Laminate, packaging bag and packaged article
The laminate structure with a high crystallinity ratio between base and sealant layers, combined with an adhesive and gas barrier, addresses the issue of impact resistance in packaging materials, enhancing durability and protection against gas permeation.
Patent Information
- Application Number
- JP2023078765
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional laminates used in packaging materials lack sufficient impact resistance, particularly against drops and impacts.
A laminate structure is designed with a base layer having a crystallinity ratio of 2.0 or more to the sealant layer, where the base layer has higher crystallinity than the sealant layer, enhancing rigidity and shock absorption properties, and optionally includes an adhesive layer for improved adhesion and a gas barrier layer for enhanced protection.
The laminate exhibits improved impact resistance, reducing the likelihood of tearing and preventing content deterioration due to gas exposure, while maintaining recyclability and environmental sustainability.
Smart Images

Figure 2024162838000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a laminate, a packaging bag, and a packaging article. [Background technology]
[0002] Packaging materials used for packaging bags and the like are required to have various properties depending on the application. Specific examples of the required properties include heat sealability and strength required for a packaging material. In order to fully satisfy each of these various performance requirements, the packaging material is generally composed of a laminate including a base layer and a sealant layer. As such a laminate, a laminate has been known that includes a gas barrier film including a substrate and an inorganic oxide layer, and a heat seal layer, in which the crystallinity of the inorganic oxide layer side of the substrate is 35% or less (see, for example, Patent Document 1 below). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 7036266 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the laminate described in Patent Document 1 above has room for improvement in terms of impact resistance against being dropped or the like.
[0005] The present disclosure has been made in consideration of the above-mentioned problems, and an object of the present disclosure is to provide a laminate, a packaging bag, and a packaging article that can improve impact resistance. [Means for solving the problem]
[0006] One aspect of the present disclosure provides a laminate comprising a base layer and a sealant layer, wherein a ratio of the crystallinity of the base layer to the crystallinity of the sealant layer is 2.0 or more, and the crystallinity is a ratio of a crystalline peak area to a total peak area measured by a parallel beam method of X-ray diffraction at a diffraction angle range of 10° to 30°. According to the above laminate, the impact resistance of the laminate can be improved.
[0007] Although it is not clear why the laminate provides the above-mentioned effects, the inventors of the present disclosure speculate that it may be as follows. That is, in the laminate of the present disclosure, the ratio of the crystallinity of the base layer to the crystallinity of the sealant layer is 2.0 or more, and the base layer has a relatively higher crystallinity than the sealant layer, so that it has high rigidity. Therefore, even if the base layer is distorted by an impact applied to the laminate, the distortion is small, and plastic deformation of the base layer is suppressed. On the other hand, the sealant layer has a relatively lower crystallinity than the base layer, so that it has excellent flexibility and high impact absorption. Therefore, even if stress due to an impact is applied to the base layer, the stress is absorbed by the sealant layer. Therefore, even if the laminate is impacted, cracks are unlikely to occur in the base layer, and the laminate is unlikely to break. In this way, it is possible to improve the impact resistance of the laminate. From the above, the inventors of the present disclosure speculate that the above-mentioned effects can be obtained by the laminate of the present disclosure.
[0008] The laminate preferably further comprises an adhesive layer between the base layer and the sealant layer. In this case, by having the laminate further include an adhesive layer between the base layer and the sealant layer, the adhesion between the base layer and the sealant layer is further improved, and peeling between the base layer and the sealant layer is suppressed.
[0009] In the above laminate, the crystallinity of the base layer is preferably greater than 35%. In this case, the impact resistance of the laminate can be improved more effectively than when the crystallinity of the base material layer is 35% or less.
[0010] The laminate has an oxygen permeability of 200 cc / m at 30°C and 70 RH%. 2 It is preferable that the temperature be less than 100°C / day atm. In this case, the oxygen permeability at 30℃ and 70RH% is 200cc / m 2 When a packaging bag is made using the laminate and contents are placed in the packaging bag to produce a packaged article, deterioration of the contents due to oxygen can be effectively suppressed, compared to when the storage temperature exceeds 100°C / day·atm.
