Resin composition and laminate
The resin composition with a (meth)acrylic resin, polycaprolactone polyol, and acrylic-modified chlorinated polyolefin addresses the issue of poor adhesion in vehicle body coatings, providing enhanced abrasion resistance and adhesion.
Patent Information
- Application Number
- JP2023083840
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-12-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing resin compositions for vehicle body coatings exhibit excellent abrasion resistance but lack sufficient adhesion to the substrate.
A resin composition containing a (meth)acrylic resin with a hydroxyl group, polycaprolactone polyol, a crosslinking agent, and acrylic-modified chlorinated polyolefin, with specific ratios and properties to enhance adhesion and maintain elongation characteristics.
The composition forms a coating layer with improved abrasion resistance and adhesion to the substrate, suitable for vehicle body applications.
Smart Images

Figure 2024167630000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition and a laminate. [Background technology]
[0002] There are known resin films that are attached to vehicle bodies for the purpose of decorating the bodies of vehicles such as automobiles and motorcycles. Such resin films generally have a laminate structure in which a pattern, characters, etc. are printed on the surface of a resin base material, and a coating layer is further provided thereon to improve abrasion resistance and suppress fading.
[0003] The resin film coating layer that is attached to the vehicle body must have sufficient stretchability to conform to the three-dimensional shape of the vehicle body. For example, Patent Document 1 describes a resin composition containing a (meth)acrylic resin having a hydroxyl group, polycaprolactone polyol, and a crosslinking agent as a material capable of forming a coating layer having excellent elongation properties. Patent Document 2 discloses a resin composition containing a hydroxyl-containing (meth)acrylic resin having a glass transition temperature of 60°C or higher, a polycaprolactone polyol, and a crosslinking agent, as a material capable of forming a coating layer having excellent elongation characteristics and improved abrasion resistance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special table number 2009-527392 [Patent Document 2] JP 2017-48264 A Summary of the Invention [Problem to be solved by the invention]
[0005] The coating layer formed from the resin composition described in Patent Document 2 exhibits excellent abrasion resistance, but there is room for improvement in adhesion to the substrate. An object of the present disclosure is to provide a resin composition capable of forming a coating layer having excellent abrasion resistance and adhesion to a substrate, and a laminate including a coating layer having excellent abrasion resistance and adhesion to a substrate. [Means for solving the problem]
[0006] Means for solving the above problems include the following embodiments. <1> A resin composition comprising a hydroxyl group-containing (meth)acrylic resin, a polycaprolactone polyol, a crosslinking agent, and an acrylic-modified chlorinated polyolefin. <2> The amount of the acrylic-modified chlorinated polyolefin is 1.0 parts by mass to 15.0 parts by mass per 100 parts by mass of the (meth)acrylic resin containing a hydroxyl group. <1> The resin composition according to claim 1. <3> The number average molecular weight of the polycaprolactone polyol is 300 or more and 2000 or less. <1> or <2> The resin composition according to claim 1. <4> The glass transition temperature of the hydroxyl group-containing (meth)acrylic resin is 50°C or higher. <1> ~ <3> 10. The resin composition according to claim 9 . <5> The crosslinking agent includes hydrogenated xylylene diisocyanate. <1> ~ <4> 10. The resin composition according to claim 9 . <6> For forming a coating layer on a substrate, <1> ~ <5> 10. The resin composition according to claim 9 . <7> The substrate comprises a resin. <6> The resin composition according to claim 1. <8> <1> ~ <7> 1. A laminate comprising a substrate and a coating layer comprising a cured product of the resin composition according to any one of the above items. <9> The substrate comprises a resin. <8> The laminate according to claim 1. Effect of the Invention
[0007] According to the present disclosure, there are provided a resin composition capable of forming a coating layer having excellent abrasion resistance and adhesion to a substrate, and a laminate including a coating layer having excellent abrasion resistance and adhesion to a substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] In the present disclosure, a numerical range indicated using "~" indicates a range including the numerical values before and after "~" as the minimum and maximum values, respectively. In addition, unless otherwise specified, the amount of each component in the composition is expressed as the total amount of multiple types of substances when each component contains multiple types of substances. In the present disclosure, (meth)acrylic means one or both of acrylic and methacrylic, (meth)acrylate means one or both of acrylate and methacrylate, and (meth)acryloyl means one or both of acryloyl and methacryloyl.
[0009] <Resin composition> The resin composition of the present disclosure contains a hydroxyl group-containing (meth)acrylic resin, a polycaprolactone polyol, a crosslinking agent, and an acrylic-modified chlorinated polyolefin.
[0010] As shown in the examples described later, a coating layer formed using the resin composition of the present disclosure exhibits excellent adhesion to a substrate. The reason for this can be considered as follows, for example.
[0011] The acrylic-modified chlorinated polyolefin contained in the resin composition of the present disclosure has polarity imparted to the molecular chain of the polyolefin by chlorination. Therefore, when a coating layer is formed on a substrate using the resin composition, the polyolefin functions to enhance the adhesion of the coating layer to the substrate. Furthermore, since the molecular chain of the polyolefin is acrylic-modified, the polyolefin has excellent compatibility with the hydroxyl group-containing (meth)acrylic resin contained as the main component in the resin composition. That is, the function of enhancing the adhesion of the coating layer imparted to the polyolefin by chlorination is further enhanced by the acrylic modification.
