Manufacturing method for metal and cold plastic processing device used for the manufacturing method

Applying a lubricating liquid with fine bubbles during cold plastic working addresses the issue of surface flaws in metal materials by preventing fusion between the metal surface and the tool, resulting in improved product quality.

JP2024167878APending Publication Date: 2024-12-04NIPPON STEEL CORPORATION

Patent Information

Application Number
JP2024014704
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2024-02-02
Publication Date
2024-12-04

AI Technical Summary

Technical Problem

Existing methods for manufacturing metal materials through cold plastic working often result in surface flaws, particularly in ultra-fine metal wires, due to the strong contact between the metal surface and the plastic working tool, which can lead to welding and the formation of solidified parts, causing defects.

Method used

The method involves applying a lubricating liquid containing fine bubbles to the surface of the plastic working tool and/or the metal material before or during cold plastic working, utilizing the buffering effect of the fine bubbles to prevent strong contact and suppress the formation of surface flaws.

Benefits of technology

The use of fine bubbles in the lubricating liquid effectively reduces the occurrence of surface flaws in metal materials by preventing the new surface from fusing with the tool, thereby enhancing the quality of the manufactured metal products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167878000001_ABST
    Figure 2024167878000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method for metal material that can suppress surface flawing of the metal material after cold plastic processing.SOLUTION: A manufacturing method for metal material includes a lubrication liquid sticking process and a cold plastic processing process. In the lubrication liquid sticking process, lubrication liquid (LU) containing fine bubbles is stuck on at least one of a plastic processing tool (2) and raw metal material (W). In the cold plastic processing process, cold plastic processing is performed on the metal raw material (LU) using the plastic processing tool (2) after the lubrication liquid (LU) is stuck on at least one of a surface of the plastic processing tool (2) and a surface of the metal raw material (W), thereby manufacturing the metal material.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a metal material and a cold plastic working apparatus used in the manufacturing method. [Background technology]

[0002] 2. Description of the Related Art A method for manufacturing a metallic material by performing cold plastic working on a metallic raw material is known. Cold plastic working can be broadly divided into (1) wire drawing, (2) cold drawing, (3) cold extrusion, and (4) cold rolling.

[0003] Metal wires such as steel cord, aluminum wire, copper wire, and titanium wire may have a wire diameter of less than 1 mm. Such ultra-fine metal wires are manufactured by wire drawing, a type of cold plastic processing. In wire drawing, a metal material is passed through a die and then drawn out of the die to produce a metal wire.

[0004] Metal bars, such as steel bars, aluminum bars, copper bars, and titanium bars, and metal tubes, such as steel pipes, aluminum pipes, copper pipes, and titanium pipes, are manufactured by cold drawing, which is a type of cold plastic processing. In cold drawing, a metal material is passed through a die and then pulled out of the die to manufacture a metal material (metal bar or metal tube).

[0005] Steel shapes, aluminum shapes, copper shapes, titanium shapes, etc. are manufactured by cold extrusion, which is a type of cold plastic processing. In cold extrusion, a stem is used to push a metal material out of a die to manufacture a metal material (metal shape).

[0006] Metal sheets such as steel sheets, aluminum sheets, copper sheets, and titanium sheets are manufactured by cold rolling, which is a type of cold plastic processing. The above-mentioned metal wires, metal bars, and metal tubes may also be manufactured by cold rolling. In cold rolling, a metal material is cold-rolled using a work roll to manufacture a metal material (metal sheet, metal wire, metal bar, metal tube).

[0007] A number of techniques for manufacturing metal materials using these cold plastic working processes have been proposed. For example, metal wire drawing techniques are disclosed in JP 2011-147963 A (Patent Document 1) and JP 2014-151357 A (Patent Document 2). Patent Document 1 discloses a technique for regenerating a lubricant whose lubricating performance has deteriorated during wire drawing. Patent Document 2 discloses a technique for efficiently removing plating debris generated during wire drawing of plated wire from the lubricant and reusing the lubricant. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2011-147963 A [Patent Document 2] JP 2014-151357 A Summary of the Invention [Problem to be solved by the invention]

[0009] However, when a metal material is manufactured by cold plastic working, defects may occur on the surface of the manufactured metal material. For example, when a metal wire is manufactured by wire drawing, the smaller the wire diameter of the metal wire, the lower the strength of the metal wire. Therefore, defects are more likely to occur on the surface of the metal wire during wire drawing. Patent Documents 1 and 2 disclose techniques related to the reuse of lubricants, but do not consider suppressing surface defects on metal materials after cold plastic working.

[0010] An object of the present invention is to provide a manufacturing method for a metal material that can suppress the occurrence of surface defects on the metal material after cold plastic working, and a cold plastic working apparatus used in the manufacturing method. [Means for solving the problem]

[0011] The manufacturing method of the metal material of this embodiment includes a lubricant application step and a cold plastic processing step. In the lubricant application step, a lubricant containing fine bubbles is applied to at least one of the surface of the plastic processing tool and the surface of the metal raw material. In the cold plastic processing step, the lubricant is applied to at least one of the surface of the plastic processing tool and the surface of the metal raw material, and then cold plastic processing is performed on the metal raw material using the plastic processing tool to manufacture the metal material.

[0012] The cold plastic processing apparatus of this embodiment is capable of performing cold plastic processing on a metal material. The cold plastic processing apparatus includes a plastic processing tool, a fine bubble generator, and a lubricant applying device. The fine bubble generator generates a lubricant containing fine bubbles. The lubricant applying device applies the lubricant containing fine bubbles to at least one of the surface of the plastic processing tool and the surface of the metal material before or during the cold plastic processing. Effect of the Invention

[0013] The method for producing a metal material according to the present embodiment can suppress the occurrence of surface defects on the metal material after cold plastic working. The cold plastic working apparatus according to the present embodiment can suppress the occurrence of surface defects on the metal material after cold plastic working. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic diagram showing an example of a cold plastic working apparatus used in the method for producing a metallic material according to the first embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a cold plastic working apparatus having another configuration different from that shown in FIG. [Diagram 3] FIG. 3 is a schematic diagram showing an example of a cold plastic working apparatus having another configuration different from those shown in FIGS. [Figure 4] FIG. 4 is a schematic diagram showing an example of a cold plastic working apparatus having another configuration different from those shown in FIGS. [Diagram 5] FIG. 5 is a schematic diagram showing an example of a cold plastic working apparatus used in the method for producing a metallic material according to the second embodiment. [Figure 6] FIG. 6 is a schematic diagram showing an example of a cold plastic working apparatus used in the method for producing a metallic material according to the third embodiment. [Figure 7] FIG. 7 is a schematic diagram for explaining cold plastic working using the cold plastic working apparatus of FIG. [Figure 8] FIG. 8 is a schematic diagram showing an example of a cold plastic working apparatus used in the method for producing a metal material according to the third embodiment, which is different from that shown in FIG. [Figure 9] FIG. 9 is a schematic diagram for explaining cold plastic working using the cold plastic working apparatus of FIG. [Figure 10] FIG. 10 is a schematic diagram showing an example of a cold plastic working apparatus used in the method for producing a metallic material according to the fourth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The manufacturing method of the metal material of this embodiment includes a lubricant application step and a cold plastic processing step. In the lubricant application step, a lubricant containing fine bubbles is applied to at least one of the surface of the plastic processing tool and the surface of the metal material. In the cold plastic processing step, after the lubricant is applied to at least one of the surface of the plastic processing tool and the surface of the metal material, cold plastic processing is performed on the metal material using the plastic processing tool to manufacture the metal material (first configuration).

[0016] When cold plastic processing is performed on a metallic material, the metallic material is restrained by plastic processing tools such as dies and work rolls and undergoes plastic deformation. During plastic deformation, a new surface is generated on the surface of the metallic material. The new surface is likely to weld to the surface of the plastic processing tool. If part of the new surface is welded to the surface of the plastic processing tool, the welded part will solidify on the surface of the plastic processing tool to form a solidified part. This solidified part will come into contact with the metallic material as it passes through the plastic processing tool, forming a defect on the surface of the metallic material (metal material).

[0017] In the manufacturing method of the metal material of the first configuration, a lubricating liquid containing fine bubbles is applied to at least one of the surface of the plastic processing tool and the surface of the metal material, and then cold plastic processing is performed. In this case, the fine bubbles in the lubricating liquid are interposed between the surface of the plastic processing tool and the surface of the metal material during cold plastic processing. At this time, it is considered that the fine bubbles have a buffering effect between the surface of the plastic processing tool and the surface of the metal material, which buffers direct collision between the surface of the plastic processing tool and the surface of the metal material. Due to this buffering effect, the fine bubbles suppress strong contact between the surface of the plastic processing tool and the newly formed surface of the metal material. Therefore, the newly formed surface of the metal material is less likely to fuse to the surface of the plastic processing tool. As a result, the occurrence of scratches is suppressed on the surface of the metal material after cold plastic processing.

[0018] The manufacturing method of the metallic material of the second aspect is the manufacturing method of the metallic material of the first aspect, in which the average particle size of the fine bubbles is 0.01 μm or more and 50.00 μm or less.

[0019] In the case of the second method for producing a metal material, the fine bubbles are fine bubbles or ultrafine bubbles. In this case, the fine bubbles can be easily interposed between the surface of the plastic processing tool and the surface of the metal material. As a result, the occurrence of scratches on the surface of the metal material can be suppressed by the buffering effect of the fine bubbles interposed between the surface of the plastic processing tool and the surface of the metal material.

[0020] The manufacturing method of the metallic material of the third aspect is the manufacturing method of the metallic material of the second aspect, in which the average particle size of the fine bubbles is not less than 0.01 μm and less than 1.00 μm.

[0021] In the case of the manufacturing method of the metal material of the third aspect, the fine bubbles are ultrafine bubbles, and therefore the fine bubbles can be more easily interposed between the surface of the plastic processing tool and the surface of the metal material.

[0022] A manufacturing method of a metallic material of a fourth aspect is a manufacturing method of a metallic material of any one of the first to third aspects, in which the metallic material contains any one of aluminum, steel, titanium, and copper as a main component.

