Method of producing conductive polymer dispersion and method of manufacturing solid electrolytic capacitor

The method of producing a conductive polymer dispersion at elevated temperatures and specific pH conditions improves the withstand voltage of solid electrolytic capacitors, addressing the need for higher voltage in power electronics applications.

JP2024167665AInactive Publication Date: 2024-12-04NIPPON CHEMI CON CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023083892
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Solid electrolytic capacitors require higher withstand voltage to meet the increasing power consumption demands in power electronics, particularly in converter and inverter circuits, while maintaining low equivalent series resistance (ESR).

Method used

A method for producing a conductive polymer dispersion by polymerizing 2-ethyl-3,4-ethylenedioxythiophene in a solution containing polystyrene sulfonic acid at a liquid temperature of 30°C or higher, adjusting the pH to 3 or more and 6 or less, and forming a solid electrolyte layer between an anode and cathode bodies using this dispersion.

Benefits of technology

The method enhances the withstand voltage of solid electrolytic capacitors, making them suitable for high-power applications by optimizing conductivity and crystallinity of the solid electrolyte layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167665000001_ABST
    Figure 2024167665000001_ABST
Patent Text Reader

Abstract

To provide a method of producing a conductive polymer dispersion for manufacturing a solid electrolytic capacitor having a high withstand voltage, and a method of manufacturing a solid electrolytic capacitor having a high withstand voltage.SOLUTION: A method of producing a conductive polymer dispersion includes a polymerization step of polymerizing 2-ethyl-3,4-ethylenedioxythiophene in liquid in which a polystyrene sulfonic acid is present. In the polymerization step, a liquid temperature during polymerization is set to 30°C or higher. The solid electrolytic capacitor is manufactured by forming a solid electrolyte layer between an anode body and a cathode body using the conductive polymer dispersion obtained by the production method.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a conductive polymer dispersion for forming a solid electrolyte of a solid electrolytic capacitor, and a method for producing a solid electrolytic capacitor. [Background technology]

[0002] An electrolytic capacitor has anode and cathode foils made of valve metals such as tantalum or aluminum. The anode foil is enlarged by forming the valve metal into a sintered or etched foil, and the enlarged surface is coated with a dielectric film by anodizing or other treatment. An electrolyte is interposed between the anode and cathode foils.

[0003] Electrolytic capacitors have the advantage that they can easily obtain a large capacitance compared to other types of capacitors because the specific surface area can be increased by expanding the surface area of ​​the anode foil. Electrolytic capacitors contain electrolyte in the form of an electrolyte solution. The contact area of ​​the electrolyte solution with the dielectric film of the anode foil increases. This makes it easier to further increase the capacitance of electrolytic capacitors.

[0004] In recent years, solid electrolytic capacitors, which use a solid electrolyte with higher conductivity than the electrolyte, have also been attracting attention. Solid electrolytic capacitors use a solid electrolyte with higher conductivity than the electrolyte, and can achieve low equivalent series resistance (ESR). Manganese dioxide and 7,7,8,8-tetracyanoquinodimethane (TCNQ) complexes are known as solid electrolytes.

[0005] In addition, conductive polymers derived from monomers with π-conjugated double bonds, such as poly(3,4-ethylenedioxythiophene) (PEDOT), which has excellent adhesion to dielectric films, are rapidly becoming popular as solid electrolytes. Conductive polymers use acid compounds such as polyanions as dopants to develop high conductivity. Therefore, solid electrolytic capacitors have the advantage of low equivalent series resistance (ESR).

