Acoustic member
The composite resin molded article with a high fibrous filler concentration and controlled crystallinity addresses moldability and sound quality issues, achieving superior mechanical strength and sound characteristics through optimized fiber distribution and interface design.
Patent Information
- Application Number
- JP2024142014
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-06-17
AI Technical Summary
Existing composite resins for acoustic members suffer from poor moldability, insufficient rigidity, and inadequate internal loss, leading to suboptimal sound characteristics when high fiber content is added.
A composite resin molded article with a fibrous filler concentration of 50% by weight or more, where the crystallinity of the base resin around the fibrous filler is higher than elsewhere, and the ends of the filler are partially defibrated, enhancing both elastic modulus and internal loss.
The solution achieves high elastic modulus and improved sound characteristics by optimizing the crystallinity and interface structure, resulting in a composite resin with enhanced mechanical strength and sound absorption properties.
Smart Images

Figure 2024167283000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite resin molding for acoustic components, which can realize a molding having excellent sound characteristics. [Background technology]
[0002] So-called "general-purpose plastics" such as polyethylene (PE), polypropylene (PP), polystyrene (PS), and polyvinyl chloride (PVC) are not only very inexpensive, but also easy to mold and are a fraction of the weight of metals or ceramics. For this reason, general-purpose plastics are often used as materials for a variety of everyday items such as bags, various types of packaging, various containers, and sheets, as well as industrial parts such as automobile parts and electrical parts, and as materials for daily necessities and miscellaneous goods.
[0003] However, general-purpose plastics have drawbacks such as insufficient mechanical strength, etc. Therefore, general-purpose plastics do not have sufficient properties required for materials used in various industrial products such as mechanical products such as automobiles, and electrical, electronic, and information products, and the current situation is that the range of applications of general-purpose plastics is limited.
[0004] On the other hand, so-called "engineering plastics" such as polycarbonate, fluororesin, acrylic resin, and polyamide have excellent mechanical properties and are used in various industrial products, including mechanical products such as automobiles, and electrical, electronic, and information products. However, engineering plastics have issues such as being expensive, difficult to recycle as monomers, and a large environmental impact.
[0005] Therefore, there is a demand for a significant improvement in the material properties (mechanical strength, etc.) of general-purpose plastics. A technology is known in which fibrous fillers such as natural fibers, glass fibers, and carbon fibers are dispersed in the resin of a general-purpose plastic to strengthen the plastic, thereby improving the mechanical strength of the general-purpose plastic. It is known that the addition of these fibrous fillers improves not only the mechanical properties but also the sound properties by increasing the internal loss inherent to the material. Among these, organic fillers such as cellulose are attracting attention because they are inexpensive and environmentally friendly when disposed of.
[0006] In audio equipment such as speakers, headphones, and various players, molded parts used in the exterior and interior parts are required to have not only mechanical strength but also improved internal loss by improving viscosity in order to improve sound characteristics. Companies are conducting research to improve the sound characteristics of composite resins. For example, a composite resin made of cellulose fiber and thermoplastic resin has been proposed, which contains about 35% cellulose fiber by weight, has a length of 0.5 to 1.0 mm, and has a fiber diameter of 50 to 60 μm (see, for example, Patent Document 1). Excellent sound characteristics are achieved by using this composite resin as a composition for molding a speaker unit mounting member. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 4179037 Summary of the Invention [Problem to be solved by the invention]
[0008] However, in the composite resin described in Patent Document 1, the moldability deteriorates when a large amount of fiber is added, and more than half of the composite resin is resin, which results in problems such as insufficient rigidity, insufficient internal loss, and insufficient sound characteristics.
