Method for graphene-based conductive adhesive and application thereof

A conductive adhesive using graphene and silver-based additives addresses the challenges of conductivity and durability in flexible electronic devices, enhancing bonding and signal percolation for improved device performance.

JP2024167255AInactive Publication Date: 2024-12-03RGT UNIV OF CALIFORNIA +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024137508
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-06-05
Filing Date
2024-08-19
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Current techniques for gluing electrical components in flexible electronic devices face challenges in achieving effective conductivity and durability, particularly in device packaging and assembly, where existing methods like sewing, mechanical fastening, and thermal bonding are inadequate.

Method used

A conductive adhesive comprising graphene nanoparticles, graphene nanosheets, graphene microparticles, and silver-based additives such as silver nanowires or silver nanoparticles, with a percolation threshold between 5% to 25%, providing electrical conductivity and adhesion.

Benefits of technology

The conductive adhesive enhances the electrical conductivity and durability of flexible electronic devices by ensuring effective bonding and percolation of electrical signals, improving device performance and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167255000001_ABST
    Figure 2024167255000001_ABST
Patent Text Reader

Abstract

To provide a method for forming a silver nano-wire which is of a conductive additive for a conductive adhesive indicative of excellent electric conductivity, thermal properties and endurance, low thermosetting temperature and mechanical flexibility and allowed to reduce effects upon an environment.SOLUTION: A method for forming a silver nano-wire includes: (a) heating up solvent; (b) forming a first solution by adding solutions of catalyst and polymer to the solvent; (c) forming a second solution by injecting a silver-based solution into the first solution; (d) centrifugally separating the second solution; and (e) extracting a silver nano-wire by cleansing the second solution with a cleansing solution.SELECTED DRAWING: Figure 50A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Application No. 62 / 593,506, filed December 1, 2017, and U.S. Provisional Application No. 62 / 680,615, filed June 5, 2018, which are incorporated herein by reference. [Background technology]

[0002] Device packaging and assembly play an important role in the modern electronics industry. Electronic components often include a printed circuit board and multiple electronic components, such as chips, energy sources, and memory devices, mounted on the circuit board. Some such electronic devices are designed to be flexible to improve durability and ease of use.

[0003] Current techniques for attaching electrical components include sewing, mechanical fastening, and thermal bonding. Summary of the Invention

[0004] Provided herein is a conductive adhesive comprising a conductive additive comprising at least one of a carbon-based additive comprising two or more of graphene nanoparticles, graphene nanosheets, and graphene microparticles, and a silver-based additive comprising silver nanowires, silver nanoparticles, or both, wherein the silver-based additive has a diameter of less than 0.5 μm, and an adhesive.

[0005] In some embodiments, the conductive adhesive has a percolation threshold of about 5% to about 25% when dry. In some embodiments, the conductive adhesive has a percolation threshold of about 5% to about 6%, about 5% to about 7%, about 5% to about 8%, about 5% to about 9%, about 5% to about 10%, about 5% to about 11%, about 5% to about 12%, about 5% to about 15%, about 5% to about 18%, about 5% to about 21%, about 5% to about 25%, about 6% to about 7%, about 6% to about 8%, about 6% to about 9%, about 6% to about 10%, about 6% to about 11%, About 6% to about 12%, about 6% to about 15%, about 6% to about 18%, about 6% to about 21%, about 6% to about 25%, about 7% to about 8%, about 7% to about 9%, about 7% to about 10%, about 7% to about 11%, about 7% to about 12%, about 7% to about 15%, about 7% to about 18%, about 7% to about 21%, about 7% to about 25%, about 8% to about 9%, about 8% to about 10%, about 8% to about 11%, about 8% to about 12%, about 8% ~ about 15%, about 8% to about 18%, about 8% to about 21%, about 8% to about 25%, about 9% to about 10%, about 9% to about 11%, about 9% to about 12%, about 9% to about 15%, about 9% to about 18%, about 9% to about 21%, about 9% to about 25%, about 10% to about 11%, about 10% to about 12%, about 10% to about 15%, about 10% to about 18%, about 10% to about 21%, about 10% to about 25%, about 11% to about The conductive adhesive has a percolation threshold of about 12%, about 11% to about 15%, about 11% to about 18%, about 11% to about 21%, about 11% to about 25%, about 12% to about 15%, about 12% to about 18%, about 12% to about 21%, about 12% to about 25%, about 15% to about 18%, about 15% to about 21%, about 15% to about 25%, about 18% to about 21%, about 18% to about 25%, or about 21% to about 25%. In some embodiments, the conductive adhesive has a percolation threshold of about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, about 12%, about 15%, about 18%, about 21%, or about 25% when dry. In some embodiments, the conductive adhesive has a percolation threshold when dry of at least about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, about 12%, about 15%, about 18%, or about 21%. In some embodiments, the conductive adhesive has a percolation threshold when dry of at most about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, about 12%, about 15%, about 18%, about 21%. It has a percolation threshold of 1%, or about 25%.

[0006] The silver-based additive can include silver nanowires, silver nanoparticles, or both. The silver-based additive can include silver nanowires, but not silver nanoparticles. The silver-based additive can include silver nanoparticles, but not silver nanowires. The silver-based additive can include silver nanowires and silver nanoparticles. Alternatively, the silver-based material can include silver nanorods, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or any combination thereof. The silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 25% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 50% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 75% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. The silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm.At least about 25% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. At least about 50% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. At least about 75% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. The silver nanowires can have an average aspect ratio of about 250:1, 300:1, 350:1, 400:1, 450:1, 500:1, 600:1, 700:1, 800:1, 900:1, or 1000:1. The silver nanowires can have an average aspect ratio of at least about 250:1, 300:1, 350:1, 400:1, 450:1, 500:1, 600:1, 700:1, 800:1, 900:1, or 1000:1.

[0007] In some embodiments, the adhesive comprises a hardener and a resin. In some embodiments, at least a portion of the conductive additive is incorporated into the hardener, the resin, or both. In some embodiments, the conductive adhesive further comprises a thinner. In some embodiments, the conductive adhesive further comprises a pigment, a silver metallic pigment, a colorant, a silver metallic colorant, a dye, or any combination thereof.

[0008] In some embodiments, the conductive adhesive has a sheet resistance when dry of about 5 ohms / sq to about 500 ohms / sq. In some embodiments, the conductive adhesive has a sheet resistance when dry of about 5 ohms / sq to about 10 ohms / sq, about 5 ohms / sq to about 20 ohms / sq, about 5 ohms / sq to about 60 ohms / sq, about 5 ohms / sq to about 70 ohms / sq, about 5 ohms / sq to about 80 ohms / sq, about 5 ohms / sq to about 90 ohms / sq, about 5 ohms / sq to about 10 ohms / sq, about 5 ohms / sq to about 20 ohms / sq, about 5 ohms / sq to about 1 ... ohms / sq to about 50 ohms / sq, about 5 ohms / sq to about 100 ohms / sq, about 5 ohms / sq to about 150 ohms / sq, about 5 ohms / sq to about 200 ohms / sq, about 5 ohms / sq to about 250 ohms / sq, about 5 ohms / sq to about 300 ohms / sq, about 5 ohms / sq to about 350 ohms / sq, about 5 ohms / sq to about 400 ohms / sq, about 5 ohms / sq to about 500 ohms / sq, about 10 ohms / sq to about 20 ohms / sq, about 10 ohms / sq to about 50 ohms / sq, about 10 ohms / sq to about 100 ohms / sq, about 10 ohms / sq to about 20 ohms / sq~about 150 ohms / sq, about 10 ohms / sq~about 200 ohms / sq, about 10 ohms / sq~about 250 ohms / sq, about 10 ohms / sq~about 300 ohms / sq, about 10 ohms / sq~about 350 ohms / sq, about 10 ohms / sq~about 400 ohms / sq, about 10 ohms / sq~about 500 ohms / sq, about 20 ohms / sq~about 50 ohms / sq, about 20 ohms / sq~about 100 ohms / sq, about 20 ohms / sq~about 150 ohms / sq, about 20 ohms / sq~about 200 ohms / sq, about 20 ohms / sq~about 250 ohms / sq, about 20 ohms / sq~approx. 300 ohms / sq, approx. 20 ohms / sq~approx. 350 ohms / sq, approx. 20 ohms / sq~approx. 400 ohms / sq, approx. 20 ohms / sq~approx. 500 ohms / sq, approx. 50 ohms / sq~approx. 100 ohms / sq, approx. 50 ohms / sq~approx. 150 ohms / sq, approx. 50 ohms / sq~approx. 200 ohms / sq, approx. 50 ohms / sq~approx. 250 ohms / sq, approx. 50 ohms / sq~approx. 300 ohms / sq, approx. 50 ohms / sq~approx. 350 ohms / sq, approx. 50 ohms / sq~approx. 400 ohms / sq, approx. 50 ohms / sq~approx. 500 ohms / sq, about 100 ohms / sq to about 150 ohms / sq, about 100 ohms / sq to about 200 ohms / sq, about 100 ohms / sq to about 250 ohms / sq, about 100 ohms / sq to about 300 ohms / sq, about 100 ohms / sq to about 350 ohms / sq, about 100 ohms / sq to about 400 ohms / sq, about 100 ohms / sq to about 500 ohms / sq, about 150 ohms / sq to about 200 ohms / sq, about 150 ohms / sq to about 250 ohms / sq, about 150 ohms / sq to about 300 ohms / sq, about 150 ohms / sq to about 350 ohms / sq,Approximately 150 ohms / sq to approximately 400 ohms / sq, approximately 150 ohms / sq to approximately 500 ohms / sq, approximately 200 ohms / sq to approximately 250 ohms / sq, approximately 200 ohms / sq to approximately 300 ohms / sq, approximately 200 ohms / sq to approximately 350 ohms / sq, approximately 200 ohms / sq to approximately 400 ohms / sq, approximately 200 ohms / sq to approximately 500 ohms / sq, approximately 250 ohms / sq to approximately 300 ohms / sq, approximately 250 ohms / sq to approximately 350 ohms / sq In one embodiment, the sheet resistance is about 250 ohms / sq to about 400 ohms / sq, about 250 ohms / sq to about 500 ohms / sq, about 300 ohms / sq to about 350 ohms / sq, about 300 ohms / sq to about 400 ohms / sq, about 300 ohms / sq to about 500 ohms / sq, about 350 ohms / sq to about 400 ohms / sq, about 350 ohms / sq to about 500 ohms / sq, or about 400 ohms / sq to about 500 ohms / sq. In some embodiments, the conductive adhesive has a sheet resistance when dry of about 5 ohms / sq, about 10 ohms / sq, about 20 ohms / sq, about 50 ohms / sq, about 100 ohms / sq, about 150 ohms / sq, about 200 ohms / sq, about 250 ohms / sq, about 300 ohms / sq, about 350 ohms / sq, about 400 ohms / sq, or about 500 ohms / sq. In some embodiments, the conductive adhesive has a sheet resistance when dry of at least about 5 ohms / sq, about 10 ohms / sq, about 20 ohms / sq, about 50 ohms / sq, about 100 ohms / sq, about 150 ohms / sq, about 200 ohms / sq, about 250 ohms / sq, about 300 ohms / sq, about 350 ohms / sq, about 400 ohms / sq, or about 500 ohms / sq. In some embodiments, the conductive adhesive has a sheet resistance when dry of at most about 5 ohms / sq, about 10 ohms / sq, about 20 ohms / sq, about 50 ohms / sq, about 100 ohms / sq, about 150 ohms / sq, about 200 ohms / sq, about 250 ohms / sq, about 300 ohms / sq, about 350 ohms / sq, about 400 ohms / sq, or about 500 ohms / sq.

[0009] In some embodiments, the conductive adhesive has a sheet resistance when dry of about 0.3 ohms / sq / mil to about 2 ohms / sq / mil. , when dry, about 0.3 ohms / sq / mil to about 0.4 ohms / sq / mil, about 0.3 ohms / sq / mil to about 0.6 ohms / sq / mil, about 0.3 ohms / sq / mil to about 0.8 ohms / sq / mil, about 0.3 ohms / sq / mil to about 1 ohm / sq / mil, about 0.3 ohms / sq / mil to about 1.2 ohms / sq / mil, about 0.3 ohms / sq / mil to about 1.4 ohms / sq / mil, about 0.3 ohms / sq / mil to about 1.6 ohms / sq / mil, about 0.3 ohms / sq / mil to about 1.8 ohms / sq / mil, about 0.3 ohms / sq / mil to about 2 ohms / sq / mil sq / mil, about 0.4 ohms / sq / mil to about 0.6 ohms / sq / mil, about 0.4 ohms / sq / mil to about 0.8 ohms / sq / mil, about 0.4 ohms / sq / mil to about 1 ohm / sq / mil, about 0.4 ohms / sq / mil to about 1.2 ohms / sq / mil, about 0.4 ohms / sq / mil to about 1.4 ohms / sq / mil, about 0.4 ohms / sq / mil to about 1.6 ohms / sq / mil, about 0.4 ohms / sq / mil to about 1.8 ohms / sq / mil, about 0.4 ohms / sq / mil to about 2 ohms / sq / mil, about 0.6 ohms / sq / mil to about 0.8 ohms / sq / mil, about 0.6 ohms / sq / mil to about 1 ohm / sq / mil, about 0.6 ohms / sq / mil to about 1.2 ohms / sq / mil, about 0.6 ohms / sq / mil to about 1.4 ohms / sq / mil, about 0.6 ohms / sq / mil to about 1.6 ohms / sq / mil, about 0.6 ohms / sq / mil to about 1.8 ohms / sq / mil, about 0.6 ohms / sq / mil to about 2 ohms / sq / mil, about 0.8 ohms / sq / mil to about 1 ohm / sq / mil, about 0.8 ohms / sq / mil to about 1.2 ohms / sq / mil, about 0.8 ohms / sq / mil to about 1.4 ohms / sq / mil sq / mil, about 0.8 ohms / sq / mil to about 1.6 ohms / sq / mil, about 0.8 ohms / sq / mil to about 1.8 ohms / sq / mil, about 0.8 ohms / sq / mil to about 2 ohms / sq / mil, about 1 ohm / sq / mil to about 1.2 ohms / sq / mil, about 1 ohm / sq / mil to about 1.4 ohms / sq / mil, about 1 ohm / sq / mil to about 1.6 ohms / sq / mil, about 1 ohm / sq / mil to about 1.8 ohms / sq / mil, about 1 ohm / sq / mil to about 2 ohms / sq / mil, about 1.2 ohms / sq / mil to about 1.4 ohms / sq / mil, about 1.having a sheet resistance of about 2 ohms / sq / mil to about 1.6 ohms / sq / mil, about 1.2 ohms / sq / mil to about 1.8 ohms / sq / mil, about 1.2 ohms / sq / mil to about 2 ohms / sq / mil, about 1.4 ohms / sq / mil to about 1.6 ohms / sq / mil, about 1.4 ohms / sq / mil to about 1.8 ohms / sq / mil, about 1.4 ohms / sq / mil to about 2 ohms / sq / mil, about 1.6 ohms / sq / mil to about 1.8 ohms / sq / mil, about 1.6 ohms / sq / mil to about 2 ohms / sq / mil, or about 1.8 ohms / sq / mil to about 2 ohms / sq / mil. In some embodiments, the conductive adhesive has a sheet resistance when dry of about 0.3 ohms / sq / mil, about 0.4 ohms / sq / mil, about 0.6 ohms / sq / mil, about 0.8 ohms / sq / mil, about 1 ohm / sq / mil, about 1.2 ohms / sq / mil, about 1.4 ohms / sq / mil, about 1.6 ohms / sq / mil, about 1.8 ohms / sq / mil, or about 2 ohms / sq / mil. In some embodiments, the conductive adhesive has a sheet resistance when dry of at least about 0.3 ohms / sq / mil, about 0.4 ohms / sq / mil, about 0.6 ohms / sq / mil, about 0.8 ohms / sq / mil, about 1 ohm / sq / mil, about 1.2 ohms / sq / mil, about 1.4 ohms / sq / mil, about 1.6 ohms / sq / mil, about 1.8 ohms / sq / mil, or about 2 ohms / sq / mil. In some embodiments, the conductive adhesive has a sheet resistance when dry of at most about 0.3 ohms / sq / mil, about 0.4 ohms / sq / mil, about 0.6 ohms / sq / mil, about 0.8 ohms / sq / mil, about 1 ohm / sq / mil, about 1.2 ohms / sq / mil, about 1.4 ohms / sq / mil, about 1.6 ohms / sq / mil, about 1.8 ohms / sq / mil, or about 2 ohms / sq / mil.

[0010] In some embodiments, the conductive adhesive has a conductivity of about 0.15 S / m to about 60 S / m when dry. In some embodiments, the conductive adhesive has a conductivity of about 0.15 S / m to about 0.3 S / m, about 0.15 S / m to about 0.5 S / m, about 0.15 S / m to about 1 S / m, about 0.15 S / m to about 2 S / m, about 0.15 S / m to about 5 S / m, about 0.15 S / m ~10S / m, 0.15S / m~20S / m, 0.15S / m~30S / m, 0.15S / m~40S / m, 0.15S / m~50S / m, 0.15S / m~60S / m, 0.3S / m~0.5S / m, 0. 3S / m~about 1S / m, about 0.3S / m~about 2S / m, about 0.3S / m~about 5S / m, about 0.3S / m~about 10S / m, about 0.3S / m~about 20S / m, about 0.3S / m~about 30S / m, about 0.3S / m~about 40S / m, about 0.3S / m~ Approx. 50S / m, approx. 0.3S / m ~ approx. 60S / m, approx. 0.5S / m ~ approx. 1S / m, approx. 0.5S / m ~ approx. 2S / m, approx. 0.5S / m ~ approx. 5S / m, approx. 0.5S / m ~ approx. 10S / m, approx. 0.5S / m ~ approx. 20S / m, approx. 0.5S / m ~ approx. 30S / m m, about 0.5S / m to about 40S / m, about 0.5S / m to about 50S / m, about 0.5S / m to about 60S / m, about 1S / m to about 2S / m, about 1S / m to about 5S / m, about 1S / m to about 10S / m, about 1S / m to about 20S / m, about 1S / m to about 30S / m m, about 1S / m to about 40S / m, about 1S / m to about 50S / m, about 1S / m to about 60S / m, about 2S / m to about 5S / m, about 2S / m to about 10S / m, about 2S / m to about 20S / m, about 2S / m to about 30S / m, about 2S / m to about 40S / m, about 2 S / m~about 50S / m, about 2S / m~about 60S / m, about 5S / m~about 10S / m, about 5S / m~about 20S / m, about 5S / m~about 30S / m, about 5S / m~about 40S / m, about 5S / m~about 50S / m, about 5S / m~about 60S / m, about 10S / m about 20 S / m, about 10 S / m to about 30 S / m, about 10 S / m to about 40 S / m, about 10 S / m to about 50 S / m, about 10 S / m to about 60 S / m, about 20 S / m to about 30 S / m, about 20 S / m to about 40 S / m, about 20 S / m to about 50 S / m, about 20 S / m to about 60 S / m, about 30 S / m to about 40 S / m, about 30 S / m to about 50 S / m, about 30 S / m to about 60 S / m, about 40 S / m to about 50 S / m, about 40 S / m to about 60 S / m, or about 50 S / m to about 60 S / m. In some embodiments, the conductive adhesive has a conductivity of about 0.15 S / m, about 0.3 S / m, about 0.5 S / m, about 1 S / m, about 2 S / m, about 5 S / m, about 10 S / m, about 20 S / m, about 30 S / m, about 40 S / m, about 50 S / m, or about 60 S / m when dry.In some embodiments, the conductive adhesive has a conductivity of at least about 0.15 S / m, about 0.3 S / m, about 0.5 S / m, about 1 S / m, about 2 S / m, about 5 S / m, about 10 S / m, about 20 S / m, about 30 S / m, about 40 S / m, or about 50 S / m when dry. In some embodiments, the conductive adhesive has a conductivity of at most about 0.3 S / m, about 0.5 S / m, about 1 S / m, about 2 S / m, about 5 S / m, about 10 S / m, about 20 S / m, about 30 S / m, about 40 S / m, about 50 S / m, or about 60 S / m when dry.

[0011] Another aspect provided herein is a conductive ink comprising a conductive additive comprising at least one of a carbon-based additive comprising two or more of graphene nanoparticles, graphene nanosheets, and graphene microparticles, and a silver-based additive comprising silver nanowires, silver nanoparticles, or both, wherein the silver-based additive has a diameter of less than 0.5 μm, and a solvent.

[0012] In some embodiments, the conductive ink has a percolation threshold of about 5% to about 25% when dry. In some embodiments, the conductive ink has a percolation threshold of about 5% to about 6%, about 5% to about 7%, about 5% to about 8%, about 5% to about 9%, about 5% to about 10%, about 5% to about 11%, about 5% to about 12%, about 5% to about 15%, about 5% to about 18%, about 5% to about 21%, about 5% to about 25%, about 6% to about 7%, about 6% to about 8%, about 6% to about 9%, about 6% to about 10%, about 6% to about 11%, about 6% to about 12%, about 6% to about 15%, about 6% to about 18%, about 6% to about 21%, about 6% to about 25%, about 7% to about 8%, about 7% to about 9%, about 7% to about 10%, about 7% to about 11%, about 7% to about 12%, about 7% to about 15%, about 7% to about 18%, about 7% to about 21%, about 7% to about 25%, about 8% to about 9%, about 8% to about 10%, about 8% to about 11%, about 8% to about 12%, about 8% to about 15%, about 8% to about 18%, about 8% to about 21%, about 8% to about 25%, about 9% to about 10%, about 9% to about 11%, about 9% to about 12%, about 9% to about 15%, about 9% to about 18%, about 9% to about 21%, about 9% to about 25%, about 10% to about 11%, about 1 The percolation threshold is from 0% to about 12%, from about 10% to about 15%, from about 10% to about 18%, from about 10% to about 21%, from about 10% to about 25%, from about 11% to about 12%, from about 11% to about 15%, from about 11% to about 18%, from about 11% to about 21%, from about 11% to about 25%, from about 12% to about 15%, from about 12% to about 18%, from about 12% to about 21%, from about 12% to about 25%, from about 15% to about 18%, from about 15% to about 21%, from about 15% to about 25%, from about 18% to about 21%, from about 18% to about 25%, or from about 21% to about 25%. In some embodiments, the conductive ink has a percolation threshold of about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, about 12%, about 15%, about 18%, about 21%, or about 25% when dry. In some embodiments, the conductive ink has a percolation threshold of at least about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, about 12%, about 15%, about 18%, or about 21% when dry. In some embodiments, the conductive ink has a percolation threshold of at most about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, about 12%, about 15%, about 18%, about 21%, or about 25% when dry.

[0013] The silver-based additive can include silver nanowires, silver nanoparticles, or both. The silver-based additive can include silver nanowires, but not silver nanoparticles. The silver-based additive can include silver nanoparticles, but not silver nanowires. The silver-based additive can include silver nanowires and silver nanoparticles. Alternatively, the silver-based material can include silver nanorods, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or any combination thereof. The silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 25% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 50% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 75% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. The silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm.At least about 25% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. At least about 50% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. At least about 75% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. The silver nanowires can have an average aspect ratio of about 250:1, 300:1, 350:1, 400:1, 450:1, 500:1, 600:1, 700:1, 800:1, 900:1, or 1000:1. The silver nanowires can have an average aspect ratio of at least about 250:1, 300:1, 350:1, 400:1, 450:1, 500:. The optical fiber may have an average aspect ratio of 1, 600:1, 700:1, 800:1, 900:1, or 1000:1.

[0014] In some embodiments, the percentage by weight of the conductive additive in the conductive ink is about 0.25% to about 20%. In some embodiments, the percentage by weight of the conductive additive in the conductive ink is about 0.25% to about 0.5%, about 0.25% to about 0.75%, about 0.25% to about 1%, about 0.25% to about 2%, about 0.25% to about 4%, about 0.25% to about 6%, about 0.25% to about 8%, about 0.25% to about 10%, about 0.25% to about 15%, about 0.25% ~ about 20%, about 0.5% to about 0.75%, about 0.5% to about 1%, about 0.5% to about 2%, about 0.5% to about 4%, about 0.5% to about 6%, about 0.5% to about 8%, about 0.5% to about 10%, about 0.5% to about 15%, about 0.5% to about 20%, about 0.75% to about 1%, about 0.75% to about 2%, about 0.75% to about 4%, about 0.75% to about 6%, about 0 .75% to about 8%, about 0.75% to about 10%, about 0.75% to about 15%, about 0.75% to about 20%, about 1% to about 2%, about 1% to about 4%, about 1% to about 6%, about 1% to about 8%, about 1% to about 10%, about 1% to about 15%, about 1% to about 20%, about 2% to about 4%, about 2% to about 6%, about 2% to about 8%, about 2% to about 10%, about 2% to about 15%, about 2 % to about 20%, about 4% to about 6%, about 4% to about 8%, about 4% to about 10%, about 4% to about 15%, about 4% to about 20%, about 6% to about 8%, about 6% to about 10%, about 6% to about 15%, about 6% to about 20%, about 8% to about 10%, about 8% to about 15%, about 8% to about 20%, about 10% to about 15%, about 10% to about 20%, or about 15% to about 20%. In some embodiments, the percentage by weight of the conductive additive in the conductive ink is about 0.25%, about 0.5%, about 0.75%, about 1%, about 2%, about 4%, about 6%, about 8%, about 10%, about 15%, or about 20%. In some embodiments, the percentage by weight of the conductive additive in the conductive ink is at least about 0.25%, about 0.5%, about 0.75%, about 1%, about 2%, about 4%, about 6%, about 8%, about 10%, or about 15%. In some embodiments, the percentage by weight of the conductive additive in the conductive ink is at most about 0.5%, about 0.75%, about 1%, about 2%, about 4%, about 6%, about 8%, about 10%, about 15%, or about 20%.

[0015] In some embodiments, the conductive ink has a viscosity of about 5 centipoise (cps) to about 40 cps. In some embodiments, the conductive ink has a viscosity of about 5 cps to about 10 cps, about 5 cps to about 15 cps, about 5 cps to about 20 cps, about 5 cps to about 25 cps, about 5 cps to about 30 cps, about 5 cps to about 35 cps, about 5 cps to about 40 cps, about 10 cps to about 15 cps, about 10 cps to about 20 cps, about 10 cps to about 25 cps, about 10 cps to about 30 cps, about 10 cps to about 35 cps, about 10 cps to about 40 cps, about 15 cps to about 20 cps. cps, about 15 cps to about 25 cps, about 15 cps to about 30 cps, about 15 cps to about 35 cps, about 15 cps to about 40 cps, about 20 cps to about 25 cps, about 20 cps to about 30 cps, about 20 cps to about 35 cps, about 20 cps to about 40 cps, about 25 cps to about 30 cps, about 25 cps to about 35 cps, about 25 cps to about 40 cps, about 30 cps to about 35 cps, about 30 cps to about 40 cps, or about 35 cps to about 40 cps. In some embodiments, the conductive ink has a viscosity of about 5 cps, about 10 cps, about 15 cps, about 20 cps, about 25 cps, about 30 cps, about 35 cps, or about 40 cps. In some embodiments, the conductive ink has a viscosity of at least about 5 cps, about 10 cps, about 15 cps, about 20 cps, about 25 cps, about 30 cps, or about 35 cps. In some embodiments, the conductive ink has a viscosity of at most about 10 cps, about 15 cps, about 20 cps, about 25 cps, about 30 cps, about 35 cps, or about 40 cps.

[0016] In some embodiments, the conductive ink has a sheet resistance when dry of about 0.1 ohm / sq / mil to about 0.8 ohm / sq / mil. In some embodiments, the conductive ink has a sheet resistance when dry of about 0.1 ohm / sq / mil to about 0.2 ohm / sq / mil, about 0.1 ohm / sq / mil to about 0.2 ohm / sq / mil. ohms / sq / mil to about 0.3 ohms / sq / mil, about 0.1 ohms / sq / mil to about 0.4 ohms / sq / mil, about 0.1 ohms / sq / mil to about 0.5 ohms / sq / mil, about 0.1 ohms / sq / mil to about 0.6 ohms / sq / mil, about 0.1 ohms / sq / mil to about 0.7 ohms / sq / mil, about 0.1 ohms / sq / mil to about 0.8 ohms / sq / mil, about 0.2 ohms / sq / mil to about 0.3 ohms / sq / mil, About 0.2 ohms / sq / mil to about 0.4 ohms / sq / mil, about 0.2 ohms / sq / mil to about 0.5 ohms / sq / mil, about 0.2 ohms / sq / mil to about 0.6 ohms / sq / mil, about 0.2 ohms / sq / mil to about 0.7 ohms / sq / mil, about 0.2 ohms / sq / mil to about 0.8 ohms / sq / mil, about 0.3 ohms / sq / mil to about 0.4 ohms / sq / mil, about 0.3 ohms / sq / mil to about 0.5 ohms / sq / mil q / mil, about 0.3 ohms / sq / mil to about 0.6 ohms / sq / mil, about 0.3 ohms / sq / mil to about 0.7 ohms / sq / mil, about 0.3 ohms / sq / mil to about 0.8 ohms / sq / mil, about 0.4 ohms / sq / mil to about 0.5 ohms / sq / mil, about 0.4 ohms / sq / mil to about 0.6 ohms / sq / mil, about 0.4 ohms / sq / mil to about 0.7 ohms / sq / mil, about 0.4 ohms / sq / mil to about 0.8 ohms / sq / mil, about 0.5 ohms / sq / mil to about 0.6 ohms / sq / mil, about 0.5 ohms / sq / mil to about 0.7 ohms / sq / mil, about 0.5 ohms / sq / mil to about 0.8 ohms / sq / mil, about 0.6 ohms / sq / mil to about 0.7 ohms / sq / mil, about 0.6 ohms / sq / mil to about 0.8 ohms / sq / mil, or about 0.7 ohms / sq / mil to about 0.8 ohms / sq / mil. In some embodiments, the conductive ink has a sheet resistance when dry of about 0.1 ohm / sq / mil, about 0.2 ohm / sq / mil, about 0.3 ohm / sq / mil, about 0.4 ohm / sq / mil, about 0.5 ohm / sq / mil, about 0.6 ohm / sq / mil, about 0.7 ohm / sq / mil, or about 0.8 ohm / sq / mil.In some embodiments, the conductive ink has a sheet resistance when dry of at least about 0.1 ohm / sq / mil, about 0.2 ohm / sq / mil, about 0.3 ohm / sq / mil, about 0.4 ohm / sq / mil, about 0.5 ohm / sq / mil, about 0.6 ohm / sq / mil, or about 0.7 ohm / sq / mil. In some embodiments, the conductive ink has a sheet resistance when dry of at most about 0.2 ohm / sq / mil, about 0.3 ohm / sq / mil, about 0.4 ohm / sq / mil, about 0.5 ohm / sq / mil, about 0.6 ohm / sq / mil, about 0.7 ohm / sq / mil, or about 0.8 ohm / sq / mil.

[0017] In some embodiments, the conductive ink further comprises at least one of a binder, a surfactant, and an antifoaming agent. In some embodiments, the conductive ink further comprises a pigment, a silver metallic pigment, a colorant, a silver metallic colorant, a dye, or any combination thereof. In some embodiments, the conductive ink has a conductivity of greater than 10 S / cm when dry.

[0018] Another aspect provided herein is a method of forming silver nanowires, the method including heating a solvent, adding a catalyst solution and a polymer solution to the solvent to form a first solution, injecting a silver-based solution into the first solution to form a second solution, centrifuging the second solution, and washing the second solution with a wash solution to extract the silver nanowires.

[0019] In some embodiments, the method further comprises heating the second solution prior to centrifuging the second solution. In some embodiments, the method further comprises cooling the second solution prior to centrifuging the second solution. In some embodiments, the solvent comprises a glycol, a polymer solution, or both. In some embodiments, washing the second solution comprises a plurality of washing cycles, including from about 2 cycles to about 6 cycles. In some embodiments, the method is carried out in a solvothermal chamber. In some embodiments, the solvent is stirred while being heated.

[0020] The silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 25% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 50% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 75% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. The silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. At least about 25% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. At least about 50% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm.At least about 75% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm.

[0021] In some embodiments, the polymer solution has a concentration of about 0.075 M to about 0.25 M. In some embodiments, the polymer solution has a concentration of about 0.075 M to about 0.1 M, about 0.075 M to about 0.125 M, about 0.075 M to about 0.15 M, about 0.075 M to about 0.175 M, about 0.075 M to about 0.2 M, about 0.075 M to about 0.225 M, about 0.075 M to about 0.25 M, about 0.1 M to about 0.125 M, about 0.1 M to about 0.15 M, about 0.1 M to about 0.175 M, about 0.1 M to about 0.2 M, about 0.1 M to about 0.225 M, about 0.1 M to about 0.25 M, about 0.125 M to about 0.1 5M, about 0.125M to about 0.175M, about 0.125M to about 0.2M, about 0.125M to about 0.225M, about 0.125M to about 0.25M, about 0.15M to about 0.175M, about 0.15M to about 0.2M, about 0.15M to about 0.225M, about 0 .15M to about 0.25M, about 0.175M to about 0.2M, about 0.175M to about 0.225M, about 0.175M to about 0.25M, about 0.2M to about 0.225M, about 0.2M to about 0.25M, or about 0.225M to about 0.25M. In some embodiments, the polymer solution has a concentration of about 0.075 M, about 0.1 M, about 0.125 M, about 0.15 M, about 0.175 M, about 0.2 M, about 0.225 M, or about 0.25 M. In some embodiments, the polymer solution has a concentration of at least about 0.075 M, about 0.1 M, about 0.125 M, about 0.15 M, about 0.175 M, about 0.2 M, about 0.225 M, or about 0.25 M. In some embodiments, the polymer solution has a concentration of up to about 0.075 M, about 0.1 M, about 0.125 M, about 0.15 M, about 0.175 M, about 0.2 M, about 0.225 M, or about 0.25 M.

