Method for manufacturing bonded substrate and method for manufacturing semiconductor device
By adjusting surface roughness and free energy, the method enhances bonding quality and reliability of semiconductor substrates, reducing defects and ensuring high-quality semiconductor devices.
Patent Information
- Application Number
- JP2023081559
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2043-05-17
AI Technical Summary
Bonding defects occur during the direct bonding of semiconductor substrates due to inadequate consideration of both surface roughness (Ra) and surface free energy, leading to poor bonding quality and reliability.
The method involves preparing substrates with an average surface roughness (Ra) of 1 nm or less and a contact angle with water of 70° or less to adjust the surface free energy, ensuring proper bonding by directly bonding substrates with appropriate surface conditions.
This approach significantly reduces bonding defects, resulting in high-quality bonded substrates and reliable semiconductor devices with improved bonding interfaces and reduced voids.
Smart Images

Figure 2024165393000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a bonded substrate and a method for manufacturing a semiconductor device, for example, a method for manufacturing a bonded substrate manufactured by bonding a SiC wafer, a GaN substrate, or the like, and a method for manufacturing a semiconductor device. [Background technology]
[0002] SiC and GaN have a wider band gap than Si, which gives them high dielectric breakdown strength, and they also have high thermal conductivity, so they are expected to be used as semiconductor materials for various semiconductor devices such as power devices and high-frequency devices. In addition, by bonding semiconductor substrates, it is possible to improve heat dissipation characteristics.
[0003] For example, Non-Patent Document 1 reports that in devices using SiC, the SiC substrate and the subsequent epitaxial growth account for half of the cost, and points out that reducing the cost of the substrate is extremely important. + A method has been proposed in which ion implantation is performed and then substrate peeling is performed. For example, Patent Document 1 states that + A method is disclosed in which ion-implanted single-crystal and polycrystalline SiC substrates are bonded together, and then the single crystal and polycrystalline substrates are separated from each other. Furthermore, Patent Document 2 also describes a wide variety of substrates. + This paper describes a method for fabricating such a device using a peeling technique, and describes a method for epitaxially growing InGaN after polishing or dry etching the surface.
[0004] Furthermore, apart from SiC, Non-Patent Document 2 proposes and discloses that a diamond substrate is bonded to a GaN substrate to improve heat dissipation characteristics.
[0005] Non-Patent Document 3 refers to the surface free energy in these substrate bondings, and states that when solids come into contact with each other, if atoms form bonds between the contacting surfaces, the surface free energy decreases, and the energy of the entire solid also decreases, which is the driving force for bonding. It also states that the requirement for bonding at this time is that the surface roughness (Ra: average surface roughness) between the substrates needs to be less than 1 nm. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2016-018890 A [Patent Document 2] Special Publication No. 2013-513963 [Non-patent literature]
[0007] [Non-Patent Document 1] Iwamuro, “Progress in High Performance and High Reliability of SiC MOSFETs”, Proceedings of the Wide Bandgap Semiconductor Society Special Open Symposium, Wide Bandgap Semiconductor Society, 2022 [Non-Patent Document 2] Shuichi Hiza, Kunihiko Nishimura, Eiji Yagyu, Mikio Yamamuki, “Development of GaN-HEMT using diamond heat dissipation substrate”, Applied Physics, 90, (3), 167 (2021) [Non-Patent Document 3] Tadatomo Suga, “Room-temperature bonding by surface activation and its mechanism”, Applied Physics, 89, (9), 498 (2020) Summary of the Invention [Problem to be solved by the invention]
[0008] Based on this knowledge about surface roughness during substrate bonding, polishing and processing are performed to an Ra of 1 nm or less, but in reality, bonding defects may occur.
[0009] Therefore, the present invention has been made to solve the above problems, and an object of the present invention is to provide a method for manufacturing a bonded substrate that can reduce the occurrence of bonding defects in bonding technology. [Means for solving the problem]
[0010] In order to achieve the above object, the present invention provides a method for producing a bonded substrate by directly bonding surfaces of two substrates, comprising the steps of: The method includes a step of preparing the two substrates based on the average surface roughness Ra and the surface free energy of the surfaces to be directly bonded, and a step of directly bonding the two substrates prepared, In the step of preparing the two substrates, The present invention provides a method for manufacturing a bonded substrate, which comprises preparing substrates whose surfaces to be directly bonded have an average surface roughness Ra of 1 nm or less, and whose surfaces to be directly bonded have a contact angle with water of 70° or less, which is an index of the surface free energy.
