Laminate, bag body, and freestanding bag
A laminate of stretched porous film and paper base material with a partial adhesive layer addresses the rigidity and material usage issues of self-standing bags, offering a cost-effective and environmentally friendly solution with enhanced breathability and rigidity.
Patent Information
- Application Number
- JP2023084080
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-12-04
AI Technical Summary
Existing self-standing bags made from stretched porous films lack rigidity and are difficult to manufacture due to the use of petroleum-derived materials, and the application of water-based emulsion adhesives reduces air permeability, limiting the choice of nonwoven fabrics and increasing costs.
A laminate is developed using a stretched porous film layer and a paper base material, with a partial water-based emulsion adhesive layer, to enhance rigidity and reduce petroleum-derived raw material usage.
The laminate provides a self-supporting bag with excellent breathability and rigidity, suitable for dehumidifiers, while reducing petroleum-derived materials and maintaining air permeability.
Smart Images

Figure 2024167771000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate of a stretched porous film and a paper substrate. [Background technology]
[0002] Stretched porous films, which are made by forming resins such as polyethylene resins into a film shape and forming fine holes in them, have a structure that allows air and other gases to pass through but not liquids, and are therefore used to package desiccants and dehumidifiers (for example, Patent Documents 1 and 2).
[0003] For example, Patent Document 1 discloses a laminate made by laminating a breathable film (stretched porous film), a non-breathable film, and a heat-sealable resin film (nonwoven fabric) as a film for covering the opening of a container containing a desiccant, etc. Contents such as a desiccant are placed in a container, the opening is covered with the laminate for storage, and when used, the non-breathable film of the laminate is peeled off, allowing the container to be used in a state in which the contents do not spill and moisture passes through the breathable film. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-315402 [Patent Document 2] JP 2016-68516 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, self-supporting bags called stand-up pouches have been increasingly used in various fields due to their excellent compressibility and flexibility. When manufacturing self-supporting bags as containers for desiccant, etc., it was thought that using a stretched porous film as the material would prevent the contents from spilling and allow moisture to pass through the breathable film. However, the rigidity of the stretched porous film alone was insufficient, making it difficult to manufacture self-supporting bags.
[0006] Therefore, in order to improve the rigidity, it has been considered to laminate the stretched porous film with another substrate (reinforcing material) that does not inhibit breathability, for example, with a nonwoven fabric as disclosed as a reinforcing layer in Patent Document 2. In laminating the stretched porous film and the nonwoven fabric, the use of an adhesive is essential to obtain sufficient laminate strength. As the adhesive, a water-based emulsion adhesive is often used for the purpose of maintaining the working environment during production and reducing the risk of fire. When using a water-based emulsion adhesive, if the adhesive is applied to the entire surface of the stretched porous film, the breathability is significantly reduced, so an adhesive layer is formed partially. From the viewpoint of adhesion when using this water-based emulsion adhesive, the nonwoven fabric that can be used is limited.
[0007] However, in recent years, there has been a strong demand for environmental friendliness, and it has become important to reduce the use of petroleum-derived raw materials in order to reduce CO2 emissions, etc. Both stretched porous films and nonwoven fabrics generally use petroleum-derived raw materials, and it is necessary to reduce these raw materials. When using stretched porous films and nonwoven fabrics in layers as described above, it is possible to make the nonwoven fabric thinner in order to reduce the amount of resin used, but this would result in insufficient rigidity and make it difficult to manufacture self-supporting bags. It is also possible to use plant-derived resins as raw materials for the nonwoven fabric, but this would result in a significant increase in costs.
[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a laminate of stretched porous films that can be used as a self-supporting bag at low cost while reducing the use of petroleum-derived raw materials. [Means for solving the problem]
[0009] In order to solve the above-mentioned problems, the present inventors conducted intensive research and discovered that by using a paper base material instead of a nonwoven fabric as a reinforcing material, a laminate of stretched porous films that can be used to manufacture self-supporting bags can be obtained, thereby completing the present invention.
