Group-iii nitride-based semiconductor light-emitting element
The introduction of a compositionally graded layer in GaN-based semiconductor lasers addresses hole leakage and absorption issues, enhancing power-to-light conversion efficiency and reducing power consumption while maintaining optical output.
Patent Information
- Application Number
- JP2023082986
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing GaN-based semiconductor lasers face issues with high power consumption and reduced optical output due to hole leakage and absorption in the n-side optical guide layer, which reduces power-to-light conversion efficiency.
A compositionally graded layer with increasing In composition between the n-side optical guide layer and the light emitting layer is introduced, creating a potential barrier to reflect holes and prevent leakage, thereby improving luminous efficiency without doping the n-side optical guide layer.
This structure enhances power-to-light conversion efficiency, reduces power consumption, and maintains optical output by minimizing hole leakage and absorption, ensuring long-term reliability and high efficiency.
Smart Images

Figure 2024166698000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a Group III nitride semiconductor light emitting device that can realize a GaN semiconductor laser device having a low operating current. [Background technology]
[0002] Semiconductor lasers have excellent features such as small size, low cost, and high output, and are therefore used in a wide range of technical fields, including IT technologies such as communications and optical disks, as well as medical and some lighting. In recent years, high-power semiconductor lasers have been used as light sources for processing various materials, such as metals, resins, and carbon fiber reinforced plastics (CFRP). In particular, laser processing machine systems with large optical outputs ranging from several hundred watts to several kilowatts have been developed and put into practical use by using light synthesis technology that bundles multiple laser emission points to increase output. Laser processing has many advantages, such as remote processing, high throughput, low power consumption, and programmability, and is widely used in industrial production sites. In recent years, GaAs-based near-infrared lasers with a wavelength of about 1 μm have been widely used as semiconductor light sources for such laser processing. This is due to the fact that semiconductor formation technology and process technology on GaAs substrates have become fully mature.
[0003] In recent years, copper, which has excellent properties such as low electrical resistance, easy workability, and high heat dissipation, has been widely used in various fields such as motors and batteries for electric vehicles (EVs). However, because copper reflects near-infrared laser light, there is an issue that when laser processing is attempted, the energy does not enter into heat, making processing difficult.
[0004] Therefore, GaN-based semiconductor lasers that emit light in the blue wavelength region (wavelength 405nm to 540nm), where copper material has low reflectance (high absorption), are used for processing copper materials. When applying GaN semiconductors to laser processing, high optical output (processing energy) is required, and high-power operation is required. To achieve such high-power operation, the semiconductor laser element needs to be sufficiently cooled and a large amount of current needs to be passed through it. In other words, a large amount of electricity is required, and from the perspective of environmental load, it is particularly important to reduce the power consumption of semiconductor lasers.
[0005] In order to reduce the power consumption of semiconductor lasers, it is necessary to efficiently convert the input power into light. In other words, it is important to increase the power-to-light conversion efficiency, which indicates the proportion of the input energy that is converted into laser light. Furthermore, by converting the input power into light with high efficiency, it is not only possible to increase the optical output, but also to prevent excess energy from turning into heat, thereby reducing the decrease in optical output caused by heat generation and the adverse effects on long-term reliability characteristics.
[0006] In a typical pn junction diode type semiconductor laser, the mechanism of generating laser light is as follows. In a semiconductor laser element, an n-type light confinement layer (cladding layer), an n-side light guide layer, an emission layer, a p-side light guide layer, and a p-type light confinement layer (cladding layer) are at least stacked in order on a substrate. Here, electrons are injected into the emission layer of the semiconductor laser element through the n-type cladding layer and the n-side light guide layer, and holes are injected through the p-type cladding layer and the p-side light guide layer. A certain percentage of these electrons recombine in the emission layer and emit light. Here, among the holes flowing from the p-type cladding layer side toward the emission layer, some diffuse beyond the emission layer to the n-side light guide layer. These holes recombine and disappear in the n-side light guide layer outside the emission layer, and become a reactive current that does not contribute to laser oscillation, which is one of the factors that increase power consumption. Several techniques have been disclosed as a method of reducing such a reactive hole current. For example, in Patent Document 1, the n-side light guide layer is doped with n-type impurities. As a result, a potential barrier is created in the n-side optical guide layer from the perspective of holes diffusing from the light-emitting layer, which causes the holes to be reflected back to the light-emitting layer where they recombine with electrons, thereby reducing the reactive current. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2000-236142 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, in the configuration described in Patent Document 1, the laser light generated in the light emitting layer propagates in the n-type doped n-side light guide layer. The laser light propagating in the n-side light guide layer is absorbed by excess electrons generated by the n-side impurities and other impurities, and cannot be extracted to the outside. Therefore, there is a problem that the optical output decreases even though the reactive current is reduced.