[0022] In some embodiments, the catalyst solution has a concentration of about 2 mM to about 8 mM. In an embodiment, the catalyst solution may be from about 2 mM to about 2.5 mM, from about 2 mM to about 3 mM, from about 2 mM to about 3.5 mM, from about 2 mM to about 4 mM, from about 2 mM to about 4.5 mM, from about 2 mM to about 5 mM, from about 2 mM to about 5.5 mM, from about 2 mM to about 6 mM, from about 2 mM to about 6.5 mM, from about 2 mM to about 7 mM, from about 2 mM to about 8 mM, from about 2.5 mM to about 3 mM, from about 2.5 mM to about 3.5 mM, from about 2.5 mM to about 4 mM, from about 2.5 mM to about 4.5 mM, from about 2.5 mM to about 5 mM, Approximately 2.5mM to approximately 5.5mM, approximately 2.5mM to approximately 6mM, approximately 2.5mM to approximately 6.5mM, approximately 2.5mM to approximately 7mM, approximately 2.5mM to approximately 8mM, approximately 3mM to approximately 3.5mM, approximately 3mM to approximately 4mM, approximately 3mM to approximately 4.5mM, approximately 3mM to about 5mM, about 3mM to about 5.5mM, about 3mM to about 6mM, about 3mM to about 6.5mM, about 3mM to about 7mM, about 3mM to about 8mM, about 3.5mM to about 4mM, about 3.5mM to about 4.5mM, about 3.5mM to about 5mM , about 3.5mM to about 5.5mM, about 3.5mM to about 6mM, about 3.5mM to about 6.5mM, about 3.5mM to about 7mM, about 3.5mM to about 8mM, about 4mM to about 4.5mM, about 4mM to about 5mM, about 4mM to about 5.5mM, Approximately 4mM to approximately 6mM, approximately 4mM to approximately 6.5mM, approximately 4mM to approximately 7mM, approximately 4mM to approximately 8mM, approximately 4.5mM to approximately 5mM, approximately 4.5mM to approximately 5.5mM, approximately 4.5mM to approximately 6mM, approximately 4.5mM to approximately 6.5mM, approximately 4.5m In some embodiments, the concentration of the soluble ... In some embodiments, the catalyst solution has a concentration of about 2 mM, about 2.5 mM, about 3 mM, about 3.5 mM, about 4 mM, about 4.5 mM, about 5 mM, about 5.5 mM, about 6 mM, about 6.5 mM, about 7 mM, or about 8 mM. In some embodiments, the catalyst solution has a concentration of at least about 2 mM, about 2.5 mM, about 3 mM, about 3.5 mM, about 4 mM, about 4.5 mM, about 5 mM, about 5.5 mM, about 6 mM, about 6.5 mM, about 7 mM, or about 8 mM.In some embodiments, the catalyst solution has a concentration of up to about 2 mM, about 2.5 mM, about 3 mM, about 3.5 mM, about 4 mM, about 4.5 mM, about 5 mM, about 5.5 mM, about 6 mM, about 6.5 mM, about 7 mM, or about 8 mM.

[0023] In some embodiments, the volume of the solvent is about 75 to about 250 times greater than the volume of the catalyst solution. In some embodiments, the volume of the solvent is about 75 to about 100, about 75 to about 125, about 75 to about 150, about 75 to about 175, about 75 to about 200, about 75 to about 225, about 75 to about 250, about 100 to about 125, about 100 to about 150, about 100 to about 175, about 100 to about 200, about 100 to about 225, about 100 to about 250, about 1 25 to about 150, about 125 to about 175, about 125 to about 200, about 125 to about 225, about 125 to about 250, about 150 to about 175, about 150 to about 200, about 150 to about 225, about 150 to about 250, about 175 to about 200, about 175 to about 225, about 175 to about 250, about 200 to about 225, about 200 to about 250, or about 225 to about 250 times greater. In some embodiments, the volume of the solvent is about 75, about 100, about 125, about 150, about 175, about 200, about 225, or about 250 times greater than the volume of the catalyst solution. In some embodiments, the volume of the solvent is at least about 75, about 100, about 125, about 150, about 175, about 200, about 225, or about 250 times greater than the volume of the catalyst solution. In some embodiments, the volume of the solvent is at most about 75, about 100, about 125, about 150, about 175, about 200, about 225, or about 250 times greater than the volume of the catalyst solution.

[0024] In some embodiments, the volume of the solvent is about 1.5 to about 6.5 times larger than the volume of the polymer solution. In some embodiments, the volume of the solvent is about 1.5 to about 2, about 1.5 to about 2.5, about 1.5 to about 3, about 1.5 to about 3.5, about 1.5 to about 4, about 1.5 to about 4.5, about 1.5 to about 5, about 1.5 to about 5.5, about 1.5 to about 6, about 1.5 to about 6.5, about 2 to about 2.5, about 2 to about 3, about 2 to about 3.5, about 2 to about 4, about 2 to about 4 .5, about 2 to about 5, about 2 to about 5.5, about 2 to about 6, about 2 to about 6.5, about 2.5 to about 3, about 2.5 to about 3.5, about 2.5 to about 4, about 2.5 to about 4.5, about 2.5 to about 5, about 2.5 to about 5.5, about 2.5 to about 6, about 2.5 to about 6.5, about 3 to about 3.5, about 3 to about 4, about 3 to about 4.5, about 3 to about 5, about 3 to about 5.5, about 3 to about 6, about 3 to about 6.5, about 3.5 to about 4, about 3.5 to about 4.5, about 3.5 to about 5, about 3.5 to about 5.5, about 3.5 to about 6, about 3.5 to about 6.5, about 4 to about 4.5, about 4 to about 5, about 4 to about 5.5, about 4 to about 6, about 4 to about 6.5, about 4.5 to about 5, about 4.5 to about 5.5, about 4.5 to about 6, about 4.5 to about 6.5, about 5 to about 5.5, about 5 to about 6, about 5 to about 6.5, about 5.5 to about 6, about 5.5 to about 6.5, or about 6 to about 6.5 times greater. In some embodiments, the volume of the solvent is about 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 4.5, about 5, about 5.5, about 6, or about 6.5 times greater than the volume of the polymer solution. In some embodiments, the volume of the solvent is at least about 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 4.5, about 5, about 5.5, about 6, or about 6.5 times greater than the volume of the polymer solution, in some embodiments, the volume of the solvent is at most 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 4.5, about 5, about 5.5, about 6, or about 6.5 times greater than the volume of the polymer solution.

[0025] In some embodiments, the silver-based solution has a concentration of about 0.05M to about 0.2M. In some embodiments, the silver-based solution has a concentration of at least about 0.05M. In some embodiments, the silver-based solution has a concentration of up to about 0.2M. In some embodiments, the silver-based solution has a concentration of about 0.05M to about 0.075M, about 0.05M to about 0.1M, about 0.05M to about 0.125M, about 0.05M to about 0.15M, about 0.05M to about 0.175M, about 0.05M to about 0.2M, about 0.075M to about 0.1M, about 0.075M to about 0.125M, about 0.075M to about 0.15M, about 0.075M to about 0.175M, The silver-based solution has a concentration of about 0.075 M to about 0.2 M, about 0.1 M to about 0.125 M, about 0.1 M to about 0.15 M, about 0.1 M to about 0.175 M, about 0.1 M to about 0.2 M, about 0.125 M to about 0.15 M, about 0.125 M to about 0.175 M, about 0.125 M to about 0.2 M, about 0.15 M to about 0.175 M, about 0.15 M to about 0.2 M, or about 0.175 M to about 0.2 M. In some embodiments, the silver-based solution has a concentration of about 0.05 M, about 0.075 M, about 0.1 M, about 0.125 M, about 0.15 M, about 0.175 M, or about 0.2 M. In some embodiments, the silver-based solution has a concentration of at least about 0.05 M, about 0.075 M, about 0.1 M, about 0.125 M, about 0.15 M, about 0.175 M, or about 0.2 M. In some embodiments, the silver-based solution has a concentration of at most about 0.05 M, about 0.075 M, about 0.1 M, about 0.125 M, about 0.15 M, about 0.175 M, or about 0.2 M.

[0026] In some embodiments, the volume of the solvent is about 1.5 to about 6.5 times greater than the volume of the silver-based solution. In some embodiments, the volume of the solvent is at least about 1.5 times greater than the volume of the silver-based solution. In some embodiments, the volume of the solvent is up to about 6.5 times greater than the volume of the silver-based solution. In some embodiments, the volume of the solvent is about 1.5 to about 2, about 1.5 to about 2.5, about 1.5 to about 3, about 1.5 to about 3.5, about 1.5 to about 4, about 1.5 to about 4.5, about 1.5 to about 5, about 1.5 to about 5.5, about 1.5 to about 6, about 1.5 to about 6.5, about 2 to about 2.5, about 2 to about 3, about 2 to about 3.5, about 2 to about 4, about 2 to about 4.5, about 2 to about 5, about 2 to about 5.5, about 2 to about 6, about 2 to about 6.5, about 2.5 to about 3, about 2.5 to about 3.5, about 2.5 to about 4, about 2.5 to about 4.5, about 2.5 to about 5, about 2.5 to about 5.5, about 2.5 ...5.5, about 2.5 to about 5.5, about 2.5 to about 5.5, about 2.5 to about 5.5, about 2.5 to about 5.5, about 2.5 to about 5.5, about 2.5 to about 5.5, about 2.5 to about 5.5, about 2.5 to about 5.5, about 2.5 to about 5.5, about 2.5 to about 5.5, about 2.5 to about 5.5, about 2.5 to about 5.5, about about 6, about 2.5 to about 6.5, about 3 to about 3.5, about 3 to about 4, about 3 to about 4.5, about 3 to about 5, about 3 to about 5.5, about 3 to about 6, about 3 to about 6.5, about 3.5 to about 4, about 3.5 to about 4.5, about 3.5 to about 5, about 3.5 to about 5.5, about 3.5 to about 6, about 3.5 to about 6.5, about 4 to about 4.5, about 4 to about 5, about 4 to about 5.5, about 4 to about 6, about 4 to about 6.5, about 4.5 to about 5, about 4.5 to about 5.5, about 4.5 to about 6, about 4.5 to about 6.5, about 5 to about 5.5, about 5 to about 6, about 5 to about 6.5, about 5.5 to about 6, about 5.5 to about 6.5, or about 6 to about 6.5 times larger. In some embodiments, the volume of the solvent is greater than the volume of the silver-based solution. In some embodiments, the volume of the solvent is at least about 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 4.5, about 5, about 5.5, about 6, or about 6.5 times greater than the volume of the silver-based solution. In some embodiments, the volume of the solvent is at least about 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 4.5, about 5, about 5.5, about 6, or about 6.5 times greater than the volume of the silver-based solution. In some embodiments, the volume of the solvent is at most about 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 4.5, about 5, about 5.5, about 6, or about 6.5 times greater than the volume of the silver-based solution.

[0027] In some embodiments, the solvent is heated to a temperature of about 75° C. to about 300° C. In some embodiments, the solvent is heated to a temperature of at least about 75° C. In some embodiments, the solvent is heated to a temperature of up to about 300° C. In some embodiments, the solvent is heated to a temperature of about 75° C. to about 100° C., about 75° C. to about 125° C., about 75° C. to about 150° C., about 75° C. to about 175° C., about 75° C. to about 200° C., about 75° C. to about 225° C., about 75° C. to about 250° C., about 75° C. to about 275° C., about 75° C. to about 300° C., about 100° C. to about 125° C., about 100° C. to about 150° C., About 100°C to about 175°C, about 100°C to about 200°C, about 100°C to about 225°C, about 100°C to about 250°C, about 100°C to about 275°C, about 100°C to about 300°C, about 125°C to about 150°C, about 125°C to about 175°C, about 125°C to about 200°C, about 125°C to about 225°C, about 125°C to about 250°C, about 125°C to about 2 75°C, about 125°C to about 300°C, about 150°C to about 175°C, about 150°C to about 200°C, about 150°C to about 225°C, about 150°C to about 250°C, about 150°C to about 275°C, about 150°C to about 300°C, about 175°C to about 200°C, about 175°C to about 225°C, about 175°C to about 250°C, about 175°C to about 275°C, about 175 The solvent is heated to a temperature of about 75° C. to about 300° C., about 200° C. to about 225° C., about 200° C. to about 250° C., about 200° C. to about 275° C., about 200° C. to about 300° C., about 225° C. to about 250° C., about 225° C. to about 275° C., about 225° C. to about 300° C., about 250° C. to about 275° C., about 250° C. to about 300° C., or about 275° C. to about 300° C. In some embodiments, the solvent is heated to a temperature of about 75° C., about 100° C., about 125° C., about 150° C., about 175° C., about 200° C., about 225° C., about 250° C., about 275° C., or about 300° C. In some embodiments, the solvent is heated to a temperature of at least about 75° C., about 100° C., about 125° C., about 150° C., about 175° C., about 200° C., about 225° C., about 250° C., about 275° C., or about 300° C. In some embodiments, the solvent is heated to a temperature of up to about 75° C., about 100° C., about 125° C., about 150° C., about 175° C., about 200° C., about 225° C., about 250° C., about 275° C., or about 300° C.

[0028] In some embodiments, the solvent is heated for about 30 minutes to about 120 minutes. In some embodiments, the solvent is heated for at least about 30 minutes. In some embodiments, the solvent is heated for up to about 120 minutes. In some embodiments, the solvent is added for about 30 minutes to about 40 minutes, about 30 minutes to about 50 minutes, about 30 minutes to about 60 minutes, about 30 minutes to about 70 minutes, about 30 minutes to about 80 minutes, about 30 minutes to about 90 minutes, about 30 minutes to about 100 minutes, about 30 minutes to about 110 minutes, about 30 minutes to about 120 minutes, about 40 minutes to about 50 minutes, about 40 minutes to about 60 minutes, about 40 minutes to about 70 minutes, about 40 minutes to about 80 minutes, about 40 minutes to about 90 minutes, about 40 minutes to about 100 minutes, about 40 minutes to about 110 minutes, about 40 minutes to about 120 minutes, about 50 minutes to about 60 minutes, about 50 minutes to about 70 minutes, about 50 minutes to about 80 minutes, about 50 minutes to about 90 minutes, about 50 minutes to about 100 minutes, about 50 minutes to about 110 minutes, about 5 ...10 minutes, about 50 minutes to about 120 minutes, about 50 minutes to about 60 minutes, about 50 minutes to about 70 minutes, about 50 minutes to about 80 minutes, about 50 minutes to about 0 minutes, 50 minutes to 120 minutes, 60 minutes to 70 minutes, 60 minutes to 80 minutes, 60 minutes to 90 minutes, 60 minutes to 100 minutes, 60 minutes to 110 minutes, 60 minutes to 120 minutes, 70 minutes to 80 minutes, 70 minutes to 90 minutes, 70 minutes to 100 minutes, 70 minutes to 110 minutes, 70 minutes to approx. In some embodiments, the solvent is heated for at least about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, about 120 minutes, about 80 minutes to about 90 minutes, about 80 minutes to about 100 minutes, about 80 minutes to about 110 minutes, about 80 minutes to about 120 minutes, about 90 minutes to about 100 minutes, about 90 minutes to about 110 minutes, about 90 minutes to about 120 minutes, about 100 minutes to about 110 minutes, about 100 minutes to about 120 minutes, or about 110 minutes to about 120 minutes. In some embodiments, the solvent is heated for at least about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, or about 120 minutes. In some embodiments, the solvent is heated for up to about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, or about 120 minutes.

[0029] In some embodiments, the second solution is heated for about 30 minutes to about 120 minutes. In some embodiments, the second solution is heated for at least about 30 minutes. In some embodiments, the second solution is heated for up to about 120 minutes. In some embodiments, the second solution is incubated for about 30 minutes to about 40 minutes, about 30 minutes to about 50 minutes, about 30 minutes to about 60 minutes, about 30 minutes to about 70 minutes, about 30 minutes to about 80 minutes, about 30 minutes to about 90 minutes, about 30 minutes to about 100 minutes, about 30 minutes to about 110 minutes, about 30 minutes to about 120 minutes, about 40 minutes to about 50 minutes, about 40 minutes to about 60 minutes, about 40 minutes to about 70 minutes, about 40 minutes to about 80 minutes, about 40 minutes to about 90 minutes, about 40 minutes to about 100 minutes, about 40 minutes to about 110 minutes, about 40 minutes to about 120 minutes, about 50 minutes to about 60 minutes, about 50 minutes to about 70 minutes, about 50 minutes to about 80 minutes, about 50 minutes to about 90 minutes, about 50 minutes to about 100 minutes, about 50 minutes to about 110 minutes, 50 minutes to 120 minutes, 60 minutes to 70 minutes, 60 minutes to 80 minutes, 60 minutes to 90 minutes, 60 minutes to 100 minutes, 60 minutes to 110 minutes, 60 minutes to 120 minutes, 70 minutes to 80 minutes, 70 minutes to 90 minutes, 70 minutes to 100 minutes, 70 minutes to 110 minutes, 70 minutes to The second solution is heated for about 120 minutes, about 80 minutes to about 90 minutes, about 80 minutes to about 100 minutes, about 80 minutes to about 110 minutes, about 80 minutes to about 120 minutes, about 90 minutes to about 100 minutes, about 90 minutes to about 110 minutes, about 90 minutes to about 120 minutes, about 100 minutes to about 110 minutes, about 100 minutes to about 120 minutes, or about 110 minutes to about 120 minutes. In some embodiments, the second solution is heated for about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, or about 120 minutes. In some embodiments, the second solution is heated for at least about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, or about 120 minutes. In some embodiments, the second solution is heated for up to about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, or about 120 minutes.

[0030] In some embodiments, stirring is performed at a speed of about 100 rpm to about 400 rpm. In some embodiments, stirring is performed at a speed of at least about 100 rpm. In some embodiments, stirring is performed at a speed of up to about 400 rpm. In some embodiments, stirring is performed at a speed of about 100 rpm to about 125 rpm, about 100 rpm to about 150 rpm, about 100 rpm to about 175 rpm, about 100 rpm to about 200 rpm, about 100 rpm to about 225 rpm, about 100 rpm to about 250 rpm, about 100 rpm to about 275 rpm, about 100 rpm to about 300 rpm, about 100 rpm to about 350 rpm, about 100 rpm to about 400 rpm, about 125 rpm to about 150 rpm. , about 125 rpm to about 175 rpm, about 125 rpm to about 200 rpm, about 125 rpm to about 225 rpm, about 125 rpm to about 250 rpm, about 125 rpm to about 275 rpm, about 125 rpm to about 300 rpm , about 125 rpm to about 350 rpm, about 125 rpm to about 400 rpm, about 150 rpm to about 175 rpm, about 150 rpm to about 200 rpm, about 150 rpm to about 225 rpm, about 150 rpm to about 250 rpm , about 150rpm to about 275rpm, about 150rpm to about 300rpm, about 150rpm to about 350rpm, about 150rpm to about 400rpm, about 175rpm to about 200rpm, about 175rpm to about 225rpm , about 175rpm to about 250rpm, about 175rpm to about 275rpm, about 175rpm to about 300rpm, about 175rpm to about 350rpm, about 175rpm to about 400rpm, about 200rpm to about 225rpm , about 200rpm to about 250rpm, about 200rpm to about 275rpm, about 200rpm to about 300rpm, about 200rpm to about 350rpm, about 200rpm to about 400rpm, about 225rpm to about 250rpm , about 225rpm to about 275rpm, about 225rpm to about 300rpm, about 225rpm to about 350rpm, about 225rpm to about 400rpm, about 250rpm to about 275rpm, about 250rpm to about 300rpm , about 250 rpm to about 350 rpm, about 250 rpm to about 400 rpm, about 275 rpm to about 300 rpm, about 275 rpm to about 350 rpm, about 275 rpm to about 400 rpm, about 300 rpm to about 350 rpm, about 300 rpm to about 400 rpm, or about 350 rpm to about 400 rpm. In some embodiments, stirring is performed at a speed of about 100 rpm, about 125 rpm, about 150 rpm, about 175 rpm, about 200 rpm, about 225 rpm, about 250 rpm, about 275 rpm, about 300 rpm, about 350 rpm, or about 400 rpm. In some embodiments, stirring is performed at a speed of at least about 100 rpm, about 125 rpm, about 150 rpm, about 175 rpm, about 200 rpm, about 225 rpm, about 250 rpm, about 275 rpm, about 300 rpm, about 350 rpm, or about 400 rpm. In some embodiments, stirring is performed at a speed of at most about 100 rpm, about 125 rpm, about 150 rpm, about 175 rpm, about 200 rpm, about 225 rpm, about 250 rpm, about 275 rpm, about 300 rpm, about 350 rpm, or about 400 rpm.

[0031] In some embodiments, centrifugation occurs for about 10 minutes to about 40 minutes. In some embodiments, centrifugation occurs for at least about 10 minutes. In some embodiments, centrifugation occurs for up to about 40 minutes. In some embodiments, centrifugation is performed for about 10 minutes to about 15 minutes, about 10 minutes to about 20 minutes, about 10 minutes to about 25 minutes, about 10 minutes to about 30 minutes, about 10 minutes to about 35 minutes, about 10 minutes to about 40 minutes, about 15 minutes to about 20 minutes, about 15 minutes to about 25 minutes, about 15 minutes to about 30 minutes, about 15 minutes to about 35 minutes, about 15 minutes to about 40 minutes, about 20 minutes to about 25 minutes, about 20 minutes to about 30 minutes, about 20 minutes to about 35 minutes, about 20 minutes to about 40 minutes, about 25 minutes to about 30 minutes, about 25 minutes to about 35 minutes, about 25 minutes to about 40 minutes, about 30 minutes to about 35 minutes, about 30 minutes to about 40 minutes, or about 35 minutes to about 40 minutes. In some embodiments, centrifugation is performed for about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, or about 40 minutes. In some embodiments, centrifugation is performed for at least about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, or about 40 minutes. In some embodiments, centrifugation is performed for up to about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, or about 40 minutes.

[0032] Another aspect provided herein is a conductive carbon-based adhesive comprising a carbon-based material and an adhesive. In some embodiments, the carbon-based material is selected from the group consisting of graphene, graphite powder, natural graphite, synthetic graphite, expanded graphite, carbon black, Timcal carbon super C45, Timcal carbon super C65, cabot carbon, carbon super P, acetylene black, fluororesin ... The carbon nanotubes may be selected from the group consisting of furnace black, carbon nanotubes, vapor grown carbon fibers, graphene oxide, and any combination thereof.

[0033] In some embodiments, the adhesive comprises about 60% to about 99.9% by weight of a conductive carbon-based adhesive. In some embodiments, the adhesive comprises at least about 60% by weight of a conductive carbon-based adhesive. In some embodiments, the adhesive comprises up to about 99.9% by weight of a conductive carbon-based adhesive. In some embodiments, the adhesive is, by weight percentage, about 60% to about 65%, about 60% to about 70%, about 60% to about 75%, about 60% to about 80%, about 60% to about 85%, about 60% to about 90%, about 60% to about 95%, about 60% to about 97%, about 60% to about 99%, about 60% to about 99.9%, about 65% to about 70%, about 65% to about 75%, about 65% to about 80%, about 65% to about 85%, about 65% to about 90%, about 65% to about 95%, about 65% ~ about 97%, about 65% to about 99%, about 65% to about 99.9%, about 70% to about 75%, about 70% to about 80%, about 70% to about 85%, about 70% to about 90%, about 70% to about 95%, about 70% to about 97%, about 70% to about 99%, about 70% to about 99.9%, about 75% to about 80%, about 75% to about 85%, about 75% to about 90%, about 75% to about 95%, about 75% to about 97%, about 75% to about 99%, about 75% to about 99.9%, about 80% to about 85 %, about 80% to about 90%, about 80% to about 95%, about 80% to about 97%, about 80% to about 99%, about 80% to about 99.9%, about 85% to about 90%, about 85% to about 95%, about 85% to about 97%, about 85% to about 99%, about 85% to about 99.9%, about 90% to about 95%, about 90% to about 97%, about 90% to about 99%, about 90% to about 99.9%, about 95% to about 97%, about 95% to about 99%, about 95% to about 99.9%, about 97% to about 99%, about 97% to about 99.9%, or about 99% to about 99.9% conductive carbon-based adhesive. In some embodiments, the adhesive comprises about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 97%, about 99%, or about 99.9% by weight of a conductive carbon-based adhesive. In some embodiments, the adhesive comprises at least about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 97%, about 99%, or about 99.9% by weight of a conductive carbon-based adhesive. In some embodiments, the adhesive comprises at most about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 97%, about 99%, or about 99.9% by weight of a conductive carbon-based adhesive.

[0034] In some embodiments, the carbon-based material comprises about 0.1% to about 40% by weight of the conductive carbon-based adhesive. In some embodiments, the carbon-based material comprises at least about 0.1% by weight of the conductive carbon-based adhesive. In some embodiments, the carbon-based material comprises up to about 40% by weight of the conductive carbon-based adhesive. In some embodiments, the carbon-based material is, by weight percentage, about 0.1% to about 0.2%, about 0.1% to about 0.5%, about 0.1% to about 1%, about 0.1% to about 5%, about 0.1% to about 10%, about 0.1% to about 15%, about 0.1% to about 20%, about 0.1% to about 25%, about 0.1% to about 30%, about 0.1% to about 35%, about 0.1% to about 40%, about 0.2% to about 0.5%, about 0.2% to about 1%, about 0.2% to about 5%, About 0.2% to about 10%, about 0.2% to about 15%, about 0.2% to about 20%, about 0.2% to about 25%, about 0.2% to about 30%, about 0.2% to about 35%, about 0.2% to about 40%, about 0.5% to about 1%, about 0.5% to about 5%, about 0.5% to about 10%, about 0.5% to about 15%, about 0.5% to about 20%, about 0.5% to about 25%, about 0.5% to about 30%, about 0.5% to about 35%, about 0.5% to about 40%, about 1% to About 5%, about 1% to about 10%, about 1% to about 15%, about 1% to about 20%, about 1% to about 25%, about 1% to about 30%, about 1% to about 35%, about 1% to about 40%, about 5% to about 10%, about 5% to about 15%, about 5% to about 20%, about 5% to about 25%, about 5% to about 30%, about 5% to about 35%, about 5% to about 40%, about 10% to about 15%, about 10% to about 20%, about 10% to about 25%, about 10% to about 30%, about 10% to about 35 %, about 10% to about 40%, about 15% to about 20%, about 15% to about 25%, about 15% to about 30%, about 15% to about 35%, about 15% to about 40%, about 20% to about 25%, about 20% to about 30%, about 20% to about 35%, about 20% to about 40%, about 25% to about 30%, about 25% to about 35%, about 25% to about 40%, about 30% to about 35%, about 30% to about 40%, or about 35% to about 40% conductive carbon-based adhesive. In some embodiments, the carbon-based material comprises about 0.1%, about 0.2%, about 0.5%, about 1%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40% conductive carbon-based adhesive by weight.In some embodiments, the carbon-based material comprises at least about 0.1%, about 0.2%, about 0.5%, about 1%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40% by weight of the conductive carbon-based adhesive. In some embodiments, the carbon-based material comprises at most about 0.1%, about 0.2%, about 0.5%, about 1%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40% by weight of the conductive carbon-based adhesive.

[0035] In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is between about 0.1% and about 10%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is at least about 0.1%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is at least about 0.1%. In some embodiments, the carbon-based material comprises graphene and the weight percentage of graphene in the carbon-based material is about 0.1% to about 0.2%, about 0.1% to about 0.5%, about 0.1% to about 1%, about 0.1% to about 2%, about 0.1% to about 3%, about 0.1% to about 4%, about 0.1% to about 5%, about 0.1% to about 6%, about 0.1% to about 7%, about 0.1% to about 8%, about 0.1% to about 10%, about 0.1% to about 15%, about 0.1% to about 20%, about 0.1% to about 35%, about 0.1% to about 40%, about 0.1% to about 50%, about 0.1% to about 65%, about 0.1% to about 70%, about 0.1% to about 85%, about 0.1% to about 150%, about 0.1% to about 200%, about 0.1% to about 25 ... .2% to about 0.5%, about 0.2% to about 1%, about 0.2% to about 2%, about 0.2% to about 3%, about 0.2% to about 4%, about 0.2% to about 5%, about 0.2% to about 6%, about 0.2% to about 7%, about 0.2% to about 8%, about 0.2% to about 10%, about 0.5% to about 1%, about 0.5% to about 2%, about 0.5% to about 3%, about 0.5% to about 4%, about 0.5% to about 5%, about 0.5% to about 6%, about 0.5 % to about 7%, about 0.5% to about 8%, about 0.5% to about 10%, about 1% to about 2%, about 1% to about 3%, about 1% to about 4%, about 1% to about 5%, about 1% to about 6%, about 1% to about 7%, about 1% to about 8%, about 1% to about 10%, about 2% to about 3%, about 2% to about 4%, about 2% to about 5%, about 2% to about 6%, about 2% to about 7%, about 2% to about 8%, about 2% to about 10%, about 3% to about 4%, about 3% to about 5% , about 3% to about 6%, about 3% to about 7%, about 3% to about 8%, about 3% to about 10%, about 4% to about 5%, about 4% to about 6%, about 4% to about 7%, about 4% to about 8%, about 4% to about 10%, about 5% to about 6%, about 5% to about 7%, about 5% to about 8%, about 5% to about 10%, about 6% to about 7%, about 6% to about 8%, about 6% to about 10%, about 7% to about 8%, about 7% to about 10%, or about 8% to about 10%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is about 0.1%, about 0.2%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 10%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is at least about 0.1%, about 0.2%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 10%.In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is at most about 0.1%, about 0.2%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 10%.

[0036] In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is between about 1% and about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at least about 1%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at most about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is about 1% to about 2%, about 1% to about 5%, about 1% to about 10%, about 1% to about 15%, about 1% to about 20%, about 1% to about 25%, about 1% to about 30%, about 1% to about 35%, about 1% to about 40%, about 2% to about 5%, about 2% to about 10%, about 2% to about 15%, about 2% to about 20%, about 2% to about 25%, about 2% to about 30%, about 2% to about 35%, about 2% to about 40%, about 5% to about 10%, about 5% to about 15%, about 5% to about 20%, about 5% to about 25%, about 5% to about 30%, about 35 ... 0%, about 5% to about 35%, about 5% to about 40%, about 10% to about 15%, about 10% to about 20%, about 10% to about 25%, about 10% to about 30%, about 10% to about 35%, about 10% to about 40%, about 15% to about 20%, about 15% to about 25%, about 15% to about 30%, about 15% to about 35%, about 15% to about 40%, about 20% to about 25%, about 20% to about 30%, about 20% to about 35%, about 20% to about 40%, about 25% to about 30%, about 25% to about 35%, about 25% to about 40%, about 30% to about 35%, about 30% to about 40%, or about 35% to about 40%. In some embodiments, the carbon-based material comprises graphite powder and the weight percentage of graphene in the carbon-based material is about 1%, about 2%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%. In some embodiments, the carbon-based material comprises graphite powder and the weight percentage of graphene in the carbon-based material is at least about 1%, about 2%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%. In some embodiments, the carbon-based material comprises graphite powder and the weight percentage of graphene in the carbon-based material is at most about 1%, about 2%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%.

[0037] In some embodiments, the adhesive is a carpenter's glue, wood glue, cyanoacrylate, contact cement, latex, library paste, rubber The conductive carbon based adhesive may further comprise a conductive filler, such as methyl cellulose, resorcinol resin, starch, butanone, dichloromethane acrylic, ethylene vinyl, phenol formaldehyde resin, polyamide, polyester, polyethylene, polypropylene, polysulfide, polyurethane, polyvinyl acetate, aliphatic, polyvinyl alcohol, polyvinyl chloride, polyvinyl chloride emulsion, silicone, styrene acrylic, epichlorohydrin, epoxide, or any combination thereof. In some embodiments, the conductive carbon based adhesive further comprises a conductive filler. In some embodiments, the conductive filler comprises silver. In some embodiments, the silver comprises silver nanoparticles, silver nanorods, silver nanowires, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or any combination thereof. In some embodiments, the conductive carbon based adhesive further comprises a thinner. In some embodiments, the thinner comprises butyl acetate, lacquer thinner, acetone, petroleum naphtha, mineral spirits, xylene, or any combination thereof.

[0038] In some embodiments, the conductive carbon-based adhesive comprises about 50% to about 99% thinner by volume. In some embodiments, the conductive carbon-based adhesive comprises at least about 50% thinner by volume. In some embodiments, the conductive carbon-based adhesive comprises up to about 99% thinner by volume. In some embodiments, the conductive carbon-based adhesive comprises about 50% to about 55%, about 50% to about 60%, about 50% to about 65%, about 50% to about 70%, about 50% to about 75%, about 50% to about 80%, about 50% to about 85%, about 50% to about 90%, about 50% to about 95%, about 50% to about 99%, about 55% to about 60%, about 55% to about 6 5%, about 55% to about 70%, about 55% to about 75%, about 55% to about 80%, about 55% to about 85%, about 55% to about 90%, about 55% to about 95%, about 55% to about 99%, about 60% to about 65%, about 60% to about 70%, about 60% to about 75%, about 60% to about 80%, about 60% to about 85%, about 60% to about 90%, about 60% to about 95%, about 60% to About 99%, about 65% to about 70%, about 65% to about 75%, about 65% to about 80%, about 65% to about 85%, about 65% to about 90%, about 65% to about 95%, about 65% to about 99%, about 70% to about 75%, about 70% to about 80%, about 70% to about 85%, about 70% to about 90%, about 70% to about 95%, about 70% to about 99%, about 75% to about 80%, about 75 % to about 85%, about 75% to about 90%, about 75% to about 95%, about 75% to about 99%, about 80% to about 85%, about 80% to about 90%, about 80% to about 95%, about 80% to about 99%, about 85% to about 90%, about 85% to about 95%, about 85% to about 99%, about 90% to about 95%, about 90% to about 99%, or about 95% to about 99% thinner. In some embodiments, the conductive carbon-based adhesive comprises about 50%, about 55%, about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, or about 99% thinner by volume. In some embodiments, the conductive carbon-based adhesive comprises at least about 50%, about 55%, about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, or about 99% thinner by volume.In some embodiments, the conductive carbon-based adhesive comprises up to about 50%, about 55%, about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, or about 99% thinner by volume.

