Laser welding joint and manufacturing method for lase welding joint
A laser welded joint with specific C, Al, and Ti compositions in high carbon steel materials and weld metal addresses blowholes and maintains strength, enhancing mechanical properties and reducing costs by omitting pickling.
Patent Information
- Application Number
- JP2023075958
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-05-02
AI Technical Summary
Laser welding of high carbon steel materials with black coating is prone to blowholes due to CO gas, and excessive addition of deoxidizing agents like Al or Ti reduces joint strength.
A laser welded joint with specific compositions of high carbon steel materials and weld metal, including a C content of 0.30% by mass or more, oxide scale thickness of 5 μm or more, and balanced Al and Ti contents of 0.03 to 0.11% by mass each, with a sum of 0.14% by mass or more, to suppress blowholes and maintain joint strength.
The solution effectively suppresses blowholes and maintains joint strength in laser welded joints, ensuring high mechanical properties and cost-effectiveness by omitting the pickling process.
Smart Images

Figure 2024160732000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laser welded joint and a method for manufacturing a laser welded joint. [Background technology]
[0002] High carbon steel sheets with a high carbon concentration are used for automotive components, especially for buses and trucks, because high strength is required for these components. In addition, to reduce costs, blackened steel sheets with oxide scale on the surface are used for these components by omitting the pickling process. In recent years, laser welding has been used to shorten welding time. However, when manufacturing joints including high carbon steel sheets and black steel sheets by laser welding, there is a problem that blowholes due to CO gas are likely to occur. On the other hand, when deoxidizers such as Al and Ti are added in excess to suppress blowholes, there is a problem that the strength of the joint decreases.
[0003] For example, in Patent Documents 1 and 2, the mechanical properties of the weld metal part are improved by adding Al or Ti to the steel plate. However, the present inventors thought that there is room for further improvement from the viewpoint of ensuring joint strength while suppressing the occurrence of blowholes. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 2003-245787 [Patent Document 2] Japanese Patent Publication No. 2000-288754 Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made in consideration of the above, and an object of the present invention is to provide a laser welded joint that can suppress the occurrence of blowholes while ensuring joint strength in a laser welded joint including a high carbon steel material and a steel material with a black scale, and a manufacturing method thereof. [Means for solving the problem]
[0006] (1) A laser welded joint according to one aspect of the present invention is A laser welded joint comprising a plurality of steel materials and a weld metal that joins the plurality of steel materials, At least one of the plurality of steel materials is a high carbon steel material having a C content of 0.30 mass% or more, At least one of the plurality of steel materials is a black-skinned steel material having an oxide scale having a thickness of 5 μm or more; The weld metal has an average C content of 0.24 mass% or more, an average Al content of 0.03 to 0.11 mass%, and an average Ti content of 0.03 to 0.11 mass%, The sum of the average Al content and the average Ti content of the weld metal is 0.14 mass % or more. (2) In the laser welded joint described in (1) above, the oxide scale may have a thickness of 20 μm or less. (3) In the laser welded joint described in (1) or (2) above, the high carbon steel material may have a plate thickness of 9.0 mm or less. (4) In the laser welded joint according to any one of (1) to (3) above, the laser welded joint may be a T-fillet laser welded joint. (5) In the laser welded joint described in (4) above, the black-scaled steel material and the high-carbon steel material may be the same steel material, and at least one of the plurality of steel materials may be butt-joined to a surface of the same steel material. (6) The laser welded joint described in (4) above may be such that the high carbon steel material is butt-joined to the surface of the black-scaled steel material. (7) A method for producing a laser welded joint according to one aspect of the present invention includes the steps of: A method for manufacturing a laser welded joint including a laser welding process for forming a weld metal for joining a plurality of steel materials, In the laser welding step, a filler is supplied and laser welding is performed; At least one of the plurality of steel materials is a high carbon steel material having a C content of 0.30 mass% or more, At least one of the plurality of steel materials is a black-skinned steel material having an oxide scale having a thickness of 5 μm or more; The weld metal has an average C content of 0.24 mass% or more, an average Al content of 0.03 to 0.11 mass%, and an average Ti content of 0.03 to 0.11 mass%, The sum of the average Al content and the average Ti content of the weld metal is 0.14 mass % or more. Effect of the Invention
[0007] According to the laser welded joint and the manufacturing method thereof of the present invention, in a laser welded joint including a high carbon steel material and a steel material with a black scale, the occurrence of blowholes can be suppressed while ensuring joint strength. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a schematic cut end view for explaining a lap laser welded joint. [Diagram 2] FIG. 2 is a schematic cut end view for explaining a T-fillet laser welded joint. [Diagram 3] FIG. 2 is a schematic cut end view for explaining a laser butt welded joint. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Laser welded joints including the above-mentioned high carbon steel and black steel have an issue of blowholes caused by CO gas. Although adding a large amount of deoxidizer to the weld metal is effective in suppressing CO gas, a new issue was found in that adding an excessive amount of Al reduces the hardenability of the weld metal, softening the weld metal and reducing the joint strength. In addition, a new issue was discovered in which excessive addition of Ti reacts with C in the weld metal to form Ti carbide, reducing the amount of C that contributes to the hardness of the weld metal, softening the weld metal, and reducing joint strength.
