Method for producing silicon clathrate electrode active material, and method for manufacturing lithium ion battery

The method of using hydrogen fluoride and water treatments to remove type I silicon clathrate and by-products enhances the efficiency of type II silicon clathrate as a negative electrode active material in lithium ion batteries, addressing the limitations of existing silicon clathrate materials.

JP2024165104APending Publication Date: 2024-11-28TOYOTA JIDOSHA KK +1

Patent Information

Application Number
JP2023080978
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing silicon clathrate electrode active materials, particularly type II silicon clathrate, face limitations in reducing expansion and contraction during charging and discharging due to the presence of type I silicon clathrate and associated by-products, which do not function effectively as electrode active materials.

Method used

A method involving the use of a hydrogen fluoride organic solvent to selectively remove type I silicon clathrate and subsequent treatment with water or an aqueous solvent to eliminate by-products such as sodium silicofluoride, thereby enhancing the efficiency of type II silicon clathrate as an electrode active material.

Benefits of technology

The method effectively reduces the content of type I silicon clathrate and by-products, improving the performance of type II silicon clathrate as a negative electrode active material in lithium ion batteries by minimizing expansion and contraction during charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165104000001_ABST
    Figure 2024165104000001_ABST
Patent Text Reader

Abstract

To provide: a method for producing a silicon clathrate electrode active material, capable of removing at least part of a type-I silicon clathrate and also capable of removing at least part of by-products; and a method for manufacturing a lithium ion battery, including the production of such a silicon clathrate electrode active material.SOLUTION: A method of the present disclosure for producing a silicon clathrate electrode active material includes the steps of: (a) providing a first silicon clathrate-containing composition containing a type-I silicon clathrate and a type-II silicon clathrate; (b) bringing the first silicon clathrate-containing composition into contact with a solution containing a hydrogen fluoride organic solvent and removing at least part of the type-I silicon clathrate to obtain a second silicon clathrate-containing composition: and (c) bringing the second silicon clathrate-containing composition into contact with water or an aqueous solvent, and removing at least part of by-products generated in the step (b).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a silicon clathrate electrode active material and a method for producing a lithium ion battery. [Background technology]

[0002] In recent years, the development of batteries has been actively carried out. For example, in the automobile industry, development of batteries for use in electric vehicles or hybrid vehicles is underway. Silicon is known as an active material for batteries, particularly lithium ion batteries.

[0003] Silicon electrode active materials have a large theoretical capacity and are effective in increasing the energy density of batteries. On the other hand, silicon electrode active materials have a problem of large expansion during charging. It is known that the expansion during charging can be suppressed by using a silicon clathrate electrode active material as the silicon electrode active material.

[0004] For example, Patent Document 1 discloses a silicon clathrate electrode active material having a silicon clathrate type II crystal phase, having voids inside the primary particles, and having a void volume of pores having a pore diameter of 100 nm or less of 0.05 cc / g or more and 0.15 cc / g or less. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2021-158004 Summary of the Invention [Problem to be solved by the invention]

[0006] There are various types of silicon clathrate crystals, including type I silicon clathrate and type II silicon clathrate. In particular, type II silicon clathrate efficiently occludes lithium in the cage structure of the crystals, and therefore expands and contracts little when the battery is charged and discharged.

[0007] Therefore, from the viewpoint of suppressing the expansion during charging and discharging of the battery, it is desirable to remove the I-type silicon clathrate, but when removing the I-type silicon clathrate, by-products may be generated. Since such by-products do not function as an electrode active material, there is a possibility that the effect of reducing the expansion and contraction during charging and discharging when the II-type silicon clathrate is used as the electrode active material is limited.

[0008] Under these circumstances, it is desirable to develop a method for removing the I-type silicon clathrate from a silicon clathrate that contains both the I-type silicon clathrate and the II-type silicon clathrate, and a method for removing at least a portion of the by-products.