[0006] A solid electrolyte containing a conductive polymer is formed by applying or impregnating a conductive polymer dispersion between an anode body and a cathode body and drying the dispersion medium. The conductive polymer dispersion is a dispersion of a conductive polymer, and for example, water is used as the dispersion medium to disperse the conductive polymer in water. The conductive polymer is produced by mixing a monomer, which becomes a monomer unit of the conductive polymer, a dopant, and an oxidizing agent, and subjecting the mixture to chemical oxidative polymerization. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2011-60980 A [Patent Document 2] JP 2014-152320 A Summary of the Invention [Problem to be solved by the invention]

[0008] Capacitors are used in various applications. For example, in the field of power electronics, a power supply circuit converts the power of an AC power source into DC power using a converter circuit, and then converts the DC power into a desired AC power using an inverter circuit. In order to suppress and smooth the pulsation of the DC output from the converter circuit before inputting it to the inverter circuit, a smoothing capacitor is provided. In addition, a decoupling capacitor is provided near a semiconductor switching element such as gallium nitride to ensure stable operation of the semiconductor switching element and to remove noise.

[0009] With the trend toward higher power in the field of power electronics, a higher withstand voltage is also required for this solid electrolytic capacitor. The present invention has been proposed to solve the above-mentioned problems, and an object of the present invention is to provide a method for producing a conductive polymer dispersion liquid that increases the withstand voltage of a solid electrolytic capacitor. [Means for solving the problem]

[0010] In order to solve the above problems, the method for producing a conductive polymer dispersion liquid of the present embodiment includes a polymerization step of polymerizing 2-ethyl-3,4-ethylenedioxythiophene in a liquid in the presence of polystyrene sulfonic acid, and in the polymerization step, the liquid temperature during polymerization is 30° C. or higher.

[0011] In the polymerization step, the liquid temperature during polymerization may be set to 30° C. or higher and 50° C. or lower.

[0012] The method may further include a step of adjusting the pH of the dispersion liquid obtained through the polymerization step and having the conductive polymer dispersed therein to a value of 3 or more and 6 or less.

[0013] Another aspect of the present invention is a method for producing a solid electrolytic capacitor, comprising forming a solid electrolyte layer between an anode body and a cathode body using the conductive polymer dispersion obtained by this production method. Effect of the Invention

[0014] According to the present invention, a solid electrolytic capacitor with high withstand voltage can be realized. [Brief description of the drawings]

[0015] [Figure 1] 1 is a graph in which the horizontal axis represents the polymerization temperature and the vertical axis represents the electrical conductivity of the solid electrolyte layer. [Diagram 2] 1 is a graph in which the horizontal axis represents the polymerization temperature and the vertical axis represents the withstand voltage of the solid electrolytic capacitor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following describes embodiments of the present invention. However, the present invention is not limited to the embodiments described below.

[0017] (Conductive polymer dispersion) A conductive polymer dispersion is a dispersion in which a conductive polymer is dispersed in a dispersion medium. The conductive polymer dispersion is used to form a solid electrolyte layer in a solid electrolytic capacitor. A solid electrolyte layer containing the conductive polymer is formed by volatilizing the dispersion medium of the conductive polymer liquid through drying.

[0018] The conductive polymer is polyethylated ethylenedioxythiophene (hereinafter referred to as Et-PEDOT) doped with polystyrene sulfonic acid (hereinafter referred to as PSS). Et-PEDOT is a polymer with ethylated ethylenedioxythiophene (hereinafter referred to as Et-EDOT) as a monomer unit. Ethylated ethylenedioxythiophene is 2-ethyl-2,3-dihydro-thieno[3,4-b][1,4]dioxine, in which an ethyl group is added to 3,4-ethylenedioxythiophene.

[0019] The dispersion medium of the conductive polymer dispersion may be any medium in which the particles or powder of Et-PEDOT doped with PSS can be dispersed. The dispersion medium is typically water, but may also be an organic solvent or a mixture of an organic solvent and water. Examples of organic solvents include polar solvents, alcohols, esters, hydrocarbons, carbonate compounds, ether compounds, chain ethers, heterocyclic compounds, and nitrile compounds.

