Processing method, processing system, and inspection device

By forming a region of reduced bonding strength and using optical interferometry to measure displacement, the method addresses the lack of quantitative accuracy in substrate separation, ensuring reliable substrate processing.

JP2024163833APending Publication Date: 2024-11-22TOKYO ELECTRON LTD

Patent Information

Application Number
JP2023175412
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2023-10-10
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing methods for determining the separation of substrates in a polymerized substrate lack quantitative accuracy, relying solely on visual inspection which fails to provide reliable judgment on the separation of substrates at reduced bonding strength regions.

Method used

A method involving irradiation with a laser beam to form a region of reduced bonding strength, followed by measuring the displacement of the substrate edges using optical interferometry to quantify the separation and determine the appropriate formation of a bonding force reduced region.

Benefits of technology

Enables accurate and quantitative inspection of peeling at the interface between substrates, ensuring proper separation and removal of the peripheral edge, enhancing the reliability of substrate processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163833000001_ABST
    Figure 2024163833000001_ABST
Patent Text Reader

Abstract

To appropriately inspect separation of a bonding strength reduction region formed at an interface between a first substrate and a second substrate in a polymerization substrate where the first substrate and the second substrate are bonded together.SOLUTION: A processing method for a polymerization substrate where a first substrate and a second substrate are bonded together comprises the steps of: emitting laser light toward an interface between the first substrate and the second substrate in a peripheral part of the first substrate to form a bonding strength reduction region where the first substrate and the second substrate are separated at the interface; measuring a displacement amount of the peripheral part where the bonding strength reduction region is formed; acquiring a feature amount for detecting separation of the first substrate and the second substrate on the basis of the displacement amount; and comparing the feature amount with a predetermined threshold to determine separation of the first substrate and the second substrate.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a processing method, a processing system, and an inspection apparatus. [Background technology]

[0002] Patent document 1 discloses a substrate processing system having a modified layer forming device that forms a modified layer inside a first substrate along the boundary between the peripheral and central portions of a first substrate to be removed, in a laminated substrate formed by bonding a first substrate and a second substrate, and an edge removal device that removes the peripheral portion of the first substrate using the modified layer as a base point. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2019 / 176589 Summary of the Invention [Problem to be solved by the invention]

[0004] The technology disclosed herein appropriately inspects for peeling in an area of ​​reduced adhesive strength formed at the interface between a first substrate and a second substrate in a laminated substrate in which a first substrate and a second substrate are bonded together. [Means for solving the problem]

[0005] One aspect of the present disclosure is a method for processing a composite substrate in which a first substrate and a second substrate are bonded together, the method including the steps of: irradiating a laser beam toward an interface between the first substrate and the second substrate at a peripheral portion of the first substrate to form a region of reduced bonding strength where the first substrate and the second substrate have peeled off at the interface; measuring an amount of displacement of the peripheral portion where the region of reduced bonding strength has been formed; acquiring a feature amount for detecting peeling between the first substrate and the second substrate based on the amount of displacement; and comparing the feature amount with a predetermined threshold value to determine peeling between the first substrate and the second substrate. Effect of the Invention

[0006] According to the present disclosure, in a laminated substrate in which a first substrate and a second substrate are bonded together, peeling in an area of ​​reduced bonding strength formed at the interface between the first substrate and the second substrate can be appropriately inspected. [Brief description of the drawings]

[0007] [Figure 1] 1 is a side view showing a schematic configuration example of a laminated wafer to be processed; [Diagram 2] FIG. 1 is a plan view illustrating a schematic configuration example of a wafer processing system. [Diagram 3] 1 is a cross-sectional view showing an adhesive strength reduction region and a peripheral modified layer formed on a laminated wafer. [Figure 4] FIG. 2 is an explanatory diagram showing main steps of wafer processing in the wafer processing system. [Diagram 5] FIG. 1 is a plan view showing a schematic configuration example of an interface modification device. [Figure 6] FIG. 2 is a side view showing a schematic configuration example of an interface modification device. [Figure 7] FIG. 2 is an explanatory diagram illustrating an example of the operation of the inspection device. [Figure 8] 11A and 11B are explanatory diagrams illustrating another operation example of the inspection device. [Figure 9] FIG. 2 is an explanatory diagram showing an inspection area set on an overlapping wafer. [Figure 10] FIG. 4 is a flowchart showing main steps of peeling determination according to the embodiment. [Figure 11] 11 is a graph showing an example of a measurement result obtained by an inspection device. [Figure 12] 11 is a graph showing an example of a measurement result obtained by an inspection device. [Figure 13] FIG. 11 is an explanatory diagram showing an example of a smoothing process for displacement amount data. [Figure 14] 11 is an explanatory diagram showing an example of a displacement amount waveform used in peeling determination according to the embodiment. FIG. [Figure 15] FIG. 13 is an explanatory diagram showing an example of a standardized displacement amount waveform. [Figure 16]11A and 11B are diagrams illustrating the peak, average, and standard deviation of the displacement amount used in the fitting process. [Figure 17] FIG. 11 is an explanatory diagram showing an example of a simulated waveform used in peeling determination according to the embodiment. [Figure 18] FIG. 13 is a diagram illustrating quartile values ​​of a displacement waveform. [Figure 19] FIG. 13 is a diagram illustrating an example of changing the interquartile range. [Figure 20] 11 is a graph showing a comparison result of feature amounts obtained by peeling determination according to the embodiment. [Figure 21] 11 is a graph showing a comparison result of feature amounts obtained by peeling determination according to the embodiment. [Figure 22] 11 is an explanatory diagram showing an example of an approximation result by a high-order function of a displacement amount waveform used in peeling determination according to the embodiment. FIG. [Diagram 23] 11 is a graph showing a comparison result of feature amounts obtained by peeling determination according to the embodiment. [Figure 24] 10 is an explanatory diagram showing an example of a signal wave created from a displacement amount waveform used in peeling determination according to the embodiment; FIG. [Diagram 25] 11 is a graph showing a comparison result of feature amounts obtained by peeling determination according to the embodiment. [Figure 26] 11 is an explanatory diagram showing a topography image of the amount of displacement acquired by an inspection device and a graph showing a waveform of the amount of displacement in a state in which the first wafer and the second wafer are peeled off in one inspection area. FIG. [Figure 27] 11 is an explanatory diagram showing a topography image of the amount of displacement acquired by an inspection device and a graph showing a waveform of the amount of displacement in a state in which the first wafer and the second wafer are partially peeled off in one inspection area. FIG. [Figure 28] 13 is a graph showing average values ​​of the amount of displacement of a protrusion in the depth direction obtained by varying the conditions for irradiating a laser beam when forming a region with reduced bonding strength. [Figure 29] 13 is a graph showing the standard deviation of the amount of displacement of a convex portion in the width direction obtained by varying the irradiation conditions of the laser light when forming a bonding strength reduced region. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In the manufacturing process of semiconductor devices, a laminated substrate in which a first substrate (a silicon substrate such as a semiconductor) having a plurality of devices such as electronic circuits formed on its surface and a second substrate are bonded together may be subjected to a process of removing the peripheral portion of the first substrate, i.e., a process known as edge trimming.

[0009] The edge trim of the first substrate is performed, for example, by using the substrate processing system disclosed in Patent Document 1. That is, a modified layer is formed by irradiating the inside of the first substrate with laser light, and the peripheral portion is removed from the first substrate using the modified layer as a base point. In addition, in the substrate processing system described in Patent Document 1, a laser light is irradiated to the interface between the first substrate and the second substrate to form a portion where the first substrate and the second substrate are peeled off and whereby the peripheral portion is appropriately removed.

[0010] Incidentally, a determination as to whether the first and second substrates have been properly peeled off at the thus-formed reduced bonding strength portion (hereinafter, "peeling determination") has conventionally been made using an image obtained by imaging the interface using, for example, an ultrasonic microscope (C-SAM). However, when using the captured image in this way, the peeling determination between the first and second substrates is usually made by visually judging the captured image, which poses a problem in that a quantitative judgment cannot be made.

[0011] The technology according to the present disclosure has been made in consideration of the above circumstances, and appropriately inspects peeling of a bonding strength weakened region formed at the interface between a first substrate and a second substrate in a laminated substrate in which a first substrate and a second substrate are bonded. Hereinafter, a substrate processing system, an inspection device, and a processing method according to the present embodiment will be described with reference to the drawings. In this specification and the drawings, elements having substantially the same functional configuration are denoted by the same reference numerals to avoid redundant description.