[0011] Thus, in the present invention, in addition to making Ra 1 nm or less for the surfaces to be directly bonded, the surface free energy is also taken into consideration. If the surface free energy is small, it is considered that the substrates will repel each other and will not be able to be bonded. Therefore, by preparing two substrates having a surface free energy of at least a moderate magnitude (specifically, using the contact angle with water as an index, the contact angle is 70° or less) and directly bonding them, it is possible to reduce bonding defects, which are partial failures to bond within the wafer surface (bonding interface). Therefore, a high-quality bonded substrate can be provided.
[0012] At this time, in the step of preparing the two substrates, By sputtering a material different from the base material onto the surface of the base material, it is possible to prepare a substrate in which the surface free energy of the surface to be directly bonded is adjusted.
[0013] In this way, even if the contact angle with water on the surface of a base material prepared for direct bonding exceeds 70°, a sputtered layer can be formed by the above-mentioned sputtering and the surface free energy of the sputtered layer can be adjusted to prepare a substrate having a surface with a contact angle with water of 70° or less.
[0014] The present invention also provides a method for manufacturing a semiconductor device, comprising the steps of: The present invention provides a method for manufacturing a semiconductor device, comprising the steps of: manufacturing the semiconductor device by using a bonded substrate manufactured by the method for manufacturing a bonded substrate according to the present invention;
[0015] The semiconductor device manufactured in this manner has a high-quality bonded substrate, and therefore peeling or the like does not occur at the bonded interface, resulting in a high-quality and highly reliable semiconductor device. Effect of the Invention
[0016] As described above, the method for manufacturing a bonded substrate of the present invention makes it possible to reduce bonding defects during substrate bonding. Furthermore, the method for manufacturing a semiconductor device of the present invention makes it possible to provide a semiconductor device with high quality and reliability. [Brief description of the drawings]
[0017] [Figure 1] 1 is a flow diagram showing an example of a method for manufacturing a bonded substrate and a method for manufacturing a semiconductor device according to the present invention. [Diagram 2] FIG. 1 is an explanatory diagram showing an example of two substrates used in the method for producing a bonded substrate of the present invention, and a bonded substrate obtained by directly bonding the two substrates. [Diagram 3] FIG. 1 is an explanatory diagram showing examples of contact angles (approximately 120° and 70° or less). [Figure 4] FIG. 4 is an explanatory view showing another example of two substrates used in the method for producing a bonded substrate of the present invention. [Diagram 5] 1 is a graph showing the contact angle on the surface of each substrate. [Figure 6] FIG. 1 is an observation view of voids in Comparative Example 1. BEST MODE FOR CARRYING OUT THEINVENTION
[0018] As mentioned above, there was a problem that bonding failure was observed in direct bonding of substrates such as semiconductor substrates. As a result of intensive research into the above problem, the present inventors realized that it is important to consider not only the surface roughness (Ra) of the substrates to be bonded, but also the surface free energy. As described in Atsushi Toyoda, "Technology of Adhesive Memos and Sticky Notes", Journal of the Japan Society for Precision Engineering, 89, (3), 233 (2023), it was found that this is similar to the phenomenon observed in the adhesion of Post-it notes. In addition, surface free energy is related to the contact angle (Shinichiro Imabayashi, "Effect of Surface Roughness on Wettability of Solid Surfaces", Review of Polarography, 115, 54, (2) (2008)), and the surface free energy can be evaluated by using the contact angle as an evaluation index. Therefore, more specifically, if the surfaces have Ra of 1 nm or less and a contact angle with water of 70° or less, bonding failure can be greatly reduced, and a method for manufacturing a bonded substrate with higher quality and reliability can be provided, and the present invention was completed. Furthermore, as a result of extensive research into the above-mentioned problems, the present inventors have found that by using the above-mentioned bonded substrate, a high-quality and highly reliable semiconductor device can be provided, and have completed the present invention.
[0019] Hereinafter, an embodiment of the present invention will be described with reference to the drawings, but the present invention is not limited thereto. First, FIG. 2 shows two substrates used in the method for producing a bonded substrate of the present invention, and a bonded substrate obtained by directly bonding the two substrates. 2, the two substrates prepared are a support substrate 1 and a bond substrate 2. Moreover, one surface 11 of the support substrate 1 and one surface 21 of the bond substrate 2 are directly bonded to produce a bonded substrate 3. The bonded portion between the surface 11 and the surface 21 is a bonded interface 31. The types of the support substrate 1 and the bond substrate 2 are not particularly limited, and may be, for example, a semiconductor substrate. More specifically, they may be a silicon substrate, or a compound semiconductor substrate such as a SiC substrate or a GaN substrate. They may also be a single crystal substrate or a polycrystalline substrate. The size and shape of the substrate are not particularly limited, and may be, for example, a circular substrate with a diameter of 200 mm. Alternatively, the substrate may be 300 mm or even 450 mm in diameter. Note that the larger the size, the more likely it is that poor bonding will occur, and the present invention is therefore more effective in reducing poor bonding.
