Resin film formation film, sheet for resin film formation, and method for manufacturing workpiece individualized piece with resin film

The resin film-forming film with epoxy resin, thiol group, and photobase generator addresses oxygen inhibition during curing, ensuring complete polymerization and reduced tackiness, enhancing semiconductor wafer processing.

JP2024160590APending Publication Date: 2024-11-14LINTEC CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023075752
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-01
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The existing resin film-forming films used in semiconductor manufacturing are inhibited by oxygen during curing with energy rays, leading to incomplete polymerization and excessive tackiness on the surface, causing transportation defects.

Method used

A resin film-forming film containing an epoxy resin, a compound with a thiol group, and a photobase generator, which minimizes polymerization inhibition by oxygen, ensuring complete curing and reduced tackiness.

Benefits of technology

The solution allows for effective curing of the resin film without oxygen inhibition, reducing surface tackiness and preventing transportation defects, ensuring smooth processing of semiconductor wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160590000001_ABST
    Figure 2024160590000001_ABST
Patent Text Reader

Abstract

To provide a resin film formation film which prevents polymerization inhibition by oxygen, a sheet for resin film formation having the same, and a method for manufacturing a workpiece individualized piece with a resin film.SOLUTION: A resin film formation film is formed into a resin film after curing, where the resin film formation film contains an epoxy resin, a compound having a thiol group, and a photobase generator.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin film-forming film, a sheet for forming a resin film, and a method for manufacturing a workpiece with a resin film. In particular, the present invention relates to a resin film-forming film that is suitably used for protecting a workpiece such as a semiconductor wafer or a workpiece such as a semiconductor chip obtained by processing the workpiece, a sheet for forming a resin film that includes the resin film-forming film, and a method for manufacturing a workpiece such as a semiconductor chip with a resin film formed thereon. [Background technology]

[0002] In recent years, semiconductor devices have been manufactured using a mounting method called flip-chip bonding. In this mounting method, when mounting a semiconductor chip having a circuit surface on which convex electrodes such as bumps are formed, the semiconductor chip is inverted (face down) so that the circuit surface of the semiconductor chip faces the chip mounting surface of the substrate, and the circuit surface of the semiconductor chip and the chip mounting surface of the substrate are wirelessly bonded. Therefore, the surface of the semiconductor chip opposite to the circuit surface (the surface on which no circuit is formed; hereinafter, also referred to as the back surface) is exposed to the outside.

[0003] If the back surface of the semiconductor chip is exposed to the outside, there is a risk of chipping such as cracks or chips occurring in the subsequent process due to impacts during transportation, etc. Therefore, in order to protect the semiconductor chip from such chipping, a hard resin film made of an organic material is often formed on the back surface of the semiconductor chip.

[0004] In addition, the semiconductor chip may be attached to the circuit-forming surface of the substrate by a resin film attached to the back surface of the semiconductor chip. The resin film-forming film for forming and adhering such a resin film is called a die bonding film. The semiconductor chip is placed on the substrate via the die bonding film by die bonding. Then, if necessary, one or more other semiconductor chips are stacked on the semiconductor chip, wire bonding is performed, and the whole is sealed with resin to produce a semiconductor package.

[0005] Such a resin film is formed by curing its precursor, an uncured resin film (hereinafter also referred to as a resin film-forming film). The resin film-forming film is attached to the back surface of a semiconductor wafer, and before or after the resin film-forming film is cured, the semiconductor wafer and the resin film-forming film or the resin film are diced and divided into a plurality of small pieces (individualized), and the resin film-forming film is then cured to form a resin film. The divided small pieces are semiconductor chips having a resin film on the back surface (semiconductor chips with a resin film).

[0006] The resin film-forming film is generally cured by heating, but may also be cured by irradiation with energy rays such as ultraviolet rays. Patent Document 1 discloses an energy ray-curable chip protection film that contains an energy ray-curable component and a photopolymerization initiator. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2009-138026 A Summary of the Invention [Problem to be solved by the invention]

[0008] In Patent Document 1, irradiation with energy rays generates radicals from a photopolymerization initiator, and these radicals polymerize and cure an energy ray-curable component such as an acrylate monomer (radical polymerization).

[0009] However, when the resin film-forming film is irradiated with energy rays while the resin film-forming film is exposed to air, polymerization inhibition due to oxygen occurs on the surface of the resin film-forming film exposed to air, and there is a problem that the surface of the resin film-forming film does not harden sufficiently.

[0010] When the curing is insufficient, the tackiness of the resin film-formed film after curing, i.e., the surface of the resin film, is not reduced to the intended level and remains. Specifically, the tackiness cannot be reduced to the same level as that when the resin film-formed film is irradiated with energy rays without being exposed to air, and remains. As a result, when the wafer on which the resin film is formed is transported to the next process, even if the transport device or transport part is brought into contact with the resin film and then separated, the resin film remains stuck and cannot be separated, which causes a transport failure.

[0011] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a resin film-forming film that does not cause polymerization inhibition due to oxygen, a resin film-forming sheet comprising the same, and a method for producing individual workpieces with a resin film. [Means for solving the problem]

[0012] The aspects of the present invention are as follows.

[0013] [1] A resin film-forming film that becomes a resin film after curing, the resin film-forming film containing an epoxy resin, a compound having a thiol group, and a photobase generator.

[0014] [2] The resin film has two main surfaces, surface A and surface B, The resin film-formed film according to [1], wherein when the probe tack value T2 of the A side after irradiation with energy rays in a state where the A side is in contact with oxygen is 0.01 N or less.

[0015] [3] The resin film has two main surfaces, surface A and surface B, The resin film-formed film according to [1] or [2] has a probe tack value variable X of 99.0% or more, where T1 is the probe tack value of side B before energy ray irradiation and T2 is the probe tack value of side A after energy ray irradiation in a state where side A is in contact with oxygen. Probe tack value variable X(%)=100×(T1-T2) / T1

[0016] [4] The resin film-forming film according to any one of [1] to [3], wherein the photobase generator is a non-ionic type.

[0017] [5] A sheet for resin film formation, comprising a resin film-forming film described in any one of [1] to [4] and a release film releasably arranged on at least one of the main surfaces, side A and side B, of the resin film-forming film.

[0018] [6] A process of attaching a resin film forming film according to any one of [1] to [4] or a resin film forming film provided on a sheet for resin film formation according to [5] to the back surface of a workpiece; A step of hardening the applied resin film forming film to form a resin film on the back surface of the workpiece to obtain a workpiece with a resin film; The method for producing individual workpieces with a resin film includes a step of singulating the workpiece with a resin film to obtain a plurality of individual workpieces with a resin film.

[0019] [7] A method for producing a resin-film-coated workpiece singulated as described in [6], in which the resin-film-forming film is hardened by irradiation with energy rays. Effect of the Invention

[0020] According to the present invention, it is possible to provide a resin film-forming film that does not cause polymerization inhibition due to oxygen, a sheet for resin film formation that includes the same, and a method for producing individual workpieces with a resin film. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a schematic cross-sectional view of an example of the sheet for resin film formation according to this embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view of an example of a work (wafer) having a resin film-forming film according to the present embodiment attached to the back surface thereof. [Diagram 3]FIG. 3 is a schematic diagram for explaining irradiation of an energy beam to a main surface (side A) of a workpiece (wafer) having a resin film-forming film according to this embodiment attached to its back surface. [Figure 4] FIG. 4 is a schematic cross-sectional view of an example of a resin film-attached workpiece (wafer) in which a resin film obtained by curing the resin film-forming film according to this embodiment is formed on the rear surface of the workpiece (wafer). [Diagram 5] FIG. 5 is a schematic cross-sectional view for illustrating how a resin-film-coated workpiece (wafer) is diced to obtain an aggregate of resin-film-coated workpiece individual pieces (chips). [Figure 6] FIG. 6 is a schematic cross-sectional view of an example of the composite sheet for resin film formation according to this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings based on specific embodiments. First, the main terms used in this specification will be explained.

[0023] The work refers to a plate-shaped body to which the resin film forming film provided in the resin film forming sheet according to this embodiment is attached and then divided into individual pieces. The resin film forming film is attached to the back surface of the work. Examples of the work include a circular wafer (including a case having an orientation flat), a rectangular panel level package, and a strip (rectangular substrate) with molded resin sealing, among which a wafer is preferred from the viewpoint of easily obtaining the effects of the present invention. The wafer may be, for example, a semiconductor wafer such as a silicon wafer, a gallium arsenide wafer, a silicon carbide wafer, a gallium nitride wafer, or an indium phosphide wafer, or an insulator wafer such as a glass wafer, a lithium tantalate wafer, or a lithium niobate wafer, or may be a reconstructed wafer made of a resin and a semiconductor used in the manufacture of a fan-out package or the like. From the viewpoint of easily obtaining the effects of the present invention, a semiconductor wafer or an insulator wafer is preferred, and a semiconductor wafer is more preferred.

[0024] Singulation of a work refers to dividing the work into individual circuits to obtain individual work pieces. For example, if the work is a wafer, the individual work pieces are chips, and if the work is a panel level package or a strip (rectangular substrate) sealed with molded resin, the individual work pieces are semiconductor packages.

