Electrostatically charged image development toner

A toner formulation with crystalline and amorphous polyester resins and a quaternary ammonium salt compound addresses charging stability and bending resistance issues by enhancing dispersibility and cross-linking, resulting in improved performance.

JP2024168068APending Publication Date: 2024-12-05KAO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023084463
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing toners face issues with charging stability and bending resistance of printed matter, particularly due to the poor compatibility and dispersibility of quaternary ammonium salt compounds in amorphous polyester resins.

Method used

A toner formulation containing crystalline and amorphous polyester resins with specific ester group concentrations, along with a quaternary ammonium salt compound, enhances dispersibility and cross-linking, improving charging stability and bending resistance.

Benefits of technology

The toner exhibits excellent charging stability and bending resistance of printed matter by leveraging the improved dispersibility and cross-linking effects of the resin and quaternary ammonium salt compound combination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168068000001
    Figure 2024168068000001
  • Figure 2024168068000002
    Figure 2024168068000002
  • Figure 2024168068000003
    Figure 2024168068000003
Patent Text Reader

Abstract

To provide an electrostatically charged image development toner having excellent electrification stability and bending resistance properties of printed matter.SOLUTION: In an electrostatically charged image development toner containing a crystalline polyester resin C, an amorphous polyester resin A, and a quaternary ammonium salt compound X, an ester group concentration of the crystalline polyester resin C is equal to or more than 6.5 mmol / g and equal to or less than 12.0 mmol / g, an ester group concentration of the amorphous polyester resin A is equal to or more than 7.5 mmol / g and is equal to or less than 10.5 mmol / g, and the content of the quaternary ammonium salt compound X is equal to or more than 8 pts.mass and is equal to or less than 30 pts.mass relative to a total 100 pts.mass of the crystalline polyester resin C and the amorphous polyester resin A.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner for developing electrostatic images used for developing latent images formed in electrophotography, electrostatic recording, electrostatic printing and the like. [Background technology]

[0002] It is known that a crystalline polyester resin is effective as a binder resin for a toner in improving the low-temperature fixing property of the toner, and its use in combination with an amorphous resin is being considered.

[0003] Patent Document 1 discloses a magnetic toner containing toner particles, the toner particles containing a binder resin and a magnetic powder, the binder resin containing a crystalline polyester resin and an amorphous polyester resin, and the magnetic powder being coated with a melamine resin.

[0004] Patent Document 2 discloses a binder resin for toner containing an amorphous polyester and a crystalline polyester obtained by condensation polymerization of an alcohol component containing an α,ω-aliphatic diol and a carboxylic acid component, in which the amorphous polyester is an amorphous polyester obtained by condensation polymerization of a carboxylic acid component and an alcohol component using, as raw material monomers, a carboxylic acid component containing at least a furan ring-containing carboxylic acid compound and / or an alcohol component containing an alcohol having a furan ring.

[0005] Patent Document 3 discloses a toner including a plurality of toner particles, the toner having a peak top of a molecular weight distribution measured by gel permeation chromatography in the range of 8,000 to 12,000 and a mass average molecular weight measured by gel permeation chromatography of 40,000 to 65,000, each of the plurality of toner particles containing a binder resin, the binder resin including an amorphous polyester resin containing plant-derived 1,2-propanediol as an alcohol component and a crystalline polyester resin having a melting point of 100°C to 120°C, and the content of the crystalline polyester resin in the binder resin is 10% by mass to 40% by mass.

[0006] Patent Document 4 discloses an invention relating to a positively charged toner for electrophotography, which contains, as binder resins, an amorphous polyester (A), an amorphous resin (B), and a crystalline resin (C), and, as a charge control agent, a positive charge control resin (D) containing a quaternary ammonium base-containing copolymer. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2016-197212 A [Patent Document 2] JP 2013-24985 A [Patent Document 3] JP 2015-102842 A [Patent Document 4] JP 2016-126156 A Summary of the Invention [Problem to be solved by the invention]

[0008] On the other hand, quaternary ammonium salt compounds have high positive chargeability, but they have problems with charge stability. In addition, there is a need to improve the folding resistance of printed matter.

[0009] The present invention relates to a toner for developing electrostatic images, which has excellent charge stability and excellent folding resistance of printed matter. [Means for solving the problem]

[0010] The present invention relates to a toner for developing electrostatic images, comprising a crystalline polyester resin C, an amorphous polyester resin A, and a quaternary ammonium salt compound X, wherein the ester group concentration of the crystalline polyester resin C is from 6.5 mmol / g to 12.0 mmol / g, the ester group concentration of the amorphous polyester resin A is from 7.5 mmol / g to 10.5 mmol / g, and the content of the quaternary ammonium salt compound X is from 8 parts by mass to 30 parts by mass, relative to 100 parts by mass of the total of the crystalline polyester resin C and the amorphous polyester resin A. Effect of the Invention

[0011] The toner for developing electrostatic images of the present invention exhibits excellent effects in terms of charge stability and folding resistance of printed matter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The electrostatic image developing toner of the present invention has a major feature in that it contains a crystalline polyester resin C and an amorphous polyester resin A each having a specific ester group concentration, and a quaternary ammonium salt compound X. The reason why the electrostatic image developing toner of the present invention has excellent charge stability and folding resistance of printed matter is not clear, but is presumed to be as follows.

[0013] Since the quaternary ammonium salt compound is in a cationic state, it is incompatible with the amorphous polyester resin and difficult to disperse in the amorphous polyester resin, and therefore the content in the toner is limited, which causes problems in the charging stability. In response to this, it has been found that the amount of the quaternary ammonium salt compound in the toner can be increased by using an amorphous polyester resin and a crystalline polyester resin with a high ester group concentration. This is because the dispersibility of the highly hydrophobic crystalline polyester resin in the amorphous polyester resin can be improved by using an amorphous polyester resin and a crystalline polyester resin with similar ester group concentrations, and the dispersibility of the quaternary ammonium salt compound in the amorphous polyester resin is also improved because the cationic site, the quaternary ammonium salt, easily interacts with the ester group, and the charging stability of the toner is improved by containing a large amount of the quaternary ammonium salt compound. Furthermore, the large amount of quaternary ammonium salt compound contained in the ink acts to cross-link the resins by being interposed between the ester groups, which is thought to increase the fixing strength of the toner on the printed matter and give the printed matter excellent bending resistance.

[0014] The ester group concentration of crystalline polyester resin C is 6.5 mmol / g or more, preferably 7.0 mmol / g or more, more preferably 7.5 mmol / g or more, and 12.0 mmol / g or less, preferably 11.5 mmol / g or less, more preferably 11.0 mmol / g or less, from the viewpoints of the charging stability of the toner and the folding resistance of the resulting printed matter.

