Coating and coated article
The solvent-based, two-component paint system with specific group compositions cures rapidly at room temperature, reducing CO2 and VOC emissions while maintaining good workability and appearance, addressing the limitations of traditional paints.
Patent Information
- Application Number
- JP2023083957
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-12-04
AI Technical Summary
Existing paints emit high levels of CO2 and VOCs, require high-temperature heating for curing, and have poor coating workability and appearance due to high viscosity at high solid content concentrations.
A solvent-based, two-component paint system comprising a paint composition with hydroxyl or amino groups, an isocyanate group-containing composition with an acyclic structure, and a solvent, allowing for room temperature curing and low viscosity, thereby reducing CO2 emissions and improving coating workability.
The paint cures quickly at room temperature, reduces VOC emissions, and maintains excellent coating workability even at high solid content concentrations, eliminating the need for heating and enhancing film appearance.
Smart Images

Figure 2024167705000001 
Figure 2024167705000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a solvent-based, two-component paint and to an object to which the paint is applied. [Background technology]
[0002] Paints applied to automobile bodies and industrial products are indispensable because they serve to decorate and improve the beauty of the substrate and to protect the substrate.
[0003] However, in the painting process, heating is required to dry the water and solvents contained in the paint and to accelerate the long-term curing reaction to shorten the process. This heating process consumes electrical energy, resulting in increased CO2 emissions. In response to this, there is a demand to reduce CO2 emissions in order to achieve carbon neutrality.
[0004] In addition, the solvents contained in paints are volatile organic compounds (VOCs). As VOC emissions are regulated in various countries around the world, paints with low VOC emissions are in demand.
[0005] Reductions in CO2 emissions can be achieved by using solvent-based paints that can be heated at low temperatures because they do not contain water, which requires high-temperature heating, and by curing at room temperature, which eliminates the need for heat treatment.
[0006] Reduction in VOC emissions is achieved by reducing the solvent content in paint. However, reducing the solvent content in the paint results in a higher solids concentration, which increases the viscosity of the paint. Furthermore, if the viscosity of the paint is high, this can lead to reduced workability during application and poor appearance of the coating film (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2004-66034 A Summary of the Invention [Problem to be solved by the invention]
[0008] As mentioned above, paints are required to not only reduce CO2 emissions and VOC emissions, but also to provide good application workability and good paint film appearance.
[0009] In order to solve the above problems, the present invention provides a coating material that can reduce CO2 emissions, reduce VOC emissions, and has excellent coating workability, and also provides an object to be coated with the coating material.
[0010] The above and other objects of the present invention and novel features of the present invention will become apparent from the description of this specification and the accompanying drawings. [Means for solving the problem]
[0011] The first paint of the present invention comprises a paint composition A having a hydroxyl group, a paint composition B having an isocyanate group and a non-cyclic structure, and a solvent.
[0012] The coating material of the second aspect of the present invention comprises a coating material composition A' having an amino group, a coating material composition B having an isocyanate group and a non-cyclic structure, and a solvent. Effect of the Invention
[0013] According to the configuration of the first paint of the present invention, it contains paint composition A having a hydroxyl group, paint composition B having an isocyanate group and a non-cyclic structure, and a solvent. This makes it possible to obtain a paint that cures in a short time at room temperature and has excellent application workability even with a high solid content concentration. By curing in a short time at room temperature, heating is unnecessary, making it possible to reduce CO2 emissions. In addition, the high solid content concentration makes it possible to reduce VOC emissions.
[0014] According to the configuration of the paint of the second aspect of the present invention, it contains a paint composition A' having an amino group, a paint composition B having an isocyanate group and a non-cyclic structure, and a solvent. This makes it possible to obtain a paint that cures in a short time at room temperature and has excellent application workability even with a high solid content concentration. By curing in a short time at room temperature, heating is unnecessary, making it possible to reduce CO2 emissions. In addition, the high solid content concentration makes it possible to reduce VOC emissions.
[0015] Problems, configurations and effects other than those described above will become apparent from the following description of the embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, the embodiments and examples of the present invention will be described with reference to text and drawings. However, the structures, materials, and other specific configurations shown in the present invention are not limited to the embodiments and examples described here, and can be appropriately combined or improved without changing the gist of the invention. Elements that are not directly related to the present invention are not shown.
