Method for joining dissimilar metallic body and hot forging metal mold
By applying a four-step heat treatment process involving solution treatment, solid-phase diffusion bonding, and simultaneous aging of precipitation hardening steel, the method addresses the inefficiencies of existing methods, enhancing the characteristics of dissimilar metal bodies and reducing costs and energy consumption.
Patent Information
- Application Number
- JP2023082247
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for joining dissimilar metal bodies, such as those involving precipitation hardening heat-resistant steel and hot work tool steel, fail to fully exhibit the characteristics of each metal material and require excessive energy and cost due to suboptimal heat treatment conditions and potential cooling cracks.
A method involving solution treatment of the precipitation hardening heat-resistant steel followed by solid-phase diffusion bonding and simultaneous aging treatment, then quenching and tempering of the hot work tool steel, reduces the number of heat treatments to four, allowing for appropriate exhibition of metal characteristics and minimizing cooling cracks.
This approach effectively reduces the cost and energy required for bonding and heat treatment while extending the life of hot forging dies by appropriately showcasing the characteristics of both metals, thereby reducing waste generation.
Smart Images

Figure 2024165765000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for joining dissimilar metal bodies by joining a first metal body made of hot work tool steel to a second metal body made of precipitation hardening heat-resistant steel, and to a hot forging die manufactured using this joining method. [Background technology]
[0002] In recent years, efforts to significantly reduce waste generation through waste prevention, reduction, recycling, and reuse have been gaining momentum. To achieve this, research and development into the reuse of metal materials is being conducted.
[0003] Conventionally, crankshafts for internal combustion engines are formed by hot forging. Hot forging is a processing method in which a structural material that has been heated to a high temperature to reduce its deformation resistance is repeatedly subjected to a high pressure load by a die, thereby transferring the shape of the die to the structural material. The die has a short lifespan because it repeatedly slides against the structural material under high temperature and high pressure. If the die has a short lifespan, not only will it be necessary to regenerate the die surface by machining, but the manufacturing costs of the die will also increase. In addition, various losses will occur, such as the need to stop the operation of the production line to replace the die and the need to adjust various conditions due to wear.
[0004] In order to suppress wear caused by sliding and to extend the life of a die, it is possible to manufacture the die from composite metals. Patent Document 1 discloses a composite die for hot forging, which includes a first buildup layer made of an alloy that emphasizes high-temperature wear resistance and a second buildup layer made of an alloy that emphasizes high-temperature strength. This die includes a flash fluidity promotion region that promotes the flow of flash (burrs) from the rough material that will become the forged product, and a flash fluidity suppression region that suppresses the flow of flash from the rough material. The first buildup layer that emphasizes high-temperature wear resistance is built up in the flash fluidity promotion region, and the second buildup layer that emphasizes high-temperature strength is built up in the flash fluidity suppression region.
[0005] Patent Document 2 discloses a heat treatment method for joining a first metal material (Inconel 718) made of a precipitation hardened heat-resistant alloy and a second metal material (3Cr-Mo-V steel) made of a non-precipitation hardened alloy. In this heat treatment method, the hardness of the first metal material is restored in a region where the hardness is decreased due to the thermal effect of joining, and in a region where the hardness is increased due to the thermal effect. Specifically, a primary heat treatment is first performed in a range where the solid solution heat treatment conditions of the first metal material and the quenching treatment conditions of the second metal material overlap (900 to 1200°C / 0.1h or more). As a result, the hardness of the region of the first metal material where the hardness is decreased due to joining is restored to the high hardness side. Then, a secondary heat treatment is performed in a range where the aging treatment conditions of the first metal material and the tempering treatment conditions of the second metal material overlap (470 to 850°C / 0.1h or more). As a result, the hardness of the region of the second metal material, which has been increased by joining, is restored to the low hardness side. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 11-347678 [Patent Document 2] Japanese Patent Application Publication No. 10-298663 Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the technology of Patent Document 1, the first overlay layer and the second overlay layer joined by overlay welding are not subjected to heat treatment after joining, so the properties of these metal materials are not fully exhibited. In addition, the technology of Patent Document 2 cannot be applied when the solid solution (solution) heat treatment conditions of the first metal material and the quenching treatment conditions of the second metal material do not overlap, or when the aging treatment conditions of the first metal material and the tempering treatment conditions of the second metal material do not overlap. Even when the heat treatment conditions overlap, the two metal materials are simultaneously heat treated, so that the heat treatment cannot be performed under optimal conditions for both metals. Thus, in the technology related to the dissimilar metal body including dissimilar metal materials, there is room for improvement in terms of appropriately exhibiting the properties of each metal material.