[0009] The present disclosure has been made in view of the above problems, and has an object to provide a Group III nitride-based semiconductor light-emitting device capable of efficiently converting input electric power into light. [Means for solving the problem]
[0010] Through intensive research by the present inventors, it has been found that in a group III nitride semiconductor light-emitting element used in a GaN semiconductor laser, a composition gradient layer in which the In composition changes from a low In composition to a high In composition is provided between the n-side optical guide layer and the light-emitting layer, a potential barrier is generated in the band structure (valence band) on the hole side, holes diffusing from the light-emitting layer side can be reflected, and leakage of holes is prevented, thereby increasing the light-emitting efficiency of the group III nitride semiconductor light-emitting element. In such a structure, while preventing leakage of holes, it is not necessary to dope the n-side optical guide layer, or even if it is doped, a very small concentration is sufficient. Therefore, there is an advantage that the absorption of laser light in the n-type optical guide layer does not substantially occur.
[0011] That is, the present disclosure provides a Group III nitride semiconductor light-emitting device comprising, in this order, a substrate, an n-type cladding layer, an n-side light guiding layer, a light-emitting layer containing In, a p-side light guiding layer, and a p-type cladding layer, and a compositionally graded layer between the n-side light guiding layer and the light-emitting layer, in which the In composition increases from the n-side light guiding layer toward the light-emitting layer, and the minimum In composition of the compositionally graded layer is lower than the In composition of a region of the n-side light guiding layer in contact with the compositionally graded layer. Effect of the Invention
[0012] According to the present disclosure, a Group III nitride semiconductor light emitting device capable of efficiently converting input electric power into light is provided. [Brief description of the drawings]
[0013] [Figure 1]FIG. 1A is a plan view of a semiconductor light-emitting device according to an embodiment of the present disclosure, and FIG. 1B is an enlarged cross-sectional view taken along line AA in FIG. 1A. [Diagram 2] Band structure and electron-hole concentration distribution diagram near the light-emitting layer in a comparative example (without a composition-graded layer) [Diagram 3] Band structure and electron-hole concentration distribution diagram in the vicinity of the light-emitting layer in the embodiment [Figure 4] Calculation results of non-radiative recombination in the embodiment and the comparative example [Diagram 5] FIG. 1 is a correlation diagram between the film thickness of a composition gradient layer and the height of a potential barrier on the valence band side for holes in an embodiment. [Figure 6] FIG. 1 is a correlation diagram between the change in thickness of the first barrier layer in the light-emitting layer and the emission wavelength in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] A preferred embodiment of the present invention will be specifically described below, but the present disclosure is not limited to this embodiment.
[0015] A Group III nitride semiconductor light emitting device (hereinafter also simply referred to as "semiconductor light emitting device") 100 according to this embodiment will be described with reference to Figs. 1A and 1B. Fig. 1A is a plan view of the semiconductor light emitting device 100 of this embodiment. Fig. 1B is a cross-sectional view of the semiconductor light emitting device 100 taken along line AA in Fig. 1A (a view of the cross section from the side indicated by the arrow). In the following, the semiconductor light emitting device 100 of this embodiment will be described taking as an example a case in which the n-side light guiding layer 3, the light emitting layer 5, the p-side light guiding layer 6, etc. contain hexagonal Group III nitride semiconductors.
