Energy augment structures for use with energy emitters and collectors

Energy augmentation structures and converters enhance electromagnetic energy capture and conversion, addressing inefficiencies in existing technologies by intensifying light emissions and improving energy collection.

JP2024167214AActive Publication Date: 2024-12-03IMMUNOLIGHT LLC
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024125940
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-12-31
Filing Date
2024-08-01
Publication Date
2024-12-03
Estimated Expiration
2040-01-30

AI Technical Summary

Technical Problem

Existing technologies for light emission and collection face inefficiencies in converting and enhancing electromagnetic energy, particularly due to rapid decay of plasmonic effects and ineffective harvesting of non-optimal light, leading to waste heat and reduced power generation.

Method used

The use of energy augmentation structures, such as electromagnetic resonators and fractal structures, to enhance electromagnetic fields and improve the efficiency of energy converters, including luminescent materials, to shift and intensify light emissions.

Benefits of technology

Enhances electromagnetic energy capture and conversion, improving the intensity and efficiency of light emission, particularly in applications like solar cells and medical procedures, by focusing and intensifying electromagnetic fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167214000001_ABST
    Figure 2024167214000001_ABST
Patent Text Reader

Abstract

To develop displays with relatively high contrast images while minimizing the amount of broadband light emitted or reflected from the displays, which may detract from the contrast of the images displayed.SOLUTION: An emission enhancement structure has: an emission enhancement structure having at least one energy augmentation structure; and an energy converter capable of receiving energy from an energy source, converting the energy, and emitting therefrom a light of energy different from the received energy. The energy converter is disposed in the vicinity of the at least one energy augmentation structure such that the emitted light is emitted with intensity larger than in the case where the converter is remote from the at least one energy augmentation structure. Also described are various uses of energy emitters, energy augmentation structures and energy collectors in a wide array of fields, such as color enhancement, and color enhancement structures including the same.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is related to U.S. Provisional Application No. 62 / 955,533, filed December 31, 2019, entitled "ENERGY AUGMENTATION STRUCTURE; ENERGY COLLECTOR CONTAINING THE SAME; AND EMISSION ENHANCEMENTS UTILIZING AT LEAST ONE ENERGY AUGMENTATION STRUCTURE," the entire disclosure of which is incorporated herein by reference. This application is related to U.S. Provisional Application No. 62 / 946,648, filed December 11, 2019, entitled "ENERGY AUGMENTATION STRUCTURE; ENERGY COLLECTOR CONTAINING THE SAME; AND EMISSION ENHANCEMENTS UTILIZING AT LEAST ONE ENERGY AUGMENTATION STRUCTURE," the entire disclosure of which is incorporated herein by reference. This application is related to U.S. Provisional Application No. 62 / 897,677, filed September 9, 2019, and entitled "ENERGY AUGMENTATION STRUCTURE; ENERGY COLLECTOR CONTAINING THE SAME; AND EMISSION ENHANCEMENTS UTILIZING AT LEAST ONE ENERGY AUGMENTATION STRUCTURE," the entire disclosure of which is incorporated herein by reference. This application is related to U.S. Provisional Application No. 62 / 855,508, filed May 31, 2019, and entitled "ENERGY AUGMENTATION STRUCTURE; ENERGY COLLECTOR CONTAINING THE SAME; AND COLOR ENHANCEMENT UTILIZING AT LEAST ONE ENERGY AUGMENTATION STRUCTURE," the entire disclosure of which is incorporated herein by reference.This application is related to U.S. Provisional Application No. 62 / 813,390, entitled "COLOR ENHANCEMENT UTILIZING AT LEAST ONE ENERGY AUGMENTATION STRUCTURE," filed March 4, 2019, the entire disclosure of which is incorporated herein by reference. This application is related to pending U.S. Application No. 16 / 599,732, filed October 11, 2019, which claims priority to U.S. Provisional Application No. 62 / 745,057, filed October 12, 2018, the entire contents of each of which are incorporated herein by reference. This application is related to U.S. Application No. 13 / 204,355, filed August 5, 2011, the entire disclosure of which is incorporated herein by reference. This application is related to U.S. Provisional Patent Application No. 61 / 371,549, filed August 6, 2010. This application is related to U.S. Provisional Patent Application No. 61 / 161,328, filed March 18, 2009, and to U.S. Provisional Patent Application No. 61 / 259,940, filed November 10, 2009, the entire disclosures of which are incorporated herein by reference. This application is related to U.S. Application No. 12 / 725,108, the entire disclosure of which is incorporated herein by reference.

[0002] This application is related to Provisional Application Nos. 60 / 954,263, filed August 6, 2007, and 61 / 030,437, filed February 21, 2008, and to U.S. Application No. 12 / 059,484, filed March 31, 2008, the entire contents of which are incorporated herein by reference. This application is also related to U.S. Application No. 11 / 935,655, filed November 6, 2007, and Provisional Application Nos. 61 / 042,561, filed April 4, 2008, 61 / 035,559, filed March 11, 2008, and 61 / 080,140, ​​filed July 11, 2008, the entire contents of which are incorporated herein by reference. This application is related to U.S. patent application Ser. No. 12 / 401,478, filed March 10, 2009, the entire contents of which are incorporated herein by reference. This application is related to U.S. patent application Ser. No. 11 / 935,655, filed November 6, 2007, and U.S. patent application Ser. No. 12 / 059,484, filed March 31, 2008, U.S. patent application Ser. No. 12 / 389,946, filed February 20, 2009, and U.S. patent application Ser. No. 12 / 417,779, filed April 3, 2009, the entire contents of which are incorporated herein by reference. [Background technology]

[0003] FIELD OF THE INVENTION The present invention relates to methods, systems, and devices for energy enhancement, with or without an energy modulation / energy conversion agent present, and in particular to be used to generate or enhance photon or electron emission and / or enhance light or photon collection.

[0004] Background Considerations Currently, light (i.e., electromagnetic radiation from radio frequencies through visible light to the X-ray wavelength range) is used in many industrial, communications, electronic, and pharmaceutical processes. Light in the infrared and visible ranges is typically generated from electrical energy sources, which, for example, heat materials to very high temperatures, where blackbody radiation occurs (such as in incandescent lamps). Light in the visible and ultraviolet ranges is typically generated by heating gases to an electrical discharge, where a transition from one electronic state of the gas atoms or molecules occurs with the emission of light. There are also semiconductor-based light sources (such as light-emitting diodes and semiconductor lasers), where electron / hole recombination in a material results in the emission of light.

[0005] Visible light is defined as electromagnetic radiation with wavelengths between 380 nm and 750 nm. Generally, electromagnetic radiation, including light, is produced by the acceleration and deceleration, or changes in motion (vibration), of electrically charged particles, such as parts of molecules (or neighboring atoms) with high thermal energy, or electrons within atoms (or molecules).

[0006] For reference, infrared (IR) radiation is just beyond the red end of the visible spectrum, and ultraviolet (UV) radiation has shorter wavelengths than violet light. The UV portion of the spectrum is divided into three regions: UVA (315-400nm), UVB (280-315nm), and UVC (100-280nm).

[0007] Industrial lamps used in lighting applications cover wavelengths in the visible range for proper white perception. The heat source, such as a heated filament, can be made with various types of conductors, such as W filaments, halogen-protected W filaments, or electrically induced high-temperature plasma (arc lamps).

[0008] The power of a radiant source (energy emitted per second) is often expressed in watts (W), but to account for the varying sensitivity of the eye to different wavelengths of light, light can also be expressed in lumens (lm). A related derived unit is W / m in a particular direction per steradian (a unit of solid angle). 2 (lm / m 2) and W / m 2 (lm / m 2 is the irradiance (illuminance) of a surface (in radiance units, or lux).

[0009] With the development of UV sources, UV radiation is increasingly being utilized for industrial, chemical, and pharmaceutical purposes. For example, UV light is known to sterilize media and promote many light-activated chemical processes, such as cross-linking of polymers in adhesives and coatings. UV sources typically use gas discharge lamps to generate emitted light in the UV range. The emitted light is then optically filtered to remove many, if not all, non-UV frequencies. UV light can also be generated in semiconductor phosphorescent materials from the excitation of these materials from high-energy sources, such as X-ray irradiation.

[0010] With the development of infrared radiation sources, infrared radiation is increasingly being utilized for communication and signaling purposes. Typically, infrared sources use broad spectrum light sources called globars to generate a broad spectrum of light centered in the infrared range, or lasers to emit very specific infrared wavelengths. In the case of broadband sources, the emitted light is optically filtered to remove many, if not all, non-infrared frequencies.

[0011] It is generally desirable to have devices, materials, and functions for converting light from one frequency range to another. Downconversion is one method of converting high-energy light to lower energy, as used in the phosphorescent materials described above. Upconversion, in which lower-energy light is converted to higher-energy light, has also been demonstrated. Typically, this process is a multiphoton absorption process, using two or more photons to promote an excited electronic state in the host medium. The host medium then emits light at a wavelength with a higher energy than the energy of the incident light that promoted the multiphoton absorption process. Both downconversion and upconversion have been studied and documented in the past.

[0012] Indeed, researchers have studied the phenomena of photoluminescence and fluorescence, which are the ability of certain solids to emit light when powered or charged by an external energy source. Many well-known phosphorescent and fluorescent materials are triggered by high-energy electrons or photons to emit lower-energy photons. Certain infrared phosphorescent materials are recognized to be able to convert infrared light into light in the visible range (violet to red).

[0013] Light properties such as radiance are particularly important for reading or display applications where the human eye must recognize and distinguish temporary or permanent images formed with visible light (e.g., as shown on road and highway signs). Televisions, computer monitors, displays, and signs use cathode ray tube (CRT) technology, in which high-energy electrons bombard a phosphorescent material that emits visible light. Televisions, computer monitors, displays, and signs have more recently used liquid crystal display or plasma display technology to produce visible images that can be distinguished by the human eye.

[0014] In these and other reading or display applications, attempts have been made to develop displays with relatively high contrast images while minimizing the amount of broadband light emitted or reflected from the display, which can detract from the contrast of the displayed image.

[0015] In general, the upconversion and downconversion discussed above have been used in many fields to convert incident wavelengths of light to different wavelengths. In one example, high-energy photons such as X-rays have been converted by absorbing the X-ray energy into a phosphorescent material, and the emission from the phosphorescent material in the ultraviolet, visible, and / or near-infrared spectrum has been used to drive photoactive reactions. In another example, infrared or near-infrared light has been upconverted by absorbing the infrared or near-infrared light into a phosphorescent material and emitting light from the phosphorescent material in the visible and / or ultraviolet spectrum. In another example, light in the visible range can be downconverted or upconverted (depending on the phosphorescent material selected) to a different band within the visible wavelength range. This shift (energy conversion) can be for color enhancement and can be used in solar cells to convert one part of the solar spectrum to another part that is more favorable for photovoltaic devices to generate electricity.

[0016] In many of these previous applications, metallic structures are placed on or near phosphorescent materials to generate a plasmonic effect, which is essentially a local field amplification very close to the outside of the metallic structure. The plasmonic effect can enhance the coupling of incident light into the phosphorescent material and / or increase the reactivity of the converted light near the receptor. While plasmons in metals can propagate along the metal, they decay evanescently in the z-direction, perpendicular to the metal / dielectric interface, with a decay length of 1 / e, on the order of half the wavelength (approximately 200 nm for wavelengths in the visible range).

[0017] Some previous applications have used photonic bandgap structures, where the material consists of a material with a periodic dielectric profile, or photonic crystal (PhC), which can prevent light of certain frequencies or wavelengths from propagating in one, two, or any number of directions within the material. In this way, light that is unsuitable or harmful to the process can be filtered out, while light that is more suitable for the process can be trapped within the photonic bandgap structure, or better confined in a photovoltaic converter.

[0018] In the field of solar cells, the addition of plasmonics, photonic band gaps, and up- and down-conversion is known in the literature. Furthermore, anti-reflection coatings and concentrators are well known in the literature.

[0019] The problem with the plasmonic effect is that, as mentioned above, the plasmon and electric field enhancement decays rapidly with distance from the metal structure, meaning that the effect is useful for only a small amount of interactions.

[0020] The problem with anti-reflective coatings is that although they do not scatter as much sunlight as they would without the coating, the transmitted light is still primarily at wavelengths that are not optimal for generating electricity.

[0021] The problem with concentrators is that in addition to concentrating light that can be converted into electricity, the concentrator also concentrates light that does not generate electricity, which generally becomes waste heat.

[0022] Photonic bandgap structures can help reflect or confine light, but there is no effective way to harvest power from the wasted light. Summary of the Invention

[0023] In one embodiment, an energy-enhancing structure is provided that is capable of capturing one or more wavelengths of electromagnetic energy and enhancing the one or more wavelengths of electromagnetic energy in at least one characteristic.

[0024] In one embodiment, the energy enhancing structure may be one or more of an electromagnetic resonator structure, a folded resonator structure, and a fractal structure having regions of enhanced electromagnetic field within the structure.

[0025] In a further embodiment, there is provided an energy collector including at least one energy-augmenting structure, and at least one energy converter capable of receiving applied electromagnetic energy, converting the applied electromagnetic energy, and emitting emitted electromagnetic energy therefrom that is shifted in wavelength or energy from the applied electromagnetic energy, wherein the energy converter is positioned proximate to the at least one energy-augmenting structure such that the emitted electromagnetic energy is emitted with at least one enhanced characteristic compared to when the energy converter is distant from the at least one energy-augmenting structure.

[0026] In one embodiment, the energy converter is arranged in an energy enhancing structure including one or more of an electromagnetic resonator structure, a folded resonator structure, and a fractal structure, any of which have regions of enhanced electromagnetic field within the resonant structure.

[0027] In one embodiment, the energy converter comprises one or more luminescent materials. As described herein, embodiments include the use of energy augmentation structures and / or energy collectors to enhance bioluminescence, chemiluminescence, photoluminescence, fluorescence, and mechanoluminescence.

[0028] In one embodiment, the energy converter includes one or more light-emitting materials, including phosphorescent, fluorescent, electroluminescent, chemiluminescent, bioluminescent, and mechanoluminescent materials, used in combination with or without the energy-augmenting structure. When used in combination with the energy-augmenting structure, the electromagnetic energy emitted from the light-emitting material is emitted with at least one enhanced characteristic compared to when the energy converter (e.g., light-emitting material) is separated from the at least one energy-augmenting structure.

[0029] In one embodiment, the energy converter includes one or more luminescent materials, such as phosphorescent materials, fluorescent materials, electroluminescent materials, chemiluminescent materials, bioluminescent materials, and mechanoluminescent materials, used with or without the energy-enhancing structure, that emit ultraviolet, visible light, near-infrared light, and infrared light. In this embodiment, UV-emitting electroluminescent or mechanoluminescent devices and materials can be used. In this embodiment, UV-emitting bioluminescent materials can be used.

[0030] In one embodiment, a color enhancement structure is provided having: a) an energy collector including at least one energy-enhancing structure; and b) an energy converter capable of converting light of a second wavelength to light of a third wavelength that is shifted in wavelength from the light of the second wavelength and emitting light of the third wavelength from the light of the second wavelength. In one embodiment, the energy converter is positioned near the at least one energy-enhancing structure such that the wavelength-shifted light is emitted with a greater intensity than if the converter were located further away from the at least one energy-enhancing structure.

[0031] In various embodiments, the color-enhancing structure comprises a portion of a paint, ink, fabric, thread, road sign, highway sign, automobile, boat, airplane, reflector, building product, concrete product, epoxy product, jewelry product, colored contact lenses, candle product, rubber product, plastic product, or other colored surface.

[0032] In another embodiment, a paint is provided that includes a pigment and a color-enhancing structure.

[0033] In another embodiment, an ink is provided that includes a dye and a color enhancing structure.

[0034] In another embodiment, a display is provided that includes a color filter or color reflective surface and a color enhancement structure.

[0035] Additional embodiments provide for the use of energy augmentation structures and energy collectors in medical procedures, solar cells, adhesives / resins, sterilization, and other end uses.

[0036] In another embodiment, the energy converter is positioned with the energy-enhancing structure such that the x-ray-induced photoluminescence or fluorescence is higher than if the energy converter (e.g., x-ray induced photoluminescent or fluorescent material) were spaced apart from the at least one energy-enhancing structure.

[0037] In another embodiment, the distributed energy collector can deliver light to different locations within a medium within a patient's body.

[0038] In another embodiment, the distributed energy collector can collect or deliver light from or to different locations within a patient, including, for example, collecting or delivering light to different locations within an organ.

[0039] In another embodiment, UV-emitting luciferases can be used alone or in combination with the energy enhancement structures described above to generate light within the patient's body.

[0040] In another embodiment, a distributed energy collector is provided having separate light-concentrating components branched together to collect sunlight for conversion to electrical power.

[0041] In another embodiment, it is provided that the above-described distributed energy collector with a separate concentrating component collects sunlight by directing the collected solar flux to a photovoltaic, thermoelectric, or thermionic emission cell.

[0042] In another embodiment, a distributed energy collector is provided that is integrated with solar power generation with a separate concentrating component within the collector to convert sunlight into electricity with the concentrating component.

[0043] In another embodiment, the distributed energy collector described above with a separate light-collecting component and / or the energy-enhancing structure described above with a region of enhanced electromagnetic field is provided so that sunlight heats the thermionic emission cell, and when the region of enhanced electromagnetic field is located near the thermionic emission cell, the enhanced electromagnetic field enhances thermionic emission.

[0044] In another embodiment, the distributed energy collectors described above can deliver light to different locations within the artificial medium for adhesive curing of the artificial medium.

[0045] In one embodiment, the energy-enhancing structures described above can be used alone to enhance the thermal cure of adhesives that are heated near the area of ​​the enhanced electromagnetic field.

[0046] In one embodiment, the energy-augmenting structure described above can be used in combination with an energy converter to promote curing of adhesives either near the region of enhanced electromagnetic field or outside the energy-augmenting structure due to their presence near the region of enhanced electromagnetic field. In the two embodiments described above, excitation of the energy-augmenting structure with an infrared laser generates the region of enhanced electromagnetic field. In embodiments with an energy converter, X-ray excitation or other high-energy sources (electrons, protons, gamma, or beta particles) can be used to stimulate light emission from the energy converter for photo-curing.

[0047] In another embodiment, the distributed energy collector described above can deliver light to different locations within the medium for sterilization of the medium.

[0048] In one embodiment, the energy-enhancing structures described above can be used alone to promote localized heating near the region of enhanced electromagnetic field.

[0049] In one embodiment, the energy-augmenting structures described above can be used in combination with an energy converter to facilitate sterilization either near the region of enhanced electromagnetic field or outside the energy-augmenting structures due to their enhanced emission from the energy converter due to their proximity to the region of enhanced electromagnetic field. In the two embodiments described above, excitation of the energy-augmenting structures with an infrared laser generates the region of enhanced electromagnetic field. In embodiments with an energy converter, x-ray excitation or other high-energy sources (electrons, protons, gamma, or beta particles) can be used to stimulate light emission from the energy converter for sterilization.

[0050] In another embodiment, there is provided an embodiment of the use of an energy-magnification structure and / or energy collector to produce a signature light emission from a surface for security applications. In one embodiment, the energy-magnification structure described above can be used in combination with an energy converter to generate emissions of different colors and intensity patterns for reading as a signature.

[0051] Another embodiment provides the use of energy enhancement structures and / or energy converters within the plasma (light emitting) capsule to facilitate the creation and maintenance of luminous plasma state ions.

[0052] In another embodiment, there is provided the use of an energy enhancement structure and / or an energy converter to enhance electron emission from a surface near the energy enhancement structure.

[0053] In one embodiment, the energy converter includes one or more electron-emitting materials. The electron-emitting material can be a photon-induced material that photoemits electrons upon exposure to UV light. The electron-emitting material can be a thermally heated material that emits electrons from a heated surface of the emitting material.

[0054] In one embodiment, the energy converter includes a nanoscale field emission tip for one or more electron emitting materials, and when used in combination with the energy enhancement structure, the electron flux emitted from the electron emitting material is higher than if the energy converter (e.g., nanoscale field emission tip) were spaced apart from the at least one energy enhancement structure.

[0055] It is to be understood that both the foregoing general description and the following detailed description of the present invention are exemplary, but are not restrictive.

[0056] A more complete understanding of the invention and many of the attendant advantages thereof will be readily obtained as the same becomes better understood by reference to the following detailed description when taken in conjunction with the accompanying drawings. [Brief explanation of the drawings]

[0057] [Figure 1] FIG. 1 is a schematic diagram illustrating an energy augmentation factor system of the present invention optionally including an energy converter. [Figure 2] FIG. 1 is a schematic diagram illustrating a folded resonator as an exemplary energy-enhancing structure of the present invention. [Figure 3] FIG. 1 illustrates a basic concept underlying one of the energy-increasing structures of the present invention. [Figure 4] 1 is a schematic diagram illustrating a staggered antenna configuration as an exemplary energy-enhancing structure of the present invention; [Figure 5] FIG. 10 is a schematic diagram illustrating the effect of electrode spacing in a folded resonator of the present invention. [Figure 6] FIG. 10 shows the spatially distributed 3 / 4λ folded resonator pattern. [Figure 7A] 1A-1C illustrate some embodiments of 3 / 4λ folded resonator patterns distributed along the surface of an object in a plane or otherwise. [Figure 7B] 1A-1C illustrate some embodiments of 3 / 4λ folded resonator patterns distributed along the surface of an object in a plane or otherwise. [Figure 7C] 1A-1C illustrate some embodiments of 3 / 4λ folded resonator patterns distributed along the surface of an object in a plane or otherwise. [Figure 8] 1-D shows patterns of 3 / 4λ folded resonators distributed along the surface of an object in a plane or otherwise, and with different orientations than those shown in FIG. 1-D. [Figure 9] FIG. 10 shows a pattern of a 3 / 4λ folded resonator having light or photon or electron emitting material deposited in the area between the opposing electrodes. [Figure 10] FIG. 10 shows a pattern of a 3 / 4λ folded resonator with patterned deposition of light or photon or electron emitting material in the area between the opposing electrodes. [Figure 11] FIG. 10 shows a pattern of a 3 / 4λ folded resonator with patterned deposition of light or photon or electron emitting material in the area between the opposing electrodes. [Figure 12] FIG. 10 shows a pattern of a 3 / 4λ folded resonator with a fractal pattern of electrical paths that loop to connect opposing electrodes due to metal traces. [Figure 13] FIG. 10 shows a fractal antenna segment where the straight sides of the metal pad have locally enhanced electric fields. [Figure 14] FIG. 14 illustrates the repeated pattern of the fractal antenna segments of FIG. 13. [Figure 15] FIG. 1 illustrates a pattern of bowtie fractal antenna segments. [Figure 16]FIG. 1 illustrates the three-dimensional fractal structure of a pair with an enhanced electric field between them. [Figure 17] FIG. 1 shows a pattern of a pair of three-dimensional fractal structures. [Figure 18] FIG. 10 shows a 3 / 4 wavelength resonator in which the distal end of the resonator antenna protrudes outward while maintaining parallelism. [Figure 19] FIG. 1 illustrates the packing configuration of three different three-quarter wavelength resonators, which are maintained in a plane with no overlapping distal ends. [Figure 20] FIG. 10 is another diagram showing the packing configuration of three different three-quarter wavelength resonators, which are maintained in a plane with their distal ends overlapping. [Figure 21] FIG. 10 is yet another diagram illustrating a packing configuration of a 3 / 4 wavelength resonator without (or deviating from) axial symmetry of the face. [Figure 22] FIG. 10 illustrates a multilevel packing configuration in parallel planes of the folded three-quarter wavelength resonator shown. [Figure 23] 23 shows a multi-level packing configuration in parallel planes, with the distal ends of the 3 / 4 wavelength resonators of FIG. 22 projecting. [Figure 24A] 1A-1C illustrate different in-plane packing configurations. [Figure 24B] FIG. 10 is another diagram illustrating a different in-plane packing configuration. [Figure 25A] 1 is a schematic diagram illustrating a distributed point concentrator / transmitter of the present invention. [Figure 25B] FIG. 25B is a schematic diagram of a cross section of the concentrator / transmitter of FIG. 25A. [Figure 26] 1A-1C are schematic diagrams showing the structure of various converters of the present invention; [Figure 27] FIG. 1 is a schematic illustration of plasmon resonance as a function of shell thickness. [Figure 28A] 10A-10C are schematic diagrams showing various other converter structures of the present invention. [Figure 28B] 10A-10C are further schematic diagrams illustrating various other converter configurations of the present invention. [Figure 28C] 1A-1D are schematic diagrams illustrating the structure of various plasmonics-active converters of the present invention. [Figure 28D] FIG. 1 is a schematic diagram of a photoactive molecule coupled to a plasmonics-active upconverter structure of the present invention. [Figure 29] 1 illustrates a mechanoluminescent emitter of the present invention; [Figure 30] FIG. 1 illustrates a composite piezoelectric / electroluminescent emitter of the present invention. [Figure 31] FIG. 31 shows the distribution of the composite emitters of FIG. 30 across a surface for light emission. [Figure 32] FIG. 31 shows the distribution of the composite emitters of FIG. 30 within a target area of ​​light emission. [Figure 33] 1 is a schematic diagram of a reflective resonator of the present invention. [Figure 34] FIG. 1 is a schematic diagram of an LED white light source with variable color temperature control. [Figure 35] 1 is a schematic diagram of an electroluminescent light source. [Figure 36] 1 is a schematic diagram of an electroluminescent light source of the present invention; [Figure 37] FIG. 1 is a schematic diagram of a compressed layer substrate configuration according to one embodiment of the present invention. [Figure 38] FIG. 38 is a schematic diagram of a coating layer formed on the compression layer substrate configuration of FIG. 37. [Figure 39] 1 is a schematic diagram of the micro-transfer printing technique of the present invention; [Figure 40] FIG. 6G is an overview of the micro-transfer printing process. [Figure 41] Schematic diagram of a micro mobile antenna on a pre-coated compressive stress glass substrate. [Figure 42] 1 is a schematic diagram showing a multi-layer structure of the present invention with an antenna (resonator) of the present invention embedded therein; [Figure 43] FIG. 1 is a schematic diagram illustrating the formation of individual microcolor enhancers of the present invention. [Figure 44] 1 is a schematic diagram of the shape of a retroreflective coating using the color-enhancing structure of the present invention. [Figure 45]1 is a schematic diagram showing the effect of the amplifier / resonator antenna of the present invention on the coating. [Figure 46] 1 is a schematic diagram of a topcoat on a painted surface including a color-enhancing structure of the present invention. [Figure 47] 1 is a schematic diagram of an electronic ink display using the color enhancement structure of the present invention; [Figure 48] FIG. 2 is another schematic diagram of an electronic ink display using the color enhancement structure of the present invention. [Figure 49] FIG. 2 is another schematic diagram of an electronic ink display using the color enhancement structure of the present invention. [Figure 50] FIG. 2 is another schematic diagram of an electronic ink display using the color enhancement structure of the present invention. [Figure 51] 1 is a schematic diagram of an IR light activated display using the color enhancement structure of the present invention. [Figure 52] FIG. 2 is another schematic diagram of an IR light activated display using the color enhancement structure of the present invention. [Figure 53] FIG. 2 is another schematic diagram of an IR light activated display using the color enhancement structure of the present invention. [Figure 54] 1 is a schematic diagram of an LCD photoactivated display in which the color filters have the color enhancement structures of the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0058] Reference will now be made in detail to several embodiments of the present invention, examples of which are illustrated in the accompanying drawings, wherein like reference characters refer to corresponding elements throughout.

[0059] As mentioned above, energy converters, such as upconversion and downconversion materials, have been used in many fields to convert incident wavelengths of light to different wavelengths. Metallic structures are placed on or near phosphorescent materials to generate a plasmonic effect, which is essentially a local field amplification in the immediate vicinity of the metallic structure. In some applications, photonic bandgap structures have been used in solar cell applications to prevent light of specific frequencies or wavelengths from propagating in one, two, or any number of directions within the material. Additionally, anti-reflective coatings and concentrators are well known in the literature.

[0060] The inventors have recognized that the shortcomings of these structures can be addressed by using the energy augmentation structures described herein, used separately or in combination with an energy converter.

[0061] A. Energy-increasing structure In the present invention, the term "energy enhancement" means causing some change in one or more wavelengths of electromagnetic energy in at least one property, including, but not limited to, intensity, power, associated electric field, associated magnetic field, wave amplitude, photonic flux, magnetic flux, phase, coherence, direction of propagation, etc. A structure that performs energy enhancement may be referred to as an "energy enhancement structure" or "energy enhancement factor." These terms are used interchangeably herein. Preferably, the energy enhancement structure is a non-plasmonic structure (a structure that does not exhibit plasmonic properties).

[0062] The energy enhancement agent can take any desired form so long as it performs the requisite function of enhancing energy applied to it and is capable of causing a change in one or more wavelengths of electromagnetic energy in at least one characteristic as described above. Examples of such energy enhancement agents include, but are not limited to, at least one non-plasmonic member selected from the group consisting of a resonator, a fractal antenna, an electrical grid pattern, an antenna, a cavity, an etalon, a nanoparticle, a microparticle, a nanostructure, and a microstructure, to name just a few.

[0063] In one embodiment, as shown generally in Figure 1, an energy enhancement factor 10 is provided that can receive or capture one or more wavelengths of electromagnetic energy representing an incident energy wave 12. Upon receiving or capturing the incident energy wave 12, the energy enhancement factor 10 can enhance one or more wavelengths of the received or captured energy wave packet 12 in at least one characteristic. As shown in Figure 1, in one embodiment, the energy enhancement factor 10 then outputs an energy wave 14 that has at least one enhanced characteristic, and the enhanced energy wave 14 is incident on a target 20. Details of the enhancement are described below.

[0064] In another embodiment, the output (amplified) energy wave 14 (i.e., one or more output wavelengths of electromagnetic energy) can be incident on an energy converter 16 (such as the upconversion and downconversion materials described above). The energy converter 16 can output photons or electrons 18 that can be directed toward a target 20. In these embodiments, the target 20 can receive the photons or electrons 18 or the output amplified energy wave 14 simultaneously or separately.

[0065] In one embodiment, the energy enhancement agent 10 may be one or more of an electromagnetic resonator structure, a folded resonator structure, and a fractal structure having regions of enhanced electromagnetic field within these structures.

[0066] FIG. 2 below illustrates a folded resonator structure 22 of the present invention.

[0067] In one embodiment of the present invention, the resonator is a curved 3 / 4λ metal structure, as shown in Figure 2, that has a "folded" configuration, forming opposing electrodes between which a strong electric field is generated. Exemplary characteristics of the "folded" antenna are listed in the following table: [Table 1]

[0068] Calculations for a theoretical 3 / 4λ and a slightly oversized antenna taking into account all the curved corners involved in creating the antenna result in this structure being 0.75 * λ and upper limit of oversize 0.78 * The size is between λ.

[0069] While the resonators shown in most of the drawings can be characterized as having a rectangular loop connecting opposing antenna sections or electrodes together, the invention is not so limited. Other "loop" shapes may be used, so long as the opposing electrodes are parallel and coplanar to one another, the loop forms an electrical path 1 / 2λ long, and the opposing electrodes are each 1 / 8λ long, thereby creating a 3 / 4λ resonator.

[0070] FIG. 3 illustrates the basic concept underlying one of the energy-enhancing structures of the present invention. The illustration in FIG. 3 shows a sine wave representing the instantaneous waveform of a light wave (incident energy flux 12), for example. The illustration shows a length λ of ¾ of a wavelength, illustrating how, in one embodiment, a ¾λ resonator is constructed, with the open ends of the resonator "folded" together to form, in this embodiment, a ¾λ folded resonator 22. As shown in FIG. 3, the folded ends create a region of enhanced, amplified electric field, indicated by the horizontal arrows between the opposing open ends. When light of nominal wavelength λ (or its harmonics 2λ, 3λ, 4λ, etc.) is folded and incident on the antenna structure, a portion of the light is coupled into the structure, establishing an amplified electric field. Because light from the sun continuously arrives at various circular polarizations, subsequent light waves continue to "pump" the electric field of the resonant structure until some "loss" mechanism limits the strength of the electric field. For resonators made of low-loss materials, a high Q factor can be obtained, which in this case can mean that the strength of the electric field between the opposing electrodes can be, for example, 100 to 1000 times the peak amplitude of the electric field vector of the incident waveform.

[0071] In another embodiment, the resonant antenna can have the following configuration shown in FIG. 4, where 3 / 4λ structures face each other and interdigitate without any "folded" structures. In the diagram of FIG. 4, the horizontal stubs are 1 / 4λ in length, the vertical extension connectors are 1 / 4 in length, and the vertical spacing between the horizontal stubs and the interdigital extension are varied as shown between Configuration 1 and Configuration 2. In one embodiment of the present invention, an energy converter, light or electron emitting material, or color emitting or color converter material (i.e., emitting material 24) is positioned within or around the region of enhanced electric field, as shown in FIG. 4.

[0072] Figure 5 shows that a variety of ¾λ folded resonators can be created with different distances between the opposing electrodes, resulting in different electric field strengths. In this way, the folded resonators of the present invention can be tailored so that the electric field strength between the opposing electrodes does not exceed the dielectric strength of any material between them. Exceeding the dielectric strength of any material between them can lead to destruction of that material, as a strong current (such as a micro-arc) will flow and destroy the material whenever the dielectric strength is exceeded. As shown, the opposing sides do not need to be exactly ⅛λ long.

[0073] In one embodiment of the present invention, an energy converter, light or electron emitting material, or color emitting or color converter material (i.e., emitting material) 24 is disposed within or around the region of enhanced electric field in the vicinity of / between the opposing electrodes. In one embodiment of the present invention, the color emitting or color converter material may itself absorb light of a certain color, such as blue light, and emit a lower energy, downshifted red light. In this case, a red phosphorescent material may be the color emitting or color converter material.

[0074] In one embodiment, a 3 / 4λ folded resonator can be designed to resonate with blue light (λ=420-440 nm), preferably at a different frequency than the blue light absorbed by the red phosphorescent material. In one embodiment, to enhance the color of an object in sunlight, a 3 / 4λ folded resonator can be designed to generate an enhanced electric field driven by infrared light from the solar spectrum (e.g., λ=700-1000 nm), such that a red phosphorescent material placed in the region of the enhanced electric field will have a brighter red emission than if the enhanced electric field were not present.

[0075] FIG. 6 illustrates a pattern of spatially distributed 3 / 4λ folded resonators 22. As will be discussed in more detail later, there are many ways to distribute the 3 / 4λ folded resonators. The present invention is not limited to the regularly spaced and uniformly sized resonators shown in FIG. 6. The distribution need not be regular, uniformly spaced, uniformly sized, or uniformly oriented. Resonators of different sizes, spacings, and orientations may result in better utilization of the full spectrum of the sun or any other light source incident on the object.

[0076] FIG. 7A illustrates a pattern of 3 / 4λ folded resonators 22 distributed along the surface of an object, in a plane or otherwise. In one embodiment, this pattern can be formed by a lithography or stamping process on a flat or curved sheet-type product, such as a glass plate. In one embodiment, the glass plate can itself be a phosphorescent plate, or it can have sections of different phosphorescent materials deposited in a pattern that aligns / matches the respective positions of the opposing electrodes of each resonator. In one embodiment, the sheet-type product can be a laminate-type product applied to a nominally white object, for example. When illuminated by the sun, the infrared portion of the solar spectrum (which normally only heats the surface) generates regions of enhanced electric field. In these regions, downconverting phosphors that convert deep blue and ultraviolet light from the solar spectrum to visible light converts the deep blue and ultraviolet light of the solar spectrum to visible light, and the enhanced electric field enhances the greater emission of visible light.

[0077] In one embodiment, the energy enhancement agent can be disposed on a perforated sheet, as shown in Figure 7B. The perforations in one embodiment are in regions of enhanced electric field so that phosphorescent or other energy conversion materials or devices can be placed in the perforations.

[0078] In one embodiment (for color enhancement), the sheet product can be a laminate-type product applied to, for example, a nominally green object. When illuminated by the sun, the infrared portion of the solar spectrum (which normally only heats surfaces) generates regions of enhanced electric field. In these regions, downconverting phosphors that convert blue, deep blue, and ultraviolet light from the solar spectrum into green light convert the blue, deep blue, and ultraviolet light from the solar spectrum into green light, and the enhanced electric field enhances the greater emission of green light.