[0020] Examples of polar solvents include N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide. Examples of alcohols include methanol, ethanol, propanol, and butanol. Examples of esters include ethyl acetate, propyl acetate, and butyl acetate. Examples of hydrocarbons include hexane, heptane, benzene, toluene, and xylene. Examples of carbonate compounds include ethylene carbonate and propylene carbonate. Examples of ether compounds include dioxane and diethyl ether. Examples of chain ethers include ethylene glycol dialkyl ether, propylene glycol dialkyl ether, polyethylene glycol dialkyl ether, and polypropylene glycol dialkyl ether. Examples of heterocyclic compounds include 3-methyl-2-oxazolidinone. Examples of nitrile compounds include acetonitrile, glutarodinitrile, methoxyacetonitrile, propionitrile, and benzonitrile.

[0021] The conductive polymer dispersion may contain additives such as polyhydric alcohols. Examples of polyhydric alcohols include polyethylene glycol, 1-hexanol, ethylene glycol, diethylene glycol, triethylene glycol, or a combination of two or more of these. Since polyhydric alcohols have a high boiling point, they remain in the solid electrolyte layer even after the conductive polymer dispersion is dried. Furthermore, the conductive polymer dispersion may contain other compounds. The other compounds are, for example, conventional additives such as organic binders, surfactants, antifoaming agents, coupling agents, antioxidants, and ultraviolet absorbers.

[0022] In this conductive polymer dispersion, the conductive polymer is produced by a polymerization process. In the polymerization process, the monomer Et-EDOT, the dopant PSS, and an oxidant are mixed and stirred until chemical oxidation polymerization is completed. After the polymerization process, residual monomers and impurities are removed by purification means such as ultrafiltration, cation exchange, and anion exchange. This results in a conductive polymer dispersion. The conductive polymer is dispersed using, for example, ultrasound. In the polymerization process, an acid or its alkali metal salt that releases PSS may be mixed in place of PSS.

[0023] It is preferable that Et-EDOT is added to the conductive polymer dispersion at a concentration of 1 mM or more and 6.25 mM or less. In this range, the conductive polymer is less likely to aggregate. In addition, in this range, the heat resistance is improved, and even if the solid electrolyte layer is exposed to a high-temperature environment, the deterioration of various characteristics of the solid electrolytic capacitor is suppressed.

[0024] The number average molecular weight of the PSS is 1,000 to 2,000,000, and preferably 10,000 to 500,000. If the number average molecular weight is less than 1,000, the conductivity of the resulting conductive polymer is insufficient and dispersibility is reduced, which is not preferred, whereas if the number average molecular weight exceeds 2,000,000, the viscosity of the mixture increases, which is not preferred.

[0025] The oxidizing agent is preferably an iron salt of an inorganic acid or an organic acid, or a persulfate. For example, ferric chloride hexahydrate, anhydrous ferric chloride, ferric nitrate nonahydrate, ferric nitrate, ferrous sulfate, ferric sulfate, ferric sulfate n-hydrate, ferric ammonium sulfate dodecahydrate, ferric perchlorate n-hydrate, ferric tetrafluoroborate, cupric chloride, cupric sulfate, cupric tetrafluoroborate, nitrosonium tetrafluoroborate, ammonium persulfate, sodium persulfate, potassium persulfate, potassium periodate, hydrogen peroxide, ozone, potassium ferric hexacyano, tetraammonium cerium (IV) sulfate dihydrate, bromine, iodine, ferric dodecylbenzenesulfonate, ferric paratoluenesulfonate, ferric naphthalenesulfonate, ferric anthraquinonesulfonate, periodic acid, iodic acid, etc. may be used as the oxidizing agent, or a single compound may be used as the oxidizing agent, or two or more compounds may be used as the oxidizing agent.