[0015] In addition, from the viewpoints of the charging stability of the toner and the folding resistance of the resulting printed matter, the ester group concentration of the amorphous polyester resin A is 7.5 mmol / g or more, preferably 7.7 mmol / g or more, more preferably 8.0 mmol / g or more, and is 10.5 mmol / g or less, preferably 10.3 mmol / g or less, more preferably 10.0 mmol / g or less.

[0016] In the present invention, the ester group concentration of the polyester resin is calculated by the following formula: When the crystalline polyester resin C and / or the amorphous polyester resin A are composed of two or more resins, the weighted average calculated according to the mass ratio of each resin is regarded as the ester group concentration of the crystalline polyester resin C or the amorphous polyester resin A.

[0017]

number

[0018] (In the formula, A is the total amount (mol) of ester bonds produced when all the raw material monomers of the polyester resin are reacted, and B is the total mass (g) of the raw material monomers constituting the polyester resin. The numbers in parentheses in the formula indicate the units of each value.)

[0019] The crystallinity of a resin is represented by a crystallinity index defined as the ratio of the softening point to the maximum endothermic peak temperature measured by a differential scanning calorimeter, that is, the value of [softening point / maximum endothermic peak temperature]. The crystalline resin is a resin having a crystallinity index of 0.6 or more, preferably 0.7 or more, more preferably 0.9 or more, and 1.4 or less, preferably 1.2 or less, more preferably 1.1 or less. On the other hand, an amorphous resin is a resin in which no endothermic peak is observed, or if an endothermic peak is observed, the crystallinity index is greater than 1.4, preferably greater than 1.5, more preferably 1.6 or more, or less than 0.6, preferably 0.5 or less. The crystallinity of the resin can be adjusted by the type and ratio of the raw material monomers, and the production conditions (e.g., reaction temperature, reaction time, cooling rate), etc. The maximum endothermic peak temperature refers to the temperature of the peak with the largest peak area among the observed endothermic peaks. In the case of a crystalline resin, the maximum endothermic peak temperature is the melting point.

[0020] In the present invention, the crystalline polyester resin C is preferably a polycondensate of an alcohol component containing an aliphatic diol and a carboxylic acid component containing an aliphatic dicarboxylic acid compound.

[0021] Examples of the aliphatic diol include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,2-butanediol, 1,3-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,2-pentanediol, 1,3-pentanediol, 2,3-pentanediol, 2,4-pentanediol, 1,6-hexanediol, 1,4-butenediol, 1,3-butanediol, 1,5-pentanediol, 1,7-heptanediol, 1,8-octanediol, neopentyl glycol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol.

[0022] The aliphatic diol has 2 or more carbon atoms, and from the viewpoint of adjusting the ester group concentration, it is preferably 14 or less, more preferably 10 or less, and further preferably 8 or less.

[0023] From the viewpoint of improving the low-temperature fixing property of the toner, the aliphatic diol preferably has a hydroxyl group at the end of the carbon chain, and is more preferably an α,ω-straight-chain alkanediol.

[0024] The content of the aliphatic diol in the alcohol component is preferably 80 mol % or more, more preferably 90 mol % or more, and further preferably 95 mol % or more, and 100 mol % or less.

[0025] Examples of alcohol components other than aliphatic diols include aromatic diols such as alkylene oxide adducts of bisphenol A, bisphenol A, hydrogenated bisphenol A, sorbitol, pentaerythritol, glycerin, trimethylolpropane and other trihydric or higher alcohols.

[0026] Examples of the aliphatic dicarboxylic acid compound include succinic acid (carbon number: 4), fumaric acid (carbon number: 4), adipic acid (carbon number: 6), suberic acid (carbon number: 8), azelaic acid (carbon number: 9), sebacic acid (carbon number: 10), dodecanedioic acid (carbon number: 12), tetradecanedioic acid (carbon number: 14), succinic acid derivatives having an alkyl group or an alkenyl group on the side chain, anhydrides of these acids, and alkyl esters of these acids having a carbon number of 1 to 3. Here, when the aliphatic dicarboxylic acid compound is an alkyl ester, the carbon number of the alkyl group is not included in the above carbon number.

[0027] The carbon number of the aliphatic dicarboxylic acid compound is preferably 4 or more, and from the viewpoint of adjusting the ester group concentration, is preferably 14 or less, more preferably 12 or less.

[0028] From the viewpoint of hydrophobicity, the content of the aliphatic dicarboxylic acid compound in the carboxylic acid component is preferably 50 mol % or more, more preferably 60 mol % or more, even more preferably 70 mol % or more, and even more preferably 80 mol % or more, and is 100 mol % or less.

[0029] Examples of other carboxylic acid components include aromatic dicarboxylic acid compounds such as phthalic acid, isophthalic acid, and terephthalic acid, and trivalent or higher carboxylic acid compounds such as trimellitic acid and pyromellitic acid.

[0030] Furthermore, the alcohol component and / or the carboxylic acid component of the crystalline polyester resin C preferably contains a monofunctional monomer from the viewpoint of the charge stability of the toner.

[0031] Examples of monofunctional monomers contained in the alcohol component include aliphatic monoalcohols such as capryl alcohol, lauryl alcohol, myristyl alcohol, palmityl alcohol, stearyl alcohol, and behenyl alcohol.

[0032] From the viewpoint of hydrophobicity, the carbon number of the aliphatic monoalcohol is preferably 10 or more, more preferably 12 or more, and even more preferably 14 or more, and from the viewpoint of low-temperature fixability, the carbon number is preferably 22 or less, more preferably 20 or less, and even more preferably 18 or less.

[0033] Examples of monofunctional monomers contained in the carboxylic acid component include aliphatic monocarboxylic acids such as capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, and behenic acid, and aliphatic monocarboxylic acid compounds such as alkyl esters of these acids in which the alkyl group has 1 to 3 carbon atoms.

[0034] From the viewpoint of hydrophobicity, the carbon number of the aliphatic monocarboxylic acid compound is preferably 10 or more, more preferably 12 or more, and even more preferably 14 or more, and from the viewpoint of low-temperature fixability, it is preferably 22 or less, more preferably 20 or less, and even more preferably 18 or less. Here, when the aliphatic monocarboxylic acid compound is an alkyl ester, the carbon number of the alkyl group is not included in the above carbon number.

[0035] The content of the monofunctional monomer in the total amount of the alcohol component and the carboxylic acid component is preferably 1 mol % or more, more preferably 3 mol % or more, and even more preferably 5 mol % or more, and from the viewpoint of low-temperature fixability, it is preferably 30 mol % or less, more preferably 20 mol % or less, and even more preferably 15 mol % or less.