[0023] A manufacturing method for a metal material according to a fifth aspect is a manufacturing method for a metal material according to any one of the first to fourth aspects, in which the number density of fine bubbles in the lubricating liquid is set to 50 bubbles / mL or more.

[0024] In the fifth embodiment of the method for producing a metal material, the fine bubble density is 50 bubbles / mL or more, so that a sufficient amount of fine bubbles is contained in the lubricating liquid. Therefore, a sufficient amount of fine bubbles is present between the surface of the plastic processing tool and the surface of the metal material during cold plastic processing. As a result, the occurrence of surface defects in the metal material after cold plastic processing can be suppressed.

[0025] A sixth aspect of the method for producing a metal material is the method for producing a metal material of any one of the first to fifth aspects, in which the plastic processing tool is a die. In the cold plastic processing step, the die is used to perform wire drawing on the metal material to produce the metal material in the form of a metal wire.

[0026] The manufacturing method of the metal material of the seventh configuration is the manufacturing method of the metal material of the sixth configuration, in which wire drawing is performed using one or more dies, and when the diameter of the through hole of the final die among the one or more dies is d (μm), the average particle size of the fine bubbles is 0.6 dμm or less.

[0027] In the seventh aspect of the method for producing a metal material, a sufficient amount of fine bubbles can be present between the surface of the through hole of the die and the surface of the metal material, which can further suppress the occurrence of surface defects in the metal material after cold plastic working.

[0028] The manufacturing method of a metal material of an eighth aspect is the manufacturing method of a metal material of any one of the first to fifth aspects, in which the plastic processing tool is a die. In the cold plastic processing step, the die is used to perform cold drawing on the metal material to manufacture the metal material that is a metal bar or a metal tube.

[0029] A ninth aspect of the method for producing a metal material is the method for producing a metal material of any one of the first to fifth aspects, in which the plastic processing tool is a die. In the cold plastic processing step, the die is used to perform cold extrusion processing on the metal material to produce a metal material that is a metal bar or a metal tube.

[0030] A tenth aspect of the method for producing a metal material is the method for producing a metal material of any one of the first to fifth aspects, in which the plastic processing tool is a work roll. In the cold plastic processing step, the work roll is used to cold roll the metal material to produce one of a metal bar, a metal tube, and a metal plate.

[0031] A manufacturing method of a metallic material of an eleventh configuration is a manufacturing method of a metallic material of any one of the first to fourth configurations, in which the cold plastic processing step performs cold plastic processing using one or more plastic processing tools. When the plastic processing tool is a die and the cold plastic processing is wire drawing or cold drawing, the area reduction rate of the metallic material at each plastic processing tool is set to 10.0% or more and less than 23.5%. When the plastic processing tool is a die and the cold plastic processing is cold extrusion, the area reduction rate of the metallic material at each plastic processing tool is set to 50.0% or more and 95.0% or less. When the plastic processing tool is a work roll and the cold plastic processing is cold rolling, the area reduction rate of the metallic material at each plastic processing tool is set to 50.0% or more and 95.0% or less. In the lubricating liquid application process, when the minimum number density N / mL defined by formula (1) is determined for each cold plastic processing using each plastic processing tool, the number density of fine bubbles in the lubricating liquid is set to be equal to or greater than the maximum value of the minimum number density N / mL. N = 50 × (P / 100) × V (1) Here, the area reduction rate (%) of the plastic processing tool defined by equation (2) is substituted for P in equation (1), and the moving speed V (mpm) of the metal material at the exit side of the plastic processing tool is substituted for V. P = {(A0-A1) / A0} × 100 (2) Here, A0 in formula (2) is the cross-sectional area (mm 2 ) is substituted, and A1 is the cross-sectional area (mm2 ) is substituted.

[0032] In the manufacturing method of the metal material of the eleventh aspect, the number density of the fine bubbles in the lubricating liquid is set to a maximum value of N bubbles / mL or more. In this case, an appropriate amount of fine bubbles is contained in the lubricating liquid, taking into consideration the type of cold plastic processing and manufacturing conditions. Therefore, a sufficient amount of fine bubbles is interposed between the surface of the plastic processing tool and the surface of the metal material during cold plastic processing. As a result, the occurrence of surface defects in the metal material after cold plastic processing can be more effectively suppressed.

[0033] The cold plastic processing device of the twelfth configuration is capable of performing cold plastic processing on a metal material. The cold plastic processing device includes a plastic processing tool, a fine bubble generator, and a lubricant applying device. The fine bubble generator generates a lubricant containing fine bubbles. The lubricant applying device applies the lubricant containing fine bubbles to at least one of the surface of the plastic processing tool and the surface of the metal material before or during the cold plastic processing.

[0034] In the cold plastic processing device of the twelfth configuration, a fine bubble generator generates a lubricant containing fine bubbles. Furthermore, a lubricant application device applies the lubricant containing fine bubbles to the surface of the plastic processing tool or the surface of the metal material. Therefore, during cold plastic processing, fine bubbles in the lubricant are present between the surface of the plastic processing tool and the surface of the metal material. As a result, the occurrence of surface defects in the metal material after cold plastic processing can be suppressed.

[0035] A cold plastic working apparatus of a thirteenth configuration is the cold plastic working apparatus of the twelfth configuration, in which the lubricant applying device includes a nozzle and a supplying device. The nozzle discharges the lubricant containing fine bubbles onto at least one of the surface of the plastic working tool and the surface of the metal material. The supplying device supplies the lubricant containing fine bubbles to the nozzle.

[0036] The cold plastic processing apparatus of the thirteenth configuration can apply a lubricating liquid containing fine bubbles to the surface of the plastic processing tool and / or the surface of the metal material by using a supply device and a nozzle.

[0037] A cold plastic processing apparatus of a fourteenth configuration is the cold plastic processing apparatus of the thirteenth configuration, in which the nozzle is disposed on the inlet side of the plastic processing tool. The nozzle discharges a lubricating liquid containing fine bubbles from the inlet side of the plastic processing tool onto at least one of the surface of the plastic processing tool and the surface of the metal material.

[0038] In the cold plastic processing device of the fourteenth configuration, the lubricating liquid containing fine bubbles is discharged from the inlet side of the plastic processing tool onto the surface of the plastic processing tool and / or the surface of the metal material. Therefore, before plastic processing is performed, the lubricating liquid containing fine bubbles is attached to the surface of the plastic processing tool and / or the surface of the metal material.

[0039] A cold plastic processing apparatus of a fifteenth configuration is the cold plastic processing apparatus of any one of the twelfth to fourteenth configurations, in which the plastic processing tool is a die capable of performing wire drawing or cold drawing on the metal material. The cold plastic processing apparatus further includes a drawing device. The drawing device draws the metal material from the plastic processing tool.

[0040] A cold plastic processing apparatus of a sixteenth configuration is the cold plastic processing apparatus of the fifteenth configuration, and the cold plastic processing apparatus is capable of performing wire drawing on a metal material. The lubricant application device includes a storage tank and an immersion mechanism. The storage tank is capable of storing lubricant containing fine bubbles. The immersion mechanism immerses the metal material in the lubricant in the storage tank at the entry side of the die before passing through the die. The die is disposed at a position where it is immersed in the lubricant in the storage tank.

[0041] In the cold plastic working device of the sixteenth configuration, the die is immersed in the lubricating liquid in the reservoir, and further, the metal material is immersed in the lubricating liquid in the reservoir at the entry side of the die, so that the lubricating liquid containing fine bubbles can be applied to the surface of the metal material before it passes through the die and to the surface of the through-hole of the die.

[0042] A cold plastic working apparatus of a seventeenth aspect is the cold plastic working apparatus of the sixteenth aspect, further comprising a drawing mechanism. The drawing mechanism draws the metal material after passing through the die from the lubricating liquid in the reservoir at the exit side of the die.

[0043] In the cold plastic working device of the seventeenth configuration, the metal material after cold plastic working is drawn out from the lubricating liquid in the reservoir, so that the metal material can be wound outside the reservoir.

[0044] The cold plastic working apparatus of an eighteenth configuration is the cold plastic working apparatus of the twelfth configuration, in which the plastic working tool is a die capable of cold extrusion working a metal material. The cold plastic working apparatus further includes a container for storing the metal material, and a stem for extruding the metal material stored in the container from the die.

[0045] A cold plastic working apparatus of a nineteenth configuration is the cold plastic working apparatus of any of the twelfth to fourteenth configurations, in which the plastic working tool is a work roll capable of cold rolling a metallic material.

[0046] Hereinafter, the manufacturing method and cold plastic working apparatus of the present embodiment will be described with reference to the drawings. In each drawing, the same or corresponding components are given the same reference numerals, and the same description will not be repeated.

[0047] [Method of manufacturing metal material according to this embodiment] The manufacturing method of the metal material of this embodiment includes a lubricant application step and a cold plastic processing step. In the lubricant application step, a lubricant containing fine bubbles is applied to at least one of the surface of the plastic processing tool and the surface of the metal raw material. In the cold plastic processing step, the lubricant is applied to at least one of the surface of the plastic processing tool and the surface of the metal raw material, and then cold plastic processing is performed on the metal raw material using the plastic processing tool to manufacture the metal material.

[0048] Here, the cold plastic working includes (1) wire drawing, (2) cold drawing, (3) cold extrusion, and (4) cold rolling. In the first embodiment, the manufacturing method of the metal material of the present embodiment will be described by taking the case where the cold plastic working is wire drawing as an example.

[0049] [First embodiment] [About cold plastic processing equipment] Fig. 1 is a schematic diagram showing an example of a cold plastic processing apparatus used in the manufacturing method of a metal material of this embodiment. Referring to Fig. 1, the cold plastic processing apparatus includes a plastic processing tool 2, a fine bubble generator 4, and a lubricant liquid attachment device 5. The cold plastic processing apparatus shown in Fig. 1 is a wire drawing apparatus. Each component will be described below.

