Resin composition, molded product, rotor and motor
A resin composition with thermosetting resin and soft magnetic particles addresses the issue of gap formation during insertion into rotor core holes, enhancing moldability and mechanical strength.
Patent Information
- Application Number
- JP2023078534
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
AI Technical Summary
Inserting a molded body made of a resin composition into the hole of a rotor core often results in gaps due to difficulties in matching the shape of the hole, especially when using sintered bodies.
A resin composition comprising a thermosetting resin and soft magnetic particles, with specific properties such as a content range of soft magnetic particles and a curing catalyst, allowing for insertion into a rotor core by transfer molding, reducing gap formation.
The resin composition effectively reduces gaps during insertion into rotor core holes, improving moldability and mechanical strength while maintaining magnetic properties.
Smart Images

Figure 2024162712000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a molded article, a rotor, and a motor. [Background technology]
[0002] As electrification continues to advance in automobiles, aircraft, and other fields, there is a demand for motors equipped in these vehicles to be more efficient and perform better.
[0003] In recent years, various studies have been conducted to improve the efficiency and performance of motors. Recent motor technologies include, for example, the technology described in Non-Patent Document 1.
[0004] Non-Patent Document 1 describes a motor in which a magnetic composite material is inserted into the flux barrier of the rotor. Non-Patent Document 1 describes that the high efficiency range of 94% can be expanded from 4,000 rpm to 8,000 rpm, and that a variable magnetic flux motor using a magnetic composite material has been realized. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] Mitsuhide Sato and 6 others, "Proposal of a variable magnetic flux motor using magnetic composite material", Institute of Electrical Engineers of Japan Study Group (Rotary Machine Study Group), November 15-16, 2021, RM-21-106, p.23-28 Summary of the Invention [Problem to be solved by the invention]
[0006] As in the technology described in Non-Patent Document 1, a rotor is known that includes a molded body made of a resin composition in the flux barrier section of the rotor core. However, according to the study by the present inventors, it was found that in such a rotor that includes a molded body made of a resin composition in the hole section of the rotor core, it may be difficult to insert the molded body into the hole without leaving any gaps.
[0007] The present invention has been developed in consideration of the above-mentioned circumstances, and provides a resin composition that can reduce the occurrence of gaps in a hole when a molded body made of the resin composition is inserted into the hole of a rotor core. [Means for solving the problem]
[0008] According to the present invention, there are provided a resin composition, a molded article, a rotor, and a motor as described below.
[0009] [1] A resin composition that can be inserted into a hole of a rotor core by transfer molding, A magnetic material comprising a thermosetting resin (A) and soft magnetic particles (B), The resin composition is a solid at 25°C. [2] The resin composition according to [1], wherein the content of the soft magnetic particles (B) in the resin composition is 50% by volume or more and 90% by volume or less, when the entire resin composition is 100% by volume. [3] The resin composition according to the above [1] or [2], wherein the soft magnetic particles (B) contain Si elements. [4] The resin composition according to any one of the above [1] to [3], wherein the soft magnetic particles (B) include crystalline particles. [5] The resin composition according to any one of the above [1] to [4], wherein the soft magnetic particles (B) include amorphous particles. [6] The resin composition according to any one of the above [1] to [5], wherein the soft magnetic particles (B) contain gas-water atomized powder. [7] The resin composition according to any one of the above [1] to [6], wherein the thermosetting resin (A) contains an epoxy resin. [8] The resin composition according to [7] above, wherein the epoxy resin is solid at 25°C. [9] The resin composition according to any one of the above [1] to [8], further comprising a silica filler (C).
[10] The resin composition according to [9], wherein the content of the silica filler (C) in the resin composition is 0.10 mass% or more and 5.00 mass% or less, when the entire resin composition is 100 mass%.
[11] The resin composition according to any one of the above [1] to
[10] , further comprising a phenol-based curing agent (D).
[12] Further comprising a curing catalyst (E), The resin composition according to any one of the above [1] to
[11] , wherein the curing catalyst (E) includes at least one selected from the group consisting of a tetra-substituted phosphonium compound, a phosphobetaine compound, an adduct of a phosphine compound and a quinone compound, and an adduct of a phosphonium compound and a silane compound.
[13] The resin composition according to any one of the above [1] to
[12] , which has a spiral flow at 175° C. of 10 cm or more and 200 cm or less.
[14] The resin composition according to any one of the above [1] to
[13] , which has a gel time at 175° C. of 30 seconds or more and 300 seconds or less.
[15] The resin composition according to any one of the above [1] to
[14] , wherein a cured product of the resin composition has a saturation magnetic flux density at 25° C. of 1.50 T or less.
[16] The resin composition according to any one of [1] to
[15] above, wherein a cured product of the resin composition has a flexural strength of 50 MPa or more and 200 MPa or less at 25°C, as measured in accordance with JIS K 6911 (2006).
[17] The resin composition according to any one of [1] to
[16] above, wherein a cured product of the resin composition has a flexural modulus at 25°C of 20,000 MPa or more and 50,000 MPa or less, as measured in accordance with JIS K 6911 (2006).
[18] The resin composition according to any one of the above [1] to
[17] , wherein a cured product of the resin composition has a glass transition temperature of 100° C. or higher and 250° C. or lower.
[19] The resin composition according to any one of the above [1] to
[18] , which is in a tablet form at 25°C.
[20] The resin composition according to any one of the above [1] to
[19] , wherein the hole of the rotor core is a flux barrier portion. [twenty one] A molded article obtained by curing the resin composition according to any one of the above [1] to
[20] . [twenty two] The molded article according to
[21] above, which is a transfer molded article. [twenty three] A rotor core having a hole, The rotor core has a plate member, A rotor, the hole containing a cured product of the resin composition according to any one of [1] to
[20] above. [twenty four] The rotor according to
[23] , wherein the rotor core has a laminate in which a plurality of the plate members are stacked. [twenty five] The rotor according to
[23] or
[24] , wherein the plate member is an electromagnetic steel plate.
