Method of manufacturing resin particle dispersion liquid and method of manufacturing toner particles
By circulating the mixture of oil and aqueous phases during emulsification, the method addresses the issue of coarse particle generation in resin particle production, achieving improved image quality and energy efficiency in toner manufacturing.
Patent Information
- Application Number
- JP2023078875
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
AI Technical Summary
Existing methods for producing resin particles in toner manufacturing generate coarse particles due to uneven phase inversion during emulsification, leading to poor image quality and increased energy consumption.
A method involving the circulation of the mixture of an oil phase and an aqueous medium during phase inversion emulsification to refine resin particles, using specific stirring mechanisms and crushers to minimize coarse particle generation and achieve a sharp particle size distribution.
This approach effectively suppresses the formation of coarse particles, resulting in a resin particle dispersion with a sharp particle size distribution, enhancing image quality and reducing energy consumption.
Smart Images

Figure 2024162897000002 
Figure 2024162897000003 
Figure 2024162897000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a resin particle dispersion and a method for producing toner particles. [Background technology]
[0002] Resin particles are widely used as toner for image forming devices such as multi-function peripherals (MFPs) and printers in various places such as offices. In order to reduce the burden on the environment, for example, reduction in power consumption by improving the low-temperature fixing property of the toner itself and reduction in energy used in the toner manufacturing process are being considered.
[0003] As a method for improving the low-temperature fixing property of a toner, a method for lowering the glass transition temperature or softening point of a resin, a method for adding a crystalline resin, etc. are widely known. As a method for achieving high image quality, it is known to improve the reproduction of fine lines by using a toner with a small particle size and narrow particle size distribution, and to improve the color reproduction and coloring degree by improving the dispersion of a colorant. In addition, a pulverization method was used as a method for manufacturing a toner, but due to the large amount of energy used in the manufacturing process and the trend toward smaller toner diameters, chemical toners such as suspension polymerization have also become mainstream.
[0004] One method for reducing the amount of chemicals used in toner production is the phase inversion emulsification method, which can reduce the amount of surfactants used. However, in the toner production process using the phase inversion emulsification method, coarse particles may be generated, so in order to achieve high image quality, it is important to make the particle size distribution of the toner particles sharp.
[0005] For example, in Patent Document 1, the maximum stirring power in a stirring tank during phase inversion emulsification is adjusted to sharpen the particle size distribution of resin particles.
[0006] In Patent Document 2, the shape of the stirring blades in the stirring tank used for phase inversion emulsification is adjusted to sharpen the particle size distribution of the resin particles. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a method for producing a resin particle dispersion liquid that suppresses the generation of coarse particles. [Means for solving the problem]
[0008] The present invention provides a method for producing a resin particle dispersion, comprising the steps of: The method includes a step of preparing an oil phase by dissolving or dispersing a binder resin in an organic solvent, and a step of adding an aqueous medium to the oil phase to perform phase inversion emulsification to obtain a dispersion of resin particles, wherein in the phase inversion emulsification, a mixture of the oil phase and the aqueous medium is stirred and the mixture is circulated, and the resin particles are refined during the circulation. A method for producing a resin particle dispersion. Effect of the Invention
[0009] According to the present invention, there is provided a method for producing a resin particle dispersion liquid that suppresses the generation of coarse particles. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic diagram illustrating an example of a stirring tank and a circulation path outside the tank used in the method for producing a resin particle dispersion of the present invention. FIG. [Diagram 2] 1 is a schematic diagram illustrating an example of a stirring tank and a circulation path within the tank used in the method for producing a resin particle dispersion of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the embodiments of the present invention will be described in detail. Note that the embodiments are not limited by the following description, and can be appropriately modified without departing from the gist of the present invention. In addition, in this specification, "to" indicating a numerical range means that the numerical values before and after it are included as the lower and upper limits, unless otherwise specified.
[0012] <Resin particle dispersion liquid manufacturing equipment> One of the factors that cause coarse particles to be generated in phase inversion emulsification is uneven distribution of phase inversion due to insufficient shear force during phase inversion emulsification, which generates coarse particles. Therefore, in the method for producing a resin particle dispersion according to this embodiment, in addition to stirring the mixture of the oil phase and the aqueous medium, the mixture is circulated and the resin particles are refined during circulation. As a result, even when the shear force is insufficient with stirring alone, the generation of coarse particles is suppressed by the refinement, and a resin particle dispersion with a sharp particle size distribution can be produced.
[0013] FIG. 1 is a schematic diagram showing an example of a stirring tank and a circulation path outside the tank used in the method for producing a resin particle dispersion according to the present embodiment. In Fig. 1, an agitator blade 2 driven by an agitator motor 3 is provided inside an agitator tank 1. The agitator motor 3 can agitate a mixed liquid 8 by rotating in one direction, or rotating in one direction and / or in the opposite direction, or rotating (rocking) in one direction and in the opposite direction at a predetermined rotation angle. The stirring tank 1 is provided with a circulation line 5 that takes the mixed liquid out of the tank from the bottom side and sends the mixed liquid to the top side of the stirring tank 1. In the example of Fig. 1, the circulation line 5 is provided with a liquid delivery pump 6 and a grinder 7. By providing a mechanism for micronizing during circulation in this way, the generation of coarse particles can be suppressed. In addition, the circulating flow of the mixed liquid accompanying the circulation shown in Fig. 1 is vertical with respect to the stirring tank, but the direction of this circulating flow is not limited to the vertical direction and may be, for example, a radial flow of the stirring tank. However, the vertical flow can enhance the dispersion effect because it crosses the circumferential flow of the mixed liquid accompanying the rotation of the stirring blade.
[0014] There are no particular limitations on the stirring blades 2 in the stirring tank, but for example, stirring blades such as paddle blades, anchor blades, helical ribbon blades, screw blades, MAXBLEND (manufactured by Sumitomo Heavy Industries Process Equipment), Supermix (manufactured by Satake Chemical Machinery Co., Ltd.), and Fullzone (manufactured by Kobelco Environmental Solutions Co., Ltd.) can be used.
[0015] There are no particular limitations on the grinder 7 as long as it is capable of refining and / or dispersing the resin particles in the mixed liquid. For example, a bead mill such as Star Mill LMZ (manufactured by Ashizawa Finetech Co., Ltd.) or a high-efficiency disperser such as Ebara Milder (manufactured by Pacific Machinery Co., Ltd.) can be used.
