Structural coating agent and infrared measurement system

The coating agent with curable resin and infrared-detectable metal powder addresses the inaccuracies and labor issues in structural inspections by enabling precise damage detection using infrared imaging, enhancing durability and safety in infrastructure monitoring.

JP2024161712AInactive Publication Date: 2024-11-20AKITA PREFECTURAL UNIVERSITY +1

Patent Information

Application Number
JP2023076659
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-20
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for inspecting the health of structures such as buildings and infrastructure are inaccurate, labor-intensive, and pose safety risks to workers, especially with declining workforce availability, and lack automation for large-scale, unmanned inspections.

Method used

A coating agent for structures containing a curable resin composition and metal powder detectable by infrared radiation, which forms a gel-like or elastomer-like cured product, allowing for precise damage detection using infrared imaging with robots or drones.

Benefits of technology

Enables accurate, efficient, and unmanned detection of structural damage, improving durability and safety while reducing labor requirements, and facilitating large-scale inspections of infrastructure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161712000002
    Figure 2024161712000002
  • Figure 2024161712000003
    Figure 2024161712000003
  • Figure 2024161712000004
    Figure 2024161712000004
Patent Text Reader

Abstract

To provide a structural coating agent that can detect damage such as cracks inside a structure composed of concrete or the like in a more simplified and accurate manner, and can also improve the durability of the structure.SOLUTION: A structural coating agent includes a curable resin composition and metal powder detectable by external rays.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating agent for structures and an infrared measurement system. [Background technology]

[0002] Many buildings, bridges, tunnels, and other structures and infrastructure (hereafter collectively referred to as "structures") have been in existence for several decades, and it is expected that the deterioration of these structures will continue to progress in the future. Therefore, the development of monitoring technology to confirm or evaluate the soundness of structures is of great social importance. Conventionally, inspection methods for evaluating the soundness of structures and determining the need for repairs have included percussion testing in which an operator diagnoses the scraping sound of a test hammer by hearing it, acoustic testing, and visual inspection to determine, for example, the risk of peeling off wall tiles. However, percussion inspection and visual inspection have problems such as variation in inspection accuracy depending on whether the worker has many years of experience or not, noise around the structure, etc. Also, ensuring the safety of workers can be an issue depending on the environment around the structure. Furthermore, with changes in social structure, including a declining birthrate and an aging population, it is predicted that it will become increasingly difficult to secure sufficient personnel to carry out inspections and to manufacture and construct structures.

[0003] Patent Document 1 discloses a polymerizable fluorescent sealing agent that contains a phosphor, a silicone oligomer or a mixture of a silicone oligomer and an oligoester acrylate, and a polymerization initiator. Moreover, Patent Document 2 discloses a concrete crack repair material that is characterized by the incorporation of an aqueous cesium carbonate solution that has X-ray contrast properties. Thus, it is known to detect cracks in structures using phosphors or X-ray contrast agents in order to evaluate the need for repairs to the structures. However, these methods cannot be performed unmanned, easily, and with high accuracy. In addition, they are not widespread as a technology for unmanned inspection of a large number of widely installed structures using AI or the like. This is because there are still issues such as cost, work time, and manpower shortages when implementing them in the maintenance management of structures such as roads, railways, bridges, tunnels, low-rise and high-rise buildings, wind turbines, levees, dams, and pipelines.

[0004] Given this background, automation and labor-saving are considered to be essential technological elements in managing the soundness of structures, not only from the perspective of improving inspection accuracy, but also from the perspective of the sustainability of society as a whole in the future. In particular, technology that can handle inspections using wall inspection robots and drones is required from the perspective of social implementation. In addition to developing technology to monitor the health of structures, there is also a strong demand for extending the lifespan and improving the durability of the structures themselves. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-219869 A [Patent Document 2] Japanese Patent Application Publication No. 7-139190 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention provides a coating agent for structures that can more easily and accurately detect damage such as cracks inside structures made of concrete, etc. The present invention also provides a coating agent for structures that can improve the durability of the structures. Furthermore, the present invention also provides a structure including a cured product formed by applying the coating agent for structures, a method for detecting damage to a structure, and a system for monitoring the soundness of a structure. [Means for solving the problem]

[0007] More specifically, the present invention provides the following aspects. [1] a curable resin composition, A metal powder detectable by infrared light; A coating agent for a structure comprising: [2] The coating agent according to [1], wherein the metal powder comprises one or more metal powders selected from the group consisting of aluminum, gold, silver, copper, nickel, cobalt, chromium, platinum, tin and iron. [3] The coating agent according to [1] or [2], wherein the metal powder comprises aluminum powder. [4] The coating agent according to any one of [1] to [3], wherein the average primary particle diameter of the metal powder, as measured by a laser diffraction / scattering method, is in the range of 5 to 50 μm. [5] The coating agent according to any one of [1] to [4], wherein the coating agent contains the metal powder in an amount of 0.1 to 10 mass % based on the total amount of the coating agent. [6] The coating agent according to any one of [1] to [5], wherein the curable resin composition forms a gel-like or elastomeric cured product upon curing. [7] The coating agent according to any one of [1] to [6], wherein the curable resin composition forms a gel-like cured product having a 1 / 4 consistency defined in JIS K 2220 in the range of 10 to 150 upon curing. [8] The coating agent according to any one of [1] to [6], wherein the curable resin composition forms an elastomeric cured product having a JIS A hardness in the range of 20 to 90 upon curing. [9] The coating agent according to any one of [1] to [8], wherein the curable resin composition comprises at least one selected from the group consisting of a curable silicone resin composition and a curable urethane resin composition.

[10] The coating agent according to any one of [1] to [9], wherein the curable resin composition comprises a curable silicone resin composition.

[11] The curable silicone resin composition, (A) an organopolysiloxane having at least two curing reactive groups in one molecule; (B) optionally, an organohydrogenpolysiloxane; (C) Hardener The coating agent according to [9] or

[10] ,

[12] The coating agent according to any one of [9] to

[11] , wherein the curable silicone resin composition is cured by one or more curing reactions selected from the group consisting of a hydrosilylation curing reaction, a condensation curing reaction, a peroxide curing reaction, a photocuring reaction, and a high-energy ray curing reaction.

[13] The coating agent according to any one of [1] to

[12] , which is used for detecting damage to a structure.

[14] The coating agent according to

[13] , wherein the detection is performed by infrared irradiation.

[15] A curable resin composition, A metal powder detectable by infrared light; A structure comprising a cured product formed by applying a coating agent for structures comprising the above-mentioned.

[16] applying a coating agent for a structure to an exterior surface of the structure, the coating agent including an infrared-detectable metal powder dispersed in a curable resin composition; and imaging the exterior surface of the structure with infrared illumination; A method for detecting damage to a structure, comprising:

[17] The method according to

[16] , wherein the imaging is performed using a fixed or movable infrared camera.

[18] The method of

[16] or

[17] , wherein the imaging is performed using a wired or wirelessly operated robot or drone, or an automated robot or drone.

[19] The method according to any one of

[16] to

[18] , further comprising analyzing the image obtained by imaging by Fourier transform.

[20] The method according to

[19] , wherein the analysis is performed to analyze one or more conditions selected from the group consisting of the presence or absence of damage to the structure, the shape of the damage, the size of the damage, and the depth of the damage.

[21] A structure having an outer surface covered with a cured product of the coating agent for structures according to any one of [1] to

[14] . Imaging means for imaging the exterior surface of the structure by infrared irradiation; and A determination means for determining whether or not the structure is damaged by analyzing the image obtained by the imaging is provided. Structural health monitoring system.

[22] Furthermore, A receiving means for receiving image information and / or a result of determining whether or not the structure is damaged; and A display means for displaying image information and / or a result of a determination of the presence or absence of damage to the structure; Equipped with The system described in

[21] .

[23] The imaging means, A wired or wireless communication means for transmitting image information and position information of the captured structure; and A storage means for storing image information and position information of the captured structure, When the determination means determines that there is damage to the structure, the display means displays position information of the structure in which the damage has been detected and / or a damaged area in the structure in which the damage has been detected.

[22] The system described in.

[24] The system described in any one of

[21] to

[23] , wherein the imaging means is a robot or drone equipped with an infrared camera.

[25] The system described in any one of

[21] to

[24] , wherein the judgment means is automated by an analysis means that detects damage to the structure by automatically comparing the learning results obtained by machine learning based on imaging data previously obtained using a similar method with the images obtained by the imaging means.

[26] The system described in any one of

[21] to

[25] , wherein the determination means includes image analysis means for analyzing the image obtained by the imaging means by Fourier transform.

[27] The system described in

[26] , wherein the image analysis means analyzes one or more conditions selected from the group consisting of the presence or absence of damage to the structure, the shape of the damage, the size of the damage, and the depth of the damage.

