Adhesive sheet, laminate member using the adhesive sheet and method for producing the same, and method for peeling the same
The adhesive sheet with a hot melt adhesive layer on both sides of a metal layer, containing silane modified substances, addresses adhesion challenges in bonding glass and plastic materials, ensuring excellent heat, cold, and water resistance, suitable for laminated members.
Patent Information
- Application Number
- JP2023079381
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing adhesive technologies for bonding glass-based and plastic-based materials using electromagnetic induction heating face challenges with adhesion, processability, heat resistance, cold resistance, and water resistance, particularly when using silane coupling agents, which are difficult to apply and provide insufficient adhesion.
An adhesive sheet with a hot melt adhesive layer on both sides of a metal layer, containing silane modified substances, is used to bond glass and plastic materials. The adhesive layer can be made of either a silane modified hot melt adhesive or a polyolefin hot melt adhesive, with specific polymer and tackifier resin compositions, and includes a primer layer for enhanced adhesion.
The adhesive sheet provides excellent heat-resistant, cold-resistant, and water-resistant adhesion, maintaining bonding under various environmental conditions, suitable for laminated members composed of glass and plastic materials.
Smart Images

Figure 2024163616000001 
Figure 2024163616000002 
Figure 2024163616000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive sheet having a hot melt adhesive layer on both sides of a metal layer, a laminated member obtained by sandwiching the adhesive sheet between a glass-based material and a plastic material, heating the hot melt adhesive layer by electromagnetic induction heating, and bonding the glass-based material and the plastic material together, a method for producing the laminated member, and a method for peeling adherends from each other by heating the laminated member again by electromagnetic induction to soften or melt the hot melt adhesive layer. [Background technology]
[0002] Glass-based materials and plastic-based materials are sometimes used by bonding them together in solar cell components, housing construction materials, automobile components, etc. Examples of glass-based materials include float glass, tempered glass, heat-resistant glass, fireproof glass, design glass, colored glass, laminated glass, antique glass, and retro glass, while examples of plastic-based materials include polyethylene, polypropylene, polystyrene, polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, and polycarbonate.
[0003] Such laminated members made of glass-based materials and plastic-based materials are often used outdoors or inside vehicles, where they are susceptible to the effects of sunlight, temperature changes, rainfall, etc., and are therefore required to be able to maintain their adhesion in a variety of environments.
[0004] As a method for joining glass-based materials and plastic-based materials, electromagnetic induction heating using an adhesive sheet with a metal layer and hot melt adhesive has been considered. In the electromagnetic dielectric heating method, eddy currents are induced by high-frequency magnetic flux from an electromagnetic induction heating device, and the thermoplastic hot melt adhesive layer melts and bonds due to Joule heating of the metal layer.
[0005] As a method for manufacturing an adhesive sheet having a hot melt adhesive on both sides of such a metal layer, there is a method in which the hot melt adhesive is heated and melted to form a film and then coated on the metal surface, or a method in which a hot melt adhesive that has already been processed into a film is bonded to the metal using a primer or the like. An example of a method for coating a film on the metal surface is the extrusion lamination method, and an example of a method for processing into a film in advance is the inflation method. The hot melt adhesive is required to have processability to be formed into a film.
[0006] Patent Document 1 proposes a resin composition consisting of an epoxy resin and an amine or amide, or a resin composition consisting of an ethylene-vinyl acetate copolymer and a tackifier resin as an adhesive for bonding glass using electromagnetic induction heating, but these have issues with adhesion to glass.
[0007] Patent Document 2 proposes a method of applying a silane coupling agent to glass in bonding glass by electromagnetic induction heating, but the adhesion is still insufficient and there is a problem that the process of applying the silane coupling agent is added. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 6-206442 [Patent Document 2] JP 2022-134737 A Summary of the Invention [Problem to be solved by the invention]
[0009] In other words, the object of the present invention is to provide a thermoplastic hot melt adhesive that is suitable for bonding glass-based materials and plastic-based materials, has excellent processability into film, and has excellent heat-resistant adhesion, cold-resistant adhesion, water resistance, etc., and is capable of maintaining adhesion under various environments, and is suitable for bonding methods using electromagnetic induction heating, as well as an adhesive sheet using the thermoplastic hot melt adhesive, and a laminated member formed by bonding glass-based materials and plastic materials. [Means for solving the problem]
[0010] As a result of extensive research, the present inventors have found a solution to the above problems and have arrived at the present invention.
[0011] The present invention relates to an adhesive sheet having adhesive layers made of hot melt adhesives on both sides of a metal layer, in which a hot melt adhesive (C1) containing a silane modified product is disposed on one side of the metal layer, and either the hot melt adhesive (C1) containing a silane modified product or a polyolefin-based hot melt adhesive (excluding hot melt adhesives containing a silane modified product) (C2) is disposed on the other side.
[0012] The present invention relates to a hot melt adhesive comprising a silane-modified product, the hot melt adhesive comprising: 100 mass% of a silane-modified product (C1); 1 to 100 mass% of a polymer (x1); 0 to 99 mass% of a polymer (y1); and 0 to 30 mass% of a tackifier resin (z1); the polymer (x1) is at least one selected from the group consisting of silane-modified polyethylene, silane-modified ethylene-unsaturated ester copolymer, silane-modified ethylene-α-olefin copolymer, silane-modified ethylene-acrylic acid copolymer, and silane-modified ethylene-(meth)acrylic acid alkyl ester copolymer, The polymer (y1) relates to an adhesive sheet which is at least one selected from the group consisting of polyethylene, ethylene-unsaturated ester copolymer, ethylene-α-olefin copolymer, ethylene-acrylic acid copolymer, and ethylene-(meth)acrylic acid alkyl ester copolymer (excluding (x1)).