[0016] As shown in FIG. 2, the circulation path may be provided inside the tank. In Fig. 2, an agitator blade 2 driven by an agitator motor 3 is provided inside an agitator tank 1. The agitator motor 3 can agitate a mixed liquid 8 by rotating in one direction, or rotating in one direction and / or in the opposite direction, or rotating (rocking) in the forward and reverse directions at a predetermined rotation angle. A circulation line 5 is provided within the mixing tank 1, which draws the mixed liquid from the bottom and delivers the mixed liquid to the upper side of the mixing tank 1. In the example of Fig. 2, a liquid feed pump 6 and a pulverizer 7 are provided in the circulation line 5. The liquid feed pump 6 and the pulverizer 7 may be unitized and placed in a unit box, and the unit box may be structured to be detachable from the inner wall of the tank, so that the unit box can be attached or detached depending on the amount of mixed liquid to be stirred in the stirring layer or the type of mixed liquid.
[0017] The method for producing a resin particle dispersion liquid and the method for producing toner particles according to the present embodiment will be described in detail below. The method for producing toner particles according to the present embodiment includes an oil phase preparation step, an aqueous phase preparation step, a phase inversion emulsification step, a solvent removal step, an aggregation step, and a fusion step, and further includes other steps such as a shell formation step, a washing step, a drying step, an annealing step, and an external addition step, as necessary. First, the raw materials of the toner particles will be described in detail.
[0018] <Organic solvent> The organic solvent can be appropriately selected, and for example, a volatile organic solvent with a boiling point of less than 100° C. is preferred from the viewpoint of ease of removal in the case of removing the organic solvent in a later step. Examples of such organic solvents include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, methanol, ethanol, isopropyl alcohol, etc. These can be used alone or in combination of two or more kinds.
[0019] When the resin to be dissolved or dispersed in the organic solvent is a resin having a polyester skeleton, ester-based solvents such as methyl acetate, ethyl acetate, and butyl acetate, or ketone-based solvents such as methyl ethyl ketone and methyl isobutyl ketone are preferred in terms of high solubility. Among these, methyl acetate, ethyl acetate, or methyl ethyl ketone, which have high solvent removability, are more preferred. Among these, ethyl acetate is even more preferred because it increases the selectivity of materials when preparing a master batch or an oil phase.
[0020] <Binding resin> The binder resin can be appropriately selected, and is preferably a resin that is soluble in an organic solvent and insoluble or almost insoluble in water.The resins used include, for example, polystyrene, styrene-acrylic copolymer, polyvinyl chloride, polyvinyl acetate, polymethacrylic acid ester, polymethyl acrylate, polyacrylic acid ester, polyacrylonitrile, epoxy resin, polyethylene, polyurethane, polyester, polyethylene terephthalate, polyamide, paraffin wax, etc. These may be used alone or in combination.From the viewpoint of obtaining good fixing property, polyester resin is more preferable.
[0021] [Polyester resin] When producing a toner for developing an electrostatic latent image in electrophotography, a toner having excellent fixing properties can be obtained by using a resin having a polyester skeleton. Examples of the resin having a polyester skeleton include polyester resins and block polymers of polyester and resins having other skeletons. Among them, the use of a polyester resin is preferred because the uniformity of the obtained toner particles is improved.
[0022] Examples of polyester resins include ring-opening polymers of lactones, condensation polymers of hydroxycarboxylic acids, and condensation polymers of polyhydric alcohols and polycarboxylic acids. From the viewpoint of freedom in design, condensation polymers of polyhydric alcohols and polycarboxylic acids are preferred.
[0023] The weight average molecular weight (Mw) of the polyester resin is usually 1,000 to 30,000, preferably 3,000 to 15,000, and more preferably 5,000 to 12,000. If it is less than 1,000, the heat resistant storage stability may deteriorate, and if it exceeds 30,000, good low temperature fixability may not be obtained.
[0024] The glass transition temperature (Tg) of the polyester resin is preferably 35 to 80° C., more preferably 40 to 70° C., and even more preferably 45 to 65° C. If it is less than 35° C., the heat-resistant storage stability of the resulting toner may deteriorate, and if it exceeds 80° C., good fixability may not be obtained.
[0025] The polyhydric alcohol includes diols and polyhydric alcohols having a valence of three or more. A diol alone or a mixture of a diol and a small amount of a polyhydric alcohol having a valence of three or more is preferred.
[0026] Examples of diols include alkylene glycols (ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, etc.); alkylene ether glycols (diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, etc.); alicyclic diols (1,4-cyclohexanedimethanol, hydrogenated bisphenol A, etc.); bisphenols (bisphenol A, bisphenol F, bisphenol S, etc.); alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts of the above alicyclic diols; 3,3'-difluoro-4,4'-dihydroxybiphenyl; bis(hydroxyphenyl)alkanes such as bis(3-fluoro-4-hydroxyphenyl)methane, 1-phenyl-1,1-bis(3-fluoro-4-hydroxyphenyl)ethane, 2,2-bis(3-fluoro-4-hydroxyphenyl)propane, 2,2-bis(3,5-difluoro-4-hydroxyphenyl)propane (also known as tetrafluorobisphenol A) and 2,2-bis(3-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane; bis(4-hydroxyphenyl)ethers such as bis(3-fluoro-4-hydroxyphenyl)ether; and alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts of the above bisphenols. Among these, alkylene glycols having 2 to 12 carbon atoms and alkylene oxide adducts of bisphenols are preferred, and alkylene oxide adducts of bisphenols and combinations of these with alkylene glycols having 2 to 12 carbon atoms are particularly preferred.
[0027] Examples of trihydric or higher polyhydric alcohols include trihydric to octahydric or higher polyhydric aliphatic alcohols (glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, etc.); trihydric or higher phenols (trisphenol PA, phenol novolac, cresol novolac, etc.); and alkylene oxide adducts of the above trihydric or higher polyphenols.
[0028] Examples of the polybasic carboxylic acid include dicarboxylic acids and polybasic carboxylic acids having three or more valences. A dicarboxylic acid alone or a mixture of a dicarboxylic acid and a small amount of a polybasic carboxylic acid having three or more valences is preferred.