[0012] In a wafer processing system 1 according to this embodiment, which will be described later, processing is performed on an overlapped wafer T as an overlapped substrate in which a first wafer W as a first substrate and a second wafer S as a second substrate are bonded together as shown in FIG. 1. A wafer is an example of a substrate. Hereinafter, in the first wafer W, the surface to be bonded to the second wafer S is referred to as a front surface Wa, and the surface opposite the front surface Wa is referred to as a back surface Wb. Similarly, in the second wafer S, the surface to be bonded to the first wafer W is referred to as a front surface Sa, and the surface opposite the front surface Sa is referred to as a back surface Sb.

[0013] The first wafer W is a semiconductor wafer such as a silicon substrate, and at least one film is laminated on the front surface Wa side. Hereinafter, the film formed on the front surface Wa side is referred to as a "laminated film". In this embodiment, the laminated film includes a device layer Dw and a bonding film Fw. The device layer Dw includes a plurality of devices. For the bonding film Fw, for example, an oxide film (THOX film, SiO2 film, TEOS film), a SiC film, a SiCN film, or an adhesive is used. The first wafer W is bonded to the second wafer S via the bonding film Fw. The peripheral portion We of the first wafer W is chamfered, and the cross section of the peripheral portion We becomes thinner toward its tip. The peripheral portion We is a portion to be removed in the edge trim described later, and is, for example, in the range of 0.5 mm to 3 mm in the radial direction from the outer end of the first wafer W. In the following description, the region radially inward of the peripheral portion We to be removed in the first wafer W may be referred to as the center portion Wc.

[0014] The second wafer S has, for example, the same configuration as the first wafer W. That is, a device layer Ds and a bonding film Fs are formed as a laminated film on the surface Sa side, and the peripheral portion is chamfered. Note that the second wafer S does not need to be a device wafer on which the device layer Ds is formed, and may be, for example, a support wafer that supports the first wafer W. In such a case, the second wafer S functions as a protective material that protects the device layer Dw of the first wafer W.

[0015] 1 shows an example in which a device layer and a bonding film are formed as laminated films on the surfaces of the first wafer W and the second wafer S. However, the type and number of laminated films are not limited to this. For example, a laser absorbing film (not shown) for absorbing the interface laser light L1 described later may be formed at the interface between the surface Wa of the first wafer W from which the peripheral portion We is removed and the device layer Dw and the bonding film Fw.

[0016] 2, the wafer processing system 1 has a configuration in which a loading / unloading station 2 and a processing station 3 are integrally connected. In the loading / unloading station 2, for example, a cassette C capable of accommodating a plurality of overlapped wafers T is loaded and unloaded between the loading / unloading station 2 and the outside. The processing station 3 is equipped with various processing devices that perform desired processing on the overlapped wafers T.

[0017] The loading / unloading station 2 is provided with a cassette mounting stage 10 on which a cassette C capable of accommodating a plurality of overlapped wafers T is mounted. A wafer transport device 20 is provided adjacent to the cassette mounting stage 10 on the positive side of the X-axis of the cassette mounting stage 10. The wafer transport device 20 moves on a transport path 21 extending in the Y-axis direction, and is configured to be able to transport the overlapped wafers T between the cassette C on the cassette mounting stage 10 and a transition device 30 described below.

[0018] In the loading / unloading station 2, a transition device 30 for transferring the overlapped wafer T between the processing station 3 and the wafer transfer device 20 is provided adjacent to the wafer transfer device 20 on the positive side of the X-axis of the wafer transfer device 20.

[0019] In the processing station 3, a wafer transfer device 40, an interface modification device 50, an internal modification device 60, an edge removal device 70 and a cleaning device 80 are arranged.

[0020] The wafer transport device 40 is provided on the X-axis positive side of the transition device 30. The wafer transport device 40 is configured to be freely movable on a transport path 41 extending in the X-axis direction, and configured to be able to transport the overlapped wafer T to the transition device 30, the interface modification device 50, the internal modification device 60, the edge removal device 70, and the cleaning device 80 in the carry-in / out station 2.

[0021] The interface modification device 50 irradiates the interface between the first wafer W and the second wafer S with laser light L1 (interface laser light, for example, a CO2 laser) to form a bonding strength reduced region Ae where the first wafer W and the second wafer S are peeled off at the peripheral portion We to be removed, as shown in Figures 3 and 4(a). The interface modification device 50 has a control device 51, which will be described later.

[0022] As shown in FIG. 5 and FIG. 6, the interface modification device 50 has a chuck 100 that holds the overlapped wafer T on its upper surface. The chuck 100 holds the back surface Sb of the second wafer S by suction with the first wafer W on the upper side and the second wafer S on the lower side. The chuck 100 is supported by a slider table 102 via an air bearing 101. A rotation mechanism 103 is provided on the lower surface side of the slider table 102. The rotation mechanism 103 has a built-in motor as a driving source. The chuck 100 is configured to be rotatable around a vertical axis by the rotation mechanism 103 via the air bearing 101. The slider table 102 is configured to be movable on a rail 106 that is provided on a base 105 and extends in the Y-axis direction via a moving mechanism 104 provided on the lower surface side of the slider table 102. The driving source of the moving mechanism 104 is not particularly limited, but a linear motor is used, for example.

[0023] A laser head 110 is provided above the chuck 100. The laser head 110 has a lens 111. The lens 111 is a cylindrical member provided on the lower surface of the laser head 110, and irradiates the inside of the laminated wafer T held by the chuck 100, more specifically, the interface between the first wafer W and the laminated film (the device layer Dw and the bonding film Fw), with a laser beam L1 for the interface. As a result, the first wafer W and the laminated film are peeled off at the portion irradiated with the laser beam L1, and a bonding strength reduced region Ae is formed where the first wafer W and the second wafer S are peeled off. The position where the bonding strength reduced region Ae is formed is not particularly limited as long as the peeling occurs at the interface between the first wafer W and the second wafer S and the bonding strength can be reduced. That is, the peeling between the first wafer W and the second wafer S may occur at the interface between the first wafer W and the laminated film as shown in the figure, or may occur at the interface between the laminated films or the interface between the second wafer S and the laminated film.

[0024] The laser head 110 is supported by a support member 112. The laser head 110 is configured to be movable up and down by an elevating mechanism 114 along a rail 113 extending in the vertical direction. The laser head 110 is also configured to be movable in the Y-axis direction by a moving mechanism 115. The elevating mechanism 114 and the moving mechanism 115 are each supported by a support column 116.

[0025] In the illustrated example, the chuck 100 is configured to rotate relatively to the laser head 110 and to move horizontally by the rotation mechanism 103 and the movement mechanism 104, but the laser head 110 may be configured to rotate relatively to the chuck 100 and to move horizontally. Also, both the chuck 100 and the laser head 110 may be configured to rotate relatively to each other and to move horizontally.

[0026] An imaging mechanism 120 is provided above the chuck 100 on the Y-axis positive side of the laser head 110. The imaging mechanism 120 includes at least one camera. An image captured by the camera is output to a control device 51 or a control device 90, which will be described later. The interface modification device 50 grasps the position of the overlapped wafer T on the chuck 100 based on the image obtained by the imaging mechanism 120, and determines the alignment of the overlapped wafer T and the irradiation position of the laser light L1 based on the image. The imaging mechanism 120 is configured to be freely raised and lowered by a lifting mechanism 121, and is further configured to be freely moved in the Y-axis direction by a moving mechanism 122. The moving mechanism 122 is supported by a support column 116.

[0027] Moreover, in the technology according to the present disclosure, the interface modification apparatus 50 has an inspection device 130 above the chuck 100 for inspecting the bonding strength reduced region Ae formed by irradiation with the laser light L1 (determining peeling between the first wafer W and the second wafer S). The inspection device 130 is a mechanism configured to be able to detect peeling between the first wafer W and the second wafer S, for example, by using light interference (optical interferometry), and has a light projecting unit 131, a light receiving unit 132, and a calculation unit 133. The light projecting unit 131 and the light receiving unit 132 constitute a measurement unit that measures the amount of displacement of the peripheral portion We where the bonding strength reduced region Ae is formed in the present disclosure, and the measurement unit is, for example, an optical interferometer.

