Foamable adhesive sheet and manufacturing method of article
The foamable adhesive sheet with controlled hardness and cohesive failure mode addresses peeling and brittleness issues, ensuring strong adhesion and durability in adhesive layers.
Patent Information
- Application Number
- JP2023079126
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
AI Technical Summary
Foamable adhesive sheets with adhesive layers on both sides, where one is foamed and the other is not, face issues with differential hardness leading to peeling and brittleness, which can cause foreign matter and structural failure.
A foamable adhesive sheet design with a first adhesive layer containing a foaming agent and a second adhesive layer without, ensuring cohesive failure mode and controlled hardness through tensile shear adhesive strength testing, with a slope of 0.20 MPa or less from 3% to 5% strain.
Enhances adhesion and durability of the second adhesive layer to the base material, preventing peeling and excessive load, improving product quality and reliability.
Smart Images

Figure 2024163487000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a foamable adhesive sheet and a method for producing an article using the same. [Background technology]
[0002] Adhesives for bonding two members are used in a variety of fields, and many bonding methods are known.
[0003] In recent years, the use of adhesive sheets containing a foaming agent (foamable adhesive sheets) instead of liquid adhesives has been proposed (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6274540 [Patent Document 2] Patent Publication No. 2021-197888 Summary of the Invention [Problem to be solved by the invention]
[0005] As a foamable adhesive sheet, for example, a foamable adhesive sheet having adhesive layers on both sides of a substrate is known. In such a foamable adhesive sheet, it has been proposed that one adhesive layer is a foamed layer containing a foaming agent and the other adhesive layer is a non-foamed layer not containing a foaming agent (for example, see Patent Documents 1 and 2).
[0006] As a method for bonding two members using a foamable adhesive sheet, for example, a method of bonding two members by placing a foamable adhesive sheet between the two members and then foaming and curing the foamable adhesive sheet can be mentioned. However, in the foamable adhesive sheet, when adhesive layers are placed on both sides of a substrate, one adhesive layer is a foamed layer and the other adhesive layer is a non-foamed layer, the hardness of the adhesive layer after curing differs depending on whether or not a foaming agent is contained. When the adhesive layer that is a non-foamed layer is cured, it tends to become hard and brittle. Therefore, after the foamable adhesive sheet is foamed and cured, the second adhesive layer after curing may peel off from the substrate. If the second adhesive layer after curing peels off from the substrate and becomes a foreign matter, and the foreign matter adheres to the member, it may lead to product failure, or if the foamable adhesive sheet has insulating properties, it may cause insulation failure. In addition, when a shear stress is applied after the foamable adhesive sheet is foamed and cured, an excessive load is applied to layers other than the second adhesive layer, which may lead to destruction.
[0007] The present disclosure has been made in consideration of the above-mentioned circumstances, and has as its main object to provide a foamable adhesive sheet in which the second adhesive layer has good adhesion to a substrate and durability after curing. [Means for solving the problem]
[0008] One embodiment of the present disclosure provides a foamable adhesive sheet having, in this order, a first adhesive layer, a substrate, and a second adhesive layer, wherein the first adhesive layer contains a first curable adhesive and a foaming agent, and the second adhesive layer contains a second curable adhesive and no foaming agent, and when a tensile shear adhesive strength test method is performed on the foamable adhesive sheet after foaming and curing, the failure mode is cohesive failure of the first adhesive layer after foaming and curing, and when a tensile shear adhesive strength test method is performed on the second adhesive layer after curing, the slope of the approximation line in the section from 3% strain to 5% strain in a stress-strain curve obtained is 0.20 MPa or less.
[0009] Another embodiment of the present disclosure provides a method for manufacturing an article, comprising: a step of placing the above-mentioned foamable adhesive sheet between a first member and a second member; and a step of foaming and curing the foamable adhesive sheet to bond the first member and the second member. Effect of the Invention
[0010] The present disclosure has an effect of providing a foamable adhesive sheet in which the second adhesive layer after curing has good adhesion to a substrate and good durability. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic cross-sectional view showing an example of a foamable adhesive sheet according to the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view illustrating a method for testing the tensile shear adhesive strength of the second adhesive layer after curing. [Diagram 3] FIG. 2 is a schematic cross-sectional view illustrating a method for testing the tensile shear adhesive strength of the first adhesive layer after foaming and curing. [Figure 4] FIG. 2 is a schematic cross-sectional view illustrating a method for testing the tensile shear adhesive strength of the first adhesive layer after foaming and curing. [Diagram 5] 1 is a graph illustrating an example of a stress-strain curve. [Figure 6] FIG. 2 is a schematic cross-sectional view illustrating a method for testing the tensile shear adhesive strength of a foamable adhesive sheet after foaming and curing. [Figure 7] FIG. 2 is a schematic cross-sectional view showing another example of a foamable adhesive sheet according to the present disclosure. [Figure 8] FIG. 2 is a schematic cross-sectional view showing an example of a method for producing an article according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following describes the embodiments of the present disclosure with reference to the drawings. However, the present disclosure can be implemented in many different forms, and is not to be construed as being limited to the description of the embodiments exemplified below. In addition, the drawings may be schematic in terms of the width, thickness, shape, etc. of each part compared to the actual form in order to make the explanation clearer, but these are merely examples and do not limit the interpretation of the present disclosure. In addition, in this specification and each figure, elements similar to those described above with respect to the previous figures may be given the same reference numerals, and detailed explanations may be omitted as appropriate.
[0013] In this specification, when describing a mode in which another component is disposed on a certain component, the term "above" or "below" includes both a case in which another component is disposed directly above or below a certain component so as to be in contact with the component, and a case in which another component is disposed above or below a certain component with another component interposed therebetween, unless otherwise specified. In addition, in this specification, when describing a mode in which another component is disposed on the surface of a certain component, the term "on the surface side" or "on the surface" includes both a case in which another component is disposed directly above or below a certain component so as to be in contact with the component, and a case in which another component is disposed above or below a certain component with another component interposed therebetween, unless otherwise specified.
[0014] In this specification, the term "sheet" also includes members called "films." In addition, the term "films" also includes members called "sheets." In addition, the numerical ranges in this specification are average value ranges.
[0015] The foamable adhesive sheet and article manufacturing method according to the present disclosure will be described in detail below.
[0016] A. Foam adhesive sheet The foamable adhesive sheet of the present disclosure has a first adhesive layer, a substrate, and a second adhesive layer, in that order; the first adhesive layer contains a first curable adhesive and a foaming agent; the second adhesive layer contains a second curable adhesive and no foaming agent; when the foamable adhesive sheet after foaming and curing is subjected to a tensile shear adhesive strength test method, the failure mode is cohesive failure of the first adhesive layer after foaming and curing; and in the stress-strain curve obtained when the tensile shear adhesive strength test method is performed on the second adhesive layer after curing, the slope of the approximation line in the section from 3% strain to 5% strain is 0.20 MPa or less.
[0017] FIG. 1 is a schematic cross-sectional view illustrating a foamable adhesive sheet according to the present disclosure. As shown in FIG. 1, the foamable adhesive sheet 10 has a first adhesive layer 1, a substrate 2, and a second adhesive layer 3 in this order. The first adhesive layer 1 contains a first curable adhesive and a foaming agent. The second adhesive layer 3 contains a second curable adhesive and does not contain a foaming agent. In addition, when the foamable adhesive sheet after foaming and curing is subjected to a tensile shear adhesive strength test method, the failure mode is cohesive failure of the first adhesive layer after foaming and curing. Furthermore, in the stress-strain curve obtained when the tensile shear adhesive strength test method is performed on the second adhesive layer after curing, the slope of the approximation line in the section from strain 3% to strain 5% is within a predetermined range.
[0018] In the present disclosure, since the first adhesive layer contains a foaming agent, when a foamable adhesive sheet is used to bond two components, the foamable adhesive sheet is foamed and cured, and the gap between the two components is filled with the foamable adhesive sheet after foaming and curing, thereby bonding the two components. Therefore, the thickness of the foamable adhesive sheet before foaming and curing can be made thinner than the gap between the two components, so that the insertability of the foamable adhesive sheet is improved. In addition, in the present disclosure, since the second adhesive layer does not contain a foaming agent, the surface of the foamable adhesive sheet on the second adhesive layer side does not have unevenness due to the foaming agent. If the surface of the foamable adhesive sheet has unevenness due to the foaming agent, it is considered that the convex part of the surface of the foamable adhesive sheet will get caught by the component. However, since the surface of the foamable adhesive sheet on the second adhesive layer side does not have unevenness due to the foaming agent, it is possible to suppress the surface of the foamable adhesive sheet on the second adhesive layer side from getting caught by the component. Therefore, the insertability of the foamable adhesive sheet can be improved. For example, the foamable adhesive sheet can be smoothly inserted into the gap between two components. Alternatively, one of the components can be smoothly inserted into the gap after the foamable adhesive sheet is placed in the hole or groove of the other component. Alternatively, one of the components and the foamable adhesive sheet can be smoothly inserted into the hole or groove of the other component. Furthermore, the surface of the foamable adhesive sheet facing the second adhesive layer can be caught by the component, thereby preventing the foaming agent from falling off and the second adhesive layer from being scraped off. Thus, the wear resistance of the second adhesive layer can be improved.
[0019] In addition, since the first adhesive layer contains a foaming agent, but only one of the two adhesive layers contains a foaming agent, the surface of the foamable adhesive sheet can be prevented from getting caught on a member, compared to when both adhesive layers contain a foaming agent. Furthermore, when inserting a second member into a gap after placing the foamable adhesive sheet in a hole or groove of the first member, by arranging the foamable adhesive sheet so that the surface on the first adhesive layer side of the foamable adhesive sheet faces the first member and the surface on the second adhesive layer side of the foamable adhesive sheet faces the second member, it is possible to prevent the surface on the second adhesive layer side of the foamable adhesive sheet from getting caught on the second member when inserting the second member into the gap after placing the foamable adhesive sheet in the hole or groove of the first member. Furthermore, when inserting the second member and the foamable adhesive sheet into a hole or groove in the first member, by arranging the surface of the foamable adhesive sheet facing the first adhesive layer toward the second member and the surface of the foamable adhesive sheet facing the second adhesive layer toward the first member, it is possible to prevent the surface of the foamable adhesive sheet facing the second adhesive layer from getting caught on the first member when the second member and the foamable adhesive sheet are inserted into the hole or groove in the first member.
[0020] In addition, in the present disclosure, since the second adhesive layer does not contain a foaming agent, the second adhesive layer after curing does not have bubbles due to the foaming agent. In other words, after foaming and curing of the foamable adhesive sheet, the surface of the second adhesive layer side after curing does not have unevenness due to bubbles. Therefore, when two members are bonded using a foamable adhesive sheet, the contact area between the second adhesive layer after curing and the members is large. Therefore, the thermal conductivity between the two members can be improved. For example, when a stator core and a coil in a stator of a rotor are bonded using a foamable adhesive sheet, the thermal conductivity between the stator core and the coil can be increased, and heat dissipation can be improved.
[0021] In the present disclosure, since the first adhesive layer contains a foaming agent and the second adhesive layer does not contain a foaming agent, the second adhesive layer after curing tends to be harder and more brittle than the first adhesive layer after foaming and curing. Therefore, after foaming and curing of the foamable adhesive sheet, the second adhesive layer after curing is likely to peel off from the substrate, which may cause foreign matter. In addition, after foaming and curing of the foamable adhesive sheet, if shear stress is applied, excessive load is applied to layers other than the second adhesive layer, which may lead to destruction. Here, for the second adhesive layer after curing, if the slope of the approximate straight line is large, the second adhesive layer after curing tends to be hard, and if the slope of the approximate straight line is small, the second adhesive layer after curing tends to be soft. For the second adhesive layer after curing, the slope of the approximate straight line is a predetermined value or less, so that the second adhesive layer after curing has an appropriate hardness. Therefore, the difference between the hardness of the second adhesive layer after curing and the hardness of the first adhesive layer after foaming and curing can be reduced. Therefore, after the foamable adhesive sheet is foamed and cured, the adhesion of the cured second adhesive layer to the substrate can be increased, thereby suppressing the generation of foreign matter. Also, after the foamable adhesive sheet is foamed and cured, when a shear stress is applied, the application of excessive load to layers other than the second adhesive layer can be suppressed, thereby improving the durability of the foamable adhesive sheet after foaming and curing.