[0010] Therefore, the inventors attempted to suppress the occurrence of blowholes without reducing the strength of a laser welded joint including a high carbon steel material by specifying the Al and Ti contents of the weld metal.
[0011] Hereinafter, the embodiments of the present invention will be described with reference to examples, but it is obvious that the present invention is not limited to the examples described below. In the following description, specific numerical values and materials may be exemplified, but other numerical values and materials may be applied as long as the effects of the present invention can be obtained. In addition, the components of the following embodiments can be combined with each other. In this specification, a numerical range expressed using "to" means a range including the numerical values before and after "to" as the lower and upper limits. In this specification, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.
[0012] In the following embodiments, the steel material includes steel plates, parts machined into shapes other than flat plates, and steel plates in which different types of steel plates are joined together.
[0013] [Laser welded joints] The laser welded joint according to this embodiment is a laser welded joint including a plurality of steel materials and a weld metal that joins the plurality of steel materials. Laser welded joints are made by arranging multiple steel materials, such as by overlapping them or butting their ends together or the plate surfaces of the steel materials together, irradiating the joint with a laser beam to melt the steel materials and filler (filler metal) in the areas irradiated with the laser beam, and solidifying the molten metal to form weld metal, and have a structure in which multiple steel materials are joined by the weld metal.
[0014] At least one of the multiple steel materials constituting the laser welded joint according to this embodiment is a high carbon steel material. Also, at least one of the multiple steel materials constituting the laser welded joint according to this embodiment is a steel material with black scale. The number of steel materials is not particularly limited and can be any number of 2 or more.
[0015] [High carbon steel] The C content (carbon amount) of the high carbon steel material is 0.30 mass % or more. By making the C content (carbon amount) of the high carbon steel material 0.30 mass % or more, high strength can be obtained. Although there is no upper limit for the C content in high carbon steel, it is preferable to keep the C content at 1.1% or less in order to suppress cracking in welds that occurs with an increase in C content.
[0016] The carbon content of steel is measured by taking chips from the inside of the high-carbon steel to a depth of 0.3 mm or more from the surface, and measuring the chips using the well-known high-frequency combustion method (combustion-infrared absorption method). Chips are taken from three locations, and the arithmetic average of the measured values is taken as the carbon content of the high-carbon steel.
[0017] [Blackened steel] Black-scaled steel is a steel that has an oxide scale with a thickness of 5 μm or more. Since the process of removing the oxide scale can be omitted, the manufacturing cost of the steel can be reduced by having at least one of the multiple steel products be a black-scaled steel that has an oxide scale with a thickness of 5 μm or more.
[0018] As the oxide scale becomes thicker, the occurrence of blowholes becomes more noticeable, particularly in steel materials having an oxide scale with a thickness of 5 μm or more. However, in the laser welded joint of this embodiment, the occurrence of blowholes can be suppressed while ensuring joint strength due to the characteristics described below.