[28] The structure described in

[15] , the method described in any one of

[16] to

[20] , or the system described in any one of

[21] to

[28] , wherein the structure comprises one or more types of infrastructure selected from the group consisting of roads, railways, bridges, tunnels, low-rise or high-rise buildings, wind turbines, embankments, dams and pipelines. Effect of the Invention

[0008] According to one aspect of the present invention, a coating agent for structures can be provided that can more easily and accurately detect damage such as cracks inside a structure made of concrete or the like. According to another aspect of the present invention, a coating agent for structures that can improve the durability of the structure can also be provided. Furthermore, according to another aspect of the present invention, a structure including a hardened product formed by applying the coating agent for structures, a method for detecting damage to a structure, and a monitoring system for the soundness of a structure can also be provided. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic diagram of the structure of a test specimen used in the examples. [Diagram 2] FIG. 2 is a photograph or a schematic diagram of test specimens A, B and C used in the examples. [Diagram 3]FIG. 3 shows photographs of the pressure tester, test specimen, infrared camera, and visible light camera used in the examples. [Figure 4] FIG. 4 is a graph showing the results of thermal image analysis by passive measurement. [Diagram 5] FIG. 5 shows images of specimen B after the destructive test taken with an infrared camera and a visible light camera. [Figure 6] FIG. 6 shows a schematic diagram of the equipment used to evaluate the relationship between strain and heat generation in reinforcing bars and a conceptual diagram of the test system. [Figure 7] FIG. 7 is a graph showing the relationship between the strain inside the test piece and the heat generated by the reinforcing bar during the destructive test, as well as the measurement results of the pressure, strain on the surface of the test piece, and temperature. [Figure 8] FIG. 8 is a conceptual diagram of a structural health monitoring system according to one embodiment of the present invention. [Figure 9] FIG. 9 is a functional block diagram of a structural health monitoring system according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The upper and lower limit values ​​of the numerical ranges described in this specification can be arbitrarily combined. For example, when the numerical range is described as "preferably 30 to 100, more preferably 40 to 80", the ranges "30 to 80" and "40 to 100" are also included in the numerical ranges described in this specification. In addition, when the numerical range is described as "preferably 30 or more, more preferably 40 or more, and preferably 100 or less, more preferably 80 or less", the ranges "30 to 80" and "40 to 100" are also included in the numerical ranges described in this specification. In addition, as a numerical range described in this specification, for example, "60 to 100" means a range of "60 or more and 100 or less."

[0011] 1. Coating agents for structures The present invention provides a coating agent for structures (coating composition for structures). The coating agent for structures of the present invention includes a curable resin composition and a metal powder detectable by infrared rays (hereinafter, also referred to as "metal powder"). The coating agent for structures according to one aspect of the present invention is used for detecting damage to a structure. The coating agent for structures according to one aspect of the present invention performs the detection by irradiating infrared rays. In this specification, a "structure" may be any structure having a joint, including, but not limited to, infrastructure such as roads, railways, bridges, tunnels, low-rise or high-rise buildings, wind turbines, levees, dams, and pipelines. Note that structures include both civil engineering structures and architectural structures, and the present invention is applicable to both of them. In this specification, "damage to a structure" includes any defect in a structure, including, but not limited to, cracks such as fissures, crevices, and fissures, float or peeling, spalling, defects, corrosion, and the like that occur inside or outside the structure.

[0012] 1.1 Curable resin composition The curable resin composition used in the present invention can be applied (coated) in a liquid state, and can form a cured layer made of the cured product on the surface of a structure by curing. The curable resin composition also functions as a binder for metal powder, which will be described later. The curable resin composition of one embodiment of the present invention forms a gel-like or elastomer-like cured product by curing. By using a curable resin composition having such properties, a cured layer is formed on the surface of a structure, and the strength and durability of the structure itself can be effectively improved. In addition, there are practical benefits such as improving the repairability of the structure and preventing the structure surface from peeling and falling off. In particular, a gel-like cured product (for example, a low crosslinking density organopolysiloxane cured product described later) is particularly suitable because it has excellent heat resistance, weather resistance, oil resistance, cold resistance, and electrical insulation, and has a low elastic modulus and low stress. In this specification, the term "gel-like" refers to a material that can be measured for 1 / 4 consistency as specified in JIS K 2220 and has a modulus of 10 3 ~10 5 The hardened product has a hardness in the range of Pa. In addition, in this specification, "elastomeric" refers to the form of a cured product whose JIS A hardness is measurable or whose hardness exceeds the upper limit of JIS A hardness measurement, and includes, for example, a cured product whose JIS D hardness is measurable. Furthermore, by using a curable resin composition that becomes gel-like or elastomeric upon curing, when damage such as cracks occurs in a structure, the gel-like or elastomeric resin or liquid resin component penetrates the damaged area or enters the broken area under its own weight to fill the voids in the damaged area, and it is possible to prevent the intrusion of rainwater, etc., even in damage that occurs after coating. This brings about the effects of suppressing deterioration of the structure and preventing corrosion of reinforcing bars (including lifting of reinforcing bars) inside the structure. Furthermore, by using a curable resin composition that becomes gel-like or elastomer-like upon curing, when imaging is performed using an infrared camera as described below, a step of heating or temperature control in advance of the location to be imaged can be omitted. This is due to the heat retention effect of the gel or elastomer. That is, for example, the curable resin composition of one embodiment of the present invention can retain heat from the wall surface of a structure that has been heated by sunlight or the like, and therefore imaging can be performed using an infrared camera without prior heating. In this way, the curable resin composition of one embodiment of the present invention has advantages in terms of preventing deterioration of a structure, improving the efficiency of imaging using an infrared camera, and the like. The coating layer obtained by using the curable resin composition has not only a heat-retaining effect but also a cold-retaining effect in that it blocks internal heat. For example, when the curable resin composition is applied to the wall surface of a building, it prevents the diffusion of heat from air conditioning and heating, thereby secondarily improving the energy-saving effect.

[0013] The gel-like cured product formed by the curable resin composition according to one embodiment of the present invention preferably has a 1 / 4 consistency defined in JIS K 2220 in the range of 10 to 150. The 1 / 4 consistency may be in the range of 10 to 130, 20 to 130, or 20 to 100. The elastomeric cured product formed from the curable resin composition according to one embodiment of the present invention preferably has a JIS A hardness in the range of 20 to 90. The hardness may be in the range of 20 to 80, 20 to 60, or 20 to 40.

[0014] A curable resin composition according to one embodiment of the present invention includes at least one selected from the group consisting of a curable silicone resin composition and a curable urethane resin composition. Hereinafter, the curable silicone resin composition and the curable urethane resin composition, which are one embodiment of the curable resin composition of the present invention, will be described in detail.

[0015] 1.1.1 Curable silicone resin composition The curable resin composition according to one embodiment of the present invention includes a curable silicone resin composition. The curable silicone resin composition may be a single type, or may be a mixture of two or more types in any ratio. The curable silicone resin composition may be a mixture of different curing systems in any ratio. By using two or more types of resins with different curing systems in combination, a cured product (including a semi-cured state) can be provided by not only one-stage curing but also two or more stages of time-dependent curing reaction.

[0016] The curable silicone resin composition of one embodiment of the present invention may contain at least one non-curable siloxane polymer, and the non-curable siloxane polymer may have a viscosity or plasticity in the range of 1 to 1,000,000 mPa·s at 25°C (viscosity exceeds 10,000,000 mPa·s), preferably in the range of 10 to 10,000 mPa·s, more preferably in the range of 100 to 5,000 mPa·s, and even more preferably in the range of 500 to 3,000 mPa·s. The non-curable siloxane polymer may be, for example, a dimethylpolysiloxane having a trimethylsiloxy end or a silanol end. In this specification, the viscosity (mPa·s) means a value measured using a rotational viscometer conforming to JIS K7117-1 at room temperature (25°C). Similarly, the plasticity refers to a value measured in accordance with the method specified in JIS K 6249 (a thickness is measured to the nearest 1 / 100 mm when a load of 1 kgf is applied to a 4.2 g spherical sample at 25°C for 3 minutes, and this value is multiplied by 100). In the present invention, a raw rubber-like non-curable siloxane polymer having a plasticity in the range of 50 to 200 may be used.

[0017] The curable silicone resin composition according to one embodiment of the present invention may be a one-liquid type package, or may be a multi-component (multi-liquid) type curable silicone resin composition in which the base agent and the crosslinking agent / curing agent components are separated into two or more packages. For example, the curable silicone resin composition used in one embodiment of the present invention is a DOWSIL TM It may be CY 52-276 gel (A&B).

[0018] In addition, from the viewpoint of preventing deterioration of the hardness, strength and durability over time, preventing environmental pollution, and preventing contact failure of electrical equipment used in the vicinity, the curable silicone resin composition of one embodiment of the present invention may have volatile low molecular weight components (low molecular weight siloxane oligomers such as M4Q structures and volatile cyclic siloxanes) removed from each constituent raw material or from the entire composition. The degree of removal is arbitrary, but if the mass loss rate when the curable silicone resin composition or its constituent components excluding the curing agent is exposed to high temperature (e.g., 200°C) for 1 hour is less than 5% by mass, preferably less than 2% by mass, the volatile siloxane oligomers are mostly removed.

[0019] The curable silicone resin composition of one embodiment of the present invention may have a viscosity at 25°C in the range of 100 to 20,000 mPa·s, preferably in the range of 200 to 4,500 mPa·s, and more preferably in the range of 300 to 4,000 mPa·s. The viscosity range of the entire composition can be designed by selecting the type of each component and their contents and / or content ratios, etc. In particular, the overall viscosity of the coating agent for structures according to the present invention can be designed by the contents of the curable resin composition and metal powder, etc.

[0020] The curable silicone resin composition according to one embodiment of the present invention has a storage modulus of 10 at 25° C. 3 ~10 6 The range may be 10 Pa, preferably 10 3 ~10 5 The range is Pa.

[0021] As described above, a gel-like cured product (for example, a low crosslink density organopolysiloxane cured product) is particularly suitable because it has excellent heat resistance, weather resistance, oil resistance, cold resistance, and electrical insulation, and has a low elastic modulus and low stress. In general, a gel-like cured product (hereinafter, sometimes referred to as "silicone gel") is an organopolysiloxane crosslinked product with a relatively low crosslink density, and from the viewpoint of flexibility, low elastic modulus, low stress, and stress buffering properties required of a gel, the loss factor tan δ of the silicone gel (measured with a viscoelasticity measuring device at a frequency of 0.1 Hz) may be in the range of 0.01 to 1.00 at 23°C to 100°C, or may be in the range of 0.03 to 0.95, 0.10 to 0.90, etc. at 23°C.