[0039] In some embodiments, the conductive carbon based adhesive has a sheet resistance of about 5 ohms / sq to about 500 ohms / sq. In some embodiments, the conductive carbon based adhesive has a sheet resistance of at least about 5 ohms / sq. In some embodiments, the conductive carbon based adhesive has a sheet resistance of up to about 500 ohms / sq. In some embodiments, the conductive carbon based adhesive has a sheet resistance of about 5 ohms / sq to about 10 ohms / sq, about 5 ohms / sq to about 20 ohms / sq, about 5 ohms / sq to about 50 ohms / sq, about 5 ohms / sq to about 10 0 ohms / sq, approx. 5 ohms / sq to approx. 150 ohms / sq, approx. 5 ohms / sq to approx. 200 ohms / sq, approx. 5 ohms / sq to approx. 250 ohms / sq, approx. 5 ohms / sq to approx. 300 ohms / sq, approx. 5 ohms / sq to approx. 350 ohms / sq, approx. 5 ohms / sq to approx. 400 ohms / sq, approx. 5 ohms / sq to approx. 500 ohms / sq, approx. 10 ohms / sq to approx. 20 ohms / sq, approx. 10 ohms / sq to approx. 50 ohms / sq, approx. 10 ohms / sq to approx. 100 ohms / sq, approx. 10 ohms / sq to approx. 150 ohms / sq, approx. 10 ohms / sq to approx. 200 ohms / sq q, about 10 ohms / sq to about 250 ohms / sq, about 10 ohms / sq to about 300 ohms / sq, about 10 ohms / sq to about 350 ohms / sq, about 10 ohms / sq to about 400 ohms / sq, about 10 ohms / sq to about 500 ohms / sq, about 20 ohms / sq to about 50 ohms / sq, about 20 ohms / sq to about 100 ohms / sq, about 20 ohms / sq to about 150 ohms / sq, about 20 ohms / sq to about 200 ohms / sq, about 20 ohms / sq to about 250 ohms / sq, about 20 ohms / sq to about 300 ohms / sq, about 20 ohms / sq to about 350 ohms / sq sq, about 20 ohms / sq to about 400 ohms / sq, about 20 ohms / sq to about 500 ohms / sq, about 50 ohms / sq to about 100 ohms / sq, about 50 ohms / sq to about 150 ohms / sq, about 50 ohms / sq to about 200 ohms / sq, about 50 ohms / sq to about 250 ohms / sq, about 50 ohms / sq to about 300 ohms / sq, about 50 ohms / sq to about 350 ohms / sq, about 50 ohms / sq to about 400 ohms / sq, about 50 ohms / sq to about 500 ohms / sq, about 100 ohms / sq to about 150 ohms / sq, about 100 ohms / sq to about 20 0 ohms / sq, about 100 ohms / sq to about 250 ohms / sq, about 100 ohms / sq to about 300 ohms / sq, about 100 ohms / sq to about 350 ohms / sq, about 100 ohms / sq to about 400 ohms / sq, about 100 ohms / sq to about 500 ohms / sq, about 150 ohms / sq to about 200 ohms / sq, about 150 ohms / sq to about 250 ohms / sq, about 150 ohms / sq to about 300 ohms / sq, about 150 ohms / sq to about 350 ohms / sq, about 150 ohms / sq to about 400 ohms / sq, about 150 ohms / sq to about 500 ohms / sq,Approximately 200 ohms / sq to approximately 250 ohms / sq, approximately 200 ohms / sq to approximately 300 ohms / sq, approximately 200 ohms / sq to approximately 350 ohms / sq, approximately 200 ohms / sq to approximately 400 ohms / sq, approximately 200 ohms / sq to approximately 500 ohms / sq, approximately 250 ohms / sq to approximately 300 ohms / sq, approximately 250 ohms / sq to approximately 350 ohms / sq, approximately 250 ohms / sq to approximately 400 ohms / sq In one embodiment, the sheet resistance is about 250 ohms / sq to about 500 ohms / sq, about 300 ohms / sq to about 350 ohms / sq, about 300 ohms / sq to about 400 ohms / sq, about 300 ohms / sq to about 500 ohms / sq, about 350 ohms / sq to about 400 ohms / sq, about 350 ohms / sq to about 500 ohms / sq, or about 400 ohms / sq to about 500 ohms / sq. In some embodiments, the conductive carbon based adhesive has a sheet resistance of about 5 ohms / sq, about 10 ohms / sq, about 20 ohms / sq, about 50 ohms / sq, about 100 ohms / sq, about 150 ohms / sq, about 200 ohms / sq, about 250 ohms / sq, about 300 ohms / sq, about 350 ohms / sq, about 400 ohms / sq, or about 500 ohms / sq. In some embodiments, the conductive carbon based adhesive has a sheet resistance of at least about 5 ohms / sq, about 10 ohms / sq, about 20 ohms / sq, about 50 ohms / sq, about 100 ohms / sq, about 150 ohms / sq, about 200 ohms / sq, about 250 ohms / sq, about 300 ohms / sq, about 350 ohms / sq, about 400 ohms / sq, or about 500 ohms / sq. In some embodiments, the conductive carbon-based adhesive has a sheet resistance of at most about 5 ohms / sq, about 10 ohms / sq, about 20 ohms / sq, about 50 ohms / sq, about 100 ohms / sq, about 150 ohms / sq, about 200 ohms / sq, about 250 ohms / sq, about 300 ohms / sq, about 350 ohms / sq, about 400 ohms / sq, or about 500 ohms / sq.

[0040] In some embodiments, the conductive carbon based adhesive has a sheet resistance of about 0.3 ohms / sq / mil to about 2 ohms / sq / mil. In some embodiments, the conductive carbon based adhesive has a sheet resistance of at least about 0.3 ohms / sq / mil, about 0.4 ohms / sq / mil, about 0.6The sheet resistance is about 0.8 ohms / sq / mil, about 1 ohm / sq / mil, about 1.2 ohms / sq / mil, about 1.4 ohms / sq / mil, about 1.6 ohms / sq / mil, about 1.8 ohms / sq / mil, or about 2 ohms / sq / mil. In some embodiments, the conductive carbon-based adhesive has a sheet resistance of at most about 0.3 ohms / sq / mil, about 0.4 ohms / sq / mil, about 0.6 ohms / sq / mil, about 0.8 ohms / sq / mil, about 1 ohm / sq / mil, about 1.2 ohms / sq / mil, about 1.4 ohms / sq / mil, about 1.6 ohms / sq / mil, about 1.8 ohms / sq / mil, or about 2 ohms / sq / mil. In some embodiments, the conductive carbon based adhesive has a thickness of about 0.3 ohms / sq / mil to about 0.4 ohms / sq / mil, about 0.3 ohms / sq / mil to about 0.6 ohms / sq / mil, about 0.3 ohms / sq / mil to about 0.8 ohms / sq / mil, about 0.3 ohms / sq / mil to about 1 ohm / sq / mil, about 0.3 ohms / sq / mil to about 1.2 ohms ... 0.3 ohms / sq / mil to about 1.6 ohms / sq / mil, 0.3 ohms / sq / mil to about 1.8 ohms / sq / mil, 0.3 ohms / sq / mil to about 2 ohms / sq / mil, 0.4 ohms / sq / mil to about 0.6 ohms / sq / mil, 0.4 ohms / sq / mil to about 0.8 ohms / sq / mil, 0.4 ohms / sq / mil to about 1 ohms / sq / mil, about 0.4 ohms / sq / mil to about 1.2 ohms / sq / mil, about 0.4 ohms / sq / mil to about 1.4 ohms / sq / mil, about 0.4 ohms / sq / mil to about 1.6 ohms / sq / mil, about 0.4 ohms / sq / mil to about 1.8 ohms / sq / mil, about 0.4 ohms / sq / mil to about 2 ohms / sq / mil, about 0.6 ohms / sq / mil to about 0.8 ohms / sq / mil q / mil, about 0.6 ohms / sq / mil to about 1 ohm / sq / mil, about 0.6 ohms / sq / mil to about 1.2 ohms / sq / mil, about 0.6 ohms / sq / mil to about 1.4 ohms / sq / mil, about 0.6 ohms / sq / mil to about 1.6 ohms / sq / mil, about 0.6 ohms / sq / mil to about 1.8 ohms / sq / mil, about 0.6 ohms / sq / mil to about 2 ohms / sq / mil, about 0.8 ohms / sq / mil to about 1 ohm / sq / mil, about 0.8 ohms / sq / mil to about 1.2 ohms / sq / mil, about 0.8 ohms / sq / mil to about 1.4 ohms / sq / mil, about 0.8 ohms / sq / mil to about 1.6 ohms / sq / mil, about 0.8 ohms / sq / mil to about 1.8 ohms / sq / mil, about 0.8 ohms / sq / mil to about 2 ohms / sq / mil, about 1 ohms / sq / mil to about 1.2 ohms / sq / mil, about 1 ohms / sq / mil to about 1.4 ohms / sq / mil, about 1 ohms / sq / mil to about 1.6 ohms / sq / mil, about 1 ohms / sq / mil to about 1.8 ohms / sq / mil, about 1 ohms / sq / mil to about 2 ohms / sq / mil 1.2 ohms / sq / mil to about 1.4 ohms / sq / mil, about 1.2 ohms / sq / mil to about 1.6 ohms / sq / mil, about 1.2 ohms / sq / mil to about 1.8 ohms / sq / mil, about 1.2 ohms / sq / mil to about 2 ohms / sq / mil, about 1.4 ohms / sq / mil to about 1.6 ohms / sq / mil, about 1.4 ohms / sq / mil to about 1.8 ohms / sq / mil, about 1.4 ohms / sq / mil to about 2 ohms / sq / mil, about 1.6 ohms / sq / mil to about 1.8 ohms / sq / mil, about 1.6 ohms / sq / mil to about 2 ohms / sq / mil, or about 1.8 ohms / sq / mil to about 2 ohms / sq / mil. In some embodiments, the conductive carbon-based adhesive has a sheet resistance of about 0.3 ohms / sq / mil, about 0.4 ohms / sq / mil, about 0.6 ohms / sq / mil, about 0.8 ohms / sq / mil, about 1 ohm / sq / mil, about 1.2 ohms / sq / mil, about 1.4 ohms / sq / mil, about 1.6 ohms / sq / mil, about 1.8 ohms / sq / mil, or about 2 ohms / sq / mil. In some embodiments, the conductive carbon based adhesive has a sheet resistance of at least about 0.3 ohms / sq / mil, about 0.4 ohms / sq / mil, about 0.6 ohms / sq / mil, about 0.8 ohms / sq / mil, about 1 ohm / sq / mil, about 1.2 ohms / sq / mil, about 1.4 ohms / sq / mil, about 1.6 ohms / sq / mil, about 1.8 ohms / sq / mil, or about 2 ohms / sq / mil. In some embodiments, the conductive carbon based adhesive has a sheet resistance of at most about 0.3 ohms / sq / mil, about 0.4 ohms / sq / mil, about 0.6 ohms / sq / mil, about 0.8 ohms / sq / mil, approx. 1 ohm / sq / mil, approx. 1.2 ohms. The substrate may have a sheet resistance of about 1.5 ohms / sq / mil, about 1.4 ohms / sq / mil, about 1.6 ohms / sq / mil, about 1.8 ohms / sq / mil, or about 2 ohms / sq / mil.

[0041] In some embodiments, the conductive carbon based adhesive has a conductivity of about 0.15 S / m to about 60 S / m. In some embodiments, the conductive carbon based adhesive has a conductivity of at least about 0.15 S / m. In some embodiments, the conductive carbon based adhesive has a conductivity of up to about 60 S / m.The actual application form is that the conductive carbon-based adhesive is about 0.15S / m to about 0.3S / m, about 0.15S / m to about 0.5S / m, about 0.15S / m to about 1S / m, about 0.15S / m to about 2S / m, about 0.15S / m to about 5S / m, about 0.15S / m to about 10S / m, about 0. 15S / m to about 20S / m, about 0.15S / m to about 30S / m, about 0.15S / m to about 40S / m, about 0.15S / m to about 50S / m, about 0.15S / m to about 60S / m, about 0.3S / m to about 0.5S / m, about 0.3S / m to about 1S / m, about 0.3S / m to about 2S / m, about 0.3S / m to about 5S / m, about 0.3S / m to about 10S / m, about 0.3S / m to about 20S / m, about 0.3S / m to about 30S / m, about 0.3S / m to about 40S / m, about 0.3S / m to about 50S / m, about 0.3S / m to about 60S / m, about 0.5S / m to about 1S / m, about 0.5S / m to about 2S / m, about 0.5S / m to about 5S / m, about 0.5S / m to about 10S / m, about 0.5S / m to about 20S / m, about 0.5S / m to about 30S / m, about 0.5S / m to about 40S / m, about 0.5S / m to about 50S / m, about 0.5S / m to about 60S / m, about 1S / m to about 2S / m, about 1S / m to about 5S / m, about 1S / m to about 10S / m, about 1S / m to about 20S / m, about 1S / m to about 30S / m, about 1S / m to about 40S / m, about 1S / m to about 50S / m, about 1S / m to about 60S / m, about 2S / m to about 5S / m, about 2S / m to about 10S / m, about 2S / m to about 20S / m, about 2S / m to about 30S / m, about 2S / m to about 40S / m, about 2S / m to about 50S / m, about 2S / m to about 60S / m, about 5S / m to about 10S / m, about 5S / m to about 20S / m, about 5S / m to about 30S / m, about 5S / m to about 40S / m, about 5S / m to about 50S / m m to about 50S / m, about 5S / m to about 60S / m, about 10S / m to about 20S / m, about 10S / m to about 30S / m, about 10S / m to about 40S / m, about 10S / m to about 50S / m, about 10S / m to about 60S / m, about 20S / m to about 30S / m, about 20S / m to about 40S / m, about There are electrical conductivities of 20 S / m to about 50 S / m, about 20 S / m to about 60 S / m, about 30 S / m to about 40 S / m, about 30 S / m to about 50 S / m, about 30 S / m to about 60 S / m, about 40 S / m to about 50 S / m, about 40 S / m to about 60 S / m, and about 50 S / m to about 60 S / m.In some embodiments, the conductive carbon-based adhesive has a conductivity of about 0.15 S / m, about 0.3 S / m, about 0.5 S / m, about 1 S / m, about 2 S / m, about 5 S / m, about 10 S / m, about 20 S / m, about 30 S / m, about 40 S / m, about 50 S / m, or about 60 S / m. In some embodiments, the conductive carbon-based adhesive has a conductivity of at least about 0.15 S / m, about 0.3 S / m, about 0.5 S / m, about 1 S / m, about 2 S / m, about 5 S / m, about 10 S / m, about 20 S / m, about 30 S / m, about 40 S / m, about 50 S / m, or about 60 S / m. In some embodiments, the conductive carbon based adhesive has a conductivity of at most about 0.15 S / m, about 0.3 S / m, about 0.5 S / m, about 1 S / m, about 2 S / m, about 5 S / m, about 10 S / m, about 20 S / m, about 30 S / m, about 40 S / m, about 50 S / m, or about 60 S / m.

[0042] In some embodiments, the conductive carbon adhesive has a sheet resistance difference of up to about 6%, 5%, 4%, 3%, 2%, or 1% between a flat position and a position with a convex bend angle of up to 180 degrees. In some embodiments, the conductive carbon adhesive has a sheet resistance difference of up to about 6%, 5%, 4%, 3%, 2%, or 1% between a flat position and a position with a concave bend angle of up to 180 degrees. In some embodiments, the conductive carbon adhesive has a sheet resistance difference of up to about 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, or 2% between a flat position and a position with a twist angle of up to 800 degrees.

[0043] In some embodiments, the conductive carbon based adhesive has a strength of at least about 20 MPa, a, 10 MPa, or 5 MPa. In some embodiments, the conductive carbon-based adhesive has a shear strength of at least about 10 MPa.

[0044] In some embodiments, the conductive carbon-based adhesive has a tensile strength of at least about 30 MPa, 25 MPa, 20 MPa, 10 MPa, or 5 MPa. In some embodiments, the conductive carbon-based adhesive has a tensile strength of at least about 20 MPa.

[0045] In some embodiments, the viscosity of the conductive adhesive is from about 10 centipoise to about 10,000 centipoise. In some embodiments, the viscosity of the conductive adhesive is at least about 10 centipoise. In some embodiments, the viscosity of the conductive adhesive is at most about 10,000 centipoise. In some embodiments, the viscosity of the conductive adhesive is from about 10 centipoise to about 20 centipoise, from about 10 centipoise to about 50 centipoise, from about 10 centipoise to about 100 centipoise, from about 10 centipoise to about 200 centipoise, from about 10 centipoise to about 500 centipoise, from about 10 centipoise to about 1,000 centipoise, from about 10 centipoise to about 2,000 centipoise, from about 10 centipoise to about 5,000 centipoise, from about 10 centipoise to about 10,000 Centipoise, about 20 centipoise to about 50 centipoise, about 20 centipoise to about 100 centipoise, about 20 centipoise to about 200 centipoise, about 20 centipoise to about 500 centipoise, about 20 centipoise to about 1,000 centipoise, about 20 centipoise to about 2,000 centipoise, about 20 centipoise to about 5,000 centipoise, about 20 centipoise to about 10,000 centipoise, about 50 centipoise to about 100 centipoise, about 50 centipoise ~ about 200 centipoise, about 50 centipoise to about 500 centipoise, about 50 centipoise to about 1,000 centipoise, about 50 centipoise to about 2,000 centipoise, about 50 centipoise to about 5,000 centipoise, about 50 centipoise to about 10,000 centipoise, about 100 centipoise to about 200 centipoise, about 100 centipoise to about 500 centipoise, about 100 centipoise to about 1,000 centipoise, about 100 centipoise to about 2,000 centipoise, about 100 centipoise to about 5,000 centipoise, about 100 centipoise to about 10,000 centipoise, about 200 centipoise to about 500 centipoise, about 200 centipoise to about 1,000 centipoise, about 200 centipoise to about 2,000 centipoise, about 200 centipoise to about 5,000 centipoise, about 200 centipoise to about 10,000 centipoise, about 500 centipoise to about 1,000 centipoise, about 500 centipoise to about 2,000 centipoise, about 500 centipoise to about 5,000 centipoise, about 500 centipoise to about 10,000 centipoise, about 1,000 centipoise to about 2,000 centipoise, about 1,000 centipoise to about 5,000 centipoise, about 1,000 centipoise to about 10,000 centipoise, about 2,000 centipoise to about 5,000 centipoise, about 2,000 centipoise to about 10,000 centipoise, or about 5,000 centipoise to about 10,000 centipoise. In some embodiments, the viscosity of the conductive adhesive is about 10 centipoise, about 20 centipoise, about 50 centipoise, about 100 centipoise, about 200 centipoise, about 500 centipoise, about 1,000 centipoise, about 2,000 centipoise, about 5,000 centipoise, or about 10,000 centipoise. In some embodiments, the viscosity of the conductive adhesive is at least about 10 centipoise, about 20 centipoise, about 50 centipoise, about 100 centipoise, about 200 centipoise, about 500 centipoise, about 1,000 centipoise, about 2,000 centipoise, about 5,000 centipoise, or about 10,000 centipoise. In some embodiments, the viscosity of the conductive adhesive is about 10 centipoise, about 20 centipoise, about 50 centipoise, about 100 centipoise, about 200 centipoise, about 500 centipoise, about 1,000 centipoise, about 2,000 centipoise, about 5,000 centipoise, or about 10,000 centipoise or less.

[0046] In some embodiments, the conductive carbon-based adhesive further comprises a pigment, a colorant, a dye, or any combination thereof. In some embodiments, the conductive carbon-based adhesive comprises at least one, at least two, at least three, at least four, or at least five colorants, dyes, pigments, or combinations thereof. In some embodiments, the pigment comprises a metal-based or metallic pigment. In some embodiments, the metallic pigment is a gold, silver, titanium, aluminum, tin, zinc, mercury, manganese, lead, iron, iron oxide, copper, cobalt, cadmium, chromium, arsenic, bismuth, antimony, or barium pigment. In some embodiments, the colorant comprises at least one metallic pigment. In some embodiments, the colorant comprises a silver metallic colorant. In some embodiments, the silver metallic colorant comprises silver nanoparticles, silver nanorods, silver nanowires, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or combinations thereof.

[0047] In some embodiments, the colorant is selected from pigments and / or dyes that are red, yellow, magenta, green, cyan, purple, black, or brown, or combinations thereof. In some embodiments, the pigment is blue, brown, cyan, green, purple, magenta, red, yellow, or combinations thereof. In some embodiments, the dye is blue, brown, cyan, green, purple, magenta, red, yellow, or combinations thereof.

[0048] In some embodiments, the yellow colorant is Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 65, 74, 83, 93, 110, 128, 151, 155, or any combination thereof. In some embodiments, the black colorant includes Color Black SI70, Color Black SI50, Color Black FW1, Color Black FW18, Acid Black 1, 11, 52, 172, 194, 210, 234, or combinations thereof. In some embodiments, the red or magenta colorant includes Pigment Red 1-10, 12, 18, 21, 23, 37, 38, 39, 40, 41, 48, 90, 112, or combinations thereof. , 122, or a combination thereof. In some embodiments, cyan or purple The colorants include Pigment Blue 15, 17, 22, Pigment Violet 1, 2, 3, 5, 19, 23, or combinations thereof. In some embodiments, the orange colorant includes Pigment Orange 48 and / or 49. In some embodiments, the purple colorant includes Pigment Violet 19 and / or 42.

[0049] Another aspect provided herein is a conductive carbon-based epoxy that includes a resin that includes a carbon-based material, an adhesive, and a hardener.

[0050] In some embodiments, the carbon-based material is graphene, graphite powder, natural graphite, synthetic graphite, expanded graphite, carbon black, Timcal carbon super C45, Timcal carbon super C65, cabot carbon, carbon super P, acetylene black, furne The nanofibers may include, for example, graphene black, carbon nanotubes, vapor grown carbon fibers, graphene oxide, or any combination thereof.

[0051] In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is between about 0.1% and about 10%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is at least about 0.1%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is at most about 10%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is between about 0.1% and about 0.2%, between about 0.1% and about 0.5%, between about 0.1% and about 1%, between about 0.1% and about 2%, between about 0.1% and about 3%, between about 0.1% and about 4%, between about 0.1% and about 5%, between about 0.1% and about 6%, between about 0.1% and about 7%, between about 0.1% and about 8%, between about 0.1% and about 10%, between about 0.2% and about 0.5 ... ~ about 1%, about 0.2% to about 2%, about 0.2% to about 3%, about 0.2% to about 4%, about 0.2% to about 5%, about 0.2% to about 6%, about 0.2% to about 7%, about 0.2% to about 8%, about 0.2% to about 10%, about 0.5% to about 1%, about 0.5% to about 2%, about 0.5% to about 3%, about 0.5% to about 4%, about 0.5% to about 5%, about 0.5% to about 6%, about 0.5% to about 7%, about 0.5% to about 8%, about 0.5% to about 10%, about 1% to about 2%, about 1% to about 3%, about 1% to about 4%, about 1% to about 5%, about 1% to about 6%, about 1% to about 7%, about 1% to about 8%, about 1% to about 1 0%, about 2% to about 3%, about 2% to about 4%, about 2% to about 5%, about 2% to about 6%, about 2% to about 7%, about 2% to about 8%, about 2% to about 10%, about 3% to about 4%, about 3% to about 5%, about 3% to about 6%, about 3% to about 7%, about 3% to about 8%, about 3% to about 10%, about 4% to about 5%, about 4% to about 6%, about 4% to about 7%, about 4% to about 8%, about 4% to about 10%, about 5% to about 6%, about 5% to about 7%, about 5% to about 8%, about 5% to about 10%, about 6% to about 7%, about 6% to about 8%, about 6% to about 10%, about 7% to about 8%, about 7% to about 10%, or about 8% to about 10%. In some embodiments, the carbon-based material comprises graphene and the weight percentage of graphene in the carbon-based material is about 0.1%, about 0.2%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 10%. In some embodiments, the carbon-based material comprises graphene and the weight percentage of graphene in the carbon-based material is at least about 0.1%, about 0.2%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 10%. In some embodiments, the carbon-based material comprises graphene and the weight percentage of graphene in the carbon-based material is at most about 0.1%, about 0.2%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 10%.

[0052] In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is between about 1% and about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at least about 1%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at most about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is about 1% to about 2%, about 1% to about 5%, about 1% to about 10%, about 1% to about 15%, about 1% to about 20%, about 1% to about 25%, about 1% to about 30%, about 1% to about 35%, about 1% to about 40%, about 2% to about 5%, about 2% to about 10%, about 2% to about 15%, about 2% to about 20%, about 2% to about 25%, about 2% to about 30%, about 2% to about 35%, about 2% to about 40%, about 5% to about 10%, about 5% to about 15%, about 5% to about 20%, about 5% to about 25%, about 5% to about 30%, about 35 ... 0%, about 5% to about 35%, about 5% to about 40%, about 10% to about 15%, about 10% to about 20%, about 10% to about 25%, about 10% to about 30%, about 10% to about 35%, about 10% to about 40%, about 15% to about 20%, about 15% to about 25%, about 15% to about 30%, about 15% to about 35%, about 15% to about 40%, about 20% to about 25%, about 20% to about 30%, about 20% to about 35%, about 20% to about 40%, about 25% to about 30%, about 25% to about 35%, about 25% to about 40%, about 30% to about 35%, about 30% to about 40%, or about 35% to about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is about 1%, about 2%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at least about 1%, about 2%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at most about 1%, about 2%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%.

[0053] In some embodiments, the adhesive is a carpenter's glue, wood glue, cyanoacrylate, contact cement, latex, library paste, rubber Methyl cellulose, resorcinol resin, starch, butanone, dichloromethane acrylate The curing agent may be selected from the group consisting of ethylene vinyl, phenol formaldehyde resin, polyamide, polyester, polyethylene, polypropylene, polysulfide, polyurethane, polyvinyl acetate, aliphatic, polyvinyl alcohol, polyvinyl chloride, polyvinyl chloride emulsion, silicone, styrene acrylic, epichlorohydrin, epoxide, or any combination thereof. In some embodiments, the curing agent may be selected from the group consisting of bisphenol A, bisphenol F, novolac, aliphatic alcohol, aliphatic polyol, glycidyl amine, triethylenetriamine, or any combination thereof. In some embodiments, the conductive carbon-based adhesive further comprises a conductive filler. In some embodiments, the conductive filler comprises silver. In some embodiments, the silver comprises silver nanoparticles, silver nanorods, silver nanowires, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or any combination thereof. In some embodiments, the conductive carbon-based adhesive further comprises a thinner. In some embodiments, the thinner comprises butyl acetate, lacquer thinner, acetone, petroleum naphtha, mineral spirits, xylene, or any combination thereof.

[0054] In some embodiments, the volume percentage of the thinner in the conductive carbon-based epoxy is about 50% to about 99%. In some embodiments, the volume percentage of the thinner is at least about 50%. In some embodiments, the volume percentage of the thinner is up to about 99%. In some embodiments, the volume percentage of the thinner is about 50% to about 55%, about 50% to about 60%, about 50% to about 65%, about 50% to about 70%, about 50% to about 75%, about 50% to about 80%, about 50% to about 85%, about 50% to about 90%, about 50% to about 95%, about 50% to about 99%, about 55% to about 60%, about 55% to about 65%, about 55% to about 70%, about 55% to about 75%, about 55% to about 80%, about 55% to about 85%, about 55% to about 90%, about 55% to about 95%, about 55% to about 99%, about 60% to about 65%, about 60% to about 70%, about 60% to about 75%, about 60% to about 80%, about 60% to about 85%, about 60% to about 90%, about 60% to about 95%, about 60% to about 99%, about 65% to about 70%, about 65% to about 75%, about 65% to about 80%, about 65% to about 85%, about 65% to about 90%, about 65% to about 95%, about 65% to about 99%, about 70% to about 75%, about 70% to about 80%, about 70% to about 85%, about 70% to about 90%, about 70% to about 95%, about 70% to about 99%, about 75% to about 80%, about 75% to about 85%, about 75% to about 90%, about 75% to about 95%, about 75% to about 99%, about 80% to about 85%, about 80% to about 90%, about 80% to about 95%, about 80% to about 99%, about 85% to about 90%, about 85% to about 95%, about 85% to about 99%, about 90% to about 95%, about 90% to about 99%, or about 95% to about 99%. In some embodiments, the volume percentage of the thinner is about 50%, about 55%, about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, or about 99%. In some embodiments, the volume percentage of the thinner is at least about 50%, about 55%, about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, or about 99%. In some embodiments, the volume percentage of the thinner is at most about 50%, about 55%, about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, or about 99%.

[0055] In some embodiments, the weight percentage of the resin in the conductive carbon-based epoxy is between about 25% and about 75%. In some embodiments, the weight percentage of the resin in the conductive carbon-based epoxy is at least about 25%. In some embodiments, the weight percentage of the resin in the conductive carbon-based epoxy is up to about 75%. In some embodiments, the weight percentage of the resin in the conductive carbon-based epoxy is about 25% to about 30%, about 25% to about 35%, about 25% to about 40%, about 25% to about 45%, about 25% to about 50%, about 25% to about 55%, about 25% to about 60%, about 25% to about 65%, about 25% to about 70%, about 25% to about 75%, about 30% to about 35%, about 30% to about 40%, about 30% to about 45%, about 30% to about 50%, about 30% to about 55%, about 30% to about 60%, about 30% to about 65%, about 30% to about 70%, about 30% to about 75%, about 35% to about 40%, about 35% to about 45%, about 35% to about 50%, about 35% to about 55%, about 35% to about 60%, about 35% to about 65%, about 35% to about 70%, about 35% to about 75%, about 40% to about 45%, about 40% to about 50%, about 40% to about 55%, about 40% to about 60%, about 40% to about 65%, about 40% to about 70%, about 40% to about 75%, about 45% to about 50%, about 45% to about 55%, about 45% to about 60%, about 45% to about 65%, about 45% to about 70%, about 45% to about 75%, about 50% to about 55%, about 50% to about 60%, about 50% to about 65%, about 50% to about 70%, about 50% to about 75%, about 55% to about 60%, about 55% to about 65%, about 55% to about 70%, about 55% to about 75%, about 60% to about 65%, about 60% to about 70%, about 60% to about 75%, about 65% to about 70%, about 65% to about 75%, or about 70% to about 75%. In some embodiments, the weight percentage of the resin in the conductive carbon-based epoxy is about 25%, about 30%, about 35%, about 40%, about 45%, about 50%, about 55%, about 60%, about 65%, about 70%, or about 75%. In some embodiments, the weight percentage of the resin in the conductive carbon-based epoxy is at least about 25%, about 30%, about 35%, about 40%, about 45%, about 50%, about 55%, about 60%, about 65%, about 70%, or about 75%. In some embodiments, the weight percentage of the resin in the conductive carbon-based epoxy is at most about 25%, about 30%, about 35%, about 40%, about 45%, about 50%, about 55%, about 60%, about 65%, about 70%, or about 75%.

[0056] In some embodiments, the resin comprises about 60% to about 99% by weight of the carbon-based material. In some embodiments, the resin comprises at least about 60% by weight of the carbon-based material. In some embodiments, the resin comprises up to about 99% by weight of the carbon-based material. In some embodiments, the resin comprises about 60% to about 65%, about 60% to about 70%, about 60% to about 75%, about 60% to about 80%, about 60% to about 85%, about 60% to about 90%, about 60% to about 95%, about 60% to about 96%, about 60% to about 97%, about 60% to about 98%, about 60% to about 99%, about 65% to about 70%, about 65% to about 75%, about 65% to about 80%, about 65% to about 85%, about 65% to about 90%, about 65% to about 95%, about 65% to about 96%, about 65% to about 97%, about 65% to about 98%, about 65% to about 99%, about 70% to about 75%, about 70% to about 80%, about 70% to about 85%, about 70% to about 90%, about 70% to about 95%, about 70% to about 96%, about 70% to about 97%, about 70% to about 98%, about 70% to about 99%, about 75% to about 80%, about 75% to about 85%, about 75% to About 90%, about 75% to about 95%, about 75% to about 96%, about 75% to about 97%, about 75% to about 98%, about 75% to about 99%, about 80% to about 85%, about 80% to about 90%, about 80% to about 95%, about 80% to about 96%, about 80% to about 97%, about 80% to about 98%, about 80% to about 99%, about 85% to about 90%, about 85% to about 95%, about 85% to about 96%, about 85% to about 97%, about 85% to about 98 %, about 85% to about 99%, about 90% to about 95%, about 90% to about 96%, about 90% to about 97%, about 90% to about 98%, about 90% to about 99%, about 95% to about 96%, about 95% to about 97%, about 95% to about 98%, about 95% to about 99%, about 96% to about 97%, about 96% to about 98%, about 96% to about 99%, about 97% to about 98%, about 97% to about 99%, or about 98% to about 99% carbon-based material. In some embodiments, the resin comprises about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 96%, about 97%, about 98%, or about 99% carbon-based material by weight.In some embodiments, the resin comprises at least about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 96%, about 97%, about 98%, or about 99% by weight of carbon-based material. In some embodiments, the resin comprises up to about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 96%, about 97%, about 98%, or about 99% by weight of carbon-based material.

[0057] In some embodiments, the conductive carbon-based epoxy is configured to cure at room temperature. In some embodiments, the conductive carbon-based epoxy has a cure time at room temperature of about 12 hours to about 48 hours. In some embodiments, the conductive carbon-based epoxy has a cure time at room temperature of at least about 12 hours to about 48 hours. In some embodiments, the conductive carbon-based epoxy has a cure time of up to about 48 hours at room temperature. In some embodiments, the conductive carbon-based epoxy is cured at room temperature for about 12 hours to about 16 hours, about 12 hours to about 20 hours, about 12 hours to about 24 hours, about 12 hours to about 28 hours, about 12 hours to about 32 hours, about 12 hours to about 36 hours, about 12 hours to about 40 hours, about 12 hours to about 44 hours, about 12 hours to about 48 hours, about 16 hours to about 20 hours, about 16 hours to about 24 hours, about 16 hours to about 28 hours, about 16 hours to about 32 hours, about 16 hours to about 36 hours, about 16 hours to about 40 hours, about 16 hours to about 44 hours, about 16 hours to about 48 hours, about 20 hours to about 24 hours, about 20 hours to about 28 hours, about 20 hours to about 32 hours, about 20 hours to about 36 hours, or about 20 hours to about 40 hours. the curing time is about 20 hours to about 44 hours, about 20 hours to about 48 hours, about 24 hours to about 28 hours, about 24 hours to about 32 hours, about 24 hours to about 36 hours, about 24 hours to about 40 hours, about 24 hours to about 44 hours, about 24 hours to about 48 hours, about 28 hours to about 32 hours, about 28 hours to about 36 hours, about 28 hours to about 40 hours, about 28 hours to about 44 hours, about 28 hours to about 48 hours, about 32 hours to about 36 hours, about 32 hours to about 40 hours, about 32 hours to about 44 hours, about 32 hours to about 48 hours, about 36 hours to about 40 hours, about 36 hours to about 44 hours, about 36 hours to about 48 hours, about 40 hours to about 44 hours, about 40 hours to about 48 hours, or about 44 hours to about 48 hours. In some embodiments, the conductive carbon-based epoxy has a cure time of about 12 hours, about 16 hours, about 20 hours, about 24 hours, about 28 hours, about 32 hours, about 36 hours, about 40 hours, about 44 hours, or about 48 hours at room temperature. In some embodiments, the conductive carbon-based epoxy has a cure time of at least about 12 hours, about 16 hours, about 20 hours, about 24 hours, about 28 hours, about 32 hours, about 36 hours, about 40 hours, about 44 hours, or about 48 hours at room temperature. In some embodiments, the conductive carbon-based epoxy has a cure time of up to about 12 hours, about 16 hours, about 20 hours, about 24 hours, about 28 hours, about 32 hours, about 36 hours, about 40 hours, about 44 hours, or about 48 hours at room temperature.

[0058] In some embodiments, the conductive carbon-based epoxy has a cure time of about 10 minutes to about 40 minutes at a temperature of 65° C. In some embodiments, the conductive carbon-based epoxy has a cure time of at least about 10 minutes at a temperature of 65° C. In some embodiments, the conductive carbon-based epoxy has a cure time of up to about 40 minutes at a temperature of 65° C. In some embodiments, the conductive carbon-based epoxy has a cure time at a temperature of 65° C. of about 10 minutes to about 15 minutes, about 10 minutes to about 20 minutes, about 10 minutes to about 25 minutes, about 10 minutes to about 30 minutes, about 10 minutes to about 35 minutes, about 10 minutes to about 40 minutes, about 15 minutes to about 20 minutes, about 15 minutes to about 25 minutes, about 15 minutes to about 30 minutes, about 15 minutes to about 35 minutes, about 15 minutes to about 40 minutes, about 20 minutes to about 25 minutes, about 20 minutes to about 30 minutes, about 20 minutes to about 35 minutes, about 20 minutes to about 40 minutes, about 25 minutes to about 30 minutes, about 25 minutes to about 35 minutes, about 25 minutes to about 40 minutes, about 30 minutes to about 35 minutes, about 30 minutes to about 40 minutes, or about 35 minutes to about 40 minutes. In some embodiments, the conductive carbon-based epoxy has a cure time of about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, or about 40 minutes at a temperature of 65° C. In some embodiments, the conductive carbon-based epoxy has a cure time of at least about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, or about 40 minutes at a temperature of 65° C. In some embodiments, the conductive carbon-based epoxy has a cure time of up to about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, or about 40 minutes at a temperature of 65° C.