[0013] The present invention relates to a polyolefin-based hot melt adhesive, the adhesive comprising: 100 mass% of a polyolefin-based hot melt adhesive (C2); 50 to 100 mass% of a polymer (x2); and 0 to 50 mass% of a tackifier resin (z2); The adhesive sheet relates to the polymer (x2), which is at least one selected from the group consisting of polyolefins, acid-modified polyolefins, ethylene-unsaturated ester copolymers, ethylene-α-olefin copolymers, ethylene-acrylic acid copolymers, and ethylene-(meth)acrylic acid alkyl ester copolymers.
[0014] The present invention relates to an adhesive sheet having a primer layer between a metal layer and an adhesive layer made of a hot melt adhesive.
[0015] A laminated member having a glass-based material, the adhesive sheet, and a plastic-based material arranged in this order, the adhesive layer adjacent to the glass-based material is a layer made of the hot melt adhesive (C1); The present invention relates to a laminated member, wherein the adhesive layer adjacent to the plastic material is a layer made of at least one of the hot melt adhesive (C1) and the hot melt adhesive (C2).
[0016] The present invention relates to a method for producing the laminated member, in which heating is performed by electromagnetic induction to bond glass-based materials and plastic-based materials to adjacent hot melt adhesives.
[0017] The present invention relates to a method for peeling off glass-based and / or plastic-based materials from a laminated member by softening or melting a hot melt adhesive through heating by electromagnetic induction. Effect of the Invention
[0018] The present invention can provide a thermoplastic hot melt adhesive sheet suitable for bonding glass-based materials and plastic-based materials, which has excellent heat-resistant adhesion, cold-resistant adhesion, water resistance, etc., and can maintain adhesion under various environments, and which is suitable for bonding methods using electromagnetic induction heating, and a laminated member in which a glass-based material and a plastic material are bonded together can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The following describes in detail an embodiment of the present invention. However, the description of the components described below is an example of an embodiment of the present invention, and the present invention is not limited to these contents as long as it does not deviate from the gist of the present invention.
[0020] In this specification, any numerical range specified using "to" is intended to include the numerical values before and after "to" as the lower and upper limit values of the range. Unless otherwise noted, the various components appearing in this specification may be used independently as a single type or as a combination of two or more types. In this specification, the melt mass-flow rate (MFR) is the amount of melt that flows out in 10 minutes measured under conditions of 190° C. and a load of 2.16 kg in accordance with JIS K 7210-1:2014.
[0021] <Adhesive sheet> The adhesive sheet of the present invention has adhesive layers made of hot melt adhesives on both sides of a metal layer. A hot melt adhesive (C1) containing a silane-modified product is disposed on one side of the metal layer, and either the hot melt adhesive (C1) containing a silane-modified product or a polyolefin-based hot melt adhesive (excluding hot melt adhesives containing a silane-modified product) (C2) is disposed on the other side.
[0022] The metal layer in the present invention has a thickness of 1 μm to 1000 μm, preferably 5 μm to 100 μm, more preferably 5 μm to 50 μm, and functions as a conductive material for generating heat by electromagnetic induction heating. As such a metal, metals such as aluminum, nickel, zinc, lead, copper, iron, silver, or various alloys are preferable, and aluminum is the most preferable.
[0023] <Hot melt adhesive containing silane modified substance (C1)> The silane-modified hot melt adhesive (C1) of the present invention preferably contains 1 to 100 mass % of the polymer (x1), 0 to 99 mass % of the polymer (y1), and 0 to 30 mass % of the tackifier resin (z1).
[0024] (Polymer (x1)) The polymer (x1) in the present invention is at least one selected from the group consisting of silane-modified polyethylene, silane-modified polypropylene, silane-modified ethylene-unsaturated ester copolymer, silane-modified ethylene-α-olefin copolymer, silane-modified ethylene-acrylic acid copolymer, and silane-modified ethylene-alkyl (meth)acrylic acid ester copolymer. The polymer (x1) is obtained by reacting polyethylene, polypropylene, ethylene-unsaturated ester copolymer, ethylene-α-olefin copolymer, ethylene-acrylic acid copolymer, or ethylene-(meth)acrylic acid alkyl ester copolymer with an organic silane compound, and for example, a silane-grafted modified product can be obtained by extracting some atoms of polyethylene from polyethylene and an organic silane compound in the presence of a polymerization initiator at a temperature equal to or higher than the decomposition temperature of the polymerization initiator, and then reacting the polyethylene with the organic silane compound. In addition, when the organic silane compound has a functional group that can react with a reactive functional group, the silane modified product can be obtained by reacting the functional group with the reactive functional group in a conventional manner.
[0025] As the polyethylene, low density polyethylene (LDPE), linear low density polyethylene (LLDPE), very low density polyethylene (VLDPE), high density polyethylene (HDPE), polyethylene polymerized using a metallocene catalyst, etc. can be used. LDPE and LLDPE are preferably used, and LDPE is most preferably used. The melt mass flow rate of the polyethylene is preferably 0.1 to 500 g / 10 min, more preferably 1 to 100 g / 10 min, and even more preferably 2 to 50 g / 10 min. LDPE and LLDPE are preferred because they are easily processed into films, etc.
