Method for producing single-end unsubstituted polythiophene and thiophene compound

The method addresses solubility and stability issues in polythiophene production by using iodobenzene-initiated polymerization, enabling stable, solvent-soluble polythiophenes for hybrid material applications.

JP2024161885APending Publication Date: 2024-11-20KANAGAWA UNIVERSITY +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024018235
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-08
Filing Date
2024-02-09
Publication Date
2024-11-20

AI Technical Summary

Technical Problem

Existing methods for producing polythiophene compounds with one end unsubstituted face challenges in solubility in general-purpose solvents and stability during purification, limiting their application in hybrid materials.

Method used

A method involving the polymerization of a thiophene compound using an iodobenzene compound as an initiator, followed by reactions with specific catalysts and reagents, results in a polythiophene unsubstituted at one end, which can be further modified to include a trialkoxysilyl group, enhancing solubility and stability.

Benefits of technology

The method enables the efficient production of polythiophenes and block copolymers that are soluble in aqueous organic solvents, stable post-purification, and suitable for surface modification of inorganic fine particles, improving the properties of hybrid materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161885000001
    Figure 2024161885000001
  • Figure 2024161885000002
    Figure 2024161885000002
  • Figure 2024161885000003
    Figure 2024161885000003
Patent Text Reader

Abstract

To provide a method for producing single-end unsubstituted polythiophenes soluble in general organic solvents, making them suitable as synthetic raw materials for polythiophenes or block copolymers selectively modified at both ends.SOLUTION: The present invention provides a method for producing single-end unsubstituted polythiophenes represented by formula (3), by polymerizing a thiophene compound represented by formula (1), with an iodobenzene compound represented by formula (2) as an initiator, in the presence of a metal catalyst. (R1-R5 independently represent a hydrogen atom, a fluorine atom, a chlorine atom, or a C1-5 alkyl group, X is a halogen, Y is a monovalent organic group with three or more oxygen atoms, and n is a natural number.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a one-end-unsubstituted polythiophene and a thiophene compound, and more specifically, to a method for producing a one-end-unsubstituted polythiophene compound that can be suitably used as a raw material for synthesizing polythiophenes or block copolymers having modified both ends, and a thiophene compound used therein. [Background technology]

[0002] In order to improve the heat resistance, mechanical properties, and electrical properties of organic materials, hybrid materials (nanocomposites) in which inorganic particles such as silica gel and titanium oxide are mixed with organic polymers have been widely studied. However, because the properties of organic and inorganic materials are fundamentally very different, problems with the above hybrid materials include the inability to introduce so many inorganic particles into the organic material, the difficulty of dispersing the inorganic particles neatly in the organic material, and the aggregation of the inorganic particles in the organic material over time.

[0003] In order to solve these problems, the surface of inorganic fine particles has been modified with organic low molecular weight compounds or organic polymers. When modifying with organic polymers, the following two methods are mainly used: (1) introducing an initiation site onto the inorganic surface and performing living polymerization from there, and (2) introducing a functional group (e.g., -Si(OR)3, -PO3H, -COOH, -SH, etc.) that can bond with inorganic substances to the end of the living polymer and reacting it with the surface of the inorganic fine particles. For example, it has been revealed that when silica fine particles surface-modified by introducing -Si(OR)3 groups to the ends of linear and multi-branched aromatic polyamides using the latter method are added to aromatic polyimides, the heat resistance is increased and the transparency is improved compared to the case of adding conventional unmodified silica (Patent Documents 1 to 3).

[0004] Thus, modifying silica particles with organic polymers is important in developing hybrid materials. In particular, conductive polymers such as polythiophene and polyaniline have been studied for their applicability to solar cells, field-effect transistors, light-emitting devices, sensors, etc. However, since these conductive polymers are colored, modifying transparent silica particles with these conductive polymers will lead to the development of new highly transparent conductive hybrid materials.

[0005] In order to obtain hybrid materials, it is necessary to control the polymer end so that it can be modified to silica particles. In this regard, polythiophenes in which one end is blocked using 3-hexylthiophene in the side chain have been produced (Non-Patent Documents 1 to 3), but the resulting polythiophenes have poor solubility in commonly used solvents such as alcohols, making it difficult to apply them to various materials. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2017 / 130905 [Patent Document 2] JP 2018-123295 A [Patent Document 3] JP 2018-127599 A [Non-patent literature]

[0007] [Non-Patent Document 1] Macromolecules, 2004, 37, 1169-1171. [Non-Patent Document 2] Macromol. Rapid Commun., 2004, 25, 1663-1666. [Non-Patent Document 3] J. Am. Chem. Soc., 2005, 127, 17542-17547. Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing a one-end-unsubstituted polythiophene which can be suitably used as a synthetic raw material for polythiophenes or block copolymers having both ends selectively modified and which is soluble in a common organic solvent, and a thiophene compound which can be used for the production of the polythiophene, can be stably stored even after purification, and is soluble in an aqueous organic solvent such as tetrahydrofuran. [Means for solving the problem]

[0009] The present inventors have found that a polythiophene having an unsubstituted 2-position at one end can be obtained by polymerizing a thiophene compound having a boronic acid ester group at the 5-position using an iodobenzene compound as an initiator, and have also found that a terminal-modified polythiophene or a block copolymer can be efficiently synthesized by using this one-end unsubstituted polythiophene, thereby completing the present invention.