[0059] In some embodiments, the conductive carbon-based epoxy has a working time of about 10 minutes to about 40 minutes. In some embodiments, the conductive carbon-based epoxy has a working time of at least about 10 minutes. In some embodiments, the conductive carbon-based epoxy has a working time of up to about 40 minutes. In some embodiments, the conductive carbon-based epoxy has a working time of about 10 minutes to about 15 minutes, about 10 minutes to about 20 minutes, about 10 minutes to about 25 minutes, about 10 minutes to about 30 minutes, about 10 minutes to about 35 minutes, about 10 minutes to about 40 minutes, about 15 minutes to about 20 minutes, about 15 minutes to about 25 minutes, about 15 minutes to about 30 minutes, about 15 minutes to about 35 minutes, about 15 minutes to about 40 minutes, about 20 minutes to about 25 minutes, about 20 minutes to about 30 minutes. The conductive carbon-based epoxy has a working time of about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, about 30 minutes, about 40 minutes, about 25 minutes, about 30 minutes, about 40 minutes, about 35 minutes, about 30 minutes, about 40 minutes, or about 35 minutes to about 40 minutes. In some embodiments, the conductive carbon-based epoxy has a working time of about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, or about 40 minutes. In some embodiments, the conductive carbon-based epoxy has a working time of at least about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, or about 40 minutes. In some embodiments, the conductive carbon-based epoxy has a working time of at most about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, or about 40 minutes.

[0060] In some embodiments, the conductive carbon-based epoxy has a sheet resistance of about 50 ohms / sq to about 300 ohms / sq. In some embodiments, the conductive carbon-based epoxy has a sheet resistance of at least about 50 ohms / sq. In some embodiments, the conductive carbon-based epoxy has a sheet resistance of up to about 300 ohms / sq. In some embodiments, the conductive carbon based epoxy has a ohm / sq to about 75 ohm / sq, about 50 ohm / sq to about 100 ohm / sq, about 50 ohm / sq to about 125 ohm / sq, about 50 ohm / sq to about 150 ohm / sq, about 50 ohm / sq to about 175 ohm / sq, about 50 ohm / sq to about 200 ohm / sq, about 50 ohm / sq to about 225 ohm / sq, about 50 ohm / sq to about 250 ohm / sq, about 50 ohm / sq to about 275 ohm / sq. q, about 50 ohms / sq to about 300 ohms / sq, about 75 ohms / sq to about 100 ohms / sq, about 75 ohms / sq to about 125 ohms / sq, about 75 ohms / sq to about 150 ohms / sq, about 75 ohms / sq to about 175 ohms / sq, about 75 ohms / sq to about 200 ohms / sq, about 75 ohms / sq to about 225 ohms / sq, about 75 ohms / sq to about 250 ohms / sq, about 75 ohms / sq to about 275 ohms / sq, about 75 ohms / sq to about 300 ohms / sq q, about 100 ohms / sq to about 125 ohms / sq, about 100 ohms / sq to about 150 ohms / sq, about 100 ohms / sq to about 175 ohms / sq, about 100 ohms / sq to about 200 ohms / sq, about 100 ohms / sq to about 225 ohms / sq, about 100 ohms / sq to about 250 ohms / sq, about 100 ohms / sq to about 275 ohms / sq, about 100 ohms / sq to about 300 ohms / sq, about 125 ohms / sq to about 150 ohms / sq, about 125 ohms / sq ~175 ohms / sq, ~125 ohms / sq~200 ohms / sq, ~125 ohms / sq~225 ohms / sq, ~125 ohms / sq~250 ohms / sq, ~125 ohms / sq~275 ohms / sq, ~125 ohms / sq~300 ohms / sq, ~150 ohms / sq~175 ohms / sq, ~150 ohms / sq~200 ohms / sq, ~150 ohms / sq~225 ohms / sq, ~150 ohms / sq~250 ohms / sq,Approximately 150 ohms / sq to approximately 275 ohms / sq, approximately 150 ohms / sq to approximately 300 ohms / sq, approximately 175 ohms / sq to approximately 200 ohms / sq, approximately 175 ohms / sq to approximately 225 ohms / sq, approximately 175 ohms / sq to approximately 250 ohms / sq, approximately 175 ohms / sq to approximately 275 ohms / sq, approximately 175 ohms / sq to approximately 300 ohms / sq, approximately 200 ohms / sq to approximately 225 ohms / sq, approximately 200 ohms / sq to approximately 250 ohms / sq In one embodiment, the sheet resistance is about 200 ohms / sq to about 275 ohms / sq, about 200 ohms / sq to about 300 ohms / sq, about 225 ohms / sq to about 250 ohms / sq, about 225 ohms / sq to about 275 ohms / sq, about 225 ohms / sq to about 300 ohms / sq, about 250 ohms / sq to about 275 ohms / sq, about 250 ohms / sq to about 300 ohms / sq, or about 275 ohms / sq to about 300 ohms / sq. In some embodiments, the conductive carbon-based epoxy has a sheet resistance of about 50 ohms / sq, about 75 ohms / sq, about 100 ohms / sq, about 125 ohms / sq, about 150 ohms / sq, about 175 ohms / sq, about 200 ohms / sq, about 225 ohms / sq, about 250 ohms / sq, about 275 ohms / sq, or about 300 ohms / sq. In some embodiments, the conductive carbon-based epoxy has a sheet resistance of at least about 50 ohms / sq, about 75 ohms / sq, about 100 ohms / sq, about 125 ohms / sq, about 150 ohms / sq, about 175 ohms / sq, about 200 ohms / sq, about 300 ohms / sq. In some embodiments, the conductive carbon-based epoxy has a sheet resistance of at most about 50 ohms / sq, about 75 ohms / sq, about 100 ohms / sq, about 125 ohms / sq, about 150 ohms / sq, about 175 ohms / sq, about 200 ohms / sq, about 225 ohms / sq, about 300 ohms / sq, about 400 ohms / sq, about 50 ohms / sq, about 75 ohms / sq, about 100 ohms / sq, about 125 ohms / sq, about 150 ohms / sq, about 175 ohms / sq, about 200 ohms / sq, about 225 ohms / sq, about 300 ohms / sq, about 400 ohms / sq, about 50 ohms / sq, about 60 ohms / sq, about 75 ohms / sq, about 80 ohms / sq, about 90 ... 250 ohms / sq, 275 ohms / sq, or 300 ohms / sq. It has a resistance.

[0061] In some embodiments, the conductive carbon-based epoxy has a sheet resistance of about 0.3 ohms / sq / mil to about 2 ohms / sq / mil. In some embodiments, the conductive carbon-based epoxy has a sheet resistance of at least about 0.3 ohms / sq / mil. In some embodiments, the conductive carbon-based epoxy has a sheet resistance of up to about 2 ohms / sq / mil. In some embodiments, the conductive carbon based epoxy is between about 0.3 ohms / sq / mil and about 0.6 ohms / sq / mil, between about 0.3 ohms / sq / mil and about 0.8 ohms / sq / mil, between about 0.3 ohms / sq / mil and about 1 ohm / sq / mil, between about 0.3 ohms / sq / mil and about 1.2 ohms / sq / mil, between about 0.3 ohms / sq / mil and about 1.4 ohms / sq / mil, between about 0.3 ohms / sq / mil and about 1.6 ohms / sq / mil, between about 0.3 ohms / sq / mil and about 0.3 ohms / sq / mil. ~ about 1.8 ohms / sq / mil, about 0.3 ohms / sq / mil to about 2 ohms / sq / mil, about 0.6 ohms / sq / mil to about 0.8 ohms / sq / mil, about 0.6 ohms / sq / mil to about 1 ohm / sq / mil, about 0.6 ohms / sq / mil to about 1.2 ohms / sq / mil, about 0.6 ohms / sq / mil to about 1.4 ohms / sq / mil, about 0.6 ohms / sq / mil to about 1.6 ohms / sq / mil, about 0.6 ohms / sq / mil to about 1.8 ohms / sq / mil mils, about 0.6 ohms / sq / mil to about 2 ohms / sq / mils, about 0.8 ohms / sq / mil to about 1 ohm / sq / mils, about 0.8 ohms / sq / mil to about 1.2 ohms / sq / mils, about 0.8 ohms / sq / mil to about 1.4 ohms / sq / mils, about 0.8 ohms / sq / mil to about 1.6 ohms / sq / mils, about 0.8 ohms / sq / mil to about 1.8 ohms / sq / mils, about 0.8 ohms / sq / mil to about 2 ohms / sq / mils, about 1 ohm / sq / mil ~1.2 ohms / sq / mil, ~1 ohm / sq / mil ~1.4 ohms / sq / mil, ~1 ohm / sq / mil ~1.6 ohms / sq / mil, ~1 ohm / sq / mil ~1.8 ohms / sq / mil, ~1 ohm / sq / mil ~2 ohms / sq / mil, ~1.2 ohms / sq / mil ~1.4 ohms / sq / mil, ~1.2 ohms / sq / mil ~1.6 ohms / sq / mil, ~1.2 ohms / sq / mil ~1.8 ohms / sq / mil, ~1.having a sheet resistance of 2 ohms / sq / mil to about 2 ohms / sq / mil, about 1.4 ohms / sq / mil to about 1.6 ohms / sq / mil, about 1.4 ohms / sq / mil to about 1.8 ohms / sq / mil, about 1.4 ohms / sq / mil to about 2 ohms / sq / mil, about 1.6 ohms / sq / mil to about 1.8 ohms / sq / mil, about 1.6 ohms / sq / mil to about 2 ohms / sq / mil, or about 1.8 ohms / sq / mil to about 2 ohms / sq / mil. In some embodiments, the conductive carbon-based epoxy has a sheet resistance of about 0.3 ohms / sq / mil, about 0.6 ohms / sq / mil, about 0.8 ohms / sq / mil, about 1 ohm / sq / mil, about 1.2 ohms / sq / mil, about 1.4 ohms / sq / mil, about 1.6 ohms / sq / mil, about 1.8 ohms / sq / mil, or about 2 ohms / sq / mil. In some embodiments, the conductive carbon-based epoxy has a sheet resistance of at least about 0.3 ohms / sq / mil, about 0.6 ohms / sq / mil, about 0.8 ohms / sq / mil, about 1 ohm / sq / mil, about 1.2 ohms / sq / mil, about 1.4 ohms / sq / mil, about 1.6 ohms / sq / mil, about 1.8 ohms / sq / mil, or about 2 ohms / sq / mil. In some embodiments, the conductive carbon-based epoxy has a sheet resistance of at most about 0.3 ohms / sq / mil, about 0.6 ohms / sq / mil, about 0.8 ohms / sq / mil, about 1 ohm / sq / mil, about 1.2 ohms / sq / mil, about 1.4 ohms / sq / mil, about 1.6 ohms / sq / mil, about 1.8 ohms / sq / mil, or about 2 ohms / sq / mil.

[0062] In some embodiments, the conductive carbon-based epoxy has a conductivity of about 0.15 S / m to about 60 S / m. In some embodiments, the conductive carbon-based epoxy has a conductivity of at least about 0.15 S / m. In some embodiments, the conductive carbon-based epoxy has a conductivity of up to about 60 S / m.The actual application form is that the conductive carbon-based products are about 0.15S / m to about 0.3S / m, about 0.15S / m to about 0.5S / m, about 0.15S / m to about 1S / m, about 0.15S / m to about 2S / m, about 0.15S / m to about 5S / m, about 0.15S / m to about 10S / m, about 0 .15S / m~about 20S / m, about 0.15S / m~about 30S / m, about 0.15S / m~about 40S / m, about 0.15S / m~about 50S / m, about 0.15S / m~about 60S / m, about 0.3S / m~about 0.5S / m, about 0.3S / m~about 1S / m, about 0.3S / m~about 2S / m , about 0.3S / m to about 5S / m, about 0.3S / m to about 10S / m, about 0.3S / m to about 20S / m, about 0.3S / m to about 30S / m, about 0.3S / m to about 40S / m, about 0.3S / m to about 50S / m, about 0.3S / m to about 60S / m, about 0.5S / m to about 1S / m, about 0.5S / m to about 2S / m, about 0.5S / m to about 5S / m, about 0.5S / m to about 10S / m, about 0.5S / m to about 20S / m, about 0.5S / m to about 30S / m, about 0.5S / m to about 40S / m, about 0.5S / m to about 50S / m, about 0.5S / m to about 60S / m, about 1S / m to about 2S / m, about 1S / m to about 5S / m, about 1S / m to about 10S / m, about 1S / m to about 20S / m, about 1S / m to about 30S / m, about 1S / m to about 40S / m, about 1S / m to about 50S / m, about 1S / m to about 60S / m, about 2S / m to about 5S / m, about 2S / m to about 10S / m, about 2S / m to about 20S / m, about 2S / m to about 30S / m, about 2S / m to about 40S / m, about 2S / m to about 50S / m, about 2S / m to about 60S / m, about 5S / m to about 10S / m, about 5S / m to about 20S / m, about 5S / m to about 30S / m, about 5S / m to about 40S / m, about 5S / m to about 50S / m m to about 50S / m, about 5S / m to about 60S / m, about 10S / m to about 20S / m, about 10S / m to about 30S / m, about 10S / m to about 40S / m, about 10S / m to about 50S / m, about 10S / m to about 60S / m, about 20S / m to about 30S / m, about 20S / m to about 40S / m, about There are electrical conductivities of 20 S / m to about 50 S / m, about 20 S / m to about 60 S / m, about 30 S / m to about 40 S / m, about 30 S / m to about 50 S / m, about 30 S / m to about 60 S / m, about 40 S / m to about 50 S / m, about 40 S / m to about 60 S / m, and about 50 S / m to about 60 S / m.In some embodiments, the conductive carbon-based epoxy has a conductivity of about 0.15 S / m, about 0.3 S / m, about 0.5 S / m, about 1 S / m, about 2 S / m, about 5 S / m, about 10 S / m, about 20 S / m, about 30 S / m, about 40 S / m, about 50 S / m, or about 60 S / m. In some embodiments, the conductive carbon-based epoxy has a conductivity of at least about 0.15 S / m, about 0.3 S / m, about 0.5 S / m, about 1 S / m, about 2 S / m, about 5 S / m, about 10 S / m, about 20 S / m, about 30 S / m, about 40 S / m, about 50 S / m, or about 60 S / m. In some embodiments, the conductive carbon-based epoxy has a conductivity of up to about 0.15 S / m, about 0.3 S / m, about 0.5 S / m, about 1 S / m, about 2 S / m, about 5 S / m, about 10 S / m, about 20 S / m, about 30 S / m, about 40 S / m, about 50 S / m, or about 60 S / m.

[0063] In some embodiments, the conductive carbon-based epoxy has a sheet resistance that differs by at most about 0.5%, 0.4%, 0.3%, or 0.2% when the conductive carbon-based epoxy is bent at a convex angle of at most about 180°.

[0064] In some embodiments, the conductive carbon-based epoxy has a sheet resistance that differs by at most about 0.5%, 0.4%, 0.3%, 0.2%, 0.15%, or 0.1% when the conductive carbon-based epoxy is bent through a re-entrant angle of at most about 180°.

[0065] In some embodiments, the conductive carbon-based epoxy has a sheet resistance that differs by up to about 5%, 4%, 3%, 2%, or 1% when the conductive carbon-based epoxy is stretched at a strain of 20%.

[0066] In some embodiments, the conductive carbon-based epoxy has a sheet resistance that differs by up to about 20%, 17%, 15%, 12%, or 10% when the conductive carbon-based epoxy is stretched at 50% strain.

[0067] In some embodiments, the conductive carbon-based epoxy further comprises a pigment, a colorant, a dye, or any combination thereof. In some embodiments, the conductive carbon-based epoxy comprises at least one, at least two, at least three, at least four, or at least five colorants, dyes, pigments, or combinations thereof. In some embodiments, the pigment comprises a metal-based or metallic pigment. In some embodiments, the metallic pigment is a gold, silver, titanium, aluminum, tin, zinc, mercury, manganese, lead, iron, iron oxide, copper, cobalt, cadmium, chromium, arsenic, bismuth, antimony, or barium pigment. In some embodiments, the colorant comprises at least one metallic pigment. In some embodiments, the colorant comprises a silver metallic colorant. In some embodiments, the silver metallic colorant comprises silver nanoparticles, silver nanorods, silver nanowires, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or combinations thereof.

[0068] In some embodiments, the colorant is selected from pigments and / or dyes that are red, yellow, magenta, green, cyan, purple, black, or brown, or combinations thereof. In some embodiments, the pigment is blue, brown, cyan, green, purple, magenta, red, yellow, or combinations thereof. In some embodiments, the dye is blue, brown, cyan, green, purple, magenta, red, yellow, or combinations thereof.

[0069] In some embodiments, the yellow colorant is Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 65, 74, 83, 93, 110, 128, 151, 155, or any combination thereof. In some embodiments, the black colorant includes Color Black SI70, Color Black SI50, Color Black FW1, Color Black FW18, Acid Black 1, 11, 52, 172, 194, 210, 234, or combinations thereof. In some embodiments, the red or magenta colorant includes Pigment Red 1-10, 12, 18, 21, 23, 37, 38, 39, 40, 41, 48, 90, 112, or combinations thereof. , 122, or a combination thereof. In some embodiments, cyan or purple The colorants include Pigment Blue 15, 17, 22, Pigment Violet 1, 2, 3, 5, 19, 23, or combinations thereof. In some embodiments, the orange colorant includes Pigment Orange 48 and / or 49. In some embodiments, the purple colorant includes Pigment Violet 19 and / or 42.

[0070] Another aspect provided herein is a method of forming a conductive carbon-based adhesive that includes forming a carbon-based material and adding an adhesive to the carbon-based material.

[0071] In some embodiments, the carbon-based material is graphene, graphite powder, natural graphite, synthetic graphite, expanded graphite, carbon black, Timcal carbon super C45, Timcal carbon super C65, cabot carbon, carbon super P, acetylene black, furne The nanofibers may include, for example, graphene black, carbon nanotubes, vapor grown carbon fibers, graphene oxide, or any combination thereof.

[0072] In some embodiments, the carbon-based material comprises about 60% to about 99.9% adhesive by weight. In some embodiments, the carbon-based material comprises at least about 60% adhesive by weight. In some embodiments, the carbon-based material comprises up to about 99.9% adhesive by weight. In some embodiments, the carbon-based material comprises about 60% to about 65%, about 60% to about 70%, about 60% to about 75%, about 60% to about 80%, or about 60% to about 85% adhesive by weight. , about 60% to about 90%, about 60% to about 95%, about 60% to about 96%, about 60% to about 97%, about 60% to about 99%, about 60% to about 99.9%, about 65% to about 70%, about 65% to about 75%, about 65% to about 80%, about 65% to about 85%, about 65% to about 90%, about 65% to about 95%, about 65% to about 96%, about 65% to about 97%, about 65% to about 99%, about 65% to about 9 9.9%, about 70% to about 75%, about 70% to about 80%, about 70% to about 85%, about 70% to about 90%, about 70% to about 95%, about 70% to about 96%, about 70% to about 97%, about 70% to about 99%, about 70% to about 99.9%, about 75% to about 80%, about 75% to about 85%, about 75% to about 90%, about 75% to about 95%, about 75% to about 96%, about 75% to about 97%, about 75% ~ about 99%, about 75% to about 99.9%, about 80% to about 85%, about 80% to about 90%, about 80% to about 95%, about 80% to about 96%, about 80% to about 97%, about 80% to about 99%, about 80% to about 99.9%, about 85% to about 90%, about 85% to about 95%, about 85% to about 96%, about 85% to about 97%, about 85% to about 99%, about 85% to about 99.9%, about 90% to about 95% , about 90% to about 96%, about 90% to about 97%, about 90% to about 99%, about 90% to about 99.9%, about 95% to about 96%, about 95% to about 97%, about 95% to about 99%, about 95% to about 99.9%, about 96% to about 97%, about 96% to about 99%, about 96% to about 99.9%, about 97% to about 99%, about 97% to about 99.9%, or about 99% to about 99.9% adhesive. In some embodiments, the carbon-based material comprises about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 96%, about 97%, about 99%, or about 99.9% adhesive by weight. In some embodiments, the carbon-based material comprises at least about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 96%, about 97%, about 99%, or about 99.9% adhesive by weight. In some embodiments, the carbon-based material comprises at most about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 96%, about 97%, about 99%, or about 99.9% adhesive by weight.

[0073] In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is about 0.1% to about 10%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is at least about 0.1%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is at most about 10%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is about 0.1% to about 0.2%, about 0.1% to about 0.5%, about 0.1% to about 1%, about 0.1% to about 2%, about 0.1% to about 3%, about 0.1% to about 4%, about 0.1% to about 5%, about 0.1% to about 6%, about 0.1% to about 7%, about 0.1% to about 8%, about 0.1% to about 10%, about 0. .2% to about 0.5%, about 0.2% to about 1%, about 0.2% to about 2%, about 0.2% to about 3%, about 0.2% to about 4%, about 0.2% to about 5%, about 0.2% to about 6%, about 0.2% to about 7%, about 0.2% to about 8%, about 0.2% to about 10%, about 0.5% to about 1%, about 0.5% to about 2%, about 0.5% to about 3%, about 0.5% to about 4%, about 0.5% to about 5%, about 0.5% to about 6%, about 0.5 % to about 7%, about 0.5% to about 8%, about 0.5% to about 10%, about 1% to about 2%, about 1% to about 3%, about 1% to about 4%, about 1% to about 5%, about 1% to about 6%, about 1% to about 7%, about 1% to about 8%, about 1% to about 10%, about 2% to about 3%, about 2% to about 4%, about 2% to about 5%, about 2% to about 6%, about 2% to about 7%, about 2% to about 8%, about 2% to about 10%, about 3% to about 4%, about 3% to about 5% , about 3% to about 6%, about 3% to about 7%, about 3% to about 8%, about 3% to about 10%, about 4% to about 5%, about 4% to about 6%, about 4% to about 7%, about 4% to about 8%, about 4% to about 10%, about 5% to about 6%, about 5% to about 7%, about 5% to about 8%, about 5% to about 10%, about 6% to about 7%, about 6% to about 8%, about 6% to about 10%, about 7% to about 8%, about 7% to about 10%, or about 8% to about 10%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is about 0.1%, about 0.2%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 10%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is at least about 0.1%, about 0.2%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 10%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is at most about 0.1%, about 0.2%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 10%.

[0074] In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is between about 1% and about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at least about 1%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at most about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is about 1% to about 2%, about 1% to about 5%, about 1% to about 10%, about 1% to about 15%, about 1% to about 20%, about 1% to about 25%, about 1% to about 30%, about 1% to about 35%, about 1% to about 40%, about 2% to about 5%, about 2% to about 10%, about 2% to about 15%, about 2% to about 20%, about 2% to about 25%, about 2% to about 30%, about 2% to about 35%, about 2% to about 40%, about 5% to about 10%, about 5% to about 15%, about 5% to about 20%, about 5% to about 25%, about 5% to about 30%, about 35 ... 0%, about 5% to about 35%, about 5% to about 40%, about 10% to about 15%, about 10% to about 20%, about 10% to about 25%, about 10% to about 30%, about 10% to about 35%, about 10% to about 40%, about 15% to about 20%, about 15% to about 25%, about 15% to about 30%, about 15% to about 35%, about 15% to about 40%, about 20% to about 25%, about 20% to about 30%, about 20% to about 35%, about 20% to about 40%, about 25% to about 30%, about 25% to about 35%, about 25% to about 40%, about 30% to about 35%, about 30% to about 40%, or about 35% to about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is about 1%, about 2%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at least about 1%, about 2%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at most about 1%, about 2%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%.

[0075] In some embodiments, the adhesive is a carpenter's glue, wood glue, cyanoacrylate, contact cement, latex, library paste, rubber The conductive filler may include, for example, methyl cellulose, resorcinol resin, starch, butanone, dichloromethane acrylic, ethylene vinyl, phenol formaldehyde resin, polyamide, polyester, polyethylene, polypropylene, polysulfide, polyurethane, polyvinyl acetate, aliphatic, polyvinyl alcohol, polyvinyl chloride, polyvinyl chloride emulsion, silicone, styrene acrylic, epichlorohydrin, epoxide, or any combination thereof. Some embodiments further include adding a conductive filler to the carbon-based material and the adhesive. In some embodiments, the conductive filler includes silver. In some embodiments, the silver includes silver nanoparticles, silver nanorods, silver nanowires, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or any combination thereof. Some embodiments further include adding a thinner to the carbon-based material and the adhesive. In some embodiments, the thinner includes butyl acetate, lacquer thinner, acetone, petroleum naphtha, mineral spirits, xylene, or any combination thereof.

[0076] Another aspect provided herein is a method of forming a conductive carbon-based epoxy that includes forming a resin that includes a carbon-based material and an adhesive, and adding a curing agent to the resin.

[0077] In some embodiments, the carbon-based material is graphene, graphite powder, natural graphite, synthetic graphite, expanded graphite, carbon black, Timcal carbon super C45, Timcal carbon super C65, cabot carbon, carbon super P, acetylene black, furne The nanofibers may include, for example, graphene black, carbon nanotubes, vapor grown carbon fibers, graphene oxide, or any combination thereof.

[0078] In some embodiments, the carbon-based material comprises about 60% to about 99.9% resin by weight. In some embodiments, the carbon-based material comprises at least about 60% resin by weight. In some embodiments, the carbon-based material comprises up to about 99.9% resin by weight. In some embodiments, the carbon-based material comprises about 60% to about 65%, about 60% to about 70%, about 60% to about 75%, about 60% to about 80%, about 60% to about 85%, about 60% to about 90%, about 60% to about 95%, about 60% to about 96%, about 60% to about 97%, about 60% to about 99%, about 60% to about 99.9%, about 65% to about 70%, about 65% to about 75%, about 65% to about 80%, about 65% to about 85%, about 6 5% to about 90%, about 65% to about 95%, about 65% to about 96%, about 65% to about 97%, about 65% to about 99%, about 65% to about 99.9%, about 70% to about 75%, about 70% to about 80%, about 70% to about 85%, about 70% to about 90%, about 70% to about 95%, about 70% to about 96%, about 70% to about 97%, about 70% to about 99%, about 70% to about 99.9%, about 75% to about 80%, about 75% to about 85%, about 75% to about 9 0%, about 75% to about 95%, about 75% to about 96%, about 75% to about 97%, about 75% to about 99%, about 75% to about 99.9%, about 80% to about 85%, about 80% to about 90%, about 80% to about 95%, about 80% to about 96%, about 80% to about 97%, about 80% to about 99%, about 80% to about 99.9%, about 85% to about 90%, about 85% to about 95%, about 85% to about 96%, about 85% to about 97%, about 85% to about 99%, about The composition comprises 5% to about 99.9%, about 90% to about 95%, about 90% to about 96%, about 90% to about 97%, about 90% to about 99%, about 90% to about 99.9%, about 95% to about 96%, about 95% to about 97%, about 95% to about 99%, about 95% to about 99.9%, about 96% to about 97%, about 96% to about 99%, about 96% to about 99.9%, about 97% to about 99%, about 97% to about 99.9%, or about 99% to about 99.9% resin. In some embodiments, the carbon-based material comprises about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 96%, about 97%, about 99%, or about 99.9% resin by weight.In some embodiments, the carbon-based material comprises at least about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 96%, about 97%, about 99%, or about 99.9% resin by weight. In some embodiments, the carbon-based material comprises at most about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 96%, about 97%, about 99%, or about 99.9% resin by weight.

[0079] In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is about 0.1% to about 10%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is at least about 0.1%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is at most about 10%. In some embodiments, the carbon-based material comprises graphene, and the weight percentage of graphene in the carbon-based material is about 0.1% to about 0.2%, about 0.1% to about 0.5%, about 0.1% to about 1%, about 0.1% to about 2%, about 0.1% to about 3%, about 0.1% to about 4%, about 0.1% to about 5%, about 0.1% to about 6%, about 0.1% to about 7%, about 0.1% to about 8%, about 0.1% to about 9%, about 0.1% to about 10%, about 0.1% to about 11%, about 0.1% to about 12%, about 0.1% to about 13%, about 0.1% to about 14%, about 0.1% to about 15%, about 0.1% to about 16%, about 0.1% to about 17%, about 0.1% to about 18%, about 0.1% to about 19%, about 0.1% to about 20%, about 0.1% to about 21%, about 0.1% to about 22%, about 0.1% to about 23%, about 0.1% to about 24%, about 0.1% to about 25%, about 0.1% to about 26%, about 0.1% to about 28%, about 0.1% to about 29%, about 0.1% to about 30%, about 0.1% to about %, about 0.1% to about 10%, about 0.2% to about 0.5%, about 0.2% to about 1%, about 0.2% to about 2%, about 0.2% to about 3%, about 0.2% to about 4%, about 0.2% to about 5%, about 0.2% to about 6%, about 0.2% to about 7%, about 0.2% to about 8%, about 0.2% to about 10%, about 0.5% to about 1%, about 0.5% to about 2%, about 0.5% to about 3%, about 0.5 % to about 4%, about 0.5% to about 5%, about 0.5% to about 6%, about 0.5% to about 7%, about 0.5% to about 8%, about 0.5% to about 10%, about 1% to about 2%, about 1% to about 3%, about 1% to about 4%, about 1% to about 5%, about 1% to about 6%, about 1% to about 7%, about 1% to about 8%, about 1% to about 10%, about 2% to about 3%, about 2% to about 4%, about 2% to about 5%, about 2% to about 6%, about 2% to about 7%, about 2% to about 8%, about 2% to about 10%, about 3% to about 4%, about 3% to about 5%, about 3% to about 6%, about 3% to about 7%, about 3% to about 8%, about 3% to about 10%, about 4% to about 5%, about 4% to about 6%, about 4% to about 7%, about 4% to about 8%, about 4% to about 10%, about 5% to about 6%, about 5% to about 7%, about 5% to about 8%, about 5% to about 10%, about 6% to about 7%, about 6% to about 8%, about 6% to about 10%, about 7% to about 8%, about 7% to about 10%, or about 8% to about 10%. In some embodiments, the carbon-based material comprises graphene and the weight percentage of graphene in the carbon-based material is about 0.1%, about 0.2%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 10%. In some embodiments, the carbon-based material comprises graphene and the weight percentage of graphene in the carbon-based material is at least about 0.1%, about 0.2%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 10%. In some embodiments, the carbon-based material comprises graphene and the weight percentage of graphene in the carbon-based material is at most about 0.1%, about 0.2%, about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 10%.

[0080] In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is between about 1% and about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at least about 1%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at most about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is about 1% to about 2%, about 1% to about 5%, about 1% to about 10%, about 1% to about 15%, about 1% to about 20%, about 1% to about 25%, about 1% to about 30%, about 1% to about 35%, about 1% to about 40%, about 2% to about 5%, about 2% to about 10%, about 2% to about 15%, about 2% to about 20%, about 2% to about 25%, about 2% to about 30%, about 2% to about 35%, about 2% to about 40%, about 5% to about 10%, about 5% to about 15%, about 5% to about 20%, about 5% to about 25%, about 5% to about 30%, about 35 ... 0%, about 5% to about 35%, about 5% to about 40%, about 10% to about 15%, about 10% to about 20%, about 10% to about 25%, about 10% to about 30%, about 10% to about 35%, about 10% to about 40%, about 15% to about 20%, about 15% to about 25%, about 15% to about 30%, about 15% to about 35%, about 15% to about 40%, about 20% to about 25%, about 20% to about 30%, about 20% to about 35%, about 20% to about 40%, about 25% to about 30%, about 25% to about 35%, about 25% to about 40%, about 30% to about 35%, about 30% to about 40%, or about 35% to about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is about 1%, about 2%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at least about 1%, about 2%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%. In some embodiments, the carbon-based material comprises graphite powder, and the weight percentage of the graphite powder in the carbon-based material is at most about 1%, about 2%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, or about 40%.

[0081] In some embodiments, the adhesive is a carpenter's glue, wood glue, cyanoacrylate, contact cement, latex, library paste, rubber Methyl cellulose, resorcinol resin, starch, butanone, dichloromethane acrylic, ethylene vinyl, phenol formaldehyde resin, polyamide, polyester, polyethylene, polypropylene, polysulfide, polyurethane, polyvinyl acetate, aliphatic, polyvinyl alcohol, polyvinyl chloride, polyvinyl chloride emulsion, silicone , styrene acrylic, epichlorohydrin, epoxide, or any combination thereof. Some embodiments further include adding a conductive filler to the resin and hardener. In some embodiments, the conductive filler comprises silver. In some embodiments, the silver comprises silver nanoparticles, silver nanorods, silver nanowires, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or any combination thereof. Some embodiments further include adding a thinner to the resin and hardener. In some embodiments, the thinner comprises butyl acetate, lacquer thinner, acetone, petroleum naphtha, mineral spirits, xylene, or any combination thereof.

[0082] In some embodiments, the method of forming the conductive carbon-based epoxy further comprises adding a pigment, a colorant, a dye, or any combination thereof. In some embodiments, the method of forming the conductive carbon-based epoxy further comprises adding at least one, at least two, at least three, at least four, or at least five colorants, dyes, pigments, or combinations thereof. In some embodiments, the pigment comprises a metal-based or metallic pigment. In some embodiments, the metallic pigment is a gold, silver, titanium, aluminum, tin, zinc, mercury, manganese, lead, iron, iron oxide, copper, cobalt, cadmium, chromium, arsenic, bismuth, antimony, or barium pigment. In some embodiments, the colorant comprises at least one metallic pigment. In some embodiments, the colorant comprises a silver metallic colorant. In some embodiments, the silver metallic colorant comprises silver nanoparticles, silver nanorods, silver nanowires, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or combinations thereof.

[0083] In some embodiments, the colorant is selected from pigments and / or dyes that are red, yellow, magenta, green, cyan, purple, black, or brown, or combinations thereof. In some embodiments, the pigment is blue, brown, cyan, green, purple, magenta, red, yellow, or combinations thereof. In some embodiments, the dye is blue, brown, cyan, green, purple, magenta, red, yellow, or combinations thereof.

[0084] In some embodiments, the yellow colorant is Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 65, 74, 83, 93, 110, 128, 151, 155, or any combination thereof. In some embodiments, the black colorant includes Color Black SI70, Color Black SI50, Color Black FW1, Color Black FW18, Acid Black 1, 11, 52, 172, 194, 210, 234, or combinations thereof. In some embodiments, the red or magenta colorant includes Pigment Red 1-10, 12, 18, 21, 23, 37, 38, 39, 40, 41, 48, 90, 112, or combinations thereof. , 122, or a combination thereof. In some embodiments, cyan or purple The colorants include Pigment Blue 15, 17, 22, Pigment Violet 1, 2, 3, 5, 19, 23, or combinations thereof. In some embodiments, the orange colorant includes Pigment Orange 48 and / or 49. In some embodiments, the purple colorant includes Pigment Violet 19 and / or 42.

[0085] Another aspect provided herein is a method of forming silver nanowires, the method including heating a solvent, adding a catalyst solution and a polymer solution to a glycol to form a first solution, injecting a silver-based solution into the first solution to form a second solution, centrifuging the second solution, and washing the second solution with a wash solution to extract the silver nanowires.

[0086] In some embodiments, the solvent comprises a glycol. In some embodiments, the glycol is ethylene glycol, polyethylene glycol 200, polyethylene glycol 400, propylene glycol, or any combination thereof.

[0087] In some embodiments, the solvent comprises a polymer solution, hi some embodiments, the polymer solution comprises a polymer comprising polyvinylpyrrolidone, sodium dodecylsulfonate, vitamin B2, poly(vinyl alcohol), dextrin, poly(methyl vinyl ether), or any combination thereof.