[0011] In the above laminate, the ratio of the thickness of the base layer to the thickness of the sealant layer is preferably 0.1 to 1.0. When the ratio of the thickness of the base layer to the thickness of the sealant layer is 0.1 or more, the ratio of the base layer having a high crystallinity and high rigidity is relatively high, so that the rigidity of the laminate can be further improved.When the ratio of the thickness of the base layer to the thickness of the sealant layer is 1.0 or less, the ratio of the sealant layer having a low crystallinity and high flexibility is relatively high, so that the impact absorption of the laminate can be further improved.
[0012] It is preferable that the laminate further includes a gas barrier layer between the base layer and the sealant layer. In this case, the gas barrier property of the laminate is further improved, so that when the laminate is used to prepare a packaging bag and contents are placed in the packaging bag to prepare a packaged article, deterioration of the contents due to gases such as oxygen can be effectively suppressed.
[0013] The content of the polyethylene resin in the entire laminate is preferably 90% by mass or more. In this case, the laminate can have higher recyclability.
[0014] Another aspect of the present disclosure provides a packaging bag obtained by using the above-mentioned laminate. According to this packaging bag, since it is obtained using the above-mentioned laminate, it is possible to improve the impact resistance, and therefore the packaging bag becomes less likely to break when subjected to an impact due to being dropped, etc.
[0015] Furthermore, still another aspect of the present disclosure provides a packaging article including the above-mentioned packaging bag and contents accommodated in the packaging bag. This packaged article can improve impact resistance, making the packaging bag less likely to break when subjected to impact due to being dropped, etc., and suppressing leakage of the contents from the packaging bag. Effect of the Invention
[0016] According to the present disclosure, a laminate, a packaging bag, and a packaging article capable of improving impact resistance are provided. [Brief description of the drawings]
[0017] [Figure 1] 1 is a cross-sectional view showing one embodiment of a laminate according to the present disclosure. [Diagram 2] FIG. 1 is a cross-sectional view of one embodiment of a packaging article according to the present disclosure. [Diagram 3] FIG. 4 is a cross-sectional view showing another embodiment of a laminate according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, preferred embodiments of the present disclosure will be described in detail. In the drawings, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted. In addition, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0019] <Laminate> First, one embodiment of a laminate according to the present disclosure will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view showing one embodiment of a laminate according to the present disclosure.
[0020] 1, the laminate 100 includes a base layer 10 and a sealant layer 30. The laminate 100 may further include an adhesive layer 20 between the base layer 10 and the sealant layer 30. The ratio of the crystallinity of the base layer 10 to the crystallinity of the sealant layer 30 is 2.0 or more. Here, the crystallinity is the ratio of the crystalline peak area to the total peak area measured by the parallel beam method of X-ray diffraction in the diffraction angle range of 10° to 30°.
[0021] According to the laminate 100, the impact resistance of the laminate 100 can be improved.
[0022] The base layer 10, the adhesive layer 20, the sealant layer 30 and the laminate 100 will be described in detail below.
[0023] (base material layer) The base layer 10 contains a resin. The resin has both crystalline and amorphous parts. A resin with a high degree of crystallinity has a high ratio of crystalline parts. Since the crystalline parts control the elastic parts in the viscoelastic behavior of the resin, a high degree of crystallinity improves the rigidity of the base layer 10. The ratio R1 of the crystallinity of the base layer 10 to the crystallinity of the sealant layer 30 may be 2.0 or more. R1 is preferably 3.0 or more, and more preferably 3.5 or more. R1 is preferably 10 or less, more preferably 8 or less, and particularly preferably 6 or less. The crystallinity of the base layer 10 is not particularly limited, but is preferably greater than 35%, more preferably 40% or more, and particularly preferably 50% or more. When the crystallinity of the base layer 10 is greater than 35%, the base layer 10 has higher rigidity than when the crystallinity of the base layer 10 is 35% or less. Therefore, even if distortion occurs in the base layer 10 due to an impact applied to the laminate 100, the distortion is smaller, plastic deformation of the base layer 10 is suppressed, and cracks are less likely to occur in the base layer 10. The crystallinity of the base layer 10 may be 100% or less. The crystallinity of the base layer 10 is preferably 90% or less, and more preferably 80% or less. When the crystallinity of the base layer 10 is 90% or less, the base layer 10 has better flexibility and higher shock absorption than when the crystallinity of the base layer 10 is more than 90%. This allows the laminate 100 to have better impact resistance. When the base layer 10 is a laminate of a plurality of layers, the crystallinity of the base layer 10 is the crystallinity of the outermost layer.