[0036] In this specification, macromonomers and hydroxycarboxylic acids are not included in the alcohol component and the carboxylic acid component.

[0037] The equivalent ratio of the carboxy group of the carboxylic acid component to the hydroxyl group of the alcohol component (COOH group / OH group) is preferably 0.8 or more, more preferably 0.9 or more, from the viewpoint of charging stability, and is preferably 1.2 or less, more preferably 1.1 or less, from the viewpoint of low-temperature fixing property.

[0038] The crystalline polyester resin C can be produced, for example, by polycondensing an alcohol component and a carboxylic acid component in an inert gas atmosphere, preferably in the presence of an esterification catalyst, and if necessary, in the presence of an esterification promoter, a polymerization inhibitor, etc., at a temperature of preferably 120°C or higher, more preferably 180°C or higher, and preferably 230°C or lower, more preferably 220°C or lower.

[0039] Examples of the esterification catalyst include tin compounds such as dibutyltin oxide and tin(II) 2-ethylhexanoate, and titanium compounds such as titanium diisopropoxybis(triethanolaminate). The amount of the esterification catalyst used is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and preferably 1.5 parts by mass or less, more preferably 1 part by mass or less, based on 100 parts by mass of the total amount of the alcohol component and the carboxylic acid component. Examples of the esterification promoter include gallic acid. The amount of the esterification promoter used is preferably 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, and preferably 0.5 parts by mass or less, more preferably 0.1 parts by mass or less, based on 100 parts by mass of the total amount of the alcohol component and the carboxylic acid component. Examples of the polymerization inhibitor include tert-butylcatechol. The amount of the polymerization inhibitor used is preferably 0.001 part by mass or more, more preferably 0.01 part by mass or more, and preferably 0.5 part by mass or less, more preferably 0.1 part by mass or less, per 100 parts by mass of the total amount of the alcohol component and the carboxylic acid component.

[0040] In the present invention, the polyester resin may be modified to such an extent that its properties are not substantially impaired. Examples of modified polyester resins include polyester resins grafted or blocked with phenol, urethane, epoxy, or the like by the methods described in JP-A-11-133668, JP-A-10-239903, JP-A-8-20636, etc., and among the modified polyester resins, urethane-modified polyester resins in which polyester resins are urethane-extended with a polyisocyanate compound are preferred.

[0041] The softening point of the crystalline polyester resin C is preferably 50°C or higher, more preferably 65°C or higher, and even more preferably 70°C or higher from the viewpoint of charging stability, and is preferably 140°C or lower, and more preferably 120°C or lower from the viewpoint of low-temperature fixing property.

[0042] The melting point of the crystalline polyester resin C is preferably 60° C. or higher, more preferably 70° C. or higher, from the viewpoint of charging stability, and is preferably 130° C. or lower, more preferably 120° C. or lower, from the viewpoint of low-temperature fixing ability.

[0043] The acid value of the crystalline polyester resin C is preferably 1 mgKOH / g or more, more preferably 3 mgKOH / g or more, from the viewpoint of low-temperature fixing property, and is preferably 20 mgKOH / g or less, more preferably 15 mgKOH / g or less, from the viewpoint of charging stability.

[0044] The content of crystalline polyester resin C in the total amount of crystalline polyester resin C and amorphous polyester resin A is preferably 3 mass% or more, more preferably 4 mass% or more, even more preferably 5 mass% or more, and even more preferably 8 mass% or more from the viewpoint of low-temperature fixability, and is preferably 30 mass% or less, more preferably 25 mass% or less, even more preferably 20 mass% or less, and even more preferably 15 mass% or less from the viewpoint of charging stability.

[0045] From the viewpoint of adjusting the ester group concentration, the amorphous polyester resin A is preferably a polycondensate of an alcohol component containing an aliphatic diol and a carboxylic acid component.

[0046] As the aliphatic diol, the same aliphatic diol as that for the crystalline polyester resin C can be exemplified.

[0047] The aliphatic diol has 2 or more carbon atoms, and from the viewpoint of adjusting the ester group concentration, it is preferably 10 or less, more preferably 8 or less, and further preferably 6 or less.

[0048] From the viewpoints of the charging stability of the toner and the folding resistance of the resulting printed matter, the aliphatic diol is preferably an aliphatic diol having a hydroxyl group bonded to a secondary carbon atom, such as 1,2-propanediol, 1,2-butanediol, 1,3-butanediol, 2,3-butanediol, 1,2-pentanediol, 1,3-pentanediol, 2,3-pentanediol, or 2,4-pentanediol, and more preferably 1,2-propanediol.

[0049] The content of the aliphatic diol in the alcohol component is preferably 80 mol % or more, more preferably 90 mol % or more, and 100 mol % or less.

[0050] Examples of the alcohol component other than the aliphatic diol include aromatic diols such as alkylene oxide adducts of bisphenol A, bisphenol A, and hydrogenated bisphenol A.

[0051] Examples of the carboxylic acid component include aromatic dicarboxylic acid compounds and aliphatic dicarboxylic acid compounds.

[0052] Examples of the aromatic dicarboxylic acid compound include phthalic acid, isophthalic acid, terephthalic acid, anhydrides of these acids, and alkyl esters of these acids having 1 to 3 carbon atoms.

[0053] Examples of the aliphatic dicarboxylic acid compound include fumaric acid, maleic acid, succinic acid, succinic acid derivatives substituted with a hydrocarbon group, glutaric acid, adipic acid, sebacic acid, anhydrides of these acids, and alkyl esters of these acids having 1 to 3 carbon atoms.

[0054] From the viewpoints of the charge stability of the toner and the folding resistance of the resulting printed matter, the carboxylic acid component preferably contains a succinic acid derivative substituted with a hydrocarbon group.

[0055] Specific examples of succinic acid derivatives substituted with a hydrocarbon group include dodecylsuccinic acid, dodecenylsuccinic acid, tetrapropenylsuccinic acid, decenylsuccinic acid, acid anhydrides thereof, and alkyl esters thereof having a carbon number of 1 to 3. Among these, from the viewpoint of low-temperature fixability, dodecenylsuccinic acid, tetrapropenylsuccinic acid, or acid anhydrides thereof are preferred, and dodecenylsuccinic anhydride is more preferred.

[0056] From the viewpoint of hydrophobicity, the number of carbon atoms in the hydrocarbon group in the succinic acid derivative is preferably 8 or more, more preferably 10 or more, even more preferably 12 or more, and is preferably 20 or less, more preferably 18 or less, even more preferably 16 or less.

[0057] From the viewpoint of amorphization, the content of the succinic acid derivative in the carboxylic acid component is preferably 2 mol % or more, more preferably 3 mol % or more, and even more preferably 4 mol % or more, and from the viewpoint of the folding resistance of the resulting printed matter, it is preferably 20 mol % or less, more preferably 18 mol % or less, and even more preferably 15 mol % or less.