[0019] In the laser welded joint of this embodiment, it is more preferable that the thickness of the oxide scale of the black-skinned steel material is 20 μm or less. By keeping the thickness of the oxide scale to 20 μm or less, paint peeling in subsequent processes is suppressed and the corrosion resistance of the steel is ensured.
[0020] The thickness of the oxide scale is measured by observing the cross section. Specifically, the blackened steel material is cut out, embedded, mirror-polished, and the thickness of the oxide scale is measured using an optical microscope or SEM. The arithmetic average value of the three measurement points is taken as the thickness of the oxide scale.
[0021] The oxide scale contains Fe and O as components, and is mainly composed of iron oxide. The term "main component" used here means that iron oxide accounts for 50 mass % or more of the oxide scale.
[0022] At least one of the steel materials included in the laser welded joint of this embodiment may be a high carbon steel material having a C content of 0.30 mass% or more and a black scale-covered steel material having an oxide scale of 5 μm or more in thickness. In other words, the high carbon steel material and the black scale-covered steel material may be the same steel material. This has the advantage that the steel sheet price is cheaper than that of pickled materials.
[0023] Black-scaled steel is produced by omitting the pickling process in the hot-rolled steel sheet manufacturing process. The thickness of the oxide scale of black-scaled steel can be adjusted by controlling the temperature and time of the hot-rolling process.
[0024] In the laser welded joint according to the present embodiment, the chemical composition of one or more of the steel materials may contain 0.03-1.70 mass% Si (silicon), 0.4-3.2 mass% Mn (manganese), and a total of 0.002-0.050 mass% P (phosphorus) and S (sulfur), with the remainder containing Fe (iron) and impurities. A steel material having such a chemical composition has high strength, and therefore can impart excellent strength to the laser welded joint.
[0025] [Weld metal] Weld metal is the part of the weld where steel materials are melted and solidified by irradiation with a laser beam during laser welding, and is the metal that melted and solidified during welding. When a filler is used during laser welding, the source of the weld metal material is the multiple steel materials being joined and the filler. Oxide scale is also a source of weld metal material. When the steel is plated, the components of the plating also melt and become the materials that make up the weld metal. In addition to the elements from these sources, oxygen and nitrogen from the air are absorbed into the weld metal, and unavoidable impurities may also be absorbed.
[0026] The weld metal that joins a plurality of steel materials, including high carbon steel materials and black-scaled steel materials, has an average C content of 0.24 mass% or more. If the average C content of the weld metal is 0.24 mass% or more, the occurrence of blowholes due to CO gas becomes noticeable.
[0027] The average Al content of the weld metal that joins a plurality of steel materials, including a high carbon steel material and a steel material with black scale, is 0.03 to 0.11 mass %. The average Ti content in the weld metal for joining a plurality of steel materials, including a high carbon steel material and a steel material with black scale, is 0.03 to 0.11 mass %.
[0028] Furthermore, the sum of the average Al content and the average Ti content of the weld metal joining a plurality of steel materials, including a high carbon steel material and a steel material with black scale, is 0.14 mass % or more.
[0029] Al (aluminum) and Ti (titanium) are elements that affect the deoxidation of weld metal. By keeping the average Al and Ti contents of the weld metal within the above ranges, it is possible to suppress the occurrence of blowholes in the weld metal and the decrease in strength of laser welded joints.
[0030] Of Al and Ti, when the weld metal contains only Al, a large amount of Al must be added to suppress blowholes that occur in the weld metal that joins multiple steel materials, including high carbon steel materials and black-scaled steel materials. As the hardenability of the weld metal decreases with increasing Al addition, if the amount of Al added is excessive, the hardenability decreases significantly, the hardness of the molten metal decreases, and the joint strength decreases. Similarly, when only Ti is contained in the weld metal, a large amount of Ti must be added to suppress blowholes that occur in the weld metal that joins multiple steel materials, including high carbon steel materials and black-scaled steel materials. Ti reacts with C in the weld metal to form Ti carbide, so if the amount of Ti added is excessive, the amount of C in the weld metal, which contributes to increasing the hardness of the weld metal, decreases significantly, and the joint strength decreases. In particular, when a welded joint contains a high-strength high-carbon steel material, the difference in hardness between the high-carbon steel material and the weld metal is large, and stress is concentrated in the weld metal, resulting in a significant decrease in joint strength.