[0009] The present disclosure aims to provide a method for producing a silicon clathrate electrode active material capable of removing at least a portion of the type I silicon clathrate and at least a portion of the by-products, and a method for producing a lithium ion battery including producing such a silicon clathrate electrode active material. [Means for solving the problem]

[0010] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> A method for producing a silicon clathrate electrode active material, comprising the steps of: (a) providing a first silicon clathrate-containing composition containing a silicon clathrate type I and a silicon clathrate type II; (b) contacting the first silicon clathrate-containing composition with a hydrogen fluoride organic solvent-containing solution to remove at least a portion of the I-type silicon clathrate to obtain a second silicon clathrate-containing composition; and (c) contacting the second silicon clathrate-containing composition with water or an aqueous solvent to remove at least a portion of the by-products produced in step (b). <Aspect 2> 2. The method of embodiment 1, wherein the organic solvent is an alcohol. <Aspect 3> 3. The method of claim 1 or 2, wherein the by-product is sodium silicofluoride. <Aspect 4> The method according to any one of aspects 1 to 3, wherein the silicon clathrate electrode active material is for use as a negative electrode active material in a lithium ion battery. <Aspect 5> Producing a silicon clathrate electrode active material by the method according to any one of aspects 1 to 4; and forming an electrode active material layer containing the silicon clathrate electrode active material; A method for producing a lithium ion battery, comprising: Effect of the Invention

[0011] According to the method of the present disclosure for producing a silicon clathrate electrode active material, at least a part of the I-type silicon clathrate can be removed, and at least a part of the by-products can be removed. In addition, the present disclosure can provide a method for producing a lithium-ion battery, which includes producing such a silicon clathrate electrode active material. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a graph showing the results of X-ray diffraction (XRD) measurement of the first silicon clathrate-containing composition of Comparative Example 4 before and after contacting with a hydrogen fluoride solution. [Diagram 2]FIG. 2 is a graph showing the results of XRD measurement of the silicon clathrate electrode active materials of Comparative Example 4 and Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0014] <<Method for producing silicon clathrate electrode active material>> The disclosed method for producing a silicon clathrate electrode active material includes: (a) providing a first silicon clathrate-containing composition containing a type I silicon clathrate and a type II silicon clathrate; (b) contacting the first silicon clathrate-containing composition with a hydrogen fluoride organic solvent-containing solution to remove at least a portion of the type I silicon clathrate to obtain a second silicon clathrate-containing composition; and (c) contacting the second silicon clathrate-containing composition with water or an aqueous solvent to remove at least a portion of the by-products generated in step (b). Includes.

[0015] The present inventors have found that there is a difference in solubility in hydrogen fluoride solution between I-type silicon clathrate and II-type silicon clathrate. In other words, since I-type silicon clathrate has higher solubility in hydrogen fluoride solution, it is considered that I-type silicon clathrate can be removed from the silicon clathrate by contacting a silicon clathrate containing I-type silicon clathrate and II-type silicon clathrate with a hydrogen fluoride solution under appropriate conditions.

[0016] However, the present inventors have reported that when the hydrogen fluoride solution, particularly a hydrogen fluoride-containing organic solvent solution, is used, sodium silicofluoride (Na 2 SiF 6 It was found that unintended by-products such as

[0017] In response to this, the present inventors have combined a treatment with a hydrogen fluoride organic solvent-containing solution and a treatment with water or an aqueous solvent to remove type I silicon clathrate by the treatment with a hydrogen fluoride organic solvent-containing solution, and to remove Na by the treatment with water or an aqueous solvent. 2 SiF 6 It has been found that by-products such as

[0018] In addition, with respect to the present disclosure, the "electrode active material" can be used as either a "positive electrode active material" or a "negative electrode active material", and is particularly used as a "negative electrode active material".

[0019] <Provision of first silicon clathrate-containing composition> The method of the present disclosure includes providing a first silicon clathrate-containing composition that contains a type I silicon clathrate and a type II silicon clathrate.

[0020] The first silicon clathrate-containing composition can be prepared by preparing a sodium silicon (NaSi) alloy and removing sodium from the NaSi alloy.