[0026] In particular, it is preferable to use an iron salt such as ferrous sulfate in combination with a peroxodisulfate as the oxidizing agent. The iron salt serves as an oxidation initiator and catalyst, and the peroxodisulfate serves as an oxidation promoter. That is, the divalent iron ion of the oxidizing agent reacts with the persulfate ion to form radical sulfate ions, and the oxidation reaction of the monomer is promoted by the radical sulfate ions. The divalent iron ion reacting with the persulfate ion becomes a trivalent iron ion, oxidizes the monomer, returns to a divalent iron ion, and reacts with the persulfate ion again, repeating this cycle. It is preferable to adjust the pH of the polymerization solution to the acidic side by adding sulfuric acid or the like. For example, the polymerization reaction is promoted by adjusting the polymerization solution to the acidic side, such as pH=1.9.

[0027] Here, from the viewpoint of setting the conductivity, which is a basic characteristic of the solid electrolyte layer, in the best range, the liquid temperature during polymerization, that is, the polymerization temperature, is 20°C or less. FIG. 1 is a graph in which the horizontal axis is the polymerization temperature and the vertical axis is the conductivity of the solid electrolyte layer. As shown in FIG. 1, when the liquid temperature during polymerization is in the range of 20°C or less, the conductivity of the solid electrolyte layer is the best. On the other hand, when the liquid temperature during polymerization is 30°C or more, the crystallinity of Et-PEDOT doped with PSS decreases. When Et-PEDOT doped with PSS, which has a low crystallinity, is included in the solid electrolyte layer, the voltage resistance of the solid electrolytic capacitor is improved. Therefore, in fields where high power is progressing, such as the power electronics field, the liquid temperature during polymerization is maintained at 30°C or more. Preferably, the liquid temperature during polymerization is maintained in the range of 30°C or more and 50°C or less.

[0028] When concentrating the conductive polymer dispersion, the pH of the conductive polymer dispersion after the polymerization reaction is adjusted to 3 or more and 6 or less. If the pH is 3 or more and 6 or less, even if the concentration of Et-PEDOT doped with PSS is increased, it is difficult for it to aggregate in the conductive polymer dispersion. In this pH adjustment step, for example, an aqueous ammonia solution may be dropped into the conductive polymer dispersion. The concentration step is, for example, ultrafiltration, in which the conductive polymer dispersion is passed through a semipermeable membrane by pressure or the like.

[0029] (Solid electrolytic capacitor) A solid electrolytic capacitor is a passive element that stores and discharges electric charge by electrostatic capacitance. In this solid electrolytic capacitor, an anode body and a cathode body on which a dielectric film is formed face each other, and a solid electrolyte layer is interposed between the anode body and the cathode body. The solid electrolytic capacitor may include an electrolytic solution in addition to the solid electrolyte layer. A separator may be inserted between the anode body and the cathode body to prevent short circuits between the anode body and the cathode body and to maintain the solid electrolyte layer.

[0030] The solid electrolyte layer includes a conductive polymer in a conductive polymer dispersion. The conductive polymer is attached between the anode body and the cathode body by immersing each of the anode body, the cathode body, and the separator in the conductive polymer dispersion and drying them. Alternatively, the conductive polymer may be attached by producing a capacitor element by winding or stacking the anode body and the cathode body with the separator interposed therebetween, and then immersing the capacitor element in the conductive polymer dispersion and drying it. In addition to immersion, the conductive polymer dispersion may be applied by drop coating or spray coating. The drying step may be repeated multiple times, and drying may be performed under reduced pressure.

[0031] The anode and cathode bodies are alternately stacked with a separator sandwiched therebetween in a stacked arrangement. In the stacked arrangement, the capacitor elements may be flat-plate type without an exterior, or may be sealed by, for example, covering the capacitor elements with a laminate film, or by molding, dip-coating, or printing with a resin such as a heat-resistant resin or an insulating resin.

[0032] Alternatively, the anode body and the cathode body are wound in a wound arrangement in which they are alternately stacked with a separator sandwiched therebetween. In the wound arrangement, for example, the capacitor element is inserted into a cylindrical exterior case with a bottom, and the open end of the exterior case is sealed with a sealing body by crimping. The sealing body is made of, for example, rubber, or a laminate of rubber and a hard substrate. Examples of rubber include ethylene propylene rubber and butyl rubber.