[0026] As the polypropylene, homo-polypropylene, random-polypropylene, block-polypropylene, polypropylene polymerized using a metallocene catalyst, etc. can be used. Random-polypropylene is preferred because it is easy to process, for example, into a film. The melt mass flow rate of the polypropylene is preferably from 0.1 to 500 g / 10 minutes, more preferably from 1 to 100 g / 10 minutes, and further preferably from 2 to 50 g / 10 minutes.
[0027] The ethylene-unsaturated ester copolymer is a copolymer of ethylene and an unsaturated ester such as vinyl acetate or vinyl propionate. Ethylene-vinyl acetate copolymer is preferred because it is easy to obtain a copolymer excellent in cold-resistant adhesion and water resistance. The melt mass flow rate of the ethylene-unsaturated ester copolymer is preferably from 0.1 to 500 g / 10 minutes, more preferably from 1 to 100 g / 10 minutes, and further preferably from 2 to 50 g / 10 minutes.
[0028] Ethylene-α-olefin copolymers are copolymers of ethylene and α-olefin monomers such as 1-butene, 1-hexene, 1-octene, 1-decene, 1-dodecene, and 4-methyl-1-pentene. Ethylene-1-octene copolymers are easy to process into films and can easily produce films with excellent cold resistance, adhesion, and water resistance.
[0029] Examples of the ethylene-acrylic acid copolymer include polyacrylic acid and copolymers of (meth)acrylic acid and ethylene, etc. Ethylene-(meth)acrylic acid copolymers are preferred because they are easily obtainable with excellent adhesion to glass. The melt mass flow rate of the ethylene-acrylic acid copolymer is preferably from 0.1 to 500 g / 10 minutes, more preferably from 1 to 100 g / 10 minutes, and further preferably from 2 to 50 g / 10 minutes.
[0030] The ethylene-(meth)acrylic acid alkyl ester copolymer is a copolymer of ethylene and an alkyl ester monomer of (meth)acrylic acid such as methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, isobutyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, cyclohexyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, or stearyl (meth)acrylate. Ethylene-methyl (meth)acrylate copolymer is preferred because it is easy to obtain a copolymer with excellent adhesion to glass and heat resistance.
[0031] The ethylene-unsaturated ester copolymer, ethylene-α-olefin copolymer, ethylene-acrylic acid copolymer, and ethylene-(meth)acrylic acid alkyl ester copolymer preferably have an unsaturated ester, α-olefin, acrylic acid, or (meth)acrylic acid alkyl ester content of 5 to 30 mass%, more preferably 10 to 25 mass%, based on the total mass. By having such a content, it is possible to obtain a hot melt adhesive having high adhesive strength and excellent film processability.
[0032] The polymer (x1) is preferably a silane-modified ethylene-methyl (meth)acrylate copolymer, an ethylene-acrylic acid copolymer, or an ethylene-octene copolymer, and from the viewpoint of water resistance, a silane-modified ethylene-methyl (meth)acrylate copolymer is more preferable.
[0033] The organosilane compound used in the production of the polymer (x1) is Silane compounds having a vinyl group, such as vinyltrichlorosilane, vinyltrimethoxysilane, and vinyltriethoxysilane; silane compounds having an epoxy group, such as 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane; Silane compounds having a styryl group, such as p-styryltrimethoxysilane, silane compounds having a (meth)acryl group, such as 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, and 3-(meth)acryloxypropyltriethoxysilane; silane compounds having an amino group, such as N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride; silane compounds having a mercapto group, such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane; Silane compounds having a sulfide group, such as bis(triethoxysilylpropyl)tetrasulfide and 3-isocyanatepropyltriethoxysilane having an isocyanate group; In view of the ease of reaction with polyethylene, polypropylene, ethylene-unsaturated ester copolymer, ethylene-α-olefin copolymer, ethylene-acrylic acid copolymer, and ethylene-(meth)acrylic acid alkyl ester copolymer, organic silane compounds having an epoxy group or a methacryl group are preferred.
[0034] The polymerization initiator used in the production of the polymer (x1) includes an azo compound, an organic peroxide, and the like.
[0035] Examples of the azo-based compound among the polymerization initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-hydroxymethylpropionitrile), and 2,2'-azobis[2-(2-imidazol-2-yl)propane].
[0036] Examples of organic peroxides among the polymerization initiators include benzoyl peroxide, t-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl)peroxydicarbonate, bis(1-tert-butylperoxy-1-methylethyl)benzene, t-butyl peroxyneodecanoate, t-butyl peroxypivalate, (3,5,5-trimethylhexanoyl)peroxide, dipropionyl peroxide, and diacetyl peroxide.
[0037] The content of the silane compound in 100 mass% of the polymer (x1) is preferably 0.01 to 10 mass%, more preferably 0.1 to 8 mass%, and even more preferably 0.5 to 5 mass%. By having such a content, it is possible to obtain a hot melt adhesive that can ensure a high level of adhesive strength to glass.
[0038] In 100% by mass of the hot melt adhesive (C1) containing the silane modified product, the polymer (x1) is preferably contained in an amount of 1 to 100% by mass, more preferably 5 to 90% by mass, and further preferably 10 to 80% by mass. By containing the polymer (x1) in an amount of 1 to 100% by mass, it is possible to obtain a hot melt adhesive that can ensure a high level of adhesive strength to glass.
