Permanent magnet, device, method for manufacturing permanent magnet, and method for manufacturing permanent magnet powder

The development of a permanent magnet with a specific composition and manufacturing process enhances coercive force and thermal stability, addressing the need for improved ThMn12 SmFe magnets, suitable for diverse applications.

JP2024162993APending Publication Date: 2024-11-21TOKIN CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023219272
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2023-12-26
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

There is a demand for permanent magnets with higher coercive force and improved thermal stability, particularly those based on ThMn12 SmFe with tetragonal structure.

Method used

A permanent magnet composition represented by (R1-xZrx)(T1-y-zCuyMz)Bc, where R is a rare earth element, T is Fe, Co, or Ni, M is C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta, or W, and the atomic ratios are adjusted to achieve high coercive force and stability, combined with a manufacturing process involving rapid cooling, crushing, molding, sintering, and aging to stabilize the crystal structure.

Benefits of technology

The resulting magnet exhibits high coercive force and thermal stability, with coercive forces exceeding 3.0 kOe and Curie temperatures over 400°C, suitable for various devices including watches, electric motors, and automotive components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162993000001_ABST
    Figure 2024162993000001_ABST
Patent Text Reader

Abstract

To provide a permanent magnet with high coercivity, a device, a method for manufacturing the permanent magnet, and a method for manufacturing permanent magnet powder.SOLUTION: A permanent magnet according to the present disclosure is a permanent magnet having a composition represented by the following formula (1). (R1-xZrx)a(T1-y-zCuyMz)bBc (1). In this formula, R represents at least one element selected from rare earth elements, T represents at least one element selected from the group consisting of Fe, Co, and Ni, M represents at least one element selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta, and W, a, b, and c each represent atomic %, x, y, and z represent the ratios of Zr, Cu, and M, respectively, and satisfy the following: 5≤a≤10, b=100-(a+c), 3≤c≤20, 0.01≤x≤0.5, 0.001≤y≤0.1, 0≤z≤0.1.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to permanent magnets, devices, methods of making permanent magnets, and methods of making permanent magnet powder. [Background technology]

[0002] There is a demand for permanent magnets with high remanence and high heat resistance. One candidate for such a magnet material is ThMn, which has high saturation magnetization and a high Curie temperature. 12 SmFe with tetragonal crystal structure 12 Compounds based on the above-mentioned compounds are also included.

[0003] Patent Document 1 describes a permanent magnet with excellent saturation magnetization and coercive force, and improved temperature characteristics of the coercive force, called ThMn 12 A permanent magnet is disclosed that is made of an alloy containing a hard magnetic phase having a tetragonal crystal structure and a non-magnetic phase.

[0004] Patent Document 2 uses ThMn as a magnet material that increases saturation magnetization. 12 A magnet material having a specific composition and a main phase consisting of a crystalline phase is disclosed. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2001-189206 A [Patent Document 2] JP 2018-125512 A Summary of the Invention [Problem to be solved by the invention]

[0006] ThMn 12 SmFe with tetragonal crystal structure 12 In addition, there is a demand for high coercivity in these compounds.

[0007] The present disclosure is devised to solve the above-mentioned problems, and aims to provide a permanent magnet with high coercivity, a device, a method for manufacturing a permanent magnet, and a method for manufacturing permanent magnet powder. [Means for solving the problem]

[0008] The permanent magnet according to the present disclosure is a permanent magnet having a composition represented by the following formula (1): Formula (1):(R 1-x Zr x ) a (T 1-y-z Cu y M z ) b B c Here, R represents at least one element selected from rare earth elements, T represents at least one element selected from the group consisting of Fe, Co, and Ni, M represents at least one element selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta, and W, a, b, and c each represent atomic %, x, y, and z each represent the ratio of Zr, Cu, and M, and satisfy the following: 5≦a≦10, b=100-(a+c), 3≦c≦20, 0.01≦x≦0.5, 0.001≦y≦0.1, 0≦z≦0.1.

[0009] The device according to the present disclosure includes the permanent magnet.