[0009] The present invention is devised to solve the above-mentioned problems, and has an object to provide a composite resin molding for acoustic components having improved sound characteristics. [Means for solving the problem]
[0010] In order to achieve the above object, the present invention provides a composite resin molding for acoustic components, comprising a base resin and a fibrous filler dispersed in the base resin, The concentration of the fibrous filler in the composite resin molding is 50% by weight or more, In the composite resin molding, the crystallinity of the base resin around the fibrous filler is higher than the crystallinity of the base resin in other locations. Effect of the Invention
[0011] The composite resin molding for acoustic components according to the present invention makes it possible to achieve both a high elastic modulus and a high internal loss in a fiber-reinforced material for acoustic components, thereby improving the sound characteristics of the product. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic see-through view showing an internal configuration of a composite resin molded product according to a first embodiment. [Figure 2A] 2 is a schematic diagram of a fibrous filler which is a constituent member of the composite resin molding according to the first embodiment. FIG. [Figure 2B] FIG. 2B is a partial enlarged view including an end portion of the fibrous filler of FIG. 2A. [Diagram 3] 1A is a 2D phase image display of a surface AFM image of the composite resin molded body according to the first embodiment, and FIG. 1B is a superimposed display of a 3D image and the phase image. [Figure 4] 1A to 1C are schematic diagrams illustrating a manufacturing process of the composite resin molded body according to the first embodiment. [Diagram 5] Table 1 shows the measurement results in each of Examples 1 to 4 and Comparative Examples 1 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] A composite resin molding for acoustic components according to a first aspect is a composite resin molding for acoustic components, comprising a base resin and a fibrous filler dispersed in the base resin, The concentration of the fibrous filler in the composite resin molding is 50% by weight or more, In the composite resin molding, the crystallinity of the base resin around the fibrous filler is higher than the crystallinity of the base resin in other locations.
[0014] A composite resin molding for acoustic components according to a second aspect is the same as in the first aspect above, wherein in the composite resin molding, the crystallinity of the base resin around the tip of the fibrous filler is higher than the crystallinity of the base resin around the center of the fibrous filler.
[0015] The composite resin molding for acoustic components according to the third aspect is the composite resin molding according to the first or second aspect above, and may have holes or cracks on the surface of the composite resin molding, the width of which may be 1 / 10 or less of the diameter of the fibrous filler.
[0016] A composite resin molding for acoustic components according to a fourth aspect is any one of the first to third aspects, in which the fibrous filler in the composite resin molding does not have to be hydrophobized in advance.
[0017] A composite resin molding for acoustic components according to a fifth aspect is any one of the first to fourth aspects, wherein the fibrous filler in the composite resin molding may be defibrated only at the ends.
[0018] A composite resin molding for acoustic members according to a sixth aspect is any one of the first to fifth aspects, wherein the fibrous filler is made of natural fibers such as cellulose.
[0019] A composite resin molding for acoustic members according to a seventh aspect is any one of the first to sixth aspects, in which the main resin may be an olefin resin.
[0020] Hereinafter, a composite resin molded article according to an embodiment will be described with reference to the drawings. In the following description, the same components are denoted by the same reference numerals, and the description will be omitted as appropriate.
[0021] (Embodiment 1) Fig. 1 is a schematic see-through view showing the internal configuration of a composite resin molded product 10 according to embodiment 1. Fig. 2A is a schematic view of a fibrous filler 2 which is a constituent member of the composite resin molded product according to embodiment 1. Fig. 2B is a partial enlarged view including an end portion 5 of the fibrous filler in Fig. 2A. The composite resin molded body 10 according to the first embodiment is made of a melt-kneaded product containing a base resin 1, a fibrous filler 2, and an additive 3. As shown in the schematic see-through view of FIG. 1, the composite resin molded body has the fibrous filler 2 and the additive 3 dispersed in the base resin 1. The concentration of the fibrous filler 2 is 50% by weight or more in the composite resin molded body 10. In addition, in the composite resin molded body 10, the crystallinity of the base resin 1 around the fibrous filler 2 is higher than the crystallinity of the base resin 1 in other locations. This makes it possible to achieve both a high elastic modulus and high internal loss, thereby improving the sound characteristics of products using this material.