[0010] That is, the present invention provides 1. In the presence of a metal catalyst, [ka] (In the formula, R 1 ~R 5 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 5 carbon atoms. The iodobenzene compound represented by the following formula (1) is used as an initiator. [ka] (In the formula, X represents a halogen, and Y represents a monovalent organic group having three or more oxygen atoms.) The thiophene compound represented by the following formula (3) is polymerized. [ka] (In the formula, n represents a natural number, R 1 ~R 5 and Y have the same meaning as above. A method for producing a one-end unsubstituted polythiophene represented by the formula: 2. Mixing the iodobenzene compound represented by the formula (2), potassium phosphate, and a metal catalyst to prepare a mixture A; a method for producing a one-terminal unsubstituted polythiophene according to item 1, which comprises mixing the mixture A obtained, water and a water-soluble organic solvent to prepare a mixture B, and mixing the mixture B with a solution of a thiophene compound represented by formula (1) to polymerize the thiophene compound; 3. A method for producing a one-terminal unsubstituted polythiophene according to 1, wherein Y is a methoxyethoxyethoxymethyl group. 4. A method for producing a one-terminal unsubstituted polythiophene represented by the formula (3) obtained by any one of the production methods 1 to 3, and a compound represented by the following formula (4): [ka] In the presence of a metal catalyst, a vinylphenylboronic acid pinacol ester compound represented by the following formula (5) is reacted with [ka] (In the formula, R 1 ~R 5 , Y and n have the same meanings as above. A method for producing a polythiophene represented by the formula: 5. The method for producing polythiophene according to 4, wherein the vinylphenylboronic acid pinacol ester compound represented by the formula (4) is added to a solution obtained by polymerizing the thiophene compound represented by the formula (1). 6. The polythiophene represented by the formula (5) obtained by the method for producing 4 is reacted with HSi(OR 8 )3(wherein, R 8 represents an alkyl group having 1 to 6 carbon atoms; [ka] (In the formula, R 1 ~R 8 , Y and n have the same meanings as above. 7. A method for producing surface-modified metal oxide particles, comprising reacting the polythiophene having a trialkoxysilyl group at one end and represented by formula (6) obtained by the method for producing 6 with metal oxide particles. 8. A polythiophene represented by the following formula (3), having a number average molecular weight of 1,000 to 100,000 and a molecular weight distribution of 1.3 or less: [ka] (In the formula, n represents a natural number, R 1 ~R 5 each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms, and Y represents a monovalent organic group having three or more oxygen atoms. 9. A polythiophene represented by the following formula (5), having a number average molecular weight of 1,000 to 100,000 and a molecular weight distribution of 1.3 or less: [ka] (In the formula, n represents a natural number, R 1 ~R 5 each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms, and Y represents a monovalent organic group having three or more oxygen atoms. 10. Polythiophene of 8 or 9, wherein Y is a methoxyethoxyethoxymethyl group. 11. A thiophene compound represented by formula (1): [ka] (In the formula, X represents a halogen, and Y represents a monovalent organic group having three or more oxygen atoms.) 12. A polythiophene having a trialkoxysilyl group at one end, represented by the following formula (6) and having a number average molecular weight of 1,000 to 100,000: [ka] (In the formula, n represents a natural number, R 1 ~R 5 each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms; R 8 represents an alkyl group having 1 to 6 carbon atoms, and Y represents a monovalent organic group having 3 or more oxygen atoms. 13. Surface-modified metal oxide particles having polythiophene having one end containing trialkoxysilyl group (12) attached to the surface of the metal oxide particles. to provide. Effect of the Invention

[0011] According to the present invention, a one-end unsubstituted polythiophene can be efficiently obtained. By using this one-end unsubstituted polythiophene, not only can a polythiophene or block copolymer further modified at the unsubstituted end be efficiently produced, but also a polythiophene having a silyl group at the end, which is useful as a surface modification material for inorganic fine particles, can be derived. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in further detail below. [1] Method for producing one-end unsubstituted polythiophene The method for producing a one-end unsubstituted polythiophene represented by the following formula (3) (hereinafter referred to as "polythiophene (3)") according to the present invention is characterized in that a thiophene compound represented by the following formula (1) (hereinafter referred to as "thiophene compound (1)") is polymerized in the presence of a metal catalyst using an iodobenzene compound represented by the following formula (2) (hereinafter referred to as "compound (2)") as an initiator.

[0013] [ka]

[0014] In the above formulas, R 1 ~R 5each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 5 carbon atoms, X represents a halogen, Y represents a monovalent organic group having three or more oxygen atoms, and n represents a natural number, preferably an integer of 2 or more.

[0015] R 1 ~R 5 The alkyl group having 1 to 5 carbon atoms may be either linear or branched, and specific examples thereof include methyl, ethyl, n-propyl, i-propyl, n-butyl, s-butyl, tert-butyl, and n-pentyl. In particular, R 1 ~R 5 As the alkyl group, an alkyl group having 1 to 3 carbon atoms is preferable, and a methyl group is more preferable.

[0016] Examples of the halogen atom for X include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Taking reactivity into consideration, a chlorine atom, a bromine atom, and an iodine atom are preferred, and a bromine atom is more preferred. The organic group of Y is preferably a polyether group, more preferably an organic group having a terminal hydroxyl group, an alkoxy group having 1 to 10 carbon atoms, or a phenoxy group, and bonded to the thiophene skeleton through a carbon atom. 6 -O-((CH2) r O) q -R 7 R is a group, r is 2 or 3 and is the same for all groups within the same substituent, q is an integer of 2 or more, 6 is an alkylene group having 1 to 5 carbon atoms, and R 7 is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a phenyl group, and the total number of carbon atoms, that is, the product of r and q and R 6 and R 7 The sum of the carbon atoms in the substituents is 5 to 20. The alkylene group having 1 to 5 carbon atoms may be either linear or branched, and specific examples thereof include methylene, ethylene, trimethylene and propylene groups, with the methylene group being preferred. The alkyl group having 1 to 10 carbon atoms may be either linear or branched. Specific examples thereof include the above-mentioned R1 ~R 5 In addition to the groups exemplified as the alkyl group having 1 to 5 carbon atoms, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl groups are also included. In particular, as the organic group for Y, a polyether group having 5 to 10 carbon atoms bonded to the thiophene skeleton via a carbon atom is preferable, and a methoxyethoxyethoxymethyl group is even more preferable.