[0010] A method for producing a permanent magnet according to the present disclosure includes preparing a molten metal having a composition represented by the following formula (1): Formula (1):(R 1-x Zr x ) a (T 1-y-z Cu y M z ) b B c wherein R represents at least one element selected from the group consisting of rare earth elements, T represents at least one element selected from the group consisting of Fe, Co, and Ni, M represents at least one element selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta, and W, a, b, and c each represent atomic %, x, y, and z each represent the ratio of Zr, Cu, and M, and the following conditions are satisfied: 5≦a≦10, b=100-(a+c), 3≦c≦20, 0.01≦x≦0.5, 0.001≦y≦0.1, 0≦z≦0.1; The molten metal is heated to 50 to 10 7 The alloy is then quenched at 300 K / sec to form an alloy, the alloy is pulverized to form a powder, the powder is molded to form a compact, the compact is sintered at a temperature range of 950°C to 1250°C to form a sintered body, the sintered body is aged at a temperature range of 700°C to 900°C, and then quenched.

[0011] A method for producing a permanent magnet powder according to the present disclosure includes preparing a molten metal having a composition represented by the following formula (1): Formula (1):(R 1-x Zr x ) a (T 1-y-z Cu y M z ) b B c wherein R represents at least one element selected from the group consisting of rare earth elements, T represents at least one element selected from the group consisting of Fe, Co, and Ni, M represents at least one element selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta, and W, a, b, and c each represent atomic %, x, y, and z each represent the ratio of Zr, Cu, and M, and the following conditions are satisfied: 5≦a≦10, b=100-(a+c), 3≦c≦20, 0.01≦x≦0.5, 0.001≦y≦0.1, 0≦z≦0.1; The molten metal is heated to 50 to 10 7 The alloy is then quenched at 300 K / sec to form an alloy, and crystallized at a temperature in the range of 700°C to 900°C. The alloy is then pulverized to form a powder. Effect of the Invention

[0012] The present disclosure makes it possible to provide a permanent magnet with high coercivity, a device, a method for manufacturing a permanent magnet, and a method for manufacturing permanent magnet powder. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a diagram showing the correlation between the half-width of the peak in the X-ray diffraction spectrum and the crystallite size of the permanent magnet according to the present embodiment. [Diagram 2] 1 shows X-ray diffraction spectra of permanent magnets of examples and comparative examples. [Diagram 3] FIG. 2 is a graph showing the correlation between the half-width of the peak in the X-ray diffraction spectrum of the permanent magnet of the example and the heat treatment temperature. [Figure 4] FIG. 4 is a diagram showing magnetization curves of permanent magnets of an example and a comparative example. [Diagram 5] 1 shows X-ray diffraction spectra of permanent magnets of examples and comparative examples. [Figure 6] 1 is a scanning transmission electron microscope image of permanent magnets of an example and a comparative example. [Figure 7] FIG. 4 is a diagram showing magnetization curves of permanent magnets of an example and a comparative example. [Figure 8] FIG. 2 is a diagram showing a crystal growth model of the permanent magnet according to the embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The permanent magnet, manufacturing method, and device of the present embodiment will be described below. Note that unless otherwise specified, the symbol "to" indicating a range of values ​​includes the lower limit and the upper limit.

[0015] [Permanent magnet] The permanent magnet according to the present embodiment is a permanent magnet having a composition represented by the following formula (1): Formula (1):(R 1-x Zr x ) a (T 1-y-z Cu y M z ) b Bc Where: R represents at least one rare earth element; T represents at least one selected from the group consisting of Fe, Co, and Ni; M represents at least one selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta, and W; a, b, and c each represent an atomic percentage; x, y, and z each represent the ratio of Zr, Cu, and M, respectively; and 5≦a≦10, b=100-(a+c), 3≦c≦20, 0.01≦x≦0.5, 0.001≦y≦0.1, The condition 0≦z≦0.1 is satisfied.

[0016] In formula (1), R represents a rare earth element. The rare earth element according to the present embodiment is a general term for elements including lanthanoids from La (lanthanum) to Lu (lutetium), Sc (scandium), and Y (yttrium). R contains at least one element selected from the rare earth elements. By containing R in a ratio within the range that satisfies formula (1), a permanent magnet having high magnetic anisotropy and high coercive force can be obtained. From the viewpoint of magnetic anisotropy and coercive force, R is preferably selected from Sm (samarium), Pr (praseodymium), Nd (neodymium), Ce (cerium), and La (lanthanum), and more preferably contains Sm. Furthermore, from the viewpoint of magnetic anisotropy and coercive force, it is preferable that 50 atomic % or more of R is Sm, preferably 80 atomic % or more is Sm, and more preferably R is substantially Sm.