[0008] Furthermore, the technology of Patent Document 2 targets a heat treatment method for dissimilar metal bodies joined by any one of arc welding, friction welding, and liquid phase diffusion bonding. However, when a dissimilar metal body is formed by joining two metal bodies by solid phase diffusion bonding, if the dissimilar metal bodies are rapidly cooled in the first heat treatment after joining, there is a risk of cooling cracks occurring due to thermal stress during cooling, transformation stress, differences in thermal expansion coefficients between the dissimilar metals, heat transfer at the joining interface, and the like.
[0009] Here, it is considered to subject the first metal material made of a precipitation hardened heat-resistant alloy to solution treatment and aging treatment, and then join the first metal material and the second metal material to each other by solid-phase diffusion bonding. However, in this case, after the three heat treatments for the solution treatment, aging treatment, and solid-phase diffusion bonding, two more heat treatments are required to quench and temper the second metal material made of a non-precipitation hardened alloy. Therefore, the cost and energy required for the joining and heat treatment are large.
[0010] In view of the above background, the present invention aims to make it possible to appropriately utilize the characteristics of the metallic materials contained in the dissimilar metallic bodies, while reducing the costs and energy required for joining and heat treatment, thereby extending the life of hot forging dies and contributing to a significant reduction in the generation of waste. [Means for solving the problem]
[0011] In order to solve the above-mentioned problems, one aspect of the present invention is a method for joining dissimilar metal bodies (2, 3) by joining a first metal body (16) made of hot work tool steel to a second metal body (17) made of precipitation hardening heat resistant steel, the method comprising the steps of: heating the second metal body to a first predetermined temperature (T1) higher than the solution temperature (e.g., 965°C) of the precipitation hardening heat resistant steel to solutionize the second metal body, quenching the second metal body, and precipitation hardening the second metal body; and after the solution treatment, heating the second metal body and the first metal body to a second predetermined temperature (T2) lower than the solution temperature of the precipitation hardening heat resistant steel and higher than the aging temperature of the precipitation hardening heat resistant steel while keeping the second metal body and the first metal body in close contact with each other under a predetermined pressure. a joining and aging process in which the second metal body and the first metal body are solid-phase diffusion bonded together and the second metal body is aged by heating the dissimilar metal body obtained by joining the second metal body to the first metal body after the joining and aging process to a third predetermined temperature (T3) that is lower than the solution temperature of the precipitation hardening heat resistant steel and higher than the quenching temperature of the hot work tool steel, and then cooling the dissimilar metal body to quench the first metal body; and a tempering process in which the dissimilar metal body is heated to a tempering temperature of the hot work tool steel that is lower than the quenching temperature after the quenching process.
[0012] According to this embodiment, since the solution treatment process of the second metal body is performed before the solid-phase diffusion bonding, the second metal body can be reliably precipitation hardened without being restricted by temperature or cooling rate. Also, since the solid-phase diffusion bonding and the aging treatment are performed simultaneously, only four heat treatments are required. Therefore, the cost and energy required for the bonding and heat treatment are reduced. In the quenching and tempering processes of the first metal body, the first metal body can be quenched and tempered without re-solutioning the second metal body and without causing cooling cracks.
[0013] In the above aspect, it is preferable that the third predetermined temperature when quenching the first metal body in the quenching process is in a temperature range of 950°C or higher and lower than 1100°C, and the precipitation hardening heat-resistant steel is a precipitation hardening Ni-base alloy that does not go into solution at temperatures lower than 950°C but goes into solution at temperatures lower than 1100°C.
[0014] According to this embodiment, the first metal body can be quenched without coarsening the grains, and the characteristics of the hot work tool steel and precipitation hardening heat resistant steel of the dissimilar metal body including the precipitation hardening Ni-based alloy can be adequately exhibited.
[0015] In the above aspect, the first predetermined temperature in the solution treatment step may be higher than a grain coarsening temperature of the hot work tool steel.