[0079] In one embodiment, the sheet product can be a laminate-type product, for example, applied to a nominally red object. When illuminated by the sun, the infrared portion of the solar spectrum (which normally only heats the surface) generates regions of enhanced electric field. In these regions, downconverting phosphors that convert green, blue, deep blue, and ultraviolet light from the solar spectrum into red light convert the green, blue, deep blue, and ultraviolet light from the solar spectrum into red light, and the enhanced electric field enhances greater emission of red light.

[0080] In one embodiment, the energy-enhancing agent may be disposed on a sheet, as shown in FIG. 7C, and then separated into discrete pieces, which may be easily added and mixed into the medium to be treated.

[0081] Figure 8 shows a pattern of 3 / 4λ folded resonators 22 distributed in a plane or otherwise along the surface of an object, with a different orientation than that shown in Figure 7. By having a different orientation, the rotating polarized solar waves may not have the electric field alignment that helps drive the 3 / 4λ folded resonators, but rather have the electric field alignment that helps drive the resonators in a different direction, and therefore are better aligned. Thus, when using a sheet-type product, layers of 3 / 4λ folded resonators with different orientations can be stacked together.

[0082] 9 illustrates a pattern of a 3 / 4λ folded resonator 22 having an energy converter, light- or electron-emitting material, or color-emitting or color converter material (i.e., emissive material 24) deposited in the region between the opposing electrodes. While shown here in plan view, the color conversion or enhancement material deposited in the region between the opposing electrodes can be deposited such that the color conversion or enhancement material has a raised top surface above the metal traces of the 3 / 4λ folded resonator. In this embodiment, the raised section provides field breakage for the fringing of the enhanced electric field between the opposing electrodes.

[0083] FIG. 10 illustrates a pattern of a 3 / 4λ folded resonator 22 having an energy converter, light- or electron-emitting material, or color-emitting or color converter material (i.e., emissive material 24) deposited in the region between the opposing electrodes. Here, as before, the color conversion or enhancement material deposited in the region between the opposing electrodes can be deposited such that the color conversion or enhancement material has a raised top surface above the metal traces of the 3 / 4λ folded resonator. In this embodiment, the raised sections block fringing fields of the enhanced electric field between the opposing electrodes. In this embodiment, the raised sections extend around corners where geometric corners further enhance the electric field.

[0084] FIG. 11 illustrates a pattern of a 3 / 4λ folded resonator 22 having an energy converter, light- or electron-emitting material, or color-emitting or color converter material (i.e., emissive material 24) deposited in the region between the opposing electrodes. Here, as before, the color conversion or enhancement material deposited in the region between the opposing electrodes can be deposited such that the color conversion or enhancement material has a raised top surface above the metal traces of the 3 / 4λ folded resonator. In this embodiment, the raised sections block fringing fields of the enhanced electric field between the opposing electrodes. In this embodiment, the raised sections extend around the corners and around the edges of the opposing electrodes, where geometric corners further enhance the electric field.

[0085] In these embodiments shown in Figures 9, 10, and 11, the energy converter, or light- or electron-emitting material, or color-emitting or color converter material (i.e., emissive material 24) is positioned near one or more energy-augmenting structures (i.e., 3 / 4λ folded resonators). Therefore, the energy-augmenting structures are preferably in a region of enhanced electric field. Enhanced electric fields can represent regions of enhanced energy, especially when a current flows that conductively couples the energy converter to one of the energy-augmenting structures. In the latter embodiment, conductively coupling the energy converter to one of the energy-augmenting structures can be advantageous. Therefore, an energy converter or color conversion or enhancement material positioned near one or more energy-augmenting structures can have a physical conductive connection between the energy converter and at least one of the energy-augmenting structures. Alternatively, the coupling can be radiative or capacitive coupling of the electric field from the resonant structure to the energy converter, or more than coupling of a color conversion or enhancement material positioned inside the energy-augmenting structure, outside the energy-augmenting structure, in a layer with the energy-augmenting structure, or in a layer above or below the energy-augmenting structure.

[0086] As used herein, near refers to the placement of one thing inside, outside, and near or adjacent to another structure, and can include the placement of one thing above or below another in any three-dimensional direction. Thus, in one embodiment of the present invention, the color conversion or enhancement material is placed near the energy-enhancing structure.

[0087] 12 shows a pattern for a 3 / 4λ folded resonator 30 with a fractal pattern of electrical paths that loop to connect opposing electrodes due to the metal trace. The fractal pattern of electrical paths in this pattern means that the metal trace can support a variety of wavelengths that are resonant with the 3 / 4λ characteristic due to the large number of loop paths available, as the width of each conductive path segment varies to allow electrical paths of various physical lengths to exist around the loop.

[0088] 13 illustrates another fractal antenna segment 32 in which the straight sides of the metal pad have regions 24 of locally enhanced electric field. Here, in one embodiment, the fractal antenna segment is designed for resonance in the infrared range, resulting in enhanced electric field regions 34 (e.g., as shown, toward the straight sides of the metal pad where blue and red phosphors (or other emitting materials 24) are deposited such that their emission enhances the enhanced electric field in those regions 34).

[0089] FIG. 14 is a diagram illustrating a repeated pattern (array) of the fractal antenna segments 32 of FIG.

[0090] FIG. 15 is a diagram illustrating a pattern (array) of bowtie fractal antenna segments, providing an alternative embodiment to the fractal antenna segments of FIG.

[0091] In one embodiment of the present invention, the resonant structure can include a three-dimensional fractal pattern. Fabrication of three-dimensional fractal structures by nanoscale anisotropic etching of silicon is known in the art, as described, for example, in “Nanoscale etching of 3d fractal structures with many applications including 3d fractal antennas and structures for filters” by Brian Wang, in the Journal of Micromechanics and Microengineering, June 23, 2013, available at www.nextbigfuture.com / 2013 / 06 / nanoscale-etching-of-3d-fractal.html, the entire contents of which are incorporated herein by reference. In one embodiment of the present invention, metal is deposited on the three-dimensional fractal structure of silicon to form a multidimensional light concentrator.

[0092] 16 is a diagram illustrating paired three-dimensional fractal structures with regions 34 of enhanced electric field between the pairs. The paired three-dimensional fractal structures are color-enhancing structures according to one embodiment of the present invention. In one embodiment of the present invention, these pyramidal structures are metallized on opposing faces, with a first loop conductor formed around the other side of the first pyramid, then connecting across the region between the pair, and then a second loop formed around the side of the second pyramid to the metallized opposite face of the second pyramid, mimicking the 3 / 4λ folded resonator shown in FIG. 3 (as viewed from above).

[0093] In one embodiment, converter (emissive) material 24 is placed near different sections of the pyramidal structure, preferably between pairs of opposing faces where enhanced electric fields exist (indicated by arrows). The three-dimensional aspect of the invention allows red, yellow, green, and blue converters (or other designated emitters) to be placed at different levels within this region of enhanced electric field.

[0094] FIG. 17 is a diagram showing a pattern (array) of the pair of three-dimensional fractal structures shown in FIG.

[0095] In these embodiments shown in Figures 12-17, the energy converter, or light- or electron-emitting material, or color-emitting or color-converter material (i.e., emitting material 24) is positioned near one or more energy-augmenting structures (i.e., 3 / 4λ folded resonators). Therefore, the energy-augmenting structures are preferably in a region of enhanced electric field. Enhanced electric fields can represent regions of enhanced energy, particularly when a current flows that conductively couples the energy converter to one of the energy-augmenting structures. In the latter embodiments, conductively coupling the energy converter to one of the energy-augmenting structures can be advantageous. Therefore, an energy converter, or light- or electron-emitting material, or color-emitting or color-converter material positioned near one or more energy-augmenting structures can have a physical conductive connection between the energy converter and at least one of the energy-augmenting structures. Alternatively, the coupling can be more than radiative coupling of the electric field from the resonant structure to the energy converter, or coupling of a color-conversion or enhancement material positioned inside the energy-augmenting structure, outside the energy-augmenting structure, in a layer with the energy-augmenting structure, or in a layer above or below the energy-augmenting structure.

[0096] The energy-enhancing structure is not limited to those shown above. Other variations are possible. Furthermore, in one embodiment of the present invention, the 3 / 4λ folded resonator need not have an inwardly folded "folded section" as shown in FIG. 3. Instead, as shown in FIG. 18, the 3 / 4λ folded resonator of the present invention can have an outwardly folded folded section with a region of enhanced electric field outside the resonator "loop." The distal end of the antenna projects outward while maintaining parallelism. Specifically, FIG. 8 is a schematic diagram of a 3 / 4λ external electrode-folded resonator 22. This external opposing electrode pair design follows the general distribution, scaling aspects, converter material placement, etc. shown in FIGS. 5-11, but the internal folded section is replaced with an external electrode pair.

[0097] In one embodiment of the present invention, the 3 / 4λ external electrode folded resonators 22 are capable of being packed into a concentric arrangement with resonators of gradually increasing or decreasing size. These resonators are maintained in a plane so that their distal ends do not overlap. Figure 19 is a schematic diagram of multiple concentric 3 / 4λ external electrode folded resonators 22. Because each of the 3 / 4λ external electrode folded resonators 22 has a different electrical length, the multiple concentric 3 / 4λ external electrode resonators are "tuned" to different wavelengths associated with their respective electrical lengths. Thus, three different frequencies are focused between the distal ends of the antenna.

[0098] In another embodiment, Figure 20 is a schematic diagram of multiple concentric 3 / 4λ outer electrode folded resonators 22 with overlapping electrodes. In one embodiment, the overlap provides a more concentrated / enhanced field region than the non-overlapping arrangement of Figure 19.

[0099] The present invention is not limited to planar concentric packing arrangements such as those shown in FIGS. 19 or 20. The three different ¾-wavelength resonators in FIG. 20 are maintained in a plane with their distal ends overlapping. These antennas are inductively coupled. In one embodiment, the present invention utilizes an axisymmetric, off-plane configuration in which the antennas are in an axially rotated, multi-frequency, interleaved ¾-wave resonator structure. FIG. 21 is a schematic diagram of an axially rotated, multi-frequency, interleaved ¾-wave resonator 22, showing three differently sized resonators (in this example) for axially rotating, multi-frequency resonance, arranged around / along a common axis. In one embodiment, in this configuration, the resulting electric field is concentrated without one electrode section perturbing the field from another.

[0100] In a further embodiment, there is provided an energy collector including at least one energy-augmenting structure and at least one energy converter capable of receiving applied electromagnetic energy, converting the applied electromagnetic energy, and emitting emitted electromagnetic energy therefrom that is shifted in wavelength or energy from the applied electromagnetic energy, wherein the energy converter is positioned proximate to the at least one energy-augmenting structure such that the emitted electromagnetic energy is emitted with at least one enhanced characteristic compared to when the energy converter is distant from the at least one energy-augmenting structure.

[0101] In one embodiment, the present invention can use different levels to place a 3 / 4λ resonator on, whether the resonator is a 3 / 4λ internal folded resonator or a 3 / 4λ external electrode resonator. This packing is shown in Figures 22 and 23 for configurations in parallel planes with the distal ends folded or protruding, respectively.

[0102] In the embodiment of the invention shown in Figure 20 with multiple concentric 3 / 4λ external electrode resonators 22, the antenna is inductively separated. This configuration allows the electric fields from three different frequencies to be focused onto a longer path. This configuration can be used to create a mirror image configuration to extend the length of the focused field, as shown in Figure 24A.

[0103] The resonator configuration in this case is mirrored with another set of antennas (folded resonators 22) to create a longer path (doubled) of the focused electric field. Additionally, the resonator antenna configuration can be arranged in more creative ways to enhance the field that focuses around the target, as shown in Figure 24B.

[0104] The configuration of Figure 25 allows the target to be enclosed within the plane of the resonator structure / antenna in order to heat and concentrate the energy around the target, thereby preventing heat dissipation in silicon, which has a high thermal conductivity. The silicon substrate in such cases can be monocrystalline, polycrystalline, or amorphous.

[0105] In one embodiment of the present invention, an "energy-enhancing structure" refers to a structure containing a converter material (or other light- or electron-emitting material) exposed to energy that stimulates light emission at a different energy (wavelength) than that exposed while in a spatial region / volume (e.g., between or around or near a folded structure or an external electrode pair) where a spatial region of the energy collector has an artificially induced higher electric field and / or higher energy density. These artificial regions can be created, for example, by using structures including, but not limited to, multi-level collecting optics, resonators, fractal antennas, and electrical grid (or electrode) patterns.

[0106] By placing a light- or electron-emitting material near the energy-augmenting structures of the present invention, whether the energy-augmenting structures are within a region of enhanced electric field or are otherwise outside of the region of enhanced electric field, the energy-augmenting structures of the present invention can generate light that can be used for a variety of applications, particularly for photostimulation of biological, chemical, and physical reactions, such as, for example, photoactivation of photoreactive drugs, photoactivation of photosensitive materials such as adhesives or lithographic photoresists, or for direct interaction with biological and chemical agents in the environment of the augmenting structure, as in sterilization.

[0107] In one embodiment, the light or electron emitting materials are arranged in an energy enhancing structure including one or more of an electromagnetic resonator structure, a folded resonator structure, and a fractal resonator structure, any of which have regions of enhanced electromagnetic field within the resonant structure.

[0108] In one embodiment, the energy converter or light or electron emitting material comprises one or more luminescent materials. As described herein, embodiments include the use of energy augmentation structures and / or energy collectors to enhance bioluminescence, chemiluminescence, photoluminescence, fluorescence, mechanoluminescence, and / or electron emission.

[0109] In one embodiment, the energy converter or light emitting material includes one or more light emitting materials, including phosphorescent materials, fluorescent materials, electroluminescent materials, chemiluminescent materials, bioluminescent materials, and mechanoluminescent materials used in combination with or without the energy-augmenting structure. When used in combination with the energy-augmenting structure, the electromagnetic energy emitted from the light emitting material is emitted with at least one enhanced characteristic compared to when the energy converter (e.g., light emitting material) is separated from the at least one energy-augmenting structure.

[0110] In one embodiment, the bioluminescent material is a UV-emitting bioluminescent material such as a catalytic luciferase and a light-emitting protein.

[0111] In one embodiment, the energy converter or light-emitting material includes one or more light-emitting materials, such as phosphorescent materials, fluorescent materials, electroluminescent materials, chemiluminescent materials, bioluminescent materials, and mechanoluminescent materials, used in combination with or without the energy-enhancing structure, which emit ultraviolet, visible light, near-infrared, and infrared light. In this embodiment, UV-emitting electroluminescent or mechanoluminescent devices and materials can be used. In this embodiment, UV-emitting bioluminescent materials can be used.

[0112] In some embodiments, the metal pattern forms a folded resonator having opposing electrodes with an electric field directed therebetween, and the converter is positioned between the opposing electrodes, within the fringe electric field of the opposing electrodes, or near the opposing electrodes. In one example, the folded resonator is a ¾λ folded resonator. In one example, the metal pattern includes at least one of Au, Ag, Cu, Al, or a transparent metal oxide. In another example, the metal pattern can be formed of a difficult-to-process metal such as Ti, W, and Mo.

[0113] In some embodiments, the metal pattern includes a pair of external electrodes with opposing electrodes having an electric field oriented between them, and the converter is disposed between the opposing electrodes, within the fringe electric field of the opposing electrodes, or near the opposing electrodes. In one example, the resonator is a 3 / 4λ external electrode pair resonator. In one example, the metal pattern includes at least one of Au, Ag, Cu, Al, or a transparent metal oxide. In another example, the metal pattern can be formed of a refractory metal such as Ti, W, or Mo.

[0114] In some embodiments, multiple resonators and multiple converters are positioned at multiple locations throughout the concentrator, hi one example, the multiple converters are positioned to convert light that is internally scattered within the concentrator.

[0115] In some embodiments of the energy-augmenting structure, the first level metal pattern (or second level metal pattern) comprises a metal core clad with a high-K dielectric followed by a cladding of a low-K dielectric. In some embodiments of the energy-augmenting structure, the first level metal pattern (or second level metal pattern) comprises a radial pattern of conductors. In some embodiments of the energy-augmenting structure, the first level metal pattern (or second level metal pattern) comprises a fractal pattern. In one example, the fractal pattern is embedded within a dielectric material.

[0116] In some embodiments of the energy increasing structure, the first level metal pattern (or second level metal pattern) comprises a three-dimensional fractal structure.

[0117] In some embodiments of the energy augmentation structure, a panel is provided that includes a first level metal pattern and a second level metal pattern, and optionally a plurality of converters formed therein or thereon. In some embodiments of the augmentation structure, a sheet is provided that includes a first level metal pattern and a second level metal pattern, and optionally a plurality of converters formed therein or thereon.

[0118] In some embodiments of the energy enhancement structure, the first level metal patterns (or second level metal patterns) are of different sizes and / or orientations relative to each other or to the second level metal patterns.

[0119] In another embodiment, the energy enhancement agent can collect or distribute light.

[0120] Figure 25A is a schematic diagram illustrating a dispersing point collector / transmitter of the present invention. It shows a distribution of branches that can collect light from dispersing points 710, or conversely, distribute light from a central light source 766 to dispersing points 710. A section of the collector / transmitter is shown in Figure 25B, showing the core metal, optional light converter material, high-K dielectric, and low-K dielectric. In this arrangement, as shown, light is confined and not lost to scattering from the collector / transmitter except at the ends.

[0121] B. Energy Converter In various embodiments of the present invention, the energy converter can be used with or without the energy augmentation factor described above. In some embodiments, the converter is for upconversion of light, e.g., from the IR range to visible electromagnetic radiation, and downconversion of light, e.g., from the UV range to visible electromagnetic radiation. In various embodiments, the present invention upconverts energy, preferably light in the visible spectrum. The present invention encompasses a variety of applications involving up- and downconversion materials with or without an energy augmentation factor to enhance electromagnetic energy emission, preferably light or photon emission. When an energy augmentation factor is present, it may be separate from or connected to the energy converter. In certain embodiments, the energy converter can have an energy augmentation factor formed on its surface by a chemical vapor deposition ("CVD") or physical vapor deposition ("PVD") process or other nanoscale "printing" method. Such embodiments may be particularly useful in methods for treating human or animal patients, where "imprinting" such an energy augmentation factor on the surface of the energy converter can ensure close proximity between the energy augmentation factor and the energy converter, maximizing interaction with the applied energy. Alternatively, the energy-enhancement factor can be formed on the surface of an inert, non-energy-transducing particle, such as formed from silica, or formed from a non-energy-transducing particle coated with a biologically and / or chemically inert coating (e.g., diamond, diamond-like carbon, or similar inert material). Such an energy-enhancement factor can then be co-administered to a human or animal patient along with an energy converter.

[0122] Suitable energy modulation agents or energy converters (the two terms are used interchangeably herein) of the present invention include, but are not limited to, biocompatible fluorescent metal nanoparticles, fluorescent dye molecules, gold nanoparticles, water-soluble quantum dots encapsulated by polyamidoamine dendrimers, luciferase (bioluminescence), biocompatible phosphorescent molecules, complex electromagnetic energy harvester molecules, and lanthanide chelates capable of intense light emission.

[0123] Alternatively, the energy modulation agent or energy converter can emit energy in a form suitable for absorption by the target site or receptor.For example, the initiation energy source can be acoustic energy, and one energy converter can receive acoustic energy and emit photon energy (e.g., sonoluminescent molecules) that can be received by another energy converter that can receive photon energy.Other examples include energy converters that receive energy at X-ray wavelengths and emit energy at UV wavelengths, preferably UV-A wavelengths.Multiple such energy converters can be used to form a cascade, transferring energy from the initiation energy source through a series of energy converters.

[0124] Resonance energy transfer (RET) is an energy transfer mechanism between two molecules with overlapping emission and absorption bands. An electromagnetic emitter can convert the incoming wavelength to a longer wavelength. For example, UV-B energy absorbed by a first molecule can be transferred to a UV-A-emitting molecule in close proximity to the UV-B-absorbing molecule via dipole-dipole interactions. Alternatively, materials that absorb shorter wavelengths can be selected to provide RET to a non-emitting molecule with an absorption band that overlaps the emission band of the transferring molecule. Alternatively, phosphorescence, chemiluminescence, or bioluminescence can be used to transfer energy to a targeting moiety or receptor, such as a photoactivator.

[0125] In a further embodiment, a biocompatible light emitting source, such as a fluorescent metal nanoparticle or a fluorescent dye molecule, is selected as the energy converter that emits light in the UV-A band. In another embodiment, the energy converter comprising the UV-A emitter can be a gold nanoparticle comprising, for example, a cluster of five gold atoms.

[0126] In another embodiment, an energy converter containing a UV- or luminescent luciferase is selected as the emission source. The luciferase can be combined with ATP or another molecule, then oxygenated with additional molecules to stimulate light emission at the desired wavelength. Alternatively, a phosphorescent source can be used as the energy converter. One advantage of phosphorescent sources is that the phosphorescent molecule or other source can be electrically or photoactivated before being inserted into the tumor, either by systemic administration or direct insertion into the tumor area. Because triplet state relaxation is subject to forbidden energy state transitions and there are a limited number of quantum mechanical energy transfer processes available to store energy in the excited triplet state and return to a lower energy state, phosphorescent materials can have longer relaxation times than fluorescent materials. Energy release can be delayed or extended from a fraction of a second to several hours. Because the energy released during phosphorescent relaxation is otherwise no different from fluorescence, the wavelength range can be selected by choosing a specific phosphorescent material.

[0127] In one embodiment, the energy converter of the present invention can include a persistent afterglow phosphorescent material that emits light in the visible to near-UV and UV ranges. In one embodiment, Eu-doped strontium aluminate is used as the energy converter so that deep UV, X-rays, or electron beams can "charge" the photoluminescence, e.g., external to the patient, and then UV photons can be emitted or injected into the target area. In another embodiment, gadolinium strontium magnesium aluminate is used so that deep UV, X-rays, or electron beams can "charge" the photoluminescence, e.g., external to the patient, and then UV photons can be emitted or injected into the target area. U.S. Patent Application Publication No. 20070221883 (the entire contents of which are incorporated herein by reference) specifically describes gadolinium-activated strontium magnesium aluminate, which has an excitation maximum at about 172 nm and emits a narrowband UV emission at about 310 nm. The '883 publication also describes another useful energy converter for the present invention, Sr(Al,Mg) 12 O 19 : Emission spectra between 300 nm and 320 nm for Gd phosphorescent materials and YMgB5O 10 :Gd, Ce and YMgB5O 10: Two 312 nm lines are mentioned for Gd, Ce, and Pr phosphorescent materials. WO2016200349 (the entire contents of which are incorporated herein by reference) describes long-lasting yellowish green-emitting phosphorescent pigments in a strontium aluminate (SrAl2O4) system that can function as energy converters in the present invention. WO2016200348 (the entire contents of which are incorporated herein by reference) describes long-lasting bluish green-emitting phosphorescent pigments in a strontium aluminate (Sr4Al14O25) system that can function as energy converters in the present invention. Xiong et al., "Recent advances in ultraviolet persistent phosphors," Optical Materials X2 (2019) (the entire contents of which are incorporated herein by reference) describes several ultraviolet persistent phosphorescent materials that may be used as energy converters in the present invention. The following table lists such persistent phosphorescent materials. [ka]

[0128] In one embodiment, CaAl2O4:Ce has an emission peak at 400 nm and a duration of 10 hours or more. 3+ For example, a phosphorescent material such as that described by Xiong et al. can be used, which is charged by X-ray irradiation outside the patient's body and then injected into the affected area to provide endogenously generated UV light.

[0129] In one embodiment, the described long-lasting phosphorescent materials can be activated ex vivo and introduced into a patient along with a psoralen (or other photoactivatable drug) by exchange of bodily fluids or, for example, by delivering the long-lasting phosphorescent material and photoactivatable drug into the patient's bloodstream.

[0130] In one embodiment, the described long-lasting phosphorescent materials can be activated in vivo by injecting the phosphorescent material into the affected area and then exposing it to X-rays.

[0131] In another embodiment, composite electromagnetic energy harvester molecules have been designed, such as the composite light harvester described in J. Am. Chem. Soc. 2005, 127, 9760-9768, the entire contents of which are incorporated herein by reference. By combining groups of fluorescent molecules within a molecular structure, a resonance energy transfer cascade can be used to harvest broadband electromagnetic radiation and result in the emission of narrowband fluorescent energy. In another embodiment, the Stokes shift of a cascaded source or series of sources can be selected to convert shorter wavelength energy, such as X-rays, into longer wavelength fluorescent emission, such as optical or UV-A.

[0132] In one embodiment, a lanthanide chelate capable of intense luminescence is used as the energy converter, hi another embodiment, a biocompatible endogenous fluorophore emitter is selected as the energy converter.

[0133] In one embodiment, the energy converter of the present invention can include a bioluminescent material that emits visible and UV light. In one embodiment, bioluminescent materials such as coelenterate luciferin analogs can be used, including amide monoanions, which are known to emit at 480 nm, and oxyluciferins, which are known to emit at 395 nm.

[0134] Among various materials, luminescent nanoparticles have attracted increasing technological and industrial interest. In the context of the present invention, nanoparticles refer to particles having a size of less than 1 micron. Although the description of the present invention describes a specific example using nanoparticles, the present invention in many embodiments is not limited to particles having a size of less than 1 micron. However, in many embodiments, the size range of less than 1 micron, particularly less than 100 nm, produces properties of special interest, such as emission lifetime, luminescence quenching, luminescence quantum efficiency, and concentrated quenching, for example, diffusion, penetration, and dispersion into media where larger particles do not move.

[0135] The present invention in various embodiments can use a wide variety of downconversion materials (or mixtures of downconversion materials), with or without energy enhancement factors, to enhance light or photon emission. These downconversion materials include quantum dots, semiconductor materials, alloys of semiconductor materials, scintillation and phosphorescent materials, materials exhibiting X-ray excited luminescence (XEOL), organic solids, metal complexes, inorganic solids, crystals, rare earth materials (lanthanides), polymers, scintillators, phosphorescent materials, and materials exhibiting excitation properties. Thus, downconversion materials for enhancing light or photon emission can convert energy from one of ultraviolet light, X-rays, and high-energy particles to visible light. Downconversion materials for enhancing light or photon emission can convert energy from higher-energy visible light to lower-energy visible light.

[0136] In one embodiment of the present invention, quantum dot mixtures with or without energy enhancement factors can be used in multiple nanoparticles. Quantum dots are generally nanometer-sized particles, and the energy state of the quantum dot material depends on the size of the quantum dot. For example, quantum dots are known to be semiconductors whose conductive properties are closely related to the size and shape of the individual crystals. Generally, the smaller the crystal size, the larger the band gap, and the greater the energy difference between the highest valence band and the lowest conduction band. Therefore, more energy is required to excite the dot, and at the same time, more energy is released when the crystal returns to its resting state. In fluorescent dye applications, this equates to a higher frequency of light emitted after excitation of the dot as the crystal size decreases, resulting in a color shift from red to blue. Quantum dots represent one way to downconvert ultraviolet light in the spectrum to a targeted wavelength or energy emission. Quantum dots represent one way to downconvert blue light in the spectrum to a targeted wavelength or energy emission.

[0137] As described in U.S. Patent No. 6,744,960 (the entire contents of which are incorporated by reference), quantum dots of different sizes produce emissions of different colors. In that work, quantum dots applicable to the present invention can comprise a variety of materials, including semiconductors such as zinc selenide (ZnSe), cadmium selenide (CdSe), cadmium sulfide (CdS), indium arsenide (InAs), and indium phosphide (InP). Another suitable material is titanium dioxide (TiO2). The size of the particles, i.e., quantum dots 18, can range from approximately 2 to 10 nm. Because the size of these particles is so small, quantum physics applies to many of the electrical and optical properties of quantum dots. One such result of applying quantum mechanics to quantum dots 18 is that quantum dots absorb a wide spectrum of light wavelengths and re-emit radiation with wavelengths longer than the wavelength of the absorbed light. The wavelength of the emitted light is determined by the size of the quantum dot. For example, a 5.0 nm diameter CdSe quantum dot emits radiation with a narrow spectral distribution centered at approximately 625 nm, while a 2.2 nm sized CdSe quantum dot 18 emits light with a central wavelength of approximately 500 nm. Semiconductor quantum dots including CdSe, InP, and InAs can emit radiation with central wavelengths ranging from 400 nm to approximately 1.5 μm. Titanium dioxide (TiO2) also emits in this range. The linewidth, or full width at half maximum (FWHM), of the emission of these semiconductor materials can range from approximately 20 to 30 nm. To produce this narrowband emission, the quantum dot simply needs to absorb light with a wavelength shorter than the wavelength of the light emitted by the dot. For example, for a 5.0 nm diameter, light from a CdSe quantum dot with a wavelength shorter than about 625 nm will be absorbed and produce an emission at about 625 nm, while a 2.2 nm quantum dot containing CdSe light with a wavelength shorter than about 500 nm will be absorbed and re-emitted at about 500 nm, although in practice the excitation or pump radiation will be at least about 50 nanometers shorter than the emitted radiation.

[0138] Specifically, in one embodiment of the present invention, quantum dot mixture (QDM) coatings can be deposited using sol-gel techniques using CVD and / or standard precipitation techniques. QDM coatings can be made with silicate structures that do not degrade UV output. Within the silicate family, silica (SiO2) is suitable for maximizing UV transmission through the coating. The coating can further include a second layer of a biocompatible glass. Such biocompatible glass and glass-ceramic compositions can include calcium, lanthanides or yttrium, silicon, phosphorus, and oxygen. Other biocompatible materials and techniques are described in the following patents, which are incorporated herein in their entireties: U.S. Patent Nos. 5,034,353, 4,786,617, 3,981,736, 3,922,155, 4,120,730, and U.S. Patent Application Publication Nos. 2008 / 0057096, 2006 / 0275368, and 2010 / 0023101.

[0139] Furthermore, the down-conversion materials of the present invention described herein can be coated with an insulating material, such as silica, which reduces the possibility of any chemical interaction between the light-emitting particles and the medium in which they are contained. These and other conversion materials described herein can be used with or without an energy enhancement factor. One of the major limiting factors for biocompatible applications of inorganic nanoparticles is their toxicity. Generally speaking, all semiconductor nanoparticles are toxic to a greater or lesser extent. For biocompatible applications, nanoparticles with as low toxicity as possible are desirable. Otherwise, the nanoparticles must remain isolated from the medium. Pure TiO2, ZnO, and Fe2O3 are biocompatible. ZnS, CAS, BaS, SrS, and Y2O3 have low toxicity, while CdTe and CdSe are toxic. Furthermore, the toxicity of nanoparticles can be reduced by adding inorganic stabilizers such as TGA or Eu 2+ , Cr 3+ or Nd 3+ Another suitable down-conversion material that is likely to be the most biocompatible is zinc sulfide, ZnS:Mn2+ , iron oxide, titanium oxide, zinc oxide, zinc oxide with small amounts of Al2O3, and AgI nanoclusters encapsulated in zeolites. For non-medical applications where toxicity may not be a significant concern, the following materials (and those listed elsewhere) may be suitable: thulium-activated lanthanum and gadolinium oxyhalides; Er 3+ Doped BaTiO3 nanoparticles, Yb 3+ Doped CsMnCl3 and RbMnCl3, BaFBr:Eu 2+ nanoparticles, cesium iodide, bismuth germanate, cadmium tungstate, and divalent Eu-doped CsBr.

[0140] In various embodiments of the present invention, the following light-emitting polymers, with or without energy enhancement factors, are also suitable as conversion materials: poly(phenylene ethynylene), poly(phenylene vinylene), poly(p-phenylene), poly(thiophene), poly(pyridyl vinylene), poly(pyrrole), poly(acetylene), poly(vinyl carbazole), poly(fluorene), etc., as well as copolymers and / or derivatives thereof.

[0141] In various embodiments of the present invention, the following materials, with or without energy enhancement factors, can be used similarly to those detailed in U.S. Patent No. 7,090,355, the entire contents of which are incorporated herein by reference. The following materials can be used for downconversion: inorganic or ceramic phosphors or nanoparticles, including, but not limited to, metal oxides, metal halides, metal chalcogenides (e.g., metal sulfides), or hybrids thereof, such as metal oxohalides and metal oxochalcogenides; laser dyes and organic small molecules, and fluorescent organic polymers; semiconductor nanoparticles, such as semiconductors of II-VI or III-V compounds, e.g., fluorescent quantum dots; organometallic molecules, e.g., metal centers, such as at least rare earth elements (e.g., Eu, Tb, Ce, Er, Tm, Pr, Ho), transition metal elements, such as Cr, Mn, Zn, Ir, Ru, V, and main group elements, such as B, Al, and Ga. The metal elements are chemically bound to organic groups to prevent fluorescence quenching from the host or solvent. Phosphorescent materials can be used, including garnet series phosphorescent materials: Ce-doped (Y m A 1-m )3(Al n B 1-n )5O 12 , where 0≦m, n≦1, where A includes other rare earth elements and B includes B and Ga. Furthermore, phosphorescent materials containing metal silicate, metal borate, metal phosphate, and metal aluminate hosts can be used. Furthermore, nanoparticle phosphorescent materials containing common rare earth elements (e.g., Eu, Tb, Ce, Dy, Er, Pr, and Tm) and transition or main group elements (e.g., Mn, Cr, Ti, Ag, Cu, Zn, Bi, Pb, Sn, and Tl) can be used as fluorescent activators. Materials such as Ca, Zn, and Cd in tungstate, metal vanadates, and ZnO can be used.

[0142] Commercially available laser dye materials, with or without energy enhancement factors, from several laser dye vendors, including Lambda Physik and Exciton, can also be used. A partial list of preferred laser dye classes includes pyrromethenes, coumarins, rhodamines, fluoresceins, and other aromatic hydrocarbons and their derivatives. Additionally, there are many polymers containing unsaturated carbon-carbon bonds that also function as fluorescent materials and have found numerous optical and fluorescent applications. For example, MEH-PPV and PPV have been used in optoelectronic devices such as polymer light-emitting diodes (PLEDs). These fluorescent polymers, with or without energy enhancement factors, can be used directly as the fluorescent layer in transparent 2-D display screens.

[0143] As mentioned above, semiconductor nanoparticles (e.g., quantum dots) can be used with or without energy enhancement factors. The term "semiconductor nanoparticle" in the art refers to inorganic crystallites with diameters between 1 nm and 1000 nm, preferably between 2 nm and 50 nm. Semiconductor nanoparticles can emit electromagnetic radiation upon excitation (i.e., they are luminescent). Nanoparticles can be homogeneous nanocrystals or composed of multiple shells. For example, nanoparticles can include a "core" of one or more first semiconductor materials surrounded by a "shell" of a second semiconductor material. The core and / or shell may be semiconductor materials, including, but not limited to, II-VI (ZnS, ZnSe, ZnTe, CdS, CdSe, CdTe, HgS, HgSe, HgTe, MgS, MgSe, MgTe, CaS, CaSe, CaTe, SrS, SrSe, SrTe, BaS, BaSe, BaTe, etc.) and III-V (GaN, GaP, GaAs, GaSb, InN, InP, InAs, InSb, etc.) and IV (Ge, Si, etc.) materials, and alloys or mixtures thereof.

[0144] Fluorescent organometallic molecules containing rare earth or transition element cations, with or without energy enhancement factors, can be used in downconversion materials. These molecules contain rare earth metal centers, such as Eu, Tb, Er, Tm, and Ce, protected with organic chelating groups. The metal centers can also contain transition elements, such as Zn, Mn, Cl, and Ir, and main group elements, such as B, Al, and Ga. These organometallic molecules are readily soluble in liquid or transparent solid host media. Some examples of such fluorescent organometallic molecules include: 1. tris(dibenzoylmethane)mono(phenanthroline)europium(III), 2. tris(8-hydroxyquinoline)erbium, 3. tris(1-phenyl-3-methyl-4-(2,2-dimethylpropan-1-oyl)pyrazolin-5-one)terbium(III), 4. bis(2-methyl-8-hydroxyquinolato)zinc, and 5. diphenylborane-8-hydroxyquinolate.