[0025] The "front surface" of a workpiece refers to the surface on which circuits, electrodes, etc. are formed, and the "back surface" of a workpiece refers to the surface on which no circuits, etc. are formed. The electrodes may be convex electrodes such as bumps.

[0026] The term "principal surface" refers to a surface that is larger in area than the other surfaces among the surfaces that constitute a plate-like body. Usually, a plate-like body has two principal surfaces and other side surfaces, and the two principal surfaces face each other. In the case of a workpiece, the "front surface" and the "rear surface" are the principal surfaces.

[0027] "(Meth)acrylate" is used as the term to refer to both "acrylate" and "methacrylate," and similar terms.

[0028] The term "energy rays" refers to ultraviolet rays, electron beams, etc., and is preferably ultraviolet rays.

[0029] Unless otherwise specified, "weight average molecular weight" is a polystyrene equivalent value measured by gel permeation chromatography (GPC). Measurements using this method are performed, for example, using a high-speed GPC device "HLC-8120GPC" manufactured by Tosoh Corporation, connected in this order to high-speed columns "TSK guard column HXL-H", "TSK Gel GMHXL", and "TSK Gel G2000 HXL" (all manufactured by Tosoh Corporation), under the following conditions: column temperature: 40°C, flow rate: 1.0 mL / min, and a differential refractometer as the detector.

[0030] The release film is a film that supports the resin film-forming film in a peelable manner. The term "film" is not limited to a specific thickness, and is used to include a sheet.

[0031] The mass ratios in the explanations of compositions such as the composition for resin film-forming films are based on the active ingredients (solid content), and do not include the solvent unless otherwise specified.

[0032] (1. Resin film forming sheet) The resin film forming sheet 1 according to this embodiment has a configuration shown in Fig. 1. The resin film forming film 10 has two opposing main surfaces. In this embodiment, the main surface 10a is surface A, and the main surface 10b is surface B. A first release film 21 supporting the resin film forming film 10 is disposed on surface A 10a, and a second release film 22 supporting the resin film forming film 10 is disposed on surface B 10b. As will be described later, in this embodiment, surface A is the main surface to be irradiated with energy rays, and surface B is the main surface to be attached to a workpiece.

[0033] The resin film forming sheet may be in the form of a long sheet having a length in the longitudinal direction that is very long relative to the length in the lateral direction. Also, the resin film forming sheet may be in the form of a sheet roll in which such a long sheet is wound up.

[0034] Furthermore, the resin film forming sheet may be a resin film forming sheet that is punched so that the resin film forming film to be attached to the workpiece has a predetermined closed shape. The predetermined closed shape is not particularly limited, but it is preferably approximately the same shape as the workpiece to be attached.

[0035] The resin film forming sheet according to this embodiment is used to attach a resin film forming film to the back surface of a work before the work is divided into individual pieces, and harden the resin film forming film to form a resin film on the back surface of the work. The work on which the resin film is formed (the work with the resin film) is divided into individual pieces by a known means (for example, blade dicing, stealth dicing (registered trademark), etc.), and a chip with the resin film is obtained as the divided work.

[0036] (2. Resin film forming film) The resin film-forming film according to the present embodiment is attached to a workpiece to form a resin film. Examples of the resin film include a protective film for protecting the workpiece or the individual pieces of the workpiece, and an adhesive film for adhering the individual pieces of the workpiece to a substrate or the like. The resin film-forming film is formed, for example, on a release film using a coating agent containing a composition for the resin film-forming film described later.

[0037] It is preferable that the resin film-forming film has adhesiveness at room temperature (23°C) or exhibits adhesiveness when heated. This allows the workpiece to be laminated to the resin film-forming film when it is overlaid on the film. Therefore, positioning can be performed reliably before the resin film-forming film is cured.

[0038] The resin film-formed film may be composed of one layer (single layer) or may be composed of two or more layers. When the resin film-formed film has multiple layers, these multiple layers may be the same or different from each other, and the combination of layers constituting these multiple layers is not particularly limited.

[0039] In this embodiment, the resin film-forming film is preferably one layer (single layer). A one-layer resin film-forming film can be easily produced because it can have high precision in thickness. In addition, if the resin film-forming film is composed of multiple layers, it is necessary to consider the adhesion between the layers and the elasticity of each layer, which may cause a risk of peeling from the adherend. If the resin film-forming film is one layer, the above risks can be reduced and the design freedom is increased. In addition, the risk of peeling between layers due to differences in thermal elasticity between layers in processes where temperature changes occur (during reflow processing or when using the device) can also be reduced.

[0040] In this embodiment, the resin film is obtained by curing the resin film-forming film according to this embodiment. That is, the resin film-forming film according to this embodiment is curable. After the workpiece is superimposed on the curable resin film-forming film, the resin film can be firmly bonded to the workpiece by curing the resin film-forming film, and a durable resin film can be formed.

[0041] The resin film is a cured product of the resin film-forming film, and is different from the resin film-forming film. Examples of the cured product include a heat-cured product and an energy ray-cured product. In this embodiment, the resin film is preferably at least an energy ray-cured product. That is, the resin film-forming film according to this embodiment is preferably at least energy ray-curable. Therefore, the resin film-forming film according to this embodiment may be heat-curable in addition to being energy ray-curable.

[0042] When the resin film-forming film is energy ray curable, it is common to use radical polymerization to cure the resin film-forming film. However, it is known that in an environment where oxygen is present, for example, in air, radical polymerization is inhibited by oxygen, resulting in insufficient polymerization. This is prominent on the surface (for example, the main surface) of the resin film-forming film that is in contact with air, and as a result, the surface becomes sticky and an unintended degree of tack remains. The surface with an unintended degree of tack remains is, for example, prone to sticking to other members, etc., and difficult to separate from other members, etc.

[0043] Therefore, when the resin film-forming film is a protective film-forming film, when transporting a workpiece on which a protective film has been formed by energy ray irradiation to the next process, for example, when a transport device is used that transports the workpiece with the protective film by adsorbing the surface of the protective film to a component member, even when an operation is performed to detach the component member from the surface, the surface of the protective film does not separate from the component member, which may result in poor transport.

[0044] Therefore, in the present embodiment, the resin film-forming film has a composition that does not cause polymerization inhibition due to oxygen, and this further suppresses poor transport caused by tack remaining after energy ray irradiation.

[0045] The resin film-formed film according to this embodiment preferably has the following physical properties regarding tack before and after energy ray irradiation.

[0046] In this embodiment, the probe tack of the main surface of the resin film-formed film after irradiating the main surface with an energy ray while the main surface is in contact with oxygen is defined as T2. That is, T2 is the probe tack value of the A surface (the A surface of the resin film) after irradiation of the energy ray on the A surface of the resin film-formed film in contact with oxygen. T2 is preferably 0.01 N or less, and more preferably 0.00 N.

[0047] By setting T2 within the above range, the resin film-formed film (resin film) after the energy ray irradiation can be easily separated from the conveying device, etc., even if the conveying device, etc., contacts the A side of the resin film when being conveyed to the next process. As a result, the occurrence of defects during conveying can be further suppressed.

[0048] In addition, the probe tack of surface B before the energy beam irradiation is set to T1. That is, the probe tack value of surface B, which is the main surface opposite surface A, before the energy beam irradiation is set to T1. Since the resin film-forming film can be easily attached to the back surface of the workpiece, T1 is preferably 0.10 N or more, more preferably 0.5 N or more, even more preferably 1 N or more, and particularly preferably 2 N or more.

[0049] In this embodiment, as shown below, the variable X of the probe tack value expressed using T1 and T2 is preferably 90% or more, more preferably 99.0% or more, even more preferably 99.5% or more, and particularly preferably 100.0%. Probe tack value variable X(%)=100×(T1-T2) / T1

[0050] By the probe tack value variable X, which indicates the relationship between the probe tack before and after the energy ray irradiation, being within the above range, the B side of the resin film-formed film can be more easily attached to the back side of the workpiece, and even if the A side of the resin film is contacted with a conveying device or the like when the resin film-formed film (resin film) after the energy ray irradiation is conveyed to the next process, it can be more easily separated from the conveying device or the like. As a result, the occurrence of defects during conveyance can be further suppressed.

[0051] In addition, the probe tack of the A-side of the resin film-formed film after energy ray irradiation in a state where the A-side of the resin film-formed film is not in contact with oxygen is defined as T3. In other words, T3 is the probe tack value of the A-side (A-side of the resin film) after irradiation of the A-side of the resin film-formed film that is not in contact with oxygen with energy ray.

[0052] In this embodiment, the difference (T2-T3) between the probe tack (T2) and the probe tack (T3), which corresponds to the degree of unintended tack, is preferably 0.01 N or less, and more preferably 0.00 N.

[0053] The state where the A-side of the resin film-formed film is in contact with oxygen means that the A-side is exposed to oxygen or a gas containing oxygen. Specifically, it means that the A-side is exposed to air. The state where the A-side of the resin film-formed film is not in contact with oxygen means that the A-side is not exposed to oxygen or a gas containing oxygen. For example, it means that the A-side is exposed to nitrogen gas. The method for measuring the probe tack will be described in detail in the examples.