[0050] [About plastic processing tool 2] 1, the plastic processing tool 2 is a die. In the first embodiment, the plastic processing tool 2 will also be referred to as a die 2 in the following description. The die 2 has a through hole in the center. The die 2 may have a known configuration. The through hole of the die 2 includes, for example, an approach and reduction section, a bearing section, and a back relief section, in that order from the entry side to the exit side of the die 2. The inner diameters of the approach and reduction sections become smaller from the entry side to the exit side of the die 2. The approach and reduction sections have the role of introducing the metal material W, which is a metal wire, into the die 2 and reducing the diameter of the metal material W. The inner diameter of the bearing section is constant. The inner diameter of the bearing section corresponds to the die diameter. The bearing section restrains the metal material W to keep the outer diameter of the metal material W constant. The inner diameter of the back relief section becomes larger from the entry side to the exit side of the die 2. The back relief section prevents the die 2 from being damaged by the metal material W.

[0051] When the cold plastic processing apparatus is a wire drawing apparatus, the cold plastic processing apparatus further includes a drawing device 3. The drawing device 3 draws the metal material W from the die 2. The drawing device 3 includes a winding device 32 and a support reel 33. The unwinding device 31 unwinds the coil-shaped metal material W. The winding device 32 draws the metal material W, which is unwound from the unwinding device 31 and passes through the die 2, from the die 2. The winding device 32 further winds up the metal material W drawn from the die 2 into a coil. The support reel 33 is arranged on the inlet side and / or outlet side of the die 2, and supports the metal material W during wire drawing. The drawing device 3 does not have to include the support reel 33.

[0052] The drawing device 3 is not limited to the above configuration. The drawing device 3 may have a configuration other than the above configuration as long as it is configured to draw the metal material W from the die 2.

[0053] [About Fine Bubble Generator 4] The fine bubble generator 4 generates a lubricating liquid LU containing fine bubbles. The fine bubble generator 4 is arranged outside a storage tank 511 in which the lubricating liquid LU is stored. In FIG. 1, one fine bubble generator 4 is arranged. However, the arrangement position and the number of the fine bubble generators 4 are not particularly limited. There may be one fine bubble generator 4 or multiple fine bubble generators 4.

[0054] The fine bubble generator 4 includes a pipe 41, a pipe 42, and a fine bubble generator 43. The pipe 41 and the pipe 42 connect a storage tank 511 and the fine bubble generator 43. The lubricating liquid LU from the storage tank 511 is introduced into the fine bubble generator 43 via the pipe 41. The fine bubble generator 43 generates fine bubbles in the lubricating liquid LU.

[0055] The method of generating fine bubbles by the fine bubble generator 43 is not particularly limited. The fine bubble generator 43 may generate fine bubbles by using dissolved gas in the lubricating liquid LU by a swirling liquid flow type. The fine bubble generator 43 may adopt any of an ejector type, a Venturi type, a pressurized dissolution type, and a fine hole type to take in external gas into the lubricating liquid LU and generate fine bubbles. The fine bubble generator 43 can be appropriately selected from known fine bubble generators. The lubricating liquid LU containing the fine bubbles is returned to the storage tank 511 via the piping 42.

[0056] The lubricating liquid LU contains water and a surfactant. That is, the lubricating liquid LU used in the manufacturing method of this embodiment is a water-soluble lubricating liquid. The surfactant may be a well-known one. For example, the surfactant is one or more selected from the group consisting of a nonionic surfactant, an anionic surfactant, an amphoteric surfactant, and a cationic surfactant.

[0057] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyalkylene alkyl phenyl ethers, polyoxy(ethylene and / or propylene) alkyl phenyl ethers, polyoxyethylene alkyl esters consisting of polyethylene glycol or ethylene oxide and higher fatty acids (e.g., having 12 to 18 carbon atoms), and polyoxyethylene sorbitan alkyl esters consisting of sorbitan, polyethylene glycol, and higher fatty acids (e.g., having 12 to 18 carbon atoms). Examples of the anionic surfactant include fatty acid salts, sulfate salts, sulfonate salts, phosphate salts, and dithiophosphate salts. Examples of amphoteric surfactants include amino acid-type and betaine-type carboxylates, sulfates, sulfonates, and phosphates. Examples of cationic surfactants include aliphatic amine salts, quaternary ammonium salts, and the like.

[0058] The lubricating fluid LU may contain other components in addition to water and surfactants, such as extreme pressure additives, rust inhibitors, preservatives, and friction reducers.

[0059] In this specification, fine bubbles refer to fine bubbles having a particle size of less than 100 μm as defined in JIS B 8741-1:2019. Note that microbubbles refer to fine bubbles having a particle size of 1.00 μm or more and less than 100.00 μm. In this specification, ultrafine bubbles refer to fine bubbles having a grain boundary of 0.01 μm or more and less than 1.00 μm.

[0060] [Lubricant deposition device 5] The lubricant application device 5 applies a lubricant LU containing fine bubbles to the surface of the metal material W before it passes through the die 2. In FIG.

[0061] The supply device 51 includes a storage tank 511, a pipe 512, and a driving source 513. The storage tank 511 is capable of storing lubricating liquid LU containing fine bubbles. One end of the pipe 512 is immersed in the lubricating liquid stored in the storage tank 511. The other end of the pipe 512 is connected to the lubricating liquid nozzle 52. The driving source 513 supplies the lubricating liquid LU in the storage tank 511 to the lubricating liquid nozzle 52 via the pipe 512. The driving source 513 is, for example, a pump.

[0062] The lubricating liquid nozzle 52 is disposed on the inlet side of the die 2. The lubricating liquid nozzle 52 receives a supply of lubricating liquid LU containing fine bubbles from a pipe 512. The lubricating liquid nozzle 52 then discharges the lubricating liquid LU containing fine bubbles to the outside, and causes the lubricating liquid LU to adhere to the surface of the metal material W before it passes through the die 2.

[0063] The cold plastic working apparatus may further include a lubricating liquid recovery device 6. The lubricating liquid recovery device 6 includes a recovery pan 61 and a recovery pipe 62. The recovery pan 61 functions as a receiver for recovering the lubricating liquid LU discharged from the lubricating liquid nozzle 52. The recovery pipe 62 discharges the lubricating liquid LU stored in the recovery pan 61 into a storage tank 511. The lubricating liquid recovery device 6 allows the lubricating liquid LU to be circulated and utilized. It is noted that the cold plastic working apparatus does not necessarily have to include the lubricating liquid recovery device 6.

[0064] [Method of manufacturing metal materials using cold plastic processing equipment] In the method for producing a metallic material of this embodiment, the above-mentioned cold plastic working apparatus is used to perform cold plastic working on a metallic material W. Hereinafter, the method for producing a metallic material of this embodiment will be described.

[0065] In the manufacturing method of the metal material of this embodiment, the lubricating liquid LU containing fine bubbles is prepared. As described above, the fine bubble generator 4 generates the lubricating liquid LU containing fine bubbles.

[0066] Furthermore, a metal material W to be subjected to cold plastic working is prepared. There are no particular limitations on the metal material W as long as it is made of a metal. The metal material W is made of a metal containing, as a main component, any one selected from the group consisting of aluminum, steel, titanium, and copper, for example. Here, "main component" means that the component is contained in an amount of 50% or more by mass.

[0067] The metal material W containing aluminum as a main component is, for example, a material made of aluminum or a material made of an aluminum alloy.

[0068] In this embodiment, the metal material W is a wire. The prepared metal material W is attached to the unwinding device 31 in a state where it is wound around a reel in a coil shape, for example.

[0069] After the above preparations, cold plastic working (wire drawing) is performed on the metallic material W. At this time, the lubricating liquid LU containing the above-mentioned fine bubbles is applied to at least one of the surface of the metallic material W before the cold plastic working and the surface of the die 2 (the surface of the through hole, i.e., the inner surface of the die). Specifically, at the inlet side of the die 2, the lubricating liquid LU containing the fine bubbles is discharged from the lubricating liquid nozzle 52 of the lubricating liquid application device 5, and the lubricating liquid LU is applied to the surface of the metallic material W before it passes through the die 2 and / or the surface (inner surface) of the die 2.

[0070] After the lubricating liquid LU containing fine bubbles is applied to the surface of the metal material W and / or the surface (inner surface) of the die 2, the metal material W is passed through the die 2 for cold plastic working (wire drawing). Specifically, the metal material W is drawn from the entry side to the exit side of the die 2 by the drawing device 3. In this case, the metal material W passes through the die 2 with the lubricating liquid LU containing fine bubbles applied to its surface. Through the above steps, the manufacturing method of this embodiment performs cold plastic working on the metal material W. As a result, the occurrence of surface defects in the manufactured metal material (metal wire) is significantly suppressed.

[0071] The reason why the manufacturing method of this embodiment significantly suppresses surface defects in the manufactured metal wire is believed to be as follows.

[0072] When cold plastic working is performed on the metallic material W, the metallic material W is restrained all around by the die 2. The metallic material W is subjected to an external force from the die 2 all around and undergoes cold plastic deformation (diameter reduction). In other words, cold plastic working is different from working in which an external force is applied to a part of the entire circumference of the workpiece, such as cutting, and is worked in a state in which the entire circumference is substantially restrained.

[0073] In this way, in cold plastic processing, plastic deformation occurs under harsh conditions with the entire circumference restrained by the die 2, and a new surface is generated on the surface of the metal material W by the plastic processing. Since the new surface is in an active state, it is likely to weld to the inner surface of the through hole of the die 2. If part of the new surface welds to the inner surface of the die 2, the welded part solidifies and forms a convex solidified part. When the metal material W passes through the die 2 during the wire drawing process, it comes into contact with the solidified part formed by welding, and linear scratches extending in the axial direction of the metal material W are formed on the surface of the metal material W.

[0074] In this embodiment, as described above, the lubricating liquid LU containing fine bubbles is applied to the surface of the metal material W or the inner surface of the die 2 at the inlet side of the die 2. In this case, the lubricating liquid LU containing fine bubbles is interposed between the entire surface of the through hole of the die 2 and the entire surface of the metal material W. At this time, the fine bubbles have a buffering effect between the surface of the through hole of the die 2 and the surface of the metal material W. Due to this buffering effect, the fine bubbles suppress strong contact between the surface of the through hole of the die 2 and the surface of the metal material W. The fine bubbles further have the effect of aggregating the surfactant in the lubricating liquid LU. Due to this aggregating effect, the fine bubbles increase the adsorption of the surfactant on the surface of the through hole of the die 2 and the surface of the metal material W.