[0016] According to this embodiment, the second metal body can be reliably precipitation hardened in the solution treatment step, or a precipitation hardening heat-resistant steel having high heat resistance and wear resistance and having a high solution treatment temperature and requiring rapid cooling such as water cooling for solution treatment can be used, thereby improving the durability of the dissimilar metal body.
[0017] In the above aspect, in the quenching process, the time for which the third predetermined temperature is maintained is the estimated shortest time estimated to be required to bring the entire first metal body to the third predetermined temperature, depending on the size of the first metal body, and the dissimilar metal body is cooled immediately after the estimated shortest time has elapsed.
[0018] According to this embodiment, the first metal body can be quenched without overaging the second metal body made of precipitation hardening heat resistant steel.
[0019] In the above aspect, the second metal body may be cooled by water cooling in the solution forming step.
[0020] According to this embodiment, the solute atoms of the precipitation hardening heat resistant steel can be reliably precipitated to harden the second metal body. Note that the first metal body is quenched by cooling, but is annealed by heating to and maintaining the aging temperature in the aging step.
[0021] In the above aspect, the dissimilar metal bodies may be cooled by air cooling or oil cooling in the quenching step.
[0022] When the first metal body made of hot work tool steel is cooled by water, there is a risk that cracks will occur in the first metal body due to thermal stress. According to this embodiment, the first metal body can be quenched without causing cracks.
[0023] In the above aspect, the quenching step may be carried out successively to the bonding and aging step.
[0024] According to this embodiment, the number of heat treatments can be reduced from four to three.
[0025] In the above aspect, it is preferable that the hardness of each of the first metal body and the second metal body after the tempering step is HRC38 or more and 47 or less.
[0026] According to this embodiment, the first metal body and the second metal body can be made to have a hardness suitable for a hot forging die.
[0027] In the above aspect, the hot work tool steel may be SKD61, and the precipitation hardening heat resistant steel may be NCF750.
[0028] According to this embodiment, it is possible to manufacture a dissimilar metal body using SKD61 and NCF750, in which the properties of these metals are appropriately exhibited.
[0029] In order to solve the above problems, one aspect of the present invention is a hot forging die (1) having a lower die (2) and an upper die (3) formed from the dissimilar metal bodies in which the second metal body is joined to the first metal body by the above-mentioned joining method, wherein the lower die and the upper die have cavities (8, 9) recessed in their respective cut surfaces (6, 7) and inclined surfaces (12, 13) formed on the outside of the cavities to suppress burrs (5) that occur between the cut surfaces, and each of the die bodies of the lower die and the upper die is formed from the first metal body, and each of the inclined surfaces of the lower die and the upper die is formed from the second metal body.
[0030] According to this embodiment, the second metal body having high heat resistance and wear resistance is provided on the inclined surface that functions as a burr suppression portion, thereby extending the life of the hot forging die. In addition, although precipitation hardening type heat resistant steel is very expensive compared to hot work tool steel, the second metal body made of precipitation hardening type heat resistant steel is provided locally on the upper and lower dies, so that the increase in material cost of the hot forging die is suppressed. Effect of the Invention
[0031] According to the above aspect, the characteristics of the metal materials contained in the dissimilar metal bodies can be appropriately exhibited, and the costs and energy required for joining and heat treatment can be reduced. [Brief description of the drawings]
[0032] [Figure 1] Cross-sectional view of a hot forging die according to an embodiment [Diagram 2] (A) Hot work tool steel, (B) Precipitation hardening heat resistant steel, and (C) Time chart showing typical thermal processes for solid-state diffusion bonding. [Diagram 3] 1 is a time chart showing the steps of joining and heat treating dissimilar metal bodies according to an embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] FIG. 1 is a cross-sectional view of a hot forging die 1 according to an embodiment. As shown in FIG. 1, the hot forging die 1 includes a lower die 2 and an upper die 3 constituting a forging die which is a composite die. The hot forging die 1 is a rough forming die for roughly processing a rough formed product 4 obtained by crushing a carbon steel-based material heated to a high temperature. The hot forging die 1 is used to form a rough forged product of an irregular part having a complex shape, not a shaft part having a simple shape such as a propeller shaft. In this embodiment, the hot forging die 1 is used to form a rough forged product of a crankshaft of an internal combustion engine. The rough forged product formed by the hot forging die 1 is formed into a final product through a second rough processing forming process if necessary, and then a finishing process, a trimming process, etc.