[0017] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result have discovered a coating material that has excellent coating workability even when it has a high solids concentration. That is, a paint containing a paint composition A containing hydroxyl groups, a paint composition B having an isocyanate group and a non-cyclic structure, and a solvent, or a paint composition A' containing an amino group, a paint composition B having an isocyanate group and a non-cyclic structure, and a solvent.
[0018] The first paint of the present invention comprises a paint composition A having a hydroxyl group, a paint composition B having an isocyanate group and a non-cyclic structure, and a solvent.
[0019] The coating material of the second aspect of the present invention comprises a coating material composition A' having an amino group, a coating material composition B having an isocyanate group and a non-cyclic structure, and a solvent.
[0020] According to the configuration of the first paint of the present invention, it contains paint composition A having a hydroxyl group, paint composition B having an isocyanate group and a non-cyclic structure, and a solvent. This makes it possible to obtain a paint that cures in a short time at room temperature and has excellent application workability even with a high solid content concentration. By curing in a short time at room temperature, heating is unnecessary, making it possible to reduce CO2 emissions. In addition, the high solid content concentration makes it possible to reduce VOC emissions.
[0021] According to the configuration of the paint of the second aspect of the present invention, it contains a paint composition A' having an amino group, a paint composition B having an isocyanate group and a non-cyclic structure, and a solvent. This makes it possible to obtain a paint that cures in a short time at room temperature and has excellent application workability even with a high solid content concentration. By curing in a short time at room temperature, heating is unnecessary, making it possible to reduce CO2 emissions. In addition, the high solid content concentration makes it possible to reduce VOC emissions.
[0022] In the paint of the first aspect of the present invention, the OH value of the paint composition A may be 228 to 1830 mgKOH / g. This composition can achieve both a high solids concentration and a low viscosity. The high solids concentration makes it possible to reduce VOC emissions, while the low viscosity provides excellent application workability.
[0023] In the coating material of the first aspect of the present invention, coating material composition B may have three or more isocyanate groups in one molecule and a molecular weight of less than 700. This composition makes it possible to realize a paint that has low viscosity, is easy to apply, and hardens in a short time at room temperature. By hardening in a short time at room temperature, heating is not required, and CO2 emissions can be reduced.
[0024] In the above-mentioned first paint of the present invention, the OH value of paint composition A is 228 to 1830 mgKOH / g, and paint composition B has three or more isocyanate groups in one molecule, a molecular weight of less than 700, and a solids concentration of the paint is 70 wt% or more. This composition can achieve both a high solids concentration and a low viscosity. The high solids concentration makes it possible to reduce VOC emissions, while the low viscosity provides excellent application workability. Furthermore, in the case of this configuration, since the resin hardens in a short time at room temperature, heating is not required, and CO2 emissions can be reduced.
[0025] The paint of the first aspect of the present invention may contain a pigment. In this configuration, the pigment can be used to provide color and hide the base.
[0026] In the coating material of the first aspect of the present invention, the solvent may be one or more of ester-based, ketone-based, and glycol ether-based solvents.
[0027] In the paint of the second aspect of the present invention, the amine value of paint composition A' may be 190 to 326 mgKOH / g. In the case of this configuration, the resin hardens in a short time at room temperature, eliminating the need for heating, and reducing CO2 emissions.
[0028] In the paint of the second aspect of the present invention, the paint composition B may have three or more isocyanate groups in one molecule and a molecular weight of less than 700. This composition makes it possible to realize a paint that has low viscosity, is easy to apply, and hardens in a short time at room temperature. By hardening in a short time at room temperature, heating is not required, and CO2 emissions can be reduced.
[0029] In the above-mentioned second paint of the present invention, the amine value of paint composition A' is 190 to 326 mgKOH / g, and paint composition B has three or more isocyanate groups in one molecule, a molecular weight of less than 700, and a solids concentration of the paint is 70 wt % or more. This composition can achieve both a high solids concentration and a low viscosity. The high solids concentration makes it possible to reduce VOC emissions, while the low viscosity provides excellent application workability. Furthermore, in the case of this configuration, since the resin hardens in a short time at room temperature, heating is not required, and CO2 emissions can be reduced.
[0030] The paint of the second aspect of the present invention may contain a pigment. In this configuration, the pigment can be used to provide color and hide the base.
[0031] In the coating material of the second aspect of the present invention, the solvent may be one or more of ester-based, ketone-based, and glycol ether-based solvents.