[0022] <Main resin> In the present embodiment, the base resin 1 is preferably a thermoplastic resin in order to ensure good moldability. Examples of thermoplastic resins include olefin resins (including cyclic olefin resins), styrene resins, (meth)acrylic resins, organic acid vinyl ester resins or derivatives thereof, vinyl ether resins, halogen-containing resins, polycarbonate resins, polyester resins, polyamide resins, thermoplastic polyurethane resins, polysulfone resins (polyethersulfone, polysulfone, etc.), polyphenylene ether resins (polymers of 2,6-xylenol, etc.), cellulose derivatives (cellulose esters, cellulose carbamates, cellulose ethers, etc.), silicone resins (polydimethylsiloxane, polymethylphenylsiloxane, etc.), rubber or elastomers (diene rubbers such as polybutadiene and polyisoprene, styrene-butadiene copolymers, acrylonitrile-butadiene copolymers, acrylic rubbers, urethane rubbers, silicone rubbers, etc.), and biomass plastics (biopolyethylene, biopolyethylene terephthalate, starch, polylactic acid, polybutylene succinate, polyhydroxyalkanoic acid, other bio-derived resins, biodegradable resins, etc.). The above resins may be used alone or in combination of two or more kinds. Note that the base resin 1 does not have to be a thermoplastic resin as long as it has good moldability, and is not limited to the above materials.
[0023] Of these thermoplastic resins, the main resin 1 is preferably an olefin-based resin having a relatively low melting point. The olefin-based resin includes homopolymers of olefin-based monomers, copolymers of olefin-based monomers, and copolymers of olefin-based monomers and other copolymerizable monomers. Examples of the olefin-based monomer include linear olefins (α-C2-20 olefins such as ethylene, propylene, 1-butene, isobutene, 1-pentene, 4-methyl-1-pentene, and 1-octene), and cyclic olefins. These olefin-based monomers may be used alone or in combination of two or more kinds. Of the above olefin-based monomers, linear olefins such as ethylene and propylene are preferred. Examples of other copolymerizable monomers include fatty acid vinyl esters such as vinyl acetate and vinyl propionate; (meth)acrylic monomers such as (meth)acrylic acid, alkyl (meth)acrylates, and glycidyl (meth)acrylates; unsaturated dicarboxylic acids or anhydrides such as maleic acid, fumaric acid, and maleic anhydride; vinyl esters of carboxylic acids (e.g., vinyl acetate and vinyl propionate); cyclic olefins such as norbornene and cyclopentadiene; and dienes such as butadiene and isoprene. These copolymerizable monomers may be used alone or in combination of two or more. Specific examples of olefin resins include copolymers of chain olefins (particularly α-C2-4 olefins) such as polyethylene (low density, medium density, high density, or linear low density polyethylene), polypropylene, ethylene-propylene copolymers, and terpolymers such as ethylene-propylene-butene-1.
[0024] <Dispersant> Next, the dispersant will be described. The composite resin molded body in this embodiment may contain a dispersant for the purpose of improving the adhesion between the fibrous filler 2 and the main resin 1, or the dispersibility of the fibrous filler 2 in the main resin 1. By improving the dispersibility, the interface between the fiber and the resin is uniformly dispersed, the vibration absorption at the interface is increased, and the sound characteristics are improved. Examples of the dispersant include various titanate-based coupling agents, silane coupling agents, unsaturated carboxylic acids, maleic acid, maleic anhydride, or modified polyolefins grafted with the anhydrides thereof, fatty acids, fatty acid metal salts, and fatty acid esters. The silane coupling agents are preferably unsaturated hydrocarbon-based or epoxy-based. The surface of the dispersant may be treated with a thermosetting or thermoplastic polymer component and modified. The content of the dispersant in the composite resin molded body in this embodiment is preferably 0.01% by mass or more and 20% by mass or less, more preferably 0.1% by mass or more and 10% by mass or less, and even more preferably 0.5% by mass or more and 5% by mass or less. If the content of the dispersant is less than 0.01% by mass, poor dispersion occurs, while if the content of the dispersant is more than 20% by mass, the strength of the composite resin molding decreases. The dispersant is appropriately selected depending on the combination of the base resin 1 and the fibrous filler 2, but if a dispersant is not required, it does not have to be added.