[0016] First, a simple configuration of the semiconductor light emitting element 100 will be described. As shown in FIG. 1B, the semiconductor light emitting device 100 includes an n-type hexagonal GaN substrate (substrate) 1 having a (0001) plane as a main surface, an n-AlGaN layer (n-type cladding layer) 2, n-GaN and i-In x1The light emitting layer 5 is a laminate of an n-side optical guide layer 3, which is a stack of GaN (x1>0), an i-InGaN layer (composition gradient layer) 4 in which the In composition increases from the n-side optical guide layer 3 side toward the light emitting layer 5 side, an InGaN composition barrier layer (first barrier layer), an InGaN quantum well layer (quantum well layer), and an InGaN barrier layer (second barrier layer), an i-InGaN layer (p-side optical guide layer) 6, and a p-Al 0.35 It has a structure in which a GaN layer (electron barrier layer) 7, a superlattice layer (p-type cladding layer) 8 which is a laminate of p-AlGaN and GaN, and a p-GaN layer (p-type contact layer) 9 are laminated in this order.
[0017] The semiconductor light emitting element 100 has an optical waveguide 20 structure. Specifically, an insulating film 10 made of SiO2 is disposed on both sides of the p-type cladding layer 8 and the p-type contact layer 9. On the other hand, a p-type electrode 11 made of a laminate of Pd and Pt, a wiring electrode 12 made of a laminate of Ti, Pt, and Au, and a pad electrode 13 made of a laminate of Ti and Au are disposed on the p-type contact layer 9. As shown in FIG. 1A, a rear coat film 15 made of a dielectric multilayer film for reflecting light in the optical waveguide 20 is disposed on one end of the optical waveguide 20. On the other hand, a front coat film 14 made of a dielectric multilayer film for emitting light is disposed on the other end of the optical waveguide 20. Furthermore, an n-type electrode 16 made of a laminate of Ti and Au is disposed on the surface of the substrate 1 opposite to the n-type cladding layer 2. In the above, the light emitting layer 5 has been described as having three layers: an InGaN composition barrier layer (first barrier layer), an InGaN quantum well layer (first quantum well layer), and an InGaN barrier layer (second barrier layer). However, the light emitting layer 5 may have a multiple quantum well structure in which barrier layers and quantum well layers are repeatedly stacked.
[0018] Next, the detailed configuration of the semiconductor light emitting device 100 will be described together with the manufacturing method. However, the film thickness and composition of each layer can be appropriately adjusted. Furthermore, in addition to the layers described below, other configurations may be included within the scope that does not impair the purpose and effect of the present disclosure.
[0019] First, the n-type cladding layer 2 to the p-type contact layer 9 are successively formed on the n-type hexagonal GaN substrate 1, the main surface of which is the (0001) plane, by metalorganic chemical vapor deposition (MOCVD). 0.03 A GaN layer (n-type cladding layer 2) is deposited to a thickness of about 3 μm. In this embodiment, trimethylgallium (TMG), trimethylindium (TMI), and trimethylaluminum (TMA) are used as Group III raw materials, silane is used as an n-type impurity, and ammonia is used as a Group V raw material as gas raw materials for film formation, but other materials may also be used. The Si concentration of the n-AlGaN layer (n-type cladding layer 2) is 1×10 18 cm -3 degree is preferred.
[0020] Next, as the first layer of the n-side optical guide layer 3, an n-GaN layer is formed to a thickness of about 250 nm in the same manner as the n-type cladding layer 2. Here, the Si concentration of the n-GaN layer is 1×10 18 cm -3 Furthermore, an i-InGaN layer, which is the remaining layer of the n-side optical guide layer 3, is laminated to a thickness of 150 nm.
[0021] Next, the composition gradient layer 4 is formed in which the In composition increases from the n-side light guide layer 3 side to the light emitting layer 5. The composition gradient layer 4 may have a minimum In composition smaller than that of the i-InGaN layer of the n-side light guide layer 3, but is more preferably 0%. On the other hand, the maximum In composition in the composition gradient layer 4 is preferably substantially the same as the In composition of the barrier layer of the light emitting layer 5 adjacent to the composition gradient layer 4. In addition, it is preferable to adjust the In composition so that the region with the lowest In composition in the composition gradient layer 4 is close to the n-side light guide layer and the region with the highest In composition is close to the barrier layer of the light emitting layer 5. In this embodiment, an i-InGaN layer (composition gradient layer 4) in which the In composition gradually increases from 0% to 3% from the boundary with the n-side light guide layer 3 to the boundary with the light emitting layer 5 is formed. The thickness of the composition gradient layer 4 is preferably thicker than 5 nm, more preferably 7 nm or more, even more preferably 10 nm or more, and even more preferably 15 nm or more. However, if the composition gradient layer is too thick, the average refractive index of that portion will decrease, which may cause problems in the optical design of the element. For this reason, the thickness of the composition gradient layer 4 is usually preferably 20 nm or less.