[0029] Examples of dicarboxylic acids include alkylene dicarboxylic acids (such as succinic acid, adipic acid, and sebacic acid); alkenylene dicarboxylic acids (such as maleic acid and fumaric acid); aromatic dicarboxylic acids (such as phthalic acid, isophthalic acid, terephthalic acid, and 2,6-naphthalenedicarboxylic acid), 3-fluorophthalic acid, 2-fluoroisophthalic acid, 2-fluoroterephthalic acid, 2,4,5,6-tetrafluoroisophthalic acid, 2,3,5,6-tetrafluoroterephthalic acid, 5-trifluoromethylisophthalic acid, 2,2-bis(4-carboxyphenyl)hexafluoropropane, 2,2-bis(3-carboxyphenyl)hexafluoropropane, 2,2'-bis(trifluoromethyl)-4,4'-biphenyldicarboxylic acid, 3,3'-bis(trifluoromethyl)-4,4'-biphenyldicarboxylic acid, and 2,2'-bis(trifluoromethyl)-3,3'-biphenyldicarboxylic acid. Among these, alkenylene dicarboxylic acids having 4 to 20 carbon atoms and aromatic dicarboxylic acids having 8 to 20 carbon atoms are preferred.
[0030] Examples of trivalent or higher polyvalent carboxylic acids include aromatic polyvalent carboxylic acids having 9 to 20 carbon atoms (eg, trimellitic acid, pyromellitic acid, etc.).
[0031] As the polyvalent carboxylic acid, the acid anhydride or lower alkyl ester (methyl ester, ethyl ester, isopropyl ester, etc.) of the above-mentioned compound may be reacted with a polyhydric alcohol.
[0032] The ratio of polyhydric alcohol to polycarboxylic acid, expressed as the equivalent ratio [OH] / [COOH] of hydroxyl group [OH] to carboxyl group [COOH], is usually 2 / 1 to 1 / 2, preferably 1.5 / 1 to 1 / 1.5, and more preferably 1.3 / 1 to 1 / 1.3.
[0033] <Coloring agent> As the colorant used in the present invention, known dyes and pigments can be used, for example, carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ochre, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, anthrazan yellow BGL, iridium yellow, etc. Soindolinone Yellow, Bengala, Red Lead, Cinnabar, Cadmium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Carmine BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Red F5R, Brilliant Carmine 6B, Pigment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkaline Blue Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake,Malachite green lake, phthalocyanine green, anthraquinone green, titanium dioxide, zinc oxide, lithopone and mixtures thereof can be used.
[0034] Regarding the colorant, a master batch may be prepared by kneading the colorant with a resin, and the master batch may be dissolved or dispersed together with a binder resin in an organic solvent to prepare the oil phase.
[0035] The resin used for preparing the master batch can be appropriately selected, but is preferably a resin that is soluble in an organic solvent and insoluble or almost insoluble in water.Examples of the resin used include polystyrene, styrene-acrylic copolymer, polyvinyl chloride, polyvinyl acetate, polymethacrylic acid ester, polymethyl acrylate, polyacrylic acid ester, polyacrylonitrile, epoxy resin, polyethylene, polyurethane, polyester, polyethylene terephthalate, polyamide, paraffin wax, etc. These may be used alone or in combination.From the viewpoint of obtaining good fixability, polyester resin is preferred.
[0036] The master batch can be prepared by kneading the above-mentioned colorant and the above-mentioned resin. For example, a general kneader such as a twin-screw extrusion kneader, a three-roll mill, or a lab plastomill can be used for the kneading process. An internal additive may be added during the kneading process. It is preferable to heat the mixture during kneading, and the heating conditions can be appropriately set.
[0037] The ratio of the resin and the colorant in preparing the master batch can be appropriately selected.
[0038] <Crystalline polyester resin> Toner particles according to the present embodiment preferably contain a crystalline resin in order to improve low-temperature fixability. Among them, crystalline polyester resins have high crystallinity and therefore exhibit thermal melting properties that show a rapid change in viscosity near the fixation start temperature (sharp melt properties). The crystalline polyester resins having such properties are obtained from polyhydric alcohols and polycarboxylic acids such as polycarboxylic acids, polycarboxylic anhydrides, and polycarboxylic esters, or derivatives thereof.
[0039] In the present invention, the crystalline polyester resin refers to a resin obtained by using a polyhydric alcohol and a polycarboxylic acid or a derivative thereof, such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester, as described above. Modified polyester resins, such as prepolymers and resins obtained by subjecting the prepolymers to a crosslinking and / or elongation reaction, do not belong to the crystalline polyester resin.
[0040] The polyhydric alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyhydric alcohol include diols and trihydric or higher alcohols.
[0041] Examples of the diol include saturated aliphatic diols. Examples of the saturated aliphatic diol include linear saturated aliphatic diols and branched saturated aliphatic diols. Among these, linear saturated aliphatic diols are preferred, and linear saturated aliphatic diols having 2 to 12 carbon atoms are more preferred. If the saturated aliphatic diol is a branched type, the crystallinity of the crystalline polyester resin may decrease, resulting in a decrease in melting point. In addition, if the carbon number of the saturated aliphatic diol exceeds 12, it becomes difficult to obtain a practical material.
[0042] Examples of the saturated aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,20-eicosanediol, etc. Among these, ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol are preferred in terms of the high crystallinity of the crystalline polyester resin and excellent sharp melt properties.
[0043] Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, etc. These may be used alone or in combination of two or more.
[0044] The polyvalent carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include divalent carboxylic acids and trivalent or higher carboxylic acids.
[0045] Examples of the divalent carboxylic acid include saturated aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, and 2,6-naphthalenedicarboxylic acid; and the like. Further examples include anhydrides of these and lower (carbon number 1 to 3) alkyl esters of these.
[0046] Examples of the trivalent or higher carboxylic acid include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and the like, as well as their anhydrides and lower (carbon number 1 to 3) alkyl esters, etc. These may be used alone or in combination of two or more.
[0047] The crystalline polyester resin is preferably composed of a linear saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a linear saturated aliphatic diol having 2 to 12 carbon atoms, which provides high crystallinity and excellent sharp melting properties, thereby enabling the toner to exhibit excellent low-temperature fixing properties.
[0048] In addition, as a method for controlling the crystallinity and softening point of a crystalline polyester resin, there can be mentioned a method of designing and using a non-linear polyester obtained by adding a trivalent or higher polyhydric alcohol such as glycerin to the alcohol component during polyester synthesis, or a trivalent or higher polycarboxylic acid such as trimellitic anhydride to the acid component and carrying out condensation polymerization.