[0025] <Fibrous filler> Next, a description will be given of the fibrous filler 2. The fibrous filler 2 (hereinafter, sometimes simply referred to as "fiber") contained in the composite resin molding in this embodiment is used primarily for the first purpose of improving mechanical properties and improving dimensional stability by reducing the linear expansion coefficient in the composite resin molding molded using the composite resin composition. For this purpose, the fibrous filler 2 preferably has a higher elastic modulus than the base resin 1, and specifically includes carbon fiber, carbon nanotube, pulp, cellulose, cellulose nanofiber, lignocellulose, lignocellulose nanofiber, basic magnesium sulfate fiber (magnesium oxysulfate fiber), potassium titanate fiber, aluminum borate fiber, calcium silicate fiber, calcium carbonate fiber, silicon carbide fiber, wollastonite, xonotlite, various metal fibers, natural fibers such as cotton, silk, wool or hemp, jute fiber, regenerated fibers such as rayon or cupra, semi-synthetic fibers such as acetate and promix, synthetic fibers such as polyester, polyacrylonitrile, polyamide, aramid, polyolefin, and further modified fibers chemically modified on the surface and end thereof. Furthermore, among these, carbons and celluloses are particularly preferred from the viewpoints of availability, high elastic modulus, and low linear expansion coefficient.
[0026] The second purpose of adding the fibrous filler 2 is to improve the sound characteristics; that is, to improve the viscosity. For this purpose, it is preferable that the fibrous filler has a certain degree of flexibility, and natural fibers such as pulp, cellulose, cellulose nanofiber, lignocellulose, lignocellulose nanofiber, cotton, silk, wool or hemp, or regenerated fibers such as jute fiber, rayon or cupra are preferable. Fibers with flexibility other than those mentioned above can also be used for this purpose. Note that the fibrous filler 2 is not limited to the above materials as long as it can improve the mechanical properties and has flexibility.
[0027] Next, the form near the interface between the fibrous filler 2 and the main resin 1 will be described. To improve the sound characteristics, that is, to improve the internal loss, it is necessary to convert vibration into thermal energy, and in the composite resin, the internal loss is improved by frictional heat caused by vibration at the interface between the fibrous filler and the resin. For this purpose, as described above, the fibrous filler has flexibility, which makes it easy to convert into vibration energy, and the internal loss is improved. Furthermore, the internal loss can be further improved by controlling the crystal state of the resin around the fibrous filler 2. As shown in the partial enlarged view including the end 5 of the fibrous filler in FIG. 2B, a structure that satisfies the above can be obtained by defibrating only the end 5 of the fibrous filler. With such a structure, the crystallinity near the tip of the fibrous filler can be made higher than that near the center. The more the shear force during kneading is increased, the more defibrated, and the higher the crystallinity. The difference in crystallinity creates a strength difference in the resin and generates an interface. By creating an interface, vibration can be absorbed at the interface and the internal loss can be improved. The tip defibrated portion is preferably 5% or more and 50% or less of the entire fiber length L of the fibrous filler 2. If the defibrated portion is less than 5% of the entire fiber length L, the specific surface area is small and therefore no increase in crystallinity is observed, whereas if it is 50% or more, the interface due to the difference in crystallinity does not increase, and in either case, the sound characteristics deteriorate. Also, near the center of the fiber, there are areas that are in contact with the resin and areas that are not in contact, and compared to the areas that are not in contact, the areas that are in contact have a higher crystallinity, and the internal loss can be improved by increasing the interfaces. Such a structure can be realized by kneading the fibrous filler in advance without hydrophobizing the filler. Also, by using fibers with defibrated tips, the center is not defibrated and the surface area does not increase significantly, so the resin does not thicken, and even if the concentration is increased, the fluidity is maintained, and the moldability can be improved.
[0028] Next, the state of existence of the fibrous filler in the composite resin molded body will be described. Depending on the molding conditions, it is possible to segregate the fibrous filler near the surface of the molded body. When a natural material is used as the fibrous filler, there are minute gaps in the fibers. Therefore, by segregating the fibrous filler near the molded body, minute gaps can be present on the surface of the molded body. Also, as described above, by not subjecting the fibrous filler to a hydrophobic treatment in advance, the base resin and the fibrous filler do not blend together, and minute gaps can be present between the base resin and the fibrous filler due to the difference in thermal shrinkage during molding. The gaps can also be segregated to the surface of the molded body due to molding. In this way, by having minute holes or cracks on the surface of the molded body, the sound absorption characteristics are increased and the sound characteristics can be improved due to the principle of Helmholtz resonance, like a perforated plate wall.