[0039] (Polymer (y1)) The polymer (y1) in the present invention is at least one selected from the group consisting of polyethylene, polypropylene, ethylene-unsaturated ester copolymer, ethylene-α-olefin copolymer, ethylene-acrylic acid copolymer, and ethylene-alkyl (meth)acrylic acid ester copolymer (excluding (x1)).
[0040] As the polymer (y1), the polyethylene, polypropylene, ethylene-unsaturated ester copolymer, ethylene-α-olefin copolymer, ethylene-acrylic acid copolymer, and ethylene-alkyl (meth)acrylic acid ester copolymer described above as the polymer (x1) can be used.
[0041] In terms of heat resistance and cold resistance, the polymer (y1) is preferably an ethylene-methyl methacrylate copolymer.
[0042] In 100% by mass of the hot melt adhesive (C1) containing the silane modified product, (y1) is preferably contained in an amount of 0 to 99% by mass, more preferably 5 to 90% by mass or less, and even more preferably 10 to 80% by mass. By using the above content, it is possible to obtain a hot melt adhesive that can ensure a high level of adhesive strength to glass and can be easily formed into a film.
[0043] (Tackifying resin (z1)) Tackifying resins are generally classified into natural tackifying resins and synthetic tackifying resins. Examples of natural tackifying resins include rosin-based tackifying resins such as gum rosin, tall oil rosin, wood rosin, hydrogenated rosin, disproportionated rosin, polymerized rosin, rosin-glycerin ester, rosin-pentaerythritol ester, maleated rosin, and hydrogenated products thereof, as well as terpene-based tackifying resins such as terpene resins, aromatic modified terpene resins, terpene phenol resins, and hydrogenated terpene resins. Rosin-based tackifying resins are preferably used because they can ensure a high level of adhesive strength to glass and are easy to use to obtain a hot melt adhesive with excellent heat resistance.
[0044] Examples of synthetic tackifier resins include aliphatic (C5) petroleum resins, aromatic (C9) petroleum resins, copolymer (C5 / C9) petroleum resins, hydrogenated petroleum resins (alicyclic petroleum resins), DCPD petroleum resins (alicyclic petroleum resins), pure monomer petroleum resins (styrene, substituted styrene petroleum resins), coumarone-indene resins, alkylphenol resins, xylene resins, etc. Aromatic (C9) and copolymer (C5 / C9) petroleum resins are preferably used because they can ensure a high level of adhesive strength to glass and are easy to use to obtain hot melt adhesives with excellent heat resistance.
[0045] As the tackifier resin (z1), any one of natural tackifier resins and synthetic tackifier resins may be used, or two or more of them may be used.
[0046] In terms of heat resistance, the tackifier resin (z1) is preferably a petroleum-based hydrocarbon resin.
[0047] The content of the tackifier resin in 100% by mass of the silane-modified hot melt adhesive (C1) is preferably 0 to 30% by mass, more preferably 0 to 20% by mass, and even more preferably 0 to 10% by mass. By using the above content, it is possible to obtain a hot melt adhesive that can ensure high levels of adhesive strength to glass and adhesive strength to plastics.
[0048] <Polyolefin-based hot melt adhesive (C2)> The polyolefin-based hot melt adhesive (C2) in the present invention is an olefin-based hot melt adhesive that does not contain a silane-modified product, and preferably contains 50 to 100 mass % of a polymer (x2) and 0 to 50 mass % of a tackifier resin (z2).
[0049] (Polymer(x2)) The polymer (x2) in the present invention is at least one polymer selected from the group consisting of polyolefins, acid-modified polyolefins, ethylene-unsaturated ester copolymers, ethylene-α-olefin copolymers, ethylene-acrylic acid copolymers, and ethylene-alkyl (meth)acrylic acid ester copolymers.
[0050] The polyolefin includes polyethylene and polypropylene. As the polyethylene, low density polyethylene (LDPE), linear low density polyethylene (LLDPE), very low density polyethylene (VLDPE), high density polyethylene (HDPE), polyethylene polymerized using a metallocene catalyst, etc. can be used. LDPE and LLDPE are preferably used because they are easy to process into films, etc., and LDPE is most preferably used. The melt mass flow rate of the polyethylene is preferably 0.1 to 500 g / 10 min, more preferably 1 to 100 g / 10 min, and even more preferably 2 to 50 g / 10 min. As the polypropylene, homo-polypropylene, random-polypropylene, block-polypropylene, polypropylene polymerized using a metallocene catalyst, etc. can be used. Random-polypropylene is preferred because it is easy to process, for example, into a film. The melt mass flow rate of the polypropylene is preferably from 0.1 to 500 g / 10 minutes, more preferably from 1 to 100 g / 10 minutes, and further preferably from 2 to 50 g / 10 minutes.
[0051] The acid-modified polyolefin is an olefin-based polymer, such as an ethylene-based polymer or a propylene-based polymer, to which one or more of α,β-unsaturated carboxylic acids, such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, etc., have been grafted. The amount of α,β-unsaturated carboxylic acid grafted is not particularly limited, but is preferably 0.001 to 10% by mass based on the total mass of the acid-modified polyolefin.