[0021] Specifically, a silicon source is reacted with a sodium source such as sodium hydride to prepare a NaSi alloy. The NaSi alloy thus prepared is then heated to remove sodium from the NaSi alloy and form a clathrate, thereby preparing a first silicon clathrate-containing composition. Alternatively, the NaSi alloy thus prepared is reacted with aluminum fluoride as a sodium trapping agent to remove sodium from the NaSi alloy and form a clathrate, thereby preparing a first silicon clathrate-containing composition.

[0022] <Removal of type I silicon clathrate> The method of the present disclosure includes contacting a first silicon clathrate-containing composition with a hydrogen fluoride organic solvent-containing solution to remove at least a portion of the type I silicon clathrate to obtain a second silicon clathrate-containing composition.

[0023] The organic solvent may be any organic solvent capable of dissolving hydrogen fluoride. The organic solvent is preferably an alcohol, more preferably a lower alcohol, and even more preferably ethanol.

[0024] The organic solvent-containing solution may be a mixed solvent of an organic solvent and water. When an organic solvent is mixed with water, any organic solvent that can dissolve hydrogen fluoride and is compatible with water may be used.

[0025] The contact method is, for example, a mixing operation such as stirring, but is not limited thereto.

[0026] The contact time may be 0.5 hours or more, 1 hour or more, or 2 hours or more, and may be 6 hours or less, 5 hours or less, or 4 hours or less.

[0027] The content ratio of the I-type silicon clathrate and the II-type silicon clathrate in the first silicon clathrate-containing composition can be calculated, for example, from the peak intensity ratio in the measurement results of X-ray diffraction (XRD).

[0028] Removal of By-Products The method of the present disclosure includes contacting the second silicon clathrate-containing composition with water or an aqueous solvent to remove at least a portion of the by-products produced in step (b).

[0029] In this disclosure, "aqueous solvent" means a mixture of water and one or more other water-miscible solvents.

[0030] The method of contacting the second silicon clathrate-containing composition with water or an aqueous solvent includes, but is not limited to, washing the silicon clathrate with water or an aqueous solvent.

[0031] When the method of contacting the second silicon clathrate-containing composition with water or an aqueous solvent is a washing operation, the amount of water or an aqueous solvent used for each washing may be 10 ml or more, 15 ml or more, or 20 ml or more, and the number of washings may be 1 or more, 2 or more, or 3 or more.

[0032] The by-product is sodium silicofluoride (Na 2 SiF 6 ) The by-product may be Na 2 SiF 6 In this case, the removal by contact described above proceeds efficiently.

[0033] The by-product is Na 2 SiF 6 In the case where the silicon clathrate electrode active material produced by the method of the present disclosure is 2 SiF 6 The ratio of the mass of the silicon clathrate particles to the total mass of the silicon clathrate particles may be 0.8 mass% or less, 0.7 mass% or less, 0.6 mass% or less, 0.5 mass% or less, 0.4 mass% or less, or 0.3 mass% or less.

[0034] <Application> The silicon clathrate electrode active material in the method of the present disclosure can be used as the negative electrode active material in a lithium ion battery.

[0035] <<How lithium-ion batteries are manufactured>> The disclosed method of making a lithium ion battery includes making a silicon clathrate electrode active material by the disclosed method and forming an electrode active material layer containing the silicon clathrate electrode active material.

[0036] For the method for producing the silicon clathrate electrode active material, reference can be made to the above description regarding the method for producing the silicon clathrate electrode active material of the present disclosure.

[0037] The method for forming the electrode active material layer is not particularly limited, and a known method can be adopted. For example, when the negative electrode active material layer contains the silicon clathrate electrode active material of the present disclosure, the electrode active material layer formed on the negative electrode current collector layer, i.e., the negative electrode active material layer, can be obtained by applying a slurry containing the silicon clathrate electrode active material to the negative electrode current collector and drying it.

[0038] The method for forming the battery is not particularly limited, and any known method can be used. Hereinafter, a method for producing a battery in which the negative electrode active material layer contains the silicon clathrate electrode active material of the present disclosure will be described.