[0012] Furthermore, one method for improving the adhesion of the coating layer is to reduce the amount of polycaprolactone polyol contained in the resin composition, but reducing the amount of polycaprolactone polyol may impair the elongation properties of the coating layer.By incorporating an acrylic-modified chlorinated polyolefin into the resin composition, it is possible to improve the adhesion of the coating layer to the substrate without reducing the amount of polycaprolactone polyol (i.e., while maintaining good elongation properties).
[0013] [(Meth)acrylic resin having hydroxyl group] The resin composition contains a (meth)acrylic resin containing a hydroxyl group. When the resin composition contains a (meth)acrylic resin containing a hydroxyl group, the hydroxyl group of the (meth)acrylic resin reacts with the crosslinking agent to form a crosslinked structure, and a coating layer containing a cured product of the resin composition is formed.
[0014] Examples of the (meth)acrylic resin containing a hydroxyl group include polymers containing structural units derived from a (meth)acrylic monomer having a hydroxyl group. In the present disclosure, a (meth)acrylic monomer refers to a compound having at least one (meth)acryloyl group.
[0015] Examples of the (meth)acrylic monomer having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 3-methyl-3-hydroxybutyl (meth)acrylate, 1,3-dimethyl-3-hydroxybutyl (meth)acrylate, 2,2,4-trimethyl-3-hydroxypentyl (meth)acrylate, 2-ethyl-3-hydroxyhexyl (meth)acrylate, polypropylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, poly(ethylene glycol-propylene glycol) mono(meth)acrylate, pentaerythritol tri(meth)acrylate, etc. These (meth)acrylic monomers having a hydroxyl group may be used alone or in combination of two or more kinds.
[0016] The (meth)acrylic resin having a hydroxyl group may contain a structural unit derived from a monomer other than the (meth)acrylic monomer having a hydroxyl group. Examples of monomers other than the (meth)acrylic monomer having a hydroxyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, isobornyl (meth)acrylate, 2-methoxy (meth)acrylate, 2-ethoxy (meth)acrylate, glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and (meth)acrylic acid. These monomers may be used alone or in combination of two or more kinds.
[0017] From the viewpoint of the abrasion resistance of the coating layer, the proportion of structural units derived from (meth)acrylic monomers having a hydroxyl group among the structural units of the (meth)acrylic resin having a hydroxyl group is preferably 7.5 mass% or more, more preferably 10 mass% or more, and even more preferably 12.5 mass% or more. From the viewpoint of the elongation properties of the coating layer, the proportion of structural units derived from (meth)acrylic monomers having a hydroxyl group among the structural units of the (meth)acrylic resin having a hydroxyl group is preferably 7.5 mass% or less, more preferably 10 mass% or less, and even more preferably 12.5 mass% or less.
[0018] From the viewpoint of heat resistance of the coating layer, the glass transition temperature of the (meth)acrylic resin having a hydroxyl group is preferably 60° C. or higher, and more preferably 65° C. or higher. From the viewpoint of the elongation properties of the coating layer, the glass transition temperature of the (meth)acrylic resin having a hydroxyl group is preferably 90° C. or lower, and more preferably 80° C. or lower.
[0019] The glass transition temperature of a (meth)acrylic resin having a hydroxyl group is a value obtained by converting the absolute temperature (unit: K) calculated by the following formula 1 into Celsius temperature (unit: ° C.). 1 / Tg=m1 / Tg1+m2 / Tg2+ +m(k-1) / Tg(k-1)+mk / Tgk (Formula 1) In formula 1, Tg1, Tg2, . . ., Tg(k-1), and Tgk are glass transition temperatures expressed as absolute temperatures (K) when each monomer constituting the (meth)acrylic resin having a hydroxyl group is made into a homopolymer. m1, m2, . . ., m(k-1), and mk represent the mole fractions of each monomer constituting the (meth)acrylic resin having a hydroxyl group, respectively, and m1+m2+. . . +m(k-1)+mk=1. To convert from absolute temperature to Celsius temperature, subtract 273 from the absolute temperature value.
[0020] In the present disclosure, the "glass transition temperature when made into a homopolymer" refers to a value described in a publicly known document or a value measured using a differential scanning calorimeter (DSC). The specific values to be used are as follows:
[0021] For the "glass transition temperature when made into a homopolymer" of the monomers shown below, the value in parentheses is used. Methyl acrylate (10°C), methyl methacrylate (105°C), ethyl acrylate (-22°C), ethyl methacrylate (65°C), n-butyl acrylate (-54°C), n-butyl methacrylate (20°C), isobutyl methacrylate (53°C), t-butyl acrylate (43°C), t-butyl methacrylate (118°C), 2-ethylhexyl acrylate (-70°C), 2-ethylhexyl methacrylate (-10°C), n-octyl Acrylate (-65°C), cyclohexyl methacrylate (104°C), benzyl acrylate (6°C), phenoxyethyl acrylate (-22°C), 2-methoxyethyl methacrylate (-50°C), glycidyl methacrylate (74°C), 4-hydroxybutyl acrylate (-80°C), 2-hydroxyethyl acrylate (-15°C), 2-hydroxyethyl methacrylate (85°C), acrylic acid (106°C), methacrylic acid (228°C).