[0022] The composition of the curable silicone resin composition of one embodiment of the present invention is not particularly limited, but may, for example, contain an organopolysiloxane having a curing reactive group as a main component, and optionally a crosslinker (e.g., an organohydrogenpolysiloxane) and a curing agent depending on the curing system. (A) an organopolysiloxane having at least two curing reactive groups in one molecule; (B) optionally, an organohydrogenpolysiloxane; (C) Hardener The present invention relates to a method for producing a semiconductor device comprising the steps of:

[0023] The curing reaction mechanism of the curable silicone resin composition of one embodiment of the present invention is not particularly limited, but examples thereof include a hydrosilylation reaction curing type between an alkenyl group and a silicon-bonded hydrogen atom, a condensation reaction curing type such as a dehydration condensation reaction curing type and a dealcoholization condensation reaction curing type between a silanol group and / or a silicon-bonded alkoxy group, a peroxide reaction curing type using an organic peroxide, a photoreaction curing type by ultraviolet irradiation, and a high-energy ray reaction curing type (radical reaction curing type) by irradiating a mercapto group or the like with high-energy rays. These curing reactions proceed by heating, irradiation with high-energy rays, or a combination of these. Among these, the hydrosilylation reaction curing type, the peroxide reaction curing type, the high-energy ray reaction curing type, and combinations of these are preferred, as they cure relatively quickly throughout and the reaction can be easily controlled, and at least the hydrosilylation reaction curing type is more preferred.

[0024] When the curing reaction is a hydrosilylation curing reaction, the curing reactive group contains at least an alkenyl group, and preferably contains an alkenyl group having 2 to 10 carbon atoms. Examples of the alkenyl group having 2 to 10 carbon atoms include a vinyl group, an allyl group, a butenyl group, and a hexenyl group. The alkenyl group having 2 to 10 carbon atoms is preferably a vinyl group.

[0025] Similarly, when the curing reaction is a hydrosilylation curing reaction, the curable silicone resin composition preferably contains an organohydrogenpolysiloxane having two or more Si-H bonds in the molecule as a crosslinking agent.In this case, the alkenyl group of the organohydrogenpolysiloxane can undergo hydrosilylation reaction with the silicon-bonded hydrogen atom of the organohydrogenpolysiloxane to form a cured product.At that time, it is necessary to use a hydrosilylation reaction catalyst described later.

[0026] In one embodiment of the present invention, the curing reaction is preferably carried out at a low temperature, for example, at 100° C. or less, preferably at 80° C. or less, and more preferably at 70° C. or less. When the curing reaction is a hydrosilylation curing reaction, high-energy radiation using a photoactive platinum complex curing catalyst or the like may be used, or the curing reaction may not proceed sufficiently at a low temperature, resulting in the formation of a gel-like cured product with a low crosslinking density.

[0027] When the curing reaction is a dehydration condensation reaction curing type or a dealcoholization condensation reaction curing type, the curing reactive group includes a silanol group (Si-OH) or a silicon atom-bonded alkoxy group. Suitable examples of the alkoxy group include alkoxy groups having 1 to 10 carbon atoms, such as a methoxy group, an ethoxy group, and a propoxy group. The alkoxy group may be bonded to a side chain or an end of the organopolysiloxane, or may be in the form of an alkylalkoxysilyl group or an alkoxysilyl group-containing group bonded to a silicon atom via another functional group. Furthermore, the organopolysiloxane having the curing reactive group may have, in addition to the dehydration condensation reaction curing type or dealcoholization condensation reaction curing type functional group, a curing reactive group based on another curing mechanism in the same molecule. For example, the organopolysiloxane may have, in addition to a silicon-bonded alkoxy group or silanol group, a hydrosilylation reactive functional group or a photopolymerizable functional group in the same molecule. In addition, since a curing-reactive functional group is not required in a peroxide curing reaction, a dehydration condensation reaction curing type or dealcoholization condensation reaction curing type curable silicone resin composition containing an organic peroxide may be used to form a gel-like cured product by a condensation reaction, and the cured product may be further secondary-cured with another curing agent such as an organic peroxide by heating or the like.

[0028] In particular, when a silicon-bonded alkoxy group is selected as the curing reactive group, the curing reactive group is preferably an alkoxysilyl group-containing group represented by the following general formula: [ka] In the formula, R 1 each independently represents the same or different monovalent hydrocarbon group having no aliphatic unsaturated bonds, and is preferably a methyl group or a phenyl group. R 2 each independently represents an alkyl group and is preferably a methyl group, an ethyl group, or a propyl group since it constitutes an alkoxy group reactive to dealcoholization condensation. R 3each independently represents an alkylene group bonded to a silicon atom, and preferably an alkylene group having 2 to 8 carbon atoms. a represents an integer of 0 to 2, and p represents an integer of 1 to 50. From the viewpoint of dealcoholization condensation reactivity, a is preferably 0, and the group is preferably a trialkoxysilyl group-containing group. In addition to the above alkoxysilyl group-containing group, the same molecule may contain a hydrosilylation reactive functional group or a photopolymerization reactive functional group.

[0029] When the curing reaction is a dehydration condensation reaction curing type or a dealcoholization condensation reaction curing type, the above-mentioned crosslinking agent is not necessary. However, for example, in order to cause the curing reaction to proceed in multiple stages, the curable silicone resin composition of one embodiment may contain an organohydrogenpolysiloxane.

[0030] In the case of dehydration condensation reaction curing type or dealcoholization condensation reaction curing type, it is preferable to use a condensation reaction catalyst as a curing agent.The condensation reaction catalyst is not particularly limited, but may be, for example, dibutyltin dilaurate, dibutyltin diacetate, tin octenate, dibutyltin dioctate, tin laurate, and other organic tin compounds; tetrabutyl titanate, tetrapropyl titanate, dibutoxybis(ethylacetoacetate), and other organic titanium compounds; other acidic compounds such as hydrochloric acid, sulfuric acid, and dodecylbenzenesulfonic acid; alkaline compounds such as ammonia and sodium hydroxide; and amine compounds such as 1,8-diazabicyclo[5.4.0]undecene (DBU), 1,4-diazabicyclo[2.2.2]octane (DABCO).

[0031] When the curing reaction is a peroxide curing reaction, the curing reactive group may be any functional group that is radically reactive with peroxide, and any peroxide curing reactive functional group such as an alkyl group, an alkenyl group, an acrylic group, a hydroxyl group, etc. may be used without limitation. However, since a peroxide curing reaction generally proceeds at a high temperature of 150° C. or higher, it is preferable to apply the method to a structure that can be cured at a high temperature.

[0032] When the curing reaction is a radical reaction curing type by irradiation with high energy rays, the above curing reactive group is a photopolymerizable functional group, and may be a mercaptoalkyl group such as a 3-mercaptopropyl group, an alkenyl group similar to that described in the hydrosilylation curing reaction, or an acrylamide group such as N-methylacrylamidopropyl. Here, the conditions for irradiating with high energy rays are not particularly limited, and examples include a method in which the curable silicone resin composition is irradiated at room temperature (e.g., 20 to 25°C) while cooling or heated to 50 to 150°C in air, in an inert gas such as nitrogen gas, argon gas, or helium gas, or in a vacuum. Among these, irradiation in air and at room temperature is preferred. Furthermore, some photopolymerizable functional groups can cause poor curing when exposed to air, and therefore, when irradiating high-energy rays, the surface of the curable silicone resin composition may optionally be covered with a synthetic resin film or the like that is transparent to high-energy rays. Here, when the curable silicone resin composition is cured at room temperature using ultraviolet light having a wavelength of 280 to 450 nm, preferably 350 to 400 nm, the cured product layer may have other curing systems involving heating, particularly the curing reactive groups and curing agents of the hydrosilylation curing reaction or the peroxide curing reaction, remaining unreacted. In this case, by selecting a heat curing reaction as the secondary curing reaction, there is an advantage that the coating agent for structures according to one embodiment of the present invention can be rapidly cured in multiple stages.

[0033] A cured product of the curable silicone resin composition according to one embodiment of the present invention is (A) the organopolysiloxane having the above-mentioned curing reactive group, (B) optionally, an organohydrogenpolysiloxane depending on the cure reaction, and (C) Hardener The silicone resin composition is formed from a curable silicone resin composition containing When the curing reaction is a hydrosilylation curing reaction, the content of each component in the curable silicone resin composition is such that, when the total amount of alkenyl groups in component (A) in the composition is taken as 1 mole, the amount of silicon-bonded hydrogen atoms in component (B) is preferably 0.25 moles or more, and more preferably 0.26 moles or more.

[0034] In addition, when the curing reaction for forming the cured product according to one embodiment of the present invention includes a hydrosilylation curing reaction, the curable silicone resin composition is (A-1) a linear organopolysiloxane having at least two curing reactive groups in one molecule, and (A-2) A resinous or branched organopolysiloxane having at least two curing reactive groups in one molecule. It is preferred that the compound contains

[0035] The (A-1) component is a linear organopolysiloxane having at least two curing reactive groups in one molecule. The properties of the (A-1) component at room temperature may be oil-like or rubber-like, and the viscosity of the (A-1) component is preferably 50 mPa·s or more at 25°C, and more preferably 100 mPa·s or more. In particular, when the curable silicone resin composition is a solvent-based composition, the (A-1) component preferably has a viscosity of 100,000 mPa·s or more at 25°C or is rubber-like with plasticity. It is also possible to use an (A-1) component with a lower viscosity.

[0036] Component (A-1) may be, for example, a dimethylsiloxane-methylvinylsiloxane copolymer capped at both molecular chain terminals with trimethylsiloxy groups, a dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymer capped at both molecular chain terminals with trimethylsiloxy groups, a dimethylpolysiloxane capped at both molecular chain terminals with dimethylvinylsiloxy groups, a methylphenylpolysiloxane capped at both molecular chain terminals with dimethylvinylsiloxy groups, a dimethylsiloxane-methylvinylsiloxane copolymer capped at both molecular chain terminals with dimethylphenylsiloxy groups, and a dimethylpolysiloxane capped at both molecular chain terminals with methylvinylsiloxy groups.