[0022] The In composition change in the composition gradient layer 4 may increase continuously or intermittently from the n-side light guide layer 3 side to the first barrier layer of the light emitting layer 5. In other words, it is sufficient that the second derivative of the In composition change with respect to the film thickness is positive in a region, and it may be negative or zero in a portion. However, it is preferable that the In composition increase continuously from the n-side light guide layer 3 side to the barrier layer of the light emitting layer 5. One method for changing the In composition in the composition gradient layer 4 is to adjust the amount of trimethylindium (TMI) gas used. Another method is to increase the amount of In taken up by lowering the growth temperature.
[0023] Next, as a part of the light-emitting layer 5, In 0.03A GaN barrier layer (first barrier layer) is formed to a thickness of 7 nm. The thickness of the first barrier layer is preferably 3 nm or more, more preferably 5 nm or more, even more preferably more than 7 nm, and particularly preferably more than 10 nm. In this embodiment, the quantum well layer of the light emitting layer 5 and the composition gradient layer 4 are separated by the first barrier layer. If the first barrier layer does not exist, carriers (electrons or holes) confined in the quantum well (layer) may quantum-couple with the composition gradient layer 4, and the emission wavelength may change through a change in quantization energy. The refractive index of the first barrier layer may be equal to or greater than the refractive index of the n-side light guide layer 3 described above, but is more preferably greater than the refractive index of the n-side light guide layer 3 from the viewpoint of the light confinement effect inside the semiconductor light emitting device 100. Next, In 0.18 A GaN quantum well layer (first quantum well layer) is deposited to a thickness of about 3.0 nm. 0.03 A GaN barrier layer (second barrier layer) is deposited to a thickness of about 10 nm. Then, an InGaN well layer (second quantum well layer) is deposited to a thickness of 3.0 nm. Finally, In 0.03 The GaN barrier layer (third barrier layer) is grown to 10 nm. Here, each barrier layer (n 0.03 If the thickness of the GaN layer is too thick, the efficiency will decrease due to radiative recombination. Therefore, it is preferable to limit the thickness of each barrier layer to about 40 nm at most. In the above example, the thicknesses of the second and third barrier layers are each set to 10 nm, but from the viewpoint of uniformity of carrier injection, the thicknesses of the first, second, and third barrier layers may be different from each other.
[0024] Next, an i-InGaN layer, i-GaN or i-AlGaN layer, or a layer made of a combination of these, which constitutes the p-side light guide layer 6, is deposited to a thickness of about 0.2 μm. From the viewpoint of light confinement inside the semiconductor light emitting device 100, it is preferable that the refractive index of the p-side light guide layer 6 is smaller than that of the light emitting layer 5 (third barrier layer), and it is also preferable that the refractive index within the p-type guide layer 6 gradually decreases from the light emitting layer 5 side toward the electron barrier layer 7 side. That is, by forming the p-side light guide layer 6 in the order of InGaN, GaN, and AlGaN from the side closer to the light emitting layer 5, the light confinement can be increased.
[0025] Next, p-Al constituting the electron barrier layer 7 0.35 GaN(Mg concentration 5×10 19 cm -3 The p-AlGaN layer is formed by depositing a 5 nm thick film of cyclopentadienyl magnesium (CpMg) with a Mg concentration of 5×10 19 cm -3 It is advisable to make it so that:
[0026] Next, p-Al constituting the p-type cladding layer 8 0.03 GaN (Mg concentration 1×10 19 cm -3 ) is deposited to a thickness of 600 nm. Furthermore, the p-GaN (Mg concentration is 1×10 20 cm -3 ) is deposited to a thickness of 10 nm.