[26] The rotor according to any one of the above
[23] to
[25] , wherein a saturation magnetic flux density at 25° C. of a cured product made of the resin composition is smaller than a saturation magnetic flux density at 25° C. of the plate member.
[27] The rotor core further includes a magnet insertion portion for inserting a magnet, The rotor according to any one of the above
[23] to
[26] , wherein the hole is a hole independent of the magnet insertion portion.
[28] The rotor core further includes a magnet insertion portion for inserting a magnet, The rotor according to any one of the above
[23] to
[26] , wherein the hole is a hole that is continuous with the magnet insertion portion.
[29] A motor comprising the rotor according to any one of
[23] to
[28] . Effect of the Invention
[0010] According to the present invention, it is possible to provide a resin composition that can reduce the occurrence of gaps in a hole when a molded article made of the resin composition is inserted into the hole of a rotor core. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a plan view illustrating an example of a rotor according to the present embodiment. [Diagram 2] FIG. 2 is a plan view illustrating an example of a rotor according to the present embodiment. [Diagram 3] FIG. 2 is a cross-sectional view illustrating an example of a rotor according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Furthermore, a numerical range of "A to B" represents A or more and B or less unless otherwise specified.
[0013] As described above, there is known a rotor that includes a molded body made of a resin composition in the flux barrier section of the rotor core, as in the technology described in Non-Patent Document 1. Here, Non-Patent Document 1 describes a magnetic composite material obtained by mixing magnetic powder and resin and sintering the mixture as the molded body made of the resin composition.
[0014] One possible method for inserting a sintered compact into a hole (e.g., a flux barrier portion, etc.) of a rotor core is to insert a sintered compact that has been machined to fit the shape of the hole into the hole. According to the study of the present inventors, it was found that in the method of cutting the sintered body, when the shape of the hole of the hole part is rounded, it may be difficult to process the sintered body to match the shape of the hole of the hole part. If the sintered body cannot be processed to match the shape of the hole, it is difficult to insert the sintered body into the hole part without leaving a gap.
[0015] The present invention has been developed in consideration of the above-mentioned circumstances, and provides a resin composition that can reduce the occurrence of gaps in a hole when a molded body made of the resin composition is inserted into the hole of a rotor core.
[0016] Fig. 1 and Fig. 2 are plan views each showing a typical example of a rotor according to the present embodiment. Fig. 3 is a cross-sectional view showing a typical example of a rotor according to the present embodiment. Note that the drawings are simplified and do not correspond to the actual dimensional ratio.
[0017] [Resin composition] The resin composition of this embodiment is a resin composition that can be inserted into the hole of a rotor core by transfer molding, and contains a thermosetting resin (A) and soft magnetic particles (B), and the resin composition is solid at 25°C.
[0018] The hole of the rotor core means a hole formed in a direction perpendicular to the surface direction of the rotor core, and may or may not be a through hole. The holes of the rotor core of the present embodiment are preferably flux barrier portions. The flux barrier portion refers to a hole for forming a magnetic gap.
[0019] A resin composition that can be inserted into the hole of a rotor core by transfer molding means, for example, a resin composition that can be inserted into the hole of a rotor core by using a transfer molding device, placing the rotor core as a mold for the transfer molding device, inserting a molten resin composition directly into the hole, and holding it as is to harden the molten resin; a resin composition that can be inserted into the hole of a rotor core by using a transfer molding device to create a molded body made by hardening a resin composition that matches the shape of the hole, and inserting the resulting molded body into the hole; etc.
[0020] The spiral flow of the resin composition of this embodiment at 175°C is preferably 10 cm or more, more preferably 20 cm or more, even more preferably 25 cm or more, even more preferably 30 cm or more, even more preferably 40 cm or more, and is preferably 200 cm or less, more preferably 180 cm or less, even more preferably 170 cm or less, even more preferably 160 cm or less. When the spiral flow of the resin composition at 175° C. is equal to or greater than the above lower limit, the flowability of the molten resin composition is good, and the resin composition can easily conform to the shape of the hole. In this specification, the spiral flow of a resin composition at 175° C. means a spiral flow measured by the following measurement method. (Measurement method) Using a low pressure transfer molding machine, the resin composition is injected into a spiral flow measurement mold conforming to ANSI / ASTM D 3123-72, and the flow length (spiral flow) is measured under the following conditions: mold temperature 175°C, injection pressure 6.9 MPa, and pressure dwell time 120 seconds.
[0021] The gel time of the resin composition of this embodiment at 175°C is preferably 30 seconds or more, more preferably 40 seconds or more, even more preferably 45 seconds or more, even more preferably 60 seconds or more, even more preferably 70 seconds or more, and preferably 300 seconds or less, more preferably 250 seconds or less, even more preferably 200 seconds or less, even more preferably 150 seconds or less, even more preferably 120 seconds or less. When the gel time of the resin composition at 175°C is equal to or greater than the lower limit, the time required for the resin composition to harden can be secured, and therefore moldability can be improved, as well as handleability and fillability.When the gel time of the resin composition at 175°C is equal to or less than the upper limit, the time required for the resin composition to harden can be shortened, and therefore production time can be shortened, and productivity can be improved. In this specification, the gel time of a resin composition at 175° C. means the gel time measured by the following measurement method. (Measurement method) The resin composition is placed on a hot plate controlled at 175°C and kneaded with a spatula at one stroke per second. The time from when the resin composition is dissolved by heat to when it hardens is measured, and this is taken as the gel time.