[0010] That is, the present invention is a laminate having a stretched porous film layer and a paper substrate, and a water-based emulsion adhesive layer partially between the stretched porous film layer and the paper substrate. The paper substrate preferably has a fiber diameter of 8 to 80 μm. The laminate has a moisture permeability of 3000 g / m 2 It is preferable that the product of the initial elastic modulus and the thickness is 200 kN / m or more in at least one of the MD direction and the TD direction. Another embodiment of the present invention is a bag, particularly a self-supporting bag, at least a part of which is constituted by the laminate. Effect of the Invention
[0011] By using the laminate of the present invention, it is possible to provide a self-supporting bag having excellent breathability, which can be used as a container for a desiccant or the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention is a laminate having a stretched porous film layer and a paper substrate, and having a water-based emulsion adhesive layer partially between the stretched porous film layer and the paper substrate.
[0013] The stretched porous film layer is a layer made of a stretched porous film, which prevents the contents from spilling and allows the laminate to have breathability. Any known stretched porous film can be used without restriction. The stretched porous film can be produced by mixing a filler with a resin, forming the film, and stretching it to make it porous.
[0014] The resin constituting the stretched porous film is not particularly limited, but for example, polyolefin can be used. The polyolefin includes those mainly composed of olefin polymers and copolymers such as ethylene, propylene, butene, etc., such as high density polyethylene, linear low density polyethylene, low density polyethylene, polypropylene, ethylene-propylene random copolymers or block copolymers, ethylene-vinyl acetate copolymers, and mixtures thereof. Among them, it is preferable to mix two or more types of polyethylene selected from high density polyethylene, linear low density polyethylene, and low density polyethylene. The density of the entire resin is 0.910 to 0.940 g / m 2 It is preferable that the melt index of the entire resin is 0.5 to 5.0 g / 10 min. When the density and melt index of the resin are within the above ranges, it is easy to obtain a stretched porous film having good breathability, mechanical properties, and excellent stretching uniformity.
[0015] The filler contained in the stretched porous film may be either an inorganic filler or an organic filler, and two or more of these may be mixed and used.
[0016] As the inorganic filler, any known filler can be used without limitation, for example, inorganic salts such as calcium carbonate, barium sulfate, calcium sulfate, barium carbonate, magnesium hydroxide, and aluminum hydroxide, inorganic oxides such as zinc oxide, magnesium oxide, and silica, silicates such as mica, vermiculite, and talc, and organic metal salts. Among the inorganic fillers, calcium carbonate is preferred from the viewpoint of cost performance and dissociation with polyolefin resin. As the organic filler, cellulose-based powders such as wood flour and pulp powder can be used.
[0017] The amount of the filler is preferably 80 parts by mass or more and 200 parts by mass or less, and more preferably 85 parts by mass or more and 160 parts by mass or less, relative to 100 parts by mass of the resin. If the filler is mixed in an amount of 80 parts by mass or more, the frequency of voids generated per unit area caused by separation of the resin and the filler can be increased. Therefore, adjacent voids are more likely to communicate with each other, and the breathability is improved. If the filler is mixed in an amount of 200 parts by mass or less, the film stretches well when stretched, and stretching is easy.
[0018] The average particle size of the filler, measured by a laser diffraction light scattering method, is preferably 10 μm or less, more preferably 0.5 to 5.0 μm, and even more preferably 0.7 to 3.0 μm. When the average particle size is within the above range, the filler has excellent dispersibility, facilitates the formation of continuous pores during stretching, and is less susceptible to film breakage during molding, making it possible to efficiently produce a stretched porous film. If the average particle size of the filler is larger than the above range, it is likely to cause pinholes, and if it is smaller, it is likely to cause draw resonance during film formation.
[0019] The filler is preferably surface-treated to improve dispersibility in resin. The surface treatment agent is preferably one that can hydrophobize the surface of the filler by coating it, and examples of the surface treatment agent include fatty acids, higher fatty acids, or metal salts thereof, as well as wax. The amount of the surface treatment agent is not particularly limited, but is preferably about 0.5 to 2.0% by mass relative to the filler, more preferably 1.5% by mass or less, and particularly preferably 1.0% by mass or less.
[0020] The stretched porous film may contain additives used in ordinary resin compositions, such as antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, neutralizing agents, lubricants, antifogging agents, antiblocking agents, antistatic agents, slip agents, colorants, plasticizers, etc.
[0021] The stretched porous film has a moisture permeability of 3000 g / m 2-24h or more is preferable, 3500g / m 2 It is more preferable that the moisture permeability is within the above range, which makes it easy to obtain a container for a desiccant or the like having sufficient breathability. The upper limit of the moisture permeability is not particularly limited, but due to the diffusion rate-limiting effect of water vapor movement, it is usually 6000 g / m 2 Less than 24 hours.