[0027] Next, the nitride semiconductor laminate structure fabricated by MOCVD is processed into a ridge stripe type laser. For example, a SiO2 insulating film (not shown) made of SiO2 with a thickness of 0.3 μm is formed on the p-type contact layer 9 by thermal CVD. Furthermore, the SiO2 insulating film is left in a stripe shape with a width of 16 μm and other regions are etched by photolithography and etching using hydrofluoric acid. At this time, the direction of the stripe is parallel to the m-axis direction of the hexagonal GaN, considering that the end face of the laser is formed by using the natural cleavage plane (m-plane) of the hexagonal nitride semiconductor.
[0028] Next, the p-type contact layer 9 and the p-type cladding layer 8 in the region where the SiO2 insulating film has been removed are etched to a depth of 0.85 μm from the upper portion where the SiO2 insulating film has been formed by inductively coupled plasma (ICP) etching, forming a ridge stripe portion that constitutes the optical waveguide 20. After that, the remaining SiO2 insulating film is removed using hydrofluoric acid. Then, the insulating film 10 made of SiO2 and having a thickness of 200 nm is formed again by thermal CVD over the entire surface of the exposed p-type cladding layer 8 including the ridge stripe portion.
[0029] Next, a resist pattern (not shown) having an opening with a width of 15.5 μm along the top surface of the ridge stripe portion (optical waveguide 20) is formed by lithography on the ridge stripe portion in the insulating film 10. Then, the SiO2 insulating film on the top surface of the ridge stripe portion is etched by reactive ion etching (RIE) using methane trifluoride (CHF3) gas, using the resist pattern as a mask, to expose the p-type contact layer 9 from the upper surface of the ridge stripe portion.
[0030] Next, a metal laminate film constituting p-type electrode 11 made of, for example, palladium (Pd) with a thickness of 40 nm and platinum (Pt) with a thickness of 35 nm is laminated on at least the p-type contact layer 9 exposed from the upper surface of the ridge stripe portion by, for example, electron beam (EB) deposition. Thereafter, the resist pattern is removed by a lift-off method to remove the metal laminate film in the region other than the upper portion of the ridge stripe, thereby forming the p-type electrode 11.
[0031] Furthermore, a wiring electrode 12 (shown by a dotted line in FIG. 1A) made of Ti (50 nm) / Pt (200 nm) / Au (100 nm) is selectively formed by lithography and lift-off so as to cover the p-type electrode 11 on the top of the ridge stripe and the side surface (insulating film 10) of the ridge stripe. The planar dimension (length) of the wiring electrode 12 in the direction parallel to the ridge stripe is 1150 μm, and the planar dimension (width) in the direction perpendicular to the ridge stripe is 150 μm. Generally, a plurality of waveguides having the same configuration are fabricated in a matrix on one laminated structure. In addition, this is divided when used. At this time, if the wiring electrodes 12 of the plurality of waveguides are connected to each other, there is a risk that the p-type electrode 11 in close contact with the wiring electrode 12 will peel off from the p-type contact layer 9 during division. Therefore, when a plurality of waveguides are formed on a laminated structure, it is desirable to form the wiring electrodes 12 of adjacent waveguides 20 so as not to be connected to each other.
[0032] Next, an Au layer having a thickness of 10 μm that constitutes the pad electrode 13 is formed by electrolytic plating on the upper part of the wiring electrode 12. With such a configuration, it becomes possible to mount a laser chip by wire bonding, and it is also possible to effectively dissipate heat generated in the light-emitting layer 5, thereby improving the reliability of the semiconductor light-emitting element 100.
[0033] Next, the back surface (substrate 1) of the laminate on which the pad electrode 13 has been formed is polished with diamond slurry to thin the substrate 1 to a thickness of about 100 μm. After that, a metal laminate film of Ti (5 nm) / Pt (10 nm) / Au (1000 nm) that constitutes the n-type electrode 16 is formed on the surface of the substrate 1 (the surface opposite to the surface on which the optical waveguide 20 is formed) by, for example, EB deposition.