[0022] On the other hand, when the slope of the approximate straight line of the second adhesive layer after curing is equal to or less than a predetermined value, if the second adhesive layer after curing becomes too soft, there is a concern that the adhesiveness of the second adhesive layer after curing will decrease. In contrast, in the present disclosure, the failure mode when the tensile shear adhesive strength test method is performed on the foamable adhesive sheet is cohesive failure of the first adhesive layer after foaming and curing. Therefore, it can be said that the adhesiveness of the second adhesive layer after curing is high. Furthermore, the adhesiveness of the first adhesive layer after foaming and curing is also high.
[0023] Therefore, by using the foamable adhesive sheet of the present disclosure, the quality and reliability of the product can be improved.
[0024] There are various known methods for testing adhesive strength, such as a tensile shear adhesive strength test method, a tensile adhesive strength test method, a peel adhesive strength test method, and a bending adhesive strength test method, but generally, the tensile shear adhesive strength is often used to evaluate adhesives. When two members are bonded together, the joint is subjected to stresses such as tensile stress, compressive stress, and shear stress, but when one member is bonded and fixed to a hole or groove in the other member, it is considered that the joint is mainly subjected to shear stress. Therefore, in this disclosure, the tensile shear adhesive strength test method is used to evaluate physical properties.
[0025] The configuration of the foamable adhesive sheet according to the present disclosure will be described below.
[0026] 1. Physical properties of foamable adhesive sheets In the present disclosure, in the stress-strain curve obtained when the tensile shear adhesive strength test method is performed on the second adhesive layer after curing, the slope of the approximation line in the section from 3% strain to 5% strain is 0.20 MPa or less, may be 0.15 MPa or less, or may be 0.10 MPa or less. When the slope is in the above range, the second adhesive layer after curing has an appropriate hardness. Therefore, the difference between the hardness of the second adhesive layer after curing and the hardness of the first adhesive layer after foaming and curing can be reduced. Therefore, after the foamable adhesive sheet is foamed and cured, the second adhesive layer after curing is suppressed from peeling off from the substrate, thereby suppressing the generation of foreign matter. In addition, after the foamable adhesive sheet is foamed and cured, it is possible to suppress the application of excessive load to layers other than the second adhesive layer, and the durability of the foamable adhesive sheet after foaming and curing can be improved. In addition, the slope is, for example, 0.05 MPa or more, may be 0.07 MPa or more, or may be 0.10 MPa or more. If the gradient is within the above range, the second adhesive layer after curing has an appropriate hardness, and therefore the adhesiveness of the second adhesive layer after curing is high. Specifically, the gradient may be 0.05 MPa or more and 0.20 MPa or less, or 0.07 MPa or more and 0.15 MPa or less.
[0027] In addition, in the present disclosure, the difference between the slope of the approximation line in the section from 3% to 5% strain in the stress-strain curve obtained when the tensile shear bond strength test method is performed on the first adhesive layer after foaming and curing and the slope of the approximation line in the section from 3% to 5% strain in the stress-strain curve obtained when the tensile shear bond strength test method is performed on the second adhesive layer after curing is preferably 0.20 MPa or less, may be 0.15 MPa or less, or may be 0.10 MPa or less. When the difference in the slope is within the above range, the difference in hardness between the second adhesive layer after curing and the first adhesive layer after foaming and curing is small. Therefore, after the foamable adhesive sheet is foamed and cured, the second adhesive layer after curing is suppressed from peeling off from the substrate, thereby suppressing the generation of foreign matter. In addition, after the foamable adhesive sheet is foamed and cured, excessive load can be suppressed from being applied to layers other than the second adhesive layer, and the durability of the foamable adhesive sheet after foaming and curing can be improved. The difference in the slope is, for example, 0.05 MPa or more, may be 0.07 MPa or more, or may be 0.10 MPa or more. If the difference in the slope is within the above range, the second adhesive layer after curing has an appropriate hardness, so that the adhesiveness of the second adhesive layer after curing is high. Specifically, the difference in the slope may be 0.05 MPa or more and 0.20 MPa or less, or 0.07 MPa or more and 0.15 MPa or less.
[0028] The tensile shear adhesive strength test method for the second adhesive layer after curing is performed according to JIS K6850:1999, which corresponds to ISO 4587, by the following method. First, a second adhesive layer having a size of 12.5 mm x 25 mm is prepared. For example, when the adhesive composition used in the second adhesive layer of the foamable adhesive sheet or its composition is known, the second adhesive layer is formed using the adhesive composition or by preparing an adhesive composition having that composition. The composition of the second adhesive layer of the foamable adhesive sheet may be analyzed, and an adhesive composition having that composition may be prepared to form the second adhesive layer. A known method may be applied as a method for analyzing the composition of the second adhesive layer. The thickness of the second adhesive layer is the same as that of the second adhesive layer of the foamable adhesive sheet. In addition, as shown in FIG. 2, two metal plates 31a and 31b having a thickness of 1.6 mm, a width of 25 mm, and a length of 100 mm are prepared. For example, cold-rolled steel plate SPCC-SD can be used as the metal plate. A spacer 32 is placed at a predetermined interval at one end of one of the metal plates 31a. The thickness of the spacer 32 is set to be equal to or greater than the thickness of the second adhesive layer minus 15 μm and equal to or less than the thickness of the second adhesive layer. The thickness of the spacer 32 is adjusted by stacking a plurality of Kapton adhesive tapes manufactured by Teraoka Seisakusho Co., Ltd. Next, the second adhesive layer 3 is placed between the spacers 32, and the other metal plate 31b is placed so that one end overlaps, and fixed with a clip or an adhesive tape such as Kapton tape to obtain a test piece. Next, the second adhesive layer of the test piece is cured. The curing conditions are appropriately adjusted according to the second curable adhesive contained in the second adhesive layer. Next, the tensile shear bond strength test method is performed on the test piece after curing in accordance with JIS K6850:1999. The measurement conditions are a tensile speed of 10 mm / min, a distance between grippers of 100 mm, a temperature of normal temperature (23° C.), and a humidity of 50% RH. For example, a Tensilon RTF1350 manufactured by A&D Co., Ltd. can be used as a tensile tester.
[0029] In addition, the tensile shear adhesive strength test method for the first adhesive layer after foaming and curing is performed according to the following method in accordance with JIS K6850:1999 corresponding to ISO 4587. First, a first adhesive layer having a size of 12.5 mm x 25 mm is prepared. For example, when the adhesive composition used in the first adhesive layer of the foamable adhesive sheet or its composition is known, the first adhesive layer is formed using the adhesive composition or by preparing an adhesive composition having that composition. In addition, the composition of the first adhesive layer of the foamable adhesive sheet may be analyzed, and an adhesive composition having that composition may be prepared to form the first adhesive layer. A known method may be applied as a method for analyzing the composition of the first adhesive layer. The thickness of the first adhesive layer is the same as that of the first adhesive layer of the foamable adhesive sheet. In addition, as shown in FIG. 3, two metal plates 31a and 31b having a thickness of 1.6 mm, a width of 25 mm, and a length of 100 mm are prepared. For example, cold-rolled steel plate SPCC-SD can be used as the metal plate. A spacer 32 is placed at a predetermined interval at one end of one of the metal plates 31a. The thickness of the spacer 32 is appropriately set according to the foaming ratio of the first adhesive layer. For example, as shown in FIG. 4, after the foamable adhesive sheet 10 is placed between the first member 20a and the second member 20b, the foamable adhesive sheet 10 is foamed and cured (not shown) to bond the first member 20a and the second member 20b. If the distance d1 between the first member 20a and the second member 20b is known, the gap d2 after the foamable adhesive sheet 10 is placed between the first member 20a and the second member 20b is first obtained. The gap d2 is obtained by subtracting the thickness t1 of the foamable adhesive sheet 10 from the distance d1. Next, the thickness of the spacer 32 is set based on the thickness of the first adhesive layer and the gap d2. The thickness of the spacer 32 is obtained by adding the thickness of the first adhesive layer and the gap d2. The thickness of the spacer 32 may be within ±5% of the value obtained by adding the thickness of the first adhesive layer and the gap d2. On the other hand, when the distance d1 between the first member 20a and the second member 20b is unknown, the expansion ratio of the first adhesive layer is first obtained. The expansion ratio here refers to the expansion ratio when the first adhesive layer is foamed and cured without being sandwiched between any members. The expansion ratio of the first adhesive layer can be obtained by foaming and curing the foamable adhesive sheet without being sandwiched between any members.In this case, the thickness of the spacer 32 is (thickness of the first adhesive layer) x (expansion ratio of the first adhesive layer) x 0.3 or more, and (thickness of the first adhesive layer) x (expansion ratio of the first adhesive layer) x 0.8 or less. However, the thickness of the spacer 32 is equal to or more than the thickness of the first adhesive layer. The thickness of the spacer 32 is adjusted by stacking a plurality of Kapton adhesive tapes manufactured by Teraoka Seisakusho Co., Ltd. Next, the first adhesive layer 1 is placed between the spacers 32, and the other metal plate 31b is placed so that one tip overlaps, and fixed with a clip or an adhesive tape such as Kapton tape to obtain a test piece. Next, the first adhesive layer of the test piece is foamed and cured. The foaming and curing conditions are appropriately adjusted according to the first curable adhesive and the foaming agent contained in the first adhesive layer. Next, the test piece after foaming and curing is subjected to a tensile shear adhesive strength test method in accordance with JIS K6850:1999. The measurement conditions are as follows: tensile speed: 10 mm / min, gripper distance: 100 mm, temperature: room temperature (23° C.), humidity: 50% RH. As a tensile tester, for example, Tensilon RTF1350 manufactured by A&D Co., Ltd. can be used.
[0030] The stress-strain curve is the relationship between the shear stress and strain obtained in the above-mentioned tensile shear bond strength test method, as shown in Figures 5(a) and (b), with the horizontal axis representing strain (%) and the vertical axis representing shear stress (MPa). The strain is the value obtained by dividing the increase in the distance between the grippers by the length of the first adhesive layer or the second adhesive layer, i.e., 12.5 mm. Figure 5(b) is an enlarged view of Figure 5(a).
[0031] In the stress-strain curve obtained by the above tensile shear bond strength test method, the approximation line in the section from 3% strain to 5% strain is obtained by linearly approximating the curve in the section from 3% strain to 5% strain by the least squares method. Then, the slope of the approximation line is obtained. The above tensile shear bond strength test method is performed three times, and the average value of the three times is used as the slope of the approximation line.
[0032] In the stress-strain curve obtained by the above tensile shear adhesive strength test method, the initial slope is the slope in the elastic region. Therefore, in the present disclosure, the initial slope is adopted. In addition, in the stress-strain curve, the shear stress tends to be unstable in the section of less than 3% strain. Therefore, in the present disclosure, the slope of the section from 3% strain to 5% strain is adopted as the initial slope.
[0033] Methods for controlling the slope of the above approximate straight line for the cured second adhesive layer include, for example, adjusting the composition of the second adhesive layer and adjusting the drying conditions when forming the second adhesive layer.