[0020] The surface 11 of the support substrate 1 and the surface 21 of the bond substrate 2, which are to be actually directly bonded to each other, both have an average surface roughness Ra (hereinafter, simply referred to as Ra) of 1 nm or less. The value of Ra is more preferably 0.9 nm or less, and furthermore, 0.8 nm or less. The smaller the value of Ra, the more preferable it is, and the lower limit can be 0 nm.
[0021] The method for measuring the average surface roughness Ra is not particularly limited and can be determined each time, but Ra can be measured using a commercially available measuring device. For example, it can be a measurement value calculated from point cloud data with a viewing angle of 100 μm measured by a confocal laser microscope (such as OPTELICS manufactured by Lasertec). Alternatively, the measurement value may be taken using, for example, a Keyence VK-X100 series laser microscope at a measurement length of 4 mm. If necessary, measurements can be taken at multiple locations (for example, five locations) and the average value can be calculated.
[0022] In addition to the above Ra condition, both surfaces 11, 21 have an appropriate level of surface free energy (hereinafter, simply referred to as SFE). Here, the SFE is expressed using the contact angle between the surfaces 11, 21 and water as an index of the SFE. A specific condition for the contact angle is 70° or less. The contact angle value can more preferably be 66° or less, furthermore 62° or less, 59° or less, or 53° or less. The smaller the contact angle value, the more preferable, and the closer to 0° the better. This is because a good bonding interface 31 can be obtained more reliably.
[0023] For an explanation of the contact angle, refer to Fig. 3. A water droplet 102 is attached onto a substrate 101 to be measured. The angle formed between the liquid surface of the water droplet 102 and the surface of the substrate 101 to be measured is contact angle 103. In the upper diagram of Fig. 3, the contact angle 103 is about 120°, but in the case of the supporting substrate 1 and the bond substrate 2 of the present invention, the contact angle is 70° or less as described above. An example of a contact angle of 70° or less is shown in the lower diagram of Fig. 3. The larger the SFE, the greater the wettability, the smaller the contact angle, and the more suitable it is for bonding.
[0024] The method for measuring the contact angle is not particularly limited and can be determined each time, but the contact angle can be measured using a commercially available measuring device (for example, contact angle meter PCA-11 manufactured by Kyowa Interface Science Co., Ltd.). For example, a 2.0 μl droplet of pure water is dropped onto a surface at one location from the syringe 104 shown in the upper diagram of Figure 3, and the contact angle can be obtained from image analysis. If necessary, measurements can be taken not only at one location but at multiple locations (e.g., five locations) to obtain an average value.
[0025] With respect to both the surface 11 of the support substrate 1 and the surface 21 of the bond substrate 2, if Ra is greater than 1 nm or the contact angle is greater than 70°, the support substrate 1 and the bond substrate 2 cannot be directly bonded, or even if they can be directly bonded, partial unbonded portions (voids) are likely to occur at the bonded interface 31 of the bonded substrate 3. On the other hand, if both Ra and the contact angle satisfy the above conditions, direct bonding is possible, and an extremely good bonded interface 31 with very few or no voids can be obtained. Furthermore, the smaller the Ra or the contact angle, the more reliably the good bonded interface 31 can be obtained.
[0026] As described above, the support substrate 1 and the bond substrate 2 can be made of a single material such as a silicon substrate, a SiC substrate, or a GaN substrate, but can also be configured to have a layer of a different material on the surface of such a substrate.