[0049] The molecular structure of the crystalline polyester resin in this embodiment can be confirmed by NMR measurement of a solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc. -1 Or 990±10cm -1 to the δ of olefin CH One example is one that has absorption based on (out-of-plane bending vibration).
[0050] As for the molecular weight of the crystalline polyester resin, from the viewpoint that a low molecular weight with a sharp molecular weight distribution is excellent in low temperature fixability, and a large amount of low molecular weight components deteriorates heat resistance storage stability, the following has been found to be preferable, for example. In the molecular weight distribution by GPC of the soluble portion in orthodichlorobenzene, the molecular weight distribution diagram with the horizontal axis being log(M) and the vertical axis being weight % has a peak position in the range of 3.5 to 4.0, the half width of the peak is 1.5 or less, and the weight average molecular weight (Mw) is preferably 3,000 to 30,000, the number average molecular weight (Mn) is 1,000 to 10,000, and Mw / Mn is 1 to 10. Furthermore, the weight average molecular weight (Mw) is preferably 5,000 to 15,000, the number average molecular weight (Mn) is preferably 2,000 to 10,000, and Mw / Mn is preferably 1 to 5.
[0051] From the viewpoint of the affinity between paper and resin, the acid value of the crystalline polyester resin is preferably 5 mgKOH / g or more in order to achieve the desired low-temperature fixability. In addition, for the preparation of fine particles by phase inversion emulsification, the acid value is more preferably 7 mgKOH / g or more. On the other hand, in order to improve hot offset resistance, the acid value is preferably 45 mgKOH / g or less. In addition, the hydroxyl value of the crystalline polyester resin is preferably 0 to 50 mgKOH / g, more preferably 5 to 50 mgKOH / g, in order to achieve a predetermined low-temperature fixability and good electrostatic chargeability.
[0052] <Release agent> Wax can be used as a release agent. The wax is not particularly limited and can be appropriately selected depending on the purpose, but a release agent with a low melting point of 50°C to 120°C is preferable. The release agent with a low melting point is dispersed in the resin, and effectively acts as a release agent between the fixing roller and the toner interface, thereby improving hot offset resistance even in an oil-less case (no release agent such as oil is applied to the fixing roller).
[0053] Suitable examples of the release agent include waxes. Examples of the waxes include natural waxes such as vegetable waxes such as carnauba wax, cotton wax, wood wax, and rice wax; animal waxes such as beeswax and lanolin; mineral waxes such as ozokerite and cerusine; and petroleum waxes such as paraffin, microcrystalline, and petrolatum. In addition to these natural waxes, synthetic hydrocarbon waxes such as Fischer-Tropsch wax and polyethylene wax; synthetic waxes such as esters, ketones, and ethers; and the like. Furthermore, fatty acid amides such as 12-hydroxystearic acid amide, stearic acid amide, phthalic anhydride, and chlorinated hydrocarbons; homopolymers or copolymers of polyacrylates such as poly-n-stearyl methacrylate and poly-n-lauryl methacrylate, which are low molecular weight crystalline polymer resins (for example, copolymers of n-stearyl acrylate and ethyl methacrylate); and crystalline polymers having long alkyl groups on the side chains may be used. These may be used alone or in combination of two or more.
[0054] The melting point of the wax is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50° C. to 120° C., and more preferably 60° C. to 90° C. If the melting point is 50° C. or higher, the wax can be prevented from adversely affecting the heat resistance storage stability, and if the melting point is 120° C. or lower, the problem of cold offset occurring during fixing at low temperatures can be effectively prevented.
[0055] The melt viscosity of the wax is preferably 5 cps to 1,000 cps, more preferably 10 cps to 100 cps, as measured at a temperature 20° C. higher than the melting point of the wax. If the melt viscosity is 5 cps or more, the release property can be prevented from decreasing, and if it is 1,000 cps or less, the effects of hot offset resistance and low-temperature fixability can be sufficiently exhibited.
[0056] The wax content in the toner is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0% by mass to 40% by mass, and more preferably 3% by mass to 30% by mass. If the wax content is 40% by mass or less, the fluidity of the toner can be prevented from deteriorating.
[0057] <External additives> The external additive is not particularly limited and can be appropriately selected depending on the purpose. For example, inorganic fine particles and polymer fine particles can be used as the external additive.
[0058] The primary particle diameter of the inorganic fine particles is preferably 5 nm to 2 μm, and more preferably 5 nm to 500 nm. The specific surface area as measured by the BET method is preferably 20 to 500 m. 2 The content of the inorganic fine particles is preferably 0.01 to 5% by mass of the toner.
[0059] Specific examples of inorganic fine particles include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, red iron oxide, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, and silicon nitride.
[0060] Examples of polymeric fine particles include polystyrene obtained by soap-free emulsion polymerization, suspension polymerization, or dispersion polymerization, methacrylate or acrylate copolymers, silicone, benzoguanamine, nylon, or other condensation polymerization systems, and polymer particles made of thermosetting resins.
[0061] Such external additives can be surface-treated to increase hydrophobicity and prevent deterioration of fluidity and electrostatic charge even under high humidity. For example, silane coupling agents, silylating agents, silane coupling agents having a fluorinated alkyl group, organic titanate coupling agents, aluminum coupling agents, silicone oils, modified silicone oils, etc. are preferred surface treatment agents.
[0062] In addition to the above, a cleaning property improver may be used as an external additive. Examples of cleaning property improvers for removing the developer remaining on the photoconductor or primary transfer medium after transfer include fatty acid metal salts such as zinc stearate, calcium stearate, and stearic acid, and polymer fine particles produced by soap-free emulsion polymerization such as polymethyl methacrylate fine particles and polystyrene fine particles. The polymer fine particles preferably have a relatively narrow particle size distribution and a volume average particle size of 0.01 μm to 1 μm.
[0063] <Method of manufacturing toner particles> Hereinafter, the method for producing toner particles according to this embodiment will be described in detail.
[0064] [Oil phase preparation process] In the oil phase preparation step, the binder resin is dissolved or dispersed in an organic solvent to prepare the oil phase. A colorant or the like may be further added to the oil phase.
[0065] The oil phase may be prepared by gradually adding the binder resin, colorant, etc. to the organic solvent while stirring the organic solvent, and dissolving or dispersing the binder resin, colorant, etc. In the case of dispersion, a known dispersing machine, for example, a bead mill or a disk mill, may be used.
