METHOD FOR MANUFACTURING RFeB-BASED MAGNET AND ALLOY FOR GRAIN BOUNDARY DIFFUSION TREATMENT USED IN THE SAME

The described method for RFeB magnets, using a Cu alloy with controlled Cu content for grain boundary diffusion, improves coercive force and squareness ratio at elevated temperatures, addressing the stability issues in automotive applications.

JP2024167834APending Publication Date: 2024-12-04DAIDO STEEL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023084189
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04

AI Technical Summary

Technical Problem

Existing RFeB magnets face challenges in maintaining high coercive force and squareness ratio at elevated temperatures, particularly around 130°C, which is crucial for applications in automobile motors.

Method used

A method involving a base material preparation, deposit preparation, adhesion, and heating process using a Cu alloy with a specific Cu content (20-40% by mass) for grain boundary diffusion treatment, ensuring heavy rare earth elements like Dy, Tb, or Ho diffuse near the surface of RFeB magnets.

Benefits of technology

The method enhances coercive force and squareness ratio at high temperatures, stabilizing magnetic properties by reducing temperature-induced fluctuations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167834000001_ABST
    Figure 2024167834000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing an RFeB-based magnet, capable of achieving a higher coercive force and a higher rectangularity ratio at high temperatures than conventional methods.SOLUTION: A method according to the present invention for manufacturing an RFeB-based magnet includes: a substrate preparation step of preparing a substrate comprising a sintered compact of an RFeB-based alloy containing rare earth elements R, Fe, and B or a hot-plastic-processed body of the alloy; a deposit preparation step of preparing a deposit containing an RHdCu alloy, which consists of a diffusion target heavy rare earth element RHd, a mixture of one or more of Dy, Tb, and Ho, and Cu, with the Cu content of 20 mass% or more and 40 mass% or less; a deposition step of depositing the deposit on the surface of the substrate; and a heating step of heating the substrate to which the deposit is deposited to a predetermined temperature at which the diffusion target heavy rare earth element RHd diffuses into a grain boundary of the substrate.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an RFeB-based sintered magnet or an RFeB-based hot plastically processed magnet (collectively referred to as an "RFeB-based magnet") whose main constituent elements are rare earth elements (hereinafter referred to as "R"), iron (Fe) and boron (B), and to an alloy used in said method. Note that an RFeB-based sintered magnet is one in which RFeB-based raw material powder is oriented in a magnetic field and then sintered, while an RFeB-based hot plastically processed magnet is one in which the crystal axes of the crystal grains are aligned by hot pressing RFeB-based raw material powder and then hot plastically processing it. [Background technology]

[0002] RFeB magnets have the advantage that their various magnetic properties, such as residual magnetic flux density, are better than those of other permanent magnets. Early RFeB magnets had the disadvantage of having a relatively low coercive force, one of their magnetic properties, but it was later discovered that the coercive force could be improved by having one or more of Dy, Tb, and Ho (hereinafter, these three elements are collectively referred to as "heavy rare earth elements") present near the surface of the crystal grains of RFeB magnets.

[0003] Heavy rare earth elements have almost no adverse effect on magnetic properties other than coercivity as long as they are present near the surface of the crystal grains of RFeB magnets, but if they are present in large amounts inside the crystal grains, they have the drawback of reducing the residual magnetic flux density. For this reason, a method of manufacturing RFeB magnets called the grain boundary diffusion method has been used (for example, Patent Documents 1 and 2). In the grain boundary diffusion method, a base material made of a sintered body is produced by sintering raw material powder of RFeB magnets, and then an attachment made of an alloy containing a heavy rare earth element is attached to the surface of the base material and heated to a temperature within a predetermined temperature range (typically 700 to 1000°C). Then, the heavy rare earth element of the attachment diffuses into the sintered body through the grain boundaries of the crystal grains of the sintered body, which is the base material, and penetrates near the surface of the crystal grains, but hardly penetrates inside the crystal grains. This makes it possible to obtain an RFeB magnet with high coercivity and suppressed reduction in residual magnetic flux density, with the heavy rare earth element being sufficiently present near the surface of the crystal grains while being almost absent inside the crystal grains.