[0075] Due to the above two actions, the fine bubbles in the lubricating liquid LU suppress the newly formed surface of the metal material W, which is generated by the strong constraint of the die 2, from coming into strong contact with the surface of the through hole of the die 2. This makes it difficult for the newly formed surface of the metal material W to fuse to the surface of the through hole of the die 2, and makes it difficult for a solidified portion to form on the surface of the through hole of the die 2. As a result, the occurrence of defects on the surface of the metal material after cold plastic working is significantly suppressed.

[0076] 1, the cold plastic working apparatus includes one plastic working tool (die) 2. However, the cold plastic working apparatus may include a plurality of plastic working tools (dies) 2.

[0077] Fig. 2 is a schematic diagram of an example of a cold plastic working apparatus having another configuration different from that of Fig. 1. Referring to Fig. 2, the cold plastic working apparatus includes a plurality of dies 2. The plurality of dies 2 are arranged in a line. The other configurations of the cold plastic working apparatus are the same as those of the cold plastic working apparatus of Fig. 1.

[0078] The manufacturing method of the metal material using the cold plastic processing apparatus of FIG. 2 is the same as the manufacturing method of the metal material using the cold plastic processing apparatus of FIG. 1. Specifically, at the inlet side of the die 2, the lubricating liquid LU containing fine bubbles is applied to the surface of the metal material W and / or the inner surface of the die 2 by the lubricating liquid nozzle 52. Then, after the lubricating liquid LU containing fine bubbles is applied to the surface of the metal material W and / or the inner surface of the die 2, the metal material W is passed through a plurality of dies 2 to perform cold plastic processing (wire drawing). As described above, even when the cold plastic processing apparatus has a plurality of dies 2, the lubricating liquid LU containing fine bubbles is applied to the surface of the metal material W and / or the inner surface of the die 2, so that the buffering action and the coagulation action of the fine bubbles can be utilized. As a result, the occurrence of scratches is suppressed on the surface of the metal material after wire drawing.

[0079] When the cold plastic processing device is equipped with a plurality of plastic processing tools (dies) 2, preferably, as shown in Fig. 3, a lubricating liquid nozzle 52 is provided on the inlet side of each plastic processing tool (die) 2. In this case, a sufficient amount of lubricating liquid LU containing fine bubbles can be applied to the surface of the metal material W before it is inserted into each plastic processing tool (die) 2 and / or to the surface (inner surface) of the plastic processing tool (die) 2. Therefore, the occurrence of defects on the surface of the metal material after cold plastic processing is more effectively suppressed.

[0080] [Preferable average particle size of fine bubbles D] In the manufacturing method of the metal material (metal wire) of this embodiment, the diameter (smallest inner diameter) of the through hole of the final die 2 among one or more dies 2 is d (μm). In this case, the average particle size D of the fine bubbles is preferably 0.6 dμm or less. Here, the minimum inner diameter d (μm) of the through hole of the die 2 is, for example, the inner diameter of the bearing portion of the through hole of the die 2 .

[0081] As described above, the fine bubbles exert a buffering effect and a flocculating effect by being present between the inner surface of the through hole of the die 2 and the surface of the metal material W. Therefore, it is preferable that the fine bubbles have a size that allows them to penetrate between the inner surface of the through hole of the die 2 and the surface of the metal material W. As described above, the smaller the wire diameter of the metal material W, the lower the strength of the metal material W. Therefore, the smaller the wire diameter of the metal material W, the more likely it is that defects will occur. Therefore, when wire drawing is performed continuously using one or more dies 2, it is preferable to adjust the average particle size of the fine bubbles to a size that allows them to be inserted between the inner surface of the through hole of the die 2 in which the final wire drawing is performed and the surface of the metal material W to be wire drawn by that die 2.

[0082] When the average particle size D of the fine bubbles is 0.6 dμm or less, it is sufficiently small relative to the minimum inner diameter d of the through holes of the die 2. Therefore, the fine bubbles can easily penetrate between the inner surface of the through holes of the die 2 and the surface of the metal material W. As a result, the buffering and coagulating effects of the fine bubbles interposed between the inner surface of the through holes of the die 2 and the surface of the metal material W can suppress the occurrence of scratches even in the metal material W having a thin wire diameter.

[0083] The lower limit of the average particle size of the fine bubbles is not particularly limited, and the preferred lower limit of the average particle size of the fine bubbles is 0.01 μm.

[0084] [Desirable fine bubble density ND (part 1)] In the manufacturing method of the metal material of this embodiment, the number density of the fine bubbles in the lubricating liquid LU is not particularly limited. Preferably, the number density ND of the fine bubbles in the lubricating liquid LU is set to 50 bubbles / mL or more.

[0085] If the number density ND of the fine bubbles is 50 bubbles / mL or more, a sufficient amount of fine bubbles is contained in the lubricating liquid LU. Therefore, during cold plastic working, a sufficient amount of fine bubbles is present between the inner surface of the through hole of the die 2 and the surface of the metal material W. As a result, the occurrence of defects in the metal wire after cold plastic working can be more effectively suppressed.

[0086] The preferred lower limit of the fine bubble number density ND is 60 bubbles / mL, more preferably 70 bubbles / mL, even more preferably 80 bubbles / mL, even more preferably 90 bubbles / mL, and even more preferably 100 bubbles / mL. The upper limit of the fine bubble number density ND is not particularly limited. The upper limit of the fine bubble number density ND is, for example, 60000 bubbles / mL, for example, 50000 bubbles / mL, for example, 40000 bubbles / mL.

[0087] [Method for measuring the average particle size D and number density ND of fine bubbles] The average particle size D (μm) and number density ND (pieces / mL) of fine bubbles are measured by the following method. 10 mL of lubricating fluid LU containing fine bubbles is collected. The particle size distribution of the fine bubbles in the collected lubricating fluid LU is determined by the quantitative laser diffraction and scattering method using a particle size distribution measuring device. A laser is irradiated onto the fine bubbles, and the scattered light is detected by a forward scattered light sensor, a side scattered light sensor, and a back scattered light sensor. The particle size distribution of the fine bubbles is determined from the light intensity distribution pattern, and the median diameter of the obtained particle size distribution is defined as the average particle size D (μm). Furthermore, in the quantitative laser diffraction and scattering method, calibration is performed using polystyrene latex standard particles with a known number density, and the difference in refractive index between the fine bubbles (air) and polystyrene latex is corrected using the Mie scattering theory. The number density ND (pieces / mL) of the fine bubbles is determined by the above method.

[0088] [Preferable fine bubble density ND (part 2)] In the manufacturing method of this embodiment, preferably, cold plastic working is performed using one or more plastic working tools (dies) 2, and further, the area reduction rate of the metal material W in the wire drawing process at each plastic working tool (die) 2 is set to 10.0% or more and less than 23.5%. In this case, when the minimum number density N / mL defined by formula (1) is determined for each plastic working tool (die) 2, preferably, the number density ND of the fine bubbles in the lubricating liquid LU is set to be equal to or more than the maximum value of the minimum number density N / mL. N = 50 × (P / 100) × V (1) Here, the area reduction rate (%) of the plastic processing tool (die) 2 defined by equation (2) is substituted for P in equation (1), and the moving speed V (mpm) of the metal material W at the exit side of the plastic processing tool (die) 2 is substituted for V. P = {(A0-A1) / A0} × 100 (2) Here, A0 in formula (2) is the cross-sectional area (mm 2 ) is substituted, and A1 is the cross-sectional area (mm 2 ) is substituted.

[0089] More specifically, the number density ND of the fine bubbles is calculated as follows. When a metal material is manufactured by performing cold plastic processing (wire drawing) using only one plastic processing tool (die) 2, the minimum number density N / mL in the cold plastic processing (die) 2 is calculated based on formulas (1) and (2). The obtained minimum number density N / mL is set as the lower limit of the preferable number density ND of the fine bubbles.

[0090] On the other hand, when a metal material is manufactured by continuously performing cold plastic processing (wire drawing) once using a plurality of plastic processing tools (dies) 2, that is, when wire drawing is performed using a plurality of plastic processing tools (dies) 2 while the metal material W unwound from the unwinding device 31 is being wound up by the winding device 32, the lower limit of the preferable number density ND of the fine bubbles is obtained by the following method. The minimum number density N / mL for each plastic processing tool (die) 2 is obtained based on formulas (1) and (2). The maximum value of the obtained minimum number densities N / mL is set as the lower limit of the preferable number density ND of the fine bubbles.

[0091] In cold plastic working, the higher the area reduction rate P, the more easily the newly formed surface of the metal material W passing through the plastic working tool (die) 2 will fuse with the inner surface of the through hole of the plastic working tool (die) 2. Also, the faster the moving speed V, the more easily the newly formed surface of the metal material W passing through the plastic working tool (die) 2 will fuse with the inner surface of the through hole of the plastic working tool (die) 2. Therefore, the preferable number density ND of the fine bubbles varies depending on the area reduction rate P and the moving speed V of the metal material W. Furthermore, when wire drawing is performed once using multiple plastic working tools (dies) 2, the preferable number density ND of the fine bubbles further varies depending on the area reduction rate P at each plastic working tool (die) and the moving speed V of the metal material W.

[0092] If the number density ND of the fine bubbles in the lubricating liquid LU is equal to or greater than the maximum value of the minimum number density N / mL, then an appropriate amount of fine bubbles is contained in the lubricating liquid LU, taking into consideration the most severe manufacturing conditions of the cold plastic working. Therefore, during the cold plastic working, a sufficient amount of fine bubbles is present between the inner surface of the through hole of the plastic working tool (die) 2 and the surface of the metal material W. As a result, the occurrence of defects in the metal material after the cold plastic working can be more effectively suppressed.

[0093] The moving speed V (mpm) of the metal material at the exit side of the plastic processing tool can be determined by a speedometer arranged at the exit side of the plastic processing tool.