[0032] The paint of the present invention contains a paint composition A having a hydroxyl group or a paint composition A' having an amino group, a paint composition B having an isocyanate group and a non-cyclic structure, and a solvent. The paint of the present invention may contain various additives, if necessary, in addition to the components of paint composition A or paint composition A', paint composition B, and the solvent.
[0033] (Hydroxyl-containing coating composition A) For the coating composition A having a hydroxyl group, various substances having a hydroxyl group (-OH) can be used. For example, there may be mentioned monohydric alcohols such as polytetramethylene ether glycol, dihydric alcohols such as polycarbonate diol, 1,2-butanediol, ethylene glycol, and tetraethylene glycol, and trihydric alcohols such as glycerin.
[0034] As a result of the inventors' investigation, it was found that a substance having an OH value of 228mgKOH / g to 1830mgKOH / g is more preferable as the hydroxyl group-containing coating composition A. Here, the OH value is the number of milligrams of potassium hydroxide (KOH) required to neutralize the acetic acid bonded to the hydroxyl group when 1g of the substance having the hydroxyl group is acetylated under the following conditions. When the number of hydroxyl groups is n and the molecular weight is M, the OH value can be calculated using the formula: OH value = 56110 × n / M. The higher the ratio of OH groups in one molecule, the larger the OH value. Examples of substances having an OH value of 228 mgKOH / g to 1830 mgKOH / g include polytetramethylene ether glycol, polycarbonate diol, 1,2-butanediol, tetraethylene glycol, and glycerin.
[0035] If the OH value is below 228 mg KOH / g, attempting to increase the concentration of solids in the paint will result in an increase in viscosity, reducing application workability, while attempting to decrease the viscosity will result in a decrease in the concentration of solids in the paint, making it difficult to achieve both high solids and low viscosity.
[0036] When the OH value exceeds 1830 mgKOH / g, there is no chemical substance that can practically support the coating composition A, so 1830 mgKOH / g is the upper limit. The reason is that substances with two hydroxyl groups bonded to one carbon are known to be unstable, and methanediol, which has the smallest number of carbon atoms, cannot exist as a stable liquid because it decomposes into formaldehyde and water. Therefore, the polyhydric alcohols with the smallest molecular weight are ethylene glycol for dihydric alcohols and glycerin for trihydric alcohols. The OH value of each is 1810 mgKOH / g for ethylene glycol (molecular weight 62, number of OH groups 2) and 1830 mgKOH / g for glycerin (molecular weight 92, number of OH groups 3), so the maximum OH value is 1830 mgKOH / g.
[0037] For these reasons, in order to achieve both high solids and low viscosity, it is more preferable that the hydroxyl group-containing coating composition A has an OH value of 228 to 1830 mgKOH / g.
[0038] (Coating composition B having isocyanate groups) For the coating composition B having an isocyanate group, among substances having an isocyanate group, substances having a non-cyclic structure, that is, those not having a cyclic structure, can be used. When a substance having a cyclic structure is used in paint composition B having an isocyanate group, the molecular weight is larger and the molecular structure is bulky compared to substances having a non-cyclic structure, which results in an increase in viscosity of the paint and a long time required for the paint to harden.
[0039] It is more preferable that the coating composition B having an isocyanate group has three or more isocyanate groups and a molecular weight of less than 700, in addition to being a non-cyclic structure.
[0040] When the number of isocyanate groups in coating composition B is 2 or less, the coating takes longer to harden compared to when the number of isocyanate groups in coating composition B is 3 or more. This is presumably because when the number of isocyanate groups is small, there are fewer opportunities for the isocyanate groups and hydroxyl groups to bond, and so hardening takes a longer time. When the molecular weight of coating composition B is 700 or more, the viscosity of the coating will be higher and it will take longer to cure the coating than when the molecular weight of coating composition B is less than 700.
[0041] In view of the above, in order to reduce the viscosity of the paint and shorten the curing time of the paint, it is more preferable that the paint composition B having isocyanate groups has a non-cyclic structure, further has three or more isocyanate groups, and has a molecular weight of less than 700.
[0042] (Additives) The paint of the present invention may contain various additives, if necessary, in addition to the respective components of paint composition A or paint composition A', paint composition B, and a solvent.
[0043] One of the additives added to paint is a pigment. Pigments can be classified into color pigments, extender pigments, anti-rust pigments, luster pigments, etc., based on their functions.