[0004] Patent Document 1 describes the use of a TbCu alloy containing 86 mass% Tb and 14 mass% Cu, which is an element other than heavy rare earth elements, as the deposit. Patent Document 2 describes the use of a TbCu alloy containing 85.4 mass% Tb and 14.6 mass% Cu as the deposit (note that Patent Document 2 describes the TbCu alloy as a comparative example with the use of a TbCuAl alloy containing Tb, Cu, and Al). Patent Document 1 describes Cu as having the role of suppressing the penetration of heavy rare earth elements into crystal grains, and Patent Document 2 describes Cu as having the role of blocking magnetic interaction between crystal grains by being present at grain boundaries. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-092121 A [Patent Document 2] JP 2020-013975 A [Patent Document 3] JP 2006-019521 A [Non-patent literature]

[0006] [Non-Patent Document 1] Keiko Heki and Atsushi Hattori, "Development of Dy-saving Nd-Fe-B hot-processed magnets using ultra-rapidly cooled powders", Sokeizai, Vol. 52, No. 8, pp. 19-24, Sokeizai Center, August 2011 Summary of the Invention [Problem to be solved by the invention]

[0007] It is generally known that the higher the temperature of a magnet, the smaller its coercive force and squareness ratio. Here, the squareness ratio is the reversal magnetic field H when the magnetization is 90% of the residual magnetic flux density in the second quadrant of the magnetization curve (demagnetization curve). k and coercive force H cj The ratio of H k / H cj This is a value expressed as: The larger the squareness ratio, the smaller the fluctuation in magnetization due to magnetic field fluctuations, meaning that the magnet has stable characteristics in a fluctuating magnetic field. Since the temperature of automobile traction motors rises to around 130°C during use, in order to use RFeB magnets in such motors, it is necessary to increase the coercive force and squareness ratio at high temperatures of around 130°C.

[0008] The problem that the present invention aims to solve is to provide a method for manufacturing an RFeB magnet that can achieve a higher coercive force and squareness ratio at high temperatures than conventional magnets. [Means for solving the problem]

[0009] The method for producing an RFeB magnet according to the present invention, which has been devised to solve the above problems, comprises the steps of: a substrate preparation step of preparing a substrate made of a sintered body of an RFeB-based alloy containing rare earth elements R, Fe, and B or a hot plastic worked body of the alloy; A heavy rare earth element R to be diffused is any one of Dy, Tb, and Ho (a heavy rare earth element), or a mixture of two or more of them. Hd and Cu, the Cu content being 20 mass% or more and 40 mass% or less. Hd a deposit preparation step of preparing a deposit containing a Cu alloy; an attachment step of attaching the attachment to a surface of the substrate; The base material to which the deposit is attached is treated with the heavy rare earth element R to be diffused. Hd a heating step of heating the substrate to a predetermined temperature at which the has.

[0010] R Hd Cu alloys are permitted to contain unavoidable impurities, but do not contain any other heavy rare earth elements R that are subject to diffusion. Hd Therefore, if the Cu content is determined (ignoring inevitable impurities), the diffusion target heavy rare earth element R Hd The content of is uniquely determined. For example, if the Cu content is 20 mass%, the diffusion target heavy rare earth element R Hd If the Cu content is 40 mass%, the heavy rare earth element R Hd The content is 60 mass %.

[0011] According to the experiment conducted by the inventor, the R contained in the deposit used in the grain boundary diffusion treatment Hd It was revealed that by increasing the Cu content in the Cu alloy to 20 mass%, which is higher than the 14 to 14.6 mass% described in Patent Documents 1 and 2, the coercive force and squareness ratio at 130°C of an RFeB magnet that has been subjected to grain boundary diffusion treatment are improved. Hd It has been revealed that when the Cu content in a Cu alloy is increased beyond 20 mass%, such large coercivity and squareness ratio can be obtained within the range of up to 40 mass%, but when the Cu content exceeds 40 mass%, the coercivity and squareness ratio decrease. Therefore, in the method for producing an RFeB magnet according to the present invention, a RFeB magnet having a Cu content of 20 mass% or more and 40 mass% or less is used. HdA grain boundary diffusion treatment is carried out using a deposit containing a Cu alloy.