[0094] [Other examples of cold plastic processing equipment (wire drawing equipment)] 1 to 3, the lubricant application device 5 of the cold plastic working device includes a plurality of lubricant nozzles 52, and the lubricant LU is applied to the surface of the metal material W before wire drawing by the lubricant nozzles 52. However, the lubricant application device 5 may have another configuration.

[0095] Fig. 4 is a schematic diagram of an example of another cold plastic processing apparatus (wire drawing apparatus) having a different configuration from that of Figs. 1 to 3. Referring to Fig. 4, the cold plastic processing apparatus (wire drawing apparatus) of this example differs from that of Figs. 1 to 3 in the configuration of the lubricating liquid adhering device 5. The other configurations of the cold plastic processing apparatus of this example are the same as those of the cold plastic processing apparatus of Figs. 1 to 3.

[0096] The lubricant application device 5 includes a storage tank 511, an immersion mechanism 53, a draw-out mechanism 54, and a support reel 55. The storage tank 511 is capable of storing the lubricant LU containing fine bubbles. Furthermore, the die 2 is immersed in the storage tank 511.

[0097] The immersion mechanism 53 immerses the metal material W in the lubricating liquid LU in the reservoir 511 at the entry side of the die 2 before it passes through the die 2 . The immersion mechanism 53 includes, for example, direction-changing reels 531 and 532. The immersion mechanism 53 changes the traveling direction of the metallic material W unwound from the unwinding device 31 so that the metallic material W proceeds to the inlet side of the die 2 immersed in the storage tank 511. Specifically, the direction-changing reel 531 changes the traveling direction of the metallic material W unwound from the unwinding device 31 so that the metallic material W is immersed in the lubricating liquid LU in the storage tank 511 at the inlet side of the die 2. Furthermore, the direction-changing reel 532 changes the traveling direction of the metallic material W so that the central axis of the metallic material W immersed in the lubricating liquid LU becomes coaxial with the central axis of the through hole of the die 2. In a state in which the metal material W is immersed in the lubricating liquid LU in the reservoir 511 by the immersion mechanism 53 and the lubricating liquid LU is sufficiently adhered to the surface of the die 2, cold plastic working (wire drawing) is performed.

[0098] The drawing mechanism 54 draws out the metal material W that has passed through the die 2 from the lubricating liquid LU in the storage tank 511. The drawing-out mechanism 54 includes, for example, direction-changing reels 541 and 542. The drawing-out mechanism 54 changes the proceeding direction of the metal material W after passing through the die 2 so that the metal material W proceeds out of the lubricating liquid LU of the storage tank 511. Specifically, the direction-changing reel 541 changes the proceeding direction of the metal material W after passing through the die 2 at the exit side of the die 2 so that the metal material W is drawn out of the lubricating liquid LU of the storage tank 511. Furthermore, the direction-changing reel 542 changes the proceeding direction of the metal material W so that the metal material W drawn out of the lubricating liquid LU of the storage tank 511 moves toward the winding device 32. The metal material W drawn out from the lubricating liquid LU in the storage tank 511 by the drawing mechanism 54 is taken up by the winding device 32.

[0099] The support reel 55 is disposed on the inlet side and / or outlet side of the die 2, and supports the metal material W during cold plastic working. The lubricant adhesion device 5 does not necessarily have to include the support reel 55.

[0100] In the case of the cold plastic working apparatus of this example, the die 2 is immersed in the lubricating liquid LU in the storage tank 511, and further, the metal material W before passing through the die 2 is also immersed in the lubricating liquid LU in the storage tank 511 at the inlet side of the die 2. Therefore, during the wire drawing process, a sufficient amount of the lubricating liquid LU can be adhered to the surface of the through hole of the die 2 and the surface of the metal material W. Therefore, during the cold plastic working, the buffering action and aggregation action of the fine bubbles in the lubricating liquid LU can be fully utilized. As a result, the occurrence of defects in the metal wire after the cold plastic working can be more effectively suppressed.

[0101] 4 includes one die 2. However, the cold plastic processing apparatus of Fig. 4 may include a plurality of dies 2. In this case, the plurality of dies 2 are arranged so as to be immersed in the lubricating liquid LU in the storage tank 511.

[0102] [Second embodiment] In the first embodiment, a method for manufacturing a metal material in which the cold plastic working is wire drawing has been described. However, the method for manufacturing a metal material in this embodiment is also applicable to cold plastic working other than wire drawing. In the second embodiment, a method for manufacturing a metal material in which the cold plastic working is cold drawing will be described.

[0103] Fig. 5 is a schematic diagram showing an example of a cold plastic processing apparatus used in the manufacturing method of a metal material of the second embodiment. Referring to Fig. 5, the cold plastic processing apparatus includes a plastic processing tool 2, a fine bubble generator 4, and a lubricant liquid attachment device 5. The cold plastic processing apparatus shown in Fig. 5 is a cold drawing device. Each component will be described below.

[0104] In FIG. 5, the plastic processing tool 2 is a die. The cold plastic processing apparatus of FIG. 5 further includes a drawing device 3. The drawing device 3 of this example includes a chuck 36. The chuck 36 holds the tip of the metal material W. In the cold plastic processing apparatus of FIG. 5, the drawing device 3 draws the metal material W held by the chuck 36, thereby performing drawing. The cold plastic processing apparatus of FIG. 5 further includes a plug 7. The plug 7 is disposed inside the metal material W, which is a metal tube, and is fixed at a predetermined position. The plug 7 maintains a constant inner diameter of the metal material (metal tube) after cold drawing during cold drawing. The drawing device 3 and plug 7 shown in FIG. 5 are of known configuration.

[0105] The configuration of the fine bubble generator 4 of the cold plastic working apparatus in Fig. 5 is the same as the configuration of the fine bubble generator 4 shown in Fig. 1 to Fig. 4. Moreover, the configuration of the lubricating liquid adhering device 5 of the cold plastic working apparatus in Fig. 5 is the same as the configuration of the lubricating liquid adhering device 5 shown in Fig. 1.

[0106] 5 shows a cold plastic working apparatus (cold drawing apparatus) for the case where the metal material W is a metal pipe, but in the manufacturing method of this embodiment, the metal material W may be a metal bar. In this case, the plug 7 in the cold plastic working apparatus is omitted.

[0107] The manufacturing method of the metal material of this embodiment also includes the same steps as those of the first embodiment. Specifically, the lubricating liquid LU containing fine bubbles generated by the fine bubble generator 4 is applied to at least one of the surface of the metal material W and the plastic processing tool (die) 2 by using the lubricating liquid application device 5. After the lubricating liquid LU containing fine bubbles is applied, the metal material is subjected to cold plastic processing (cold drawing) by using the plastic processing tool (die) 2 to manufacture the metal material (metal bar or metal tube). In this embodiment, the [preferable average particle size D of the fine bubbles], [preferable number density ND of the fine bubbles (part 1)], and [preferable number density ND of the fine bubbles (part 2)] described in the first embodiment can also be adopted.

[0108] However, in [Preferred number density ND of fine bubbles (part 2)], the area reduction rate of the metal material W at each plastic processing tool (die) 2 in cold drawing is set to 10.0% or more and 23.5% or less. In this case, when the minimum number density N / mL defined by formula (1) is determined for each plastic processing tool (die) 2, the number density ND of the fine bubbles in the lubricating liquid LU is preferably set to be equal to or more than the maximum value of the minimum number density N / mL. N = 50 × (P / 100) × V (1) Here, the area reduction rate (%) of the plastic processing tool (die) 2 defined by equation (2) is substituted for P in equation (1), and the moving speed V (mpm) of the metal material W at the plastic processing tool (die) 2 is substituted for V. P = {(A0-A1) / A0} × 100 (2) Here, A0 in formula (2) is the cross-sectional area (mm 2 ) is substituted, and A1 is the cross-sectional area (mm 2 ) is substituted.

[0109] More specifically, the number density ND of the fine bubbles is calculated as follows. When a metal material is manufactured by performing cold plastic processing (cold drawing) using only one plastic processing tool (die) 2, the minimum number density N / mL in the cold plastic processing (die) 2 is calculated based on formulas (1) and (2). The obtained minimum number density N / mL is set as the lower limit of the preferable number density ND of the fine bubbles.

[0110] On the other hand, when a metal material is manufactured by performing cold plastic processing (cold drawing) continuously once using multiple plastic processing tools (dies) 2, the lower limit of the preferable number density ND of the fine bubbles is obtained by the following method. The minimum number density N / mL for each plastic processing tool (die) 2 is obtained based on formulas (1) and (2). The maximum value of the obtained minimum number densities N / mL is set as the lower limit of the preferable number density ND of the fine bubbles.

[0111] [Third embodiment] The manufacturing method of the metal material of this embodiment is also applicable to cold plastic working other than wire drawing and cold drawing. In the third embodiment, a manufacturing method of the metal material in the case where the cold plastic working is cold extrusion will be described.

[0112] Fig. 6 is a schematic diagram showing an example of a cold plastic processing apparatus used in the manufacturing method of a metal material of the third embodiment. Referring to Fig. 6, the cold plastic processing apparatus includes a plastic processing tool 2, a fine bubble generator 4, and a lubricant liquid attachment device 5. The plastic processing tool 2 is a die. The cold plastic processing apparatus further includes a container 70 and a stem 80. The container 70 and the stem 80 shown in Fig. 6 have well-known configurations. The cold plastic processing apparatus shown in Fig. 6 is a direct extrusion cold plastic processing apparatus. The cold plastic processing apparatus may further include a lubricant liquid recovery device 6 as shown in Fig. 6.

[0113] The configuration of the fine bubble generator 4 of the cold plastic working apparatus in Fig. 6 is the same as the configuration of the fine bubble generator 4 shown in Fig. 1 to Fig. 4. Moreover, the configuration of the lubricating liquid adhering device 5 of the cold plastic working apparatus in Fig. 6 is the same as the configuration of the lubricating liquid adhering device 5 shown in Fig. 1.