[0044] Coloring pigments are added to impart color or conceal the base material. Examples of coloring pigments that can be added include titanium oxide, zinc oxide, iron oxide, carbon black, and Colt Blue. The pigment is appropriately selected based on the color to be imparted. The extender pigment is added to impart hardness and adjust the specific gravity and viscosity. Examples of the extender pigment that can be added include silica, talc, kaolin, and calcium carbonate. The anti-rust pigment is added to suppress corrosion. Examples of the anti-rust pigment that can be used include aluminum phosphate, zinc phosphate, and zinc molybdate. The luster pigment is added to impart a sense of luster by light interference or light reflection. Examples of the luster pigment include aluminum flakes, titanium oxide-coated mica, and iron oxide-coated mica. In addition, there are pigments that have rust-preventing properties, such as molybdenum, lead suboxide, and basic lead chromate.
[0045] In addition, additives such as a thickener for adjusting the viscosity of the coating, a surface conditioner for improving the appearance of the coating film, and an ultraviolet absorber for improving the durability of the coating film may be added as appropriate.
[0046] The additives shown here are merely examples, and the present invention is not limited to these additives. Additives to be added can be appropriately selected depending on the desired coating film properties.
[0047] (solvent) Solvents are added to adjust the viscosity of the paint, adjust the curing time which varies depending on the curing temperature, and improve coating workability. As the solvent, ester-based, ketone-based, and glycol ether-based solvents having a chemical structure that does not react with an isocyanate group can be used. From the perspective of reducing the environmental impact, it is also desirable for the solvent to be non-compliant with the Pollutant Release and Transfer Register (PRTR) Law and non-compliant with the Hazardous Air Pollutants (HAPs) listed in the Air Pollution Control Law.
[0048] Examples of the solvent include butyl acetate, cyclohexanone, propylene glycol methyl ether, 3-methoxy-3-methylbutyl acetate, 3-methoxybutyl acetate, ethyl 3-ethoxypropionate, propylene glycol monomethyl ether propionate, and propylene glycol diacetate. These solvents may be used alone or in combination. The solvents shown here are merely examples, and the present invention is not limited to these solvents.
[0049] As a result of the above, a paint (urethane paint) is composed of paint composition A having a hydroxyl group, paint composition B having an isocyanate group, additives, and a solvent. Urethane paint has a short curing time of less than 6.0 hours at room temperature, and because it is a high-solid paint (solid content concentration of 70wt% or more), it also emits little VOC. In addition, because urethane paint has a low viscosity, it is possible to obtain paint that is easy to apply.
[0050] The molar ratio of hydroxyl groups in coating composition A to isocyanate groups in coating composition B is appropriately adjusted depending on the desired physical properties of the coating film, and may be 1.05 to 1.20, but is preferably 1.1.
[0051] Next, an embodiment in which a coating composition A' having an amino group is used in place of the coating composition A having a hydroxyl group will be described.
[0052] (Paint composition A' having amino groups) For the coating composition A' having an amino group, various substances having an amino group (-NH2) can be used. Examples of such compounds include polyaspartic acid esters, N-(β-aminoethyl)isopropanolamine, 1,3-bisaminomethylcyclohexane, N,N'-(2-methyl-1,5-pentanediyl)bis-,1,1',4,4'-tetraethyl ester, N,N'-(methylenedi-4,1-cyclohexanedyl)bisaspartic acid tetraethyl ester, and bis(4-(1,2-bis(ethoxycarbonyl)ethylamino)-3-methylcyclohexyl)methane.
[0053] As a result of the inventors' investigations, it was found that a substance having an amine value of 190 mgKOH / g to 326 mgKOH / g is more preferable as the coating composition A' having an amino group. An example of a substance having an amine value of 190 mgKOH / g to 326 mgKOH / g is polyaspartic acid ester.
[0054] If the amine value is below 190 mg KOH / g, the coating will take a long time to cure. If the amine value is greater than 326 mg KOH / g, the coating will take a longer time to cure. From the above, in order for the coating material to harden in a short time, it is more preferable that the amine value of the coating material composition A' having an amino group is 190 mgKOH / g to 326 mgKOH / g.