[0034] The semiconductor light emitting element 100 in the wafer state is cleaved (primary cleavage) along the m-plane so that the length in the m-axis direction is, for example, 1200 μm. Next, a front coat film 14 is formed on the cleavage plane from which the laser light is emitted, and a rear coat film 15 is formed on the opposite cleavage plane, for example, by using an electron cyclotron resonance (ECR) sputtering method. Here, a dielectric film such as a SiO2 single layer film is used as the material for the front coat film 14. A dielectric film such as a ZrO2 / SiO2 laminated film is used as the material for the rear coat film 15. A highly efficient semiconductor light emitting element 100 can be configured by setting the reflectance of the front side (light emission side) of the semiconductor light emitting element 100 to, for example, 6% and the rear side (opposite side to the light emission side) to, for example, 95%. In addition, when an external resonant optical system is used in which a semiconductor laser (semiconductor light emitting element 100) is combined with a condenser lens or the like arranged on the laser optical axis outside the semiconductor laser to oscillate, the front side reflectance is preferably 1% or less. Next, the semiconductor light emitting element 100 that has been primarily cleaved is cleaved (secondarily cleaved) along the a-plane between the optical waveguides 20 that are formed with a pitch of, for example, 200 μm in the a-axis direction, thereby completing a laser chip.
[0035] (Luminous efficiency of semiconductor light emitting devices) Here, the above-mentioned semiconductor light emitting device 100 is a pn junction semiconductor light emitting device, and in particular has a structure in which a composition gradient layer 4 in which the In composition gradually changes is disposed between the n-side light guiding layer 3 and the light emitting layer 5. With such a structure, it is possible to form a layer having a potential barrier between the light emitting layer 5 and the n-side light guiding layer 3 in the valence band. As a result, it is possible to prevent the diffusion of holes into the n-side light guiding layer 3 and improve the light emitting efficiency of the semiconductor laser.
[0036] Here, FIG. 2(a) shows the calculation results of the band structure of the conduction band and the valence band of a semiconductor light-emitting device as a comparative example, and FIG. 2(b) shows the calculation results of the electron and hole concentration of the semiconductor light-emitting device. The semiconductor light-emitting device has the same structure as the above-mentioned semiconductor light-emitting device, except that it does not have the composition gradient layer 4. The calculation was performed by solving the Schrodinger-Poisson equation taking into account the polarization charge of each layer. The physical property parameters of the nitride-based semiconductor used in the calculation were the values shown in Non-Patent Document 1 (Nitride Semiconductor Devices, J. Piprek, J Principles and Simulation, 2007, WILEY-VCH). The symbols 3 to 6 in FIG. 2(a) and (b) are numbers corresponding to the symbols of each component of the semiconductor light-emitting device 100 in FIG. 1B, and respectively indicate the n-side light guide layer 3, the light-emitting layer 5, and the p-side light guide layer. Note that in the comparative example shown in FIG. 2(a) and (b) as the calculation results, the composition gradient layer 4 is not present and is not shown. As shown in the band structure diagram in Figure 2(a), electrons diffuse from the n-side conduction band and holes diffuse from the p-side valence band. Both recombine in the quantum well layer (QW) of the light-emitting layer 5, and a part of them is converted into laser light.
[0037] Here, holes injected from the p-side optical guide layer (InGaN layer) 6 into the light-emitting layer 5 are reflected by a potential barrier when passing through a region with a small valence band energy value. Looking at the valence band side band structure (lower diagram) of FIG. 2(a), the value of the valence band energy between the p-side optical guide layer 6 and the light-emitting layer 5 is the smallest. In other words, there is practically no barrier for holes injected from the p-side optical guide layer 6 into the light-emitting layer 5 from the light-emitting layer 5 to the n-side optical guide layer (InGaN layer) 3. Therefore, holes that do not combine with electrons in the quantum well light-emitting layer diffuse toward the n-side optical guide layer 3. This is also shown in the carrier concentration graph of FIG. 2(b), where the hole concentration in the n-side optical guide layer 3 is as high as the carrier concentration in the p-side optical guide layer 6. Here, if electrons and holes exist spatially at the same time in a region other than the light-emitting layer 5, both gradually disappear due to non-radiative recombination. Such disappearance does not contribute to laser oscillation and results in energy loss. Therefore, if it is possible to reduce the concentration of holes flowing from the light emitting layer 5 toward the n-side light guiding layer 3, that is, if a potential barrier can be provided that reflects the holes in the vicinity of the n-side light guiding layer 3, it is expected that the operating efficiency of the semiconductor laser can be improved.