[0034] The lower die 2 has an upwardly facing parting surface 6 that extends horizontally, and the upper die 3 has a corresponding downwardly facing parting surface 7. Cavities 8, 9 corresponding to the contour of the rough forged product of a crankshaft are recessed into the parting surface 6 of the lower die 2 and the parting surface 7 of the upper die 3, respectively. The parts of the parting surfaces 6, 7 near the cavities 8, 9 are flash lands 10, 11 against which the flash 5 subjected to high pressure slides when part of the rough forged product 4 flows out laterally from between the cavities 8, 9 to become flash. The flash lands 10, 11 of the lower die 2 and the upper die 3 extend horizontally and parallel to each other.
[0035] On the outer sides of both flash lands 10, 11, inclined surfaces 12, 13 are provided which are parallel to each other and inclined with respect to the flash lands 10, 11. The inclined surfaces 12, 13 are inclined downward toward the outside. During forging, these inclined surfaces 12, 13 suppress the spread of burrs 5 which slide between the flash lands 10, 11 while being held at high pressure by the flash lands 10, 11. This promotes the filling of the rough formed product 4 into the cavities 8, 9. In other words, the inclined surfaces 12, 13 are burr suppressing portions which suppress the burrs 5 which are generated between the flash lands 10, 11 of the parting surfaces 6, 7.
[0036] The lower die 2 and the upper die 3 are dissimilar metal bodies formed of dissimilar metals. Specifically, the lower die 2 and the upper die 3 each include a first metal body 16 made of hot work tool steel that constitutes the majority of the die, and a second metal body 17 made of hardened heat-resistant steel to which the first metal body 16 is joined. The first metal body 16 forms the die body of the lower die 2 and the upper die 3.
[0037] The second metal body 17 is formed in a plate shape to form the outer portions of the flash lands 10, 11 and the inclined surfaces 12, 13 of the parting surfaces 6, 7 of the lower die 2 and the upper die 3, and is joined to the first metal body 16 by solid-state diffusion bonding. Since the second metal body 17 is not provided on the inner portions of the flash lands 10, 11, it is not necessary to form the second metal body 17 into a complex shape that follows the contour of the rough molded product 4 of the crankshaft.
[0038] The second metal body 17 is made of hot work tool steel and has higher heat resistance and wear resistance than the first metal body 16. The second metal body 17 is provided on the inclined surfaces 12, 13 which function as burr suppression sections in this manner, thereby extending the life of the hot forging die 1. In addition, although precipitation hardening heat resistant steel is very expensive compared to hot work tool steel, the second metal body 17 made of precipitation hardening heat resistant steel is provided locally on the lower die 2 and the upper die 3, so that an increase in the material cost of the hot forging die 1 is suppressed.
[0039] The first metal body 16 is preferably made of a metal material (first metal material) having high heat resistance and wear resistance and excellent toughness among hot work tool steels, and in this embodiment, is made of SKD61. SKD61 is an alloy steel for hot work dies, specified in JIS G 4404:2015 Alloy Tool Steel. JIS specifies the heat treatment temperature, cooling method, hardness, etc. of SKD61. Quenching of SKD61 is specified as 1020°C and air cooling, and tempering of SKD61 is specified as 550°C and air cooling. However, the quenching temperature and tempering temperature of SKD61 are not limited to these, and may be set to an appropriate temperature so as to exhibit appropriate characteristics such as hardness and toughness according to the application of the first metal body 16.
[0040] Figure 2 is a time chart showing typical heat treatment steps for (A) hot work tool steel and (B) precipitation hardening heat resistant steel. As shown in Figure 2(A), for example, SKD61 hot work tool steel is quenched by heating to 1020°C and then cooling by air cooling (quenching step), and then tempered by heating to 650°C (tempering step).
[0041] In JIS G 4404, the quenched and tempered hardness of SKD61 is specified as HV (Vickers hardness) 513. HV513 can be converted to HRC (Rockwell C scale hardness) 50. In addition, the annealing temperature of SKD61 is specified as 820 to 870°C, and the annealed hardness is specified as HBW (HBW is Brinell hardness (10 mm ball load 29.4 kN)) 229 or less.