[0012] In addition, according to an experiment conducted by the inventor, R Hd By setting the Cu content in the Cu alloy to 20 mass % or more and 40 mass % or less, it is possible to make the absolute values ​​of the temperature change rate α of the remanent magnetic flux density and the temperature change rate β of the coercive force at 130°C smaller than when the Cu content is less than 20 mass % or more than 40 mass %. Here, the temperature change rate α (or β) is a value that represents the slope of a graph with temperature on the horizontal axis and remanent magnetic flux density (or coercive force) on the vertical axis, and the smaller the absolute value, the smaller the change in remanent magnetic flux density (or coercive force) with temperature changes. In particular, the temperature change rate α of the remanent magnetic flux density is R Hd When the Cu content in the Cu alloy becomes less than 20 mass%, the temperature change rate β of the coercive force decreases significantly, and when the Cu content exceeds 40 mass%, the temperature change rate β of the coercive force decreases significantly. Therefore, by setting the Cu content to be between 20 mass% and 40 mass% inclusive, stable characteristics can be obtained in both the residual magnetic flux density and the coercive force.

[0013] In the present invention, the order of the substrate preparation step and the attachment preparation step does not matter. One of the substrate preparation step and the attachment preparation step may be performed first and the other may be performed later, or both steps may be performed simultaneously in parallel.

[0014] In the present invention, the form of the deposit is not particularly limited. For example, Hd The Cu alloy lump, foil, powder, etc. may be directly attached (contacted) to the surface of the substrate, or R Hd Alternatively, a Cu alloy powder may be dispersed in a dispersant such as liquid or grease to prepare an attachment, and then the dispersant may be attached to the surface of the substrate. Hd The higher the Cu content in the Cu alloy, the more difficult it becomes to pulverize the alloy ingot. If the Cu content exceeds 40 mass%, it becomes difficult to reduce the particle size (for example, to a median of 10 μm or less). However, in the present invention, the Cu content is set to 40 mass% or less, so that no problems with pulverization occur.

[0015] In the present invention, the base material preferably has a C (carbon) content of 0.10 mass% or less and an O (oxygen) content of 0.10 mass% or less. More preferably, these contents are both 0.05 mass% or less. By lowering the C and O contents in the base material in this way, C and O are less likely to be present in the grain boundaries of the base material, and therefore the heavy rare earth element R to be diffused during the heating step is more likely to be present in the grain boundaries of the base material. Hd The diffusion of the heavy rare earth element R through the grain boundaries into the base material is prevented by the presence of C and O. Hd Since this makes it easier for the magnetic material to reach the surfaces of the crystal grains in the substrate, the coercive force can be further improved.

[0016] The alloy for grain boundary diffusion treatment according to the present invention is a sintered body of an RFeB-based alloy containing rare earth elements R, Fe, and B, or a hot plastic processed body of said alloy, and is then heated to a predetermined temperature to form a diffusion target heavy rare earth element R, which is any one of Dy, Tb, and Ho, or a mixture of two or more of them. Hd An alloy used in a grain boundary diffusion treatment in which the alloy is diffused into the grain boundaries of the substrate, The heavy rare earth element R to be diffused Hd and Cu, the Cu content being 20 mass% or more and 40 mass% or less. Hd It is a Cu alloy. Effect of the Invention

[0017] By using the method for producing an RFeB magnet and the alloy for grain boundary diffusion treatment according to the present invention, it is possible to obtain an RFeB magnet that has a higher coercive force and squareness ratio at high temperatures than conventional magnets. [Brief description of the drawings]