[0022] Regarding the "glass transition temperature when made into a homopolymer" of a monomer other than the above-mentioned monomers, the value described in the Polymer Handbook (4th edition, Wiley-Interscience; the same applies hereinafter) is adopted, and when there is no description in the Polymer Handbook, the glass transition temperature of the homopolymer obtained by the following measurement method is adopted.
[0023] Specifically, a differential scanning calorimeter (DSC) is used to measure the temperature of a sample (i.e., homopolymer) of 10 mg in a nitrogen gas flow at a temperature rise rate of 10° C. / min, and the inflection point of the obtained DSC curve is taken as the glass transition temperature of the homopolymer. As the differential scanning calorimeter, for example, a differential scanning calorimeter (trade name: Discovery DSC 2500) manufactured by TA Instruments Japan Co., Ltd. can be suitably used. However, the differential scanning calorimeter is not limited to this.
[0024] The glass transition temperature of the (meth)acrylic resin having a hydroxyl group can be adjusted by appropriately selecting the types and ratio of (meth)acrylic monomers that are polymerization components of the (meth)acrylic resin having a hydroxyl group. In an embodiment, the polymerization component of the (meth)acrylic resin having a hydroxyl group may include 2-hydroxyethyl acrylate (2HEA), or may include 2-hydroxyethyl acrylate (2HEA) and one or more selected from methyl methacrylate (MMA), n-butyl acrylate (n-BA), n-butyl methacrylate (n-BMA), and acrylic acid (AA).
[0025] From the viewpoint of the abrasion resistance of the coating layer, the weight average molecular weight of the (meth)acrylic resin having a hydroxyl group is preferably 7,000 or more. From the viewpoint of the elongation properties of the coating layer and the workability during the formation of the coating layer, the weight average molecular weight of the (meth)acrylic resin having a hydroxyl group is preferably 20,000 or less.
[0026] The weight-average molecular weight of the (meth)acrylic resin having a hydroxyl group can be determined by gel permeation chromatography using a standard polystyrene conversion method. More specifically, the weight-average molecular weight can be determined under the conditions of using a Tosoh Corporation "HLC-8220" as the GPC analysis system device, two Tosoh Corporation "TSKgel Super Multipore HZ-H" columns connected in series, a differential refractometer (RI) built into the GPC analysis system device as the detector, tetrahydrofuran as the mobile phase, a flow rate of 0.35 mL / min, and a column temperature of 40°C.
[0027] From the viewpoint of the abrasion resistance of the coating layer, the hydroxyl value of the (meth)acrylic resin having a hydroxyl group is preferably 25 mgKOH / g or more. From the viewpoint of the elongation properties of the coating layer, the hydroxyl value of the (meth)acrylic resin having a hydroxyl group is preferably 100 mgKOH / g or less.
[0028] The hydroxyl value of the (meth)acrylic resin having a hydroxyl group can be determined by the method described in JIS K0070:1992.
[0029] The (meth)acrylic resin having a hydroxyl group can be obtained by polymerizing a (meth)acrylic monomer having a hydroxyl group alone or a mixture of a (meth)acrylic monomer having a hydroxyl group and other monomers by a method such as solution polymerization, bulk polymerization, or emulsion polymerization.
[0030] [Polycaprolactone polyol] The resin composition of the present disclosure includes a polycaprolactone polyol. When the resin composition contains polycaprolactone polyol, a coating layer having excellent elongation properties can be formed.
[0031] The polycaprolactone polyol preferably has two or more hydroxyl groups, and more preferably has three to five hydroxyl groups, per molecule. When one molecule of polycaprolactone polyol has two or more hydroxyl groups, the crosslinking reaction proceeds sufficiently. Furthermore, when the number of hydroxyl groups per molecule of polycaprolactone polyol is 3 or more, the crystallinity of the polycaprolactone polyol is low, and the polycaprolactone polyol is sufficiently compatible with other components and easily dispersed uniformly in the resin composition. When the number of hydroxyl groups per molecule of the polycaprolactone polyol is 5 or less, the crosslink density falls within an appropriate range, and the elongation properties of the coating layer are sufficiently maintained.
[0032] Polycaprolactone polyol can be obtained by reacting a compound (polyol) having a plurality of hydroxyl groups in the molecule with caprolactone.
