Nitride semiconductor device and method for manufacturing nitride semiconductor device
By integrating Mg and Group 13 elements like Al or Be in the p-type region of nitride semiconductor devices and activating them through heat treatment, the challenge of Mg segregation is overcome, resulting in a highly doped p-type region with improved ohmic contact and device performance.
Patent Information
- Application Number
- JP2023080128
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-27
AI Technical Summary
Forming a highly doped p-type region in nitride semiconductor devices is challenging due to Mg segregation during ion implantation, which decreases concentration and hinders effective ohmic contact.
Incorporating a nitride semiconductor device with a p-type region containing Mg concentrations between 3×10^18 cm^-3 and 1×10^21 cm^-3, along with a Group 13 element or acceptor element like Al or Be, and performing heat treatment to activate Mg, thereby forming a highly concentrated p-type region.
This approach allows for the realization of a highly doped p-type region with improved ohmic contact, reducing Mg segregation and enhancing the solid solubility limit, leading to better device performance.
Smart Images

Figure 2024164556000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a nitride semiconductor device and a method for manufacturing a nitride semiconductor device. [Background technology]
[0002] A nitride semiconductor device having a vertical MOS (Metal Oxide Semiconductor) structure is known (see, for example, Patent Document 1). In addition, in a nitride semiconductor device, it is possible to control p-type conductivity by using magnesium (Mg) as a dopant (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-096744 A [Patent Document 2] JP 2014-086698 A Summary of the Invention [Problem to be solved by the invention]
[0004] In order to realize a good ohmic contact in a nitride semiconductor device, it is necessary to selectively form a high-concentration p-type region in the nitride semiconductor. However, when attempting to form a high-concentration p-type region by ion implantation, Mg tends to segregate and the concentration tends to decrease, making it difficult to achieve this. The present disclosure has been made in consideration of the above-mentioned problem, and aims to provide a nitride semiconductor device and a method for manufacturing a nitride semiconductor device capable of realizing a high-concentration p-type region. [Means for solving the problem]
[0005] In order to solve the above problems, a nitride semiconductor device according to an embodiment of the present disclosure includes a nitride crystal layer and a p-type region provided in the nitride crystal layer. 18 cm-3 More than 1×10 21 cm -3 Mg and 3×10 17 cm -3 5×10 or more 21 cm -3 At least one of a Group 13 element and an acceptor element is included in the following concentration:
[0006] In the method for manufacturing a nitride semiconductor device according to one embodiment of the present disclosure, 3×10 18 cm -3 More than 1×10 21 cm -3 and introducing Mg at a concentration of 3×10 17 cm -3 5×10 or more 21 cm -3 and performing a heat treatment on the nitride crystal layer into which the Mg has been ion-implanted and into which the Group 13 element and / or the acceptor element has been introduced, thereby activating the Mg and forming a p-type region in the nitride crystal layer. Effect of the Invention
[0007] According to the present disclosure, it is possible to provide a nitride semiconductor device capable of realizing a highly-concentrated p-type region and a method for manufacturing the nitride semiconductor device. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a plan view showing a configuration example of a GaN semiconductor device according to a first embodiment of the present disclosure. [Diagram 2] FIG. 2 is a cross-sectional view showing a configuration example of the GaN semiconductor device according to the first embodiment of the present disclosure. [Diagram 3] FIG. 3 is an enlarged cross-sectional view of FIG. 2, showing one vertical MOSFET. [Figure 4] FIG. 4 is a model diagram showing the atomic bonding state of a Mg-doped GaN crystal. [Diagram 5] FIG. 5 is a graph showing the results of first-principles calculations of the internal pressure of a GaN crystal when the Ga site of the GaN crystal is substituted with B, Al, Li, or Be. [Figure 6] FIG. 6 is a graph showing the results of calculations, by first principles, of the internal pressure of a GaN crystal in the case where the Ga site of the GaN crystal is substituted with Mg and at least one of Al and Be. [Figure 7] 7A to 7C are cross-sectional views illustrating a process sequence of a first manufacturing method for a GaN semiconductor device according to the first embodiment of the present disclosure. [Figure 8] 8A to 8C are cross-sectional views illustrating a process sequence of a first manufacturing method for a GaN semiconductor device according to the first embodiment of the present disclosure. [Figure 9] 9A to 9C are cross-sectional views illustrating a second manufacturing method example of a GaN semiconductor device according to the first embodiment of the present disclosure in the order of steps. [Figure 10] 10A to 10C are cross-sectional views illustrating a second manufacturing method of a GaN semiconductor device according to the first embodiment of the present disclosure in the order of steps. [Figure 11] 11A to 11C are cross-sectional views illustrating a third manufacturing method example of a GaN semiconductor device according to the first embodiment of the present disclosure in the order of steps. [Figure 12] 12A to 12C are cross-sectional views illustrating a third manufacturing method example of a GaN semiconductor device according to the first embodiment of the present disclosure in the order of steps. [Figure 13] 13A to 13C are cross-sectional views illustrating a fourth manufacturing method example of a GaN semiconductor device according to the first embodiment of the present disclosure in the order of steps. [Figure 14] 14A to 14C are cross-sectional views illustrating a fourth manufacturing method example of a GaN semiconductor device according to the first embodiment of the present disclosure in the order of steps. [Figure 15] FIG. 15 is a cross-sectional view showing a configuration of a vertical MOSFET according to a modification of the first embodiment of the present disclosure. [Figure 16] FIG. 16 is a cross-sectional view illustrating a configuration example of a vertical MOSFET according to the second embodiment of the present disclosure. [Figure 17] FIG. 17 is a cross-sectional view showing a configuration of a vertical MOSFET according to Modification 1 of Embodiment 2 of the present disclosure. [Figure 18]FIG. 18 is a cross-sectional view showing a configuration of a vertical MOSFET according to Modification 2 of Embodiment 2 of the present disclosure. [Figure 19] FIG. 19 is a cross-sectional view illustrating a configuration example of a pn diode according to the third embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The following describes an embodiment of the present disclosure. In the following description of the drawings, the same or similar parts are denoted by the same or similar reference numerals. However, it should be noted that the drawings are schematic, and the relationship between thickness and planar dimensions, the thickness ratio of each device and each member, and the like are different from the actual ones. Therefore, the specific thickness and dimensions should be determined with reference to the following description. In addition, it goes without saying that the drawings include parts with different dimensional relationships and ratios.
[0010] In the following description, directions may be described using the terms X-axis direction, Y-axis direction, and Z-axis direction. For example, the X-axis direction and the Y-axis direction are parallel to the surface 10a of the GaN substrate 10 described below. The Z-axis direction is perpendicular to the surface 10a of the GaN substrate 10. The X-axis direction, the Y-axis direction, and the Z-axis direction are mutually orthogonal.
[0011] In the following description, the positive direction of the Z axis may be referred to as "up" and the negative direction of the Z axis may be referred to as "down". "Up" and "down" do not necessarily mean the vertical direction with respect to the ground. In other words, the directions of "up" and "down" are not limited to the direction of gravity. "Up" and "down" are merely convenient expressions for specifying the relative positional relationship in regions, layers, films, substrates, etc., and do not limit the technical idea of the present disclosure. For example, if the paper is rotated 180 degrees, "up" will of course become "down" and "down" will become "up".
[0012] In the following description, the case where the first conductivity type is p-type and the second conductivity type is n-type will be described as an example. However, the conductivity types may be selected in the reverse relationship, with the first conductivity type being n-type and the second conductivity type being p-type. Furthermore, + or - added to p or n means that the semiconductor region has a relatively high or low impurity concentration, respectively, compared to a semiconductor region without + or -. However, even if the semiconductor regions are assigned the same p and p (or n and n), it does not mean that the impurity concentrations of the respective semiconductor regions are strictly the same.