[0027] FIG. 4 shows another example of two substrates (support substrate 1 and bond substrate 2). In the example of FIG. 4, the surface of substrate 4 has sputtered layer 5 obtained by sputtering a material different from substrate 4. The entire configuration combining substrate 4 and sputtered layer 5 corresponds to support substrate 1 and bond substrate 2. In this case, surface 51 of sputtered layer 5 corresponds to surface 11 of support substrate 1 and surface 21 of bond substrate 21. That is, surface 51 of sputtered layer 5 satisfies the above-mentioned numerical conditions for Ra and contact angle. For example, the base material 4 may be a SiC substrate or a GaN substrate, and the sputtered layer 5 may be a Si layer, but is not limited to these materials. An advantage of such a configuration is that, even if the surface of the base material 4 once prepared does not satisfy the above conditions of Ra and contact angle, the surface can be modified by forming the sputtered layer 5 to form a good surface 51 that satisfies the above conditions. The sputtered layer 5 is not limited to one layer, and may be multiple layers. In this case, the Ra and contact angle of the outermost layer must be within the ranges specified by the present invention. The method of forming the layer is not limited to the sputtering method, and various known methods may be used.
[0028] Hereinafter, a method for manufacturing a bonded substrate and a method for manufacturing a semiconductor device according to the present invention using supporting substrate 1 and bond substrate 2 in FIG. 2 (or FIG. 4) will be described. The flow of the bonded substrate manufacturing method and semiconductor device manufacturing method of the present invention is shown in Figure 1. Overall, the process consists of preparing two substrates (step 1), directly bonding the two substrates (manufacturing the bonded substrate) (step 2), and manufacturing the semiconductor device using the bonded substrate (step 3).
[0029] Each step will be described below. (Step 1: Prepare two boards) First, two substrates to be directly bonded are prepared. When preparing these substrates, the Ra and SFE of the surfaces to be directly bonded are used as the criteria. More specifically, as described above, a substrate is prepared having a surface with Ra of 1 nm or less and a contact angle with water (an index of SFE) of 70° or less. That is, a support substrate 1 having a surface 11 and a bond substrate 2 having a surface 21 in FIG. 2 that satisfy both the above conditions of Ra and contact angle are prepared. The support substrate 1 and the bond substrate 2 may be prepared from a single material, or may be prepared from a base material 4 and a sputtered layer 5 made of a different material as shown in FIG. For example, a single crystal or polycrystalline material may be prepared, polished using various polishing devices such as a double-sided polishing device or a single-sided polishing device as necessary, or the sputtered layer 5 may be formed by sputtering using a target, thereby adjusting the surface condition to satisfy the above conditions of Ra and contact angle.
[0030] (Step 2: Direct bonding of two substrates) The surface 11 of the support substrate 1 and the surface 21 of the bond substrate 2 (the bond substrate 2 is shown upside down in Figures 1 and 2) are bonded together in an opposing relationship to directly bond these surfaces to produce the bonded substrate 3. Since both of the surfaces 11, 21 to be directly bonded satisfy the above-mentioned conditions of Ra and contact angle, the occurrence of bonding failure can be reduced, and a good bonded substrate 3 with very few voids (or no voids) at the bonding interface 31 can be obtained.
[0031] At this time, the bonding strength may be improved by subjecting the bonded substrate 3 to a heat treatment as necessary. If it is necessary to thin the bond substrate portion after bonding, this may be done using an existing known technique such as an ion implantation peeling method.
[0032] (Step 3: Manufacturing a semiconductor device using a bonded substrate) Next, the semiconductor device 6 is manufactured using the bonded substrate 3 manufactured as described above. The bond substrate portion of the bonded substrate 3 may be appropriately subjected to various treatments such as heat treatment, oxide film formation, etching, and photoresist treatment to obtain a desired device. By using the bonded substrate 3, it is possible to eliminate or reduce the number of epitaxial growth steps for fabricating the device layer, and to obtain the semiconductor device 6 at low cost. In addition, since the bonded substrate 3 manufactured by the manufacturing method of the present invention has a good and high-quality bonded interface 31, the semiconductor device 6 manufactured can also be of high quality and high reliability. In other words, reliability can be maintained without worrying about peeling or the like. EXAMPLES
[0033] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. (Examples 1-3, Comparative Example 1) A 4H-SiC single crystal substrate with a diameter of 200 mm, a thickness of 355 μm, n-type, resistivity of 10 Ω·cm, and an off-angle of 4° to the (0001) plane was prepared as a bond substrate. The surface of this substrate was polished using silica as an abrasive, resulting in a flattened surface with an average surface roughness Ra of 0.8 nm. Ra was a measured value calculated from point cloud data with a viewing angle of 100 μm measured using OPTELICS manufactured by Lasertec.