[0054] The thickness of the resin film-formed film is not particularly limited, but is preferably 100 μm or less, 80 μm or less, 60 μm or less, or 45 μm or less. The thickness of the resin film-formed film is preferably 5 μm or more, 10 μm or more, or 13 μm or more. The thickness of the resin film-formed film can be arbitrarily selected and set from the above upper and lower limit values. When the thickness of the resin film-formed film is within the above range, the performance of the obtained resin film becomes better.

[0055] The thickness of the resin film-formed film means the thickness of the entire resin film-formed film. For example, the thickness of a resin film-formed film composed of multiple layers means the total thickness of all layers constituting the resin film-formed film.

[0056] (2.1. Composition for resin film-forming film) In this embodiment, the resin film-forming film is formed using a composition constituting the resin film-forming film (composition for resin film-forming film). The composition for resin film-forming film is a resin composition containing at least an epoxy resin as a curable component (B), a compound (C) having a thiol group, and a photobase generator (D).

[0057] (2.2. Curing component) The curable component (B) cures the resin film-forming film to form a resin film as a cured product. As described above, since the resin film is preferably an energy ray cured product, the curable component may be a component containing at least an energy ray curable component.

[0058] In this embodiment, the curable component (B) is an epoxy resin. The epoxy resin may be any epoxy resin that is cured by a compound having a thiol group, which will be described later. Specifically, examples of the epoxy resin include glycidyl ethers of phenols such as bisphenol A, bisphenol F, resorcinol, phenyl novolac, and cresol novolac; glycidyl ethers of alcohols such as butanediol, polyethylene glycol, and polypropylene glycol; glycidyl ethers of carboxylic acids such as phthalic acid, isophthalic acid, and tetrahydrophthalic acid; glycidyl-type or alkylglycidyl-type epoxy resins in which active hydrogen bonded to nitrogen atoms such as aniline isocyanurate is replaced with a glycidyl group; and so-called alicyclic epoxides in which epoxy is introduced by, for example, oxidizing carbon-carbon double bonds in the molecule, such as vinylcyclohexane diepoxide, 3,4-epoxycyclohexylmethyl-3,4-dicyclohexanecarboxylate, and 2-(3,4-epoxy)cyclohexyl-5,5-spiro(3,4-epoxy)cyclohexane-m-dioxane. In addition, epoxy resins having a biphenyl skeleton, a dicyclohexadiene skeleton, a naphthalene skeleton, or the like can also be used.

[0059] The molecular weight (formula weight) of the epoxy resin is preferably 300 or more and less than 50,000, 300 or more and less than 10,000, 300 or more and less than 5,000, or 300 or more and less than 3,000. The epoxy equivalent of the epoxy resin is preferably 50 to 5,000 g / eq, more preferably 100 to 2,000 g / eq, and even more preferably 150 to 1,000 g / eq.

[0060] The content of the curable component (B) when the total weight of the composition for resin film-forming film (solid content equivalent) is 100 parts by mass is preferably 3 to 50 parts by mass, 6 to 35 parts by mass, or 8 to 20 parts by mass. By blending the curable components in the above ratios, it is easy to increase the variable X of the probe tack value, it is easy to make the probe tack (T2) of the resin film-forming film (resin film) after curing smaller, and it is easy to make T2-T3 smaller.

[0061] (2.3. Compounds having a thiol group) In this embodiment, a compound (C) having a thiol group (-SH) is used as an auxiliary (curing agent) for curing the epoxy resin as the curable component (B).

[0062] A compound having a thiol group is activated by the action of a base, by abstracting hydrogen therefrom (i.e., by deprotonation). By deprotonation, the curing reaction with the epoxy resin, which is the curable component, proceeds sufficiently.

[0063] Examples of the compound having a thiol group include compounds represented by the following structural formulas 1 to 3.

[0064] [ka] In structural formula 1, X 1 , X 2 , X 3 and X 4 each independently represents a monovalent group having a thiol group or a hydrogen atom; X 1 , X 2 , X 3 and X 4 At least two of the groups are monovalent groups having a thiol group.

[0065] [ka] In structural formula 2, X 5 , X 6 and X 7 each independently represents a monovalent group having a thiol group or a hydrogen atom; X 5 , X 6 and X 7 At least two of the groups are monovalent groups having a thiol group.

[0066] [ka] In structural formula 3, X 8 and X 9 each independently represents a monovalent group having a thiol group, R1 R represents an alkylene group. 1 may be an alkylene group having 2 to 10 carbon atoms.

[0067] In this embodiment, the compound having a thiol group is more preferably a compound having two or more thiol groups, even more preferably a compound having three or more thiol groups, and particularly preferably a compound having four or more thiol groups.

[0068] Furthermore, the thiol group may be any of a primary thiol group, a secondary thiol group, and a tertiary thiol group, but in this embodiment, a primary thiol group or a secondary thiol group is preferable, and a secondary thiol group is more preferable.

[0069] In structural formulas 1 to 3, when the group having a thiol group is a secondary thiol group, it may be a group represented by formula 4, and when the group having a thiol group is a primary thiol group, it may be a group represented by formula 5 or 6.

[0070] [ka] In formula 4, R 2 represents an alkylene group. 3 represents an alkylene group. 4 R represents an alkylene group. 2 R may be an alkylene group having 1 to 8 carbon atoms. 3 and R 4 may be an alkylene group having 2 to 10 carbon atoms.

[0071] Examples of compounds having two or more thiol groups and containing a primary thiol group include pentaerythritol trippropanethiol, 1,2-ethanedithiol, 1,3-propanedithiol, 1,4-butanedithiol, 2,3-butanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,8-octanedithiol, 1,10-decanedithiol, 1,3-benzenedithiol, 1,4-benzenedithiol, 4,4'-thiobisbenzenethiol, 4,4'-biphenyldithiol, 1,5-dimercaptonaphthalene, 4,5 -Bis(mercaptomethyl)-ortho-xylene, 1,3,5-benzenetrithiol, 1,4-butanediol bis(thioglycolate), dithioethythritol, 3,6-dioxa-1,8-octanedithiol, 3,7-dithia-1,9-nonanedithiol, bis(2-mercaptoethyl)sulfide, ethylene glycol bis(mercaptoacetate), ethylene glycol bis(3-mercaptopropionate), ethylene glycol bis(3-mercaptoisobutyrate), butanediol bis(mercaptoacetate), butane Diol bis(3-mercaptopropionate), butanediol bis(3-mercaptoisobutyrate), pentaerythritol tri(mercaptoacetate), pentaerythritol tri(3-mercaptopropionate), pentaerythritol tri(3-mercaptoisobutyrate), pentaerythritol tetrakis(mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptoisobutyrate), trimethylolethane(mercaptoacetate) ester), trimethylolethane (3-mercaptopropionate), trimethylolethane (3-mercaptoisobutyrate), trimethylolpropane tris(mercaptoacetate), trimethylolpropane tris(3-mercaptopropionate), trimethylolpropane tris(3-mercaptoisobutyrate), dipentaerythritol hexakis(mercaptoacetate), dipentaerythritol hexakis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptoisobutyrate), 1,Examples of the esters include 4-bis(3-mercaptopropyloxy)butane, tris[(3-mercaptopropionyloxy)ethyl]isocyanurate, and tetraethylene glycol bis(3-mercaptopropionate).

[0072] Examples of the compound having two or more thiol groups and containing a secondary thiol group include pentaerythritol tetrakis(3-mercaptobutyrate) shown in the following structural formula 7, 1,3,5-tris(2-(3-mercaptobutyryloxy)ethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione shown in the following structural formula 8, 1,4-bis(3-mercaptobutyryloxy)butane shown in the following structural formula 9, and ethylene glycol. Examples of suitable mercaptobutyrates include butanediol bis(3-mercaptobutyrate), pentaerythritol tri(3-mercaptobutyrate), trimethylolethane (3-mercaptobutyrate), trimethylolpropane tris(3-mercaptobutyrate), and dipentaerythritol hexakis(3-mercaptobutyrate).

[0073] Among these, as the compound having a thiol group, pentaerythritol tetrakis(3-mercaptobutyrate) is preferred since it has better curing reactivity and the storage stability of the resin film-forming film is relatively excellent.

[0074] [ka]

[0075] [ka]

[0076] [ka]

[0077] The content of the compound (C) having a thiol group when the total weight of the composition for resin film-forming film (solid content equivalent) is 100 parts by mass is preferably 1 to 20 parts by mass, 2.5 to 15 parts by mass, 4 to 12 parts by mass, or 5 to 10 parts by mass. By setting the content of the compound (C) having a thiol group within the above range, it is easy to increase the variable X of the probe tack value, it is easy to make the probe tack (T2) of the resin film-forming film (resin film) after curing smaller, and it is easy to make T2-T3 smaller.