[0037] The component (A-2) is a resinous or branched-chain organopolysiloxane having at least two curing reactive groups in one molecule, and is particularly preferably a resinous curing reactive organopolysiloxane (organopolysiloxane resin) having at least two curing reactive groups in one molecule. The component (A-2) is, for example, RSiO 2 / 2 Units (D units) and RSiO 3 / 2 Resins consisting of units (T units) (wherein R is, independently of one another, a monovalent organic group or a hydroxyl group) and having at least two curing reactive groups, hydroxyl groups or hydrolyzable groups in the molecule; resins consisting of only T units and having at least two curing reactive groups, hydroxyl groups or hydrolyzable groups in the molecule; and RSiO 1 / 2 Units (M units) and SiO 4 / 2 A resin consisting of units (Q units) and having at least two curing reactive groups, hydroxyl groups or hydrolyzable groups in the molecule. In particular, RSiO 1 / 2 Units (M units) and SiO 4 / 2It is preferable to use a resin (also called MQ resin) that is made up of units (Q units) and has at least two curing reactive groups, hydroxyl groups, or hydrolyzable groups in the molecule. The hydroxyl groups or hydrolyzable groups are directly bonded to silicon in the T units or Q units in the resin, and are groups derived from the raw silane or generated as a result of hydrolysis of the silane.

[0038] The curing reactive functional groups of the (A-1) component and the (A-2) component may be functional groups related to the same curing reaction mechanism, or may be functional groups related to different curing reaction mechanisms. The curing reactive functional groups of the (A-1) component and the (A-2) component may be functional groups related to two or more different curing reaction mechanisms in the same molecule. For example, the (A-1) component or the (A-2) component may be an organopolysiloxane having a photopolymerizable functional group and / or a hydrosilylation reactive functional group and a condensation reactive functional group in the same molecule, and the structure of the (A-1) component is linear, and the structure of the (A-2) component is resinous or branched. When a hydrosilylation reaction is used in either the primary curing reaction or the secondary curing reaction, it is preferable to include the (A-2) component, and the (A-2) component is preferably a resinous or branched organopolysiloxane having functional groups related to two or more different curing reaction mechanisms.

[0039] The (A-2) component is preferably a resinous organopolysiloxane having a hydrosilylation reactive group and / or a radical reactive group when heated under high-energy radiation or in the presence of an organic peroxide.Specifically, the (A-2) component may be, for example, an MQ resin, an MDQ resin, an MTQ resin, an MDTQ resin, a TD resin, a TQ resin, or a TDQ resin, etc., which are composed of any combination of triorganosiloxy units (M units) (organo groups are only methyl groups, methyl groups and vinyl groups or phenyl groups), diorganosiloxy units (D units) (organo groups are only methyl groups, methyl groups and vinyl groups or phenyl groups), monoorganosiloxy units (T units) (organo groups are methyl groups, vinyl groups or phenyl groups) and siloxy units (Q units).

[0040] The component (B) is an organohydrogenpolysiloxane, and is an optional crosslinking component or molecular chain extension component. The component (B) is preferably contained when the curing reactive functional group is an alkenyl group and the curing agent contains a hydrosilylation reaction catalyst. The component (B) is preferably an organohydrogenpolysiloxane having two or more Si-H bonds in the molecule. The desired hardness and pot life (working time) can be controlled by optimizing the content (substance amount ratio) of silicon-bonded hydrogen atoms in the component (B) relative to the curing reactive functional group (e.g., alkenyl group) in the component (A), the amount of the component (C), and the type of the curing retarder described later.

[0041] Examples of component (B) include methylphenylpolysiloxanes capped at both molecular chain terminals with dimethylhydrogensiloxy groups, dimethylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with dimethylhydrogensiloxy groups, diphenylpolysiloxanes capped at both molecular chain terminals with dimethylhydrogensiloxane groups, methylhydrogenpolysiloxanes capped at both molecular chain terminals with trimethylsiloxy groups, methylhydrogensiloxane-dimethylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxy groups, methylhydrogensiloxane-dimethylsiloxane copolymers capped at both molecular chain terminals with dimethylhydrogensiloxy groups, and mixtures of two or more of these organopolysiloxanes. In one embodiment of the present invention, component (B) may be a methylhydrogensiloxane-dimethylsiloxane copolymer capped at both molecular chain terminals with trimethylsiloxy groups and having a viscosity of 1 to 500 mPa s at 25° C. Component (B) may also contain a resinous organohydrogenpolysiloxane resin.

[0042] Component (C) is a curing agent and contains one or more curing agents selected from the following hydrosilylation reaction catalysts, organic peroxides, and photopolymerization initiators.

[0043] The hydrosilylation catalyst includes, for example, platinum-based catalysts, rhodium-based catalysts, and palladium-based catalysts, and is preferably a platinum-based catalyst because it can significantly accelerate curing. The platinum-based catalyst may be, for example, platinum fine powder, chloroplatinic acid, an alcohol solution of chloroplatinic acid, a platinum-alkenylsiloxane complex, a platinum-olefin complex, a platinum-carbonyl complex, or a catalyst in which these platinum-based catalysts are dispersed or encapsulated in a thermoplastic resin such as a silicone resin, a polycarbonate resin, or an acrylic resin. Among them, platinum-alkenylsiloxane complexes are preferred. The alkenylsiloxane may be 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane, alkenylsiloxanes in which a portion of the methyl groups of these alkenylsiloxanes have been substituted with ethyl groups, phenyl groups, or the like, or alkenylsiloxanes in which the vinyl groups of these alkenylsiloxanes have been substituted with allyl groups, hexenyl groups, or the like. In particular, 1,3-divinyl-1,1,3,3-tetramethyldisiloxane is preferred because the platinum-alkenylsiloxane complex has good stability. Examples of catalysts that promote the hydrosilylation reaction include non-platinum metal catalysts such as iron, ruthenium, and iron / cobalt.

[0044] In addition, the curing agent used in one embodiment of the present invention may be a platinum-containing hydrosilylation catalyst in the form of fine particles dispersed or encapsulated in a thermoplastic resin. The use of such an encapsulated curing agent provides the advantages of improved storage stability of the cured reactive silicone gel and controllability of the curing reaction by temperature, in addition to the advantages of improved handling and pot life of the composition.

[0045] In one embodiment of the present invention, a hydrosilylation catalyst such as a photoactive platinum complex curing catalyst that accelerates the hydrosilylation reaction by irradiation with high energy rays such as ultraviolet rays other than heating may be used. The hydrosilylation catalyst may be a β-diketone platinum complex or a platinum complex having a cyclic diene compound as a ligand. Specifically, the hydrosilylation catalyst may be, for example, a trimethyl(acetylacetonato) platinum complex, a trimethyl(2,4-pentanedionato) platinum complex, a trimethyl(3,5-heptanedionato) platinum complex, a trimethyl(methylacetoacetate) platinum complex, a bis(2,4-pentanedionato) platinum complex, a bis(2,4-hexanedionato) platinum complex, a bis(2,4-heptanedionato) platinum complex, a bis(3,5-heptanedionato) platinum complex, or a bis(2,4-hexanedionato) platinum complex. (1,5-cyclooctadienyl)dimethylplatinum complex, (1,5-cyclooctadienyl)diphenylplatinum complex, (1,5-cyclooctadienyl)dipropylplatinum complex, (2,5-norboradiene)dimethylplatinum complex, (2,5-norboradiene)diphenylplatinum complex complex, (cyclopentadienyl)dimethyl platinum complex, (methylcyclopentadienyl)diethyl platinum complex, (trimethylsilylcyclopentadienyl)diphenyl platinum complex, (methylcycloocta-1,5-dienyl)diethyl platinum complex, (cyclopentadienyl)trimethyl platinum complex, (cyclopentadienyl)ethyl dimethyl platinum complex, (cyclopentadienyl)acetyl dimethyl platinum complex, (methylcyclopentadienyl)trimethyl platinum complex, (methylcyclopentadienyl)trihexyl platinum complex, (trimethylsilylcyclopentadienyl)trimethyl platinum complex, (trimethylsilylcyclopentadienyl)trihexyl platinum complex, (dimethylphenylsilylcyclopentadienyl)triphenyl platinum complex, and (cyclopentadienyl)dimethyl trimethylsilyl methyl platinum complex.

[0046] When a curing agent that accelerates the hydrosilylation reaction upon irradiation with high-energy rays is used, the formation of a cured product (cured layer) can be promoted using a curable silicone resin composition as a raw material without a heating operation.

[0047] The content of the hydrosilylation reaction catalyst is preferably an amount such that, when the entire curable silicone resin composition is taken as 100 parts by mass, the metal atoms are in the range of 0.01 to 500 ppm, 0.01 to 100 ppm, or 0.01 to 50 ppm, in mass units.

[0048] The organic peroxides may be alkyl peroxides, diacyl peroxides, peroxide esters, and peroxide carbonates.

[0049] The alkyl peroxides may be, for example, dicumyl peroxide, di-tert-butyl peroxide, di-tert-butylcumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, tert-butylcumyl, 1,3-bis(tert-butylperoxyisopropyl)benzene, and 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxonane.

[0050] The diacyl peroxides may be, for example, benzoyl peroxides such as tp-methylbenzoyl peroxide, lauroyl peroxide, and decanoyl peroxide.

