Modified cellulose fiber and resin composition containing modified cellulose fiber

By bonding amines with hydrocarbon groups to anion-modified cellulose fibers, the dispersibility and strength of cellulose-resin composites are enhanced, addressing the issue of aggregate formation and improving material strength.

JP2024163870APending Publication Date: 2024-11-22KAO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024076405
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-05-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When cellulose fibers are composited with resin, poor dispersibility can lead to aggregate formation, reducing the strength of the composite material.

Method used

A modified cellulose fiber is developed by bonding two or more types of amines with chain hydrocarbon or alicyclic hydrocarbon groups to an anion-modified cellulose fiber via ionic or amide bonds, enhancing dispersibility without the need for a curing agent.

Benefits of technology

The modified cellulose fiber exhibits excellent dispersibility in resin, reducing aggregate formation and improving the mechanical strength of the composite material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163870000001
    Figure 2024163870000001
  • Figure 2024163870000002
    Figure 2024163870000002
  • Figure 2024163870000003
    Figure 2024163870000003
Patent Text Reader

Abstract

To provide a modified cellulose fiber excellent in dispersibility and a resin composition containing the modified cellulose fiber.SOLUTION: Modified cellulose fibers formed by bonding two or more amines having a chain hydrocarbon group or an alicyclic hydrocarbon group and an anionic modified cellulose fiber via an ionic bond or an amide bond, and a modified cellulose fiber dispersion containing the modified cellulose fiber and an organic medium, a modified cellulose fiber dispersion containing such modified cellulose fiber and an organic solvent, and a resin composition containing such modified cellulose fibers and resins.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a modified cellulose fiber and a resin composition containing the modified cellulose fiber. [Background technology]

[0002] Traditionally, plastic materials derived from petroleum, a finite resource, have been widely used, but in recent years, technologies with less impact on the environment have come into the spotlight. Against this technological background, materials made from cellulose fibers, a biomass that exists in abundance in nature, have been attracting attention.

[0003] For example, cellulose nanofibers (CNFs) have excellent strength and are known to act as reinforcing materials when added in small amounts to composites with resins, etc. (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2006-241450 A Summary of the Invention [Problem to be solved by the invention]

[0005] There are various types of resins currently in use, each with different characteristics and properties. When cellulose fibers are composited with resins, if the fibers are poorly dispersible in the resin, agglomerates may form, which may lead to a decrease in strength. Therefore, there is a demand for further improvement in the dispersibility of cellulose fibers. The present invention relates to a modified cellulose fiber having excellent dispersibility and a resin composition containing the modified cellulose fiber. [Means for solving the problem]

[0006] The present invention relates to the following [1] to [6]. [1] A modified cellulose fiber comprising two or more amines having a chain hydrocarbon group or an alicyclic hydrocarbon group and an anion-modified cellulose fiber bonded via an ionic bond or an amide bond. [2] The modified cellulose fiber according to [1], wherein the amine comprises a secondary amine and a tertiary amine. [3] The modified cellulose fiber according to [2], wherein the molar ratio of the secondary amine to the tertiary amine (secondary amine / tertiary amine) is 10 / 90 or more and 90 / 10 or less. [4] A modified cellulose fiber dispersion comprising the modified cellulose fiber according to any one of [1] to [3] above and an organic medium. [5] A modified cellulose fiber dispersion comprising the modified cellulose fiber according to any one of [1] to [3] above and an organic solvent. [6] A resin composition comprising the modified cellulose fiber according to any one of [1] to [3] above and a resin. Effect of the Invention

[0007] According to the present invention, it is possible to provide a modified cellulose fiber having excellent dispersibility and a resin composition containing the modified cellulose fiber. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The inventors have investigated the blending of various resins with modified cellulose fibers and have found that when modified cellulose fibers are blended with a resin that uses a hardener, the dispersibility of the modified cellulose fibers decreases and agglomerates may form. As a result of further investigations, the inventors have unexpectedly found that modified cellulose fibers prepared using two or more amines having a chain hydrocarbon group or an alicyclic hydrocarbon group have excellent dispersibility in resins that use a curing agent, and can reduce the formation of aggregates.

[0009] The mechanism by which the modified cellulose fiber of the present invention exhibits such excellent dispersibility is not clear, but the following is presumed. That is, it is considered that the ionic interaction between the amine having high compatibility with hydrophobic media such as resins and the anionic groups on the cellulose fibers among the two or more amines exhibits repulsive forces between the cellulose fibers. On the other hand, it is considered that the amine having low compatibility with hydrophobic media interacts with acids other than the cellulose fibers or alkalis other than the amines used to modify the cellulose, thereby preventing the acids other than the cellulose fibers or alkalis other than the amines used to modify the cellulose from interfering with the ionic interaction. It is presumed that the difference in compatibility between the two or more amines and hydrophobic media is one of the factors that exhibit the above effect.

[0010] [Modified cellulose fibers] The modified cellulose fiber in the present invention is a cellulose fiber in which two or more amines having a chain hydrocarbon group or an alicyclic hydrocarbon group are bonded to an anion-modified cellulose fiber, and the amines are bonded to the anion-modified cellulose fiber via an ionic bond or an amide bond. In this specification, the chain hydrocarbon group or the alicyclic hydrocarbon group may be referred to as a "modifying group".

[0011] The amine is preferably bonded to the anionic group of the anion-modified cellulose fiber via an ionic bond or an amide bond, and the amine is preferably bonded to the anionic group of the anion-modified cellulose fiber via a hydroxymethyl group (-CH 2 It is more preferred that the alkyl group (--OH) is attached to the carboxy group which has been converted to a carboxy group (--COOH).

[0012] In this specification, the term "glucose portion" means a portion consisting of glucose units, and in the case of unmodified cellulose fibers, it means the entire glucose unit, in the case of anion-modified cellulose fibers, it means the entire glucose unit including the anionic group bonded to the glucose unit, and in the case of modified cellulose fibers, it means the entire glucose unit excluding the chain hydrocarbon group or alicyclic hydrocarbon group bonded to the glucose unit. That is, the glucose unit in this specification also includes glucose units in which the hydroxymethyl group has been converted to a carboxy group.