[0066] After the oil phase is prepared, it may be neutralized with an alkaline aqueous solution. Examples of the alkaline aqueous solution include an aqueous ammonia solution and sodium hydroxide. Neutralizing the oil phase has the advantage of improving the water dispersibility of the resin and facilitating phase inversion emulsification.
[0067] [Phase inversion emulsification process] In the phase inversion emulsification step, an aqueous medium is added to the oil phase to effect phase inversion emulsification to produce a resin particle dispersion. By passing through the phase inversion step of the water-in-oil dispersion to the oil-in-water dispersion, granulation can be performed with a reduced amount of surfactant used.
[0068] The aqueous medium is not particularly limited as long as it causes phase inversion emulsification, and can be appropriately selected according to the purpose. For example, water, a solvent miscible with water, a mixture thereof, etc. can be mentioned. These can be used alone or in combination of two or more. Among these, water is preferred.
[0069] The solvent miscible with water is not particularly limited as long as it causes phase inversion emulsification, and can be appropriately selected depending on the purpose, and examples thereof include alcohol, dimethylformamide, tetrahydrofuran, cellosolves, lower ketones, etc. Examples of the alcohol include methanol, isopropanol, ethylene glycol, etc. Examples of the lower ketones include acetone, methyl ethyl ketone, etc.
[0070] During phase inversion emulsification, in addition to stirring the resin particle dispersion, a production device as shown in Figures 1 and 2 is used in which the resin particle dispersion is circulated and the resin particles are refined during circulation, thereby suppressing the generation of coarse particles and enabling the production of a resin particle dispersion with a sharp particle size distribution.
[0071] [Solvent removal process] In the solvent removal step, the organic solvent is removed from the obtained resin particle dispersion liquid.
[0072] In order to remove the organic solvent from the obtained resin particle dispersion, a method can be adopted in which the temperature of the entire system is gradually raised while being stirred, and the organic solvent in the droplets is evaporated and removed.
[0073] Alternatively, the obtained resin particle dispersion may be sprayed into a dry atmosphere while being stirred to completely remove the organic solvent from the droplets, or the resin particle dispersion may be reduced in pressure while being stirred to evaporate and remove the organic solvent.
[0074] These means may be used alone or in combination.
[0075] The drying atmosphere into which the resin particle dispersion is sprayed generally includes, for example, air, nitrogen, carbon dioxide, a gas obtained by heating a combustion gas, etc., and in particular, various air streams heated to a temperature equal to or higher than the boiling point of the highest boiling point solvent used. In such a method, the desired quality can be sufficiently obtained by a short-time treatment using a spray dryer, a belt dryer, a rotary kiln, etc.
[0076] [Agglutination process] The resulting resin particle dispersion is agitated to aggregate the particles to a desired particle size, thereby obtaining aggregated particles.
[0077] To achieve flocculation, existing methods such as adding a flocculant or adjusting the pH can be used. When adding a flocculant, it may be added as is, but it is preferable to make an aqueous solution of the flocculant, since this can avoid localized high concentration. It is also preferable to add the flocculant gradually while monitoring the particle size of the resin particles.
[0078] The temperature of the dispersion during aggregation is preferably near the glass transition temperature Tg of the resin used. If the temperature of the resin particle dispersion is too low, aggregation does not proceed very well, resulting in poor efficiency. If the temperature of the resin particle dispersion is too high, the aggregation rate increases, resulting in the generation of coarse particles and a deterioration in particle size distribution.
[0079] When the target particle size is reached, aggregation is stopped by adding a salt with a low ionic valence or a chelating agent, adjusting the pH, lowering the temperature of the dispersion, adding a large amount of an aqueous medium to dilute the concentration, or the like.
[0080] By the above method, a dispersion of aggregated particles can be obtained.
[0081] As the flocculant, a known one can be used. For example, metal salts of monovalent metals such as sodium and potassium, metal salts of divalent metals such as calcium and magnesium, and metal salts of trivalent metals such as iron and aluminum can be used. The amount of the flocculant to be added is not particularly limited and can be selected appropriately.
[0082] [Fusing process] Next, the obtained aggregated particles are fused by heat treatment to reduce unevenness and to make them spherical. Fusion can be performed by heating the dispersion of the aggregated particles while stirring. The temperature of the liquid is preferably near a temperature above the glass transition temperature Tg of the resin used.
[0083] By the above method, a toner particle dispersion liquid can be obtained.
[0084] [Cleaning process] The toner particle dispersion obtained by the above method may contain sub-materials such as aggregating agents in addition to the toner particles, so washing is carried out in order to extract only the toner particles from the dispersion.
[0085] The washing method of the toner particles includes, for example, a centrifugation method, a vacuum filtration method, a filter press method, etc., but is not particularly limited in the present invention. Any of the methods can obtain a cake of toner particles, but if the toner particles cannot be sufficiently washed in one operation, the obtained cake may be dispersed again in an aqueous medium to make a slurry, and the process of extracting the toner particles by any of the above methods may be repeated. In addition, if washing is performed by the vacuum filtration method or the filter press method, a method may be adopted in which the aqueous medium is penetrated into the cake to wash away the secondary materials that are incorporated in the toner particles.
[0086] The aqueous medium used for this washing may be water or a mixed solvent of water and an alcohol such as methanol or ethanol, etc. Considering the cost and the environmental load due to wastewater treatment, it is preferable to use water.
[0087] [Drying process] Since the washed toner particles contain a large amount of the aqueous medium, the toner particles can be obtained by drying and removing the aqueous medium.
[0088] For the drying method, a dryer such as a spray dryer, a vacuum freeze dryer, a reduced pressure dryer, a stationary shelf dryer, a movable shelf dryer, a fluidized bed dryer, a rotary dryer, or an agitator dryer can be used.
[0089] The dried toner particles are preferably dried until the moisture content is finally reduced to less than 1%. In addition, the dried toner particles may be in a state of soft aggregation. If this causes inconvenience during use, the toner particles may be disintegrated using a device such as a jet mill, a Henschel mixer, a super mixer, a coffee mill, an Oster blender, or a food processor to break up the soft aggregation.
[0090] [Annealing process] In this embodiment, annealing may be performed. When a crystalline resin is added, annealing after drying causes phase separation between the non-crystalline resin and the crystalline resin, improving fixability. Specifically, the toner may be stored for 10 hours or more at a temperature near the glass transition temperature Tg of the resin.