[0028] The light projector 131 is held by the chuck 100 and irradiates light toward the overlapped wafer T after the bonding strength reduced region Ae has been formed by irradiation with the laser light L1. The light irradiated from the light projector 131 may be laser light, white light, or any other type of light. The light irradiated from the light projector 131 may be translucent or reflective with respect to the first wafer W (silicon). The light receiving unit 132 receives light irradiated from the light projecting unit 131 and reflected by the overlapped wafer T. When the light irradiated from the light projecting unit 131 is reflective with respect to the first wafer W, the light receiving unit 132 receives light reflected by the back surface Wb of the first wafer W as shown in Fig. 7. On the other hand, when the light irradiated from the light projecting unit 131 is transparent with respect to the first wafer W, the light receiving unit 132 receives light reflected by the laminated film (device layer Dw and bonding film Fw) formed at the interface between the first wafer W and the second wafer S and the bonding strength reduction region Ae as shown in Fig. 8. The calculation unit 133 calculates the amount of displacement of the peripheral portion We based on the light reception result by the light receiving unit 132, and further calculates a feature amount, which will be described later, based on the amount of displacement of the peripheral portion We. The calculation unit 133 outputs the calculated feature amount to the control device 51 or the control device 90, which will be described later. The control device 51 or the control device 90 determines (peel determination) whether or not a bonding strength reduced region Ae is properly formed at the interface between the first wafer W and the second wafer S, that is, whether or not peeling has properly occurred, based on the feature amount from the calculation unit 133. Furthermore, the calculation unit 133 generates a topography image of the displacement amount of the peripheral portion We based on the light reception result by the light receiving unit 132, that is, the optical interference fringes.

[0029] The internal reforming device 60 irradiates the inside of the first wafer W with laser light L2 (internal laser light, for example, a YAG laser) to form a peripheral reformed layer M1 that serves as a base point for peeling off the peripheral portion We, as shown in FIG. 3 and FIG. 4(b). The internal reforming device 60 has a control device 61, which will be described later. The configuration of the internal reforming device 60 is not particularly limited, but in one example, the internal reforming device 60 may have a configuration similar to that of the interface reforming device 50. In this case, the internal reforming device 60 is configured to be able to irradiate the laminated wafer T (first wafer W) on the chuck with internal laser light L2 instead of interface laser light L1.

[0030] As shown in FIG. 4(c), the edge removal device 70 removes the edge portion We of the first wafer W, i.e., performs edge trimming, using the bonding strength reduced area Ae and the edge modified layer M1 as base points. Any method for edge trimming can be selected. In one example, the edge removal device 70 may insert, for example, a wedge-shaped blade B. Also, for example, an air blow or a water jet may be sprayed toward the edge portion We to apply an impact to the edge portion We.

[0031] The cleaning device 80 performs a cleaning process on the first wafer W and the second wafer S after the edge trimming by the edge removing device 70, and removes particles from these wafers. The cleaning method can be selected arbitrarily.

[0032] The above-mentioned wafer processing system 1 is provided with a control device 51, a control device 61, and a control device 90. The control device 51 controls the operation of the interface modification device 50 individually. The control device 51 also functions as a control unit that individually controls the inspection device 130. The control device 61 controls the operation of the internal modification device 60 individually. The control device 90 controls a series of wafer processing in the wafer processing system 1. The control devices 51, 61, and 90 are, for example, computers and have a program storage unit (not shown). The program storage unit stores a program for controlling the processing of the laminated wafer T in the wafer processing system 1. The program storage unit also stores a program for controlling the operation of the drive systems of the above-mentioned various processing devices and the transport device, etc., to realize the wafer processing in the wafer processing system 1, which will be described later. The above-mentioned programs may be recorded in a computer-readable storage medium and installed in the control devices 51, 61, and 90 from the storage medium. The above-mentioned storage medium may be temporary or non-temporary.

[0033] Next, a description will be given of wafer processing performed using the wafer processing system 1 configured as above. In this embodiment, the first wafer W and the second wafer S are bonded together to form an overlapped wafer T in advance.

[0034] First, a cassette C storing a plurality of overlapped wafers T is placed on the cassette placement table 10 of the carry-in / out station 2. Next, the overlapped wafers T are removed from the cassette C by the wafer transfer device 20 and transferred to the interface modification device 50 via the transition device 30 and the wafer transfer device 40.

[0035] In the interface modification device 50, a laser head 110 irradiates a predetermined irradiation area of ​​the overlapped wafer T with pulsed interface laser light L1, causing peeling at the interface between the first wafer W and the second wafer S (the interface between the first wafer W and the laminated film in the illustrated example) as shown in Figures 3 and 4(a). The irradiation area of ​​the laser light L1 is determined as an annular area having a desired radial width, for example, based on the outer edge of the first wafer W. The radial width of the irradiation area is set to a width that can appropriately remove the peripheral portion We of the first wafer W to be removed.

[0036] In the interface modification apparatus 50, the irradiation position of the laser light L1 at the interface between the first wafer W and the second wafer S is peeled off in this manner, thereby forming a bonding strength reduced region Ae where the bonding strength between the first wafer W and the second wafer S is reduced. In the edge trimming described below, the peripheral portion We of the first wafer W, which is the target for removal, is removed, and the presence of the bonding strength reduced region Ae in this manner makes it possible to appropriately remove the peripheral portion We.

[0037] When the bonding strength reduced region Ae is formed at the interface between the first wafer W and the second wafer S, next, an inspection (separation judgment) is performed to check whether the bonding strength reduced region Ae is properly formed, that is, whether the first wafer W and the second wafer S are properly separated. Note that a detailed method of the separation judgment in the interface modification device 50 (inspection device 130) will be described later.

[0038] When it is determined in the peeling judgment that the bonding strength reduced region Ae is not properly formed, that is, when it is determined that the first wafer W and the second wafer S are not properly peeled off, the overlapped wafer T is carried out from inside the interface modification apparatus 50 by the wafer transfer device 40, and the next overlapped wafer T is carried into the interface modification apparatus 50. The overlapped wafer T carried out from the interface modification apparatus 50 is, for example, discarded or collected. Alternatively, when it is determined that the bonding strength reduced region Ae has not been properly formed, the bonding strength reduced region Ae may be reformed by irradiating the overlapped wafer T with the interface laser light L1 again. In this case, the irradiation position of the laser light L1 may be set to the entire peripheral portion We, or may be set to only the portion where the first wafer W and the second wafer S have not been properly peeled off. The reformation conditions for the bonding strength reduced region Ae may be fed back to the formation conditions for the bonding strength reduced region Ae for the overlapped wafer T to be processed next in the wafer processing system 1.

[0039] On the other hand, when the peeling judgment determines that the bonding strength reduced area Ae has been properly formed over the entire peripheral portion We, i.e., when it is determined that the first wafer W and the second wafer S have been properly peeled off, the overlapped wafer T with the bonding strength reduced area Ae formed thereon is transported by the wafer transport device 40 to the internal modification device 60.

[0040] In the internal modification device 60, the internal laser light L2 is irradiated to a predetermined irradiation position inside the first wafer W to form a peripheral modified layer M1 as shown in Figures 3 and 4(b). The peripheral modified layer M1 serves as a base point for removing the peripheral portion We in the edge trimming described later.

[0041] When the peripheral modified layer M1 is formed, a crack C1 extends from the peripheral modified layer M1 into the first wafer W in the thickness direction of the first wafer W. The upper end of the crack C1 reaches, for example, the back surface Wb of the first wafer W. The lower end of the crack C1 extends toward the radial inner end of the bonding strength reduction region Ae formed by the interface modification device 50. The crack C1, like the peripheral modified layer M1, serves as a base point for removing the peripheral portion We.

[0042] In the above, the position where the peripheral modified layer M1 is formed is determined according to a preset removal (trim) width of the peripheral portion We, but the position where the peripheral modified layer M1 is formed may be determined based on, for example, the bonding strength reduced region Ae formed by the interface modification device 50. More specifically, the peripheral modified layer M1 may be formed by irradiating the laser light L2 along the radially inner end of the bonding strength reduced region Ae formed by the interface modification device 50. In this way, the position where the peripheral modified layer M1 is formed may be determined so that the peripheral modified layer M1 is not radially outward from the radially inner end of the bonding strength reduced region Ae.

[0043] Once the peripheral modified layer M1 is formed inside the first wafer W, the overlapped wafer T is then transported by the wafer transport device 40 to the peripheral removal device 70. In the peripheral removal device 70, as shown in Fig. 4(c), removal of the peripheral portion We of the first wafer W, i.e., edge trimming, is performed. At this time, the peripheral portion We is peeled off from the center portion Wc of the first wafer W using the peripheral modified layer M1 and the crack C1 as base points, and is also completely peeled off from the second wafer S using the bonding strength reduced region Ae as base point.