[0013] <Embodiment 1> (Configuration example) FIG. 1 is a plan view showing a configuration example of a GaN (gallium nitride) semiconductor device 100 (an example of a "nitride semiconductor device" of the present disclosure) according to embodiment 1 of the present disclosure. FIG. 2 is a cross-sectional view showing a configuration example of the GaN semiconductor device 100 according to embodiment 1 of the present disclosure. FIG. 2 shows a cross section taken along line AA' in the plan view of FIG. 1. FIG. 3 is an enlarged view of the cross-sectional view of FIG. 2, showing one vertical MOSFET 1.
[0014] GaN semiconductor device 100 shown in Figures 1 and 2 is a power device. As shown in Figures 1 and 2, GaN semiconductor device 100 includes a GaN substrate 10 having a front surface 10a and a back surface 10b, and a plurality of vertical MOSFETs (Metal Oxide Semiconductor Field Effect Transistors) 1 provided on GaN substrate 10. The vertical MOSFET 1 is an example of a "field effect transistor" of the present disclosure. For example, multiple vertical MOSFETs 1 are repeatedly provided in one direction (e.g., the X-axis direction). One vertical MOSFET 1 is a repeated unit structure, and this unit structure is arranged side by side in one direction.
[0015] As shown in Figures 1 to 3, GaN substrate 10 has an n+ type GaN single crystal substrate 11 (an example of a "nitride crystal substrate" in the present disclosure) and an n- type GaN layer 12 (an example of a "nitride crystal layer" in the present disclosure) provided on GaN single crystal substrate 11. The GaN single crystal substrate 11 is, for example, an n+ type c-plane GaN single crystal substrate. The n-type impurities contained in the GaN single crystal substrate 11 are one or more of Si (silicon), O (oxygen) and Ge (germanium). As an example, the GaN single crystal substrate 11 contains Si as an n-type impurity, and the impurity concentration of Si in the GaN single crystal substrate 11 is 5×10 17 cm -3 That's all.
[0016] The GaN single crystal substrate 11 has a dislocation density of 1×10 7 cm -2 The GaN single crystal substrate 11 may be a low dislocation freestanding substrate having a dislocation density of less than 100 nm. When the GaN single crystal substrate 11 is a low dislocation freestanding substrate, the dislocation density of the GaN layer 12 formed on the GaN single crystal substrate 11 is also low. Furthermore, by using a low dislocation freestanding substrate, it is possible to reduce leakage current in the power device even when a large-area power device is formed on the GaN substrate 10. This enables the manufacturing equipment to manufacture power devices with a high yield rate. Furthermore, it is possible to prevent ion-implanted impurities from diffusing deeply along the dislocations during heat treatment.
[0017] The GaN layer 12 is a single crystal GaN layer epitaxially grown on one surface of the GaN single crystal substrate 11. The GaN layer 12 is formed by doping with an n-type impurity during the epitaxial growth process. The n-type impurity is, for example, Si. The GaN layer 12 is formed by doping with, for example, 1×10 15 cm -3 5×10 or more 16 cm -3 Contains the following concentrations:
[0018] The vertical MOSFET 1 has a p-type well region 13 and a p+ type contact region 15 provided on the front surface 10a (i.e., the front surface of the n-type GaN layer 12) of the GaN substrate 10. The vertical MOSFET 1 also includes a gate insulating film 21 provided on the front surface 10a of the GaN substrate 10, a gate electrode 22 provided on the gate insulating film 21, a source electrode 25 provided on the front surface 10a of the GaN substrate 10 and in contact with the source region 23 and the contact region 15, and a drain electrode 26 provided on the back surface 10b of the GaN substrate 10 and in contact with the n+ type GaN single crystal substrate 11. A P-type well region 13, an n+ type source region 23, and a p+ type contact region 15 (an example of the "p-type region" in the present disclosure) are provided on the surface 10a (i.e., the surface of the n-type GaN layer 12) side of the GaN substrate 10. Hereinafter, the p-type well region 13 is also referred to as the p-type GaN layer.
[0019] The well region 13 is a p-type layer formed by ion-implanting a p-type impurity such as Mg on the surface 10a side of the GaN substrate 10 and activating the p-type impurity by heat treatment. The well region 13 is formed by ion-implanting a p-type impurity such as Mg at a concentration of 1×10 17 cm -3 More than 3×10 18 cm -3 The well region 13 faces the surface 10a of the GaN substrate 10. The surface of the well region 13 is in contact with the gate insulating film 21. The channel of the vertical MOSFET 1 is formed on the surface of the well region 13 in contact with the gate insulating film 21 and in the vicinity thereof.
[0020] The source region 23 is an n+ type layer formed by ion-implanting n-type impurities such as Si or O into the surface 10a of the GaN substrate 10 and activating the n-type impurities by heat treatment. 19 cm -3 5×10 or more 20 cm -3The source regions 23 are provided in the well region 13 below both sides of the gate electrode 22, and face the surface 10a of the GaN substrate 10. The source regions 23 are located inside the well region 13 and are in contact with the well region 13.
[0021] The contact region 15 is, for example, a p+ type layer formed by ion-implanting a p-type impurity such as Mg into the front surface 10a side of the GaN substrate 10 and activating the p-type impurity by heat treatment. 18 cm -3 More than 1×10 21 cm -3 More preferably, it is present at a concentration of 1×10 19 cm -3 More than 2×10 20 cm -3 Contains the following concentrations:
[0022] In addition, in order to relax the compressive stress field formed around Mg, the contact region 15 is doped with at least one of a Group 13 element and an acceptor element at a concentration of 3×10 17 cm -3 5×10 or more 21 cm -3 Containing at a concentration of 5×10 or less, more preferably 5×10 18 cm -3 More than 4×10 20 cm -3 The group 13 element is, for example, at least one of B and Al, and the acceptor element is, for example, at least one of Li and Be. For example, the contact region 15 is formed by doping Al with a concentration of 3×10 17 cm -3 5×10 or more 21 cm -3 Containing at a concentration of 5×10 or less, more preferably 5×10 18 cm -3 More than 4×10 20 cm -3 Contains the following concentrations:
[0023] As described above, the GaN layer 12 is a single crystal GaN layer epitaxially grown on one surface of the GaN single crystal substrate 11. The well region 13 and the contact region 15 are provided in this single crystal GaN layer. As a result, the lattice constants of the contact region 15 in the X-axis direction (an example of the "first direction" in the present disclosure) and the Y-axis direction (an example of the "second direction" in the present disclosure) are equal to the lattice constants of the GaN single crystal substrate 11 in the X-axis direction and the Y-axis direction, respectively.
[0024] The contact region 15 faces the front surface 10a of the GaN substrate 10. The contact region 15 is located inside the well region 13 and is in contact with the well region 13. The contact region 15 also is in contact with the source region 23. The well region 13 is connected to the source electrode 25 via the contact region 15. As a result, the potential of the well region 13 is fixed to the potential of the source electrode 25 (for example, a reference potential such as the ground potential (GND)).
[0025] The gate insulating film 21 is, for example, a SiO2 film. The gate insulating film 21 may be a single layer film including any one of an Al2O3 film, a SiON film, an AlSiO film, and an AlON film, or may be a laminated film including any one or more of a SiO2 film, an Al2O3 film, a SiON film, an AlSiO film, and an AlON film. The thickness of the gate insulating film 21 is, for example, 50 nm or more and 150 nm or less, for example, 100 nm.
[0026] The gate electrode 22 is adjacent to a region where a channel is formed (hereinafter, referred to as a channel region) via the gate insulating film 21. The gate electrode 22 is made of polysilicon doped with a metal such as Al, Ti, Ni, or W, or an impurity. The gate electrode 22 may also be made of a silicide such as WSi or NiSi. The source electrode 25 is in ohmic contact with the source region 23, which is an n+ type layer, and the contact region 15, which is a p+ type layer. The drain electrode 26 is in ohmic contact with the other surface of the n+ type GaN single crystal substrate 11 (i.e., the surface opposite to the surface in contact with the GaN layer 12).
[0027] The source electrode 25 and the drain electrode 26 are made of Al or an Al-Si alloy, Ni, a Ni alloy, a Ti-Al alloy, a Ni-Au alloy, or the like. The source electrode 25 may have a barrier metal layer between itself and the source region 23. The drain electrode 26 may have a barrier metal layer between itself and the n+ type GaN single crystal substrate 11. The barrier metal layer may be made of Ti (titanium).