[0051] Examples of peroxy esters include 1,1,3,3-tetramethylbutylperoxyneodecanoate, α-cumylperoxyneodecanoate, tert-butylperoxyneodecanoate, tert-butylperoxyneoheptanoate, tert-butylperoxypivalate, tert-hexylperoxypivalate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, tert-amylperoxy-2-ethylhexanoate, t tert-butylperoxy-2-ethylhexanoate, tert-butylperoxyisobutyrate, di-tert-butylperoxyhexahydroterephthalate, tert-amylperoxy-3,5,5-trimethylhexanoate, tert-butylperoxy-3,5,5-trimethylhexanoate, tert-butylperoxyacetate, tert-butylperoxybenzoate, and di-butylperoxytrimethyladipate, and the like.

[0052] The peroxycarbonates may be, for example, di-3-methoxybutyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, diisopropyl peroxydicarbonate, tert-butylperoxyisopropyl carbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, dicetyl peroxydicarbonate, and dimyristyl peroxydicarbonate.

[0053] The organic peroxide preferably has a half-life of 10 hours at a temperature of 70° C. or higher, and may be at least 90° C. or at least 95° C. The organic peroxide may be, for example, p-methylbenzoyl peroxide, dicumyl peroxide, di-t-butyl peroxide, di-t-hexyl peroxide, t-butylcumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 1,3-bis(tert-butylperoxyisopropyl)benzene, di-(2-t-butylperoxyisopropyl)benzene, and 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxonane.

[0054] The content of the organic peroxide is not particularly limited, but is preferably within a range of 0.05 to 10 parts by mass, or within a range of 0.10 to 5.0 parts by mass, based on 100 parts by mass of the entire curable silicone resin composition.

[0055] The photopolymerization initiator is a component that generates radicals when irradiated with high-energy rays such as ultraviolet rays or electron beams. Examples of the photopolymerization initiator include acetophenone and its derivatives such as acetophenone, dichloroacetophenone, trichloroacetophenone, tert-butyltrichloroacetophenone, 2,2-diethoxyacetophenone, and p-dimethylaminoacetophenone; benzoin and its derivatives such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin butyl ether, and benzoin n-butyl ether; benzophenone and its derivatives such as benzophenone, 2-chlorobenzophenone, p,p'-dichlorobenzophenone, and p,p'-bisdiethylaminobenzophenone; p-dimethylaminopropiophenone, Michler's ketone, benzil, benzil dimethyl ketal, tetramethylthiuram monosulfide, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, azoisobutyronitrile, benzo Examples of the phenyl ether ester include isopropyl alcohol, ...

[0056] The amount of the photopolymerization initiator added is preferably within the range of 0.1 to 10 parts by mass when the total amount of the curable silicone resin composition is taken as 100 parts by mass.

[0057] In addition, when the silicone gel of one embodiment of the present invention contains a photopolymerization initiator as a curing agent, the silicone gel may contain, as an optional component, a photosensitizer such as n-butylamine, di-n-butylamine, tri-n-butylphosphine, allylthiourea, s-benzylisothiuronium-p-toluenesulfinate, triethylamine, or diethylaminoethyl methacrylate.

[0058] The curable silicone resin composition of one embodiment of the present invention may contain components other than the above-mentioned components, as long as the technical effect of the present invention is not impaired.Specific examples of such optional components include curing retarders; adhesion promoters; non-reactive organopolysiloxanes such as polydimethylsiloxane or polydimethyldiphenylsiloxane; antioxidants such as phenols, quinones, amines, phosphorus, phosphite, sulfur, or thioethers; light stabilizers such as triazoles or benzophenones; flame retardants such as phosphate esters, halogens, phosphorus, or antimony; one or more antistatic agents such as cationic surfactants, anionic surfactants, or nonionic surfactants; dyes; pigments; reinforcing fillers; thermally conductive fillers; dielectric fillers; electrically conductive fillers; and release components.In addition, optional additives such as infrared sensitizers, water repellents, and water penetration inhibitors, which will be described later, may be included.

[0059] In particular, the reinforcing filler is a component that can impart mechanical strength to the coating agent for structures of the present invention and improve thixotropy, and may further improve the mechanical strength, shape retention, surface releasability, etc. of the cured product. The reinforcing filler may be, for example, an inorganic filler such as fumed silica fine powder, precipitated silica fine powder, calcined silica fine powder, fumed titanium dioxide fine powder, quartz fine powder, calcium carbonate fine powder, diatomaceous earth fine powder, aluminum oxide fine powder, aluminum hydroxide fine powder, zinc oxide fine powder, zinc carbonate fine powder, etc. These inorganic fillers may be inorganic fillers that have been surface-treated with a treating agent such as an organoalkoxysilane, such as methyltrimethoxysilane; an organohalosilane, such as trimethylchlorosilane; an organosilazane, such as hexamethyldisilazane; or a siloxane oligomer, such as an α,ω-silanol group-blocked dimethylsiloxane oligomer, an α,ω-silanol group-blocked methylphenylsiloxane oligomer, or an α,ω-silanol group-blocked methylvinylsiloxane oligomer.

[0060] The curable silicone resin composition of one embodiment of the present invention is preferably blended with a hydrosilylation reaction inhibitor as a curing retarder.Specifically, the hydrosilylation reaction inhibitor may be, for example, alkyne alcohols such as 2-methyl-3-butyn-2-ol, 3,5-dimethyl-1-hexyn-3-ol, 2-phenyl-3-butyn-2-ol, 1-ethynyl-1-cyclohexanol, etc.; enyne compounds such as 3-methyl-3-penten-1-yne, 3,5-dimethyl-3-hexen-1-yne, etc.; alkenyl-containing low molecular weight siloxanes such as tetramethyltetravinylcyclotetrasiloxane, tetramethyltetrahexenylcyclotetrasiloxane, etc.; alkynyloxysilanes such as methyl-tris(1,1-dimethylpropynyloxy)silane, vinyl-tris(1,1-dimethylpropynyloxy)silane, etc. The content of the curing retarder is preferably within a range of 10 to 10,000 ppm by mass relative to the curable silicone resin composition.

[0061] The curable silicone resin composition of one embodiment of the present invention preferably contains, as an adhesion promoter, an organosilicon compound having at least one alkoxy group bonded to a silicon atom in each molecule. The alkoxy group may be a methoxy group, an ethoxy group, a propoxy group, a butoxy group, a methoxyethoxy group, or the like, with a methoxy group being preferred. In addition, groups bonded to silicon atoms in the organosilicon compound other than alkoxy groups may be halogen-substituted or unsubstituted monovalent hydrocarbon groups such as alkyl groups, alkenyl groups, aryl groups, aralkyl groups, and halogenated alkyl groups; glycidoxyalkyl groups such as 3-glycidoxypropyl group and 4-glycidoxybutyl group; epoxycyclohexylalkyl groups such as 2-(3,4-epoxycyclohexyl)ethyl group and 3-(3,4-epoxycyclohexyl)propyl group; epoxyalkyl groups such as 3,4-epoxybutyl group and 7,8-epoxyoctyl group; acrylic group-containing monovalent organic groups such as 3-methacryloxypropyl group; and hydrogen atoms. The organosilicon compound preferably has a group capable of reacting with an alkenyl group or a silicon-bonded hydrogen atom in the curable silicone resin composition, and more specifically, preferably has a silicon-bonded hydrogen atom or an alkenyl group. In addition, since it can provide good adhesion to various substrates, it is preferable that the organosilicon compound has at least one epoxy-containing monovalent organic group in one molecule.Such an organosilicon compound may be, for example, an organosilane compound, an organosiloxane oligomer, an alkyl silicate, etc.The molecular structure of the organosiloxane oligomer or alkyl silicate may be linear, partially branched linear, branched, cyclic, or network, and among them, linear, branched, or network is preferable. Specific examples of the organosilicon compound include silane compounds such as 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 3-methacryloxypropyltrimethoxysilane; siloxane compounds having at least one silicon-bonded alkenyl group or silicon-bonded hydrogen atom, and at least one silicon-bonded alkoxy group in one molecule, a mixture of a silane compound or siloxane compound having at least one silicon-bonded alkoxy group and a siloxane compound having at least one silicon-bonded hydroxy group and at least one silicon-bonded alkenyl group in one molecule, methyl polysilicate, ethyl polysilicate, and epoxy group-containing ethyl polysilicate. The adhesion promoter is preferably a low-viscosity liquid, and its viscosity is preferably within the range of 1 to 500 mPa s at 25° C. The content of the adhesion promoter is preferably within the range of 0.01 to 10 parts by mass relative to 100 parts by mass of the curable silicone resin composition.

[0062] From the standpoint of uniform dispersion during mixing, the reinforcing filler, cure retarder, and adhesion promoter are preferably added when the curable silicone resin composition is prepared.

[0063] 1.1.2 Curable urethane resin composition The curable resin composition of one embodiment of the present invention includes a curable urethane resin composition. The curable urethane resin composition may be one type alone or a mixture of two or more types at any ratio. The curable urethane resin composition of one embodiment of the present invention may be a one-liquid type package in which an active hydrogen group-containing compound and an excess of polyisocyanate react with each other in the presence of moisture in the air to cure, or may be a two-liquid type package in which a polyisocyanate and an active hydrogen group-containing compound are mixed in any ratio before use to cure. In one embodiment of the present invention, a two-liquid type curable urethane resin composition is preferred because it is easy to adjust the curing speed.

[0064] Polyisocyanates have two or more isocyanate groups in one molecule. The polyisocyanate is not particularly limited, but examples thereof include aromatic diisocyanates such as m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 2,4'- or 4,4'-diphenylmethane diisocyanate, 2,4- or 2,6-tolylene diisocyanate, 4,4'-toluidine diisocyanate, and 4,4'-diphenyl ether diisocyanate; Aromatic ring-containing aliphatic diisocyanates such as 1,3- or 1,4-xylylene diisocyanate; Aliphatic diisocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, norbornane diisocyanate, and 2,6-diisocyanate methyl caproate; Alicyclic diisocyanates such as 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, and 1,4-bis(isocyanatomethyl)cyclohexane; and The polyisocyanates may be polyisocyanates that are used in the production of ordinary polyurethane resins, such as carbodiimide-modified products, biuret-modified products, allophanate-modified products, dimers, trimers, etc. of these diisocyanates. The polyisocyanates may be used alone or in combination of two or more kinds.