[0022] The glass transition temperature of a cured product made from the resin composition of the present embodiment is preferably 100°C or higher, more preferably 110°C or higher, even more preferably 120°C or higher, and even more preferably 130°C or higher. There is no particular upper limit, but it may be, for example, 250°C or lower, or 200°C or lower. When the glass transition temperature of the cured product made of the resin composition is equal to or higher than the above lower limit, a rotor suitable for use in high-temperature environments can be provided. In this specification, the glass transition temperature of a cured product made of a resin composition means a glass transition temperature measured by the following measurement method. (Measurement method) The resin composition is injected and molded using a low-pressure transfer molding machine at a mold temperature of 175°C, injection pressure of 9.8MPa, and pressure retention time of 300 seconds to obtain a rectangular molded body with a width of 10 mm, a thickness of 1.5 mm, and a length of 55 mm. The molded body obtained is then post-cured under atmospheric conditions at 175°C for 4 hours to prepare a test piece for measuring the glass transition temperature. The glass transition temperature of the test piece for measuring the glass transition temperature is measured using a viscoelasticity measuring device under conditions of a measurement temperature range of 25°C to 300°C and a heating rate of 5°C / min.
[0023] The flexural strength at 25°C of the cured product made of the resin composition of this embodiment is, from the viewpoint of further improving the mechanical strength of the rotor, preferably 50 MPa or more, more preferably 70 MPa or more, and even more preferably 90 MPa or more, and the upper limit is not particularly limited, but may be, for example, 200 MPa or less, 170 MPa or less, or 150 MPa or less. The flexural modulus at 25°C of the cured product made of the resin composition of this embodiment is, from the viewpoint of further improving the mechanical strength of the rotor, preferably 20,000 MPa or more, more preferably 25,000 MPa or more, and even more preferably 27,000 MPa or more, and the upper limit is not particularly limited, but may be, for example, 50,000 MPa or less, or 48,000 MPa or less. In this specification, the flexural strength at 25° C. and the flexural modulus at 25° C. of a cured product made of a resin composition refer to values measured by the following measurement method. (Measurement method) The resin composition is injected and molded using a low-pressure transfer molding machine at a mold temperature of 175°C, injection pressure of 9.8MPa, and pressure retention time of 300 seconds to obtain a rectangular molded body with a width of 10 mm, a thickness of 4 mm, and a length of 80 mm. The molded body obtained is then post-cured under atmospheric conditions at 175°C for 4 hours to prepare a test piece. The flexural strength and flexural modulus at 25°C of the test piece are measured in accordance with JIS K 6911 (2006) at a loading rate of 2 mm / min.
[0024] The saturation magnetic flux density at 25°C of a cured product made of the resin composition of this embodiment is preferably 1.50 T or less, more preferably 1.40 T or less, even more preferably 1.30 T or less, even more preferably 1.20 T or less, even more preferably 1.15 T or less, even more preferably 1.10 T or less, even more preferably 1.05 T or less, and even more preferably 1.00 T or less, and the lower limit is not particularly limited, and may be, for example, 0.20 T or more, or 0.30 T or more. In this specification, the saturation magnetic flux density at 25° C. of a cured product made of a resin composition means a saturation magnetic flux density measured by the following measurement method. (Measurement method) The resin composition is injected and molded using a low-pressure transfer molding machine at a mold temperature of 175°C, injection pressure of 9.8MPa, and pressure retention time of 300 seconds to obtain a cylindrical molded body with a diameter of 16 mmΦ and a height of 32 mm. The molded body is then post-cured under atmospheric conditions at 175°C for 4 hours to prepare a test piece for measuring saturation magnetic flux density. An external magnetic field of 100 kA / m is applied to the test piece for measuring saturation magnetic flux density at room temperature (25°C) using a DC / AC magnetization characteristic tester. The saturation magnetic flux density at 25°C is measured.
[0025] The resin composition of this embodiment is solid at 25°C. The shape of the resin composition of the present embodiment is not particularly limited, but is preferably in the form of a tablet at 25° C. When the resin composition is in the form of a tablet, the storage property and handling property of the resin composition are further improved, and the resin composition is easily applicable to transfer molding. The resin composition of the present embodiment is preferably in an uncured or semi-cured state.
[0026] Hereinafter, each of the components of the resin composition of the present embodiment will be described.
[0027] <Thermosetting resin (A)> The resin composition of the present embodiment contains a thermosetting resin (A). The thermosetting resin (A) is not particularly limited and may include, for example, at least one selected from the group consisting of epoxy resins, oxetane resins, (meth)acrylate resins, unsaturated polyester resins, diallyl phthalate resins, and maleimide resins, and preferably includes an epoxy resin.
[0028] Examples of the epoxy resin include at least one selected from the group consisting of bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, tetramethylbisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol E type epoxy resins, bisphenol M type epoxy resins, bisphenol P type epoxy resins, and bisphenol Z type epoxy resins; novolac type epoxy resins such as phenol novolac type epoxy resins and cresol novolac type epoxy resins; biphenyl type epoxy resins, biphenyl aralkyl type epoxy resins, aryl alkylene type epoxy resins, naphthalene type epoxy resins, anthracene type epoxy resins, phenoxy type epoxy resins, dicyclopentadiene type epoxy resins, norbornene type epoxy resins, adamantane type epoxy resins, fluorene type epoxy resins, trisphenylmethane type epoxy resins, and xyloc type epoxy resins.
[0029] The epoxy resin preferably includes at least one selected from the group consisting of bisphenol A type epoxy resin, trisphenylmethane type epoxy resin, biphenyl aralkyl type epoxy resin, cresol novolac type epoxy resin, Xylok type epoxy resin, and biphenyl type epoxy resin, more preferably includes at least one selected from the group consisting of triphenylmethane type epoxy resin, biphenyl aralkyl type epoxy resin, and cresol novolac type epoxy resin, and further preferably includes a biphenyl aralkyl type epoxy resin.
[0030] The epoxy resin is preferably a solid at 25° C. When the epoxy resin is a solid at 25° C., it becomes easy to prepare a resin composition that is a solid at 25° C., a resin composition that is in a tablet form at 25° C., or the like.