[0034] In the method of adjusting the composition of the second adhesive layer, as described later, by including soft particles in the second adhesive layer, the hardness of the second adhesive layer after curing tends to be small, and the slope of the above-mentioned approximate straight line tends to be small. In addition, in the second adhesive layer containing an epoxy resin and a curing agent, if the number of functional groups of the epoxy resin is the same, the hardness of the second adhesive layer after curing tends to be small, and the slope of the above-mentioned approximate straight line tends to be small, by reducing the molecular weight of the epoxy resin. In addition, in the second adhesive layer containing an epoxy resin and a curing agent, by reducing the content of the multifunctional epoxy resin, the crosslink density after curing is reduced, so that the hardness of the second adhesive layer after curing tends to be small, and the slope of the above-mentioned approximate straight line tends to be small.
[0035] In the present disclosure, when a tensile shear adhesive strength test method is performed on a foamable adhesive sheet after foaming and curing, the failure mode is cohesive failure of the first adhesive layer after foaming and curing. If the failure mode is cohesive failure of the first adhesive layer after foaming and curing, it can be said that the second adhesive layer after curing has a higher strength than the first adhesive layer after foaming and curing.
[0036] The tensile shear adhesive strength test method for the foamed and cured foamable adhesive sheet is performed according to the following method in accordance with JIS K6850:1999, which corresponds to ISO 4587. First, a foamable adhesive sheet measuring 12.5 mm x 25 mm is prepared. As shown in FIG. 6, two metal plates 31a and 31b each having a thickness of 1.6 mm, a width of 25 mm, and a length of 100 mm are prepared. For example, a cold-rolled steel plate SPCC-SD can be used as the metal plate. A spacer 32 is placed at a predetermined interval at one end of one of the metal plates 31a. The thickness of the spacer 32 is appropriately set according to the foaming ratio of the first adhesive layer. For example, as shown in FIG. 4, after disposing the foamable adhesive sheet 10 between the first member 20a and the second member 20b, the foamable adhesive sheet 10 is foamed and cured (not shown) to bond the first member 20a and the second member 20b. If the distance d1 between the first member 20a and the second member 20b is known, the thickness of the spacer 32 is set to the above distance d1. The thickness of the spacer 32 may be within the above distance d1 ±5%. On the other hand, if the distance d1 between the first member 20a and the second member 20b is unknown, the foaming ratio of the first adhesive layer is first obtained. The foaming ratio here refers to the foaming ratio when the first adhesive layer is foamed and cured without being sandwiched between any members. The foaming ratio of the first adhesive layer can be obtained by foaming and curing the foamable adhesive sheet without being sandwiched between any members. In this case, the thickness of the spacer 32 is {(thickness of the foamable adhesive sheet)-(thickness of the first adhesive layer)}+(thickness of the first adhesive layer)×(expansion ratio of the first adhesive layer)×0.3 or more, and {(thickness of the foamable adhesive sheet)-(thickness of the first adhesive layer)}+(thickness of the first adhesive layer)×(expansion ratio of the first adhesive layer)×0.8 or less. However, the thickness of the spacer 32 is greater than or equal to the thickness of the foamable adhesive sheet. The thickness of the spacer 32 is adjusted by stacking multiple sheets of Kapton adhesive tape manufactured by Teraoka Seisakusho Co., Ltd. Next, the foamable adhesive sheet 10 is placed between the spacers 32, and the other metal plate 31b is placed so that one tip overlaps, and fixed with a clip or an adhesive tape such as Kapton tape to obtain a test piece. Next, the first adhesive layer of the test piece is foamed and cured, and the second adhesive layer is cured.The foaming and curing conditions are appropriately adjusted according to the first curable adhesive and foaming agent contained in the first adhesive layer and the second curable adhesive contained in the second adhesive layer. Next, the test piece after foaming and curing is subjected to a tensile shear bond strength test method in accordance with JIS K6850:1999. The measurement conditions are a tensile speed of 10 mm / min, temperature at room temperature (23°C), and humidity of 50% RH. For example, a Tensilon RTF1350 manufactured by A&D Co., Ltd. can be used as a tensile tester. Next, the fracture surface of the test piece is visually observed.
[0037] The failure mode being cohesive failure of the first adhesive layer after foaming and curing means that the cohesive failure rate inside the first adhesive layer after foaming and curing is 90% or more. The cohesive failure rate is the ratio of the area of the cohesive failure part inside the first adhesive layer to the total adhesive area. The above tensile shear adhesive strength test method is performed three times, and the above cohesive failure rate is the average value of the three measurements.
[0038] The foamable adhesive sheet of the present disclosure preferably has high adhesiveness after foaming and curing. The shear adhesive strength may be, for example, 2.1 MPa or more, or 2.3 MPa or more at 23°C. The shear adhesive strength may be, for example, 0.27 MPa or more, 0.55 MPa or more, or 0.58 MPa or more at 200°C. For example, in a high-strength acrylic foam adhesive tape that does not require heating, the shear adhesive strength is about 1 MPa or more and 2 MPa or less at room temperature, and there is no heat resistance at 200°C. Therefore, if the shear adhesive strength is in the above range at 23°C, there is an advantage in terms of strength. Also, if the shear adhesive strength is in the above range at 200°C, it can be applied to applications that require heat resistance around an automobile engine or similar.
[0039] The shear adhesive strength of the foamable adhesive sheet after foaming and curing is measured by the above-mentioned tensile shear adhesive strength test method, and the shear adhesive strength is defined as the maximum shear stress at break.
[0040] The foamable adhesive sheet in the present disclosure preferably has good shape retention. The bending moment based on JIS P8125-2:2017 corresponding to ISO 2493 is, for example, 3 gf·cm or more, and may be 5 gf·cm or more. On the other hand, the bending moment may be, for example, less than 40 gf·cm, and may be less than 30 gf·cm. Conventionally, in adhesive sheets, a method of increasing the bending moment to improve shape retention and insertion into narrow gaps is common. In response to this, the inventors of the present disclosure have found that shape retention can be guaranteed by devising the shape, and that a high bending moment has other disadvantages, so that in consideration of other characteristics, it is preferable that the bending moment be within the above range. If the bending moment is smaller than the above range, it may be difficult to maintain the shape even by devising folding or the like. In addition, if the bending moment is larger than the above range, the shape will return to its original state after folding, so it is necessary to heat the sheet during folding or to make a crease in the fold. Heating the sheet reduces its lifespan, and striations can reduce the insulation properties of that area.
[0041] In the foamable adhesive sheet of the present disclosure, it is preferable that the electrical insulation after foaming and curing is high. The dielectric breakdown voltage based on JIS C2107:2011 corresponding to IEC 60454-2 is, for example, preferably 1 kV or more, more preferably 3 kV or more. When the dielectric breakdown voltage is in the above range, it is possible to apply it to rust prevention and around copper wires. In addition, in the foamable adhesive sheet of the present disclosure, the thermal conductivity after foaming and curing is, for example, preferably 0.1 W / mK or more, more preferably 0.15 W / mK or more. When the thermal conductivity is in the above range, it is possible to miniaturize parts and promote the curing reaction during heating.
[0042] 2.First adhesive layer The first adhesive layer of the present disclosure is disposed on one side of the substrate and contains a first curable adhesive and a foaming agent.
[0043] (1) Physical properties of the first adhesive layer The first adhesive layer in the present disclosure is preferably substantially non-tacky. Specifically, the tack of the first adhesive layer is preferably less than 0.1 N, may be 0.05 N or less, or may be 0.02 N or less. When the tack of the first adhesive layer is within the above range, the first adhesive layer becomes substantially non-tacky (tack-free). In addition, the slipperiness of the first adhesive layer becomes good, and the insertability of the foamable adhesive sheet can be improved.
[0044] Here, the tack of the first adhesive layer is measured by a probe tack test. Specifically, a cylindrical stainless steel probe with a diameter of 5 mm is pressed against the surface of the first adhesive layer of the foamable adhesive sheet under conditions of a temperature of 23±5°C and a humidity of 50±30%RH with a load of 0.1 N and a speed of 30 mm / min, and after holding for 1.0 second, it is peeled off at a speed of 30 mm / min, and the load at the time of peeling is measured. This measurement is performed five times, and the average value is taken as the tack. For example, a tack tester "TAC-II" manufactured by RHESCA can be used as the probe tack tester.
[0045] In the present disclosure, an example of a method for controlling the tackiness of the first adhesive layer is a method for adjusting the composition of the first adhesive layer. Specifically, the tackiness of the first adhesive layer can be reduced by using an epoxy resin that is solid at room temperature or a curing agent that is solid at room temperature in the first adhesive layer containing an epoxy resin and a curing agent. In addition, the tackiness of the first adhesive layer can be reduced by including an epoxy resin with a high softening temperature or an epoxy resin with a large weight average molecular weight in the first adhesive layer containing an epoxy resin and a curing agent. For example, the tackiness of the first adhesive layer can be reduced by including multiple types of epoxy resins with different softening temperatures in the first adhesive layer, that is, by including one epoxy resin and another epoxy resin whose softening temperature is 25° C. or higher and 10° C. or higher than the softening temperature of the one epoxy resin in the first adhesive layer. Also, for example, the first adhesive layer can be made to contain multiple types of epoxy resins with different weight average molecular weights, that is, the first adhesive layer can be made to contain one epoxy resin and another epoxy resin whose weight average molecular weight is 370 or more and is 300 or more greater than the weight average molecular weight of the one epoxy resin, thereby reducing the tack of the first adhesive layer. More specifically, the first adhesive layer containing an epoxy resin and a curing agent can be made to contain a first epoxy resin with a low softening temperature and a low molecular weight, and a second epoxy resin with a high softening temperature and a high molecular weight, as described below, as the epoxy resin. Also, the first adhesive layer containing an epoxy resin and a curing agent can be made to contain an acrylic resin compatible with the epoxy resin, as described below, thereby reducing the tack of the first adhesive layer.
[0046] Here, non-tacky is generally used mainly to mean low adhesive strength. In the present disclosure, "substantially non-tacky" means that the tack is less than 0.1 N.
[0047] "Adhesion" is a concept that is included in "bonding." The two are sometimes distinguished in that "adhesion" is used to mean a temporary adhesive phenomenon, whereas "bonding" is used to mean a substantially permanent adhesive phenomenon (Iwanami Shoten Physics and Chemistry Dictionary, 5th Edition). "Adhesiveness" and "adhesive strength" refer to the property of adhering through pressure and the adhesive strength at that time.
[0048] In this specification, the "adhesiveness of the adhesive layer" and the "adhesive strength of the adhesive layer" refer to the adhesiveness and adhesive strength of the adhesive layer before curing, unless otherwise specified. In addition, in this specification, the "adhesiveness of the adhesive layer" and the "adhesive strength of the adhesive layer" refer to the adhesiveness and adhesive strength of the adhesive layer after curing, unless otherwise specified.
[0049] (2) Material of the first adhesive layer (a) a first curing adhesive The first curable adhesive contained in the first adhesive layer in the present disclosure may be a curable adhesive generally used in the adhesive layer of an adhesive sheet. Examples of the first curable adhesive include a heat-curable adhesive and a light-curable adhesive. Among them, a heat-curable adhesive is preferred. A heat-curable adhesive can be applied even when the member does not have transparency, such as a metal member.
[0050] Examples of the first curable adhesive include epoxy resin adhesives, acrylic resin adhesives, phenol resin adhesives, unsaturated polyester resin adhesives, alkyd resin adhesives, urethane resin adhesives, and thermosetting polyimide resin adhesives.
[0051] The first curable adhesive is preferably an epoxy resin adhesive. That is, the first curable adhesive preferably contains an epoxy resin and a curing agent. In general, the epoxy resin adhesive has a hard and tough cured film, and is suitable for bonding hard material members such as metal and glass members. In addition, the epoxy resin adhesive generally has excellent heat resistance, insulating properties, chemical resistance, etc., has small curing shrinkage, and can be used in a wide range of applications.