[0024] The crystallinity of the substrate layer 10 can be adjusted by controlling the degree of elongation of the resin film used for the substrate layer 10, or the thermal history during or after the production of the resin film. For example, if the resin film that will become the substrate layer 10 after film formation is slowly cooled, the crystallinity of the substrate layer 10 increases, and if it is rapidly cooled, the crystallinity of the substrate layer 10 decreases. It is also possible to improve the crystallinity of the substrate layer 10 by adding an additive such as a crystal nucleating agent.
[0025] Examples of the resin include polyolefin resins and polyester resins.
[0026] Examples of polyolefin resins include polyethylene-based resins and polypropylene-based resins. A polyethylene-based resin is a resin that contains ethylene as a structural unit. Examples of polyethylene-based resins include ethylene homopolymers and copolymers of ethylene and other monomers. The proportion of ethylene in polyethylene is, for example, 80 mol % or more. Examples of other monomers include α-olefins, vinyl acetate, acrylic esters, and the like. The α-olefin may be an olefin having a carbon number in the range of 3 to 20. Examples of the α-olefin include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 3-methyl-1-butene, 4-methyl-1-pentene, and 6-methyl-1-heptene. Examples of polyethylene resins include high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), very low density polyethylene (VLDPE), ethylene-vinyl acetate copolymer, ionomer resin, ethylene-acrylic acid copolymer, ethylene-methyl acrylate copolymer, ethylene-methacrylic acid copolymer, ethylene-propylene copolymer, etc. These may be used alone or in combination of two or more. Here, high density polyethylene has a density of 0.942 g / cm 3 Medium density polyethylene has a density of 0.930 g / cm or more. 3 More than 0.942g / cm 3 Low density polyethylene is polyethylene with a density of less than 0.910 g / cm 3 More than 0.930g / cm 3 Linear low density polyethylene has a density of less than 0.910 g / cm 3 More than 0.930cm 3 Ultra-low density polyethylene has a density of less than 0.910 g / cm 3 It is polyethylene having a molecular weight of less than 1.001. The density is a value obtained by a method in accordance with JIS K7112:1999. The polypropylene resin is a resin that contains propylene as a structural unit and does not contain ethylene as a structural unit. Examples of the polypropylene resin include homopolypropylene, block polypropylene, and random polypropylene.
[0027] Examples of polyester resins include polyethylene terephthalate, polyethylene naphthalate, etc. These may be used alone or in combination of two or more.
[0028] The resin may be a resin obtained using a raw material (monomer) obtained from a fossil fuel or a resin obtained using a raw material (monomer) derived from biomass, but from the viewpoint of reducing the environmental load, it is preferable that the resin is a resin obtained using a raw material derived from biomass. Alternatively, the resin may be a recycled resin. The recycled resin may be a mechanically recycled resin or a chemically recycled resin.
[0029] The base layer 10 may contain at least one additive selected from a filler, an antistatic agent, a plasticizer, a lubricant, an antioxidant, and the like, as necessary.
[0030] The substrate layer 10 may be an unstretched film or a stretched film. The stretched film may be a uniaxially stretched film or a biaxially stretched film. The substrate layer 10 may be composed of either a stretched film or an unstretched film. The substrate layer 10 may also be a laminate of at least one stretched film and at least one unstretched film. The substrate layer 10 can improve mechanical strength and dimensional stability by having a biaxially stretched film.