[0044] After the peripheral portion We of the first wafer W is removed, the overlapped wafer T is then transported by the wafer transport device 40 to the cleaning device 80. In the cleaning device 80, the first wafer W and / or the second wafer S after the peripheral portion We has been removed are cleaned.

[0045] Thereafter, the laminated wafer T which has been subjected to all the processes is transferred by the wafer transfer device 20 to the cassette C on the cassette mounting table 10 via the transition device 30. In this manner, a series of wafer processes in the wafer processing system 1 is completed.

[0046] Next, a detailed method of inspecting (determining whether or not there is separation) between the first wafer W and the second wafer S in the above-mentioned interface modification apparatus 50 (inspection apparatus 130) will be described.

[0047] When determining whether the first wafer W and the second wafer S have been peeled off, first, light is sequentially emitted from the light-projecting unit 131 toward each of a plurality of predetermined inspection regions R (four in the example shown in FIG. 9) on the peripheral portion We, and the light reflected from the overlapped wafer T is received by the light-receiving unit 132 (S1 in FIG. 10).

[0048] When the light receiving unit 132 receives the reflected light from the overlapped wafer T, the calculation unit 133 then calculates a graph showing the relationship between the radial position of the overlapped wafer T and the amount of displacement (S2 in FIG. 10). FIGS. 11 and 12 show the graph in one inspection region R as an example. The radial position of the overlapped wafer T (the horizontal axis in FIGS. 11 and 12) indicates the coordinate position in the radial direction of the overlapped wafer T in one inspection region R shown in FIG. The displacement amount (vertical axis in Figures 11 and 12) indicates the reflection height of the light irradiated from the light-projecting unit 131, and indicates the height position of the back surface Wb of the first wafer W when the light is reflective with respect to the first wafer W, and indicates the height position of the laminate film or the top surface of the bonding strength reduction region Ae when the light is transparent with respect to the first wafer W.

[0049] When the bonding strength reduced region Ae is formed by irradiation with the laser beam L1, a displacement occurs due to peeling between the first wafer W and the second wafer S, as shown in Fig. 7 and Fig. 8. Specifically, the front surface Wa of the first wafer W changes to a substantially concave shape, which displaces the height position of the front surface Wa compared to the non-formed portion of the bonding strength reduced region Ae. Also, the back surface Wb changes to a substantially convex shape corresponding to the substantially concave shape of the front surface Wa, which displaces the height position of the back surface Wb compared to the non-formed portion of the bonding strength reduced region Ae. In the technology disclosed herein, the displacement of the height positions of the front surface Wa and back surface Wb accompanying the formation of this bonding strength reduced region Ae is detected, and this displacement amount is converted into a feature quantity and treated, thereby quantitatively determining whether or not a bonding strength reduced region Ae has been formed at the interface between the first wafer W and the second wafer S.

[0050] Next, the control device 51 or the control device 90 acquires a feature quantity from the detected displacement amount (S3 in FIG. 10). As the feature quantity to be acquired, at least one of (1) half-width, (2) interquartile range, (3) peak ratio, (4) area, (5) frequency component, or (6) convexity statistics, which will be described later, can be selected. Details of each feature quantity will be described later.

[0051] Once the feature amount has been acquired, the feature amount is then compared with a predetermined threshold value (S4 in FIG. 10). Any value can be used as the threshold value used here as long as it is a value that can properly detect the peeling of the first wafer W and the second wafer S (the formation of the bonding strength reduced area Ae). For example, a feature amount obtained from a reference overlapped wafer T that is different from the overlapped wafer T to be inspected may be used as the threshold value. More specifically, a feature amount obtained in a similar procedure when the first wafer W and the second wafer S are properly peeled off (the bonding strength reduced area Ae is properly formed) may be used as the threshold value.

[0052] If the peeling judgment (S4 in FIG. 10) determines that the bonding strength reduced area Ae has not been properly formed (the first wafer W and the second wafer S have not been properly peeled off), as described above, a process for re-forming the bonding strength reduced area Ae is performed on the overlapped wafer T (S5 in FIG. 10), or the overlapped wafer T is discarded or recovered (S6 in FIG. 10).

[0053] On the other hand, if the peeling judgment (S4 in FIG. 10) determines that the bonding strength reduction region Ae has been properly formed (the first wafer W and the second wafer S have been properly peeled off), the overlapped wafer T is transported to the internal modification device 60 (S7 in FIG. 10) as described above.

[0054] The peeling determination in the interface modification device 50 (inspection device 130) is performed as described above. According to the inspection apparatus 130 of this embodiment, a non-destructive method using optical interference technology can be used to quantitatively determine whether the bonding strength reduction region Ae has been properly formed inside the overlapped wafer T, i.e., whether the first wafer W and the second wafer S have been properly peeled off.

[0055] In the above example, light from the light projector 131 is sequentially irradiated toward a plurality of inspection regions R that are determined in advance on the peripheral portion We (S1 in FIG. 10), and peeling judgment is performed for the plurality of inspection regions R at once (S4 in FIG. 10). However, the method of peeling judgment is not limited to this, and instead of performing peeling judgment for the plurality of inspection regions R at once, a series of operations shown in S1 to S4 in FIG. 10 may be performed sequentially for one inspection region R. More specifically, peeling judgment may be performed for one inspection region R, and when it is determined that the bonding strength reduced region Ae has been appropriately formed in the one inspection region R, peeling judgment may be performed for the next inspection region R.

[0056] Next, the details of each of the above-mentioned feature quantities used in the peeling judgment will be described. Note that the feature quantities shown below may be used alone in the peeling judgment, or two or more feature quantities may be used in combination.

[0057] (1) Half-width First, the half-width as a feature amount will be described. When using the half-width as a feature, first, if there is noise in the actual measured value of the displacement amount data obtained by the inspection device 130 (see FIG. 12), the displacement amount data based on the actual measured value is smoothed as shown in FIG. 13 to obtain a waveform of the displacement amount data (hereinafter referred to as a "displacement amount waveform"). This smoothing process may be omitted, for example, when no noise is observed in the measured values ​​of the variable data (see FIG. 11), in other words, when the measured values ​​of the displacement data are already smooth (when the measured values ​​of the displacement can be regarded as a waveform). Therefore, the measured values ​​of the displacement data may be used after being smoothed, or may be used as the displacement waveform as it is.

[0058] Next, the peeled portion of the first wafer W and the second wafer S is extracted from the horizontal axis of the displacement waveform (the radial position of the overlapped wafer T). As described above, the bonding strength reduced region Ae is formed by irradiating the interface between the first wafer W and the second wafer S with the laser light L1 in a pulsed manner. In the bonding strength reduced region Ae, a peeled portion is formed in which the first wafer W is largely peeled off from the second wafer S (the amount of displacement is large) by direct irradiation with the laser light L1. In addition, around the peeled portion directly below the irradiation with the laser light L1, there are, for example, a portion where the laser light L1 is not directly irradiated due to the pulse interval of the laser light L1, where no peeling has occurred at the interface between the first wafer W and the second wafer S, and a portion where peeling has occurred between the first wafer W and the second wafer S but the amount of peeling (the amount of displacement) is smaller than that of the peeled portion (for convenience, these will be referred to as "non-peeled portion" in the following description).

[0059] In the peeling judgment according to the technology of the present disclosure, a peeling judgment is made as to whether or not the first wafer W and the second wafer S are properly peeled off (whether or not peeling was achieved by the irradiation of the laser beam L1) at the peeled portion in the bonding strength reduced area Ae directly below the irradiation of the laser beam L1. Therefore, in order to properly make a peeling judgment at the peeled portion, a range corresponding to the peeled portion including the position directly below the irradiation of the laser beam L1 is extracted from the displacement amount waveform as shown in FIG.

[0060] The order of smoothing and extraction of the displacement amount data is not limited to the above, and extraction of the peeled portion may be performed prior to smoothing.

[0061] Next, if the bottom value (minimum value) of the displacement (vertical axis) in each extracted peeled portion is a negative value, at least the vertical axis (displacement) of the displacement waveform is converted (standardized or offset) so that the bottom value becomes "0", as shown in Figure 15. Specifically, when standardizing the displacement waveform, the displacement in each peeled portion is converted so that the minimum value on the vertical axis (displacement) is "0" and the maximum value is "1." Furthermore, when offsetting the displacement amount waveform, the displacement amount at each peeled portion is converted so that the minimum value on the vertical axis (displacement amount) becomes "0". In this manner, in converting the vertical axis of the displacement waveform, at least the minimum value of the displacement is converted so that the minimum value of the displacement becomes "0".