[0088] In some embodiments, the polymer has a molecular weight of about 10,000 to about 40,000. In some embodiments, the polymer has a molecular weight of at least about 10,000. In some embodiments, the polymer has a molecular weight of up to about 40,000.In some embodiments, the polymer may be from about 10,000 to about 12,500, from about 10,000 to about 15,000, from about 10,000 to about 17,500, from about 10,000 to about 20,000, from about 10,000 to about 22,500, from about 10,000 to about 25,000, from about 10,000 to about 27,500, from about 10,000 to about 30,000, from about 10,000 to about 35,000, from about 10,000 to about 40,000, from about 12,500 to about 15,000, from about 12,500 to about 17,500, from about 12,500 to about 20,000, 12,500 to about 22,500, about 12,500 to about 25,000, about 12,500 to about 27,500, about 12,500 to about 30,000, about 12,500 to about 35,000, about 12,500 to about 40,000, about 15,000 to about 17,500, about 15,000 to about 20,000, about 15,000 to about 22,500, about 15,000 to about 25,000, about 15,000 to about 27,500, about 15,000 to about 30,000, about 15,000 to about 35,000, about 15,000 to about 40,000, about 17, 500 to about 20,000, about 17,500 to about 22,500, about 17,500 to about 25,000, about 17,500 to about 27,500, about 17,500 to about 30,000, about 17,500 to about 35,000, about 17,500 to about 40,000, about 20,000 to about 22,500, about 20,000 to about 25,000, about 20,000 to about 27,500, about 20,000 to about 30,000, about 20,000 to about 35,000, about 20,000 to about 40,000, about 22,500 to about 25,000, about 22,500 about 27,500, about 22,500 to about 30,000, about 22,500 to about 35,000, about 22,500 to about 40,000, about 25,000 to about 27,500, about 25,000 to about 30,000, about 25,000 to about 35,000, about 25,000 to about 40,000, about 27,500 to about 30,000, about 27,500 to about 35,000, about 27,500 to about 40,000, about 30,000 to about 35,000, about 30,000 to about 40,000, or about 35,000 to about 40,000.In some embodiments, the polymer has a molecular weight of about 10,000, about 12,500, about 15,000, about 17,500, about 20,000, about 22,500, about 25,000, about 27,500, about 30,000, about 35,000, or about 40,000. In some embodiments, the polymer has a molecular weight of at least about 10,000, about 12,500, about 15,000, about 17,500, about 20,000, about 22,500, about 25,000, about 27,500, about 30,000, about 35,000, or about 40,000. In some embodiments, the polymer has a molecular weight of up to about 10,000, about 12,500, about 15,000, about 17,500, about 20,000, about 22,500, about 25,000, about 27,500, about 30,000, about 35,000, or about 40,000.

[0089] In some embodiments, the polymer solution has a concentration of about 0.075M to about 0.25M. In some embodiments, the polymer solution has a concentration of at least about 0.075M. In some embodiments, the polymer solution has a concentration of up to about 0.25M. In some embodiments, the polymer solution has a concentration of about 0.075M to about 0.1M, about 0.075M to about 0.125M, about 0.075M to about 0.15M, about 0.075M to about 0.175M, about 0.075M to about 0.2M, about 0.075M to about 0.225M, about 0.075M to about 0.25M, about 0.1M to about 0.125M, about 0.1M to about 0.15M, about 0.1M to about 0.1 75M, about 0.1M to about 0.2M, about 0.1M to about 0.225M, about 0.1M to about 0.25M, about 0.125M to about 0.15M, about 0.125M to about 0 .175M, about 0.125M to about 0.2M, about 0.125M to about 0.225M, about 0.125M to about 0.25M, about 0.15M to about 0.175M, about 0 The polymer solution has a concentration of about 0.15 M to about 0.2 M, about 0.15 M to about 0.225 M, about 0.15 M to about 0.25 M, about 0.175 M to about 0.2 M, about 0.175 M to about 0.225 M, about 0.175 M to about 0.25 M, about 0.2 M to about 0.225 M, about 0.2 M to about 0.25 M, or about 0.225 M to about 0.25 M. In some embodiments, the polymer solution has a concentration of about 0.075 M, about 0.1 M, about 0.125 M, about 0.15 M, about 0.175 M, about 0.2 M, about 0.225 M, or about 0.25 M. In some embodiments, the polymer solution has a concentration of at least about 0.075 M, about 0.1 M, about 0.125 M, about 0.15 M, about 0.175 M, about 0.2 M, about 0.225 M, or about 0.25 M. In some embodiments, the polymer solution has a concentration of at most about 0.075 M, about 0.1 M, about 0.125 M, about 0.15 M, about 0.175 M, about 0.2 M, about 0.225 M, or about 0.25 M.

[0090] In some embodiments, the solvent is heated to a temperature of about 75° C. to about 300° C. In some embodiments, the solvent is heated to a temperature of at least about 75° C. In some embodiments, the solvent is heated to a temperature of up to about 300° C. In some embodiments, the solvent is heated to a temperature of about 75° C. to about 100° C., about 75° C. to about 125° C., about 75° C. to about 150° C., about 75° C. to about 175° C., about 75° C. to about 200° C., about 75° C. to about 225° C., about 75° C. to about 250° C., about 75° C. to about 275° C., about 75° C. to about 300° C., about 100° C. to about 125° C., about 100° C. to about 150° C., About 100°C to about 175°C, about 100°C to about 200°C, about 100°C to about 225°C, about 100°C to about 250°C, about 100°C to about 275°C, about 100°C to about 300°C, about 125°C to about 150°C, about 125°C to about 175°C, about 125°C to about 200°C, about 125°C to about 225°C, about 125°C to about 250°C, about 125°C to about 2 75°C, about 125°C to about 300°C, about 150°C to about 175°C, about 150°C to about 200°C, about 150°C to about 225°C, about 150°C to about 250°C, about 150°C to about 275°C, about 150°C to about 300°C, about 175°C to about 200°C, about 175°C to about 225°C, about 175°C to about 250°C, about 175°C to about 275°C, about 175 The solvent is heated to a temperature of about 75° C. to about 300° C., about 200° C. to about 225° C., about 200° C. to about 250° C., about 200° C. to about 275° C., about 200° C. to about 300° C., about 225° C. to about 250° C., about 225° C. to about 275° C., about 225° C. to about 300° C., about 250° C. to about 275° C., about 250° C. to about 300° C., or about 275° C. to about 300° C. In some embodiments, the solvent is heated to a temperature of about 75° C., about 100° C., about 125° C., about 150° C., about 175° C., about 200° C., about 225° C., about 250° C., about 275° C., or about 300° C. In some embodiments, the solvent is heated to a temperature of at least about 75° C., about 100° C., about 125° C., about 150° C., about 175° C., about 200° C., about 225° C., about 250° C., about 275° C., or about 300° C. In some embodiments, the solvent is heated to a temperature of up to about 75° C., about 100° C., about 125° C., about 150° C., about 175° C., about 200° C., about 225° C., about 250° C., about 275° C., or about 300° C.

[0091] In some embodiments, the solvent is heated for about 30 minutes to about 120 minutes. In some embodiments, the solvent is heated for at least about 30 minutes. In some embodiments, the solvent is heated for up to about 120 minutes. In some embodiments, the solvent is heated for about 30 minutes to about 40 minutes, about 30 minutes to about 50 minutes, about 30 minutes to about 60 minutes, about 30 minutes to about 70 minutes, about 30 minutes to about 80 minutes, about 30 minutes to about 90 minutes, about 30 minutes to about 100 minutes, about 30 minutes to about 110 minutes, about 30 minutes to about 120 minutes, about 40 minutes to about 50 minutes, about 40 minutes to about 60 minutes, about 40 minutes to about 70 minutes, about 40 minutes to about 8 ... 0 minutes to about 90 minutes, about 40 minutes to about 100 minutes, about 40 minutes to about 110 minutes, about 40 minutes to about 120 minutes, about 50 minutes to about 60 minutes, about 50 minutes to about 70 minutes, about 50 minutes to about 80 minutes, about 50 minutes to about 90 minutes, about 50 minutes to about 100 minutes, about 50 minutes to about 110 minutes, about 50 minutes to about 120 minutes, about 60 minutes to about 70 minutes, about 60 minutes to about 80 minutes, about 60 minutes to about 90 minutes, about 60 minutes to about 10 minutes 0 minutes, about 60 minutes to about 110 minutes, about 60 minutes to about 120 minutes, about 70 minutes to about 80 minutes, about 70 minutes to about 90 minutes, about 70 minutes to about 100 minutes, about 70 minutes to about 110 minutes, about 70 minutes to about 120 minutes, about 80 minutes to about 90 minutes, about 80 minutes to about 100 minutes, about 80 minutes to about 110 minutes, about 80 minutes to about 120 minutes, about 90 minutes to about 100 minutes, about 90 minutes to about 110 minutes, about 90 minutes to about 120 minutes, about 100 minutes to about 110 minutes, about 100 minutes to about 120 minutes, or about 110 minutes to about 120 minutes. In some embodiments, the solvent is heated for about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, or about 120 minutes. In some embodiments, the solvent is heated for at least about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, or about 120 minutes. In some embodiments, the solvent is heated for up to about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, or about 120 minutes.

[0092] In some embodiments, the solvent is stirred while being heated, hi some embodiments, the stirring is accomplished by a magnetic stir bar.

[0093] In some embodiments, stirring is performed at a speed of about 100 rpm to about 400 rpm. In some embodiments, stirring is performed at a speed of at least about 100 rpm. In some embodiments, stirring is performed at a speed of up to about 400 rpm.In some embodiments, the stirring is at about 100 rpm to about 125 rpm, about 100 rpm to about 150 rpm, about 100 rpm to about 175 rpm, about 100 rpm to about 200 rpm, about 100 rpm to about 225 rpm, about 100 rpm to about 250 rpm, about 100 rpm to about 275 rpm, about 100 rpm to about 300 rpm, about 100 rpm to about 350 rpm, about 100 rpm to about 400 rpm, about 125 rpm to about 150 rpm, about 125 rpm to about 175 rpm, about 125 rpm to about 200 rpm, about 1 25rpm to approx. 225rpm, approx. 125rpm to approx. 250rpm, approx. 125rpm to approx. 275rpm, approx. 125rpm to approx. 300rpm, approx. 125rpm to approx. 350rpm, approx. 125rpm to approx. 400rpm, approx. 150rpm to approx. 0rpm~about 200rpm, about 150rpm~about 225rpm, about 150rpm~about 250rpm, about 150rpm~about 275rpm, about 150rpm~about 300rpm, about 150rpm~about 350rpm, about 150rpm~about 400rpm, about 175rpm pm~about 200rpm, about 175rpm~about 225rpm, about 175rpm~about 250rpm, about 175rpm~about 275rpm, about 175rpm~about 300rpm, about 175rpm~about 350rpm, about 175rpm~about 400rpm, about 200rp m ~ approx. 225 rpm, approx. 200 rpm ~ approx. 250 rpm, approx. 200 rpm ~ approx. 275 rpm, approx. 200 rpm ~ approx. 300 rpm, approx. 200 rpm ~ approx. 350 rpm, approx. 200 rpm ~ approx. 400 rpm, approx. The mixing is performed at a speed of about 275 rpm, about 225 rpm to about 300 rpm, about 225 rpm to about 350 rpm, about 225 rpm to about 400 rpm, about 250 rpm to about 275 rpm, about 250 rpm to about 300 rpm, about 250 rpm to about 350 rpm, about 250 rpm to about 400 rpm, about 275 rpm to about 300 rpm, about 275 rpm to about 350 rpm, about 275 rpm to about 400 rpm, about 300 rpm to about 350 rpm, about 300 rpm to about 400 rpm, or about 350 rpm to about 400 rpm.In some embodiments, the stirring is performed at a speed of about 100 rpm, about 125 rpm, about 150 rpm, about 175 rpm, about 200 rpm, about 225 rpm, about 250 rpm, about 275 rpm, about 300 rpm, about 350 rpm, or about 400 rpm. In some embodiments, the stirring is performed at a speed of at least about 100 rpm, about 125 rpm, about 150 rpm, about 175 rpm, about 200 rpm, about 225 rpm, about 250 rpm, about 275 rpm, about 300 rpm, about 350 rpm, or about 400 rpm. In some embodiments, the stirring is performed at a speed of at least about 100 rpm, about 125 rpm, about 150 rpm, about 175 rpm, about 200 rpm, about 225 rpm, about 250 rpm, about 275 rpm, about 300 rpm, about 350 rpm, or about 400 rpm. This is done at a speed of 0 rpm.

[0094] In some embodiments, the catalyst solution comprises a catalyst including (chlorides) CuCl2, CuCl, NaCl, PtCl2, AgCl, FeCl2, FeCl3, tetrapropylammonium chloride, tetrapropylammonium bromide, or any combination thereof.

[0095] In some embodiments, the catalyst solution has a concentration of about 2 mM to about 8 mM. In some embodiments, the catalyst solution has a concentration of at least about 2 mM. In some embodiments, the catalyst solution has a concentration of up to about 8 mM. In some embodiments, the catalyst solution has a concentration of about 2 mM to about 2.5 mM, about 2 mM to about 3 mM, about 2 mM to about 3.5 mM, about 2 mM to about 4 mM, about 2 mM to about 4.5 mM, about 2 mM to about 5 mM, about 2 mM to about 5.5 mM, about 2 mM to about 6 mM, about 2 mM to about 6.5 mM, about 2 mM to about 7 mM, about 2 mM to about 8 mM, about 2.5 mM to about 3 mM, about 2.5 mM to about 3.5 mM, about 2.5 mM to about 4 mM, about 2.5 mM to about 4.5 mM, about 2.5 mM to about 5 mM, about 2.5mM to about 5.5mM, about 2.5mM to about 6mM, about 2.5mM to about 6.5mM, about 2.5mM to about 7mM, about 2.5mM to about 8mM, about 3mM to about 3.5mM, about 3mM to about 4mM, about 3mM to about 4.5mM , about 3mM to about 5mM, about 3mM to about 5.5mM, about 3mM to about 6mM, about 3mM to about 6.5mM, about 3mM to about 7mM, about 3mM to about 8mM, about 3.5mM to about 4mM, about 3.5mM to about 4.5mM, about 3.5mM to about 5 mM, about 3.5 mM to about 5.5 mM, about 3.5 mM to about 6 mM, about 3.5 mM to about 6.5 mM, about 3.5 mM to about 7 mM, about 3.5 mM to about 8 mM, about 4 mM to about 4.5 mM, about 4 mM to about 5 mM, about 4 mM to about 5.5 mM, about 4 mM to about 6 mM, about 4 mM to about 6.5 mM, about 4 mM to about 7 mM, about 4 mM to about 8 mM, about 4.5 mM to about 5 mM, about 4.5 mM to about 5.5 mM, about 4.5 mM to about 6 mM, about 4.5 mM to about 6.5 mM, about 4.5 5 mM to about 7 mM, about 4.5 mM to about 8 mM, about 5 mM to about 5.5 mM, about 5 mM to about 6 mM, about 5 mM to about 6.5 mM, about 5 mM to about 7 mM, about 5 mM to about 8 mM, about 5.5 mM to about 6 mM, about 5.5 mM to about 6.5 mM, about 5.5 mM to about 7 mM, about 5.5 mM to about 8 mM, about 6 mM to about 6.5 mM, about 6 mM to about 7 mM, about 6 mM to about 8 mM, about 6.5 mM to about 7 mM, about 6.5 mM to about 8 mM, or about 7 mM to about 8 mM. In some embodiments, the catalyst solution has a concentration of about 2 mM, about 2.5 mM, about 3 mM, about 3.5 mM, about 4 mM, about 4.5 mM, about 5 mM, about 5.5 mM, about 6 mM, about 6.5 mM, about 7 mM, or about 8 mM.In some embodiments, the catalyst solution has a concentration of at least about 2 mM, about 2.5 mM, about 3 mM, about 3.5 mM, about 4 mM, about 4.5 mM, about 5 mM, about 5.5 mM, about 6 mM, about 6.5 mM, about 7 mM, or about 8 mM. In some embodiments, the catalyst solution has a concentration of at most about 2 mM, about 2.5 mM, about 3 mM, about 3.5 mM, about 4 mM, about 4.5 mM, about 5 mM, about 5.5 mM, about 6 mM, about 6.5 mM, about 7 mM, or about 8 mM.

[0096] In some embodiments, the volume of the solvent is about 75 to about 250 times greater than the volume of the catalyst solution. In some embodiments, the volume of the solvent is at least about 75 times greater than the volume of the catalyst solution. In some embodiments, the volume of the solvent is at most about 250 times greater than the volume of the catalyst solution. In some embodiments, the volume of the solvent is about 75 to about 100, about 75 to about 125, about 75 to about 150, about 75 to about 175, about 75 to about 200, about 75 to about 225, about 75 to about 250, about 100 to about 125, about 100 to about 150, about 100 to about 175, about 100 to about 200, about 100 to about 225, about 100 to about 250, about 1 25 to about 150, about 125 to about 175, about 125 to about 200, about 125 to about 225, about 125 to about 250, about 150 to about 175, about 150 to about 200, about 150 to about 225, about 150 to about 250, about 175 to about 200, about 175 to about 225, about 175 to about 250, about 200 to about 225, about 200 to about 250, or about 225 to about 250 times greater. In some embodiments, the volume of the solvent is about 75, about 100, about 125, about 150, about 175, about 200, about 225, or about 250 times greater than the volume of the catalyst solution. In some embodiments, the volume of the solvent is at least about 75, about 100, about 125, about 150, about 175, about 200, about 225, or about 250 times greater than the volume of the catalyst solution. In some embodiments, the volume of the solvent is up to about 75, about 100, about 125, about 150, about 175, about 200, about 225, or about 250 times greater than the volume of the catalyst solution.

[0097] In some embodiments, the volume of the solvent is about 1.5 to about 6.5 times greater than the volume of the polymer solution. In some embodiments, the volume of the solvent is at least about 1.5 times greater than the volume of the polymer solution. In some embodiments, the volume of the solvent is at most about 6.5 times greater than the volume of the polymer solution. In some embodiments, the volume of the solvent is about 1.5 to about 2, about 1.5 to about 2.5, about 1.5 to about 3, about 1.5 to about 3.5, about 1.5 to about 4, about 1.5 to about 4.5, about 1.5 to about 5, about 1.5 to about 5.5, about 1.5 to about 6, about 1.5 to about 6.5, about 2 to about 2.5, about 2 to about 3, about 2 to about 3.5, about 2 to about 4, about 2 to about 4.5, about 2 to about 5, about 2 to about 5.5, about 2 to about 6, about 2 to about 6.5, about 2.5 to about 3, about 2.5 to about 3.5, about 2.5 to about 4, about 2.5 to about 4.5, about 2.5 to about 5, about 2.5 to about 5. ... about 6, about 2.5 to about 6.5, about 3 to about 3.5, about 3 to about 4, about 3 to about 4.5, about 3 to about 5, about 3 to about 5.5, about 3 to about 6, about 3 to about 6.5, about 3.5 to about 4, about 3.5 to about 4.5, about 3.5 to about 5, about 3.5 to about 5.5, about 3.5 to about 6, about 3.5 to about 6.5, about 4 to about 4.5, about 4 to about 5, about 4 to about 5.5, about 4 to about 6, about 4 to about 6.5, about 4.5 to about 5, about 4.5 to about 5.5, about 4.5 to about 6, about 4.5 to about 6.5, about 5 to about 5.5, about 5 to about 6, about 5 to about 6.5, about 5.5 to about 6, about 5.5 to about 6.5, or about 6 to about 6.5 times larger. In some embodiments, the volume of the solvent is about 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 4.5, about 5, about 5.5, about 6, or about 6.5 times greater than the volume of the polymer solution. In some embodiments, the volume of the solvent is at least about 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 4.5, about 5, about 5.5, about 6, or about 6.5 times greater than the volume of the polymer solution. In some embodiments, the volume of the solvent is at most about 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 4.5, about 5, about 5.5, about 6, or about 6.5 times greater than the volume of the polymer solution.

[0098] In some embodiments, the silver-based solution comprises a silver-based material that includes AgNO3.

[0099] In some embodiments, the silver-based solution has a concentration of about 0.05M to about 0.2M. In some embodiments, the silver-based solution has a concentration of at least about 0.05M. In some embodiments, the silver-based solution has a concentration of up to about 0.2M. In some embodiments, the silver-based solution has a concentration of about 0.05M to about 0.075M, about 0.05M to about 0.1M, about 0.05M to about 0.125M, about 0.05M to about 0.15M, about 0.05M to about 0.175M, about 0.05M to about 0.2M, about 0.075M to about 0.1M, about 0.075M to about 0.125M, about 0.075M to about 0.15M, about 0.075M to about 0.175M, The silver-based solution has a concentration of about 0.075 M to about 0.2 M, about 0.1 M to about 0.125 M, about 0.1 M to about 0.15 M, about 0.1 M to about 0.175 M, about 0.1 M to about 0.2 M, about 0.125 M to about 0.15 M, about 0.125 M to about 0.175 M, about 0.125 M to about 0.2 M, about 0.15 M to about 0.175 M, about 0.15 M to about 0.2 M, or about 0.175 M to about 0.2 M. In some embodiments, the silver-based solution has a concentration of about 0.05 M, about 0.075 M, about 0.1 M, about 0.125 M, about 0.15 M, about 0.175 M, or about 0.2 M.

[0100] In some embodiments, the volume of the solvent is about 1.5 to about 6.5 times larger than the volume of the silver-based solution. In some embodiments, the volume of the solvent is at least about 1.5 times larger than the volume of the silver-based solution. In some embodiments, the volume of the solvent is up to about 6.5 times larger than the volume of the silver-based solution. In some embodiments, the volume of the solvent is about 1 to about 6.5 times larger than the volume of the silver-based solution. .5 to about 2, about 1.5 to about 2.5, about 1.5 to about 3, about 1.5 to about 3.5, about 1.5 to about 4, about 1.5 to about 4.5, about 1.5 to about 5, about 1.5 to about 5.5, about 1.5 to about 6, about 1.5 to about 6.5, about 2 to about 2.5, about 2 to about 3, about 2 to about 3.5, about 2 to about 4, about 2 to about 4.5, about 2 to about 5, about 2 to about 5.5, about 2 to about 6, about 2 to about 6.5, about 2.5 to about 3, about 2.5 to about 3.5, about 2.5 to about 4, about 2.5 to about 4.5, about 2.5 to about 5, about 2.5 to about 5.5, about 2.5 to about 6, about 2.5 to about 6.5, about 3 to about 3.5, about 3 to about 4, about 3 to about 4.5, about 3 to about 5, about 3 to about 5.5, about 3 to about 6, about 3 to about 6.5, about 3.5 to about 4, about 3.5 to about 4.5, about 3.5 to about 5, about 3.5 to about 5.5, about 3.5 to about 6, about 3.5 to about 6.5, about 4 to about 4.5, about 4 to about 5, about 4 to about 5.5, about 4 to about 6, about 4 to about 6.5, about 4.5 to about 5, about 4.5 to about 5.5, about 4.5 to about 6, about 4.5 to about 6.5, about 5 to about 5.5, about 5 to about 6, about 5 to about 6.5, about 5.5 to about 6, about 5.5 to about 6.5, or about 6 to about 6.5 times larger. In some embodiments, the volume of the solvent is about 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 4.5, about 5, about 5.5, about 6, or about 6.5 times larger than the volume of the silver-based solution. In some embodiments, the volume of the solvent is at least about 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 4.5, about 5, about 5.5, about 6, or about 6.5 times larger than the volume of the silver-based solution. In some embodiments, the volume of the solvent is at most about 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 4.5, about 5, about 5.5, about 6, or about 6.5 times larger than the volume of the silver-based solution.

[0101] In some embodiments, the silver-based solution is injected into the first solution for about 1 second to about 900 seconds. In some embodiments, the silver-based solution is injected into the first solution for at least about 1 second. In some embodiments, the silver-based solution is injected into the first solution for up to about 900 seconds. In some embodiments, the silver-based solution is injected into the first solution for about 1 second to about 2 seconds, about 1 second to about 5 seconds, about 1 second to about 10 seconds, about 1 second to about 50 seconds, about 1 second to about 100 seconds, about 1 second to about 200 seconds, about 1 second to about 300 seconds, about 1 second to about 400 seconds, about 1 second to about 600 seconds, about 1 second to about 800 seconds, about 1 second to about 900 seconds, about 2 seconds to about 5 seconds, about 2 seconds to about 10 seconds, about 2 seconds to about 50 seconds, about 2 seconds to about 100 seconds, about 2 seconds to about 200 seconds, about 2 seconds to about 300 seconds, about 2 seconds to about 40 seconds, about 2 seconds to about 50 seconds, about 2 seconds to about 50 seconds, about 2 seconds to about 2 ... 0 seconds, approximately 2 seconds to approximately 600 seconds, approximately 2 seconds to approximately 800 seconds, approximately 2 seconds to approximately 900 seconds, approximately 5 seconds to approximately 10 seconds, approximately 5 seconds to approximately 50 seconds, approximately 5 seconds to approximately 100 seconds, approximately 5 seconds to approximately 200 seconds, approximately 5 seconds to approximately 300 seconds, approximately 5 seconds to approximately 400 seconds, approximately 5 seconds to approximately 600 seconds, approximately 5 seconds to approximately 800 seconds, approximately 5 seconds to approximately 900 seconds, approximately 10 seconds to approximately 50 seconds, approximately 10 seconds to approximately 100 seconds, approximately 10 seconds to approximately 200 seconds, approximately 10 seconds to approximately 300 seconds, approximately 10 seconds to approximately 400 seconds, approximately 10 seconds to approximately 600 seconds, 10 seconds to 800 seconds, 10 seconds to 900 seconds, 50 seconds to 100 seconds, 50 seconds to 200 seconds, 50 seconds to 300 seconds, 50 seconds to 400 seconds, 50 seconds to 600 seconds, 50 seconds to 800 seconds, 50 seconds to 800 seconds Approximately 900 seconds, approximately 100 seconds to approximately 200 seconds, approximately 100 seconds to approximately 300 seconds, approximately 100 seconds to approximately 400 seconds, approximately 100 seconds to approximately 600 seconds, approximately 100 seconds to approximately 800 seconds, approximately 100 seconds to approximately 900 seconds, approximately 200 seconds to approximately 300 seconds, approximately 20 The first solution is injected for 0 seconds to about 400 seconds, about 200 seconds to about 600 seconds, about 200 seconds to about 800 seconds, about 200 seconds to about 900 seconds, about 300 seconds to about 400 seconds, about 300 seconds to about 600 seconds, about 300 seconds to about 800 seconds, about 300 seconds to about 900 seconds, about 400 seconds to about 600 seconds, about 400 seconds to about 800 seconds, about 400 seconds to about 900 seconds, about 600 seconds to about 800 seconds, about 600 seconds to about 900 seconds, or about 800 seconds to about 900 seconds. In some embodiments, the silver-based solution is injected into the first solution for about 1 second, about 2 seconds, about 5 seconds, about 10 seconds, about 50 seconds, about 100 seconds, about 200 seconds, about 300 seconds, about 400 seconds, about 600 seconds, about 800 seconds, or about 900 seconds.In some embodiments, the silver-based solution is infused into the first solution for at least about 1 second, about 2 seconds, about 5 seconds, about 10 seconds, about 50 seconds, about 100 seconds, about 200 seconds, about 300 seconds, about 400 seconds, about 600 seconds, about 800 seconds, or about 900 seconds. In some embodiments, the silver-based solution is infused into the first solution for at most about 1 second, about 2 seconds, about 5 seconds, about 10 seconds, about 50 seconds, about 100 seconds, about 200 seconds, about 300 seconds, about 400 seconds, about 600 seconds, about 800 seconds, or about 900 seconds.

[0102] Some embodiments further include heating the second solution prior to the process of centrifuging the second solution.

[0103] In some embodiments, the second solution is heated for about 30 minutes to about 120 minutes. In some embodiments, the second solution is heated for at least about 30 minutes. In some embodiments, the second solution is heated for up to about 120 minutes. In some embodiments, heating of the second solution is for about 30 minutes to about 40 minutes, about 30 minutes to about 50 minutes, about 30 minutes to about 60 minutes, about 30 minutes to about 70 minutes, about 30 minutes to about 80 minutes, about 30 minutes to about 90 minutes, about 30 minutes to about 100 minutes, about 30 minutes to about 110 minutes, about 30 minutes to about 120 minutes, about 40 minutes to about 50 minutes, about 40 minutes to about 60 minutes, about 40 minutes to about 70 minutes, about 40 minutes to about 80 minutes, about 40 minutes to about 90 minutes, about 40 minutes to about 100 minutes, about 40 minutes to about 110 minutes, about 40 minutes to about 120 minutes, about 50 minutes to about 60 minutes, about 50 minutes to about 70 minutes, about 50 minutes to about 80 minutes, about 50 minutes to about 90 minutes, about 50 minutes to about 100 minutes, about 50 minutes to about 1 10 minutes, 50 minutes to 120 minutes, 60 minutes to 70 minutes, 60 minutes to 80 minutes, 60 minutes to 90 minutes, 60 minutes to 100 minutes, 60 minutes to 110 minutes, 60 minutes to 120 minutes, 70 minutes to 80 minutes, 70 minutes to 90 minutes, 70 minutes to 100 minutes, 70 minutes to 110 minutes, 70 minutes to 12 minutes In some embodiments, heating of the second solution is performed for about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, about 120 minutes, about 110 minutes, about 120 minutes, about 100 minutes, about 110 minutes, about 120 minutes, or about 120 minutes. In some embodiments, heating of the second solution is performed for about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, or about 120 minutes. In some embodiments, the heating of the second solution is carried out for at least about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, or about 120 minutes. In some embodiments, the heating of the second solution is carried out for up to about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, or about 120 minutes.

[0104] In some embodiments, centrifugation is performed at a speed of about 1,500 rpm to about 6,000 rpm. In some embodiments, centrifugation is performed at a speed of at least about 1,500 rpm. In some embodiments, centrifugation is performed at a speed of up to about 6,000 rpm. In some embodiments, centrifugation is performed at a speed of about 1,500 rpm to about 2,000 rpm, about 1,500 rpm to about 2,500 rpm, about 1,500 rpm to about 3,000 rpm, about 1,500 rpm to about 3,500 rpm, about 1,500 rpm to about 4,000 rpm, about 1,500 rpm to about 4,500 rpm, about 1,500 rpm to about 5,000 rpm, about 1,500 rpm to about 5,500 rpm, about 1,500 rpm to about 6,000 rpm, Approx. 2,000rpm to approx. 2,500rpm, approx. 2,000rpm to approx. 3,000rpm, approx. 2,000rpm to approx. 3,500rpm, approx. 2,000rpm to approx. 4,000rpm, approx. 2,000rpm to approx. 4,500rpm , about 2,000rpm to about 5,000rpm, about 2,000rpm to about 5,500rpm, about 2,000rpm to about 6,000rpm, about 2,500rpm to about 3,000rpm, about 2,500rpm to about 3,500rpm m, about 2,500rpm to about 4,000rpm, about 2,500rpm to about 4,500rpm, about 2,500rpm to about 5,000rpm, about 2,500rpm to about 5,500rpm, about 2,500rpm to about 6,000r pm, approximately 3,000rpm to approximately 3,500rpm, approximately 3,000rpm to approximately 4,000rpm, approximately 3,000rpm to approximately 4,500rpm, approximately 3,000rpm to approximately 5,000rpm, approximately 3,000rpm to approximately 5,500 rpm, approximately 3,000rpm to approximately 6,000rpm, approximately 3,500rpm to approximately 4,000rpm, approximately 3,500rpm to approximately 4,500rpm, approximately 3,500rpm to approximately 5,000rpm, approximately 3,500rpm to approximately 5,50 0rpm, about 3,500rpm to about 6,000rpm, about 4,000rpm to about 4,500rpm, about 4,000rpm to about 5,000rpm, about 4,000rpm to about 5,500rpm, about 4,000rpm to about 6,00 0 rpm, about 4,500 rpm to about 5,000 rpm, about 4,500 rpm to about 5,500 rpm, about 4,500 rpm to about 6,000 rpm, about 5,000 rpm to about 5,500 rpm, about 5,000 rpm to about 6,000 rpm, or about 5,500 rpm to about 6,000 rpm. In some embodiments, centrifugation is performed at a speed of about 1,500 rpm, about 2,000 rpm, about 2,500 rpm, about 3,000 rpm, about 3,500 rpm, about 4,000 rpm, about 4,500 rpm, about 5,000 rpm, about 5,500 rpm, or about 6,000 rpm. In some embodiments, centrifugation is performed at a speed of at least about 1,500 rpm, about 2,000 rpm, about 2,500 rpm, about 3,000 rpm, about 3,500 rpm, about 4,000 rpm, about 4,500 rpm, about 5,000 rpm, about 5,500 rpm, or about 6,000 rpm. In some embodiments, centrifugation is performed at a speed of up to about 1,500 rpm, about 2,000 rpm, about 2,500 rpm, about 3,000 rpm, about 3,500 rpm, about 4,000 rpm, about 4,500 rpm, about 5,000 rpm, about 5,500 rpm, or about 6,000 rpm.

[0105] In some embodiments, centrifugation occurs for about 10 minutes to about 40 minutes. In some embodiments, centrifugation occurs for at least about 10 minutes. In some embodiments, centrifugation occurs for up to about 40 minutes. In some embodiments, centrifugation is performed for about 10 minutes to about 15 minutes, about 10 minutes to about 20 minutes, about 10 minutes to about 25 minutes, about 10 minutes to about 30 minutes, about 10 minutes to about 35 minutes, about 10 minutes to about 40 minutes, about 15 minutes to about 20 minutes, about 15 minutes to about 25 minutes, about 15 minutes to about 30 minutes, about 15 minutes to about 35 minutes, about 15 minutes to about 40 minutes, about 20 minutes to about 25 minutes, about 20 minutes to about 30 minutes, about 20 minutes to about 35 minutes, about 20 minutes to about 40 minutes, about 25 minutes to about 30 minutes, about 25 minutes to about 35 minutes, about 25 minutes to about 40 minutes, about 30 minutes to about 35 minutes, about 30 minutes to about 40 minutes, or about 35 minutes to about 40 minutes. In some embodiments, centrifugation is performed for about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, or about 40 minutes. In some embodiments, centrifugation is performed for at least about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, or about 40 minutes. In some embodiments, centrifugation is performed for up to about 10 minutes, about 15 minutes, about 20 minutes, about 25 minutes, about 30 minutes, about 35 minutes, or about 40 minutes.

[0106] Some embodiments further include cooling the second solution prior to the process of centrifuging the second solution. In some embodiments, the second solution is cooled to room temperature. In some embodiments, the washing solution comprises ethanol, acetone, water, or any combination thereof.