[0091] [External addition process] Toner particles obtained in this embodiment may be added or mixed with external additives such as inorganic fine particles, polymeric fine particles, and cleaning aids in order to impart fluidity, chargeability, cleaning properties, and the like.
[0092] Specific mixing means include a method in which an impact force is applied to the mixture by blades rotating at high speed, and a method in which the mixture is introduced into a high-speed air current, accelerated, and the particles collide with each other or the composite particles with an appropriate collision plate.
[0093] Examples of equipment include an Angmill (manufactured by Hosokawa Micron Corporation), a modified I-type mill (manufactured by Japan Pneumatic Co., Ltd.) with reduced grinding air pressure, a hybridization system (manufactured by Nara Machinery Works, Ltd.), a Cryptron system (manufactured by Kawasaki Heavy Industries, Ltd.), and an automatic mortar.
[0094] Through the above steps, toner particles can be obtained.
[0095] <Measurement method> [Particle size of dispersion liquid] The particle size of the resin particle dispersion in the present invention can be measured, for example, using a Nanotrack particle size distribution analyzer UPA-EX150 (Nikkiso Co., Ltd., dynamic light scattering method / laser Doppler method). As a specific measurement method, the dispersion in which the resin particles are dispersed is adjusted to a measurement concentration range and measured. At that time, a background measurement is performed in advance using only the dispersion solvent of the dispersion. With this measurement method, it is possible to measure the volume average particle size range of the resin fine particles used in the present invention, from several tens of nm to several μm. In the present invention, the particle size refers to the volume average particle size (volume average diameter).
[0096] [Melting point and glass transition temperature Tg] The melting point and the glass transition temperature Tg can be measured, for example, using a DSC system (differential scanning calorimeter) ("Q-200", manufactured by TA Instruments). Specifically, the melting point and glass transition temperature of a sample can be measured by the following procedure. First, about 5.0 mg of the target sample is placed in an aluminum sample container, the sample container is placed on a holder unit, and set in an electric furnace. Next, in a nitrogen atmosphere, the sample is heated from -80°C to 150°C at a heating rate of 10°C / min (first heating). After that, the sample is cooled from 150°C to -80°C at a heating rate of 10°C / min, and further heated to 150°C at a heating rate of 10°C / min (second heating). During each of the first and second heating, a DSC curve is measured using a differential scanning calorimeter ("Q-200", manufactured by TA Instruments). From the obtained DSC curves, the DSC curve at the first temperature rise can be selected using the analysis program in the Q-200 system, and the glass transition temperature at the first temperature rise of the target sample can be obtained. Similarly, the DSC curve at the second temperature rise can be selected, and the glass transition temperature at the second temperature rise of the target sample can be obtained. In the present invention, Tg refers to the glass transition temperature at the second heating step.
[0097] [Molecular weight] The molecular weight of the polyester resin, vinyl copolymer resin, etc. used is measured by GPC (gel permeation chromatography) under the following conditions, unless otherwise specified. Equipment: HLC-8220GPC (Tosoh Corporation) Column: TSKgel SuperHZM-Mx3 ·Temperature: 40℃ Solvent: THF (tetrahydrofuran) ·Flow rate: 0.35mL / min Sample: 0.01mL of sample with a concentration of 0.05 to 0.6% From the molecular weight distribution of the toner resin measured under the above conditions, the weight average molecular weight Mw is calculated using a molecular weight calibration curve prepared from a monodisperse polystyrene standard sample. The monodisperse polystyrene standard sample is 5.8×10 2 , 1.085×10 4 , 5.95×10 4 , 3.2×10 5 , 2.56×10 6 , 2.93×10 3 , 2.85×10 4 , 1.48×10 5 , 8.417×10 5 , 7.5×10 6 Ten items from the above were used. EXAMPLES
[0098] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples.
[0099] <Preparation of polyester resin 1> In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 2 mol ethylene oxide adduct of bisphenol A / 3 mol propylene oxide adduct of bisphenol A (molar ratio 40 / 60) as a diol component, terephthalic acid / adipic acid (molar ratio 85 / 15) as a dicarboxylic acid component, and 3.5 mol% trimethylolpropane based on the total monomer amount were added so that the molar ratio of hydroxyl group to carboxylic acid (OH / COOH) was 1.2. Furthermore, 1,000 ppm of tetrabutyl orthotitanate based on the total monomer amount was added as a condensation catalyst, and the temperature was raised to 230°C over 2 hours under a nitrogen stream, and the reaction was carried out for 5 hours while distilling off the generated water. Then, the mixture was reacted for 4 hours under reduced pressure of 5mmHg to 15mmHg, and cooled to 180°C. Then, 1.0 mol% of trimellitic anhydride based on the total monomer amount and 200 ppm of tetrabutyl orthotitanate based on the total monomer amount were added, and the mixture was reacted at normal pressure and 180°C for 1 hour. Then, the mixture was further reacted for 3 hours under reduced pressure of 5mmHg to 20mmHg. In this way, a [polyester resin 1] was obtained, which has a glass transition temperature Tg of 57°C and a weight average molecular weight of 7,700, as determined from the DSC curve of the first heating cycle by DSC.
[0100] 390 parts by weight of 0.1 mol / L Na3PO4 aqueous solution was added to 1,150 parts by weight of pure water, and the mixture was stirred at 10,000 rpm using a mechanical disperser CLEARMIX (registered trademark) (manufactured by M-Technique Co., Ltd.) To this, 58 parts by weight of 1.0 mol / L CaCl2 aqueous solution was gradually added to prepare a dispersion containing Ca3(PO4)2. A polymerizable monomer composition was prepared by mixing and dissolving 80 parts by weight of styrene, 20 parts by weight of n-butyl acrylate, and 2.7 parts by weight of 2,2-azobis(2,4-dimethylvaleronitrile), and the mixture was added to the dispersion stirred at 8,000 rpm using CLEARMIX, and further stirred for 30 minutes. Thus, a polymerizable monomer composition dispersion was prepared.
[0101] This polymerizable monomer composition dispersion was put into a reaction vessel equipped with a stirring device, a temperature sensor, a cooling tube, and a nitrogen inlet tube, and polymerization treatment was carried out for 5 hours at a temperature of 60°C in the reaction vessel while stirring under a nitrogen stream. Furthermore, the temperature in the reaction vessel was raised to 80°C and polymerization treatment was carried out for 10 hours, and then the reaction vessel was cooled to room temperature. As a result, a binder resin was produced, and hydrochloric acid was added to the produced binder resin to dissolve Ca3(PO4)2, followed by washing with water, filtration, and drying to produce amorphous [vinyl resin 1]. The weight average molecular weight Mw of [vinyl resin 1] was 35,000, and the glass transition temperature Tg was 55°C.