[0031] The content of the thermosetting resin (A) in the resin composition, when the entire resin composition is taken as 100 mass%, is preferably 0.50 mass% or more, more preferably 1.00 mass% or more, even more preferably 1.50 mass% or more, even more preferably 1.80 mass% or more, even more preferably 2.00 mass% or more, even more preferably 2.20 mass% or more, and is preferably 10.00 mass% or less, more preferably 8.00 mass% or less, even more preferably 6.00 mass% or less, and even more preferably 4.00 mass% or less.
[0032] The resin composition of the present embodiment may contain only one type of thermosetting resin (A), or may contain two or more types of thermosetting resins (A). In addition, even if the thermosetting resins (A) are the same type, those having different molecular weights may be used in combination.
[0033] <Soft magnetic particles (B)> The resin composition of the present embodiment contains soft magnetic particles (B). Soft magnetism refers to ferromagnetism with a small coercive force, and generally, ferromagnetism with a coercive force of 800 A / m or less is called soft magnetism. The soft magnetic particles (B) are iron-based particles whose main component is iron atoms (iron atoms have the largest mass content in the chemical composition), and more specifically, are iron alloys whose chemical composition has the largest mass content of iron atoms.
[0034] The soft magnetic particles (B) may contain elements other than iron as constituent elements. The soft magnetic particles (B) contain at least one element selected from the group consisting of B, C, N, O, Al, Si, P, S, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Cd, In, and Sn as an element other than iron, and preferably contain at least one element selected from the group consisting of Si, Ni, and Co, and more preferably contain Si element.
[0035] The soft magnetic particles (B) preferably contain at least one type selected from the group consisting of crystalline particles and amorphous particles. The soft magnetic particles (B) more preferably contain crystalline particles. Moreover, the soft magnetic particles (B) more preferably contain amorphous particles.
[0036] The soft magnetic particles (B) preferably include gas-water atomized powder. The gas-water atomized powder can be prepared by an atomization method using a mixture of water and gas as a pressure fluid. The gas-water atomized powder is a non-spherical atomized powder, which is different from the spherical atomized powder and the irregularly shaped water atomized powder. Gas-water atomized powder has the high sphericity characteristic of gas atomized powder and the high strength of the compacted powder characteristic of water atomized powder, and a resin composition containing gas-water atomized powder as the soft magnetic particles (B) can give a cured product with improved fluidity and moldability as well as improved mechanical strength.
[0037] The particle size of the soft magnetic particles (B) is not particularly limited, but it is preferable to use a combination of large soft magnetic particles with a median size of 20 μm or more and 300 μm or less and small soft magnetic particles with a median size of less than 20 μm. The median diameter of the large particle size soft magnetic particles is preferably 25 μm or more, more preferably 30 μm or more, even more preferably 35 μm or more, and preferably 280 μm or less, more preferably 250 μm or less, even more preferably 200 μm or less, even more preferably 150 μm or less, even more preferably 100 μm or less. The median diameter of the small particle size soft magnetic particles is preferably 18 μm or less, more preferably 15 μm or less, and even more preferably 12 μm or less. The lower limit is not particularly limited, but may be, for example, 0.5 μm or more, or 1 μm or more.
[0038] The median diameter can be obtained, for example, by a laser diffraction / scattering type particle size distribution measuring device. Specifically, the soft magnetic particles (B) are measured in a wet state by a SALD-7500nano manufactured by Shimadzu Corporation, a particle size distribution curve is obtained when the particles are measured on a volume basis, and the median diameter can be obtained by analyzing this distribution curve.
[0039] The content of the soft magnetic particles (B) in the resin composition is preferably 50% by volume or more, more preferably 60% by volume or more, even more preferably 65% by volume or more, and preferably 90% by volume or less, more preferably 85% by volume or less, even more preferably 80% by volume or less, even more preferably 75% by volume or less, when the entire resin composition is taken as 100% by volume. By setting the content [volume %] of the soft magnetic particles (B) in the resin composition within the above range, the saturation magnetic flux density at 25° C. of the cured product made of the resin composition can be adjusted to a more appropriate range.
[0040] The content of the soft magnetic particles (B) in the resin composition, when the entire resin composition is taken as 100% by mass, is preferably 85.00% by mass or more, more preferably 88.00% by mass or more, even more preferably 90.00% by mass or more, and is preferably 98.00% by mass or less, more preferably 97.00% by mass or less, even more preferably 95.00% by mass or less, and even more preferably 94.00% by mass or less. By setting the content [mass %] of the soft magnetic particles (B) in the resin composition within the above range, the saturation magnetic flux density at 25° C. of the cured product made of the resin composition can be adjusted to a more appropriate range.
[0041] The resin composition of the present embodiment may contain only one type of soft magnetic particles (B), or may contain two or more types.
[0042] <Silica filler (C)> The resin composition of the present embodiment preferably further contains a silica filler (C) from the viewpoints of appropriately adjusting the melt viscosity of the resin composition and further improving the fluidity of the melt of the resin composition. The silica filler (C) is not particularly limited and includes, for example, a crystalline silica filler, a fused silica filler, and the like, and among these, a fused silica filler is preferable.
[0043] The median diameter of the silica filler (C) is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 0.4 μm or more, and is preferably 3.0 μm or less, more preferably 2.8 μm or less, even more preferably 2.5 μm or less. The median diameter of the silica filler (C) means the median diameter obtained from a particle size distribution curve measured on a volume basis, and can be measured, for example, using a laser diffraction particle size distribution measuring device.
[0044] The content of the silica filler (C) in the resin composition of this embodiment, when the entire resin composition is taken as 100 mass%, is preferably 0.10 mass% or more, more preferably 0.20 mass% or more, even more preferably 0.25 mass% or more, and is preferably 5.00 mass% or less, more preferably 4.00 mass% or less, even more preferably 3.00 mass% or less, even more preferably 2.00 mass% or less.
[0045] The resin composition of the present embodiment may contain only one type of silica filler (C), or may contain two or more types.