[0017] The permanent magnet according to the present embodiment contains Zr in a range in which the ratio (atomic %) of R to Zr (zirconium) is (1-x):x. By containing Zr within the above range, the content of the M element, which will be described later, can be suppressed while the content of ThMn 12 The crystal structure of the ThMn type can be stabilized, resulting in an improvement in saturation magnetization. 12From the viewpoint of stabilizing the crystal structure of the type, x may be 0.01 to 0.5, and from the viewpoint of magnetic anisotropy and coercive force, it is preferable that x is 0.2 or less.

[0018] The total content ratio (a) of R and Zr in the entire permanent magnet according to the present embodiment is ThMn 12 In order to have the type crystal structure as the main phase, a is 5 to 10. In order to increase magnetization, a is preferably 9 or less.

[0019] In formula (1), T represents at least one element selected from the group consisting of Fe (iron), Co (cobalt), and Ni (nickel). Each element of T contributes to the magnetization of the permanent magnet. In order to increase the magnetization, it is preferable that T contains Fe. In order to increase the Curie temperature and improve the heat resistance, it is preferable that T contains Co. In order to increase the magnetization, it is preferable that 50 atomic % or more of T is Fe, and it is preferable that 60 atomic % or more is Fe. In addition, for example, when Fe and Co are used in combination, the ratio of Fe to Co (atomic %) is preferably 60:40 to 95:5, and more preferably 70:30 to 80:20. In the permanent magnet according to the present embodiment, the content ratio of T is expressed as (1-yz).

[0020] From the viewpoint described later, the content ratio (y) of Cu (copper) may be from 0.001 to 0.1, and more preferably from 0.005 to 0.05.

[0021] In formula (1), M represents at least one element selected from the group consisting of C (carbon), N (nitrogen), Al (aluminum), Si (silicon), P (phosphorus), Ti (titanium), V (vanadium), Cr (chromium), Mn (manganese), Nb (niobium), Mo (molybdenum), Hf (hafnium), Ta (tantalum), and W (tungsten). Each element of M is selected from the group consisting of ThMn 12 Although it is possible to improve the stability of the crystal structure, this is not essential in the permanent magnet according to the present embodiment, and it is sufficient that the M content (z) is 0 to 0.1.

[0022] The total content ratio (b) of T, Cu, and M in the entire permanent magnet according to this embodiment can be expressed as 100-(a+c), where ThMn 12 In order to have the type crystal structure as the main phase, b is 70 to 92. In order to increase magnetization, b is preferably 75 or more, and more preferably 77 or more.

[0023] Furthermore, the permanent magnet according to this embodiment contains 3 to 20 atomic % of B (boron). By containing B and Cu within the above ranges, the crystallite size decreases and the coercive force increases. From the viewpoint of further increasing the coercive force, the B content (c) is preferably 3 or more, and more preferably 5 or more. On the other hand, from the viewpoint of suppressing a decrease in saturation magnetization, the B content (c) is preferably 20 or less, and more preferably 15 or less.

[0024] Furthermore, the permanent magnet according to the present embodiment may contain precipitates of boride containing M in formula (1). For example, when the permanent magnet according to the present embodiment contains Ti as M, the permanent magnet may contain precipitates of titanium boride. Note that the precipitates are not limited to borides, and for example, when the permanent magnet according to the present embodiment contains Ti and C as M, the permanent magnet may contain precipitates of carbides such as titanium carbide.

[0025] The boride or carbide precipitates contained in the permanent magnet according to this embodiment are preferably finer because this allows the crystal grain size of the 1-12 phase to be smaller, and the average Feret diameter of the precipitates is preferably less than 20 nm.

[0026] Here, the Feret diameter is defined as the distance between two parallel lines circumscribing the measurement object, and the maximum value is called the maximum Feret diameter. The Feret diameter and the maximum Feret diameter are obtained by analyzing the observation image obtained from, for example, a scanning electron microscope or a transmission electron microscope using image processing software. Therefore, the average Feret diameter of precipitates is the average value of the maximum Feret diameters of precipitates present within the observation field, and the average Feret diameter of main phase crystal grains is the average value of the maximum Feret diameters of main phase crystal grains present within the observation field.

[0027] The permanent magnet according to the present embodiment may contain inevitable impurities within the scope of the effects of the present disclosure. The inevitable impurities are elements that are inevitably mixed in from the raw materials or manufacturing process and are not included in formula (1) (elements other than R, T, M, Zr, Cu, and B). Specific examples include, but are not limited to, O (oxygen), S (sulfur), Sn (tin), etc. The proportion of inevitable impurities in the permanent magnet according to the present embodiment is preferably 5 atomic % or less, more preferably 1 atomic % or less, and even more preferably 0.1 atomic % or less, relative to the total amount of the permanent magnet according to the present embodiment.