[0022] The stretched porous film has a basis weight of 10 to 100 g / m 2 It is preferable that the thickness is 40 to 60 g / m 2 When the basis weight is within the above range, it becomes easy to make the physical properties of the laminate suitable for a self-supporting bag.
[0023] The stretched porous film preferably has a thickness of 10 to 100 μm, more preferably 40 to 60 μm. When the thickness is within the above range, it becomes easy to make the physical properties of the laminate suitable for a self-supporting bag.
[0024] The method for producing the stretched porous film is not particularly limited, and a conventionally known method for producing a stretched porous film may be appropriately adopted, and the film formed from a resin composition containing a resin, a filler, and other additives may be stretched at least uniaxially. Specifically, the resin composition is formed into a film shape by a T-die method, an inflation method, or the like, and stretched at least uniaxially in-line or off-line, and if necessary, biaxially stretched and wound up to obtain a stretched porous film having small holes formed therein that allow gas to pass through but do not allow liquid to pass through. The conditions for film formation and stretching may be appropriately set based on conventionally known techniques.
[0025] The laminate of the present invention is characterized by having a paper substrate. This makes it possible to obtain a laminate of stretched porous films that can be used as a self-supporting bag at low cost while reducing the amount of petroleum-derived raw materials used. As described above, the stretched porous film alone does not have enough rigidity to be used as a self-supporting bag, but by using a paper substrate as a reinforcing material, it is possible to make it have sufficient rigidity. The paper substrate has high rigidity due to strong bonding between fibers, and has high affinity with aqueous emulsion adhesives due to the high hydrophilicity of the fibers, so it is presumed that the paper substrate can achieve both sufficient adhesion and rigidity.
[0026] The paper constituting the paper base layer is not particularly limited, and for example, fine paper, special fine paper, medium quality paper, coated paper, art paper, cast coated paper, Japanese paper, imitation paper, kraft paper, etc. can be used, but among them, kraft paper with excellent strength is particularly suitable. In order to make the most of the strength, kraft paper is often unbleached, which causes less damage to the cellulose fibers, but it can be used with or without bleaching, and it can be freely selected, such as using bleached paper when design is important, or using unbleached paper when the natural texture of the material is important. Regarding wood fibers, long fiber rich coniferous wood has excellent breaking strength, and hardwood rich wood has excellent elasticity, so it is sufficient to select according to the performance that is important.
[0027] The fiber diameter of the paper constituting the paper base material is preferably 8 to 80 μm, and more preferably 20 to 50 μm. By having the fiber diameter within this range, it becomes easy to achieve both adhesiveness and rigidity.
[0028] The weight of the paper base material is 30 to 150 g / m 2 It is preferable that the thickness is 50 to 100 g / m 2 It is more preferable that the basis weight is 30 g / m 2 By setting the value to 150 g / m or more, it is easy to ensure the strength of the laminate. 2 By satisfying this condition, curling and wrinkling can be easily suppressed, and further, good seal strength can be easily achieved when the laminate is made into a bag.
[0029] The initial elastic modulus of the paper substrate in the MD direction is preferably 1500 MPa or more, more preferably 2000 MPa or more. The initial elastic modulus of the paper substrate in the TD direction is preferably 1000 MPa or more, more preferably 1500 MPa or more. By having the initial elastic modulus above the above value, it is easy to impart rigidity to the laminate and make it usable as a self-supporting bag. The upper limit of the initial elastic modulus is not particularly limited, but is generally 6000 MPa or less in the MD direction and 3000 MPa or less in the TD direction.
[0030] The paper base material preferably has a thickness of 50 to 200 μm, more preferably 100 to 150 μm. By having the thickness within this range, it becomes easy to make the physical properties of the laminate suitable for a self-supporting bag.
[0031] The laminate of the present invention partially has an aqueous emulsion adhesive layer between the stretched porous film layer and the paper substrate, which means that the stretched porous film and the paper substrate are partially bonded by the aqueous emulsion adhesive.
[0032] Although acrylic adhesives and rubber adhesives are also known as adhesives for resins, compared to these solvent-based adhesives, water-based emulsion adhesives are superior in that they are environmentally friendly and have high work safety. As water-based emulsion adhesives, adhesives in which one or more types of resin such as vinyl acetate resin, ethylene-vinyl acetate resin, acrylic resin, and urethane resin are dispersed are known, but from the viewpoint of adhesion and processing stability, ethylene-vinyl acetate resin adhesives in which ethylene-vinyl acetate resin is the main resin component are preferred. These adhesives may contain a curing agent.