[0028] That is, the source electrode 25 and the drain electrode 26 may be a laminate of a Ti layer and an Al layer, or a laminate of a Ti layer and an Al-Si alloy layer. The source electrode 25 may also serve as a source pad (not shown), or may be an electrode provided separately from the source pad. The drain electrode 26 may also serve as a drain pad (not shown), or may be an electrode provided separately from the drain pad.
[0029] (Formation of compressive stress field) Figure 4 is a model diagram showing the atomic bonding state of a GaN crystal doped with Mg. The present inventors performed structural optimization of Mg in a GaN crystal using first-principles calculations. As a result, it was found that when the lattice constant of a GaN crystal is fixed, a compressive stress field is formed within the crystal because Mg has a larger atomic radius than Ga.
[0030] A more detailed explanation will be given. In FIG. 4, d1 indicates the center-to-center distance in the c-axis direction between Ga atoms and N atoms after structural optimization. d2 indicates the center-to-center distance in the c-axis direction between Mg atoms and N atoms after structural optimization. The center-to-center distance d1 of Ga-N is 1.974 Å, and the center-to-center distance d2 of Mg-N is 2.057 Å. d2 is 4.2% larger than d1. Since the atomic radius of Mg atoms is larger than that of Ga atoms, the center-to-center distance between Mg atoms and N atoms is larger. In the first-principles calculation performed by the present inventor, the internal pressure of the GaN crystal containing Mg shown in FIG. 4 was 0.406 GPa. It was found that a compressive stress field was formed inside the crystal because the pressure inside the crystal was a positive value.
[0031] (Relaxation of compressive stress field) The present inventors have succeeded in substituting atoms other than Mg for the Ga sites in the crystal where the compressive stress field is formed, thereby transforming this compressive stress field into a state in which there is no Mg (defect-free crystal) or into a state in which the current solubility limit of Mg is 3e18cm -3 We thought that if we could relax the compressive stress field, we could relax the solubility limit due to strain even in GaN crystals with a high concentration of Mg, and introduce more Mg into the Ga site.
[0032] Therefore, the present inventors performed the same calculations for several elements used as dopants in GaN crystals as for Mg, and plotted the internal pressure of the GaN crystal as shown in FIG. 5. FIG. 5 is a graph showing the results of first-principles calculations of the internal pressure of a GaN crystal when the Ga site of the GaN crystal is substituted with boron (B), aluminum (Al), lithium (Li), or beryllium (Be). FIG. 5 shows the pressure (GPa) inside the crystal when the GaN lattice constant is fixed. For comparison, FIG. 5 also shows the internal pressure when the Ga site is substituted with Mg.
[0033] As shown in Figure 5, it was found that doping GaN crystal with B, Al, Li, or Be forms a tensile stress field within the crystal. From this result, it was found that by adding B, Al, Li, or Be together with Mg to GaN crystal, the compressive stress field formed by Mg can be offset by the tensile stress field formed by B, Al, Li, or Be. B and Al are group 13 elements, and Li and Be are acceptor elements. Since these elements do not become n-type dopants, doping them together with Mg does not inhibit high-concentration p-type conduction by Mg (i.e., formation of a p+ type layer).
[0034] Fig. 6 is a graph showing the results of calculations using first-principles calculations of the internal pressure of a GaN crystal when the Ga site of the GaN crystal is substituted with at least one of Al and Be and Mg. Fig. 6 shows the pressure (GPa) inside the crystal when the GaN lattice constant is fixed. For comparison, Fig. 6 also shows the internal pressure when the Ga site is substituted with only Mg.
[0035] In addition, the item on the horizontal axis of FIG. 6, "Al+Mg substitution (Ga)", means that Ga sites are substituted with Al and Mg in a ratio of 1:1, and the Al and Mg after substitution are separated from each other. "Al+Mg (adjacent) substitution (Ga)" means that the atomic ratio of Al and Mg is 1:1, these atoms (elements) are substituted at Ga sites, and the Al and Mg after substitution are adjacent to each other. "Al+3Mg+Be substitution (Ga)" means that the atomic ratio of Al, Mg, and Be is 1:3:1, these atoms (elements) are substituted at Ga sites, and the Al, Mg, and Be after substitution are separated from each other. The same applies to the other items.
[0036] As shown in Figure 6, it was found that by introducing at least one of Al and Be together with Mg, the internal pressure can be significantly reduced and brought closer to zero (=defect-free crystal) compared to the case where only Mg is introduced. The first-principles calculations shown in Figure 6 found that by introducing Al in a 1:1 ratio to Mg, the compressive stress field due to Mg can be brought close to zero (0) GPa, regardless of whether Mg and Al are adjacent to each other or not.
[0037] In the first-principles calculations shown in Figure 6, a slight compressive stress field remains when the Al supply is 1:1 with respect to Mg. However, it was also found that when the Al supply is increased to 1:2 with respect to Mg, the compressive stress field disappears completely, and instead the tensile stress field induced by Al becomes dominant. In addition, according to the results of the first-principles calculations by the present inventors, it was found that the higher the Mg concentration in the GaN crystal, the higher the internal pressure, and the lower the Mg concentration, the lower the internal pressure.18 cm -3 More than 1×10 21 cm -3 It was found that the internal pressure was reduced by introducing Al at all Mg concentrations within the following range.
[0038] The present inventors also used first-principles calculations to calculate the stress field induced by Mg in wurtzite nitride crystals that have a group 13 element other than Ga as a cation. As a result, it was found that in AlN crystals, which are a type of wurtzite nitride crystal and have a short distance between the cation and nitrogen, a larger compressive stress field is induced by Mg substitution. For this reason, it is expected that stress relaxation by this technology (in the case of AlN crystals, substitution with at least one of B and Be) is effective not only for GaN crystals but also for AlN crystals. For other mixed crystal systems, it is expected that stress relaxation by this technology is effective when a compressive stress field is induced by Mg substitution.
[0039] (Manufacturing method) Next, a method for manufacturing the GaN semiconductor device 100 shown in Figures 1 to 3 will be described. Four manufacturing methods will be described here. The GaN semiconductor device 100 can be manufactured by using any of the manufacturing methods 1 to 4.
[0040] (1) Manufacturing method example 1 7 and 8 are cross-sectional views showing a first manufacturing method example of the GaN semiconductor device 100 according to the first embodiment of the present disclosure in the order of steps. Note that, Figs. 7 and 8 show the manufacturing method of one vertical MOSFET 1 out of multiple vertical MOSFETs 1 repeatedly arranged in the X-axis direction in the order of steps. The GaN semiconductor device 100 is manufactured by various types of equipment, such as a film forming equipment, an exposure equipment, an etching equipment, an ion implantation equipment, and a heat treatment equipment. Hereinafter, these equipments are collectively referred to as manufacturing equipment.
[0041] As shown in step ST1 of FIG. 7, the manufacturing equipment epitaxially grows an n− type GaN layer 12 on one surface of an n+ type GaN single crystal substrate 11. Next, as shown in step ST2 of FIG. 7, the manufacturing equipment ions-implants Mg as an acceptor element into a region (hereinafter, well formation region) 13' in the GaN substrate 10 where the p-type well region 13 (see FIG. 3) is to be formed. This ion implantation is also called Mg(p-) ion implantation. For example, the manufacturing equipment forms a mask (not shown) on the surface 10a of the GaN substrate 10. The mask is a SiO2 film or photoresist that can be selectively removed from the GaN substrate 10. The mask has a shape that opens above the well formation region 13' and covers above the other regions. The manufacturing equipment ions-implants Mg into the surface 10a side of the GaN substrate 10 on which the mask is formed. Here, the Mg concentration in the well formation region 13' is 1×10 18 cm -3 After the ion implantation, the mask is removed from the GaN substrate 10.