[0058] Furthermore, the alcohol component and / or the carboxylic acid component of the amorphous polyester resin A may contain a trivalent or higher monomer from the viewpoint of adjusting the softening point.

[0059] Examples of trihydric or higher alcohols contained in the alcohol component include glycerin, trimethylolpropane, and pentaerythritol.

[0060] Examples of trivalent or higher carboxylic acid compounds contained in the carboxylic acid component include 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, pyromellitic acid, anhydrides of these acids, and alkyl esters having an alkyl group with a carbon number of 1 to 3. Of these, trimellitic acid compounds are preferred.

[0061] The content of trivalent or higher monomers in the total amount of the alcohol component and the carboxylic acid component is preferably 1 mol % or more, more preferably 3 mol % or more, and is preferably 20 mol % or less, more preferably 15 mol % or less.

[0062] The alcohol component may appropriately contain a monohydric alcohol, and the carboxylic acid component may appropriately contain a monovalent carboxylic acid compound.

[0063] From the viewpoint of adjusting the softening point of the polyester resin, the equivalent ratio of the carboxy group of the carboxylic acid component to the hydroxyl group of the alcohol component (COOH group / OH group) is preferably 0.6 or more, more preferably 0.7 or more, even more preferably 0.75 or more, and is preferably 1.2 or less, more preferably 1.15 or less.

[0064] The polycondensation reaction conditions of the alcohol component and the carboxylic acid component of the amorphous polyester resin A are the same as those of the crystalline polyester resin C, except that the suitable reaction temperature is 130°C or higher, more preferably 170°C or higher, and 250°C or lower, more preferably 240°C or lower.

[0065] The softening point of the amorphous polyester resin A is preferably 70°C or higher, more preferably 90°C or higher, and even more preferably 100°C or higher from the viewpoint of charging stability, and is preferably 170°C or lower, more preferably 160°C or lower, and even more preferably 150°C or lower from the viewpoint of low-temperature fixing ability.

[0066] From the viewpoints of low-temperature fixability and fixing width, the amorphous polyester resin A may be composed of resins having different softening points. The difference in softening point between the two resins is preferably 10° C. or more, more preferably 20° C. or more, and is preferably 60° C. or less, more preferably 40° C. or less.

[0067] The softening point of the amorphous polyester resin having a higher softening point (resin AH) is preferably 100°C or higher, more preferably 110°C or higher, and even more preferably 120°C or higher, from the viewpoint of fixing width, and is preferably 170°C or lower, more preferably 160°C or lower, and even more preferably 150°C or lower, from the viewpoint of low-temperature fixing ability.

[0068] Furthermore, the softening point of the amorphous polyester resin (resin AL) having a lower softening point is preferably 70°C or higher, more preferably 90°C or higher, and even more preferably 100°C or higher, from the viewpoint of charging stability, and is preferably 130°C or lower, more preferably 125°C or lower, and even more preferably 120°C or lower, from the viewpoint of low-temperature fixing ability.

[0069] The mass ratio of resin AH to resin AL (resin AH / resin AL) is preferably 10 / 90 or more, more preferably 20 / 80 or more, even more preferably 30 / 70 or more, and is preferably 90 / 10 or less, more preferably 80 / 20 or less, even more preferably 75 / 25 or less.

[0070] The glass transition temperature of the amorphous polyester resin A is preferably 40° C. or higher, more preferably 50° C. or higher, from the viewpoint of charging stability, and is preferably 80° C. or lower, more preferably 70° C. or lower, from the viewpoint of low-temperature fixability.

[0071] The acid value of the amorphous polyester resin A is preferably 1 mgKOH / g or more, more preferably 3 mgKOH / g or more, from the viewpoint of low-temperature fixing property, and is preferably 20 mgKOH / g or less, more preferably 18 mgKOH / g or less, from the viewpoint of charging stability.

[0072] The content of amorphous polyester resin A in the total amount of crystalline polyester resin C and amorphous polyester resin A is, from the viewpoint of charging stability, preferably 70% by mass or more, more preferably 75% by mass or more, even more preferably 80% by mass or more, and even more preferably 85% by mass or more, and from the viewpoint of low-temperature fixability, preferably 97% by mass or less, more preferably 96% by mass or less, even more preferably 95% by mass or less, and even more preferably 92% by mass or less.

[0073] The mass ratio of crystalline polyester resin C to amorphous polyester resin A (crystalline polyester resin C / amorphous polyester resin A) is, from the viewpoint of low-temperature fixability, preferably 3 / 97 or more, more preferably 4 / 96 or more, even more preferably 5 / 95 or more, and even more preferably 8 / 92 or more, and, from the viewpoint of charging stability, is preferably 30 / 70 or less, more preferably 25 / 75 or less, even more preferably 20 / 80 or less, and even more preferably 15 / 85 or less.

[0074] In the toner, the crystalline polyester resin C and the amorphous polyester resin A are contained as binder resins.

[0075] The total content of the crystalline polyester resin C and the amorphous polyester resin A in the binder resin is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 100% by mass.

[0076] The content of the binder resin in the toner is preferably 60% by mass or more, more preferably 70% by mass or more, and is preferably less than 100% by mass, more preferably 98% by mass or less, and even more preferably 95% by mass or less.

[0077] As the quaternary ammonium salt compound X, from the viewpoints of the charge stability of the toner and the folding resistance of the resulting printed matter, a quaternary ammonium salt-containing resin, which is a polymeric quaternary ammonium salt compound, is preferred, and a quaternary ammonium salt-containing styrene-based resin is more preferred.

[0078] The quaternary ammonium salt-containing styrene-based resin is not particularly limited, but is preferably, for example, a copolymer of a styrene monomer (M1) and / or a (meth)acrylic acid alkyl ester monomer (M2) and a quaternary ammonium salt of a dialkylaminoalkyl (meth)acrylate monomer (M3).

[0079] The styrene monomer (M1) is styrene, and does not include styrene derivatives such as α-methylstyrene, p-methylstyrene, and p-chlorostyrene.

[0080] Examples of the (meth)acrylic acid alkyl ester monomer (M2) include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, propyl (meth)acrylate, amyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate. The alkyl group preferably has 4 or more and 12 or less carbon atoms. Of these, butyl (meth)acrylate or 2-ethylhexyl (meth)acrylate is preferred, and butyl (meth)acrylate is more preferred.