[0039] The method for manufacturing a battery according to the present disclosure may include, in addition to manufacturing a silicon clathrate electrode active material and forming a negative electrode active material layer containing the silicon clathrate electrode active material, arranging, in this order, a negative electrode current collector layer, a negative electrode active material layer, an electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer.

[0040] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, copper, a copper alloy, and copper plated or vapor-deposited with nickel, chromium, carbon, or the like may be used, but is not limited to these.

[0041] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0042] <Negative electrode active material layer> The negative electrode active material layer of the present disclosure is a layer containing a negative electrode active material, and optionally an electrolyte, a conductive assistant, and a binder.

[0043] (Negative electrode active material) The negative electrode active material comprises a silicon clathrate electrode active material of the present disclosure.

[0044] (electrolyte) The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in lithium ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.

[0045] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li 2 SP 2 S 5 System (Li 7 P 3 S 11 , Li 3 P.S. 4 , Li 8 P 2 S 9 etc.), Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2 , LiI-Li 2 SP 2 S 5 , LiI-LiBr-Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -GeS 2 (Li 13 GeP 3 S 16 , Li 10 GeP 2 S 12 etc.), LiI-Li 2 SP 2 O 5 , LiI-Li 3 PO 4 -P 2 S 5 , Li 7 - x P.S. 6 - x Clx etc.; or combinations thereof, but are not limited to these.

[0046] The sulfide solid electrolyte may be a glass or a crystallized glass (glass ceramic).

[0047] When the negative electrode active material layer contains a solid electrolyte, the mass ratio of the silicon clathrate electrode active material to the solid electrolyte in the negative electrode active material layer (mass of silicon clathrate electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0048] The electrolyte preferably contains a supporting salt and a solvent.

[0049] As a supporting salt (lithium salt) of the electrolyte having lithium ion conductivity, for example, LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 Inorganic lithium salts such as LiCF 3 SO 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , LiN(FSO 2 ) 2 , LiC(CF 3 SO 2 ) 3 Examples of organic lithium salts include those mentioned above.

[0050] Examples of the solvent used in the electrolytic solution include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolytic solution preferably contains two or more kinds of solvents.

[0051] (Conductive assistant) The conductive assistant is not particularly limited. For example, the conductive assistant may be VGCF (Vapor Grown Carbon Fiber), acetylene black (AB), Ketjen Black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.

[0052] (binder) The binder is not particularly limited. For example, the binder may be a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), or styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.

[0053] The thickness of the negative electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.

[0054] <Electrolyte layer> The electrolyte layer includes at least an electrolyte. The electrolyte layer may include a binder, etc., if necessary, in addition to the electrolyte. For the electrolyte and the binder, the above description regarding the negative electrode active material layer of the present disclosure can be referred to.

[0055] The thickness of the electrolyte layer is, for example, 0.1 to 300 μm, and preferably 0.1 to 100 μm.

[0056] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally an electrolyte, a conductive assistant, a binder, and the like.

[0057] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material is lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganate (LiMn 2 O 4 ), LiCo1 / 3 Ni 1 / 3 Mn 1 / 3 O 2 , Li 1+x Mn 2-x-y MyO 4 Li-Mn spinel substituted with different elements having a composition represented by the formula (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO 4 , M may be one or more metals selected from Fe, Mn, Co, and Ni), but is not limited thereto.

[0058] The positive electrode active material may have a coating layer. The coating layer is a layer containing a material that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials that constitute the coating layer include LiNbO 3 In addition, Li 4 Ti 5 O 12 , Li 3 PO 4 These include, but are not limited to, the following.

[0059] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0060] For the electrolyte, the conductive assistant, and the binder, reference can be made to the above descriptions regarding the negative electrode active material layer of the present disclosure.

[0061] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 50:50.

[0062] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.