[0018] [Figure 1] 1 is a graph showing the results of an experiment conducted at a temperature of 130° C., showing the relationship between the Cu content of the alloy for grain boundary diffusion treatment used in the RFeB-based magnet manufacturing methods of the present embodiment and the comparative example, and the residual magnetic flux density Br of the manufactured RFeB-based sintered magnet. [Diagram 2]1 is a graph showing the results of an experiment conducted at a temperature of 130° C., showing the relationship between the Cu content of the alloy for grain boundary diffusion treatment used in the RFeB-based magnet manufacturing methods of the present embodiment and the comparative example, and the coercive force Hcj of the manufactured RFeB-based sintered magnet. [Diagram 3] 1 is a graph showing the results of an experiment conducted at a temperature of 130° C., showing the relationship between the Cu content of the alloy for grain boundary diffusion treatment used in the RFeB-based magnet manufacturing methods of the present embodiment and the comparative example, and the squareness ratio SQ of the manufactured RFeB-based sintered magnet. [Figure 4] 1 is a graph showing the results of an experiment conducted at a temperature of 130° C., showing the relationship between the Cu content of the alloy for grain boundary diffusion treatment used in the RFeB-based magnet manufacturing methods of this embodiment and the comparative example, and the temperature change rate α of the remanence of the RFeB-based sintered magnet produced. [Diagram 5] 1 is a graph showing the results of an experiment conducted at a temperature of 130° C., showing the relationship between the Cu content of the alloy for grain boundary diffusion treatment used in the RFeB-based magnet manufacturing methods of this embodiment and the comparative example, and the temperature change rate β of the coercivity of the manufactured RFeB-based sintered magnet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] An embodiment of a method for producing an RFeB magnet and an alloy for grain boundary diffusion treatment according to the present invention will be described with reference to Figures 1 to 5. In the method for producing an RFeB magnet of this embodiment, the following steps are carried out: a substrate preparation step, an attachment preparation step, an attachment step, and a heating step. Either the substrate preparation step or the attachment preparation step may be carried out first, or both steps may be carried out simultaneously. The attachment step is carried out after the substrate preparation step and the attachment preparation step, and the heating step is carried out after the attachment step.

[0020] In the substrate preparation step, a substrate is prepared that is made of an RFeB-based sintered body or an RFeB-based hot plastically worked body that contains a rare earth element R (typically a light rare earth element Nd and / or Pr), Fe, and B. The RFeB-based sintered body may be prepared by a pressing method in which the raw material RFeB-based alloy powder is press-molded while being oriented by a magnetic field, and then sintered, or by a PLP (press-less process) method in which the RFeB-based alloy powder is oriented by a magnetic field in a mold without being press-molded, and then sintered as is, as described in Patent Document 3. The PLP method is preferable in that it can increase the coercive force and can produce an RFeB-based sintered magnet body with a complex shape without machining. The RFeB-based hot plastically worked magnet body can be produced by the method described in Non-Patent Document 1.

[0021] The composition ratio of R, Fe, and B is typically 2:14:1 in atomic ratio, but may deviate slightly from this ratio. In addition, elements other than R, Fe, and B may be added. For example, part of Fe may be replaced with Co and / or Ni, or additive elements such as Cu, Al, and Ga may be included. In addition, it is permissible to contain unavoidable impurities such as C, N, and O. The shape of the substrate is not particularly limited, and may be, for example, a rectangular parallelepiped, a shape obtained by curving a rectangular parallelepiped into an arch, or a shape obtained by changing one of the six faces of a rectangular parallelepiped into a convex arch-shaped curved surface.

[0022] In the deposit preparation step, the alloy for grain boundary diffusion treatment of this embodiment, R Hd A deposit containing a Cu alloy is prepared. Hd Cu alloy is a diffusion target heavy rare earth element R Hd and Cu, and except for unavoidable impurities, Hd Contains no elements other than Cu. Hd R contained in Cu alloy Hd R is a heavy rare earth element consisting of Dy, Tb and Ho. H It is one of the above, or a mixture of two or three of them. Hd R in Cu alloys HdThe content of R is in the range of 60 mass% to 80 mass%, and the remainder is Cu. Therefore, the content of Cu is 20 mass% to 40 mass%. Hd and Cu content R Hd By carrying out a grain boundary diffusion treatment using a deposit containing a Cu alloy as described below, it is possible to increase the coercive force and squareness ratio of an RFeB magnet at 130°C.

[0023] R contained in the deposit Hd The Cu alloy may be in the form of a block, foil, powder, etc. Hd When preparing Cu alloys, R Hd As the Cu content in the Cu alloy increases, it becomes more difficult to pulverize the alloy ingot. In this embodiment, however, by setting the Cu content to 40 mass% or less, it is possible to obtain powdered R having a small particle size (for example, 10 μm or less in the median). Hd Cu alloys can be easily produced. Hd The Cu alloy may be used as it is as an attachment, or may be dispersed in a dispersant such as liquid or grease. In the examples described later, powdered R Hd A Cu alloy is mixed with silicone grease.

[0024] In the adhesion step, the adhesion material prepared in the adhesion material preparation step is adhered to the surface of the substrate prepared in the substrate preparation step. When using a lump-shaped or foil-shaped adhesion material, it is brought into contact with the surface of the substrate. When using a powder-shaped adhesion material, it may be adhered to the surface of the substrate as is, but it is preferable to adhere the powder in a state dispersed in a dispersant as described above, since it is difficult to peel off from the substrate.