[0081] As the quaternary ammonium salt of a dialkylaminoalkyl (meth)acrylate monomer (M3), there may be mentioned a compound represented by the formula (I):

[0082] [ka]

[0083] (In the formula, R 1 is a hydrogen atom or a methyl group, R 2 is an alkylene group having 1 to 5 carbon atoms, R 3 ~R 5 each independently represents an alkyl group having 1 to 5 carbon atoms. Preferred is a compound represented by the following formula:

[0084] In formula (I), R 1R is preferably a methyl group. 2 Examples of R include a methylene group, an ethylene group, a propylene group, and a butylene group, and among these, an ethylene group is preferred. 3 ~R 5 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an n-butyl group, a tert-butyl group, and the like. Among these, a methyl group or an ethyl group is preferred, and an ethyl group is more preferred.

[0085] Examples of dialkylaminoalkyl (meth)acrylates include dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dipropylaminoethyl (meth)acrylate, dibutylaminoethyl (meth)acrylate, and the like. Among these, diethylaminoethyl (meth)acrylate is preferred because it is inexpensive.

[0086] Examples of methods for producing a quaternary ammonium salt-containing styrene-based resin include a method in which a dialkylaminoalkyl (meth)acrylate is quaternized using a paratoluenesulfonic acid alkyl ester in a conventional manner to obtain a quaternary ammonium salt of a dialkylaminoalkyl (meth)acrylate monomer (M3), which is then mixed with a styrene monomer (M1) and / or a (meth)acrylic acid alkyl ester monomer (M2), and copolymerized in the presence of a polymerization initiator.

[0087] Examples of paratoluenesulfonic acid alkyl esters include methyl paratoluenesulfonate, ethyl paratoluenesulfonate, and propyl paratoluenesulfonate. Among these, methyl paratoluenesulfonate is preferred because it can be easily quaternized.

[0088] The amount of the paratoluenesulfonic acid alkyl ester used is preferably 0.8 mol or more, more preferably 1 mol or more, and preferably 1.5 mol or less, more preferably 1.2 mol or less, per mol of the dialkylaminoalkyl (meth)acrylate to be reacted therewith.

[0089] As the copolymerization method, any method such as solution polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. may be used. However, solution polymerization is preferred because it is relatively easy to control the mass average molecular weight of the resulting copolymer and the reaction operation is easy.

[0090] Examples of the solvent used in the solution polymerization include ketone-based solvents such as methyl ethyl ketone and methyl isobutyl ketone, alcohol-based solvents such as normal butanol and isobutanol, ester-based solvents such as ethyl acetate and isobutyl acetate, and aromatic hydrocarbon solvents such as toluene and xylene. Among these, ketone-based solvents or alcohol-based solvents are preferred from the viewpoint of the solubility of the copolymer.

[0091] As the polymerization initiator, peroxide initiators such as tert-butylperoxy-2-ethylhexanoate, tert-amylperoxy-2-ethylhexanoate, 1,1-di(tert-butylperoxy)cyclohexane, and dibenzoyl peroxide, and azo initiators such as 2,2'-azobis(2-methylbutyronitrile) can be used.

[0092] The amount of the polymerization initiator used is preferably 0.5 parts by mass or more and 10 parts by mass or less based on 100 parts by mass of the total of the monomers.

[0093] In the quaternary ammonium salt-containing styrene-based resin, the content of styrene monomer (M1) units in the total amount of styrene monomer (M1) units, (meth)acrylic acid alkyl ester monomer (M2) units, and dialkylaminoalkyl (meth)acrylate quaternary ammonium salt (M3) units is preferably 40 mass% or more, more preferably 50 mass% or more, and preferably 80 mass% or less, more preferably 75 mass% or less.

[0094] In the quaternary ammonium salt-containing styrene-based resin, the content of (meth)acrylic acid alkyl ester monomer (M2) units in the total amount of styrene monomer (M1) units, (meth)acrylic acid alkyl ester monomer (M2) units, and dialkylaminoalkyl (meth)acrylate quaternary ammonium salt (M3) units is preferably 5 mass% or more, more preferably 10 mass% or more, and is preferably 40 mass% or less, more preferably 35 mass% or less.

[0095] In the quaternary ammonium salt-containing styrene-based resin, the content of quaternary ammonium salt of dialkylaminoalkyl (meth)acrylate (M3) units in the total amount of styrene monomer (M1) units, (meth)acrylic acid alkyl ester monomer (M2) units, and quaternary ammonium salt of dialkylaminoalkyl (meth)acrylate (M3) units is preferably 0.5 mass% or more, more preferably 1 mass% or more, and is preferably 35 mass% or less, more preferably 30 mass% or less.

[0096] Commercially available products of the quaternary ammonium salt group-containing styrene-based resin include, for example, "FCA-201-PS" and "FCA-701-PT" (both manufactured by Fujikura Chemical Industries, Ltd.).

[0097] The softening point of the quaternary ammonium salt-containing styrene-based resin is preferably 140° C. or lower, more preferably 135° C. or lower, and even more preferably 130° C. or lower, from the viewpoint of improving the grindability of the toner to obtain small toner particles and from the viewpoint of low-temperature fixing property, and is preferably 90° C. or higher, more preferably 95° C. or higher, and even more preferably 100° C. or higher, from the viewpoint of storage stability.

[0098] The glass transition temperature of the quaternary ammonium salt-containing styrene-based resin is preferably 90° C. or lower, more preferably 85° C. or lower, and even more preferably 80° C. or lower, from the viewpoint of improving the grindability of the toner to obtain small toner particles and from the viewpoint of low-temperature fixability, and is preferably 35° C. or higher, more preferably 40° C. or higher, and even more preferably 45° C. or higher, from the viewpoint of storage stability.

[0099] Other quaternary ammonium salt compounds X include, for example, compounds of the formula (II):

[0100] [ka]

[0101] (In the formula, R 6 ~R 8 each independently represents an alkyl group having 1 to 5 carbon atoms; R 9 represents an alkylene group having 1 to 5 carbon atoms. Examples of commercially available quaternary ammonium salt compounds represented by formula (II) include "Bontron P-51" (manufactured by Orient Chemical Industries, Ltd., R 6 ~R 8 : butyl group, R 9 : methylene group).

[0102] The content of the quaternary ammonium salt compound X is, relative to 100 parts by mass in total of the crystalline polyester resin C and the amorphous polyester resin A, 8 parts by mass or more, preferably 10 parts by mass or more, and more preferably 12 parts by mass or more, from the viewpoint of the charging stability of the toner and the folding resistance of the obtained printed matter, and is 30 parts by mass or less, preferably 25 parts by mass or less, and more preferably 18 parts by mass or less, from the viewpoint of dispersibility in the binder resin.

[0103] The toner of the present invention may contain other charge control agents within the range that does not impair the effects of the present invention.