[0078] (2.4. Photobase Generator) In this embodiment, the composition for resin film-forming film contains a photobase generator (D) as a catalyst for controlling the deprotonation of the compound (C) having a thiol group. The photobase generator is also called a photoanionic polymerization initiator (photo base generator), and is a compound that generates a base by irradiation with energy rays. The generated base abstracts hydrogen from the compound (C) having the above-mentioned thiol group, and the deprotonation of the compound having the thiol group progresses. Since the generation of the base can be controlled by irradiation with energy rays, the compound (C) having the above-mentioned thiol group can be used as a latent curing agent with excellent storage stability. In addition, when radical polymerization is used to form the resin film, the photobase generator may generate radicals in addition to a base.

[0079] The photobase generator may be a photobase generator having an ionic bond in its molecular structure (ionic photobase generator), or may be a photobase generator not having an ionic bond in its molecular structure (nonionic photobase generator). In this embodiment, from the viewpoint of storage stability of the resin film-forming film containing the photobase generator, a nonionic photobase generator is preferred.

[0080] Examples of ionic photobase generators include compounds containing carboxylates, salts containing borate anions, quaternary ammonium salts, carbamates, etc. in their molecular structure. Examples of such compounds include (8E)-8-ethylidene-4-methoxy-5,6,7,8-tetrahydronaphthalene-1-carboxylic acid 1,8-diazabicyclo[5,4,0]undec-7-ene, 1,2-diisopropyl-3-[bis(dimethylamino)methylene]guanidium 2-(3-benzoylphenyl)propionate, 1,2-dicyclohexyl-4,4,5,5-tetramethyldiguanidine n-butyltriphenylborate, and 2-(9-oxoxanthen-2-yl)propionic acid 1,5,7-triazabicyclo[4,4,0]dec-5-ene.

[0081] Examples of the non-ionic photobase generator include a photobase generator represented by the following general formula (α1).

[0082] [ka] In the formula (α1), n ​​represents an integer of 0 to 4. 11 Rα represents at least one substituent selected from the group consisting of an alkyl group having 1 to 18 carbon atoms, an alkenyl group having 2 to 18 carbon atoms, an alkynyl group having 2 to 18 carbon atoms, an aryl group having 6 to 12 carbon atoms, an acyl group having 1 to 18 carbon atoms, an aroyl group having 7 to 18 carbon atoms, a nitro group, a cyano group, an alkoxy group having 1 to 18 carbon atoms, an alkylthio group having 1 to 18 carbon atoms, a hydroxyl group, and a halogen atom. 12 represents a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, an alkynyl group having 2 to 18 carbon atoms, an aryl group having 6 to 12 carbon atoms, an acyl group having 1 to 18 carbon atoms, an aroyl group having 7 to 18 carbon atoms, a nitro group, a cyano group, an alkoxy group having 1 to 18 carbon atoms, an alkylthio group having 1 to 18 carbon atoms, a hydroxyl group, or a halogen atom. Xα1 represents an amino group.

[0083] In formula (α1), n ​​generally represents an integer of 0 to 4, preferably an integer of 1 to 2, and more preferably 2. When n is 2, the substitution position of R1 is -CHRα on the benzene ring as specified in formula (α1).12 When the bonding position with - is the 1st position and the bonding position with -NO2 is the 2nd position, the 4th and 5th positions are preferable.

[0084] In formula (α1), Rα 11 represents at least one substituent selected from the group consisting of an alkyl group having 1 to 18 carbon atoms, an alkenyl group having 2 to 18 carbon atoms, an alkynyl group having 2 to 18 carbon atoms, an aryl group having 6 to 12 carbon atoms, an acyl group having 1 to 18 carbon atoms, an aroyl group having 7 to 18 carbon atoms, a nitro group, a cyano group, an alkoxy group having 1 to 18 carbon atoms, an alkylthio group having 1 to 18 carbon atoms, a hydroxyl group, and a halogen atom; 11 When there are a plurality of, they may be different from each other.

[0085] Rα in formula (α1) 11 Examples of the alkyl group having 1 to 18 carbon atoms represented by include a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an iso-butyl group, a sec-butyl group, a t-butyl group, a n-pentyl group, a n-hexyl group, a n-heptyl group, a n-octyl group, a n-nonyl group, a n-decyl group, a n-undecyl group, and a n-dodecyl group, and an alkyl group having 2 to 6 carbon atoms is preferable.

[0086] Rα in formula (α1) 11 Examples of the alkenyl group having 2 to 18 carbon atoms represented by include a vinyl group, a propenyl group, a 1-butenyl group, an iso-butenyl group, a 1-pentenyl group, a 2-pentenyl group, a 2-methyl-1-butenyl group, a 3-methyl-1-butenyl group, a 2-methyl-2-butenyl group, a 2,2-dicyanovinyl group, a 2-cyano-2-methylcarboxyvinyl group, and a 2-cyano-2-methylsulfonevinyl group.

[0087] Rα in formula (α1) 11 Examples of the alkynyl group having 2 to 18 carbon atoms represented by include an ethynyl group, a 1-propynyl group, and a 1-butynyl group.

[0088] Rα in formula (α1) 11Examples of the aryl group having 6 to 12 carbon atoms represented by include a phenyl group, a naphthyl group, and a tolyl group, and an aryl group having 6 to 10 carbon atoms is preferable.

[0089] Rα in formula (α1) 11 Examples of the acyl group having 1 to 18 carbon atoms represented by include a formyl group, an acetyl group, an ethylcarbonyl group, an n-propylcarbonyl group, an iso-propylcarbonyl group, an n-butylcarbonyl group, an n-pentylcarbonyl group, an iso-pentylcarbonyl group, a neo-pentylcarbonyl group, a 2-methylbutylcarbonyl group, and a nitrobenzylcarbonyl group.

[0090] Rα in formula (α1) 11 Examples of the aroyl group having 7 to 18 carbon atoms represented by the formula (1) include a benzoyl group, a toluoyl group, a naphthoyl group, and a phthaloyl group.

[0091] Rα in formula (α1) 11 Examples of the alkoxy group having 1 to 18 carbon atoms represented by include a methoxy group, an ethoxy group, an n-propoxy group, an iso-propoxy group, an n-butoxy group, an iso-butoxy group, a sec-butoxy group, a t-butoxy group, an n-pentoxy group, an iso-pentoxy group, a neo-pentoxy group, an n-hexyloxy group, and an n-dodecyloxy group.

[0092] Rα in formula (α1) 11 Examples of the alkylthio group having 1 to 18 carbon atoms represented by the formula (I) include a methylthio group, an ethylthio group, an n-propylthio group, an iso-propylthio group, an n-butylthio group, an iso-butylthio group, a sec-butylthio group, a t-butylthio group, an n-pentylthio group, an iso-pentylthio group, a 2-methylbutylthio group, a 1-methylbutylthio group, a neo-pentylthio group, a 1,2-dimethylpropylthio group, and a 1,1-dimethylpropylthio group.

[0093] Rα in formula (α1) 11 The halogen atom represented by the formula (I) includes a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0094] Rα in formula (α1) 11 Rα is preferably an alkoxy group having 1 to 18 carbon atoms, more preferably an alkoxy group having 1 to 10 carbon atoms, further preferably an alkoxy group having 1 to 4 carbon atoms, and particularly preferably a methoxy group. 11 If there are multiple Rα 11 is preferably an alkoxyl group, and all Rα 11 More preferably, is an alkoxy group.

[0095] In formula (α1), Rα 12 represents a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, an alkynyl group having 2 to 18 carbon atoms, an aryl group having 6 to 12 carbon atoms, an acyl group having 1 to 18 carbon atoms, an aroyl group having 7 to 18 carbon atoms, a nitro group, a cyano group, an alkoxy group having 1 to 18 carbon atoms, an alkylthio group having 1 to 18 carbon atoms, a hydroxyl group, or a halogen atom.

[0096] Rα in formula (α1) 12 The alkyl group having 1 to 18 carbon atoms, the alkynyl group having 2 to 18 carbon atoms, the aryl group having 6 to 12 carbon atoms, the acyl group having 1 to 18 carbon atoms, the aroyl group having 7 to 18 carbon atoms, the alkoxy group having 1 to 18 carbon atoms, the alkylthio group having 1 to 18 carbon atoms, and the halogen atom represented by Rα in the formula (α1) are as follows: 11 Examples of the alkyl group having 1 to 18 carbon atoms, the alkynyl group having 2 to 18 carbon atoms, the aryl group having 6 to 12 carbon atoms, the acyl group having 1 to 18 carbon atoms, the aroyl group having 7 to 18 carbon atoms, the alkoxy group having 1 to 18 carbon atoms, the alkylthio group having 1 to 18 carbon atoms, and the halogen atom represented by the formula (I) are the same as those represented by the formula (I).

[0097] Rα in formula (α1) 12 is preferably a hydrogen atom or an alkyl group having 1 to 18 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, even more preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and particularly preferably a hydrogen atom.

[0098] In formula (α1), Xα1 represents an amino group. The amino group represented by Xα1 in formula (α1) may be either a substituted amino group or an unsubstituted amino group (NH2 group), and the substituted amino group may be either a mono-substituted amino group or a di-substituted amino group.