[0062] At this time, the minimum value of the horizontal axis (radial position) in each peeled portion may be offset and aligned so that the minimum value of the radial position (horizontal axis) becomes "0".

[0063] Next, the displacement waveform is fitted using the Gaussian function shown in the following formula (1).

number

[0064] Finally, the full width at half maximum (FWHM) of each peeled portion in the bonding strength reduced region Ae is calculated using the following formula (2).

number

[0065] In this embodiment, the full width at half maximum (FWHM) obtained as described above is used as a feature amount, and is compared with a half width that is a threshold value obtained in advance to perform the above-mentioned separation determination. That is, if the obtained full width at half maximum satisfies the threshold value, it is determined that the first wafer W and the second wafer S are appropriately separated, and if the obtained full width at half maximum does not satisfy the threshold value, it is determined that the first wafer W and the second wafer S are not separated.

[0066] In the above example, a Gaussian function is used to calculate the half-width, but instead of this, for example, a Lorentzian function may be used.

[0067] (2) Interquartile range Next, the interquartile range as a feature amount will be described. When the interquartile range and the peak ratio, area or frequency component described later are used as the feature amount, as described later, the displacement amount data based on the actual measured value obtained by the inspection device 130 is smoothed, the peeled portion is extracted, and the vertical axis of the displacement amount waveform is transformed (vertical axis standardization or offset) in the same manner as when the half-width described above is used as the feature amount. In the following, in order to avoid making the explanation using the drawings complicated, the explanation will be given with reference to a simulated waveform (see FIG. 17) that simulates the displacement amount waveform after the smoothing process, extraction process, and vertical axis transformation (standardization is used as an example in the following explanation).

[0068] In FIG. 17, the solid line indicates an example in which the first wafer W and the second wafer S are normally peeled off, and the displacement amount (peak value) at the center of the peeled portion is sufficiently larger than the displacement amount at the end of the peeled portion. The dashed line indicates the first comparative example in which the peeling of the first wafer W and the second wafer S was not performed normally, and although peeling occurred in the center of the peeled portion (the peak value was large), the peeling width (radial width of the peeling) was smaller than in the examples. The dotted line indicates a second comparative example in which the peeling of the first wafer W and the second wafer S was not performed normally, and shows a case in which the displacement amount (peak value) at the center of the peeled portion is not sufficiently large compared to the displacement amount at the end of the peeled portion (the difference in the displacement amounts is small). The semi-dashed line indicates a third comparative example in which the peeling between the first wafer W and the second wafer S was not performed normally, and no peeling between the first wafer W and the second wafer S occurred even in the central part, which corresponds to the peeled part.

[0069] When using the interquartile range as a feature, first, the displacement waveform is obtained by obtaining and smoothing the displacement data from the actual measurements as described above. Then, the peeling portion is extracted from the displacement waveform, and the displacement waveform is standardized to convert the vertical axis (displacement) of the displacement waveform so that the minimum value of the displacement is "0" and the maximum value is "1".

[0070] Next, quartiles Q1 to Q3 (see FIG. 18) of the acquired displacement waveform are acquired. The quartiles indicate the displacement amounts at the median (second quartile Q2), 1 / 4 value (first quartile Q1), and 3 / 4 value (third quartile Q3) when the radial position start point is the minimum value and the end point is the maximum value in the displacement waveform of the extracted peeled portion.

[0071] Next, the acquired second quartile Q2 is compared with the first quartile Q1 and the third quartile Q3. Here, when the peeling width of the peeled portion is small (corresponding to the first comparative example), the first quartile Q1 and the third quartile Q3 are smaller than the second quartile Q2 as shown in Fig. 18. Therefore, by comparing the second quartile Q2 with the first quartile Q1 and the third quartile Q3, it can be determined that the first wafer W and the second wafer S have not been properly peeled off.

[0072] On the other hand, when the first quartile Q1 to the third quartile Q3 are the same, it may be difficult to determine whether peeling has been performed properly (corresponding to the Example), whether the peak value is small (corresponding to the second Comparative Example), or whether peeling has not occurred (corresponding to the third Comparative Example). Therefore, following the comparison of the second quartile Q2 with the first quartile Q1 and the third quartile Q3, the acquisition positions of the first quartile Q1 and the third quartile Q3 are moved toward the end (outside) of the displacement waveform. In other words, the data extraction range is controlled to be expanded from the quartile range toward the end (outside). The acquisition positions of the first quartile Q1' and the third quartile Q3' after the range change can be set to the 10% position and the 90% position of the displacement waveform, as shown as an example in FIG. 19.

[0073] Fig. 20 is a graph showing the first quartile Q1' and the third quartile Q3' after the range change in each of the Example and Comparative Examples 1 to 3. As shown in Fig. 20, it can be seen that the quartile after the range change in the Example is larger than the quartile after the change in the Comparative Examples 1 to 3. This is because, when comparing the Example and Comparative Examples 1 to 3, the rise in the amount of displacement (the slope of the amount of displacement) at the end of the peeled portion is larger.

[0074] Therefore, in this embodiment, the first quartile Q1' and the third quartile Q3' after the range change obtained as described above are used as feature amounts, and are compared with a quartile that is a threshold value obtained in advance, thereby performing the above-mentioned separation determination. That is, if the obtained quartile satisfies the threshold value, it is determined that the first wafer W and the second wafer S are appropriately separated, and if the obtained quartile does not satisfy the threshold value, it is determined that the first wafer W and the second wafer S are not separated. It is desirable that the threshold value used for judging peeling is preset within a range between the quartiles in the embodiment shown in FIG. 20 and the quartiles in Comparative Example 1, for example.

[0075] (3) Peak ratio Next, the peak ratio as a feature amount will be described. When the peak ratio is used as a feature, first, as described above, a displacement waveform is obtained by acquiring and smoothing displacement data based on actual measurements obtained by the inspection device 130. Then, peeled portions are extracted from the displacement waveform, and the displacement waveform is standardized to convert the vertical axis (displacement) of the displacement waveform so that the minimum displacement value is "0" and the maximum displacement value is "1." Subsequently, the first quartile Q1' and the third quartile Q3' after the range change are obtained by the same method as in the case where the interquartile range is used as the feature amount described above.

[0076] Next, in this embodiment, instead of using the acquired quartiles as they are as feature quantities, a peak ratio (PR) is calculated using the following formula (3).

number

[0077] Fig. 21 is a graph showing the peak ratios (PR) in each of the example and comparative examples 1 to 3. As shown in Fig. 21, it can be seen that the peak ratio in the example is larger than the peak ratios in comparative examples 1 to 3. This is because, in the above formula (3), as the peeling progresses at the end of the peeled portion of the inspected laminated wafer T and the displacement amount increases, the difference from the peak value (displacement amount) of the displacement amount in the ideal state decreases, and the calculated peak ratio approaches "1".

[0078] Therefore, in this embodiment, the peak ratio obtained as described above is used as a feature amount, and is compared with a previously obtained threshold peak ratio to perform the above-mentioned separation determination. That is, if the obtained peak ratio is larger than the threshold peak ratio, it is determined that the first wafer W and the second wafer S are appropriately separated, and if the obtained peak ratio is smaller than the threshold peak ratio, it is determined that the first wafer W and the second wafer S are not separated. It is desirable that the threshold value used for judging peeling is preset within a range between the peak ratio in the embodiment shown in FIG. 21 and the peak ratio in Comparative Example 1, for example.

[0079] (4)Area Next, the area as a feature amount will be described. When the area is used as a feature, first, as described above, a displacement waveform is obtained by acquiring and smoothing displacement data based on actual measurements obtained by the inspection device 130. Then, peeled portions are extracted from the displacement waveform, and the displacement waveform is standardized to convert the vertical axis (displacement) of the displacement waveform so that the minimum displacement value is "0" and the maximum displacement value is "1."

[0080] Next, the acquired deformation amount waveform (see FIG. 17) at the peeled portion is approximated by a higher-order function (see FIG. 22). Furthermore, the area of ​​region X (see FIG. 22) surrounded by the graph and coordinate axes indicated by the obtained approximation formula is calculated. The calculated area of ​​region X corresponds to the cross-sectional area of ​​the peeled portion of the bonding strength reduction region Ae formed by the irradiation of the laser beam L1, in other words, the cross-sectional area of ​​the air layer (void).