[0145] Specific examples of red-emitting down-conversion materials include those described above and europium complexes such as those described in Japanese Patent Publication No. 2003-26969, in which a β-diketone ligand is coordinated to europium to form a europium complex capable of red fluorescence. Other specific examples of rare earth element complexes include complexes containing lanthanum (Ln), europium (Eu), terbium (Tb), and gadolinium (Gd), and combinations thereof. Europium (Eu) complexes can emit red fluorescence when irradiated with ultraviolet light at a wavelength ranging from 365 nm to 410 nm. Terbium (Tb) can emit green fluorescence when irradiated with ultraviolet light at a wavelength of 365 nm.

[0146] In other down-conversion embodiments, the down-conversion material that emits red light may include europium, the light-emitting particles that emit green light may include terbium, and the light-emitting particles that emit blue or yellow light may include cerium (and / or thulium). In up-conversion embodiments, the up-conversion material that emits red light may include praseodymium, the light-emitting particles that emit green light may include erbium, and the light-emitting particles that emit blue light may include thulium. In embodiments, the conversion material may be light-emitting particles comprised of fluorescent molecules that emit different colors (e.g., red, green, and blue) or different wavelengths or energies of light. In embodiments, the conversion material may be light-emitting particles comprised of pure organic or organometallic dyes with or without energy enhancement factors.

[0147] In addition to rare earth complex combinations, such as a combination of a europium complex and a terbium complex, it is also possible to employ a combination of a europium complex and an uncomplexed green-emitting phosphor, or a combination of a terbium complex and an uncomplexed red-emitting phosphor.

[0148] Other downconverter materials (which may be used with or without an energy enhancement factor) include, for example, ZnS, PbS, SbS3, MoS2, PbTe, PbSe, BeO, MgO, Li2CO3, Ca(OH)2, MoO3, SiO2, Al2O3, TeO2, SnO2, KBr, KCl, and NaCl. These materials may contain dopants to tune their emission properties, as described above. Examples of suitable doped (or alloyed) glass systems include Y2O3:Gd, Y2O3:Dy, Y2O3:Tb, Y2O3:Ho, Y2O3:Er, Y2O3:Tm, Gd2O3:Eu, Y2O2S:Pr, Y2O2S:Sm, Y2O2S:Eu, Y2O2S:Tb, Y2O2S:Ho, Y2O2S:Er, Y2O2S:Dy, Y2O2S:Tm, ZnS:Ag:Cl (blue), ZnS:Cu:Al (green), Y2O2S:Eu (red), Y2O3:Eu (red), YVO4:Eu (red), and Zn2SiO4:Mn (green).

[0149] More specifically, with regard to downconverter materials suitable for the present invention, U.S. Pat. No. 4,705,952 (the contents of which are incorporated herein by reference) describes an infrared-triggered phosphor that, when triggered by infrared radiation, stores energy in the form of visible light at a first wavelength and emits energy in the form of visible light at a second wavelength. The phosphor in U.S. Pat. No. 4,705,952 is a composition of alkaline earth metal sulfide, rare earth dopant, and fusible salt. The phosphor in U.S. Pat. No. 4,705,952 is more specifically a phosphor made from strontium sulfide, barium sulfide, and mixtures thereof, such as dopants from the rare earth series and europium oxide, and mixtures thereof, and fusible salts of fluorides, chlorides, bromides, and iodides of, for example, lithium, sodium, potassium, cesium, magnesium, calcium, strontium, and barium, and mixtures thereof. The materials described in U.S. Patent No. 4,705,952, with or without an energy enhancement factor, are useful in various embodiments of the present invention. In one example, infrared-triggered phosphorescent materials are used in combination with a folded resonator, where reception of a microwave or IR signal locally heats and triggers emission. (This application is particularly suited to color enhancement and / or security applications.)

[0150] In other embodiments of the present invention, the downconverter material (or a mixture of downconverter materials, which may be used with or without an energy enhancement factor) may comprise Y2O3:Li. Sun et al., "Luminescent properties of Li+ doped nanosized Y2O3:Eu," Solid State Comm. 119 (2001) 393-396 (the entire contents of which are incorporated herein by reference) describes such a material. Hou et al., "Luminescent properties nano-sized Y2O3:Eu fabricated by co-precipitation method," Journal of Alloys and Compounds, vol. 494, issue 1-2, April 2, 2010, pp. 382-385 (the entire contents of which are incorporated herein by reference) describe that nano-sized yttria (Y2O3) powder was successfully synthesized by a co-precipitation method. The powder was well crystallized, the particles were nearly spherical, and the dispersibility was good. Eu 3+ The quenching concentration of ions was 9 mol%, which is much higher than that of the microscale powders. The incorporation of Li+ ions significantly enhanced the luminescence intensity. The highest luminescence intensity was observed in the 4 mol% Li+-doped Y2O3:Eu powder (Y 0.87 EU 0.09 Li 0.04 )2O3), the fluorescence intensity increased by 79%. Yi et al. “Improved cathodoluminescent characteristics of Y2O3:Eu 3+ thin films by Li-doping,” Appl. Phys. A87, 667-671 (2007) (the entire contents of which are incorporated herein by reference) 3+ and Li-doped Y2O3:Eu 3+ The cathodoluminescence spectra for both films and methods for making these materials are described.

[0151] Specific downconverting materials may also include at least one or more of Y2O3, Y2O3:Gd, Y2O2S, NaYF4, NaYbF4, YAG, YAP, Nd2O3, LaF3, LaCl3, La2O3, TiO2, LuPO4, YVO4, YbF3, YF3, Na-doped YbF3, ZnS, ZnSe, MgS, CaS, Zn2SiO4:Mn, LaOBr:Tm, and alkali lead silicates, such as SiO2, BO3, Na2O, KO, PbO, MgO, or Ag compositions, and combinations, alloys, or layers thereof. Additionally, the downconverting material may be a sulfur-containing phosphorescent material, which may be useful, for example, in rubber vulcanization or other photoactivation processes. An example of such a sulfur-containing phosphorescent material is (Sr,Ca)Ga2S4. Other examples include phosphorescent particles such as SrGa2S4, CaGa2S 4、 The downconverting material includes a thiogallate host material selected from the group consisting of BaGa2S4, MgGa2S4, and solid solutions thereof. The particle size of such phosphorescent materials can be controlled from 25 nm to 300 microns, as described in US6,153,123A. The downconverting material can include a dopant containing at least one of Er, Eu, Yb, Tm, Nd, Mn, Sb, Tb, Ce, Y, U, Pr, La, Gd, and other rare earth species or combinations thereof. The dopant can be included in a concentration ranging from 0.01% to 50% molar concentration. It may be preferable to use a combination of dopants rather than a single dopant, such as Mn and Sb in a silicate matrix.

[0152] In other embodiments, the present invention can enhance specific wavelengths or energies of light emitted from a material or surface using a wide variety of upconversion materials (or mixtures of upconverters), with or without an energy enhancement factor. These upconversion materials can include materials similar to those discussed above for downconversion, but typically include doped or impurity states in the host crystal that provide the upconversion pumping mechanism. Thus, upconversion materials for enhancing wavelength or energy emission can convert energy from near-infrared, infrared, and microwave radiation. Upconversion materials for enhancing color emission can convert energy from lower-energy visible light to higher-energy visible light.

[0153] In one example, lanthanide-doped oxide nanoparticles can be excited with near-infrared light, such as 980 nm and 808 nm laser light, to produce visible light in various portions (various wavelengths or energies) of the red, green, and blue spectrum, depending on the selected dopant trivalent rare earth ion(s), their concentrations, and the host lattice.

[0154] The lanthanide-doped oxides suitable for the present invention differ from conventional multiphoton upconversion processes, in which, for example, the absorption of two photons is required in a simultaneous event to promote an electron from a valence band state directly to an upper-level conduction band state where relaxation across the band gap of the material produces fluorescence. Here, co-doping creates band gap states in NaYF4 to induce Y 3+ Ions, 2 F 5 / 2 , have an energy state that can be pumped by a single photon event, from which another single photon absorption event can populate an even higher state. Once in this excited state, a transition to a higher energy radiative state is possible, and then light emission occurs. 2 F 5 / 2 It has higher energy than the incident light that pumps the energy state. In other words, Yb3+ Aeon 2 F 5 / 2 The energy state is the state where 980 nm light is absorbed, which allows the formation of a cluster. 4 F 7 / 2 It serves as the basis for transitions to higher energy states, such as 4 F 7 / 2 The transition from the energy state produces a visible emission.

[0155] U.S. Patent No. 7,008,559 (the entire contents of which are incorporated herein by reference) describes the upconversion capabilities of ZnS, where excitation at 767 nm produces emission in the visible range. The materials described in U.S. Patent No. 7,008,559 (ZnS and Er) 3+ Doped BaTiO3 nanoparticles and Yb 3+ Doped CsMnCl3, with or without an energy enhancement factor, are suitable for various embodiments of the present invention.

[0156] Furthermore, materials designated as upconversion materials in the present invention (with or without energy enhancement) include CdTe, CdSe, ZnO, CdS, YO, MgS, CaS, SrS, and BaS. Such upconversion materials can be any semiconductor, more specifically, but not limited to, sulfide, telluride, selenide, and oxide semiconductors, and nanoparticles thereof, e.g., ZnO, CdS, Y2O3, MgS, CaS, SrS, and BaS. 1-x Mn x S y , Zn 1-x Mn x Se y , Zn 1-x Mn x Te y , Cd 1-x MnS y , Cd 1-x Mn x Se y , Cd 1-x Mn x Te y , Pb 1-x Mn x S y , Pb1-x Mn x Se y 、Pb 1-x Mn x Te y 、Mg 1-x MnS y 、Ca 1-x Mn x S y 、Ba 1-x Mn x S y 及びSr 1-x 等等(式中、0 < x ≦ 1、及び0 < y ≦ 1)であり得る。上記の半導体の複合化合物もまた、本発明での使用が企図されている。例えば、(M 1-z N z ) 1-x Mn x A 1-y B y (M = Zn、Cd、Pb、Ca、Ba、Sr、Mg; N = Zn、Cd、Pb、Ca、Ba、Sr、Mg; A = S、Se、Te、O; B = S、Se、Te、O; 0 < x ≦ 1、0 < y ≦ 1、0 < z ≦ 1)。このような複合化合物の2つの例は、Zn 0.4 Cd 0.4 Mn 0.2 S及びZn 0.9 Mn 0.1 S 0.8 Se 0.2 である。追加の変換材料には、絶縁性及び非導電性材料が含まれ、いくつかの例示的な化合物を挙げれば、BaF2、BaFBr、及びBaTiO3がある。本発明に適切な遷移及び希土類イオンを共ドープした半導体は、硫化物、テルル化物、セレン化物及び酸化物半導体及びそれらのナノ粒子を含み、例えばZnS; Mn; Er; ZnSe; Mn、Er; MgS; Mn、Er; CaS; Mn、Er; ZnS; Mn、Yb; ZnSe; Mn、Yb; MgS; Mn、Yb; CaS; Mn、Ybなど、及びそれらの複合化合物(M 1-z N z ) 1-x (Mn q R 1-q ) x A 1-y B y(M=Zn, Cd, Pb, Ca, Ba, Sr, Mg; N=Zn, Cd, Pb, Ca, Ba, Sr, Mg; A=S, Se, Te, O; B=S,...0 <z≦1、o<q≦1)がある。

[0157] Some nanoparticles, e.g., ZnS:Tb 3+ , Er 3+ ;ZnS:Tb 3+ ;Y2O3:Tb 3+ ;Y2O3:Tb 3+ , Er3 + ;ZnS:Mn 2+ ;ZnS:Mn,Er 3+ are known in the art to work for both downconversion and upconversion emissions and would be suitable for the present invention, with or without an energy enhancement factor. In upconversion embodiments, light-emitting particles that emit red light may include praseodymium, light-emitting particles that emit green light may include erbium, and light-emitting particles that emit blue light may include thulium.

[0158] Typically, the upconversion process requires one or more additional rare earth dopants, such as Er, Eu, Yb, Tm, Nd, Tb, Ce, Y, U, Pr, La, Gd, and other rare earth species, or combinations thereof, doped into a dielectric crystal (any size >0.1 nm) containing at least one of YO, YO2O2S, NaYF4, NaYbF4, YAG, YAP, Nd2O3, LaF3, LaCl3, La2O3, TiO2, LuPO4, YVO4, YbF3, YF3, Na-doped YbF3, or SiO2, where the incident radiation is at a longer wavelength than the emitted radiation from the crystal. The emitted wavelength is entirely based on the selected dopant ion(s) and their associated and relative concentrations within the host crystal. In the case of upconversion in a YO host crystal, to achieve blue emission (approximately 450–480 nm), one could synthesize [YO; Yb (3%), Tm (0.2%)], where Yb and Tm are the percentages of Y atoms doped into the crystal relative to 100%. Similarly, typical green upconversion materials are [YO; Yb (5%), Ho (1%)] and [YO; Yb (2%), Er (1%)], and typical red upconversion materials are [YO; Yb (10%), Er (1%)] and [YO; Yb (5%), Eu (1%)]. The concentrations of the dopants relative to each other and the crystal matrix must be adjusted for every combination, and there are multiple ways to achieve multiple wavelengths or energy emissions from the same dopant.

[0159] Tm 3+ Upconversion of red light at a wavelength of about 650 nm in doped fluorozirconate glasses can be used in the present invention to generate blue light. In this system, the blue light consists of two emission bands: one at 450 nm due to the 1D2 → 3H4 transition, and the other at 475 nm due to the 1G4 → 3H6 transition. The emission intensity of both bands has been observed by others to vary quadratically with pump power. At 0.2 mol % or more of Tm 3+In concentrated glasses, cross-relaxation processes occur, reducing the upconversion efficiency.

[0160] Visible light emission upon excitation in the near infrared (NIR) was observed for LuPO4:Yb in chloroform. 3+ , Tm 3+ , and YbPO4:Er 3+ It has been observed in optically clear colloidal solutions of nanocrystals, and excitation at 975 nm has been shown by others to produce visible emission in the blue, green, or red spectral regions.

[0161] Tellurium and germanium oxides (tellurites and germanates) are also suitable upconverters. These glasses can be doped with, for example, Tm, Yb, Ho, Er, Pr.

[0162] Yb 3+ Doped BaZrO3 is also suitable for upconversion. 3+ and / or Tm 3+ Doping is also suitable for tuning the emission wavelength.

[0163] In another embodiment, Nd prepared by the Morss method 3+ :Cs2NaGdCl6 and Nd 3+ , Yb 3+ Polycrystalline powder samples of CsNaGdCl have been reported to be upconverters suitable for the present invention. These materials exhibit upconversion emissions around 538 nm (green), 603 nm (orange), and 675 nm (red) under 785 nm irradiation, with the upconversion sequences being 4G7 / 2 → 4I9 / 2, (4G7 / 2 → 4I11 / 2; 4G5 / 2 → 4I9 / 2), and (4G7 / 2 → 4I13 / 2; 4G5 / 2 → 4I11 / 2), respectively.

[0164] In another embodiment, Nd 3+ and Ho 3+Co-doped base ZrF4 fluoride glass has been reported to be an upconverter and is suitable for the present invention. Among the upconversion luminescence of ZrF4 fluoride glass, the green emission was very strong, while the blue and red emission intensities were very weak.

[0165] In another embodiment, Tm 3+ / Yb 3+ Co-doped TeO2-Ga2O3-R2O (R = Li, Na, K) glasses have been reported to be upconverters and are suitable for the present invention. These materials exhibited strong blue upconversion emission centered at 476 nm and weak red emission at 650 nm under 977 nm excitation.

[0166] In another embodiment, [Ru(dmb)] in the presence of anthracene or 9,10-diphenylanthracene 2+ Metal-to-ligand charge transfer (MLCT) transitions in (dmb = 4,4'-dimethyl-2,2'-bipyridine) have been reported to be upconverters, making them suitable for the present invention. Upconverted singlet fluorescence due to triplet-triplet annihilation at low excitation powers has been reported. In particular, 9,10-diphenylanthracene (DPA) (used instead of anthracene) showed higher efficiency for upconversion. In these experiments, researchers of this material system hypothesized that DPA increased the singlet fluorescence quantum yield (λ = 0.95) compared to anthracene (λ = 0.27). This work demonstrated an improvement in green-to-blue light upconversion to approximately 24.4 ± 6.1, comparable to that of, for example, commercially available green laser pointers (λ = 0.95). ex This allows for direct visualization of the process at low excitation powers (e.g., 532 nm, <5 mW peak power).

[0167] In certain embodiments, additional energy converters include, but are not limited to, the following (not ranked by priority or usefulness): CaF2, ZnF2, KMgF3, ZnGa2O4, ZnAl2O4, Zn2SiO4, Zn2GeO4, Ca5(PO4)3F, Sr5(PO4)3F, CaSiO3, MgSiO3, ZnS, MgGa2O4, LaAl 11 O 18 , Zn2SiO4, Ca5(PO4)3F, Mg4Ta2O9, CaF2, LiAl5O8, LiAlO2, CaPO3, AlF3, and LuPO4:Pr 3+ Examples further include alkaline earth chalcogenide phosphorescent materials, which are exemplified below by the following non-exhaustive list: MgS:Eu 3+ , CaS:Mn 2+ , CaS:Cu, CaS:Sb, CaS:Ce 3+ , CaS:Eu 2+ , CaS:Eu 2+ Ce 3+ , CaS:Sm 3+ , CaS:Pb 2+ , CaO:Mn 2+ , CaO:Pb 2+ .

[0168] Further examples include ZnS type phosphorescent materials including various derivatives: ZnS:Cu,Al(Cl), ZnS:Cl(Al), ZnS:Cu,I(Cl), ZnS:Cu, ZnS:Cu,In.

[0169] Also included are IIIb-Vb phosphorescent materials, compounds containing elements from groups IIIb and Vb of the periodic table. These semiconductors include BN, BP, BSb, AlN, AlP, AlAs, AlSb, GaN, GaP, GaAs, GaSb, InN, InP, InAs, and InSb. These materials may contain donors and acceptors that cooperate to induce light-emitting diodes. These donors include, but are not limited to, Li, Sn, Si, Li, Te, Se, S, and O. Acceptors include, but are not limited to, C, Be, Mg, Zn, Cd, Si, and Ge. Also included are primary GaP light-emitting diodes, including, but not limited to: GaP:Zn,O, GaP:NN, GaP:N, and GaP, which emit red, yellow, green, and pure green light, respectively.

[0170] The materials can further include materials such as GaAs with the following types of compositional variations: In 1-y (Ga 1-x Al x ) y P.

[0171] Also included is silicon carbide SiC, which is commercially relevant as an emission platform for blue light-emitting diodes. These include the polytypes 3C-SiC, 6H-SiC, and 4H-SiC, with donors such as N and Al and acceptors such as Ga and B.

[0172] Further examples include the following composition (Sr,Ca,Ba)5(PO4)3Cl:Eu 2+ , BaMgAl 16 O 27 :EU 2+ , CeMgAl 11 O 19 :Ce 3+ :Tb 3+ , LaPO4:Ce 3+ :Tb 3+ , GdMgB5O 10 :Ce3:Tb 3+ , Y2O3:Eu 3+ , (Ba,Ca,Mg)5(PO4)3Cl:Eu 2+ , 2SrO0.84 P2O50.16B2O3:Eu 2+ , SrAl 14 O 25 :EU 2+ Multiband emissive materials include, but are not limited to:

[0173] Also included are materials typically used in fluorescent high-pressure mercury discharge lamps. These can be excited by X-rays and are exemplified by the following system designation: Phosphate (Sr,M) (PO4)2:Sn 2+ , Mg or Zn activator, germanate 4MgO.GeO2:Mn 4+ , 4(MgO,MgF2)GeO2:Mn 4+ , Yttrium Y2O3:Eu 3+ , vanadate YVO4:Eu 3+ , Y(P,V)O4:Eu 3+ , Y(P,V)O4:In + , halo silicate Sr2Si3O 82 SrCl2:Eu 2+ , aluminate (Ba,Mg)2Al 16 O 24 :EU 2+ , (Ba,Mg)2Al 16 O 24 :EU 2+ , Mn 2+ , Y2O3Al2O3:Tb 3+ .

[0174] Another grouping by host compound includes halophosphate phosphors, phosphate phosphors, silicate phosphors, aluminate phosphors, borate phosphors, tungstate phosphors, and other phosphor chemical compositions. Halophosphates include, but are not limited to: 3Ca3(PO4)2.Ca(F,Cl)2:Sb 3+ , 3Ca3(PO4)2.Ca(F,Cl)2:Sb 3+ / Mn 2+ , Sr 10 (PO4)6Cl2:Eu 2+ , (Sr, Ca) 10 (PO4)6Cl2:Eu 2+ , (Sr, Ca)10 (PO4)6.nB2O3:Eu 3+ , (Sr, Ca, Mg) 10 (PO4)6Cl2:Eu 2+ Phosphorescent materials include, but are not limited to: Sr2P2O7:Sn 2+ , (Sr,Mg)3(PO4)2:Sn 2+ , Ca3(PO4)2.Sn 2+ , Ca3(PO4)2:Tl + , (Ca,Zn)3(PO4)2:Tl + , Sr2P2O7:Eu 2+ , SrMgP2O7:Eu 2+ , Sr3(PO4)2:Eu 2+ , LaPO4:Ce 3+ , Tb 3+ , La2O3.0.2SiO2.0.9P2O5:Ce 3+ .Tb 3+ , BaO.TiO2.P2O5. Silicate phosphorescent material, Zn2SiO4:Mn 2+ , CaSiO3:Pb 2+ / Mn 2+ , (Ba, Sr, Mg) . 3Si2O7:Pb 2+ , BaSi2O5:Pb 2+ , Sr2Si3O 8. 2SrCl2:Eu 2+ ,Ba3MgSi2O8:Eu 2+ , (Sr,Ba)Al2Si2O8:Eu 2+ .

[0175] Aluminate phosphors include, but are not limited to: LiAlO2:Fe 3+ , BaAlO 13 :EU 2+ , BaMgAl 16 O 27 :EU 2+ , BaMgAl 16 O 27 :EU 2+ / Mn 2+ , SrAl 14 O 25 :EU 2+ , CeMgAl 11O 19 :Ce 3+ / Tb 3+ .

[0176] Borate phosphors include: Cd2B2O5:Mn 2+ , SrB4O7F:Eu 2+ , GdMgB5O 10 :Ce 3+ / Tb 3+ , GdMgB5O 10 :Ce 3+ / Mn 3+ , GdMgB5O 10 :Ce 3+ / Tb 3+ / Mn 2+ .

[0177] Tungstate phosphors include, but are not limited to, CaWO4, (Ca,Pb)WO4, and MgWO4. Other phosphors include Y2O3:Eu 3+ , Y(V,P)O4:Eu 2+ , YVO4:Dy 3+ , MgGa2O4:Mn 2+ , 6MgO.As2O5:Mn 2+ , 3.5MgO.0.5MgF2.GeO2:Mn 4+ is.

[0178] Activators for various doped phosphorescent materials include, but are not limited to: Tl + , Pb 2+ , Ce 3+ ,EU 2+ , WO4 2- , Sn 2+ , Sb 3+ , Mn 2+ , Tb 3+ ,EU 3+ , Mn 4+ , Fe 3+ . Luminescent center Tl + is used in the following chemical composition: (Ca,Zn)3(PO4)2:Tl + , Ca3(PO4)2:Tl + Luminescent center Mn 2+ is MgGa2O4:Mn2+ , BaMgAl 16 O 27 :EU 2+ / Mn 2+ , Zn2SiO4:Mn 2+ , 3Ca3(PO4)2.Ca(F,Cl)2:Sb 2+ / Mn 2+ , CaSiO3:Pb 2+ / Mn 2+ , Cd2B2O5:Mn 2+ , CdB2O5:Mn 2+ , GdMgB5O 10 :Ce 3+ / Mn 2+ , GdMgB5O 10 :Ce 3+ / Tb 3+ / Mn 2+ The luminescent center Sn2+ is used in the chemical composition: Sr2P2O7:Sn 2+ , (Sr,Mg)3(PO4)2:Sn 2+ . T emission center Eu 2+ is used in the following chemical composition: SrB4O7F:Eu 2+ , (Sr,Ba)Al2Si2O8:Eu 2+ , Sr3(PO4)2:Eu 2+ , Sr2P2O7:Eu 2+ , Ba3MgSi2O8:Eu 2+ , Sr 10 (PO4)6Cl2:Eu 2+ , BaMgAl 16 O 27 :EU 2+ / Mn 2+ , (Sr, Ca) 10 (PO4)6Cl2:Eu 2+ T luminescent center Pb 2+ is used in the following chemical composition: (Ba,Mg,Zn)3Si2O7:Pb 2+ , BaSi2O5:Pb 2+ , (Ba,Sr)3Si2O7:Pb 2+ .

[0179] Luminescent center Sb 2+is used in the following chemical composition: 3Ca3(PO4)2.Ca(F,Cl)2:Sb 3+ , 3Ca3(PO4)2.Ca(F,Cl)2:Sb 3+ / Mn 2+ .

[0180] Luminescent center Tb 3+ is used in the following chemical composition: CeMgAl 11 O 19 :Ce 3+ / Tb 3+ , LaPO4:Ce 3+ / Tb 3+ , Y2SiO5:Ce 3+ / Tb 3+ , GdMgB5O 10 :Ce 3+ / Tb 3+ Luminescent center Eu 3+ It is used in the following chemical composition: Y2O3:Eu 3+ , Y(V,P)O4:Eu 3+ Luminescent center Dy 3+ is used in the following chemical composition: YVO4:Dy 3+ Luminescent center Fe 3+ is used in the following chemical composition: LiAlO2:Fe 3+ Luminescent center Mn 4+ is used in the following chemical composition: 6MgO.As2O5:Mn 4+ , 3.5MgO0.5MgF2.GeO2:Mn 4+ Luminescent center Ce 3+ is used in the following chemical composition: Ca2MgSi2O7:Ce 3+ and Y2SiO5:Ce 3+ Luminescent center WO4 2- It is used in the following chemical compositions: CaWO4, (Ca, Pb)WO4, MgWO4. The luminescent center is TiO4 4- is used with the following chemical composition: BaO.TiO2.P2O5.

[0181] Additional phosphorescent chemistries of interest using X-ray excitation include, but are not limited to, the k-edges of these phosphorescent materials. Low energy excitation can result in strong emission in low kedge materials. Some of these chemistries and their corresponding kedges are shown below. BaFCl:Eu 2+ 37.38 keV BaSO4:Eu 2+ 37.38 keV CaWO469.48keV Gd2O2S:Tb 3+ 50.22 keV LaOBr:Tb 3+ 38.92 keV LaOBr:Tm 3+ 38.92 keV La2O2S:Tb 3+ 38.92 keV Y2O2S:Tb 3+ 17.04 keV YTaO467.42keV YTaO4:Nb 67.42keV ZnS:Ag 9.66keV (Zn,Cd)S:Ag 9.66 / 26.7keV

[0182] These materials can be used alone or in combination of two or more. Various compositions can be prepared to obtain a desired output wavelength or spectrum of wavelengths. In the present invention, the selection of phosphorescent materials can be chosen such that, under irradiation with X-rays or other high energy sources, the light emitted from the phosphorescent material can have exemplary properties including, for example: Emission in the wavelength range of 190-250 nm, Emission in the wavelength range of 330-340 nm.

[0183] Mechanoluminescent materials (organic and inorganic) In another embodiment of the present invention, mechanoluminescent materials can be used as energy converters, optionally in conjunction with the energy enhancement structures described above.

[0184] Mechanoluminescent materials convert ultrasonic or mechanical energy (such as vibrations naturally present in items such as motors or vibrations driven by transducers) into visible light, where, for example, the mechanoluminescent material is placed near (e.g., between, around, or inside) a folded structure or a pair of external electrodes.

[0185] In one embodiment, the electromagnetic wave energy enhancement agent captures electromagnetic energy of one or more wavelengths and enhances the electromagnetic energy of one or more wavelengths with at least one property (e.g., electric field strength in the vicinity of the mechanoluminescent material), while at the same time the mechanoluminescent material can be considered an energy converter that converts ultrasonic or mechanical energy into electromagnetic radiation (i.e., emitted light).

[0186] In one embodiment of the present invention, increasing the electric field in the folded structure or the external electrode pair increases the luminescence of the mechanoluminescent material, and the energy used to establish the electric field in the folded structure or the external electrode pair is supplied separately from the mechanical energy that drives the mechanoluminescence.

[0187] Various mechanoluminescent materials suitable for the present invention, with or without an energy enhancement factor, include: ZnS:Mn 2+ , SrAl2O4:Eu 2+ , ZnS:Cu, SrAMgSi2O7:Eu 2+ (A=Ca,Sr,Ba), KCl, KI, KBr, NaF, NaCl, LiF, RbCl, RbBr, RbI, MgO, SrAl2O4, CaAl2O4, Sr 1-x Ba x Al2O4(x=0, 0.1, 0.2, 0.4), Sr 0.9 Ca 0.1 Al2O4, Zn2Ge 0.9 Si 0.1 O4, MgGa2O4, ZnGa2O4, ZnAl2O4, ZnS, ZnTe, (ZnS) 1-x (MnTe) x(x<1 / 4), CaZnOS, BaZnOS, Ca2MgSi2O7, Sr2MgSi2O7, Ba2MgSi2O7, SrCaMgSi2O7, SrBaMgSi2O7, Sr n MgSiO 5+n (1≦n≦2), Ca2Al2SiO7, Sr2Al2SiO7, CaYAl3O7, CaAl2Si2O8, Ca 1-x Sr x Al2Si2O8(x<0.8), SrMg2(PO4)2, Ba 1-x Ca x TiO3(0.25 <x<0.8)、Ba 1-x Ca x TiO3, LiNbO3, Sr2SnO4, (Ca,Sr,Ba)2SnO4, Sr3Sn2O7, Sr3(Sn,Si)2O7, Sr3(Sn,Ge)2O7 , Ca3Ti2O7, CaNb2O6, Ca2Nb2O7, Ca3Nb2O8, BaSi2O2N2, SrSi2O2N2, CaZr(PO4)2, ZrO2.

[0188] In one embodiment, europium-holmium co-doped strontium aluminate, alone or in combination with an energy enhancement factor, can be used as a mechanoluminescent material (i.e., energy converter). Europium-holmium co-doped strontium aluminate and other mechanoluminescent materials convert acoustic or sonic energy into photon emission, which may or may not be located in proximity to an energy enhancement factor.

[0189] In "Novel Mechano-Luminescent Sensors Based on Piezoelectric / Electroluminescent Composites," Sensors (Basel). 2011;11(4):3962-396, the entire contents of which are incorporated by reference, Yanim Jia describes a mechano-luminescent composite made of piezoelectric and electroluminescent materials. In this composite device, when stress is applied to the piezoelectric layer, charges are induced on both the top and bottom surfaces of the piezoelectric layer due to the piezoelectric effect. These induced charges result in light output from the electroluminescent layer due to the electroluminescent effect.

[0190] Now, in one embodiment of the present invention, with or without an energy enhancement factor, such a composite material made from a piezoelectric material and an electroluminescent material, hereinafter a "composite mechanoluminescent emitter," provides a structure that emits light when stimulated with mechanical or vibrational energy, such as from an acoustic or ultrasonic transducer.

[0191] Electroluminescent and phosphorescent materials (organic and inorganic): The present invention in various embodiments can utilize organic fluorescent molecules or inorganic particles that can have crystalline, polycrystalline, or amorphous microstructures for the converters or fluorescence and phosphorescence (optionally including the energy enhancement structures described above).

[0192] The list of inorganic molecules that can be used with or without energy enhancement factors for the electroluminescent and phosphorescent materials described below includes, but is not limited to, the following inorganic electroluminescent phosphorescent materials: SrS:Ce 3+ CaGa2S4:Ce 3+ SrS:Cu + CaS:Pb 2+ BaAl2S4:Eu 2+ ZnS:Tb 3+ ZnMgS:Mn 2+ SrGa2S4:Eu 2+ CaAl2S4:Eu 2+ BaAl2S4:Eu 2+ ZnS:Mn 2+ MgGa2O4:Eu 3+ (Ca,Sr)Y2S4:Eu 2+ BaAl2S4:Eu 2+

[0193] Organic molecules that are capable of phosphorescence under the influence of an electric field are also of interest herein. Examples of organic fluorescent compounds with high quantum yields include: naphthalene, pyrene, Perylene, anthracene, phenanthrene, p-terphenyl, p-quatphenyl, trans-stilbene, tetraphenylbutadiene, Distyrylbenzene, 2,5-diphenyloxazole, 4-methyl-7-diethylaminocoumarin, 2-phenyl-5-(4-biphenyl)-1,3,4-oxadiazole, 3-phenylcarbostyril, 1,3,5-triphenyl-2-pyrazoline, 1,8-naphthoylene-1',2'-bezimidazole, 4-Amino-N-phenyl-naphthalimide.

[0194] The inorganic fluorescent and phosphorescent materials detailed herein are numerous, and various examples are provided by way of illustration and not limitation, and can be used with or without energy enhancement factors. Furthermore, these materials can be doped with specific ions (activators or combinations of activators) that can occupy lattice structure sites in the case of crystalline or polycrystalline materials, or network-forming sites or cross-linked and / or non-cross-linked sites in amorphous materials. These compounds can include the following example materials (not ranked in order of preference or usefulness): CaF2, ZnF2, KMgF3, ZnGa2O4, ZnAl2O4, Zn2SiO4, Zn2GeO4, Ca5(PO4)3F, Sr5(PO4)3F, CaSiO3, MgSiO3, ZnS, MgGa2O4, LaAl 11 O 18 , Zn2SiO4, Ca5(PO4)3F, Mg4Ta2O9, CaF2, LiAl5O8, LiAlO2, CaPO3, AlF3.

[0195] Also included are alkaline earth chalcogenide phosphorescent materials, which are next exemplified by the following non-exhaustive list: MgS:Eu 3+ , CaS:Mn 2+ , CaS:Cu, CaS:Sb, CaS:Ce 3+ , CaS:Eu 2+ , CaS:Eu 2+ Ce 3+ , CaS:Sm 3+ , CaS:Pb 2+ , CaO:Mn 2+ , CaO:Pb 2+ .

[0196] Examples include ZnS-type phosphors, including various derivatives. ZnS:Cu, Al(Cl), ZnS:Cl(Al), ZnS:Cu,I(Cl), ZnS:Cu, ZnS:Cu, In.

[0197] IIIb-Vb phosphorescent materials, compounds containing elements from groups IIIb and Vb of the periodic table, are suitable as converter materials. These semiconductors include BN, BP, BSb, AlN, AlP, AlAs, AlSb, GaN, GaP, GaAs, GaSb, InN, InP, InAs, and InSb. These materials have donors and acceptors that cooperate to produce light-emitting diodes. Donors include Li, Sn, Si, Li, Te, Se, S, and O. Acceptors include C, Be, Mg, Zn, Cd, Si, and Ge. For example, GaP light-emitting diodes include GaP:Zn, O, GaP:NN, GaP:N, and GaP, which emit red, yellow, green, and pure green light, respectively.

[0198] The blended materials further include materials such as GaAs with the following types of compositional variations: In1-y(Ga1-xAlx)yP (a simple example is presented).

[0199] Silicon carbide (SiC) as a light-emitting platform is commercially relevant for blue light-emitting diodes. These include the polytypes 3C-SiC, 6H-SiC, and 4H-SiC, with donors such as N and Al and acceptors such as Ga and B.

[0200] Multiband emissive materials suitable for the converter material include, for example, the following compositions: (Sr,Ca,Ba)5(PO4)3Cl:Eu 2+ , BaMgAl 16 O 27 :EU 2+ , CeMgAl 11 O 19 :Ce 3+ :Tb 3+ , LaPO4:Ce 3+ :Tb 3+ , GdMgB5O 10 :Ce 3+ :Tb 3+ , Y2O3:Eu 3+ , (Ba,Ca,Mg)5(PO4)3Cl:Eu 2+ , 2SrO 0.84 P2O5 .0.16B2O3:Eu 2+ , SrAl 14 O 25 :EU 2+ .