[0028] The content ratio of each element in the permanent magnet according to this embodiment can be measured, for example, by using energy dispersive X-ray spectrometry (EDX).

[0029] The permanent magnet according to the present embodiment satisfies the composition of the above formula (1), and thus has a composition of ThMn 12 The permanent magnet has crystal grains made of a main phase having a crystal structure of the ThMn type, and crystal grain boundaries that are the boundaries between the crystal grains. Furthermore, by including B and Cu, fine segregation of Cu occurs within the crystal grains, and the crystallite size of the 1-12 phase becomes small. As a result, the permanent magnet according to the present embodiment has a ThMn 12 The crystalline structure has excellent stability, saturation magnetization, and heat resistance, and has a particularly high coercive force.

[0030] In addition, when the permanent magnet according to the present embodiment contains boride or carbide precipitates, ThMn 12 In the main phase crystal grains having the crystal structure of the type, it is preferable that the average Feret diameter (average crystal grain size) is less than 100 nm, and the variation coefficient of the Feret diameter is less than 0.4. Here, the variation coefficient is an index representing the variation in the size of the crystal grains, and is obtained by dividing the standard deviation of the Feret diameter by the average Feret diameter.

[0031] As an example, the permanent magnet according to this embodiment can have a coercive force (Hcj) of more than 3.0 kOe. As an example, the permanent magnet according to this embodiment can have a Curie temperature of more than 400° C. The grain boundary structure can be observed using a scanning transmission electron microscope (STEM). The Curie temperature can be measured using a vibrating sample magnetometer (VSM). The coercive force can be determined from a JH curve obtained using a DC magnetization characteristic analyzer.

[0032] [device] The present disclosure can further provide a device having the permanent magnet according to the present embodiment. Specific examples of such devices include watches, electric motors, various instruments, communication devices, computer terminals, speakers, video disks, sensors, etc. In addition, the permanent magnet of the present disclosure is unlikely to deteriorate in magnetic force even in high environmental temperatures, and therefore can be suitably used in angle sensors used in the engine compartment of automobiles, ignition coils, drive motors for HEVs (hybrid electric vehicles), etc.

[0033] [Manufacturing method of permanent magnets] The method for producing a permanent magnet according to the present embodiment includes the steps of: (I) preparing a molten metal having a composition represented by the above formula (1); and (II) mixing the molten metal with 50 to 10 7 The process comprises the steps of (II) rapidly cooling at 300 K / sec to form an alloy, (III) pulverizing the alloy to form a powder, (IV) molding the powder to form a green body, (V) sintering the green body at a temperature range of 950°C to 1250°C to form a sintered body, and (VI) aging the sintered body at a temperature range of 700°C to 900°C, followed by rapid cooling.

[0034] By the manufacturing method according to the present embodiment, ThMn 12It is possible to suitably manufacture the permanent magnet according to the present embodiment having fine crystallites made of a main phase having a crystal structure of this type.

[0035] First, a molten metal having a composition represented by formula (1) is prepared (step (I)). The molten metal may be prepared by purchasing a commercially available alloy having the desired composition, or by mixing the elements to obtain the desired composition. If there is a possibility that the elements may evaporate in a later process, the composition after the permanent magnet is manufactured is adjusted to satisfy formula (1). The prepared alloy is melted to obtain a molten metal. The melting method may be appropriately selected from arc melting, high-frequency melting, etc.

[0036] Next, pour the molten metal into a 50-10 7 The molten metal is then rapidly cooled at a cooling rate of 50 K / sec or more (step (II)). By rapidly cooling the molten metal at a cooling rate of 50 K / sec or more, an amorphous phase can be formed, and fine crystallites can be obtained by heat treatment, resulting in a permanent magnet with high coercive force.

[0037] The alloy after quenching may be further heat-treated to homogenize the structure. 3 ~10 6 K / sec is preferable. Furthermore, in order to form an amorphous phase by quenching, it is preferable that the alloy is made into a flake shape. In order to facilitate quenching, the thickness of the flakes is preferably 1 to 100 μm, and more preferably 20 to 90 μm. Since the alloy contains boron, the viscosity is reduced, and flakes of the above thickness are easily obtained when the molten metal is quenched by the melt spun method or the like.