[0025] In the heating step, the substrate surface with the deposit attached thereto is heated to a predetermined temperature. The temperature during this heating is set to, for example, a temperature within a range of 600 to 1000° C. However, the predetermined temperature is not limited to this range, and the diffusion target heavy rare earth element R Hd It is sufficient that the temperature is such that the metal diffuses into the substrate through the grain boundaries of the substrate. EXAMPLES

[0026] Hereinafter, an example and a comparative example will be described in which an RFeB magnet was manufactured using the RFeB magnet manufacturing method of this embodiment and an alloy for grain boundary diffusion treatment. In these examples and comparative examples, a substrate was used in which an RFeB sintered body produced by the PLP method using an RFeB magnet powder having the same composition was cut into a rectangular parallelepiped of 24 mm x 15 mm x 9.4 mm. The composition of the RFeB sintered body is Nd: 25.0 mass%, Pr: 4.7 mass%, Co: 1.4 mass%, B: 0.98 mass%, Al: 0.2 mass%, Cu: 0.1 mass%, Ga: 0.2 mass%, Zr: 0.1 mass%, C: 0.04 mass%, O: 0.04 mass%, N: 0.03 mass%, Fe: balance (excluding unavoidable impurities, etc.). The rare earth elements contained in the RFeB magnet powder (and the RFeB sintered body and base material made from the powder) are only the above-mentioned Nd and Pr (total of 29.66 mass%), and no heavy rare earth elements are contained. Furthermore, this base material has low contents of C and O, both of which are 0.10 mass% or less, and even 0.05 mass% or less. As a result, by carrying out the grain boundary diffusion treatment described below using this base material, the heavy rare earth element R to be diffused can be reduced. Hd The diffusion of the heavy rare earth element R through the grain boundaries into the base material is prevented by the presence of C and O. Hd Since this makes it easier for the magnetic material to reach the surfaces of the crystal grains in the substrate, the coercive force can be further improved.

[0027] As the alloy for grain boundary diffusion treatment, in Examples 1 to 3, the diffusion target heavy rare earth element R Hd R is a material having a content of Tb and Cu within the range of this embodiment. HdA Cu (TbCu) alloy was prepared. In addition, as alloys for grain boundary diffusion treatment of comparative examples, TbCu alloys (Comparative Examples 1 and 2) having a lower Tb content than the present embodiment, TbCu alloys (Comparative Examples 3 and 4) having a higher Tb content than the present embodiment, an alloy containing only Tb (Comparative Example 5), a TbAl alloy containing only Tb and Al (containing no Cu) (Comparative Example 6), and a TbCuAl alloy containing Tb, Cu, and Al (Comparative Example 7) were prepared. The compositions of the alloys for grain boundary diffusion treatment of these examples and comparative examples are shown in Table 1. Table 1 also shows the pulverization efficiency (described later) for some alloys for grain boundary diffusion treatment. [Table 1]

[0028] All of the alloys for grain boundary diffusion treatment in the examples and comparative examples were manufactured as powdered alloys for grain boundary diffusion treatment by preparing alloy ingots by arc melting and then pulverizing them by the following method. First, the alloy ingot was heated to a temperature in the range of 400 to 500°C in a hydrogen atmosphere to allow hydrogen to be absorbed in the alloy ingot. By absorbing hydrogen in this way, the alloy ingot becomes embrittled. Next, the alloy ingot with absorbed hydrogen was heated to a temperature in the range of 400 to 500°C in a vacuum to release hydrogen from the alloy ingot. Thereafter, the alloy ingot was pulverized by a jet mill in a nitrogen atmosphere, and the particles pulverized to a predetermined particle size or less were collected to obtain a powder of the alloy for grain boundary diffusion treatment having a median particle size of about 10 μm.

[0029] The pulverization efficiency shown in Table 1 is expressed as a percentage by dividing the mass of the powder pulverized to a predetermined particle size or less by the jet mill and collected by the mass of the alloy ingot fed into the jet mill. The pulverization efficiency decreases as the Cu content increases, and is only 12.9% in Comparative Example 4 (Tb: 50 mass%, Cu: 50 mass%). However, in the present embodiment (Examples 1 to 3), the Cu content is 40 mass% or less, so the pulverization efficiency can be made higher than that of Comparative Example 4.