[0114] 6, the lubricant application device 5 uses the lubricant nozzle 52 to apply the lubricant LU containing fine bubbles to the surface of the metal material W before it is inserted into the container 70. The lubricant application device 5 further uses the lubricant nozzle 52 to apply the lubricant LU containing fine bubbles to the inner surface of the plastic processing tool (die) 2 before the cold extrusion process.

[0115] After a lubricating liquid LU containing fine bubbles is applied to the surface of the metal material W and the inner surface of the plastic processing tool (die) 2, the metal material W is inserted into a container 70 as shown in Fig. 7, and pressure is applied to the metal material W by a stem 80 to perform cold extrusion. In this cold plastic processing device, the metal material W is extruded in the direction in which the stem 80 advances.

[0116] In FIG. 6, the lubricant applying device 5 applies the lubricant LU containing fine bubbles to the surface of the metal material W before cold extrusion using the lubricant nozzle 52. However, the lubricant applying device 5 may have a configuration different from that of the lubricant nozzle 52. For example, the lubricant applying device 5 may include a storage tank for storing the lubricant LU containing fine bubbles. In this case, the lubricant applying device 5 immerses the metal material W before cold extrusion in the storage tank and applies the lubricant LU containing fine bubbles to the surface of the metal material W.

[0117] The cold plastic processing apparatus for performing cold extrusion is not limited to those shown in Fig. 6 and Fig. 7. Fig. 8 is a schematic diagram showing another example of a cold plastic processing apparatus for performing cold extrusion, which has a configuration different from that shown in Fig. 6. The cold plastic processing apparatus shown in Fig. 8 is an indirect extrusion cold plastic processing apparatus. The cold plastic processing apparatus of FIG. 8 includes a plastic processing tool 2, a fine bubble generator 4, and a lubricant application device 5. The plastic processing tool 2 is a die. The cold plastic processing apparatus further includes a container 70 and a stem 80. The plastic processing tool (die) 2 is attached to the end of the stem 80. The stem 80 has a through hole. The through hole of the stem 80 is arranged coaxially with the through hole of the plastic processing tool (die) 2. The cold plastic processing apparatus may further include a lubricant recovery device 6, as shown in FIG. 8.

[0118] The configuration of the fine bubble generator 4 of the cold plastic working apparatus in Fig. 8 is the same as the configuration of the fine bubble generator 4 shown in Fig. 1 to Fig. 4. Moreover, the configuration of the lubricating liquid adhering device 5 of the cold plastic working apparatus in Fig. 8 is the same as the configuration of the lubricating liquid adhering device 5 shown in Fig. 1.

[0119] In the cold plastic processing apparatus shown in Fig. 8, the lubricant application device 5 uses the lubricant nozzle 52 to apply the lubricant LU containing fine bubbles to the surface of the metal material W before it is inserted into the container 70. The lubricant application device 5 further uses the lubricant nozzle 52 to apply the lubricant LU containing fine bubbles to the inner surface of the plastic processing tool (die) 2 before the cold extrusion process. As shown in Fig. 8, the lubricant application device 5 may also use the lubricant nozzle 52 to apply the lubricant LU to the inner surface of the through-hole of the stem 80.

[0120] After the lubricating liquid LU containing fine bubbles is applied to the surface of the metal material W and the inner surface of the plastic processing tool (die) 2, the metal material W is inserted into a container 70 as shown in Fig. 9, and pressure is applied to the metal material W by a stem 80 to perform cold extrusion. In this cold plastic processing device, the metal material W is extruded in the direction opposite to the direction in which the stem 80 advances.

[0121] In the above-mentioned cold plastic processing device for cold extrusion, the lubricating liquid LU containing fine bubbles is applied to the surface of the metal material W and the inner surface of the plastic processing tool (die) 2 before cold extrusion, and then cold extrusion is performed. This makes it possible to more effectively suppress the occurrence of defects in the metal material after hot extrusion.

[0122] In this embodiment, the [preferable average particle size D of the fine bubbles], [preferable number density ND of the fine bubbles (part 1)], and [preferable number density ND of the fine bubbles (part 2)] described in the first embodiment can also be adopted.

[0123] However, in [Preferred number density ND of fine bubbles (part 2)], the area reduction rate of the metal material W at each plastic processing tool (die) 2 in cold extrusion is set to 50.0% or more and 95.0% or less. In this case, when the minimum number density N / mL defined by formula (1) is calculated for each plastic processing tool (die) 2, the number density ND of the fine bubbles in the lubricating liquid LU is preferably set to be equal to or more than the maximum value of the minimum number density N / mL. N = 50 × (P / 100) × V (1) Here, the area reduction rate (%) of the plastic processing tool (die) 2 defined by equation (2) is substituted for P in equation (1), and the moving speed V (mpm) of the metal material W at the plastic processing tool (die) 2 is substituted for V. P = {(A0-A1) / A0} × 100 (2) Here, A0 in formula (2) is the cross-sectional area (mm 2 ) is substituted, and A1 is the cross-sectional area (mm 2 ) is substituted.

[0124] More specifically, the number density ND of the fine bubbles is calculated as follows. When a metal material is manufactured by performing cold plastic processing (cold extrusion) using only one plastic processing tool (die) 2, the minimum number density N / mL in the cold plastic processing (die) 2 is calculated based on formulas (1) and (2). The obtained minimum number density N / mL is set as the lower limit of the preferable number density ND of the fine bubbles.

[0125] [Fourth embodiment] The manufacturing method of the metal material of this embodiment is also applicable to cold plastic working other than wire drawing, cold drawing, and cold extrusion. In the fourth embodiment, a manufacturing method of the metal material in the case where the cold plastic working is cold rolling will be described.

[0126] Fig. 10 is a schematic diagram showing an example of a cold plastic processing apparatus used in the manufacturing method of a metal material according to the fourth embodiment. Referring to Fig. 10, the cold plastic processing apparatus includes a plastic processing tool 2, a fine bubble generator 4, and a lubricant liquid attachment device 5. The cold plastic processing apparatus shown in Fig. 10 is a cold rolling apparatus. Each component will be described below.

[0127] In Fig. 10, the plastic processing tool 2 is a work roll. Specifically, in Fig. 10, a pair of work rolls is arranged as the plastic processing tool 2. Each of the pair of work rolls 2 is supported by a corresponding support roll 20. The configuration of the fine bubble generator 4 of the cold plastic processing apparatus in Fig. 10 is the same as the configuration of the fine bubble generator 4 shown in Figs. 1 to 4. Moreover, the configuration of the lubricating liquid application device 5 of the cold plastic processing apparatus in Fig. 10 is the same as the configuration of the lubricating liquid application device 5 shown in Fig. 1.

[0128] FIG. 10 shows a cold plastic processing apparatus (cold rolling apparatus) in the case where the metal material W is a metal plate. However, in the manufacturing method of this embodiment, the metal material W may be any one of a metal wire, a metal bar, and a metal tube. In these cases, a caliber is formed on a pair of work rolls, and a groove is formed by the pair of work rolls. In the case where the metal material W is any one of a metal wire, a metal bar, and a metal tube, the cold plastic processing apparatus may include three or more work rolls. In the case where the cold plastic processing apparatus includes three work rolls, each work roll is arranged at a pitch of 120° around the central axis of the metal material W. In this case, the groove is formed by the three work rolls. In the case where the cold plastic processing apparatus includes four work rolls, each work roll is arranged at a pitch of 90° around the central axis of the metal material W. In this case, the groove is formed by the four work rolls.

[0129] The manufacturing method of the metal material of this embodiment also includes the same steps as those of the first embodiment. Specifically, the lubricating liquid LU containing fine bubbles generated by the fine bubble generator 4 is applied to at least one of the surface of the metal material W and the plastic processing tool (work roll) 2 by using the lubricating liquid application device 5. Then, after the lubricating liquid LU containing fine bubbles is applied, the metal material W is subjected to cold plastic processing (cold rolling) by using the plastic processing tool (work roll) 2 to manufacture the metal material. In this embodiment, the [preferable average particle size D of the fine bubbles], [preferable number density ND of the fine bubbles (part 1)], and [preferable number density ND of the fine bubbles (part 2)] described in the first embodiment can also be adopted.

[0130] However, in [Preferred number density of fine bubbles ND (part 2)], the area reduction rate of the metal material W at each plastic processing tool (work roll) 2 in cold rolling is set to 50.0% or more and 95.0% or less. In this case, when the minimum number density N / mL defined by formula (1) is determined for each plastic processing tool (work roll) 2, the number density ND of the fine bubbles in the lubricating liquid LU is preferably set to be equal to or more than the maximum value of the minimum number density N / mL. N = 50 × (P / 100) × V (1) Here, the area reduction rate (%) of the plastic working tool (work roll) 2 defined by equation (2) is substituted for P in equation (1), and the moving speed V (mpm) of the metal material W at the plastic working tool (work roll) 2 is substituted for V. P = {(A0-A1) / A0} × 100 (2) Here, A0 in formula (2) is the cross-sectional area (mm 2 ) is substituted, and A1 is the cross-sectional area (mm 2 ) is substituted.

[0131] More specifically, the number density ND of the fine bubbles is calculated as follows. When a metal material is manufactured by performing cold plastic processing (cold rolling) using only one plastic processing tool (work roll) 2, the minimum number density N / mL in the cold plastic processing (work roll) 2 is calculated based on formulas (1) and (2). The obtained minimum number density N / mL is set as the lower limit of the preferable number density ND of the fine bubbles.

[0132] On the other hand, when a metal material is manufactured by continuously performing cold plastic processing (cold rolling) using multiple plastic processing tools (work rolls) 2, the lower limit of the preferable number density ND of the fine bubbles is determined by the following method. The minimum number density N / mL for each plastic processing tool (work roll) 2 is determined based on formulas (1) and (2). The maximum value of the obtained minimum number densities N / mL is set as the lower limit of the preferable number density ND of the fine bubbles. EXAMPLES

[0133] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0134] Wiredrawing was carried out using a lubricating liquid containing fine bubbles and a lubricating liquid not containing fine bubbles for the metal wires (metallic materials) with the test numbers shown in Table 1. Hereinafter, the wiredrawing process using the lubricating liquid containing fine bubbles will be referred to as "wiredrawing process A." Also, the wiredrawing process using the lubricating liquid not containing fine bubbles will be referred to as "wiredrawing process B."