[0055] A paint (urea paint) can be formed by the paint composition A' having an amino group, the paint composition B having an isocyanate group, an additive, and a solvent. In addition, in the paint containing the paint composition A' having an amino group, the additives and solvents that can be used are the same as those used in the paint containing the paint composition A having a hydroxyl group.
[0056] Each of the coating composition A and the coating composition A' may be used alone or in combination of two or more kinds.
[0057] It is preferable that Coating Composition A and Coating Composition A' have an aliphatic chemical structure in order to suppress yellowing, but they may contain aromatic compounds depending on the desired properties of the coating film. EXAMPLES
[0058] Specific examples of the paint will be described below. In each of the examples and comparative examples described below, the ratio of isocyanate groups to OH groups is set to 1.1.
[0059] (Paint film test) Further, for the paints prepared in each of the Examples and Comparative Examples, a coating test was carried out under test conditions in accordance with JIS K 5600 to examine the properties of the coating.
[0060] [Curing time at room temperature] The time taken for coating composition A or a coating material obtained by mixing coating composition A, coating composition B, additives, and a solvent to harden at room temperature was measured.
[0061] [Adhesion] The adhesion of the coating was examined according to the method specified in JIS K 5600 Part 5, Section 6 "Adhesion (Cross-cut Method)". If the adhesion result was classified as Class 0, it was marked with a circle.
[0062] [Scratch hardness] The scratch hardness of the coating film was examined according to the method specified in JIS K 5600 Part 5, Section 4, "Scratch hardness (pencil method)." Coatings with a scratch hardness of H or higher were marked with an O.
[0063] [Salt spray resistance] The salt spray resistance of the coating was investigated according to the method specified in JIS K 5600 Part 7, Section 1 "Neutral salt spray resistance". Tests were conducted with and without scratches, and a mark of "O" was given to the coating surface that showed no abnormalities after 720 hours of immersion for the without scratches, and to the coating surface that showed no rust and only slight deterioration after 240 hours for the with scratches.
[0064] [Resistance to repeated heat and humidity] The resistance of the coating to repeated exposure to heat and humidity was examined according to the method specified in JIS K 5600, Part 7, Section 4, "Resistance to repeated exposure to heat and humidity." Cases where no abnormalities were observed after 10 cycles were marked with an O.
[0065] Example 1 Coating composition A used polycarbonate diol with a solid content of 100 wt% and an OH value of 228 mgKOH / g. Coating composition B used polyisocyanate (coating composition B1) with a solid content of 75 wt%, a non-cyclic chemical structure, three isocyanate groups, and a molecular weight of 476. 1.0 g of coating composition A, 1.2 g of coating composition B1, and 0.5 g of butyl acetate as a solvent were each used and mixed. The resulting coating had a solids concentration of 72 wt% and a viscosity of 100 mPa·s. The curing time of the coating at room temperature was 2.5 h.
[0066] Example 2 1,2-butanediol with a solid content of 100 wt% and an OH value of 1245 mgKOH / g was used for the coating composition A. The coating composition B1 was used for the coating composition B, as in Example 1. 1.0 g of coating composition A and 6.5 g of coating composition B1 (containing 1.6 g of ethyl acetate as a solvent) were used and mixed. The resulting coating had a solids concentration of 79 wt% and a viscosity of 74 mPa·s. The curing time of the coating at room temperature was 6.0 h.
[0067] Example 3 Polytetramethylene glycol having a solid content of 100 wt % and an OH value of 499 mgKOH / g was used for the coating composition A. The coating composition B1 was used for the coating composition B, as in Example 1. 1.0 g of coating composition A and 2.6 g of coating composition B1 (containing 0.6 g of ethyl acetate as a solvent) were used and mixed. The resulting coating had a solids concentration of 80 wt% and a viscosity of 99 mPa·s. The curing time of the coating at room temperature was 6.0 h.
[0068] Example 4 A polyhydric alcohol having a solid content of 85 wt% and an OH value of 1830 mgKOH / g was used for the coating composition A. The coating composition B1 was used for the coating composition B, as in Example 1. 1.0 g of coating composition A and 7.3 g of coating composition B1 (containing 2.0 g of ethyl acetate as a solvent) were used and mixed. The resulting coating had a solids concentration of 76 wt% and a viscosity of 120 mPa·s. The curing time of the coating at room temperature was 6.0 hours.