[0029] Fig. 3(a) is a 2D phase image of an atomic force microscope (AFM) image of the surface of the composite resin molded product according to embodiment 1. Fig. 3(b) is a superimposed display of a 3D image and a phase image. As shown in FIG. 3(a), the composite resin molding has minute holes and cracks 6 near the surface. Sound characteristics can be further improved by controlling the width of the minute holes and cracks 6 near the surface of the composite resin molding. It is desirable that the width of the short side of the holes and cracks 6 is 1 / 10 or less of the diameter of the fibrous filler. The upper limit of the width of the short side of the holes and cracks 6 has been determined by simulation, and if it is larger than 1 / 10 of the filler diameter, resonance is difficult to occur inside the holes, and sound characteristics are not sufficiently improved. Therefore, it is desirable that it is 1 / 10 or less of the diameter of the fibrous filler. Such cracks 6 can be controlled by the original fiber state, the difference in thermal contraction between the resin and the fiber, and the molding conditions.
[0030] When pellets of the composite resin composition used in the manufacture of a composite resin molded body are applied to a primary exterior component such as the exterior body of a speaker, the composite resin composition containing a fibrous filler is required to have colorability. In order for the composite resin composition to have colorability, the whiteness of the composite resin composition must be maintained, and the whiteness of the added fibrous filler must be maintained. The higher the L value in color difference measurement of the fibrous filler, the better. The L value (brightness) in the Lab color system of the fibrous filler that improves the colorability of the molded body has been experimentally calculated, and it is preferable that the L value is 85 or more.
[0031] Next, the characteristics of the fibrous filler 2 will be described. The types of the main resin 1 and the fibrous filler 2 are as described above. However, if the fibrous filler 2 is too soft relative to the main resin 1, i.e., if the elastic modulus is small, the composite resin composition and the composite resin molded body after molding will have a small elastic modulus as a whole, and as a result, the strength will decrease. On the other hand, if the fibrous filler 2 is too hard relative to the main resin 1, i.e., if the elastic modulus is large, the sound vibration will not be sufficiently attenuated during attenuation, and the sound characteristics will deteriorate. Therefore, in the relationship between the elastic modulus of the main resin 1 and the fibrous filler 2, it is preferable that the elastic modulus of the fibrous filler 2 is higher, and the difference between them is as small as possible. The optimal relationship is calculated from the simulation results, and it is preferable that the difference in elastic modulus between the main resin 1 and the fibrous filler 2 is within 20 GPa.
[0032] Furthermore, the fibrous filler is present in the composite resin molding in an amount of 50% by weight or more, which makes it possible to realize excellent sound characteristics and a high elastic modulus.
[0033] <Method of manufacturing composite resin molded body> Next, a method for producing the composite resin molded body will be described with reference to Fig. 4. Fig. 4 is a flow diagram illustrating a process for producing the composite resin molded body according to the first embodiment. (1) The base resin, fibrous filler, and additives are put into a melt-kneading processing device and melt-kneaded in the device. This melts the base resin, and the fibrous filler and additives are dispersed in the molten base resin. At the same time, the shearing action of the device promotes defibration of agglomerates of the fibrous filler, allowing the fibrous filler to be finely dispersed in the base resin. At this time, the ends of the fibrous filler are also defibrated.
[0034] Conventionally, fibrous fillers have been used after the fibers have been defibrated in advance through pretreatment such as wet dispersion. However, when the fibrous filler is defibrated in advance in the solvent used in wet dispersion, it is easier to defibrate than in a molten base resin, so it is difficult to defibrate only the ends, and the entire fibrous filler ends up in a defibrated state. In addition, there was a problem that the number of processes increased by adding pretreatment, which reduced productivity.