[0052] In addition, when the first curable adhesive is an epoxy resin adhesive, the first curable adhesive preferably further contains an acrylic resin compatible with the epoxy resin. By using an acrylic resin compatible with the epoxy resin, the toughness of the first adhesive layer can be increased. This can improve the adhesiveness after foaming and curing.
[0053] Hereinafter, an example will be described in which the first curable adhesive is an epoxy resin adhesive.
[0054] (i) Epoxy resin The epoxy resin in the present disclosure is a compound that has at least one epoxy group or glycidyl group and is cured by a crosslinking polymerization reaction in combination with a curing agent. The epoxy resin also includes a monomer having at least one epoxy group or glycidyl group.
[0055] As the epoxy resin, an epoxy resin generally used in the adhesive layer of an adhesive sheet can be used. In particular, the curable adhesive preferably contains, as the epoxy resin, a first epoxy resin having a softening temperature of 50° C. or higher and an epoxy equivalent of 5000 g / eq or less, and a second epoxy resin having a softening temperature higher than that of the first epoxy resin and a weight average molecular weight of 20,000 or more. By using the first epoxy resin and the second epoxy resin in combination, an adhesive sheet having good adhesion and blocking resistance after foaming and curing can be obtained. Furthermore, the tackiness (tackiness) of the first adhesive layer can be reduced, and an adhesive sheet having good slip properties can be obtained.
[0056] For example, when only improving the adhesiveness after foaming and curing, it is more effective to use an epoxy resin with a low molecular weight (low epoxy equivalent) than an epoxy resin with a high molecular weight (high epoxy equivalent). However, when an epoxy resin with a low molecular weight (low epoxy equivalent) is used, the epoxy resins with low molecular weight (low epoxy equivalent) are assimilated with each other when the adhesive sheet is wound into a roll, for example, and blocking is likely to occur.
[0057] In contrast, when a first epoxy resin having a relatively low softening temperature (relatively high crystallinity) and a low molecular weight (low epoxy equivalent) is used, the first epoxy resin melts rapidly and changes to a low-viscosity liquid when the temperature reaches or exceeds the softening temperature. Therefore, it is easy to improve the adhesiveness after foaming and curing. On the other hand, since the first epoxy resin has a relatively high crystallinity, it can suppress the occurrence of blocking compared to an epoxy resin having a relatively low crystallinity or an epoxy resin having no crystallinity. However, when only the first epoxy resin is used, there is a possibility that the effect of suppressing the occurrence of blocking is insufficient or the adhesiveness (tackiness) of the first adhesive layer becomes too high. Therefore, by further using a second epoxy resin having a relatively high softening temperature (relatively low crystallinity) and a high molecular weight, it is possible to improve the effect of suppressing the occurrence of blocking and to suppress the adhesiveness (tackiness) of the first adhesive layer to a low level.
[0058] (i-1) First epoxy resin The first epoxy resin has a softening temperature of 50° C. or higher and an epoxy equivalent of 5000 g / eq or lower. The first epoxy resin has a relatively low softening temperature (relatively high crystallinity) compared to the second epoxy resin described below. The first epoxy resin has relatively high crystallinity and a low molecular weight, which makes it easy to improve adhesion and blocking resistance after foaming and curing. In addition, the first epoxy resin has a low molecular weight, which makes it possible to increase the crosslink density, and a first adhesive layer having good mechanical strength, chemical resistance, and curing properties can be obtained. In addition, the first epoxy resin is preferably an epoxy resin that is solid at room temperature (23° C.).
[0059] The softening temperature of the first epoxy resin is usually 50° C. or higher, and may be 55° C. or higher, or may be 60° C. or higher. On the other hand, the softening temperature of the first epoxy resin is, for example, 150° C. or lower. The softening temperature is measured by the ring and ball method in accordance with JIS K7234:1986.
[0060] The epoxy equivalent of the first epoxy resin is, for example, 5000 g / eq or less, may be 3000 g / eq or less, may be 1000 g / eq or less, or may be 600 g / eq or less. On the other hand, the epoxy equivalent of the first epoxy resin is, for example, 90 g / eq or more, may be 100 g / eq or more, or may be 110 g / eq or more. The epoxy equivalent is the number of grams of a resin containing 1 gram equivalent of an epoxy group. The epoxy equivalent is measured by a method conforming to JIS K7236:2009, which corresponds to ISO 3001 (Plastics Epoxy compounds-Determination of epoxy equivalent).
[0061] The first epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher functional epoxy resin.
[0062] The weight average molecular weight (Mw) of the first epoxy resin is usually smaller than the weight average molecular weight (Mw) of the second epoxy resin described below. The Mw of the first epoxy resin is, for example, 6,000 or less, and may be 4,000 or less, or may be 3,000 or less. On the other hand, the Mw of the first epoxy resin is, for example, 400 or more. Mw is a value calculated in terms of polystyrene as measured by gel permeation chromatography (GPC).
[0063] The melt viscosity of the first epoxy resin at 150°C is, for example, 0.005 Pa·s or more, may be 0.015 Pa·s or more, may be 0.03 Pa·s or more, may be 0.05 Pa·s or more, or may be 0.1 Pa·s or more. If the melt viscosity is too low, good foaming properties may not be obtained. In addition, if the melt viscosity of the first epoxy resin is too low (if the crystallinity of the first epoxy resin is too high), the adhesion (tackiness) of the resulting first adhesive layer may be high. The reason for this is presumably that if the melt viscosity of the first epoxy resin is too low (if the crystallinity of the first epoxy resin is too high), when it is mixed with the second epoxy resin or the acrylic resin, its crystallinity is greatly reduced, and the Tg of the entire adhesive composition is reduced. On the other hand, the melt viscosity of the first epoxy resin at 150°C is, for example, 10 Pa·s or less, may be 5 Pa·s or less, or may be 2 Pa·s or less. If the melt viscosity is too high, the uniformity of the resulting first adhesive layer may be reduced. The melt viscosity is measured in accordance with JIS K6862:1984, which corresponds to ISO 2555 (Determination of Brookfield RV viscosity of Resins in the liquid state or as emulsions or dispersions), using a Brookfield type single cylinder rotational viscometer and a thermocell for heating the solution.
[0064] Next, the constitution of the first epoxy resin will be described. Examples of the first epoxy resin include aromatic epoxy resins, aliphatic epoxy resins, alicyclic epoxy resins, and heterocyclic epoxy resins. Specific examples of the first epoxy resin include bisphenol-type epoxy resins, novolac-type epoxy resins, and modified epoxy resins. Examples of the bisphenol-type epoxy resins include bisphenol A-type epoxy resins and bisphenol F-type epoxy resins. Examples of the novolac-type epoxy resins include bisphenol A novolac-type epoxy resins and cresol novolac-type epoxy resins. Examples of the modified epoxy resins include urethane-modified epoxy resins and rubber-modified epoxy resins. Other specific examples include biphenyl-type epoxy resins, stilbene-type epoxy resins, triphenolmethane-type epoxy resins, alkyl-modified triphenolmethane-type epoxy resins, triazine nucleus-containing epoxy resins, dicyclopentadiene-modified phenol-type epoxy resins, naphthalene-type epoxy resins, glycol-type epoxy resins, and pentaerythritol-type epoxy resins. The first epoxy resin may be one type or two or more types.
[0065] Bisphenol A type epoxy resins can exist in a liquid state at room temperature or in a solid state at room temperature depending on the number of repeating units of the bisphenol skeleton. Bisphenol A type epoxy resins having, for example, 2 to 10 bisphenol skeletons in the main chain are solid at room temperature. In particular, bisphenol A type epoxy resins are preferred in that they can improve heat resistance.
[0066] In particular, the first epoxy resin is preferably a bisphenol A novolac type epoxy resin represented by the following general formula (1).
[0067] [ka]
[0068] In the general formula (1), R 1 is C m H2m (m is 1 or more and 3 or less), 2 and R 3 are each independently p H 2p+1 (p is 1 or more and 3 or less), and n is 0 or more and 10 or less.
[0069] In the general formula (1), R 1 m in is 1, that is, R 1 is preferably -CH2-. Similarly, R 2 and R 3 p in is 1, that is, R 2 and R 3 is preferably -CH3. Furthermore, the hydrogen bonded to the benzene ring in general formula (1) may be substituted with other elements or other groups.
[0070] The content of the first epoxy resin may be, for example, 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, or 25 parts by mass or more, when the resin component contained in the first adhesive layer is 100 parts by mass. If the content of the first epoxy resin is too small, the adhesiveness and blocking resistance after foaming and curing may be reduced. On the other hand, the content of the first epoxy resin may be, for example, 90 parts by mass or less, 80 parts by mass or less, 70 parts by mass or less, 60 parts by mass or less, 50 parts by mass or less, or 40 parts by mass or less, when the resin component contained in the first adhesive layer is 100 parts by mass. If the content of the first epoxy resin is too high, the content of the second epoxy resin and the acrylic resin will be relatively low, and it may be difficult to balance the blocking resistance, the adhesion of the first adhesive layer to the substrate, and the adhesiveness after foaming and curing.
[0071] (i-2) Second epoxy resin The second epoxy resin has a higher softening temperature than the first epoxy resin and a weight average molecular weight of 20,000 or more. The second epoxy resin has a relatively high softening temperature (relatively low crystallinity) compared to the above-mentioned first epoxy resin. The second epoxy resin has relatively low crystallinity and high molecular weight, so that it is easy to improve blocking resistance. Furthermore, the second epoxy resin has relatively low crystallinity and high molecular weight, so that it is possible to suppress an increase in adhesion (tackiness) caused by the first epoxy resin. Moreover, it is preferable that the second epoxy resin is an epoxy resin that is solid at room temperature (23°C).
[0072] The weight average molecular weight (Mw) of the second epoxy resin is usually larger than the weight average molecular weight (Mw) of the first epoxy resin. The Mw of the second epoxy resin is usually 20,000 or more, may be 30,000 or more, or may be 35,000 or more. On the other hand, the Mw of the second epoxy resin is, for example, 100,000 or less.
[0073] The epoxy equivalent of the second epoxy resin may be larger, smaller, or the same as that of the first epoxy resin. The epoxy equivalent of the second epoxy resin is, for example, 4000 g / eq or more, 5000 g / eq or more, or 6000 g / eq or more. On the other hand, the epoxy equivalent of the second epoxy resin is, for example, 20000 g / eq or less.
[0074] The second epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher functional epoxy resin.
[0075] The softening temperature of the second epoxy resin is usually higher than that of the first epoxy resin. The difference between the two is, for example, 10° C. or more, and may be 20° C. or more, or may be 30° C. or more. The softening temperature of the second epoxy resin is, for example, 80° C. or more, and may be 90° C. or more. On the other hand, the softening temperature of the second epoxy resin is, for example, 180° C. or less.
[0076] The composition of the second epoxy resin is the same as that of the first epoxy resin described above, and therefore the description thereof will be omitted here.
[0077] The content of the second epoxy resin may be, for example, 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, 35 parts by mass or more, 40 parts by mass or more, or 45 parts by mass or more, when the resin component contained in the first adhesive layer is taken as 100 parts by mass. If the content of the second epoxy resin is too small, the blocking resistance may be reduced. On the other hand, the content of the second epoxy resin may be, for example, 90 parts by mass or less, 85 parts by mass or less, 80 parts by mass or less, or 75 parts by mass or less, when the resin component contained in the first adhesive layer is taken as 100 parts by mass. If the content of the second epoxy resin is too high, the contents of the first epoxy resin and the acrylic resin become relatively small, and it may be difficult to balance the blocking resistance, the adhesion of the first adhesive layer to the substrate, and the adhesion after foaming and curing.