[0107] In some embodiments, washing the second solution includes a plurality of washing cycles including about 2 cycles to about 6 cycles. In some embodiments, washing the second solution includes a plurality of washing cycles including at least about 2 cycles. In some embodiments, washing the second solution includes a plurality of washing cycles including up to about 6 cycles. In some embodiments, washing the second solution includes a plurality of washing cycles including about 2 cycles to about 3 cycles, about 2 cycles to about 4 cycles, about 2 cycles to about 5 cycles, about 2 cycles to about 6 cycles, about 3 cycles to about 4 cycles, about 3 cycles to about 5 cycles, about 3 cycles to about 6 cycles, about 4 cycles to about 5 cycles, about 4 cycles to about 6 cycles, or about 5 cycles to about 6 cycles. In some embodiments, washing the second solution includes a plurality of washing cycles including about 2 cycles, about 3 cycles, about 4 cycles, about 5 cycles, or about 6 cycles.

[0108] Some embodiments further include dispersing the silver nanowires in a dispersion solution, hi some embodiments, the dispersion solution comprises ethanol, acetone, and water, or any combination thereof.

[0109] In some embodiments, the method is carried out in air. In some embodiments, the method is carried out in a solvothermal chamber. In some embodiments, the method is carried out under high pressure.

[0110] Another aspect provided herein is a conductive ink. The conductive ink can include a conductive additive. The conductive additive can include a carbon-based conductive additive, a silver-based conductive additive, or both. The conductive ink can include a conductive carbon-based ink. The conductive ink can include a conductive silver-based ink. The conductive carbon-based ink can include a conductive graphene-based ink. The conductive graphene-based ink can include a binder solution including a binder and a first solvent, a reduced graphene oxide dispersion including reduced graphene oxide and a second solvent, a third solvent, a conductive additive, a surfactant, and an antifoaming agent.

[0111] In some embodiments, the conductive ink further comprises a pigment, a colorant, a dye, or any combination thereof. In some embodiments, the conductive ink comprises at least one, at least two, at least three, at least four, or at least five colorants, dyes, pigments, or combinations thereof. In some embodiments, the pigment comprises a metal-based or metallic pigment. In some embodiments, the metallic pigment is a gold, silver, titanium, aluminum, tin, zinc, mercury, manganese, lead, iron, iron oxide, copper, cobalt, cadmium, chromium, arsenic, bismuth, antimony, or barium pigment. In some embodiments, the colorant comprises at least one metallic pigment. In some embodiments, the colorant comprises a silver metallic colorant. In some embodiments, the silver metallic colorant comprises silver nanoparticles, silver nanorods, silver nanowires, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or combinations thereof.

[0112] In some embodiments, the colorant is selected from pigments and / or dyes that are red, yellow, magenta, green, cyan, purple, black, or brown, or combinations thereof. In some embodiments, the pigment is blue, brown, cyan, green, purple, magenta, red, yellow, or combinations thereof. In some embodiments, the dye is blue, brown, cyan, green, purple, magenta, red, yellow, or combinations thereof.

[0113] In some embodiments, the yellow colorant is Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 65, 74, 83, 93, 110, 128, 151, 155, or any combination thereof. In some embodiments, the black colorant includes Color Black SI70, Color Black SI50, Color Black FW1, Color Black FW18, Acid Black 1, 11, 52, 172, 194, 210, 234, or combinations thereof. In some embodiments, the red or magenta colorant includes Pigment Red 1-10, 12, 18, 21, 23, 37, 38, 39, 40, 41, 48, 90, 112, or combinations thereof. , 122, or a combination thereof. In some embodiments, cyan or purple The colorants include Pigment Blue 15, 17, 22, Pigment Violet 1, 2, 3, 5, 19, 23, or combinations thereof. In some embodiments, the orange colorant includes Pigment Orange 48 and / or 49. In some embodiments, the purple colorant includes Pigment Violet 19 and / or 42.

[0114] In some embodiments, at least one of the first solvent, the second solvent, and the third solvent comprises water and an organic solvent. In some embodiments, the organic solvent comprises ethanol, isopropyl alcohol, N-methyl-2-pyrrolidone, cyclohexanone, terpineol, 3-methoxy-3-methyl-1-butanol, 4-hydroxyl-4-methyl-pentan-2-one, methyl isobutyl ketone, or any combination thereof. nothing.

[0115] In some embodiments, the weight percentage of at least one of the first solvent, the second solvent, and the third solvent in the conductive ink is between about 1% and about 99%. In some embodiments, the weight percentage of at least one of the first solvent, the second solvent, and the third solvent in the conductive ink is at least about 1%. In some embodiments, the weight percentage of at least one of the first solvent, the second solvent, and the third solvent in the conductive ink is up to about 99%. In some embodiments, the mass percentage of at least one of the first solvent, the second solvent, and the third solvent in the conductive ink is from about 1% to about 2%, from about 1% to about 5%, from about 1% to about 10%, from about 1% to about 20%, from about 1% to about 30%, from about 1% to about 40%, from about 1% to about 50%, from about 1% to about 60%, from about 1% to about 70%, from about 1% to about 80%, from about 1% to about 99%, from about 2% to about 5%, from about 2% to about 10%, About 2% to about 20%, about 2% to about 30%, about 2% to about 40%, about 2% to about 50%, about 2% to about 60%, about 2% to about 70%, about 2% to about 80%, about 2% to about 99%, about 5% to about 10%, about 5% to about 20%, about 5% to about 30%, about 5% to about 40%, about 5% to about 50%, about 5% to about 60%, about 5% to about 70%, about 5% to about 80%, about 5% to about 99%, about 10% to about 20%, about 10% to about 30%, About 10% to about 40%, about 10% to about 50%, about 10% to about 60%, about 10% to about 70%, about 10% to about 80%, about 10% to about 99%, about 20% to about 30%, about 20% to about 40%, about 20% to about 50%, about 20% to about 60%, about 20% to about 70%, about 20% to about 80%, about 20% to about 99%, about 30% to about 40%, about 30% to about 50%, about 30% to about 60%, about 30% to about 70%, about 30 % to about 80%, about 30% to about 99%, about 40% to about 50%, about 40% to about 60%, about 40% to about 70%, about 40% to about 80%, about 40% to about 99%, about 50% to about 60%, about 50% to about 70%, about 50% to about 80%, about 50% to about 99%, about 60% to about 70%, about 60% to about 80%, about 60% to about 99%, about 70% to about 80%, about 70% to about 99%, or about 80% to about 99%.In some embodiments, the weight percentage of at least one of the first solvent, the second solvent, and the third solvent in the conductive ink is about 1%, about 2%, about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80%, or about 99%. In some embodiments, the weight percentage of at least one of the first solvent, the second solvent, and the third solvent in the conductive ink is at least about 1%, about 2%, about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, or about 80%. In some embodiments, the mass percentage of at least one of the first solvent, the second solvent, and the third solvent in the conductive ink is at most about 2%, about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80%, or about 99%.

[0116] In some embodiments, the binder solution includes a binder and a first solvent. In some embodiments, the binder includes a polymer. In some embodiments, the polymer includes a synthetic polymer. In some embodiments, the synthetic polymer includes carboxymethylcellulose, polyvinylidene fluoride, poly(vinyl alcohol), poly(vinyl pyrrolidone), poly(ethylene oxide), ethyl cellulose, or any combination thereof. In some embodiments, the binder is a dispersion. In some embodiments, the binder includes carboxymethylcellulose, polyvinylidene fluoride, poly(vinyl alcohol), poly(vinyl pyrrolidone), poly(ethylene oxide), ethyl cellulose, or any combination thereof.

[0117] In some embodiments, the weight percentage of the binder solution in the conductive ink is from about 0.5% to about 99%. In some embodiments, the weight percentage of the binder solution in the conductive ink is at least about 0.5%. In some embodiments, the weight percentage of the binder solution in the conductive ink is up to about 99%. In some embodiments, the weight percentage of the binder solution in the conductive ink is from about 0.5% to about 1%, from about 0.5% to about 2%, About 0.5% to about 5%, about 0.5% to about 10%, about 0.5% to about 20%, about 0.5% to about 30%, about 0.5% to about 40%, about 0.5% to about 50%, about 0.5% to about 70%, about 0.5% to about 90%, about 0.5% to about 99%, about 1% to about 2%, about 1% to about 5%, about 1% to about 10%, about 1% to about 20%, about 1% to about 30%, about 1% to about 40%, about 1% to about 5 0%, about 1% to about 70%, about 1% to about 90%, about 1% to about 99%, about 2% to about 5%, about 2% to about 10%, about 2% to about 20%, about 2% to about 30%, about 2% to about 40%, about 2% to about 50%, about 2% to about 70%, about 2% to about 90%, about 2% to about 99%, about 5% to about 10%, about 5% to about 20%, about 5% to about 30%, about 5% to about 40%, about 5% to about 50%, about 5% to about 70%, about 5% to about 90%, about 5% to about 99%, about 10% to about 20%, about 10% to about 30%, about 10% to about 40%, about 10% to about 50%, about 10% to about 70%, about 10% to about 90%, about 10% to about 99%, about 20% to about 30%, about 20% to about 40%, about 20% to about 50%, about 20% to about 70%, about 20% to about 90%, about 20% to about 99%, About 30% to about 40%, about 30% to about 50%, about 30% to about 70%, about 30% to about 90%, about 30% to about 99%, about 40% to about 50%, about 40% to about 70%, about 40% to about 90%, about 40% to about 99%, about 50% to about 70%, about 50% to about 90%, about 50% to about 99%, about 70% to about 90%, about 70% to about 99%, or about 90% to about 99%. In some embodiments, the weight percentage of the binder solution in the conductive ink is up to about 99%. In some embodiments, the weight percentage of the binder solution in the conductive ink is about 0.5%, about 1%, about 2%, about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 70%, about 90%, or about 99%. In some embodiments, the weight percentage of the binder solution in the conductive ink is at least about 0.5%, about 1%, about 2%, about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80%, about 90%, about 95%, or about 99%.Alternatively, or in combination, in some embodiments, the weight percentage of the binder solution in the conductive ink is about 0.5%, about 1%, about 2%, about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80%, about 90%, about 95%, or about 99% or less.

[0118] In some embodiments, the concentration of the binder solution is from about 0.5% to about 2%. In some embodiments, the concentration of the binder solution is at least about 0.5%. In some embodiments, the concentration of the binder solution is at most about 2%. In some embodiments, the concentration of the binder solution is about 0.5% to about 0.625%, about 0.5% to about 0.75%, about 0.5% to about 0.875%, about 0.5% to about 1%, about 0.5% to about 1.25%, about 0.5% to about 1.5%, about 0.5% to about 1.75%, about 0.5% to about 2%, about 0.625% to about 0.75%, about 0.625% to about 0.875%, about 0.625% to about 1%, about 0.625% to about 1.25%, about 0.625% to about 1.5%, about 0.625% to about 1.75%, about 0.625% to about 2%, about 0.75% to about 0.875%, about 0.75% about 1%, about 0.75% to about 1.25%, about 0.75% to about 1.5%, about 0.75% to about 1.75%, about 0.75% to about 2%, about 0.875% to about 1%, about 0.875% to about 1.25%, about 0.875% to about 1.5%, about 0.875% to about 1.75%, about 0.875% to about 2%, about 1% to about 1.25%, about 1% to about 1.5%, about 1% to about 1.75%, about 1% to about 2%, about 1.25% to about 1.5%, about 1.25% to about 1.75%, about 1.25% to about 2%, about 1.5% to about 1.75%, about 1.5% to about 2%, or about 1.75% to about 2%. In some embodiments, the concentration of the binder solution is about 0.5%, about 0.625%, about 0.75%, about 0.875%, about 1%, about 1.25%, about 1.5%, about 1.75%, or about 2%. In some embodiments, the concentration of the binder solution is at least about 0.5%, about 0.625%, about 0.75%, about 0.875%, about 1%, about 1.25%, about 1.5%, about 1.75%, or about 2%. In some embodiments, the concentration of the binder solution is no more than about 0.5%, about 0.625%, about 0.75%, about 0.875%, about 1%, about 1.25%, about 1.5%, about 1.75%, or about 2%.

[0119] In some embodiments, the reduced graphene oxide dispersion comprises reduced graphene oxide (RGO) and a second solvent.

[0120] In some embodiments, the weight percentage of the RGO dispersion in the conductive ink is between about 0.25% and about 1%. In some embodiments, the weight percentage of the RGO dispersion in the conductive ink is at least about 0.25%. In some embodiments, the weight percentage of the RGO dispersion in the conductive ink is at most about 1%. In some embodiments, the mass percentage of the RGO dispersion in the conductive ink is about 0.25% to about 0.375%, about 0.25% to about 0.5%, about 0.25% to about 0.625%, about 0.25% to about 0.75%, about 0.25% to about 1%, about 0.375% to about 0.5%, about 0.375% to about 0.625%, about 0.375% to about 0.75%, about 0.375% to about 1%, about 0.5% to about 0.625%, about 0.5% to about 0.75%, about 0.5% to about 1%, about 0.625% to about 0.75%, about 0.625% to about 1%, or about 0.75% to about 1%. In some embodiments, the weight percentage of the RGO dispersion in the conductive ink is about 0.25%, about 0.375%, about 0.5%, about 0.625%, about 0.75%, or about 1%. In some embodiments, the weight percentage of the RGO dispersion in the conductive ink is at least about 0.25%, about 0.375%, about 0.5%, about 0.625%, about 0.75%, or about 1%. In some embodiments, the weight percentage of the RGO dispersion in the conductive ink is no more than about 0.25%, about 0.375%, about 0.5%, about 0.625%, about 0.75%, or about 1%.

[0121] In some embodiments, the concentration by weight of RGO in the RGO dispersion is about 3% to about 12%. In some embodiments, the concentration by weight of RGO in the RGO dispersion is at least about 3%. In some embodiments, the concentration by weight of RGO in the RGO dispersion is up to about 12%. In some embodiments, the concentration by weight of RGO in the RGO dispersion is about 3% to about 4%, about 3% to about 5%, about 3% to about 6%, about 3% to about 7%, about 3% to about 8%, about 3% to about 9%, about 3% to about 10%, about 3% to about 11%, about 3% to about 12%, about 4% to about 5%, about 4% to about 6%, about 4% to about 7%, about 4% to about 8%, about 4% to about 9%, about 4% to about 10%, about 4% to about 11%, about 4% to about 12%, about 5% to about 6%, about 5% to about 7%, about 5% to about 8%, about 5% to about 9%, about 5% to about 10%, about 4% to about 11%, about 4% to about 12%, about 5% to about 6%, about 5% to about 7%, about 5% to about 8%, about 5% to about 9%, or about 5% to about 10%. 0%, about 5% to about 11%, about 5% to about 12%, about 6% to about 7%, about 6% to about 8%, about 6% to about 9%, about 6% to about 10%, about 6% to about 11%, about 6% to about 12%, about 7% to about 8%, about 7% to about 9%, about 7% to about 10%, about 7% to about 11%, about 7% to about 12%, about 8% to about 9%, about 8% to about 10%, about 8% to about 11%, about 8% to about 12%, about 9% to about 10%, about 9% to about 11%, about 9% to about 12%, about 10% to about 11%, about 10% to about 12%, or about 11% to about 12%. In some embodiments, the concentration by weight of RGO in the RGO dispersion is about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, or about 12%. In some embodiments, the concentration by weight of RGO in the RGO dispersion is at least about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, or about 12%. In some embodiments, the concentration by weight of RGO in the RGO dispersion is no more than about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, or about 12%.

[0122] In some embodiments, the weight percentage of RGO in the conductive ink is about 0.1% to about 99%. In some embodiments, the weight percentage of RGO in the conductive ink is at least about 0.1%. In some embodiments, the weight percentage of RGO in the conductive ink is up to about 99%. In some embodiments, the weight percentage of RGO in the conductive ink is about 0.1% to about 0.2%, about 0.1% to about 0.5%, about 0.1% to about 1%, about 0.1% to about 10%, about 0.1% to about 20%, about 0.1% to about 40%, about 0.1% to about 60%, about 0.1% to about 80%, about 0.1% to about 90%, about 0.1% to about 99%, about 0.2% to about 0.5%, about 0.2% to about 1%, about 0.2% to about 10%, about 0.2% to about 20%, about 0.2% to about 40%, about 0.2% to about 60%, about 0.2% to about 80%, about 0.2% to about 90%, about 0.2% to about 99%, about 0.5% to about 1%, about 0.5% to about 10%, about 0.5% to about 20%, about 0.5% to about 40%, about 0.5% to about 60%, about 0.5% to about 80%, about 0.5% to about 90%, about 0.5% to about 99%, about 1% to about 10%, about 1% to about 20%, about 1% to about 40%, about 1% to about 60%, about 1% to about 80%, about 1% to about 90%, about 1% to about 99%, about 10% to about 20%, about 10% to about 40%, about 10% to about 60%, about 10% to about 80%, about 10% to about 90%, about 10% to about 99%, about 20% to about 40%, about 20% to about 60%, about 20% to about 80%, about 20% to about 90%, about 20% to about 99%, about 40% to about 60%, about 40% to about 80%, about 40% to about 90%, about 40% to about 99%, about 60% to about 80%, about 60% to about 90%, about 60% to about 99%, about 80% to about 90%, about 80% to about 99%, or about 90% to about 99%. In some embodiments, the mass percentage of RGO in the conductive ink is about 0.1%, about 0.2%, about 0.5%, about 1%, about 10%, about 20%, about 40%, about 60%, about 80%, about 90%, or about 99%. In some embodiments, the mass percentage of RGO in the conductive ink is at least about 0.1%, about 0.2%, about 0.5%, about 1%, about 10%, about 20%, about 40%, about 60%, about 80%, about 90%, or about 99%. In some embodiments, the mass percentage of RGO in the conductive ink is no more than about 0.1%, about 0.2%, about 0.5%, about 1%, about 10%, about 20%, about 40%, about 60%, about 80%, about 90%, or about 99%.

[0123] In some embodiments, the conductive additive comprises a carbon-based material. In some embodiments, the carbon-based material comprises paracrystalline carbon. In some embodiments, the paracrystalline carbon comprises carbon black, acetylene black, channel black, furnace black, lamp black, thermal black, or any combination thereof.

[0124] In some embodiments, the conductive additive comprises silver, hi some embodiments, the silver comprises silver nanoparticles, silver nanorods, silver nanowires, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or any combination thereof.

[0125] In some embodiments, the weight percentage of the conductive additive in the conductive ink is between about 2% and about 99%. In some embodiments, the weight percentage of the conductive additive in the conductive ink is at least about 2%. In some embodiments, the weight percentage of the conductive additive in the conductive ink is at most about 99%. In some embodiments, the weight percentage of the conductive additive in the conductive ink is between about 2% and about 5%, between about 2% and about 10%, between about 2% and about 20%, between about 2% and about 30%, between about 2% and about 40%, between about 2% and about 50%, between about 2% and about 60%, between about 2% and about 70%, between about 2% and about 80%, between about 2% and about 90%, between about 2% and about 99%, between about 5% and about 10%, between about 5% and about 20%, between about 5% and about 30%, between about 5% and about 40%, between about 5% to about 50%, about 5% to about 60%, about 5% to about 70%, about 5% to about 80%, about 5% to about 90%, about 5% to about 99%, about 10% to about 20%, about 10% to about 30%, about 10% to about 40%, about 10% to about 50%, about 10% to about 60%, about 10% to about 70%, about 10% to about 80%, about 10% to about 90%, about 10% to about 99%, about 20% to about 30%, about 20% to about 40%, about 20% to about 5 0%, about 20% to about 60%, about 20% to about 70%, about 20% to about 80%, about 20% to about 90%, about 20% to about 99%, about 30% to about 40%, about 30% to about 50%, about 30% to about 60%, about 30% to about 70%, about 30% to about 80%, about 30% to about 90%, about 30% to about 99%, about 40% to about 50%, about 40% to about 60%, about 40% to about 70%, about 40% to about 80%, about 40% to about 90%, about 40% to about 99%, about 50% to about 60%, about 50% to about 70%, about 50% to about 80%, about 50% to about 90%, about 50% to about 99%, about 60% to about 70%, about 60% to about 80%, about 60% to about 90%, about 60% to about 99%, about 70% to about 80%, about 70% to about 90%, about 70% to about 99%, about 80% to about 90%, about 80% to about 99%, or about 90% to about 99%. The weight percentage of the additive is about 2%, about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80%, about 90%, or about 99%. In some embodiments, the weight percentage of the conductive additive in the conductive ink is at least about 2%, about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80%, about 90%, or about 99%. In some embodiments, the weight percentage of the conductive additive in the conductive ink is no more than about 2%, about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80%, about 90%, or about 99%.

[0126] Some embodiments further include a surfactant. In some embodiments, the surfactant includes an acid, a non-ionic surfactant, or any combination thereof. In some embodiments, the acid includes perfluorooctanoic acid, perfluorooctane sulfonate, perfluorohexane sulfonic acid, perfluorononanoic acid, perfluorodecanoic acid, or any combination thereof. In some embodiments, the non-ionic surfactant includes polyethylene glycol alkyl ether, octaethylene glycol monododecyl ether, pentaethylene glycol monododecyl ether, polypropylene glycol alkyl ether, glucoside alkyl ether, decyl glucoside, lauryl glucoside, octyl glucoside, polyethylene glycol octyl phenyl ether, dodecyl dimethylamine oxide, polyethylene glycol alkyl phenyl ether, polyethylene glycol octyl phenyl ether, Triton X-100, polyethylene glycol alkyl phenyl ether, nonoxynol-9, glycerol alkyl ester polysorbate, sorbitan alkyl ester, polyethoxylated tallow amine, Dynol 604, or any combination thereof. any combination of.

[0127] In some embodiments, the large amount of water in water-based conductive inks increases the surface tension of the ink. However, in some applications, such as inkjet printing, low and controlled surface tension and viscosity are required to maintain stable jetting from the printhead nozzles. In some embodiments, the addition of surfactants reduces the surface tension of the ink because as the surfactant units move to the water / air interface, their relative attraction weakens when the non-polar surfactant heads are exposed.

[0128] In some embodiments, the weight percentage of the surfactant in the conductive ink is between about 0.5% and about 10%. In some embodiments, the weight percentage of the surfactant in the conductive ink is at least about 0.5%. In some embodiments, the weight percentage of the surfactant in the conductive ink is at most about 10%. In some embodiments, the weight percentage of the surfactant in the conductive ink is about 0.5% to about 1%, about 0.5% to about 2%, about 0.5% to about 3%, about 0.5% to about 4%, about 0.5% to about 5%, about 0.5% to about 6%, about 0.5% to about 7%, about 0.5% to about 8%, about 0.5% to about 9%, about 0.5% to about 10%, about 1% to about 2%, about 1% to about 3%, about 1% to about 4%, about 1% to about 5%, about 1% to about 6%, about 1% to about 7%, about 1% to about 8%, about 1% to about 9%, about 1% to about 10%, about 2% to about 3%, about 2% to about 4%, about 2% to about 5%, about 2% to about 6%, about 2% to about 7%, or about 2% to about 8%. , about 2% to about 9%, about 2% to about 10%, about 3% to about 4%, about 3% to about 5%, about 3% to about 6%, about 3% to about 7%, about 3% to about 8%, about 3% to about 9%, about 3% to about 10%, about 4% to about 5%, about 4% to about 6%, about 4% to about 7%, about 4% to about 8%, about 4% to about 9%, about 4% to about 10%, about 5% The weight percentage of the surfactant in the conductive ink is about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 6%, about 5%, about 6%, about 7%, about 8%, about 9%, about 6%, about 7%, about 9%, about 10%, about 8%, about 9%, about 10 ... %, about 7%, about 8%, about 9%, or about 10%. In some embodiments, the weight percentage of surfactant in the conductive ink is about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, or about 10% or less.

[0129] Some embodiments further include an antifoaming agent, the antifoaming agent comprising an insoluble oil, a silicone, a glycol, a stearate, an organic solvent, Surfynol DF-1100, an alkyl polyacrylate, or any combination thereof. In some embodiments, the insoluble oil comprises a mineral oil, a vegetable oil, a white oil, or any combination thereof. In some embodiments, the silicone comprises a polydimethylsiloxane, a silicone glycol, a fluorosilicone, or any combination thereof. In some embodiments, the glycol comprises a polyethylene glycol, an ethylene glycol, a propylene glycol, or any combination thereof. In some embodiments, the stearate comprises a glycol stearate, a stearin, or any combination thereof. In some embodiments, the organic solvent comprises ethanol, isopropyl alcohol, N-methyl-2-pyrrolidone, cyclohexanone, terpineol, 3-methoxy-3-methyl-1-butanol, 4-hydroxyl-4-methyl-pentan-2-one, methyl isobutyl ketone, or any combination thereof.

[0130] In some embodiments, the weight percentage of the defoaming agent in the conductive ink is from about 0.5% to about 10%. In some embodiments, the weight percentage of the defoaming agent in the conductive ink is at least about 0.5%. In some embodiments, the weight percentage of the defoaming agent in the conductive ink is at most about 10%. In some embodiments, the mass percentage of the defoaming agent in the conductive ink is from about 0.5% to about 1%, from about 0.5% to about 2%, from about 0.5% to about 3%, from about 0.5% to about 4%, from about 0.5% to about 5%, from about 0.5% to about 6%, from about 0.5% to about 7%, from about 0.5% to about 8%, from about 0.5% to about 9%, from about 0.5% to about 10%, from about 1% to about 2%, from about 1% to about 3%, from about 1% to about 4%, from about 1% to about 5%, from about 1% to about 6%, from about 1% to about 7%, from about 1% to about 8%, from about 1% to about 9%, from about 1% to about 10%, from about 2% to about 3%, from about 2% to about 4%, from about 2% to about 5%, from about 2% to about 6%, from about 2% to about 7%, from about 2% to about 8%, About 2% to about 9%, about 2% to about 10%, about 3% to about 4%, about 3% to about 5%, about 3% to about 6%, about 3% to about 7%, about 3% to about 8%, about 3% to about 9%, about 3% to about 10%, about 4% to about 5%, about 4% to about 6%, about 4% to about 7%, about 4% to about 8%, about 4% to about 9%, about 4% to about 10%, about 5% to The mass percentage of the defoaming agent in the conductive ink is about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%. In some embodiments, the mass percentage of the defoaming agent in the conductive ink is about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, or about 10%. In some embodiments, the weight percentage of the defoaming agent in the conductive ink is at least about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, or about 10%. In some embodiments, the weight percentage of the defoaming agent in the conductive ink is no more than about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, or about 10%.

[0131] In some embodiments, the solids content by weight of the conductive ink is between about 2.5% and about 10.5%. In some embodiments, the solids content by weight of the conductive ink is at least about 2.5%. In some embodiments, the solids content by weight of the conductive ink is at most about 10.5%. In some embodiments, the solids content by weight of the conductive ink is between about 2.5% and about 3.5%, between about 2.5% and about 4.5%, between about 2.5% and about 5.5%, between about 2.5% and about 6.5%, between about 2.5% and about 7.5%, between about 2.5% and about 8.5%, between about 2.5% and about 9.5%, between about 2.5% and about 10.5%, between about 3.5% and about 4.5%, between about 3.5% and about 5.5%, between about 3.5% and about 6.5%, between about 3.5% and about 7.5%, between about 3. 5% to about 8.5%, about 3.5% to about 9.5%, about 3.5% to about 10.5%, about 4.5% to about 5.5%, about 4.5% to about 6.5%, about 4.5% to about 7.5%, about 4.5% to about 8.5%, about 4.5% to about 9.5%, about 4.5% to about 10.5%, about 5.5% to about 6.5%, about 5.5% to about 7.5%, about 5.5% to about 8.5%, about 5.5% to In some embodiments, the solids content by weight of the conductive ink is about 2.5%, about 3.5%, about 4.5%, about 5.5%, about 6.5%, about 7.5%, about 8.5%, about 9.5%, about 10.5%. In some embodiments, the solids content by weight of the conductive ink is about 2.5%, about 3.5%, about 4.5%, about 5.5%, about 6.5%, about 7.5%, about 8.5%, about 9.5%, or about 10.5%. In some embodiments, the solids content by weight of the conductive ink is at least about 2.5%, about 3.5%, about 4.5%, about 5.5%, about 6.5%, about 7.5%, about 8.5%, about 9.5%, or about 10.5%. In some embodiments, the solids content by weight of the conductive ink is no more than about 2.5%, about 3.5%, about 4.5%, about 5.5%, about 6.5%, about 7.5%, about 8.5%, about 9.5%, or about 10.5%.

[0132] In some embodiments, the viscosity of the conductive ink is from about 10 centipoise to about 10,000 centipoise. In some embodiments, the viscosity of the conductive ink is at least about 10 centipoise. In some embodiments, the viscosity of the conductive ink is at most about 10,000 centipoise. In some embodiments, the viscosity of the conductive ink is from about 10 centipoise to about 20 centipoise, from about 10 centipoise to about 50 centipoise, from about 10 centipoise to about 100 centipoise, from about 10 centipoise to about 200 centipoise, from about 10 centipoise to about 500 centipoise, from about 10 centipoise to about 1,000 centipoise, from about 10 centipoise to about 2,000 centipoise, from about 10 centipoise to about 5,000 centipoise, from about 10 centipoise to about 10,000 Centipoise, about 20 centipoise to about 50 centipoise, about 20 centipoise to about 100 centipoise, about 20 centipoise to about 200 centipoise, about 20 centipoise to about 500 centipoise, about 20 centipoise to about 1,000 centipoise, about 20 centipoise to about 2,000 centipoise, about 20 centipoise to about 5,000 centipoise, about 20 centipoise to about 10,000 centipoise, about 50 centipoise to about 100 centipoise, about 50 centipoise ~ about 200 centipoise, about 50 centipoise to about 500 centipoise, about 50 centipoise to about 1,000 centipoise, about 50 centipoise to about 2,000 centipoise, about 50 centipoise to about 5,000 centipoise, about 50 centipoise to about 10,000 centipoise, about 100 centipoise to about 200 centipoise, about 100 centipoise to about 500 centipoise, about 100 centipoise to about 1,000 centipoise, about 100 centipoise to about 2,000 centipoise, about 100 centipoise to about 5,000 centipoise, about 100 centipoise to about 10,000 centipoise, about 200 centipoise to about 500 centipoise, about 200 centipoise to about 1,000 centipoise, about 200 centipoise to about 2,000 centipoise, about 200 centipoise to about 5,000 centipoise, about 200 centipoise to about 10,000 centipoise, about 500 centipoise to about 1,000 centipoise, about 500 centipoise to about 2,000 centipoise, about 500 centipoise to about 5,000 centipoise, about 500 centipoise to about 10,000 centipoise, about 1,000 centipoise to about 2,000 centipoise, about 1,000 centipoise to about 5,000 centipoise, about 1,000 centipoise to about 10,000 centipoise, about 2,000 centipoise to about 5,000 centipoise, about 2,000 centipoise to about 10,000 centipoise, or about 5,000 centipoise to about 10,000 centipoise. In some embodiments, the viscosity of the conductive ink is about 10 centipoise, about 20 centipoise, about 50 centipoise, about 100 centipoise, about 200 centipoise, about 500 centipoise, about 1,000 centipoise, about 2,000 centipoise, about 5,000 centipoise, or about 10,000 centipoise. In some embodiments, the viscosity of the conductive ink is at least about 10 centipoise, about 20 centipoise, about 50 centipoise, about 100 centipoise, about 200 centipoise, about 500 centipoise, about 1,000 centipoise, about 2,000 centipoise, about 5,000 centipoise, or about 10,000 centipoise. In some embodiments, the viscosity of the conductive ink is no greater than about 10 centipoise, about 20 centipoise, about 50 centipoise, about 100 centipoise, about 200 centipoise, about 500 centipoise, about 1,000 centipoise, about 2,000 centipoise, about 5,000 centipoise, or about 10,000 centipoise.

[0133] In some embodiments, the conductive ink has a viscosity of about 2,300 centipoise to about 2,400 centipoise. In some embodiments, the conductive ink has a viscosity of at least about 2,300 centipoise. In some embodiments, the conductive ink has a viscosity of up to about 2,400 centipoise. In some embodiments, the conductive ink has a viscosity of about 2,300 centipoise to about 2,310 centipoise, about 2,300 centipoise to about 2,320 centipoise, about 2,300 centipoise to about 2,330 centipoise, about 2,300 centipoise to about 2,340 centipoise, about 2,300 centipoise to about 2,350 centipoise, about 2,300 centipoise to about 2,360 centipoise, about 2,300 centipoise to about 2,370 centipoise, about 2,300 centipoise about 2,380 centipoise, about 2,300 centipoise to about 2,390 centipoise, about 2,300 centipoise to about 2,400 centipoise, about 2,310 centipoise to about 2,320 centipoise, about 2,310 centipoise to about 2,330 centipoise, about 2,310 centipoise to about 2,340 centipoise, about 2,310 centipoise to about 2,350 centipoise, about 2,310 centipoise to about 2,360 centipoise, about 2,310 centipoise to about 2,3 70 centipoise, about 2,310 centipoise to about 2,380 centipoise, about 2,310 centipoise to about 2,390 centipoise, about 2,310 centipoise to about 2,400 centipoise, about 2,320 centipoise to about 2,330 centipoise, about 2,320 centipoise to about 2,340 centipoise, about 2,320 centipoise to about 2,350 centipoise, about 2,320 centipoise to about 2,360 centipoise, about 2,320 centipoise to about 2,370 centipoise 2,320 centipoise to about 2,380 centipoise, about 2,320 centipoise to about 2,390 centipoise, about 2,320 centipoise to about 2,400 centipoise, about 2,330 centipoise to about 2,340 centipoise, about 2,330 centipoise to about 2,350 centipoise, about 2,330 centipoise to about 2,360 centipoise, about 2,330 centipoise to about 2,370 centipoise, about 2,330 centipoise to about 2,380 centipoise, about 2,330 centipoise to about 2,390 centipoise, about 2,330 centipoise to about 2,400 centipoise, about 2,340 centipoise to about 2,350 centipoise, about 2,340 centipoise to about 2,360 centipoise, about 2,340 centipoise to about 2,370 centipoise, about 2,340 centipoise to about 2,380 centipoise about 2,340 centipoise to about 2,390 centipoise, about 2,340 centipoise to about 2,400 centipoise, about 2,350 centipoise to about 2,360 centipoise, about 2,350 centipoise to about 2,370 centipoise, about 2,350 centipoise to about 2,380 centipoise, about 2,350 centipoise to about 2,390 centipoise centipoise, about 2,350 centipoise to about 2,400 centipoise, about 2,360 centipoise to about 2,370 centipoise, about 2,360 centipoise to about 2,380 centipoise, about 2,360 centipoise to about 2,390 centipoise, about 2,360 centipoise to about 2,400 centipoise, about 2,370 centipoise to about In some embodiments, the conductive ink has a viscosity of about 2,300 centipoise, about 2,310 centipoise, about 2,380 centipoise, about 2,370 centipoise to about 2,390 centipoise, about 2,370 centipoise to about 2,400 centipoise, about 2,380 centipoise to about 2,390 centipoise, about 2,380 centipoise to about 2,400 centipoise, or about 2,390 centipoise to about 2,400 centipoise. 0 centipoise, about 2,320 centipoise, about 2,330 centipoise, about 2,340 centipoise, about 2,350 centipoise, about 2,360 centipoise, about 2,370 centipoise, about 2,380 centipoise, about 2,390 centipoise, or about 2,400 centipoise.