[0013] The amine preferably includes a primary amine, a secondary amine, or a tertiary amine. When a primary amine is bonded to a carboxy group via an ionic bond, the bond pattern is as shown in the following formula a; when a secondary amine is bonded to a carboxy group via an ionic bond, the bond pattern is as shown in the following formula b; and when a tertiary amine is bonded to a carboxy group via an ionic bond, the bond pattern is as shown in the following formula c. The modifying groups 1 to 3 are chain hydrocarbon groups or alicyclic hydrocarbon groups. The modifying groups 1 to 2 in formula b may be the same or different, but are preferably the same. The modifying groups 1 to 3 in formula c may be the same or different, but are preferably the same.

[0014] [ka]

[0015] When a primary amine is bonded to a carboxy group via an amide bond, the bond is as shown in the following formula d, and when a secondary amine is bonded to a carboxy group via an amide bond, the bond is as shown in the following formula e. The modifying groups 1 and 2 are chain hydrocarbon groups or alicyclic hydrocarbon groups. The modifying groups 1 and 2 in formula e may be the same or different, but are preferably the same.

[0016] [ka]

[0017] (modifying group) The modifying group in the present invention is a chain hydrocarbon group or an alicyclic hydrocarbon group. One or a combination of two or more of these modifying groups may be bonded to the anion-modified cellulose fiber.

[0018] (a) Hydrocarbon group The chain hydrocarbon group may be a monovalent group, such as a linear or branched chain saturated hydrocarbon group, or a linear or branched chain unsaturated hydrocarbon group. The alicyclic hydrocarbon group may be a monovalent group, such as a saturated or unsaturated alicyclic hydrocarbon group, with a saturated alicyclic hydrocarbon group being preferred. From the viewpoint of suppressing the formation of aggregates, the number of carbon atoms in each hydrocarbon group is preferably 6 or more, more preferably 7 or more, and even more preferably 8 or more, and from the same viewpoint, it is preferably 22 or less, more preferably 18 or less, and even more preferably 14 or less. The hydrocarbon group may have a substituent described later, and a part of the hydrocarbon group may be substituted with a hydrogen nitride group.

[0019] The linear or branched chain saturated hydrocarbon group is preferably a linear chain saturated hydrocarbon group from the viewpoint of suppressing the formation of aggregates. Examples of the linear saturated hydrocarbon group include a propyl group, an isopropyl group, a butyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, a pentyl group, a tert-pentyl group, an isopentyl group, a hexyl group, an isohexyl group, a heptyl group, an octyl group, a 2-ethylhexyl group, a nonyl group, a decyl group, a dodecyl group, a tridecyl group, a tetradecyl group, an octadecyl group, a docosyl group, and an octacosanyl group.

[0020] Examples of the chain unsaturated hydrocarbon group include a propenyl group, a butenyl group, an isobutenyl group, an isoprenyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, a dodecenyl group, a tridecenyl group, a tetradecenyl group, and an octadecenyl group.

[0021] Examples of the saturated alicyclic hydrocarbon group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclononyl group, a cyclodecyl group, a cyclododecyl group, a cyclotridecyl group, a cyclotetradecyl group, and a cyclooctadecyl group.

[0022] (b) Further Substituents The modifying group may further have a substituent. Examples of the substituent include alkoxy groups having 1 to 6 carbon atoms, such as methoxy, ethoxy, propoxy, isopropoxy, butoxy, isobutoxy, sec-butoxy, tert-butoxy, pentyloxy, isopentyloxy, and hexyloxy; methoxycarbonyl, ethoxycarbonyl, propoxycarbonyl, isopropoxycarbonyl, butoxycarbonyl, isobutoxycarbonyl, sec-butoxycarbonyl, and tert-butoxy. Examples of such groups include alkoxy-carbonyl groups having 1 to 6 carbon atoms in the alkoxy group, such as t-butoxycarbonyl, pentyloxycarbonyl, and isopentyloxycarbonyl groups; halogen atoms, such as fluorine, chlorine, bromine, and iodine atoms; acyl groups having 1 to 6 carbon atoms, such as acetyl and propionyl groups; aralkyl groups; aralkyloxy groups; alkylamino groups having 1 to 6 carbon atoms; dialkylamino groups having an alkyl group of 1 to 6 carbon atoms; and hydroxy groups.

[0023] (Anion-modified cellulose fiber) Anion-modified cellulose fibers are cellulose fibers having an anionic group, such as one or more groups selected from the group consisting of a carboxy group, a (phosphorous) group, and a sulfonic acid group, in the molecule. From the viewpoint of availability and effectiveness, anion-modified cellulose fibers having a carboxy group as the anionic group (referred to as "oxidized cellulose fibers") are preferred, and a hydroxymethyl group (-CH) at the C6 position of the glucose unit constituting the cellulose fiber is preferred. 2More preferred is an anion-modified cellulose fiber in which the anionic groups (OH) are selectively converted to carboxy groups (referred to as "TEMPO-oxidized cellulose fiber"). The counter ion of the anionic group is preferably a proton.

[0024] The anionic group content in the anion-modified cellulose fiber is preferably 0.1 mmol / g or more, more preferably 0.4 mmol / g or more, even more preferably 0.6 mmol / g or more, even more preferably 0.7 mmol / g or more, and even more preferably 0.8 mmol / g or more, from the viewpoint of stable introduction of the modifying group. Also, from the viewpoint of improving the handling property, it is preferably 3 mmol / g or less, more preferably 2.5 mmol / g or less, even more preferably 2 mmol / g or less, even more preferably 1.9 mmol / g or less, and even more preferably 1.8 mmol / g or less. The "anionic group content" means the total amount of anionic groups in the glucose portion constituting the cellulose fiber, and is specifically measured by the method described in the Examples below.

[0025] [Method for producing modified cellulose fibers] The modified cellulose fiber can be produced, for example, by introducing anionic groups into raw cellulose fiber to produce an anionically modified cellulose fiber (step 1), and then bonding the anionically modified cellulose fiber with two or more types of amines (step 2).

[0026] (Process 1) (a) Raw cellulose fiber As the cellulose fiber that is the raw material for the anion-modified cellulose fiber, natural cellulose is preferred from an environmental perspective, and examples thereof include wood pulp such as coniferous pulp and broadleaf pulp; cotton pulp such as cotton linter and cotton lint; non-wood pulp such as straw pulp and bagasse pulp; bacterial cellulose, etc., and these can be used alone or in combination of two or more.