[0042] The grain-coarsening temperature at which the structure of SKD61 becomes coarse is 1100°C. If SKD61 is heated to 1100°C or higher during quenching, the structure of SKD61 becomes coarse, and the toughness after quenching and tempering decreases. In other words, the first metal body 16 made of SKD61 becomes brittle and is not suitable for a forging die body that generates high pressure. Therefore, SKD61 needs to be quenched at a temperature lower than 1100°C.
[0043] On the other hand, the inventors have confirmed through experiments that SKD61 can obtain a predetermined hardness after quenching and tempering by heating it to a predetermined quenching temperature or higher, even if it is not heated to 1020°C as specified by JIS. Here, the predetermined hardness may be HRC38 or higher, which is a hardness sufficient for rough forging of irregular-shaped parts, and is preferably HRC41 or higher. Specifically, the inventors have confirmed through experiments that by heating SKD61 to 950°C or higher, the hardness of SKD61 after quenching and tempering becomes HRC38 or higher, more specifically, HRC41 or higher.
[0044] That is, during quenching, it is preferable to heat SKD61 to a temperature equal to or higher than the quenching temperature of 950° C. and lower than the grain coarsening temperature of 1100° C. In the case of this embodiment, since NCF750 is solutionized at 965° C. as described later, it is preferable to heat SKD61 to a temperature equal to or higher than 950° C. and lower than 965° C. during quenching.
[0045] The second metal body 17 is preferably made of a metal material (second metal material) having higher heat resistance and wear resistance and excellent toughness than the metal material of the first metal body 16, and in this embodiment, is made of NCF750. NCF750 is a superalloy steel specified in JIS G 4901 Corrosion-resistant and heat-resistant superalloy bar, 4902 Corrosion-resistant and heat-resistant superalloy plate: 2019.
[0046] Also, in Appendix A (reference) of JIS G 4902, examples of heat treatment conditions for NCF750 are described. As the solution heat treatment of NCF750, (S1) 1135-1165°C quenching and (S2) 965-995°C quenching are described. As the aging treatment of NCF750, (H1) S1 solution heat treatment, hold at 800-830°C for 24 hours, air cool to room temperature, hold at 690-720°C for 20 hours, and then quench. Furthermore, as the aging treatment, (H2) S2 solution heat treatment, hold at 720°C-740°C for 8 hours, furnace cool to 610-630°C, further age at that temperature and then air cool, with a total aging time of 18 hours is described. However, the solution treatment temperature and aging treatment of NCF750 are not limited to these, and may be set to an appropriate temperature so as to exhibit appropriate characteristics such as hardness and toughness according to the application of the second metal body 17.
[0047] Metal materials conforming to the NCF750 standard include DSALOY (registered trademark) X-750 manufactured by Daido Steel Co., Ltd. and Inconel (registered trademark) X750 manufactured by Special Metal Corporation. These are precipitation hardened Ni-based alloys. Instead of being made of NCF750, the second metal body 17 may be made of DSA760 manufactured by Daido Steel Co., Ltd., which is a Ni-based alloy similar to NCF750 and has excellent high-temperature wear resistance and corrosion resistance.
[0048] As shown in Fig. 2(B), NCF750, which is a precipitation hardening type heat resistant steel, is heat treated in accordance with the above (H1). For example, NCF750 is solution treated by heating to 1150°C and then quenching with water cooling (W / C) (solution treatment step), and then aging treated by heating to 850°C and holding for 16 hours (aging step).
[0049] In JIS G 4902, the hardness of NCF750 is specified for each heat treatment (applicable thickness is more than 0.6 mm and less than 6 mm). In the case of only solution heat treatment (S1) or (S2), the hardness of NCF750 is specified as HBW321 or less, HRC35 or less, and HV335 or less. In the case of aging treatment (H1) after solution heat treatment, the hardness of NCF750 is specified as HBW262 or more, HRC26 or more, and HV270 or more. In the case of aging treatment (H2) after solution heat treatment, the hardness of NCF750 is specified as HBW302-363, HRC32-40, and HV313-382.
[0050] In this embodiment, NCF750 is used for the rough forging die for irregular shaped parts as described above, and therefore the hardness of NCF750 is preferably HRC38 or more, and more preferably HRC41 or more.