[0104] The toner of the present invention may contain additives such as a colorant, a release agent, a charge control agent, a magnetic powder, a flowability improver, a conductivity adjuster, a reinforcing filler such as a fibrous substance, an antioxidant, and a cleaning property improver, in addition to the binder resin and the quaternary ammonium salt compound X.

[0105] As the colorant, dyes, pigments, magnetic materials, etc. used as colorants for toners can be used. For example, carbon black, phthalocyanine blue, permanent brown FG, brilliant fast scarlet, pigment red 122, pigment green B, rhodamine-B base, solvent red 49, solvent red 146, solvent blue 35, quinacridone, carmine 6B, isoindoline, disazo yellow, etc. can be mentioned. In the present invention, the toner may be either a black toner or a color toner.

[0106] From the viewpoint of improving the image density and low-temperature fixability of the toner, the content of the colorant is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and preferably 40 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less, relative to 100 parts by mass of the binder resin.

[0107] Examples of the release agent include hydrocarbon waxes such as polypropylene wax, polyethylene wax, polypropylene-polyethylene copolymer wax, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax, and oxides thereof; ester waxes such as carnauba wax, montan wax, and deacidified waxes thereof, and fatty acid ester wax; fatty acid amides, fatty acids, higher alcohols, and fatty acid metal salts. These may be used alone or in combination of two or more.

[0108] The melting point of the release agent is preferably 60° C. or higher, more preferably 70° C. or higher, from the viewpoint of charging stability, and is preferably 160° C. or lower, more preferably 140° C. or lower, even more preferably 120° C. or lower, and even more preferably 110° C. or lower, from the viewpoint of low-temperature fixing ability.

[0109] The content of the release agent is, from the viewpoint of the low-temperature fixing property and charging stability of the toner and the viewpoint of dispersibility in the binder resin, preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 1.5 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 7 parts by mass or less, relative to 100 parts by mass of the binder resin.

[0110] The toner may be a toner obtained by any conventionally known method such as a melt kneading method, an emulsion aggregation method, or a suspension polymerization method, and may also be a toner having a core-shell structure, but from the viewpoint of charge stability, a pulverized toner by a melt kneading method is preferred. In the case of a pulverized toner by a melt kneading method, for example, a binder resin containing a crystalline polyester resin C and an amorphous polyester resin A, a quaternary ammonium salt compound X, and, if necessary, raw materials such as a colorant, a release agent, and a charge control agent are uniformly mixed in a mixer such as a Henschel mixer, and then melt kneaded in an internal kneader, a single-screw or twin-screw extruder, an open roll type kneader, or the like, and cooled, pulverized, and classified to produce the toner.

[0111] In the toner of the present invention, it is preferable to use an external additive in order to improve transferability. Examples of the external additive include inorganic fine particles such as silica, alumina, titania, zirconia, tin oxide, and zinc oxide, and organic fine particles such as melamine resin fine particles and polytetrafluoroethylene resin fine particles, and two or more of them may be used in combination. Among these, silica is preferable, and from the viewpoint of the transferability of the toner, hydrophobic silica that has been hydrophobized is more preferable.

[0112] Examples of hydrophobic treatment agents for hydrophobizing the surface of silica particles include hexamethyldisilazane (HMDS), dimethyldichlorosilane (DMDS), cyclic silazane, silicone oil, aminosilane, octyltriethoxysilane (OTES), and methyltriethoxysilane.

[0113] From the viewpoints of the chargeability, fluidity, and transferability of the toner, the average particle size of the external additive is preferably 5 nm or more, more preferably 10 nm or more, and even more preferably 15 nm or more, and is preferably 250 nm or less, more preferably 200 nm or less, and even more preferably 90 nm or less.

[0114] The external addition treatment by mixing the toner particles with the external additives can be carried out according to a conventional method, and a mixer such as a Henschel mixer can be used.

[0115] From the viewpoint of the electrostatic chargeability, fluidity, and transferability of the toner, the content of the external additive is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.3 parts by mass or more, relative to 100 parts by mass of the toner particles before being treated with the external additive, and is preferably 5 parts by mass or less, and more preferably 3 parts by mass or less.

[0116] The volume median particle size (D 50 ) is preferably 3 μm or more, more preferably 4 μm or more, and is preferably 15 μm or less, more preferably 10 μm or less. 50 ) refers to the particle size at which the cumulative volume frequency calculated by volume fraction is 50% calculated from the smallest particle size. In addition, when the toner is treated with an external additive, the volume median particle size of the toner particles before treatment with the external additive is regarded as the volume median particle size of the toner.

[0117] The toner of the present invention can be used as it is as a toner for one-component development, or as a toner for two-component development mixed with a carrier, in an image forming apparatus of a one-component development system or a two-component development system, respectively. EXAMPLES

[0118] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Physical properties of resins and the like can be measured by the following methods.

[0119] [Softening point of resin] Using a flow tester "CFT-500D" (Shimadzu Corporation), 1g of sample is heated at a temperature increase rate of 6℃ / min while applying a load of 1.96MPa with the plunger, and extruding the sample from a nozzle with a diameter of 1mm and a length of 1mm. The amount of plunger descent of the flow tester is plotted against the temperature, and the temperature at which half of the sample has flowed out is taken as the softening point.

[0120] [Maximum endothermic peak temperature of resin] Using a differential scanning calorimeter "Q-100" (manufactured by TA Instruments Japan, Inc.), weigh 0.01 to 0.02 g of sample into an aluminum pan, cool from room temperature (25°C) to 0°C at a rate of 10°C / min, and maintain at 0°C for 1 minute. Then, measure at a rate of 10°C / min. The temperature of the peak with the largest peak area among the observed endothermic peaks is regarded as the maximum endothermic peak temperature. For crystalline resins, the maximum endothermic peak temperature is regarded as the melting point.

[0121] [Glass transition temperature of amorphous resin] Using a differential scanning calorimeter "Q-100" (manufactured by TA Instruments Japan Co., Ltd.), 0.01 to 0.02 g of sample is weighed into an aluminum pan, heated to 200°C, and cooled from that temperature to 0°C at a rate of 10°C / min. The sample is then heated at a rate of 10°C / min and the endothermic peak is measured. The glass transition temperature is the temperature at the intersection of the extension of the baseline below the maximum endothermic peak temperature and the tangent line showing the maximum slope from the rising part of the peak to the top of the peak.

[0122] [Acid value of resin] Measurements are performed based on the method of JIS K 0070:1992, except that the measurement solvent is changed from the ethanol and ether mixture specified in JIS K 0070 to a mixture of acetone and toluene (acetone:toluene = 1:1 (volume ratio)) for amorphous resins, and a mixture of chloroform and dimethylformamide (chloroform:dimethylformamide = 7:3 (volume ratio)) for crystalline resins.