[0030] The powder of the alloy for grain boundary diffusion treatment in Examples 1 to 3 and Comparative Examples 1 to 3 and 5 to 7 obtained as described above was mixed with silicone grease to produce a deposit (note that for Comparative Example 4, which has a low crushing efficiency, no subsequent experiments were performed). This deposit was applied to two surfaces (24 mm x 15 mm surfaces) of a rectangular parallelepiped substrate. In all Examples and Comparative Examples, the amount of the deposit applied was adjusted so that the mass of Tb contained in the deposit was 0.8% of the mass of the substrate, including both surfaces.

[0031] Then, for each of the Examples and Comparative Examples 1 to 3 and 5 to 7, the base material with the attached material was heated to a temperature of 915°C and maintained for 30 hours to carry out a grain boundary diffusion treatment. After heating at 400 to 500°C for 30 minutes as an aging treatment, each of the two surfaces with the attached material was ground by 0.15 mm to form into a rectangular parallelepiped of 24 mm x 15 mm x 9.1 mm, and finally cut into a rectangular parallelepiped of 7 mm x 7 mm x 9.1 mm to obtain an RFeB-based sintered magnet.

[0032] For the RFeB based sintered magnets obtained in each of the Examples and Comparative Examples 1 to 3 and 5 to 7, various magnetic properties were measured at 130°C, which corresponds to the temperature during use of an automobile traction motor (note that for Comparative Example 7, measurements were performed on two RFeB based sintered magnets from different production lots). The measured magnetic properties were the residual magnetic flux density B r , coercive force H cj , squareness ratio SQ(=H k / H cj The temperature change rate of the residual magnetic flux density, α, and the temperature change rate of the coercive force, β, are shown in Table 2. The relationship between the Cu content of the alloy for grain boundary diffusion treatment used and each magnetic property is shown in Table 2 for the residual magnetic flux density, B r The coercive force H cjThe squareness ratio SQ is shown in Fig. 2, the rate of change in remanence α is shown in Fig. 4, and the rate of change in coercivity β is shown in Fig. 5. In each graph, Examples 1 to 3 are shown with black circles, and Comparative Examples 1 to 3 and 5 to 7 are shown with white symbols. Of the white symbols showing each comparative example, the circles indicate TbCu (however, the Cu content is less than 20 mass% or more than 40 mass%, which is outside the range of this embodiment), the equilateral triangles indicate Tb alone, the squares indicate TbAl, and the diamonds indicate TbCuAl, respectively, used as the alloy for grain boundary diffusion treatment. [Table 2]

[0033] From these experimental results, the residual magnetic flux density B r , coercive force H cj and the squareness ratio SQ is the coercive force H cj In all cases except for the squareness ratio SQ, the magnetic properties of Examples 1 to 3 were higher than those of Comparative Examples 1 to 3 and 5 to 7. cj is slightly larger than those of Examples 1 to 3, and the squareness ratio SQ is slightly larger than that of Example 1, but the residual magnetic flux density B r was smaller than those of Examples 1 to 3 (and also smaller than the other Comparative Examples). Thus, the RFeB based sintered magnets of Examples 1 to 3 have a residual magnetic flux density B r While suppressing the decrease in coercivity H cj and the squareness ratio SQ can be increased. Hd When the Cu content of the Cu alloy (TbCu alloy) is 20 to 30 mass % (Examples 1 and 2), the coercive force H cj On the other hand, R Hd When the Cu content of the Cu alloy (TbCu alloy) is set to 30 to 40 mass % (Examples 2 and 3), the coercive force H cj (While suppressing the decrease in residual magnetic flux density B r will become higher.

[0034] The temperature change rate α of the residual magnetic flux density at 130°C has a negative value in all of the examples and comparative examples. This is because the value of the residual magnetic flux density decreases as the temperature increases. The absolute value of the obtained α value is smaller in Examples 1 to 3 than in Comparative Examples 1 to 3 and 5 to 7. The fact that the absolute value of α is small indicates that when a temperature change occurs near 130°C, the residual magnetic flux density B r This means that the change in is small and stable. In the comparative examples, the absolute value of α is large in Comparative Examples 1, 2, and 5 to 7, in which the Cu content of the alloy for grain boundary diffusion treatment is less than 20 mass%, in particular, so that α can be significantly improved by making the Cu content 20 mass% or more.