[0069] Example 5 A polyhydric alcohol having a solid content of 100 wt % and an OH value of 868 mgKOH / g was used for the coating composition A. The coating composition B1 was used for the coating composition B, as in Example 1. 1.0 g of coating composition A and 4.6 g of coating composition B1 (containing 1.2 g of ethyl acetate as a solvent) were used and mixed. The resulting coating had a solids concentration of 80 wt% and a viscosity of 98 mPa·s. The curing time of the coating at room temperature was 6.0 h.
[0070] Comparative Example 1 For the coating composition A, acrylic polyol 1 having a solid content of 69 wt % and an OH value of 117 mgKOH / g was used. For the coating composition B, the same coating composition B1 as in Example 1 was used. 1.0 g of coating composition A (acrylic polyol 1) and 0.6 g of coating composition B1 (containing 0.4 g of ethyl acetate as a solvent) were used and mixed. The resulting paint had a solids concentration of 72 wt% and a high viscosity of 600 mPa·s. The curing time of the coating at room temperature was 6.0 hours.
[0071] Comparative Example 2 The coating composition A used was acrylic polyol 2 having a solid content of 60 wt % and an OH value of 84 mgKOH / g. The coating composition B used was the same coating composition B1 as in Example 1. 1.0 g of coating composition A (acrylic polyol 2) and 0.4 g of coating composition B1 (containing 0.5 g of butyl acetate as a solvent) were used and mixed. The resulting paint had a solids concentration of 65 wt%, and was not a high-solid paint. The viscosity at this stage was 200 mPa·s, which was high. The curing time of the coating at room temperature was 6.0 hours.
[0072] Comparative Example 3 Coating composition A used polycarbonate diol as in Example 1. Coating composition B used polyisocyanate (coating composition B2) having a solids concentration of 75 wt%, an acyclic chemical structure, three isocyanate groups, and a molecular weight of 730. 1.0 g of coating composition A and 1.5 g of coating composition B2 (containing 0.4 g of ethyl acetate as a solvent) were used and mixed. The resulting paint had a solids concentration of 85 wt%. Its viscosity was 1000 mPa·s, which was high. The curing time of the coating at room temperature was long, at 144 hours.
[0073] Comparative Example 4 Coating composition A used polycarbonate diol as in Example 1. Coating composition B used polyisocyanate (coating composition B3) having a solids concentration of 100 wt%, a cyclic chemical structure, three isocyanate groups, and a molecular weight of 654. 1.0 g of coating composition A and 0.8 g of coating composition B3 were mixed. The resulting paint had a solids concentration of 100 wt%. Its viscosity was 530 mPa·s, which was high. The curing time of the coating at room temperature was long, at 144 hours.
[0074] Comparative Example 5 Coating composition A used polycarbonate diol as in Example 1. Coating composition B used polyisocyanate (coating composition B4) having a solids concentration of 100 wt%, an acyclic chemical structure, two isocyanate groups, and a molecular weight of 519. 1.0 g of coating composition A and 1.1 g of coating composition B4 were mixed. The resulting paint had a solids concentration of 100 wt%. Its viscosity was high at 120 mPa·s. The coating was still uncured after 168 hours at room temperature.
[0075] Example 6 For coating composition A', a diamine (coating composition A'1) having a solid content of 100 wt % and an amine value of 243 mg KOH / g was used. For coating composition B, coating composition B1 was used as in Example 1. 1.0 g of coating composition A'1 and 1.3 g of coating composition B1 (containing 0.3 g of ethyl acetate as a solvent) were used and mixed. The resulting coating had a solids concentration of 88 wt% and a viscosity of 100 mPa·s. The curing time of the coating at room temperature was 5 min.
[0076] Example 7 For coating composition A', a diamine (coating composition A'2) having a solid content of 90 wt % and an amine value of 190 mg KOH / g was used. For coating composition B, coating composition B1 was used as in Example 1. 1.0 g of coating composition A'2 and 1.0 g of coating composition B1 (containing 0.3 g of butyl acetate as a solvent) were used and mixed. The resulting coating had a solids concentration of 88 wt% and a viscosity of 100 mPa·s. The curing time of the coating at room temperature was 6.0 hours.
[0077] Example 8 For coating composition A', a diamine (coating composition A'3) having a solid content of 90 wt % and an amine value of 199 mg KOH / g was used. For coating composition B, coating composition B1 was used as in Example 1. 1.0 g of coating composition A'3 and 1.0 g of coating composition B1 (containing 0.1 g of butyl acetate as a solvent) were used and mixed. The resulting coating had a solids concentration of 87 wt% and a viscosity of 100 mPa·s. The curing time of the coating at room temperature was 1.0 h.