[0065] The active hydrogen group-containing compound is not particularly limited, and may be, for example, polyamine or polyol.In addition, generally, the curable resin in which polyamine is mainly used as the active hydrogen group-containing compound and the active hydrogen group-containing compound and polyisocyanate are bonded mainly by urea bond may be called urea resin, and the curable resin in which polyol is mainly used as the active hydrogen group-containing compound and the active hydrogen group-containing compound and polyisocyanate are bonded mainly by urethane bond may be called urethane resin, but in this specification, both are not particularly distinguished and are collectively called curable urethane resin composition.

[0066] Examples of polyamines include aliphatic polyamines such as ethylenediamine, diethylenetriamine, triethylenetetramine, hexamethylenediamine, and polyoxyalkylenepolyamines; Alicyclic polyamines such as isophorone diamine, norbornene diamine, and hydrogenated xylylene diamine; Aromatic ring-containing aliphatic polyamines such as xylylenediamine; The aromatic polyamine may be 3,5-diethyl-2,4-diaminotoluene, 3,5-diethyl-2,6-diaminotoluene, 4,4'-diaminodiphenylmethane, 2,4-tolylenediamine, 2,6-tolylenediamine, 1,1'-dichloro-4,4'-diaminodiphenylmethane, 3,3'-dichloro-4.4'-diaminodiphenylmethane, 1,1',2,2'-tetrachloro-4,4'-diaminodiphenylmethane, 1,3,5-triethyl-2,6-diaminobenzene, 3,3',5,5'-tetraethyl-4,4'-diaminodiphenyl-methane, N,N'-bis(t-butyl)-4,4'-diaminodiphenyl-methane, or di(methylthio)toluenediamine.

[0067] Examples of polyols include low molecular weight diols such as ethylene glycol, propanediol, 1,4-butylene glycol, 1,3-butylene glycol, 1,2-butylene glycol, 1,6-hexanediol, neopentyl glycol, alkanediol, diethylene glycol, triethylene glycol, dipropylene glycol, cyclohexanedimethanol, alkane-1,2-diol, hydrogenated bisphenol A, 1,4-dihydroxy-2-butene, 2,6-dimethyl-1-octene-3,8-diol, bishydroxyethoxybenzene, xylene glycol, bishydroxyethylene terephthalate, bisphenol A, and bisphenol F; low molecular weight triols such as glycerin, 2-methyl-2-hydroxymethyl-1,3-propanediol, 2,4-dihydroxy-3-hydroxymethylpentane, 1,2,6-hexanetriol, 1,1,1-tris(hydroxymethyl)propane, 2,2-bis(hydroxymethyl)-3-butanol, and aliphatic triols with carbon numbers from 8 to 24; Low molecular weight polyols with four or more hydroxyl groups in one molecule, such as pentaerythritol; polyhydric alcohol ethers obtained by intermolecular dehydration condensation of the above-mentioned low molecular weight diols, the above-mentioned low molecular weight triols, and the above-mentioned low molecular weight polyols having four or more hydroxyl groups per molecule, such as diethylene glycol, dipentaerythritol, and ditrimethylolpropane; Polytetramethylene glycol obtained by ring-opening polymerization of tetrahydrofuran; natural fat polyols such as castor oil; The polyolefin polyols may be polybutadiene polyol, polyisoprene polyol, or hydrogenated products thereof. These active hydrogen group-containing compounds may be used alone or in combination of two or more.

[0068] 1.2 Metal powder The metal powder used in the present invention may have any property detectable by infrared rays. By containing the metal powder having such property, the coating agent for structures of the present invention can easily and highly accurately detect damage to structures by imaging with an infrared camera. Without being bound by theory, the metal powder dispersed in the curable resin composition flows to damaged areas such as cracks due to gravity and accumulates at the damaged areas, making it possible to detect temperature differences with an infrared camera. As a result, even fine damage that is difficult to see with the naked eye can be detected with high accuracy by imaging with an infrared camera. The metal powder according to one embodiment of the present invention is preferably made from a metal having a high reflectance. By using a metal having a high reflectance, deterioration of the curable resin composition due to exposure to ultraviolet rays in an outdoor environment can be prevented or reduced. The metal powder may be, for example, one or more selected from the group consisting of aluminum, gold, silver, copper, nickel, cobalt, chromium, platinum, tin, and iron. Among them, the metal powder preferably contains aluminum powder from the viewpoint of relatively easy procurement of raw materials. In addition, the metal powder may be partially in the form of a metal oxide.

[0069] The metal powder of one embodiment of the present invention has an average primary particle size measured by a laser diffraction / scattering method in the range of preferably 5 to 50 μm, more preferably 5 to 30 μm, and even more preferably 10 to 25 μm. By using a metal powder having an average primary particle size within the above range, the dispersibility in the curable resin composition can be improved, and the function as a coating agent for structures can be well maintained.

[0070] The amount of the metal powder in one embodiment of the present invention is not particularly limited, but is preferably in the range of 0.1 to 10 mass % relative to the total amount of the coating agent for structures, more preferably in the range of 0.5 to 8.0 mass %, even more preferably in the range of 0.5 to 5.0 mass %, and particularly preferably in the range of 1.0 to 3.0 mass %. By setting the blending amount of the metal powder in the above range, the dispersibility in the curable resin composition can be improved, and the function as a coating agent for structures can be maintained well. Also, by setting the blending amount of the metal powder to the lower limit or more, the detection accuracy by infrared rays can be improved. The upper limit of the amount of metal powder does not prevent the amount of metal powder from being set to more than 10% by mass. The amount of metal powder may be designed to exceed 10% by mass as long as the effects of the present invention are not impaired.

[0071] 1.3 Infrared sensitizers / infrared imaging agents The coating agent for structures according to one embodiment of the present invention may further contain a known infrared sensitizer or infrared imaging agent. The infrared sensitizer or infrared imaging agent may be, for example, a cyanine compound, a phthalocyanine compound, a dithiol metal complex, a naphthoquinone compound, a diimmonium compound, an azo compound, or the like. Among them, from the viewpoint of compatibility with silicone, one or more compounds selected from phthalocyanine-based and cyanine-based compounds are preferred. The coating agent for structures according to one embodiment of the present invention may contain an iodine-based additive, which not only prevents deterioration of the coating caused by ultraviolet light but also enables deterioration detection by imaging using visible light.

[0072] 1.4 Optional components The coating agent for structures according to one embodiment of the present invention may optionally contain other components that are widely used in the fields of civil engineering or architecture.The other components may be, for example, plasticizers, ultraviolet absorbers, water repellents, water penetration inhibitors, AE agents (air entraining agents), water reducers (preferably AE water reducers, particularly high performance AE water reducers), waterproofing agents, water resistance agents, defoamers, curing agents, release agents, shrinkage reducing agents, surface aesthetic improvers, setting accelerators, setting retarders, self-leveling agents, paints, surface repair materials, thickeners, expansion agents, rust inhibitors, inorganic fibers, organic fibers, organic polymers, silica fume, fly ash, and blast furnace slag powder.

[0073] 2. Manufacturing method of coating agent for structures The method for producing the coating agent for structures of the present invention is not particularly limited, and may be, for example, a method having a step of uniformly stirring the curable resin composition of one embodiment of the present invention described in the above "1.1 Curable resin composition" and "1.2 Metal powder", the metal powder, and, if necessary, other additives. The equipment used in the stirring step is not particularly limited, and for example, a mechanical stirring means (mixer, etc.) for the purpose of uniform mixing can be used. The coating agent for structures of one embodiment of the present invention may be in the form of a one-liquid type, or may be a multi-liquid type composition consisting of a plurality of separated liquid packages.

[0074] 3.Structures The present invention provides a structure including a cured product formed by applying the coating agent for structures according to one embodiment of the present invention. The cured product may form a cured layer made of the cured product on the outer surface of the structure. The explanations in "1.1 Curable resin composition" and "1.2 Metal powder" above regarding the curable resin composition and metal powder contained in the cured product also apply to this embodiment. Specific examples of the structure are as explained in "1. Coating agent for structures" above.

[0075] The method of applying the coating agent for structures to the structure is not particularly limited, and may be manual work such as brush coating, roller brush coating, spatula coating, etc., or machine work such as pump-type spraying, air spray coating, airless spray coating, dip coating, etc., or machine work such as electrostatic coating, electrodeposition coating, powder coating, etc. Among these, brush coating is preferred from the viewpoint of application to joints, but is not limited thereto. In addition, a cured layer may be formed by attaching a gel-like or elastomeric cured material prepared in advance to the structure in the form of a peelable laminate.

[0076] The thickness of the cured product or cured layer may be, for example, in the range of 0.1 to 10 mm, preferably in the range of 0.1 to 8 mm, and more preferably in the range of 0.5 to 5 mm.

[0077] 4. Methods for detecting damage to structures The present invention provides a method for detecting damage to a structure, comprising applying a coating agent for a structure to an exterior surface of the structure, the coating agent including an infrared-detectable metal powder dispersed in a curable resin composition, and imaging the exterior surface of the structure by infrared irradiation. The explanations in "1.1 Curable resin composition" and "1.2 Metal powder" above about the curable resin composition and the metal powder also apply to this embodiment. Specific examples of the structure are as explained in "1. Coating agent for structure" above. The explanations in "3. Structure" above about the method of applying the coating agent for structure to the outer surface of the structure and the thickness of the cured product or cured layer also apply to this embodiment.