[0052] As the ethylene-unsaturated ester copolymer, the ethylene-α-olefin copolymer, the ethylene-acrylic acid copolymer, and the ethylene-(meth)acrylic acid alkyl ester copolymer, the ethylene-unsaturated ester copolymer, the ethylene-α-olefin copolymer, the ethylene-acrylic acid copolymer, and the ethylene-(meth)acrylic acid alkyl ester copolymer described in the polymer (x1) can be used.
[0053] The polymer (x2) is preferably an ethylene-methyl methacrylate copolymer or an acid-modified olefin, and more preferably an acid-modified olefin, since it is easier to obtain a polymer having excellent heat resistance and cold resistance.
[0054] The content of the polymer (x2) in 100% by mass of the hot melt adhesive (C2) is preferably 50 to 100% by mass, more preferably 70 to 100% by mass, and further preferably 80 to 95% by mass. A content of 50 to 100% by mass is preferable because a high level of adhesive strength to plastics can be ensured.
[0055] (Tackifier resin (z2)) The tackifier resin (z2) may be the same as the tackifier resin (z1). The content of the tackifier resin (z2) in 100% by mass of the hot melt adhesive (C2) is preferably 0 to 50% by mass, more preferably 0 to 30% by mass, and even more preferably 0 to 20% by mass. A content of 0 to 50% by mass is preferable because it is possible to ensure a high level of adhesive strength to plastics.
[0056] The hot melt adhesives (C1) and (C2) may further contain additives, etc., to prevent thermal deterioration, thermal decomposition, blocking, etc., and to ensure processability such as film processing and extrusion lamination, within the scope of the present invention. Examples of additives include colorants such as titanium oxide, organic lubricants such as erucic acid amide, inorganic lubricants such as calcium carbonate, antioxidants such as hindered phenols, antiblocking agents such as silicone, antistatic agents, fillers, etc. The antioxidant can prevent thermal deterioration and thermal decomposition of the hot melt adhesive.
[0057] Representative examples of antioxidants include high molecular weight hindered polyhydric phenols, triazine derivatives, high molecular weight hindered phenols, dialkyl phenol sulfides, 2,2-methylene-bis-(4-methyl-6-tert-butylphenol), 4,4-methylene-bis-(2,6-di-tert-butylphenol), 2,6-di-tert-butylphenol-p-cresol, 2,5-di-tert-butylhydroquinone, 2,2,4-trimethyl-1,2-dihydroquinone, dibutyl dithiocarbamate nickel, 1-oxy-3-methyl-4-isopropylbenzene, 4,4-butylidenebis-(3-methyl-6-tert-butylphenol), and 2-mercaptobenzimidazole.
[0058] The melt mass flow rate of the hot melt adhesives (C1) and (C2) is preferably 0.1 to 1000 g / 10 min., more preferably 0.5 to 500 g / 10 min., and even more preferably 1 to 100 g / 10 min. When the MFR of the hot melt adhesive is 0.1 to 1000 g / 10 min., it is easy to form a film.
[0059] <Method of manufacturing adhesive sheet> The adhesive sheet of the present invention can be produced by laminating a hot melt adhesive in the form of a film onto a metal foil such as an aluminum foil using a slot coater, gravure coater, roll coater, extrusion laminator or the like.
[0060] The adhesive sheet of the present invention preferably has a primer layer between the metal layer and the adhesive layer made of the hot melt adhesive. The presence of the primer layer increases the adhesive strength between the metal layer and the hot melt adhesive. The primer layer is not particularly limited, but a thermosetting adhesive is preferred in terms of adhesive strength between the metal foil and the hot melt adhesive. Examples of the thermosetting adhesive include polyester-based and polyisocyanate-based adhesives, etc. Among these, polyester-based adhesives tend to provide sufficient adhesive strength between the metal layer and the hot melt adhesive layer.
[0061] When the adhesive sheet has a primer layer, it can be manufactured by coating and drying a thermosetting adhesive on a metal foil, and laminating the hot melt adhesive in a film form on the metal foil using a slot coater, gravure coater, roll coater, extrusion laminator, etc., or by coating and drying a thermosetting adhesive on a metal foil and pressing it with a single layer film of hot melt adhesive. By laminating the metal foil and hot melt adhesive and then aging in an atmosphere of 40 to 80°C (adjusting appropriately depending on the type of thermosetting adhesive used), an adhesive sheet with stronger adhesion can be obtained.
[0062] <Laminated materials> The laminated member of the present invention is composed of a glass-based material, an adhesive sheet, and a plastic-based material arranged in this order, and the adhesive layer in contact with the glass-based material is a layer made of the hot melt adhesive (C1), and the adhesive layer in contact with the plastic-based material may be a layer made of either the hot melt adhesive (C1) or the hot melt adhesive (C2), but is more preferably a layer made of the hot melt adhesive (C2) in terms of adhesion and water resistance.
[0063] The manufacturing method of the laminated member is a method of heating by electromagnetic induction and bonding the glass-based material and the plastic-based material to the adjacent hot melt adhesive. Heating by electromagnetic induction can be performed using an electromagnetic induction heating device or the like. Heating may be performed from either the glass-based material or the plastic-based material, or from the outside of both.
[0064] Electromagnetic induction heating refers to raising the temperature of the metal parts of a magnetic body by electrical energy transferred from a high frequency current transmitting conductor, typically an induction coil.