[0033] The anode body and the cathode body are foil bodies made of valve metal. Valve metals include aluminum, tantalum, niobium, niobium oxide, titanium, hafnium, zirconium, zinc, tungsten, bismuth, and antimony. The purity of the anode foil is preferably 99.9% or more, and that of the cathode body is preferably 99% or more, but impurities such as silicon, iron, copper, magnesium, and zinc may be included. In addition, when the solid electrolytic capacitor is a flat type, a solid electrolyte layer may be formed on the anode body so as to cover the dielectric film, and then a metal paste such as silver paste may be printed and dried. This silver layer corresponds to the cathode of the solid electrolytic capacitor.

[0034] The anode body has a porous structure on the surface as a sintered body obtained by sintering a valve metal powder or an etched foil obtained by etching a stretched foil. The porous structure is composed of tunnel-like pits, spongy pits, or voids between densely packed powder particles. The porous structure is typically formed by direct current etching or alternating current etching in an acidic aqueous solution containing halogen ions such as hydrochloric acid, or by vapor deposition or sintering metal particles or the like on the core. The cathode body may also have a porous structure on the surface as necessary.

[0035] The dielectric film is the dielectric layer of a solid electrolytic capacitor, and is typically an oxide film formed on the surface of an anode body. If the anode body is an aluminum foil, the dielectric film is an aluminum oxide layer obtained by oxidizing the porous structure region. This dielectric film is formed by applying a voltage in a solution that does not contain halogen ions, such as an aqueous solution of adipic acid or boric acid. The cathode body may also be formed with a dielectric film as necessary, and may further include a layer of metal nitride, metal carbide, or metal carbonitride formed by vapor deposition, or one containing carbon on the surface.

[0036] Examples of the separator include cellulose papers such as kraft, Manila hemp, esparto, hemp, and rayon, and mixed papers thereof; polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and derivatives thereof; polytetrafluoroethylene-based resins, polyvinylidene fluoride-based resins, vinylon-based resins, polyamide-based resins such as aliphatic polyamides, semi-aromatic polyamides, and fully aromatic polyamides; polyimide-based resins, polyethylene resins, polypropylene resins, trimethylpentene resins, polyphenylene sulfide resins, acrylic resins, and polyvinyl alcohol resins. These resins can be used alone or in combination.

[0037] The solvent of the electrolyte is not particularly limited, but a protonic organic polar solvent or an aprotic organic polar solvent can be used. As the protonic polar solvent, monohydric alcohols, polyhydric alcohols, oxyalcohol compounds, etc. are typified, such as ethylene glycol or propylene glycol. As the aprotic polar solvent, sulfones, amides, lactones, cyclic amides, nitriles, sulfoxides, etc. are typified, such as sulfolane, γ-butyrolactone, ethylene carbonate, or propylene carbonate.

[0038] The solute contained in the electrolytic solution includes anion and cation components, and is typically an organic acid such as adipic acid or benzoic acid or its salt, an inorganic acid such as boric acid or phosphoric acid or its salt, or a complex compound of an organic acid such as borodisalicylic acid and an inorganic acid or its ion-dissociable salt, and is used alone or in combination of two or more. Examples of the salts of these organic acids, salts of inorganic acids, and at least one salt of a complex compound of an organic acid and an inorganic acid include ammonium salts, quaternary ammonium salts, quaternary amidinium salts, amine salts, sodium salts, potassium salts, etc. An acid that becomes an anion and a base that becomes a cation may be added separately to the electrolytic solution as solute components. EXAMPLES

[0039] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0040] (Examples 1 to 3) Each conductive polymer dispersion was prepared by the manufacturing methods of Examples 1 to 3 and Comparative Examples 1 to 3. The manufacturing methods of Examples 1 to 3 and Comparative Examples 1 to 3 have the following in common. First, 73.798 g of PSS, which is a dopant, was added to 879.619 mL of pure water. To this PSS aqueous solution, an oxidizing agent having the composition formula FeSO was added. 4 Add 18.775 g of ferrous sulfate, whose chemical formula is H 2 SO 4122.061 g of sulfuric acid was added.