[0078] Example 9 For the coating composition A', a diamine (coating composition A'4) having a solid content of 90 wt % and an amine value of 326 mg KOH / g was used. For the coating composition B, the same coating composition B1 as in Example 1 was used. 1.0 g of coating composition A'4 and 1.7 g of coating composition B1 (containing 0.5 g of ethyl acetate as a solvent) were used and mixed. The resulting coating had a solids concentration of 81 wt% and a viscosity of 100 mPa·s. The curing time of the coating at room temperature was 6.0 hours.
[0079] Comparative Example 6 For the coating composition A', N-(β-aminoethyl)isopropanolamine, which is a diamine having a solid content of 100 wt% and an OH value of 100 mgKOH / g, was used. For the coating composition B, the same coating composition B1 as in Example 1 was used. 1.0 g of coating composition A' and 0.2 g of coating composition B1 (containing 0.1 g of butyl acetate as a solvent) were each used and mixed. The resulting paint had a solids concentration of 92 wt% and a viscosity of 90 mPa·s. However, the coating film remained fluid even after 168 hours at room temperature, and no hardened coating film was obtained.
[0080] Comparative Example 7 For the coating composition A', 1,3-bisaminomethylcyclohexane (1,3-BAC), an amine-containing substance with a solid content of 100 wt% and an OH value of 789 mgKOH / g, was used. For the coating composition B, the same coating composition B1 as in Example 1 was used. 1.0 g of coating composition A' and 4.1 g of coating composition B1 (containing 1.0 g of ethyl acetate as a solvent) were used and mixed. The resulting paint had a solids concentration of 80 wt%. The viscosity at this time was 80 mPa s. However, the coating film remained fluid even after 168 hours at room temperature, and no hardened coating film was obtained.
[0081] For Examples 1 to 5 and Comparative Examples 1 to 5, which used coating composition A having a hydroxyl group, the properties of each composition, the properties of the coating material, and the results of the coating film test are shown in Table 1. For Examples 6 to 9 and Comparative Examples 6 and 7, which used coating composition A' having an amino group, the properties of each composition, the properties of the coating material, and the results of the coating film test are shown in Table 2.
[0082] [Table 1]
[0083] [Table 2]
[0084] As can be seen from Table 1, in all of Examples 1 to 5, the solids concentration of the paint after mixing was greater than 70 wt%, and the viscosity of the paint was 120 mPa·s or less, achieving both high solids and low viscosity. The OH value of the coating composition A in Examples 1 to 5 is 228 to 1830 mgKOH / g. The curing time of the coating film at room temperature was short, at 2.5 hours for Example 1 and 6.0 hours for Examples 2 to 5.
[0085] The OH value of the acrylic polyol 1 in the coating composition A of Comparative Example 1 was 117 mgKOH / g, which was lower than 228 mgKOH / g. In Comparative Example 1, the solids concentration of the coating after mixing was 72 wt%, and the viscosity of the coating was 600 mPa s, so that high solids and low viscosity could not be achieved at the same time. The OH value of the acrylic polyol 2 in the coating composition A of Comparative Example 2 was 84 mgKOH / g, which is less than 228 mgKOH / g. In Comparative Example 2, the solids concentration of the coating after mixing was 65 wt%, and the viscosity of the coating was 200 mPa s, so that high solids and low viscosity could not be achieved at the same time. The results of Examples 1 to 5 and Comparative Examples 1 and 2 show that coating composition A having an OH value of 228 to 1830 mgKOH / g can achieve both high solids and low viscosity.
[0086] In Examples 1 to 5, the molecular weight of the polyisocyanate in coating composition B (coating composition B1) was 476. The polyisocyanate of coating composition B in Comparative Example 3 (coating composition B2) had a large molecular weight of 730. In Comparative Example 3, the coating had a high viscosity of 1000 mPa·s and a long curing time at room temperature of 144 hours. From the results of Examples 1 to 5 and Comparative Example 3, it is clear that the smaller the molecular weight of the coating composition B, the more preferable it is.