[0078] The ratio of the first epoxy resin to the total of the first epoxy resin and the second epoxy resin is, for example, 5 mass% or more, optionally 10 mass% or more, optionally 15 mass% or more, or optionally 20 mass% or more, whereas the ratio of the first epoxy resin is, for example, 80 mass% or less, optionally 75 mass% or less, or optionally 60 mass% or less.
[0079] Furthermore, the total proportion of the first epoxy resin and the second epoxy resin to all epoxy resins contained in the first adhesive layer is, for example, 50 mass% or more, optionally 70 mass% or more, optionally 90 mass% or more, or optionally 100 mass%.
[0080] (ii) Acrylic resin The acrylic resin in the present disclosure is a resin compatible with the epoxy resin. Since the acrylic resin is compatible with the epoxy resin, it is easy to improve the toughness of the first adhesive layer. As a result, the adhesion of the first adhesive layer to the substrate can be improved. In addition, the improved toughness of the adhesive layer can improve the adhesion after foaming and curing. Furthermore, it is considered that the acrylic resin acts as a compatibilizer for the foaming agent (for example, a foaming agent whose shell portion is an acrylonitrile copolymer resin), and uniformly disperses and foams, thereby improving the adhesion after foaming and curing. In addition, the compatibility of the acrylic resin with the epoxy resin can maintain a high hardness of the surface of the first adhesive layer. On the other hand, if the acrylic resin is incompatible with the epoxy resin, a soft portion is formed on the surface of the first adhesive layer, making the interface with the adherend less slippery, and workability may be reduced.
[0081] The acrylic resin in the present disclosure is compatible with the epoxy resin. Here, the compatibility of the acrylic resin with the epoxy resin is confirmed, for example, by observing the cross section of the first adhesive layer of the adhesive sheet with a scanning electron microscope (SEM) or a transmission electron microscope (TEM) to see that no micron-sized islands are generated. More specifically, the average particle size of the islands is preferably 1 μm or less. In particular, the average particle size of the islands may be 0.5 μm or less, or may be 0.3 μm or less. It is preferable to have a large number of samples, for example, 100 or more. The area to be observed is in the range of 100 μm × 100 μm, or, when the average thickness of the first adhesive layer is 100 μm or less, in the range of the average thickness × 100 μm.
[0082] The weight average molecular weight (Mw) of the acrylic resin is, for example, 50,000 or more, may be 70,000 or more, or may be 100,000 or more. The first epoxy resin has a relatively high crystallinity, and the melt viscosity (or dynamic viscoelasticity) during heating becomes too low, which may cause shrinkage during hardening after foaming (between the end of foaming of the foaming agent and the hardening of the adhesive composition). However, by using an acrylic resin having a certain molecular weight, it is possible to prevent the melt viscosity from becoming too low, and shrinkage is less likely to occur during hardening after foaming. On the other hand, the Mw of the acrylic resin is, for example, 1,500,000 or less. The weight average molecular weight of the acrylic resin is measured by GPC (eluent: THF, standard substance: PS, sample: 20 μL, flow rate: 1 mL / min, column temperature: 40° C.).
[0083] The glass transition temperature (Tg) of the acrylic resin is, for example, 90° C. or higher, and may be 100° C. or higher. On the other hand, the Tg of the acrylic resin is, for example, 180° C. or lower. Tg is measured by a differential scanning calorimeter (DSC) in accordance with JIS K7121:2012, which corresponds to ISO 3146.
[0084] Acrylic resin has a storage modulus (E') of 1 x 10 at the foaming start temperature. 6 Pa or less. When E' at the foaming start temperature is low, the fluidity is improved and good foaming properties can be obtained. On the other hand, E' at the foaming start temperature may be, for example, 1×10 5 The foaming initiation temperature is a temperature that differs depending on the type of foaming agent. When two or more foaming agents are used, the foaming initiation temperature is the initiation temperature of the main foaming reaction.
[0085] Acrylic resin has a storage modulus (E') of 1 x 10 at the curing start temperature. 5Pa or more. As described above, shrinkage may occur during curing after foaming (from the end of foaming of the foaming agent to the curing of the adhesive composition), but by having a large E' at the curing start temperature, shrinkage can be suppressed and good shape retention can be obtained. The curing start temperature is a temperature that differs depending on the type of curing agent. In addition, when two or more types of curing agents are used as the curing agent, the start temperature of the main curing reaction is taken as the curing start temperature.
[0086] In addition, the average storage modulus (E') of acrylic resin at temperatures between 0°C and 100°C is 1×10 6 The average value of storage modulus (E') before foaming may be high, so that good blocking resistance can be obtained. On the other hand, the average value of storage modulus (E') at 0°C or higher and 100°C or lower may be, for example, 1 x 10 8 Pa or less.
[0087] The storage modulus (E') of the acrylic resin is measured by a dynamic viscoelasticity measurement method conforming to JIS K7244-1:1998. The measurement conditions are as follows: attachment mode: compression mode, frequency: 1Hz, temperature: -30℃ to 200℃, heating rate: 10℃ / min. The device used is the solid viscoelasticity analyzer "RSA-III" manufactured by TA Instruments.
[0088] The acrylic resin may have a polar group, such as an epoxy group, a hydroxyl group, a carboxyl group, a nitrile group, or an amide group.
[0089] The acrylic resin may be a homopolymer of an acrylic acid ester monomer, a mixed component containing two or more of the above homopolymers, or a copolymer of two or more of the acrylic acid ester monomers, a component containing one or more copolymers. The acrylic resin may also be a mixed component of the above homopolymer and the above copolymer. The "acrylic acid" of the acrylic acid ester monomer also includes the concept of methacrylic acid. Specifically, the acrylic resin may be a mixture of a methacrylate polymer and an acrylate polymer, or an acrylic acid ester polymer such as acrylate-acrylate, methacrylate-methacrylate, or methacrylate-acrylate. Among them, the acrylic resin preferably contains a copolymer of two or more of the acrylic acid ester monomers ((meth)acrylic acid ester copolymer).
[0090] Examples of the monomer components constituting the (meth)acrylic acid ester copolymer include the monomer components described in JP 2014-065889 A. The monomer components may have the above-mentioned polar group. Examples of the (meth)acrylic acid ester copolymer include ethyl acrylate-butyl acrylate-acrylonitrile copolymer, ethyl acrylate-acrylonitrile copolymer, and butyl acrylate-acrylonitrile copolymer. Note that "acrylic acid" such as methyl acrylate and ethyl acrylate also includes "methacrylic acid" such as methyl methacrylate and ethyl methacrylate.
[0091] The (meth)acrylic acid ester copolymer is preferably a block copolymer, and more preferably an acrylic block copolymer such as a methacrylate-acrylate copolymer. Examples of (meth)acrylates constituting the acrylic block copolymer include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, and benzidyl acrylate. These "acrylic acids" also include "methacrylic acid."
[0092] Specific examples of methacrylate-acrylate copolymers include acrylic copolymers such as methyl methacrylate-butyl acrylate-methyl methacrylate (MMA-BA-MMA) copolymers. MMA-BA-MMA copolymers also include block copolymers of polymethyl methacrylate-polybutyl acrylate-polymethyl methacrylate (PMMA-PBA-PMMA).
[0093] The acrylic copolymer may not have a polar group, or may be a modified product having the above-mentioned polar group partially introduced therein. The modified product is easily compatible with the epoxy resin, and therefore the adhesiveness is further improved.
[0094] Among them, the acrylic resin is preferably a (meth)acrylic acid ester copolymer having a first polymer portion having a glass transition temperature (Tg) of 10° C. or lower and a second polymer portion having a glass transition temperature (Tg) of 20° C. or higher. Such a (meth)acrylic acid ester copolymer has the first polymer portion that becomes a soft segment and the second polymer portion that becomes a hard segment.
[0095] The manifestation of the above-mentioned effect can be presumed as follows: By using an acrylic resin having both a soft segment and a hard segment, such as the above-mentioned (meth)acrylic acid ester copolymer, the hard segment contributes to heat resistance, and the soft segment contributes to toughness or flexibility, so that a first adhesive layer having good heat resistance, toughness, and flexibility can be obtained.
[0096] At least one of the first polymer portion and the second polymer portion contained in the (meth)acrylic acid ester copolymer has compatibility with epoxy resins. When the first polymer portion has compatibility with epoxy resins, flexibility can be increased. When the second polymer portion has compatibility with epoxy resins, cohesion and toughness can be increased.
[0097] When either the first polymer portion or the second polymer portion is incompatible with the epoxy resin, the (meth)acrylic acid ester copolymer has a compatible portion, which is a polymer portion that is compatible with the epoxy resin, and an incompatible portion, which is a polymer portion that is incompatible with the epoxy resin. In this case, when the (meth)acrylic acid ester copolymer is added to the adhesive composition, the compatible portion is compatible with the epoxy resin, and the incompatible portion is incompatible with the epoxy resin, so that fine phase separation occurs. As a result, a fine sea-island structure is developed. The sea-island structure varies depending on the type of (meth)acrylic acid ester copolymer, the compatibility of the first polymer portion and the second polymer portion contained in the (meth)acrylic acid ester copolymer, and the presence or absence of modification by introduction of a polar group, and examples thereof include a sea-island structure in which the compatible portion of the cured epoxy resin and the (meth)acrylic acid ester copolymer is a sea, and the incompatible portion of the (meth)acrylic acid ester copolymer is an island, a sea-island structure in which the incompatible portion of the (meth)acrylic acid ester copolymer is a sea, and the compatible portion of the cured epoxy resin and the (meth)acrylic acid ester copolymer is an island, and a sea-island structure in which the (meth)acrylic acid ester copolymer is a sea, and the cured epoxy resin is an island. By having such a sea-island structure, stress can be easily dispersed, so that interfacial destruction can be avoided, and excellent adhesion can be obtained after foaming and curing.
[0098] The (meth)acrylic acid ester copolymer is preferably a block copolymer, and more preferably an ABA block copolymer in which the compatible portion is polymer block A and the incompatible portion is polymer block B. Furthermore, it is preferable that the ABA block copolymer is an ABA block copolymer in which the first polymer portion is an incompatible portion, the second polymer portion is an compatible portion, the first polymer portion is polymer block B, and the second polymer portion is polymer block A. By using such an ABA block copolymer as the acrylic resin, in the case of a sea-island structure in which the compatible portion of the cured epoxy resin and the (meth)acrylic acid ester copolymer is the sea, and the incompatible portion of the (meth)acrylic acid ester copolymer is the island, the island portion can be made small. In addition, in the case of a sea-island structure in which the incompatible portion of the (meth)acrylic acid ester copolymer is the sea, and the compatible portion of the cured epoxy resin and the (meth)acrylic acid ester copolymer is the island, or in the case of a sea-island structure in which the (meth)acrylic acid ester copolymer is the sea, and the cured epoxy resin is the island, the sea portion can be made small.
[0099] The (meth)acrylic acid ester copolymer may be a modified product in which the above-mentioned polar group is introduced into a part of the first polymer segment or the second polymer segment.
[0100] The Tg of the first polymer portion contained in the above (meth)acrylic acid ester copolymer is 10°C or lower, and may be in the range of -150°C or higher and 10°C or lower, or in the range of -130°C or higher and 0°C or lower, or in the range of -110°C or higher and -10°C or lower.
[0101] The Tg of the first polymer portion is calculated according to the following formula based on the Tg(K) of each homopolymer described in "POLYMERHANDBOOK, Third Edition" (published by John Wiley & Sons, Inc.). 1 / Tg(K)=W1 / Tg1+W2 / Tg2+····+W n / Tg n W n : Mass fraction of each monomer Tgn : Tg(K) of the homopolymer of each monomer, and publicly available values such as those in the Polymer Handbook (3rd Ed., J. Brandrup and EH Immergut, WILEY INTERSCIENCE) may be used. The same applies to the Tg of the second polymer portion described below.