[0099] Specific examples of the compound represented by formula (α1) include the following compounds (α1-1) to (α1-7).

[0100] [ka]

[0101] Further, examples of non-ionic photobase generators include coumaric acid-type photobase generators represented by the following general formula (α2), which have better stability as materials and better efficiency in generating a base when irradiated with energy rays.

[0102] [ka] In general formula (α2), Rα 21 and Rα 22 Rα are each independently a hydrogen atom or an organic group and may be the same or different. 21 and Rα 22 may be bonded to form a ring structure, and may contain a heteroatom bond. 21 and Rα 22 At least one of Rα is an organic group. 23 and Rα 24 Rα are each independently a hydrogen atom, a halogen atom, a hydroxyl group, a mercapto group, a sulfide group, a silyl group, a silanol group, a nitro group, a nitroso group, a sulfino group, a sulfo group, a sulfonato group, a phosphino group, a phosphinyl group, a phosphono group, a phosphonato group, or an organic group, and may be the same or different. 25 , Rα 26 , Rα 27 and Rα 28are each independently a hydrogen atom, a halogen atom, a hydroxyl group, a mercapto group, a sulfide group, a silyl group, a silanol group, a nitro group, a nitroso group, a sulfino group, a sulfo group, a sulfonato group, a phosphino group, a phosphinyl group, a phosphono group, a phosphonato group, an amino group, an ammonio group, or an organic group, and may be the same or different. 25 , Rα 26 , Rα 27 and Rα 28 Two or more of Rα may be bonded to form a ring structure, and may contain a heteroatom bond. 29 is a hydrogen atom or an organic group.

[0103] In general formula (α2), Rα 21 and Rα 22 From the viewpoint of the basicity of the generated base, it is preferable that both of the groups are alkyl groups or are bonded to each other to form an alkylene chain having a cyclic structure, and it is most preferable that both of the groups are bonded to each other to form an alkylene chain having a cyclic structure. The number of carbon atoms constituting the alkyl group or alkylene chain is preferably 1 to 20, and more preferably 1 to 8.

[0104] In general formula (α2), Rα 23 and Rα 24 are preferably a hydrogen atom or an alkyl group, and most preferably both are hydrogen atoms. The alkyl group preferably has 1 to 20 carbon atoms, and more preferably has 1 to 8 carbon atoms.

[0105] In general formula (α2), Rα 25 , Rα 26 , Rα 27 and Rα 28 are preferably hydrogen atoms, alkyl groups, or alkoxy groups, and most preferably all hydrogen atoms. The alkyl groups preferably have 1 to 20 carbon atoms, and more preferably have 1 to 8 carbon atoms. The alkoxy groups preferably have 1 to 20 carbon atoms, and more preferably have 1 to 8 carbon atoms.

[0106] In general formula (α2), Rα 29 is preferably a hydrogen atom or an organic group which is a protecting group that can be removed by irradiation with energy rays and / or heating, and is most preferably a hydrogen atom.

[0107] The coumaric acid type compound represented by the general formula (α2) is preferably the following compound (α2-1).

[0108] [ka]

[0109] Furthermore, as the non-ionic photobase generator, a urethane compound (α3)-1 represented by the following general formula is also preferred.

[0110] [ka]

[0111] In addition, as the non-ionic photobase generator, an oxime ester compound is also preferred. As the oxime ester compound, any compound that generates a basic substance upon irradiation with light can be used. In addition, a compound having two oxime ester groups in the molecule can also be preferably used, and specifically, an oxime ester compound having a carbazole structure represented by the following general formula (α4) can be mentioned.

[0112] [ka] In general formula (α4), Xα4 represents a hydrogen atom, an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a phenyl group, a phenyl group (substituted with an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, an amino group, an alkylamino group having 1 to 8 carbon atoms, or a dialkylamino group), a naphthyl group (substituted with an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, an amino group, an alkylamino group having 1 to 8 carbon atoms, or a dialkylamino group), and Yα4 and Zα4 each represent a hydrogen atom, an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a halogen group, a phenyl group, a phenyl group (substituted with an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, Arα4 represents a bond, an alkylene having 1 to 10 carbon atoms, vinylene, phenylene, biphenylene, pyridylene, naphthylene, thiophene, anthrylene, thienylene, furylene, 2,5-pyrrole-diyl, 4,4'-stilbene-diyl, or 4,2'-styrene-diyl; and n is an integer of 0 or 1.

[0113] In particular, in the general formula (α4), it is preferable that Xα4 and Yα4 are each a methyl group or an ethyl group, Zα4 is a methyl group or a phenyl group, n is 0, and Arα4 is a bond, phenylene, naphthylene, thiophene, or thienylene.

[0114] Furthermore, preferred carbazole oxime ester compounds include compounds represented by the following general formula (α5).

[0115] [ka] In general formula (α5), Rα 51Rα represents an alkyl group having 1 to 4 carbon atoms, or a phenyl group which may be substituted with a nitro group, a halogen atom, or an alkyl group having 1 to 4 carbon atoms. 52 Rα represents an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a phenyl group which may be substituted with an alkyl group or an alkoxy group having 1 to 4 carbon atoms. 53 Rα may be linked via an oxygen atom or a sulfur atom, and represents an alkyl group having 1 to 20 carbon atoms which may be substituted with a phenyl group, or a benzyl group which may be substituted with an alkoxy group having 1 to 4 carbon atoms. 54 represents a nitro group or an acyl group represented by Xα5-C(═O)—, where Xα5 represents an aryl group which may be substituted with an alkyl group having 1 to 4 carbon atoms, a thienyl group, a morpholino group, a thiophenyl group, or a structure represented by the following formula:

[0116] [ka]

[0117] Among the above-mentioned nonionic photobase generators, the coumaric acid type photobase generators represented by the above general formula (α2) are preferred, and the compound represented by (α2-1) is more preferred.

[0118] The content of the photobase generator (D) when the total weight of the composition for resin film-forming film (solid content equivalent) is 100 parts by mass is preferably 0.1 to 2 parts by mass, 0.2 to 1.5 parts by mass, 0.3 to 1 part by mass, or 0.4 to 0.7 parts by mass. By blending the photobase generator in the above ratio, it is easy to increase the variable X of the probe tack value, it is easy to make the probe tack (T2) of the resin film-forming film (resin film) after curing smaller, and it is easy to make T2-T3 smaller.

[0119] The photobase generator can be synthesized as a condensation product by referring to the examples described in, for example, JP-A-2009-80452, JP-A-2011-52214, JP-A-2021-177210, and JP-A-2019-45735.

[0120] (2.5. Polymer Component) In this embodiment, the composition for the resin film-forming film preferably contains a polymerizable component in addition to the above-mentioned curable component (B), the compound (C) having a thiol group, and the photobase generator (D). The polymer component (A) is a component that can be considered to be formed by a polymerization reaction of a polymerizable compound. The polymer component imparts film-forming properties (film-forming properties) to the resin film-forming film while imparting appropriate tack, thereby ensuring uniform attachment of the resin film-forming film to the workpiece. The weight-average molecular weight of the polymer component is usually in the range of 50,000 to 2,000,000, preferably 100,000 to 1,500,000, and particularly preferably 200,000 to 1,000,000. As such a polymer component, for example, acrylic resin, urethane resin, phenoxy resin, silicone resin, saturated polyester resin, etc. are used, and in particular, acrylic resin is preferably used.

[0121] Examples of the acrylic resin include (meth)acrylic acid ester copolymers consisting of a (meth)acrylic acid ester monomer and a structural unit derived from a (meth)acrylic acid derivative. The (meth)acrylic acid ester monomer here preferably includes a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 18 carbon atoms, specifically methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, etc. Examples of the (meth)acrylic acid derivative include (meth)acrylic acid, glycidyl (meth)acrylate, hydroxyethyl (meth)acrylate, etc.

[0122] In this embodiment, in order to control the adhesiveness to the workpiece and the adhesive properties, it is preferable to introduce a hydroxyl group into the acrylic resin using hydroxyethyl acrylate or the like.

[0123] The glass transition temperature of the acrylic resin is preferably −70° C. to 40° C., −60° C. to 30° C., −50° C. to 25° C., −40° C. to 20° C., or −35° C. to 15° C. By setting the glass transition temperature of the acrylic resin within the above range, the tack of the resin film-forming film is appropriately increased, the adhesive strength of the resin film-forming film to the workpiece is improved, and it becomes easier to appropriately improve the adhesive strength of the resin film to the workpiece.

[0124] When an acrylic resin has m types of structural units (m is an integer of 2 or more), the glass transition temperature of the acrylic resin can be calculated as follows: That is, when m types of monomers that derive the structural units in the acrylic resin are each assigned a unique number from 1 to m in sequence and named "monomer m", the glass transition temperature (Tg) of the acrylic resin can be calculated using the Fox formula shown below.