[0065] The method for peeling the glass-based material and / or the plastic-based material from the laminated member is a method for softening or melting the hot melt adhesive by heating with electromagnetic induction, and peeling the glass-based material and / or the plastic-based material from the laminated member. Heating may be performed from either the glass-based material or the plastic-based material, or from the outside of both. EXAMPLES
[0066] The present invention will be described in more detail below with reference to examples, but the following examples are not intended to limit the scope of the invention. In the examples, "parts" and "%" represent "parts by mass" and "% by mass", respectively, unless otherwise specified.
[0067] <Production of polymer (x1)> (Production Example 1: Production of Polymer x1-1) x1-1: 100 parts of low density polyethylene (Petrothene 212 (MFR 13 g / 10 min) manufactured by Tosoh Corporation) were blended with 8 parts of a silane coupling agent (KBE-903 manufactured by Shin-Etsu Chemical Co., Ltd.) and 2 parts of an organic peroxide (Perbutyl P-40 manufactured by NOF Corporation). The preblend was placed in a hopper and fed to an extruder using a screw feeder to produce a silane modified material (MFR 7 g / 10 min). Extruder: IKG twin screw extruder PMT32-40.5 Barrel temperature: 220℃ (feed inlet 180℃) Screw rotation speed: 100 rpm Feeding rate: 10kg / hr
[0068] (Production Example 2: Production of Polymer x1-2) x1-2: The same procedure as for x1-1 was repeated, except that the low-density polyethylene was replaced with an ethylene-vinyl acetate copolymer (Ultrathene 526 (MFR 25 g / 10 min, vinyl acetate content 7%) manufactured by Tosoh Corporation), and the silane coupling agent (Dynasylan VTEO manufactured by EVONIK) was replaced with 5 parts, and the organic peroxide (Lupelox DTA manufactured by Arkema Yoshitomi Co., Ltd.) was replaced with 1 part.
[0069] (Production Example 3: Production of Polymer x1-3) x1-3: The same procedure as for x1-1 was repeated, except that the low-density polyethylene was replaced with an ethylene-methyl methacrylate copolymer (Acryft WH303-F (MFR 7 g / 10 min, methyl methacrylate content 18%) manufactured by Sumitomo Chemical Co., Ltd.), and the silane coupling agent (KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.) was replaced with 3 parts, and the organic peroxide (Lupelox DTA manufactured by Arkema Yoshitomi Co., Ltd.) was replaced with 1 part.
[0070] (Production Example 4: Production of Polymer x1-4) x1-4: The same procedure as for x1-1 was repeated except that low-density polyethylene was pre-blended with 100 parts by weight of an ethylene-acrylic acid copolymer (Nucrel N1525 (MFR 25 g / 10 min, acrylic acid content 15%) manufactured by Mitsui Dow Chemical Co., Ltd.), 1 part by weight of a silane coupling agent (KBE-403 manufactured by Shin-Etsu Chemical Co., Ltd.) and 0.5 parts by weight of an organic peroxide (Perbutyl P-40 manufactured by NOF Corp.).
[0071] (Production Example 5: Production of Polymer x1-5) x1-5: The same procedure as for x1-4 was repeated, except that the ethylene-acrylic acid copolymer was replaced with an ethylene-octene copolymer (Engage 8411 (MFR 18 g / 10 min) manufactured by Dow Chemical Company).
[0072] (Production Example 6: Production of Polymer x1-6) x1-6: The same procedure was performed as for x1-3, except that the ethylene-methyl methacrylate copolymer was replaced with chlorinated polyethylene.
[0073] <Production of hot melt adhesive containing silane modified material (C1-1)> 100 parts of x1-1 as the silane modified substance (x1), 0.1 parts of an antioxidant, and 0.1 parts of a slip agent were preblended in a Henschel mixer for 5 minutes. The preblended product was put into a hopper and fed to an extruder using a screw feeder to produce a hot melt adhesive (C1) containing the silane modified substance as an essential component. Extruder: IKG twin screw extruder PMT32-40.5 Barrel temperature: 160℃ (feed inlet 100℃) Screw rotation speed: 100 rpm Feeding rate: 10kg / hr
[0074] [Production of C1-2 to C1-5] It was produced in the same manner as C1-1, except that the silane-modified product (x1) shown in Table 1 was used.
[0075] [Production of C1-6 to C1-18] It was produced in the same manner as C1-1, except that the silane-modified product (x1), polymer (y1), and tackifier resin (z) shown in Table 1 were used.
[0076] <Production of polyolefin-based hot melt adhesive (C2-1)> 90 parts of x2-1 as polymer (x2), 10 parts of z-1 as tackifier resin (z), 0.1 part of antioxidant and 0.1 part of slip agent were preblended in a Henschel mixer for 5 minutes. The preblended mixture was put into a hopper and fed to an extruder using a screw feeder to produce a polyolefin-based hot melt adhesive (C2). Extruder: IKG twin screw extruder PMT32-40.5 Barrel temperature: 160℃ (feed inlet 100℃) Screw rotation speed: 100 rpm Feeding rate: 10kg / hr
[0077] [Production of C2-2 to C2-12 and HM-1] It was produced in the same manner as C2-1, except that the materials were changed as shown in Table 2.
[0078] The abbreviations for materials listed in Tables 1 and 2 will be explained below.