[0017] Specific examples of compound (2) include iodobenzene, 2-iodotoluene, and 4-iodotoluene. The amount of compound (2) used is not particularly limited, but is preferably in the range of 0.002 to 0.2 moles per mole of thiophene compound (1) as a substrate. In consideration of the selectivity and reaction efficiency of the subsequent polymerization reaction, the amount is more preferably in the range of 0.001 to 0.3 moles, and even more preferably in the range of 0.05 to 0.2 moles.

[0018] The metal catalyst used in the present invention may be, for example, a palladium catalyst or nickel catalyst that is suitably used for regioselective polymerization, as listed in RD McCullough, Adv. Mater., 1998, 10(2), 93-116 and the references cited therein. Specific examples include bis(triphenylphosphine)palladium dichloride (Pd(PPh3)Cl2), palladium(II) acetate (Pd(OAc)2), tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), tetrakis(triphenylphosphine)nickel (Ni(PPh3)4), nickel(II) acetylacetonate (Ni(acac)2), dichloro(2,2'-bipyridine)nickel, and dibromobis(triphenylphosphine)nickel (Ni(PPh3)2Br2). Ligand-containing nickel and palladium catalysts can also be used, and specific examples thereof include nickel and palladium catalysts containing tri-t-butylphosphine, triadamantylphosphine, 1,3-bis(2,4,6-trimethylphenyl)imidazolidinium chloride, 1,3-bis(2,6-diisopropylphenyl)imidazolidinium chloride, or 1,3-diadamantylimidazolidinium chloride, chloro(2-dicyclohexylphosphino-2',6'-dimethoxy-1,1'-biphenyl)[2-(2'-amino-1,1'-biphenyl)]palladium(II) (SPhos Pd G2), (2-dicyclohexylphosphino-2',6'-dimethoxybiphenyl)[2-(2'-amino-1,1'-biphenyl)]palladium(II) methanesulfonate (SPhos Pd G3), and the like. Nickel and palladium catalysts in which the ligands are combinations of those listed above can also be used.

[0019] In particular, in the present invention, a palladium catalyst is preferably used, and among them, from the viewpoint of reactivity, SPhos Pd G2 and SPhos Pd G3 are more preferable, and SPhos Pd G2 is even more preferable.

[0020] The amount of the metal catalyst used is not particularly limited, but is typically in the range of 0.1 to 20 mol %, preferably 0.5 to 20 mol %, and more preferably 1 to 10 mol %, based on the amount of the thiophene compound (1).

[0021] In the production method of the present invention, it is preferable to add 2-dicyclohexylphosphino-2',6'-dimethoxybiphenyl (SPhos) to the reaction system in order to promote the catalytic effect. The amount of the added thiophene compound (1) is typically 0.2 to 40 mol%, preferably 1.0 to 40 mol%, more preferably 2.0 to 20 mol%. Furthermore, in the production method of the present invention, it is preferable to add tripotassium phosphate to the reaction system in an amount of typically 1 to 50 moles, preferably 2 to 25 moles, more preferably 5 to 15 moles, per mole of thiophene compound (1).

[0022] The solvent used in the polymerization reaction is not particularly limited as long as it does not adversely affect the reaction, and examples thereof include saturated aliphatic hydrocarbons such as pentane, hexane, heptane, octane, nonane, decane, and cyclohexane; aromatic hydrocarbons such as benzene, toluene, ethylbenzene, propylbenzene, o-xylene, m-xylene, p-xylene, o-ethyltoluene, m-ethyltoluene, and p-ethyltoluene; and ethers such as dimethyl ether, ethyl methyl ether, diethyl ether, dipropyl ether, butyl methyl ether, t-butyl methyl ether, dibutyl ether, cyclopentyl methyl ether, diphenyl ether, tetrahydrofuran (THF), 2-methyltetrahydrofuran, and 1,4-dioxane. These may be used alone or in combination of two or more. Among them, water-soluble organic solvents are preferred, and tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, and the like are more preferred.

[0023] In the production method of the present invention, it is preferable to carry out the reaction in a water-containing system in order to activate the metal catalyst used. In this case, it is more preferable to add water, particularly pure water, after the addition of the solvent used.

[0024] The temperature of the polymerization reaction is not particularly limited, but taking into consideration the reactivity of the leaving group, it is preferably about -20 to 80°C, more preferably about -10 to 70°C, and more preferably about -5 to 60°C. After the polymerization reaction, the reaction is quenched with an acid such as hydrochloric acid to obtain polythiophene (3). In this case, the concentration of the acid is not particularly limited, and is usually about 1 to 12M, preferably about 3 to 10M, and more preferably about 4 to 7M. After quenching with acid, the pure polythiophene (3) can be obtained by conventional post-treatment and purification. This polythiophene (3) is characterized by a number average molecular weight of 1,000 to 100,000 and a molecular weight distribution of 1.3 or less. The number average molecular weight is a polystyrene-equivalent value measured by GPC (hereinafter the same).

[0025] In the production method of the present invention, the initiator compound (2), the thiophene compound (1), the metal catalyst, the solvent, etc. may be added in any order, but it is preferable to use the following method. That is, in this method, compound (2), tripotassium phosphate, and a metal catalyst such as a palladium catalyst are mixed to prepare mixture A, and the obtained mixture A, water, and a water-soluble organic solvent are mixed to prepare mixture B, which is then mixed with a solution of thiophene compound (1) to polymerize thiophene compound (1). In this case, the methods for preparing mixtures A and B and the method for mixing mixture B with a solution of thiophene compound (1) are also arbitrary. However, a preferred method is to add a water-soluble organic solvent to mixture A prepared by mixing compound (2), tripotassium phosphate, and a metal catalyst, and then add water dropwise to prepare mixture B, and then add this mixture B to a solution of thiophene compound (1) in a water-soluble organic solvent to polymerize thiophene compound (1).