[0034] Next, the following was prepared as a supporting substrate. First, a 4H-SiC single crystal substrate was prepared, which was the same as the bond substrate. A poly-SiC substrate of the same size as the bond substrate was also prepared. The surfaces of each were polished in the same manner as above, and the Ra was flattened to 0.8 nm. In addition, a 4H-SiC single crystal substrate similar to the bond substrate was prepared, and the surface was polished in the same manner as above to flatten it to Ra of 0.8 nm, after which silicon was sputtered onto it. The surface of the sputtered layer had Ra of 0.8 nm. In addition, a poly-SiC substrate of the same size as the bond substrate was prepared, and the surface was polished in the same manner as above to flatten it to Ra of 0.8 nm, after which silicon was sputtered on it. The surface of the sputtered layer had Ra of 0.8 nm.
[0035] The contact angle of each surface of (1) 4H-SiC single crystal substrate (for bond substrate, for support substrate), (2) poly-SiC substrate (for support substrate), (3) silicon-sputtered 4H-SiC single crystal substrate (for support substrate), and (4) silicon-sputtered poly-SiC substrate (for support substrate) was measured using a contact angle meter PCA-11 manufactured by Kyowa Interface Science Co., Ltd. (2 μl of water was used). Measurements were taken at five points and the average value was calculated. The results of the contact angle measurements are shown in Figure 5. As shown in Figure 5, (2) only the poly-SiC substrate had a large contact angle of 83°, indicating that the surface free energy was small. On the other hand, the contact angle of (1) the 4H-SiC single crystal substrate was 53°, and the contact angles of (3) the silicon-sputtered 4H-SiC single crystal substrate and (4) the silicon-sputtered poly-SiC substrate were 62°, which were small, indicating that the surface free energies were relatively large.
[0036] Next, direct bonding of these substrates was attempted in the following combinations. (Example 1) (1)+(1): 4H-SiC single crystal substrates Ra: both 0.8nm Contact angle: both 53° (Example 2) (1)+(3): 4H-SiC single crystal substrate and silicon-sputtered 4H-SiC single crystal substrate Ra: both 0.8nm Contact angle: (1) 53°, (3) 62° (Example 3) (1)+(4): 4H-SiC single crystal substrate and silicon sputtered poly-SiC substrate Ra: both 0.8nm Contact angle: (1) 53°, (4) 62° (Comparative Example 1) (1)+(2): 4H-SiC single crystal substrate and poly-SiC substrate Ra: both 0.8nm Contact angle: (1) 53°, (2) 83°
[0037] Here, assuming that condition A is [Ra is 1 nm or less] and condition B is [contact angle is 70° or less], bonding was possible in Example 1-3 which satisfied both conditions A and B. Furthermore, when confirmed with an ultrasonic microscope, no locations where bonding was not possible were confirmed within the wafer surface (bonding interface of the bonding substrate). On the other hand, in Comparative Example 1, which satisfied condition A but did not satisfy condition B, bonding was possible. However, it was confirmed by an ultrasonic microscope that there were some areas on the wafer surface where bonding was not possible. Figure 6 shows an observation image of a void, which is a bonding failure area.
[0038] In the following, (1) 4H-SiC single crystal substrates, (2) poly-SiC substrates, (3) silicon-sputtered 4H-SiC single crystal substrates, and (4) silicon-sputtered poly-SiC substrates with various Ra and contact angles were prepared and combined to attempt direct bonding. (Examples 4-6, Comparative Example 2) Direct bonding was attempted under the following conditions. (Example 4) (1)+(1): 4H-SiC single crystal substrates Ra: Both 0.9 nm Contact angle: both 56° (Example 5) (1)+(3): 4H-SiC single crystal substrate and silicon-sputtered 4H-SiC single crystal substrate Ra: Both 0.9 nm Contact angle: (1) 56°, (3) 66° (Example 6) (1) + (4): 4H-SiC single crystal substrate and silicon sputtered poly-SiC substrate Ra: Both 0.9 nm Contact angle: (1) 56°, (4) 66° (Comparative Example 2) (1)+(2): 4H-SiC single crystal substrate and poly-SiC substrate Ra: Both 0.9 nm Contact angle: (1) 56°, (2) 86°
[0039] Bonding was possible in Example 4-6, which satisfied both conditions A and B. Furthermore, when observed with an ultrasonic microscope, no voids were found within the wafer surface. On the other hand, in Comparative Example 2, which satisfied condition A but did not satisfy condition B, bonding was possible. However, it was confirmed by an ultrasonic microscope that there were voids in the wafer surface. The number of voids was greater than in Comparative Example 1, and they were also larger in size.