[0201] Other materials suitable as converter materials include those used in fluorescent high-pressure mercury discharge lamps, which can be excited by X-rays, and are exemplified by the following system designations: Phosphate (Sr, M)(PO4)2:Sn 2+ , Mg or Zn activator, germanate 4MgO.GeO2:Mn 4+ , 4(MgO,MgF2)GeO2:Mn 4+ , Yttrium Y2O3:Eu 3+ , vanadate YVO4:Eu 3+ , Y(P,V)O4:Eu 3+ , Y(P,V)O4:In + , halo silicate Sr2Si3O8 . 2SrCl2:Eu 2+ , aluminate (Ba,Mg)2Al 16 O 24 :EU 2+ , (Ba,Mg)2Al 16 O 24 :EU 2+ , Mn 2+ , Y2O3Al2O3:Tb 3+ .

[0202] Another grouping by host compound includes halophosphate phosphors, phosphate phosphors, silicate phosphors, aluminate phosphors, borate phosphors, tungstate phosphors, and other phosphor chemical compositions.

[0203] Halophosphates include, by way of example: 3Ca3(PO4)2.Ca(F,Cl)2:Sb 3+ , 3Ca3(PO4)2.Ca(F,Cl)2:Sb 3+ / Mn 2+ , Sr 10 (PO4)6Cl2:Eu 2+ , (Sr, Ca) 10 (PO4)6Cl2:Eu2+ , (Sr, Ca) 10 (PO4)6.nB2O3:Eu 3+ , (Sr, Ca, Mg) 10 (PO4)6Cl2:Eu 2+ Examples of phosphate phosphorescent materials include: Sr2P2O7:Sn 2+ , (Sr,Mg)3(PO4)2:Sn 2+ , Ca3(PO4)2.Sn 2+ , Ca3(PO4)2:Tl + , (Ca,Zn)3(PO4)2:Tl + , Sr2P2O7:Eu 2+ , SrMgP2O7:Eu 2+ , Sr3(PO4)2:Eu 2+ , LaPO4:Ce 3+ , Tb 3+ , La2O3 . 0.2SiO2 . 0.9P2O5:Ce 3+ .Tb 3+ , BaO . TiO2 . P2O5. Silicate phosphorescent material, Zn2SiO4:Mn 2+ , CaSiO3:Pb 2+ / Mn 2+ , (Ba, Sr, Mg) . 3Si2O7:Pb 2+ , BaSi2O5:Pb 2+ , Sr2Si3O8 . 2SrCl2:Eu 2+ , Ba3MgSi2O8:Eu 2+ , (Sr,Ba)Al2Si2O8:Eu 2+ .

[0204] Aluminate phosphorescent materials include: LiAlO2:Fe 3+ , BaAlO 13 :EU 2+ , BaMgAl 16 O 27 :EU 2+ , BaMgAl 16 O 27 :EU 2+ / Mn 2+ , SrAl14 O 25 :EU 2+ , CeMgAl 11 O 19 :Ce 3+ / Tb 3+ .

[0205] Borate phosphorescent materials include: Cd2B2O5:Mn 2+ , SrB4O7F:Eu 2+ , GdMgB5O 10 :Ce 3+ / Tb 3+ , GdMgB5O 10 :Ce 3+ / Mn 3+ , GdMgB5O 10 :Ce 3+ / Tb 3+ / Mn 2+ .

[0206] Tungstate phosphorescent materials include: CaWO4, (Ca,Pb)WO4, MgWO4. Other phosphorescent materials include Y2O3:Eu 3+ , Y(V,P)O4:Eu 2+ , YVO4:Dy 3+ , MgGa2O4:Mn 2+ , 6MgO . As2O5:Mn 2+ , 3.5MgO . 0.5MgF2 . GeO2:Mn 4+ .

[0207] Activators associated with various doped phosphorescent materials include the following list: Tl + , Pb 2+ , Ce 3+ ,EU 2+ , WO4 2- , Sn 2+ , Sb 3+ , Mn 2+ , Tb 3+ ,EU 3+ , Mn 4+ , Fe 3+ .

[0208] In various embodiments, the luminescent center T1+ can be used in the following chemical compositions: (Ca,Zn)3(PO4)2:Tl + , Ca3(PO4)2:Tl + .

[0209] Similarly, the luminescent center Mn2+ can be used in the following chemical compositions: MgGa2O4:Mn 2+ , BaMgAl 16 O 27 :EU 2+ / Mn 2+ , Zn2SiO4:Mn 2+ , 3Ca3(PO4)2 . Ca(F,Cl)2:Sb 2+ / Mn 2+ , CaSiO3:Pb 2+ / Mn 2+ , Cd2B2O5:Mn 2+ , CdB2O5:Mn 2+ , GdMgB5O 10 :Ce 3+ / Mn 2+ , GdMgB5O 10 :Ce 3+ / Tb 3+ / Mn 2+ .

[0210] Furthermore, the luminescent center Sn 2+ is available in the following chemical compositions: Sr2P2O7:Sn 2+ , (Sr,Mg)3(PO4)2:Sn 2+ .

[0211] Luminescent center Eu 2+ It can also be used in the following chemical compositions: SrB4O7F:Eu 2+ , (Sr,Ba)Al2Si2O8:Eu 2+ , Sr3(PO4)2:Eu 2+ , Sr2P2O7:Eu 2+ , Ba3MgSi2O8:Eu 2+ , Sr 10 (PO4)6Cl2:Eu2+ , BaMgAl 16 O 27 :EU 2+ / Mn 2+ , (Sr, Ca) 10 (PO4)6Cl2:Eu 2+ .

[0212] Luminescent center Pb 2+ It can be used in the following chemical compositions: (Ba,Mg,Zn)3Si2O7:Pb 2+ , BaSi2O5:Pb 2+ , (Ba,Sr)3Si2O7:Pb 2+ .

[0213] Luminescent center Sb 2+ It can be used in the following chemical compositions: 3Ca3(PO4)2 . Ca(F,Cl)2:Sb 3+ , 3Ca3(PO4)2 . Ca(F,Cl)2:Sb 3+ / Mn 2+ .

[0214] The luminescent center Tb3+ can be used in the following chemical compositions: CeMgAl 11 O 19 :Ce 3+ / Tb 3+ , LaPO4:Ce 3+ / Tb 3+ , Y2SiO5:Ce 3+ / Tb 3+ , GdMgB5O 10 :Ce 3+ / Tb 3+ .

[0215] Luminescent center Eu 3+ It can be used in the following chemical compositions: Y2O3:Eu 3+ , Y(V,P)O4:Eu 3+ .

[0216] Luminescent center Dy 3+It can be used in the following chemical compositions: YVO4:Dy 3+ .

[0217] Luminescent center Fe 3+ It can be used in the following chemical compositions: LiAlO2:Fe 3+ .

[0218] Luminescent center Mn 4+ It can be used in the following chemical compositions: 6MgO . As2O5:Mn 4+ , 3.5MgO . 0.5MgF2 . GeO2:Mn 4+ .

[0219] Luminescent center Ce 3+ It can be used in the following chemical compositions: Ca2MgSi2O7:Ce 3+ and Y2SiO5:Ce 3+ .

[0220] Luminescent center WO4 2- It can be used in the following chemical compositions: CaWO4, (Ca,Pb)WO4, MgWO4.

[0221] Luminescent center TiO4 4- It can be used in the following chemical compositions: BaO . TiO2 . P2O5.

[0222] In various embodiments of the present invention, phosphorescent chemistries utilized with X-ray excitation can be used with or without an energy enhancement factor. Of particular interest are the kedges of these phosphorescent materials. Low energy excitation can result in strong emission in low kedge materials. Some of these chemistries and corresponding kedges include: BaFCl:Eu 2+ 37.38 keV BaSO4:Eu 2+ 37.38 keV CaWO469.48keV Gd2O2S:Tb 3+ 50.22 keV LaOBr:Tb 3+ 38.92 keV LaOBr:Tm 3+ 38.92 keV La2O2S:Tb 3+ 38.92 keV Y2O2S:Tb 3+ 17.04 keV YTaO467.42keV YTaO4:Nb 67.42keV ZnS:Ag 9.66keV (Zn,Cd)S:Ag 9.66 / 26.7keV

[0223] In one embodiment of the present invention, light from these materials (e.g., excited by high-energy particles including X-rays, gamma rays, protons, and electrons) can be modulated by including these materials in proximity to (including within) the color enhancement structures described herein. For example, in medical treatments where X-rays excite phosphorescence to photostimulate a patient's response, infrared radiation can be applied simultaneously with irradiation by high-energy particles to drive the resonance of the energy enhancement structures described herein, and the X-ray phosphors will enhance their emission in the presence of an increased electric field. In another example, in medical or scientific instruments, an electric field can be applied simultaneously with irradiation by high-energy particles to enhance the emission from these X-ray phosphors.

[0224] Electroluminescent Materials: Various materials used in the electroluminescence of the present invention, with or without an energy enhancement factor, can include, but are not limited to: 4,4',4''-Tris[phenyl(m-tolyl)amino]triphenylamine (m-MTDATA) N,N'-bis(3-methylphenyl)-N,N'-diphenylbenzidine (TPD) 4,4',4''-Tris[phenyl(m-tolyl)amino]triphenylamine (m-MTDATA) N,N'-bis(3-methylphenyl)-N,N'-diphenylbenzidine (TPD) Tris-(8-hydroxyquinoline)aluminum 2,4,6-tris(2-pyridyl)-s-triazine (TPT) [ka] 2,2',2''-(1,3,5-benzinetriyl)-tris(1-phenyl-1-H-benzimidazole)Alq [ka] 2,2',2''-(1,3,5-benzinetriyl)-tris(1-phenyl-1-H-benzimidazole) TPBI [ka] 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline, BCP2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline, BCP [ka]

[0225] Plasmonics Enhancement Structures: Figure 26 is a schematic diagram depicting an upconverter or downconverter material (i.e., a photoactive material) according to one embodiment of the present invention utilized in the color enhancement / enhancement structures described herein, with or without an energy enhancement factor. Figure 26 illustrates several structural configurations for placing a dielectric core upconverter or downconverter material (nanometer-sized scale) near a metal shell. Incident light of wavelength λ interacts with the upconverting dielectric core. The interaction of light λ with the dielectric core generates secondary radiation at a λ frequency having a wavelength shorter than λ and correspondingly higher energy than λ. While the exact physical mechanism of upconversion may depend on the specific upconversion material and process used in a particular application, the following description is provided for discussion and illustration purposes.

[0226] In the situation of Figure 26, when wavelength λ interacts with the dielectric core, three separate processes are well understood for the upconversion process involving trivalent rare earth ions. These three processes are: 1) Excited state absorption: Two photons are absorbed consecutively by the same ion, exciting it to one or more states. 2) Energy transfer upconversion, which is the transfer of excitation from one ion to another ion that is already in an excited state. 3) A multiphoton cooperative process, in which two nearby excited ions are collectively ejected from a virtual state.

[0227] Regardless of which of these processes occurs between the selected ion(s) and the host lattice, the end result will be photons of greater energy than the excitation energy being emitted from the host lattice due to the upconversion or downconversion process.

[0228] Thus, the particular ions to be activated (whether dopant ions or lattice host ions, such as in neodymium oxide) are selected based on the host material being processed, such that the dopant ions or dielectric core host ions are in an ionic state that is pumpable by the NIR source that generates the resulting radiation λ2.

[0229] Thus, in one embodiment, the present invention provides an upconversion or downconversion material configured to generate a second wavelength λ2 having higher or lower energy than the first wavelength λ1 upon exposure to a first wavelength λ1. The system can include a metallic structure (e.g., a metallic shell covering a portion of the nanoparticle) disposed in association with the nanoparticle. The system can also include an acceptor disposed in a medium proximate to the nanoparticle. When activated by the second wavelength λ2, the acceptor can fluoresce to generate visible light. In one embodiment of the present invention, the physical properties of the metallic structure (such as those depicted above and below in the figures) are set to values ​​such that the surface plasmon resonance of the metallic structure resonates at a frequency that provides spectral overlap with either the first wavelength λ1 or the second wavelength λ2. This system, with the metallic structure disposed in association with the upconversion or downconversion nanoparticle, becomes a converter utilized in the color enhancement / boosting structures described herein.

[0230] Within the context of the present invention, the term "physical property" of a metal shell or core may refer to any property of the metal itself or the dimensions or shape of the shell or core that affects the surface plasmon resonance frequency. Such physical properties may include, but are not limited to, the electrical conductivity, radial dimensions, chemical composition, or crystalline state of the metal shell or core.

[0231] In various embodiments, the metallic structure can be a metallic shell encapsulating at least a portion of the nanoparticles within the metallic shell, where the conductivity, radial dimension, or crystalline state of the metallic shell sets a surface plasmon resonance in the metallic structure to resonate at a frequency that provides spectral overlap with either the first wavelength λ1 or the second wavelength λ2. In various embodiments, the metallic structure can be a multi-layer metallic shell encapsulating at least a portion of the nanoparticles within the metallic shell, where the conductivity, radial dimension, or crystalline state of the metallic shell sets a surface plasmon resonance in the metallic structure to resonate at the first wavelength λ1 and the second wavelength λ2. This feature allows for emission of λ1 and amplification of λ2.

[0232] In various embodiments, the metallic structures can be metal particles present in one or more multi-structures. These multi-structures can have a variety of shapes, including, for example, spheres, spheroids, rods, cubes, triangles, pyramids, pillars, crescents, tetrahedrons, stars, or combinations thereof, and are disposed adjacent to the nanoparticles. The conductivity, dimensions (e.g., lateral dimensions or thickness), or crystalline state of the metallic structures configure the surface plasmon resonance in the metallic particles or rods to resonate at a frequency that provides spectral overlap with either the first wavelength λ1 or the second wavelength λ2. Such shapes are described in the figures of this application and in the figures of U.S. Application No. 12 / 401,478, which are incorporated by reference in their entireties. The choice of shape can affect the frequency of the surface plasmon resonance. The plasmon bandwidth is known to vary with the shape of the nanoparticle (e.g., prolate spheroid or oblate spheroid). The article "Spectral bounds on plasmon resonances for Ag and Au prolate and oblate nanospheroids," in the Journal of Nanophotonics, Vol. 2, pp. 29501 (September 26, 2008), the entire contents of which are incorporated by reference, shows the plasmon resonance shifts for Ag shaping and Au shaping for prolate and oblate spheroids. In one embodiment of the present invention, as the aspect ratio of the metal structures of the present invention increases, the prolate spheroid resonances are red-shifted relative to an unbounded sphere (under the assumption of the Drude dispersion model). Meanwhile, as the spheroids become flatter, the oblate spheroid resonances "blue-shift," but reach a limit.

[0233] In various embodiments, the metallic structure disposed in association with the upconversion or downconversion nanoparticle can be a metallic structure disposed within the nanoparticle, where the conductivity or dimensions (e.g., lateral dimensions or thickness) of the metallic structure set the surface plasmon resonance in the metallic structure to resonate at a frequency that provides spectral overlap with either the first wavelength λ1 or the second wavelength λ2. In various embodiments, the metallic structure can be a metallic multilayer structure disposed within the nanoparticle, where the conductivity or dimensions (e.g., lateral dimensions or thickness) of the metallic structure set the surface plasmon resonance in the metallic structure to resonate at the frequencies of the first wavelength λ1 and the second wavelength λ2. This function allows for the emission of λ1 and again allows for the amplification of λ2.

[0234] In another embodiment, the present invention provides a nanoparticle structure comprising a sub-1000 nm dielectric core and a metallic structure disposed in association with the nanoparticle. The dielectric core comprises at least one of Y2O3, Y2O2S, NaYF4, NaYbF4, YAG, YAP, Nd2O3, LaF3, LaCl3, La2O3, TiO2, LuPO4, YVO4, YbF3, YF3, Na-doped YbF3, or SiO2. In certain embodiments, such nanoparticle structures can exhibit surface plasmon resonance in the metallic structure to enhance light upconversion from a first wavelength λ1 to a second wavelength λ2.

[0235] As described above, the shell (or other structure) is specifically designed with a layer thickness (or, e.g., lateral dimension) to enhance the photon upconversion process through plasmon enhancement. The shell thickness (or other physical property) is "tuned" to the absorption process by having a dimension such that the plasmons (i.e., electron oscillations) within the shell have a resonance at a frequency that results in spectral overlap with the target absorption band. Thus, if upconversion is stimulated by NIR light at 980 nm, the shell thickness is "tuned" to a thickness such that the plasmon resonance also resonates at a frequency of 980 nm (or nearby, as plasmon resonances are typically broad at these wavelengths).

[0236] The plasmon resonant shell can be made of a number of transition metals, including, but not limited to, gold, silver, platinum, palladium, nickel, ruthenium, rhenium, copper, and cobalt, or combinations, alloys, or layers thereof. Such plasmon resonant shells can also be made of combinations of metals and non-metals. When formed from gold nanoshells, the recommended thickness for resonating with 980 nm light is approximately 3.5 nm, surrounding an 80 nm upconverting core, as predicted by an extension of Mie theory calculations. (See Jain et al., Nanolett. 2007, 7(9), 2854, the entire contents of which are incorporated herein by reference.) Figure 27, reproduced from Jain et al., demonstrates the invention's ability to "tune" the metal shell to have spectral overlap with the excitation and / or emission radiation wavelengths.

[0237] In one embodiment of the present invention, the metal structure disposed in association with the upconversion or downconversion nanoparticles may be an alloy, such as, for example, an Au:Ag alloy. The alloy content may be configured to tune the frequency of the surface plasmon resonance. In one embodiment of the present invention, the metal structure may be an alloy, such as, for example, a Pt:Ag alloy. The alloy content may be configured to tune the frequency of the surface plasmon resonance. In one embodiment of the present invention, the metal structure may be an alloy, such as, for example, a Pt:Au alloy. The alloy content may be configured to tune the frequency of the surface plasmon resonance.

[0238] In one embodiment of the present invention, the converter nanoparticles can be an alloy of two or more materials. In this embodiment, the alloy can have a composition of two or more materials, where the composition is set to a value such that excitation of the alloy at a first wavelength λ1 produces emission at a second wavelength λ2. In one embodiment of the present invention, the nanoparticles can be an alloy of zinc sulfide and zinc selenide. In one embodiment of the present invention, the nanoparticles can be an alloy of zinc sulfide and cadmium sulfide.

[0239] In one embodiment of the invention, the zinc sulfide and zinc selenide nanoparticle alloys can have an alloy content designed to provide a predetermined surface plasmon resonance. In one embodiment of the invention, the zinc sulfide and cadmium sulfide nanoparticle alloys can have an alloy content designed to provide a predetermined surface plasmon resonance.

[0240] Some techniques for producing nanoparticles and nanoalloys suitable for the present invention are described in their entirety in the following documents, which are incorporated herein in their entirety: U.S. Patent Nos. 7,645,318, 7,615,169, 7,468,146, 7,501,092, U.S. Patent Application Publication Nos. 2009 / 0315446, 2008 / 0277270, 2008 / 0277267, 2008 / 0277268, and WO2009 / 133138.

[0241] In one embodiment of the present invention, the thickness of the metal shell disposed in association with the upconversion or downconversion nanoparticle is set according to the absorption frequency (or emission frequency, as the case may be) of the particular dopant ion in the dielectric core that enhances the overall efficiency of the upconverted light emission process. Thus, the shell thickness can be thought of as a tool to enhance the absorption at λ in one example, the emission at λ in another example, or as an enhancement feature that in combination enhances the overall net process in other situations.

[0242] Additionally, plasmon-phonon coupling can be used to lower the resonant frequency by tuning the band some distance off resonance. This may be useful for optimizing the resonant energy transfer process for the purpose of shifting the output color to a color desired for the surface being painted, stained, or displayed. In one example, Figure 27 shows an example of plasmon resonance shift as a function of shell thickness.

[0243] Here, in one embodiment of the present invention, the ability to generate stimulated emission at a targeted wavelength or color or energy is complemented by the ability to engineer nanoparticles with engineered absorption bands. Such absorbing materials may further function to improve the monochromaticity of light observed from, for example, paints, inks, dyes, or otherwise reflective surfaces treated with the color enhancing compositions of the present invention.

[0244] Details of the preparation of this nanoparticle system are contained in U.S. Application No. 12 / 725,108, the entire contents of which are incorporated herein by reference. The absorption spectrum of YO alone (lower trace) is quite featureless, showing a triangular and shallow absorption band near 200 nm associated with scattering and absorption by YO nanoparticles extending into the visible portion of the spectrum. On the other hand, the gold-coated YO (upper trace) shows a strong absorption band at 546 nm, characteristic of the plasmonic resonance band due to the gold shell around the YO core. The red-shift of the plasmon absorption to 546 nm is consistent with the presence of a gold shell around the dielectric core.

[0245] In one embodiment of the present invention, the converter material for the upconverter dielectric core can include a wide variety of dielectric materials, as described above. In various embodiments of the present invention, the upconverter dielectric core more specifically includes an oxide material doped with a lanthanide. Lanthanides include lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu). Other suitable dielectric core materials include non-lanthanide elements such as yttrium (Y) and scandium (Sc). Thus, suitable dielectric core materials include Y2O3, Y2O2S, NaYF4, NaYbF4, Na-doped YbF3, YAG, YAP, Nd2O3, LaF3, LaCl3, La2O3, TiO2, LuPO4, YVO4, YbF3, YF3, or SiO2. These dielectric cores can be doped with Er, Eu, Yb, Tm, Nd, Tb, Ce, Y, U, Pr, La, Gd, and other rare earth species or combinations thereof.

[0246] Lanthanides usually exist as trivalent cations, in which case their electron configuration is (Xe)4f n and n is 1(Ce 3+) to 14(Lu 3+ ) Transitions within the F-type manifold are responsible for many of the photophysical properties of lanthanide ions, such as long-lived emission and sharp absorption and emission lines. F-type electrons are protected from external perturbations by filled 5s and 5p orbitals, resulting in line-shaped spectra. F-F type electronic transitions are Laporte forbidden, resulting in long excited-state lifetimes in the microsecond to millisecond range.

[0247] Therefore, examples of doped materials in the present invention include oxides such as yttrium oxide, neodymium oxide, and aluminum oxide, as well as yttrium sodium fluoride and nanocrystalline perovskites and garnets, such as yttrium aluminum garnet (YAG) and yttrium aluminum perovskite (YAP). Of these materials, doping is required for some, but not all, of these materials to promote upconversion efficiency. In various embodiments of the present invention, the host nanocrystals are doped with trivalent rare earth lanthanide ions from the lanthanide series elements listed above.

[0248] More specifically, in various embodiments of the present invention, these dopant pairs are introduced to make more energy states more accessible in the host crystal. The activation and pumping of these energy states strictly follows the principles described above. The doping concentration in the present invention can range from approximately 0.2% to 20% per ion entering the host lattice, or by weight or mole percent variation. The efficiency of the upconversion process in specific bands of these materials can be modulated by the doping percentage to induce and enhance targeted emission. Lanthanide-doped upconverters can use the following molar percent dopant compositions, but are not limited to: 5% Er, 10% Yb, 0.2% Tm + 3% Yb, and 1% Er + 10% Yb.

[0249] The size of the nanocrystals also affects the efficiency of the upconversion process, since larger nanocrystals accommodate more sites for dopant ions in the host lattice, resulting in higher emission from the same doped host than smaller nanocrystals. While the dopant percentages listed above are not strictly fixed, these numbers provide a basic guide for typical proportions used to achieve specific dielectric core materials of the present invention.

[0250] Also, in one embodiment of the present invention, some of these host crystals (e.g., neodymium oxide) may not require special doping to facilitate upconversion, as was seen in one example with Nd2O3 at an excitation wavelength of 587 nm, which produced emissions at 372 nm, 402 nm, and 468 nm. See Que, W et al., Journal of Applied Physics 2001, vol. 90, pg. 4865, the entire contents of which are incorporated herein by reference. In one embodiment of the present invention, neodymium oxide is doped with Yb 3+ Doping with Nd 3+ ions at lower energy Yb 3+ Upconversion is enhanced by sensitizing with an activator.

[0251] In one embodiment of the present invention, the dielectric core is coated, for example with a metal shell, to enhance electron-phonon coupling and thereby increase the upconversion or downconversion efficiency, as described above. In another embodiment of the present invention, the shell can include a SiO and / or TiO coating, which, in one embodiment, is coated on doped YO upconverting nanoparticles, thereby potentially increasing the upconversion efficiency compared to uncoated nanocrystals. In another embodiment of the present invention, the shell can include a SiO and / or TiO coating, which, in one embodiment, is coated on doped YO downconverting nanoparticles, thereby potentially increasing the downconversion efficiency compared to uncoated nanocrystals. Furthermore, in one embodiment of the present invention, the coating can be a polymer. In one embodiment, the coating is provided on a NaYF:Ln / NaYF dielectric core. Such a coating can increase the upconversion efficiency compared to uncoated upconverters.

[0252] In another embodiment of the present invention, the phonon modes of undoped host lattice (e.g., YO) nanocrystals are modulated by, for example, Au, Ag, Pt, and Pd shells of various thicknesses. In various embodiments of the present invention, an upconverter dielectric core-shell system includes the following upconverting nanocrystals: YO:Ln with a NaYF shell; YO:Ln with an Au(Ag,Pt) shell; NaYF:Ln with a YO shell; and NaYF:Ln with an Au(Ag,Pt) shell. In this system, the core diameter and the outer / inner diameter of the metal coating can be configured to anticipate tunable plasmon mode overlap.

[0253] In other embodiments discussed below, metal coatings or metal structures disposed in association with upconversion or downconversion nanoparticles can reside within the dielectric, and the relative position of the metal structures to the dielectric structure can enhance plasmon resonance. These structures with internal metal structures are sometimes referred to as metal-core upconverters or metal-core downconverters. Metal-core technology for energy conversion is useful because it utilizes metal nanoparticles with improved surface morphology compared to shell coatings on core dielectrics. The metal or metal alloy of the internal-core metal energy converter can be selected to tailor its plasmonic activity. These structures with external metal structures are sometimes referred to as core upconverters or core downconverters.

[0254] In various embodiments of the present invention, the dielectric core of an upconverter or downconverter can be coated with a thiol-terminated silane to provide a coating of SiO around the core with similar reactivity to YO. In one embodiment of the present invention, the above methodology is used to synthesize core-shell nanoparticles, such as YO:Ln with a NaYF shell, YO:Ln with an Au(Ag,Pt) shell, NaYF:Ln with a YO shell, or NaYF:Ln with an Au(Ag,Pt) shell, where the core-shell diameter can vary from 2 to 20 nm. In these material systems, a tuned ratio of core-to-shell diameters can enable plasmon-phonon resonance, amplifying the absorption and / or upconverted emission of NIR light. In these material systems, controlling the core-shell diameter is one factor determining size-dependent effects and subsequent tuning of the plasmon-phonon resonance.

[0255] In one embodiment of the present invention, the upconverter dielectric core can be a mixed core-shell material, including, for example, semiconducting YO and NaYF cores doped with various Ln-series metals, which have been shown to have high upconversion efficiencies. These doped YO and NaYF cores have shells of Au (Ag, Pt, Pd) or undoped YO and NaYF matrices, which have the potential to enhance or tune the phonon modes required for energy transfer in the upconversion process. Solubility can be enhanced by the addition of, for example, thiolated organics (Au shell), organic chain triethanolsilane (YO shell), and trioctylphosphine-oleic amine (NaYF shell). All core-shell nanoparticles can be further solubilized in colloidal suspensions by adding triarginine peptides, polyethylene glycol, and polyethyleneimine surfactants.

[0256] Figure 28A shows some of the various embodiments of converter structures of the present invention that can be designed: (a) a structure comprising upconverter (UC) molecules bound to metal (gold) nanoparticles; (b) a structure comprising UC-containing nanoparticles capped with metal nanoparticles; (c) a metal nanoparticle capped with a UC-containing nanocap; (d) a UC-containing nanoparticle capped with a metal nanocap; (e) a metal nanoparticle capped with a UC nanoshell; (f) a UC-containing nanoparticle capped with a metal nanoshell; and (g) a UC-containing nanoparticle capped with a metal nanoshell with a protective coating layer.

[0257] The configuration (although shown with UC-containing materials in FIG. 28A) is applicable to enhancing downconverting materials such as quantum dots or phosphorescent materials described herein. Additionally, in one embodiment of the present invention, a dielectric spacer (e.g., a silicate, as described below) can be used with the structure of FIGS. 6A-b to space particle-type metal structures. In another embodiment of the present invention, a dielectric spacer can be used with the structure of FIG. 28A to space metal layers, whether these layers are partial or continuous metal layers. See the schematic diagram in FIG. 28B.

[0258] In various embodiments of the present invention, the multilayer metallic nanoshells discussed herein have the potential to electromagnetically enhance two spectral regions. Thus, the metallic structures of the present invention can be used in upconversion mode to enhance both excitation at wavelength λ1 and emission at wavelength λ2. This feature can also be used in downconversion to primarily enhance emission at wavelength λ2, potentially for excitation at wavelength λ1.

[0259] Such metallic structures in various embodiments of the present invention include conductive materials made of, for example, metals, or doped glasses or doped semiconductors. These conductive materials can be in the form of pure or nearly pure elemental metals, alloys of such elemental metals, or layers of conductive materials, regardless of constituents. The conductive materials can include non-metallic materials as minor constituents that do not render the composite insulating at the level of incorporation (as described above).

[0260] Similarly, in various embodiments of the present invention, the up- or down-converting material can include at least one of a dielectric, a glass, or a semiconductor. The up- or down-converting material can include an alloy of two or more dielectric materials, an alloy of two or more glasses, or an alloy of two or more semiconductors.

[0261] Thus, Figure 28A depicts an embodiment of the present invention in which a dielectric core is supplemented with a shell. The shell can include a metal layer of a predetermined thickness. The metal layer can include materials such as nickel, gold, iron, silver, palladium, platinum, copper, and combinations thereof. The metal layer can also be made of a combination of metal and non-metal. The shell acts as a plasmonic shell, allowing surface plasmons to form in the metal between the dielectric core and the external environment, which acts as the external dielectric. The shell may not be a complete shell (as shown). Partial metal shells or metal shells of various thicknesses are also permissible in the present invention.

[0262] As explained below, the metal shell in another embodiment of the invention acts as a scattering center for UV light, which, even if absorbed by the paint or coating layer, at least contributes to localized heating of the paint or coating layer material and is scattered from the paint or coated layer.

[0263] Figure 28C shows yet another embodiment of plasmonics-active nanostructures with engineerable upconverting (UC) materials: (a) metal nanoparticles, (b) UC nanoparticle cores covered with metal nanocaps, (c) spherical metal nanoshells covering UC spheroid cores, (d) flat metal nanoshells covering UC spheroid cores, (e) metal nanoparticle cores covered with UC nanoshells, (f) metal nanoshells with protective coating layers, (g) multi-layered metal nanoshells covering UC spheroid cores, (h) multi-nanoparticle structures, (i) metal nanocubes and nanotriangles / nanoprisms, and (j) metal cylinders.

[0264] Figure 28D shows yet another embodiment of a plasmonics-active nanostructure with an upconverting material having linked photoactive (PA) molecules that can be engineered. For example, in the case of psoralen (as the PA molecule), the length of the linker between the PA molecule and the UC material or metal surface is tailored so that the PA molecule is long enough to be active (attach to DNA) and short enough to allow efficient excitation of light from the UC to efficiently excite the PA molecule. Figure 28D shows (a) a PA molecule bound to a UC nanoparticle, (b) a nanoparticle comprising a UC material covered with metal nanoparticles, (c) a metal nanoparticle covered with a UC material nanocap, (D) a nanoparticle comprising a UC material covered with a metal nanocap, (e) a metal nanoparticle covered with a UC material nanoshell, (f) a nanoparticle comprising a UC material covered with a metal nanoshell, and (g) a nanoparticle comprising a UC material covered with a metal nanoshell with a protective coating layer.

[0265] The plasmonic effect is advantageous in the upconverter and downconverter structures of the present invention. The plasmonic effect can increase the local intensity of light received or emitted from the upconverter and / or downconverter structures of the present invention. The plasmonic effect can occur throughout the electromagnetic range when appropriate nanostructures, nanoscale dimensions, and metal types are used. The plasmonic effect can occur across a wide range of the electromagnetic spectrum, from gamma rays and X-rays to ultraviolet, visible, infrared, microwave, and radio frequency energy. However, for practical reasons, visible and NIR light are used with metallic structures, such as silver and gold nanoparticles, because the plasmonic resonances of silver and gold occur in the visible and NIR regions, respectively.

[0266] In various embodiments, nanoparticles of neodymium- and ytterbium-doped yttrium oxide, europium- and ytterbium-doped yttrium oxide, and any combination of rare earth trivalent ions doped into neodymium oxide nanocrystals can be used. While the dual-doped yttrium oxide compositions of neodymium and ytterbium, and dual-doped europium and ytterbium are new to the yttrium oxide host lattice, such dual-doped systems have been shown to work in other host lattices, such as YAG.

[0267] These dual-doped lanthanide glasses have been shown to efficiently upconvert in bulk materials, allowing for the creation of novel upconverter structures at the nanoscale. These yttrium oxide nanostructures of the present invention offer advantages. Small-scale synthesis methodologies for creating nanoscale yttrium oxide are easier to control and manufacture with yttrium oxide than with YAG. The yttrium oxide host structure scintillates via downconversion. For example, these combinations of dopants in yttrium oxide can provide a predetermined emission color for the yttrium oxide nanocrystals for the color transfer of the present invention.

[0268] In one embodiment of the present invention, the dual dopant allows excitation of either ion in the host glass. For example, excitation with 980 nm light excites ytterbium ions. Energy transfer from one excited state of the ytterbium ions to another dopant provides a mechanism for upconversion emission of light in the visible and NIR spectral regions.

[0269] Upconversion phosphors can be used that have chemical compositions similar to the downconversion fluorescent materials discussed above. Upconversion phosphors can include laser dyes, e.g., small organic molecules that can be excited by absorption of at least two infrared photons with visible light emission. Upconversion phosphors can include fluorescent polymers, e.g., a class of polymers that can be excited by absorption of at least two infrared photons with visible light emission. Upconversion phosphors can include inorganic or ceramic particles or nanoparticles, including conventional upconversion phosphors (e.g., metal fluorides, metal oxides) that can be excited by absorption of at least two infrared photons with visible light emission. Upconversion phosphors can include semiconductor particles, including nanoparticles such as II-VI or III-V compound semiconductors, such as quantum dots, as described in detail above under "downconversion" semiconductors.

[0270] Fluorescent upconversion inorganic phosphorescent materials can include, but are not limited to, metal oxides, metal halides, metal chalcogenides (e.g., sulfides), or hybrids thereof, such as metal oxohalides and metal oxochalcogenides. Fluorescent upconversion inorganic phosphorescent materials are typically rare earth elements (Yb 3+ , Er 3+ , Tm 3+ Some example hosts include, but are not limited to, NaYF4, YF3, BaYF5, LaF3, La2MoO8, LaNbO4, and LnO2S, where Ln is a rare earth element such as Y, La, or Gd.

[0271] These converters (and other energy converters described herein that receive energy and produce light or electron emission) can optionally include any of the energy-magnification structures described above.

[0272] In various embodiments of the present invention, energy converters can be used with the above-mentioned energy enhancement factors for color enhancement. In some embodiments, the converters are for upconversion of light, e.g., from the IR range to visible electromagnetic radiation, and for downconversion of light, e.g., from the UV range to visible electromagnetic radiation. In various embodiments, the present invention upconverts energy, preferably light in the visible spectrum. The present invention encompasses a variety of applications that include up- and downconversion materials, with or without energy enhancement factors, to enhance the color of displayed objects. These application areas can include paints for signs, walls, cars, buildings, boats, and airplanes. These application areas include display monitors, computer monitors, telephone displays, watch dials, and instrument dials, to name a few.

[0273] Among various materials, luminescent nanoparticles have attracted increasing technological and industrial interest. In the context of the present invention, nanoparticles refer to particles having a size of less than 1 micron. Although the description of the present invention describes a specific example using nanoparticles, the present invention in many embodiments is not limited to particles having a size of less than 1 micron. However, in many embodiments, the size range of less than 1 micron, particularly less than 100 nm, produces properties of special interest, such as emission lifetime, luminescence quenching, luminescence quantum efficiency, and concentrated quenching, for example, diffusion, penetration, and dispersion into media where larger particles do not move.