[0134] In some embodiments, the density of the conductive ink at a temperature of about 20° C. is about 2.5 g / cm 3 ~Approx. 10.5g / cm 3 In some embodiments, the density of the conductive ink at a temperature of about 20° C. is at least about 2.5 g / cm 3 In some embodiments, about 2 At a temperature of 0°C, the density of the conductive ink is up to about 10.5 g / cm 3 Some In an embodiment, the density of the conductive ink at a temperature of about 20° C. is about 2.5 g / cm 3 ~About 3. 5g / cm 3 , about 2.5g / cm 3 ~Approx. 4.5g / cm 3 , about 2.5g / cm 3 ~Approx. 5.5g / cm 3 , about 2.5g / cm 3 ~Approx. 6.5g / cm 3 , about 2.5g / cm 3 ~Approx. 7.5g / cm 3 , about 2.5g / cm 3 ~about 8.5g / cm 3 , about 2.5g / cm 3 ~Approx. 9.5g / cm 3 , about 2.5g / cm 3 ~Approx. 10.5g / cm 3 , about 3.5g / cm 3 ~Approx. 4.5g / cm 3 , about 3.5g / cm 3 ~Approx. 5.5g / cm 3 , about 3.5g / cm 3 ~Approx. 6.5g / cm 3 , about 3.5g / cm 3 ~Approx. 7.5g / cm 3 , about 3.5g / cm 3 ~about 8.5g / cm 3 , about 3.5g / cm 3 ~Approx. 9.5g / cm 3 , about 3.5g / cm 3 ~Approx. 10.5g / cm 3 , about 4.5g / cm 3 ~Approx. 5.5g / cm 3 , about 4.5g / cm 3 ~Approx. 6.5g / cm 3 , about 4.5g / cm 3 ~Approx. 7.5g / cm 3 , about 4.5g / cm 3 ~about 8.5g / cm 3 , about 4.5g / cm 3 ~Approx. 9.5g / cm3 , about 4.5g / cm 3 ~Approx. 10.5g / cm 3 , about 5.5g / cm 3 ~Approx. 6.5g / cm 3 , about 5.5g / cm 3 ~Approx. 7.5g / cm 3 , about 5.5g / cm 3 ~about 8.5g / cm 3 , about 5.5g / cm 3 ~Approx. 9.5g / cm 3 , about 5.5g / cm 3 ~Approx. 10.5g / cm 3 , about 6.5g / cm 3 ~Approx. 7.5g / cm 3 , about 6.5g / cm 3 ~about 8.5g / cm 3 , about 6.5g / cm 3 ~Approx. 9.5g / cm 3 , about 6.5g / cm 3 ~Approx. 10.5g / cm 3 , about 7.5g / cm 3 ~about 8.5g / cm 3 , about 7.5g / cm 3 ~Approx. 9.5g / cm 3 , about 7.5g / cm 3 ~Approx. 10.5g / cm 3 , about 8.5g / cm 3 ~Approx. 9.5g / cm 3 , about 8.5g / cm 3 ~Approx. 10.5g / cm 3 , or about 9.5 g / cm 3 ~Approx. 10.5g / cm 3 In some embodiments, the density of the conductive ink at a temperature of about 20° C. is Maximum approx. 10.5g / cm 3 In some embodiments, the conductivity at a temperature of about 20° C. The density of the ink is approximately 2.5g / cm 3 , about 3.5g / cm 3 , about 4.5g / cm 3 , about 5 .5g / cm 3 , about 6.5g / cm 3, about 7.5g / cm 3 , about 8.5g / cm 3 , about 9.5g / cm 3 , or about 10.5 g / cm 3 In some embodiments, the density of the conductive ink at a temperature of about 20° C. is at least about 2.5 g / cm 3 , about 3.5g / cm 3 , about 4.5g / cm 3 , about 5.5g / cm 3 , about 6.5g / cm 3 , about 7.5g / cm 3 , about 8.5g / cm 3 , about 9.5g / cm 3 , or about 10.5 g / cm 3 Some implementations In this state, the density of the conductive ink at a temperature of about 20° C. is about 2.5 g / cm 3 , about 3.5g / cm 3 , about 4.5g / cm 3 , about 5.5g / cm 3 , about 6.5g / cm 3 , about 7.5g / cm 3 , about 8.5g / cm 3 , about 9.5g / cm 3 , or about 10.5 g / cm 3 The following is the result.

[0135] Optionally, in some embodiments, the conductive ink may be about 40 μm thick. 2 / g ~ approx. 2,4 00m 2 Optionally, in some embodiments, the conductive ink has a surface area of ​​1 / g. is at least about 40m 2 Optionally, in some embodiments, the surface area is The conductive ink can be applied to a maximum of 2,400 m 2 1 / g of surface area. In some embodiments, the conductive ink is about 40 μm. 2 / g~about 80m 2 / g, approx. 40m 2 / g ~ approx. 120m2 / g, about 40m 2 / g~about 240m 2 / g, about 40m 2 / g~about 480m 2 / g, about 40m 2 / g~about 1,000m 2 / g, about 40m 2 / g~about 1,400m 2 / g, about 40m 2 / g~about 1,800m 2 / g, about 40m 2 / g~about 2,200m 2 / g, about 40m 2 / g~about 2,400m 2 / g, about 80m 2 / g~about 120m 2 / g, about 80m 2 / g~about 240m 2 / g, about 80m 2 / g~about 480m 2 / g, about 80m 2 / g~about 1,000m 2 / g, About 80m 2 / g~about 1,400m 2 / g, about 80m 2 / g~about 1,800m 2 / g, about 80m 2 / g~about 2,200m 2 / g, about 80m 2 / g~about 2,400m 2 / g, about 120m 2 / g ~About 240m 2 / g, about 120m 2 / g~about 480m 2 / g, about 120m 2 / g~about 1,000m 2 / g, about 120m 2 / g~about 1,400m 2 / g, about 120m 2 / g~about 1,800m 2 / g, about 120m 2 / g~about 2,200m 2 / g, about 120m 2 / g ~ approx. 2,400m 2 / g, about 240m 2 / g ~ approx. 480m 2 / g, approx. 240m 2 / g ~ approx. 1,000m 2 / g, approx. 240m 2 / g ~ approx. 1,400m 2 / g, approx. 240m 2 / g ~ approx. 1,800m 2 / g, approx. 240m 2 / g ~ approx. 2,200m 2 / g, approx. 240m 2 / g ~ approx. 2,400m 2 / g, approx. 480m 2 / g ~ approx. 1,000m 2 / g, approx. 480m 2 / g ~ approx. 1,400m 2 / g, approx. 480m 2 / g ~ approx. 1,800m 2 / g, approx. 480m 2 / g ~ approx. 2,200m 2 / g, approx. 480m 2 / g ~ approx. 2,400m 2 / g, approx. 1,000m 2 / g ~ approx. 1,400m 2 / g, approx. 1,000m 2 / g ~ approx. 1,800m 2 / g, approx. 1,000m 2 / g ~ approx. 2,200m 2 / g, approx. 1,000m 2 / g ~ approx. 2,400m 2 / g, approx. 1,400m 2 / g ~ approx. 1,800m 2 / g, approx. 1,40 0m 2 / g ~ approx. 2,200m 2 / g, approx. 1,400m 2 / g ~ approx. 2,400m 2 / g, approx. 1,800m 2 / g ~ approx. 2,200m 2 / g, approx. 1,800m 2 / g ~ approx. 2,400m 2 / g, or approximately 2,200 m 2 / g ~ approx. 2,400m2 Optionally, in some embodiments, the conductive ink has a surface area of ​​about 40 m 2 / g, approx. 80m 2 / g, approx. 120m 2 / g, about 240m 2 / g, approx. 480m 2 / g, approx. 1,000m 2 / g, approx. 1,400m 2 / g, approx. 1,800m 2 / g, approx. 2,200m 2 / g, or approximately 2,400 m 2 / g surface area Optionally, in some embodiments, the conductive ink has a thickness of at least about 40 μm. 2 / g, approx. 80m 2 / g, approx. 120m 2 / g, approx. 240m 2 / g, approx. 480m 2 / g, approx. 1,000m 2 / g, approx. 1,400m 2 / g, approx. 1,800m 2 / g, approx. 2,200m 2 / g, or approximately 2,400 m 2 Optionally, in some embodiments, the conductor has a surface area of ​​1 / g. The conductive ink is approximately 40 m 2 / g, approx. 80m 2 / g, approx. 120m 2 / g, approx. 240m 2 / g, approx. 480m 2 / g, approx. 1,000m 2 / g, approx. 1,400m 2 / g, approx. 1,800m 2 / g, approx. 2,200m 2 / g, or approximately 2,400 m 2 / g or less.

[0136] Optionally, in some embodiments, the conductive ink has a conductivity of about 400 S / m to about 1,600 S / m. Optionally, in some embodiments, the conductive ink has a conductivity of at least about 400 S / m. Optionally, in some embodiments, the conductive ink has a conductivity of up to about 1,600 S / m. Optionally, in some embodiments, the conductive ink may have a viscosity of about 400 S / m to about 500 S / m, about 400 S / m to about 600 S / m, about 400 S / m to about 700 S / m, about 400 S / m to about 800 S / m, about 400 S / m to about 900 S / m, about 400 S / m to about 1,000 S / m, about 400 S / m to about 1,200 S / m, about 400 S / m to about 1,400 S / m, about 400 S / m to about 1,600 S / m, about 500 S / m to about 600 S / m, about 500 S / m ~700S / m, 500S / m~800S / m, 500S / m~900S / m, 500S / m~1,000S / m, 500S / m~1,200S / m, 500S / m~1,400S / m, 500S / m m ~ approx. 1,600S / m, approx. 600S / m ~ approx. 700S / m, approx. 600S / m ~ approx. 800S / m, approx. 600S / m ~ approx. 900S / m, approx. 600S / m ~ approx. 1,000S / m, approx. 600S / m ~ approx. 1,200S / m, approx. 600S / m m ~ approx. 1,400S / m, approx. 600S / m ~ approx. 1,600S / m, approx. 700S / m ~ approx. 800S / m, approx. 700S / m ~ approx. 900S / m, approx. 700S / m ~ approx. 1,000S / m, approx. 700S / m ~ approx. 1,200S / m, approx. 70 0S / m ~ approx. 1,400S / m, approx. 700S / m ~ approx. 1,600S / m, approx. 800S / m ~ approx. 900S / m, approx. 800S / m ~ approx. 1,000S / m, approx. 800S / m ~ approx. 1,200S / m, approx. 800S / m ~ approx. 1,400S / m, about 800S / m to about 1,600S / m, about 900S / m to about 1,000S / m, about 900S / m to about 1,200S / m, about 900S / m to about 1,400S / m, about 900S / m to about 1,600S / m, about 1,000S / m to about 1,200S / m, about 1,000S / m to about 1,400S / m, about 1,000S / m to about 1,600S / m, about 1,200S / m to about 1,400S / m, about 1,200S / m to about 1,600S / m, or about 1,400S / m Optionally, in some embodiments, the conductive ink has a conductivity of about 400 S / m, about 500 S / m, about 600 S / m, about 700 S / m, about 800 S / m, about 900 S / m, about 1,000 S / m, about 1,200 S / m, about 1,400 S / m, or about 1,600 S / m. Optionally, in some embodiments, the conductive ink has a conductivity of at least about 400 S / m, about 500 S / m, about 600 S / m, about 700 S / m, about 800 S / m, about 900 S / m, about 1,000 S / m, about 1,200 S / m, about 1,400 S / m, or about 1,600 S / m. Optionally, in some embodiments, the conductive ink has a conductivity of about 400 S / m, about 500 S / m, about 600 S / m, about 700 S / m, about 800 S / m, about 900 S / m, about 1,000 S / m, about 1,200 S / m, about 1,400 S / m, or about 1,600 S / m or less.

[0137] Optionally, in some embodiments, the conductive ink has a C:O mass ratio of about 2:1 to about 40:1. Optionally, in some embodiments, the conductive ink has a C:O mass ratio of at least about 2:1. Optionally, in some embodiments, the conductive ink has a C:O mass ratio of up to about 40:1. Optionally, in some embodiments, the conductive ink has a C:O mass ratio of about 2:1 to about 4:1, about 2:1 to about 6:1, about 2:1 to about 8:1, about 2:1 to about 10:1, about 2:1 to about 15:1, about 2:1 to about 20:1, about 2:1 to about 25:1, about 2:1 to about 30:1, about 2:1 to about 34:1, about 2:1 to about 40:1, about 4:1 to about 6:1, about 4:1 to about 8:1, about 4:1 to about 10:1, about 4:1 to about 15:1, about 4:1 to about 20:1, about 4:1 to about 25:1, about 4:1 to about 30:1, about 4:1 to about 34:1, about 4:1 to about 40:1, about 6:1 to about 8:1, about 6:1 to about 10:1, about 6:1 to about 15:1, about 6:1 to about 20:1, about 6:1 to about 25:1, about 6:1 to about 30:1, about 6:1 to about 34:1, about 6:1 to about 40:1, about 8:1 to about 10:1, about 8:1 to about 15:1, about 8:1 to about 20:1, about 8:1 to about 25:1, about 8:1 to about 30:1, about 8:1 to about 34:1, about 8:1 to about 40:1, about 10:1 to about 15:1, about 10:1 to about 20:1, about 10:1 to about 25:1, about 10:1 to about 30:1, about 10:1 to about 34:1, about 10:1 to about 40:1, about 15:1 to about 20:1, about 15:1 to about 25:1, about 15: The C:O mass ratio may be from about 1 to about 30:1, from about 15:1 to about 34:1, from about 15:1 to about 40:1, from about 20:1 to about 25:1, from about 20:1 to about 30:1, from about 20:1 to about 34:1, from about 20:1 to about 40:1, from about 25:1 to about 30:1, from about 25:1 to about 34:1, from about 25:1 to about 40:1, from about 30:1 to about 34:1, from about 30:1 to about 40:1, or from about 34:1 to about 40:1. Optionally, in some embodiments, the conductive ink has a C:O mass ratio of about 2:1, about 4:1, about 6:1, about 8:1, about 10:1, about 15:1, about 20:1, about 25:1, about 30:1, about 34:1, or about 40:1.Optionally, in some embodiments, the conductive ink has a C:O mass ratio of at least about 2:1, about 4:1, about 6:1, about 8:1, about 10:1, about 15:1, about 20:1, about 25:1, about 30:1, about 34:1, or about 40:1. Optionally, in some embodiments, the conductive ink has a C:O mass ratio of no more than about 2:1, about 4:1, about 6:1, about 8:1, about 10:1, about 15:1, about 20:1, about 25:1, about 30:1, about 34:1, or about 40:1.

[0138] In some embodiments, the conductive ink is a conductive graphene hydrate.

[0139] In some embodiments, the graphene ink has a resistivity of between about 0.01 ohm / sq / mil and about 60 ohm / sq / mil when dry. In some embodiments, the graphene ink has a resistivity of at least about 0.01 ohm / sq / mil when dry. In some embodiments, the graphene ink has a resistivity of up to about 60 ohm / sq / mil when dry. In some embodiments, the graphene ink has a resistivity of between about 0.01 ohm / sq / mil and about 0.05 ohm / sq / mil when dry, between about 0.01 ohm / sq / mil and about 0.1 ohm / sq / mil when dry. 0.01 ohms / sq / mil to about 0.5 ohms / sq / mil, about 0.01 ohms / sq / mil to about 1 ohm / sq / mil, about 0.01 ohms / sq / mil to about 5 ohms / sq / mil, about 0.01 ohms / sq / mil to about 10 ohms / sq / mil, about 0.01 ohms / sq / mil to about 20 ohms / sq / mil, about 0.01 ohms / sq / mil to about 30 ohms / sq / mil, about 0.01 ohms / sq / mil to about 40 ohms / sq / mil, about 0.01 ohms / sq / mil to about 50 ohms / sq / mil, about 0.01 ohms / sq / mil / mil to about 60 ohms / sq / mil, about 0.05 ohms / sq / mil to about 0.1 ohms / sq / mil, about 0.05 ohms / sq / mil to about 0.5 ohms / sq / mil, about 0.05 ohms / sq / mil to about 1 ohm / sq / mil, about 0.05 ohms / sq / mil to about 5 ohms / sq / mil, about 0.05 ohms / sq / mil to about 10 ohms / sq / mil, about 0.05 ohms / sq / mil to about 20 ohms / sq / mil, about 0.05 ohms / sq / mil to about 30 ohms / sq / mil, about 0.05 ohms / sq / mil to about 40 ohms / sq / mil, about .05 ohms / sq / mil to about 50 ohms / sq / mil, about 0.05 ohms / sq / mil to about 60 ohms / sq / mil, about 0.1 ohms / sq / mil to about 0.5 ohms / sq / mil, about 0.1 ohms / sq / mil to about 1 ohm / sq / mil, about 0.1 ohms / sq / mil to about 5 ohms / sq / mil, about 0.1 ohms / sq / mil to about 10 ohms / sq / mil, about 0.1 ohms / sq / mil to about 20 ohms / sq / mil, about 0.1 ohms / sq / mil to about 30 ohms / sq / mil, about 0.1 ohms / sq / mil to about 40 ohms / sq / mil, about 0.1 ohms / sq / mil to about 50 ohms / sq / mil, about 0.1 ohms / sq / mil to about 60 ohms / sq / mil, about 0.5 ohms / sq / mil to about 1 ohm / sq / mil, about 0.5 ohms / sq / mil to about 5 ohms / sq / mil, about 0.5 ohms / sq / mil to about 10 ohms / sq / mil, about 0.5 ohms / sq / mil to about 20 ohms / sq / mil, about 0.5 ohms / sq / mil to about 30 ohms / sq / mil, about 0.5 ohms / sq / mil to about 40 ohms / sq / mil, about 0.5 ohms / sq / mil to about 50 ohms / sq / mil, about 0.5 ohms / sq / mil to about 60 ohms / sq / mil, about 1 ohm / sq / mil to about 5 ohms / sq / mil, about 1 ohm / sq / mil to about 10 ohms / sq / mil, about 1 ohm / sq / mil to about 20 ohms / sq / mil, about 1 ohm / sq / mil to about 30 ohms / sq / mil, about 1 ohm / sq / mil to about 40 ohms / sq / mil, about 1 ohm / sq / mil to about 50 ohms / sq / mil, about 1 ohm / sq / mil to about 6 0 ohms / sq / mil, about 5 ohms / sq / mil to about 10 ohms / sq / mil, about 5 ohms / sq / mil to about 20 ohms / sq / mil, about 5 ohms / sq / mil to about 30 ohms / sq / mil, about 5 ohms / sq / mil to about 40 ohms / sq / mil, about 5 ohms / sq / mil to about 50 ohms / sq / mil, about 5 ohms / sq / mil to about 60 ohms / sq / mil, about 10 ohms / sq / mil to about 20 ohms / sq / mil, About 10 ohms / sq / mil to about 30 ohms / sq / mil, about 10 ohms / sq / mil to about 40 ohms / sq / mil, about 10 ohms / sq / mil to about 50 ohms / sq / mil, about 10 ohms / sq / mil to about 60 ohms / sq / mil, about 20 ohms / sq / mil to about 30 ohms / sq / mil, about 20 ohms / sq / mil to about 40 ohms / sq / mil, about 20 ohms / sq / mil to about 50 ohms / sq / mil, about 20 ohms / sq / mil to about 50 ohms / sq / mil In some embodiments, the resistivity is from about 30 ohms / sq / mil to about 60 ohms / sq / mil, from about 30 ohms / sq / mil to about 40 ohms / sq / mil, from about 30 ohms / sq / mil to about 50 ohms / sq / mil, from about 30 ohms / sq / mil to about 60 ohms / sq / mil, from about 40 ohms / sq / mil to about 50 ohms / sq / mil, from about 40 ohms / sq / mil to about 60 ohms / sq / mil, or from about 50 ohms / sq / mil to about 60 ohms / sq / mil. In some embodiments, the graphene ink has a resistivity when dry of about 0.01 ohm / sq / mil, about 0.05 ohm / sq / mil, about 0.1 ohm / sq / mil, about 0.5 ohm / sq / mil, about 1 ohm / sq / mil, about 5 ohm / sq / mil, about 10 ohm / sq / mil, about 20 ohm / sq / mil, about 30 ohm / sq / mil, about 40 ohm / sq / mil, about 50 ohm / sq / mil, or about 60 ohm / sq / mil. In some embodiments, the graphene ink has a resistivity when dry of at least about 0.01 ohm / sq / mil, about 0.05 ohms / sq / mil, approx. 0.1 ohms / sq / mil, approx. 0.5 ohms / sq. In some embodiments, the resistivity is about 1 ohm / sq / mil, about 1 ohm / sq / mil, about 5 ohm / sq / mil, about 10 ohm / sq / mil, about 20 ohm / sq / mil, about 30 ohm / sq / mil, about 40 ohm / sq / mil, about 50 ohm / sq / mil, or about 60 ohm / sq / mil. In some embodiments, the graphene ink when dry has a resistivity of at most about 0.01 ohm / sq / mil, about 0.05 ohm / sq / mil, about 0.1 ohm / sq / mil, about 0.5 ohm / sq / mil, about 1 ohm / sq / mil, about 5 ohm / sq / mil, about 10 ohm / sq / mil, about 20 ohm / sq / mil, about 30 ohm / sq / mil, about 40 ohm / sq / mil, about 50 ohm / sq / mil, or about 60 ohm / sq / mil.

[0140] Those skilled in the art will recognize improvements and modifications to this disclosure, and all such improvements and modifications are deemed to be within the scope of the concepts disclosed herein. [Brief description of the drawings]

[0141] The novel features of the present disclosure are set forth with particularity in the appended claims. A better understanding of the features and advantages of the present disclosure will be obtained by reference to the following detailed description that sets forth illustrative embodiments, in which the principles of the disclosure are utilized, and in which:

[0142] [Figure 1] 1 shows an exemplary diagram of the structure of a conductive dispersion according to one or more embodiments described herein. [Diagram 2] 1 shows an exemplary image of a conductive carbon-based adhesive according to one or more embodiments described herein. [Diagram 3] 1 shows an exemplary image of a first package of conductive carbon-based adhesive according to one or more embodiments described herein. [Figure 4] 1 shows an exemplary image of a second package of conductive carbon-based adhesive according to one or more embodiments described herein. [Diagram 5] FIG. 1 shows an example image of an electronic circuit comprising a battery powering different light emitting diodes (LEDs) through wires formed by a conductive carbon-based adhesive deposited on paper, according to one or more embodiments described herein. [Figure 6] 1 shows an example image of an electronic circuit in which a battery simultaneously powers three different LEDs through wires formed by a conductive carbon-based adhesive deposited on paper, according to one or more embodiments described herein. [Figure 7] 1 shows an exemplary image of an electronic component being bonded to a circuit board using a conductive carbon-based adhesive according to one or more embodiments described herein. [Figure 8] 8A shows an exemplary image of a film with a conductive carbon-based adhesive deposited on a flexible substrate, according to one or more embodiments described herein. FIG. 8B shows an exemplary image of a folded film with a conductive carbon-based adhesive deposited on a flexible substrate, according to one or more embodiments described herein. [Figure 9] 1 shows an exemplary image of an exemplary apparatus for testing the electrical properties of a conductive carbon-based adhesive. [Figure 10] 1 shows a graph of a voltage-current curve for an exemplary conductive carbon-based adhesive according to one or more embodiments described herein. [Figure 11] 1 shows a graph of voltage-current curves for different exemplary conductive adhesive films made with different amounts of conductive additive according to one or more embodiments described herein. [Figure 12] 1 shows an image of a contact pad with an exemplary conductive carbon-based adhesive according to one or more embodiments described herein. [Figure 13] Figure 13A shows a graph of the sheet resistance of an exemplary first conductive carbon-based adhesive, Figure 13B shows a graph of the sheet resistance of an exemplary second conductive carbon-based adhesive, and Figure 13C shows a graph of the sheet resistance of an exemplary third conductive carbon-based adhesive. [Figure 14A]1 shows a bar graph of sheet resistance of an exemplary conductive adhesive according to one or more embodiments described herein. [Figure 14B] 1 shows a graph comparing the resistivity of graphene and metal wires according to one or more embodiments described herein. [Figure 15A] 1 shows images of an exemplary apparatus for testing the electrical properties of a film including an exemplary conductive carbon-based adhesive under different bending angles, according to one or more embodiments described herein. [Figure 15B] 1 shows an image of an exemplary apparatus for testing the electrical properties of an unbent film including an exemplary conductive carbon-based adhesive according to one or more embodiments described herein. [Figure 15C] 1 shows an image of an exemplary apparatus for testing the electrical properties of a bent film including an exemplary conductive graphene adhesive according to one or more embodiments described herein. [Figure 16] 16A shows a diagram of an exemplary apparatus for testing the electrical properties of an unbent film including a conductive carbon-based adhesive according to one or more embodiments described herein. FIG. 16B shows a diagram of an exemplary apparatus for testing the electrical properties of a bent film including a conductive carbon-based adhesive according to one or more embodiments described herein. [Figure 17] Figure 17A shows a diagram of a film with a conductive carbon-based adhesive in a convex bend according to one or more embodiments described herein. Figure 17B shows an example graph showing the relationship between convex bend distance and resistance change for an example film including a conductive carbon-based adhesive. [Figure 18] Figure 18A shows a diagram of a film with a conductive carbon-based adhesive in a concave bend according to one or more embodiments described herein. Figure 18B shows an example graph showing the relationship between the concave bend distance and the resistance change for an example film including a conductive carbon-based adhesive. [Figure 19]19A shows an exemplary graph illustrating the relationship between twist angle and resistance change for an exemplary conductive carbon-based adhesive film including a conductive carbon-based adhesive according to one or more embodiments described herein. FIG. 19B shows an exemplary current-voltage graph for an exemplary film with a conductive carbon-based adhesive twisted at 0 degrees and 720 degrees. [Figure 20] 1 shows images of an exemplary film including a conductive carbon-based adhesive at different twist angles according to one or more embodiments described herein. [Figure 21] 13A-13C show images of an exemplary conductive carbon based adhesive sample preparation for tensile strength testing. [Figure 22A] FIG. 1 illustrates a tensile strength diagram according to one or more embodiments described herein. [Figure 22B] 13 shows an image of a tensile hook of a prepared tensile strength test specimen of an exemplary conductive carbon based adhesive. [Figure 22C] 1 shows an image of a bonded joint of a prepared tensile strength test specimen of an exemplary conductive carbon-based adhesive. [Figure 23A] 1 shows a first image of an exemplary conductive carbon based adhesive sample preparation for shear strength testing. [Figure 23B] FIG. 13 shows a second image of an exemplary conductive carbon based adhesive sample preparation for shear strength testing. [Figure 24] Figure 24A shows a shear strength diagram according to one or more embodiments described herein, and Figure 24B shows an image of a bonded joint of a prepared shear strength test specimen of an exemplary conductive carbon-based adhesive. [Diagram 25] 25A shows a first image of an exemplary adhesive tensile strength test specimen preparation without conductive graphene, and FIG. 25B shows a second image of an exemplary adhesive tensile strength test specimen preparation without conductive graphene, according to one or more embodiments described herein. [Figure 26] 13A-13D show images of prepared tensile and shear stress samples of an exemplary conductive carbon-based adhesive and an exemplary adhesive without conductive graphene, according to one or more embodiments described herein. [Figure 27] 1 shows a first image of a tensile and shear stress testing apparatus according to one or more embodiments described herein. [Figure 28] 1 shows a second image of a tensile and shear stress testing apparatus according to one or more embodiments described herein. [Figure 29] 1 illustrates a graph showing the relationship between temperature and cure time of an epoxy as it changes from a liquid state to a gel state to a solid state according to one or more embodiments described herein. [Diagram 30] 1 shows a flowchart of an exemplary method for preparing a conductive carbon-based epoxy according to one or more embodiments described herein. [Diagram 31] FIG. 1 shows a diagram of an exemplary resin composition according to one or more embodiments described herein. [Diagram 32] FIG. 1 shows a diagram of an exemplary curing agent composition according to one or more embodiments described herein. [Figure 33A] 1 illustrates an image of two parts of an exemplary conductive carbon-based epoxy according to one or more embodiments described herein. [Figure 33B] 1 shows an image of an exemplary dispense and mix package of a two-part conductive carbon-based epoxy including a resin and a hardener, according to one or more embodiments described herein. [Figure 33C] 1 illustrates images of dispensing and mixing of an exemplary conductive carbon-based epoxy according to one or more embodiments described herein. [Diagram 34] FIG. 13 shows another image of an exemplary dispense and mix package of a two-part conductive carbon-based epoxy including a resin and a hardener, according to one or more embodiments described herein. [Diagram 35] 1 shows an exemplary image of a substrate coated with an exemplary conductive carbon-based epoxy according to one or more embodiments described herein. [Diagram 36]36A shows a first image of an exemplary apparatus for forming a conductive carbon-based epoxy according to one or more embodiments described herein, and FIG 36B shows a second image of an exemplary apparatus for forming a conductive carbon-based epoxy according to one or more embodiments described herein. [Figure 37] Figure 37A shows an image of an open circuit comprising a battery, three LEDs, a wire, and a film comprising an exemplary conductive carbon-based epoxy, according to one or more embodiments described herein. Figure 37B shows an image of a closed circuit comprising a battery, three LEDs, a wire, and a film comprising an exemplary conductive carbon-based epoxy, according to one or more embodiments described herein. [Figure 38] 1 shows an image of an apparatus for testing the electrical properties of an exemplary conductive carbon-based epoxy, according to one or more embodiments described herein. [Figure 39] 1 shows a current-voltage graph of an exemplary conductive carbon-based epoxy according to one or more embodiments described herein. [Diagram 40] 40A shows a graph illustrating the sheet resistance at four locations of an exemplary conductive carbon-based epoxy according to one or more embodiments described herein, and FIG 40B shows a bar graph of the sheet resistance of two conductive graphene epoxies with different amounts of carbon additive according to one or more embodiments described herein. [Figure 41A] 1 illustrates a graph showing the relationship between twist angle and resistance change for an exemplary conductive carbon-based epoxy, according to one or more embodiments described herein. [Figure 41B] 1 illustrates a current-voltage graph of an exemplary conductive carbon-based epoxy twisted at 0 degrees and 720 degrees according to one or more embodiments described herein. [Diagram 42]42A shows an image of a test setup for measuring the resistance change of an exemplary conductive carbon-based epoxy without tensile strain, according to one or more embodiments described herein, and FIG 42B shows an image of a test setup for measuring the resistance change of an exemplary conductive carbon-based epoxy with tensile strain, according to one or more embodiments described herein. [Diagram 43] 1 illustrates a graph depicting the relationship between tensile strain and resistance change for an exemplary conductive carbon-based epoxy, according to one or more embodiments described herein. [Diagram 44] 44A shows a diagram of a film with a conductive carbon-based epoxy having a convex bend according to one or more embodiments described herein, and FIG. 44B shows a graph illustrating the relationship between convex bend distance and resistance change for an exemplary film with a conductive carbon-based epoxy. [Diagram 45] 45A shows a diagram of a film with a conductive carbon-based epoxy undergoing a concave bend according to one or more embodiments described herein, and FIG 45B shows an example graph illustrating the relationship between concave bend distance and resistance change for an example film with a conductive carbon-based epoxy. [Diagram 46] 1 shows an image of an exemplary conductive ink according to one or more embodiments described herein. [Figure 47] 1 shows diagrams of silver nanostructures and microstructures with less than percolation, a 15% percolation threshold, and a less than 1% percolation threshold, according to one or more embodiments described herein. [Figure 48] 1 shows transmission electron microscope (TEM) images of exemplary silver nanowires and nanoparticles according to one or more embodiments described herein. [Figure 49] 1 shows TEM images of exemplary long silver nanowires and nanoparticles according to one or more embodiments described herein. [Figure 50A] 1 shows a first TEM image of an exemplary silver nanowire according to one or more embodiments described herein. [Figure 50B] 1 shows a second TEM image of an exemplary silver nanowire according to one or more embodiments described herein. [Figure 51A] 1 shows a first image of an exemplary apparatus for forming silver nanowires according to one or more embodiments described herein. [Figure 51B] 1 shows a second image of an exemplary apparatus for forming silver nanowires according to one or more embodiments described herein. [Figure 51C] 13 shows a third image of an exemplary apparatus for forming silver nanowires according to one or more embodiments described herein. [Fig. 51D] 13 shows a fourth image of an exemplary apparatus for forming silver nanowires according to one or more embodiments described herein. [Figure 51E] 13 shows a fifth image of an exemplary apparatus for forming silver nanowires according to one or more embodiments described herein. [Figure 52] Figure 52A shows an image of an exemplary sealed solvothermal chamber for forming silver nanoparticles, and Figure 52B shows an image of an exemplary silver dispersion formed in a solvothermal chamber by a method according to the present disclosure. [Diagram 53] 1 shows optical microscope images of an exemplary film comprising gas and silver produced in a solvothermal chamber by a method according to the present disclosure. [Figure 54] 6 shows TEM images of exemplary silver nanowires and nanoparticles formed with a binder. [Figure 55] 4 shows images of silver dispersions formed with and without a binder. [Figure 56] Images of exemplary stable and non-stable silver dispersions are shown, where the silver dispersion on the left remains stable after one week, while the silver dispersion on the right separates into solution and precipitate. [Figure 57] 1 shows an image of an exemplary conductive ink according to one or more embodiments described herein. [Figure 58]1 shows a chart comparing exemplary inks of the present disclosure against currently available conductive inks according to one or more embodiments described herein. [Figure 59A] 1 illustrates an exemplary image of adhering an electronic component to a circuit board using conductive ink, according to one or more embodiments described herein. [Figure 59B] 1 illustrates an exemplary first image of securing a defogger using conductive ink, according to one or more embodiments described herein. [Figure 59C] 1 illustrates an exemplary first image of securing a defogger using conductive ink, according to one or more embodiments described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0143] Certain aspects of the present disclosure relate to conductive adhesives and inks comprising carbon- and silver-based materials, such as graphene and graphene / carbon composites, that exhibit excellent electrical conductivity, thermal properties, durability, low cure temperatures, mechanical flexibility, and reduced environmental impact.

[0144] Currently, lead-based soldering materials are used to electrically connect two or more components, but such products can be toxic and environmentally unfriendly. However, alternative conductive materials (e.g., graphene and silver) offer similar or better efficacy without the dangers and side effects of current solders. Unlike toxic lead solders, conductive adhesives and inks made with graphene are carbon-based, therefore non-toxic, and curing occurs at room temperature, making them environmentally friendly. Such conductive adhesives and inks can use additives to enable a variety of applications and improved electrical properties.

[0145] In some existing methods of electronics manufacturing, lead-based solders are applied to attach and bond various electronic components together or to printed circuit boards. However, due to the health and environmental impacts of lead, global regulations have been enacted to restrict the use of lead. In addition, lead-based soldering has limited patterning resolution and may not be able to keep up with the shrinking scale of components in modern electronics packages. Furthermore, lead-based solders may be too brittle and not durable to be used in flexible electronic devices. Finally, because lead-based solders must be heated to high temperatures during component bonding to flow into all gaps before curing, such materials cannot be used to bond heat-sensitive components.

[0146] Conductive adhesives are an alternative to lead-based solders and exhibit low curing temperatures and high thermal and mechanical stress recovery. Therefore, there is currently an unmet need for lead-free conductive adhesives to improve the safety, speed, durability, and performance of integrated electrical products, as well as manufacturing methods for making such conductive adhesives in an environmentally friendly manner. Conductive adhesive

[0147] Provided herein is a conductive adhesive comprising a conductive additive and an adhesive. The conductive additive can include a carbon-based material. The conductive additive can include a silver-based material. The conductive additive can include a carbon-based material and a silver-based material.