[0125]

number

[0126]

number

[0127] For Tgk, values ​​listed in the Polymer Data Handbook, Adhesive Handbook, Polymer Handbook, etc. can be used. For example, the Tgk of the homopolymer of methyl acrylate is 10°C, the Tgk of the homopolymer of n-butyl acrylate is -54°C, the Tgk of the homopolymer of methyl methacrylate is 105°C, the Tgk of the homopolymer of 2-hydroxyethyl acrylate is -15°C, the Tgk of the homopolymer of glycidyl methacrylate is 41°C, the Tgk of the homopolymer of 2-ethylhexyl acrylate is -70°C, the Tgk of the homopolymer of ethyl acrylate is -24°C, and the Tgk of the homopolymer of 4-acryloylmorpholine is 145°C.

[0128] When the total weight of the composition for resin film-forming film is 100 parts by mass, the content of the polymer component (A) is preferably 5 to 60 parts by mass, 8 to 50 parts by mass, 10 to 40 parts by mass, or 12 to 30 parts by mass. By setting the content of the polymer component within the above range, it becomes easier to control the adhesion of the resin film-forming film, and it becomes easier to set the probe tack (T1) of the resin film-forming film within the above range.

[0129] (2.6. Filler) By containing the filler (E) in the resin film-forming film, the resin film obtained by resinifying the resin film-forming film can have a thermal expansion coefficient that is easier to adjust, and by bringing this thermal expansion coefficient closer to the thermal expansion coefficient of the workpiece (e.g., a semiconductor wafer), the adhesive reliability of the resin film-coated workpiece obtained using the resin film-forming film is improved. In addition, by containing the filler (E) in the resin film-forming film, a hard resin film can be obtained, and the moisture absorption rate of the resin film can be reduced, further improving the adhesive reliability of the resin film-coated workpiece.

[0130] The filler (E) may be either an organic filler or an inorganic filler, but is preferably an inorganic filler from the viewpoint of shape stability at high temperatures.

[0131] Examples of preferred inorganic fillers include powders of silica, alumina, talc, calcium carbonate, red iron oxide, silicon carbide, boron nitride, etc.; beads of these inorganic fillers that are spherical; surface-modified products of these inorganic fillers; single crystal fibers of these inorganic fillers; glass fibers, etc. Among these, silica and surface-modified silica are preferred. The surface-modified silica is preferably surface-modified with a coupling agent, and more preferably surface-modified with a silane coupling agent.

[0132] The average particle size of the filler is preferably 0.02 to 10 μm, 0.05 to 5 μm, or 0.10 to 3 μm.

[0133] By setting the average particle size of the filler within the above range, the composition for resin film-forming film has good handleability, and as a result, the quality of the composition for resin film-forming film and the resin film-forming film tends to be stable.

[0134] In this specification, unless otherwise specified, the term "average particle size" refers to the particle size (D50) at an integrated value of 50% in a particle size distribution curve determined by a laser diffraction scattering method.

[0135] The content of the filler when the total weight of the composition for resin film forming film is 100 parts by mass is preferably 15 to 80 parts by mass, 30 to 75 parts by mass, 40 to 70 parts by mass, or 50 to 70 parts by mass.

[0136] By setting the lower limit of the filler content to the above value, the adhesive reliability of the resin-film-coated workpiece obtained by using the resin film-forming film is further improved. Also, by setting the upper limit of the filler content to the above value, it becomes easier to set the probe tack (T1) of the resin film-forming film to the above range, and the adhesive strength of the resin film-forming film with the workpiece is improved, and the adhesive strength of the resin film with the workpiece is appropriately improved.

[0137] (2.7. Colorants) The resin film-forming film preferably contains a colorant (F), which conceals the back surface of the workpiece such as a chip, thereby blocking various electromagnetic waves generated in electronic devices and reducing malfunction of the workpiece such as a chip.

[0138] As the colorant (F), for example, known ones such as organic pigments, organic dyes, inorganic pigments, etc. In this embodiment, inorganic pigments are preferred.

[0139] Examples of inorganic pigments include carbon black, cobalt-based pigments, iron-based pigments, chromium-based pigments, titanium-based pigments, vanadium-based pigments, zirconium-based pigments, molybdenum-based pigments, ruthenium-based pigments, platinum-based pigments, ITO (indium tin oxide)-based pigments, and ATO (antimony tin oxide)-based pigments. Among these, it is particularly preferable to use carbon black. Carbon black can block electromagnetic waves in a wide wavelength range.

[0140] The amount of colorant in the resin film-forming film varies depending on the thickness of the resin film-forming film. For example, when the thickness of the resin film-forming film is 25 μm, the content of the colorant is preferably 0.01 to 10 parts by mass, 0.03 to 7 parts by mass, or 0.05 to 4 parts by mass when the total weight of the composition for the resin film-forming film is 100 parts by mass.

[0141] The average particle size of the colorant (particularly carbon black) is preferably 1 to 500 nm, 3 to 100 nm, or 5 to 50 nm. When the average particle size of the colorant is within the above range, it is easy to control the light transmittance within a desired range.

[0142] (2.8. Other Additives) The composition for resin film-forming film may contain other additives, such as coupling agents, crosslinking agents, plasticizers, antistatic agents, antioxidants, gettering agents, tackifiers, release agents, etc., within the range that does not impair the effects of the present invention.

[0143] (3. Release film) The release film is a film that can support the resin film-forming film in a releasable manner. The release film may be composed of one layer (single layer) or two or more layers of substrate, and the surface of the substrate may be subjected to a release treatment in order to control the releasability. That is, the surface of the substrate may be modified, or a material (release agent layer) not derived from the substrate may be formed on the surface of the substrate.

[0144] The substrate is not particularly limited as long as it is a material that can support the resin film until it is attached to the workpiece, and is usually composed of a film primarily made of a resin-based material (hereinafter referred to as a "resin film").

[0145] Specific examples of the resin film include polyethylene film, polypropylene film, polybutene film, polybutadiene film, polymethylpentene film, polyvinyl chloride film, vinyl chloride copolymer film, polyethylene terephthalate film, polyethylene naphthalate film, polybutylene terephthalate film, polyurethane film, ethylene vinyl acetate copolymer film, ionomer resin film, ethylene-(meth)acrylic acid copolymer film, ethylene-(meth)acrylic acid ester copolymer film, polystyrene film, polycarbonate film, polyimide film, and fluororesin film. Crosslinked films of these films are also used. Furthermore, laminated films of these films may be used. In this embodiment, a polyethylene terephthalate film is preferred from the viewpoints of environmental safety, cost, and the like.

[0146] The above resin film may contain various additives such as a colorant, a flame retardant, a plasticizer, an antistatic agent, a lubricant, and a filler.

[0147] The release agent layer is obtained by applying a coating agent containing a composition for a release agent layer to one side of a substrate, and then drying and curing the coating. The composition for the release agent layer is not particularly limited as long as it is a material that can impart releasability from the resin film-forming film to the substrate. In this embodiment, the composition for the release agent layer is preferably, for example, an alkyd-based release agent, a silicone-based release agent, a fluorine-based release agent, an unsaturated polyester-based release agent, a polyolefin-based release agent, or a wax-based release agent, and among these, a silicone-based release agent is preferable. The thickness of the release agent layer is not particularly limited, but is preferably 30 nm or more and 200 nm or less.

[0148] The thickness of the release film is not particularly limited, but is preferably 15 to 100 μm, more preferably 25 to 80 μm, and even more preferably 35 to 60 μm.

[0149] In addition, when the release films 21, 22 are formed on both main surfaces (side A 10a, side B 10b) of the resin film-forming film 10 as shown in Fig. 1, it is preferable that the peeling force of one release film is made large to be a heavy release type release film, and the peeling force of the other release film is made small to be a light release type release film. Furthermore, it is preferable that the surface on the light release type release film side is the main surface (side B) to be attached to the work, and the surface on the heavy release type release film side is the main surface (side A) to be irradiated with energy rays. In addition, the peeling force can be measured, for example, at a peeling speed of 300 mm / min and a peeling angle of 180° in an environment of 23°C and relative humidity of 50%.

[0150] (4. Method for producing resin film-forming film and sheet for resin film-forming) The method for producing the resin film-forming film is not particularly limited. The film is produced using the above-mentioned composition for resin film-forming film, or a composition obtained by diluting the composition for resin film-forming film with a solvent (the above two compositions are referred to as "coating agent"). The coating agent is prepared by mixing the components constituting the composition for resin film-forming film by a known method.

[0151] The obtained coating agent is applied to the release surface of the first release film 21 using a coating machine such as a roll coater, a knife coater, a roll knife coater, an air knife coater, a die coater, a bar coater, a gravure coater, or a curtain coater, and dried as necessary to form a resin film-forming film on the first release film 21.

[0152] Next, the release surface of the second release film 22 is further laminated to the exposed surface of the resin film-forming film formed on the first release film 21, thereby obtaining the sheet for resin film formation 1 shown in FIG.

[0153] (5. Method for manufacturing individual workpieces with resin film) As an example of a method for manufacturing a resin film-coated workpiece singulated product using the resin film-forming film according to this embodiment, a method for obtaining a resin film-coated workpiece singulated product by singulating a workpiece to which a resin film-forming film is attached will be described.