[0026] The compound (2) and the metal catalyst to be used may be commercially available products or those produced by a conventionally known method. As described in detail in the Examples, the thiophene compound (1) can be obtained by converting a 2-halogenated thiophene compound represented by the following formula (A) into a compound represented by the formula (B), and then reacting the compound with N-methyliminodiacetic acid.

[0027] [ka] (In the formula, X and Y have the same meanings as above.)

[0028] [2] Synthesis of polythiophene with both ends modified The polythiophene (3) obtained by the above-mentioned production method can be modified by using the hydrogen atom at the 2-position of the thiophene ring remaining at the terminal thereof. For example, polythiophene (3) can be subjected to a coupling reaction with a vinylphenylboronic acid pinacol ester compound (hereinafter referred to as "compound (4)") represented by formula (4) in the presence of a metal catalyst to obtain a polythiophene (hereinafter referred to as "polythiophene (5)") modified at both ends (hereinafter referred to as "polythiophene (5)") represented by formula (5). In this case, polythiophene (5) also has the characteristics of a number average molecular weight of 1,000 to 100,000 and a molecular weight distribution of 1.3 or less.

[0029] [ka] (In the formula, R 1 ~R 5 , Y and n have the same meanings as above.)

[0030] Specific examples of metal catalysts include ligand-containing nickel and palladium catalysts, with palladium catalysts being preferred. Specific examples of these catalysts include those similar to those exemplified in the polymerization reaction above. In the coupling reaction, too, SPhos Pd G2 and SPhos Pd G3 are more preferred from the viewpoint of reactivity, with SPhos Pd G2 being even more preferred. The amount of the catalyst used may be a so-called catalytic amount, and is preferably 40 mol % or less, more preferably 20 mol % or less, based on the raw material polythiophene (3). The above coupling reaction can also be carried out by adding compound (4) directly to a solution obtained by polymerizing thiophene compound (1) without isolating polythiophene (3). In this case, it is not necessary to newly add a metal catalyst used in the coupling reaction.

[0031] Also during the coupling reaction, tripotassium phosphate is preferably added to the system in an amount of typically 0.1 to 10 moles, preferably 0.5 to 5 moles, and more preferably 1 to 3 moles, per mole of the raw material polythiophene (3).

[0032] In the above coupling reaction, a base can also be used. Specific examples thereof include inorganic bases such as sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium hydrogen carbonate, potassium hydrogen carbonate, potassium phosphate, sodium carbonate, potassium carbonate, lithium carbonate, and cesium carbonate; amines such as methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, propylamine, dipropylamine, tripropylamine, isopropylamine, diisopropylamine, triisopropylamine, butylamine, dibutylamine, tributylamine, diisopropylethylamine, pyridine, imidazole, quinoline, collidine, pyrrolidine, piperidine, morpholine, and N-methylmorpholine; sodium acetate, potassium acetate, and lithium acetate. When a base is used, its amount is not particularly limited, but is preferably about 1 to 10 moles per mole of the starting polythiophene (3).

[0033] The reaction solvent is not particularly limited as long as it is stable under the reaction conditions and does not adversely affect the reaction, and examples thereof include water; alcohols such as methanol and ethanol; amines such as triethylamine; aprotic polar organic solvents such as dimethylformamide, dimethylsulfoxide, dimethylacetamide, and N-methylpyrrolidone; ethers such as diethyl ether, diisopropyl ether, methyl t-butyl ether, cyclopentyl methyl ether, THF, and 1,4-dioxane; aliphatic hydrocarbons such as pentane, hexane, heptane, and petroleum ether; aromatic hydrocarbons such as benzene, toluene, xylene, mesitylene, chlorobenzene, dichlorobenzene, nitrobenzene, and tetralin; halogenated hydrocarbons such as chloroform, dichloromethane, carbon tetrachloride, and dichloroethane; lower fatty acid esters such as methyl acetate, ethyl acetate, butyl acetate, and methyl propionate; and nitriles such as acetonitrile, propionitrile, and butyronitrile. These solvents can be appropriately selected in consideration of the ease of reaction, and may be used alone or in combination of two or more. The above-mentioned solvents may be used as water-free solvents by using an appropriate dehydrating agent or drying agent.

[0034] The reaction temperature can be from -100°C to the boiling point of the reaction solvent used, preferably from -50 to 200°C, more preferably from 20 to 150°C. The reaction time is usually about 0.1 to 1,000 hours, preferably 0.5 to 100 hours. After completion of the reaction, the reaction mixture is post-treated and, if necessary, purified according to a conventional method to obtain polythiophene (5).

[0035] [3] Synthesis of polythiophene having silyl groups at the terminals The polythiophene (5) obtained by the above-mentioned production method can be derived into a polythiophene compound having a silyl group, such as a trialkoxysilyl group, at the terminal, by using the terminal alkenyl group as a foothold. For example, polythiophene (5) was reacted with HSi(OR 8)3(wherein, R 8 represents an alkyl group having 1 to 6 carbon atoms.) to obtain a polythiophene having a trialkoxysilyl group at one end represented by the following formula (6) (hereinafter referred to as "polythiophene (6)." In this case, polythiophene (6) also has the characteristics of a number average molecular weight of 1,000 to 100,000 and a molecular weight distribution of 1.3 or less.

[0036] [ka] (In the formula, R 1 ~R 8 , Y and n have the same meanings as above.)

[0037] Above R 8 Specific examples of the alkyl group having 1 to 6 carbon atoms may be either linear or branched, and specific examples thereof include methyl, ethyl, n-propyl, i-propyl, n-butyl, s-butyl, tert-butyl, n-pentyl, and n-hexyl groups. In particular, R 1 ~R 5 As the alkyl group, an alkyl group having 1 to 3 carbon atoms is preferable, and a methyl group is more preferable. Specific examples of trialkoxysilanes include trimethoxysilane, triethoxysilane, tri-n-propoxysilane, and tri-i-propoxysilane.