[0135] [Table 1]

[0136] The "Metal Material" column in Table 1 indicates the type of metal wire used for each test number. "Al" means that the metal wire was a metal wire whose main component was aluminum. "Fe" means that the metal wire was a steel wire. "Cu" means that the metal wire was a metal wire whose main component was Cu. "Ti" means that the metal wire was a metal wire whose main component was Ti.

[0137] For each test number, in the wiredrawing process A, a wiredrawing device having the configuration shown in Fig. 4 was used. In the wiredrawing process B, a wiredrawing device having the configuration shown in Fig. 4 was used, but the fine bubble generator 4 was stopped.

[0138] The lubricating liquid in both wire drawing A and wire drawing B contained water and a surfactant. Polyoxyethylene alkyl ether (3 mass%) was used as the surfactant in both cases. The concentration of the surfactant in the lubricating liquid was the same for all test numbers, and was also the same for wire drawing A and wire drawing B for each test number.

[0139] In wire drawing process A, fine bubbles having the average particle size shown in the "Average particle size D (μm)" column of Table 1 were added to the lubricating liquid at the number density shown in the "Number density ND (pieces / mL)" column of Table 1 using a fine bubble generator 4.

[0140] In each test number, in both wire drawing A and wire drawing B, the metal wire was drawn multiple times using one or multiple dies 2 to obtain a metal wire having a diameter as shown in the "Diameter after wire drawing (μm)" column in Table 1. In each test number, the diameter d (μm) of the through hole of the final die 2 was the same as the diameter as shown in the "Diameter after wire drawing (μm)" column in Table 1. The number of dies used in each test number is shown in the "Number of dies used" column in Table 1. When wire drawing was performed multiple times, after one wire drawing was performed in the wire drawing device of FIG. 4, the die 2 was replaced and the next wire drawing was performed. The reduction in area in each die was set to 10.0% or more and less than 23.5%.

[0141] In each test number, the area reduction rate and the moving speed at each die were the same for both wire drawing A and wire drawing B. The "area reduction rate P (%) at maximum N" column and the "moving speed V (mpm) at maximum N" column in Table 1 show the area reduction rate P (%) and moving speed V (mpm) at maximum N, respectively, in the wire drawing for each test number. Here, "at maximum N" means the wire drawing at which the minimum number density N / mL, which is the maximum value among the multiple minimum number densities N / mL obtained at each die, was obtained when the minimum number density N / mL defined by formula (1) was obtained for each wire drawing with each die. In addition, the "maximum N" column shows the maximum value among the multiple minimum number densities N / mL obtained at each die.

[0142] Under the above conditions, wiredrawing A and wiredrawing B were performed for each test number. A 10m long sample was taken from the metal wire produced by each wiredrawing process. The number of defects 50μm or longer in the axial direction of the metal wire was counted on the surface of the sample. The defects were confirmed by observation at 100x magnification using an optical microscope. The defect density per meter (defects / m) was calculated based on the number of confirmed defects. For each test number, the defect density of the metal wire obtained by wiredrawing A and the defect density of the metal wire obtained by wiredrawing B were calculated. Based on the obtained defect density, the defect density ratio X was calculated using the following formula. Defect density ratio X = Defect density in wire drawing process A / Defect density in wire drawing process B The obtained flaw density ratio is shown in the "Flaw density ratio X" column of Table 1.

[0143] [Evaluation Results] Referring to Table 1, the defect density ratio was less than 1.0 for all test numbers. In other words, by performing wire drawing using a lubricating liquid containing fine bubbles, the occurrence of defects in the manufactured metal wire was suppressed compared to wire drawing using a lubricating liquid not containing fine bubbles.

[0144] In addition, the average particle size of the fine bubbles was outside the range of 0.6 dμm or less in test numbers 1, 13, 21, and 33. In addition, the number density ND of the fine bubbles was less than 50 bubbles / mL in test numbers 8, 9, 12, 20, 28, 29, 32, and 40. Therefore, in the manufacturing methods of these test numbers, the occurrence of defects in the metal wire was suppressed more than in the wire drawing process using a lubricating liquid that did not contain fine bubbles, but the defect number density ratio was higher than that of the other test numbers.

[0145] In test numbers 11, 18, 19, 31, 38 and 39, the average particle size of the fine bubbles was 0.6 dμm or less, and the number density ND of the fine bubbles was 50 bubbles / mL or more, but the number density ND of the fine bubbles was less than the maximum value of the minimum number density N. Therefore, the defect number density ratio was higher than that in test numbers 2 to 4, 7, 10, 14, 15, 22 to 24, 27, 30, 34, 35, 41 to 44, in which the average particle size of the fine bubbles was 0.6 dμm or less, the number density ND of the fine bubbles was 50 bubbles / mL or more, and the number density ND of the fine bubbles was greater than the maximum value of the minimum number density N.

[0146] In test numbers 5, 6, 16, 17, 25, 26 and 36, the average particle size of the fine bubbles was less than 1.00 μm, which means that they were ultra-fine bubbles. Therefore, the flaw density ratio was significantly lower than that of the other test numbers. EXAMPLES

[0147] Cold extrusion was carried out using a lubricating liquid containing fine bubbles and a lubricating liquid not containing fine bubbles for metal bars (metal materials) with each test number shown in Table 2. Hereinafter, the cold extrusion process using a lubricating liquid containing fine bubbles will be referred to as "cold extrusion process A." Also, the cold extrusion process using a lubricating liquid not containing fine bubbles will be referred to as "cold extrusion process B."

[0148] [Table 2]

[0149] The "Metal material" column in Table 2 indicates the type of metal bar (metal material) used for each test number. For each test number, the cold extrusion process A used a cold extrusion device with the configuration shown in Figure 6. For cold extrusion process B, the cold extrusion device with the configuration shown in Figure 6 was used, but the fine bubble generator 4 was stopped.

[0150] The lubricating liquid in both cold extrusion processing A and cold extrusion processing B contained water and a surfactant. Polyoxyethylene alkyl ether (3 mass%) was used as the surfactant in both cases. The concentration of the surfactant in the lubricating liquid was the same for all test numbers, and was also the same for cold extrusion processing A and cold extrusion processing B for each test number.

[0151] In the cold extrusion process A, a fine bubble generator 4 was used to add fine bubbles having the average particle size shown in the "Average particle size D (μm)" column of Table 1, at the number density shown in the "Number density ND (pieces / mL)" column of Table 2, to the lubricating liquid.

[0152] For each test number, in both cold extrusion process A and cold extrusion process B, cold extrusion was performed once using die 2 on the metal material (metal bar).

[0153] For each test number, the area reduction rate and the moving speed at each die were the same for both cold extrusion A and cold extrusion B. The "area reduction rate P (%) at maximum N" column and the "moving speed V (mpm) at maximum N" column in Table 2 show the area reduction rate P (%) and the moving speed V (mpm) at maximum N (in this example, the minimum number density N in one cold extrusion) in the cold extrusion for each test number.

[0154] Under the above conditions, cold extrusion A and cold extrusion B were performed for each test number to manufacture a metal bar. A sample with an axial length of 500 mm was taken from the manufactured metal bar. The number of defects with a length of 50 μm or more in the axial direction of the metal bar was counted on the surface (outer peripheral surface) of the sample. The defects were confirmed by observation at a magnification of 100 times using an optical microscope. Based on the number of confirmed defects, the defect number density per 1 m (pieces / m) was calculated. For each test number, the defect number density of the metal bar obtained by cold extrusion A and the defect number density of the metal bar obtained by cold extrusion B were calculated. Based on the obtained defect number density, the defect number density ratio X was calculated using the following formula. Defect density ratio X = Defect density in cold extrusion process A / Defect density in cold extrusion process B The obtained flaw density ratios are shown in the "Flaw density ratio X" column of Table 2.

[0155] [Evaluation Results] Referring to Table 2, the defect density ratio was less than 1.0 for all test numbers. In other words, by performing cold extrusion using a lubricating liquid containing fine bubbles, the occurrence of defects in the manufactured metal bar was suppressed compared to cold extrusion using a lubricating liquid not containing fine bubbles.

[0156] In addition, the average particle size of the fine bubbles exceeded 50.00 μm in test number 1. In addition, the number density ND of the fine bubbles was less than 50 bubbles / mL in test numbers 8, 9, 12, and 20. Therefore, in the manufacturing methods of these test numbers, the occurrence of defects in the metal bar was suppressed more than in the cold extrusion process using a lubricating liquid that did not contain fine bubbles, but the defect number density ratio was higher than that of the other test numbers.

[0157] In test numbers 11, 18, and 19, although the fine bubble number density ND was 50 bubbles / mL or more, the fine bubble number density ND was less than the maximum value of the minimum number density N. Therefore, the flaw number density ratio was higher than that of test numbers 2 to 7, 10, and 13 to 17, in which the average particle size of the fine bubbles was 50.00 μm or less, the fine bubble number density ND was 50 bubbles / mL or more, and the fine bubble number density ND was greater than the maximum value of the minimum number density N.

[0158] In test numbers 5, 6, 16, and 17, the average particle size of the fine bubbles was less than 1.00 μm, which means they were ultra-fine bubbles. Therefore, the flaw density ratio was significantly lower than that of the other test numbers. EXAMPLES

[0159] Cold rolling was carried out using a lubricant containing fine bubbles and a lubricant not containing fine bubbles for the metal plates (metal materials) with the test numbers shown in Table 3. Hereinafter, the cold rolling using a lubricant containing fine bubbles will be referred to as "cold rolling A." Also, the cold rolling using a lubricant not containing fine bubbles will be referred to as "cold rolling B."

[0160] [Table 3]

[0161] The "Metal Material" column in Table 3 indicates the type of metal plate (metal material) used for each test number. For each test number, a cold rolling device with the configuration shown in Fig. 10 was used in cold rolling A. A cold extrusion device with the configuration shown in Fig. 10 was used in cold rolling B, but the fine bubble generator 4 was stopped.