[0274] In various embodiments, the present invention can use a wide variety of down-conversion materials (or mixtures of down-conversion materials), with or without energy enhancement factors, to enhance the light of a particular color that can be observed by a viewer. These down-conversion materials can include quantum dots, semiconductor materials, alloys of semiconductor materials, scintillation and phosphorescent materials, materials that exhibit X-ray excited luminescence (XEOL), organic solids, metal complexes, inorganic solids, crystals, rare earth materials (lanthanides), polymers, scintillators, phosphorescent materials, and materials that exhibit excitation properties. Thus, down-conversion materials for enhancing color emission can convert energy from one of ultraviolet light, X-rays, and high-energy particles to visible light. Down-conversion materials for enhancing color emission can convert energy from higher-energy visible light to lower-energy visible light, with or without energy enhancement factors.

[0275] In one embodiment of the present invention, quantum dot mixtures with or without energy enhancement factors can be used for color enhancement. Quantum dots are generally nanometer-sized particles, and the energy state of the quantum dot material depends on the size of the quantum dot. For example, quantum dots are known to be semiconductors whose conductive properties are closely related to the size and shape of the individual crystallites. Generally, the smaller the crystallite size, the larger the band gap, i.e., the greater the energy difference between the highest valence band and the lowest conduction band. Therefore, more energy is required to excite the dot, and at the same time, more energy is released when the crystallite returns to its resting state. In fluorescent dye applications, this equates to a higher frequency of light emitted after excitation of the dot as the crystallite size decreases, resulting in a color shift from red to blue. Quantum dots represent one way to downconvert ultraviolet light in the spectrum to a target color emission, such as green emission. Quantum dots represent one way to downconvert blue light in the spectrum to a target color emission, such as green emission.

[0276] As described in U.S. Patent No. 6,744,960 (the entire contents of which are incorporated by reference), quantum dots of different sizes produce emissions of different colors. In that work, quantum dots applicable to the present invention can comprise a variety of materials, including semiconductors such as zinc selenide (ZnSe), cadmium selenide (CdSe), cadmium sulfide (CdS), indium arsenide (InAs), and indium phosphide (InP). Another suitable material is titanium dioxide (TiO2). The size of the particles, i.e., quantum dots 18, can range from approximately 2 to 10 nm. Because the size of these particles is so small, quantum physics applies to many of the electrical and optical properties of quantum dots. One such result of applying quantum mechanics to quantum dots 18 is that quantum dots absorb a wide spectrum of light wavelengths and re-emit radiation with wavelengths longer than the wavelength of the absorbed light. The wavelength of the emitted light is determined by the size of the quantum dot. For example, a 5.0 nm diameter CdSe quantum dot emits radiation with a narrow spectral distribution centered at approximately 625 nm, while a 2.2 nm sized CdSe quantum dot 18 emits light with a central wavelength of approximately 500 nm. Semiconductor quantum dots including CdSe, InP, and InAs can emit radiation with central wavelengths ranging from 400 nm to approximately 1.5 μm. Titanium dioxide (TiO2) also emits in this range. The linewidth, or full width at half maximum (FWHM), of the emission of these semiconductor materials can range from approximately 20 to 30 nm. To produce this narrowband emission, the quantum dot simply needs to absorb light with a wavelength shorter than the wavelength of the light emitted by the dot. For example, for a 5.0 nm diameter, light from a CdSe quantum dot with a wavelength shorter than about 625 nm will be absorbed and produce an emission at about 625 nm, while a 2.2 nm quantum dot containing CdSe light with a wavelength shorter than about 500 nm will be absorbed and re-emitted at about 500 nm, although in practice the excitation or pump radiation will be at least about 50 nanometers shorter than the emitted radiation.

[0277] Specifically, in one embodiment of the present invention, quantum dot mixture (QDM) coatings can be deposited using sol-gel techniques using CVD and / or standard precipitation techniques, with or without energy enhancement factors. QDM coatings can be made with silicate structures that do not reduce UV output. Within the silicate family, silica (SiO2) is suitable for maximizing UV transmission through the coating. The coating can further include a second layer of a biocompatible glass. Such biocompatible glass and glass-ceramic compositions can include calcium, lanthanides or yttrium, silicon, phosphorus, and oxygen. Other biocompatible materials and techniques are described in the following patents, which are incorporated herein in their entireties: U.S. Patent Nos. 5,034,353, 4,786,617, 3,981,736, 3,922,155, 4,120,730, and U.S. Patent Application Nos. 2008 / 0057096, 2006 / 0275368, and 2010 / 0023101.

[0278] Furthermore, the down-conversion materials of the present invention described herein can be coated with an insulating material, such as silica, which reduces the possibility of any chemical interaction between the light-emitting particles and the medium in which they are contained. These and other conversion materials described herein can be used with or without an energy enhancement factor. One of the major limiting factors for biocompatible applications of inorganic nanoparticles is their toxicity. Generally speaking, all semiconductor nanoparticles are toxic to a greater or lesser extent. For biocompatible applications, nanoparticles with as low toxicity as possible are desirable. Otherwise, the nanoparticles must remain isolated from the medium. Pure TiO2, ZnO, and Fe2O3 are biocompatible. ZnS, CAS, BaS, SrS, and Y2O3 have low toxicity, while CdTe and CdSe are toxic. Furthermore, the toxicity of nanoparticles can be reduced by adding inorganic stabilizers such as TGA or Eu 2+ , Cr 3+ or Nd 3+Another suitable down-conversion material that is likely to be the most biocompatible is zinc sulfide, ZnS:Mn 2+ , iron oxide, titanium oxide, zinc oxide, zinc oxide with small amounts of Al2O3, and zeolite-encapsulated AgI nanoclusters. For non-medical applications where toxicity may not be a significant concern, the following materials (and those listed elsewhere) may be suitable: thulium-activated lanthanum and gadolinium oxyhalides, Er 3+ Doped BaTiO3 nanoparticles, Yb 3+ Doped CsMnCl3 and RbMnCl3, BaFBr:Eu 2+ nanoparticles, cesium iodide, bismuth germanate, cadmium tungstate, and divalent Eu-doped CsBr.

[0279] In various embodiments of the present invention, the following light-emitting polymers are also suitable as conversion materials, with or without energy enhancement factors: poly(phenylene ethynylene), poly(phenylene vinylene), poly(p-phenylene), poly(thiophene), poly(pyridyl vinylene), poly(pyrrole), poly(acetylene), poly(vinyl carbazole), poly(fluorene), etc., as well as copolymers and / or derivatives thereof.

[0280] In various embodiments of the present invention, the following materials can be used similarly to those detailed in U.S. Patent No. 7,090,355, the entire contents of which are incorporated herein by reference. For down-conversion, the following materials can be used, with or without an energy enhancement factor: inorganic or ceramic phosphors or nanoparticles, including, but not limited to, metal oxides, metal halides, metal chalcogenides (e.g., metal sulfides), or hybrids thereof, such as metal oxohalides and metal oxochalcogenides; laser dyes and organic small molecules, and fluorescent organic polymers; semiconductor nanoparticles, such as semiconductors of II-VI or III-V compounds, e.g., fluorescent quantum dots; organometallic molecules containing a metal center, e.g., at least rare earth elements (e.g., Eu, Tb, Ce, Er, Tm, Pr, Ho), transition metal elements, such as Cr, Mn, Zn, Ir, Ru, V, and main group elements, such as B, Al, and Ga. The metal elements are chemically bound to organic groups to prevent fluorescence quenching from the host or solvent. Phosphorescent materials can be used, including garnet series phosphorescent materials: Ce-doped (Y m A 1-m )3(Al n B 1-n )5O 12 , where 0≦m, n≦1, where A includes other rare earth elements and B includes B and Ga. Additionally, phosphorescent materials containing metal silicate, metal borate, metal phosphate, and metal aluminate hosts can be used. Furthermore, nanoparticle phosphorescent materials containing common rare earth elements (Eu, Tb, Ce, Dy, Er, Pr, Tm, etc.) and transition or main group elements (Mn, Cr, Ti, Ag, Cu, Zn, Bi, Pb, Sn, Ti) can be used as fluorescence activators. Materials such as Ca, Zn, Cd in tungstates, metal vanadates, and ZnO can be used with or without energy enhancement factors.

[0281] Commercially available laser dye materials, with or without energy enhancement factors, from several laser dye vendors, including Lambda Physik and Exciton, can also be used. Some preferred laser dye classes include pyrromethenes, coumarins, rhodamines, fluoresceins, and other aromatic hydrocarbons and their derivatives. Additionally, there are many polymers containing unsaturated carbon-carbon bonds that also function as fluorescent materials and have numerous optical and fluorescent applications. For example, MEH-PPV and PPV have been used in optoelectronic devices such as polymer light-emitting diodes (PLEDs). These fluorescent polymers can be used directly as the fluorescent layer in transparent 2-D display screens.

[0282] As mentioned above, semiconductor nanoparticles (e.g., quantum dots) can be used with or without energy enhancement factors. The term "semiconductor nanoparticle" in the art refers to inorganic crystallites with diameters between 1 nm and 1000 nm, preferably between 2 nm and 50 nm. Semiconductor nanoparticles can emit electromagnetic radiation upon excitation (i.e., they are luminescent). Nanoparticles can be homogeneous nanocrystals or composed of multiple shells. For example, nanoparticles can include a "core" of one or more first semiconductor materials surrounded by a "shell" of a second semiconductor material. The core and / or shell may be semiconductor materials, including, but not limited to, II-VI (ZnS, ZnSe, ZnTe, CdS, CdSe, CdTe, HgS, HgSe, HgTe, MgS, MgSe, MgTe, CaS, CaSe, CaTe, SrS, SrSe, SrTe, BaS, BaSe, BaTe, etc.) and III-V (GaN, GaP, GaAs, GaSb, InN, InP, InAs, InSb, etc.) and IV (Ge, Si, etc.) materials, and alloys or mixtures thereof.

[0283] Fluorescent organometallic molecules containing rare earth or transition element cations can be used in downconversion materials, with or without an energy enhancement factor. Such molecules include rare earth metal centers such as Eu, Tb, Er, Tm, and Ce protected with organic chelating groups. The metal centers can also include transition elements such as Zn, Mn, Cl, and Ir, as well as main group elements such as B, Al, and Ga. Such organometallic molecules are readily soluble in liquid or transparent solid host media. Some examples of such fluorescent organometallic molecules include: 1. tris(dibenzoylmethane)mono(phenanthroline)europium(III), 2. tris(8-hydroxyquinoline)erbium, 3. tris(1-phenyl-3-methyl-4-(2,2-dimethylpropan-1-yl)pyrazolin-5-one)terbium(III), 4. bis(2-methyl-8-hydroxyquinolato)zinc, and 5. diphenylborane-8-hydroxyquinolate.

[0284] Specific examples of red-emitting down-conversion materials include those described above and europium complexes such as those described in Japanese Patent Publication No. 2003-26969, in which a β-diketone ligand is coordinated to europium to form a europium complex capable of red fluorescence. Other specific examples of rare earth element complexes include complexes containing lanthanum (Ln), europium (Eu), terbium (Tb), and gadolinium (Gd), and combinations thereof. Europium (Eu) complexes can emit red fluorescence when irradiated with ultraviolet light having a wavelength ranging from 365 nm to 410 nm. Terbium (Tb) can emit green fluorescence when irradiated with ultraviolet light having a wavelength of 365 nm.

[0285] In other down-conversion embodiments, with or without an energy enhancement factor, the down-conversion material that emits red light may include europium, the light-emitting particles that emit green light may include terbium, and the light-emitting particles that emit blue or yellow light may include cerium (and / or thulium). In up-conversion embodiments, the up-conversion material that emits red light may include praseodymium, the light-emitting particles that emit green light may include erbium, and the light-emitting particles that emit blue light may include thulium. In embodiments, the conversion material may be light-emitting particles comprised of fluorescent molecules that emit different colors (e.g., red, green, and blue). In embodiments, the conversion material may be light-emitting particles comprised of pure organic or organometallic dyes, with or without an energy enhancement factor.

[0286] In addition to rare earth complex combinations, such as a combination of a europium complex and a terbium complex, it is also possible to employ a combination of a europium complex and an uncomplexed green-emitting phosphor, or a combination of a terbium complex and an uncomplexed red-emitting phosphor.

[0287] Other downconverter materials with or without energy enhancement factors include, for example, ZnS, PbS, SbS3, MoS2, PbTe, PbSe, BeO, MgO, Li2CO3, Ca(OH)2, MoO3, SiO2, Al2O3, TeO2, SnO2, KBr, KCl, and NaCl. These materials can contain dopants to tailor their emission characteristics, as described above. Examples of suitable doped (or alloyed) glass systems include Y2O3:Gd, Y2O3:Dy, Y2O3:Tb, Y2O3:Ho, Y2O3:Er, Y2O3:Tm, Gd2O3:Eu, Y2O2S:Pr, Y2O2S:Sm, Y2O2S:Eu, Y2O2S:Tb, Y2O2S:Ho, Y2O2S:Er, Y2O2S:Dy, Y2O2S:Tm, ZnS:Ag:Cl (blue), ZnS:Cu:Al (green), Y2O2S:Eu (red), Y2O3:Eu (red), YVO4:Eu (red), and Zn2SiO4:Mn (green).

[0288] More specifically, with regard to downconverter materials suitable for the present invention, with or without an energy enhancement factor, U.S. Pat. No. 4,705,952 (the contents of which are incorporated herein by reference) describes an infrared-triggered phosphor that, when triggered by infrared light, stores energy in the form of visible light at a first wavelength and emits energy in the form of visible light at a second wavelength. The phosphor in U.S. Pat. No. 4,705,952 was a composition of alkaline earth metal sulfide, rare earth dopant, and fusible salt. The phosphor in U.S. Pat. No. 4,705,952 is more specifically a phosphor made from strontium sulfide, barium sulfide, and mixtures thereof, including dopants from the rare earth series and europium oxide, and mixtures thereof, and including fusible salts of fluorides, chlorides, bromides, and iodides of lithium, sodium, potassium, cesium, magnesium, calcium, strontium, and barium, and mixtures thereof. The materials described in US Pat. No. 4,705,952, with or without energy enhancement factors, are useful in various embodiments of the present invention.

[0289] In another embodiment of the present invention, the downconverter material (or mixture of downconverter materials) can include Y2O3:Li. Sun et al., "Luminescent properties of Li+ doped nanosized Y2O3:Eu," Solid State Comm. 119 (2001) 393-396 (the entire contents of which are incorporated herein by reference), describes such a material. Hou et al., "Luminescent properties nano-sized Y2O3:Eu fabricated by co-precipitation method," Journal of Alloys and Compounds, vol. 494, issue 1-2, April 2, 2010, pp. 382-385 (the entire contents of which are incorporated herein by reference), describe that nano-sized yttria (Y2O3) powder was successfully synthesized by the co-precipitation method. The powder was well crystallized, the particles were nearly spherical, and the dispersibility was good. Eu 3+ The quenching concentration of ions was 9 mol%, which is much higher than that of the microscale powders. The incorporation of Li+ ions significantly enhanced the luminescence intensity. The highest luminescence intensity was observed in the 4 mol% Li+-doped Y2O3:Eu powder (Y 0.87 EU 0.09 Li 0.04 )2O3), the fluorescence intensity increased by 79%. Yi et al., "Improved cathodoluminescent characteristics of Y2O3:Eu 3+ thin films by Li-doping,” Appl. Phys. A 87, 667-671 (2007) (the entire contents of which are incorporated herein by reference) 3+ and Li-doped Y2O3:Eu 3+ The cathodoluminescence spectra for both films and methods for making these materials are described.

[0290] In other embodiments, the present invention can use a wide variety of upconversion materials (or mixtures of upconverters), with or without energy enhancement factors, to enhance specific colors of light observable from a reflective material or surface. These upconversion materials can include materials similar to those discussed above for downconversion, but typically include doped or impurity states in the host crystal that provide the upconversion pumping mechanism. Thus, upconversion materials for enhancing color emission can convert energy from any of near-infrared, infrared, and microwave radiation. Upconversion materials for enhancing color emission can convert energy from lower-energy visible light to higher-energy visible light.

[0291] Upconversion materials, with or without energy enhancement factors, can be used in various ways to enhance visible light emission by converting infrared radiation from the solar spectrum (such as in the case of sunlight exposure) or blackbody spectrum (such as in the case of incandescent lamps). In one example, lanthanide-doped oxide nanoparticles can be excited with near-infrared radiation, such as 980 nm and 808 nm laser light, to produce visible light in various portions of the red, green, and blue spectrum, depending on the selected dopant trivalent rare earth ion(s), their concentrations, and the host lattice.

[0292] The lanthanide-doped oxides suitable for the present invention differ from conventional multiphoton upconversion processes in which, for example, the absorption of two photons is required in a simultaneous event to promote an electron from a valence band state directly to an upper-level conduction band state where relaxation across the band gap of the material produces fluorescence. Here, co-doping creates a band gap state in NaYF4 to induce a luminescence in the Yb 3+ Ions, 2 F 5 / 2, have an energy state that can be pumped by a single photon event, from which another single photon absorption event can populate an even higher state. Once in this excited state, a transition to a higher energy radiative state is possible, from which emission occurs. 2 F 5 / 2 The energy state of the pumping light is higher than the energy of the incident light. In other words, Yb 3+ Aeon 2 F 5 / 2 The energy state is the state where 980 nm light is absorbed, which allows the formation of a cluster. 4 F 7 / 2 It serves as the basis for transitions to higher energy states, such as 4 F 7 / 2 The transition from the energy state produces a visible emission.

[0293] U.S. Patent No. 7,008,559 (the entire contents of which are incorporated herein by reference) describes the upconversion capabilities of ZnS, where excitation at 767 nm produces emission in the visible range. The materials described in U.S. Patent No. 7,008,559 (ZnS and Er) 3+ Doped BaTiO3 nanoparticles and Yb 3+ Doped CsMnCl3, with or without an energy enhancement factor, are suitable for various embodiments of the present invention.

[0294] Furthermore, materials designated as upconversion materials in the present invention, with or without an energy enhancement factor, include CdTe, CdSe, ZnO, CdS, YO, MgS, CaS, SrS, and BaS. Such upconversion materials can be any semiconductor, more specifically, but not limited to, sulfide, telluride, selenide, and oxide semiconductors, and nanoparticles thereof, e.g., ZnO, CdS, Y2O3, MgS, CaS, SrS, and BaS. 1-x Mn x S y , Zn 1-x Mn x Se y , Zn 1-x Mn xTe y 、Cd 1-x MnS y 、Cd 1-x Mn x Se y 、Cd 1-x Mn x Te y 、Pb 1-x Mn x S y 、Pb 1-x Mn x Se y 、Pb 1-x Mn x Te y 、Mg 1-x MnS y 、Ca 1-x Mn x S y 、Ba 1-x Mn x S​​​​​​​​​​​​​​​​​​​​​​​​​​​​​Additional conversion materials include insulating and non-conductive materials, with some exemplary compounds being BaF2, BaFBr, and BaTiO3. Transition and rare earth ion co-doped semiconductors suitable for the present invention include sulfide, telluride, selenide, and oxide semiconductors and nanoparticles thereof, such as ZnS; Mn; Er; ZnSe; Mn, Er; MgS; Mn, Er; CaS; Mn, Er; ZnS; Mn, Yb; ZnSe; Mn, Yb; MgS; Mn, Yb; CaS; Mn, Yb, etc., and their composite compounds (M 1-z N z ) 1-x (Mn q R 1-q ) x A 1-y B y (M=Zn, Cd, Pb, Ca, Ba, Sr, Mg; N=Zn, Cd, Pb, Ca, Ba, Sr, Mg; A=S, Se, Te, O; B=S,...0 <z≦1、o<q≦1)がある。

[0295] Some nanoparticles, e.g., ZnS:Tb 3+ ,Er 3+ ;ZnS:Tb 3+ ;Y2O3:Tb 3+ ;Y2O3:Tb 3+ ,Er3 + ;ZnS:Mn 2+ ;ZnS:Mn,Er 3+ are known in the art to work for both downconversion and upconversion emissions and are suitable for the present invention, with or without an energy enhancement factor. In upconversion embodiments, light-emitting particles that emit red light may include praseodymium, light-emitting particles that emit green light may include erbium, and light-emitting particles that emit blue light may include thulium.

[0296] Typically, the upconversion process requires the addition of one or more rare earth dopants, such as Er, Eu, Yb, Tm, Nd, Tb, Ce, Y, U, Pr, La, Gd, and other rare earth species, or combinations thereof, doped into a dielectric crystal (any size >0.1 nm) containing at least one of YO, YO2O2S, NaYF4, NaYbF4, YAG, YAP, Nd2O3, LaF3, LaCl3, La2O3, TiO2, LuPO4, YVO4, YbF3, YF3, Na-doped YbF3, or SiO2, where the incident radiation is at a longer wavelength than the emitted radiation from the crystal. The emitted wavelength is entirely based on the selected dopant ion(s) and their associated and relative concentrations within the host crystal. In the case of upconversion in a YO host crystal, to achieve blue emission (approximately 450–480 nm), one could synthesize [YO; Yb (3%), Tm (0.2%)], where Yb and Tm are the percentages of Y atoms doped into the crystal relative to 100%. Similarly, typical green upconversion materials are [YO; Yb (5%), Ho (1%)] and [YO; Yb (2%), Er (1%)], and typical red upconversion materials are [YO; Yb (10%), Er (1%)] and [YO; Yb (5%), Eu (1%)]. The concentrations of the dopants relative to each other and the crystal matrix must be adjusted for every combination, and there are multiple ways to achieve multiple colors from the same dopant, with or without an energy enhancement factor.

[0297] Tm 3+ Upconversion of red light at a wavelength of about 650 nm in doped fluorozirconate glasses can be used in the present invention to generate blue light. In this system, the blue light consists of two emission bands: one at 450 nm due to the 1D2 → 3H4 transition, and the other at 475 nm due to the 1G4 → 3H6 transition. The emission intensity of both bands has been observed by others to vary quadratically with excitation power. At concentrations of 0.2 mol % or more of Tm 3+In concentrated glasses, cross-relaxation processes occur, reducing the upconversion efficiency.

[0298] Visible light emission upon excitation in the near infrared (NIR) was observed for LuPO4:Yb in chloroform. 3+ , Tm 3+ , and YbPO4:Er 3+ It has been observed in optically transparent colloidal solutions of nanocrystals, and excitation at 975 nm has been shown by others to produce visible emission in the blue, green, or red spectral regions.

[0299] Tellurium and germanium oxides (tellurites and germanates) are also suitable upconverters. These glasses can be doped with, for example, Tm, Yb, Ho, Er, Pr.

[0300] Yb 3+ Doped BaZrO3 is also suitable for upconversion. 3+ and / or Tm 3+ Doping is also suitable for tuning the emission wavelength.

[0301] In another embodiment, Nd prepared by the Morss method 3+ :Cs2NaGdCl6 and Nd 3+ ,Yb 3+ Polycrystalline powder samples of CsNaGdCl have been reported to be the largest upconverters and are suitable for the present invention. These materials exhibit upconversion emissions around 538 nm (green), 603 nm (orange), and 675 nm (red) under 785 nm irradiation, with the upconversion sequences being 4G7 / 2 → 4I9 / 2, (4G7 / 2 → 4I11 / 2; 4G5 / 2 → 4I9 / 2), and (4G7 / 2 → 4I13 / 2; 4G5 / 2 → 4I11 / 2), respectively.

[0302] In another embodiment, Nd 3+ and Ho 3+Co-doped base ZrF4 fluoride glass has been reported to be an upconverter and is suitable for the present invention. Among the upconversion luminescence of ZrF4 fluoride glass, the green emission was very strong, while the blue and red emission intensities were very weak.

[0303] In another embodiment, Tm 3+ / Yb 3+ Co-doped TeO2-Ga2O3-R2O (R = Li, Na, K) glasses have been reported to be upconverters and are suitable for the present invention. These materials exhibited strong blue upconversion emission centered at 476 nm and weak red emission at 650 nm under 977 nm excitation.

[0304] In another embodiment, the metal-to-ligand charge transfer (MLCT) transition in the presence of anthracene or 9,10-diphenylanthracene is [Ru(dmb)] 2+ (dmb = 4,4'-dimethyl-2,2'-bipyridine) has been reported to be an upconverter and is suitable for the present invention. Upconverted singlet fluorescence due to triplet-triplet annihilation at low excitation power has been reported. In particular, 9,10-diphenylanthracene (DPA) (used instead of anthracene) showed higher efficiency for upconversion. In these experiments, researchers of this material system hypothesized that DPA increased the singlet fluorescence quantum yield (λ = 0.95) compared to anthracene (λ = 0.27). This work demonstrated an improvement in the upconversion of green to blue light to approximately 24.4 ± 6.1, which is comparable to the quantum yield of, for example, a commercially available green laser pointer (λ = 0.95). ex This allows for direct visualization of processes at low excitation powers (e.g., 532 nm, <5 mW peak power).

[0305] The structures described herein for color enhancement by energy-enhancing structures are referred to as color-enhancing / energy-enhancing structures or energy-enhancing / enhancing structures.

[0306] By locating an energy converter, or color conversion or enhancement material, near the energy-enhancing structures of the present invention, whether the energy-enhancing structures are within a region of enhanced electric field or otherwise outside of the region of enhanced electric field, the color-enhancing / energy-enhancing structures or energy-enhancing / enhancing structures of the present invention can generate light that can be used for a variety of applications, particularly for photostimulation of biological, chemical, and physical reactions, such as, for example, photoactivation of photoreactive drugs, photoactivation of photosensitive materials such as adhesives or lithographic photoresists, or for direct interaction with biological and chemical agents in the environment of the augmenting structure, as in sterilization.

[0307] Thus, in one embodiment of the present invention, the color-enhancing structures described herein can receive polychromatic light from a variety of light sources, such as sunlight, incandescent light bulbs, fluorescent light bulbs, and LED light sources, each having a different wavelength or wavelength band. At these different wavelength bands, the resonator is "matched" or "tuned" to those wavelengths, and a strong electric field is established, particularly between a pair of external electrodes or a pair of folded resonator electrodes, if used. In these regions of strong electric field, color converters (up and / or down phosphorescent materials) can be placed that can capture light from one of the different wavelengths or wavelength bands and emit light from another wavelength or wavelength band. In one embodiment, the strong electric field increases the intensity of the light emitted from the phosphorescent material. Furthermore, unlike the plasmonics described above, where the electric field enhancement is limited to a region within 100-200 nm of the metal, the resonator establishes an increased electric field within the volume of the external electrode pair, or folded resonator electrode pair if used, such that the phosphorescent material near and within the external electrode pair (or folded resonator electrode pair) exhibits greater intensity than if the converter were further from the resonator.

[0308] In view of the above, the present invention is generally directed to methods and systems for color enhancement utilizing color enhancement structures, having: a) an energy collector including at least one energy enhancement structure; and b) an energy converter capable of converting and emitting light of a second wavelength / quantum of electromagnetic energy at a third wavelength that is wavelength / energy shifted from the second wavelength / quantum of electromagnetic energy. In one embodiment, the energy converter is positioned proximate to the at least one energy enhancement structure such that the wavelength-shifted light is emitted with a greater intensity than if the converter were located farther from the at least one energy enhancement structure. For ease of understanding, the term "wavelength" is used to describe the electromagnetic energy entering the energy converter, although the electromagnetic energy may be better described in certain embodiments based on its energy level or intensity.

[0309] By placing an energy converter or color conversion or enhancement material near the energy enhancement structure of the present invention, regardless of whether the energy enhancement structure is within the region of an enhanced electric field or otherwise outside the region of an enhanced electric field, the color enhancement / enhancement structure or energy enhancement / enhancement structure of the present invention can enhance the conversion of one form of energy to another, such as the conversion of one or more wavelengths of light to other wavelengths of light, or the conversion of one or more wavelengths of light to electrical energy, or the conversion of one or more wavelengths of light to heat.

[0310] The conversion of one or more wavelengths of light to other wavelengths of light is useful for color transfer and color enhancement applications. The conversion of one or more wavelengths of light to electrical energy is useful, for example, for harvesting solar energy using solar cells. The conversion of one or more wavelengths of light to heat is also useful, for example, for harvesting solar energy using thermoelectric cells or other heat-to-electrical energy devices such as thermoelectric generators.

[0311] In some embodiments of the color / energy enhancement structure, the color enhancement structure includes a multidimensional concentrator including a first level metal pattern and a second level metal pattern offset laterally or axially from the first level metal pattern. At least one of the metal patterns optionally includes a first resonator dimensioned to resonate with light of a first wavelength. The first resonator may be one of a folded structure or an external electrode pair structure, as described above. The color enhancement structure includes a converter capable of converting light of a second wavelength into and emitting light of a third wavelength that is wavelength-shifted from the second wavelength. The converter is positioned with the first resonator such that the wavelength-shifted light is emitted with a greater intensity than if the converter were spaced apart from the first resonator.

[0312] In some embodiments, the energy converter is disposed proximate to the at least one energy augmentation structure, conductively coupling the energy converter to the at least one energy augmentation structure.

[0313] For example, in some embodiments, an energy converter disposed proximate to at least one energy augmentation structure includes a physical, conductive connection between the energy converter and the at least one energy augmentation structure.

[0314] Color / Energy Enhancement Structures, In some embodiments of the color enhancement structure, the energy converter comprises a downconverter that converts ultraviolet or blue light to red, yellow, or green light. In some embodiments of the color enhancement / energy enhancement structure, the energy converter comprises an upconverter that converts infrared or red light to yellow, green, or blue light.

[0315] In some embodiments of the color-enhancing / energy-boosting structure, the metal pattern includes a folded resonator having opposing electrodes with an electric field oriented between them, and the converter is positioned between the opposing electrodes, within the fringing electric field of the opposing electrodes, or near the opposing electrodes. In one example, the folded resonator is a ¾λ folded resonator. In one example, the metal pattern includes at least one of Au, Ag, Cu, Al, or a transparent metal oxide. In another example, the metal pattern can be formed of a refractory metal such as Ti, W, or Mo.

[0316] In some embodiments of the color-enhancing / energy-boosting structure, the metal pattern includes a pair of external electrodes with opposing electrodes having an electric field oriented between them, and the converter is positioned between the opposing electrodes, within the fringe electric field of the opposing electrodes, or near the opposing electrodes. In one example, the resonator is a 3 / 4λ external electrode pair resonator. In one example, the metal pattern includes at least one of Au, Ag, Cu, Al, or a transparent metal oxide. In another example, the metal pattern can be formed of a refractory metal such as Ti, W, or Mo.

[0317] Color Enhancement / Energy Enhancement Structures In some embodiments of the color enhancement structure, there is an anti-reflective film disposed on at least one of the metal patterns or the converter.

[0318] In some embodiments of the color / energy enhancing structure, the first resonator comprises a plurality of resonators, the converter comprises a plurality of converters, and the plurality of converters are arranged at a plurality of locations throughout the concentrator. In one example, the plurality of converters are positioned to convert light that is internally scattered within the concentrator.

[0319] In some embodiments of the color / energy enhancement structure, the first level metal pattern (or second level metal pattern) comprises a metal core clad with a high-K dielectric followed by a cladding of a low-K dielectric. In some embodiments of the color / energy enhancement structure, the first level metal pattern (or second level metal pattern) comprises a radial pattern of conductors. In some embodiments of the color / energy enhancement structure, the first level metal pattern (or second level metal pattern) comprises a fractal pattern. In one example, the fractal pattern is embedded within a dielectric material.

[0320] In some embodiments of the color-enhancing / energy-enhancing structure, the first level metal pattern (or second level metal pattern) comprises a three-dimensional fractal structure.

[0321] In some embodiments of the color / energy enhancing structure, the concentrator comprises a transparent panel with a first level metal pattern and a second level metal pattern, and optionally a plurality of converters formed therein. In some embodiments of the color / energy enhancing structure, the concentrator comprises a transparent sheet with a first level metal pattern and a second level metal pattern, and optionally a plurality of converters formed therein.

[0322] In some embodiments of the color-enhancing / energy-enhancing structure, the first level metal patterns (or second level metal patterns) are of different sizes and / or orientations relative to each other or to the second level metal patterns.

[0323] Indeed, Figure 29 is a schematic diagram of a reflective resonator of the present invention that includes a mechanoluminescent material. In this example, the mechanoluminescent material is disposed between a folded resonator structure, but the mechanoluminescent material can also be disposed between a pair of external electrodes. Thus, in one embodiment, the electromagnetic energy enhancement factor captures and amplifies one or more wavelengths of electromagnetic energy with at least one characteristic (e.g., the electric field strength near the mechanoluminescent material), while at the same time the mechanoluminescent material can be considered an energy converter that converts ultrasonic or mechanical energy into electromagnetic radiation (i.e., emitted light).

[0324] In one embodiment of the present invention, increasing the electric field in the folded structure or the pair of external electrodes increases the luminescence of the mechanoluminescent material, and the energy used to establish the electric field in the folded structure or the pair of external electrodes is provided separately from the mechanical energy that drives the mechanoluminescence.

[0325] For example, the reflective resonator of Figure 29 can be placed adjacent to the exhaust stack of an engine or other waste heat dissipator. In one embodiment, the reflective resonator of Figure 29 is attached to a stainless steel arm that is connected to the heat stack. The stainless steel couples mechanical vibrations to the reflective resonator while thermally isolating the reflective resonator from the exhaust stack, allowing even inorganic mechanoluminescent materials to be used.

[0326] When the engine begins to exhibit higher levels of vibration or vibrations at various frequencies, the intensity of the emitted light will change, providing a visible light signal that indicates the engine or machine is under stress due to power load or wear or mechanical failure.

[0327] In one embodiment of the present invention, the reflective structure shown in FIG. 29 need not include a resonator and its resonant element. In one embodiment of the present invention, the reflective structure shown in FIG. 29 can be placed directly on a machine that operates at relatively low temperatures, around 100°C. In this embodiment, the reflective structure need not include a resonator and its resonant element. However, if a resonator and its resonant element are present, a laser, such as a 656 nm laser, can "probe" the resonator and enhance the machine emission "on demand." In this way, early detection of developing mechanical problems can be detected.

[0328] Various mechanoluminescent materials suitable for the present invention include: ZnS:Mn 2+ , SrAl2O4:Eu 2+ , ZnS:Cu, SrAMgSi2O7:Eu 2+ (A=Ca,Sr,Ba), KC, KI, KBr, NaF, NaCl, LiF, RbCl, RbBr, RbI, MgO, SrAl2O4, CaAl2O4, Sr 1-x Ba x Al2O4(x=0, 0.1, 0.2, 0.4), Sr 0.9 Ca 0.1 Al2O4, Zn2Ge 0.9 Si 0.1 O4, MgGa2O4, ZnGa2O4, ZnAl2O4, ZnS, ZnTe, (ZnS) 1-x (MnTe) x (x<1 / 4), CaZnOS, BaZnOS, Ca2MgSi2O7, Sr2MgSi2O7, Ba2MgSi2O7, SrCaMgSi2O7, SrBaMgSi2O7, Sr n MgSiO 5+n (1≦n≦2), Ca2Al2SiO7, Sr2Al2SiO7, CaYAl3O7, CaAl2Si2O8, Ca 1-x Sr x Al2Si2O8(x<0.8), SrMg2(PO4)2, Ba 1-x Ca x TiO3(0.25 <x<0.8)、Ba 1-x Ca xTiO3,LiNbO3, Sr2SnO4, (Ca,Sr,Ba)2SnO4, Sr3Sn2O7, Sr3(Sn,Si)2O7, Sr3(Sn,Ge)2O7 , Ca3Ti2O7, CaNb2O6, Ca2Nb2O7, Ca3Nb2O8, BaSi2O2N2, SrSi2O2N2, CaZr(PO4)2, ZrO2.

[0329] Yanim Jia, in "Novel Mechano-Luminescent Sensors Based on Piezoelectric / Electroluminescent Composites," Sensors (Basel). 2011;11(4):3962-396, the entire contents of which are incorporated by reference, describes a mechano-luminescent composite made from piezoelectric and electroluminescent materials. In this composite device, when stress is applied to the piezoelectric layer, charges are induced on both the top and bottom surfaces of the piezoelectric layer due to the piezoelectric effect. These induced charges result in light output from the electroluminescent layer due to the electroluminescent effect.

[0330] In one embodiment of the present invention, such a composite material made from a piezoelectric material and an electroluminescent material, hereafter a "composite mechanoluminescent emitter," provides a structure that emits light when stimulated with mechanical or vibrational energy, such as from an acoustic or ultrasonic transducer. Details of various electroluminescent materials that can be used in composite mechanoluminescent emitters are provided in the next section, where only the electroluminescent material is positioned near opposing resonator electrodes.