[0038] Specific examples of platinum catalysts include chloroplatinic acid, platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex, tetrakistriphenylphosphine platinum, dichlorobistriphenylphosphine platinum, dichlorobisacetonitrile platinum, dichlorobisbenzonitrile platinum, dichlorocyclooctadiene platinum, and platinum-activated carbon.

[0039] The amount of the platinum catalyst used is, for example, preferably from 0.0001 to 2 mol, and more preferably from 0.01 to 1 mol, per 1 mol of the polythiophene (6).

[0040] The reaction temperature is not particularly limited, but is preferably 0 to 100° C., more preferably 10 to 50° C. The reaction time is also not particularly limited, but is preferably 0.1 to 10 hours, more preferably 0.2 to 5 hours. The reaction atmosphere is preferably an inert gas atmosphere such as nitrogen or argon. After the reaction, the target product can be recovered by distillation, reprecipitation purification, or the like.

[0041] A solvent can be used in the reaction. Examples of the solvent include ether solvents such as diethyl ether, tetrahydrofuran, and dioxane, ester solvents such as ethyl acetate and butyl acetate, and aprotic polar solvents such as acetonitrile, N,N-dimethylformamide, and N-methylpyrrolidone. These solvents may be used alone or in combination of two or more.

[0042] [4]Surface-modified metal oxide fine particles The polythiophene (6) obtained by the above-mentioned production method can be used as a surface treatment agent for metal oxides by taking advantage of its terminal trialkoxysilyl group, and as a result, metal oxide fine particles whose surfaces are modified with polythiophene can be obtained. The metal oxide particles are not particularly limited, and may be appropriately selected from various conventionally known metal oxides such as SiO2, SnO2, TiO2, WO3, ZnO, ZrO2, In2O3, Sb2O5, etc., depending on the application, etc. From the viewpoints of versatility and transparency, SiO2 is preferred. The size of the metal oxide particles is not particularly limited, but from the viewpoint of versatility, it is preferably 5 nm to 10 μm, from the viewpoint of elastic modulus, it is more preferably 10 nm to 10 μm, and from the viewpoint of transparency, it is even more preferably 10 to 100 nm, and further preferably 10 to 50 nm.

[0043] The method for modifying the surface of metal oxide particles with polythiophene (6) can be a known method, and an example of such a method includes adding polythiophene (6) to a dispersion of metal oxide particles, heating the mixture to 50 to 80° C., and treating the mixture for 1 to 10 hours. EXAMPLES

[0044] The present invention will be described in more detail below with reference to synthesis examples and examples, but the present invention is not limited to the following examples. The measuring devices used in the examples are as follows. [GPC] Equipment: Shodex GPC-101 (Showa Denko Co., Ltd.) Column: Shodex KF-804L x 2 (Showa Denko Co., Ltd.) Column temperature: 40℃ Solvent: Chloroform 1mL / min Detector: UV (254 nm), RI Calibration curve: Standard polystyrene [ 1 H-NMR] Equipment: JEOL ECA-500 and ECA-600 [ 13 C-NMR] Equipment: JEOL ECA-500 and ECA-600 [IR] Equipment: JASCO FT / IR-410 [TG-DTA] Equipment: Seiko Instruments Inc. TG / DTA 6200 [MALDI-TOFF] Equipment: AXIMA-CFR plus Shimadzu / Kratos Reflection ion mode: Laser (λ=337nm) Matrix:1,8-dihydroxy-9[10H]-anthracenone

[0045] [Synthesis Example 1]: Synthesis of compound (a) [ka]

[0046] The reaction was carried out in a 100 mL recovery flask. Into a flask, 6.1661 g (51.3 mmol) of diethylene glycol monomethyl ether and 2.765 g (69.1 mmol) of sodium hydroxide were added and stirred at 0°C. In a separately prepared 50 mL eggplant flask, 7.810 g (50.0 mmol) of p-toluenesulfonyl chloride and 30 mL of THF were added and stirred, and then added to the solution in the previously prepared 100 mL eggplant flask. After stirring at room temperature for 20 hours, 1 M hydrochloric acid was added, extracted with methylene chloride, washed with a saturated aqueous solution of sodium bicarbonate, and dried over anhydrous magnesium sulfate. After filtration and distillation of the solvent under reduced pressure, 12.288 g of compound (a) was obtained as a colorless, transparent liquid (crude yield 109%). Various spectral data of compound (a) are shown below.

[0047] 1 H NMR(600MHz, CDCl3) δ 7.80(d, J=8.4Hz, 2H), 7.34(d, J=7.8Hz, 2H), 4.17(t, J=5.1Hz, 2H), 3.69(t, J=4.8Hz, 2H), 3.58(t, J=4.5Hz, 2H), 3.48(t, J=4.5Hz, 2H), 3.35(s, 2H),2.45(s, 2H) 13 C NMR(150MHz, CDCl3) δ 144.7, 132.7, 129.6, 127.7, 71.6, 70.4, 69.1, 68.4, 58.8,21.4 IR (neat) 2881, 1598, 1452, 1358, 1292, 1177, 1111, 1018, 923, 817, 777, 664, 555 cm -1 .

[0048] [Synthesis Example 2]: Synthesis of compound (b) [ka]

[0049] The reaction was carried out in a 50 mL recovery flask. In a flask, 2.9029 g (25.4 mmol) of 3-thiophenemethanol, 8.391 g (30.6 mmol) of compound (a), 0.8221 g (2.55 mmol) of tetrabutylammonium bromide (TBAB), 5.7150 g (101.9 mmol) of finely crushed potassium hydroxide, and 1 mL of water were added and stirred. After the potassium hydroxide had dissolved to some extent, 25 mL of THF was added. After stirring at room temperature for 45.5 hours, water was added, and the mixture was extracted with methylene chloride, washed with saturated sodium bicarbonate, and dried over anhydrous magnesium sulfate. The crude product obtained by filtration and distilling off the solvent under reduced pressure was purified by column chromatography (SiO2; ethyl acetate / hexane = 1 / 1 (v / v)) to obtain 5.1321 g (90% yield) of compound (b) as a pale yellow liquid. Various spectral data of compound (b) are shown below.