[0042] Next, the manufacturing equipment ions-implants Si as a donor element into a region (hereinafter, source formation region) 23' in the GaN substrate 10 where an n+ type source region 23 (see FIG. 3) is to be formed. This ion implantation is also called Si(n+) ion implantation. For example, the manufacturing equipment forms a mask (not shown) on the surface 10a of the GaN substrate 10. The mask has a shape that opens above the source formation region 23' and covers the above of other regions. The manufacturing equipment ions-implants Si into the surface 10a side of the GaN substrate 10 on which the mask has been formed. Here, the Si concentration in the source formation region 23' is, for example, 1×10 19 cm -3 After the ion implantation, the mask is removed from the GaN substrate 10.
[0043] Next, as shown in step ST3 of FIG. 7, the manufacturing equipment ions-implants Al, as an example of "at least one of a group 13 element and an acceptor element" of the present disclosure, into a region (hereinafter, contact formation region) 15' in the GaN substrate 10 where the p+ type contact region 15 (see FIG. 3) is to be formed. This ion implantation is also referred to as Al ion implantation. For example, the manufacturing equipment forms a mask (not shown) on the surface 10a of the GaN substrate 10. The mask has a shape that opens above the contact formation region 15' and covers above the other regions. The manufacturing equipment ions-implants Al into the surface 10a side of the GaN substrate 10 on which the mask has been formed. Here, the Al concentration in the contact formation region 15' is 3×10 17 cm -3 5×10 or more 21 cm -3 Below (for example, 1.5×10 19 cm -3 ) Al is ion-implanted.
[0044] Next, as shown in step ST4 of FIG. 8, the manufacturing equipment ions-implants Mg into the contact formation region 15' of the GaN substrate 10. This ion-implantation is also called Mg(p+) ion-implantation. For example, the manufacturing equipment ions-implants Mg into the front surface 10a of the GaN substrate 10 using the same mask as that used for the Al ion-implantation. Here, the Mg concentration in the contact formation region 15' is set to 3×10 18 cm -3 More than 1×10 21 cm -3 Below (for example, 1×10 19 cm -3 ) Mg ions are implanted.
[0045] Next, the manufacturing equipment ions-implants nitrogen (N) into the contact formation region 15' of the GaN substrate 10. This ion implantation is also called N ion implantation. For example, the manufacturing equipment ions-implants N into the front surface 10a side of the GaN substrate 10 using the same mask as that used for the Al ion implantation and p+ ion implantation. Here, the N concentration in the contact formation region 15' is, for example, 1×10 19 cm -3After the ion implantation, the mask is removed from the GaN substrate 10 in the manufacturing equipment. The N ion implantation is performed to suppress the generation of nitrogen vacancies during the heat treatment described below. However, in the first embodiment of the present disclosure, the N ion implantation may be omitted. Even if the N ion implantation is not performed, the p+ type contact region 15 (see FIG. 3) can be formed.
[0046] In addition, in step ST1 of FIG. 7 to step ST4 of FIG. 8, various ion implantations are performed in the order of Mg(p-) ion implantation, Si(n+) ion implantation, Al ion implantation, Mg(p+) ion implantation, and N ion implantation. However, in the embodiment of the present disclosure, the order of ion implantation is not limited to this. Mg(p-) ion implantation, Si(n+) ion implantation, Al ion implantation, Mg(p+) ion implantation, and N ion implantation may be performed in any order. Even if they are performed in any order, the GaN semiconductor device 100 shown in FIG. 1 to FIG. 3 can be manufactured.
[0047] Next, the manufacturing equipment forms a protective film 14 on the surface 10a of the GaN substrate 10. The protective film 14 is, for example, an aluminum nitride (AlN) film. As a result, the contact formation region 15' and the like of the GaN substrate 10 are covered with the protective film 14. Note that in the first embodiment of the present disclosure, the formation of the protective film 14 is not essential and may be omitted.
[0048] Next, the manufacturing equipment performs a heat treatment on the GaN substrate 10 at a maximum temperature of 1300° C. to 2000° C., for example. This heat treatment is, for example, a rapid heating process. This heat treatment may also be performed in a high-pressure N2 atmosphere, for example, at 500 MPa. This heat treatment activates the Mg and Si ions implanted into the GaN substrate 10. As a result, as shown in step ST5 of FIG. 8, a p-type well region 13, an n+ type source region 23, and a p+ type contact region 15 are formed in the GaN substrate 10. This heat treatment also makes it possible to recover to some extent defects caused by various ion implantations in GaN substrate 10. After the heat treatment, protective film 14 is removed from surface 10a of GaN substrate 10 by the manufacturing equipment.
[0049] Next, the manufacturing equipment forms a gate insulating film 21 (see FIG. 3) on the front surface 10a of the GaN substrate 10. Next, the manufacturing equipment forms a gate electrode 22 (see FIG. 3) and a source electrode 25 (see FIG. 3). Next, the manufacturing equipment forms a drain electrode 26 (see FIG. 3) on the back surface 10b side of the GaN substrate 10. Through these steps, a GaN semiconductor device 100 including a vertical MOSFET 1 is completed.
[0050] (2) Manufacturing method example 2 In the above-described manufacturing method example 1, the case where Al is doped into the GaN layer 12 by ion implantation has been described. However, in the first embodiment of the present disclosure, the Al doping is not limited to ion implantation. The Al doping may be performed by epitaxially growing an Al-doped layer 31 on the GaN layer 12, as described below.
[0051] 9 and 10 are cross-sectional views showing a process sequence of a second manufacturing method of the GaN semiconductor device 100 according to the first embodiment of the present disclosure. As shown in step ST11 of FIG. 9, the manufacturing equipment epitaxially grows an n-type GaN layer 12 and an Al-doped layer 31 in this order on one surface of an n+ type GaN single crystal substrate 11. The Al-doped layer 31 is a single crystal GaN layer containing Al. For example, the Al-doped layer 31 contains 1.5×10 19 cm -3 The Al-doped layer 31 has a thickness of 20 nm or more and 100 nm or less. In this example, the GaN layer 12 and the Al-doped layer 31 are an example of the "nitride crystal layer" of the present disclosure.
[0052] 9, the manufacturing equipment ions-implants Mg as an acceptor element into the well formation region 13' of the GaN substrate 10 including the Al-doped layer 31. As in manufacturing method example 1, this Mg(p-) ion implantation is performed using a mask (not shown). Here, as in manufacturing method example 1, the Mg concentration in the well formation region 13' is set to, for example, 1×10 18 cm -3 Mg ions are implanted so that
[0053] 9, the manufacturing equipment ions-implants Si as a donor element into the source formation region 23' of the GaN substrate 10 including the Al-doped layer 31. As in manufacturing method example 1, this Si(n+) ion implantation is performed using a mask (not shown). Here, as in manufacturing method example 1, the Si concentration in the source formation region 23' is set to, for example, 1×10 19 cm -3 Si ions are implanted so that
[0054] 10, the manufacturing equipment ions-implants Mg into the contact formation region 15' of the GaN substrate 10 including the Al-doped layer 31. As in manufacturing method example 1, this Mg(p+) ion implantation is performed using a mask (not shown). Here, as in manufacturing method example 1, the Mg concentration in the contact formation region 15' is set to, for example, 1×10 19 cm -3 Mg ions are implanted so that: Mg(p+) ion implantation energy is set so that the Mg implantation peak depth from the surface 10a of the GaN substrate 10 is shallower than the thickness of the Al-doped layer 31. In other words, the Mg(p+) ion implantation energy is set so that the Mg implantation peak depth is located within the Al-doped layer 31.
[0055] As a result, a part of the Al-doped layer 31 becomes the contact formation region 15′. The contact formation region 15′ is doped with 1.5×10 19 cm -3 and Mg at a concentration of 1×10 19 cm -3Contains at a concentration of. As in manufacturing method example 1, the manufacturing apparatus may ion-implant nitrogen (N) into the GaN substrate 10 or form a protective film before performing heat treatment to activate Mg and the like. The implantation of N and the formation of the protective film are optional. As in manufacturing method example 1, Mg(p-) ion implantation, Si(n+) ion implantation, Mg(p+) ion implantation, and N ion implantation may be performed in any order.