[0038] The crystallite size of the crystal structure can be evaluated by X-ray diffraction spectrum using, for example, the θ-2θ method. Specifically, a permanent magnet is irradiated with characteristic X-rays of CuKα in the range of θ=20° to 90°, and the X-ray diffraction spectrum of the permanent magnet is measured. The crystallite size is then calculated from the full width at half maximum (FWHM) of multiple 1-12 phase X-ray spectra including the 211 plane, and the average value is taken as the crystallite size. Figure 1 shows the full width at half maximum (FWHM) of the peak corresponding to the 211 plane of the 1-12 phase. (211)) versus crystallite size, with a larger half-width indicating a smaller crystallite size.

[0039] Next, the alloy is pulverized (step (III)). As an example of a method for pulverizing the alloy, the alloy is first coarsely pulverized in an inert atmosphere using a pulverizer such as a disk mill. If the pulverization is poor, the alloy may be subjected to a hydrogen absorption treatment in advance. The hydrogen absorption treatment embrittles the alloy, making it easier to pulverize it coarsely.

[0040] Next, the coarsely pulverized product is further pulverized into fine powder. The pulverization may be dry pulverization or wet pulverization. For example, the dry pulverization may be a jet mill method. For example, the wet pulverization may be a wet ball mill method. A lubricant may be added to impart lubricity to the powder during pulverization. The mixture of the organic solvent and the fine powder after pulverization is dried in an inert gas. The average particle size of the powder after pulverization is preferably 1 to 10 μm, which enables the sintering time in the sintering step described below to be shortened and also allows the production of a uniform permanent magnet.

[0041] Next, the obtained powder is pressure-molded to obtain a green body of a desired shape (step (IV)). In the present disclosure, pressure molding in a constant magnetic field is preferable in order to align the crystal orientation of the powder and improve the magnetic properties. The relationship between the direction of the magnetic field and the pressing direction is not particularly limited, and may be appropriately selected depending on the shape of the product, etc. For example, when manufacturing a ring magnet or a thin plate magnet, a parallel magnetic field press can be used in which a magnetic field is applied parallel to the pressing direction. On the other hand, in terms of excellent magnetic properties, a perpendicular magnetic field press in which a magnetic field is applied perpendicular to the pressing direction is preferable.

[0042] The strength of the magnetic field is not particularly limited, and may be, for example, 15 kOe or less or 15 kOe or more depending on the application of the product. In particular, from the viewpoint of excellent magnetic properties, it is preferable to perform pressure molding in a magnetic field of 15 kOe or more. The pressure during pressure molding may be appropriately adjusted depending on the size, shape, etc. of the product. For example, it may be 0.5 to 2.0 ton / cm. 2That is, in the method for producing a permanent magnet according to the present embodiment, from the viewpoint of magnetic properties, the powder is subjected to a magnetic field of 15 kOe or more and a pressure of 0.5 to 2.0 ton / cm is applied perpendicular to the magnetic field. 2 It is particularly preferable to carry out the pressing at the following pressures:

[0043] Next, the molded body is sintered to obtain a sintered body (step (V)). The sintering temperature is preferably 950 to 1250°C, more preferably 950 to 1100°C. If the temperature is too low, the sintered body will not be densified, and the residual magnetic flux density (Br) will decrease. If the temperature is too high, the crystal grains will become coarse, leading to a decrease in coercive force. Furthermore, there is a risk of the 1-12 phase decomposing. Furthermore, the sintering time is preferably 20 to 240 minutes, more preferably 60 to 120 minutes. From the viewpoint of suppressing oxidation, the sintering step is preferably performed in a vacuum of 1000 Pa or less or in an inert gas atmosphere, and from the viewpoint of increasing the density of the sintered body, it is preferable to sinter in a vacuum of 1000 Pa or less, preferably 100 Pa or less.

[0044] After step (V), the obtained sintered body is preferably subjected to aging treatment. 12 The aging treatment temperature is preferably 700 to 900°C, more preferably 800 to 900°C. If the temperature is too low, the aging treatment does not proceed and the crystal structure is difficult to homogenize, leading to a decrease in magnetic properties. If the temperature is too high, the crystal grains become coarse, leading to a decrease in coercive force. In addition, the 1-12 phase may decompose. The heat treatment time may be, for example, 0.5 to 20 hours, preferably 1 to 10 hours.