[0033] The term "partially having an aqueous emulsion adhesive layer" means that there is an area on the surface of the stretched porous film where the aqueous emulsion adhesive is not present to the extent that sufficient breathability is obtained in the laminate, since if the aqueous emulsion adhesive is applied to the entire surface of the stretched porous film, breathability cannot be obtained. The proportion of the aqueous emulsion adhesive layer on the surface of the stretched porous film is not particularly limited, and it is sufficient to control it to the extent that the laminate has sufficient laminate strength and breathability. For example, the proportion of the aqueous emulsion adhesive layer relative to the total area of the surface of the stretched porous film layer that is bonded to the paper substrate can be preferably 20 to 50%, more preferably 30 to 40%. By setting the proportion of the aqueous emulsion adhesive to be equal to or more than the lower limit, it becomes easy to increase the laminate strength of the laminate, and by setting it to be equal to or less than the upper limit, it becomes easy to increase the breathability of the laminate.
[0034] The laminate of the present invention has a moisture permeability of 3000 g / m 2 -24h or more is preferable, 3500g / m 2 It is more preferable that the moisture permeability is within the above range, which makes it easy to obtain a container for a desiccant or the like having sufficient breathability. The upper limit of the moisture permeability is not particularly limited, but due to the diffusion rate-limiting effect of water vapor movement, it is usually 6000 g / m 2 Less than 24 hours.
[0035] The moisture permeability of the laminate of the present invention depends on the moisture permeability of the stretched porous film and the coating area of the aqueous emulsion adhesive layer, since the moisture permeability of the paper substrate is generally higher than that of the stretched porous film. Therefore, in order to obtain an appropriate moisture permeability of the laminate of the present invention, it is sufficient to select a stretched porous film and adjust the proportion of the aqueous emulsion adhesive on the surface of the stretched porous film.
[0036] The laminate preferably has a product of initial elastic modulus and thickness of 200 kN / m or more in at least one of the MD and TD directions, more preferably 250 kN / m or more. The initial elastic modulus represents the rigidity of the material per cross-sectional area and is an index of resistance to deformation. If the initial elastic modulus of the laminate is high, the bag body made of the laminate is less likely to deform when it is erected, and is easier to stand on its own. However, as described above, since the initial elastic modulus is the rigidity of the material per cross-sectional area, the ease of standing on its own is also affected by the thickness of the laminate. Therefore, by increasing the product of the initial elastic modulus and thickness of the laminate, the rigidity of the laminate can be increased to make it easier to stand on its own. If the product of the initial elastic modulus and thickness of the laminate is too low, it is difficult to make the bag stand on its own, even if the bag is manufactured using the laminate. If the product of the initial elastic modulus and thickness is high in either the MD or TD direction, it is possible to manufacture a self-supporting bag by adjusting the direction of the laminate to manufacture the bag body. There is no particular upper limit to the product of the initial elastic modulus and thickness, but it is usually 500 kN / m or less in the MD direction and 300 kN / m or less in the TD direction.
[0037] The product of the initial elastic modulus and the thickness in the MD direction may be calculated by measuring the initial elastic modulus of the laminate in the MD direction and the thickness of the laminate, respectively.Similarly, the product of the initial elastic modulus and the thickness in the TD direction may be calculated by measuring the initial elastic modulus of the laminate in the TD direction and the thickness of the laminate, respectively.
[0038] The initial elastic modulus of the laminate is preferably 1000 MPa or more in either the MD direction or the TD direction, more preferably 1500 MPa or more, and even more preferably 1700 MPa or more. This makes it easy to adjust the physical properties to enable the production of a self-supporting bag. There is no particular upper limit to the initial elastic modulus, but it is usually 3000 MPa or less. In general, a paper substrate has a higher elastic modulus than a stretched porous film, so the initial elastic modulus of the laminate depends on the physical properties of the paper substrate.
[0039] The thickness of the laminate is preferably 100 to 250 μm, more preferably 150 to 200 μm. When the thickness of the laminate is within the above range, it is easy to obtain physical properties suitable for a self-supporting bag. The thickness of the laminate can be adjusted by the type of stretched porous film, the type of paper base material, the type and application amount of the aqueous emulsion adhesive, and the pressing conditions during the production of the laminate.