[0056] Next, the manufacturing equipment performs a heat treatment on the GaN substrate 10 at a maximum temperature of 1300° C. to 2000° C., for example. This heat treatment is, for example, a rapid heating process. This heat treatment may also be performed in a high-pressure N2 atmosphere, for example, at 500 MPa. This heat treatment activates the Mg and Si ions implanted into the GaN substrate 10. As a result, as shown in step ST15 of FIG. 10, a p-type well region 13, an n+ type source region 23, and a p+ type contact region 15 are formed in the GaN substrate 10.
[0057] This heat treatment can also recover to some extent defects caused by various ion implantations in the GaN substrate 10. Furthermore, in Manufacturing Method Example 2, since the contact formation region 15' is formed in the Al-doped layer 31, there is no need to implant Al ions, and there are no crystal defects caused by Al ion implantation. This may further reduce crystal defects caused by ion implantation, compared to Manufacturing Method Example 1.
[0058] The thickness of the Al-doped layer 31 is 20 nm or more and 100 nm or less. This thickness is thinner than that of general AlGaN. The Al concentration in the Al-doped layer 31 is 3×10 17 cm -3 5×10 or more 21 cm -3 For example, 1.5×10 19 cm -3As long as the Al-doped layer 31 is thin and the Al concentration is within the above range, the change in the lattice constant of GaN can be minimized even when the Al-doped layer 31 is disposed on the GaN layer 12. In addition, the deterioration of controllability of the conduction characteristics due to spontaneous polarization can be sufficiently suppressed. The subsequent steps are the same as those in Manufacturing Method Example 1. The manufacturing equipment forms the gate insulating film 21, the gate electrode 22, the source electrode 25, and the drain electrode 26 shown in Fig. 3. Through these steps, a GaN semiconductor device 100 including a vertical MOSFET 1 is completed.
[0059] (3) Manufacturing method example 3 The Al doping is not limited to ion implantation or epitaxial growth. The Al doping may be performed by thermal diffusion from a film containing Al to the GaN layer 12. The film may be an MgAl mixture containing Mg as well as Al. The p+ type contact region 15 may be formed by thermally diffusing Al and Mg from the MgAl mixture to the GaN layer 12.
[0060] 11 and 12 are cross-sectional views showing a process sequence of a third manufacturing method for a GaN semiconductor device 100 according to the first embodiment of the present disclosure. In step ST21 in FIG. 11, the steps up to the step of forming a well formation region 13′ and a source formation region 23′ are the same as steps ST1 and ST2 shown in FIG.
[0061] After the well formation region 13' and the source formation region 23' are formed, the manufacturing equipment forms an MgAl mixture 33 (an example of the "first film" of the present disclosure and also an example of the "second film" of the present disclosure) containing Mg and Al on the surface 10a of the GaN substrate 10, as shown in step ST22 of FIG. 11. The MgAl mixture 33 is, for example, Al3Mg2. The Al3Mg2 is formed by, for example, a sputtering method, an electron beam evaporation method, a thermal evaporation method, or the like.
[0062] Before forming the MgAl mixture 33, nitrogen (N) ions may be implanted into the region of the GaN layer 12 where the MgAl mixture 33 is to be disposed (i.e., the contact formation region 15'). Here, the N concentration in the region where the MgAl mixture 33 is to be disposed is set to, for example, 2×10 19 cm -3 N ions may be implanted so that
[0063] 12, the manufacturing equipment performs a heat treatment (an example of the "first heat treatment" and an example of the "second heat treatment" of the present disclosure) on the entire substrate including the MgAl mixture 33 and the GaN layer 12, thereby thermally diffusing Mg and Al from the MgAl mixture 33 to the GaN layer 12. The heat treatment for thermally diffusing Mg and Al is performed, for example, in an N2 atmosphere at a maximum temperature of 800° C. for a treatment time of 5 minutes at the maximum temperature. As a result, Mg and Al are introduced into the contact formation region 15'. After introducing Mg and Al into the contact formation region 15 ′, the manufacturing equipment removes the MgAl mixture 33 from the surface 10 a of the GaN substrate 10 .
[0064] Next, the manufacturing equipment performs a heat treatment on the GaN substrate 10 at a maximum temperature of 1300° C. to 2000° C., for example. This heat treatment is, for example, a rapid heating process. This heat treatment may also be performed in a high-pressure N2 atmosphere, for example, at 500 MPa. This heat treatment activates the Mg and Si introduced into the GaN substrate 10. As a result, as shown in step ST24 of FIG. 12, a p-type well region 13, an n+ type source region 23, and a p+ type contact region 15 are formed in the GaN substrate 10.
[0065] This heat treatment can also recover to some extent defects caused by various ion implantations in the GaN substrate 10. Furthermore, in manufacturing method example 3, Al and Mg are introduced into the contact formation region 15' by thermal diffusion rather than ion implantation. This may further reduce crystal defects caused by ion implantation compared to manufacturing method example 1. The subsequent steps are the same as those in Manufacturing Method Example 1. The manufacturing equipment forms the gate insulating film 21, the gate electrode 22, the source electrode 25, and the drain electrode 26 shown in Fig. 3. Through these steps, a GaN semiconductor device 100 including a vertical MOSFET 1 is completed.
[0066] (Manufacturing method example 4) In the first embodiment of the present disclosure, the second and third manufacturing methods may be combined. For example, Al may be introduced into the GaN layer 12 by epitaxially growing the Al-doped layer 31. Mg may be introduced into the GaN layer 12 by forming a film (e.g., an Mg film) serving as a Mg supply source on the Al-doped layer 31 and thermally diffusing Mg from this film into the Al-doped layer 31.
[0067] 13 and 14 are cross-sectional views showing a fourth manufacturing method example of the GaN semiconductor device 100 according to the first embodiment of the present disclosure in the order of steps. In step ST31 in Fig. 13, the steps up to the step of forming the Al-doped layer 31 and the step of forming the well formation region 13' and the source formation region 23' are the same as steps ST11, ST12, and ST13 shown in Fig. 9.
[0068] 13, after the well formation region 13′ and the source formation region 23′ are formed, the manufacturing equipment forms an Mg film 35 (an example of the “first film” of the present disclosure) on the front surface 10a of the GaN substrate 10. The Mg film 35 is formed by, for example, a sputtering method, an electron beam evaporation method, a thermal evaporation method, or the like. Before forming the Mg film 35, nitrogen (N) ions may be implanted into the region of the GaN layer 12 where the Mg film 35 is to be disposed (i.e., the contact formation region 15'). Here, the N concentration in the region where the Mg film 35 is to be disposed is set to, for example, 2×10 19 cm -3 N ions may be implanted so that
[0069] 14, the manufacturing equipment performs a heat treatment (an example of the "first heat treatment" of the present disclosure) on the entire substrate including the Mg film 35 and the GaN layer 12 to thermally diffuse Mg from the Mg film 35 to the GaN layer 12. The heat treatment for thermally diffusing Mg is performed, for example, in an N2 atmosphere at a maximum temperature of 800° C. for a treatment time of 5 minutes at the maximum temperature. As a result, Mg is introduced into the contact formation region 15'. After introducing Mg into the contact formation region 15' containing Al, the manufacturing equipment removes the Mg film 35 from the surface 10a of the GaN substrate 10.
[0070] Next, the manufacturing equipment performs a heat treatment on the GaN substrate 10 at a maximum temperature of 1300° C. to 2000° C., for example. This heat treatment is, for example, a rapid heating process. This heat treatment may also be performed in a high-pressure N2 atmosphere, for example, at 500 MPa. This heat treatment activates the Mg and Si introduced into the GaN substrate 10. As a result, as shown in step ST34 of FIG. 14, a p-type well region 13, an n+ type source region 23, and a p+ type contact region 15 are formed in the GaN substrate 10.
[0071] This heat treatment can also recover to some extent defects caused by various ion implantations in the GaN substrate 10. Furthermore, in manufacturing method example 4, Al and Mg are introduced into the contact formation region 15' not by ion implantation, but by forming an Al-doped layer 31 and thermally diffusing Mg. This may further reduce crystal defects caused by ion implantation compared to manufacturing method example 1. The subsequent steps are the same as those in Manufacturing Method Example 1. The manufacturing equipment forms the gate insulating film 21, the gate electrode 22, the source electrode 25, and the drain electrode 26 shown in Fig. 3. Through these steps, a GaN semiconductor device 100 including a vertical MOSFET 1 is completed.