[0331] FIG. 30 is a schematic diagram of a composite mechanoluminescent emitter composed of piezoelectric and electroluminescent materials, which in one embodiment may be the mechanoluminescent emitter of FIG.

[0332] In another embodiment, the composite mechanical light emitter can be used without the need for any resonator structure. Figure 31 is a schematic diagram showing composite mechanical light emitters distributed over a sector of interest to generate light therefrom. Figure 31 shows that ultrasound transducers can be used to stimulate / activate these composite mechanical light emitters.

[0333] In color enhancement applications, the application of ultrasonic energy can alter the color emission from a surface. Such applications may be for security systems where an item contains a pattern of multiple mechanical light emitters. The pattern is not apparent until activated with ultrasonic or acoustic energy, at which point light of a predetermined wavelength is emitted. The emitted light may be visible or infrared, depending on the type of detector used to detect the emitted light.

[0334] In a related application of these composite mechanical light emitters, Figure 32 is a schematic diagram showing composite mechanical light emitters distributed within a target medium to generate light therein or therefrom. In this invention, the light can be turned on and off, changing the on / off state of the ultrasound transducer and the intensity of the light. There are no power leads that encounter the target medium. There is no space taken up by batteries or control elements to switch the power on and off. The composite mechanical light emitters can be miniaturized. The composite mechanical light emitters can be concentrated within a container. In some embodiments, the container is not completely filled, and tilting the container allows the composite mechanical light emitters within the container to be repositioned.

[0335] Electroluminescent and phosphorescent materials (organic and inorganic): The present invention in various embodiments, with or without energy enhancement factors, can utilize organic fluorescent molecules or inorganic particles that can have crystalline, polycrystalline, or amorphous microstructures for the converters or fluorescence and phosphorescence (optionally including the energy enhancement structures described above).

[0336] A list of inorganic molecules that can be used in resonant structures to enhance color emission includes, but is not limited to, the following inorganic electroluminescent phosphorescent materials: SrS:Ce 3+ CaGa2S4:Ce 3+ SrS:Cu+ CaS:Pb 2+ BaAl2S4:Eu 2+ ZnS:Tb 3+ ZnMgS:Mn 2+ SrGa2S4:Eu 2+ CaAl2S4:Eu 2+ BaAl2S4:Eu 2+ ZnS:Mn 2+ MgGa2O4:Eu 3+ (Ca,Sr)Y2S4:Eu 2+ BaAl2S4:Eu 2+

[0337] Organic molecules that are capable of phosphorescence under the influence of an electric field are also of interest herein. Organic fluorescent compounds with high quantum yields include, by way of example: naphthalene, pyrene, Perylene, anthracene, phenanthrene, p-terphenyl, p-quatphenyl, trans-stilbene, tetraphenylbutadiene, Distyrylbenzene, 2,5-diphenyloxazole, 4-methyl-7-diethylaminocoumarin, 2-phenyl-5-(4-biphenyl)-1,3,4-oxadiazole, 3-phenylcarbostyril, 1,3,5-triphenyl-2-pyrazoline, 1,8-naphthoylene-1',2'-bezimidazole, 4-Amino-N-phenyl-naphthalimide.

[0338] The inorganic fluorescent and phosphorescent materials detailed herein are numerous, and various examples are provided by way of illustration and not limitation. Furthermore, these materials can be doped with specific ions (activators or combinations of activators) that can occupy lattice structure sites in the case of crystalline or polycrystalline materials, or network-forming sites or cross-linked and / or non-cross-linked sites in amorphous materials. These compounds can include the following example materials (not ranked in order of preference or usefulness): CaF2, ZnF2, KMgF3, ZnGa2O4, ZnAl2O4, Zn2SiO4, Zn2GeO4, Ca5(PO4)3F, Sr5(PO4)3F, CaSiO3, MgSiO3, ZnS,MgGa2O4, LaAl 11 O 18 , Zn2SiO4, Ca5(PO4)3F,Mg4Ta2O9, CaF2, LiAl5O8, LiAlO2, CaPO3, AlF3.

[0339] Also included are alkaline earth chalcogenide phosphorescent materials, which are next exemplified by the following non-exhaustive list: MgS:Eu 3+ , CaS:Mn 2+ , CaS:Cu, CaS:Sb, CaS:Ce 3+ , CaS:Eu 2+ , CaS:Eu 2+ Ce 3+ , CaS:Sm 3+ , CaS:Pb 2+ , CaO:Mn 2+ , CaO:Pb 2+ .

[0340] Examples include ZnS-type phosphors, including various derivatives. ZnS:Cu, Al(Cl), ZnS:Cl(Al), ZnS:Cu, I(Cl), ZnS:Cu, ZnS:Cu, In.

[0341] IIIb-Vb phosphorescent materials, compounds containing elements from groups IIIb and Vb of the periodic table, are suitable as converter materials. These semiconductors include BN, BP, BSb, AlN, AlP, AlAs, AlSb, GaN, GaP, GaAs, GaSb, InN, InP, InAs, and InSb. These materials have donors and acceptors that cooperate to produce light-emitting diodes. Donors include Li, Sn, Si, Li, Te, Se, S, and O. Acceptors include C, Be, Mg, Zn, Cd, Si, and Ge. For example, GaP light-emitting diodes include GaP:Zn, O, GaP:NN, GaP:N, and GaP, which emit red, yellow, green, and pure green light, respectively.

[0342] Compounded materials further include materials such as GaAs with the following type of compositional variation: In1-y(Ga1-xAlx)yP (a simple example is given). Silicon carbide SiC as a light-emitting platform is commercially relevant for blue light-emitting diodes. These include the polytypes 3C-SiC, 6H-SiC, and 4H-SiC with donors such as N or Al and acceptors such as Ga or B.

[0343] Multiband emissive materials suitable for the converter material include, for example, the following compositions: (Sr,Ca,Ba)5(PO4)3Cl:Eu 2+ , BaMgAl 16 O 27 :EU 2+ , CeMgAl 11 O 19 :Ce 3+ :Tb 3+ , LaPO4:Ce 3+ :Tb 3+ , GdMgB5O 10 :Ce 3+ :Tb 3+ , Y2O3:Eu 3+ , (Ba,Ca,Mg)5(PO4)3Cl:Eu 2+ , 2SrO 0.84 P2O5 . 0.16B2O3:Eu 2+ , SrAl 14 O25 :EU 2+ .

[0344] Other materials suitable as converter materials include those used in fluorescent high-pressure mercury discharge lamps, which can be excited by X-rays, and are exemplified by the following family designations: Phosphate (Sr,M)(PO4)2:Sn 2+ , Mg or Zn activator, germanate 4MgO.GeO2:Mn 4+ , 4(MgO,MgF2)GeO2:Mn 4+ , Yttrium Y2O3:Eu 3+ , vanadate YVO4:Eu 3+ , Y(P,V)O4:Eu 3+ , Y(P,V)O4:In + , halo silicate Sr2Si3O8 . 2SrCl2:Eu 2+ , aluminate (Ba,Mg)2Al 16 O 24 :EU 2+ , (Ba,Mg)2Al 16 O 24 :EU 2+ , Mn 2+ , Y2O3Al2O3:Tb 3+ .

[0345] Another grouping of materials suitable as host compound converter materials includes halophosphate phosphors, phosphate phosphors, silicate phosphors, aluminate phosphors, borate phosphors, tungstate phosphors, and other phosphor chemical compositions.

[0346] Halophosphates include, by way of example: 3Ca3(PO4)2.Ca(F,Cl)2:Sb 3+ , 3Ca3(PO4)2.Ca(F,Cl)2:Sb 3+ / Mn 2+ , Sr 10 (PO4)6Cl2:Eu 2+ , (Sr, Ca) 10 (PO4)6Cl2:Eu 2+ , (Sr, Ca) 10(PO4)6.nB2O3:Eu 3+ , (Sr, Ca, Mg) 10 (PO4)6Cl2:Eu 2+ Phosphorescent materials include: Sr2P2O7:Sn 2+ , (Sr,Mg)3(PO4)2:Sn 2+ , Ca3(PO4)2.Sn 2+ , Ca3(PO4)2:Tl + , (Ca,Zn)3(PO4)2:Tl + , Sr2P2O7:Eu 2+ , SrMgP2O7:Eu 2+ , Sr3(PO4)2:Eu 2+ , LaPO4:Ce 3+ , Tb 3+ , La2O3 . 0.2SiO2 . 0.9P2O5:Ce 3+ .Tb 3+ , BaO . TiO2 . P2O5. Silicate phosphorescent material, Zn2SiO4:Mn 2+ , CaSiO3:Pb 2+ / Mn 2+ , (Ba, Sr, Mg) . 3Si2O7:Pb 2+ , BaSi2O5:Pb 2+ , Sr2Si3O8 . 2SrCl2:Eu 2+ , Ba3MgSi2O8:Eu 2+ , (Sr,Ba)Al2Si2O8:Eu 2+ .

[0347] Aluminate phosphorescent materials include: LiAlO2:Fe 3+ , BaAlO 13 :EU 2+ , BaMgAl 16 O 27 :EU 2+ , BaMgAl 16 O 27 :EU 2+ / Mn 2+ , SrAl 14 O 25 :EU2+ , CeMgAl 11 O 19 :Ce 3+ / Tb 3+ .

[0348] Borate phosphorescent materials include: Cd2B2O5:Mn 2+ , SrB4O7F:Eu 2+ , GdMgB5O 10 :Ce 3+ / Tb 3+ , GdMgB5O 10 :Ce 3+ / Mn 3+ , GdMgB5O 10 :Ce 3+ / Tb 3+ / Mn 2+ .

[0349] Tungstate phosphorescent materials include: CaWO4, (Ca,Pb)WO4, MgWO4. Other phosphorescent materials include Y2O3:Eu 3+ , Y(V,P)O4:Eu 2+ , YVO4:Dy 3+ , MgGa2O4:Mn 2+ , 6MgO . As2O5:Mn 2+ , 3.5MgO . 0.5MgF2 . GeO2:Mn 4+ .

[0350] Activators associated with various doped phosphorescent materials include the following list: Tl + , Pb 2+ , Ce 3+ ,EU 2+ , WO4 2- , Sn 2+ , Sb 3+ , Mn 2+ , Tb 3+ ,EU 3+ , Mn 4+ , Fe 3+ .

[0351] In various embodiments, the luminescent center T1+ can be used in the following chemical compositions: (Ca,Zn)3(PO4)2:Tl + , Ca3(PO4)2:Tl + .

[0352] Similarly, the luminescent center Mn2+ can be used in the following chemical compositions: MgGa2O4:Mn 2+ , BaMgAl 16 O 27 :EU 2+ / Mn 2+ , Zn2SiO4:Mn 2+ , 3Ca3(PO4)2 . Ca(F,Cl)2:Sb 2+ / Mn 2+ , CaSiO3:Pb 2+ / Mn 2+ , Cd2B2O5:Mn 2+ , CdB2O5:Mn 2+ , GdMgB5O 10 :Ce 3+ / Mn 2+ , GdMgB5O 10 :Ce 3+ / Tb 3+ / Mn 2+ .

[0353] Furthermore, the luminescent center Sn 2+ is available in the following chemical compositions: Sr2P2O7:Sn 2+ , (Sr,Mg)3(PO4)2:Sn 2+ .

[0354] Luminescent center Eu 2+ It can also be used in the following chemical compositions: SrB4O7F:Eu 2+ , (Sr,Ba)Al2Si2O8:Eu 2+ , Sr3(PO4)2:Eu 2+ , Sr2P2O7:Eu 2+ , Ba3MgSi2O8:Eu 2+ , Sr 10 (PO4)6Cl2:Eu 2+, BaMgAl 16 O 27 :EU 2+ / Mn 2+ , (Sr, Ca) 10 (PO4)6Cl2:Eu 2+ .

[0355] Luminescent center Pb 2+ It can be used in the following chemical compositions: (Ba,Mg,Zn)3Si2O7:Pb 2+ , BaSi2O5:Pb 2+ , (Ba,Sr)3Si2O7:Pb 2+ .

[0356] Luminescent center Sb 2+ It can be used in the following chemical compositions: 3Ca3(PO4)2 . Ca(F,Cl)2:Sb 3+ , 3Ca3(PO4)2 . Ca(F,Cl)2:Sb 3+ / Mn 2+ .

[0357] The luminescent center Tb3+ can be used in the following chemical compositions: CeMgAl 11 O 19 :Ce 3+ / Tb 3+ , LaPO4:Ce 3+ / Tb 3+ , Y2SiO5:Ce 3+ / Tb 3+ , GdMgB5O 10 :Ce 3+ / Tb 3+ .

[0358] Luminescent center Eu 3+ It can be used in the following chemical compositions: Y2O3:Eu 3+ , Y(V,P)O4:Eu 3+ .

[0359] Luminescent center Dy 3+It can be used in the following chemical compositions: YVO4:Dy 3+ .

[0360] Luminescent center Fe 3+ It can be used in the following chemical compositions: LiAlO2:Fe 3+ .

[0361] Luminescent center Mn 4+ It can be used in the following chemical compositions: 6MgO . As2O5:Mn 4+ , 3.5MgO . 0.5MgF2 . GeO2:Mn 4+ .

[0362] Luminescent center Ce 3+ It can be used in the following chemical compositions: Ca2MgSi2O7:Ce 3+ and Y2SiO5:Ce 3+ .

[0363] Luminescent center WO4 2- It can be used in the following chemical compositions: CaWO4, (Ca,Pb)WO4, MgWO4.

[0364] Luminescent center TiO4 4- It can be used in the following chemical compositions: BaO . TiO2 . P2O5.

[0365] Various embodiments of the present invention can utilize phosphorescent chemistries that utilize X-ray excitation. Of particular interest are the kedges of these phosphorescent materials. Low energy excitation can result in strong emission in low kedge materials. Some of these chemistries and their corresponding kedges include: BaFCl:Eu 2+ 37.38 keV BaSO4:Eu 2+ 37.38 keV CaWO469.48keV Gd2O2S:Tb 3+ 50.22 keV LaOBr:Tb 3+ 38.92 keV LaOBr:Tm 3+ 38.92 keV La2O2S:Tb 3+ 38.92 keV Y2O2S:Tb 3+ 17.04 keV YTaO467.42keV YTaO4:Nb 67.42keV ZnS:Ag 9.66keV (Zn,Cd)S:Ag 9.66 / 26.7keV

[0366] In one embodiment of the present invention, light from these materials (e.g., excited by high-energy particles including X-rays, gamma rays, protons, and electrons) can be modulated by including these materials in proximity to (including within) the color enhancement structures described herein. For example, in medical treatments where X-rays excite phosphorescence to photostimulate a patient's response, infrared radiation can be applied simultaneously with irradiation by high-energy particles to drive the resonance of the color enhancement / energy enhancement structures described herein, and the X-ray phosphors enhance their emission in the presence of an increased electric field. In another example, in medical or scientific equipment, an applied electric field can be present to enhance the emission from these X-ray phosphors simultaneously with irradiation by high-energy particles.

[0367] C. Color-enhancing structure The present invention provides methods, systems, and devices that use phosphorescent, fluorescent, and scintillating materials, or other energy conversion materials and devices described herein, with or without the above-described energy-enhancing structures, to enhance the effectiveness and / or efficiency of light emission from a medium. With the energy-enhancing structures, the present invention can create localized regions of intense electric fields to enhance or accelerate the emission of light, photons, or electrons in materials proximate those localized regions.

[0368] Phosphorescent Devices: Having previously described a number of converter materials that can be used in the present invention for color enhancement, Figure 33 is a schematic diagram of a reflective resonator of the present invention in which a converter material (such as the phosphorescent and other luminescent materials listed above) is used inside a 3 / 4λ folded resonator in which one side of the metal traces is made of transparent indium tin oxide and the other side is a reflective metal such as Au, Ag, Al, Cu, etc. Alternatively, the resonator can have an external electrode pair structure (instead of the folded structure shown), with the converter material present inside the electrode pair.

[0369] Figure 34 is a schematic diagram of an LED white light source with variable color temperature control. The structure closely follows that described in U.S. Patent Application Publication No. 2007 / 0215890, the entire contents of which are incorporated herein by reference.

[0370] As shown above, in this embodiment, a conventional blue LED is attached to a submount using solder bumps or other means. The surface of the submount has metallic contact pads to which the LED is electrically connected. The contact pads connect to other conductors formed around or on the underside of the submount for connection to a power source, such as a current source. In one embodiment of the color enhancement invention, the submount is electrically connected to an electric field applicator. The electric field applicator, as shown, can be a simple grid element with different controllable voltages established at each of the levels shown, allowing the electric fields within the red and green phosphorescent plates to be adjusted. By increasing or decreasing the electric field within the red or green phosphorescent plates, the intensity of the red and green light can be continuously adjusted on demand as needed.

[0371] In one embodiment of the color enhancement invention, the submount is not electrically connected to the electric field applicator, and the electric field applicator can be a folded resonator such as the 3 / 4λ folded resonator described above, or a 3 / 4λ resonator with a pair of external electrodes. Here, the wavelength of the 3 / 4λ folded resonator or the 3 / 4λ pair of external electrodes resonator is approximately 5 to 10 microns, particularly for high-power LED operation where waste heat is generated.

[0372] As per the '890 publication, the LEDs can be formed using AlInGaN material and preferably emit blue light with a peak wavelength of about 460-470 nm to match the spectral distribution of conventional blue filters in LCDs. Other emission wavelengths that are also considered blue may also be suitable, such as 440-480 nm. The top surface of a blue LED has a typical size of 1 mm. 2 It may be any of the following sizes:

[0373] Disposed above the LEDs are red and green phosphorescent plates. The size of each plate may match the size of the LED or may be slightly larger or smaller depending on the LED's emission pattern, tolerances, and phosphorescent plate characteristics. The plates may extend beyond the LED surface by as much as 25%. In one embodiment, the plates are smaller than the LEDs (e.g., up to 50% smaller), allowing for a larger blue component in the white light or for green and red phosphorescent plates to be placed side-by-side. The use of thin LEDs results in slight side emission, which is mixed with the white light in the backlight box.

[0374] As in the '890 publication, the thickness of each phosphor plate can be between 50 and 300 microns, depending on the type of phosphor used, the type of blue LED used (e.g., higher power LEDs may require thicker plates), the density of the phosphor, and other factors understood by those skilled in the art.

[0375] Electroluminescent Device: Figure 35 is a schematic diagram of an electroluminescent light source. A typical modern electroluminescent (EL) device has two co-layered organic materials. The EL device consists of a transparent indium tin oxide (ITO) anode, a hole transport layer (HTL), and an electron transport layer (ETL), with various examples including a metallic cathode made of alloy metals. The flow of electron current (charge carrier flow) supplies electrons to the emissive layer. The generation and flow of holes (charge carriers) in the emissive layer can recombine with electrons in the emissive layer to output light.

[0376] FIG. 36 is a schematic diagram of an electroluminescent light source of the present invention having an electroluminescent medium within a folded resonant electrode.

[0377] Various materials used to coat the ejection layer of the present invention can include, but are not limited to: 4,4',4''-Tris[phenyl(m-tolyl)amino]triphenylamine (m-MTDATA) N,N'-bis(3-methylphenyl)-N,N'-diphenylbenzidine (TPD) 4,4',4''-Tris[phenyl(m-tolyl)amino]triphenylamine (m-MTDATA) N,N'-bis(3-methylphenyl)-N,N'-diphenylbenzidine (TPD) Tris-(8-hydroxyquinoline)aluminum 2,4,6-tris(2-pyridyl)-s-triazine (TPT) [ka] 2,2',2''-(1,3,5-benzinetriyl)-tris(1-phenyl-1-H-benzimidazole)Alq [ka] 2,2',2''-(1,3,5-benzinetriyl)-tris(1-phenyl-1-H-benzimidazole) TPBI [ka] 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline, BCP2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline, BCP [ka]

[0378] In another embodiment, an optically transparent anode such as indium tin oxide (ITO) is used. The converter material is disposed on the capacitive portion of the curved antenna, exposing the organic layers consisting of a hole transport layer (HTL), an electron transport layer (ETL), and a metal cathode. The electromagnetic energy coupled to the antenna in this example can operate from the RF and microwave ranges to the IR and UV ranges.

[0379] In the embodiment of Figure 3-2, the energy converter or color conversion or enhancement material is located near the energy enhancement structure (i.e., the 3 / 4λ folded resonator). Thus, the energy enhancement structure is preferably in a region of enhanced electric field between the folded opposing electrodes. In one embodiment of the present invention, the enhanced electric field is in a region of enhanced energy because there is a current conductively coupling the energy converter (electroluminescent material) to one energy enhancement structure (the 3 / 4λ folded resonator).

[0380] Plasmonic enhancement structure for color enhancement device: The color enhancement devices described above can utilize the plasmonic enhancement structures described above. As noted above, FIG. 26 is a schematic representation of an upconverter or downconverter material (i.e., a photoactive material) according to one embodiment of the present invention, utilized in the color enhancement / enhancement structures described herein, with or without an energy enhancement factor. FIG. 26 illustrates several structural configurations for placing a dielectric core upconverter or downconverter material (nanometer-sized scale) near a metal shell. Incident light of wavelength λ interacts with the upconverting dielectric core. The interaction of light λ with the dielectric core generates secondary radiation at a λ frequency having a wavelength shorter than λ and correspondingly higher energy than λ. While the exact physical mechanism of upconversion may depend on the specific upconversion material and process used in a particular application, the following description is provided for discussion and illustration.

[0381] In the context of Figure 26, three separate processes are well understood for the upconversion process involving trivalent rare earth ions when wavelength λ interacts with the dielectric core. These three processes are: 1) Excited state absorption: Two photons are absorbed consecutively by the same ion, exciting it to one or more states. 2) Energy transfer upconversion, which is the transfer of excitation from one ion to another ion that is already in an excited state. 3) A multiphoton cooperative process, in which two nearby excited ions are collectively ejected from a virtual state.

[0382] Regardless of which of these processes occurs between the selected ion(s) and the host lattice, the end result will be photons of greater energy than the excitation energy being emitted from the host lattice due to the upconversion or downconversion process.

[0383] Thus, the particular ions activated (whether dopant ions or lattice host ions, such as in neodymium oxide) are selected based on the host material being processed, to provide an ionic state in which the dopant ions or dielectric core host ions are pumpable by an NIR source to generate the resulting radiation λ2.

[0384] Thus, in one embodiment, the present invention provides an upconversion or downconversion material configured to generate a second wavelength of radiation λ2 having higher or lower energy than the first wavelength λ1 when exposed to a first wavelength of radiation λ1. The system can include a metallic structure (e.g., a metallic shell covering a portion of the nanoparticle) disposed in association with the nanoparticle. The system can also include an acceptor disposed in a medium proximate to the nanoparticle. When activated by the second wavelength λ2, the acceptor can fluoresce to generate visible light. In one embodiment of the present invention, the physical properties of the metallic structure (such as those depicted above and below in the figures) are set to values ​​such that the surface plasmon resonance of the metallic structure resonates at a frequency that provides spectral overlap with either the first wavelength λ1 or the second wavelength λ2. This system, with the metallic structure disposed in association with the upconversion or downconversion nanoparticle, becomes a converter utilized in the color enhancement / boosting structures described herein.

[0385] Within the context of the present invention, the term "physical property" of a metal shell or core may refer to any property of the metal itself or the dimensions or shape of the shell or core that affects the surface plasmon resonance frequency. Such physical properties may include, but are not limited to, the electrical conductivity, radial dimensions, chemical composition, or crystalline state of the metal shell or core.

[0386] In various embodiments, the metallic structure can be a metallic shell encapsulating at least a portion of the nanoparticles within the metallic shell, where the electrical conductivity, radial dimension, or crystalline state of the metallic shell sets the surface plasmon resonance in the metallic structure to resonate at a frequency that provides spectral overlap with either the first wavelength λ1 or the second wavelength λ2. In various embodiments, the metallic structure can be a multi-layer metallic shell encapsulating at least a portion of the nanoparticles within the metallic shell, where the electrical conductivity, radial dimension, or crystalline state of the metallic shell sets the surface plasmon resonance in the metallic structure to resonate at the first wavelength λ1 and the second wavelength λ2. This feature allows for emission at λ1 and amplification at λ2.

[0387] In various embodiments, the metallic structures can be metal particles present in one or more multi-structures. These multi-structures can have a variety of shapes, including, for example, spheres, spheroids, rods, cubes, triangles, pyramids, pillars, crescents, tetrahedrons, stars, or combinations thereof, and are positioned adjacent to the nanoparticles, where the conductivity, dimensions (e.g., lateral dimensions or thickness), or crystalline state of the metallic structures configure the surface plasmon resonance in the metallic particles or rods to resonate at a frequency that provides spectral overlap with either the first wavelength λ1 or the second wavelength λ2. Such shapes are described in the figures of this application and in the figures of U.S. Application No. 12 / 401,478, which are incorporated by reference in their entirety. The choice of shape can affect the frequency of the surface plasmon resonance. It is known that the plasmon bandwidth varies with the shape of the nanoparticle (e.g., prolate spheroid or oblate spheroid). The article "Spectral bounds on plasmon resonances for Ag and Au prolate and oblate nanospheroids," in the Journal of Nanophotonics, Vol. 2, pp. 029501 (September 26, 2008), the entire contents of which are incorporated by reference, shows the plasmon resonance shifts for Ag shaping and Au shaping for prolate and oblate spheroids. In one embodiment of the present invention, as the aspect ratio of the metal structures of the present invention increases, the prolate spheroid resonances red-shift relative to an unbounded sphere (under the assumption of the Drude dispersion model). Meanwhile, as the spheroids become flatter, the oblate resonances "blue-shift," but reach a limit.

[0388] In various embodiments, the metallic structure disposed in association with the upconversion or downconversion nanoparticle can be a metallic structure disposed within the nanoparticle, where the conductivity or dimensions (e.g., lateral dimensions or thickness) of the metallic structure set the surface plasmon resonance in the metallic structure to resonate at a frequency that provides spectral overlap with either the first wavelength λ1 or the second wavelength λ2. In various embodiments, the metallic structure can be a metallic multilayer structure disposed within the nanoparticle, where the conductivity or dimensions (e.g., lateral dimensions or thickness) of the metallic structure set the surface plasmon resonance in the metallic structure to resonate at the frequencies of the first wavelength λ1 and the second wavelength λ2. This capability again allows for radiation at λ1 and amplification at λ2.

[0389] In another embodiment, the present invention provides a nanoparticle structure comprising a sub-1000 nm dielectric core and a metallic structure disposed in association with the nanoparticle. The dielectric core material comprises at least one of Y2O3, Y2O2S, NaYF4, NaYbF4, YAG, YAP, Nd2O3, LaF3, LaCl3, La2O3, TiO2, LuPO4, YVO4, YBF3, YF3, Na-doped YbF3, or SiO2. In certain embodiments, such nanoparticle structures can exhibit surface plasmon resonance in the metallic structure to enhance light upconversion from a first wavelength λ1 to a second wavelength λ2.

[0390] As described above, the shell (or other structure) is specifically designed with a layer thickness (or, e.g., lateral dimension) to enhance the photon upconversion process through plasmon enhancement. The shell thickness (or other physical property) is "tuned" to the absorption process by having a dimension where the plasmons (i.e., electron oscillations) within the shell have a resonant frequency that results in spectral overlap with the target absorption band. Thus, if upconversion is stimulated by NIR light at 980 nm, the shell thickness is "tuned" to a thickness where the plasmon resonance also resonates at a frequency of 980 nm (or nearby, as plasmon resonances are typically broad at these wavelengths).

[0391] The plasmon resonant shell can be made of a number of transition metals, including, but not limited to, gold, silver, platinum, palladium, nickel, ruthenium, rhenium, copper, and cobalt, or combinations, alloys, or layers thereof. Such plasmon resonant shells can also be made of combinations of metals and non-metals. When formed from gold nanoshells, the recommended thickness for resonating with 980 nm light is approximately 3.5 nm, surrounding an 80 nm upconverting core, as predicted by an extension of Mie theory calculations. (See Jain et al., Nanolett. 2007, 7(9), 2854, the entire contents of which are incorporated herein by reference.) Figure 27, reproduced from Jain et al., demonstrates the invention's ability to "tune" the metal shell to have spectral overlap with the excitation and / or emission radiation wavelengths.

[0392] In one embodiment of the present invention, the metal structure disposed in association with the upconversion or downconversion nanoparticles may be an alloy, such as, for example, an Au:Ag alloy. The alloy content may be configured to tune the frequency of the surface plasmon resonance. In one embodiment of the present invention, the metal structure may be an alloy, such as, for example, a Pt:Ag alloy. The alloy content may be configured to tune the frequency of the surface plasmon resonance. In one embodiment of the present invention, the metal structure may be an alloy, such as, for example, a Pt:Au alloy. The alloy content may be configured to tune the frequency of the surface plasmon resonance.

[0393] In one embodiment of the present invention, the converter nanoparticles can be an alloy of two or more materials. In this embodiment, the alloy can have a composition of the two or more materials set to a composition value such that excitation of the alloy at a first wavelength λ1 produces radiation at a second wavelength λ2. In one embodiment of the present invention, the nanoparticles can be an alloy of zinc sulfide and zinc selenide. In one embodiment of the present invention, the nanoparticles can be an alloy of zinc sulfide and cadmium sulfide.

[0394] In one embodiment of the invention, the zinc sulfide and zinc selenide nanoparticle alloys can have an alloy content designed to provide a predetermined surface plasmon resonance. In one embodiment of the invention, the zinc sulfide and cadmium sulfide nanoparticle alloys can have an alloy content designed to provide a predetermined surface plasmon resonance.

[0395] Some techniques for producing nanoparticles and nanoalloys suitable for the present invention are described in their entirety in the following documents, which are incorporated herein in their entirety: U.S. Patent Nos. 7,645,318, 7,615,169, 7,468,146, 7,501,092, U.S. Patent Application Publication Nos. 2009 / 0315446, 2008 / 0277270, 2008 / 0277267, 2008 / 0277268, and WO2009 / 133138.

[0396] In one embodiment of the present invention, the thickness of the metal shell disposed in association with the upconversion or downconversion nanoparticle is set according to the absorption frequency (or emission frequency, as the case may be) of the particular dopant ion in the dielectric core that enhances the overall efficiency of the upconverted light emission process. Thus, the shell thickness can be thought of as a tool to enhance the absorption at λ in one example, the emission at λ in another example, or as an enhancement feature that in combination enhances the overall net process in other situations.

[0397] Additionally, plasmon-phonon coupling can be used to lower the resonant frequency by tuning the band some distance off resonance. This may be useful for optimizing the resonant energy transfer process for the purpose of shifting the output color to a color desired for the surface being painted, stained, or displayed. In one example, Figure 27 shows an example of plasmon resonance shift as a function of shell thickness.

[0398] Here, in one embodiment of the present invention, the ability to generate stimulated emission at a targeted wavelength or color or energy is complemented by the ability to engineer nanoparticles with engineered absorption bands. Such absorbing materials may further function to improve the monochromaticity of light observed from, for example, paints, inks, dyes, or otherwise reflective surfaces treated with the color enhancing compositions of the present invention.

[0399] Details of the preparation of this nanoparticle system are contained in U.S. Application No. 12 / 725,108, the entire contents of which are incorporated herein by reference. The absorption spectrum of YO alone (lower trace) is quite featureless, showing absorption due to triarginine and shallow slopes near 200 nm associated with scattering and absorption by YO nanoparticles extending into the visible portion of the spectrum. On the other hand, the gold-coated YO (upper trace) shows a strong absorption band at 546 nm, characteristic of the plasmonic resonance band due to the gold shell around the YO core. The red-shift of the plasmon absorption to 546 nm is consistent with the presence of a gold shell around the dielectric core.

[0400] In one embodiment of the present invention, the converter material for the upconverter dielectric core can include a wide variety of dielectric materials, as described above. In various embodiments of the present invention, the upconverter dielectric core more specifically includes an oxide material doped with a lanthanide. Lanthanides include lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu). Other suitable dielectric core materials include non-lanthanide elements such as yttrium (Y) and scandium (Sc). Thus, suitable dielectric core materials include Y2O3, Y2O2S, NaYF4, NaYbF4, Na-doped YbF3, YAG, YAP, Nd2O3, LaF3, LaCl3, La2O3, TiO2, LuPO4, YVO4, YbF3, YF3, or SiO2. These dielectric cores can be doped with Er, Eu, Yb, Tm, Nd, Tb, Ce, Y, U, Pr, La, Gd, and other rare earth species or combinations thereof.

[0401] Lanthanides usually exist as trivalent cations, in which case their electron configuration is (Xe)4f n and n is 1(Ce 3+) to 14(Lu 3+ ) Transitions within the F-type manifold are responsible for many of the photophysical properties of lanthanide ions, such as long-lived emission and sharp absorption and emission lines. F-type electrons are protected from external perturbations by filled 5s and 5p orbitals, resulting in line-shaped spectra. F-F type electronic transitions are Laporte forbidden, resulting in long excited-state lifetimes in the microsecond to millisecond range.

[0402] Thus, examples of doped materials in the present invention include oxides such as yttrium oxide, neodymium oxide, and aluminum oxide, as well as yttrium sodium fluoride and nanocrystalline perovskites and garnets, such as yttrium aluminum garnet (YAG) and yttrium aluminum perovskite (YAP). Of these materials, some, but not all, require doping to promote upconversion efficiency. In various embodiments of the present invention, the host nanocrystals are doped with trivalent rare earth lanthanide ions from the lanthanide series elements listed above.

[0403] More specifically, in various embodiments of the present invention, these dopant pairs are introduced to make more energy states more accessible in the host crystal. The activation and pumping of these energy states strictly follows the principles described above. The doping concentration in the present invention can range from approximately 0.2% to 20% per ion entering the host lattice, or by weight or mole percent variation. The efficiency of the upconversion process in specific bands of these materials can be modulated by the doped percentage to induce and enhance targeted emission. Lanthanide-doped upconverters can use the following molar percent dopant compositions, but are not limited to: 5% Er, 10% Yb, 0.2% Tm + 3% Yb, and 1% Er + 10% Yb.

[0404] The size of the nanocrystals also affects the efficiency of the upconversion process, since larger nanocrystals accommodate more sites for dopant ions in the host lattice, resulting in higher emission from the same doped host than smaller nanocrystals. While the dopant percentages listed above are not strictly fixed, these numbers provide a basic guide for typical proportions used to achieve specific dielectric core materials of the present invention.

[0405] Also, in one embodiment of the present invention, some of these host crystals (e.g., neodymium oxide) may not require special doping to facilitate upconversion, as was seen in one example with Nd2O3 at an excitation wavelength of 587 nm, which produced emissions at 372 nm, 402 nm, and 468 nm. See Que, W et al., Journal of Applied Physics 2001, vol. 90, pg. 4865, the entire contents of which are incorporated herein by reference. In one embodiment of the present invention, neodymium oxide is doped with Yb 3+ Doping with Nd 3+ ions at lower energy Yb 3+ Upconversion is enhanced by sensitizing with an activator.

[0406] In one embodiment of the present invention, the dielectric core is coated, for example with a metal shell, to enhance electron-phonon coupling and thereby increase the upconversion or downconversion efficiency, as described above. In another embodiment of the present invention, the shell can include a SiO and / or TiO coating, which, in one embodiment, is coated on doped YO upconverting nanoparticles, thereby potentially increasing the upconversion efficiency compared to uncoated nanocrystals. In another embodiment of the present invention, the shell can include a SiO and / or TiO coating, which, in one embodiment, is coated on doped YO downconverting nanoparticles, thereby potentially increasing the downconversion efficiency compared to uncoated nanocrystals. Furthermore, in one embodiment of the present invention, the coating can be a polymer. In one embodiment, the coating is provided on a NaYF:Ln / NaYF dielectric core. Such a coating can increase the upconversion efficiency compared to uncoated upconverters.

[0407] In another embodiment of the present invention, the phonon modes of undoped host lattice (e.g., YO) nanocrystals are modulated by, for example, Au, Ag, Pt, and Pd shells of various thicknesses. In various embodiments of the present invention, an upconverter dielectric core-shell system includes upconverting nanocrystals such as YO:Ln with a NaYF shell, YO:Ln with an Au(Ag,Pt) shell, NaYF:Ln with a YO shell, and NaYF:Ln with an Au(Ag,Pt) shell. In this system, the core diameter and the outer / inner diameter of the metal coating can be configured to dimensions expected to tune the plasmon mode overlap.