[0079] (metal layer) Aluminum: Aluminum foil (20μm, 700μm) Copper: Copper foil (500μm) Stainless steel: Stainless steel (SUS304) foil (1000μm) Nickel: Nickel foil (200 μm)
[0080] (Polymer (y1)) y1-1: Ethylene-vinyl acetate copolymer (Tosoh Ultrathene 540 (MFR 3g / 10min, vinyl acetate content 10%)) y1-2: Ethylene-methyl methacrylate copolymer (Sumitomo Chemical Co., Ltd. Acryft WD301-F (MFR 7g / 10min, methyl methacrylate content 10%)) y1-3: Low density polyethylene (Tosoh Corporation's Petrothene 225 (MFR 3.7 g / 10 min)) y1-4: Random polypropylene (Novatec FL02A (MFR 12g / 10min) manufactured by Japan Polypropylene Corporation)
[0081] (Polymer(x2)) x2-1: Ethylene-vinyl acetate copolymer (Tosoh Ultrasen 540 (MFR 3g / 10min, vinyl acetate content 10%)) x2-2: Ethylene-methyl methacrylate copolymer (Sumitomo Chemical Co., Ltd. Acryliff WD301-F (MFR 7g / 10min, methyl methacrylate content 10%)) x2-3: Low density polyethylene (Tosoh Corporation's Petrothene 225 (MFR 3.7g / 10min)) x2-4: Acid-modified olefin (Mitsubishi Chemical Modic F534A (MFR 3.5g / 10min))
[0082] (Other polymers) T1: Chlorinated polyethylene (Resonac's Elaslen 303JB (MFR 25g / 10min)) T2: Styrene-based elastomer (Kuraray Septon 2063 (MFR 2g / 10min))
[0083] (Tackifying resin (z)) z-1: Petroleum-based hydrocarbon resin (Arcon M-115, manufactured by Arakawa Chemical Industries, Ltd.) z-2: Petroleum-based hydrocarbon resin (Arcon P-140, manufactured by Arakawa Chemical Industries, Ltd.) z-3: Disproportionated rosin ester (Haritac FK125, manufactured by Harima Chemicals) z-4: Hydrogenated terpene resin (Yasuhara Chemical's Clearon P-125)
[0084] Antioxidant: BASF Irganox 1010 Slip agent: Croda Ink Slip C
[0085] [Table 1]
[0086] [Table 2]
[0087] [Example 1: Production of adhesive sheet] The thermosetting adhesive A described later was applied at a dry weight of 0.3 g / m2 after the solvent had evaporated. 2 The primer layer was formed by applying the adhesive on aluminum with a wire bar so that the adhesive was heated to about 30-45°C. The drying conditions were 80°C for 1 minute. Next, single-layer films of hot melt adhesives C1-1 and C2-1 were produced using an inflation molding machine. The single-layer film of C1-1 was pressed onto the primer layer using a pressure roll. Furthermore, the thermosetting adhesive A was applied to the aluminum surface of the aluminum / primer layer / hot melt adhesive laminate film in the same manner as above, and dried to form a primer layer. Next, the single-layer film of C2-1 was pressed onto the primer layer using a pressure roll. After that, aging was performed for 4 days in an environment of 40°C to obtain an adhesive sheet. The processing conditions are shown below. Inflation molding machine: Labtech Resin temperature: 100~170℃ (adjust as appropriate) Nip roll speed: 6m / min
[0088] [Examples 2 to 34 and Comparative Examples 1 to 7: Production of Adhesive Sheets] Adhesive sheets were produced in the same manner as in Example 1, except that the hot melt adhesive, the metal layer, and the thermosetting adhesive forming the primer layer were changed to those shown in Tables 3-5.
[0089] The materials listed in Tables 3 to 5 will be explained.
[0090] (Thermosetting adhesive) Main ingredient Toyo Morton EL-510 (polyester) Toyo Morton TM-K76 (polyester) Hardener Toyo Morton CAT-RT80 (polyisocyanate type) · Toyo Morton CAT-RT85 (polyisocyanate type) [Thermosetting adhesive A] The thermosetting adhesive base material EL-510 and the curing agent CAT-RT80 were mixed in a weight ratio of 15 / 3 and diluted with ethyl acetate to a solid content of 8%. [Thermosetting adhesive B] The thermosetting adhesive base material TM-K76 and the curing agent CAT-RT85 were mixed in a weight ratio of 100 / 7 and diluted with ethyl acetate to a solid content of 30%.
[0091] (Glass-based materials) Tempered glass: stronger than ordinary glass Laminated glass: Two sheets of glass bonded together with an intermediate film such as synthetic resin.
[0092] (Plastic materials) PP: Polypropylene PE: Polyethylene PET: Polyethylene terephthalate PBT: Polybutylene terephthalate
[0093] [Example 1: Production of laminated members] The adhesive sheet C1 produced in Example 1 above and the glass-based material were sandwiched together so that the adhesive sheet C2 and the plastic-based material were in contact, and the applicator part (coil) of an electromagnetic induction heating device (an all-over bonding device manufactured by Achilles Corporation) was pressed against the glass-based material side and heated for 60 seconds. Even after heating was stopped, the applicator part (coil) of the electromagnetic induction heating device was kept pressed against the hot melt adhesive layer for approximately 5 seconds until the hot melt adhesive layer cooled, thereby producing a laminated member.
[0094] [Examples 2 to 34 Production of Laminated Members] A laminated member was produced in the same manner as in Example 1, except that the adhesive sheet produced in the corresponding example was used.
[0095] [Comparative Examples 1 to 5: Production of Laminated Members] A laminated member was produced in the same manner as in Example 1, except that the adhesive sheet C2-11 produced in the corresponding comparative example and the plastic substrate were sandwiched so that the other side of the adhesive sheet was in contact with the glass substrate.