[0050] 1 H NMR (600MHz, CDCl3) δ 7.29(dd, J=4.8 and 3.0Hz, 1H), 7.22(s, 1H), 7.08(d, J=4.8Hz, 1H), 4.58(s, 2H), 3.68-3.63 (m, 6H), 3.56(t, J=4.5Hz, 2H), 3.39(s, 3H) 13 C NMR (150MHz,CDCl3) δ 139.3, 127.2, 125.8, 122.7, 71.8, 70.5, 70.4, 69.2, 58.9 IR (neat) 2873, 1350, 1103, 856, 781 cm -1 .

[0051] [Synthesis Example 3] Synthesis of compound (c) [ka]

[0052] The reaction was carried out in a brown 100 mL recovery flask wrapped in aluminum foil. Compound (b) 5.022g (23.2mmol) and THF 70mL were added to a flask and stirred at 0℃. N-bromosuccinimide 3.9230g (22.0mmol) was added thereto and stirred at 0℃ for 16.5 hours, after which water was added, THF was removed under reduced pressure, extracted with hexane, washed with 10% aqueous sodium thiosulfate solution, and dried over anhydrous magnesium sulfate. The crude product obtained by filtration and removing the solvent under reduced pressure was distilled at 125-130℃ using a ribbon heater to obtain compound (c) 5.4637g (yield 84%) as a transparent liquid. Various spectral data of compound (c) are shown below.

[0053] 1 H NMR (400MHz, CDCl3) δ 7.24 (d, J=8.8Hz, 1H), 7.00(d, J=5.6Hz, 1H), 4.51(s, 2H), 3.66-3.64(m, 6H), 3.56(t, J=4.6Hz, 2H), 3.39(s, 3H) 13 C NMR (100MHz, CDCl3) δ 138.0, 128.0,125.7, 110.9, 71.7, 70.3, 69.2, 66.9, 58.8 IR (neat) 3103, 2873, 1456, 1416, 1350, 1120, 1106, 992, 826, 734, 690 cm -1 .

[0054] [Synthesis Example 4] Synthesis of compound (d) [ka]

[0055] The reaction was carried out under an argon atmosphere and nitrogen flow using a 20 mL eggplant flask equipped with a three-way cock. 0.285 mL (2.03 mmol) of diisopropylamine and 5.5 mL of THF were added to the flask and stirred at -78 ° C. 0.675 mL (1.86 mmol) of 2.76 M n-butyllithium hexane solution was added dropwise thereto and stirred at -78 ° C for 45 minutes to synthesize LDA. 0.5024 g (1.70 mmol) of compound (c) was added to a 10 mL pear flask equipped with a three-way cock under an argon atmosphere and nitrogen flow, replaced with argon, added 2.76 mL of THF under nitrogen flow, and stirred at -78 ° C. The solution of compound (c) was added dropwise to the LDA solution at -78 ° C for 20 minutes. After stirring at -78°C for 45 minutes, 0.93mL (4.05mmol) of trimethylborate was added dropwise under a nitrogen stream, the mixture was returned to room temperature, and stirred for 41 hours. 6mL of 1M hydrochloric acid was added, the mixture was stirred for 15 minutes, and the organic layer and aqueous layer were separated using a separatory funnel. The organic layer was washed with a saturated aqueous solution of ammonium chloride. The combined aqueous layer was extracted with ether, and the combined organic layer was washed with a saturated aqueous solution of sodium chloride. The mixture was dried over anhydrous sodium sulfate, filtered, and the solvent was distilled off under reduced pressure to obtain 0.5346g (yield 93%) of crude product of compound (d). Various spectral data of compound (d) are shown below.

[0056] 1 H NMR (400MHz, DMSO-d6) δ 8.37(s, 2H), 7.56(s, 1H), 4.40(s, 2H), 3.54-3.50(m, 6H), 3.42(t, J=5.0Hz, 2H), 3.23(s, 3H) 13 C NMR (100MHz, DMSO-d6) δ 138.5, 128.7, 127.2, 110.3, 71.3, 69.7, 69.7, 69.3, 66.2, 58.1; IR (neat) 3232, 2872, 2364, 2257, 1448, 1280, 1198, 1029, 992, 928, 883, 825, 730, 647, 549 cm -1 .

[0057] [Example 1] Synthesis of compound (e) [ka]

[0058] The reaction was carried out in a 100 mL recovery flask equipped with a three-way cock under an argon atmosphere and a nitrogen stream. A flask was charged with 4.066 g (10.2 mmol) of compound (d), 4.4974 g (30.6 mmol) of N-methyliminodiacetic acid, and 4.6 g of 4A molecular sieves. The atmosphere was replaced with argon, and 120 mL of dry DMF was added under a nitrogen stream. After stirring at 120°C for 26 hours, the mixture was cooled to room temperature, water was added, and the 4A molecular sieves were removed by filtration. The solution was poured into a separatory funnel, 1 M hydrochloric acid was added, extracted with chloroform, washed with a saturated aqueous sodium chloride solution, and dried over anhydrous magnesium sulfate. The crude product obtained by filtering and distilling off the solvent under reduced pressure was purified by column chromatography (SiO2; ethyl acetate) to obtain 2.5454 g of a white solid (yield 56%, mp 62-63°C). Compound (e) 1 The H-NMR spectrum data is shown below.

[0059] 1 H NMR (400MHz, DMSO-d6) δ 7.14(s, 1H), 4.40(s, 1H), 4.38-4.33(d, J=17.2Hz, 2H), 4.16-4.12(d, J=17.2Hz, 2H), 3.54-3.50(m, 6H), 3.44-3.41(m, 2H), 3.23(s, 3H), 2.67(s, 3H).