[0033] As the polycaprolactone polyol, a commercially available product may be used. Commercially available polycaprolactone polyols include Plaxel 305 (molecular weight 550, number of hydroxyl groups 3), Plaxel 303 (molecular weight 310, number of hydroxyl groups 3), Plaxel 208 (molecular weight 830, number of hydroxyl groups 2), Plaxel 210 (molecular weight 1000, number of hydroxyl groups 2), Plaxel 212 (molecular weight 1250, number of hydroxyl groups 2), and Plaxel 213 (molecular weight 1300, number of hydroxyl groups 1). Plaxel 220 (molecular weight 2000, number of hydroxyl groups 2), Plaxel 308 (molecular weight 850, number of hydroxyl groups 3), Plaxel 309 (molecular weight 900, number of hydroxyl groups 3), Plaxel 312 (molecular weight 1250, number of hydroxyl groups 3), Plaxel 320 (molecular weight 2000, number of hydroxyl groups 3) and Plaxel 410 (molecular weight 1000, number of hydroxyl groups 4), as well as Ingevi TY's CAPA2085 (molecular weight 830, 2 hydroxyl groups), CAPA2100 (molecular weight 1000, 2 hydroxyl groups), CAPA2121 (molecular weight 1250, 2 hydroxyl groups), CAPA2125 (molecular weight 1250, 2 hydroxyl groups), CAPA2200 (molecular weight 2000, 2 hydroxyl groups), CAPA2201 (molecular weight 2000, 2 hydroxyl groups), C Examples of the polycaprolactone polyol include APA2205 (molecular weight 2000, 2 hydroxyl groups), CAPA2209 (molecular weight 2000, 2 hydroxyl groups), CAPA3091 (molecular weight 900, 3 hydroxyl groups), CAPA3121J (molecular weight 1200, 3 hydroxyl groups), CAPA3201 (molecular weight 2000, 3 hydroxyl groups) and CAPA4101 (molecular weight 1000, 4 hydroxyl groups). One type of polycaprolactone polyol may be used alone, or two or more types may be used in combination.
[0034] From the viewpoint of the abrasion resistance of the coating layer, the molecular weight of the polycaprolactone polyol is preferably 300 or more, more preferably 400 or more, and even more preferably 500 or more. From the viewpoint of workability during formation of the coating layer, the molecular weight of the polycaprolactone polyol is preferably 1,500 or less, more preferably 1,000 or less, and even more preferably 600 or less.
[0035] The molecular weight of the above-mentioned polycaprolactone polyol is a number average molecular weight, and is measured in the same manner as the weight average molecular weight of the above-mentioned (meth)acrylic resin having a hydroxyl group.
[0036] From the viewpoint of the elongation properties of the coating layer, the content of polycaprolactone polyol in the resin composition is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, per 100 parts by mass of the (meth)acrylic resin having a hydroxyl group. From the viewpoint of the abrasion resistance of the coating layer and adhesion to the substrate, the content of polycaprolactone polyol in the resin composition is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 30 parts by mass or less, per 100 parts by mass of the (meth)acrylic resin having a hydroxyl group.
[0037] [Crosslinking agent] The resin composition of the present disclosure includes a crosslinking agent. The crosslinking agent reacts with the hydroxyl groups of the (meth)acrylic resin and the hydroxyl groups of the polycaprolactone polyol, thereby curing the resin composition.
[0038] From the viewpoint of reactivity with hydroxyl groups, the crosslinking agent is preferably a compound having an isocyanate group, and more preferably a compound having two or more isocyanate groups in one molecule (polyisocyanate). Examples of the polyisocyanate include hexamethylene diisocyanate (HDI), tolylene diisocyanate (TDI), xylylene diisocyanate (XDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), and hydrogenated products thereof. The polyisocyanate may be in the form of an isocyanurate. The resin composition may contain one type of crosslinking agent or two or more types of crosslinking agents.
[0039] From the viewpoint of the abrasion resistance of the coating layer, HDI and hydrogenated XDI are preferred as the crosslinking agent. From the viewpoint of workability (particularly blocking resistance) during the formation of the coating layer, hydrogenated XDI is more preferable as the crosslinking agent. From the viewpoint of suppressing yellowing due to ultraviolet rays or the like, the crosslinking agent is preferably a compound that does not contain an aromatic ring.
[0040] The content of the crosslinking agent in the resin composition is preferably such that the amount of crosslinkable groups in the crosslinking agent is 0.6 to 1.5 equivalents relative to the total amount (1 equivalent) of the hydroxyl groups of the (meth)acrylic resin and the hydroxyl groups of the polycaprolactone polyol, and more preferably 0.9 to 1.2 equivalents.
[0041] [Acrylic modified chlorinated polyolefin] The resin composition of the present disclosure includes an acrylic-modified chlorinated polyolefin. In the present disclosure, the acrylic-modified chlorinated polyolefin means a chlorinated polyolefin that has been subjected to an acrylic modification. The chlorinated polyolefin means a polyolefin into which chlorine has been introduced.
[0042] As the polyolefin in the acrylic modified chlorinated polyolefin, a polymer comprising structural units derived from an α-olefin such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, or 1-octene can be used without any particular limitation. From the viewpoint of adhesion and compatibility, the polyolefin is preferably a propylene homopolymer or a propylene copolymer containing a structural unit derived from propylene. The proportion of propylene-derived structural units in the propylene copolymer is preferably 50 mol % or more, more preferably 70 mol % or more, and even more preferably 80 mol % or more, of all structural units.
[0043] The method for chlorinating the polyolefin is not particularly limited. For example, the polyolefin may be chlorinated by blowing chlorine gas into a polyolefin dissolved in a solvent such as chloroform.
[0044] The weight average molecular weight of the chlorinated polyolefin is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 20,000 or more. The weight average molecular weight of the chlorinated polyolefin is preferably 200,000 or less, more preferably 90,000 or less, and even more preferably 70,000 or less.
[0045] The weight average molecular weight of the chlorinated polyolefin is measured in the same manner as the weight average molecular weight of the above-mentioned (meth)acrylic resin having a hydroxyl group.