[0063] <Positive electrode current collector layer> The material used for the positive electrode current collector layer is not particularly limited, and any material that can be used as a positive electrode current collector for a battery can be appropriately adopted. For example, SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium, zinc, etc., and these metals plated or vapor-deposited with nickel, chromium, carbon, etc. may be used, but is not limited to these.

[0064] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0065] The lithium ion battery produced by the method of the present disclosure may be a liquid battery containing an electrolytic solution as an electrolyte layer, or may be a solid battery having a solid electrolyte layer as an electrolyte layer. In the present disclosure, a "solid-state battery" means a battery using at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. The solid-state battery of the present disclosure may also be an all-solid-state battery, i.e., a battery using only a solid electrolyte as an electrolyte.

[0066] The lithium ion battery produced by the method of the present disclosure may be a primary battery or a secondary battery.

[0067] Examples of the shape of the lithium ion battery include a coin type, a laminate type, a cylindrical type, and a square type. EXAMPLES

[0068] 《Synthesis of silicon clathrate electrode active material》 <Alloying> (Synthesis Examples 1 to 6 and Comparative Synthesis Examples 1 to 4) As a silicon (Si) source, Si powder (Kojundo Kagaku, SIEPB32) was prepared. This Si powder and metallic lithium (Li) were weighed out in a molar ratio of Li / Si=4.0, and the weighed Si powder and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon (LiSi) alloy. The obtained LiSi alloy was reacted with ethanol in an argon atmosphere and treated with hydrogen fluoride (HF) to obtain a Si powder having voids inside the primary particles, i.e., a Si powder having a porous structure.

[0069] A sodium silicon (NaSi) alloy was produced using Si powder having a porous structure and sodium hydride (NaH) as a sodium (Na) source. The NaH used was washed with hexane in advance. NaH and Si powder having a porous structure were weighed out so that the molar ratio was 1.05:1, and the weighed NaH and Si powder having a porous structure were mixed in a cutter mill. The resulting mixture was heated in a heating furnace under an argon atmosphere at 500°C for 40 hours to obtain a powdered NaSi alloy.

[0070] <Clathrate formation> Aluminum Fluoride (AlF 3 The ratio of the amount of the substance of NaSi alloy to the amount of the substance of NaSi alloy was 0.36. 3 The powdered reaction raw materials were mixed in a cutter mill to obtain reaction raw materials. The obtained powdered reaction raw materials were placed in a stainless steel reaction vessel and heated in a heating furnace under an argon atmosphere at 330°C for 60 hours to obtain a reaction product containing silicon clathrate. The obtained reaction product was dissolved in HNO 3 and H 2The reaction product was washed with an acid using a mixed solvent of 10:90 by volume of O, and the by-products in the reaction product were removed. After washing, the reaction product was filtered, and the filtered solid was dried at 120° C. for 3 hours or more to obtain a powdered first silicon clathrate-containing composition.

[0071] The manufacturing conditions of each example, the ratio of the components contained in the first silicon clathrate-containing composition, and the ratio of the mass of the II-type silicon clathrate to the total mass of the I-type silicon clathrate and the II-type silicon clathrate are shown in Table 1. The ratio of the components contained was calculated from the peak intensity ratio in the XRD measurement results. In addition, in Table 1 and Table 2 described later, "II-type" indicates the II-type silicon clathrate, and "I-type" indicates the I-type silicon clathrate.

[0072] [Table 1]

[0073] <Removal of Type I Silicon Clathrate and By-Products> Example 1 100 ml of ethanol was added to 2.2 g of the first silicon clathrate-containing composition of Synthesis Example 1 and stirred. 3.71 ml of 46 wt % HF aqueous solution was added thereto. This solution was reacted by stirring for 3 hours to remove the I-type silicon clathrate. The resulting reaction solution was filtered to obtain a second silicon clathrate-containing composition.

[0074] The second silicon clathrate-containing composition was washed four times with 25 ml of ion-exchanged water, and then washed eight times with 25 ml of ethanol. After washing, the composition was dried overnight at 120° C. to obtain the silicon clathrate electrode active material of Example 1.