[0102] The first polymer portion contained in the (meth)acrylic acid ester copolymer may be a homopolymer or a copolymer, but is preferably a homopolymer. The monomer component and polymer component constituting the first polymer portion may be a monomer component and polymer component capable of obtaining a first polymer portion having a Tg in a predetermined range, and examples thereof include acrylate monomers such as butyl acrylate, 2-ethylhexyl acrylate, isononyl acrylate, and methyl acrylate, other monomers such as vinyl acetate, acetal, and urethane, polar group-containing monomers containing the above-mentioned polar groups, and copolymers such as EVA.
[0103] The Tg of the second polymer portion contained in the above (meth)acrylic acid ester copolymer is 20°C or higher, and may be in the range of 20°C or higher and 150°C or lower, 30°C or higher and 150°C or lower, or 40°C or higher and 150°C or lower.
[0104] The second polymer portion contained in the (meth)acrylic acid ester copolymer may be a homopolymer or a copolymer, but is preferably a homopolymer. The monomer component constituting the second polymer portion may be any monomer component capable of obtaining a second polymer portion having a Tg in a predetermined range, and examples thereof include acrylic acid ester monomers such as methyl methacrylate, other monomers such as acrylamide, styrene, vinyl chloride, amide, acrylonitrile, cellulose acetate, phenol, urethane, vinylidene chloride, methylene chloride, and methacrylonitrile, and polar group-containing monomers containing the above-mentioned polar groups.
[0105] A specific example of the (meth)acrylic acid ester copolymer having the above-mentioned first polymer portion and second polymer portion is the above-mentioned MMA-BA-MMA copolymer.
[0106] The content of the acrylic resin may be, for example, 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, 7 parts by mass or more, or 10 parts by mass or more, when the resin component contained in the first adhesive layer is taken as 100 parts by mass. If the content of the acrylic resin is too small, the adhesion of the first adhesive layer to the substrate and the adhesion after foaming and curing may be reduced. On the other hand, the content of the acrylic resin may be, for example, 60 parts by mass or less, 50 parts by mass or less, 40 parts by mass or less, 35 parts by mass or less, or 30 parts by mass or less, when the resin component contained in the first adhesive layer is taken as 100 parts by mass. If the content of the acrylic resin is too high, the contents of the first epoxy resin and the second epoxy resin become relatively small, and it may be difficult to balance the blocking resistance, the adhesion of the first adhesive layer to the substrate, and the adhesion after foaming and curing.
[0107] (iii) Hardener The curing agent in the present disclosure is appropriately selected according to the type of the first curing adhesive. When the first curing adhesive is, for example, an epoxy resin adhesive, the curing agent may be a curing agent generally used in epoxy resin adhesives. The curing agent is preferably solid at 23°C. A curing agent that is solid at 23°C can extend the storage stability (pot life) compared with a curing agent that is liquid at 23°C. The curing agent may be a latent curing agent. The curing agent may be a curing agent that undergoes a curing reaction by heat, or may be a curing agent that undergoes a curing reaction by light. The curing agent may be used alone or in combination of two or more types.
[0108] The reaction initiation temperature of the curing agent is, for example, 110°C or higher, and may be 130°C or higher. If the reaction initiation temperature is too low, the reaction starts early, and curing occurs in a state where the flexibility and fluidity of the resin component is low, and uniform curing may be difficult to occur. On the other hand, the reaction initiation temperature of the curing agent is, for example, 200°C or lower. If the reaction initiation temperature is too high, the resin component may deteriorate. In addition to the epoxy resin, when a resin with high heat resistance, such as a phenolic resin, is used, the resin component is less deteriorated, so the reaction initiation temperature of the curing agent may be, for example, 300°C or lower. The reaction initiation temperature of the curing agent can be determined by differential scanning calorimetry (DSC).
[0109] Specific examples of the curing agent include imidazole-based curing agents, phenol-based curing agents, amine-based curing agents, acid anhydride-based curing agents, isocyanate-based curing agents, and thiol-based curing agents.
[0110] Examples of imidazole-based curing agents include imidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-isopropylimidazole, 2-phenylimidazole, carboxylates of imidazole compounds, and adducts with epoxy compounds. It is also preferable that the imidazole-based curing agent has a hydroxyl group. Since crystallization occurs due to hydrogen bonds between hydroxyl groups, the reaction initiation temperature tends to be high.
[0111] Examples of the phenol-based curing agent include phenol resins. Examples of the phenol resin include resol-type phenol resins and novolac-type phenol resins. From the viewpoint of the adhesion of the first adhesive layer to the substrate, phenol-type novolac resins having a Tg of 110° C. or less are particularly preferred. In addition, a phenol-based curing agent and an imidazole-based curing agent may be used in combination. In this case, it is preferred to use an imidazole-based curing agent as a curing catalyst.
[0112] The phenol resin is preferably a biphenyl type from the viewpoint of heat resistance. The phenol resin may be a resin in which the phenol nucleus is modified. By modifying the phenol nucleus, for example, the heat resistance can be further improved.
[0113] Examples of the amine-based curing agent include aliphatic amines, aromatic amines, alicyclic amines, and polyamidoamines. Examples of the aliphatic amines include diethylenetriamine (DETA), triethylenetetramine (TETA), and metaxylylenediamine (MXDA). Examples of the aromatic amines include diaminodiphenylmethane (DDM), m-phenylenediamine (MPDA), and diaminodiphenylsulfone (DDS). Examples of the amine-based curing agent include dicyandiamide-based curing agents such as dicyandiamide (DICY), organic acid dihydrazide-based curing agents, amine adduct-based curing agents, and ketimine-based curing agents.
[0114] Examples of the acid anhydride-based curing agent include alicyclic acid anhydrides (liquid acid anhydrides) and aromatic acid anhydrides. Examples of the alicyclic acid anhydrides (liquid acid anhydrides) include hexahydrophthalic anhydride (HHPA), methyltetrahydrophthalic anhydride (MTHPA), etc. Examples of the aromatic acid anhydrides include trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), benzophenonetetracarboxylic acid (BTDA), etc.
[0115] The isocyanate-based curing agent may, for example, be a blocked isocyanate.
[0116] Examples of the thiol-based curing agent include ester-bonded thiol compounds, aliphatic ether-bonded thiol compounds, and aromatic ether-bonded thiol compounds.
[0117] The content of the curing agent is, for example, 1 part by mass or more and 40 parts by mass or less, when the resin component contained in the first adhesive layer is 100 parts by mass. For example, when an imidazole-based curing agent is used as the main component as the curing agent, the content of the curing agent is, for example, 1 part by mass or more and 15 parts by mass or less, when the resin component contained in the first adhesive layer is 100 parts by mass. On the other hand, when a phenol-based curing agent is used as the main component as the curing agent, the content of the curing agent is, for example, 5 parts by mass or more and 40 parts by mass or less, when the resin component contained in the first adhesive layer is 100 parts by mass. In addition, using an imidazole-based curing agent or a phenol-based curing agent as the main component as the curing agent means that the mass ratio of the imidazole-based curing agent or the phenol-based curing agent is the highest in the curing agent.
[0118] (b) Foaming agent The foaming agent contained in the first adhesive layer in the present disclosure may be a foaming agent generally used in the adhesive layer of an adhesive sheet. The foaming agent may be a foaming agent that undergoes a foaming reaction due to heat or a foaming agent that undergoes a foaming reaction due to light.
[0119] The foaming start temperature of the foaming agent is preferably equal to or higher than the softening temperature of the base of the curable adhesive such as epoxy resin, and equal to or lower than the activation temperature of the curing reaction of the base of the curable adhesive such as epoxy resin. The foaming start temperature of the foaming agent is, for example, 70°C or higher, and may be 100°C or higher. If the foaming start temperature is too low, the reaction starts early, and foaming occurs in a state where the flexibility and fluidity of the resin component are low, and it may be difficult to generate uniform foaming. On the other hand, the foaming start temperature of the foaming agent is, for example, 210°C or lower. If the foaming start temperature is too high, the resin component may deteriorate.
[0120] The softening temperature of the base material of the curable adhesive such as an epoxy resin is measured by the ring and ball method specified in JIS K7234:1986.
[0121] Examples of the foaming agent include organic foaming agents and inorganic foaming agents. Examples of the organic foaming agent include azo foaming agents such as azodicarbonamide (ADCA), azobisformamide, and azobisisobutyronitrile, fluorinated alkane foaming agents such as trichloromonofluoromethane, hydrazine foaming agents such as paratoluenesulfonylhydrazide, semicarbazide foaming agents such as p-toluenesulfonylsemicarbazide, triazole foaming agents such as 5-morpholyl-1,2,3,4-thiatriazole, and N-nitroso foaming agents such as N,N-dinitrosoterephthalamide. Examples of the inorganic foaming agent include ammonium carbonate, ammonium hydrogen carbonate, ammonium nitrite, ammonium borohydride, and azides.
[0122] Alternatively, a microcapsule type foaming agent may be used as the foaming agent. The microcapsule type foaming agent preferably has a core made of a thermal expansion agent such as a hydrocarbon and a shell made of a resin such as an acrylonitrile copolymer.
[0123] The average particle size of the foaming agent may be, for example, 7 μm or more, 10 μm or more, 13 μm or more, or 17 μm or more. On the other hand, the average particle size of the foaming agent is preferably equal to or less than the average thickness of the first adhesive layer, and may be, for example, 44 μm or less, 30 μm or less, or 24 μm or less.
[0124] The average particle size of the foaming agent is the particle size at 50% of the cumulative value in the particle size distribution obtained by the laser diffraction scattering method. In addition, when measuring the average particle size of the foaming agent, the first adhesive layer is dissolved in a solvent to separate the foaming agent. The solvent is not particularly limited as long as it can dissolve components other than the foaming agent contained in the first adhesive layer, and is appropriately selected depending on the type of the first curable adhesive contained in the first adhesive layer, and for example, a solvent used in the adhesive composition used to form the first adhesive layer can be used. Specifically, methyl ethyl ketone, ethyl acetate, toluene, etc. can be used.
[0125] The content of the foaming agent may be, for example, 0.5 parts by mass or more, 2 parts by mass or more, 3 parts by mass or more, 4 parts by mass or more, or 5 parts by mass or more, based on 100 parts by mass of the resin component contained in the first adhesive layer. On the other hand, the content of the foaming agent may be, for example, 25 parts by mass or less, 20 parts by mass or less, or 15 parts by mass or less, based on 100 parts by mass of the resin component contained in the first adhesive layer. If the content of the foaming agent is too small, the expansion ratio of the first adhesive layer is small, so that the gap between the two members cannot be sufficiently filled, and the adhesiveness after foaming and curing may decrease. On the other hand, if the content of the foaming agent is too large, the content of the first curable adhesive is relatively small, so that the cohesive force decreases, and the adhesiveness after foaming and curing may decrease.
[0126] (c) Other ingredients In the present disclosure, for example, when the first curable adhesive is an epoxy resin adhesive, the first adhesive layer may contain only an epoxy resin and an acrylic resin as the resin component, or may further contain other resins such as urethane resins.
[0127] The total ratio of the first epoxy resin, the second epoxy resin and the acrylic resin to the resin components contained in the first adhesive layer is, for example, 70 mass% or more, optionally 80 mass% or more, optionally 90 mass% or more, or optionally 100 mass%.
[0128] The content of the resin component in the first adhesive layer is, for example, 60% by mass or more, optionally 70% by mass or more, optionally 80% by mass or more, or optionally 90% by mass or more.
[0129] The first adhesive layer may contain, as necessary, for example, a silane coupling agent, a filler, an antioxidant, a light stabilizer, an ultraviolet absorber, a lubricant, a plasticizer, an antistatic agent, a crosslinking agent, and a colorant. Examples of the silane coupling agent include epoxy-based silane coupling agents. Examples of the filler include inorganic fillers such as calcium carbonate, aluminum hydroxide, magnesium hydroxide, antimony trioxide, zinc borate, molybdenum compounds, and titanium dioxide. Examples of the antioxidant include phenol-based antioxidants and sulfur-based antioxidants.