[0041] The mixture was stirred with a stirrer and dissolved oxygen was removed by nitrogen bubbling. The mixture was then stirred with a homogenizer for 2 hours. 5.747 g of the monomer Et-EDOT was added to the mixture, and the mixture was homogenized and stirred with a stirrer for 30 minutes. The amount of PSS and Et-EDOT mixed was adjusted so that the molar ratio of PSS was twice that of Et-EDOT.

[0042] Next, an oxidizing agent with the molecular formula (NH 4 )S 2 O 8 The mixture was further mixed with an aqueous solution prepared by dissolving 15.408 g of ammonium peroxodisulfate represented by the following formula in 84.592 mL of pure water to initiate polymerization.

[0043] During the polymerization, the mixed liquid was maintained at each polymerization temperature corresponding to Examples 1 to 3 and Comparative Examples 1 to 3. The polymerization temperature in Comparative Example 1 was 0°C, the polymerization temperature in Comparative Example 2 was 10°C, and the polymerization temperature in Comparative Example 3 was 20°C. The polymerization temperature in Example 1 was 30°C, the polymerization temperature in Example 2 was 40°C, and the polymerization temperature in Example 3 was 50°C. The polymerization time was 24 hours, and homogenizer treatment and stirring with a stirrer were continued during the polymerization.

[0044] After 24 hours, ion exchange resin was added to the mixture and stirred for another 24 hours. The ion exchange resin was then removed from the mixture and ultrafiltered to remove the remaining monomer, dopant, and oxidant. After ion exchange and ultrafiltering, the conductive polymer was refined using a high-pressure homogenizer. Thus, the conductive polymer dispersions of Examples 1 to 3 and Comparative Examples 1 to 3 were prepared.

[0045] (Voltage Test) Solid electrolytic capacitors were produced using the conductive polymer dispersions of Examples 1 to 3 and Comparative Examples 1 to 3. The conductive polymer dispersions of Examples 1 to 3 and Comparative Examples 1 to 3 were adjusted to pH 4 by adding ammonia. Furthermore, these conductive polymer dispersions were added with 10 wt % ethylene glycol relative to the conductive polymer dispersion, and 85 wt % sorbitol relative to the solid content, i.e., the total weight of the conductive polymer and sorbitol.

[0046] The anode body is an aluminum foil with a purity of 99.99%. The surface of this aluminum foil was enlarged by DC etching. A dielectric film of aluminum oxide was formed on the enlarged aluminum foil by chemical conversion treatment. In the chemical conversion treatment, the anode was immersed in an aqueous boric acid solution and a voltage was applied while a constant current was passed through it. The voltage was applied until the chemical conversion voltage reached 946V.

[0047] An insulating resist layer was printed on the anode body except for the region to be the anode, and the anode body was dried. After printing the insulating resist layer, the anode body was immersed in the conductive polymer dispersion liquid of Examples 1 to 3 and Comparative Examples 1 to 3, and the conductive polymer was attached to the dielectric film. After the anode body was pulled out of the conductive polymer dispersion liquid, the anode body was left to stand for 10 minutes in a temperature environment of 60°C, and further left to stand for 30 minutes in a temperature environment of 110°C. In this way, the anode body was dried, and a solid electrolyte layer of the conductive polymer was formed on the anode body.

[0048] After the solid electrolyte layer was formed, carbon paste was applied onto the solid electrolyte layer and allowed to harden by leaving it in a 110°C environment for 30 minutes. Furthermore, silver paste was applied onto the carbon layer and copper foil was attached as a lead terminal at the same time. The silver paste was allowed to harden by leaving it in a 110°C environment for 30 minutes with the copper foil attached to the silver paste before hardening. The above carbon layer, silver layer, and copper foil layer correspond to the cathode body of the solid electrolytic capacitor.