[0031] The average carbon content of the weld metal is measured by taking chips from the inside of the weld metal at a depth of 0.3 mm or more from the surface, and measuring the chips using the well-known high-frequency combustion method (combustion-infrared absorption method). Chips are taken from three locations, and the arithmetic average of the measured values is taken as the average carbon content of the weld metal. The average Al and Ti contents of the weld metal are measured by taking chips from the inside of the weld metal at a depth of 0.3 mm or more from the surface, dissolving the chips in acid, and performing ICP analysis on the solution. Chips are taken from three locations, and the arithmetic average of the measured values is taken as the average Al content of the weld metal or the average Ti content of the weld metal, respectively.
[0032] It should be noted that weld metal can be distinguished from steel material by visual inspection. The surface of steel material is basically formed with few irregularities. On the other hand, since weld metal has been melted once, a wave pattern called ripples is often formed on its surface, and it is from such surface differences that weld metal and steel material can be distinguished.
[0033] In the laser welded joint of this embodiment, by containing both Al and Ti and setting the average Al content and average Ti content within the above ranges, the occurrence of blowholes in the weld metal and a decrease in strength of the laser welded joint can be suppressed.
[0034] The plurality of steel materials are base materials of the laser welded joint. The thickness of the steel materials at the portions to be joined by the weld metal is not particularly limited as long as it is suitable for laser welding, but in the laser welded joint of this embodiment, it is more preferable that the plate thickness of the high carbon steel material is 9.0 mm or less. By setting the plate thickness of the high carbon steel material to 9.0 mm or less, the oxygen concentration in the weld metal increases, and the effects of the laser welded joint of this embodiment described above become more pronounced.
[0035] There is no particular lower limit on the plate thickness of the high carbon steel material, but from the viewpoint of the mechanical properties of the member, the plate thickness of the high carbon steel material is preferably 2.0 mm or more.
[0036] (Example of laser welded joint) The shape of the laser welded joint of this embodiment will be exemplified below. In the example shown in Fig. 1 and Fig. 2, a steel plate is used as the steel material. Various forms of laser welded joints according to this embodiment are shown in Figures 1 and 2. However, the laser welded joints to which the present invention is applied are not limited to these examples, and the present invention can be applied to any shape of laser welded joint and its manufacturing method as long as the requirements of the present invention are met. Note that the X-, Y-, and Z-coordinate axes in Figures 1 and 2 are mutually orthogonal.
[0037] Laser welding generally has the problem that the width of the welded portion formed by the weld metal is narrow, making it difficult for oxygen mixed in the molten metal to escape, making blowholes prone to occur.
[0038] FIG. 1 is a schematic cut end view for explaining a lap laser welded joint in which at least a portion of the steel plates to be joined overlap each other. The cut surface of the laser welded joint 1 in FIG. 1 is a plane perpendicular to the extension direction of the weld metal (the traveling direction of the laser beam) and is parallel to the X- and Z-coordinate axes. The laser welded joint 1 shown in FIG. 1 includes a steel plate 11, a steel plate 12 overlapped on the steel plate 11, and a weld metal 20 formed across the plate thickness direction of the steel plate 11 and the steel plate 12. The steel plate 11 has one plate surface 11a and the other plate surface 11b, and the steel plate 12 has one plate surface 12a and the other plate surface 12b. In this example, the plate surface 11b of the steel plate 11 and the plate surface 12a of the steel plate 12 face each other.
[0039] Black scale (oxide scale) 13 is formed on the surfaces of sheet surfaces 12a and 12b of steel sheet 12. That is, in the laser welded joint of the present embodiment, steel sheet 11 is a high carbon steel sheet, steel sheet 12 is a steel sheet with black scale, and they are joined by weld metal 20. The steel plate 11 may be a steel plate with black scale, and the steel plate 12 may be a high carbon steel plate.