[0154] The method for producing individual workpieces with a resin film according to this embodiment includes at least the following steps 1 to 3. Step 1: A process of attaching the above-mentioned resin film to the back side of the workpiece Step 2: The attached resin film forming film is cured to form a resin film on the back side of the workpiece, obtaining a workpiece with a resin film. Step 3: A step of dividing the resin-film-coated workpiece into individual pieces to obtain a plurality of resin-film-coated workpiece individual pieces.

[0155] In this embodiment, in step 2, it is preferable to cure the resin film by irradiating it with energy rays.

[0156] The manufacturing method of the resin film-attached workpiece singulated product, which includes the above-mentioned steps 1 to 3 and hardens the resin film-forming film by irradiation with energy rays in step 2, will be described with reference to the drawings. In the following, the case will be described where the resin film-forming sheet is a protective film-forming sheet, the resin film-forming film is a protective film-forming film, the resin film is a protective film, the workpiece is a wafer, the workpiece singulated product is a chip, the first release film is a heavy release type release film, and the second release film is a light release type release film.

[0157] (Process 1) The resin film forming sheet (protective film forming sheet) 1 shown in Fig. 1 is stored as a wound sheet roll, and when used, is unwound from the sheet roll and the protective film forming film is cut into a predetermined shape. The predetermined shape may be substantially the same as the shape of the work 6 to be attached.

[0158] The second release film 22 is peeled off from the protective film-forming sheet 1, and the B side 10b of the protective film-forming film 10 is attached to the back surface 6b of the workpiece 6 (wafer) as shown in Fig. 2. That is, the B side 10b is the main surface to be attached to the workpiece. As described above, since the probe tack (T1) of the B side to be attached to the workpiece is within the above range, the protective film-forming film 10 is well attached and fixed to the workpiece 6 before the energy beam irradiation.

[0159] (Process 2) After the attachment, as shown in FIG. 3, the first release film 21 is peeled off to expose the A-side 10a of the protective film-forming film 10. The exposed A-side 10a of the protective film-forming film 10 is irradiated with energy rays ER from an energy ray irradiation source 80. This causes the protective film-forming film 10 to harden and form a protective film 11, and as shown in FIG. 4, a wafer 100 with a protective film is obtained. The illuminance and light amount of the energy rays may be set to conditions that allow the protective film-forming film to be sufficiently hardened. In this embodiment, for example, the illuminance of the energy rays is 30 to 280 mW / cm. 2 The amount of energy is 500-5000mJ / cm 2 This can be done as follows.

[0160] Since step 2 is performed under air, by peeling off the first release film, the A-side 10a of the protective film-forming film comes into contact with oxygen. However, since the protective film-forming film has the above-mentioned composition, even if the A-side 10a of the protective film-forming film is irradiated with energy rays while it is in contact with oxygen, polymerization inhibition due to oxygen does not occur. Therefore, the A-side 10a is also sufficiently cured, and the tack of the A-side 11a of the cured protective film-forming film (protective film) can be reduced to an intended level. Furthermore, the tack is easily reduced to a level at which the above-mentioned conveyance failure does not occur.

[0161] (Step 3) After the obtained wafer with the protective film is transported, the wafer with the protective film and ring frame 7 are attached to a known dicing sheet 80 as shown in Fig. 5, and the wafer with the protective film is diced by a known dicing method to obtain a chip having the protective film 11 (chip with the protective film 100a). If necessary, laser marking or the like may be performed on the protective film.

[0162] The obtained chip with the protective film is picked up and collected by a suction collet or the like. The picked up chip with the protective film may be transported to the next process, or may be temporarily stored in a tray, tape, or the like and transported to the next process after a predetermined period of time. The chip with the protective film 100a transported to the next process is mounted on a substrate.

[0163] (6. Modifications) In the above-mentioned embodiment, the curing reaction is controlled by using a photobase generator that generates a base by irradiating the photobase generator with energy rays, but a photobase generator that generates a base by heating in addition to energy ray irradiation may be used. In particular, an ion-type photobase generator that can generate a base by heating at 100 to 200°C is preferable. In addition, deprotonation of thiol groups by the base released by energy ray irradiation and curing reaction may be further promoted by heating in addition to energy ray irradiation. The heating temperature in this case is preferably 50 to 200°C.

[0164] By using such a photobase generator, a curing reaction caused by energy ray irradiation or a curing reaction caused by heating can be selected depending on the application, etc., and the resin film-forming film can be appropriately cured.

[0165] In the above-mentioned embodiment, the resin film-forming film is a protective film-forming film, but the resin film-forming film may be an adhesive film-forming film such as a die bonding film. For example, when a known dicing sheet is attached to the resin film-forming film side of a workpiece with a resin film-forming film containing a photobase generator, and the workpiece is diced by a known dicing method, and then the resin film-forming film is cured by irradiating energy rays. In each workpiece with a resin film-forming film, the resin film-forming film located on the cut surface by dicing is exposed to air, but polymerization inhibition due to oxygen does not occur. Therefore, even if the resin film-forming film is exposed to air located on the cut surface, the tack can be reduced to an intended level after energy irradiation. Thereby, for example, when picking up and peeling off from the dicing sheet, the risk that the residue of the resin film-forming film that is insufficiently cured by energy rays remains on the dicing sheet can be reduced. When the resin film-forming film is an adhesive film-forming film, it is preferable that the resin film-forming film is heat-curable in order to enhance adhesion, in addition to being energy-ray curable. This makes it easier to bond, for example, a circuit board and an individual workpiece more firmly using thermal curing.

[0166] In the above embodiment, the sheet 1 for resin film formation shown in FIG. 1 has been described as a structure including a resin film-forming film, but the structure including a resin film-forming film may be a composite sheet for resin film formation having a resin film-forming film and a support sheet that supports the resin film-forming film. The support sheet may be anything other than a release film, as long as it has a structure that can support the resin film-forming film. Here, the support sheet is preferably an adhesive sheet having a substrate and an adhesive layer.

[0167] The base material of the adhesive sheet can be any known material as long as it is suitable for processing of a workpiece, for example, dicing of a wafer, etc. Usually, it is made of a film mainly made of a resin-based material (resin film).

[0168] The adhesive layer of the adhesive sheet may be composed of a non-energy ray curable adhesive, or may be composed of an energy ray curable adhesive. Examples of non-energy ray curable adhesives include acrylic adhesives, rubber adhesives, silicone adhesives, urethane adhesives, polyester adhesives, and polyvinyl ether adhesives. The energy ray curable adhesive may be mainly composed of a polymer having energy ray curability, or may be mainly composed of a mixture of a polymer not having energy ray curability and an energy ray curable monomer and / or oligomer.

[0169] 6 shows an example of the configuration of the composite sheet 2 for resin film formation. The composite sheet 2 for resin film formation has a configuration including an adhesive sheet 4 formed by laminating an adhesive layer 42 on one surface of a substrate 41, a resin film-forming film 10 laminated such that an A surface 10a is in contact with the adhesive layer 42 of the adhesive sheet 4, and a release film 23 arranged on a B surface 10b of the resin film-forming film 10. Furthermore, an adhesive layer for a jig (not shown) may be arranged on the peripheral portion of the resin film-forming film 10. The adhesive layer for a jig is a layer for adhering the composite sheet for resin film formation to a jig such as a ring frame.

[0170] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES

[0171] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0172] (Preparation of resin film forming sheet) A sheet for resin film formation was prepared as follows using a coating agent containing the composition for resin film formation described below.

[0173] (Coating agent containing composition for resin film-forming film) The following components were mixed in the compounding ratio (solid content equivalent) shown in Table 1, and diluted with methyl ethyl ketone to a solid content concentration of 50 mass % to prepare a coating agent containing a composition for a resin film-forming film.

[0174] (A) Polymer Component (A-1): (meth)acrylic acid ester copolymer obtained by copolymerizing 10 parts by mass of n-butyl acrylate, 70 parts by mass of methyl acrylate, 5 parts by mass of glycidyl methacrylate, and 15 parts by mass of 2-hydroxyethyl acrylate (weight average molecular weight: 400,000, glass transition temperature: -1°C) (A-2): (meth)acrylic acid ester copolymer obtained by copolymerizing 33 parts by mass of n-butyl acrylate, 27 parts by mass of methyl acrylate, 25 parts by mass of 4-acryloylmorpholine, and 15 parts by mass of 2-hydroxyethyl acrylate (weight average molecular weight: 700,000, glass transition temperature: 2°C). (B) Epoxy resin: Bisphenol A type epoxy resin (Mitsubishi Chemical Corporation, jER828, liquid at 23°C and 1 atm, molecular weight 370, softening point 93°C, epoxy equivalent 184-194g / eq) (C) Compound having a thiol group: pentaerythritol tetrakis(3-mercaptobutyrate) (manufactured by Resonac, KarenzMT (registered trademark) PE1) (D) Photobase generator: non-ionic photobase generator (a compound having the following chemical structure, E)-N-cyclohexyl-N-((E)-(cyclohexylimino)(piperidin-1-yl)methyl)-3-(2-hydroxyphenyl)acrylamide) [ka] (E) Filler: Silica filler (fused silica filler, average particle size 8 μm) (F) Coloring agent (F-1) Black pigment (a pigment obtained by mixing 32 parts by mass of a phthalocyanine blue pigment (Pigment Blue 15:3), 18 parts by mass of an isoindolinone yellow pigment (Pigment Yellow 139), and 50 parts by mass of an anthraquinone red pigment (Pigment Red 177), and pigmentizing the mixture such that the total amount of the three pigments / amount of styrene acrylic resin was 1 / 3 (mass ratio).) (F-2) Carbon black (Mitsubishi Chemical Corporation, MA-600B, average particle size 20 nm) (G) Energy ray curable compound (G-1) ε-caprolactone-modified tris-(2-acryloxyethyl) isocyanurate (manufactured by Shin-Nakamura Chemical Co., Ltd., A-9300-1CL, trifunctional UV-curable compound) (G-2) Urethane acrylate (KJ Chemicals, Quick cure 8100EA70) (H) Photoradical initiator (H-1) 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one (IGM Resins, Omnirad® 127D) (H-2) 2-(Dimethylamino)-1-(4-morpholinophenyl)-2-benzyl-1-butanone (IGM Resins, Omnirad® 369) (I) Ultraviolet absorber: hydroxyphenyltriazine-based ultraviolet absorber (manufactured by BASF, Tinuvin (registered trademark) 479).