[0078] In one embodiment of the present invention, the infrared rays irradiated to the external surface of the structure may be infrared rays having a wavelength of 1 to 14 μm. In addition, the infrared rays irradiated in one embodiment of the present invention may be near infrared rays having a wavelength of 1 to 2.3 μm, mid infrared rays having a wavelength of 3 to 5 μm, or far infrared rays having a wavelength of 8 to 14 μm.

[0079] In one embodiment of the present invention, the camera used for imaging is preferably a fixed or movable infrared camera. In this specification, the infrared camera refers to a camera capable of visualizing infrared light emitted from an object, and the type of the camera is not particularly limited and can be appropriately selected from known infrared cameras such as a thermography camera and a thermal camera depending on the purpose. In addition, the means for fixing or moving the infrared camera is not particularly limited, and any known means can be used. In addition, the direction of movement is not particularly limited, and any means capable of moving in any direction may be used.

[0080] In one embodiment of the present invention, imaging using an infrared camera may be performed using a robot or drone operated by wire or wirelessly, or an infrared camera mounted on an automated robot or drone. This allows efficient inspection of a large number of structures installed over a wide area. Furthermore, by employing an automated robot or drone, imaging itself can be performed unmanned, which can contribute to solving social problems such as a shortage of workers. The robot is not particularly limited, but includes, for example, a wall inspection robot and a wall-moving robot.

[0081] The method according to an aspect of the present invention may further include analyzing the image obtained by the imaging by Fourier transform. The Fourier transform may be a discrete Fourier transform (DFT), a fast Fourier transform (FFT), or the like. The method according to an aspect of the present invention further includes analyzing one or more conditions selected from the group consisting of the presence or absence of damage to the structure, the shape of the damage, the size of the damage, and the depth of the damage, by analyzing the Fourier transform image obtained by the Fourier transform process. These analyses can be performed using a computer capable of Fourier transform processing. In addition, a process for predicting damage through comparison with finite element analysis (FEM) may be combined.

[0082] 5. Structural health monitoring system The present invention provides a monitoring system for the soundness of a structure, comprising: a structure whose outer surface is covered with a cured product of a coating agent for structures according to one aspect of the present invention, an imaging means for imaging the outer surface of the structure by irradiating it with infrared rays, and a determination means for analyzing the image obtained by the imaging and determining at least the presence or absence of damage to the structure. In this specification, "soundness" refers to a state in which a structure such as a building can exist without being damaged (collapsed) even if its strength is reduced due to factors such as forces (acceleration) due to earthquakes, deterioration over time, or water infiltration from the surface. For example, it refers to a state in which there is no risk of a structure being damaged (collapsed) even if it is subjected to external forces such as vibration, wind, or sunlight.

[0083] Next, the monitoring system according to one embodiment of the present invention will be described in more detail with reference to Figs. 8-9. In Fig. 8, a structure 1 is a structure according to one embodiment of the present invention, and the description of the structure in "3. Structure" above also applies to this embodiment. The drone 2 is an example of a robot or drone equipped with an infrared camera, and has an imaging means 21 as shown in Fig. 9. The description of the infrared camera and the robot or drone in "4. Method for detecting damage to a structure" above also applies to this embodiment. The computer 3 can be a general computer device such as a PC equipped with a calculation device such as a CPU (Central Processing Unit) or a GPU (Graphical Processing Unit), a main memory device such as a RAM (Random Access Memory), an auxiliary memory device such as a HDD (Hard Disk Drive), an SSD (Solid State Drive), or a flash memory, a display, various input / output devices, etc.

[0084] The drone 2 preferably includes a wired or wireless communication means 22 for transmitting captured image information (including position information such as GPS; the same applies below) to a device such as a computer 3 equipped with a determination means 31. The drone 2 also preferably includes a storage means 23 for temporarily storing the captured image information. Although not shown, the drone 2 (or robot) itself may be configured to include the determination means 31. In this case, the drone 2 (or robot) transmits the determination result, such as the presence or absence of damage to the structure, to an external device such as a computer 3 via the communication means 22. In this case, the drone 2 (or robot) preferably also includes an analysis means 32 and an image analysis means 33, which will be described later.

[0085] The computer 3 includes a determination means 31. The computer 3 is preferably automated by an analysis means 32 that detects damage to the structure by automatically comparing a learning result obtained by machine learning based on imaging data previously obtained using a similar method with an image obtained by the imaging means. The analysis means 32 has a function of determining the presence or absence of damage to the structure by an algorithm based on machine learning such as deep learning using a large amount of accumulated learning data.

[0086] The computer 3 preferably includes an image analysis means 33 that analyzes the image obtained by the imaging means 21 by Fourier transform. The Fourier transform is as explained in "4. Method for detecting damage to a structure" above. The image analysis means 33 preferably has an algorithm set therein for analyzing one or more conditions selected from the group consisting of the presence or absence of damage to the structure, the shape of the damage, the size of the damage, and the depth of the damage. By using a computer having these configurations, it becomes possible to automatically determine on the computer whether a structure is damaged or not based on image information of the captured structure. When a drone or robot has these configurations, it becomes possible for the drone or robot alone to automatically determine whether a structure is damaged or not without using an external computer.

[0087] The computer 3 preferably includes a receiving means 34 for receiving image information transmitted from the drone 2 and / or a determination result such as the presence or absence of damage to the structure. The computer 3 preferably includes a display means 35 for displaying image information captured by the drone 2 and / or a determination result such as the presence or absence of damage to the structure. The display means 35 preferably further displays location information of the inspected structure. The location information here includes not only the location of the structure, but also the inspection area where the inspection was performed and the damage area where damage was detected, as described below.

[0088] Here, as described above, it is preferable that the drone 2 acquires location information together with the image information of the captured structure. In this case, for example, the computer 3 may be configured to store the location information transmitted from the drone 2 and manage the structure whose soundness has been inspected based on the location information. Furthermore, as an example of a method for managing the soundness of a structure using location information, the following method, not shown, can be given. That is, for a certain structure (or a group of structures consisting of a plurality of structures), areas are divided in advance, and each area is identified by a method such as numbering, and the inspection area of ​​the structure is divided into a plurality of areas (for example, S1, S2, S3, etc.). At this time, it is preferable for the computer to associate and store the identification number of each inspection area with the location information. Then, the computer transmits the identification number and location information of the inspection area to be inspected to a drone or the like. Then, after receiving the information, the drone or the like takes an image of the structure in the inspection area based on the information. This makes it possible to automate the inspection of structures and to make the management of inspected structures more efficient. In addition, if the structure to be inspected is one that has been installed by a specific business operator, etc., it is preferable that the same operations as those described above can be performed by inputting and storing in advance into a computer any signs or other marks affixed by that business operator. Furthermore, it is preferable to install signs such as metal reflectors, barcodes, QR codes (registered trademark), and RFID tags at identification points that serve as management criteria for structures. By adding these to the measurement information / imaging information, it is possible to identify and manage damaged areas with high accuracy, which is a practical benefit.

[0089] By being equipped with these configurations, the monitoring system of one embodiment of the present invention is capable of unmanned, automatic inspection of a large number of structures installed over a wide area, and can contribute to solving social problems such as a shortage of workers. EXAMPLES

[0090] The present invention will be further described below based on examples, but the present invention is not limited to the following examples.

[0091] <Test system considerations> Based on the principles of infrared thermography, if there is no significant difference between the air temperature and the temperature of the test piece when measuring indoors with an infrared camera, the surface of the test piece is heated using a halogen lamp, etc. This creates a temperature difference between the inside and surface of the test piece, making it possible to measure cracks and lifting. However, in the outdoors, it is expected that the measurement will be affected by the outside air temperature, the material and color of the object to be measured, the influence of the spectral reflectance, the measurement distance, etc. Therefore, in this example, taking these influences into consideration, a coating agent for structures containing a curable silicone resin composition (which becomes gel-like when cured) with added aluminum powder was applied to the surface of the test specimen, and an infrared thermal image analysis technique was considered that combines the heat retention effect of the gel of the curable silicone resin composition with a preventive measure against deterioration of concrete, etc.

[0092] <Construction of test system> The size of the specimen was 300 × 400 × 1000 mm, and it was made of ordinary concrete with a thickness of 2 cm covering the reinforcing bars, as shown in Figure 1. To measure the effect of strength on the top and bottom of the specimen, a through hole of φ 65 mm was intentionally drilled in the specimen to simulate a defect in the concrete pillar. Figures 2(A) and (B) show the shapes of specimens A and B, respectively. The through-holes in specimen A were located 235 mm below the center of the specimen, to the left of the vertical centerline (Figure 2(A)), while the through-holes in specimen B were located 235 mm above the center of the specimen, to the right of the vertical centerline (Figure 2(B)). A structural coating agent was applied to the entire front surface of both specimens A and B, except for the top 300 mm. Specimen C was a specimen without through-holes, and the surface temperature was measured at the locations numbered in Figure 2(C). The coating agent for structures used was a curable silicone resin composition (CY52-276, Dow Toray) that turns into a gel when cured, with about 1% aluminum powder with an average primary particle size of 10-20 μm measured by laser diffraction and scattering added. This resin is resistant to ultraviolet rays, does not harden over time, and retains its gel-like properties but does not retain water. When used, the first and second liquids were mixed in equal parts and cured for about 1 hour.