[0045] Next, the heat-treated sintered body is quenched (step (VI)). The homogenized crystal structure is maintained by quenching. The quenching rate in step (VI) may be 60 to 250° C. / min, and preferably 100 to 250° C. / min.

[0046] In this way, ThMn 12 It is possible to manufacture the permanent magnet according to the present embodiment having fine crystallites made of a main phase having a crystal structure of this type.

[0047] [Manufacturing method of permanent magnet powder] The method for producing the permanent magnet powder according to the present embodiment includes the steps of: preparing a molten metal having a composition represented by the above formula (1); and heating the molten metal for 50 to 10 minutes. 7 The method includes a step (II) of rapidly cooling the alloy at 300 K / sec to form an alloy, a step (III) of crystallizing the alloy at a temperature in the range of 700°C to 900°C, and a step (IV) of pulverizing the alloy to form a powder.

[0048] By the manufacturing method according to the present embodiment, ThMn 12 It is possible to suitably manufacture the permanent magnet powder according to the present embodiment having fine crystallites made of a main phase having a crystal structure of this type.

[0049] First, a molten metal having a composition represented by formula (1) is prepared (step (I)). 7 The mixture is then quenched at 300 K / sec (step (II)). These steps can be performed using the same techniques as steps (I) and (II) in the above-mentioned method for producing a permanent magnet, and the details will be omitted to avoid repetitive explanation.

[0050] Next, the alloy is crystallized at a temperature in the range of 700 to 900°C (step (III)). To increase the coercive force of the permanent magnet, a higher heat treatment temperature is preferable, and it is particularly preferable to perform the heat treatment at 800 to 900°C. If the temperature is too low, the main phase crystals will not precipitate. On the other hand, if the temperature is too high, the crystal grains will become coarse, leading to a decrease in coercive force. In addition, there is a risk of the 1-12 phase decomposing.

[0051] After step (III), the obtained alloy is pulverized to obtain a powder (step (IV)). This step can be performed by using the same method as step (III) in the above-mentioned method for producing a permanent magnet, and the details are omitted.

[0052] In this way, ThMn 12 It is possible to produce the permanent magnet powder according to the present embodiment having fine crystallites made of a main phase having a crystal structure of this type. EXAMPLES

[0053] The present disclosure will be specifically described below with reference to examples and comparative examples, but the present disclosure is not limited to these descriptions.

[0054] Example 1 The raw material elements were weighed in predetermined amounts so as to obtain the composition of Example 1 shown in Table 1, and a master alloy was obtained by high-frequency melting. The master alloy was again high-frequency melted and the liquid was quenched by the melt-spanning method to obtain alloy flakes. The alloy flakes were coarsely pulverized in a vibration mill and finely pulverized in a wet ball mill to obtain raw material powder. The raw material powder was molded into a green compact by pressing in a magnetic field. The green compact was sintered at 950°C and subsequently aged at 900°C. After aging, the permanent magnet of the sintered body of Example 1 was obtained by quenching.

[0055] (Examples 2 to 8) The raw material elements were weighed in predetermined amounts so as to obtain the compositions of Examples 2 to 8 shown in Table 1, and alloy flakes were produced in the same manner as in Example 1. The alloy flakes were heated at 900°C to cause crystal precipitation. The alloy flakes were then coarsely pulverized in a vibration mill to obtain magnet powder.

[0056] (Comparative Examples 1 to 3) Magnet powders were obtained in the same manner as in Examples 2 to 8, except that the raw material elements were weighed out in predetermined amounts so as to obtain the compositions of Comparative Examples 1 to 3 shown in Table 1.

[0057] [evaluation] The X-ray diffraction spectra of the permanent magnets of the above-mentioned examples and comparative examples were measured, and the half-width (FWHM) of the peak corresponding to the 211 plane of the crystal structure of the 1-12 phase was obtained from the obtained X-ray diffraction spectra, and the crystallite size was calculated. In addition, the JH curve of each permanent magnet was measured using a DC magnetization characteristic analyzer to obtain the coercive force (Hcj). The results are shown in Table 1.

[0058] [Table 1]

[0059] As shown in Table 1, the permanent magnets of Examples 1 to 8, which satisfy the composition of formula (1) above, i.e., have a Cu ratio (y) of 0.001 or more and contain 3.0 atomic % or more of B (boron), have crystallite sizes of less than 45 nm and are shown to have high coercive force.