[0040] The laminate strength between the stretched porous film and the paper substrate in the laminate is preferably 1.5 N / 15 mm or more, more preferably 2.0 N / 15 mm or more. If the laminate strength is too low, laminate lifting is likely to occur, which can cause line trouble during bag making and deterioration of the product appearance.
[0041] The basis weight of the laminate is 80 to 200 g / m 2 It is preferable that the thickness is 100 to 150 g / m 2 It is more preferable that the weight per unit area of the laminate is within the above range, so that the laminate can have suitable physical properties as a self-supporting bag. Since the amount of the aqueous emulsion adhesive layer in the laminate is usually small, the weight per unit area of the laminate is approximately equal to the sum of the weight per unit area of the stretched porous film and the weight per unit area of the paper substrate.
[0042] The ratio of petroleum-derived raw materials in the laminate is preferably 50% or less, and more preferably 25% or less. The ratio of petroleum-derived raw materials is the mass ratio of petroleum-derived raw materials in all materials used in the laminate. In general, it is equivalent to the mass ratio of the resin component (excluding special resins such as plant-derived resins). In addition, the amount of petroleum-derived raw materials used in the laminate is 60 g / m 2 It is preferable that the thickness is less than 30 g / m 2 The amount of the petroleum-derived raw materials used can be calculated from the basis weight of the laminate and the proportion of the petroleum-derived raw materials.
[0043] The method for producing the laminate of the present invention is not particularly limited, but it can be easily produced, for example, by applying an aqueous emulsion adhesive to a part of the surface of a stretched porous film or a paper substrate using a gravure roll or the like, and then overlapping and pressing the other. The conditions such as the pressing time and temperature may be appropriately adjusted depending on the physical properties of the stretched porous film, the paper substrate, and the aqueous emulsion adhesive.
[0044] The use of the laminate of the present invention is not particularly limited, but a bag, particularly a self-supporting bag, made of the laminate of the present invention can be mentioned as a preferred use. As described above, the laminate of the present invention has excellent breathability, and is therefore suitable as a container for dehumidifiers and the like. In addition, the laminate of the present invention has excellent rigidity, and can be used as a self-supporting bag. Therefore, by using the self-supporting bag made of the laminate of the present invention as a container for dehumidifiers and the like, it becomes easy to store the dehumidifier in a container with excellent compressibility and flexibility, and to install it in a narrow space. In addition, the bag made of the laminate of the present invention can reduce the amount of petroleum-derived raw materials used compared to the case where a stretched porous film is laminated with a resin nonwoven fabric, or compared to conventionally used containers, and can be a more environmentally friendly container. EXAMPLES
[0045] The present invention will be described in more detail below based on examples, but the present invention is not limited to the following examples.
[0046] [Evaluation method] Each physical property value was measured by the following methods.
[0047] (1) Weight A sample of 10 cm x 10 cm was cut from the specimen and its mass was measured using a balance. The basis weight was calculated from the area and mass of this sample.
[0048] (2) Moisture permeability Ten samples measuring 10 cm x 10 cm were taken from the specimen. The moisture permeability of these samples was measured under the conditions of 40°C, relative humidity 60%, measurement time 24 hours, and pure water method in accordance with ASTM E96, and the average value was calculated.
[0049] (3) Laminate strength A test piece 15 mm wide and 150 mm long was cut from the laminate to prepare a test piece, and the peeled portion was pulled at a chuck distance of 50 mm and a pulling speed of 200 mm / min to measure the laminate strength.
[0050] (4) Initial elastic modulus In accordance with JIS K 7127, measurements were performed with a chuck distance of 50 mm and a test speed of 0.5 mm / min, and the initial elastic modulus was calculated from the slope of two points, 0.2% strain and 0.7% strain.
[0051] (5) Thickness of the laminate The thickness of the sample measured in measuring the initial elastic modulus was regarded as the thickness of the laminate.
[0052] (6) Fiber diameter The surfaces of the nonwoven fabric and paper were observed using an electron microscope, and the fiber diameters were measured. The fiber diameters of three fibers, thick, medium, and thin, were measured by visual estimation, and the average value was calculated.
[0053] (7) Independence test Two test pieces 100 mm wide (TD) and 300 mm long (MD) were cut from the laminate, and stacked with the stretched porous film surfaces facing each other, and the periphery was heat sealed to a width of 2 mm to create a 4-pack sealed test specimen. The lower 50 mm of this test specimen in the length direction was sandwiched and fixed between two iron blocks, and the upper 250 mm in the length direction was allowed to stand on its own. If it could stand on its own, it was evaluated as passing (◯), and if it fell over, it was evaluated as failing (×).