[0123] [Melting point of release agent] Using a differential scanning calorimeter "Q100" (manufactured by TA Instruments Japan, Inc.), 0.02 g of sample is weighed into an aluminum pan, heated to 200°C, and then cooled from 200°C to 0°C at a rate of 10°C / min. The sample is then heated at a rate of 10°C / min, the amount of heat is measured, and the maximum endothermic peak temperature is taken as the melting point.

[0124] [Volume Median Particle Size and CV Value of Resin Particles, Quaternary Ammonium Salt Compound Particles, Colorant Particles, and Release Agent Particles] (1) Measuring device: Laser diffraction type particle size measuring device "LA-920" (manufactured by Horiba, Ltd.) (2) Measurement conditions: Put the sample dispersion in a measurement cell, add distilled water, and measure the volume median particle size (D 50 ) and the volume average particle size are measured. The CV value is calculated according to the following formula. CV value (%) = (Standard deviation of particle size distribution / Volume average particle size) x 100

[0125] [Solid Content Concentration of Resin Particle Dispersion, Quaternary Ammonium Salt Compound Dispersion, Colorant Particle Dispersion, and Release Agent Particle Dispersion] Using an infrared moisture meter "FD-230" (Kett Electric Laboratory Co., Ltd.), 5 g of the measurement sample is dried at a drying temperature of 150°C and measurement mode 96 (monitoring time 2.5 minutes, fluctuation range 0.05%), and the moisture content (mass%) of the dispersion is measured. The solid content concentration is calculated according to the following formula. Solid concentration (mass%) = 100-moisture (mass%)

[0126] [Volume Median Particle Size of Agglomerated Particles] Measuring instrument: "Coulter Multisizer (registered trademark) III" (manufactured by Beckman Coulter, Inc.) Aperture diameter: 50μm Analysis software: "Multisizer (registered trademark) III version 3.51" (Beckman Coulter, Inc.) Electrolyte: "Isoton (registered trademark) II" (manufactured by Beckman Coulter, Inc.) Measurement conditions: The sample dispersion is added to 100 mL of the electrolyte to adjust the concentration so that the particle size of 30,000 particles can be measured in 20 seconds. Then, 30,000 particles are measured and the volume median particle size (D 50 ) is required.

[0127] [Average particle size of external additives] The average particle size refers to the number-average particle size, and is calculated by measuring the particle sizes (average of major and minor diameters) of 500 particles in a scanning electron microscope (SEM) photograph and averaging these by number.

[0128] [Volume median particle size of toner (D 50 )〕 Measuring instrument: "Coulter Multisizer (registered trademark) III" (manufactured by Beckman Coulter, Inc.) Aperture diameter: 50μm Analysis software: "Multisizer (registered trademark) III version 3.51" (Beckman Coulter, Inc.) Electrolyte: "Isoton (registered trademark) II" (manufactured by Beckman Coulter, Inc.) Dispersion liquid: Polyoxyethylene lauryl ether "Emulgen (registered trademark) 109P" (manufactured by Kao Corporation, HLB (Griffin) = 13.6) was dissolved in the electrolyte to adjust the concentration to 5% by mass. Dispersion conditions: 10 mg of the measurement sample is added to 5 mL of the dispersion liquid, and dispersed for 1 minute using an ultrasonic disperser (machine name: US-1, manufactured by SND Co., Ltd., output: 80 W). Then, 25 mL of electrolyte is added, and the mixture is further dispersed for 1 minute using the ultrasonic disperser to prepare a sample dispersion liquid. Measurement conditions: The sample dispersion was added to 100 mL of the electrolyte to adjust the concentration so that the particle size of 30,000 particles could be measured in 20 seconds. Then, 30,000 particles were measured, and the volume median particle size (D 50 ) is required.

[0129] [Toner Circularity] The circularity of the toner particles is measured under the following conditions. Measurement equipment: Flow-type particle image analyzer "FPIA-3000" (Sysmex Corporation) Preparation of dispersion: A dispersion of toner particles is prepared by diluting it with deionized water so that the solid content concentration becomes 0.001 to 0.05% by mass. Measurement mode: HPF measurement mode

[0130] Preparation of alkenyl succinic anhydride 1 (1) Propylene tetramer (manufactured by Nippon Oil Corporation, product name: "Light Tetramer") was used and fractionated under heating conditions of 183 to 208°C to obtain an alkylene compound (a). The obtained alkylene compound (a) had 40 peaks in gas chromatography mass spectrometry described below. The distribution of the alkylene compounds was measured according to the analysis of alkylene compound A by mass spectrometry gas chromatography in JP 2014-013384 A, and the C9H 18 :0.5% by mass, C 10 H 20 :4% by mass, C 11 H 22 :20% by mass, C 12 H 24 :66% by mass, C 13 H 26 :9% by mass, C 14 H 28 : 0.5% by mass (6 peaks corresponding to alkylene compounds having 9 to 14 carbon atoms).

[0131] (2) 542.4 g of alkylene compound (a), 157.2 g of maleic anhydride, 0.4 g of antioxidant "Chelex-O" (SC Organic Chemical Co., Ltd., Triisooctyl phosphite), and 0.1 g of butyl hydroquinone as a polymerization inhibitor were charged into a 1 L autoclave manufactured by Nitto Koatsu Co., Ltd., and pressurized nitrogen replacement (0.2 MPaG) was repeated three times. After stirring was started at 60 ° C, the temperature was raised to 230 ° C over 1 hour and the reaction was carried out for 6 hours. The pressure when the reaction temperature was reached was 0.3 MPaG. After the reaction was completed, the mixture was cooled to 80 ° C, returned to normal pressure (101.3 kPa), and transferred to a 1 L four-neck flask. The mixture was heated to 180 ° C with stirring, and the remaining alkylene compound was distilled off at 1.3 kPa for 1 hour. Subsequently, the mixture was cooled to room temperature (25° C.) and then returned to normal pressure (101.3 kPa) to obtain 406.1 g of the target product, alkenyl succinic anhydride A. The average molecular weight of alkenyl succinic anhydride A calculated from the acid value was 268.

[0132] Resin manufacturing example 1 The alcohol component, carboxylic acid component, esterification catalyst, and esterification promoter shown in Tables 1 and 2 were placed in a 5-liter four-neck flask equipped with a nitrogen inlet tube, a dehydration tube equipped with a fractionating tube through which hot water of 98°C was passed, a stirrer, and a thermocouple, and the mixture was kept at 180°C for 1 hour under a nitrogen atmosphere, and then heated from 180°C to 235°C at a rate of 10°C / h, and then polycondensed at 235°C for 5 hours. The reaction was further carried out at 235°C under a reduced pressure of 10 kPa until the softening points shown in Tables 1 and 2 were reached, to obtain amorphous polyester resins (resins AH1 to AH4, AH6 to AH7, and AL1 to AL5). The physical properties are shown in Tables 1 and 2.