[0027] The average fiber diameter of the raw cellulose fibers is not particularly limited, but from the viewpoints of handleability and cost, it is preferably 5 μm or more, more preferably 7 μm or more, and from the same viewpoints, it is preferably 500 μm or less, more preferably 300 μm or less. The average fiber diameter of the raw cellulose fibers is determined by the method described in the Examples below.

[0028] The average fiber length of the raw cellulose fibers is not particularly limited, but from the viewpoints of availability and cost, it is preferably 5 μm or more, more preferably 25 μm or more, and from the same viewpoints, it is preferably 5,000 μm or less, more preferably 3,000 μm or less. The average fiber length of the raw cellulose fibers can be measured according to the method described in the Examples below.

[0029] (b) Method for introducing anionic groups Methods for introducing carboxy groups as anionic groups into cellulose fibers include, for example, a method of oxidizing hydroxy groups of the cellulose fibers to convert them into carboxy groups, and a method of reacting the hydroxy groups of the cellulose fibers with at least one selected from the group consisting of compounds having a carboxy group, acid anhydrides of compounds having a carboxy group, and derivatives thereof.

[0030] Examples of methods for oxidizing hydroxy groups in cellulose fibers include the method described in JP 2015-143336 A or JP 2015-143337 A, in which 2,2,6,6-tetramethyl-1-piperidine-N-oxyl (TEMPO) is used as a catalyst to react an oxidizing agent such as sodium hypochlorite and a bromide such as sodium bromide with raw cellulose fibers. By oxidizing cellulose fibers using TEMPO as a catalyst, the hydroxymethyl group at C6 position in the glucose unit constituting the cellulose fibers is selectively converted to a carboxy group, and the above-mentioned TEMPO-oxidized cellulose fibers can be obtained.

[0031] As a method for introducing sulfonic acid groups as anionic groups into cellulose fibers, a method of adding sulfuric acid to cellulose fibers and heating the fibers can be given. Methods for introducing (phosphorous) groups as anionic groups into cellulose fibers include a method for mixing a powder or an aqueous solution of (phosphorous) group or a (phosphorous) derivative with dry or wet cellulose fibers, a method for adding an aqueous solution of (phosphorous) group or a (phosphorous) derivative to a dispersion of cellulose fibers, etc. Methods for introducing phosphate groups as anionic groups into cellulose fibers include, for example, a method described in Japanese Patent No. 7196051 in which raw cellulose fibers are impregnated with a mixed aqueous solution of ammonium dihydrogen phosphate and urea to convert hydroxyl groups of the cellulose fibers into phosphoric esters. When these methods are employed, in general, a powder or an aqueous solution of phosphorous acid or a phosphorous acid derivative is mixed or added, followed by dehydration and heating.

[0032] (Process 2) The bond between the anion-modified cellulose fiber and two or more kinds of amines is achieved by reacting the anion-modified cellulose fiber with an amine (also called a "modifying compound"), which is a compound for introducing a modifying group into an anionic group. One of the features of the present invention is that two or more kinds of amines are used in step 2. The order of the reaction between the anion-modified cellulose fiber and two or more kinds of amines is not particularly limited, and for example, an amine with a small molecular weight may be reacted first, an amine with a large molecular weight may be reacted first, or all the amines may be reacted simultaneously. A preferred embodiment is one in which a tertiary amine is reacted first, and then a secondary amine is reacted.

[0033] As a method for binding the modifying group, (1) when binding via an ionic bond, JP 2015-143336 A can be referenced, and (2) when binding via an amide bond, JP 2015-143337 A can be referenced. After completion of step 2, post-treatment may be appropriately carried out in order to remove unreacted compounds, etc. Examples of methods for the post-treatment include filtration, centrifugation, dialysis, etc.

[0034] (Amine) In the present invention, two or more kinds of amines are used, and from the viewpoint of production, it is preferable to use 2 to 4 kinds of amines, and it is more preferable to use 2 kinds of amines. The amine is preferably a compound having an amino group and a chain hydrocarbon group or an alicyclic hydrocarbon group, such as a primary amine, a secondary amine, or a tertiary amine, and from the viewpoint of suppressing the formation of aggregates, those containing a secondary amine and a tertiary amine are more preferable. Specific examples of the chain hydrocarbon group or the alicyclic hydrocarbon group are as described above.

[0035] The molecular weight of the amine is, from the viewpoint of suppressing the formation of aggregates, preferably 100 or more, more preferably 200 or more, and even more preferably 300 or more, while, from the same viewpoint, it is preferably 10,000 or less, more preferably 2,000 or less, even more preferably 1,000 or less, and even more preferably 500 or less.

[0036] Specific examples of such amines include preferred primary amines such as hexadecylamine, stearylamine, and oleylamine, preferred secondary amines such as didecylamine, dioctylamine, didodecylamine, and ditridecylamine, and preferred tertiary amines such as trihexylamine, trioctylamine, tridecylamine, and tridodecylamine.

[0037] When a secondary amine and a tertiary amine are used as the amines, the molar ratio of the secondary amine to the tertiary amine (secondary amine / tertiary amine) is preferably 10 / 90 or more, more preferably 20 / 80 or more, and even more preferably 40 / 60 or more, from the viewpoint of suppressing the formation of aggregates, while from the same viewpoint, it is preferably 90 / 10 or less, more preferably 80 / 20 or less, and even more preferably 60 / 40 or less.

[0038] (Refining process) By micronizing the cellulose fibers at any stage of the production method of the modified cellulose fibers (for example, before step 1, before step 2, and after step 2), the cellulose fibers on the micrometer scale can be micronized to the nanometer scale. By reducing the average fiber diameter to the nanometer size, the dispersibility in the resin is improved, which is preferable.

[0039] The micronization treatment can be carried out by a known micronization treatment method. For example, when obtaining modified cellulose fibers having an average fiber diameter of nanometer size, a treatment method using a grinder such as a mass colloider or a treatment method using a high-pressure homogenizer in a medium may be carried out.