[0054] Examples 1 to 3 and Comparative Examples 1 to 4 are shown below. Table 1 shows the evaluation results of the constituent materials and the laminate.
[0055] Example 1 Stretched porous film (Tokuyama, product name: Poram PH-50, moisture permeability 5480g / m 2 The laminate was then dry laminated with a water-based emulsion adhesive, an ethylene-vinyl acetate resin adhesive (Saiden Chemical's product name: Saivinol PZ-905) to which a hardener (Sanden Chemical's product name: Saivinol E-106) had been added. The adhesive was applied in a checkered pattern using a gravure roll, with a coating area of 36%. The lamination was performed at a lamination roll temperature of 90°C and a line speed of 40 m / min, and the laminate was then aged at 80°C for one week. The obtained laminate had high laminate strength that did not peel off (the substrate would be destroyed) in the laminate strength measurement test, had a high product of initial elastic modulus and thickness, passed the self-supporting test, and had high moisture permeability. It was suitable as a substrate for self-supporting bags for desiccant, etc.
[0056] [Example 2] A laminate was produced in the same manner as in Example 1, except that the kraft paper reinforcing material was changed to a product name: unbleached light-weight packaging base paper (manufactured by Oji Materia). The obtained laminate had high laminate strength that did not peel off in the laminate strength measurement test, a high product of initial elastic modulus and thickness, passed the self-supporting test, and had high moisture permeability. It was suitable as a base material for self-supporting bags for desiccant, etc.
[0057] [Example 3] A laminate was produced in the same manner as in Example 1, except that the kraft paper reinforcing material was changed to a product named Kujira (manufactured by Oji Materia). The obtained laminate had a laminate strength that did not peel off in the laminate strength measurement test, a high product of initial elastic modulus and thickness, passed the self-supporting test, and had high moisture permeability. It was suitable as a base material for self-supporting bags for desiccant, etc.
[0058] [Comparative Example 1] A laminate was produced in the same manner as in Example 1, except that the kraft paper reinforcing material was changed to a nonwoven fabric (product name: Dila 0903WHO (manufactured by Unitika)). The obtained laminate passed the self-supporting test, but had low laminate strength and some lifting was observed in the finish. It was not suitable as a base material for self-supporting bags for desiccant, etc.
[0059] [Comparative Example 2] A laminate was produced in the same manner as in Example 1, except that the kraft paper reinforcing material was changed to a nonwoven fabric (product name: Marix 20451FLV (manufactured by Unitika)). The obtained laminate had high lamination strength, but failed the self-supporting test, and was therefore not suitable as a base material for self-supporting bags for desiccant or the like.
[0060] [Comparative Example 3] A laminate was produced in the same manner as in Example 1, except that the kraft paper reinforcing material was changed to a nonwoven fabric (product name: Eltas Flat EH5045C (manufactured by Asahi Kasei Eltas)). The obtained laminate had high lamination strength, but failed the self-supporting test, and was therefore not suitable as a base material for self-supporting bags for desiccant or the like.
[0061] [Comparative Example 4] A laminate was produced in the same manner as in Example 1, except that the kraft paper reinforcing material was changed to a nonwoven fabric (product name: Tyvek 1056D (manufactured by Asahi DuPont Flash Spun Products)). The obtained laminate had high lamination strength, but failed the self-supporting test, and was therefore not suitable as a base material for self-supporting bags for desiccant or the like.
[0062] [Table 1]
Claims
1. A laminate comprising a stretched porous film layer and a paper substrate, the laminate partially comprising an aqueous emulsion adhesive layer between the stretched porous film layer and the paper substrate.
2. The laminate according to claim 1, wherein the paper base material has a fiber diameter of 8 to 80 μm.
3. Moisture permeability is 3000g / m 2 A laminate according to claim 1, having a product of initial elastic modulus and thickness of 200 kN / m or more in at least one of the MD and TD directions for 24 h or more.
4. A bag, at least a part of which is made of the laminate according to any one of claims 1 to 3.
5. A self-supporting bag, at least a portion of which is made of the laminate according to any one of claims 1 to 3.
Citation Information
Patent Citations
Packaging method
JP1997315402A
Gas-permeable packaging material
JP2016068516A