[0102] <Masterbatch production> [Polyester resin 1] and Pigment Red 269 were premixed in a ratio of 1:1 using a Henschel mixer (Mitsui Miike Chemical Engineering Co., Ltd., FM20B), and then melted and kneaded at a temperature of 130°C using a twin-screw kneader (Ikegai Co., Ltd., PCM-30). The resulting kneaded product was rolled to a thickness of 2.7 mm using a roller, cooled to room temperature using a belt cooler, and coarsely pulverized to 200 μm to 300 μm using a hammer mill. In this way, [Master batch] was obtained.
[0103] <Preparation of Crystalline Polyester Resin Dispersion C-1> 1,6-hexanediol and sebacic acid were charged into a stirring tank equipped with a nitrogen inlet tube, a dehydration tube, and a thermocouple so that the ratio of OH groups to COOH groups (OH / COOH) was 1.1. The reaction was carried out while draining water along with 500 ppm of titanium tetraisopropoxide relative to the mass of the charged raw materials, and the temperature was finally raised to 235°C and the reaction was carried out for 1 hour. After that, the reaction was carried out for 6 hours under a reduced pressure of 10 mmHg or less. After that, the temperature was set to 185°C, trimellitic anhydride was added so that the molar ratio with COOH groups was 0.053, and the reaction was carried out for 2 hours with stirring to obtain [Crystalline polyester resin C-1]. Into the stirring tank, 55 parts by weight of [Crystalline polyester resin C-1], 40 parts by weight of methyl ethyl ketone, and 5 parts by weight of 2-propyl alcohol were added. Then, the mixture was stirred while being heated at the melting point temperature of [Crystalline polyester resin C-1] to dissolve [Crystalline polyester resin C-1]. Then, 28% by weight of ammonia aqueous solution was added so that the neutralization rate was 400%. The neutralization rate was calculated from the acid value of [Crystalline polyester resin C-1]. Furthermore, 130 parts by weight of ion-exchanged water was gradually added to carry out phase inversion emulsification, and then the solvent was removed. Then, ion-exchanged water was added to adjust the solid content concentration (concentration of crystalline polyester resin) to 25% by mass, and [Crystalline polyester resin dispersion C-1], which is a binder resin dispersion for toner, was obtained. The particle size of the crystalline polyester resin in [Crystalline polyester resin dispersion C-1] was 200 nm.
[0104] <Production of wax emulsion 1> To 100 parts by weight of ion-exchanged water, 28 parts by weight of HNP-9 (manufactured by Nippon Seiro) as a wax and Sanisol B50 as a surfactant were added. This was dispersed in a homogenizer while being heated to 90°C, to obtain [Wax Emulsion 1]. The solid content was 30%.
[0105] [Example 1] <Oil phase preparation process and aqueous phase preparation process> 120 parts by weight of ethyl acetate was added to 90 parts by weight of [Polyester resin 1] and 20 parts by weight of [Master batch], and the mixture was stirred to dissolve or disperse. Then, 5 parts by weight of a 28% by mass aqueous ammonia solution was added while stirring to achieve a neutralization rate of 500%, to prepare an oil phase. A surfactant ABS (alkylbenzene sulfonate) was added to 300 parts by weight of ion-exchanged water so that the concentration was 1% relative to the ion-exchanged water to prepare an aqueous phase.
[0106] <Phase inversion emulsification process> Using the equipment shown in Figure 1, which has a stirring tank with anchor blades, piping for circulating the stirring tank, a pump, and a disk mill, an oil phase was added to the stirring tank, and then the water phase was gradually added to the oil phase to perform phase inversion emulsification. During transfer emulsification, in addition to stirring in the mixing tank, the mixture of the oil and water phases was circulated using a pump and the mixture was refined using a disk mill.
[0107] After the phase inversion emulsification, the solvent was removed to obtain [Resin Particle Dispersion 1]. The solid content was adjusted to 20%.
[0108] [Example 2] [Resin particle dispersion 2] was obtained in the same manner as in Example 1, except that in the oil phase preparation step of Example 1, [polyester resin 1] was replaced with [vinyl resin 1].
[0109] [Example 3] Resin particle dispersion 3 was obtained in the same manner as in Example 1, except that 5 parts by weight of the 28% by mass aqueous ammonia solution was not added in the oil phase preparation step.
[0110] [Example 4] [Resin particle dispersion 4] was obtained in the same manner as in Example 1, except that in the phase inversion emulsification step of Example 1, a stirring tank having a paddle blade was used instead of the anchor blade.
[0111] [Comparative Example 1] [Resin particle dispersion 5] was obtained in the same manner as in Example 1, except that in the phase inversion emulsification step of Example 1, the mixed liquid of the oil phase and the water phase was not circulated or atomized.
[0112] [Comparative Example 2] A resin particle dispersion 6 was obtained in the same manner as in Example 2, except that in the phase inversion emulsification step of Example 2, the mixed liquid of the oil phase and the water phase was not circulated or atomized.
[0113] [Comparative Example 3] [Resin particle dispersion 7] was obtained in the same manner as in Example 3, except that in the phase inversion emulsification step of Example 3, the mixed liquid of the oil phase and the water phase was not circulated or atomized.
[0114] [Comparative Example 4] [Resin particle dispersion 8] was obtained in the same manner as in Example 4, except that in the phase inversion emulsification step of Example 4, the mixed liquid of the oil phase and the water phase was not circulated or atomized.
[0115] Using the resin particle dispersion of each example, toner particles were prepared as follows.
[0116] <Aggregation process and fusion process> 100 parts by weight of [Resin Particle Dispersion 1], 5.0 parts by weight of [Crystalline Polyester Resin Dispersion C-1], 5.0 parts by weight of [Wax Emulsion 1], and 300 parts by weight of ion-exchanged water were placed in a container and stirred for 1 minute. Next, 20 parts by weight of 5% magnesium chloride solution was dropped based on the solid content, and the mixture was stirred for another 5 minutes, and then heated to 60°C. After that, when the particle size reached 5.0 μm, 40 parts by weight of sodium chloride was added to terminate the aggregation process, and [Aggregated Slurry 1] was obtained. [Aggregated Slurry 1] was heated to 70°C while stirring, and cooled when the desired circularity of 0.96 was reached, and [Toner Dispersion 1] was obtained.