[0031] In order to enhance adhesion to the adhesive layer 20, the surface of the base material layer 10 facing the adhesive layer 20 may be subjected to various pretreatments such as corona treatment, plasma treatment, ozone treatment, and frame treatment, or a coating layer such as an easy-adhesion layer may be provided.
[0032] The thickness of the substrate layer 10 is not particularly limited, and is, for example, 10 μm or more and 200 μm or less. From the viewpoint of reducing materials to reduce environmental load, and from the viewpoint of obtaining excellent heat resistance, impact resistance, and gas barrier properties, the thickness of the substrate layer 10 may be 20 μm or more, 25 μm or more, 30 μm or more, or 40 μm or more. The thickness of the substrate layer 10 may be 100 μm or less, 60 μm or less, or 50 μm or less. The ratio of the thickness of the substrate layer 10 to the thickness of the laminate 100 is, for example, 5% or more.
[0033] The ratio R2 of the thickness of the base layer 10 to the thickness of the sealant layer 30 is not particularly limited, but R2 is preferably 0.1 or more, more preferably 0.15 or more, and particularly preferably 0.20 or more. When R2 is 0.1 or more, the proportion of the base material layer 10 having a high degree of crystallinity and high rigidity is relatively high, so that the rigidity of the laminate 100 can be further improved.
[0034] R2 is preferably 1.0 or less, more preferably 0.7 or less, even more preferably 0.4 or less, and particularly preferably 0.3 or less. When R2 is 1.0 or less, the proportion of the sealant layer 30 having a low degree of crystallinity and high flexibility is relatively high, so that the impact absorption of the laminate 100 can be further improved.
[0035] (Adhesive layer) The adhesive layer 20 is a layer that bonds the base material layer 10 and the sealant layer 30. When the laminate 100 has the adhesive layer 20, the adhesion between the base material layer 10 and the sealant layer 30 is further enhanced, and peeling between the base material layer 10 and the sealant layer 30 is suppressed.
[0036] The adhesive layer 20 may be an adhesive layer formed using an adhesive.
[0037] Examples of the adhesive include known adhesives such as urethane adhesives, polyester adhesives, polyamide adhesives, epoxy adhesives, and isocyanate adhesives.
[0038] The oxygen permeability of the adhesive layer 20 is preferably 150 cc / m 2 ·day·atm or less, and more preferably 100cc / m 2 ·day·atm or less, and more preferably 80cc / m 2 ·day·atm or less, and particularly preferably 50cc / m 2 ·day·atm or less. Oxygen permeability is 150cc / m 2 A viscosity of 100 psi or less can sufficiently improve the gas barrier properties of the laminate 100. Specific examples of such adhesives include "Maxive" manufactured by Mitsubishi Gas Chemical Company, Inc. and "Paslim" manufactured by DIC Corporation.
[0039] The adhesive layer 20 may or may not contain a biomass component, but preferably contains a biomass component from the viewpoint of reducing the environmental load. Specific examples of the biomass component include the "DIC Dry BM Series" manufactured by DIC Corporation and the "ECOAD Series" manufactured by Toyo Ink Co., Ltd. The biomass component may be included as a component of the adhesive, or may be included as a component other than the adhesive.
[0040] The adhesive may be an adhesive containing an organic solvent or an adhesive containing no organic solvent, but from the viewpoint of reducing the environmental load, an adhesive containing no organic solvent (solvent-free adhesive) is preferable.
[0041] The thickness of the adhesive layer 20 is not particularly limited and may be, for example, 1 μm or more. By making the thickness of the adhesive layer 20 2 μm or more, sufficient adhesive strength can be obtained. The thickness of the adhesive layer 20 may be 2 μm or more. The thickness of adhesive layer 20 may be 50 μm or less, 5 μm or less, or 3 μm or less.
[0042] (Sealant layer) The sealant layer 30 contains a resin. As the resin, the same resin as that used in the base layer 10 can be used. As the resin, linear low-density polyethylene is preferable.