[0040] Also, the steel plate 11 may be a black-skinned steel plate and a high-carbon steel plate (a steel plate having an oxide scale with a thickness of 5 μm or more and a C content of 0.30 mass %), and the steel plate 12 may be another steel plate. Moreover, both the steel plate 11 and the steel plate 12 may be black-scaled steel plates and high-carbon steel plates.
[0041] The example in Fig. 1 is an example in which a laser beam is irradiated from the plate surface 11a side (positive side of the Z coordinate axis) of the steel plate 11 to form the weld metal 20. In the example in Fig. 1, the weld metal 20 is formed over the entire plate thickness direction of the steel plate 11 and the steel plate 12. However, the lap laser welded joint is not limited to the example in Fig. 1, and the weld metal 20 may be formed over the entire plate thickness direction of the steel plate 11, and the weld metal 20 may be formed from one plate surface 12a to one plate surface 12b of the steel plate 12 up to the middle of the plate thickness direction.
[0042] (T-shaped fillet laser welded joint) FIG. 2 is a schematic cross-sectional end view illustrating a fillet laser welded joint (also called a T-fillet welded joint) in which an end face of one steel plate is joined onto the plate face of another steel plate and a weld metal is formed at a corner formed by the plate faces of the steel plates. Steel plate 11 in Fig. 2 has one plate surface 11a and the other plate surface 11b, and steel plate 12 has one plate surface 12a and the other plate surface 12b. In laser welded joint 1 shown in Fig. 2, the plate surfaces of steel plate 11 and steel plate 12 are arranged perpendicular to each other, end surface 11A of steel plate 11 abuts plate surface 12a of steel plate 12, and weld metal 20 is formed at the corner formed by steel plate 11 and steel plate 12. The cut surface of laser welded joint 1 in Fig. 2 is a surface perpendicular to the extension direction of the weld metal (the traveling direction of the laser beam) and is parallel to the X coordinate axis and the Z coordinate axis.
[0043] The positional relationship between the surface of the steel plate 11 and the surface of the steel plate 12 is not limited to being vertical, and may be such that these surfaces intersect. In addition, the end surface of one steel plate may not abut the surface of the other steel plate, and a gap may be formed between these steel plates. The weld metal 20 may be formed over the entire length of the corner, or may be formed intermittently or partially along the corner. In addition, the end surfaces of the steel plates to be joined are not limited to being linear, and may have a predetermined shape required as a manufactured part. In addition, the surface of the steel plates to be joined is not limited to being flat, and may have partial irregularities, notches, etc.
[0044] In the above-mentioned T-shaped fillet welded joint, the steel plate 11 may be a high carbon steel plate and the steel plate 12 may be a black-skinned steel plate, or the steel plate 11 may be a black-skinned steel plate and the steel plate 12 may be a high carbon steel plate. Also, the steel plate 11 may be a black-skinned steel plate and a high-carbon steel plate (a steel plate having an oxide scale with a thickness of 5 μm or more and a C content of 0.30 mass %), and the steel plate 12 may be another steel plate. Moreover, both the steel plate 11 and the steel plate 12 may be black-scaled steel plates and high-carbon steel plates.
[0045] In the laser welded joint of this embodiment, it is more preferable that the laser welded joint is a T-fillet laser welded joint. As the Al content of laser weld metal increases, the viscosity of the molten metal decreases. However, by using T-shaped welding, the contact area between the surface of the steel plate and the molten weld metal increases, resulting in stable welding.
[0046] In the laser welded joint of this embodiment, when the laser welded joint is a T-fillet welded joint, it is more preferable that a high carbon steel material is butted against the surface of a steel material with black scale and joined. Alternatively, when the steel material with black scale and the high carbon steel material are the same steel material, it is more preferable that another steel material is butted against the surface of the same steel material and joined. That is, in the example of Fig. 2, it is preferable that the steel plate 11 is a high carbon steel plate and the steel plate 12 is a steel plate with black scale. Alternatively, it is preferable that the steel plate 12 is a steel plate with black scale and a high carbon steel plate, and the steel plate 11 is another steel plate. By butting the surface of the steel material with black scale with another steel material, the oxygen concentration in the weld metal becomes high, and the effect of the present invention becomes remarkable, which is preferable. In the example of Fig. 2, by making the steel plate 12 a steel material with black scale, the amount of oxygen supplied from the black scale (not shown) formed on the plate surface 12a of the steel plate 12 to the weld metal 20 increases.