[0040] Examples of the medium include water; alcohols having 1 to 6 carbon atoms, preferably 1 to 4 carbon atoms, such as methanol, ethanol, propanol, and 1-methoxy-2-propanol (PGME); ketones having 3 to 6 carbon atoms, such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; esters having 2 to 4 carbon atoms, such as ethyl acetate and butyl acetate; saturated or unsaturated hydrocarbons having 1 to 6 carbon atoms; aromatic hydrocarbons such as benzene and toluene; halogenated hydrocarbons such as methylene chloride and chloroform; lower alkyl ethers having 2 to 5 carbon atoms; and polar solvents such as N,N-dimethylformamide (DMF), N,N-dimethylacetamide, and dimethylsulfoxide. These can be used alone or in combination of two or more. The amount of the medium used may be an amount that can disperse the cellulose fibers to be refined, and is preferably 1 mass or more, more preferably 2 mass or more, and preferably 500 mass or less, and more preferably 200 mass or less, relative to the target cellulose fibers.

[0041] As the device used in the micronization treatment, a known dispersing machine is preferably used in addition to the high-pressure homogenizer. For example, a disintegrator, a beater, a low-pressure homogenizer, a grinder, a mass colloider, a cutter mill, a ball mill, a jet mill, a single-screw extruder, a twin-screw extruder, an ultrasonic agitator, a household juicer mixer, etc. can be used. In addition, the solid content of the cellulose fiber to be subjected to the micronization treatment is preferably 50 mass% or less.

[0042] (Short fiber processing) At any stage in the process for producing the modified cellulose fibers, the cellulose fibers may be subjected to a fiber shortening treatment. The fiber shortening treatment can be achieved by subjecting the target cellulose fibers to the following treatment methods (i) to (iii), either alone or in combination. (i) Alkaline treatment (ii) Acid Treatment (iii) One or more treatment methods selected from the group consisting of heat treatment, ultraviolet treatment, electron beam treatment, mechanical treatment, and enzyme treatment.

[0043] [Properties of modified cellulose fibers] The main properties of the modified cellulose fiber of the present invention are as follows:

[0044] (Crystal structure) The modified cellulose fiber preferably has a cellulose I type crystal structure from the viewpoint of strength expression of the separation membrane. The crystallinity of the modified cellulose fiber is preferably 10% or more, more preferably 15% or more, and even more preferably 20% or more from the viewpoint of strength expression of the separation membrane. In addition, from the viewpoint of raw material availability, it is preferably 90% or less, more preferably 85% or less, even more preferably 80% or less, and even more preferably 75% or less. In this specification, the crystallinity of the cellulose fiber is the cellulose I type crystallinity calculated from the diffraction intensity value by the X-ray diffraction method, and can be measured according to the method described in the Examples below. In addition, the cellulose I type refers to the crystalline form of natural cellulose, and the cellulose I type crystallinity refers to the proportion of the amount of crystalline regions in the entire cellulose fiber. The presence or absence of the cellulose I type crystal structure can be determined by the presence of a peak at 2θ=22.6° in X-ray diffraction measurement.

[0045] (Average fiber diameter) The modified cellulose fibers are preferably those that have been subjected to a micronization treatment to have nanometer sizes. Therefore, the average fiber diameter of the modified cellulose fibers is preferably 1 nm or more, more preferably 2 nm or more, from the viewpoints of handling, availability, and cost, and is preferably 300 nm or less, more preferably 200 nm or less, even more preferably 150 nm or less, and even more preferably 120 nm or less, from the viewpoints of improving handling and dispersibility.

[0046] (average fiber length) The average fiber length of the modified cellulose fiber is preferably 10 nm or more, more preferably 30 nm or more, and even more preferably 50 nm or more from the viewpoint of strength expression of the separation membrane, while it is preferably 1000 nm or less, more preferably 500 nm or less, and even more preferably 300 nm or less from the viewpoint of dischargeability and handleability.

[0047] (average aspect ratio) The average aspect ratio of the modified cellulose fiber is preferably 5 or more, more preferably 10 or more, and even more preferably 20 or more from the viewpoint of the strength expression of the separation membrane, while it is preferably 300 or less, more preferably 200 or less, and even more preferably 100 or less from the viewpoint of dischargeability and handleability. The average fiber diameter, average fiber length and average aspect ratio of the modified cellulose fiber can be determined by the method described in the Examples below.

[0048] (Amount of modified group bonded and introduction rate) The amount of the modifying group bonded to the modified cellulose fiber is preferably 0.01 mmol / g or more from the viewpoint of affinity with the resin component contained in the separation membrane, and from the same viewpoint, is preferably 3.0 mmol / g or less. When any two or more kinds of modifying groups are simultaneously introduced into the modified cellulose fiber as the modifying groups, it is preferable that the total amount of the modifying groups bonded is within the above range.

[0049] From the viewpoint of dispersibility, the introduction rate of the modifying group in the modified cellulose fiber is preferably 10 mol% or more, the higher the better, and is preferably 100 mol%. When any two or more types of modifying groups are simultaneously introduced as the modifying group, it is preferable that the introduction rate is within the above range as long as the total introduction rate does not exceed the upper limit of 100 mol%.

[0050] The bonded amount and introduction rate of the modifying group can be adjusted by the type and amount of the amine, which is the modifying compound, the reaction temperature, the reaction time, the type of solvent, etc. The bonded amount (mmol / g) and introduction rate (mol%) of the modifying group refer to the amount and ratio of the modifying group introduced (bonded) to the anionic group in the modified cellulose fiber. For example, when the anionic group is a carboxy group, the bonded amount and introduction rate of the modifying group in the modified cellulose fiber are calculated by the method described in the Examples below.

[0051] [Modified cellulose fiber dispersion] The modified cellulose fiber of the present invention has excellent dispersibility, and therefore, by blending it with various organic media, the mechanical strength of the dispersion can be improved. Therefore, the modified cellulose fiber dispersion of the present invention contains the modified cellulose fiber of the present invention and an organic medium.

[0052] (organic medium) The organic medium in the present invention includes an organic solvent and a resin. The modified cellulose fiber and the organic solvent are referred to as a "modified cellulose fiber dispersion", and the modified cellulose fiber and the resin are referred to as a "resin composition". The resin composition of the present invention may further contain an organic solvent.

[0053] (a) Resin The resin can be selected according to the application and the desired characteristics or physical properties, and may be any of a thermosetting resin, a photocurable resin, and a thermoplastic resin. In the present invention, even in the case of a thermosetting resin that is prone to forming aggregates, the formation of aggregates can be effectively suppressed. The resin may be used alone or in combination of two or more kinds.