[0043] The crystallinity of the sealant layer 30 is not particularly limited, but is preferably 5% or more, and more preferably 10% or more. When the crystallinity of the sealant layer 30 is 5% or more, the sealant layer 30 has a higher rigidity than when the crystallinity of the sealant layer 30 is less than 5%, so that even if distortion occurs in the sealant layer 30 due to an impact applied to the laminate 100, the distortion is smaller, plastic deformation of the sealant layer 30 is suppressed, and cracks are less likely to occur in the sealant layer 30.
[0044] The crystallinity of the sealant layer 30 may be 20% or less, 15% or less, or 13% or less. When the crystallinity of the sealant layer 30 is 20% or less, the sealant layer 30 has better flexibility and higher impact absorption than when the crystallinity of the sealant layer 30 is more than 20%. Therefore, the impact resistance of the laminate 100 can be further improved. When the sealant layer 30 is a laminate of a plurality of layers, the crystallinity of the sealant layer 30 is the crystallinity of the outermost layer. The crystallinity of the sealant layer 30 can be adjusted in the same manner as the crystallinity of the base layer 10 .
[0045] The sealant layer 30 preferably has a melting point lower than that of the base layer 10. In this case, when the laminate 100 is heat-sealed, it is possible to heat-seal the sealant layer 30 while suppressing melting of the base layer 10. In addition, by heating the laminate 100, the base layer 10 and the sealant layer 30 can be easily separated, and material recycling can be easily performed for each of the base layer 10 and the sealant layer 30.
[0046] The sealant layer 30 may contain various additives, such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, a tackifier, and an antistatic agent, as necessary.
[0047] The thickness of the sealant layer 30 is not particularly limited and is appropriately adjusted depending on the application of the laminate 100. The thickness of the sealant layer 30 may be, for example, 10 μm or more, 25 μm or more, 30 μm or more, 40 μm or more, or 50 μm or more. The thickness of the sealant layer 30 may be 200 μm or less, 180 μm or less, 160 μm or less, 150 μm or less, 120 μm or less, or 100 μm or less.
[0048] (Laminate) The oxygen permeability of the laminate 100 at 30° C. and 70% RH is not particularly limited, but is preferably 200 cc / m 2 It is preferable that the temperature be less than 100°C / day atm. In this case, the oxygen permeability at 30℃ and 70RH% is 200cc / m 2 Compared to the case where the storage temperature exceeds 100°C / day·atm, when a packaging bag is made using the laminate 100 and contents are placed in the packaging bag to produce a packaged article, deterioration of the contents due to oxygen can be effectively suppressed.
[0049] The oxygen permeability of the laminate 100 at 30° C. and 70% RH is more preferably 100 cc / m 2 ·day·atm or less, and particularly preferably 50cc / m 2 ·day·atm or less.
[0050] In the laminate 100, both the base layer 10 and the sealant layer 30 may contain a polyethylene-based resin. In this case, the proportion of the polyethylene-based resin in the entire laminate 100 is not particularly limited, but is preferably 90% by mass or more. By making the proportion of the polyethylene-based resin in the entire laminate 100 90% by mass or more, it becomes possible for the laminate 100 to have higher recyclability. The proportion of the polyethylene resin in the entire laminate 100 is more preferably 75% by mass or more, and particularly preferably 90% by mass or more.
[0051] <Packaged goods> Next, an embodiment of the packaging article of the present disclosure will be described with reference to Fig. 2. Fig. 2 is a cross-sectional view showing one embodiment of the packaging article of the present disclosure.
[0052] As shown in FIG. 2, the packaged article 500 includes a packaging bag 400 and a content C contained in the packaging bag 400. The packaging bag 400 is obtained by using a pair of laminates 100. The packaging bag 400 is obtained, for example, by placing the sealant layers 30 of a pair of laminates 100 facing each other and bonding the peripheral portions. The packaging bag 400 is composed of a storage section that stores the content C and an adhesive section provided around the storage section. The adhesive section is a portion formed by bonding the sealant layers 30 of opposing laminates 100 to each other, and the storage section is a portion where the sealant layers 30 of opposing laminates 100 are not bonded to each other.