[0060] [Example 2] Synthesis of one-end unsubstituted polythiophene (f) [ka]

[0061] The reaction was carried out in a 20 mL recovery flask equipped with a three-way stopcock. To a flask, 44.5 mg (0.099 mmol) of compound (e) was added, the atmosphere was replaced with argon, 8.5 mL of dry THF was added under a nitrogen stream, and after degassing, the atmosphere was replaced with argon and stirred at 45°C. In a 5mL pear-shaped flask equipped with a three-way cock, 2.09mg (0.0096mmol) of 2-iodotoluene, 214.0mg (1.01mmol) of tripotassium phosphate, 3.67mg (0.0089mmol) of SPhos, and 3.63mg (0.0050mmol) of SPhos Pd G2 were added and replaced with argon (mixture A). 1.0mL of dry THF and 0.36mL of distilled water were added thereto under a nitrogen stream, and after degassing, the mixture was replaced with argon and stirred at 50°C for 2 hours (mixture B). Using a cannula under a nitrogen stream, mixture B was added to the solution of compound (e) and stirred at 45°C for 19 hours. 6M hydrochloric acid was added, extracted with chloroform, washed with a saturated aqueous sodium chloride solution, and dried over anhydrous magnesium sulfate. The crude product obtained by filtration and distilling off the solvent under reduced pressure was purified by precipitation purification (chloroform / hexane, ether) to obtain 19.1 mg (yield 87%) of one-terminal unsubstituted polythiophene (f) as a black-red solid. GPC of the obtained product was measured (M n =5,060,M w / M n = 1.16). One-end unsubstituted polythiophene (f) 1 The H-NMR spectrum data is shown below.

[0062] 1 H NMR (400MHz, CDCl3) δ 7.44-7.42(m, 1H), 7.25(m, n H), 7.24-7.23(m, 3H), 4.67 (s, 2n H), 3.74-3.63(m, 6n H), 3.57-3.54(m, 2n H), 3.37(s, 3n H), 2.49(s, 3H).

[0063] [Example 3] Synthesis of polythiophene (g) modified at both ends [ka]

[0064] The reaction was carried out in a 20 mL recovery flask equipped with a three-way stopcock. To a flask, 45.0 mg (0.10 mmol) of compound (e) was added, the atmosphere was replaced with argon, 8.5 mL of dry THF was added under a nitrogen stream, and after degassing, the atmosphere was replaced with argon and stirred at 45°C. In a 5mL pear-top flask equipped with a three-way cock, 2.76mg (0.012mmol) of 2-iodotoluene, 212.0mg (1.00mmol) of tripotassium phosphate, 3.31mg (0.0080mmol) of SPhos, and 3.82mg (0.0053mmol) of SPhos Pd G2 were added and replaced with argon (mixture A). Under a nitrogen stream, 1.0mL of dry THF and 0.36mL of distilled water were added, degassed, replaced with argon, and stirred at 50℃ for 2 hours (mixture B). Using a cannula under a nitrogen stream, mixture B was added to the solution of compound (e), and the polymerization reaction was carried out by stirring at 45℃ for 21.5 hours.

[0065] In addition, 24.55 mg (0.11 mmol) of 4-vinylphenylboronic acid pinacol ester and 42 mg (0.20 mmol) of tripotassium phosphate were added to a 5 ml pear-shaped flask equipped with a three-way cock and purged with argon. 2.0 mL of dry THF and 0.2 mL of distilled water were added under a nitrogen stream, and the mixture was degassed, purged with argon, and stirred at 45°C. This solution was added to the solution obtained after the previous polymerization reaction using a cannula under a nitrogen stream and stirred overnight at 45°C. 6 M hydrochloric acid was added, extracted with chloroform, washed with a saturated aqueous sodium chloride solution, and dried over anhydrous magnesium sulfate. The crude product obtained by filtering and distilling off the solvent under reduced pressure was purified by precipitation purification (chloroform / hexane, ether) to obtain 19.7 mg (yield 88%) of polythiophene modified at both ends as a reddish-white solid. GPC and MALDI-TOF MS of the obtained product were measured (M n =5,020,M w / M n = 1.17). As a result, it was confirmed that the desired polythiophene with both ends capped and a narrow molecular weight distribution was obtained. 1 The H-NMR spectrum data is shown below.

[0066] 1 H NMR (400MHz, CDCl3) δ 7.54-7.51 (d, J=8.0Hz, 2H), 7.48-7.46(d, J=8.0Hz, 2H), 7.44-7.41(m, 1H), 7.25 (m, n H), 7.23-7.22 (m, 3H), 6.78-6.72 (dd, J=10.8 and 17.8Hz, 1H), 5.83-5.79(d, J=18.0Hz, 1H), 5.32-5.29(d, J=11.2Hz, 1H), 4.66(s, 2n H), 3.74-3.67(m, 6n H), 3.57-3.55(m, 2n H), 3.37(s, 3nH), 2.49(s, 3H).

[0067] [Example 4] Synthesis of polythiophene with triethoxysilane (h) [ka]

[0068] The reaction was carried out in a glove box using a 10 mL eggplant flask equipped with a three-way cock heated with a heat gun under reduced pressure drying. 5.8 mg (0.011 mmol) of HPtCl6·6H2O was added to the flask. 25.3 mg (0.011 mmol) of polythiophene (g) modified at both ends and 5 ml of dry THF were added to a separately prepared vial. The latter solution and 30.22 ml (1.07 mmol) of HSi(OEt) were added to the former flask and stirred at room temperature for 30 minutes. The flask was removed from the glove box and stirred at 55°C for 5 hours. The solvent was distilled off under reduced pressure, and precipitation purification was performed with good solvent dry THF and poor solvent dry hexane under a nitrogen stream to obtain 17.5 mg (65% yield) of the desired polythiophene (h) with triethoxysilane. 1 The H-NMR spectrum data is shown below.