[0051] In this embodiment, the second metal body 17 made of NCF750 and the first metal body 16 made of SKD61 are bonded by solid-phase diffusion bonding. Solid-phase diffusion bonding is a bonding method performed at a temperature below the melting point of the base materials, in which the base materials are brought into close contact with each other, and pressure is applied under a temperature condition below the melting point of the base materials so as to minimize plastic deformation, and the bonding is performed by utilizing atomic diffusion that occurs between the bonding surfaces. In solid-phase diffusion bonding, the base materials that are in close contact with each other are heated and pressurized in a controlled atmosphere so that the bonding surfaces are not oxidized, and are bonded by utilizing atomic diffusion.
[0052] As shown in Fig. 2(C), in solid-phase diffusion bonding, the second metal body 17 and the first metal body 16 are pressurized and brought into close contact with each other, heated to a temperature below the melting points of SKD61 and NCF750 (e.g., 1050°C), and the pressurized state and temperature are maintained for a predetermined time determined according to the temperature (e.g., 4 hours in the case of 1050°C). As a result, atoms diffuse between the bonding surfaces, and the second metal body 17 and the first metal body 16 are bonded to each other (bonding process). In solid-phase diffusion bonding, the higher the temperature, the shorter the holding time is, and the lower the temperature, the longer the holding time is required, as shown by the imaginary line in the figure.
[0053] Next, a manufacturing method of the hot forging die 1 configured as above will be described. The lower die 2 and the upper die 3 are both made of dissimilar metal bodies and are manufactured by the same method. In the following description, they will be referred to as dissimilar metal bodies.
[0054] 3 is a time chart showing the process of joining and heat treatment of dissimilar metal bodies according to the embodiment. As shown in the figure, first, a solid solution treatment is performed only on the second metal body 17. Specifically, the second metal body 17 is placed in a furnace and heated to 1150°C to solutionize the second metal body 17, and then the dissimilar metal bodies are quenched by water cooling to precipitation harden the second metal body 17 (solid solution process). This 1150°C is a first predetermined temperature T1 that is higher than the solution temperature of NCF750. As described above, the minimum temperature for the solid solution heat treatment of NCF750 specified in JIS is 965°C (S2), and 1150°C is higher than this and higher than 1035°C (S2).
[0055] The first predetermined temperature T1 is preferably a temperature higher than 1100°C, which is the grain coarsening temperature of SKD61. This ensures that the second metal body 17 is precipitation hardened in the solution treatment process. Alternatively, other precipitation hardening heat-resistant steels having higher heat resistance and wear resistance and having a higher solution treatment temperature than NCF750 and requiring rapid cooling such as water cooling for solution treatment can be used. This improves the durability of the dissimilar metal bodies.
[0056] In the solution forming step, the second metal body 17 is cooled by water cooling, whereby the solute atoms of NCF750 are reliably precipitated and the second metal body 17 is hardened.
[0057] Next, the second metal body 17 and the first metal body 16 forming the mold body are placed in a furnace for solid-phase diffusion bonding, heated to 900°C while in close contact with each other under a predetermined pressure, and held at 900°C for 16 hours. 900°C is the second predetermined temperature T2 that is lower than the solution temperature of NCF750 and higher than the aging temperature of NCF750. As described above, the minimum solution heat treatment temperature of NCF750 described in JIS is 965°C (S2), and the minimum aging temperature is 720°C (H2). In other words, the second predetermined temperature T2 is set to 900°C, which is lower than 965°C and higher than 720°C. 16 hours is the time set as necessary to age the second metal body 17 at 900°C and to perform solid-phase diffusion bonding between the second metal body 17 and the first metal body 16 at 900°C. As a result, the second metal body 17 and the first metal body 16 are solid-phase diffusion bonded together, and the second metal body 17 is aged (joining and aging process). This joining process results in a dissimilar metal body in which the first metal body 16 made of hot work tool steel is joined to the second metal body 17 made of precipitation hardening heat resistant steel. After the joining and aging process, the dissimilar metal bodies are removed from the furnace.