[0053] Impact resistance can be improved according to the packaged article 500. Therefore, the packaging bag 400 is less likely to break when subjected to impact due to being dropped or the like, and leakage of the contents from the packaging bag 400 is suppressed.
[0054] (Contents) The contents C are not particularly limited and may be appropriately selected depending on the application of the packaging bag 400. The contents C are not particularly limited, and examples of the contents C include food, shampoo, rinse, body soap, detergent, and the like.
[0055] (packaging bag) The pair of laminates 100 constituting the packaging bag 400 may have the same configuration as each other, or may have different configurations from each other.
[0056] The packaging bag 400 may have a half-cut line, and may further have an easy-open processed part at both ends or one end of the half-cut line. Examples of the easy-open processed part include a group of scars, and a V-shaped, U-shaped, or I-shaped notch.
[0057] In the adhesive portion of the packaging bag 400, the sealant layers 30 of the pair of laminates 100 may be directly bonded to each other by heat sealing (see FIG. 2), or may be bonded to each other by an adhesive.
[0058] (Method of manufacturing packaging articles) Next, a method for producing a packaged article 500 using the laminate 100 will be described.
[0059] First, a pair of laminates 100 is prepared. Then, the sealant layers 30 of the pair of laminates 100 are placed opposite each other, and the sealant layers 30 are bonded together. At this time, a part of the peripheral portion of the laminate is bonded to form a U-shape to form a bonded portion, and a non-bonded portion (unbonded portion) is also formed. In this manner, a packaging bag having an opening formed by the unbonded portion is obtained.
[0060] Next, the contents C are filled in through the opening of the packaging bag. Thereafter, the sealant layers 30 of the laminate 100 are bonded together at the unbonded portions, so that the unbonded portions also become bonded portions. In this manner, a packaged article 500 including the packaging bag 400 and the contents C contained therein can be manufactured.
[0061] Although the preferred embodiment of the present disclosure has been described above, the present disclosure is not limited to the above embodiment. For example, the laminate of the present disclosure may further include a gas barrier layer 50 between the base layer 10 and the adhesive layer 20, as in the laminate 200 shown in FIG. 3. When the laminate 100 further includes the gas barrier layer 50, the gas barrier property of the laminate 200 is further improved. The gas barrier layer 50 has a barrier property against gases such as water vapor or oxygen.
[0062] The gas barrier layer 50 contains an inorganic compound. The inorganic compound contains at least one of a metal and an inorganic oxide. Metals include aluminum, silicon, etc. Inorganic oxides include aluminum oxide and silica, etc. The gas barrier layer 50 can be produced by a vacuum deposition method or the like.
[0063] The laminate 200 may further include a printed layer, for example, between the gas barrier layer 50 and the adhesive layer 20 . The printed layer may not contain chlorine from the viewpoint of suppressing coloration and odor generation when the printed layer is remelted. The printed layer may be formed of a biomass material from the viewpoint of environmental consideration. The printing layer is a layer formed by using ink made of, for example, a urethane-based, acrylic-based, nitrocellulose-based, or rubber-based binder resin to which various pigments, plasticizers, drying agents, stabilizers, etc. are added. This printing layer can display characters, pictures, etc.
[0064] The ink may be either water-based or oil-based, but is preferably water-based. Water-based inks use water or alcohol as a solvent, and therefore can further reduce the environmental impact. In particular, when the adhesive is a solventless adhesive, the use of water-based ink as the ink can significantly reduce the environmental impact. In addition, the ink may be biomass ink or not, but from the viewpoint of reducing the environmental impact, it is preferable that the ink is biomass ink. Here, biomass ink refers to ink containing components obtained from biological resources (biomass) such as cotton, pulp, rice bran, vegetable oil, and angiosperm seeds.