[0072] (Effects of the First Embodiment) As described above, the GaN semiconductor device 100 according to the first embodiment of the present disclosure has an n-type GaN layer 12 and a p+ type contact region 15 provided in the GaN layer 12. The contact region 15 has a 3×10 18 cm -3 More than 1×10 21 cm -3 Mg and 3×10 17 cm -3 5×10 or more 21 cm -3 At least one of a Group 13 element and an acceptor element is included in the following concentration:
[0073] According to this, in the p+ type contact region 15, the compressive stress field formed by Mg can be offset by the compressive stress field formed by at least one of the group 13 elements and the acceptor element (e.g., Al). This allows the compressive stress field formed around Mg to be relaxed, and the solid solubility limit of Mg to be improved. It is possible to increase the amount of Mg entering the Ga site, and suppress the segregation of Mg, so that a high-concentration p+ type region (in this example, the p+ type contact region 15) can be realized. A good ohmic connection can be realized between the p+ type contact region 15 and the source electrode 25.
[0074] (Modification of the first embodiment) In the above-mentioned embodiment 1, the p+ type contact region 15 is exemplified as the "p type region" of the present disclosure. However, the "p type region" of the present disclosure is not limited to the p+ type contact region. The "p type region" of the present disclosure may be, for example, a p+ type layer for maintaining a withstand voltage, or may be both a p+ type contact region and a p+ type layer for maintaining a withstand voltage.
[0075] Fig. 15 is a cross-sectional view showing a configuration of a vertical MOSFET 1A according to a modification of the first embodiment of the present disclosure. As shown in Fig. 15, in the vertical MOSFET 1A, a GaN substrate 10 has a p+-type buried layer 17 disposed between a p--type well region 13 and an n--type GaN layer 12 (drift region). In this modification, each of the p+-type contact region 15 and the p+-type buried layer 17 is an example of the "p-type region" of the present disclosure.
[0076] The p+ type buried layer 17 is formed, for example, by ion-implanting a p-type impurity such as Mg into the surface 10a side of the GaN substrate 10 and activating the p-type impurity by heat treatment. The p+ type buried layer 17 is formed by ion-implanting Mg as a p-type impurity into the surface 10a side of the GaN substrate 10 and activating the p-type impurity by heat treatment. 18 cm -3 More than 1×10 21 cm -3 The peak concentration of Mg in the depth direction of the p+ type buried layer 17 is, for example, 5×10 18 cm -3 or more, preferably 8×10 19 cm -3 More preferably, it is 1×10 19 cm -3 That's all.
[0077] In addition, in order to relax the compressive stress field formed around Mg, the p+ type buried layer 17 is doped with at least one of a group 13 element and an acceptor element at a concentration of 3×10 17 cm -3 5×10 or more 21 cm -3 More preferably, it is present at a concentration of 2×10 18 cm -3 5×10 or more 21 cm -3 The group 13 element is, for example, at least one of B and Al, and the acceptor element is, for example, at least one of Li and Be. As an example, the p+ type buried layer 17 contains 3×10 Al as the above-mentioned Group 13 element. 17 cm -3 5×10 or more 21 cm -3 More preferably, it is present at a concentration of 2×1018 cm -3 5×10 or more 21 cm -3 The p+ type buried layer 17 has a thickness of, for example, 0.1 μm or more and 0.5 μm or less.
[0078] By disposing p+ type buried layer 17 between p- type well region 13 and n- type GaN layer 12 (drift region), a depletion layer spreads between p+ type buried layer 17 and the drift region, improving the breakdown voltage between p+ type buried layer 17 and the drift region. For example, when the input voltage to gate electrode 22 is at a low level (i.e., when the gate is off), p+ type buried layer 17 can increase the breakdown voltage of vertical MOSFET 1A compared to a case where p+ type buried layer 17 is not provided. The GaN semiconductor device according to the modification of the first embodiment includes a plurality of vertical MOSFETs 1A shown in Fig. 15. Each vertical MOSFET 1A is a repeated unit structure. In the GaN semiconductor device according to this modification, the unit structures are arranged side by side in one direction (for example, the X-axis direction).
[0079] As described above, the vertical MOSFET 1A according to the modification of the first embodiment has the p+ type contact region 15 and the p+ type buried layer 17 provided in the n- type GaN layer 12. The p+ type contact region 15 and the p+ type buried layer 17 each have a 3×10 18 cm -3 More than 1×10 21 cm -3 Mg and 3×10 17 cm -3 5×10 or more 21 cm -3 and at least one of a Group 13 element and an acceptor element (eg, Al) in the following concentrations:
[0080] According to this, in each of the p+ type contact region 15 and the p+ type buried layer 17, the compressive stress field formed by Mg can be offset by the compressive stress field formed by Al. This allows the compressive stress field formed around Mg to be alleviated, and the solid solubility limit of Mg to be improved. It is possible to increase the amount of Mg entering the Ga site and suppress the segregation of Mg, so that a high concentration p type region (in this example, the p+ type contact region 15 and the p+ type buried layer 17) can be realized. In addition, by disposing p+ type buried layer 17 between p- type well region 13 and n- type GaN layer 12 (drift region), a depletion layer spreads between p+ type buried layer 17 and the drift region, so that, for example, the breakdown voltage when the gate is off can be increased.
[0081] <Embodiment 2> In the above-described second embodiment, the vertical MOSFETs 1 and 1A have a planar structure. However, the vertical MOSFET having a “p-type region” of the present disclosure may have a trench gate structure instead of the planar structure.
[0082] (Configuration example) 16 is a cross-sectional view showing a configuration example of a vertical MOSFET 1B according to embodiment 2 of the present disclosure. As shown in FIG. 16, the vertical MOSFET 1B according to embodiment 2 has a trench gate structure. Specifically, the vertical MOSFET 1E has a trench H provided in a GaN substrate 10. The trench H opens on the front surface 10a side of the GaN substrate 10. The trench H is formed deeper than the p-type well region 13, and the bottom of the trench H reaches the n-type GaN layer 12.
[0083] A gate insulating film 21 and a gate electrode 22 are disposed inside the trench H. The gate insulating film 21 covers the inner side and bottom surface of the trench H. The gate electrode 22 is embedded in the trench H via the gate insulating film 21. In the vertical MOSFET 1B, a region of the p-type well region 13 facing the gate electrode 22 via the gate insulating film 21 provided on the inner side surface of the trench H serves as a channel region.
[0084] (Effects of the second embodiment) In the vertical MOSFET 1B, the p+ type contact region 15 has a capacitance of 3×10 18 cm -3 More than 1×10 21 cm -3 Mg and 3×10 17 cm -3 5×10 or more 21 cm -3 and at least one of a Group 13 element and an acceptor element (eg, Al) in the following concentrations:
[0085] According to this, as in the vertical MOSFET 1 according to the first embodiment, in the p+ contact region 15, the compressive stress field formed around Mg can be relaxed, and the solid solubility limit of Mg can be improved. Since the amount of Mg entering the Ga site can be increased and segregation of Mg can be suppressed, a high-concentration p-type region (in this example, the p+ contact region 15) can be realized. A good ohmic connection can be realized between the p+ contact region 15 and the source electrode 25. In addition, the vertical MOSFET 1B has a trench gate structure, which allows for miniaturization. The channel density can be improved, which allows for a low on-resistance.
[0086] (Modification of the second embodiment) (1) Variation 1 Fig. 17 is a cross-sectional view showing a configuration of a vertical MOSFET 1C according to Modification 1 of Embodiment 2 of the present disclosure. As shown in Fig. 17, the vertical MOSFET 1C according to Modification 1 of Embodiment 2 has a p+-type buried layer 17 disposed between a p--type well region 13 and an n--type GaN layer 12 (drift region), similar to the vertical MOSFET 1A according to Modification 1 of Embodiment 1 (see Fig. 15). In Modification 1, each of the p+-type contact region 15 and the p+-type buried layer 17 is an example of the "p-type region" of the present disclosure.
