a weld metal test piece. The mechanical properties of the weld metal were evaluated in accordance with "Tensile and impact test method for weld metal" specified in JIS Z 3111:2005, and an A0 tensile test piece was taken from the weld metal test piece to evaluate the tensile strength by a tensile test, and a V-notch test piece was taken to evaluate the low-temperature toughness by a Charpy impact test at -196°C. The evaluation criteria for mechanical properties were as follows: ◯ (good) for a tensile strength of 640 MPa or more and a Charpy impact value of 25 J or more at -196°C, and among these, ⊚ (excellent) for a tensile strength of 670 MPa or more. Also, × (poor) for a tensile strength less than 640 MPa or a Charpy impact value less than 25 J at -196°C.

[0041] [Welding workability evaluation] Furthermore, in order to evaluate the welding workability, gas-shielded arc welding was performed using the above flux-cored wire under the welding conditions for the evaluation test of the welding workability shown in the following Table 1. In this example, two types of welding positions were used: horizontal fillet welding and vertical upward fillet welding.

[0042] <Bead shape evaluation> The bead shape was evaluated in accordance with AWS A5.22 15.2.2. The bead shape was evaluated as follows: those that met the AWS standard criteria were rated as ◯ (good), and those that did not meet the criteria and had a convex bead shape were rated as × (bad).

[0043] <Evaluation of slag removability> The welded joint was given a slight impact with a hammer, and the slag removability was evaluated by checking whether the slag had peeled off. The evaluation criteria for slag removability were as follows: ◯ (good) if the slag peeled off naturally or if it peeled off due to a slight impact, and × (bad) if the slag was burned onto the surface of the bead and did not peel off.

[0044] The component compositions of the produced wires and calculated values ​​based on specific components are shown in Tables 2 and 3 below, and the evaluation results are shown in Table 4 below. In Table 2, "Na+K" represents the total amount of Na and K in the wire. In addition, in the column of "Calculated value based on specific components" in Table 3, α=0.02×[Si]+[Cr]+1.20×[Mo]+0.3×[Ti]+0.30 γ=24×[C]+28×[N]+0.25×[Mn]+0.5×[Cu]+1.10×[Ni], and θ is a value calculated by the following formula (I). θ=4.1×α-3.2×γ-32.3 (I) In the above formula, [Si] is the Si content expressed as mass% relative to the total mass of the wire, [Cr] is the Cr content expressed as mass% relative to the total mass of the wire, [Mo] is the Mo content expressed as mass% relative to the total mass of the wire, [Ti] is the Ti content expressed as mass% relative to the total mass of the wire, [C] is the C content expressed as mass% relative to the total mass of the wire, [N] is the N content expressed as mass% relative to the total mass of the wire, [Mn] is the Mn content expressed as mass% relative to the total mass of the wire, [Cu] is the Cu content expressed as mass% relative to the total mass of the wire, and [Ni] is the Ni content expressed as mass% relative to the total mass of the wire.

[0045] [Table 1]

[0046] [Table 2]

[0047] [Table 3]

[0048] [Table 4]

[0049] As shown in Tables 2 to 4 above, Wires Nos. 1 to 11, which are examples of the invention, had excellent mechanical properties and welding workability because the wire components and θ obtained from formula (1) were within the range of the present invention.

[0050] On the other hand, in Wire No. 12, which is a comparative example, the contents of each component were within the range of the present invention, but since θ calculated by formula (I) exceeded the upper limit of the range of the present invention, the low temperature toughness was reduced.

[0051] In the comparative example, Wire No. 13, the Cr, Ni and C contents in the wire exceeded the upper limits of the ranges of the present invention, and θ also exceeded the upper limits of the ranges of the present invention, so that the low temperature toughness was significantly reduced.

[0052] In the comparative examples, wire Nos. 14 to 16, the Al2O3 content in the wire was below the lower limit of the range of the present invention, and therefore the bead shape and slag removability in vertical upward fillet welding were poor, and the slag removability in horizontal fillet welding was also poor. Wire No. 16 also had reduced low temperature toughness.

[0053] In the comparative wires No. 17 to 20, the Al content in the wire exceeded the upper limit of the range of the present invention, so that the bead shape and slag removability in vertical upward fillet welding were poor, and the slag removability in horizontal fillet welding was also poor. In addition, these wires also had reduced low temperature toughness.

[0054] Wire No. 21, which is a comparative example, had a Mo content exceeding the upper limit of the range of the present invention, and therefore had a reduced low-temperature toughness.

[0055] Fig. 1 is a graph showing the relationship between the tensile strength and θ of wires of the invention examples and comparative examples, with the tensile strength (MPa) on the vertical axis and θ on the horizontal axis. Note that the dashed line shown in Fig. 1 is an approximation line obtained by linearly approximating each point. As shown in FIG. 1, it was shown that the tensile strength decreased as the value of θ calculated by the formula (I) decreased.

[0056] As described above in detail, the flux-cored wire for gas-shielded arc welding according to the present embodiment provides a weld metal with good bead shape and slag removability, and an excellent balance between tensile strength and low-temperature toughness.

Claims

1. A flux-cored wire for gas shielded arc welding, the wire having an outer sheath filled with flux, For the total mass of wire, Fe: 40% by mass or more and 70% by mass or less, Cr: 15.0% by mass or more and 25.0% by mass or less, Ni: 5.0% by mass or more and 11.0% by mass or less, Si: 0.5% by mass or more and 3.0% by mass or less, Mn: 0.5% by mass or more and 5.0% by mass or less, Total amount of Na and K: 0.05% by mass or more and 1.0% by mass or less, TiO 2 : 3.0% by mass or more and 9.0% by mass or less, ZrO 2 : more than 1.0% by mass and not more than 4.0% by mass, A 2 O 3 : Contains 0.3% by mass or more and 2.0% by mass or less, C: less than 0.015% by mass, Ti: 1.0% by mass or less, Mo: 2.0% by mass or less, Cu: 0.5% by mass or less, Al: 0.9% by mass or less, N: 0.040% by mass or less, F: 0.30% by mass or less, A flux-cored wire, characterized in that θ calculated by the following formula (I) is 10.0 or more and 30.0 or less. θ=4.1×α-3.2×γ-32.3...(I) However, when the Si content with respect to the total mass of the wire is [Si] in mass%, the Cr content with respect to the total mass of the wire is [Cr] in mass%, the Mo content with respect to the total mass of the wire is [Mo] in mass%, the Ti content with respect to the total mass of the wire is [Ti] in mass%, the C content with respect to the total mass of the wire is [C] in mass%, the N content with respect to the total mass of the wire is [N] in mass%, the Mn content with respect to the total mass of the wire is [Mn] in mass%, the Cu content with respect to the total mass of the wire is [Cu] in mass%, and the Ni content with respect to the total mass of the wire is [Ni] in mass%, α=0.02×[Si]+[Cr]+1.20×[Mo]+0.3×[Ti]+0.30 Let γ=24×[C]+28×[N]+0.25×[Mn]+0.5×[Cu]+1.10×[Ni].

2. moreover, For the total mass of wire, The flux-cored wire according to claim 1, further comprising: Bi: 0.001 mass % or more and 0.10 mass % or less.