[0408] In other embodiments discussed below, metal coatings or metal structures disposed in association with upconversion or downconversion nanoparticles can reside within the dielectric, and the relative position of the metal structures to the dielectric structure can enhance plasmon resonance. These structures with internal metal structures are sometimes referred to as metal-core upconverters or metal-core downconverters. Metal-core technology for energy conversion is useful because it utilizes metal nanoparticles with improved surface morphology compared to shell coatings on core dielectrics. The metal or metal alloy of the internal-core metal energy converter can be selected to tailor its plasmonic activity. These structures with external metal structures are sometimes referred to as core upconverters or core downconverters.

[0409] In various embodiments of the present invention, the dielectric core of an upconverter or downconverter can be coated with a thiol-terminated silane to provide a coating of SiO around the core with similar reactivity to YO. In one embodiment of the present invention, the above methodology is used to synthesize core-shell nanoparticles such as YO:Ln with a NaYF shell, YO:Ln with an Au(Ag,Pt) shell, NaYF:Ln with a YO shell, or NaYF:Ln with an Au(Ag,Pt) shell, where the core-shell diameters can vary from 2 to 20 nm. In these material systems, tuned core-to-shell diameter ratios enable plasmon-phonon resonance, which should amplify the absorption and / or upconverted emission of NIR light. In these material systems, control of the core-shell diameter is one factor determining size-dependent effects and subsequent tuning of the plasmon-phonon resonance.

[0410] In one embodiment of the present invention, the upconverter dielectric core can be a mixed core-shell material, including, for example, semiconducting YO and NaYF cores doped with various Ln-series metals, which have been shown to have high upconversion efficiencies. These doped YO and NaYF cores have shells of Au (Ag, Pt, Pd) or undoped YO and NaYF matrices, which have the potential to enhance or tune the phonon modes required for energy transfer in the upconversion process. Solubility can be enhanced by the addition of, for example, thiolated organics (Au shell), organic chain triethanolsilane (YO shell), and trioctylphosphine-oleic amine (NaYF shell). All core-shell nanoparticles can be further solubilized in colloidal suspensions by adding triarginine peptides, polyethylene glycol, and polyethyleneimine surfactants.

[0411] Figure 28A shows some of the various embodiments of converter structures of the present invention that can be designed: (a) a structure comprising upconverter (UC) molecules bound to metal (gold) nanoparticles; (b) a structure comprising UC-containing nanoparticles capped with metal nanoparticles; (c) a metal nanoparticle capped with a UC-containing nanocap; (d) a UC-containing nanoparticle capped with a metal nanocap; (e) a metal nanoparticle capped with a UC nanoshell; (f) a UC-containing nanoparticle capped with a metal nanoshell; and (g) a UC-containing nanoparticle capped with a metal nanoshell with a protective coating layer.

[0412] The configuration (although shown with UC-containing materials in FIG. 28A) is applicable to enhancing downconverting materials such as quantum dots or phosphorescent materials described herein. Additionally, in one embodiment of the present invention, a dielectric spacer (e.g., a silicate, as described below) can be used with the structure of FIGS. 6A-b to space particle-type metal structures. In another embodiment of the present invention, a dielectric spacer can be used with the structure of FIG. 28A to space metal layers, whether these layers are partial or continuous metal layers. See the schematic diagram in FIG. 28B.

[0413] In various embodiments of the present invention, the multilayer metallic nanoshells discussed herein have the potential to electromagnetically enhance two spectral regions. Thus, the metallic structures of the present invention can be used in upconversion mode to enhance both excitation at wavelength λ1 and emission at wavelength λ2. This feature can also be used in downconversion to primarily enhance emission at wavelength λ2, potentially used for excitation at wavelength λ1.

[0414] Such metallic structures in various embodiments of the present invention include conductive materials made of, for example, metals, or doped glasses or doped semiconductors. These conductive materials can be in the form of pure or nearly pure elemental metals, alloys of such elemental metals, or layers of conductive materials, regardless of constituents. The conductive materials can include non-metallic materials as minor constituents that do not render the composite insulating at the level of incorporation (as described above).

[0415] Similarly, in various embodiments of the present invention, the up- or down-converting material can include at least one of a dielectric, a glass, or a semiconductor. The up- or down-converting material can include an alloy of two or more dielectric materials, an alloy of two or more glasses, or an alloy of two or more semiconductors.

[0416] Thus, Figure 28A depicts an embodiment of the present invention in which a dielectric core is supplemented with a shell. The shell can include a metal layer of a predetermined thickness. The metal layer can include materials such as nickel, gold, iron, silver, palladium, platinum, copper, and combinations thereof. The metal layer can also be made of a combination of metal and non-metal. Surface plasmons can form in the metal between the dielectric core and the external environment, which acts as a shell plasmon shell, and the external environment, which acts as an external dielectric. The shell may not be a complete shell (as shown). Partial metal shells or metal shells of various thicknesses are also permissible in the present invention.

[0417] As explained below, the metal shell in another embodiment of the invention acts as a scattering center for UV light, which, even if absorbed by the paint or coating layer, at least contributes to localized heating of the paint or coating layer material and is scattered from the paint or coated layer.

[0418] Figure 28C shows yet another embodiment of plasmonics-active nanostructures with engineerable upconverting (UC) materials: (a) metal nanoparticles, (b) UC nanoparticle cores covered with metal nanocaps, (c) spherical metal nanoshells covering UC spheroid cores, (d) flat metal nanoshells covering UC spheroid cores, (e) metal nanoparticle cores covered with UC nanoshells, (f) metal nanoshells with protective coating layers, (g) multilayer metal nanoshells covering UC spheroid cores, (h) multi-nanoparticle structures, (i) metal nanocubes and nanotriangles / nanoprisms, and (j) metal cylinders.

[0419] Figure 28D shows yet another embodiment of a plasmonics-active nanostructure with an upconverting material having linked photoactive (PA) molecules that can be engineered. For example, in the case of psoralen (as the PA molecule), the length of the linker between the PA molecule and the UC material or metal surface is tailored so that the PA molecule is long enough to be active (attach to DNA) and short enough to allow efficient excitation of light from the UC to efficiently excite the PA molecule. Figure 28D shows (a) a PA molecule bound to a UC nanoparticle, (b) a nanoparticle comprising a UC material covered with metal nanoparticles, (c) a metal nanoparticle covered with a UC material nanocap, (D) a nanoparticle comprising a UC material covered with a metal nanocap, (e) a metal nanoparticle covered with a UC material nanoshell, (f) a nanoparticle comprising a UC material covered with a metal nanoshell, and (g) a nanoparticle comprising a UC material covered with a metal nanoshell with a protective coating layer.

[0420] The plasmonic effect is advantageous in the upconverter and downconverter structures of the present invention. The plasmonic effect can increase the local intensity of light received or emitted from the upconverter and / or downconverter structures of the present invention. The plasmonic effect can occur throughout the electromagnetic range when appropriate nanostructures, nanoscale dimensions, and metal types are used. The plasmonic effect can occur across a wide range of the electromagnetic spectrum, from gamma rays and X-rays to ultraviolet, visible, infrared, microwave, and radio frequency energy. However, for practical reasons, visible and NIR light are used with metallic structures, such as silver and gold nanoparticles, because the plasmonic resonances of silver and gold occur in the visible and NIR regions, respectively.

[0421] In various embodiments, nanoparticles of neodymium- and ytterbium-doped yttrium oxide, europium- and ytterbium-doped yttrium oxide, and any combination of rare earth trivalent ions doped into neodymium oxide nanocrystals can be used. While the dual-doped yttrium oxide compositions of neodymium and ytterbium, and dual-doped europium and ytterbium are new to the yttrium oxide host lattice, such dual-doped systems have been shown to work in other host lattices, such as YAG.

[0422] These dual-doped lanthanide glasses have been shown to efficiently upconvert in bulk materials, thereby providing novel upconverter structures at the nanoscale. These yttrium oxide nanostructures of the present invention offer advantages. Small-scale synthesis methodologies for creating nanoscale yttrium oxide are easier to control and manufacture with yttrium oxide than with YAG. The yttrium oxide host structure scintillates through downconversion. For example, these combinations of dopants in yttrium oxide can provide a predetermined emission color for the yttrium oxide nanocrystals for the color transfer of the present invention.

[0423] In one embodiment of the present invention, the dual dopant allows excitation of either ion in the host glass. For example, excitation with 980 nm light excites ytterbium ions. Energy transfer from one excited state of the ytterbium ions to another dopant provides a mechanism for upconversion emission of light in the visible and NIR spectral regions.

[0424] Upconversion phosphors can be used that have chemical compositions similar to the downconversion fluorescent materials discussed above. Upconversion phosphors can include laser dyes, e.g., small organic molecules that can be excited by absorption of at least two infrared photons with visible light emission. Upconversion phosphors can include fluorescent polymers, e.g., a class of polymers that can be excited by absorption of at least two infrared photons with visible light emission. Upconversion phosphors can include inorganic or ceramic particles or nanoparticles, including conventional upconversion phosphors (e.g., metal fluorides, metal oxides) that can be excited by absorption of at least two infrared photons with visible light emission. Upconversion phosphors can include semiconductor particles, including nanoparticles such as II-VI or III-V compound semiconductors, such as quantum dots, as described in detail above under "downconversion" semiconductors.

[0425] Fluorescent upconversion inorganic phosphorescent materials can include, but are not limited to, metal oxides, metal halides, metal chalcogenides (e.g., sulfides), or hybrids thereof, such as metal oxohalides and metal oxochalcogenides. Fluorescent upconversion inorganic phosphorescent materials typically contain rare earth elements (e.g., Yb 3+ , Er 3+ , Tm 3+ ) are doped. Some example hosts include, but are not limited to, NaYF4, YF3, BaYF5, LaF3, La2MoO8, LaNbO4, and LnO2S, where Ln is a rare earth element such as Y, La, or Gd.

[0426] In accordance with the present invention, these upconversion and downconversion materials are mixtures of color emitters configured to emit visible light at a first wavelength λ1 in response to absorption of light or energy across a wavelength band within and outside the visible spectrum when exposed to a light source, where the emission of visible light is enhanced relative to the amount of light emitted solely by reflection of the first wavelength λ1.

[0427] The color emitter particles can have a diameter of less than about 1000 nanometers. The light-emitting particles (up or down) can include a metallic structure disposed relative to the particle. The physical properties of the metallic structure can be set to values ​​that cause a surface plasmon resonance in the metallic structure to resonate at a frequency that provides spectral overlap with any of the first wavelengths λ1. The physical properties of the metallic structure can be set to values ​​that cause a surface plasmon resonance in the metallic structure to resonate at a frequency that provides enhanced emission at the first wavelength λ1.

[0428] Other Applications of Color Enhancement / Enhancement Structures: As described in more detail below, mixtures of the above color emitters and color enhancement structures (optionally including the above energy enhancement factors) can be used in displays. The mixtures of the above color emitters and color enhancement structures can be color-emitting pixel display elements. The mixtures of the above color emitters and color enhancement structures can be components of color filters. The mixtures of the above color emitters and color enhancement structures can be components of color filters for displays. The mixtures of the above color emitters and color enhancement structures can be components of colored surfaces. The mixtures of the above color emitters and color enhancement structures can be components of colored reflective surfaces. The mixtures of the above color emitters and color enhancement structures can be components of colored reflective surfaces in pixels for displays. The mixtures of the above color emitters and color enhancement structures can be components of white-light-emitting pixel display elements. The mixtures of the color emitters can be paint components. The mixtures of the above color emitters and color enhancement structures can be components disposed on glass beads of retroreflective paint. The mixture of color emitters and color-enhancing structures described above can be a component of a binder layer that secures the glass beads in the retroreflective paint to the base paint. The mixture of color emitters can be a component of an ink.

[0429] The mixture of color emitters and color enhancement structures can be at least one of red, blue, and green emitters configured to generate red, blue, and green emissions from an upconversion process. The mixture of color emitters and color enhancement structures can be at least one of red, blue, and green emitters configured to generate red, blue, and green emissions from a downconversion process. The mixture of color emitters and color enhancement structures can be at least one of red, blue, and green emitters configured to generate red, blue, and green emissions from a mixture of upconverters and downconverters.

[0430] The color emitter mixture included in the color enhancement structure can be a fluorescent emitter including at least one of europium, terbium, cerium, and erbium, or a combination thereof. The color emitter and color enhancement structure mixture can include a first material configured to emit a first visible color in response to absorption of ultraviolet light and a second material configured to emit a second visible color in response to absorption of infrared light, where the second visible color is different from the first visible color. The color emitter and color enhancement structure mixture can include a third material configured to emit a third visible color in response to absorption of ultraviolet light, where the third visible color is different from the first and second visible colors. The first, second, and third visible colors can be primary colors or mixtures of primary colors. Alternatively, or in addition, the color emitter and color enhancement structure mixture can include a third material configured to emit a third visible color in response to absorption of infrared light. The third visible color may be different from the first visible color and the second visible color.

[0431] The mixture of color emitters and color enhancement structures may include a first material configured to emit a first visible color in response to absorption of ultraviolet light and a second material configured to emit a second visible color in response to absorption of infrared light. The second visible color may be substantially the same color as the first visible color. The mixture of color emitters and color enhancement structures may include a third material configured to emit a third visible color in response to absorption of ultraviolet light. The third visible color may be different from the first and second visible colors. Alternatively, or in addition, the mixture of color emitters and color enhancement structures may include a third material configured to emit a third visible color in response to absorption of infrared light. The third visible color may be different from the first and second visible colors. The first, second, and third visible colors may be primary colors or mixtures of primary colors.

[0432] The mixture of color emitters and color enhancement structures can include a metal structure disposed in association with the nanoparticle emitters. The metal structure can be a metal shell, including at least one of a spherical shell, an oblate shell, a crescent-shaped shell, or a multi-layer shell. The metal structure can be at least one of Au, Ag, Cu, Ni, Pt, Pd, Co, Ru, Rh, Al, Ga, or a combination, alloy, or layer thereof. The nanoparticle emitters can be at least one of YO, YO2O, YO2S, NaYF, NaYbF, YAG, YAP, NdO, LaF, LaCl, LaO, TiO, LuPO, YVO, YbF, YF, Na-doped YbF, or SiO or an alloy or layer thereof. The nanoparticle emitters can include dopants including at least one of Er, Eu, Yb, Tm, Nd, Tb, Ce, Y, U, Pr, La, Gd, and other rare earth species or combinations thereof. The dopants can have a concentration between 0.01% and 50% molar.

[0433] The color emitters are Y2O3;ZnS;ZnSe;MgS;CaS;Mn, ErZnSe;Mn, ErMgS;Mn, ErCaS;Mn, ErZnS;Mn, YbZnSe;Mn, YbMgS;Mn, YbCaS;Mn, YbZnS:Tb 3+ , Er 3+ ;ZnS:Tb 3+ ;Y2O3:Tb 3+ ;Y2O3:Tb 3+ , Er3 + ;ZnS:Mn 2+ ;ZnS:Mn, Er 3+ The color emitter may be a downconverter including at least one of alkali lead silicates, including compositions of SiO2, B2O3, Na2O, K2O, PbO, MgO, or Ag, and combinations, alloys, or layers thereof. The color emitter may be a dielectric upconverter including at least one of Y2O3, Y2O2S, NaYF4, NaYbF4, YAG, YAP, Nd2O3, LaF3, LaCl3, La2O3, TiO2, LuPO4, YVO4, YbF3, YF3, Na-doped YbF3, or SiO2 or alloys or layers thereof. The dielectric upconverter may have a particle size in at least one range of 2 to 1000 nm, 2 to 100 nm, 2 to 50 nm, 2 to 20 nm, or 2 to 10 nm. The dielectric upconverter can include at least one dopant selected from Er, Eu, Yb, Tm, Nd, Tb, Ce, Y, U, Pr, La, Gd, and other rare earth species, or combinations thereof. The dopant can have a concentration of 0.01% to 50% molar. A metal structure can be disposed in association with the dielectric upconverter, the metal structure including at least one of Au, Ag, Cu, Ni, Pt, Pd, Co, Ru, Rh, Al, Ga, or alloys or layers thereof. The dielectric upconverter can be configured to exhibit visible emission upon interaction with NIR light.

[0434] Methods for applying antennas to particles used as pigments and dyes for color enhancement: In various embodiments, the present invention provides color enhancement of various paint pigments and dyes. The fabrication of these "micro color enhancement augmentation devices" is described below.

[0435] In one embodiment, a glass substrate is used as the carrier in that case. The glass substrate can be made of a variety of compositions, including soda-lime silicate, borosilicate, and sodium aluminosilicate.

[0436] In this embodiment, the glass substrate is exposed to a molten form of potassium salt, KNb3, to exchange the sodium in the glass for potassium in the molten bath. During this ion exchange, the outermost layer is compressed because the potassium ions are larger than the sodium ions. The compressed layer is characterized by its penetration depth and potassium concentration. Sodium aluminosilicates with a gamma ratio Γ greater than 1 provide a glass vehicle with a shallow potassium penetration depth and high potassium concentration. The gamma ratio Γ in this case refers to the ratio of the number of moles of Al2O3 to NaO2 in the glass chemistry. In this way, a thin potassium-rich layer under high compression is formed on a sodium-rich glass layer under tension. Figure 37 is a schematic diagram of a compressed layer substrate configuration according to one embodiment of the present invention.

[0437] The glass substrate is then coated with a slurry containing paint pigments or dyes dissolved or mixed in a solvent (if desired). The slurry can be applied using a variety of techniques, including but not limited to spin coating, draw bar, Mayer bar, screen printing, or simply printing using an inkjet printer equipped to handle solvents. The substrate is then dried at low temperature to remove the solvent. The "painted" layer is now ready to receive the antenna.

[0438] Figure 38 is a schematic diagram of a coating layer formed on the compressed layer substrate configuration of Figure 37. At this stage, the glass substrate may have a paint pigment or dye coating or a phosphorescent material layer applied as a coating. The present invention can have any of the converters described herein for the coating layer. In this example, the compressed layer thickness may be approximately 5 microns thick. Coatings containing pigments, dyes, phosphorescent materials, or other converters may be in the 3 micron thick range.

[0439] The antenna (or resonator) structure is created on a separate substrate, preferably a silicon wafer coated with a thin glass chemistry. The wafer on which the antenna is created undergoes various steps of photodefinable lithography-type steps such as chemistry, etching, and metallization to lay out the desired antenna structure. Once the antenna is ready, a laser can drill through the glass layer attached to the silicon wafer. Laser drilling can be performed in columns and rows to identify each antenna structure.

[0440] The antenna structure is now ready to be transferred using, for example, microtransfer printing techniques, as depicted in the process shown in Figure 39. A source wafer has the desired antenna pattern. A patterned stamp picks up multiple antennas and transfers them to a target substrate (in this case, a glass substrate coated with paint pigment).

[0441] This process is known as it can be used to transfer small nano- and micro-sized features from a source to a target substrate. The source substrate can be a wafer on which various devices are finely fabricated, such as integrated circuits, LEDs, or in this case, antennas. The target wafer can be various other substrates, such as plastic, glass, ceramic, or paper. Figure 40 provides an overview of this process.

[0442] In one embodiment of the present invention, the antenna structure is transferred from a Si wafer containing lithographically defined antennas to a glass substrate precoated with pigments or dyes or phosphorescent materials or other converters. Figure 41 is a schematic diagram of a micro-transferred antenna on a precoated compressive stress glass substrate.

[0443] Once the antenna is placed on the glass substrate, an optional coating is applied to the glass layer. Preferably, this optional coating is similar to a previously applied coating of paint pigment, dye, or phosphorescent coating. The glass substrate has a multilayer structure with the antenna (resonator) of the present invention embedded in a pigment or organic dye, as shown in the schematic diagram. Figure 42 is a schematic diagram showing the multilayer structure of the present invention with the antenna (resonator) of the present invention embedded therein.

[0444] To facilitate the release of the antenna embedded in the paint pigment, a diamond scribe is used to penetrate the compressive layer and bridge it to the tensile region. Once this is achieved, instantaneous fragmentation of the glass into tiny pieces occurs. When released from the glass dome, the glass shatters into millions of projectiles.

[0445] Figure 43 is a schematic diagram illustrating the formation of individual micro-color energy enhancing agents of the present invention. When glass is shattered, the resulting shards contain a glass portion with a coating thereon that has an antenna embedded therein.

[0446] Stainless steel, aluminum, and copper are some examples of materials that do not necessarily require a coating, painting, staining, or sealed protective layer. Coated surfaces are almost always a particular color chosen to enhance the object's appeal.

[0447] As explained at http: / / www.howeverythingworks.org / supplements / paint.pdf, pigment particles in paint are responsible for the paint's opacity or color. Pure white paint contains pigments that do not absorb light but scatter it in random directions. White pigment particles are transparent and have a relatively high refractive index. The pigment particles are embedded in a polymer layer. When light attempts to pass through the paint, some of the light is reflected at every boundary between the polymer and the pigment, and most of the light does not reach the other side of the layer. Because the pigment particles in paint are typically coarsely and randomly oriented, the pigment particles scatter light in all directions, making the paint appear white. This high reflectivity gives paint its hiding power, or the ability to prevent light from reaching the material below the paint and then returning to the paint's surface.

[0448] Paints with very high refractive index pigments are ideal for hiding the surfaces they cover. The pigment's absorption of light gives the paint its color. For example, a pigment that absorbs blue light will give the paint a yellow tint. The reflected light will have the color characteristic of the non-absorbing color in the spectrum. In other words, colored pigments give the paint its color by selectively absorbing part of the spectrum of light that strikes the paint.

[0449] U.S. Pat. No. 4,283,320 (the entire contents of which are incorporated herein by reference) describes an opacifying latex paint having a small particle film-forming latex binder combined with a small amount of opacifying pigment, and a significant amount of non-film-forming polymer particles (plastic pigments) to provide a semi-gloss latex paint composition with excellent hard enamel surfaces along with desirable film integrity properties. The plastic pigment particles of U.S. Pat. No. 4,283,320 are approximately 0.1 to 0.5 microns in size and contain 0.2 to 2% copolymerized monomers containing carboxylic acid groups. The semi-gloss plastic pigment latex paint of U.S. Pat. No. 4,283,320 is formulated with a pigment volume content (PVC) of between approximately 30% and 45%, significantly higher than conventional high-quality enamel latex paints. In one embodiment of the present invention, the color-enhancing mixture described herein is applied to the latex paint of U.S. Pat. No. 4,283,320 or to the painted surface of U.S. Pat. No. 4,283,320.

[0450] U.S. Patent No. 5,134,186 (the entire contents of which are incorporated herein by reference) describes a paint having a film-forming agent and a polymer composition. The polymer composition comprises about 30 to about 50 weight percent of a substantially non-self-polymerizable monomer and about 50 to about 70 weight percent of a copolymerizable monomer having a water-soluble homopolymer. In one embodiment of the present invention, the color-enhancing mixture described herein is applied to the latex paint of U.S. Patent No. 5,134,186 or to the painted surface of U.S. Patent No. 5,134,186.

[0451] U.S. Patent No. 4,789,694 (the entire contents of which are incorporated herein by reference) describes a paint coating composition having a cation-free functional emulsion polymer mixture adapted to co-react at room temperature with glycoluril to provide a cured thermosetting paint film. Curing involves copolymerizing ethylenically unsaturated monomers, including functional monomers but excluding amine monomers, in an aqueous polymerization medium, followed by ion exchange of the resulting reactive emulsion polymer. The glycoluril can be processed through the ion exchange step either individually or in combination with the reactive emulsion polymer. In one embodiment of the present invention, the color-enhancing mixture described herein is applied to the latex paint of U.S. Patent No. 4,789,694 or to the painted surface of U.S. Patent No. 4,789,694.

[0452] U.S. Patent No. 4,613,633 (the entire contents of which are incorporated herein by reference) describes a copolymer latex having non-uniform polymer particles particularly suitable for coating paper, and a paper coating composition containing this latex that provides coated paper with improved adaptability for blister packaging and printing. In one embodiment of the present invention, the color enhancing mixture described herein is applied to the latex paint of U.S. Patent No. 4,613,633 or to the painted surface of U.S. Patent No. 4,613,633.

[0453] U.S. Patent No. 7,682,435 (the entire contents of which are incorporated herein by reference) describes an oil-based pigmented ink composition comprising at least a pigment, a polymer compound, and an organic solvent, wherein the organic solvent comprises 20 to 90% by weight of methoxybutyl acetate based on the total ink composition, and particularly comprises, as other organic solvents, 1 to 50% by weight of a nitrogen-containing and / or oxygen-containing heterocyclic compound and / or 1 to 50% by weight of a (poly)alkylene glycol derivative based on the total ink composition. The oil-based pigmented ink composition has a flash point of 61° C. or higher, a viscosity of 2.0 to 6.5 cp at 25° C., and a surface tension of 20 to 40 mN / m at 25° C. In one embodiment of the present invention, the color-enhancing mixture described herein is applied to the oil-based colored ink of U.S. Patent No. 7,682,435 or to a painted surface of U.S. Patent No. 7,682,435.

[0454] U.S. Patent Application Publication No. 20090088500 (the entire contents of which are incorporated herein by reference) describes an oil-based ink composition comprising a colorant, an organic solvent, and a polymer compound, and optionally an alkylamine ethylene oxide derivative as a pH adjuster, wherein when ions in the ink composition migrate to water, the pH of the aqueous phase is 5.5 to 10. This oil-based ink composition prevents nozzle plate corrosion and has improved storage stability, ensuring printer reliability, such as inkjet stability, even after long-term storage and can withstand outdoor use environments. In one embodiment of the present invention, the color enhancement mixture described herein is applied to the oil-based ink composition of U.S. Patent Application Publication No. 20090088500.

[0455] In general, the color enhancing mixtures and color enhancing / boosting structures described hereinabove can be applied to other paints or inks to enhance the color perceived by the viewer.

[0456] The human eye is not an instrument for measuring precise wavelengths of light. Instead, it sees three distinct wavelength ranges. The retina of the human eye contains specialized cells that detect only certain wavelengths of light. Some of these cells detect reddish light, some greenish light, and some bluish light. These three types of color-sensitive cells are called cones. Cones are most abundant in the fovea, a region of high visual acuity near the center of the retina. Retinal cells are more sensitive to light than cones but cannot distinguish between colors. Rod cells detect light and dark. These three types of color sensors are sometimes thought to allow humans to see only three colors. However, stimulating two or more of the color sensors simultaneously results in the perception of various colors. Each sensor informs the brain about the amount of light being seen, and the brain blends the responses to interpret them as a specific color.

[0457] In general, a particular wavelength of visible light stimulates all three types of cone cells to some degree. However, the cells do not respond equally to each wavelength of light. When exposed to 680 nm (680 nanometers) light, the cones specialized for reddish light respond much more strongly than the cones specialized for greenish or bluish light. This strong response by the red sensors causes the light to appear red. Yellow light, at 580 nm, is intermediate between red and green light. Both red-sensitive cones and green-sensitive cones respond moderately when exposed to yellow light. The brain interprets this balanced response as yellow light.

[0458] However, the same response can be evoked from the retina by exposing it to an equal mixture of pure red and green light. Again, both red-sensitive and green-sensitive cones respond appropriately, and even if there is no pure yellow light at 580 nm reaching the retina, it appears to the brain as yellow light. Similarly, by combining pure red, green, and blue light, we can see virtually any color. The only problem is selecting the pure red, green, and blue wavelengths. This is the technique used in television: it creates relatively pure red, green, and blue light with dots of phosphorescent material, "tricking" the eye into seeing any color across the visible spectrum.

[0459] So, in a red paint, the paint absorbs light that stimulates the green or blue sensors in the human eye. All that's left is reflected light that stimulates the red sensors, and therefore the eye perceives the paint as red. Most paint pigments are based on specific molecules that absorb light in specific wavelength ranges. Many metal compounds, such as copper, chromium, iron, antimony, nickel, and lead, absorb specific wavelengths of light and appear brighter. Starting with white light, paint of any color can be created by removing various amounts of the three primary colors of light. If all light is removed, the paint appears black. Yellow pigments absorb some blue light, and cyan pigments absorb some red light. What's left is mostly green light. The more of each primary pigment added to a paint, the more completely the paint absorbs that color of light, and the deeper the color.

[0460] Ink is similar to paint, except that it contains dissolved dyes rather than solid pigment particles. Ink does not contain any reflective white pigments. Ink itself can be transparent, but tends to be colored. Ink reflects light depending on the paper underneath. Paper is primarily composed of cellulose, a transparent natural polymer. Because cellulose is finely divided in paper, it reflects light from each side, making the paper appear white. Often, white paint pigment is applied to paper during manufacturing to make it even whiter.

[0461] In one aspect of the present invention, the usual dynamics of light absorption in paint, which normally results only in heating of the paint, is altered to one in which the absorbed light (normally lost from absorption) emits a light color that is the intended paint color. Thus, the brightness of the paint, ink, or coating is enhanced over that normally lost through absorption, particularly in paints or inks containing the color-enhancing structures described above. Furthermore, "color shift" from the ultraviolet or infrared bands of light outside the visible range, which normally contribute nothing to the perceived light reflected to the eye, provides an additional source of color enhancement.

[0462] In the past, fluorescent inks were produced using fluorescent pigments that absorb in the visible light range and replace the organic or inorganic color pigments typically used in printing inks. To identify the fluorescent image formed on the image print, the image print must be irradiated with ultraviolet light as excitation light. When the image print is irradiated with ultraviolet light, the ultraviolet light is absorbed by the fluorescent material in the fluorescent image, thereby emitting fluorescence in the visible range. This fluorescence can be recognized by visual observation or using a camera, and represents a limited demonstration of the concepts utilized and further expanded by the present invention. In one aspect of the present invention, a mixture of down-converting particles tuned to specific excitation and emission is used in place of fixed phosphor particles and in the aforementioned color enhancement structure. In one aspect of the present invention, a mixture of down-converting particles tuned to specific excitation and emission is used in place of or as a complement to the mixture of down-converting particles and in the aforementioned color enhancement structure.

[0463] As described in U.S. Patent No. 6,744,960 (the entire contents of which are incorporated herein by reference) and applicable to the present invention, pump radiation can include natural light, i.e., sunlight, or artificial light, such as from UV or blue light-emitting diodes (LEDs) or fluorescent lamps. The light incident on the fluorescent structure need only include radiation with wavelengths within the absorption spectrum of the quantum dots. Because the absorption spectrum of quantum dots includes wavelengths shorter than the emission wavelengths from the quantum dots, the pump radiation includes wavelengths shorter than the emitted wavelengths. For example, sunlight can be used to pump a fluorescent structure 10 having a layer of quantum dots containing 5.0 nm diameter CdSe particles that emit at a wavelength of 625 nm. This is because the sun emits light over a broad spectrum, including light with wavelengths at least 50 nm shorter than 625 nm. Alternatively, such a fluorescent structure can be pumped with one or more light-emitting diodes (LEDs) that provide light at, for example, 550 nm. Ultraviolet light sources, such as incandescent lamps or UV LEDs, can also excite a layer of quantum dots.

[0464] The fluorescent structures applicable to the present invention, as described in U.S. Patent No. 6,744,960, can be used in a variety of applications requiring bright, narrow-band illumination. For example, colored lighting sources are useful for creating signage, artistic or architectural designs, and brightly colored areas such as outlines, bands, and borders on products where bright colors serve aesthetic or functional purposes, including, but not limited to, furniture, automobiles, appliances, electronic devices, clothing, or other objects. These fluorescent structures are advantageously capable of producing intense colored light illumination during the day when exposed to sunlight. Because quantum dots do not degrade when exposed to ultraviolet light such as that produced by the sun, the structures have a long lifespan and can be incorporated into architectural features, such as borders that highlight building rooftops during the day.

[0465] Yet, unlike U.S. Patent No. 6,744,960, in the present invention, upconverting particles stimulated by IR light from natural or artificial sources complement the fluorescence, resulting in a much brighter structure. Furthermore, the mixture of the above-described downconverter and color-enhancing / boosting structures can be tailored to utilize a broader spectrum of "out-of-band" color regions from natural or artificial radiation sources, e.g., to emit specific colors or primary colors.

[0466] Yet another embodiment of the present invention provides a light-emitting composition comprising a first color emitter configured to emit visible light at a target color in response to absorbing energy at a first band of wavelengths when exposed to an energy source, and a second color emitter configured to emit visible light offset from the target color in response to absorbing energy at the first band of wavelengths when exposed to an energy source, such that the intensity of light observable at the target color is increased relative to reflected white light without the emission from the first and second color emitters, particularly when the color-enhancing / augmenting structures described above are included in the composition. Furthermore, by offsetting the emission relative to the target color, the resulting color appears richer to the human eye. The offset can be 5, 10, 15, 20, 25, 30 nm, or more. The offset can be a positive or negative offset from the target color. More specifically, the purity or chromaticity of the color can be altered by the offsets defined above.

[0467] In another embodiment, the offset value can create a saturation quality that makes the target color appear different under different lighting conditions. For example, a room painted a particular target color by blending different color emitters will appear different at night (under artificial lighting conditions) than in daylight. The offset can be 50, 100, 150, 200, 250, 300 nm or more. The offset can be a positive or negative offset from the target color.

[0468] Additionally, the target color can be varied from the original color by adding white pigment to create a lighter version or black pigment to create a darker version.

[0469] Table 2 included below contains recognized wavelength intervals for the major visible color bands. [Table 2]

[0470] One area of ​​particular application for color-shifting particle mixtures is their use as a coating on glass beads for use in retroreflective paints. Figure 7 shows a schematic diagram of the geometry of retroreflective paints. The glass beads function as optical elements that direct incident light back toward the observer along a reflective path that is nearly, if not perfectly, aligned with the incident light ray. Instead of diffuse scattering, the light is directed backward and appears brighter than "normal." In the present invention, the color-shifting particle mixtures and the color-enhancing / augmenting structures described above are applied to a paint binder or, as shown in Figure 44, as a color converter layer on the glass beads, converting light (not the color of the painted surface) to the color of the painted surface (or a combination of primary color emissions that simulates the color of the painted surface), achieving additional light enhancement.

[0471] There are two classes of retroreflective beads for traditional retroreflective road paint applications: IGB-I and IGB-II. IGB-I is used to mix with the paint before stripping the road. As the paint layer wears off, the beads are exposed, improving the visibility of the road markings. IGB-II is used and dropped onto the freshly stripped paint surface of the road, instantly improving nighttime driver visibility. Table 3 (adapted from http: / / www.indoglassbeads.com / road-marking-glass-beading.htm) presents the recognized specifications for these materials. [Table 3]

[0472] U.S. Patent No. 5,650,213 (the entire contents of which are incorporated herein by reference) describes a retroreflective composition having a nonvolatile matrix material, a volatile component, and a plurality of retroreflective microsphere beads, wherein the ratio of the volume of the matrix material to the volume of the retroreflective microsphere beads ranges from 75% to 185%. The retroreflective microsphere beads in U.S. Patent No. 5,650,213 were 20 to 200 microns in diameter, composed of glass, and had refractive indices ranging from 1.7 to 2.5. In one embodiment of the present invention, these and other retroreflective compositions include the color-enhancing mixture of the present invention (optionally the color-enhancing / augmenting structure described above) coated thereon or onto the coating composition itself.

[0473] Thus, in the present invention, for example, glass beads of blue paint have downconverters and upconverters in the color converter layer and include the above-described color enhancing / boosting structures on the glass beads so that white light (e.g., from a car headlight) converts more of its UV and IR light to blue light, thereby producing more blue light reflected from the blue painted surface. Alternatively, for a green painted surface, white light converts more of its UV and IR light to green, thereby producing more green light reflected from the glass beads on the painted surface.

[0474] In one embodiment of the present invention, retroreflection bounces light rays around a 3D reflective surface to send them back toward the light source. The micro color enhancers (resonator / antenna structures) of the present invention are added to glass beads to form, in one embodiment, paint additives, such as for coating highway panels. Figure 45 is a schematic diagram showing the effect of the amplifier / resonator antenna of the present invention on a coating.