[0087] The configuration of the p+ type buried layer 17 shown in Fig. 17 is the same as the configuration of the p+ type buried layer 17 shown in Fig. 15. That is, the p+ type buried layer 17 is formed by doping 3 × 10 Mg as a p-type impurity. 18 cm -3 More than 1×10 21 cm -3 In order to relax the compressive stress field formed around Mg, the p+ type buried layer 17 contains at least one of a group 13 element and an acceptor element (for example, Al) at a concentration of 3×10 17 cm -3 5×10 or more 21 cm -3 More preferably, it is present at a concentration of 1×10 18 cm -3 More than 2×10 21 cm -3 Contains the following concentrations:
[0088] With this configuration, as in the modified example of the first embodiment, it is possible to relax the compressive stress field formed around Mg in each of the p+ type contact region 15 and the p+ type buried layer 17, and improve the solid solubility limit of Mg. It is possible to increase the amount of Mg entering the Ga site and suppress the segregation of Mg, so that it is possible to realize a high-concentration p-type region (in this example, the p+ type contact region 15 and the p+ type buried layer 17).
[0089] In addition, p+ type buried layer 17 having a higher p-type impurity concentration than p- type well region 13 is disposed between p- type well region 13 and n- type GaN layer 12 (drift region). For example, p+ type buried layer 17 is disposed away from the channel region and exists to a position deeper than the bottom of trench H. This causes a depletion layer to expand between p+ buried layer 17 and the drift region, and electric field concentration at the trench bottom is alleviated, so that, for example, the breakdown voltage when the gate is off can be increased.
[0090] (2) Variation 2 Fig. 18 is a cross-sectional view showing a configuration of a vertical MOSFET 1D according to Modification 2 of Embodiment 2 of the present disclosure. As shown in Fig. 18, in the vertical MOSFET 1D according to Modification 2 of Embodiment 2, a p+ type buried layer 17 is disposed at the bottom of a trench H. For example, the p+ type buried layer 17 is formed wider in the X-axis direction and the Y-axis direction than the bottom of the trench H. The p+ type buried layer 17 is continuously provided from a position shallower than the bottom surface of the trench H (i.e., a position closer to the front surface 10a) to a position deeper than the bottom surface of the trench H (i.e., a position closer to the back surface 10b). As a result, the bottom of the trench H, including its corner portions HC, is covered with the p+ type buried layer 17.
[0091] Even with this configuration, it is possible to realize a high-concentration p-type region (p+ type contact region 15 and p+ type buried layer 17) as in the first modification of the second embodiment described above. In addition, the bottom of trench H is close to drain electrode 26, and the electric field tends to concentrate particularly at corners HC, but the depletion layer spreads from p+ type buried layer 17 arranged at the bottom of trench H toward the drift region side, so that the electric field concentration at the bottom of trench H and its corners HC can be alleviated. This makes it possible to prevent the gate insulating film 21 from being destroyed due to the electric field concentration at the bottom of trench H and its corners HC.
[0092] 18 shows an embodiment in which p+ type buried layer 17 is formed wider than the bottom of trench H. However, modification 2 is not limited to this. p+ type buried layer 17 does not have to be formed wider than the bottom of trench H. For example, p+ type buried layer 17 may be formed to have the same width as the bottom of trench H.
[0093] 18 shows an embodiment in which p+ type buried layer 17 is formed from a position shallower than the bottom surface of trench H to a position deeper than the bottom surface of trench H. However, modification 2 is not limited to this. It is sufficient that p+ type buried layer 17 is in contact with the bottom surface of trench H. For example, p+ type buried layer 17 may be formed from a position at the same depth as the bottom surface of trench H to a position deeper than the bottom surface of trench H.
[0094] <Embodiment 3> The application of the "p-type region" of the present disclosure is not limited to field effect transistors. The "p-type region" of the present disclosure may be applied to, for example, pn diodes. Fig. 19 is a cross-sectional view showing a configuration example of a pn diode 2 according to embodiment 3 of the present disclosure. As shown in Fig. 19, the pn diode 2 includes a GaN substrate 10 having an n+ type GaN single crystal substrate 11 and an n- type GaN layer 12, a p- type well region 13 provided in the GaN substrate 10 and in contact with the n- type GaN layer 12, and a p+ type layer 18 provided in the GaN substrate 10 and in contact with the well region 13. The p+ type layer 18 is located inside the p- type well region 13 and faces the surface 10a of the GaN substrate 10.
[0095] In the pn diode 2, the p+ type layer 18 and the p- type well region 13 are an anode region, and the n+ type GaN single crystal substrate 11 and the n- type GaN layer 12 are a cathode region. In the third embodiment, the p+ type layer 18 is an example of the "p type region" of the present disclosure. The pn diode 2 also includes an anode electrode 125 provided on the front surface 10a of the GaN substrate 10 in contact with the p+ type layer 18, and a cathode electrode 126 provided on the back surface 10b of the GaN substrate 10 in contact with the n+ type GaN single crystal substrate 11. The anode electrode 125 and the cathode electrode 126 are made of, for example, Al or an Al-Si alloy. The anode electrode 125 and the cathode electrode 126 may have a barrier metal layer between them and the GaN substrate 10. Ti may be used as the material of the barrier metal layer.
[0096] The configuration of the p+ type layer 18 is the same as the configuration of the p+ type contact region 15 described in, for example, the first and second embodiments. That is, the p+ type layer 18 is formed by doping 3×10 Mg as a p-type impurity. 18 cm -3 More than 1×10 21 cm -3 More preferably, it is present at a concentration of 1×10 19 cm -3 More than 2×10 20 cm -3 In addition, the p+ type layer 18 contains at least one of a group 13 element and an acceptor element (e.g., Al) at a concentration of 3×10 17 cm -3 5×10 or more 21 cm -3 Containing at a concentration of 5×10 or less, more preferably 5×10 18 cm -3 More than 4×10 20 cm -3 Contains the following concentrations:
[0097] With this configuration, in the p+ type layer 18 constituting the anode region of the pn diode 2, the compressive stress field formed by Mg can be offset by the compressive stress field formed by Al. This allows the compressive stress field formed around Mg to be alleviated, and the solid solubility limit of Mg to be improved. It is possible to increase the amount of Mg entering the Ga site, and suppress the segregation of Mg, so that a high concentration p+ type region (in this example, the p+ type layer 18) can be realized. A good ohmic connection can be realized between the p+ type layer 18 and the anode electrode 125.
[0098] <Other embodiments> As described above, the present disclosure has been described with reference to the first to third embodiments and their modifications. However, the description and drawings forming a part of this disclosure should not be understood as limiting the present disclosure. Various alternative embodiments and modifications will be apparent to those skilled in the art from this disclosure. For example, FIG. 1 shows a case where the shape of the p+ type contact region 15 in plan view from the Z-axis direction is a strip extending in the Y-axis direction. However, the shape of the contact region 15 in plan view from the Z-axis direction is not limited to a strip. The shape of the p+ type contact region 15 in plan view from the Z-axis direction may be a polygon such as a square, hexagon, or octagon, or may be a circle.
[0099] Thus, the present disclosure naturally includes various embodiments not described herein. At least one of various omissions, substitutions, and modifications of components can be made without departing from the spirit of the above-mentioned embodiments 1 to 3 and their modifications. Furthermore, the effects described in this specification are merely examples and are not limited thereto, and other effects may also be present. The technical scope of the present disclosure is defined only by the invention-specific matters related to the scope of the claims that are appropriate from the above description.