[0130] (3) Configuration of the first adhesive layer The thickness of the first adhesive layer is not particularly limited, but is preferably equal to or greater than the average particle size of the foaming agent. The thickness of the first adhesive layer is, for example, 10 μm or more, may be 15 μm or more, or may be 20 μm or more. If the first adhesive layer is too thin, there is a possibility that the adhesion to the substrate and the adhesiveness after foaming and curing cannot be sufficiently obtained. On the other hand, the thickness of the first adhesive layer is, for example, 200 μm or less, may be 150 μm or less, or may be 100 μm or less. If the first adhesive layer is too thick, there is a possibility that the surface quality will deteriorate.
[0131] Here, the thickness of the first adhesive layer is a value measured from a cross section of the adhesive sheet in the thickness direction observed with a transmission electron microscope (TEM), a scanning electron microscope (SEM) or a scanning transmission electron microscope (STEM), and is the average value of the thicknesses at 10 randomly selected points. The same method of measuring the average thickness of other layers of the foamable adhesive sheet is also applied.
[0132] The first adhesive layer can be foamed at an expansion ratio of, for example, 1.5 times or more and 15 times or less. The expansion ratio may be, for example, 3.5 times or more, 4 times or more, or 4.5 times or more. The expansion ratio may be, for example, 9 times or less, 8.5 times or less, or 8 times or less. If the expansion ratio is too small, the gap between the two members cannot be filled sufficiently, and the adhesiveness after foaming and curing may decrease. If the expansion ratio is too large, the porosity of the first adhesive layer after foaming and curing may increase, and the adhesiveness after foaming and curing may decrease.
[0133] Here, the expansion ratio is calculated by the following formula. Expansion ratio (times) = thickness of the first adhesive layer after foaming and hardening / thickness of the first adhesive layer before foaming and hardening
[0134] The first adhesive layer may be a continuous layer or a discontinuous layer. Examples of the discontinuous layer include a pattern such as a stripe or a dot. The surface of the first adhesive layer may have an uneven shape such as an embossed shape.
[0135] The first adhesive layer can be formed, for example, by applying an adhesive composition containing the above-mentioned first curable adhesive and a foaming agent, etc., and then removing the solvent. Examples of the application method include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, bar coating, wire bar coating, die coating, lip coating, dip coating, etc.
[0136] The adhesive composition may or may not contain a solvent. In this specification, the solvent is used in a broad sense including not only a strict solvent (a solvent that dissolves a solute) but also a dispersion medium. The solvent contained in the adhesive composition is volatilized and removed when the adhesive composition is applied and dried to form a first adhesive layer.
[0137] The adhesive composition can be obtained by mixing the above-mentioned components and kneading and dispersing them as necessary.As a mixing and dispersing method, a general kneading and dispersing machine, for example, a two-roll mill, a three-roll mill, a pebble mill, a tron mill, a Szegvari attritor, a high-speed impeller dispersing machine, a high-speed stone mill, a high-speed impact mill, a disperser, a high-speed mixer, a ribbon blender, a co-kneader, an intensive mixer, a tumbler, a blender, a disperser, a homogenizer, or an ultrasonic dispersing machine can be used.
[0138] 3.Second adhesive layer The second adhesive layer of the present disclosure is disposed on the surface of the substrate opposite the first adhesive layer, contains a second curable adhesive, and is substantially free of a blowing agent.
[0139] (1) Physical properties of the second adhesive layer The second adhesive layer of the present disclosure is preferably substantially non-tacky. The tack of the second adhesive layer is similar to the tack of the first adhesive layer.
[0140] (2) Material for the second adhesive layer (a) a second curable adhesive The second curable adhesive contained in the second adhesive layer in the present disclosure is the same as the first curable adhesive used in the first adhesive layer.
[0141] (b) Other ingredients The other components contained in the second adhesive layer in the present disclosure are similar to the other components used in the first adhesive layer.
[0142] The second adhesive layer may contain soft particles. When the second adhesive layer contains soft particles, the slope of the approximate straight line tends to be smaller. Therefore, the slope of the approximate straight line can be easily adjusted to be within a predetermined range.
[0143] The soft particles include, for example, hollow particles obtained by foaming a foaming agent so as to have a cavity inside. The hollow particles are preferably hollow particles obtained by foaming a microcapsule type foaming agent. The microcapsule type foaming agent is the same as the microcapsule type foaming agent used in the first adhesive layer.
[0144] The soft particles may be non-metallic particles having flexibility, such as rubber particles and resin particles. Examples of the resin particles include melamine resin particles, acrylic resin particles, acrylic-styrene copolymer particles, polycarbonate particles, polyethylene particles, polystyrene particles, polyvinyl chloride particles, cross-linked urethane resin particles, and silicone resin particles.
[0145] The second adhesive layer does not substantially contain a foaming agent. The second adhesive layer does not substantially contain a foaming agent means that the content of the foaming agent in the second adhesive layer is 1% by mass or less. The content of the foaming agent in the second adhesive layer is preferably 0.5% by mass or less, more preferably 0% by mass. The foaming agent is the same as the foaming agent used in the first adhesive layer.
[0146] (3) Configuration of the second adhesive layer The thickness of the second adhesive layer is the same as that of the first adhesive layer. If the thickness of the second adhesive layer is too thick, the gap between the two components cannot be filled with the foamable adhesive sheet after foaming and curing, and the adhesiveness after foaming and curing may decrease.
[0147] The second adhesive layer may be a continuous layer or a discontinuous layer. The surface of the second adhesive layer may have an uneven shape such as an embossed shape.
[0148] The method for forming the second adhesive layer is the same as the method for forming the first adhesive layer.
[0149] 4.Base material The substrate in the present disclosure is, for example, a member that supports the first adhesive layer and the second adhesive layer.
[0150] The substrate in the present disclosure is preferably insulating. The substrate is preferably in the form of a sheet. The substrate may have a single layer structure or a multi-layer structure. The substrate may or may not have a porous structure inside.
[0151] Examples of the substrate include a resin substrate and a nonwoven fabric.
[0152] Examples of the resin contained in the resin substrate include polyester resin, polycarbonate, polyarylate, polyurethane, polyamide resin, polyimide resin, polysulfone resin, polyether ketone resin, polyphenylene sulfide (PPS), modified polyphenylene oxide, etc. Examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate, polyethylene naphthalate (PEN), and aromatic polyester. Examples of the polyamide resin include polyamide and polyether amide. Examples of the polyimide resin include polyimide, polyether imide, and polyamide imide. Examples of the polysulfonic acid resin include polysulfone and polyether sulfone. Examples of the polyether ketone resin include polyether ketone and polyether ether ketone. In addition, liquid crystal polymer (LCP) may be used as the resin.
[0153] The glass transition temperature of the resin is, for example, 80° C. or higher, may be 140° C. or higher, or may be 200° C. or higher.
[0154] Examples of the nonwoven fabric include nonwoven fabrics containing fibers such as cellulose fibers, polyester fibers, nylon fibers, aramid fibers, polyphenylene sulfide fibers, liquid crystal polymer fibers, glass fibers, metal fibers, and carbon fibers.
[0155] The substrate may be subjected to a surface treatment in order to enhance adhesion to the first adhesive layer or the second adhesive layer.
[0156] The thickness of the substrate is not particularly limited, and may be, for example, 2 μm or more, 5 μm or more, or 9 μm or more. The thickness of the substrate is, for example, 200 μm or less, 100 μm or less, or 50 μm or less.
[0157] 5. First and second intermediate layers The foamable adhesive sheet of the present disclosure may have a first intermediate layer between the substrate and the first adhesive layer. The foamable adhesive sheet of the present disclosure may have a second intermediate layer between the substrate and the second adhesive layer. By disposing the first intermediate layer or the second intermediate layer, the adhesion of the first adhesive layer or the second adhesive layer to the substrate can be improved. Furthermore, by disposing the first intermediate layer or the second intermediate layer, for example, it is possible to relieve the stress applied to the bent portion when the foamable adhesive sheet is folded, or to relieve the stress applied to the cut portion when the foamable adhesive sheet is cut. As a result, it is possible to suppress lifting or peeling of the first adhesive layer or the second adhesive layer from the substrate when the foamable adhesive sheet is bent or cut.
[0158] For example, in the foamable adhesive sheet 10 shown in Fig. 7, a first intermediate layer 4 is disposed between the substrate 2 and the first adhesive layer 1, and a second intermediate layer 5 is disposed between the substrate 2 and the second adhesive layer 3. Note that, although the foamable adhesive sheet 10 in Fig. 7 has both the first intermediate layer 4 and the second intermediate layer 5, it may have only one of them.
[0159] The foamable adhesive sheet may have at least one of a first intermediate layer and a second intermediate layer; for example, it may have only the first intermediate layer disposed between the substrate and the first adhesive layer, or it may have only the second intermediate layer disposed between the substrate and the second adhesive layer, or it may have both the first intermediate layer disposed between the substrate and the first adhesive layer, and the second intermediate layer disposed between the substrate and the second adhesive layer.
[0160] The material contained in the first intermediate layer and the second intermediate layer is not particularly limited as long as it can increase the adhesion between the substrate and the first adhesive layer or the second adhesive layer and can relieve stress, and is appropriately selected depending on the materials of the substrate, the first adhesive layer, and the second adhesive layer, etc. Examples include polyester, polyvinyl chloride, polyvinyl acetate, polyurethane, a polymer obtained by copolymerizing at least two or more of these, a crosslinked product thereof, and a mixture thereof.
[0161] The crosslinked body is a crosslinked body obtained by crosslinking the above-mentioned resin with a curing agent. Examples of the curing agent include isocyanate-based curing agents. In addition, for example, when the reactive group / NCO equivalent is 1, it is preferable to add the isocyanate-based curing agent in a ratio of 0.5% by mass or more and 20% by mass or less to the resin.
[0162] In particular, the first intermediate layer and the second intermediate layer preferably contain a crosslinked resin. The crosslinked resin is one that does not melt even at high temperatures. This can improve the adhesive strength at high temperatures, i.e., heat resistance.
[0163] The thickness of the first intermediate layer and the second intermediate layer is not particularly limited, but may be, for example, 0.1 μm or more, may be 0.5 μm or more, or may be 1 μm or more. If the first intermediate layer or the second intermediate layer is too thin, the effect of suppressing peeling of the first adhesive layer or the second adhesive layer from the substrate when the foamable adhesive sheet is bent or cut may not be sufficiently obtained. On the other hand, the thickness of the first intermediate layer and the second intermediate layer may be, for example, 4 μm or less, or may be 3.5 μm or less. Since the first intermediate layer and the second intermediate layer themselves usually do not have high heat resistance, if the first intermediate layer or the second intermediate layer is too thick, the heat resistance (adhesive strength at high temperatures) may decrease.
[0164] The first intermediate layer and the second intermediate layer can be formed, for example, by applying a resin composition and removing the solvent. Examples of the application method include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, bar coating, wire bar coating, die coating, lip coating, and dip coating.
[0165] 7. Foam adhesive sheet The thickness of the foamable adhesive sheet in the present disclosure is, for example, 10 μm or more, and may be 20 μm or more, whereas the thickness of the foamable adhesive sheet is, for example, 1000 μm or less, and may be 200 μm or less.
[0166] The use of the foamable adhesive sheet in the present disclosure is not particularly limited. The foamable adhesive sheet in the present disclosure can be used, for example, when two members are bonded together by disposing the foamable adhesive sheet between the two members, foaming and curing the first adhesive layer of the foamable adhesive sheet, and curing the second adhesive layer. Specifically, the foamable adhesive sheet in the present disclosure is used to bond a stator core and a coil in a stator that constitutes a motor.