[0093] <Experiments and Results> (1) Study of thermal image analysis using passive measurements To compare the effects on thermal images with and without surface heating, the rear of test specimen A was heated at 900 W for approximately 20 minutes using a carbon heater DC-S097 (Yamazen), and a destructive test was conducted after a further 30 minutes had passed. Since the thermal conductivity of concrete is 1.6 W / m K, which is approximately 61.05 times that of air, 0.026 W / m K, the measurement time was determined taking into account the thermal conductivity of the atmosphere. For the destructive test, a maximum pressure of 220 kN was applied to the test specimen from above for approximately 20 minutes using a pressure testing machine (Fig. 3). The surface temperatures of the test specimens were measured simultaneously using thermocouples at four locations: (1) the center 50 mm downward from the top end of the front surface, (2) the center 250 mm downward from the top end of the front surface, (3) the center 50 mm downward from the top end of the back surface, and (4) the center 250 mm downward from the top end of the back surface. Figure 4(a) shows the temperature change of specimen A by passive measurement after heating, and Figure 4(b) shows the measurement results of specimen B by passive measurement performed at room temperature without heating. The temperature change on the back and front of the specimens measured by thermocouples from the start to the end of the test was 4.0 °C for specimen A and 0.6 °C for specimen B. (2) Evaluation of preventive work After coating the entire underside surface of both specimens A and B with a thickness of approximately 0.1 mm, except for the upper 300 mm of the front, a destructive test was conducted and the damage and falling state of fragments were observed in the areas where the coating agent was applied and the areas where it was not applied. Figure 5(a) shows a thermal image of specimen B taken with an infrared camera after the destructive test. Figure 5(b) shows an image of specimen B taken with a visible light digital camera, recorded at the same time and at the same location as the infrared camera. Note that the elapsed time after pressure application is the same in both Figures 5(a) and (b). In each figure, it can be seen that the "cracks" and "floats" were generated by the shear force generated diagonally downward from the right and the pressure applied from above. In particular, it was confirmed that the scattering and collapse of concrete fragments due to compression failure was suppressed in the lower part of the specimen where the coating was applied (Figure 5(a)), and that the "floats" state, which are difficult to detect with a visible light camera, can be measured with an infrared camera (arrow in Figure 5(b)). The infrared camera used was the AVIO R450 series manufactured by Nippon Avionics, and the visible light digital camera used was the HDR-PJ670 manufactured by Sony. Although photographs of test specimen A were omitted, similar results to those of test specimen B were confirmed. (3) Evaluation of the relationship between rebar strain and heat generation The strain and heat generation in specimen C were measured using the strain measurement system WIMO from Taiheiyo Cement Corporation. Specimen C has the same shape and size as specimens A and B in Figure 2, and was created by pouring concrete after fixing the RFID strain measurement sensor WIMO-SSN-1390 to the center of the internal reinforcing steel pillar φ13 × 900 mm. Also, unlike specimens A and B, specimen C is in a sound condition without any missing parts (through holes). Figure 6(a) shows the RFID strain measurement sensor fixed inside specimen C, and Figure 6(b) shows the measurement method using the strain measurement system. This device receives the measurement results of the temperature and strain inside the concrete from the surface of the specimen using a reader / writer and analyzes them on a PC. In this experiment, the relationship between the strain of the reinforcing steel pillar inside the specimen during the compression fracture test and the heat generation due to deformation was recorded using radio wave measurement in the 920 MHz band. Figure 7(a) shows the strain inside the test piece and the heat generated by the rebar during the destructive test, and Figure 7(b) shows the measurement results of the pressure, strain, and temperature on the surface of the test piece. We measured how the heat generated by the pressure of the rebar inside the test piece affected the thermal imaging camera that measured the radiant heat on the surface of the test piece, but it was proven that no heat was generated that would affect the images taken by the infrared camera. [Industrial Applicability]

[0094] A structure having a cured product (cured layer) formed by applying the coating agent for structures of the present invention has improved repairability and anti-peeling properties (durability) of the structure, and also has detectability of internal cracks and the like by imaging with an infrared camera. The method of inspecting the structure using an infrared camera is more accurate than an acoustic method, and can be carried out more easily and in a shorter time than existing X-ray detection methods and detection methods using phosphors. In addition, the inspection method using an infrared camera can quickly and accurately inspect the presence or absence of deterioration of the structure by imaging with an infrared camera alone, so that it can realize the inspection of a large number of wide-ranging structures, especially structures that are difficult to inspect by man. In addition, the inspection method is easy to implement in society and commercially disseminate, and can be applied to infrastructure facilities that are difficult to inspect by man, such as high-rise buildings and wind turbines used in offshore wind power generation facilities. In addition, the coating agent for structures according to the present invention has an effect as a functional coating / paint as a preventive measure, and also contributes to the so-called energy-saving effect of buildings by blocking internal heat. [Explanation of symbols]

[0095] 1 structure 2. Drone 21 Imaging means 22 Means of communication 23 Memory means 3. Computer 31 Judgment means 32 Analytical tools 33 Image Analysis Methods 34 Receiving means 35 Display means

Claims

1. A curable resin composition; A metal powder detectable by infrared light; A coating agent for a structure comprising:

2. 2. The coating agent according to claim 1, wherein the metal powder comprises one or more metal powders selected from the group consisting of aluminum, gold, silver, copper, nickel, cobalt, chromium, platinum, tin and iron.

3. The coating agent according to claim 1 or 2, wherein the metal powder comprises an aluminum powder.

4. 4. The coating agent according to claim 1, wherein the average primary particle size of the metal powder is in the range of 5 to 50 μm as measured by a laser diffraction / scattering method.

5. The coating agent according to any one of claims 1 to 4, wherein the coating agent contains the metal powder in an amount of 0.1 to 10 mass% based on the total amount of the coating agent.

6. The coating agent according to any one of claims 1 to 5, wherein the curable resin composition forms a gel-like or elastomeric cured product upon curing.

7. The coating agent according to any one of claims 1 to 6, wherein the curable resin composition forms a gel-like cured product having a 1 / 4 consistency defined in JIS K 2220 in the range of 10 to 150 upon curing.

8. The coating agent according to any one of claims 1 to 6, wherein the curable resin composition forms an elastomeric cured product having a JIS A hardness in the range of 20 to 90 upon curing.

9. The coating agent according to any one of claims 1 to 8, wherein the curable resin composition comprises at least one selected from the group consisting of a curable silicone resin composition and a curable urethane resin composition.

10. The coating agent according to any one of claims 1 to 9, wherein the curable resin composition comprises a curable silicone resin composition.

11. The curable silicone resin composition comprises: (A) an organopolysiloxane having at least two curing reactive groups in one molecule; (B) optionally, an organohydrogenpolysiloxane; (C) Hardener The coating agent according to claim 9 or 10, comprising:

12. The coating agent according to any one of claims 9 to 11, wherein the curable silicone resin composition is cured by one or more curing reactions selected from the group consisting of a hydrosilylation curing reaction, a condensation curing reaction, a peroxide curing reaction, a photocuring reaction, and a high-energy ray curing reaction.

13. The coating agent according to any one of claims 1 to 12, which is used for detecting damage to a structure.

14. 14. The coating agent of claim 13, wherein the detection is performed by infrared irradiation.

15. A curable resin composition; A metal powder detectable by infrared light; A structure comprising a cured product formed by applying a coating agent for structures comprising the above-mentioned.

16. applying a coating for the structure to an exterior surface of the structure, the coating comprising an infrared detectable metal powder dispersed in a curable resin composition; and imaging the exterior surface of the structure with infrared illumination; A method for detecting damage to a structure, comprising:

17. The method of claim 16 , wherein the imaging is performed with a fixed or movable infrared camera.

18. 18. The method of claim 16 or 17, wherein the imaging is performed using a wired or wirelessly operated robot or drone, or an automated robot or drone.

19. The method according to any one of claims 16 to 18, further comprising analysing the image obtained by imaging by Fourier transformation.

20. The method according to claim 19, wherein the analysis is performed to analyze one or more conditions selected from the group consisting of the presence or absence of damage to the structure, the shape of the damage, the size of the damage, and the depth of the damage.

21. A structure whose outer surface is covered with a cured product of the coating agent for structures according to any one of claims 1 to 14. Imaging means for imaging the exterior surface of the structure by infrared irradiation; and A determination means for determining whether or not the structure is damaged by analyzing the image obtained by the imaging is provided. Structural health monitoring system.

22. moreover, A receiving means for receiving image information and / or a result of determining whether or not the structure is damaged; and A display means for displaying image information and / or a result of a determination of the presence or absence of damage to the structure; Equipped with 22. The system of claim 21.

23. The imaging means, A wired or wireless communication means for transmitting image information and position information of the captured structure; and A storage means for storing image information and position information of the captured structure, When the determination means determines that there is damage to the structure, the display means displays position information of the structure in which the damage has been detected and / or a damaged area in the structure in which the damage has been detected.

23. The system of claim 22.

24. The system according to any one of claims 21 to 23, wherein the imaging means is a robot or a drone equipped with an infrared camera.

25. The system according to any one of claims 21 to 24, wherein the determination means is automated by an analysis means that detects damage to the structure by automatically comparing the image obtained by the imaging means with a learning result obtained by machine learning based on imaging data previously obtained using a similar method.

26. The system according to any one of claims 21 to 25, wherein the determination means comprises image analysis means for analyzing the image obtained by the imaging means by Fourier transformation.

27. The system according to claim 26, wherein the image analysis means performs analysis of one or more conditions selected from the group consisting of the presence or absence of damage to the structure, the shape of the damage, the size of the damage, and the depth of the damage.

28. 19. The structure of claim 15, the method of any one of claims 16 to 20, or the system of any one of claims 21 to 28, wherein the structure comprises one or more infrastructures selected from the group consisting of roads, railways, bridges, tunnels, low or high rise buildings, wind turbines, dikes, dams and pipelines.

Citation Information

Patent Citations

  • Repair material for crack of concrete having x-ray shadowing capacity, and research and repair method for crak of concrete using the repair material

    JP1995139190A

  • Polymerizable fluorescent sealant and method for gap filling for building

    JP2000219869A

Cited By

  • Information providing device, information providing method, and program

    JP2026100968A

  • Information provision device, information provision method, and program

    JP7886931B2