[0035] In contrast, in the manufacturing process of the composite resin molding in this embodiment, a pretreatment by wet dispersion for the purpose of defibrating the fibrous filler is not performed, and instead, a melt kneading treatment (all-dry method) is performed together with the base resin and dispersant, etc. In this method, by not performing a wet dispersion treatment of the fibrous filler, it is possible to partially defibrate only the ends of the fibrous filler as described above, and the number of steps is reduced, thereby improving productivity.
[0036] In order to prepare the fibrous filler of the present embodiment by the all-dry method, it is preferable to apply high shear stress during kneading, and specific kneading methods include a single-shaft kneader, a twin-shaft kneader, a roll kneader, a Banbury mixer, and combinations thereof. From the viewpoint of being easy to apply high shear and having high mass productivity, a continuous twin-shaft kneader and a continuous roll kneader are particularly preferable. Any kneading method other than the above may be used as long as it is a method that can apply high shear stress.
[0037] (2) The composite resin composition extruded from the melt kneading device is cut into pellets using a pelletizer, etc. Pelletization methods include air hot cutting, underwater hot cutting, and strand cutting, which are performed immediately after the resin is melted, as well as crushing methods in which a molded body or sheet is molded and then crushed and cut.
[0038] (3) The pellets can be injection molded to produce a composite resin molding. By mixing the fibrous filler in the pellets as described above, it is possible to obtain an injection molded article having excellent elastic modulus, impact resistance, and appearance.
[0039] Hereinafter, examples and comparative examples of the experiments conducted by the inventors will be described.
[0040] Example 1 In Example 1, a pulp-dispersed polypropylene composite resin molding was produced by the following production method.
[0041] (1) Softwood pulp (manufactured by Mitsubishi Paper Mills, product name: NBKP Celgar) was used as the starting material for the fibrous filler. This softwood pulp was crushed in a crusher to obtain the fibrous filler. End defibration was adjusted during the crushing process. (2) A mixture of polypropylene (manufactured by Prime Polymer Co., Ltd., product name: J108M) as a base resin, the above-mentioned fibrous filler, and maleic anhydride (manufactured by Sanyo Chemical Industries, Ltd., product name: UMEX) as an additive were weighed out so that the weight ratio of base resin to fibrous filler to additive was 42.9:55.0:2.1, and dry-blended. (3) The mixture was then melted, kneaded, and dispersed in a twin-screw kneader (KRC Kneader, manufactured by Kurimoto Iron Works, Ltd.). The shear force can be changed by changing the screw configuration of the twin-screw kneader, and a medium shear type was used in Example 1. The resin melt was hot-cut to produce pulp-dispersed polypropylene pellets.
[0042] (4) Using the prepared pulp-dispersed polypropylene pellets, composite resin molded body test pieces were prepared using an injection molding machine (180AD manufactured by Japan Steel Works, Ltd.). The test piece preparation conditions were resin temperature 190°C, mold temperature 60°C, injection speed 60mm / s, and holding pressure 80Pa. The shape of the test piece was changed depending on the evaluation items described below. A size 1 dumbbell was prepared for elastic modulus measurement, and a 60mm square, 1.6mm thick plate was prepared for hydrophilicity measurement. The obtained pulp-dispersed polypropylene composite resin molded body test pieces were evaluated by the following methods.
[0043] (Fiber end defibrability) The obtained pulp-dispersed polypropylene pellets were immersed in a xylene solvent to dissolve the polypropylene, and the shape of the remaining pulp fibers was observed by SEM. The ends of the fibers were found to be in a defibrated state.
[0044] (Elastic modulus of composite resin molding) A tensile test was carried out using the No. 1 dumbbell-shaped test piece obtained. The elastic modulus was evaluated as follows: less than 3.0 GPa was x, 3.0 GPa or more but less than 4.0 GPa was △, and 4.0 GPa or more was ◯. The elastic modulus of the test piece was 4.3 GPa, and was evaluated as ◯.