[0075] (Examples 2 to 6) 75 ml of ion-exchanged water and 20 ml of ethanol were added to 2.2 g of the first silicon clathrate-containing composition of Synthesis Examples 2 to 6, and the mixture was stirred. 4.5 ml of 46 wt % HF aqueous solution was added thereto. The solution was stirred for 3 hours to react, and the I-type silicon clathrate was removed. The resulting reaction liquid was filtered to obtain a second silicon clathrate-containing composition.

[0076] The second silicon clathrate-containing composition was washed three times with 50 ml of ion-exchanged water, and further washed once with 20 ml of ethanol. After washing, it was dried overnight at 120° C. to obtain the silicon clathrate electrode active materials of Examples 2 to 6.

[0077] (Comparative Examples 1 to 4) The silicon clathrate electrode active materials of Comparative Examples 1 to 4 were obtained in the same manner as in Example 1, except that the first silicon clathrate-containing compositions of Comparative Synthesis Examples 1 to 4 were used, washing with ion-exchanged water was not performed to remove by-products, and the drying temperature was set to 60°C.

[0078] Table 2 shows the production conditions for each example, the ratio of components contained in the silicon clathrate electrode active material, and the ratio of the mass of the II-type silicon clathrate to the total mass of the I-type silicon clathrate and the II-type silicon clathrate.

[0079] Moreover, the XRD measurement results before and after the first silicon clathrate-containing composition of Comparative Example 4 was contacted with a hydrogen fluoride solution are shown in Fig. 1. Furthermore, the XRD measurement results of Comparative Example 4, and the silicon clathrate electrode active material of Example 1, which has the same ratio of components as Comparative Example 4 and the first silicon clathrate-containing composition, are shown in Fig. 2. Note that in each Example and Comparative Example, the Example number corresponds to the Synthesis Example number, and the Comparative Example number corresponds to the Comparative Synthesis Example number, respectively.

[0080] [Table 2]

[0081] As shown in Table 2 and Figures 1 and 2, the silicon clathrate electrode active material of the example in which the first silicon clathrate-containing composition was contacted with hydrogen fluoride in an ethanol-containing solution and the resulting second silicon clathrate-containing composition was contacted with water had a low content of I-type silicon clathrate and a low content of the by-product Na 2 SiF 6 The content was low.

Claims

1. A method for producing a silicon clathrate electrode active material, comprising the steps of: (a) providing a first silicon clathrate-containing composition containing a type I silicon clathrate and a type II silicon clathrate; (b) contacting the first silicon clathrate-containing composition with a hydrogen fluoride organic solvent-containing solution to remove at least a portion of the I-type silicon clathrate to obtain a second silicon clathrate-containing composition; and (c) contacting the second silicon clathrate-containing composition with water or an aqueous solvent to remove at least a portion of the by-products produced in step (b).

2. The method of claim 1 , wherein the organic solvent is an alcohol.

3. The method of claim 1 , wherein the by-product is sodium silicofluoride.

4. 10. The method of claim 1, wherein the silicon clathrate electrode active material is for use as an anode active material in a lithium ion battery.

5. Producing a silicon clathrate electrode active material by the method according to any one of claims 1 to 4; and forming an electrode active material layer containing the silicon clathrate electrode active material; A method for producing a lithium ion battery, comprising:

Citation Information

Patent Citations

  • Method for producing purified silicon fine particles

    JP2021042112A

  • Method for manufacturing negative electrode active material

    JP2023043948A

  • Active material, negative electrode layer, battery, and manufacturing method thereof

    JP2023044620A

  • Negative electrode active material, negative electrode comprising negative electrode active material, secondary battery comprising negative electrode, and method for preparing negative electrode active material

    WO2023033370A1

  • Active material, negative electrode layer, battery and these manufacturing methods

    JP2021158004A

Cited By

  • Method for manufacturing porous silicon clathrate electrode active material and method for manufacturing lithium ion battery

    JP2024168549A

  • Method for manufacturing porous silicon clathrate electrode active material and method for manufacturing lithium ion battery

    JP7754136B2