[0162] The lubricating liquid in both cold rolling A and cold rolling B contained water and a surfactant. Polyoxyethylene alkyl ether (3 mass%) was used as the surfactant in both cases. The concentration of the surfactant in the lubricating liquid was the same for all test numbers, and was also the same for cold rolling A and cold rolling B for each test number.

[0163] In cold rolling A, fine bubbles having the average particle size shown in the "Average particle size D (μm)" column of Table 3 and the number density shown in the "Number density ND (pieces / mL)" column of Table 3 were added to the lubricating liquid using a fine bubble generator 4.

[0164] For each test number, in both cold rolling A and cold rolling B, cold rolling was performed once on the metal material (metal plate) using the work roll 2.

[0165] For each test number, the area reduction rate and travel speed for each work roll were the same for both cold rolling A and cold rolling B. The "area reduction rate P (%) at maximum N" column and the "travel speed V (mpm) at maximum N" column in Table 3 show the area reduction rate P (%) and travel speed V (mpm) at maximum N (in this example, the minimum number density N in one cold rolling pass) in cold rolling for each test number.

[0166] Under the above conditions, cold rolling A and cold rolling B were performed for each test number to manufacture metal plates. A sample with a length of 500 mm in the rolling direction was taken from the manufactured metal plate. The number of defects with a length of 50 μm or more in the rolling direction of the metal plate was counted on the surface (outer peripheral surface) of the sample. The defects were confirmed by observation at a magnification of 100 times using an optical microscope. Based on the number of confirmed defects, the defect number density per 1 m (pieces / m) was calculated. For each test number, the defect number density of the metal plate obtained by cold rolling A and the defect number density of the metal plate obtained by cold rolling B were calculated. Based on the obtained defect number density, the defect number density ratio X was calculated using the following formula. Defect density ratio X = Defect density in cold rolling A / Defect density in cold rolling B The obtained flaw density ratios are shown in the “Flaw density ratio X” column of Table 3.

[0167] [Evaluation Results] Referring to Table 3, the defect density ratio was less than 1.0 for all test numbers. In other words, by performing cold rolling using a lubricating liquid containing fine bubbles, the occurrence of defects in the manufactured metal sheet was suppressed compared to cold rolling using a lubricating liquid not containing fine bubbles.

[0168] In addition, the average particle size of the fine bubbles exceeded 50.00 μm in test number 1. In addition, the number density ND of the fine bubbles was less than 50 bubbles / mL in test numbers 8, 9, and 12. Therefore, in the manufacturing methods of these test numbers, the occurrence of defects in the metal plate was suppressed more than in cold rolling using a lubricating liquid that did not contain fine bubbles, but the defect number density ratio was higher than that of the other test numbers.

[0169] In test numbers 2 to 7 and 11, although the fine bubble number density ND was 50 bubbles / mL or more, the fine bubble number density ND was less than the maximum value of the minimum number density N. Therefore, the flaw number density ratio was higher than that in test numbers 10 and 13 to 17, in which the average particle size of the fine bubbles was 50.00 μm or less, the fine bubble number density ND was 50 bubbles / mL or more, and the fine bubble number density ND was greater than the maximum value of the minimum number density N.

[0170] In test numbers 16 and 17, the average particle size of the fine bubbles was less than 1.00 μm, which meant that they were ultra-fine bubbles. Therefore, the flaw density ratio was significantly lower than that of the other test numbers.

[0171] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure. [Explanation of symbols]

[0172] 2 Dice 3 Extraction device 4 Fine bubble generator 5 Lubricating liquid deposition device 53 Immersion mechanism 54 Drawer mechanism

Claims

1. a lubricating liquid application step of applying a lubricating liquid containing fine bubbles to at least one of a surface of a plastic processing tool and a surface of a metal material; a cold plastic processing step of applying the lubricating liquid to at least one of a surface of the plastic processing tool and a surface of the metallic raw material, and then performing cold plastic processing on the metallic raw material using the plastic processing tool to manufacture a metallic material; Equipped with A method for manufacturing metal materials.

2. The method for producing a metal material according to claim 1, The average particle size of the fine bubbles is 0.01 μm or more and 50.00 μm or less. A method for manufacturing metal materials.

3. The method for producing a metal material according to claim 2, The average particle size of the fine bubbles is 0.01 μm or more and less than 1.00 μm. A method for manufacturing metal materials.

4. The method for producing a metal material according to claim 1, The metal material is mainly composed of any one of aluminum, steel, titanium, and copper. A method for manufacturing metal materials.

5. The method for producing a metal material according to claim 1, The number density of the fine bubbles in the lubricating liquid is 50 bubbles / mL or more. A method for manufacturing metal materials.

6. A method for producing a metal material according to any one of claims 1 to 5, The plastic processing tool is a die, In the cold plastic working step, Using the die, a wire drawing process is performed on the metal material to produce the metal material in the form of a metal wire. A method for manufacturing metal materials.

7. The method for producing a metal material according to claim 6, The wire drawing is performed using one or more of the dies; When the diameter of the through hole of the final die among the one or more dies is d (μm), The average particle size of the fine bubbles is 0.6 dμm or less. A method for manufacturing metal materials.

8. A method for producing a metal material according to any one of claims 1 to 5, The plastic processing tool is a die, In the cold plastic working step, Using the die, cold drawing is performed on the metal material to produce the metal material which is a metal bar or a metal tube. A method for manufacturing metal materials.

9. A method for producing a metal material according to any one of claims 1 to 5, The plastic processing tool is a die, In the cold plastic working step, Using the die, cold extrusion is performed on the metal material to produce the metal material which is a metal bar or a metal tube. A method for manufacturing metal materials.

10. A method for producing a metal material according to any one of claims 1 to 5, the plastic processing tool is a work roll, In the cold plastic working step, cold rolling the metal material using the work roll to produce the metal material, which is any one of a metal bar, a metal tube, and a metal plate; A method for manufacturing metal materials.

11. A method for producing a metal material according to any one of claims 1 to 4, In the cold plastic working step, The cold plastic working is carried out using one or more of the plastic working tools; When the plastic processing tool is a die and the cold plastic processing is wire drawing or cold drawing, the reduction in area of ​​the metal material at each of the plastic processing tools is 10.0% or more and less than 23.5%, When the plastic processing tool is a die and the cold plastic processing is cold extrusion, the reduction in area of ​​the metal material at each of the plastic processing tools is 50.0% or more and 95.0% or less; When the plastic processing tool is a work roll and the cold plastic processing is cold rolling, the reduction in area of ​​the metal material at each of the plastic processing tools is 50.0% or more and 95.0% or less; In the lubricating liquid application step, When the minimum number density N / mL defined by formula (1) is determined for each of the cold plastic working processes using each of the plastic working tools, the number density of the fine bubbles in the lubricating liquid is set to be equal to or greater than the maximum value of the minimum number density N / mL. A method for manufacturing metal materials. N=50×(P / 100)×V (1) Here, the area reduction rate (%) of the plastic processing tool defined by equation (2) is substituted for P in equation (1), and the moving speed V (mpm) of the metal material at the exit side of the plastic processing tool is substituted for V. P={(A0-A1) / A0}×100 (2) Here, A0 in the formula (2) is the cross-sectional area (mm 2 ) is substituted, and A1 is the cross-sectional area (mm 2 ) is substituted.

12. A cold plastic working apparatus capable of performing cold plastic working on a metal material, A plastic processing tool; A fine bubble generator for generating a lubricating liquid containing fine bubbles; and a lubricant applying device that applies the lubricant containing the fine bubbles to at least one of a surface of the plastic processing tool and a surface of the metal material before or during the cold plastic processing. Cold plastic processing equipment.

13. The cold plastic working apparatus according to claim 12, The lubricant applying device includes: a nozzle for discharging the lubricating liquid containing the fine bubbles onto at least one of a surface of the plastic processing tool and a surface of the metal material; A supply device that supplies the lubricating liquid containing the fine bubbles to the nozzle. Cold plastic processing equipment.

14. The cold plastic working apparatus according to claim 13, The nozzle is disposed on the inlet side of the plastic processing tool, and discharges the lubricating liquid containing the fine bubbles from the inlet side of the plastic processing tool onto at least one of the surface of the plastic processing tool and the surface of the metal material. Cold plastic processing equipment.

15. The cold plastic working apparatus according to any one of claims 12 to 14, The plastic processing tool is a die capable of performing wire drawing or cold drawing on the metal material, The cold plastic working apparatus further comprises: A drawing device is provided for drawing the metal material from the plastic processing tool. Cold plastic processing equipment.

16. The cold plastic working apparatus according to claim 15, The cold plastic processing device is capable of performing the wire drawing process on the metal material, The lubricant applying device includes: A storage tank capable of storing the lubricating liquid containing the fine bubbles; an immersion mechanism for immersing the metal material in the lubricating liquid in the reservoir at an inlet side of the die before the metal material passes through the die; The die is placed in a position in the reservoir where it is immersed in the lubricating liquid. Cold plastic processing equipment.

17. The cold plastic working apparatus according to claim 16, further comprising: a withdrawal mechanism for withdrawing the metal material from the lubricating liquid in the reservoir after passing through the die at an exit side of the die; Cold plastic processing equipment.

18. The cold plastic working apparatus according to claim 12, the plastic processing tool is a die capable of cold extrusion processing the metal material, The cold plastic working apparatus further comprises: A container for storing the metal material; a stem for pushing the metal material contained in the container out of the die; Equipped with Cold plastic processing equipment.

19. The cold plastic working apparatus according to any one of claims 12 to 14, The plastic processing tool is a work roll capable of cold rolling the metal material. Cold plastic processing equipment.

Citation Information

Patent Citations

  • Rubricant painting for metal plastic deformation

    JP1977142648A

  • Method for drawing metallic wire

    JP1995080537A

  • Method and device for manufacturing copper wire

    JP2004249293A

  • Aqueous lubricant composition and working method

    JP2009173814A

  • Industrial oil agent and manufacturing method of industrial oil agent

    JP2019203047A

Cited By

  • Processing methods

    JP7866237B1

  • Processing method

    WO2026088652A1