[0046] <Phenol-based hardener (D)> The resin composition of the present embodiment further contains a phenol-based curing agent (D). The phenol-based curing agent (D) preferably contains any skeleton selected from the group consisting of a novolac skeleton and a biphenyl skeleton, from the viewpoint of further improving the durability of the cured product made of the resin composition.
[0047] The phenol-based curing agent (D) preferably contains at least one selected from the group consisting of novolac-type phenolic resins, biphenylaralkyl-type phenolic resins, and xylok-type phenolic resins, and more preferably contains a biphenylaralkyl-type phenolic resin.
[0048] The content of the phenol-based curing agent (D) in the resin composition of the present embodiment is preferably 0.10 mass% or more, more preferably 0.50 mass% or more, even more preferably 1.00 mass% or more, and even more preferably 1.50 mass% or more, and is preferably 10.00 mass% or less, more preferably 8.00 mass% or less, even more preferably 5.00 mass% or less, and even more preferably 3.00 mass% or less.
[0049] The resin composition of the present embodiment may contain only one type of phenol-based curing agent (D), or may contain two or more types.
[0050] <Curing catalyst (E)> The resin composition of the present embodiment preferably further contains a curing catalyst (E). The curing catalyst (E) refers to a component that accelerates the curing reaction of the thermosetting resin (A), and may also be called a curing accelerator. As the curing catalyst (E), at least one selected from the group consisting of phosphorus atom-containing compounds such as organic phosphines, tetra-substituted phosphonium compounds, phosphobetaine compounds, adducts of phosphine compounds and quinone compounds, and adducts of phosphonium compounds and silane compounds; imidazoles (imidazole curing accelerators) such as 2-methylimidazole and 2-phenylimidazole; and nitrogen atom-containing compounds such as amidines and tertiary amines, exemplified by 1,8-diazabicyclo[5.4.0]undecene-7 and benzyldimethylamine, and quaternary salts of amidines and amines, can be used.
[0051] From the viewpoints of appropriately adjusting the gel time of the resin composition and further improving the mechanical strength of a cured product made of the resin composition, the curing catalyst (E) preferably contains a phosphorus atom-containing compound, and more preferably contains at least one selected from the group consisting of a tetra-substituted phosphonium compound, a phosphobetaine compound, an adduct of a phosphine compound and a quinone compound, and an adduct of a phosphonium compound and a silane compound. By using a latent curing catalyst, a resin composition having excellent moldability can be obtained.
[0052] The content of the curing catalyst (E) in the resin composition of the present embodiment is preferably 0.01 mass% or more, more preferably 0.02 mass% or more, even more preferably 0.05 mass% or more, and preferably 1.00 mass% or less, more preferably 0.80 mass% or less, even more preferably 0.50 mass% or less, even more preferably 0.20 mass% or less.
[0053] The resin composition of the present embodiment may contain only one type of curing catalyst (E), or may contain two or more types.
[0054] <Other ingredients> The resin composition of the present embodiment may further contain other components.
[0055] The resin composition of the present embodiment may further contain a coupling agent from the viewpoint of further improving the mechanical strength of a cured product made of the resin composition. The coupling agent is not particularly limited, and for example, a known coupling agent can be used, and preferably a silane coupling agent can be used. The coupling agent may be used alone or in combination of two or more kinds.
[0056] The content of the coupling agent in the resin composition of the present embodiment, when the entire resin composition is taken as 100 mass%, is, from the viewpoint of further improving the mechanical strength of the cured product made of the resin composition, preferably 0.05 mass% or more, more preferably 0.10 mass% or more, and is preferably 1.00 mass% or less, more preferably 0.80 mass% or less, and even more preferably 0.50 mass% or less.
[0057] The resin composition of the present embodiment may further contain a release agent. The release agent includes at least one selected from the group consisting of, for example, carnauba wax, stearic acid, montanic acid, metal stearates, polyethylene oxide, and copolymers of 1-alkene and maleic anhydride, and among these, preferably includes at least one selected from the group consisting of carnauba wax, stearic acid, and copolymers of 1-alkene and maleic anhydride.
[0058] The content of the release agent in the resin composition of the present embodiment, when the entire resin composition is taken as 100% by mass, is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and is preferably 2.00% by mass or less, more preferably 1.00% by mass or less, and even more preferably 0.50% by mass or less.
[0059] The resin composition of the present embodiment may further contain an adhesion assistant. The adhesion aid is not particularly limited, and for example, a known adhesion aid can be used. Among them, an azole compound can be preferably used. The adhesion aid may be used alone or in combination of two or more kinds.
[0060] The content of the adhesion aid in the resin composition of this embodiment, when the entire resin composition is taken as 100 mass%, is preferably 0.01 mass% or more, more preferably 0.02 mass% or more, and is preferably 0.50 mass% or less, more preferably 0.20 mass% or less.
[0061] The resin composition of the present embodiment may further contain a stress reducing agent. The low stress agent is not particularly limited, and for example, a polybutadiene compound, an acrylonitrile butadiene copolymer compound, silicone oil, silicone rubber, etc. can be used, and among these, silicone oil can be preferably used. The stress reducing agent may be used alone or in combination of two or more kinds.
[0062] The content of the low stress agent in the resin composition of this embodiment is preferably 0.01 mass% or more, more preferably 0.02 mass% or more, and preferably 0.50 mass% or less, more preferably 0.30 mass% or less, when the entire resin composition is 100 mass%.
[0063] The resin composition of the present embodiment may further contain other components such as a dispersant, a colorant, an anticorrosive agent, a dye, a pigment, and a flame retardant. The content of each of the other components in the resin composition of the present embodiment is an appropriate amount.
[0064] [Method of producing resin composition] The resin composition of the present embodiment can be industrially produced, for example, by first (1) mixing the components using a mixer, (2) then kneading using a roll at about 90° C. for 5 minutes or more, preferably about 10 minutes, to obtain a kneaded mixture, (3) cooling the kneaded mixture, and (4) pulverizing the mixture. In this manner, a powdered resin composition can be obtained.