[0065] The base material layer 10 and the gas barrier layer 50 may be bonded to each other via an adhesive layer 40 as shown in FIG. 3, but the base material layer 10 and the gas barrier layer 50 may also be bonded directly to each other.
[0066] 2, the packaging bag 400 is formed using a pair of laminates 100, but the laminate 200 may be used instead of the laminate 100. The packaging bag may be produced by folding one of the laminates 100, 200 with the sealant layer 30 on the inside and bonding the overlapping peripheral portions together.
[0067] 2, the shape of the packaging bag 400 may be a standing pouch-shaped packaging bag, a two-sided bag, a three-sided bag, a four-sided bag, a palm-shaped bag, or a gusset bag. The packaging bag 400 may be provided with a spout or a synthetic resin fastener that can be repeatedly sealed by fitting a strip-shaped protrusion and a strip-shaped groove.
[0068] The embodiments of the present disclosure have been described above, and the outline of the present disclosure is as follows. [1] A laminate comprising a base layer and a sealant layer, wherein the ratio of the crystallinity of the base layer to the crystallinity of the sealant layer is 2.0 or more, and the crystallinity is the ratio of a crystalline peak area to a total peak area measured by a parallel beam X-ray diffraction method at a diffraction angle range of 10° to 30°. [2] The laminate according to [1], further comprising an adhesive layer between the base layer and the sealant layer. [3] The laminate according to [1] or [2], wherein the crystallinity of the base layer is greater than 35%. [4] Oxygen permeability at 30℃ and 70% RH is 200cc / m 2 The laminate according to any one of [1] to [3], wherein the maximum permeability is 1.0·day·atm or less. [5] The laminate according to any one of [1] to [4], wherein the ratio of the thickness of the base layer to the thickness of the sealant layer is 0.1 to 1.0. [6] The laminate according to any one of [1] to [5], further comprising a gas barrier layer between the base layer and the sealant layer. [7] The laminate according to any one of [1] to [6], wherein the content of the polyethylene resin in the entire laminate is 90 mass % or more. [8] A packaging bag obtained by using the laminate according to any one of [1] to [7]. [9] A packaging article comprising the packaging bag described in [8] and contents contained within the packaging bag. EXAMPLES
[0069] The present disclosure will be described more specifically with reference to the following examples, but the present disclosure is not limited to these examples.
[0070] Example 1 First, the base layer had a thickness of 25 μm, a crystallinity of 54.1%, and a density of 0.93 g / cm 3 A biaxially oriented polyethylene film was prepared. Next, a silicon oxide (SiOx) vapor deposition film having a thickness of 30 nm was formed as an inorganic compound layer on one surface of the base layer by using a vacuum deposition apparatus using an electron beam heating method. Next, an adhesive was applied onto the substrate layer and dried to form an adhesive layer having a thickness of 2 μm. The adhesive used was a mixture of 23 parts by mass of a solvent made by mixing ethyl acetate and methanol at a mass ratio of 1:1, 16 parts by mass of "Maxive C93T" manufactured by Mitsubishi Gas Chemical Co., Ltd., and 5 parts by mass of "Maxive M-100" manufactured by Mitsubishi Gas Chemical Co., Ltd. A sealant layer having a thickness of 120 μm, a crystallinity of 14.8%, and a density of 0.91 g / cm 3 A polyethylene film of this type was laminated to the base layer. In this way, a laminate was produced.
[0071] Example 2 The substrate layer has a thickness of 25 μm, a crystallinity of 71.8%, and a density of 0.96 g / cm 3 A laminate was produced in the same manner as in Example 1, except that a uniaxially oriented polyethylene film made of high density polyethylene ("PE3K-H" manufactured by Futamura Chemical Co., Ltd.) was used.
[0072] Example 3 The sealant layer has a thickness of 120 μm, a crystallinity of 11.2%, and a density of 0.91 g / cm 3 A laminate was produced in the same manner as in Example 1, except that a polyethylene film made of the linear low-density polyethylene resin was used.