[0175] A first release film (manufactured by Lintec Corporation, SP-PET382150, thickness 38 μm) consisting of a polyethylene terephthalate (PET) film with a silicone-based release agent layer formed on one side thereof, and a second release film (manufactured by Lintec Corporation, SP-PET381031, thickness 38 μm) consisting of a PET film with a silicone-based release agent layer formed on one side thereof were prepared.

[0176] The coating agent containing the resin film-forming film composition prepared above was applied to the release surface of the first release film by a knife coater so that the thickness of the resin film-forming film finally obtained was 25 μm, and then dried at 120 ° C. for 2 minutes using an oven to form a resin film-forming film. Next, the release surface of the second release film was placed on the resin film-forming film and both were bonded together to obtain sheets for resin film formation of Examples 1 and 2 and Comparative Examples 1 and 2, which consist of the first release film, the resin film-forming film (thickness: 25 μm), and the second release film.

[0177] [Table 1]

[0178] The obtained sheet for resin film formation was subjected to the following measurements and evaluations.

[0179] (Probe tack (T1) of side B of resin film forming film before curing) The resin film-forming sheet obtained in the examples and comparative examples was cut into a size of 10 mm x 10 mm, the second release film (light release type release film) was peeled off, and the exposed B side of the resin film-forming film (in FIG. 1, B side 10b) was attached to a probe tack tester fixture (20 g) to prepare a test piece. Under an environment of 23°C and relative humidity of 50%, a probe tack tester (manufactured by Tester Sangyo Co., Ltd., TE-6001) was used to measure the probe tack of the B side of the resin film-forming film before curing by contacting the probe (probe diameter: 5.05 mmφ) of the probe tack tester with the B side (in FIG. 1, B side 10b) of the second release film side of the resin film-forming film and then peeling it off under the conditions of a contact speed of 1 mm / sec, a contact time of 1 second, and a peeling speed of 1 mm / sec. This measurement was performed seven times by changing the test piece. The average value of five measured values ​​excluding the maximum and minimum values ​​out of the seven measured values ​​was taken as T1. The results are shown in Table 1.

[0180] (Probe tack (T2) of side A of resin film after energy ray irradiation in a state where side A is in contact with oxygen) The resin film-forming sheets obtained in the examples and comparative examples were cut to a size of 25 mm x 25 mm, the second release film (light release type release film) was peeled off, and the good adhesion surface of a good adhesion PET (PET38A-4100, manufactured by Toyobo Co., Ltd.) having a thickness of 38 μm and a size of 25 mm x 25 mm was thermally laminated (70°C, 1 m / min) to the B side (side B 10b in Figure 1) of the exposed resin film-forming film to obtain a laminate sample having a configuration of PET film / resin film-forming film / first release film.

[0181] The laminate sample was cut into a size of 10 mm x 10 mm, and the first release film (heavy release type release film) was peeled off to expose the A side (A side 10a in Fig. 1) of the resin film-forming film. 2 , light intensity is 2000mJ / cm 2 Under the conditions, the exposed A side of the resin film-forming film was irradiated with ultraviolet light under air to harden the resin film-forming film to form a resin film. After the energy ray irradiation, the resin film was left to stand for 2 hours. After the 2-hour stand, the A side of the resin film was attached to a probe tack tester fixture (20 g). Using a probe tack tester (TE-6001, manufactured by Tester Sangyo Co., Ltd.) in an environment of 23°C and relative humidity of 50%, the probe tack of the A side after the energy ray irradiation of the A side was measured by contacting the probe (probe diameter: 5.05 mmφ) of the probe tack tester to the A side of the resin film and then peeling it off under the conditions of a contact speed of 1 mm / sec, a contact time of 1 second, and a peeling speed of 1 mm / sec. This measurement was performed 7 times by changing the test piece. The average value of five measured values ​​excluding the maximum and minimum values ​​out of the seven measured values ​​was taken as T2. The results are shown in Table 1. In cases where the resin film did not adhere sufficiently to the jig (20 g) of the probe tack tester, it was attached using a 5 μm thick adhesive acrylic resin and used for measurement. However, since the probe of the probe tack tester was only in contact with the resin film, there was no effect on T2.

[0182] From the calculated T1 and T2, the variable X of the probe tack value shown below was calculated. The results are shown in Table 1. Probe tack value variable X(%)=100×(T1-T2) / T1

[0183] (Probe tack (T3) of side A of resin film after energy ray irradiation when side A is not in contact with oxygen) The probe tack of the A-side of the resin film was measured and T3 was calculated by the same method as the measurement method of T2 described above, except that the ultraviolet irradiation was performed not in air but in a nitrogen atmosphere in which the air was replaced with nitrogen gas. The results are shown in Table 1. Note that for Comparative Example 2, the probe tack (T3) was not evaluated because the variable X of the probe tack value was not within the above-mentioned preferable range.

[0184] From the calculated T2 and T3, the difference between the probe tack (T2) and the probe tack (T3) shown below was calculated. The results are shown in Table 1. Difference between probe tack (T2) and probe tack (T3) = T2-T3

[0185] From Table 1, it was confirmed that when the resin film-forming film contains the above-mentioned components, the difference between the probe tack (T2) and the probe tack (T3) falls within the above-mentioned range, and even after irradiating the A-side of the resin film-forming film with energy rays while the A-side is in contact with oxygen, no unintended tack remains. [Industrial Applicability]

[0186] The resin film of the present invention can be suitably used as a resin film to be cured by energy rays in an environment in contact with oxygen. [Explanation of symbols]

[0187] 1...Resin film forming sheet 10...Resin film forming film 21…First release film 22...Second release film 2…Composite sheet for forming resin film 10...Resin film forming film 4...Adhesive sheet 100...Wafer with resin film (protective film) 100a…Chip with resin film (protective film) 11...Resin film

Claims

1. A resin film-forming film that becomes a resin film after curing, The resin film-formed film includes an epoxy resin, a compound having a thiol group, and a photobase generator.

2. The resin film-forming film has a surface A and a surface B as main surfaces, The resin film according to claim 1, wherein when the probe tack value T2 of the A side after irradiation with energy rays in a state where the A side is in contact with oxygen is 0.01 N or less.

3. The resin film-forming film has a surface A and a surface B as main surfaces, The resin film according to claim 1 or 2, wherein the probe tack value of the B side before the energy ray irradiation is T1, and the probe tack value of the A side after the energy ray irradiation in a state where the A side is in contact with oxygen is T2, the probe tack value variable X shown below is 99.0% or more. Probe tack value variable X (%) = 100 x (T1 - T2) / T1

4. The resin film according to claim 1 or 2, wherein the photobase generator is a non-ionic type.

5. 3. A sheet for resin film formation comprising: the resin film-forming film according to claim 1 or 2; and a release film releasably arranged on at least one of the main surfaces, the A surface and the B surface, of the resin film-forming film.

6. A step of attaching the resin film-forming film according to claim 1 or 2 to a back surface of a workpiece; A step of hardening the applied resin film forming film to form a resin film on the back surface of the workpiece to obtain a workpiece with a resin film; and a step of singulating the resin-film-coated workpiece to obtain a plurality of resin-film-coated workpiece singulations.

7. A step of attaching a resin film forming film provided in the sheet for resin film formation according to claim 5 to a back surface of a workpiece; A step of hardening the applied resin film forming film to form a resin film on the back surface of the workpiece to obtain a workpiece with a resin film; and a step of singulating the resin-film-coated workpiece to obtain a plurality of resin-film-coated workpiece singulations.

8. The method for producing an individual workpiece with a resin film according to claim 6, wherein the resin film-forming film is cured by irradiation with energy rays.

9. The method for producing an individual workpiece with a resin film according to claim 7, wherein the resin film-forming film is cured by irradiation with energy rays.

Citation Information

Patent Citations

  • Energy ray-curable chip protecting film

    JP2009138026A