[0045] (Evaluation of sound characteristics of composite resin moldings) The obtained test pieces were used to evaluate the sound characteristics through viscoelasticity test evaluation. Specifically, tan δ, which is linked to the sound absorption characteristics, was calculated from the viscoelasticity measurement results, and the sound vibration absorption was evaluated. In addition, a simple speaker housing was actually created, and sound was generated inside it, and a human sensory evaluation was performed. In the sensory evaluation, it was confirmed that the larger the tan δ, the better the sound sounded without any mixed sounds, and the smaller the tan δ, the worse the sound sounded with the previous sound remaining and mixed with noise. In terms of sound vibration absorption, tan δ that was 0.05 or more smaller than the tan δ of the current resin speaker was evaluated as ×, tan δ within ±0.05 of the current resin speaker was evaluated as △, tan δ that was 0.05 or more larger than the tan δ of the current resin speaker was evaluated as ◯, and tan δ that was 0.1 or more larger than the tan δ of the current resin speaker was evaluated as ◎. The evaluation result of the sound characteristics of the same test piece was ◎.
[0046] Example 2 In Example 2, the fibrous filler concentration was changed to 70% by weight, the base resin was changed to 27.9% by weight, and the other material conditions and process conditions were the same as in Example 1 to produce pulp-dispersed polypropylene pellets and molded bodies. Evaluations were also performed in the same manner as in Example 1.
[0047] Example 3 In Example 3, the rotation speed during kneading was reduced to a low shear force that did not defibrate the ends of the fibrous filler, and other than that, pulp-dispersed polypropylene pellets and a molded body were produced in the same manner as in Example 1. Evaluations were also performed in the same manner as in Example 1.
[0048] Example 4 In Example 4, the pre-grinding conditions of the pulp, which is a fibrous filler, were changed so that the cracks caused by the pulp in the molded product would become larger, but the pulp-dispersed polypropylene pellets and molded product were produced in the same manner as in Example 1. The evaluation was also performed in the same manner as in Example 1.
[0049] Comparative Example 1 In Comparative Example 1, the fibrous filler concentration was changed to 30% by weight, the base resin was changed to 67.9% by weight, and the other material conditions and process conditions were the same as in Example 1 to produce pulp-dispersed polypropylene pellets and molded bodies. Evaluations were also performed in the same manner as in Example 1.
[0050] Comparative Example 2 In Comparative Example 2, the starting pulp was hydrophobized in advance with a silane coupling agent, and the other material conditions and process conditions were the same as in Example 1 to produce pulp-dispersed polypropylene pellets and a molded body. Evaluations were also performed in the same manner as in Example 1.
[0051] Comparative Example 3 In Comparative Example 3, the molding conditions were changed to extremely slow cooling so that the resin crystallinity near the fibrous filler was almost the same as that of the other areas, and the resin crystallinity around the tip and center of the fibrous filler was also almost the same. Other than that, pulp-dispersed polypropylene pellets and a molded body were produced in the same manner as in Example 1. Evaluations were also performed in the same manner as in Example 1.
[0052] Comparative Example 4 In Comparative Example 4, except that glass short fibers were used as the fibrous filler, pulp-dispersed polypropylene pellets and a molded body were produced in the same manner as in Example 1. The evaluations were also performed in the same manner as in Example 1.
[0053] The measurement results for each of Examples 1 to 4 and Comparative Examples 1 to 4 are shown in Table 1 of FIG.
[0054] As is clear from Table 1 in Figure 5, in Example 2 in which the fibrous filler concentration was changed to 70% by weight, the modulus of elasticity increased with the increased concentration, but the way in which the resin crystallized and the cracks on the surface of the molded body were the same as in Example 1, and it was confirmed that the sound characteristics were also good. It was confirmed that a composite resin with a high modulus of elasticity and good sound characteristics can be obtained if the fibrous filler is end-defibrated and not hydrophobized in advance, the crystallinity near the fibrous filler is greater than the crystallinity of other locations, and even with regard to the crystallinity near the fibrous filler, the crystallinity near the tip is greater than the crystallinity near the center of the fibrous filler, and the crack width near the surface of the molded body is 1 / 10 or less of the filler diameter.
[0055] In Example 3, where the ends of the fibrous filler were not defibrated, the degree of crystallinity near the tips of the fibrous filler was almost equal to the degree of crystallinity near the center of the fibrous filler, and the number of interfaces with differences in elastic modulus was reduced, resulting in sound characteristics that were not as good as those of Example 1.