[0148] The silver-based additive can include silver nanowires, silver nanoparticles, or both. The silver-based additive can include silver nanowires, but not silver nanoparticles. The silver-based additive can include silver nanoparticles, but not silver nanowires. The silver-based additive can include silver nanowires and silver nanoparticles. Alternatively, the silver-based material can include silver nanorods, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or any combination thereof. The silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 25% of the silver nanowires are sized to be about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.6 μm, about 0.7 μm, about 0.8 μm, about 0.9 ... At least about 50% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 50% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 75% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. The silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. At least about 25% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. At least about 50% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. At least about 75% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. The silver nanowires can have an average aspect ratio of about 250:1, 300:1, 350:1, 400:1, 450:1, 500:1, 600:1, 700:1, 800:1, 900:1, or 1000:1.The silver nanowires can have an average aspect ratio of at least about 250:1, 300:1, 350:1, 400:1, 450:1, 500:1, 600:1, 700:1, 800:1, 900:1, or 1000:1.

[0149] The carbon-based material can include two or more of graphene nanoparticles, graphene nanosheets, and graphene microparticles. The carbon-based material can include graphene nanoparticles and graphene nanosheets. The carbon-based material can include graphene nanoparticles and graphene microparticles. The carbon-based material can include graphene nanosheets and graphene microparticles. The carbon-based material can include graphene nanoparticles, graphene nanosheets, and graphene microparticles. FIG. 1 shows an exemplary diagram of a conductive adhesive 100 including a carbon-based material, the carbon-based material including zero-dimensional nanoparticles 101 (shown as dots), two-dimensional nanosheets 102 (shown as lines), three-dimensional microparticles 103 (shown as sticks), and adhesive 104. The zero-dimensional nanoparticles 101 can include carbon black nanoparticles. The two-dimensional nanosheets 102 can include graphene. The three-dimensional microparticles 103 can include graphene microparticles. In some embodiments, the carbon-based material and adhesive can self-assemble to establish sufficient percolation (interconnectivity) and therefore electrical conductivity.

[0150] Alternatively, the carbon-based material may be graphite powder, natural graphite, synthetic graphite, expanded graphite, carbon black, Timcal carbon super C45, Timcal carbon super C65, cabot carbon, carbon super P, acetylene black, furnace black, carbon nanotube, etc. The material may include carbon fiber, vapor grown carbon fiber, graphene oxide, or any combination thereof.

[0151] Alternatively, the silver-based material may be a silver nanorod, a silver nanoflower, a silver nanofiber, or a silver nanoparticle. The nanoparticles may include ratelets, silver nanoribbons, silver nanocubes, silver bipyramids, or any combination thereof.

[0152] Adhesives include carpenter's glue, wood glue, cyanoacrylate, contact cement, latex, library paste, rubber glue, methylcellulose, The conductive adhesive may include a solcinol resin, a starch, a butanone, a dichloromethane acrylic, an ethylene vinyl, a phenol formaldehyde resin, a polyamide, a polyester, a polyethylene, a polypropylene, a polysulfide, a polyurethane, a polyvinyl acetate, an aliphatic, a polyvinyl alcohol, a polyvinyl chloride, a polyvinyl chloride emulsion, a silicone, a styrene acrylic, an epichlorohydrin, an epoxide, or any combination thereof. In some embodiments, the conductive adhesive further includes a thinner. In some embodiments, the thinner includes butyl acetate, a lacquer thinner, an acetone, a petroleum naphtha, a mineral spirit, a xylene, or any combination thereof.

[0153] In some embodiments, the conductive adhesive further comprises a pigment, a colorant, a dye, or any combination thereof. In some embodiments, the conductive carbon-based adhesive comprises at least one, at least two, at least three, at least four, or at least five colorants, dyes, pigments, or combinations thereof. In some embodiments, the pigment comprises a metal-based or metallic pigment. In some embodiments, the metallic pigment is a gold, silver, titanium, aluminum, tin, zinc, mercury, manganese, lead, iron, iron oxide, copper, cobalt, cadmium, chromium, arsenic, bismuth, antimony, or barium pigment. In some embodiments, the colorant comprises at least one metallic pigment. In some embodiments, the colorant comprises a silver metallic colorant. In some embodiments, the silver metallic colorant comprises silver nanoparticles, silver nanorods, silver nanowires, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or combinations thereof. In some embodiments, the colorant is selected from pigments and / or dyes that are red, yellow, magenta, green, cyan, purple, black, or brown, or combinations thereof. In some embodiments, the pigment is blue, brown, cyan, green, purple, magenta, red, yellow, or combinations thereof. In some embodiments, the dye is blue, brown, cyan, green, purple, magenta, red, yellow, or combinations thereof. Yellow colorants may include Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 65, 74, 83, 93, 110, 128, 151, 155, or combinations thereof. In some embodiments, the black colorant includes Color Black SI70, Color Black SI50, Color Black FW1, Color Black FW18, Acid Black 1, 11, 52, 172, 194, 210, 234, or a combination thereof. In some embodiments, the red or magenta colorant includes Pigment Red 1-10, 12, 18, 21, 23, 37, 38, 39, 40, 41, 48, 90, 112, 122, or a combination thereof. In some embodiments, the cyan or purple colorant includes Pigment Blue 15, 17, 22, Pigment Violet 1, 2, 3, 5, 19, 23, or a combination thereof. In some embodiments, the orange colorant includes Pigment Orange 48 and / or 49. In some embodiments, the purple colorant includes Pigment Violet 19 and / or 42.

[0154] FIG. 2 shows an image of an exemplary conductive adhesive. As shown, the conductive adhesive may be dark in color or may be pigmented to produce a bright color. According to FIG. 3, the conductive adhesive may be stored in a squeeze bottle, dispensed from a squeeze bottle, or both. Alternatively, according to FIG. 4, the conductive adhesive may be stored in a syringe, dispensed from a syringe, or both. Those skilled in the art will readily recognize that any container currently used for adhesives, epoxies, or other curable substances may be used to package and dispense the conductive adhesive of the present disclosure. Such packaging of the conductive adhesive should allow an operator, machine, or both to collect and / or dispense the conductive graphene. Some embodiments In the conductive adhesive packaging, an operator can dispense an amount of the conductive adhesive into the dispenser. In some embodiments, the conductive adhesive packaging further includes a mixing rod, a dispensing element, or any combination thereof.

[0155] Exemplary applications of the conductive adhesives disclosed herein are illustrated in FIGS. 5-7. According to FIG. 5, the exemplary conductive adhesive can be used to form an electronic circuit on a substrate between a battery and a light emitting diode (LED) light. As seen in the top row, when no battery is connected, the LED light is off. However, connecting the battery terminals to the exemplary conductive adhesive wires can power red, yellow, and green LEDs, from left to right, respectively. The substrate can include paper, wood, aluminum, silicone, or any other non-conductive or low-conductive material. Similarly, according to FIG. 6, the circuit formed by the exemplary conductive adhesive between a lithium coin cell battery can simultaneously light up three LEDs in parallel (e.g., red, orange, and yellow). In some embodiments, the circuit formed by the conductive adhesive deposited on the substrate can form an electronic device, such as a touch-sensitive device, a flexible device, a disconnection warning feature, or a shape-sensitive device. In some embodiments, the electronic device can be tweaked by changing the shape of the adhesive deposited on the substrate, the amount of adhesive deposited on the substrate, or both.

[0156] As further shown in FIG. 7, the exemplary conductive adhesive can be used as a replacement for lead-based solders to bond different electronic components to a circuit board. The bonding can be performed at room temperature. As such, the bonding can be performed by inserting one or more leads of an electrical component (e.g., an LED) into one or more holes or onto one or more pads in a motherboard, depositing the conductive adhesive between the one or more leads and the holes or pads, and subsequently drying the conductive adhesive. In some embodiments, the conductive adhesive is used instead of a harness and cable to provide both electrical and mechanical connections. Method for forming conductive adhesive

[0157] Also provided herein is a method of forming a conductive adhesive, comprising forming a conductive additive and adding an adhesive to the conductive additive. The conductive additive can include a carbon-based material. The conductive additive can include a silver-based material. The conductive additive can include a carbon-based material and a silver-based material.

[0158] In some embodiments, the carbon-based material is graphene, graphite powder, natural graphite, synthetic graphite, expanded graphite, carbon black, Timcal carbon super C45, Timcal carbon super C65, cabot carbon, carbon super P, acetylene black, furne The silver-based material may include silver nanoparticles, silver nanorods, silver nanowires, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or any combination thereof.

[0159] In some embodiments, the conductive adhesive comprises about 60% to about 99.9% adhesive by weight. In some embodiments, the conductive adhesive comprises about 0.1% to about 40% conductive additive by weight. In some embodiments, the conductive additive comprises graphene, and the weight percentage of graphene in the conductive adhesive is about 0.1% to about 10%. In some embodiments, the conductive additive comprises graphite powder, and the weight percentage of graphite powder in the conductive adhesive is about 1% to about 40%.

[0160] Adhesives include carpenter's glue, wood glue, cyanoacrylate, contact cement, latex, library paste, rubber glue, methylcellulose, and resin. The resin may include rucinol resin, starch, butanone, dichloromethane acrylic, ethylene vinyl, phenol formaldehyde resin, polyamide, polyester, polyethylene, polypropylene, polysulfide, polyurethane, polyvinyl acetate, aliphatic, polyvinyl alcohol, polyvinyl chloride, polyvinyl chloride emulsion, silicone, styrene acrylic, epichlorohydrin, epoxide, or any combination thereof.

[0161] Some embodiments further include adding a thinner to the carbon-based material and the adhesive. In some embodiments, the thinner includes butyl acetate, lacquer thinner, acetone, petroleum naphtha, mineral spirits, xylene, or any combination thereof. In some embodiments, the conductive adhesive includes about 50% to about 99% thinner by volume.

[0162] Some embodiments further include adding a pigment, a colorant, a dye, or any combination thereof to the conductive additive and the adhesive. In some embodiments, the conductive adhesive includes at least one, at least two, at least three, at least four, or at least five colorants, dyes, pigments, or combinations thereof. In some embodiments, the pigment includes a metal-based or metallic pigment. In some embodiments, the metallic pigment is a gold, silver, titanium, aluminum, tin, zinc, mercury, manganese, lead, iron, iron oxide, copper, cobalt, cadmium, chromium, arsenic, bismuth, antimony, or barium pigment. In some embodiments, the colorant includes at least one metallic pigment. In some embodiments, the colorant includes a silver metallic colorant. In some embodiments, the silver metallic colorant includes silver nanoparticles, silver nanorods, silver nanowires, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or combinations thereof. In some embodiments, the colorants are selected from pigments and / or dyes that are red, yellow, magenta, green, cyan, purple, black, or brown, or combinations thereof. In some embodiments, the pigments are blue, brown, cyan, green, purple, magenta, red, yellow, or combinations thereof. In some embodiments, the dyes are blue, brown, cyan, green, purple, magenta, red, yellow, or combinations thereof. Yellow colorants include Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 65, 74, 83, 93, 110, 128, 151, 155, or combinations thereof. In some embodiments, the black colorant includes Color Black SI70, Color Black SI50, Color Black FW1, Color Black FW18, Acid Black 1, 11, 52, 172, 194, 210, 234, or a combination thereof. In some embodiments, the red or magenta colorant includes Pigment Red 1-10, 12, 18, 21, 23, 37, 38, 39, 40, 41, 48, 90, 112, 122, or a combination thereof. In some embodiments, the cyan or purple colorant includes Pigment Blue 15, 17, 22, Pigment Violet 1, 2, 3, 5, 19, 23, or a combination thereof. In some embodiments, the orange colorant includes Pigment Orange 48 and / or 49. In some embodiments, the purple colorant includes Pigment Violet 19 and / or 42. Conductive Adhesives: Performance

[0163] FIG. 8A is an image of a film comprising an exemplary conductive carbon-based adhesive deposited and dried on a flexible substrate (e.g., a transparent flexible substrate). FIG. 8B is an image of a folded film comprising an exemplary conductive carbon-based adhesive deposited and dried on a flexible substrate. The ability of the dried conductive carbon-based adhesive to bend and warp with the flexible substrate demonstrates that the conductive carbon-based adhesive can withstand compressive and tensile forces, enabling its use in flexible electronic devices. Furthermore, such an ability allows the use of the exemplary conductive carbon-based adhesive in non-flexible electronic devices under pressure.

[0164] 9 is an exemplary image of an exemplary apparatus for testing the electrical properties of a sheet comprising a dried conductive carbon-based adhesive with contact pads formed of silver paste and copper tape. As shown, alligator clips can be used to connect the contact pads of the sheet to an electrochemical workstation for electrical performance characterization, and a ruler indicates the strain applied to the exemplary sheet.

[0165] FIG. 10 is a graph of the voltage-current curve of an exemplary conductive carbon-based adhesive. As can be seen, as the voltage increases from about -1V to about 1V, the current increases from about -3mA to about 3mA. FIG. 11 is a graph of the voltage-current curve of exemplary conductive adhesive films made with different amounts of carbon-based conductive additive, G1 having a higher amount of carbon-based material than G2, which has a higher amount of carbon-based material than G3. As shown, as the voltage increases from about -1V to about 1V, the current of the G1 sample increases from about -5mA to about 5mA. As shown, as the voltage increases from about -1V to about 1V, the current of the G2 sample increases from about -10mA to about 10mA. As shown, as the voltage increases from about -1V to about 1V, the current of the G3 sample increases from about -50mA to about 55mA. In some embodiments, the conductive carbon-based adhesive has a conductivity of about 0.15S / m to about 60S / m.

[0166] FIG. 12 is an image of an exemplary conductive carbon-based adhesive coated contact pad. In some embodiments, the contact pads include silver contact pads. In some embodiments, the contact pads are arranged in four rows of 20 pads. The contact pads can be used to test the electrical performance of the exemplary film at multiple locations. As shown, the contact pads are arranged in a grid of first, second, third, and fourth contact pads, with each grid comprising 5×5 rows of individual contact pads.

[0167] 13A-13C show sheet resistances of exemplary conductive carbon-based adhesives having various amounts of carbon-based material. FIG. 13A is a graph of the sheet resistance of an exemplary first conductive carbon-based adhesive with four contact pad grids. As shown, the first grid exhibits a sheet resistance of about 250 ohms / sq to about 260 ohms / sq, the second grid exhibits a sheet resistance of about 210 ohms / sq to about 250 ohms / sq, the third grid exhibits a sheet resistance of about 225 ohms / sq to about 250 ohms / sq, and the fourth grid exhibits a sheet resistance of about 210 ohms / sq to about 240 ohms / sq. FIG. 13B is a graph of the sheet resistance of an exemplary second conductive carbon-based adhesive with four contact pad grids, the second conductive carbon-based adhesive including a smaller amount of carbon-based material than the first conductive carbon-based adhesive. As shown, the first grid exhibits a sheet resistance of about 75 ohms / sq to about 85 ohms / sq, the second grid exhibits a sheet resistance of about 72 ohms / sq to about 81 ohms / sq, the third grid exhibits a sheet resistance of about 77 ohms / sq to about 83 ohms / sq, and the fourth grid exhibits a sheet resistance of about 75 ohms / sq to about 88 ohms / sq. Figure 13C is a graph of the sheet resistance of an exemplary third conductive carbon based adhesive at four contact pad grids, the third conductive carbon based adhesive including a smaller amount of carbon based material than the second conductive carbon based adhesive. As shown, the first grid exhibits a sheet resistance of about 15 ohms / sq to about 16 ohms / sq, the second grid exhibits a sheet resistance of about 13 ohms / sq to about 15 ohms / sq, the third grid exhibits a sheet resistance of about 13 ohms / sq to about 15 ohms / sq, and the fourth grid exhibits a sheet resistance of about 13 ohms / sq to about 14 ohms / sq.

[0168] FIG. 14A is a bar graph comparing the sheet resistance of the first, second, and third exemplary conductive carbon based adhesives when dried on a substrate, where the first conductive carbon based adhesive has a greater amount of carbon based material than the third conductive carbon based adhesive, which has a greater amount of carbon based material than the second conductive carbon based adhesive. As shown, increasing the amount of carbon based material decreases the sheet resistance, resulting in a sheet resistance of approximately 225 ohms / sq for the first, second, and third conductive carbon based adhesives, respectively. , 75 ohms / sq, and 10 ohms / sq. In some embodiments, the conductive carbon based adhesive has a sheet resistivity of about 5 ohms / sq to about 500 ohms / sq. In some embodiments, the conductive carbon based adhesive has a sheet resistivity of about 0.3 ohms / sq / mil to about 2 ohms / sq / mil. FIG. 14B shows a graph comparing the resistivity of graphene and metal wire. As can be seen, the use of graphene improves the electrical properties of the adhesive, epoxy, and ink due to its higher resistivity of about 8,000 μΩ / cm compared to 10 μΩ / cm for metal wire.

[0169] 15A-15C show an exemplary apparatus for testing the electrical properties of a conductive carbon-based adhesive dried on a substrate under different bending angles. FIG. 15A is an image of an exemplary apparatus for testing the electrical properties of a film including an exemplary conductive carbon-based adhesive under different bending angles. FIG. 15B is an image of an exemplary apparatus for testing the electrical properties of a film including an exemplary conductive carbon-based adhesive, with the film in an unbent state. FIG. 15C is an image of an exemplary apparatus for testing the electrical properties of a film including an exemplary conductive graphene, with the film in a bent state. FIG. 16A is a diagram of an exemplary apparatus for testing the electrical properties of a film in an unbent state. FIG. 16B is a diagram of an exemplary apparatus for testing the electrical properties of a film in a bent state.

[0170] FIG. 17A is a diagram of a film including a dried conductive carbon-based adhesive that is bent convexly, where L=length of the film, ΔL=distance traveled by the unfixed end of the film, and L′=distance between the ends of the bent film. In one example, L=3.4, and the film is bent to about 180 degrees with ΔL=L=3.4. FIG. 17B is an exemplary graph showing the relationship between the distance of the convex bend and the resistance change for an exemplary film including a conductive carbon-based adhesive. As shown, FIG. 17B shows a Y-axis representing R / Ro percentage values ​​from 100% to 102% in increments of 0.4%, and an X-axis representing ΔL values ​​from 0 to 4 inches in increments of 0.5 inches. Thus, the relationship between the change in resistance and the distance traveled appears to be approximately flat. In some embodiments, the conductive carbon-based adhesive has a sheet resistance difference of up to about 6%, 5%, 4%, 3%, 2%, or 1% between the flat position and the position of the convex bent angle of up to 180 degrees. In some embodiments, the conductive carbon-based adhesive has a sheet resistance difference of up to about 1.5% between a flat position and a position at a convex bend angle of up to 180 degrees. Such a low change in sheet resistance means that the carbon-based adhesives described herein can be used in flexible electronics without suffering loss of functionality.

[0171] FIG. 18A is a diagram of a dried film including a dried conductive carbon-based adhesive that is bent concavely, where L=length of the film, ΔL=distance traveled by the unfixed end of the film, and L′=distance between the ends of the bent film. FIG. 18B is an exemplary graph showing the relationship between the distance of the concave bend and the resistance change for an exemplary film including a conductive carbon-based adhesive. As shown, FIG. 18B shows a Y-axis representing R / Ro percentage values ​​from 100% to 102% in 0.4% increments, and an X-axis representing ΔL values ​​from 0 to 4 inches in 0.5 inch increments. Thus, FIG. 18B may imply a negative correlation between the distance traveled and the resistance change. In some embodiments, the conductive carbon-based adhesive has a sheet resistance difference of up to about 6%, 5%, 4%, 3%, 2%, or 1% between the flat position and the position of the concave bent angle of up to 180 degrees. In some embodiments, the conductive carbon-based adhesive has a sheet resistance difference of up to about 2% between the flat position and the concave bent angle position of up to 180 degrees. Such a low change in sheet resistance further means that the carbon-based adhesives described herein can be used in flexible electronics without suffering functionality loss.

[0172] FIG. 19A shows the resistance change (95% to 102% in 1% increments) of an exemplary dried film containing a conductive carbon-based adhesive versus twist angle (from 0 degrees to 800 degrees in 100 degree increments). 1 is a graph showing the relationship between the resistance and the surface resistance, which when twisted, reduces by less than 6%, 5%, 4%, 3%, or 2%. In some embodiments, the resistance change of an exemplary conductive carbon-based adhesive film including a conductive carbon-based adhesive is less than 3% when twisted. In some embodiments, the conductive carbon-based adhesive has a sheet resistance difference of up to about 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, or 2% between the flat position and the position with a twist angle of up to 800 degrees. In some embodiments, the conductive carbon-based adhesive has a sheet resistance difference of up to about 3% between the flat position and the position with a twist angle of up to 800 degrees. This low sheet resistance delta indicates that the carbon-based adhesives described herein can be used in flexible electronics without degrading electrical functionality.

[0173] FIG. 19B is a current-voltage graph of an exemplary film with a dried conductive carbon-based adhesive on a substrate twisted at 0 degrees and 720 degrees. The graph shows an X-axis with values ​​from -1.2V to 1.2V in 0.2V increments and a Y-axis with values ​​from -0.4mA to 0.4mA in 0.1mA increments. As shown, the film twisted at 720 degrees shows about 0.05mA less current at the same voltage than the film twisted at 0 degrees. FIG. 20 shows images of an exemplary film with a conductive carbon-based adhesive at twist angles of 0, 90, 180, 270, 360, 450, 540, 630, and 720 degrees.

[0174] The strength of an adhesive can be defined by its tensile strength or adhesive strength. In some embodiments, the tensile strength of an adhesive is measured by preparing an exemplary sample, gluing two blocks together using the adhesive, and applying a force to pull the blocks apart at room temperature. FIG. 21 shows an image of an exemplary conductive carbon-based adhesive sample preparation for tensile strength testing. In some embodiments, the adhesive is applied to wood using a squeegee. FIG. 22A is a diagram of the adhesive connecting two blocks and under tensile stress. FIG. 22B is an image of a tensile hook of a prepared tensile strength test sample of an exemplary conductive carbon-based adhesive. FIG. 22C is an image of a bonded joint of a prepared tensile strength test sample of an exemplary conductive carbon-based adhesive. In some embodiments, the tensile strength test sample is prepared by applying the adhesive to a piece of wood, clamping the piece to another piece of wood, curing the conductive carbon-based adhesive overnight, and attaching a threaded hook to each end of the tensile strength test sample. In some embodiments, the conductive carbon-based adhesive has a shear strength of at least about 30 MPa, 25 MPa, 20 MPa, 10 MPa, or 5 MPa.

[0175] In some embodiments, the strength of an adhesive is defined by its shear strength or adhesive strength. In some embodiments, the shear strength of an adhesive is measured by preparing an exemplary sample, gluing two blocks together using an adhesive, and applying a shear force to pull the blocks apart in a direction parallel to the adhesive surface at room temperature. Figure 23A is a first image of an exemplary conductive carbon-based adhesive sample preparation for shear strength testing. Figure 23B is a second image of an exemplary conductive carbon-based adhesive sample preparation for shear strength testing.

[0176] FIG. 24A is a diagram of shear strength. FIG. 24B is an image of a bonded joint of a prepared shear strength test specimen of an exemplary conductive carbon-based adhesive. FIG. 25A is a first image of an exemplary adhesive tensile strength test specimen preparation without conductive graphene. FIG. 25B is a second image of an exemplary adhesive tensile strength test specimen preparation without conductive graphene. FIG. 26 is an image of a prepared tensile and shear stress specimen of an exemplary conductive carbon-based adhesive and an exemplary adhesive without conductive graphene. FIG. 27 is a first image of a tensile and shear stress test apparatus with a hanging scale, a specimen, and a water bucket, where water added to the water bucket increases the force on the specimen. FIG. 28 is a second image of the tensile and shear stress test apparatus. In some embodiments, the conductive carbon-based adhesive has a shear strength of at least about 20 MPa, 15 MPa, 10 MPa, or 5 MPa.

[0177] Therefore, conductive adhesives are useful in a variety of applications, such as bonding, sauntering, splicing, bridging, shorting, printed electronics, flexible electronics, antenna formation, energy harvesting, composites, etc. Conductive Epoxy can be used for electrical wiring, wiring boards, or any electrical formation or modification. Conductive adhesives can dry at room temperature, making them an alternative to traditional soldering that cannot be used at high temperatures.

[0178] Currently available conductive epoxies require a conductive additive concentration by weight of approximately 80%-90% to achieve electrical percolation. However, this high concentration reduces the adhesive material's adhesive effectiveness, which becomes brittle and weak when dry. Furthermore, such high concentrations of expensive conductive additives (e.g., silver) are often prohibitively expensive. In contrast, the conductive epoxies disclosed herein require a lower conductive additive concentration for electrical percolation and are therefore more robust and economical.

[0179] Provided herein is a conductive epoxy that includes a conductive additive and an adhesive. The conductive epoxy can include a two-part epoxy. The conductive epoxy can be configured to bond a wide range of materials, including, but not limited to, wood, plastic, metal, ceramic, fabric, encapsulants, and electronic components. The conductive epoxy can be configured to bond two similar materials, two dissimilar materials, or both. The conductive carbon-based epoxy can be used as a versatile filler for gap bonding, surface repair, and lamination.

[0180] The conductive additive can include a carbon-based material. The conductive additive can include a silver-based material. The conductive additive can include a carbon-based material and a silver-based material. In some embodiments, at least a portion of the conductive additive is incorporated into the resin, the hardener, or both. In some embodiments, at least a portion of the conductive additive is incorporated into the resin and not into the hardener. In some embodiments, at least a portion of the conductive additive is incorporated into the hardener and not into the resin. In some embodiments, the concentration of the conductive additive in the conductive epoxy is about 0.5% to about 10%. In some embodiments, the concentration of the conductive additive in the conductive epoxy is from about 0.5% to about 1%, from about 0.5% to about 2%, from about 0.5% to about 3%, from about 0.5% to about 4%, from about 0.5% to about 5%, from about 0.5% to about 6%, from about 0.5% to about 7%, from about 0.5% to about 8%, from about 0.5% to about 9%, from about 0.5% to about 10%, from about 1% to about 2%, from about 1% to about 3%, from about 1% to about 4%, from about 1% to about 5%, from about 1% to about 6%, from about 1% to about 7%, from about 1% to about 8%, from about 1% to about 9%, from about 1% to about 10%, from about 2% to about 3%, from about 2% to about 4%, from about 2% to about 5%, from about 2% to about 6%, from about 2% to about 7%, from about 2% to about 8%, About 2% to about 9%, about 2% to about 10%, about 3% to about 4%, about 3% to about 5%, about 3% to about 6%, about 3% to about 7%, about 3% to about 8%, about 3% to about 9%, about 3% to about 10%, about 4% to about 5%, about 4% to about 6%, about 4% to about 7%, about 4% to about 8%, about 4% to about 9%, about 4% to about 10%, about 5% to The concentration of the conductive additive in the conductive epoxy is about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%. In some embodiments, the concentration of the conductive additive in the conductive epoxy is about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, or about 10%. In some embodiments, the concentration of the conductive additive in the conductive epoxy is at least about 0.5%, about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, or about 9%.In some embodiments, the concentration of the conductive additive in the conductive epoxy is up to about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, or about 10%.

[0181] The silver-based additive may include silver nanowires, silver nanoparticles, or both. The silver-based additive may include silver nanowires, but may not include silver nanoparticles. The silver-based additive may include silver nanoparticles, but may not include silver nanowires. The silver-based additive may include silver nanowires and silver nanoparticles. Alternatively, the silver-based material may include silver nanorods, silver nanoflowers, silver nanofibers, silver nanoplatelets, silver nanoribbons, silver nanocubes, silver bipyramids, or any combination thereof. The silver nanowires may have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 25% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 50% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. At least about 75% of the silver nanowires can have a diameter of less than about 1 μm, about 0.9 μm, about 0.8 μm, about 0.7 μm, about 0.6 μm, about 0.5 μm, about 0.4 μm, about 0.3 μm, about 0.2 μm, about 0.1 μm, about 0.09 μm, about 0.08 μm, about 0.07 μm, about 0.06 μm, or about 0.05 μm. The silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm.At least about 25% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. At least about 50% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. At least about 75% of the silver nanowires can have a length greater than about 10 μm, about 15 μm, about 20 μm, about 25 μm, about 30 μm, about 35 μm, about 40 μm, about 45 μm, about 50 μm, about 55 μm, about 60 μm, about 65 μm, about 70 μm, or about 75 μm. The silver nanowires can have an average aspect ratio of about 250:1, 300:1, 350:1, 400:1, 450:1, 500:1, 600:1, 700:1, 800:1, 900:1, or 1000:1. The silver nanowires can have an average aspect ratio of at least about 250:1, 300:1, 350:1, 400:1, 450:1, 500:1, 600:1, 700:1, 800:1, 900:1, or 1000:1.

[0182] The carbon-based material may include two or more of graphene nanoparticles, graphene nanosheets, and graphene microparticles. The carbon-based material may include graphene nanoparticles and graphene nanosheets. The carbon-based material may include graphene nanoparticles and graphene microparticles. The carbon-based material may include graphene nanosheets and graphene microparticles. The carbon-based material may include graphene nanoparticles, graphene nanosheets, and graphene microparticles. Alternatively, the carbon-based material may be graphite powder, natural graphite, synthetic graphite, expanded graphite, carbon black, Timcal carbon super C45, Timcal carbon super C65, cabot carbon, carbon super P, acetylene black, furnace black, carbon nanotubes, vapor grown. It may include carbon fiber, graphene oxide, or any combination thereof.

[0183] The adhesive may include a resin and a curing agent. The curing agent may include graphene nanoparticles and graphene nanosheets. The curing agent may include graphene nanoparticles and graphene microparticles. The curing agent may include graphene nanosheets and graphene microparticles. The curing agent may include graphene nanoparticles, graphene nanosheets, and graphene microparticles. The curing agent may include silver nanowires and silver nanoparticles. The curing agent may include silver nanowires but not silver microparticles. The curing agent may include silver microparticles but not silver nanowires. The curing agent may include silver nanowires, graphene nanoparticles, and graphene nanosheets but not silver nanoparticles. The curing agent may include silver nanowires, graphene nanoparticles, and graphene microparticles but not silver nanoparticles. The curing agent may include silver nanowires, graphene nanosheets, and graphene microparticles but not silver nanoparticles. The curing agent may include silver nanowires, graphene nanoparticles, graphene nanosheets, and graphene microparticles but not silver nanoparticles. The curing agent may include silver nanowires, graphene nanoparticles, graphene nanosheets, and graphene microparticles but not silver nanoparticles. The curing agent can include silver nanoparticles, graphene nanowires, and graphene nanosheets, but cannot include silver nanowires. The curing agent can include silver nanoparticles, graphene nanowires, and graphene microparticles, but cannot include silver nanowires. The curing agent can include silver nanoparticles, graphene nanosheets, and graphene microparticles, but cannot include silver nanowires. The curing agent can include silver nanoparticles, graphene nanowires, graphene nanosheets, and graphene microparticles, but cannot include silver nanowires. In some embodiments, the conductive additive comprises about 60% to about 99.9% of the curing agent by weight. In some embodiments, the conductive additive comprises about 60% to about 99.9% of the resin by weight.

[0184] The resin can include graphene nanoparticles and graphene nanosheets. The resin can include graphene nanoparticles and graphene microparticles. The resin can include graphene nanosheets and graphene microparticles. The resin can include graphene nanoparticles, graphene nanosheets, and graphene microparticles. The resin can include silver nanowires and silver nanoparticles. The resin can include silver nanowires but not silver microparticles. The resin can include silver microparticles but not silver nanowires. The resin can include silver nanowires, graphene nanoparticles, and graphene nanosheets but not silver nanoparticles. The resin can include silver nanowires, graphene nanoparticles, and graphene nanosheets but not silver nanoparticles. The resin can include silver nanowires, graphene nanoparticles, and graphene microparticles but not silver nanoparticles. The resin can include silver nanowires, graphene nanosheets, and graphene microparticles but not silver nanoparticles. The resin can include silver nanowires, graphene nanoparticles, graphene nanosheets, and graphene microparticles but not silver nanoparticles. The resin can include silver nanowires, graphene nanoparticles, graphene nanosheets, and graphene microparticles but not silver nanoparticles. The resin can include silver nanoparticles, graphene nanowires, and graphene nanosheets but not silver nanowires. The resin may include silver nanoparticles, graphene nanowires, graphene microparticles, but not silver nanowires. The resin may include silver nanoparticles, graphene nanosheets, and graphene microparticles, but not silver nanowires. The resin may include silver nanoparticles, graphene nanowires, graphene nanosheets, and graphene microparticles, but not silver nanowires.

[0185] Some embodiments further include a thinner in the resin and hardener, hi som...

Claims

1. (a) heating the solvent; (b) adding the catalyst solution and the polymer solution to a solvent to form a first solution; (c) injecting a silver-based solution into the first solution to form a second solution; (d) centrifuging the second solution; and (e) washing the second solution with a washing solution to extract the silver nanowires; 16. A method for forming silver nanowires comprising:

2. The method of claim 1 , further comprising heating the second solution prior to centrifuging the second solution.

3. 10. The method of claim 1, further comprising cooling the second solution prior to centrifuging the second solution.

4. (a) a diameter of less than about 0.5 μm; (b) a length of about 10 μm to about 75 μm.

5. The method of claim 1 , wherein the solvent comprises a glycol, a polymer solution, or both.

6. The method of claim 1 , wherein the polymer solution has a concentration of about 0.075M to about 0.25M.

7. The method of claim 1 , wherein the catalyst solution has a concentration of about 2 mM to about 8 mM.

8. The method of claim 1, wherein the volume of the solvent is from about 75 to about 250 times greater than the volume of the catalyst solution.

9. The method of claim 1 , wherein the volume of the solvent is about 1.5 to about 6.5 times greater than the volume of the polymer solution.

10. The method of claim 1 , wherein the silver-based solution has a concentration of about 0.05M to about 0.2M.

11. The method of claim 1 , wherein the volume of the solvent is about 1.5 to about 6.5 times greater than the volume of the silver-based solution.

12. The method of claim 1 , wherein the solvent is heated to a temperature of about 75° C. to about 300° C.

13. The method of claim 1 , wherein the solvent is heated for about 30 minutes to about 120 minutes.

14. The method of claim 1 , wherein the solvent is stirred while being heated.

15. The method of claim 1 , wherein the second solution is heated for about 30 minutes to about 120 minutes.

16. The method of claim 1, wherein the centrifugation is performed at a speed of about 1,500 rpm to about 6,000 rpm.

17. The method of claim 1, wherein the centrifugation is carried out for about 10 minutes to about 40 minutes.

18. The method of claim 1 , wherein washing with the second solution comprises a plurality of washing cycles, including from about 2 cycles to about 6 cycles.

19. The method of claim 1 carried out in a solvothermal chamber.

Citation Information

Patent Citations

  • Preparation method of silver nanowire

    CN106735294A

  • Method for manufacturing laminate with conductive pattern

    JP2017117001A

  • Organic light emitting device with outcoupling layer for improved light extraction

    US20120025172A1

  • Conductive film, method for manufacturing same, touch panel, and solar cell

    WO2011125981A1

  • Metal complex compositions and mixture thereof

    WO2012124770A1