[0065] The resin composition in tablet form at 25° C. can be obtained by tableting the powdered resin composition.
[0066] [Molded body] The molded article of this embodiment is a molded article obtained by curing the resin composition of this embodiment.
[0067] The molded article of this embodiment is preferably a transfer molded article. The term "transfer molded article" as used herein means a molded article obtained by curing a melt of a resin composition using a transfer molding device. The term "transfer molded article" is intended to include a molded article obtained by further post-curing the above-mentioned molded article.
[0068] The method for producing the molded article of the present embodiment is not particularly limited, but may be, for example, a method of transfer molding a resin composition using a known transfer molding device. Specifically, a method of injecting a preheated resin composition into a mold with a plunger and holding the molded article in the mold to harden the molten resin composition is exemplified. The various conditions in transfer molding are not particularly limited, but for example, the temperature for preheating the resin composition is 60°C to 100°C, the mold temperature is 100°C to 200°C, and the pressure for injecting the molten resin composition into the mold is 0.5 MPa to 5.0 MPa. The temperature for melting the resin composition can be considered to be the same as the mold temperature. When the molded article is post-cured, it can be post-cured, for example, by heating it in air at 175° C. for 4 hours.
[0069] [rotor] The rotor 100 of this embodiment will be described with reference to the drawings. The rotor 100 includes a rotor core 80 having a hole 20, the rotor core 80 having a plate member 85, and the hole 20 contains a cured product 30 made of a resin composition.
[0070] The rotor core 80 preferably has a laminated body in which a plurality of plate members 85 are stacked. Here, the number of the plate members 85 is not particularly limited, but may be, for example, 2 to 500, or 10 to 300. Examples of the laminate in which plate members 85 are laminated include a laminate in which plate members 85 are laminated together by crimping, and a laminate in which plate members 85 are laminated together by bonding them with an adhesive.
[0071] The plate member 85 is not particularly limited, and for example, an electromagnetic steel plate, a permendur plate, an amorphous metal plate, etc. can be used, with the electromagnetic steel plate being preferred among these.
[0072] The rotor core 80 has a hole 20 . The hole portion 20 means a hole formed in a direction perpendicular to the surface direction of the rotor core, and may or may not be a through hole. The hole 20 is preferably a flux barrier portion. The flux barrier portion means a hole for forming a magnetic gap. The rotor core 80 needs to have at least one hole 20, and may have a plurality of holes 20.
[0073] The shape of the hole 20 in a plan view is not particularly limited and may be, for example, a rectangle, a circle, etc. The shape of the hole 20 in a plan view is preferably a rounded shape such as a circle, from the viewpoint of suppressing stress concentration and further improving the strength of the rotor.
[0074] The rotor core 80 may further have a magnet insertion portion 50 for inserting a magnet (not shown). The magnet insertion portion 50 is a hole formed in a direction perpendicular to the surface direction of the rotor core 80, and may or may not be a through hole. The rotor core 80 may have multiple magnet inserts 50 .
[0075] When the rotor core 80 further includes the magnet insertion portion 50, the hole portion 20 may be a hole independent of the magnet insertion portion 50. A hole independent of the magnet insertion portion 50 means a hole such as the hole portion 20 illustrated in FIG.
[0076] When the rotor core 80 further includes the magnet insertion portion 50, the hole portion 20 may be a hole that is continuous with the magnet insertion portion 50. A hole that is continuous with the magnet insertion portion 50 means a hole such as the hole portion 20 shown in FIG. In FIG. 2, the center of the hole is magnet insertion portion 50 for inserting a magnet, and both ends of the hole are hole portions 20.
[0077] In the rotor 100, it is preferable that the saturation magnetic flux density at 25°C of the cured product 30 made of the resin composition is smaller than the saturation magnetic flux density at 25°C of the plate member 85.
[0078] The rotor 100 may further include a magnet (not shown) and the like.
[0079] The method for manufacturing the rotor 100 is not particularly limited, but preferably includes a step of inserting a cured product 30 made of the resin composition into the hole of the rotor core by transfer molding the resin composition of this embodiment. The preferred conditions when the resin composition is transfer molded are the same as those in the above-mentioned method for producing a molded article of this embodiment.
[0080] [motor] The motor of this embodiment includes a rotor 100 . The motor of the present embodiment may further include, in addition to the rotor 100, a shaft, a bearing, a stator, a bracket, and the like.
[0081] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES
[0082] The present embodiment will be described in detail below based on examples, but the present embodiment is not limited to the descriptions of these examples.
[0083] [Raw materials] First, the raw materials used in the examples will be described. Details of the raw materials listed in Table 1 are shown below.