[0056] In Example 4, in which the cracks caused by the pulp were made larger when the molded body was formed, the sound absorption properties deteriorated and the sound characteristics were not as good as those of Example 1.
[0057] In Comparative Example 1, in which the fibrous filler concentration was 30% by weight, the elastic modulus was low and the sound characteristics were also poor.
[0058] In Comparative Example 2, where the starting pulp was hydrophobized in advance, the crystallinity near the fibrous filler was almost the same as the crystallinity of the other areas, and the crystallinity near the tip of the fibrous filler was almost the same as the crystallinity near the center of the fibrous filler. In addition, the resin and the fibrous filler were well compatible, and there were no cracks on the surface of the molded product. These factors resulted in poor sound characteristics.
[0059] In comparison example 3, in which the degree of crystallinity of the resin near the fibrous filler was approximately the same as the degree of crystallinity elsewhere, and in which the degree of crystallinity of the resin around the tip and center of the fibrous filler was also approximately the same, the result was slightly worse sound characteristics.
[0060] In Comparative Example 4, in which short glass fibers were used as the fibrous filler, the elastic modulus was considerably high, but the sound absorption was poor, and the sound characteristics were not as good as those of Example 1.
[0061] From the above evaluation, it was confirmed that a composite resin molding with a high elastic modulus and good sound characteristics can be obtained if the fibrous filler content is 50% by weight or more, the ends of the fibrous filler are defibrated and not previously treated to be hydrophobic, the crystallinity near the fibrous filler is greater than the crystallinity of locations other than the fibrous filler, and the crystallinity near the tip of the fibrous filler is greater than the crystallinity near the center of the fibrous filler, and the crack width near the surface of the molding is 1 / 10 or less of the filler diameter.
[0062] In addition, the present disclosure includes appropriate combinations of any of the various embodiments and / or examples described above, and can achieve the effects of each embodiment and / or example. [Industrial Applicability]
[0063] The composite resin molded body for acoustic components according to the present invention can provide a molded body having superior mechanical strength and sound characteristics compared to conventional general-purpose resins. The composite resin molded body for acoustic components according to the present invention can improve the sound characteristics of the base resin, and can be used as an acoustic component such as a speaker, a housing component for sound-emitting electronic devices, home appliances, etc., a substitute for engineering plastics, or a substitute for metal materials. It can also be used as a building material or an automobile component. [Explanation of symbols]
[0064] 1. Base resin 2. Fibrous filler 3 Additives 4 Defibration site 5 End 6. Crack
Claims
1. A composite resin molding for acoustic components, comprising a base resin and a fibrous filler dispersed in the base resin, The concentration of the fibrous filler in the composite resin molding is 50% by weight or more, A composite resin molding for acoustic components, wherein the crystallinity of the base resin around the fibrous filler is higher than the crystallinity of the base resin in other areas of the composite resin molding.
2. A composite resin molding for acoustic components as described in claim 1, wherein in the composite resin molding, the crystallinity of the base resin around the tip of the fibrous filler is higher than the crystallinity of the base resin around the center of the fibrous filler.
3. 3. The composite resin molding for acoustic components according to claim 1, wherein the surface of the composite resin molding has holes or cracks, the width of which is 1 / 10 or less of the diameter of the fibrous filler.
4. 4. The composite resin molding for acoustic members according to claim 1, wherein the fibrous filler in the composite resin molding is not previously hydrophobized.
5. The composite resin molding for acoustic members according to claim 1 , wherein only the ends of the fibrous filler in the composite resin molding are defibrated.
6. The composite resin molding for acoustic members according to claim 1 , wherein the fibrous filler is a fiber made of natural fiber such as cellulose.
7. The composite resin molding for acoustic members according to claim 1 , wherein the base resin is an olefin resin.
Citation Information
Patent Citations
Molding composition, speaker unit mounting member using it, and speaker system using them
JP2004320670A
Polyolefin composite material, method for producing the same, and molded product thereof
JP2005307192A
Composite resin molding
JP2019085529A
Fiber composite resin composition and manufacturing method therefor
JP2019157049A
Composite resin molding
JP2020029546A