[0047] In the above example, the width and length of the weld metal 20 formed by laser welding are not particularly limited, and may be designed appropriately to match the desired joint strength and the shape of the steel materials to be joined. In addition, the weld metal 20 is not limited to a linear shape, and may be curved or bent on the plate surface of the steel materials, for example.
[0048] Welds that contain weld metal formed by laser welding are characterized by a relatively narrow fusion width compared to the penetration depth, and can be distinguished from welds that have a wide surface fusion width such as arc welding. Specifically, if the penetration depth is 1.5 times or more the fusion width (the wider side if both the front and back surfaces are fused), it is considered to be a laser weld.
[0049] In the laser welded joint according to this embodiment, it is more preferable that the chemical composition of the weld metal joining the high carbon steel material and the black scale steel material is as follows, in mass %: C: 0.24 to 1.1% Silicon: 0.03 to 1.5% Mn: 0.4-3.5% Al: 0.03 to 0.11% Ti: 0.03 to 0.11% P: 0.1% or less S: 0.1% or less Cu:0.3 or less Remainder: Fe and impurities By having such a chemical composition, the laser welded joint according to this embodiment has the advantage that blowholes are suppressed and joint strength can be further ensured. Note that a weld metal other than the weld metal joining the high carbon steel material and the black scale steel material may have the above chemical composition.
[0050] [Method of manufacturing laser welded joints] A method for manufacturing the laser welded joint according to the present embodiment will be described below. This manufacturing method allows the laser welded joint according to the present embodiment to be suitably manufactured. However, it is self-evident that a laser welded joint obtained by a method other than the manufacturing method described below can be regarded as the laser welded joint according to the present embodiment as long as it satisfies the above-mentioned requirements.
[0051] The method for manufacturing a laser welded joint according to this embodiment is as follows: A process of preparing a plurality of steel materials (S1: preparation process); A process of arranging a plurality of steel materials (S2: arranging process); and a laser welding process (S3: laser welding process) for forming a weld metal for joining a plurality of steel materials.
[0052] In the preparation step, the steel materials to be joined are prepared. The thickness, chemical composition, and the like of the steel materials to be joined can be the same as those in the above-mentioned embodiment.
[0053] In the arrangement process, the steel materials prepared in the preparation process are arranged in predetermined positions. In the arrangement process, the steel materials are appropriately arranged so as to form the above-mentioned lap laser welded joint, T-shaped fillet laser welded joint, etc. according to the shape of the product to be manufactured.
[0054] In the laser welding process, the multiple steel materials arranged in the above-mentioned arrangement process are laser-welded. In the laser welding process, a laser beam is irradiated onto the steel materials to melt the multiple steel materials, and the molten metal solidifies between the multiple steel materials to form a weld metal, thereby joining the multiple steel materials together.
[0055] In the laser welding process, a filler is supplied and laser welding is performed to form a weld metal. The filler is, for example, a filler wire such as a solid wire or a flux-cored wire. In this embodiment, the weld metal is a part of the welded part, and refers to a metal that melts and solidifies during welding. Here, the "molten and solidified metal" refers to both a metal derived from the molten steel material (base material) and a metal derived from the molten filler. Therefore, the weld metal refers to a metal in which a part of the steel material and the filler are melted and mixed together.
[0056] When the filler contains Al and Ti as its chemical composition, the weld metal also contains Al and Ti derived from the filler. The chemical composition of the filler is preferably as follows: C: 0.02 to 0.35% Silicon: 0.005 to 2.000% Mn: 0.4-3.0% Al: 0.01 to 1.00% Ti: 0.01 to 1.00%
[0057] The laser beam conditions are not particularly limited, but it is preferable to use a commonly used solid-state laser such as a CO2 laser, fiber laser, or disk laser. A semiconductor laser may also be used. From the viewpoint of productivity, the welding speed is preferably 2 m / min or more. For the shielding gas, helium is preferably used for the CO2 laser. For the solid-state laser or semiconductor laser, argon or air is preferably used, but it is not necessary to use it. The laser output is preferably in the range of 2 to 30 kW.