[0096] [Comparative Examples 6 and 7: Production of Laminated Members] Laminated members were produced in the same manner as in Comparative Examples 1 to 5, except that a silane coupling agent (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.) was applied to the surface of the glass-based material.
[0097] <Adhesiveness> The laminated members prepared by the above method were left for 24 hours, and then the shear strength of the glass-based material and the adhesive sheet, and the shear strength of the plastic material and the adhesive sheet were measured using a tensile strength tester (Shimadzu Autograph AGS) at a tensile speed of 200 mm / min, 23°C, and 65% relative humidity. ○: 100N / cm 2 End △: 50N / cm 2 More than 100N / cm 2 less than ×:50N / cm 2 less than <Heat-resistant adhesiveness> The laminated members prepared by the above method were left in an oven at 80°C for 1,000 hours, and then left at 23°C and 65% relative humidity for 24 hours. The shear strength of the glass-based material and adhesive sheet, and the shear strength of the plastic material and adhesive sheet were measured using a tensile strength tester (Shimadzu Autograph AGS) at a tensile speed of 200 mm / min, 23°C, and 65% relative humidity. ○: 100N / cm 2 End △: 50N / cm 2 More than 100N / cm 2 less than ×:50N / cm 2 less than <Cold resistance adhesiveness> The laminated members prepared by the above method were left in a freezer at -20°C for 1,000 hours, and then left at 23°C and 65% relative humidity for 24 hours. The shear strength of the glass-based material and adhesive sheet, and the shear strength of the plastic material and adhesive sheet were measured using a tensile strength tester (Shimadzu Autograph AGS) at a tensile speed of 200 mm / min, 23°C, and 65% relative humidity. ○: 100N / cm 2 End △: 50N / cm 2 More than 100N / cm 2 less than ×:50N / cm 2 less than <Water resistant adhesion> The laminated members prepared by the above method were left in water at 23°C for 24 hours, and then the shear strength of the glass-based material and adhesive sheet, and the shear strength of the plastic material and adhesive sheet were measured using a tensile strength tester (Shimadzu Autograph AGS) at a tensile speed of 200 mm / min, 23°C, and 65% relative humidity. ○: 100N / cm 2 End △: 50N / cm 2 More than 100N / cm 2 less than ×:50N / cm 2 less than
[0098] [Table 3]
[0099]
Table 4
[0100]
Table 5
Claims
1. An adhesive sheet having an adhesive layer made of a hot melt adhesive on both sides of a metal layer, A hot melt adhesive (C1) containing a silane-modified product is disposed on one surface of the metal layer, An adhesive sheet having disposed on the other surface thereof either a hot melt adhesive containing a silane-modified material (C1) or a polyolefin-based hot melt adhesive (excluding hot melt adhesives containing a silane-modified material) (C2).
2. The hot melt adhesive (C1) containing a silane modified product contains 1 to 100 mass% of a polymer (x1), 0 to 99 mass% of a polymer (y1), and 0 to 30 mass% of a tackifier resin (z1), in 100 mass% of the silane modified product; the polymer (x1) is at least one selected from the group consisting of silane-modified polyethylene, silane-modified polypropylene, silane-modified ethylene-unsaturated ester copolymer, silane-modified ethylene-α-olefin copolymer, silane-modified ethylene-acrylic acid copolymer, and silane-modified ethylene-alkyl (meth)acrylic acid ester copolymer, The polymer (y1) is at least one selected from the group consisting of polyethylene, polypropylene, ethylene-unsaturated ester copolymer, ethylene-α-olefin copolymer, ethylene-acrylic acid copolymer, and ethylene-(meth)acrylic acid alkyl ester copolymer (excluding (x1)); The adhesive sheet according to claim 1.
3. The hot melt adhesive (C2) contains 100% by mass of a polyolefin-based hot melt adhesive, and the hot melt adhesive (C2) contains 50 to 100% by mass of a polymer (x2) and 0 to 50% by mass of a tackifier resin (z2). The polymer (x2) is at least one selected from the group consisting of polyolefins, acid-modified polyolefins, ethylene-unsaturated ester copolymers, ethylene-α-olefin copolymers, ethylene-acrylic acid copolymers, and ethylene-(meth)acrylic acid alkyl ester copolymers. The adhesive sheet according to claim 1 or 2.
4. 4. The adhesive sheet according to claim 3, further comprising a primer layer between the metal layer and the adhesive layer made of a hot melt adhesive.
5. A laminated member comprising a glass-based material, the adhesive sheet according to claim 4, and a plastic-based material arranged in this order, the adhesive layer adjacent to the glass-based material is a layer made of the hot melt adhesive (C1); The adhesive layer adjacent to the plastic material is a layer consisting of at least one of the hot melt adhesive (C1) and the hot melt adhesive (C2). Laminated material.
6. 6. The method for producing a laminated member according to claim 5, wherein the glass-based material and the plastic-based material are bonded to the adjacent hot melt adhesive by heating using electromagnetic induction.
7. A method for peeling glass-based materials and / or plastic-based materials from a laminated member according to claim 5, comprising softening or melting the hot melt adhesive by heating using electromagnetic induction.
Citation Information
Patent Citations
Adhering method of glass holder, and glass holder
JP1994206442A
Bonding method
JP2022134737A
Cited By
Encapsulating sheet and system board for system board on which the processor is mounted.
JP2026111479A