[0038] Similar calculation results for the semiconductor light emitting device of this embodiment are shown in Fig. 3. Fig. 3(a) shows the calculation results for the band structures of the conduction band and valence band of the semiconductor light emitting device of this embodiment, and Fig. 3(b) shows the calculation results for the electron and hole concentrations of the semiconductor light emitting device. This embodiment differs from the above comparative example in that it has a compositionally graded layer 4 between the n-side light guiding layer 3 and the light emitting layer 5.
[0039] As shown in the lower diagram of FIG. 3(a), the conduction band energy of the semiconductor light emitting device of this embodiment has a large negative value in the region of the compositionally graded layer (i-InGaN layer) 4. This is because band bending occurs in the compositionally graded layer 4 due to the polarization charge of InGaN. As shown in the lower diagram of FIG. 3(a), in this embodiment, a potential barrier of about 140 meV occurs. Therefore, holes that pass through the light emitting layer 5 from the p-side light guiding layer (InGaN layer) 6 are reflected by this potential barrier. As a result, as shown in FIG. 3(b), the concentration of holes that reach the n-side light guiding layer (InGaN layer) 5 is reduced to about 1 / 10 of that in the comparative example shown in FIG. 2.
[0040] 4 shows the results of calculating the non-radiative recombination rate (the rate at which non-radiative recombination occurs) in this embodiment and the comparative example. Comparing the non-radiative recombination rates in the n-side optical guide layer 3, it can be seen that the non-radiative recombination rate of the embodiment of the present invention shown by the solid line in the figure is lower than the non-radiative recombination rate of the comparative example shown by the dotted line. This is because the potential barrier due to the composition gradient layer 4 shown in FIG. 3 reduces the concentration of holes reaching the n-side optical guide layer (InGaN layer) 3, and non-radiative recombination also decreases.
[0041] 5 shows the results of calculating the value of the potential barrier when the film thickness of the compositionally graded layer 4 is changed in this embodiment. The larger the potential barrier due to the compositionally graded layer 4 shown in FIG. 3, the more preferable it is. In addition, considering the effective mass of holes in GaN-based materials, the potential barrier is preferably 100 meV or more, and 200 meV or more is particularly effective. Therefore, as shown in FIG. 5, the film thickness of the compositionally graded layer 4 is preferably more than 5 nm, and more preferably more than 10 nm.
[0042] FIG. 6 shows the results of calculating the emission wavelength when the film thickness of the first barrier layer (QB) included in the light emitting layer 5, i.e., the barrier layer adjacent to the composition gradient layer 4, is changed in the embodiment of the present disclosure (in other words, the distance from the end of the composition gradient layer 4 on the light emitting layer 5 side to the nearest quantum well layer). When the film thickness of the first barrier layer (QB) is thin, the quantum well layer in the light emitting layer 5 and the electrons in the composition gradient layer 4 are quantum coupled, and the emission wavelength changes. This may cause an unintended wavelength change in the element design, and when a multiple quantum well structure is used, light is emitted at different wavelengths between different wells, which causes a decrease in the light emission efficiency of the semiconductor light emitting device 100. In this embodiment, when the light emitting layer 5 has only one quantum well layer, the emission wavelength is 450 nm. When multiple quantum wells (multiple quantum well layers) are used, it is preferable that the emission wavelength difference between the quantum wells is at least 3 nm, more preferably 0.1 nm or less. Furthermore, even when a single quantum well (single quantum well layer) is used, it is desirable that the deviation from the design value is 3 nm or less, more preferably 0.1 nm or less. Therefore, as shown in FIG. 6, the thickness of the first barrier layer is preferably more than 7 nm, and more preferably more than 10 nm.