[0087] In Examples 1 to 5, the chemical structure of the polyisocyanate in Coating Composition B (Coating Composition B1) was a non-cyclic structure. The polyisocyanate of coating composition B in Comparative Example 4 (coating composition B3) had a cyclic chemical structure. In Comparative Example 4, the coating had a high viscosity of 530 mPa s and a long curing time of 144 hours at room temperature. From the results of Examples 1 to 5 and Comparative Example 4, it is preferable that the chemical structure of coating composition B is a non-cyclic structure.
[0088] In Examples 1 to 5, the polyisocyanate of coating composition B (coating composition B1) had three isocyanate groups. The polyisocyanate of coating composition B in Comparative Example 5 (coating composition B4) had two isocyanate groups. Comparative Example 5 retained fluidity even after 168 hours at room temperature and did not harden into a coating film. From the results of Examples 1 to 5 and Comparative Example 5, it is preferable that coating composition B has three or more isocyanate groups.
[0089] As can be seen from Table 2, in all of Examples 6 to 9, the solids concentration of the paint after mixing was >70 wt%, and the viscosity of the paint was 100 mPa·s, achieving both high solids and low viscosity. The amine value of the coating compositions A' of Examples 6 to 9 is 190 to 326 mgKOH / g. The curing time of the coating film at room temperature was short, at 5 minutes for Example 6, 6.0 hours for Examples 7 and 9, and 1.0 hour for Example 8.
[0090] The N-(β-aminoethyl)isopropanolamine in the coating composition A' of Comparative Example 6 had an amine value of 100 mgKOH / g, which was less than 190 mgKOH / g. Furthermore, the coating composition of Comparative Example 6 had fluidity even after 168 hours at room temperature and did not harden into a coating film. The amine value of 1,3-bisaminomethylcyclohexane in the coating composition A' of Comparative Example 7 was 789 mgKOH / g, exceeding 326 mgKOH / g. Furthermore, the coating composition of Comparative Example 7 had fluidity even after 168 hours at room temperature and did not harden into a coating film. From the results of Examples 6 to 9 and Comparative Examples 6 and 7, it is apparent that the amine value of coating composition A' is preferably 190 to 326 mgKOH / g.
[0091] In Examples 1 to 9, the same coating composition B1 was used as the coating composition B. Similarly to coating composition B1, even if another coating composition is used as coating composition B, which has an acyclic chemical structure, three or more isocyanate groups, and a molecular weight of less than 700, good coatings and coating films (substrates) can be obtained, similar to Examples 1 to 9.
[0092] The present invention is not limited to the above-described embodiments and examples, and includes various modified examples. For example, the above-described embodiments and examples have been described in detail to easily explain the present invention, and the present invention is not necessarily limited to those having all of the configurations described.
Claims
1. A coating composition A having a hydroxyl group; A coating composition B having an isocyanate group and a non-cyclic structure; Contains solvent paint.
2. A coating composition A' having an amino group; A coating composition B having an isocyanate group and a non-cyclic structure; Contains solvent paint.
3. The paint according to claim 1, wherein the OH value of the paint composition A is 228 to 1830 mg KOH / g.
4. 2. The paint according to claim 1, wherein said paint composition B has three or more isocyanate groups in one molecule and a molecular weight of less than 700.
5. The paint composition A has an OH value of 228 to 1830 mgKOH / g, and the paint composition B has three or more isocyanate groups in one molecule, a molecular weight of less than 700, and a solids concentration of 70 wt% or more.
6. 10. The coating of claim 1 comprising a pigment.
7. 2. The coating material according to claim 1, wherein the solvent is at least one of an ester type, a ketone type, and a glycol ether type.
8. The paint according to claim 2, wherein the amine value of said paint composition A' is 190 to 326 mg KOH / g.
9. 3. The paint according to claim 2, wherein said paint composition B has three or more isocyanate groups in one molecule and a molecular weight of less than 700.
10. The paint according to claim 2, wherein the amine value of the paint composition A' is 190 to 326 mgKOH / g, and the paint composition B has three or more isocyanate groups in one molecule, a molecular weight of less than 700, and a solids concentration of 70 wt % or more.
11. 3. The coating of claim 2 comprising a pigment.
12. 3. The coating material according to claim 2, wherein the solvent is at least one of an ester type, a ketone type, and a glycol ether type.
13. An object to be coated with the coating material according to claim 1 or 2.
Citation Information
Patent Citations
Method of forming multi-layer coating film and water-base coating composition
JP2004066034A