[0054] In the present invention, from the viewpoint of strength, thermal properties, and the like, the resin preferably contains a thermosetting resin. Examples of the thermosetting resin include epoxy resins, unsaturated polyester resins, vinyl ester resins, acrylic resins, phenol resins, urea resins, melamine resins, aniline resins, polyimide resins, bismaleimide resins, etc. These thermosetting resins may be used alone or in combination of two or more kinds.

[0055] Among the thermosetting resins, epoxy resins are preferred. Examples of epoxy resins include glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, alkene oxides, triglycidyl isocyanurate, etc. The epoxy resins may be used alone or in combination of two or more kinds.

[0056] (b) Organic solvent The organic solvent may be a commonly used organic solvent or an organic medium containing a reactive functional group.

[0057] From the viewpoint of dispersibility of the modified cellulose fiber, the organic solvent used in the present invention preferably has a dielectric constant at 25° C. of 75 or less, more preferably 55 or less, even more preferably 45 or less, and preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more. The dielectric constant of the solvent can be measured at 25° C. using a liquid dielectric meter Model 871 (manufactured by Nippon Luft Co., Ltd.).

[0058] Specific preferred examples of the organic solvent include alcohols such as methanol, ethanol, isopropyl alcohol, 2-butanol, 1-pentanol, octyl alcohol, glycerin, ethylene glycol, and propylene glycol; carboxylic acids such as acetic acid; hydrocarbons such as hexane, heptane, octane, decane, and liquid paraffin; aromatic hydrocarbons such as toluene and xylene; amides such as dimethyl sulfoxide, N,N-dimethylformamide (DMF), dimethylacetamide, and acetanilide; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; and halogens such as methylene chloride and chloroform. Examples of the oil-soluble organic solvent include olefins, carbonates such as ethylene carbonate, propylene carbonate, dimethyl carbonate, and diethyl carbonate, esters such as methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl butyrate, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, and polyoxyethylene fatty acid esters, polyethers such as polyethylene glycol and polyoxyethylene alkyl ethers, silicone oils such as polydimethylsiloxane, acetonitrile, propionitrile, ester oils, salad oils, soybean oils, and castor oils. These oils may be used alone or in combination of two or more.

[0059] Examples of organic media containing reactive functional groups include acrylates such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, n-hexyl acrylate, n-hexyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, and phenyl glycidyl ether acrylate; urethane prepolymers such as hexamethylene diisocyanate urethane prepolymer and phenyl glycidyl ether acrylate toluene diisocyanate urethane prepolymer; glycidyl ethers such as n-butyl glycidyl ether, 2-ethylhexyl glycidyl ether, glycidyl ether of stearic acid, styrene oxide, phenyl glycidyl ether, nonylphenyl glycidyl ether, butylphenyl glycidyl ether, 1,6-hexanediol diglycidyl ether, ethylene glycol diglycidyl ether, and diethylene glycol diglycidyl ether; chlorostyrene, methoxystyrene, butoxystyrene, and vinyl benzoic acid.

[0060] (Other ingredients) The modified cellulose fiber dispersion of the present invention can contain, as other components other than those mentioned above, plasticizers, crystal nucleating agents, fillers (inorganic fillers, organic fillers), hydrolysis inhibitors, flame retardants, antioxidants, lubricants such as hydrocarbon waxes and anionic surfactants, ultraviolet absorbers, antistatic agents, antifogging agents, light stabilizers, pigments, antifungal agents, antibacterial agents, foaming agents, surfactants; starches, polysaccharides such as alginic acid; natural proteins such as gelatin, glue, and casein; inorganic compounds such as tannins, zeolites, ceramics, and metal powders; fragrances; flow regulators; leveling agents; conductive agents; ultraviolet dispersion agents; deodorants, etc., within a range that does not impair the effects of the present invention. Similarly, it is also possible to add other polymer materials and other resin compositions within a range that does not impair the effects of the present invention.

[0061] (Method for preparing modified cellulose fiber dispersion) The modified cellulose fiber dispersion of the present invention can be prepared by dispersing the above-mentioned modified cellulose fiber and organic medium together with a curing agent, a curing accelerator and / or other components, if necessary, in a high-pressure homogenizer. Alternatively, the modified cellulose fiber dispersion of the present invention can be prepared by stirring these raw materials in a Henschel mixer, a planetary centrifugal mixer, or the like, or by melt-kneading them in a known kneader such as an internal kneader, a single-screw or twin-screw extruder, or an open-roll kneader.

[0062] [Modified cellulose fiber dispersion] The modified cellulose fiber dispersion of the present invention contains modified cellulose fibers and the above organic solvent.

[0063] From the viewpoint of productivity, the content of modified cellulose fiber in the dispersion of the present invention is preferably 0.01 mass% or more, more preferably 0.1 mass% or more, even more preferably 0.5 mass% or more, and even more preferably 1.0 mass% or more, while from the viewpoint of dispersibility, it is preferably 20 mass% or less, more preferably 10 mass% or less, even more preferably 5 mass% or less, and even more preferably 3 mass% or less.

[0064] The content of glucose moieties in the modified cellulose in the dispersion of the present invention is, from the viewpoint of productivity, preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.5% by mass or more, and even more preferably 1.0% by mass or more, while, from the viewpoint of dispersibility, it is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, and even more preferably 2% by mass or less.

[0065] The content of the organic solvent in the dispersion of the present invention is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more from the viewpoint of dispersibility, while it is preferably 99.99% by mass or less, more preferably 99.9% by mass or less, and even more preferably 99.5% by mass or less from the viewpoint of productivity.

[0066] [Resin composition] The resin composition of the present invention contains modified cellulose fibers and the above-mentioned resin, and may further contain an organic solvent as a solvent.

[0067] When the resin composition contains an organic solvent, the content of the modified cellulose fiber in the resin composition of the present invention is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, even more preferably 0.5 mass% or more, and even more preferably 1 mass% or more from the viewpoint of resin reinforcement, while from the viewpoint of dispersibility, it is preferably 10 mass% or less, more preferably 5 mass% or less. On the other hand, when the resin composition does not contain an organic solvent, the content of the modified cellulose fiber in the resin composition of the present invention is preferably 10% by mass or more, more preferably 15% by mass or more, from the viewpoint of reinforcing the resin, and is preferably 80% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less, from the viewpoint of dispersibility.