[0167] The method for producing the foamable adhesive sheet of the present disclosure is not particularly limited and may be appropriately selected depending on the layer structure of the foamable adhesive sheet.
[0168] B. Method of Manufacturing the Article The method for manufacturing an article according to the present disclosure includes a placement step of placing the above-mentioned foamable adhesive sheet between a first member and a second member, and a bonding step of foaming and curing the foamable adhesive sheet to bond the first member and the second member.
[0169] 8(a)-(b) are process diagrams showing an example of a method for manufacturing an article according to the present disclosure. First, as shown in FIG. 8(a), a foamable adhesive sheet 10 is disposed between a first member 20a and a second member 20b. Next, as shown in FIG. 8(b), the first adhesive layer of the foamable adhesive sheet 10 is foamed and cured by heating or the like, and the second adhesive layer is cured. The first member 20a and the second member 20b are bonded (joined) by the foamed and cured adhesive sheet 11. This results in an article 100 in which the adhesive sheet 11 is disposed between the first member 20a and the second member 20b.
[0170] The method for producing the article according to the present disclosure will now be described.
[0171] 1. Foam adhesive sheet The foamable adhesive sheet used in the method for producing an article according to the present disclosure is the same as the foamable adhesive sheet described above.
[0172] 2.Placement process In the disposing step in the present disclosure, the method of disposing the adhesive sheet between the first member and the second member is not particularly limited. For example, there may be mentioned a method of inserting a foamable adhesive sheet into the gap between the first member and the second member, a method of disposing a foamable adhesive sheet in a hole or groove of the first member, and then inserting the second member into the gap after disposing the foamable adhesive sheet in the hole or groove of the first member, and a method of inserting the second member on which the foamable adhesive sheet is disposed, into the hole or groove of the first member.
[0173] The material and shape of the first member and the second member are not particularly limited and may be appropriately selected depending on the application. Examples of the first member and the second member include a stator core and a coil in a stator that constitutes a motor.
[0174] 3.Gluing process In the bonding step of the present disclosure, the method of foaming and curing the first adhesive layer of the foamable adhesive sheet and the method of curing the second adhesive layer can be, for example, heating or light irradiation. Among them, it is preferable to foam and cure the first adhesive layer and cure the second adhesive layer by heating. The method by heating can be applied even when the first member and the second member do not have transparency, such as a metal member.
[0175] The heating conditions are appropriately set depending on the type of the first curable adhesive and foaming agent contained in the first adhesive layer, the type of the second curable adhesive contained in the second adhesive layer, the type of the base material, etc. The heating temperature is, for example, 130° C. or higher and 200° C. or lower. The heating time is, for example, 3 minutes or higher and 3 hours or lower.
[0176] The present disclosure is not limited to the above-mentioned embodiment. The above-mentioned embodiment is merely an example, and any embodiment that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0177] [material] The components used in the adhesive composition are shown below. Epoxy resin A: Bisphenol A phenoxy type, solid at room temperature, epoxy equivalent: 7500~8500g / eq, Mw50,000, bifunctional Epoxy resin B: Bisphenol A type, solid at room temperature, epoxy equivalent 2400-3300g / eq, softening temperature 144℃, Mw3,800, bifunctional Epoxy resin C: Bisphenol A novolac type, solid at room temperature, epoxy equivalent 200-220g / eq, softening temperature 70℃, multifunctional Acrylic resin: PMMA-PBuA-PMMA (some acrylamide groups), Tg-20℃, 120℃, Mw150,000 Hardener: α-(hydroxy(or dihydroxy)phenylmethyl)-ω-hydropoly[biphenyl-4,4'-diylmethylene(hydroxy(or dihydroxy)phenylenemethylene)] Curing catalyst: 2-phenyl-4,5-dihydroxymethylimidazole, average particle size: 3μm, melting point: 230℃, reaction start temperature: 145℃~155℃, active region: 155℃~173℃) Foaming agent: Thermally expandable microcapsules, average particle size 10μm~16μm, expansion start temperature 123℃~133℃, maximum expansion temperature 168℃~178℃, core: hydrocarbon, shell: thermoplastic polymer Hollow particles: Microballoons made by expanding thermally expandable microcapsules, average particle size 15μm~25μm Solvent: Methyl ethyl ketone
[0178] [Examples 1 to 6, Comparative Example 1] A polyethylene naphthalate (PEN) film (thickness 100 μm) was used as the substrate. A polyester polymer and a curing agent (polyisocyanate) were diluted with methyl ethyl ketone (MEK) so that the solid content was 15 mass % to prepare a resin composition. The resin composition was applied to one surface of the substrate using a bar coater and dried in an oven at 100° C. for 1 minute to form a first intermediate layer. Furthermore, a second intermediate layer was formed on the other surface of the substrate in the same manner as the first intermediate layer.
[0179] Next, the adhesive composition shown in Table 1 below was applied to the surface of the first intermediate layer opposite the substrate using an applicator so that the thickness after application was 58 μm. Then, the surface was dried in an oven at 100° C. for 3 minutes to form a first adhesive layer. Furthermore, the adhesive composition shown in Table 1 below was applied to the surface of the second intermediate layer opposite the substrate using an applicator so that the thickness after application was 48 μm. Then, the surface was dried in an oven at 100° C. for 3 minutes to form a second adhesive layer. This resulted in a foamable adhesive sheet in which the first adhesive layer, the first intermediate layer, the substrate, the second intermediate layer, and the second adhesive layer were arranged in this order.
[0180] [evaluation] (1) Shear adhesive strength test method (1-1) First adhesive layer after foaming and hardening The adhesive composition shown in Table 1 below was applied to a 38 μm thick silicone-treated polyethylene terephthalate (PET) separator using an applicator so that the thickness after application was 58 μm. It was then dried in an oven at 100° C. for 3 minutes to form a first adhesive layer.
[0181] The first adhesive layer after foaming and curing was subjected to the shear bond strength test method as described in the above section "A. Foamable adhesive sheet 1. Physical properties of foamable adhesive sheet" to measure the shear bond strength. In addition, the slope of the approximation line in the section from 3% strain to 5% strain in the stress-strain curve was determined. In the shear bond strength test method, the spacer thickness was 180 μm. The foaming and curing conditions were 160°C and 8.5 minutes (3.5 minutes for temperature increase and 5 minutes for retention) using a heat press machine.
[0182] (1-2) Second adhesive layer after curing The adhesive composition shown in Table 1 below was applied to a 38 μm thick silicone-treated polyethylene terephthalate (PET) separator using an applicator so that the thickness after application was 48 μm. The composition was then dried in an oven at 100° C. for 3 minutes to form a second adhesive layer.
[0183] The shear adhesive strength test method was carried out on the second adhesive layer after curing as described in the above section "A. Foamable adhesive sheet 1. Physical properties of foamable adhesive sheet" to measure the shear adhesive strength. In addition, the slope of the approximation line in the stress-strain curve from 3% strain to 5% strain was determined. In the shear adhesive strength test method, the spacer thickness was 35 μm. The curing conditions were 160°C, 8.5 minutes (3.5 minutes for temperature rise, 5 minutes for holding) using a heat press machine.
[0184] (1-3) Foamable adhesive sheet after foaming and curing The foamable adhesive sheet after foaming and curing was subjected to the shear bond strength test method as described in the above section "A. Foamable adhesive sheet 1. Physical properties of foamable adhesive sheet" to measure the shear bond strength. The fracture surface of the test piece was also visually observed. In the shear bond strength test method, the spacer thickness was 338 μm. The foaming and curing conditions were 160°C and 8.5 minutes (3.5 minutes for temperature increase and 5 minutes for retention) using a heat press machine.
[0185] (2) Adhesion A cross-cut test was performed three times on the surface of the second adhesive layer of the foamable adhesive sheet after foaming and curing, conforming to JIS K5600-5-6:1999, and the number of squares that peeled off was counted. The cut interval was 1 mm. The tape used was Nitto Denko Corporation's adhesive tape No. 31B. The tape peeling conditions were peeling speed: 3 m / s to 5 m / s, peeling angle: approximately 60°.
[0186] [Table 1]
[0187] [Table 2]
[0188] In Examples 1 to 6, the slope of the approximate straight line in the stress-strain curve for the cured second adhesive layer was within a predetermined range, and the fracture mode was cohesive failure of the first adhesive layer, so the adhesion of the cured second adhesive layer to the substrate was good. On the other hand, in Comparative Example 1, the slope of the approximate straight line in the stress-strain curve for the cured second adhesive layer was large, so the adhesion of the cured second adhesive layer to the substrate was poor.
[0189] The present disclosure provides the following [1] to [3]. [1] A foamable adhesive sheet having a first adhesive layer, a substrate, and a second adhesive layer in this order, The first adhesive layer contains a first curable adhesive and a foaming agent, the second adhesive layer comprises a second curable adhesive and does not contain a foaming agent; when the foamable adhesive sheet after foaming and curing is subjected to a tensile shear adhesive strength test, the failure mode is cohesive failure of the first adhesive layer after foaming and curing, A foamable adhesive sheet, in which in a stress-strain curve obtained when the second adhesive layer after curing is subjected to a tensile shear adhesive strength test method, the slope of the approximation line in the section from 3% strain to 5% strain is 0.20 MPa or less. [2] The foamable adhesive sheet according to [1], wherein the difference between the slope of the approximation line in the section from 3% strain to 5% strain in a stress-strain curve obtained when the first adhesive layer after foaming and curing is subjected to a tensile shear adhesive strength test method and the slope of the approximation line in the section from 3% strain to 5% strain in a stress-strain curve obtained when the second adhesive layer after curing is subjected to a tensile shear adhesive strength test method is 0.20 MPa or less. [3] A step of placing the foamable adhesive sheet according to [1] or [2] between a first member and a second member; a bonding step of foaming and curing the foamable adhesive sheet to bond the first member and the second member; A method for producing an article having the following structure: [Explanation of symbols]
[0190] 1 … First adhesive layer 2...Base material 3...Second adhesive layer 4 … First middle layer 5…Second intermediate layer 10... Foam adhesive sheet 11 ... Adhesive sheet 20a … First member 20b … second member 100 … Goods
Claims
1. A foamable adhesive sheet having a first adhesive layer, a substrate, and a second adhesive layer in this order, The first adhesive layer comprises a first curable adhesive and a foaming agent; the second adhesive layer comprises a second curable adhesive and does not contain a blowing agent; when the foamable adhesive sheet after foaming and curing is subjected to a tensile shear adhesive strength test, the failure mode is cohesive failure of the first adhesive layer after foaming and curing; A foamable adhesive sheet, in which in a stress-strain curve obtained when the second adhesive layer after curing is subjected to a tensile shear adhesive strength test method, the slope of the approximation line in the section from 3% strain to 5% strain is 0.20 MPa or less.
2. 2. The foamable adhesive sheet according to claim 1, wherein the difference between the slope of the approximation line in the section from 3% strain to 5% strain in a stress-strain curve obtained when a tensile shear adhesive strength test method is performed on the first adhesive layer after foaming and curing, and the slope of the approximation line in the section from 3% strain to 5% strain in a stress-strain curve obtained when a tensile shear adhesive strength test method is performed on the second adhesive layer after curing, is 0.20 MPa or less.
3. a step of placing the foamable adhesive sheet according to claim 1 or 2 between a first member and a second member; a bonding step of foaming and curing the foamable adhesive sheet to bond the first member and the second member; A method for producing an article having the following structure:
Citation Information
Patent Citations
Heating expansion sheet
JP2022178658A
Foamable adhesive sheet and method for manufacturing article
JP2023052744A
Adhesive tape, article, motor, and method for producing article
WO2015190235A1
Machining center
JP1987074540A
Insulation sheet for rotary electric machine
JP2021197888A