[0081] Fig. 23 is a graph showing the area of ​​region X obtained in each of the Example and Comparative Examples 1 to 3. As shown in Fig. 23, it can be seen that the area of ​​region X in the Example is larger than the area of ​​region X in Comparative Examples 1 to 3. This is because the peak value of the displacement amount waveform in the Example is larger than the peak value of the displacement amount waveform in Comparative Examples 1 to 3, in other words, the volume of the formed peeled portion is larger.

[0082] Therefore, in this embodiment, the area of ​​the region X obtained as described above is used as a feature amount, and is compared with a previously acquired threshold area to perform the above-mentioned separation determination. That is, if the obtained area of ​​the region X is larger than the threshold area, it is determined that the first wafer W and the second wafer S are appropriately separated, and if the obtained area of ​​the region X is smaller than the threshold area, it is determined that the first wafer W and the second wafer S are not separated. The area used for peeling judgment is desirably set in advance within a range between the area in the embodiment shown in FIG. 23 and the area in Comparative Example 1, for example.

[0083] (5) Frequency components Next, frequency components as feature quantities will be described. When using frequency components as features, first, as described above, a displacement waveform is obtained by acquiring and smoothing displacement data based on actual measurements obtained by the inspection device 130. Then, peeled portions are extracted from the displacement waveform, and the displacement waveform is standardized to convert the vertical axis (displacement) of the displacement waveform so that the minimum and maximum displacement values ​​are "0" and "1".

[0084] Next, a signal wave is created (see FIG. 24) from the acquired deformation waveform (see FIG. 17) at the peeled portion. Specifically, the deformation waveform shown in FIG. 17 is arranged alternately on the positive side and the negative side in the time axis direction (horizontal axis in FIG. 24) so ​​that the signal wave forms a half cycle. Furthermore, the created signal wave is Fourier transformed to acquire the frequency spectrum of the signal wave.

[0085] 25 shows the frequency spectrum obtained in each of the Example and Comparative Examples 1 to 3. As can be seen from the frequency spectrum obtained by Fourier transform, the frequency components obtained from the displacement waveforms of the Example and Comparative Examples 1 to 3 are different. This is considered to be due to, for example, differences in the peak value of the signal wave and the inclination angle of the rising portion of the displacement waveform.

[0086] Therefore, in this embodiment, the difference in the frequency spectrum acquired as described above, that is, the frequency components of the displacement amount waveform, are used as features to perform the above-mentioned separation judgment. For example, the acquired frequency components are compared with frequency components acquired when the first wafer W and the second wafer S, which serve as a reference, are properly separated, and if the similarity of these frequency components meets a predetermined threshold (the similarity is large), it is judged that the first wafer W and the second wafer S are properly separated, and if the threshold is not met (the similarity is small), it is judged that the first wafer W and the second wafer S are not separated.

[0087] In the above description, a signal wave is created from the deformation amount waveform shown in Fig. 17, and a frequency spectrum is acquired. However, if the state of separation between the first wafer W and the second wafer S can be detected by the frequency spectrum obtained by Fourier transform, in other words, if a difference in frequency components between when separation occurs appropriately and when separation does not occur can be recognized, then the graphs showing the actual measured values ​​of the displacement amount data shown in Figs. 11 and 12, for example, may be Fourier transformed.

[0088] (6) Convexity statistics Next, the convexity statistics as a feature amount will be described. When using the convexity statistics as a feature amount, first, the displacement amount is measured by the inspection device 130, and the actual value of the displacement amount data is obtained. In this embodiment, in order to make it easier to grasp the displacement amount, the back surface Wb of the first wafer W is ground, and then the displacement amount is measured by the inspection device 130. Note that grinding the back surface Wb of the first wafer W before measuring the displacement amount is optional and may be omitted. Next, the displacement amount data is smoothed as described above, and a displacement amount waveform is obtained.

[0089] Fig. 26 is a graph showing a topography image of the displacement amount acquired by the inspection device 130 and a displacement amount waveform in a state in which the first wafer W and the second wafer S are peeled off in one inspection region R shown in Fig. 9. In the topography image shown in Fig. 26(a), the peeled portion P1 shown in dark gray is the portion where the first wafer W and the second wafer S are peeled off. In this one inspection region R, the first wafer W and the second wafer S are completely peeled off. Furthermore, in one inspection region R, displacement waveforms are obtained at a plurality of, for example, five, measurement points. The displacement waveform shown in Fig. 26(b) shows the displacement waveform at measurement point (1) among measurement points (1) to (5) in the topography image of Fig. 26(a). A protrusion Q1 in the displacement waveform has a depth (depth direction displacement) of H1 and a width (width direction displacement) of D1, indicating peeling between the first wafer W and the second wafer S. The width direction displacement of protrusion Q1 is, in other words, the width of the bonding strength reduction region Ae. 26(a), the vertical and horizontal axes indicate the radial position of the overlapped wafer T. In addition, in the displacement amount waveform in FIG. 26(b), the vertical axis indicates the displacement amount, and the horizontal axis indicates the radial position of the overlapped wafer T.

[0090] Fig. 27 is a graph showing a topography image of the displacement amount acquired by the inspection device 130 and a displacement amount waveform in a state in which the first wafer W and the second wafer S are partially peeled off in another inspection region R shown in Fig. 9. In the topography image shown in Fig. 27(a), the partially peeled part P2, which is a mixture of dark gray and light gray, is a part where the first wafer W and the second wafer S are partially peeled off. In this other inspection region R, there is a mixture of parts where the first wafer W and the second wafer S are peeled off and parts where they are not peeled off, and this state is called partial peeling. In addition, displacement waveforms are obtained at a plurality of, for example, five, measurement points in another inspection region R. The displacement waveform shown in Fig. 27(b) shows the displacement waveform at measurement point (1) among measurement points (1) to (5) in the topography image in Fig. 27(a). The depth H2 of convex portion Q2 in the displacement waveform is smaller than the depth H1 of convex portion Q1, and the width D2 of convex portion Q2 is smaller than the width D1 of convex portion Q1, indicating partial peeling between the first wafer W and the second wafer S.

[0091] In this embodiment, the acquired displacement waveform is used as is to calculate the convexity statistics. Note that the peeled portion may be extracted from the displacement waveform.

[0092] As described above, the first wafer W and the second wafer S are judged for separation by acquiring the displacement amount waveforms at multiple measurement points in the inspection area R. Specifically, in the separation judgment, in addition to the above-mentioned separation state and partial separation state, an unseparated state is also judged. An unseparated state is a state in which the first wafer W and the second wafer S are not separated at all.

[0093] The determination of peeling or non-peeling is made based on the average value of the depth direction displacement of the convex portion for the displacement waveforms of multiple measurement points. If the absolute value of the average value of the depth direction displacement is equal to or greater than a predetermined threshold (or equal to or less than the threshold), it is determined that peeling has occurred. On the other hand, if the absolute value of the average value of the depth direction displacement is smaller than the threshold (or larger than the threshold), it is determined that non-peeling has occurred. FIG. 28 is a graph showing the average value of the depth direction displacement of the convex portion obtained by varying the irradiation conditions of the laser light when forming the bonding strength reduced region Ae. In the graph, the vertical axis shows the average value of the depth direction displacement of the convex portion, and the horizontal axis shows the irradiation conditions of the laser light. The irradiation conditions of the laser light were varied from No. 1 to No. 9. In this case, in the cases of No. 1 to No. 3 and No. 5 to No. 9, the absolute value of the average value of the depth direction displacement is equal to or greater than the threshold value, and it is determined that peeling has occurred. On the other hand, in the case of No. 4, the absolute value of the average value of the depth direction displacement is smaller than the threshold value, and it is determined that peeling has not occurred. In this example, it is also possible to determine that peeling has occurred when the average value of the depth direction displacement is negative, and that peeling has not occurred when the average value of the depth direction displacement is positive.

[0094] The determination of peeling and partial peeling is made based on the standard deviation of the width direction displacement of the convex portion for the displacement waveforms at multiple measurement points. If the standard deviation of the width direction displacement is equal to or less than a predetermined threshold (or equal to or greater than the threshold), it is determined to be peeling. On the other hand, if the standard deviation of the width direction displacement is greater than the threshold (or less than the threshold), it is determined to be partial peeling. 29 is a graph showing the standard deviation of the width direction displacement of the convex portion obtained by varying the irradiation conditions of the laser beam when forming the bonding strength reduced region Ae. In the graph, the vertical axis indicates the standard deviation of the width direction displacement of the convex portion, and the horizontal axis indicates the irradiation conditions of the laser beam. The irradiation conditions of the laser beam were varied from No. 1 to No. 9. In this case, in the cases of No. 1, No. 5, and No. 6, the standard deviation of the width direction displacement is equal to or less than the threshold value, and it is determined that peeling has occurred. On the other hand, in the cases of No. 2 to No. 4 and No. 7 to No. 9, the standard deviation of the width direction displacement is greater than the threshold value, and it is determined that partial peeling has occurred.