[0068] When the resin composition contains an organic solvent, the content of the modified cellulose fiber in the resin composition of the present invention is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, even more preferably 0.5 mass% or more, and even more preferably 1 mass% or more from the viewpoint of resin reinforcement, while from the viewpoint of dispersibility, it is preferably 5 mass% or less, more preferably 3 mass% or less. On the other hand, when the resin composition does not contain an organic solvent, the content of the modified cellulose fiber in the resin composition of the present invention is preferably 1 mass% or more, more preferably 10 mass% or more, from the viewpoint of reinforcing the resin, and is preferably 80 mass% or less, more preferably 20 mass% or less, and even more preferably 15 mass% or less, from the viewpoint of dispersibility.

[0069] When the resin composition contains an organic solvent, the resin content in the resin composition of the present invention is preferably 1 mass % or more, more preferably 3 mass % or more, and even more preferably 5 mass % or more from the viewpoint of dispersibility, while it is preferably 50 mass % or less, more preferably 20 mass % or less, and even more preferably 10 mass % or less from the viewpoint of resin reinforcement. On the other hand, when the resin composition does not contain an organic solvent, the resin content in the resin composition of the present invention is preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 65 mass% or more from the viewpoint of dispersibility, while from the viewpoint of resin reinforcement, it is preferably 90 mass% or less, more preferably 85 mass% or less, and even more preferably 80 mass% or less.

[0070] The resin composition of the present invention may further contain an organic solvent. The organic solvent referred to here is the organic solvent in the above-mentioned "(b) organic solvent". When the organic solvent is contained, the content thereof is preferably 40% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more from the viewpoint of dispersibility, while it is preferably 99% by mass or less, more preferably 95% by mass or less, and even more preferably 93% by mass or less from the viewpoint of productivity.

[0071] When the resin is a thermosetting resin, the resin composition of the present invention may contain a curing agent and a curing accelerator. The curing agent can be appropriately selected according to the type of resin. For example, when the resin is an epoxy resin, the curing agent may be, for example, an inorganic acid such as hydrochloric acid, nitric acid, phosphoric acid, etc.; an alkali metal hydroxide such as potassium hydroxide, sodium hydroxide, etc.; an amine-based curing agent such as 2-ethyl-4-methylimidazole; a phenolic resin-based curing agent such as a triazine skeleton-containing phenol; an acid anhydride-based curing agent; a polymercaptan-based curing agent; a latent curing agent such as a boron trifluoride-amine complex, dicyandiamide, or a carboxylic acid hydrazide. The curing agent may be used alone or in combination of two or more kinds. The curing agent may also act as a curing accelerator.

[0072] The curing accelerator can also be appropriately selected depending on the type of resin, and examples of the curing accelerator when the resin is an epoxy resin include phosphines, amines, etc. The curing accelerator may be used alone or in combination of two or more kinds.

[0073] The ratio of the curing agent can be appropriately selected depending on the type of resin and curing agent, and is preferably 0.1 to 300 parts by mass, for example, per 100 parts by mass of the resin. The ratio of the curing accelerator can be appropriately selected depending on the type of curing agent, and is preferably 0.01 to 100 parts by mass, for example, relative to 100 parts by mass of the epoxy resin. EXAMPLES

[0074] The present invention will be specifically described below with reference to examples. Note that the following examples are merely illustrative of the present invention and do not imply any limitation. Note that "normal pressure" refers to 101.3 kPa, and "normal temperature" refers to 25°C.

[0075] [Average fiber diameter and average fiber length of various cellulose fibers] Depending on the size of the cellulose fibers to be measured, one of the following two measurement methods was selected for measurement. (1) Deionized water or N,N-dimethylformamide (DMF) was added to the cellulose fibers to be measured to prepare a dispersion with a content of 0.0001% by mass. The dispersion was dropped onto mica and dried to prepare an observation sample, and the fiber height (difference in height between where the fibers are present and where they are not) of the cellulose fibers in the observation sample was measured using an atomic force microscope (AFM) (Nanoscope II Tapping mode AFM, manufactured by Digital Instruments; the probe used was Point Probe (NCH), manufactured by Nanosensors). At that time, 100 cellulose fibers were extracted from the microscope image in which the cellulose fibers could be confirmed, and the average fiber diameter was calculated from the fiber height. The average fiber length was calculated from the distance in the fiber direction.

[0076] (2) Deionized water was added to the cellulose fibers to be measured to prepare a dispersion with a content of 0.01% by mass. The dispersion was measured using a wet dispersion type image analysis particle size distribution meter (manufactured by Jusco International, IF-3200) under the following conditions: front lens: 2x, telecentric zoom lens: 1x, image resolution: 0.835 μm / pixel, syringe inner diameter: 6515 μm, spacer thickness: 500 μm, image recognition mode: ghost, threshold: 8, analysis sample amount: 1 mL, sampling: 15%. The length of the short axis of the cellulose fibers approximated as a rectangle was taken as the fiber diameter, and the length of the long axis was taken as the fiber length. The respective values ​​were measured for 100 cellulose fibers, and the average values ​​were calculated.

[0077] [Anionic Group Content of Anion-Modified Cellulose Fiber] Cellulose fibers to be measured with a dry mass of 0.5 g were placed in a beaker, and deionized water or a mixed solvent of methanol / deionized water = 2 / 1 (volume ratio) was added to make a total of 55 mL, to which 5 mL of 0.01 M sodium chloride aqueous solution was added to prepare a dispersion. The dispersion was stirred until the cellulose fibers to be measured were sufficiently dispersed. 0.1 M hydrochloric acid was added to the dispersion to adjust the pH to 2.5 to 3, and an automatic titration device (manufactured by DKK-TOA, AUT-701) was used to drop 0.05 M sodium hydroxide aqueous solution into the dispersion under the condition of a waiting time of 60 seconds, and the conductivity and pH value were measured every minute. The measurement was continued until the pH was about 11, and a conductivity curve was obtained. The sodium hydroxide titration amount was determined from this conductivity curve, and the anionic group content of the cellulose fibers to be measured was calculated by the following formula. Anionic group content (mmol / g) = [amount of sodium hydroxide solution titrated (mL) × concentration of sodium hydroxide solution (0.05M)] / [mass of cellulose fiber to be measured (0.5g)]