[0084] <Soft magnetic particles (B)> Magnetic powder 1: amorphous magnetic powder (manufactured by Epson Atmix Corporation, product name: KUAMET6B2 150C01, median diameter: 40 μm, Fe content: 87.6 mass%, Si content: 6.7 mass%) Magnetic powder 2: crystalline magnetic powder (manufactured by Daido Steel Co., Ltd., product name: DAPMS7-100, gas water atomized powder, median diameter: 60 μm, Fe content: 93.4 mass%, Si content: 6.5 mass%) Magnetic powder 3: crystalline magnetic powder (manufactured by Daido Steel Co., Ltd., product name: DAPMS3-100, gas water atomized powder, median diameter: 70 μm, Fe content: 96.7 mass%, Si content: 3.0 mass%) Magnetic powder 4: crystalline magnetic powder (manufactured by Epson Atmix Corporation, product name: Fe-3.5Si-4.5Cr_PF-20F, median diameter: 10 μm, Fe content: 91.9 mass%, Si content: 3.5 mass%) Magnetic powder 5: amorphous magnetic powder (manufactured by Epson Atmix Corporation, product name: AW2-08_PF-3F, median diameter: 3 μm, Fe content: 87.4 mass%, Si content: 6.8 mass%) Magnetic powder 6: crystalline magnetic powder (manufactured by Shinto Kogyo Co., Ltd., product name: FSC-2, median diameter: 2 μm, Fe content: 91.1 mass%, Si content: 3.5 mass%)
[0085] <Coupling Agent> Coupling agent 1: Phenylaminopropyltrimethoxysilane (manufactured by Dow Corning Toray Co., Ltd., product name: CF-4083)
[0086] <Thermosetting resin (A)> Epoxy resin 1: biphenyl aralkyl type epoxy resin (manufactured by Nippon Kayaku Co., Ltd., product name: NC-3000L, solid at 25°C)
[0087] <Phenol-based hardener (D)> Phenolic resin 1: Phenol aralkyl resin containing biphenylene skeleton (manufactured by Meiwa Kasei Co., Ltd., product name: MEH-7851SS)
[0088] <Release agent> Wax 1: Synthetic wax (copolymer of 1-alkene and maleic anhydride) Wax 2: Stearic acid (NOF Corporation, product name: powdered stearic acid Sakura fine powder) Wax 3: Carnauba wax (manufactured by Toa Kasei Co., Ltd., product name: TOWAX-132)
[0089] <Adhesion aid> Adhesion aid 1: Compound containing benzotriazole-based compounds (manufactured by ADEKA Corporation, product name: Adeka STAB CDA-1M)
[0090] <Low stress agent> Silicone oil 1: Silicone oil (manufactured by Toray Dow Corning, product name: FZ-3730)
[0091] <Curing catalyst (E)> Curing catalyst 1: Tetraphenylphosphonium bis(naphthalene-2,3-dioxy)phenylsilicate (Sumitomo Bakelite Co., Ltd.) Curing catalyst 2: Tetraphenylphosphonium 4,4'-sulfonyldiphenolate (Sumitomo Bakelite Co., Ltd.)
[0092] <Silica filler (C)> Silica filler 1: Fused silica (median diameter 0.5 μm)
[0093] [Examples 1 to 4] <Preparation of resin composition> Each component shown in Table 1 was prepared in the ratio [parts by mass] shown in Table 1, and the soft magnetic particles were first mixed while the other components were added thereto and mixed uniformly to obtain the respective mixtures. The resulting mixture was then kneaded at 100° C. for 10 minutes. After kneading, the resulting kneaded product was cooled to room temperature to become solid, and then crushed and tableted. As a result, tablet-shaped resin compositions in Examples 1 to 4 were obtained, respectively. The obtained tablet-shaped resin compositions in Examples 1 to 4 were solid at 25°C.
[0094] <Preparation of transfer molded body 1 by curing resin composition> The tablet-like resin compositions obtained in Examples 1 to 4 were injection molded using a low-pressure transfer molding machine (manufactured by Kotaki Seiki Co., Ltd., product name: KTS-30) at a mold temperature of 175°C, injection pressure of 9.8 MPa, and pressure retention time of 300 seconds to obtain cylindrical transfer molded bodies with a diameter of 16 mmΦ and a height of 32 mm. The obtained molded bodies were then post-cured under atmospheric conditions at 175°C for 4 hours to obtain transfer molded bodies 1 each formed by curing the cylindrical resin composition.
[0095] <Preparation of transfer molded body 2 by curing resin composition> The tablet-like resin compositions obtained in Examples 1 to 4 were injection molded using a low-pressure transfer molding machine (manufactured by Kotaki Seiki Co., Ltd., product name: KTS-30) at a mold temperature of 175°C, injection pressure of 9.8 MPa, and pressure retention time of 300 seconds to obtain rectangular transfer molded bodies having a width of 10 mm, a thickness of 1.5 mm, and a length of 55 mm. The obtained molded bodies were then post-cured under atmospheric conditions at 175°C for 4 hours to obtain transfer molded bodies 2 each consisting of a cured rectangular resin composition.
[0096] <Preparation of transfer molded body 3 by curing resin composition> The tablet-like resin compositions obtained in Examples 1 to 4 were injection molded using a low-pressure transfer molding machine (manufactured by Kotaki Seiki Co., Ltd., product name: KTS-30) under conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a pressure retention time of 300 seconds, to obtain rectangular transfer molded bodies having a width of 10 mm, a thickness of 4 mm, and a length of 80 mm. The obtained molded bodies were then post-cured under atmospheric conditions at 175°C for 4 hours, to obtain transfer molded bodies 3 each formed by curing the rectangular resin composition.
[0097] It is difficult to apply transfer molding to a resin composition that is not solid at 25°C.
[0098] [measurement] <Content of soft magnetic particles (B) relative to the entire resin composition [volume %]> The content [volume %] of the soft magnetic particles (B) relative to the entire resin composition was calculated using the volume of the obtained pellet-shaped resin composition and the volume of the soft magnetic particles (B) calculated from the density and content of the soft magnetic particles (B) in the resin composition.
[0099] <Spiral flow of resin composition at 175°C> Using a low pressure transfer molding machine (manufactured by Kotaki Seiki Co., Ltd., product name: KTS-30), the resin composition was injected into a metal mold for measuring spiral flow in accordance with ANSI / ASTM D 3123-72, and the flow length (spiral flow) was measured under the following conditions: mold temperature 175°C, injection pressure 6.9 MPa, and pressure dwell time 120 seconds. Spiral flow is a parameter of fluidity, and the larger the value, the better the fluidity. The unit is cm.
[0100] <Gel time of resin composition at 175°C> The resin composition was placed on a hot plate controlled at 175°C and kneaded with a spatula at one stroke per second. The time from when the resin composition was dissolved by heat to when it hardened was measured and this was taken as the gel time. The smaller the gel time value, the faster the hardening.