[0060] 2(a) to (d) show X-ray diffraction spectra of Example 2 and Comparative Examples 1 to 3, which were heated at 700°C, 800°C, and 900°C after quenching (As-Q: As-Quenched in the figure), respectively. The heating times are as shown in FIG. 2(a) to (d). The peak corresponding to the 211 plane of the 1-12 phase is indicated by a ▼ mark in the figure. The 1-12 phase diffraction peak of Example 2 is broadened compared to Comparative Examples 1 to 3. Since Example 2 has a higher B (boron) content compared to Comparative Examples 1 to 3, it can be seen that an amorphous phase is formed during quenching and the crystal grains are refined by the heat treatment.

[0061] Figure 3 shows the correlation between the half-width of the peak in the X-ray diffraction spectrum and the heat treatment temperature when the composition of B (boron) is changed in the sample of Example 2. As shown in Figure 3, when the content of B (boron) increases, the half-width tends to increase even when a high-temperature heat treatment is performed, which indicates that crystal growth is suppressed.

[0062] 4(a) and (b) show magnetization curves of samples of Example 2 and Comparative Example 1 that were quenched (As-Q) and then heated at 700°C, 800°C, and 900°C for 60 minutes. As shown in FIG. 4(a), it can be seen that the coercive force increased due to the heat treatment in Example 2. On the other hand, as shown in FIG. 4(b), in Comparative Example 1, the increase in coercive force due to the heat treatment was small.

[0063] FIG. 5 is a diagram showing the correlation between the amount of added B (boron) and the crystal grain size. The X-ray diffraction spectra of permanent magnets when the concentration of B (boron) contained in the permanent magnet is set to 0.8 atomic %, 2.0 atomic %, 4.0 atomic %, 5.0 atomic %, 6.0 atomic %, and 8.0 atomic %. The permanent magnets with a B (boron) concentration of 0.8 atomic % and the permanent magnets with a B (boron) concentration of 5.0 atomic % correspond to Comparative Example 2 and Example 2, respectively. FIG. 5(a) is an X-ray diffraction spectrum of a permanent magnet after quenching (As-Q), and FIG. 5(b) is an X-ray diffraction spectrum of a permanent magnet heated at 900°C for 60 minutes. From the obtained X-ray diffraction spectrum, it can be seen that the peak of the 1-12 phase broadens with an increase in the amount of added B (boron), and the addition of B (boron) suppresses crystal growth even when a high-temperature heat treatment is performed.

[0064] Figure 6 shows scanning transmission electron microscope (STEM) images of the permanent magnet after heating at 900°C for 60 minutes. Figure 6(a) shows a STEM image of the permanent magnet of Example 2, and Figure 6(b) shows a STEM image of Comparative Example 2. The areas surrounded by circles indicate the areas where Ti-B phase (boride) precipitates were observed.

[0065] Figure 7 shows the magnetization curves of the permanent magnets of Example 2 and Comparative Example 2, which were heated at 900°C for 60 minutes. It can be seen that the coercive force increases with an increase in the amount of B (boron) added. Furthermore, the magnetization curve of the permanent magnet of Example 2 showed good squareness.

[0066] From the above STEM images and magnetization curves, the average Feret diameter of the Ti-B phase, the average Feret diameter of the 1-12 phase, and the variation coefficient of the Feret diameter of the 1-12 phase were determined. The results are shown in Table 2.

[0067] [Table 2]

[0068] As shown in Table 2, the permanent magnet of Comparative Example 2, in which B (boron) was less than 3.0 atomic %, had a large average Feret diameter of the boride precipitates and an average Feret diameter of the 1-12 phase, and further had a large coefficient of variation of the Feret diameter of the 1-12 phase, i.e., the variation in size of the Feret diameter (crystal grain size) of the 1-12 phase was large.

[0069] From the results shown in the examples, the mechanism of grain refinement expected when the permanent magnet according to the present disclosure contains boride or carbide precipitates will be explained with reference to Figure 8. Figure 8(a) is a crystal growth model of Example 2, i.e., a permanent magnet whose form after quenching is amorphous, and Figure 8(b) is a crystal growth model of Comparative Example 2, i.e., a permanent magnet whose form after quenching is crystalline.

[0070] When the morphology after quenching is amorphous, fine 1-12 phase crystals and borides or carbides begin to precipitate due to heat treatment. These borides or carbides inhibit the growth of 1-12 phase crystals, so that fine and uniform crystal grains are formed after heat treatment.