[0058] Thereafter, the dissimilar metal bodies are placed in a furnace and heated to 950°C, and then cooled by air or oil to quench the first metal body 16 (quenching step). This 950°C is a third predetermined temperature T3 that is higher than the aging temperature of NCF750 and is higher than the quenching temperature at which SKD61 is quenched (as described above, the temperature at which the hardness of SKD61 after quenching and tempering becomes HRC38 or higher, more specifically HRC41 or higher). In addition, this third predetermined temperature T3 (950°C) needs to be lower than the solution temperature of NCF750. The inventors have confirmed that the minimum solution temperature of NCF750 described in JIS G 4902 is 965, and that 950°C is lower than this and does not cause NCF750 to be solutionized, that is, 950°C is lower than the solution temperature of NCF750.
[0059] After the quenching process, the dissimilar metal body is heated to 550°C and tempered (tempering process). This 550°C is the tempering temperature of SKD61, which is lower than the quenching temperature of SKD61. Thereafter, the dissimilar metal body is cooled, thereby completing the manufacture of the dissimilar metal body, i.e., the lower die 2 or the upper die 3.
[0060] The lower die 2 or the upper die 3 is manufactured in this manner, and the hardness of each of the first metal body 16 and the second metal body 17 after the tempering process is HRC 38 or more and HRC 47 or less, which is a hardness suitable for the hot forging die 1. The hardness of each of the first metal body 16 and the second metal body 17 after the tempering process is preferably HRC 41 or more and HRC 43 or less.
[0061] In this method of joining dissimilar metal bodies, the second metal body 17 is first subjected to a solution treatment, and then the second metal body 17 and the first metal body 16 are subjected to solid-phase diffusion bonding and aging treatment of the second metal body 17 at the same time. In other words, since the solution treatment of the second metal body 17 is performed before the solid-phase diffusion bonding, the second metal body 17 can be reliably precipitation hardened without being restricted by the temperature and cooling rate of SKD61. In addition, since the solid-phase diffusion bonding and aging treatment are performed at the same time, the heat treatment required five times is reduced to four times as shown in FIG. 2. This reduces the cost and energy required for joining and heat treatment.
[0062] In this joining method, after the joining and aging process, a quenching process is performed in which the dissimilar metal bodies are heated to 950°C and then cooled, and then a tempering process is performed in which the dissimilar metal bodies are heated to 550°C. As a result, the first metal body 16 is quenched without the second metal body 17 being solutionized in the quenching process, and the first metal body 16 is tempered in the tempering process. These processes allow the properties of the hot work tool steel and precipitation hardening heat resistant steel contained in the dissimilar metal bodies to be properly exhibited.
[0063] In this way, since the third predetermined temperature T3 when quenching the first metal body 16 in the quenching process is in the temperature range of 950°C or higher and lower than 1100°C, the first metal body 16 made of SKD61 is quenched without coarsening the grains. Also, since NCF750 (precipitation hardening heat resistant steel) constituting the second metal body 17 is a precipitation hardening Ni-based alloy that does not go into solution at temperatures lower than the quenching temperature of 950°C but goes into solution at temperatures lower than 1100°C, the properties of the hot work tool steel and precipitation hardening heat resistant steel contained in the dissimilar metal bodies are properly exhibited.
[0064] In the quenching process, the time for which the dissimilar metal body is held at 950°C (third predetermined temperature T3) is the estimated shortest time required to bring the entire first metal body 16 to 950°C, depending on the size of the first metal body 16, and the dissimilar metal body is immediately cooled after the estimated shortest time has elapsed. This allows the first metal body 16 to be quenched without the second metal body 17 made of NCF750 (precipitation hardening heat resistant steel) becoming overaged.
[0065] If the first metal body 16 made of hot work tool steel is cooled by water in the quenching process, thermal stress may cause cracks to occur in the first metal body 16. In this embodiment, the dissimilar metal body is cooled by air cooling, so that the first metal body 16 is quenched without causing cracks.
[0066] In addition, by using SKD61 as the hot work tool steel for the first metal body 16 and NCF750 as the precipitation hardening heat resistant steel for the second metal body 17, a dissimilar metal body is manufactured in which these properties are appropriately exhibited.
[0067] Although the description of the specific embodiment is finished above, the present invention is not limited to the above embodiment and modified examples, and can be widely modified and implemented. For example, as shown by imaginary lines in Fig. 3, the tempering process may be performed consecutively to the joining and aging process, that is, without cooling the dissimilar metal bodies. In this case, the time from when the dissimilar metal bodies are heated to 900°C to when the temperature rise for quenching begins may be 9 hours. With this method, the number of heat treatments can be reduced from four to three.