[0100] The present disclosure can also be configured as follows. (1) A nitride crystal layer; a p-type region provided in the nitride crystal layer, The p-type region is 3×10 18 cm -3 More than 1×10 21 cm -3 Mg at the following concentrations: 3×10 17 cm -3 5×10 or more 21 cm -3 and at least one of a Group 13 element and an acceptor element in the following concentrations: (2) The nitride semiconductor device according to (1), wherein the Group 13 element is at least one of B and Al. (3) The nitride semiconductor device according to (1) or (2), wherein the acceptor element is at least one of Li and Be. (4) Further comprising a nitride crystal substrate; the nitride crystal layer is provided on one surface of the nitride crystal substrate, The nitride semiconductor device according to any one of (1) to (3), wherein a lattice constant of the p-type region in a first direction parallel to the one surface and a lattice constant in a second direction parallel to the one surface and intersecting the first direction are equal to the lattice constants of the nitride crystal substrate in the first direction and the second direction, respectively. (5) a p-type well region provided in the nitride crystal layer; a field effect transistor provided in the nitride crystal layer, the field effect transistor having a channel formed in the well region; The nitride semiconductor device according to any one of (1) to (4), wherein the p-type region has a higher concentration of the acceptor element than the well region and is electrically connected to the well region. (6) a diode provided in the nitride crystal layer, The nitride semiconductor device according to any one of (1) to (4), wherein the p-type region is an anode region of the diode. (7) 3×10 in the nitride crystal layer18 cm -3 More than 1×10 21 cm -3 introducing Mg at a concentration of The region in which the Mg is introduced in the nitride crystal layer is filled with 3×10 17 cm -3 5×10 or more 21 cm -3 introducing at least one of a group 13 element and an acceptor element at a concentration of and performing a heat treatment on the nitride crystal layer into which the Mg and at least one of the Group 13 element and the acceptor element have been introduced to activate the Mg, thereby forming a p-type region in the nitride crystal layer. (8) The method further comprises the step of ion-implanting N into a region of the nitride crystal layer into which the Mg is introduced, In the step of forming the p-type region, The method for producing a nitride semiconductor device according to (7) above, further comprising the step of subjecting the nitride crystal layer into which N has been ion-implanted to the heat treatment. (9) forming a protective film on the nitride crystal layer into which the Mg has been introduced and into which the N has been ion-implanted; In the step of forming the p-type region, The method for manufacturing a nitride semiconductor device according to (8) above, further comprising subjecting the nitride crystal layer on which the protective film is formed to the heat treatment. (10) The step of introducing Mg into the nitride crystal layer comprises: The method for producing a nitride semiconductor device according to any one of (7) to (9) above, wherein the Mg is ion-implanted into the nitride crystal layer. (11) The step of introducing Mg into the nitride crystal layer comprises: forming a first film containing Mg on the nitride crystal layer; The method for manufacturing a nitride semiconductor device according to any one of (7) to (9), further comprising: subjecting the nitride crystal layer on which the first film is formed to a first heat treatment, thereby thermally diffusing the Mg from the first film to the nitride crystal layer. (12) The step of introducing at least one of the Group 13 element and the acceptor element into the nitride crystal layer includes: The method for producing a nitride semiconductor device according to any one of (7) to (11) above, wherein at least one of the Group 13 element and the acceptor element is ion-implanted into the nitride crystal layer. (13) The step of introducing at least one of the Group 13 element and the acceptor element includes: forming a second film containing at least one of the Group 13 element and the acceptor element on the nitride crystal layer; The method for manufacturing a nitride semiconductor device according to any one of (7) to (11), further comprising: performing a second heat treatment on the nitride crystal layer on which the second film is formed, thereby thermally diffusing at least one of the Group 13 element and the acceptor element from the second film to the nitride crystal layer. [Explanation of symbols]
[0101] 1, 1A, 1B, 1C, 1D, 1E Vertical MOSFET 2 pn diode 10 GaN substrate 10a surface 10b back side 11 GaN single crystal substrate 12 GaN layers 13 Well Area 13´ Well formation area 14 Protective film 15 Contact Area 15´ Contact formation area 17 p+ buried layer 18 p+ type layer 21 Gate insulating film 22 Gate electrode 23 Source Region 23´ Source formation region 25 Source electrode 26 Drain electrode 31 Al-doped layer 33 MgAl mixture 35 Mg film 100 GaN semiconductor device 125 Anode Electrode 126 Cathode Electrode d1, d2 Center distance H Trench HC corner
Claims
1. A nitride crystal layer; a p-type region provided in the nitride crystal layer, The p-type region is 3×10 18 cm -3 Above 1 x 10 21 cm -3 Mg at the following concentrations: 3×10 17 cm -3 Above 5 x 10 21 cm -3 and at least one of a Group 13 element and an acceptor element in the following concentrations:
2. The nitride semiconductor device according to claim 1 , wherein said Group 13 element is at least one of B and Al.
3. 3. The nitride semiconductor device according to claim 1, wherein the acceptor element is at least one of Li and Be.
4. Further comprising a nitride crystal substrate; the nitride crystal layer is provided on one surface of the nitride crystal substrate, 3. The nitride semiconductor device according to claim 1, wherein a lattice constant of said p-type region in a first direction parallel to said one surface and a lattice constant in a second direction parallel to said one surface and intersecting said first direction are equal to each of the lattice constants of said nitride crystal substrate in said first direction and said second direction, respectively.
5. a p-type well region provided in the nitride crystal layer; a field effect transistor provided in the nitride crystal layer, the field effect transistor having a channel formed in the well region; 3 . The nitride semiconductor device according to claim 1 , wherein said p-type region has a higher concentration of said acceptor element than said well region and is electrically connected to said well region.
6. a diode provided in the nitride crystal layer, 3. The nitride semiconductor device according to claim 1, wherein said p-type region is an anode region of said diode.
7. 3×10 on the nitride crystal layer 18 cm -3 Above 1 x 10 21 cm -3 Introducing Mg at a concentration of The region in which the Mg is introduced in the nitride crystal layer is 17 cm -3 Above 5 x 10 21 cm -3 doping at least one of a group 13 element and an acceptor element at a concentration of and a step of performing a heat treatment on the nitride crystal layer into which the Mg and at least one of the group 13 element and the acceptor element have been introduced to activate the Mg, thereby forming a p-type region in the nitride crystal layer.
8. further comprising a step of ion-implanting N into a region of the nitride crystal layer into which the Mg is introduced, In the step of forming the p-type region, The method for manufacturing a nitride semiconductor device according to claim 7 , wherein the heat treatment is performed on the nitride crystal layer into which the N ions are implanted.
9. forming a protective film on the nitride crystal layer into which the Mg has been introduced and into which the N has been ion-implanted; In the step of forming the p-type region, The method for manufacturing a nitride semiconductor device according to claim 8 , further comprising the step of: subjecting said nitride crystal layer on which said protective film is formed to said heat treatment.
10. The step of introducing Mg into the nitride crystal layer includes:
9. The method for manufacturing a nitride semiconductor device according to claim 7, wherein the Mg is ion-implanted into the nitride crystal layer.
11. The step of introducing Mg into the nitride crystal layer includes: forming a first film containing Mg on the nitride crystal layer; 9. The method for manufacturing a nitride semiconductor device according to claim 7, further comprising the step of: subjecting the nitride crystal layer on which the first film is formed to a first heat treatment, thereby thermally diffusing the Mg from the first film into the nitride crystal layer.
12. The step of introducing at least one of the Group 13 element and the acceptor element into the nitride crystal layer includes:
9. The method for manufacturing a nitride semiconductor device according to claim 7, wherein the method is performed by ion-implanting at least one of the Group 13 element and the acceptor element into the nitride crystal layer.
13. The step of introducing at least one of the Group 13 element and the acceptor element includes: forming a second film containing at least one of the Group 13 element and the acceptor element on the nitride crystal layer; 9. The method for manufacturing a nitride semiconductor device according to claim 7, further comprising: performing a second heat treatment on the nitride crystal layer on which the second film is formed, thereby thermally diffusing at least one of the Group 13 element and the acceptor element from the second film to the nitride crystal layer.
Citation Information
Patent Citations
Nitride semiconductor device manufacturing method
JP2014086698A
VERTICAL GaN-BASED SEMICONDUCTOR DEVICE MANUFACTURING METHOD AND VERTICAL GaN-BASED SEMICONDUCTOR DEVICE
JP2019096744A
Cited By