[0078] [Amount of modified group bonded and introduction rate of modified cellulose fiber] The amount of modified groups bonded to the modified cellulose fibers was determined by the following IR measurement method, and the amount of bonded and the introduction rate were calculated by the following formula. Specifically, the IR measurement was performed by measuring the infrared absorption spectrum of the dried modified cellulose fibers by the ATR method using an infrared absorption spectrometer (IR) (Nicolet 6700, manufactured by Thermo Fisher Scientific), and the amount of bonded and the introduction rate of the modified groups were calculated by formulas A and B. The following describes the case where the anionic group is a carboxy group, i.e., the case of oxidized cellulose fibers. The following "1720 cm" -1 The peak intensity of "is the peak intensity derived from the carbonyl group. In the case of an anionic group other than the carboxy group, the value of the wave number is appropriately changed, and the bond amount and introduction rate of the modifying group can be calculated. <Formula A-1 (in the case of ionic bond)> Amount of modified group bound (mmol / g) = a × (bc) ÷ b a: Carboxylic group content of oxidized cellulose fiber (mmol / g) b: 1720 cm of oxidized cellulose fiber -1 Peak intensity of c: 1720 cm of modified cellulose fiber -1 Peak intensity of <Formula A-2 (in the case of amide bond)> Amount of modified group bound (mmol / g) = de d: Carboxylic group content of oxidized cellulose fiber (mmol / g) e: Carboxylic group content of modified cellulose fiber (mmol / g) <Formula B> Modification group introduction rate (mol%) = 100 × f / g f: Amount of modified group bound (mmol / g) g: Carboxylic group content of oxidized cellulose fiber (mmol / g)

[0079] [Content of each ingredient] The content of each component was calculated from the blended amount of each component.

[0080] [Confirmation of crystal structures in various cellulose fibers] The crystal structures of various cellulose fibers, such as cellulose fiber, anion-modified cellulose fiber, and modified cellulose fiber, were confirmed by measurement under the following conditions using a diffractometer (MiniFlexII, manufactured by Rigaku Corporation). Measurement pellet preparation conditions: A pressure of 10 to 20 MPa was applied to the target cellulose fiber using a tablet forming machine to produce pellets with an area of ​​320 mm 2 Smooth pellets measuring ×1 mm in thickness were prepared. X-ray diffraction analysis conditions: step angle 0.01°, scan speed 10° / min, measurement range: diffraction angle 2θ=5~40° X-ray source: Cu / Kα-radiation, tube voltage: 15kv, tube current: 30mA Peak splitting conditions: After removing background noise, the peaks were fitted with a Gaussian function so that the error between 2θ=13° and 23° was within 5%.

[0081] The degree of crystallinity of the cellulose type I crystal structure was calculated based on the following formula (A) using the area of ​​the X-ray diffraction peak obtained by the above-mentioned peak division. Cellulose type I crystallinity (%) = [I cr / (I cr +I am )]×100 (A) [In the formula, I cr is the area of ​​the diffraction peak of the lattice plane (002 plane) (diffraction angle 2θ = 22-23°) in X-ray diffraction, I am indicates the area of ​​the diffraction peak of the amorphous part (diffraction angle 2θ = 18.5°).

[0082] Preparation Example 1 (Preparation of Short Anion-Modified Cellulose Fiber) [Anion-modified cellulose fiber] Anion-modified cellulose fibers having the physical properties shown in Table 1 were used as raw materials.

[0083] [Table 1]

[0084] Such anionically modified cellulose fibers can be prepared, for example, by the TEMPO oxidation treatment described below.

[0085] [TEMPO oxidation treatment] In a 2L PP beaker equipped with a mechanical stirrer and stirring blades, 10 g of bleached coniferous kraft pulp fiber as the raw material natural cellulose fiber and 990 g of deionized water are weighed and stirred at 25°C and 100 rpm for 30 minutes. Next, 0.13 g of 2,2,6,6-tetramethyl-1-piperidine-N-oxyl (TEMPO), 1.3 g of sodium bromide, and 35.5 g of 10.5 mass% sodium hypochlorite aqueous solution are added in this order to 10 g of the pulp fiber. Next, pH stat titration is performed using an automatic titration device, and 0.5 M sodium hydroxide aqueous solution is dropped to maintain the pH at 10.5. The reaction is carried out at a stirring speed of 100 rpm and 25°C for 120 minutes. Next, 0.01 M hydrochloric acid is added thereto while stirring to make the pH of the suspension 2. Next, the solid content is filtered out by suction filtration. The solids are dispersed in deionized water and filtered off by suction filtration. This operation is repeated until the conductivity of the filtrate is 200 μS / cm or less. The resulting solids are dehydrated to obtain anion-modified cellulose fibers.

[0086] [Preparation of Short Anion-Modified Cellulose Fibers] Anionically modified cellulose fibers having the physical properties shown in Table 1 were subjected to alkaline hydrolysis and hot water treatment to prepare short anionically modified cellulose fibers having the physical properties shown in Table 2.

[0087] [Table 2]

[0088] Such shortened anionically modified cellulose fibers can be prepared, for example, by the following alkaline hydrolysis treatment and hot water treatment.

[0089] [Alkaline hydrolysis treatment] A suspension of anion-modified cellulose fibers with a solid content of 144.5 g and physical properties shown in Table 1 is diluted with 1000 g of deionized water, to which 1.4 g of 35% hydrogen peroxide solution (1 part by mass of hydrogen peroxide per 100 parts by mass of the solid content of the raw cellulose fibers) is added, and the pH is adjusted to 12 with 1 M aqueous sodium hydroxide solution. Then, an alkaline hydrolysis treatment is performed at 80°C for 2 hours (solid content of the suspension of anion-modified cellulose fibers is 4.3% by mass). After cooling the suspension to room temperature, 0.01 M hydrochloric acid is added to adjust the pH of the suspension to 2. The solid content of the suspension is filtered off by suction filtration.