[0058] When manufacturing a joint containing high carbon and black-scaled steel materials by laser welding, there has been a problem in that blowholes due to CO gas are likely to occur. However, according to the laser-welded joint and its manufacturing method of the above embodiment, it is possible to suppress the occurrence of blowholes while ensuring joint strength.
[0059] The laser welded joint according to the above embodiment can be preferably used for automobile parts. Examples of automobile parts to which the laser welded joint according to the above embodiment can be applied include A-pillars, B-pillars, roof rails, side sills, floor cross members, bumpers, crash boxes, instrument panel reinforcements, seat frames, battery cases, ladder frames, etc. In particular, the laser welded joint and the manufacturing method thereof according to the above embodiment make it possible to manufacture automobile, bus, and truck components having laser welds with reduced blowholes. EXAMPLES
[0060] The present invention will be specifically described below by way of examples, but the present invention is not limited thereto.
[0061] Steel plates BM1 to BM9 were prepared with the chemical compositions (balance including Fe and impurities) shown in Table 1. In the following table, conditions that do not satisfy the requirements of the present invention are underlined.
[0062] Laser welding was performed while supplying filler wires WI1 to WI6 shown in Table 2, and laser welded joints were produced by welding two steel plates in the combinations shown in Table 3. Specifically, laser welding was performed using the combinations of steel plates shown in Table 3, with steel plate 1 and steel plate 2 positioned to obtain the weld shape shown in Table 3. In the case of T-shaped fillet welding, steel plate 1 was set as the flange side and steel plate 2 was set as the web side, and welding was performed by butting the end face of steel plate 2 against the surface of steel plate 1.
[0063] The laser welding conditions were as follows: Welding speed: 3m / min Wire feed speed: Adjusted to achieve the desired dilution ratio. -Butt gap: Adjusted according to the wire feed rate. Laser output: Adjusted to +0.25kW, which is the output that penetrates to the back surface. Shielding gas: Ar (argon)
[0064] [Table 1]
[0065] [Table 2]
[0066] [Table 3]
[0067] The dilution ratio was the ratio of the volume of the inserted wire to the volume of the weld metal. In other words, the dilution ratio indicates the ratio of the volume of the wire to the volume of the weld metal. Taking into account the gaps between the steel materials during welding, the cross-sectional shape of the weld metal was considered to be filled with wire except for the part of the base steel material, and this ratio was calculated to be the dilution ratio.
[0068] The composition of the weld metal of each laser welded joint shown in Table 3 was measured as follows. The average C content of the weld metal was measured by collecting chips from inside the weld metal at a depth of 0.3 mm or more from the surface, and the collected chips were measured using the well-known high-frequency combustion method (combustion-infrared absorption method). Chips were collected from three locations, and the arithmetic average of the respective measured values was taken as the average C content of the weld metal. The average Al content and average Ti content of the weld metal were measured by collecting chips from inside the weld metal at a depth of 0.3 mm or more from the surface, and dissolving the collected chips in acid, and then performing ICP analysis on the solution. Chips were collected from three locations, and the arithmetic average of the respective measured values was taken as the average Al content of the weld metal or the average Ti content of the weld metal, respectively.
[0069] (Blowhole evaluation) A blowhole evaluation test was carried out for each laser welded joint. Specifically, an X-ray transmission test was conducted to check for the presence or absence of blowholes. The BH occupancy rate was determined as the ratio of the length of the area where blowholes existed to the total length of the weld line. If the BH occupancy rate was 30% or less, it was rated as ○ (Good), and if it was over 30%, it was rated as × (Bad). These results are shown in Table 3. In Table 3, the BH occupancy rate is shown in parentheses.
[0070] (Measurement of strength) Each laser welded joint was heat-treated to reduce the base material hardness to about 500HV, since cracks may occur especially in welds with a high carbon content. The welds were then cut to a width of 30mm to create T-shaped tensile test pieces as shown in Figure 2 and butt tensile test pieces as shown in Figure 3. Tensile tests were conducted on these test pieces. The joint strength was calculated by dividing the maximum load (N) by the plate thickness x plate width (30mm), and a joint strength of 1650MPa or more was rated as ○ (Good), and a joint strength of less than 1650MPa was rated as × (Bad). The results are shown in Table 3.