[0043] In the gradient layer of FIG. 3(a) showing the band structure of an embodiment of the present disclosure, a positive potential is generated in the conduction band on the n-side light guide layer 3 side. This potential acts as a barrier for electrons, and may cause a voltage increase when electrons are injected from the n-side light guide layer 3 to the light emitting layer 5. According to studies by the inventors, the effective mass of an electron is lighter than that of a hole, and therefore the voltage increase due to the potential barrier is slight (about 0.05 V). Furthermore, in order to eliminate such a potential barrier, the composition gradient layer 4 may be doped with an n-type impurity. For example, 1×10 18 cm -3 By doping the composition gradient layer 4 with n-type impurities, such a potential barrier can be substantially eliminated. On the other hand, since the composition gradient layer 4 is a region where the laser light is guided, when n-type impurities are doped, the concentration is set to 2×10 18 cm -3 It is preferable to keep it below this.
[0044] (others) As a crystal growth method for forming the above-mentioned semiconductor light-emitting element, in addition to the MOCVD method, a growth method capable of growing a GaN-based blue-violet semiconductor laser structure, such as a molecular beam epitaxy (MBE) method or a chemical beam epitaxy (CBE) method, may be used. In addition, when AlGaN and GaN are laminated, or when GaN and InGaN are laminated, the composition of In or Al may be adjusted so as to gradually change at the interface between them. In addition, in the above-mentioned embodiment, the case where each layer is made of a GaN-based material has been described, but other material systems that generate polarization by changing the composition, such as a structure in which AlGaAs or InGaAs is laminated on GaAs, a structure in which InGaAsP or AlGaAsP is laminated on InP, or a structure in which GaInSb is laminated on GaSb, may also be used.
[0045] Furthermore, in this embodiment, the chip is divided into chips with a width of 200 μm, but it may be an array element in which a plurality of light emitting elements are formed in succession.
[0046] In this embodiment, a pn junction type semiconductor laser has been described, but the laser may be a pn junction type semiconductor LED or a unipolar electron conduction type quantum cascade laser as long as the laser has a structure in which electrons are conducted in the stacking direction and there is a potential in layers having different compositions. [Industrial Applicability]
[0047] The group III semiconductor light emitting device of the present disclosure is applicable to a wide range of technical fields, such as high-power semiconductor lasers, communications, IT technologies such as optical discs, medicine, and some lighting. [Explanation of symbols]
[0048] 1 Board 2 n-type cladding layer 3. N-side optical guide layer 4 Compositionally graded layer 5. Light-emitting layer 6 p-side optical guide layer 7. Electron barrier layer 8 p-type cladding layer 9 p-type contact layer 10. Insulating film 11 p-type electrode 12 Wiring electrode 13 Pad electrode 14 Front coat film 15 Rear coat film 16 n-type electrode
Claims
1. a substrate, an n-type cladding layer, an n-side optical guide layer, an In-containing light-emitting layer, a p-side optical guide layer, and a p-type cladding layer, in this order; a composition gradient layer between the n-side optical guide layer and the light emitting layer, in which the In composition increases from the n-side optical guide layer toward the light emitting layer; and the lowest In composition of the composition gradient layer is lower than the In composition of a region of the n-side optical guide layer that is in contact with the composition gradient layer; Group III nitride semiconductor light emitting device.
2. 2. The Group III nitride semiconductor light emitting device according to claim 1, A Group III nitride semiconductor light emitting device, wherein the composition gradient layer has a thickness of more than 5 nm.
3. 3. The Group III nitride semiconductor light emitting device according to claim 2, A Group III nitride semiconductor light emitting device, wherein the composition gradient layer has a thickness of more than 10 nm.
4. The Group III nitride semiconductor light-emitting device according to any one of claims 1 to 3, the light emitting layer includes a barrier layer disposed adjacent to the composition gradient layer, and a quantum well layer disposed adjacent to the barrier layer; A Group III nitride semiconductor light emitting device, wherein the refractive index of the barrier layer is equal to or higher than the refractive index of the n-side optical guide layer.
5. 5. The Group III nitride semiconductor light emitting device according to claim 4, A Group III nitride semiconductor light emitting device, wherein the barrier layer has a thickness of more than 7 nm.
6. 5. The Group III nitride semiconductor light emitting device according to claim 4, A Group III nitride semiconductor light emitting device, wherein the barrier layer has a thickness of more than 10 nm.
Citation Information
Patent Citations
Nitride semiconductor laser
JP2000236142A