[0090] [Hot water treatment] The solids obtained by the alkaline hydrolysis treatment are dispersed in deionized water, and the solids are separated by suction filtration. This operation is repeated until the conductivity of the filtrate reaches 200 μS / cm or less. Deionized water is added to the suspension so that the solids content in the suspension is 5% by mass, and the suspension is stirred at 95° C. for 12 hours, and then cooled to room temperature to obtain an aqueous suspension of shortened anion-modified cellulose fibers. The aqueous suspension of shortened anion-modified cellulose fibers is centrifuged to obtain shortened anion-modified cellulose fibers.

[0091] Example 1 (Preparation of modified cellulose fiber and resin composition) To 17.5 g (solid content 5 g) of the shortened anion-modified cellulose fiber having the physical properties shown in Table 2, 481 g of ethanol and amine compound 1 shown in Table 3 were added in a mass ratio shown in Table 3, and the mixture was stirred at room temperature for 1 hour. Thereafter, the obtained ethanol dispersion was treated with a twin-screw high-pressure homogenizer (Nano-Veita L-ES, manufactured by Yoshida Kikai Kogyo Co., Ltd.) at 150 MPa for 5 passes.

[0092] Amine compound 2 shown in Table 3 was added to 48.8 g of the ethanol dispersion collected from the ethanol dispersion after the homogenizer treatment in a mass ratio shown in Table 3, and the mixture was stirred at room temperature for 30 minutes. After the stirring was completed, 48.8 g of cyclohexanone was further added, and 48.8 g of the solvent was distilled off from the obtained dispersion using an evaporator under reduced pressure at 70°C. In this way, a dispersion of modified cellulose fibers was prepared in which two or more amines having chain hydrocarbon groups were bonded via ionic bonds. The obtained modified cellulose fibers had a structure in which two types of chain hydrocarbon groups, a trioctyl group derived from trioctylamine and a ditridecyl group derived from ditridecylamine, were bonded via ionic bonds.

[0093] To the resulting dispersion, a resin was added in a mass ratio shown in Table 3, and the mixture was stirred at room temperature for 30 minutes. In this manner, a resin composition of the present invention was prepared. Thereafter, the solvent was distilled off using an evaporator under reduced pressure at 85° C. until the solvent content reached the mass ratio shown in Table 3. The obtained dispersion was allowed to cool to room temperature, and then a curing agent was added to the dispersion in the mass ratio shown in Table 3, followed by stirring at room temperature to obtain a composition. The composition thus obtained is also included in the resin composition of the present invention. For the evaluation of dispersibility below, the composition obtained here was used as a sample.

[0094] Examples 2 to 6 (Preparation of modified cellulose fibers and resin compositions) The modified cellulose fibers and resin compositions of each example were prepared in the same manner as in Example 1, except that the mass ratios and types of each component, such as the shortened anion-modified cellulose fibers and the amine compounds, were changed to those shown in Table 3.

[0095] Comparative Examples 1 to 3 (Preparation of Modified Cellulose Fibers and Resin Compositions) The modified cellulose fibers and resin compositions of each comparative example were prepared in the same manner as in Example 1, except that the mass ratios and types of each component, such as the shortened anion-modified cellulose fibers and the amine compounds, were changed to those shown in Table 3. In the comparative examples, amine compound 2 was not used, so the obtained modified cellulose fibers had a structure in which one type of chain hydrocarbon group, a trioctyl group derived from trioctylamine, was contained via an ionic bond.

[0096] [Method of evaluating dispersibility] The dispersibility of the modified cellulose fiber was evaluated based on the maximum length of the aggregates in the sample as follows: the longer the maximum length of the aggregates, the worse the dispersibility. A drop of sample was placed on a slide glass, and a cover glass was placed on top. Using a digital microscope (Keyence Corporation, VHX6000) set to a magnification of 150x, aggregates in the sample were observed within the obtained field of view. The length of the long side of the largest aggregate among the aggregates was taken as the maximum length of the aggregate in each example.

[0097] The compositions and evaluation results of each of the examples and comparative examples are summarized in the following Table 3. The mass ratios shown in Table 3 were calculated from the masses of the respective reagents.

[0098] [Table 3]

[0099] From Table 3, it was found that the maximum length of the aggregates was longer in the Comparative Example than in the Examples, which indicated that the modified cellulose fiber having two types of hydrocarbon groups had better dispersibility.

[0100] [reagent] In the above examples, the following reagents were used without any special purification. Tertiary amines Trioctylamine: Fujifilm Wako Pure Chemical Industries, Ltd. (molecular weight: 354) Tridodecylamine: Farmin T20 (Kao Corporation) (molecular weight: 522) Secondary amines Ditridecylamine: Farmin D30I (Kao Corporation) (molecular weight: 382) Didodecylamine: Fujifilm Wako Pure Chemical Industries, Ltd. (molecular weight: 354) Dioctylamine: Fujifilm Wako Pure Chemical Industries, Ltd. (molecular weight: 241) Resin and hardener Epoxy resin: jER828 (Mitsubishi Chemical) 0.1 mol / L hydrochloric acid, ethanolic: Sigma-Aldrich Japan 0.1 mol / L potassium hydroxide solution (alcoholic): Kanto Chemical [Industrial Applicability]

[0101] The modified cellulose fiber and resin composition of the present invention can be used in various molded product fields such as home appliance parts, electronics, aerospace, civil engineering and construction, automobiles, and vehicle-mounted applications.

Claims

1. A modified cellulose fiber comprising two or more amines each having a chain hydrocarbon group or an alicyclic hydrocarbon group and an anion-modified cellulose fiber bonded via an ionic bond or an amide bond.

2. 2. The modified cellulose fiber of claim 1, wherein the amines include secondary and tertiary amines.

3. The modified cellulose fiber according to claim 2, wherein the molar ratio of the secondary amine to the tertiary amine (secondary amine / tertiary amine) is 10 / 90 or more and 90 / 10 or less.

4. A modified cellulose fiber dispersion comprising the modified cellulose fiber according to any one of claims 1 to 3 and an organic medium.

5. A modified cellulose fiber dispersion comprising the modified cellulose fiber according to any one of claims 1 to 3 and an organic solvent.

6. A resin composition comprising the modified cellulose fiber according to any one of claims 1 to 3 and a resin.

Citation Information

Patent Citations

  • Fiber-reinforced composite material and method for production thereof and precursor for producing fiber-reinforced composite material

    JP2006241450A