[0049] The withstand voltage of these solid electrolytic capacitors was measured. A high-voltage DC power supply (HV1.5K-02XP, manufactured by Takasago Manufacturing Co., Ltd.) was used for the withstand voltage measurement. The measurement was performed at room temperature, with the applied voltage increasing from 0V to 1V per second. The voltage when a current of 20mA flows through the solid electrolytic capacitor being measured was determined as the withstand voltage of the solid electrolytic capacitor.

[0050] Table 1 below shows the withstand voltage (V) and polymerization temperature (°C) of the solid electrolytic capacitors produced using the conductive polymer dispersions of Examples 1 to 3 and Comparative Examples 1 to 3. Based on Table 1 below, a graph was produced as shown in Figure 2, with the polymerization temperature on the horizontal axis and the withstand voltage of the solid electrolytic capacitor on the vertical axis. Six solid electrolytic capacitors were produced each time, and the withstand voltage values ​​in Table 1 below are the average values ​​of the six. (Table 1) TIFF2024167665000002.tif71161

[0051] 2, comparing the solid electrolytic capacitors produced using the conductive polymer dispersions of Comparative Examples 1 to 3, the withstand voltage of Comparative Example 1 was the highest, and the withstand voltage of Comparative Example 3 was the lowest. The conductive polymer dispersion of Comparative Example 1 was produced by setting the polymerization temperature at 0° C., and the conductive polymer dispersion of Comparative Example 3 was produced by setting the polymerization temperature at 20° C. Thus, it was confirmed that up to a polymerization temperature of 20° C., the withstand voltage tended to decrease as the polymerization temperature was increased.

[0052] On the other hand, the solid electrolytic capacitors produced using the conductive polymer dispersions of Examples 1 to 3 had a higher withstand voltage than Comparative Example 1. The conductive polymer dispersions of Examples 1 to 3 were produced by setting the polymerization temperature at 30°C or higher. That is, when the polymerization temperature was 20°C or lower, the withstand voltage decreased as the polymerization temperature increased, but when the polymerization temperature was 30°C or higher, the withstand voltage suddenly exceeded that when the polymerization temperature was 0°C. Moreover, it was confirmed that, within the range of polymerization temperatures of 50°C or lower, the withstand voltage improved as the polymerization temperature increased.

[0053] In this way, the process includes a polymerization step in which Et-EDOT is polymerized in a liquid containing PSS, and the liquid temperature during the polymerization step is kept at 30°C or higher, thereby improving the voltage resistance of the solid electrolytic capacitor.

Claims

1. The method includes a polymerization step of polymerizing 2-ethyl-3,4-ethylenedioxythiophene in a liquid in which polystyrene sulfonic acid is present, In the polymerization step, the liquid temperature during polymerization is 30° C. or higher. A method for producing a conductive polymer dispersion, comprising:

2. In the polymerization step, the liquid temperature during polymerization is 30° C. or higher and 50° C. or lower.

2. A method for producing the conductive polymer dispersion according to claim 1,

3. The method further comprises a step of adjusting the pH of the dispersion liquid obtained through the polymerization step and having the conductive polymer dispersed therein to a pH of 3 or more and 6 or less.

3. The method for producing the conductive polymer dispersion according to claim 1 or 2,

4. forming a solid electrolyte layer between an anode body and a cathode body using the conductive polymer dispersion obtained by the manufacturing method according to claim 1 or 2; A method for producing a solid electrolytic capacitor comprising the steps of:

Citation Information

Patent Citations

  • Solid electrolytic capacitor

    JP2011060980A

  • Electroconductive polymer-containing coating material for forming a transparent electroconductive pattern, transparent electroconductive pattern-formed object, and method for manufacturing the same