[0040] (Examples 7-9, Comparative Example 3) Direct bonding was attempted under the following conditions. (Example 7) (1)+(1): 4H-SiC single crystal substrates Ra: Both 1.0 nm Contact angle: both 59° (Example 8) (1)+(3): 4H-SiC single crystal substrate and silicon-sputtered 4H-SiC single crystal substrate Ra: Both 1.0 nm Contact angle: (1) 59°, (3) 70° (Example 9) (1) + (4): 4H-SiC single crystal substrate and silicon sputtered poly-SiC substrate Ra: Both 1.0 nm Contact angle: (1) 59°, (4) 70° (Comparative Example 3) (1)+(2): 4H-SiC single crystal substrate and poly-SiC substrate Ra: Both 1.0 nm Contact angle: (1) 59°, (2) 89°
[0041] Bonding was possible in Example 7-9, which satisfied both conditions A and B. Furthermore, when observed with an ultrasonic microscope, no voids were found within the wafer surface. On the other hand, in Comparative Example 3, which satisfied condition A but did not satisfy condition B, bonding was possible. However, it was confirmed by an ultrasonic microscope that there were voids in the wafer surface. The number of voids was greater than in Comparative Example 2, and the size of the voids was also larger.
[0042] (Comparative Examples 4-7) Direct bonding was attempted under the following conditions. (Comparative Example 4) (1)+(1): 4H-SiC single crystal substrates Ra: Both 1.2 nm Contact angle: both 62° (Comparative Example 5) (1)+(3): 4H-SiC single crystal substrate and silicon-sputtered 4H-SiC single crystal substrate Ra: (1) 1.2 nm, (3) 1.0 nm Contact angle: (1) 62°, (3) 70° (Comparative Example 6) (1)+(4): 4H-SiC single crystal substrate and silicon sputtered poly-SiC substrate Ra: (1) 1.2 nm, (4) 1.0 nm Contact angle: (1) 62°, (4) 70° (Comparative Example 7) (1) + (2): 4H-SiC single crystal substrate and poly-SiC substrate Ra: (1) 1.2 nm, (2) 1.0 nm Contact angle: (1) 62°, (2) 89°
[0043] In both Comparative Example 4-6, which satisfied condition B but did not satisfy condition A, and Comparative Example 7, which did not satisfy either condition A or B, bonding was not possible.
[0044] In addition, GaN single crystal substrates, poly-GaN substrates, silicon-sputtered GaN single crystal substrates, and silicon-sputtered poly-GaN substrates with various Ra and contact angles were prepared, and direct bonding was attempted by combining these. As a result, when both conditions A and B were satisfied, bonding was possible and no voids were observed within the wafer surface. On the other hand, when even one of conditions A and B was not satisfied, bonding was not possible, or even if bonding was possible, numerous voids were found within the wafer surface.
[0045] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]
[0046] 1... supporting substrate, 2... bond substrate, 3... joining substrate, 4... base material, 5...sputtered layer, 6...semiconductor device, 11...Directly bonded surface of the support substrate; 21...directly bonded surface of the bond substrate; 31...bonding interface of bonded substrate, 51...surface of sputtered layer, 101...Substrate to be measured, 102...Water drop, 103...Contact angle, 104...Syringe.
Claims
1. A method for manufacturing a bonded substrate by directly bonding surfaces of two substrates, comprising the steps of: The method includes a step of preparing the two substrates based on the average surface roughness Ra and the surface free energy of the surfaces to be directly bonded, and a step of directly bonding the two substrates prepared, In the step of preparing the two substrates, A method for manufacturing a bonded substrate, comprising: preparing substrates whose surfaces to be directly bonded have an average surface roughness Ra of 1 nm or less, and whose surfaces to be directly bonded have a contact angle with water of 70° or less, which is an index of the surface free energy.
2. In the step of preparing the two substrates, 2. The method for manufacturing a bonded substrate according to claim 1, further comprising the step of: preparing a substrate in which the surface free energy of the surface to be directly bonded is adjusted by sputtering a material different from the base material onto the surface of the base material.
3. A method for manufacturing a semiconductor device, comprising:
3. A method for manufacturing a semiconductor device, comprising the steps of: manufacturing the semiconductor device by using a bonded substrate manufactured by the method for manufacturing a bonded substrate according to claim 1 or 2.
Citation Information
Patent Citations
Method for manufacturing SOI substrate
JP2010034523A
Semiconductor substrate structure and power semiconductor device
JP2019210162A
Composite substrate, and manufacturing method thereof
JP2021018998A
Semiconductor substrate, manufacturing method thereof, and semiconductor device
JP2023501646A
How to reuse circuit boards
JP2013513963A