[0046] From the viewpoint of improving the adhesion of the coating layer to the substrate, the chlorine content of the acrylic-modified chlorinated polyolefin is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more. From the viewpoint of the abrasion resistance of the coating layer, the chlorine content of the acrylic-modified chlorinated polyolefin is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less. The above chlorine content is the chlorine content in the polyolefin excluding the mass of the (meth)acrylic monomer used in the acrylic modification treatment.
[0047] The type of (meth)acrylic monomer used for the acrylic modification of the chlorinated polyolefin is not particularly limited, and can be selected depending on the desired physical properties of the acrylic-modified chlorinated polyolefin. The (meth)acrylic monomer used for the acrylic modification is not particularly limited, and may be selected from those mentioned above as the (meth)acrylic monomers constituting the structural units of the (meth)acrylic resin having a hydroxyl group. The (meth)acrylic monomer used for the acrylic modification may be one type alone or two or more types.
[0048] From the viewpoint of further enhancing the adhesion of the coating layer to the substrate, it is preferable that the (meth)acrylic monomer used for the acrylic modification of the chlorinated polyolefin contains a (meth)acrylic monomer having a hydroxyl group (hereinafter also referred to as monomer A).
[0049] Examples of the monomer A include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 3-methyl-3-hydroxybutyl (meth)acrylate, 1,3-dimethyl-3-hydroxybutyl (meth)acrylate, 2,2,4-trimethyl-3-hydroxypentyl (meth)acrylate, 2-ethyl-3-hydroxyhexyl (meth)acrylate, polypropylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, poly(ethylene glycol-propylene glycol) mono(meth)acrylate, pentaerythritol tri(meth)acrylate, etc. Among these, 2-hydroxyethyl (meth)acrylate is preferred.
[0050] The proportion of monomer A in the (meth)acrylic monomer used for the acrylic modification of the chlorinated polyolefin is preferably 0.1 mol % or more, more preferably 1 mol % or more, even more preferably 2 mol % or more, and even more preferably 3 mol % or more. The proportion of monomer A in the (meth)acrylic monomer used for the acrylic modification of the chlorinated polyolefin is preferably 30 mol % or less, more preferably 20 mol % or less, even more preferably 15 mol % or less, and even more preferably 10 mol % or less.
[0051] The (meth)acrylic monomer used for the acrylic modification of the chlorinated polyolefin preferably contains a (meth)acrylic monomer having an unsubstituted alkyl group having 4 or more carbon atoms (hereinafter also referred to as monomer B). The alkyl group in monomer B may be linear, branched or cyclic, and is preferably linear or cyclic. The number of carbon atoms in the alkyl group is preferably 18 or less, more preferably 10 or less, and even more preferably 8 or less.
[0052] Examples of the monomer B include n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, and cyclohexyl (meth)acrylate. Among these, n-butyl (meth)acrylate and cyclohexyl (meth)acrylate are preferred.
[0053] The proportion of monomer B in the (meth)acrylic monomer used for the acrylic modification of the chlorinated polyolefin is preferably 25 mol % or more, more preferably 30 mol % or more, and even more preferably 40 mol % or more. The proportion of monomer B in the (meth)acrylic monomer used for the acrylic modification of the chlorinated polyolefin is preferably 90 mol % or less, more preferably 80 mol % or less, even more preferably 70 mol % or less, and even more preferably 60 mol % or less.
[0054] When the (meth)acrylic monomer used for the acrylic modification of the chlorinated polyolefin contains monomer A and monomer B, the molar ratio (monomer A / monomer B) is preferably 1 / 100 to 1 / 1.5, more preferably 1 / 50 to 1 / 2, and even more preferably 1 / 50 to 1 / 4.
[0055] The (meth)acrylic monomer used for the acrylic modification of the chlorinated polyolefin may include a (meth)acrylic monomer that does not fall under (meth)acrylic monomer A or (meth)acrylic monomer B. For example, it may include a (meth)acrylic monomer having an alkoxy group such as 2-methoxyethyl (meth)acrylate, a (meth)acrylic monomer having an unsubstituted alkyl group having 3 or less carbon atoms such as methyl (meth)acrylate, (meth)acrylic acid, etc.
[0056] The method for carrying out the acrylic modification of the chlorinated polyolefin is not particularly limited, and can be carried out by a known graft polymerization method such as a solution method, a melting method, etc. For example, the acrylic modification of the chlorinated polyolefin may be carried out by reacting the chlorinated polyolefin dissolved in a solvent with a (meth)acrylic monomer in the presence of a radical reaction initiator.
[0057] The acrylic-modified chlorinated polyolefin may be in a state of a mixture with a polymer of a (meth)acrylic monomer that has not reacted with the chlorinated polyolefin during the acrylic modification treatment. In this case, the content of the component derived from the (meth)acrylic monomer in the mixture is preferably 1% by mass to 94% by mass, more preferably 5% by mass to 90% by mass.
[0058] In the above, the "component derived from a (meth)acrylic monomer" is a concept including a component derived from a (meth)acrylic monomer that has reacted with a chlorinated polyolefin during the acrylic modification treatment, and a component derived from a (meth)acrylic monomer that has not reacted with a chlorinated polyolefin.
[0059] The acrylic-modified chlorinated polyolefin may be acid-modified with an α,β-unsaturated carboxylic acid or a derivative thereof. From the viewpoint of ease of introduction into polyolefin, the α,β-unsaturated carboxylic acid or a derivative thereof is preferably maleic anhydride.