[0071] On the other hand, when the morphology after quenching is crystalline, crystals and boride or carbide precipitates are generated at the time of quenching. Also, the amount of precipitates is small, so they cannot inhibit crystal growth, and the 1-12 phase crystal grains increase during heat treatment. Therefore, after heat treatment, crystal grains with large grain sizes and large variations in grain size are formed.

[0072] In this way, the permanent magnet according to the present disclosure is a ThMn 12 By having fine crystallites consisting of a main phase having a crystal structure of this type, it is possible to have a high coercive force.

Claims

1. A permanent magnet having a composition represented by the following formula (1): Formula (1): (R 1-x Zr x ) a (T 1-y-z Cu y M z ) b B c Where: R represents at least one rare earth element; T represents at least one selected from the group consisting of Fe, Co, and Ni; M represents at least one selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta, and W; a, b, and c each represent an atomic percentage; x, y, and z each represent the ratio of Zr, Cu, and M, respectively; and 5≦a≦10, b=100-(a+c), 3≦c≦20, 0.01≦x≦0.5, 0.001≦y≦0.1, 0≦z≦0.1 is satisfied; Permanent magnet.

2. ThMn 12 A main phase having a crystal structure of the type In the X-ray diffraction spectrum, the half-width of the X-ray diffraction peak corresponding to the 211 plane of the crystal structure is 0.20° or more.

2. The permanent magnet according to claim 1.

3. The crystallite size of the crystal structure calculated from the X-ray diffraction spectrum is less than 45 nm.

3. The permanent magnet according to claim 2.

4. Having boride or carbide precipitates with an average Feret diameter of less than 20 nm; A permanent magnet according to any one of claims 1 to 3.

5. ThMn 12 In the main phase crystal grains having a crystal structure of the type, the average Feret diameter is less than 100 nm and the variation coefficient of the Feret diameter is less than 0.4; 5. The permanent magnet according to claim 4.

6. The permanent magnet according to any one of claims 1 to 3, wherein 50 atomic % or more of the R is Sm.

7. The permanent magnet according to any one of claims 1 to 3, wherein 50 atomic % or more of T is Fe.

8. The permanent magnet according to any one of claims 1 to 3, having a coercive force of more than 3 kOe.

9. The permanent magnet according to any one of claims 1 to 3, having a Curie temperature of more than 400°C.

10. A device comprising a permanent magnet according to any one of claims 1 to 3.

11. A molten metal having a composition represented by the following formula (1) is prepared, Formula (1): (R 1-x Zr x ) a (T 1-y-z Cu y M z ) b B c Where: R represents at least one selected from rare earth elements; T represents at least one selected from the group consisting of Fe, Co, and Ni; M represents at least one selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta, and W; a, b, and c each represent an atomic percentage; x, y, and z each represent the ratio of Zr, Cu, and M, respectively; and 5≦a≦10, b=100-(a+c), 3≦c≦20, 0.01≦x≦0.5, 0.001≦y≦0.1, 0≦z≦0.1 is satisfied, The molten metal is heated to 50 to 10 7 The alloy is then quenched at 100 K / sec to form an alloy. The alloy is pulverized to form a powder; The powder is molded into a molded body, The compact is sintered at a temperature in the range of 950° C. to 1250° C. to obtain a sintered compact. The sintered body is subjected to aging treatment at a temperature range of 700°C to 900°C, and then quenched. How permanent magnets are manufactured.

12. A molten metal having a composition represented by the following formula (1) is prepared, Formula (1): (R 1-x Zr x ) a (T 1-y-z Cu y M z ) b B c Where: R represents at least one selected from rare earth elements; T represents at least one selected from the group consisting of Fe, Co, and Ni; M represents at least one selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta, and W; a, b, and c each represent an atomic percentage; x, y, and z each represent the ratio of Zr, Cu, and M, respectively; and 5≦a≦10, b=100-(a+c), 3≦c≦20, 0.01≦x≦0.5, 0.001≦y≦0.1, 0≦z≦0.1 is satisfied, The molten metal is heated to 50 to 10 7 The alloy is then quenched at 100 K / sec to form an alloy. The alloy is crystallized at a temperature in the range of 700° C. to 900° C., The alloy is pulverized to obtain a powder. How permanent magnet powder is manufactured.

Citation Information

Patent Citations

  • Permanent magnet

    JP2001189206A

  • Magnet material, permanent magnet, rotary electric machine, and vehicle

    JP2018125512A