[0035] The temperature coefficient of coercivity β at 130°C has a negative value in all Examples and Comparative Examples, similar to the case of α, indicating that the higher the temperature, the smaller the value of coercivity. The absolute value of β is smaller in Examples 1 to 3 than in Comparative Examples 1 to 3, 5, and 6. The smaller absolute value of β indicates that when a temperature change occurs near 130°C, the coercivity H cj This means that the change in is small and stable. In particular, in the comparative examples, the absolute value of β is large in Comparative Example 3, in which the Cu content of the alloy for grain boundary diffusion treatment exceeds 40 mass %, so that β can be significantly improved by setting said content to 40 mass % or less. Note that, although the absolute value of β in Comparative Example 7 is slightly smaller than that in Examples 1 to 3, the absolute value of the aforementioned α is larger than that in Examples 1 to 3 (and also than that in Comparative Example 2, in which the Cu content of the alloy for grain boundary diffusion treatment is smaller).

[0036] The present invention is not limited to the above-mentioned embodiment and examples, and various modifications are possible. For example, in the above-mentioned examples, a TbCu alloy containing only Tb as a heavy rare earth element was used as the alloy for grain boundary diffusion treatment, but a R alloy containing only Dy, only Ho, Tb and Dy, Tb and Ho, Dy and Ho, or Tb, Dy and Ho as a heavy rare earth element may be used. Hd A Cu alloy may be used as the alloy for grain boundary diffusion treatment.

[0037] In the above example, R HdAlthough the Cu alloy powder mixed with silicone grease was applied to the substrate as the adhesion material, the powder may be mixed with a grease or liquid other than silicone grease to be used as the adhesion material. Hd Instead of Cu alloy powder, foil-shaped R Hd Cu alloy and lump R Hd The grain boundary diffusion treatment may be carried out by using a Cu alloy as an attachment and heating it in a state where it is attached to (in contact with) the base material.

[0038] In the above examples, a substrate made from RFeB-based magnet powder having a specific composition was used, but the composition of the RFeB-based magnet powder is not limited to the above examples. For example, a substrate made from RFeB-based magnet powder containing a heavy rare earth element may be used. Also, in the above examples, an RFeB-based sintered magnet was used as the substrate, but an RFeB-based hot plastic processing magnet may be used as the substrate.

Claims

1. a substrate preparation step of preparing a substrate made of a sintered body of an RFeB-based alloy containing rare earth elements R, Fe, and B or a hot plastic worked body of the alloy; Heavy rare earth element R to be diffused is any one of Dy, Tb and Ho or a mixture of two or more of them. Hd and Cu, the Cu content being 20 mass% or more and 40 mass% or less. Hd a deposit preparation step of preparing a deposit containing a Cu alloy; an attachment step of attaching the attachment to a surface of the substrate; The base material to which the deposit is attached is treated with the heavy rare earth element R to be diffused. Hd a heating step of heating the substrate to a predetermined temperature at which the The method for producing an RFeB magnet includes the steps of:

2. The deposit is R Hd 2. The method for producing an RFeB magnet according to claim 1, further comprising the step of: forming a powder of a Cu alloy;

3. 3. The method for producing an RFeB magnet according to claim 1, wherein the base material has a C content of 0.10 mass % or less and an O content of 0.10 mass % or less.

4. The heavy rare earth element R to be diffused, which is any one of Dy, Tb, and Ho or a mixture of two or more of them, is attached to a substrate made of a sintered body of an RFeB-based alloy containing rare earth elements R, Fe, and B, or a hot plastic processed body of the alloy, and then heated to a predetermined temperature. Hd An alloy used in a grain boundary diffusion treatment in which the alloy is diffused into the grain boundaries of the substrate, The heavy rare earth element R to be diffused Hd and Cu, the Cu content being 20 mass% or more and 40 mass% or less. Hd A Cu alloy for grain boundary diffusion treatment.

Citation Information

Patent Citations

  • Method and apparatus for manufacturing magnetically anisotropic rare earth sintered magnet

    JP2006019521A

  • RFeB BASED SINTERED MAGNET

    JP2020013975A

  • Manufacturing method of r-t-b based permanent magnet

    JP2020092121A