[0117] <Cleaning and drying processes> (1) 100 parts of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (at 12,000 rpm for 10 minutes), and then filtered. (2): 900 parts of ion-exchanged water was added to the filter cake of (1), and ultrasonic vibration was applied and mixed with a TK homomixer (rotation speed 12,000 rpm for 30 minutes), and then the mixture was filtered under reduced pressure. This operation was repeated until the electrical conductivity of the slurry liquid became 10 μC / cm or less, and then the mixture was filtered to obtain [Filter cake 1]. The [filter cake 1] was dried in a circulating air dryer at 45° C. for 72 hours and sieved through a 75 μm mesh to obtain [colored resin particles 1].
[0118] <External addition process> To 100 parts by weight of [Colored Resin Particles 1], 2.5 parts by weight of inorganic fine particles TS530 manufactured by Cabosil Corporation was added, and mixed for 10 minutes at 40 m / s in a Henschel mixer to obtain toner particles of Example 1.
[0119] [Examples 2 to 4, Comparative Examples 2 to 4] Toner particles of Examples 2 to 4 and Comparative Examples 2 to 4 were obtained in the same manner as in Example 1, except that in the aggregation step, [Resin particle dispersion 1] was changed to each resin particle dispersion.
[0120] [Example 5] A toner of Example 5 was obtained in the same manner as in Example 1, except that in the aggregation step of Example 1, 5.0 parts by weight of [Crystalline Polyester Resin Dispersion C-1] was not added.
[0121] [Comparative Example 5] A toner of Comparative Example 5 was obtained in the same manner as in Example 5, except that in the phase inversion emulsification step of Example 5, the mixed liquid of the oil phase and the water phase was not circulated and pulverized.
[0122] <Evaluation method> [Amount of coarse particles] Measurements were made using a laser diffraction particle size distribution analyzer (LA-960), and the particle size was evaluated on a four-level scale according to the percentage of particles with a particle size of 2 μm or more. (Evaluation Criteria) ◎(Excellent): 1% or less ○(Good): 3% or less △(Acceptable): 5% or less × (not allowed): 6% or more
[0123] [Low temperature fixability] Using the fixing unit of a color multifunction printer (imagio MP C4500, manufactured by Ricoh Co., Ltd.), a 0.6 mg / cm2 ink was applied to plain paper. 2 The temperature at which cold offset occurred was measured and rated on a four-point scale. (Evaluation Criteria) ◎(Excellent): Less than 120℃ ○(Good): 120℃ or higher and less than 125℃ △(OK): 125℃ or higher and lower than 130℃ ×(Not possible): 130℃ or higher
[0124] Table 1 shows the evaluation results of the toners of the examples and comparative examples.
[0125] [Table 1]
[0126] From Table 1, it was confirmed that the generation of coarse particles was suppressed in the resin particles obtained in each Example. In contrast, it was confirmed that the amount of coarse particles was large in the resin particles obtained in each Comparative Example under all conditions, which was problematic in practical use.
[0127] Therefore, the resin particles obtained in each example can be said to be high-quality toner particles because, in the phase inversion emulsification process, the mixture of the oil phase and the aqueous medium is stirred and the mixture is circulated, and the resin particles are refined during circulation, thereby suppressing the generation of coarse particles.
[0128] Although the embodiment has been described above, the above embodiment is presented as an example, and the present invention is not limited to the above embodiment. The above embodiment can be implemented in various other forms, and various combinations, omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims.
[0129] The aspects of the embodiment of the present invention are as follows, for example. <1> A method for producing a resin particle dispersion comprising the steps of: preparing an oil phase by dissolving or dispersing a binder resin in an organic solvent; and adding an aqueous medium to the oil phase to perform phase inversion emulsification to obtain a dispersion of resin particles, wherein, in the phase inversion emulsification, a mixture of the oil phase and the aqueous medium is stirred while the mixture is circulated, and the resin particles are micronized during the circulation. <2> The method is characterized in that the mixed liquid is stirred in a tank and circulated outside the tank, and the resin particles are micronized during circulation. <1> 2. A method for producing a resin particle dispersion according to claim 1 . <3> The binder resin is a polyester resin. <1> or <2> 2. A method for producing a resin particle dispersion according to claim 1 . <4> The oil phase is neutralized with an alkaline aqueous solution. <1> ~ <3> 10. The method for producing a resin particle dispersion according to claim 9, <5> <1> ~ <4> 2. A method for producing toner particles, using a resin particle dispersion obtained by any one of the methods described above. <6> A crystalline polyester resin and a release agent are added. <5> 2. A method for producing toner particles according to claim 1 . [Explanation of symbols]
[0130] 1 Mixing tank 2 Mixing blade 3 Stirring motor 4 Agitation shaft 5 Circulation Line 6 Liquid delivery pump 7. Crusher (Disperser) 8 Mixed liquid [Prior art documents] [Patent documents]
[0131] [Patent Document 1] JP 2022-151291 A [Patent Document 2] Japanese Patent Application Publication No. 09-114135
Claims
1. A method for producing a resin particle dispersion comprising the steps of: preparing an oil phase by dissolving or dispersing a binder resin in an organic solvent; and adding an aqueous medium to the oil phase to perform phase inversion emulsification to obtain a dispersion of resin particles, wherein, in the phase inversion emulsification, a mixture of the oil phase and the aqueous medium is stirred while the mixture is circulated, and the resin particles are micronized during the circulation.
2. 2. The method for producing a resin particle dispersion liquid according to claim 1, wherein the mixed liquid is stirred in a tank and circulated outside the tank, and the resin particles are micronized during circulation.
3. The method for producing a resin particle dispersion liquid according to claim 1 , wherein the binder resin is a polyester resin.
4. The method for producing a resin particle dispersion liquid according to claim 1 , wherein the oil phase is neutralized with an alkaline aqueous solution.
5. A method for producing toner particles, comprising using a resin particle dispersion obtained by the method according to any one of claims 1 to 4.
6. 6. The method for producing toner particles according to claim 5, further comprising the step of adding a crystalline polyester resin and a releasing agent.
Citation Information
Patent Citations
Manufacture of electrophotographic toner
JP1997114135A
Method for producing resin particle dispersion, method for producing toner for developing electrostatic image and toner for developing electrostatic image
JP2022151291A