[0071] (Paint adhesion) For paint adhesion, the electrodeposition-coated test pieces were subjected to the cross-cut test specified in JIS K5600 to evaluate the degree of paint peeling. If the surface condition of the cross-cut area was classified as 0 to 2 in JIS K5600, it was rated as ○ (Good), and if it was classified as 3 to 5, it was rated as × (Bad). The results are shown in Table 3.
[0072] As can be seen from the results in Table 3, the laser welded joint according to the present invention was able to suppress the occurrence of blowholes while ensuring joint strength.
[0073] In Nos. 1 to 21, the same steel plates were T-fillet welded. In Nos. 22 to 25, steel plates with different oxide scale thicknesses were T-fillet welded. In Nos. 26 to 30, the steel plates were butt welded.
[0074] In Comparative Examples 1 and 2, since low carbon steel material was used, the problem of blowholes did not occur, but the joint strength decreased. In Comparative Examples 3 to 7 and 15 to 17, the total average Al content and average Ti content was small, so blowholes occurred and the joint strength decreased. In Comparative Examples 8 to 14 and 18, the average Al content and the average Ti content were excessive, so the weld metal softened and the joint strength decreased.
[0075] In contrast, in the example of the laser welded joint according to the present invention, the occurrence of blowholes could be suppressed while ensuring the joint strength. [Industrial Applicability]
[0076] INDUSTRIAL APPLICABILITY The laser welded joint and the manufacturing method thereof according to the present invention can suppress the occurrence of blowholes while ensuring joint strength, and are therefore extremely useful industrially. [Explanation of symbols]
[0077] 1 Laser welded joints 11, 12 Steel plate (steel material) 13 Black scale (oxidized scale) 20 Welding metal
Claims
1. A laser welded joint comprising a plurality of steel materials and a weld metal that joins the plurality of steel materials, At least one of the plurality of steel materials is a high carbon steel material having a C content of 0.30 mass% or more, At least one of the plurality of steel materials is a black-skinned steel material having an oxide scale having a thickness of 5 μm or more; The weld metal has an average C content of 0.24 mass% or more, an average Al content of 0.03 to 0.11 mass%, and an average Ti content of 0.03 to 0.11 mass%, The sum of the average Al content and the average Ti content of the weld metal is 0.14 mass% or more. Laser welded joints.
2. The thickness of the oxide scale is 20 μm or less. The laser welded joint of claim 1.
3. The plate thickness of the high carbon steel material is 9.0 mm or less. The laser welded joint of claim 1.
4. The laser welded joint is a T-fillet laser welded joint.
4. The laser welded joint according to claim 1 .
5. The black-scaled steel material and the high-carbon steel material are the same steel material, and at least one of the plurality of steel materials is butt-joined to a surface of the same steel material. The laser welded joint of claim 4.
6. The high carbon steel material is butt-joined to the surface of the black-scaled steel material. The laser welded joint of claim 4.
7. A method for manufacturing a laser welded joint including a laser welding process for forming a weld metal for joining a plurality of steel materials, In the laser welding step, a filler is supplied and laser welding is performed; At least one of the plurality of steel materials is a high carbon steel material having a C content of 0.30 mass% or more, At least one of the plurality of steel materials is a black-skinned steel material having an oxide scale having a thickness of 5 μm or more; The weld metal has an average C content of 0.24 mass% or more, an average Al content of 0.03 to 0.11 mass%, and an average Ti content of 0.03 to 0.11 mass%, The sum of the average Al content and the average Ti content of the weld metal is 0.14 mass% or more. A method for manufacturing laser welded joints.
Citation Information
Patent Citations
Butt laser beam welding method for high carbon steel sheet
JP1992237584A
Pretreatment method for laser melding
JP1994079485A
Laser welded joint and method for producing the same
JP2002239763A
Continuous hot rolling method
JP3304982B2
Cutting assembly and method for manufacturing same
US20190210150A1