[0095] (Functions and Effects of the Substrate Processing Method According to the Technique of the Present Disclosure) As described above, according to the wafer processing system 1 relating to the technology of the present disclosure, it is possible to quantitatively determine, using the inspection device 130, whether or not the first wafer W and the second wafer S have been properly peeled off in the bonding strength reduction region Ae formed by the interface modification device 50 as described above.

[0096] 9, the description has been given taking as an example a case where the inspection regions R are set at four locations in the circumferential direction of the overlapped wafer T, but the number of the set inspection regions R is not limited thereto as long as it is possible to detect that the bonding strength reduction region Ae is appropriately formed all around the overlapped wafer T. Specifically, the inspection regions R are set at least at two locations in the circumferential direction of the overlapped wafer T, and preferably all around the overlapped wafer T.

[0097] In the above embodiment, the inspection device 130 for inspecting the bonding strength reduced region Ae is disposed inside the interface modification device 50, but the inspection device 130 may be disposed outside the interface modification device 50. The inspection device 130 may be disposed independently in, for example, the processing station 3 of the wafer processing system 1, or may be disposed independently outside the wafer processing system 1. In this case, a first inspection device that inspects the bonding strength reduced area Ae using light that is reflective to the first wafer W, and a second inspection device that inspects the bonding strength reduced area Ae using light that is transparent to the first wafer W may be independently disposed in the processing station 3. In this case, even if, for example, one of the devices cannot be used due to maintenance or a malfunction, or if there is a change in the structure of the first wafer W that constitutes the inspected laminated wafer T, the inspection of the bonding strength reduced area Ae can be performed while continuing wafer processing in the wafer processing system 1.

[0098] In the above embodiment, the irradiation conditions of the laser beam when forming the bonding strength reduced region Ae may be feedback-controlled based on at least one of the displacement amount measured in S1 of Fig. 10 and the feature amount acquired in S3 of Fig. 10. The irradiation conditions of the laser beam include, for example, the power of the laser beam, the voltage of the laser beam, the duty ratio of the laser beam, the frequency of the laser beam, the irradiation pitch of the laser beam, and the like.

[0099] For example, when the displacement amount is smaller than a predetermined threshold, the laser light irradiation conditions are feedback-controlled.Similarly, when the feature amount is smaller than a predetermined threshold, the laser light irradiation conditions are feedback-controlled. For example, when the inspection device 130 is disposed inside the interface modification device 50 as in the above embodiment, the control device 51 or the control device 90 feedback-controls the laser light irradiation conditions. Also, when the inspection device 130 is disposed independently in the processing station 3 of the wafer processing system 1, the control device 90 feedback-controls the laser light irradiation conditions. Also, when the inspection device 130 is disposed independently outside the wafer processing system 1, a control device (not shown) provided outside the wafer processing system 1 feedback-controls the laser light irradiation conditions.

[0100] In the above feedback control, the threshold value of the displacement amount and the threshold value of the feature amount may be stored in a database of the control device 90 for each condition of the overlapped wafer T. For example, the threshold value varies depending on the type and thickness of the film formed on the surface of the first wafer W of the overlapped wafer T. Therefore, a threshold value that matches the conditions of the overlapped wafer T to be processed is read from the database, and the displacement amount or the feature amount is compared with the read threshold value to perform feedback control.

[0101] When the parameter of the laser light irradiation condition that is feedback controlled is greater than a predetermined threshold value, for example, it may be determined that an apparatus abnormality has occurred, and an alarm or a maintenance message may be issued. Such an alarm or maintenance message may be issued, for example, by the control device 90.

[0102] Also, for example, when the displacement amount is smaller than a predetermined threshold at only some of the measurement points among the multiple measurement points, it may be determined that there is an abnormality in the device or the wafer, and an alarm may be issued. Similarly, when the feature amount is smaller than a predetermined threshold at only some of the measurement points, an alarm may be issued. Such an alarm may be issued by, for example, the control device 90.

[0103] Also, for example, when processing a plurality of overlapped wafers T, if the displacement amount of only some of the overlapped wafers T is smaller than a predetermined threshold, it may be determined that there is an abnormality in the apparatus or the wafer, and an alarm may be issued. Similarly, if the feature amount of only some of the overlapped wafers T is smaller than a predetermined threshold, an alarm may be issued. Such an alarm is issued, for example, by the control device 90.

[0104] The wafer processing system 1 of the above embodiment may be provided with a display panel (not shown). The display panel is, for example, a monitor or a touch panel, and may be directly attached to the wafer processing system 1 or may be capable of being viewed remotely. The display panel displays various information such as the above-mentioned displacement amount, feature amount, feedback control, etc. Also, an operator can operate the display panel to set, for example, the irradiation conditions of the laser light.

[0105] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. For example, the components of the above-described embodiments may be arbitrarily combined. From such an arbitrary combination, the actions and effects of each of the components in the combination can be obtained as a matter of course, and other actions and effects that are obvious to a person skilled in the art from the description of this specification can be obtained.

[0106] In addition, the effects described in this specification are merely explanatory or exemplary and are not limiting. In other words, the technology according to the present disclosure may achieve other effects that are apparent to a person skilled in the art from the description of this specification in addition to or in place of the above effects. [Explanation of symbols]

[0107] 1. Wafer Processing System 50 Interface Modification Equipment 51 Control device 90 Control device 130 Inspection Equipment Ae Welding force decrease area L1 (interface) laser light S 2nd wafer T Polymerized Wafer W First wafer We Periphery

Claims

1. A method for treating a laminated substrate in which a first substrate and a second substrate are bonded together, comprising the steps of: a step of irradiating a peripheral portion of the first substrate with a laser beam toward an interface between the first substrate and the second substrate to form a bonding strength reduced region at the interface where the first substrate and the second substrate are peeled off; measuring the amount of displacement of the peripheral portion where the bonding strength reduced region is formed; acquiring a feature amount for detecting peeling between the first substrate and the second substrate based on the displacement amount; and comparing the feature amount with a predetermined threshold value to determine peeling between the first substrate and the second substrate.

2. The step of acquiring the feature amount includes: acquiring a displacement waveform from the actual measurement value of the displacement; converting at least a minimum value of the displacement in the displacement waveform; fitting the displacement waveform with a Gaussian function; and obtaining a half-width from a standard deviation of the displacement waveform after fitting; The processing method according to claim 1 , wherein in the step of determining peeling, the half-width is used as the feature amount and compared with the threshold value.

3. The step of acquiring the feature amount includes: acquiring a displacement waveform from the actual measurement value of the displacement; converting at least a minimum value of the displacement in the displacement waveform; Dividing the separation portion between the first substrate and the second substrate in the displacement waveform by an interquartile range; obtaining quartile values ​​from the interquartile range; and and widening the interquartile range to change the positions at which the first and third quartiles of the quartiles are obtained; The processing method according to claim 1 , wherein in the step of determining peeling, the first quartile value and the third quartile value after changing the acquisition position are used as the feature amount and compared with the threshold value.

4. The step of acquiring the feature amount includes: acquiring a displacement waveform from the actual measurement value of the displacement; converting at least a minimum value of the displacement in the displacement waveform; Dividing the separation portion between the first substrate and the second substrate in the displacement waveform by an interquartile range; obtaining quartile values ​​from the interquartile range; and widening the interquartile range to change the positions at which the first and third quartiles of the quartiles are obtained; calculating a ratio of the first quartile value and the third quartile value after changing the acquisition position to a second quartile value of the quartile values ​​acquired in advance at the time of peeling off the first substrate and the second substrate; The processing method according to claim 1 , wherein in the step of determining peeling, the ratio is used as the feature amount and compared with the threshold value.

5. The step of acquiring the feature amount includes: acquiring a displacement waveform from the actual measurement value of the displacement; converting at least a minimum value of the displacement in the displacement waveform; approximating the displacement waveform by a high-order function; Calculating the area of ​​a region surrounded by the approximated displacement amount and coordinate axes; The processing method according to claim 1 , wherein in the step of determining peeling, the area is used as the feature amount and compared with the threshold value.