[0060] When the acrylic-modified chlorinated polyolefin is acid-modified, the degree of modification is preferably more than 0 mass % and not more than 20 mass %, and more preferably more than 0 mass % and not more than 10 mass %. The degree of modification is the proportion by mass of the α,β-unsaturated carboxylic acid or its derivative in the total mass of the chlorinated polyolefin and the α,β-unsaturated carboxylic acid or its derivative used for the acid modification.
[0061] The weight average molecular weight of the acrylic-modified chlorinated polyolefin is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 20,000 or more. The weight average molecular weight of the acrylic-modified chlorinated polyolefin is preferably 200,000 or less, more preferably 90,000 or less, and even more preferably 70,000 or less.
[0062] The weight average molecular weight of the acrylic-modified chlorinated polyolefin is measured in the same manner as the weight average molecular weight of the above-mentioned hydroxyl group-containing (meth)acrylic resin.
[0063] From the viewpoint of adhesion of the coating layer to the substrate, the content of the acrylic-modified chlorinated polyolefin in the resin composition is preferably 1.0 part by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 5.0 parts by mass or more, per 100 parts by mass of the (meth)acrylic resin having a hydroxyl group. From the viewpoint of the abrasion resistance of the coating layer, the content of the acrylic-modified chlorinated polyolefin in the resin composition is preferably 15.0 parts by mass or less, more preferably 10.0 parts by mass or less, and even more preferably 8.0 parts by mass or less, per 100 parts by mass of the (meth)acrylic resin having a hydroxyl group.
[0064] [Other ingredients] The resin composition of the present disclosure may contain other components as necessary, such as a solvent, a leveling agent, a light stabilizer, an antioxidant, a plasticizer, a surfactant, a colorant, a glitter, and a filler.
[0065] Examples of the solvent include ketone-based solvents such as cyclohexanone, isophorone, diacetone alcohol, acetone, methyl ethyl ketone, methyl isobutyl ketone, and methylcyclohexanone, ester-based solvents such as ethyl acetate, propyl acetate, butyl acetate, propylene glycol monomethyl ether acetate, butyl cellosolve acetate, and carbitol acetate, aliphatic hydrocarbon-based solvents such as hexane, cyclohexane, octane, mineral spirits, and kerosene, aromatic hydrocarbon-based solvents such as toluene, xylene, and 1,2,4-trimethylbenzene, and halogen-based solvents such as methylene chloride, chloroform, carbon tetrachloride, dichloroethane, dichloroethylene, trichloroethylene, tetrachloroethylene, chlorobenzene, and dichlorobenzene. The solvents may be used alone or in combination of two or more.
[0066] When forming a coating layer using a resin composition by screen printing, it is preferable to use a solvent with an evaporation rate ratio of 0.3 or less. Here, the evaporation rate ratio is the relative speed value of each solvent when the evaporation rate of butyl acetate is set to 1. The smaller the evaporation rate ratio of the solvent, the slower the evaporation rate. When the resin composition contains a solvent with an evaporation rate ratio of 0.3 or less, plate drying during screen printing is suppressed, and workability tends to improve.
[0067] Examples of the leveling agent include fluorine-based leveling agents, silicon-based leveling agents, and acrylic leveling agents. The leveling agent is oriented on the surface when the coating layer formed from the resin composition dries, and uniforms the surface tension of the coating layer. As a result, appearance defects such as floating spots and repelling are prevented, and wetting with the substrate is improved. Specific examples of the leveling agent include "Polyflow" (acrylic leveling agent manufactured by Kyoeisha Chemical Co., Ltd.), "Disparlon" (Kusumoto Chemical Co., Ltd.), and "BYK" (BYK Japan). The leveling agent may be used alone or in combination of two or more types.
[0068] Specific examples of the defoaming agent include "DOWSIL" (Dow Toray Co., Ltd., silicone-based defoaming agent), "Shin-Etsu Silicone" (Shin-Etsu Chemical Co., Ltd.), TSF451 series, TFH450 series (Momentive Performance Materials), etc. The defoaming agent may be used alone or in combination of two or more types. When the resin composition contains a defoaming agent, the content of the defoaming agent is preferably 0.1 to 0.5 parts by mass per 100 parts by mass of the (meth)acrylic resin containing a hydroxyl group.
[0069] Specific examples of the ultraviolet absorbing agent include "Tinuvin 400" (BASF). The ultraviolet absorbing agent may be used alone or in combination of two or more kinds. When the resin composition contains an ultraviolet absorber, the content of the ultraviolet absorber is preferably 1 to 3 parts by mass based on 100 parts by mass of the (meth)acrylic resin containing a hydroxyl group.
[0070] Specific examples of light stabilizers include "Tinuvin 770" (BASF). The light stabilizers may be used alone or in combination of two or more. When the resin composition contains a light stabilizer, the content of the light stabilizer is preferably 1 part by mass to 3 parts by mass based on the (meth)acrylic resin containing a hydroxyl group.
[0071] As the colorant, any known colorant can be used as appropriate, but from the viewpoint of light resistance, pigments are preferred.