[0073] Comparative Example 1 The substrate layer has a thickness of 30 μm, a crystallinity of 23.2%, and a density of 0.947 g / cm 3A laminate was produced in the same manner as in Example 1, except that an unstretched polyethylene film made of high density polyethylene was used.
[0074] <Crystallization degree> The crystallinity of the substrate layer and the sealant layer was determined by X-ray diffraction using a parallel beam method. Specifically, the crystallinity was determined as follows. First, the X-ray diffraction pattern of the base layer was obtained by out-of-plane measurement using a wide-angle X-ray diffractometer manufactured by Rigaku Corporation, scanning the diffraction angle range of 10° to 30° with 2θ / θ. The characteristic X-ray, CuKα, was used as the X-ray. The X-ray was collimated by a multilayer mirror and made incident on the surface of the base layer, and the diffracted X-ray was detected by a scintillation detector equipped with a flat collimator. From the obtained X-ray diffraction pattern, the peak area of the crystalline component and the halo pattern area of the amorphous component were determined, and the ratio of the peak area of the crystalline component to the sum of these areas (100%) was calculated as the crystallinity A (%) of the base layer. The crystallinity B of the sealant layer was determined in the same manner as above. Table 1 shows the crystallinity A of the base layer, the crystallinity B of the sealant layer, and the R1 (=A / B) results.
[0075] <Impact resistance> (1) Preparation of packaging items A rectangular sheet measuring 400 mm x 300 mm was cut out from the laminate of the Examples and Comparative Examples, folded in half, and both edges extending from the folded part were heat-sealed to prepare a packaging bag. At this time, an opening for inserting the contents was formed in the packaging bag. The dimensions of the packaging bag were 200 mm x 300 mm. Next, each packaging bag was filled with 1200 mL of tap water, and the opening was sealed. In this way, a packaged article was prepared. (2) Drop bag test The drop bag test was carried out by storing the packaged article obtained as described above in an environment at 5° C. for one day, and then dropping it from a height of 1 m ten times. (3) Test results The number of packaged articles whose packaging bags were torn was counted. The results are shown in Table 1. In Table 1, the results are shown as "number of packaged articles whose packaging bags were torn / 10." The number of packaged articles whose packaging bags were torn is an index of the impact resistance of the laminate.
[0076] [Table 1]
[0077] The results shown in Table 1 show that the number of torn packages in the packages of Examples 1 to 3 was significantly smaller than that in the package of Comparative Example 1. From the above, it was confirmed that the laminate of the present disclosure can improve impact resistance. [Explanation of symbols]
[0078] Reference Signs List 10: substrate layer; 20, 40: adhesive layer; 30: sealant layer; 50: gas barrier layer; 100, 200: laminate; 400: packaging bag; 500: packaged article; C: contents.
Claims
1. A substrate layer and a sealant layer are provided. A laminate, wherein the ratio of the crystallinity of the base layer to the crystallinity of the sealant layer is 2.0 or more, and the crystallinity is the ratio of a crystalline peak area to a total peak area measured by a parallel beam method of X-ray diffraction at a diffraction angle range of 10° to 30°.
2. The laminate of claim 1 further comprising an adhesive layer between the substrate layer and the sealant layer.
3. The laminate of claim 1 , wherein the substrate layer has a crystallinity of greater than 35%.
4. Oxygen permeability at 30°C and 70% RH is 200cc / m 2 2. The laminate according to claim 1, wherein the thermal expansion coefficient is 0.05-0.55×day·atm or less.
5. 2. The laminate according to claim 1, wherein the ratio of the thickness of the base layer to the thickness of the sealant layer is 0.1 to 1.
0.
6. The laminate according to claim 1 , further comprising a gas barrier layer between the substrate layer and the sealant layer.
7. The laminate according to claim 1 , wherein the content of the polyethylene resin in the entire laminate is 90 mass % or more.
8. A packaging bag obtained by using the laminate according to any one of claims 1 to 7.
9. The packaging bag according to claim 8, and contents contained within the packaging bag.
Citation Information
Patent Citations
Gas barrier film, laminate, and packaging material
JP7036266B1