[0101] <Glass transition temperature of cured product made of resin composition> The glass transition temperature of transfer molding 2 (i.e., a transfer molding obtained by curing a rectangular resin composition having a width of 10 mm, a thickness of 1.5 mm, and a length of 55 mm) was measured using a viscoelasticity measuring device (manufactured by Hitachi High-Tech Corporation, product name: DMA7100) under conditions of a measurement temperature range of 25°C to 300°C and a heating rate of 5°C / min.
[0102] <Flexural strength at 25°C and flexural modulus at 25°C of cured product made of resin composition> The bending strength and bending modulus at 25°C of transfer molding 3 (i.e., a rectangular transfer molding obtained by curing a resin composition with a width of 10 mm, a thickness of 4 mm, and a length of 80 mm) were measured at a loading rate of 2 mm / min in accordance with JIS K 6911 (2006).
[0103] <Saturation magnetic flux density at 25°C of the cured product made of the resin composition> An external magnetic field of 100 kA / m was applied to the transfer molded body 1 (i.e., a cylindrical transfer molded body having a diameter of 16 mm and a height of 32 mm, obtained by curing a resin composition) at room temperature (25°C) using a DC / AC magnetization characteristic tester (manufactured by Metron Giken Co., Ltd., product name: MTR-3368). Thus, the saturation magnetic flux density at 25°C was measured.
[0104] The results of the above measurements for the resin compositions and transfer molded articles of Examples 1 to 4 are shown in Table 1.
[0105] [Table 1]
[0106] In Examples 1 to 4, transfer molded bodies 1 to 3 with different shapes were obtained, respectively. In particular, as the transfer molded body 1, a rounded cylindrical molded body was obtained. That is, according to the resin composition of this embodiment, transfer molding can be performed. By transfer molding the resin composition, a molded body that matches the shape of the hole can be obtained. Therefore, according to the resin composition of this embodiment, it can be understood that it is possible to reduce the occurrence of gaps in the hole when a molded body made of the resin composition is inserted into the hole of the rotor core. [Explanation of symbols]
[0107] 20 hole 30 Cured product made of resin composition 50 Magnet insertion part 80 rotor core 85 Plate members 100 rotors
Claims
1. A resin composition that can be inserted into a hole of a rotor core by transfer molding, A magnetic material comprising a thermosetting resin (A) and soft magnetic particles (B), The resin composition is a solid at 25°C.
2. The resin composition according to claim 1, wherein the content of the soft magnetic particles (B) in the resin composition is 50% by volume or more and 90% by volume or less when the entire resin composition is taken as 100% by volume.
3. The resin composition according to claim 1 , wherein the soft magnetic particles (B) contain elemental Si.
4. The resin composition according to claim 1 or 2, wherein the soft magnetic particles (B) include crystalline particles.
5. The resin composition according to claim 1 or 2, wherein the soft magnetic particles (B) include amorphous particles.
6. The resin composition according to claim 1 or 2, wherein the soft magnetic particles (B) comprise a gas-water atomized powder.
7. The resin composition according to claim 1 or 2, wherein the thermosetting resin (A) comprises an epoxy resin.
8. The resin composition according to claim 7, wherein the epoxy resin is a solid at 25°C.
9. The resin composition according to claim 1 or 2, further comprising a silica filler (C).
10. The resin composition according to claim 9, wherein the content of the silica filler (C) in the resin composition is 0.10 mass% or more and 5.00 mass% or less, when the entire resin composition is 100 mass%.
11. The resin composition according to claim 1 or 2, further comprising a phenol-based curing agent (D).
12. Further comprising a curing catalyst (E), 3. The resin composition according to claim 1, wherein the curing catalyst (E) comprises at least one selected from the group consisting of a tetra-substituted phosphonium compound, a phosphobetaine compound, an adduct of a phosphine compound and a quinone compound, and an adduct of a phosphonium compound and a silane compound.
13. 3. The resin composition according to claim 1, having a spiral flow at 175°C of 10 cm or more and 200 cm or less.
14. The resin composition according to claim 1 or 2, which has a gel time at 175°C of 30 seconds or more and 300 seconds or less.
15. The resin composition according to claim 1 or 2, wherein a cured product of the resin composition has a saturation magnetic flux density of 1.50 T or less at 25° C.
16. The resin composition according to claim 1 or 2, wherein a cured product of the resin composition has a flexural strength at 25°C measured in accordance with JIS K 6911 (2006) of 50 MPa or more and 200 MPa or less.
17. The resin composition according to claim 1 or 2, wherein a cured product of the resin composition has a flexural modulus at 25°C measured in accordance with JIS K 6911 (2006) of 20,000 MPa or more and 50,000 MPa or less.
18. The resin composition according to claim 1 or 2, wherein a glass transition temperature of a cured product of the resin composition is 100° C. or higher and 250° C. or lower.
19. The resin composition according to claim 1 or 2, which is in a tablet form at 25°C.
20. The resin composition according to claim 1 , wherein the hole portion of the rotor core is a flux barrier portion.
21. A molded article obtained by curing the resin composition according to claim 1 or 2.
22. The molded article according to claim 21, which is a transfer molded article.
23. A rotor core having a hole, The rotor core has a plate member, A rotor, comprising a cured product of the resin composition according to claim 1 or 2 in the hole.
24. The rotor according to claim 23 , wherein the rotor core has a laminate in which a plurality of the plate members are stacked.
25. The rotor according to claim 23 , wherein the plate members are electromagnetic steel plates.
26. The rotor according to claim 23 , wherein a saturation magnetic flux density at 25° C. of a cured product made of the resin composition is smaller than a saturation magnetic flux density at 25° C. of the plate member.
27. The rotor core further includes a magnet insertion portion for inserting a magnet, The rotor of claim 23 , wherein the aperture is a hole separate from the magnet insert.
28. The rotor core further includes a magnet insertion portion for inserting a magnet, The rotor of claim 23 , wherein the aperture is continuous with the magnet insert.
29. A motor comprising a rotor according to claim 23.