6. The step of acquiring the feature amount includes: acquiring a displacement waveform from the actual measurement value of the displacement; converting at least a minimum value of the displacement in the displacement waveform; generating a signal wave based on the displacement waveform; and performing a Fourier transform on the signal wave to obtain a frequency spectrum. The processing method according to claim 1 , wherein in the step of determining peeling, peeling between the first substrate and the second substrate is determined using a frequency component obtained from the frequency spectrum as the feature amount.

7. In the step of measuring the amount of displacement, the amount of displacement is measured at a plurality of points on the peripheral portion, The step of acquiring the feature amount includes: acquiring a displacement waveform from the actual measurement value of the displacement; obtaining either an average value of depths of convex portions in the displacement amount waveforms at the multiple points or a standard deviation of widths of the convex portions in the displacement amount waveforms at the multiple points; The processing method according to claim 1 , wherein in the step of determining peeling, one of an average value of the depths of the protrusions and a standard deviation of the widths of the protrusions is used as the feature amount and compared with the threshold value.

8. The processing method according to claim 7 , wherein in the step of determining separation, an average value of the depths of the protrusions is compared with the threshold value to determine whether or not the first substrate and the second substrate have been separated.

9. The processing method according to claim 7 , wherein in the step of determining peeling, a standard deviation of widths of the convex portions is compared with the threshold value to determine peeling or partial peeling between the first substrate and the second substrate.

10. The step of acquiring the feature amount includes: The processing method according to any one of claims 1 to 9, further comprising smoothing noise in the actual measured values ​​of the amount of displacement.

11. 10. The processing method according to claim 1, further comprising feedback-controlling an irradiation condition of the laser light in the step of forming the bonding strength reduced region, based on at least one of the displacement amount and the feature amount.

12. The processing method according to any one of claims 1 to 9, further comprising issuing an alarm when the peeling is abnormal based on at least one of the displacement amount and the feature amount.

13. forming an edge modification layer along a boundary between a peripheral portion of the first substrate and a central portion of the first substrate; The processing method according to any one of claims 1 to 9, further comprising removing the peripheral portion starting from the peripheral modified layer and the bonding strength reduced region.

14. A processing system for processing a laminated substrate in which a first substrate and a second substrate are bonded together, comprising: an interface modification device that irradiates a laser beam toward an interface between the first substrate and the second substrate in a peripheral portion of the first substrate to form a bonding strength reduced region at the interface where the first substrate and the second substrate are peeled off; an inspection device that inspects the first substrate and the second substrate for peeling in the bonding strength reduced region; A control device, The control device, when inspecting the peeling by the inspection device, A control for measuring a displacement amount of the peripheral portion where the bonding strength reduced region is formed; Control for acquiring a feature amount for detecting peeling between the first substrate and the second substrate based on the amount of displacement; and and comparing the feature amount with a predetermined threshold value to determine whether or not peeling has occurred between the first substrate and the second substrate.

15. The control device includes: When acquiring the feature amount, A control for acquiring a displacement amount waveform from the actual measurement value of the displacement amount; A control for converting at least a minimum value of the displacement amount in the displacement amount waveform; Control of fitting the displacement waveform with a Gaussian function; and performing control to obtain a half-width from a standard deviation of the displacement waveform after fitting; When judging the peeling, The processing system according to claim 14 , wherein control is executed to compare the half-width as the feature amount with the threshold value.

16. The control device includes: When acquiring the feature amount, A control for acquiring a displacement amount waveform from the actual measurement value of the displacement amount; A control for converting at least a minimum value of the displacement amount in the displacement amount waveform; Controlling the separation portion between the first substrate and the second substrate in the displacement amount waveform by dividing the separation portion into an interquartile range; A control for obtaining an interquartile value from the interquartile range; and executing control to expand the interquartile range and change the acquisition positions of the first quartile value and the third quartile value of the quartile value; When judging the peeling, The processing system according to claim 14 , further comprising a control for performing a comparison with the threshold value using the first quartile value and the third quartile value after the acquisition position is changed as the feature amount.

17. The control device includes: When acquiring the feature amount, A control for acquiring a displacement amount waveform from the actual measurement value of the displacement amount; A control for converting at least a minimum value of the displacement amount in the displacement amount waveform; Controlling the separation portion between the first substrate and the second substrate in the displacement amount waveform by dividing the separation portion into an interquartile range; A control for obtaining an interquartile value from the interquartile range; Control of expanding the interquartile range to change the acquisition positions of the first quartile value and the third quartile value of the quartile value; and calculating a ratio of the first quartile value and the third quartile value after the change of the acquisition position to a second quartile value of the quartile values ​​acquired in advance at the time of peeling the first substrate and the second substrate; When judging the peeling, The processing system according to claim 14 , wherein control is executed to compare the ratio with the threshold value as the characteristic amount.

18. The control device includes: When acquiring the feature amount, A control for acquiring a displacement amount waveform from the actual measurement value of the displacement amount; A control for converting at least a minimum value of the displacement amount in the displacement amount waveform; A control for approximating the displacement waveform by a high-order function; and calculating an area of ​​a region surrounded by the approximated displacement amount and the coordinate axes. When judging the peeling, The processing system according to claim 14 , wherein control is executed to compare the area as the feature amount with the threshold value.

19. The control device includes: When acquiring the feature amount, A control for acquiring a displacement amount waveform from the actual measurement value of the displacement amount; A control for converting at least a minimum value of the displacement amount in the displacement amount waveform; A control for generating a signal wave based on the displacement waveform; and performing a Fourier transform on the signal wave to obtain a frequency spectrum. When judging the peeling, The processing system according to claim 14 , wherein control is executed to determine peeling between the first substrate and the second substrate, using a frequency component obtained from the frequency spectrum as the feature amount.

20. The control device includes: When measuring the amount of displacement, Executing a control to measure the amount of displacement at a plurality of points in the peripheral portion; When acquiring the feature amount, A control for acquiring a displacement amount waveform from the actual measurement value of the displacement amount; and acquiring either an average value of depths of convex portions in the displacement amount waveforms at the multiple points or a standard deviation of widths of the convex portions in the displacement amount waveforms at the multiple points; When judging the peeling, The processing system according to claim 14 , wherein control is executed to compare one of an average depth of the convex portions and a standard deviation of the width of the convex portions as the feature amount with the threshold value.

21. The control device includes: When judging the peeling, The processing system according to claim 20 , further comprising a control for comparing the average depth of the convex portions with the threshold value to determine whether or not the first substrate and the second substrate have been peeled off.

22. The control device includes: When judging the peeling, The processing system according to claim 20 , further comprising a control for comparing a standard deviation of widths of the convex portions with the threshold value to determine whether or not separation or partial separation has occurred between the first substrate and the second substrate.

23. The control device includes: When acquiring the feature amount, The processing system according to any one of claims 14 to 22, further comprising a control for smoothing noise in the actual measured value of the amount of displacement.

24. The processing system according to any one of claims 14 to 22, wherein the control device feedback controls the irradiation conditions of the laser light when forming the bonding strength reduction region based on at least one of the displacement amount and the feature amount.

25. The processing system according to any one of claims 14 to 22, wherein the control device executes control to issue an alarm if the peeling is abnormal, based on at least one of the displacement amount and the feature amount.

26. an internal modification device for forming a peripheral modification layer along a boundary between a peripheral portion of the first substrate and a central portion of the first substrate; 23. The processing system according to claim 14, further comprising: a peripheral removal device that removes the peripheral portion from the peripheral modified layer and the bonding strength reduced region.

27. 1. An inspection apparatus for inspecting peeling between a first substrate and a second substrate in a bonded laminated substrate in a peripheral portion of the first substrate and a bonding strength reduced region formed at an interface between the first substrate and the second substrate, comprising: a measuring unit for measuring a displacement amount of the peripheral portion where the bonding strength reduced region is formed; A control unit, The control unit, when inspecting the peeling by the inspection device, Control of measuring the displacement amount by the measurement unit; Control for acquiring a feature amount for detecting peeling between the first substrate and the second substrate based on the amount of displacement; and and comparing the feature amount with a predetermined threshold value to determine whether or not peeling has occurred between the first substrate and the second substrate.

Citation Information

Patent Citations

  • Substrate processing system, substrate processing method, and computer storage medium

    WO2019176589A1

Cited By

  • Method for extracting line scan data in raman hyperspectral measurement device

    KR102877820B1

  • Laser machining device, substrate processing system, and laser machining method

    WO2026126805A1