[0068] In addition, the shape of the hot forging die 1 is not limited to this, and the dissimilar metal body may be used in dies other than the hot forging die 1 or tools other than dies. In addition, the specific configuration and arrangement of each member or part, the quantity, material, specific procedure of each process, temperature, time, etc. can be appropriately changed within the scope of the present invention. In addition, all of the components shown in the above embodiment are not essential and can be selected as appropriate. [Explanation of symbols]
[0069] 1: Hot forging die 2: Lower mold 3: Upper mold 4: Rough molded product 5: Bali 6:Cross surface 7:Cross surface 8: Cavity 9: Cavity 10: Flash Land 11: Flashland 12: Inclined surface 13: Inclined surface 16:First metal body 17:Second metal body T1: 1st predetermined temperature T2: 2nd predetermined temperature T3: 3rd predetermined temperature
Claims
1. A method for joining dissimilar metal bodies, comprising joining a first metal body made of hot work tool steel and a second metal body made of precipitation hardening heat resistant steel, A solution treatment process in which the second metal body is heated to a first predetermined temperature higher than the solution temperature of the precipitation hardening heat resistant steel, the second metal body is solutionized, and then the second metal body is quenched to precipitation harden the second metal body; a joining and aging process in which, after the solution treatment process, the second metal body and the first metal body are heated to a second predetermined temperature lower than the solution temperature of the precipitation hardening heat resistant steel and higher than the aging temperature of the precipitation hardening heat resistant steel while being in close contact with each other with a predetermined pressure, and the second predetermined temperature is maintained for a predetermined time according to the second predetermined temperature, thereby performing solid-phase diffusion bonding between the second metal body and the first metal body and aging treatment of the second metal body; a quenching process in which, after the joining and aging process, the dissimilar metal body obtained by joining the second metal body to the first metal body is heated to a third predetermined temperature that is lower than the solution temperature of the precipitation hardening heat resistant steel and higher than the quenching temperature of the hot work tool steel, and then cooled to quench the first metal body; a tempering step of heating the dissimilar metal bodies to a tempering temperature of the hot work tool steel, the tempering temperature being lower than the quenching temperature, after the quenching step.
2. the third predetermined temperature when quenching the first metal body in the quenching step is in a temperature range of 950° C. or more and lower than 1100° C., 2. The joining method according to claim 1, wherein the precipitation hardening heat resistant steel is a precipitation hardening Ni-based alloy which does not go into solution at a temperature lower than 950°C and goes into solution at a temperature lower than 1100°C.
3. The joining method according to claim 2 , wherein the first predetermined temperature in the solution treatment is higher than a grain coarsening temperature of the hot work tool steel.
4. The joining method according to any one of claims 1 to 3, wherein in the quenching step, a time for holding the third predetermined temperature is an estimated shortest time estimated to be required to bring the entire first metal body to the third predetermined temperature depending on a size of the first metal body, and the dissimilar metal bodies are cooled immediately after the estimated shortest time has elapsed.
5. The joining method according to any one of claims 1 to 3, wherein the second metal body is cooled by water cooling in the solution forming step.
6. The joining method according to any one of claims 1 to 3, wherein the dissimilar metal bodies are cooled by air cooling or oil cooling in the quenching step.
7. The joining method according to any one of claims 1 to 3, wherein the quenching step is carried out consecutively to the joining and aging step.
8. The joining method according to any one of claims 1 to 3, wherein the hardness of each of the first metal body and the second metal body after the tempering step is HRC 38 or more and 47 or less.
9. The joining method according to any one of claims 1 to 3, wherein the hot work tool steel is SKD61 and the precipitation hardening heat resistant steel is NCF750.
10. A hot forging die including a lower die and an upper die formed by the dissimilar metal bodies in which the second metal body is joined to the first metal body by the joining method according to claim 1, the lower die and the upper die each have a cavity recessed in a cut surface thereof, and an inclined surface formed on the outside of the cavity in order to suppress burrs generated between the cut surfaces; Each of the lower mold and the upper mold has a mold body formed from the first metal body, A hot forging die, wherein each of the inclined surfaces of the lower die and the upper die is formed by the second metal body.
Citation Information
Patent Citations
Joining heat treatment for dissimilar metallic materials
JP1998298663A
Composite die for hot forging
JP1999347678A