[0069] 1H NMR (400 MHz, CDCl3) δ 7.48-7.46 (d, J = 8.0 Hz, 2 H), 7.44-7.42 (m, 1 H), 7.25 (s, n H), 7.23-7.22 (m, 5 H), 7.13 (s, 1 H), 4.69-4.67 (m, 2n H), 4.53 (m, 2 H), 3.74-3.67 (m, 6n H), 3.74-3.67 (m, 6 H), 3.58-3.55 (m 2n H), 3.38-3.36 (s, 3n H), 2.73-2.65 (m, 2 H) 2.50 (s, 3 H), 1.31-1.26 (m,9 H), 0.90-0.83 (m, 2 H).

[0070] [Example 5] Synthesis of polythiophene-attached silica sol (j) 12 g of 1,3-dimethylimidazolidinone (hereinafter referred to as DMI) was added to 10 g of MT-ST (methanol silica sol manufactured by Nissan Chemical Industries, Ltd.), and the methanol was removed using an evaporator to obtain a DMAI sol (i). Next, 1 ml of a THF solution in which 60 mg of the polythiophene with triethoxysilane (h) prepared in Example 4 was dissolved was added, and the THF was removed using an evaporator. After that, the mixture was heated at 70°C for 5 hours to obtain the target polythiophene DMI sol (j). As a result of checking the methanol solubility of the polythiophene with triethoxysilane (h) THF solution and the polythiophene DMI sol (j), the polythiophene with triethoxysilane (h) THF solution precipitated, but the polythiophene DMI sol (j) did not precipitate, and it was confirmed that the polythiophene with triethoxysilane (h) reacted with the silica particle surface.

Claims

1. In the presence of a metal catalyst, 【Chemistry 1】 (In the formula, R 1 ~R 5 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 5 carbon atoms. The iodobenzene compound represented by the following formula (1) is used as an initiator. 【Chemistry 2】 (In the formula, X represents a halogen, and Y represents a monovalent organic group having three or more oxygen atoms.) The thiophene compound represented by the following formula (3) is polymerized. 【Chemistry 3】 (In the formula, n represents a natural number, R 1 ~R 5 and Y have the same meaning as above. A method for producing a one-end unsubstituted polythiophene represented by the following formula:

2. The iodobenzene compound represented by the formula (2), potassium phosphate, and a metal catalyst are mixed to prepare a mixture A, The method for producing one-end unsubstituted polythiophene according to claim 1, further comprising mixing the obtained mixture A, water and a water-soluble organic solvent to prepare a mixture B, and mixing the mixture B with a solution of the thiophene compound represented by the formula (1), thereby polymerizing the thiophene compound.

3. 2. The method for producing a one-terminal unsubstituted polythiophene according to claim 1, wherein the Y is a methoxyethoxyethoxymethyl group.

4. A one-terminal unsubstituted polythiophene represented by the formula (3) obtained by the method according to any one of claims 1 to 3 and a one-terminal unsubstituted polythiophene represented by the following formula (4): 【Chemistry 4】 In the presence of a metal catalyst, a vinylphenylboronic acid pinacol ester compound represented by the following formula (5) is reacted with 【Chemistry 5】 (In the formula, R 1 ~R 5 , Y and n are as defined above.) A method for producing a polythiophene represented by the formula:

5. 5. The method for producing polythiophene according to claim 4, wherein the vinylphenylboronic acid pinacol ester compound represented by the formula (4) is added to a solution in which the thiophene compound represented by the formula (1) has been polymerized.

6. The polythiophene represented by the formula (5) obtained by the method according to claim 4 is reacted with a platinum catalyst to form HSi(OR 8 ) 3 (In the formula, R 8 represents an alkyl group having 1 to 6 carbon atoms. 【Chemistry 6】 (In the formula, R 1 ~R 8 , Y and n are as defined above.)

7. A method for producing surface-polythiophene-modified metal oxide particles, comprising reacting the polythiophene having a trialkoxysilyl group at one end and represented by formula (6) obtained by the method according to claim 6 with metal oxide particles.

8. A polythiophene represented by the following formula (3), having a number average molecular weight of 1,000 to 100,000 and a molecular weight distribution of 1.3 or less: 【Chemistry 7】 (In the formula, n represents a natural number, R 1 ~R 5 each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms, and Y represents a monovalent organic group having three or more oxygen atoms.

9. A polythiophene represented by the following formula (5), having a number average molecular weight of 1,000 to 100,000 and a molecular weight distribution of 1.3 or less: 【Chemistry 8】 (In the formula, n represents a natural number, R 1 ~R 5 each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms, and Y represents a monovalent organic group having three or more oxygen atoms.

10. 10. The polythiophene according to claim 8, wherein Y is a methoxyethoxyethoxymethyl group.

11. A thiophene compound represented by formula (1): 【Chemistry 9】 (In the formula, X represents a halogen, and Y represents a monovalent organic group having three or more oxygen atoms.)

12. A polythiophene having a trialkoxysilyl group at one end, represented by the following formula (6) and having a number average molecular weight of 1,000 to 100,000. 【Chemistry 10】 (In the formula, n represents a natural number, R 1 ~R 5 each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 5 carbon atoms; R 8 represents an alkyl group having 1 to 6 carbon atoms, and Y represents a monovalent organic group having 3 or more oxygen atoms.

13. 13. A surface-modified metal oxide fine particle comprising a metal oxide particle having the polythiophene having a trialkoxysilyl group at one end thereof according to claim 12 attached to the surface of the metal oxide particle.

Citation Information

Patent Citations

  • Aromatic polyamide and surface modifier

    JP2018123295A

  • Hyper-branched aromatic polyamide and surface-modification agent

    JP2018127599A

  • Aromatic polyamide surface modifier of silica sol

    WO2017130905A1