[0072] The resin composition of the present disclosure is suitable as a material for a coating layer provided on a substrate, particularly when the substrate contains a resin. The method for forming a coating layer using the resin composition is not particularly limited, and can be performed by screen printing, gravure printing, bar coating, knife coating, roll coating, blade coating, die coating, spray coating, electrostatic coating, dip coating, or the like.
[0073] The thickness of the coating layer formed using the resin composition of the present disclosure is not particularly limited and can be selected according to the application. For example, it can be in the range of 1 μm to 100 μm, and preferably in the range of 3 μm to 20 μm.
[0074] <Laminate> The laminate of the present disclosure includes a substrate and a coating layer containing a cured product of the resin composition described above. The laminate may include a member other than the coating layer and the substrate as necessary. For example, it may include a layer containing a pressure-sensitive adhesive or adhesive for attaching the laminate to an adherend, or it may include a printed layer on which a pattern, letters, etc. are printed. The printed layer may be provided between the coating layer and the substrate.
[0075] The material of the substrate is not particularly limited. Examples include resin, metal, ceramics, paper, wood, and combinations thereof. Since the coating layer contained in the laminate of the present disclosure has excellent elongation properties, a substrate having flexibility can also be used. The thickness of the substrate is not particularly limited and can be selected according to the application. For example, it can be in the range of 20 μm to 500 μm, and preferably in the range of 30 μm to 100 μm.
[0076] Examples of resins that can be used as the substrate include polyvinyl chloride, polyvinylidene chloride, polyvinylidene fluoride, poly(ethylene-tetrafluoroethylene), polycarbonate, polyester, poly(meth)acrylate, polyolefin, polyamide, polyvinyl alcohol, polystyrene, polyurethane, etc. These resins may be used alone or in combination of two or more. When two or more resins are used in combination, they may be mixed and used, or two or more substrates made of different resins may be used in combination.
[0077] Among the above resins, polyvinyl chloride allows easy adjustment of the elongation properties of the substrate by adding a plasticizer, etc. Therefore, even if the shape of the adherend surface to which the laminate is attached is complex, the laminate can be made to sufficiently conform to the shape of the adherend.
[0078] The coating layer is formed by applying the above-mentioned resin composition onto a substrate or a printing layer provided as necessary, and curing the composition. The method of applying the resin composition is not particularly limited, and examples thereof include screen printing, gravure printing, bar coating, knife coating, roll coating, blade coating, die coating, spray coating, electrostatic coating, and dip coating. Among these, screen printing is preferred. The method of curing the resin composition is not particularly limited, and can be performed using hot air drying, an oven, a hot plate, or the like.
[0079] The thickness of the coating layer is not particularly limited and can be selected according to the application. For example, it can be in the range of 1 μm to 100 μm, and preferably in the range of 3 μm to 20 μm.
[0080] When the laminate includes a printed layer between the coating layer and the substrate, the method for forming the printed layer is not particularly limited. For example, the printed layer is formed by applying a resin composition containing a resin, a colorant, a solvent, etc., to the substrate by a method such as screen printing, and optionally through steps such as drying and curing.
[0081] The laminate of the present disclosure has excellent abrasion resistance of the coating layer and excellent adhesion to the substrate, and is therefore suitable for use as a film, sticker, etc. that is attached to the body of a vehicle or an object installed outdoors. EXAMPLES
[0082] The present invention will be specifically illustrated below with reference to examples, but the present invention is not limited to these examples in any way.
[0083] [Preparation of resin composition] Resin compositions having the compositions (parts by mass, calculated as solid content) shown in Table 1 were prepared.
[0084] [Table 1]
[0085] Details of the materials shown in Table 1 are as follows. Resin 1: (meth)acrylic resin consisting of a monomer composition of MMA (81.5 parts by mass), n-BA (5 parts by mass), 2HEA (12.5 parts by mass) and AA (1.0 part by mass), weight average molecular weight 8000, glass transition temperature 72°C Resin 2: (meth)acrylic resin consisting of a monomer composition of MMA (78.0 parts by mass), n-BA (8 parts by mass), 2HEA (12.5 parts by mass) and AA (1.5 parts by mass), weight average molecular weight 8000, glass transition temperature 66°C Resin 3: (meth)acrylic resin consisting of a monomer composition of MMA (85.5 parts by mass), 2HEA (13.0 parts by mass) and AA (1.5 parts by mass), weight average molecular weight 8000, glass transition temperature 83°C Resin 4: (meth)acrylic resin having a monomer composition of MMA (47.0 parts by mass), n-BMA (32.0 parts by mass), n-BA (7 parts by mass), 2HEMA (13.0 parts by mass) and AA (1.0 part by mass), weight average molecular weight 8000, glass transition temperature 55°C
[0086] PCL1: Polycaprolactone polyol with a molecular weight of 550 and three hydroxyl groups per molecule PCL2: Polycaprolactone polyol with a molecular weight of 310 and three hydroxyl groups per molecule PCL3: Polycaprolactone polyol with a molecular weight of 850 and three hydroxyl groups per molecule PCL4: Polycaprolactone polyol with a molecular weight of 2000 and three hydroxyl groups per molecule
[0087] Crosslinking agent 1: HDI-based crosslinking agent (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate HK") Crosslinking agent 2: Hydrogenated XDI-based crosslinking agent (manufactured by Mitsui Takeda Chemicals, Inc., product name "Takenate D-120N") Crosslinking agent 3: IPDI-based crosslinking agent (manufactured by Mitsui Takeda Chemicals, Inc., product name "Takenate D-140N")
[0088] PO1: Chlorinated polyolefin (acrylic modified, Nippon Paper Industries Co., Ltd., product name "Super Chron 224H", solid content 55.0%) PO2: Chlorinated polyolefin (non-acrylic modified, Nippon Paper Industries Co., Ltd., product name "Super Chron 813A", solid content 55.0%)
[0089] In addition to the components shown in Table 1, each resin composition contained an antifoaming agent (0.5 parts by mass), an ultraviolet absorber (2.0 parts by mass), a light stabilizer (2.0 parts by mass), acetylacetone (8.4 parts by mass) as a crosslinking retarding solvent, and a mixed solvent (30 parts by mass) of butyl cellosolve acetate (manufactured by Taishin Chemical Co., Ltd.) and Solvesso 100 (manufactured by Mitsubishi Shoji Chemical Co., Ltd.) in a 1:1 volume ratio as a dilution solvent.