[0475] In addition to their use in traffic signs and other coating applications, these retroreflective / resonator structures can be applied in many applications where light is used to scan an object and "read" the reflected light, as well as in barcode applications.

[0476] Figure 46 shows a schematic diagram of a painted surface with a color transfer layer disposed as a topcoat. As before, the blue paint of the color-enhancing / augmenting structure described above has a color converter layer downconverter and / or upconverter applied to the topcoat, so that white light (e.g., light from a car's headlights) has more UV and IR light converted to blue light, thereby producing more blue light reflected from the blue painted surface. Alternatively, in the case of a green painted surface, white light has its UV and IR light converted to more green light, thereby producing more green light reflected from the glass beads on the painted surface.

[0477] In another embodiment, colors in the visible portion of the spectrum are also color-shifted. The blue paint of the color-enhancing / augmenting structure described above has a color converter layer downconverter and / or upconverter applied to the topcoat, with deep blue and red-green light converting white light (e.g., light from a car headlight) to more blue light, thereby producing more blue light reflected from the blue painted surface. Alternatively, in the case of a green painted surface, white light converts its blue and red light to more green light, thereby producing more green light reflected from the glass beads on the painted surface.

[0478] In other words, in the color converter layer of the present invention, along with the color enhancement / boosting structure described above, a red paint or ink has color-shifting particles that downconvert light with a higher energy than red (e.g., blue light) and / or upconvert light with a lower energy than red (e.g., near-infrared and infrared light). Similarly, a green paint or ink has color-shifting particles that downconvert light with a higher energy than green (e.g., blue light) and / or upconvert light with a lower energy than green (e.g., red, near-infrared, and infrared light). Similarly, a blue paint or ink has color-shifting particles that downconvert light with a higher energy than blue (e.g., UV light) and / or upconvert light with a lower energy than blue (e.g., green, red, near-infrared, and infrared light).

[0479] Cosmetics: Cosmetics are substances used to improve a person's appearance or smell. Cosmetics include, but are not limited to, skin care creams, lotions, powders, perfumes, lipstick, fingernail and toe polish, eye and facial makeup, perms, colored contact lenses, hair color, hairsprays and gels, deodorants, baby products, bath oils, bubble baths, bath salts, butters, and many other types of products. A subset of cosmetics is called "makeup," which refers primarily to colored products intended to alter the wearer's appearance. Many manufacturers distinguish between beautifying cosmetics and caring cosmetics.

[0480] In one aspect of the invention, the above color mixtures with the above color enhancing / boosting structures are included in those cosmetic products intended to alter the appearance of the user. In one aspect of the invention, the above color mixtures are included in cosmetic products used to protect the body from the harmful effects of UV aging.

[0481] Therefore, suitable products for inclusion of the above-mentioned color mixture with the above-mentioned color-enhancing / enhancing structure include, but are not limited to, lipstick, lip gloss, lip liner, lip plumper, lip balm, lip conditioner, lip primer, and lip booster. These products also include foundations, usually liquid, cream, or powder, used to smooth out the face, cover spots, or uneven skin tone. These products may also include powders used to give a matte finish or hide minor blemishes or blemishes. These products may also include lipstick, blusher, or blusher, and blusher, used to enhance the color of the cheeks and make the cheekbones appear more defined. These products may also include bronzers, used to add a touch of color to the skin by adding a golden or bronze glow. These products may also include mascara, used to darken, lengthen, or thicken eyelashes (available in natural colors such as brown and black, but also in bolder colors such as blue, pink, and purple). These products include eyeliners, eye shadows, eye shimmers, eye glitter pencils, various colored pencils used to color and highlight eyelids, eyebrow pencils, creams, waxes, gels, and powders used to color and define eyebrows. These products may further include nail polishes used to color fingernails and toenails. These products may further include concealers and makeup used to cover any skin imperfections.

[0482] The general category of cosmetics also includes skin care products. These include creams and lotions that moisturize the face and body, sunscreens that protect the skin from UV damage, and treatment products that repair or conceal skin problems (such as acne, wrinkles, and dark circles under the eyes). Cosmetics can be liquid or cream emulsions, both pressed and loose powders, dispersions, and anhydrous creams or sticks.

[0483] In this application, the color mixture of the present invention with the color enhancing / boosting structure described above can both provide color transfer functionality (as detailed above), but can also mitigate UV photodamage to skin or hair exposed to UV light irradiation. Thus, the cosmetic product can additionally or optionally provide a protective coating having a mixture of light-scattering and light-emitting particles configured, upon exposure to UV light, to convert a first portion of the UV light to visible light, emit a portion of the visible light from the mixture, and reflect a second portion of the UV light from the mixture so that the second portion of the UV light is not absorbed by the skin or hair.

[0484] For example, and without limitation to the details described below, UV light from the sun that strikes a protective coating may reflect more than 50% of the UV light due to the change in refractive index between air and the protective coating. That portion of the UV light that enters the inner layer of the protective coating is converted to visible light. The other portion of the UV light is scattered from the protective coating and does not strike the underlying surface.

[0485] In any case, the color transfer mixture of the present invention can comprise a cosmetically acceptable medium that is compatible with all skin, lip, or hair materials with which it comes into contact. When these compositions with the above-mentioned color enhancing / boosting structures are to be applied in the form of an emulsion, the composition can optionally additionally comprise a surfactant, preferably in an amount of 0 to 30% by weight, preferably 0.01 to 30% by weight, based on the total weight of the composition. The emulsion can be a single emulsion or multiple emulsions. The color transfer mixture of the present invention can be present in any one or more of these phases.

[0486] Depending on the intended use, the composition with the color-enhancing / enhancing structure described above may further comprise at least one film-forming polymer, particularly for mascara, eyeliner, or lacquer-type hair compositions. The polymer may be dissolved or dispersed in a cosmetically acceptable medium, possibly combined with at least one coalescing agent and / or at least one plasticizer. The composition with the color-enhancing / enhancing structure described above according to the present invention may also comprise a fatty phase, particularly comprising at least one liquid fat and / or at least one fat that is solid at ambient temperature and atmospheric pressure. The liquid fat, often referred to as oil, may constitute 0 to 90% by weight, preferably 0.01 to 85% by weight, based on the total weight of the fatty phase. The solid or pasty fat may be selected, in particular, from waxes, gums, and mixtures thereof. The composition may comprise 0 to 50% by weight, preferably 0.01 to 40% by weight, and in particular 0.1 to 30% by weight, of the solid or pasty fat, based on the total weight of the composition.

[0487] The composition according to the present invention with the above-described color-enhancing / increasing structure can further comprise from 0 to 30%, preferably from 0.01 to 35% by weight, of other particles, based on the total weight of the composition. These particles can in particular be pigments, pearlescent pigments or fillers other than the color mixture of the present invention. The presence of these other particles in particular makes it possible to render the composition opaque.

[0488] Compositions with the above color enhancing / boosting structures according to the present invention may also contain ingredients conventionally present in such compositions, such as preservatives, antioxidants, thickeners, fragrances, moisturizers, sun filters, essential oils, plant extracts and vitamins.

[0489] In one embodiment of the present invention, the color transfer mixture of the present invention can be used in shampoos, conditioners, gels, styling compounds, sprays, and other beauty products. In one embodiment of the present invention, the color transfer mixture of the present invention with the color enhancing / boosting structure described above is added to these hair and beauty products, for example, to increase hair shine. Hair shine is a property of the finish and top surface of the hair. Standard hair treatments "repair," or fill in, torn surfaces in the hair caused by aging, excessive washing, etc. In this embodiment of the present invention, the color converter in the hair treatment also fills in the destroyed surface. The effect is to fill and smooth the surface, resulting in a hair surface that reflects more visible light and scatters less diffusely.

[0490] The color transfer mixtures of the present invention with the above color enhancing / boosting structures can include (in addition to the upconverters and downconverters described herein) many other emulsions and conditioning agents such as those described in U.S. Patent Application No. 2005 / 0136258, U.S. Patent Application No. 2005 / 0265935, U.S. Patent Application No. 2006 / 0083762, U.S. Patent Application No. 2006 / 0165621, U.S. Patent Application No. 2007 / 0274938, and U.S. Patent No. 7,608,237, the entire contents of each of which patent documents are incorporated herein by reference.

[0491] Displays: In conventional electronic ink displays, or electrophoretic displays, titanium dioxide particles approximately 1 micrometer in diameter are dispersed in a hydrocarbon oil. A dark dye is added to the oil, along with a surfactant or charging agent that gives the particles an electric charge. This mixture is placed between two parallel conductive plates, typically separated by a gap of 10 to 100 Φm. When a voltage is applied to the two plates, the particles electrophoretically migrate to the plates, which then acquire an opposite charge to the particle's charge. When the particles are on the front (viewing) side of the display, they appear white because the high-refractive index "white" titanium dioxide particles scatter light back to the viewer. When the particles are on the back side of the display, the display appears dark because incident light is absorbed by the colored dye. If the rear electrode is divided into several small picture elements (pixels), an image can be formed by applying appropriate voltages to each area of ​​the display, creating a pattern of reflective and absorptive areas.

[0492] U.S. Patent Application Publication No. 20040257330 (the entire contents of which are incorporated herein by reference) describes details of the formation of conventional electronic ink displays that can be applied to the basic components shown in the displays of the present invention. U.S. Patent Application Publication No. 20...

Claims

1. 1. An energy emitter comprising: at least one energy increasing structure; and an energy converter capable of receiving energy from an energy source and converting the energy to emit therefrom an emitted light of higher or lower energy than the received energy, the energy converter being positioned proximate to the at least one energy-augmenting structure such that the emitted light is emitted at a higher intensity than if the energy converter were remote from the at least one energy-augmenting structure or if the energy-augmenting structure were not present; The energy emitter.

2. The emitter of claim 1 , wherein the at least one energy-enhancing structure comprises a structure in which a locally enhanced electric field exists in a portion of the structure when the structure receives electromagnetic energy.

3. The emitter of claim 2 , wherein the at least one energy-enhancing structure comprises at least one resonator dimensioned to resonate with applied electromagnetic energy.

4. The emitter of claim 3 , wherein the resonator comprises a folded resonator.

5. The emitter of claim 4 , wherein the folded resonator comprises conductors arranged in a fractal pattern.

6. 5. The emitter of claim 4, wherein the folded resonator comprises a 3 / 4 wavelength resonator having opposed ends folded inwardly from a center of the folded resonator with a gap between the opposed ends.

7. The emitter of claim 6 , wherein the locally enhanced electric field is near the opposing ends.

8. 5. The emitter of claim 4, wherein the folded resonator comprises a 3 / 4 wavelength resonator having opposed ends folded outward from a center of the folded resonator with a gap between the opposed ends.

9. The emitter of claim 8 , wherein the locally enhanced electric field is near the opposing ends.

10. The emitter of claim 3 , wherein the resonator comprises a fractal pattern.

11. The emitter of claim 10 , wherein the fractal pattern comprises a three-dimensional fractal pattern.

12. The emitter of claim 3 , wherein the at least one resonator comprises a plurality of resonators.

13. The emitter of claim 12 , wherein the resonator is disposed in a sheet.

14. The emitter of claim 13 , wherein the sheet comprises a sheet for placement in a medium to be processed.

15. The emitter of claim 13 , wherein the sheet comprises a flexible sheet for placement within a medium to be processed.

16. The emitter of claim 13 , wherein the sheet comprises a rigid sheet for placement within a medium to be processed.

17. The emitter of claim 13 , wherein the plurality of resonators comprises an array of the resonators arranged in a sheet.

18. The emitter of claim 12 , wherein the resonators each comprise a free-standing resonator.

19. The emitter of claim 18 , wherein the free-standing resonator is disposed within a medium being treated.

20. 10. The emitter of claim 1 , wherein the at least one energy-enhancing structure comprises a first level metal pattern and a second level metal pattern offset at least one of laterally or axially from the first level metal pattern.

21. 21. The emitter of claim 20, wherein at least one of the metallic patterns includes a first resonator dimensioned to resonate with applied electromagnetic energy.

22. the at least one of the metal patterns includes a folded resonator having opposing electrodes with an electric field directed therebetween; 22. The emitter of claim 21 , wherein the energy converter is positioned between the opposing electrodes or within a fringe electric field of the opposing electrodes.

23. 23. The emitter of claim 22, wherein the opposing electrodes are oriented toward the exterior of the folded resonator and are parallel to each other.

24. 23. The emitter of claim 22, wherein the opposing electrodes are oriented toward the interior of the folded resonator and are parallel to each other.

25. 23. The emitter of claim 22, wherein the folded resonator comprises a 3 / 4λ folded resonator.

26. 21. The emitter of claim 20, wherein said at least one of said metallic patterns comprises a plurality of said folded resonators arranged concentrically and optionally coplanar with one another such that an outer opposing electrode of each folded resonator does not spatially overlap with an outer opposing electrode of another of said plurality of folded resonators.

27. 21. The emitter of claim 20, wherein said at least one of said metallic patterns comprises a plurality of said folded resonators arranged concentrically, optionally coplanar with one another, such that an outer opposing electrode of each folded resonator spatially overlaps with an outer opposing electrode of one or more others of said plurality of folded resonators.

28. 10. The emitter of claim 1, wherein the at least one energy-enhancing structure comprises at least one of Au, Ag, Cu, Al, a transparent metal oxide, or a refractory metal.

29. 10. The emitter of claim 1, further comprising an anti-reflective film disposed on the at least one energy augmentation structure or the energy converter.

30. The emitter of claim 1 , wherein the at least one energy enhancing structure is disposed proximate a down-conversion material that includes the energy converter.

31. The emitter of claim 1 , wherein the at least one energy-enhancing structure is disposed proximate an upconversion material that includes the energy converter.

32. The emitter of claim 1 , wherein the at least one energy-enhancing structure is disposed proximate a phosphorescent material that includes the energy converter.

33. The emitter of claim 1 , wherein the at least one energy-magnifying structure is disposed proximate a piezoelectric device that includes the energy converter.

34. 34. The emitter of claim 33, wherein the piezoelectric device is configured to receive sonic or acoustic energy and emit at least one of ultraviolet or visible light in response to absorbing the sonic or acoustic energy.

35. The emitter of claim 1 , wherein the at least one energy-enhancing structure is disposed proximate a mechanical light-emitting device that includes the energy converter.

36. 36. The emitter of claim 35, wherein the mechanical light emitting device is configured to receive sonic or acoustic energy and emit at least one of ultraviolet or visible light in response to absorbing the sonic or acoustic energy.

37. The emitter of claim 1 , wherein the at least one energy-enhancing structure is disposed within a plasma capsule device that contains the energy converter.

38. 40. The emitter of claim 37, wherein the plasma capsule device is configured to receive radio frequency or microwave energy and emit at least one of ultraviolet or visible light in response to absorption of the radio frequency or microwave energy.

39. 2. The emitter of claim 1, wherein the at least one energy-enhancing structure is disposed proximate an X-ray stimulated phosphor material that includes the energy converter.

40. 40. The emitter of claim 39, wherein the x-ray stimulated phosphor emits one of ultraviolet or visible light in response to absorbing x-rays.

41. 41. The emitter of claim 40, wherein the x-ray stimulated phosphor emits one of the ultraviolet or visible light for a time of at least 1 minute after x-ray stimulation.

42. 41. The emitter of claim 40, wherein the x-ray stimulated phosphor emits one of the ultraviolet or visible light for a time period of at least 10 minutes after x-ray stimulation.

43. 41. The emitter of claim 40, wherein the x-ray stimulated phosphor emits one of the ultraviolet or visible light for a time of at least 60 minutes after x-ray stimulation.

44. 40. The emitter of claim 39, wherein the x-ray stimulated phosphor emits lower energy x-rays in response to absorbing higher energy x-rays.

45. 10. The emitter of claim 1, wherein the energy received from the energy source is one or more selected from acoustic waves, sound waves, radio waves, microwaves, far infrared, near infrared, visible light, UV, x-rays, gamma light, electron beams, and proton beams.

46. The emitter of claim 1 , wherein the energy converter disposed proximate the at least one energy augmentation structure includes a conductive coupling of the energy converter to the at least one energy augmentation structure.

47. 47. The emitter of claim 46, wherein the conductive coupling comprises a physical conductive connection between the energy converter and the at least one energy-magnifying structure.

48. 2. The emitter of claim 1 , wherein the energy converter comprises either or both of: (i) a downconverter that converts ultraviolet or blue light to red, yellow, or green light; or (ii) an upconverter that converts infrared or red light to yellow, green, or blue light.

49. The emitter of claim 1 , wherein the at least one energy-enhancing structure comprises a plurality of energy collectors.

50. 50. The emitter of claim 49, wherein the energy converter is positioned to convert energy scattered internally within the energy collector.

51. 50. The emitter of claim 49, wherein the energy collector comprises a metal core clad with a high K dielectric followed by a cladding of a low K dielectric.

52. 50. The emitter of claim 49, wherein the energy collector comprises a radial collector pattern.

53. The emitter of claim 7 , wherein the energy collector comprises a fractal pattern.

54. 54. The emitter of claim 53, wherein the fractal pattern is embedded within a dielectric material.

55. 10. The emitter of claim 1 , wherein the at least one energy-enhancing structure comprises at least one component of a paint, ink, fabric, thread, a road sign, a highway sign, an automobile, a boat, an airplane, a reflector, a building product, a concrete product, an epoxy product, a jewelry product, a tinted contact lens, a candle product, a rubber product, a plastic product, a tinted surface, a solar cell, a plasma capsule, an x-ray detector, or a sterilizer.

56. 10. The emitter of claim 1, wherein the energy converter comprises at least one component of a paint, ink, fabric, thread, a road sign, a highway sign, an automobile, a boat, an airplane, a reflector, a building product, a concrete product, an epoxy product, a jewelry product, a tinted contact lens, a candle product, a rubber product, a plastic product, a tinted surface, a solar cell, a plasma capsule, an x-ray detector, or a sterilizer.

57. The emitter of claim 1 , wherein the energy converter comprises a tinted reflective surface component.

58. 10. The emitter of claim 1, wherein the energy converter comprises a colored reflective surface component in a pixel for a display.

59. The emitter of claim 1 , wherein the energy converter comprises a component of a white light emitting pixel display element.

60. The emitter of claim 1 , wherein the energy converter comprises a component disposed in retroreflective paint.

61. The emitter of claim 1 , wherein the energy converter comprises an ink component.

62. 10. The emitter of claim 1, wherein the energy converter comprises at least one of a red, blue, and green emitter configured to produce red, blue, and green emissions from an upconversion process.

63. 4. The emitter of claim 3, wherein the energy converter comprises at least one of a red, blue, and green emitter configured to produce red, blue, and green emissions from an upconversion process.

64. 10. The emitter of claim 1, wherein the energy converter comprises at least one of a red, blue, and green emitter configured to produce red, blue, and green emissions from a down-conversion process.

65. 4. The emitter of claim 3, wherein the energy converter comprises at least one of a red, blue, and green emitter configured to produce red, blue, and green emissions from a down-conversion process.

66. 10. The emitter of claim 1, wherein the energy converter comprises at least one of a red, blue, and green emitter configured to produce red, blue, and green emissions from a mixture of up-converters and down-converters.

67. 4. The emitter of claim 3, wherein the energy converter comprises at least one of a red, blue, and green emitter configured to produce red, blue, and green emissions from a mixture of up-converters and down-converters.

68. 10. The emitter of claim 1, wherein the energy converter comprises a mixture of fluorescent emitters including at least one of europium, terbium, cerium, and erbium or combinations thereof.

69. 4. The emitter of claim 3, wherein the energy converter comprises a mixture of fluorescent emitters including at least one of europium, terbium, cerium, and erbium or combinations thereof.

70. The energy converter comprises: a first material configured to emit a first visible color in response to absorption of ultraviolet light; and 10. The emitter of claim 1 , comprising: a second material configured to emit a second visible color in response to absorption of infrared radiation, the second visible color being different from the first visible color.

71. 71. The emitter of claim 70, wherein the energy converter further comprises a third material configured to emit a third visible color in response to absorbing the ultraviolet light, the third visible color being different from the first visible color and the second visible color.

72. 72. The emitter of claim 71 , wherein the first visible color, the second visible color, and the third visible color are primary colors.

73. 71. The emitter of claim 70, wherein the energy converter further comprises a third material configured to emit a third visible color in response to absorption of the infrared radiation, the third visible color being different from the first visible color and the second visible color.

74. The energy converter comprises: a first material configured to emit a first visible color in response to absorption of ultraviolet light; and 10. The emitter of claim 1 , comprising: a second material configured to emit a second visible color in response to absorption of infrared radiation, the second visible color being substantially the same color as the first visible color.

75. 75. The emitter of claim 74, wherein the energy converter further comprises a third material configured to emit a third visible color in response to absorbing the ultraviolet light, the third visible color being different from the first visible color and the second visible color.

76. 75. The emitter of claim 74, wherein the energy converter further comprises a third material configured to emit a third visible color in response to absorption of the infrared radiation, the third visible color being different from the first visible color and the second visible color.

77. 77. The emitter of claim 76, wherein the first visible color, the second visible color, and the third visible color are at least two of primary colors.

78. The emitter of claim 3 , wherein the energy converter comprises a tinted reflective surface component.

79. 4. The emitter of claim 3, wherein the energy converter comprises a colored reflective surface component within a pixel for a display.

80. The emitter of claim 3 , wherein the energy converter comprises a component of a white light emitting pixel display element.

81. The emitter of claim 3 , wherein the energy converter comprises a component disposed in retroreflective paint.

82. The emitter of claim 3 , wherein the energy converter comprises an ink component.

83. 4. The emitter of claim 3, wherein the energy converter comprises at least one of a red, blue, and green emitter configured to produce red, blue, and green emissions from an upconversion process.

84. 21. The emitter of claim 20, wherein the energy converter comprises at least one of a red, blue, and green emitter configured to produce red, blue, and green emissions from an upconversion process.

85. 4. The emitter of claim 3, wherein the energy converter comprises at least one of a red, blue, and green emitter configured to produce red, blue, and green emissions from a down-conversion process.

86. 21. The emitter of claim 20, wherein the energy converter comprises at least one of a red, blue, and green emitter configured to produce red, blue, and green emissions from a down-conversion process.

87. 4. The emitter of claim 3, wherein the energy converter comprises at least one of a red, blue, and green emitter configured to produce red, blue, and green emissions from a mixture of up-converters and down-converters.

88. 21. The emitter of claim 20, wherein the energy converter comprises at least one of a red, blue, and green emitter configured to produce red, blue, and green emissions from a mixture of up-converters and down-converters.

89. 4. The emitter of claim 3, wherein the energy converter comprises a mixture of fluorescent emitters including at least one of europium, terbium, cerium, and erbium or combinations thereof.

90. 21. The emitter of claim 20, wherein the energy converter comprises a mixture of fluorescent emitters including at least one of europium, terbium, cerium, and erbium or combinations thereof.

91. The energy converter comprises: a first material configured to emit a first visible color in response to absorption of ultraviolet light; and 4. The emitter of claim 3 comprising a second material configured to emit a second visible color in response to absorption of infrared radiation, the second visible color being different from the first visible color.

92. 92. The emitter of claim 91 , wherein the energy converter further comprises a third material configured to emit a third visible color in response to absorbing the ultraviolet light, the third visible color being different from the first visible color and the second visible color.

93. 93. The emitter of claim 92, wherein the first visible color, the second visible color, and the third visible color are primary colors.

94. 92. The emitter of claim 91 , wherein the energy converter further comprises a third material configured to emit a third visible color in response to absorption of the infrared radiation, the third visible color being different from the first visible color and the second visible color.

95. The energy converter comprises: a first material configured to emit a first visible color in response to absorption of ultraviolet light; and 4. The emitter of claim 3, a second material configured to emit a second visible color in response to absorption of infrared radiation, the second visible color being substantially the same color as the first visible color.

96. 96. The emitter of claim 95, wherein the energy converter further comprises a third material configured to emit a third visible color in response to absorbing the ultraviolet light, the third visible color being different from the first visible color and the second visible color.

97. 96. The emitter of claim 95, wherein the energy converter further comprises a third material configured to emit a third visible color in response to absorption of the infrared radiation, the third visible color being different from the first visible color and the second visible color.

98. 98. The emitter of claim 97, wherein the first visible color, the second visible color, and the third visible color are at least two of primary colors.

99. 10. The emitter of claim 1 , wherein the at least one energy-enhancing structure comprises a metallic conductor comprising at least one of Au, Ag, Cu, Ni, Pt, Pd, Co, Ru, Rh, Al, Ga, or combinations or alloys or layers thereof.

100. The energy converter is Y 2 O 3 , Y 2 O 2 S, NaYF 4 , NaYbF 4 ,YAG,YAP,Nd 2 O 3 , LaF 3 , LaCl 3 , La 2 O 3 , TiO 2 , LuPO 4 , Y.V.O. 4 , YbF 3 , Y.F. 3 , Na-doped YbF 3 or SiO 2 10. The emitter of claim 1 comprising at least one of:

101. 101. The emitter of claim 100, wherein the energy converter further comprises a dopant comprising at least one of Er, Eu, Yb, Tm, Nd, Tb, Ce, Y, U, Pr, La, Gd and other rare earth species, or combinations thereof.

102. The emitter of claim 101, wherein the dopant is included in a concentration of 0.01% to 50% molar concentration.

103. The energy converter is Y 2 O 3 ;ZnS;ZnSe;MgS;CaS;Mn,ErZnSe;Mn,ErMgS;Mn,ErCaS;Mn,ErZnS;Mn,YbZnSe;Mn,YbMgS;Mn,YbCaS;Mn,YbZnS:Tb 3+ , Er 3+ ZnS:Tb 3+ ; Y 2 O 3 : Tb 3+ ; Y 2 O 3 : Tb 3+ , Er3 + ZnS:Mn 2+ ;ZnS:Mn,Er 3+ 10. The emitter of claim 1 comprising a downconverter comprising at least one of:

104. The energy converter is Y 2 O 3 , Y 2 O 2 S, NaYF 4 , NaYbF 4 , YAG, YAP, Nd 2 O 3 , LaF 3 , LaCl 3 , La 2 O 3 , TiO 2 , LuPO 4 , Y.V.O. 4 , YbF 3 , Y.F. 3 , Na-doped YbF 3 or SiO 2 13. The emitter of claim 1 , further comprising an upconverter comprising at least one of:

105. The energy converter is Tm 3+ Doped fluorozirconate glass, LuPO 4 : Yb 3+ , Tm 3+ , and YbPO 4 :Er 3+ Nanocrystals, tellurium and germanium oxides, at least one of Tm, Yb, Ho, Er, or Pr doped tellurium and germanium oxides, Yb 3+ Doped BaZrO 3 , Nd 3+ :Cs 2 NaGdCl 6 , Nd 3+ , Yb 3+ :Cs 2 NaGdCl 6 , Nd 3+ and Ho 3+ Co-doped base ZrF 4 Fluoride glass, Tm 3+ / Yb 3+ -co-doped TeO 2 -Ga 2 O 3 -R 2 O (R = Li, Na, K) glasses and metal-to-ligand charge transfer (MLCT) transition materials, and [Ru(dmb) 3 ] 2+ 10. The emitter of claim 1 including an upconverter including at least one MLCT transition material including (dmb=4,4'-dimethyl-2,2'-bipyridine).

106. Pigments, and 2. The emitter of claim 1 . Including, paint.

107. Dyes, and 2. The emitter of claim 1 . Including, ink.

108. At least one of a color filter or a color reflective surface; and 13. An optical display comprising an emitter according to claim 1 included in the color filter or as part of the color reflective surface.

109. 1. A protective coating for mitigating UV light damage to an object exposed to UV light radiation, comprising: A mixture of light scattering particles and the emitter of claim 1, The mixture, when exposed to UV light, converting a first portion of the UV light into visible light; Emitting a portion of the visible light from the mixture; the protective coating configured to reflect a second portion of the UV light away from the mixture such that the second portion of the UV light is not absorbed by the object.

110. 1. A light emitting composition comprising: a first color emitter configured to emit visible light in a first target color when exposed to an energy source with energy above or below the visible light spectrum; a second color emitter configured to emit visible light at a second target color when exposed to the energy source; and 2. The emitter of claim 1 . The light emitting composition comprising:

111. A color emitter, a first color emitter configured to emit visible light at a first target color in response to absorption of energy over a first band of wavelengths when exposed to an energy source; a second color emitter configured to emit visible light at a second target color in response to absorption of energy over a second band of wavelengths when exposed to the energy source; and The color emitter comprises an emitter according to claim 1 . Including, cosmetics.

112. 112. The product of claim 111, wherein the cosmetic product is a skin cream.

113. 112. The product of claim 111, wherein the cosmetic product is a mascara.

114. 112. The product of claim 111, wherein the cosmetic product is at least one member selected from the group consisting of shampoo, hair conditioner, hair gel, hair styling compound, hair spray, and hair cream.

115. 112. The product of claim 111, wherein the cosmetic product is a lip balm.

116. 112. The product of claim 111, wherein the cosmetic product is a blush.

117. 1. A method for enhancing visible light emission from a surface, comprising: Providing at least one emitter according to claim 1 on said surface; exposing the surface and the at least one color-enhancing structure to energy applied from an energy source; and converting a portion of the applied energy into visible light, thereby emitting the visible light in at least one target color; The method comprising:

118. 1. A method for enhancing visible light emission from a coating, comprising: Providing at least one of the structures of claim 1 in or near the surface of the paint; exposing the surface and the at least one structure to energy applied from an energy source; and emitting said visible light in at least one target color by converting a portion of said applied energy into said visible light; The method comprising:

119. 1. A method for enhancing visible light emission from an ink, comprising: Providing the ink with at least one of the structures of claim 1; exposing the ink and the at least one color enhancing structure to energy applied from an energy source; and emitting said visible light in at least one target color by converting a portion of said applied energy into said visible light; The method comprising:

120. 1. A method for enhancing visible light emission from a display, comprising: Providing a color filter or color reflecting surface of the display with at least one of the structures of claim 1; exposing the color filter or color reflective surface and the at least one color enhancement structure to applied energy from an energy source; and emitting said visible light in at least one target color by converting a portion of said applied energy into said visible light; The method comprising:

121. 1. An energy or color enhancement device comprising: an energy collector including at least one energy augmentation structure; and an energy converter capable of receiving applied electromagnetic energy, converting said applied electromagnetic energy and emitting therefrom a wavelength of emitted energy shifted to a wavelength / energy from said applied electromagnetic energy, said energy converter being disposed proximate to said energy-magnifying structure; The energy or color enhancement device, wherein the energy augmentation structure is configured to provide an electric field between opposing elements of the structure.

122. 1. An energy or color enhancement device comprising: an energy collector including at least one energy augmentation structure; and an energy converter capable of receiving applied electromagnetic energy, converting said applied electromagnetic energy and emitting therefrom a wavelength of emitted energy shifted to a wavelength / energy from said applied electromagnetic energy, said energy converter being disposed proximate to said energy-magnifying structure; The energy or color enhancement device, wherein the energy collector collects energy from a branch antenna.

123. 123. The device of claim 122, wherein each array element of the branched antenna comprises a metallic core and a dielectric cladding.

124. 1. An energy or color enhancement device comprising: an energy collector, optionally including at least one energy augmentation structure; and an energy converter including a mechano-luminescent emitter capable of receiving at least one of acoustic, vibrational, and ultrasonic energy and converting said received energy and emitting therefrom a wavelength of light from the energy converter; The energy or color enhancement device.

125. 125. The device of claim 124, wherein the mechanoluminescent emitter comprises a piezoelectric material connected to an electroluminescent material thereby forming a composite emitter.

126. An energy-enhancing structure capable of capturing one or more wavelengths of electromagnetic energy and enhancing said one or more wavelengths of electromagnetic energy in at least one characteristic.

127. 127. The energy-enhancing emitter of claim 126, wherein the energy-enhancing structure is at least one non-plasmonic member selected from the group consisting of a resonator, a fractal antenna, an electrical grid pattern, an antenna, a cavity, an etalon, a nanoparticle, a microparticle, a nanostructure, and a microstructure.

128. 127. The energy augmentation structure of claim 126 comprising a folded resonator having opposing electrodes with an electric field directed therebetween.

129. 129. The energy augmentation structure of claim 128, wherein the opposing electrodes are oriented toward the exterior of the folded resonator and are parallel to each other.

130. 129. The energy augmentation structure of claim 128, wherein the opposing electrodes are oriented toward an interior of the folded resonator and are parallel to each other.

131. 129. The energy augmentation structure of claim 128, wherein the folded resonator comprises a 3 / 4λ folded resonator.

132. 129. The energy augmentation structure of claim 128, wherein the folded resonator is a plurality of the folded resonators arranged concentrically, optionally coplanar with one another, such that an outer opposing electrode of each folded resonator does not spatially overlap with an outer opposing electrode of another of the plurality of folded resonators.

133. 129. The energy augmentation structure of claim 128, wherein the folded resonator is a plurality of the folded resonators arranged concentrically, optionally coplanar with one another, such that an outer opposing electrode of each folded resonator spatially overlaps with one or more other outer opposing electrodes of the plurality of folded resonators.

134. An energy collector comprising at least one energy augmentation structure and at least one energy converter capable of receiving applied electromagnetic energy, converting the applied electromagnetic energy and emitting emitted electromagnetic energy therefrom that is shifted in wavelength or energy from the applied electromagnetic energy, the energy converter being positioned near the at least one energy augmentation structure such that the emitted electromagnetic energy is emitted with at least one enhanced characteristic compared to when the energy converter is distant from the at least one energy augmentation structure.

135. 135. The energy collector of claim 134, wherein the at least one energy converter is at least one member selected from the group consisting of phosphorescent materials, luminophores, electroluminescent particles, upconverters, downconverters, and scintillators.

136. 135. The energy collector of claim 134, wherein the energy enhancing structure is at least one non-plasmonic member selected from the group consisting of a resonator, a fractal antenna, an electrical grid pattern, an antenna, a cavity, an etalon, a nanoparticle, a microparticle, a nanostructure, and a microstructure.

137. 135. The energy collector of claim 134, wherein disposing the energy converter proximate the at least one energy augmentation structure comprises conductively coupling the at least one energy converter to the at least one energy augmentation structure.

138. 138. The energy collector of claim 137, wherein conductively coupling comprises having the at least one energy converter proximate to the at least one energy augmentation structure, physically positioned within the at least one energy augmentation structure, or positioned within a generated electric field of the at least one energy augmentation structure.

139. 138. The energy collector of claim 137, wherein conductively coupling comprises a physical conductive connection between the at least one energy converter and the at least one energy augmentation structure.

140. 135. The energy collector of claim 134, wherein the applied electromagnetic energy is selected from radio waves, microwaves, far infrared, near infrared, visible light, UV, x-rays, gamma rays, electron beam, and proton beam.

141. 135. The energy collector of claim 134, wherein the at least one energy-enhancing structure comprises a first resonator dimensioned to resonate with the applied electromagnetic energy, the first resonator optionally comprising a fractal pattern.

142. 135. The energy collector of claim 134, wherein the energy-augmenting structure comprises a folded resonator having opposing electrodes with an electric field directed therebetween.

143. 141. The energy collector of claim 140, wherein the opposing electrodes are directed toward the outside of the folded resonator and are parallel to each other.

144. 141. The energy collector of claim 140, wherein the opposing electrodes are oriented toward the interior of the folded resonator and are parallel to each other.

145. 143. The energy collector of claim 142, wherein the folded resonator comprises a 3 / 4λ folded resonator.

146. 143. The energy collector of claim 142, wherein the folded resonator is a plurality of folded resonators arranged concentrically, optionally coplanar with one another, such that an outer opposing electrode of each folded resonator does not spatially overlap with an outer opposing electrode of another of the plurality of folded resonators.

147. 143. The energy collector of claim 142, wherein the folded resonator is a plurality of folded resonators arranged concentrically, optionally coplanar with one another, such that an outer opposing electrode of each folded resonator spatially overlaps with an outer opposing electrode or electrodes of one or more others of the plurality of folded resonators.

Citation Information

Patent Citations

  • Surface emission semiconductor laser having interference filter

    JP2005217428A

  • Resonant cavity color conversion el device and organic el display device using the same

    JP2009205928A

  • Non-invasive energy upconversion method and system for insitu photobiomodulation

    JP2012524795A

  • Enhanced Emission from Plasmonic Coupled Emitters for Solid-State Lighting