[0090] [Laminated body production] An adhesive-treated polyvinyl chloride film (manufactured by Nippon Carbide Industries Co., Ltd., product name "Hi-ESCAL 0010H") was used as the substrate, and a printed layer was formed on the substrate by screen printing using color inks. The color ink was prepared by adding a mixed solvent (30 parts by mass) of butyl cellosolve acetate (manufactured by Taishin Chemical Co., Ltd.) and Solvesso 100 (manufactured by Mitsubishi Shoji Chemical Co., Ltd.) in a 1:1 volume ratio to 70 parts by mass of red ink (manufactured by Teikoku Ink Co., Ltd., product name "VK911"). The resin composition was applied by screen printing to the surface of the substrate on which the printed layer was formed so that the thickness after drying would be 9 μm. The resin composition was then cured by heating and drying at 80° C. for 60 minutes to form a coating layer.
[0091] [Adhesion evaluation] The coating layer was cut into 100 grids (10 × 10) spaced 1 mm apart. The surface of the laminate with the coating layer was then attached to an aluminum plate. 48 hours after attachment, the laminate was rapidly peeled off from the aluminum plate at an angle of 90°, and the degree of peeling of the coating layer from the substrate was evaluated based on the number (N) of grids remaining on the aluminum plate. Those in which no peeling of the coating layer occurred (N=0) were rated as "A," those in which slight peeling of the coating layer occurred (N=1 or more but less than 50) were rated as "B," and those in which significant peeling of the coating layer occurred (N=50 or more) were rated as "C." The results are shown in Table 1.
[0092] [Evaluation of wear resistance] The laminate was left to stand for 168 hours in an environment of 23°C and 50% RH. The laminate was then cut into a size of 100 mm x 100 mm, and the adhesive surface was attached to an aluminum plate. A CS-10 abrasion wheel was attached to a Taber abrasion tester (Toyo Seiki Seisakusho Co., Ltd., MODEL 5130), and the abrasion wheel was rotated on the coating layer at a load of 500 g and a speed of 60 revolutions per minute, and the abrasion resistance of the coating layer was evaluated from the rotation speed of the abrasion wheel when the substrate was exposed. Those in which the substrate was not exposed even after 1000 revolutions of the abrasive wheel were rated as "A", those in which the substrate was exposed between 500 and 1000 revolutions were rated as "B", and those in which the substrate was exposed in less than 500 revolutions were rated as "C". The results are shown in Table 1.
[0093] As shown in Table 1, the laminates of the examples prepared using resin compositions containing a hydroxyl group-containing (meth)acrylic resin, a polycaprolactone polyol, a crosslinking agent, and an acrylic-modified chlorinated polyolefin exhibited superior abrasion resistance and adhesion to substrates compared with the laminates of the comparative examples prepared using resin compositions that did not contain a chlorinated polyolefin or contained a non-acrylic-modified chlorinated polyolefin.
Claims
1. A resin composition comprising a hydroxyl group-containing (meth)acrylic resin, a polycaprolactone polyol, a crosslinking agent, and an acrylic-modified chlorinated polyolefin.
2. 2. The resin composition according to claim 1, wherein the amount of the acrylic-modified chlorinated polyolefin is 1.0 to 15.0 parts by mass per 100 parts by mass of the (meth)acrylic resin containing a hydroxyl group.
3. The resin composition according to claim 1 , wherein the polycaprolactone polyol has a number average molecular weight of 300 or more and 2,000 or less.
4. The resin composition according to claim 1, wherein the hydroxyl group-containing (meth)acrylic resin has a glass transition temperature of 50° C. or higher.
5. The resin composition of claim 1 , wherein the crosslinking agent comprises hydrogenated xylylene diisocyanate.
6. The resin composition according to any one of claims 1 to 5, for forming a coating layer on a substrate.
7. The resin composition according to claim 6 , wherein the substrate comprises a resin.
8. A laminate comprising a coating layer comprising a cured product of the resin composition according to any one of claims 1 to 5 and a substrate.
9. The laminate according to claim 8 , wherein the substrate comprises a resin.
Citation Information
Patent Citations
Method of forming an article having a decorative surface
JP2009527392A
Ink and laminate
JP2017048264A