[0133] Resin manufacturing example 2 The alcohol component, carboxylic acid component other than trimellitic anhydride, esterification catalyst, and esterification promoter shown in Table 2 were placed in a 5-liter four-neck flask equipped with a nitrogen inlet tube, a dehydration tube equipped with a fractionating tube through which hot water of 98 ° C. was passed, a stirrer, and a thermocouple, and the mixture was kept at 180 ° C. for 1 hour under a nitrogen atmosphere, and then heated from 180 ° C. to 235 ° C. at a rate of 10 ° C. / h, and then polycondensed at 235 ° C. for 5 hours. The temperature was then lowered to 210 ° C., and trimellitic anhydride shown in Table 2 was added, and the mixture was reacted at 210 ° C. for 1 hour, and then the reaction was continued at 210 ° C. under a reduced pressure of 10 kPa until the softening point shown in Table 2 was reached, to obtain an amorphous polyester resin (resin AH5). The physical properties are shown in Table 2.

[0134] [Table 1]

[0135] [Table 2]

[0136] Resin manufacturing example 3 The alcohol component and carboxylic acid component shown in Table 3 were placed in a 5-liter four-neck flask equipped with a thermometer, a stainless steel stirring rod, a downflow condenser, and a nitrogen inlet tube, and the temperature was raised to 200°C over 8 hours in a nitrogen atmosphere in a mantle heater. Then, an esterification catalyst shown in Table 3 was added, and the reaction was carried out at 8.0 kPa until the softening point shown in Table 3 was reached, obtaining crystalline polyester resins (resins C1 to C4, C7 to C8). The physical properties are shown in Table 3.

[0137] Resin manufacturing example 4 The alcohol component, carboxylic acid component, and polymerization inhibitor shown in Table 3 were placed in a 5-liter four-neck flask equipped with a thermometer, a stainless steel stirring rod, a downflow condenser, and a nitrogen inlet tube, and the temperature was raised to 200°C over 8 hours in a nitrogen atmosphere in a mantle heater. Then, the esterification catalyst shown in Table 3 was added, and the reaction was carried out at 8.0 kPa until the softening point shown in Table 3 was reached, obtaining crystalline polyester resins (resins C5 to C6). The physical properties are shown in Table 3.

[0138] [Table 3]

[0139] Example 1, Examples 4 to 11, 13 to 17, Comparative Examples 1 and 2 [Melt-kneading method] 100 parts by mass of the binder resin shown in Table 4, 5 parts by mass of a colorant "ECB-301" (manufactured by Dainichi Seikagaku Co., Ltd., phthalocyanine blue (PB15:3)), 3 parts by mass of a release agent "Carnauba Wax C1" (manufactured by Kato Yoko Co., Ltd., melting point: 83°C), 3 parts by mass of a release agent "HNP-9" (manufactured by Nippon Seiro Co., Ltd., paraffin wax, melting point: 75°C), and 15 parts by mass of a positively charged charge control agent "FCA-201-PS" (manufactured by Fujikura Kasei Co., Ltd., softening point: 119°C, glass transition temperature: 65°C), which is a quaternary ammonium salt-containing styrene-based resin, were mixed in a Henschel mixer.

[0140] The obtained mixture was melt-kneaded using a co-rotating twin screw extruder with a kneading section total length of 1560 mm, a screw diameter of 42 mm, and a barrel inner diameter of 43 mm at a screw rotation speed of 200 r / min and a barrel set temperature of 100° C. to obtain a melt-kneaded product. The mixture was fed at a rate of 20 kg / h and the average residence time was about 18 seconds.

[0141] The resulting molten mixture was cooled, coarsely crushed, and then pulverized in a jet mill. The pulverized mixture was classified using an air classifier (manufactured by Nippon Pneumatic Mfg. Co., Ltd.) to obtain the volume median particle size (D 50 ) yielded 7.0 μm toner particles.

[0142] 100 parts by mass of the obtained toner particles and 0.5 parts by mass of hydrophobic silica "TG820F" (manufactured by Cabot Corporation, hydrophobic treatment agent: HMDS and cyclic silazane, average particle diameter 8 nm) and 1.0 part by mass of hydrophobic silica "NA50Y" (manufactured by Nippon Aerosil Co., Ltd., hydrophobic treatment agent: silicone oil and aminosilane, average particle diameter 40 nm) as external additives were mixed in a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 3000 r / min (circumferential speed 32 m / sec) for 3 minutes to obtain a toner.

[0143] Examples 2 and 3, Comparative Example 3 A toner was obtained in the same manner as in Example 1, except that the amount of the positively charged charge control agent ("FCA-201-PS") used was changed to the number of parts shown in Table 4.

[0144] Example 12 A toner was obtained in the same manner as in Example 1, except that 15 parts by mass of "BONTRON P-51" (manufactured by Orient Chemical Industries Co., Ltd.) was used instead of "FCA-201-PS" as the positively charged charge control agent.

[0145] Example 18 A toner was obtained in the same manner as in Example 1, except that the melt-kneading was performed using a continuous open-roll type twin-screw kneader "Kneedex" (manufactured by Mitsui Mining Co., Ltd.) instead of the same-rotation twin-screw extruder. The continuous open-roll type twin-screw kneader had a roll outer diameter of 0.14 m and an effective roll length of 0.8 m, and the operating conditions were a rotation speed of the high-rotation roll (front roll) of 75 r / min (circumferential speed 33 m / min), a rotation speed of the low-rotation roll (rear roll) of 50 r / min (circumferential speed 22 m / min), and a roll gap of 0.1 mm. The heating and cooling medium temperatures in the rolls were set to 140°C on the raw material input side of the high-rotation roll and 110°C on the kneaded material discharge side, and 65°C on the raw material input side of the low-rotation roll and 30°C on the kneaded material discharge side. The feed rate of the raw material mixture was 10 kg / h, and the average residence time was about 5 minutes.

[0146] Example 19 [Emulsion aggregation method] <Preparation of aqueous dispersion of core resin particles> 600g of methyl ethyl ketone was put into a 5-liter container equipped with a stirrer, reflux condenser, dropping funnel, thermometer and nitrogen inlet tube, and 128g of resin AL1 and 22g of resin C1 were added at 60°C and dissolved. 5% by mass of sodium hydroxide aqueous solution was added to the obtained solution so that the degree of neutralization was 60 mol% with respect to the acid value of the resin, and the mixture was stirred for 30 minutes to obtain a mixture. Then, 675g of deionized water was added over 77 minutes. Next, while stirring at 250r / min, methyl ethyl ketone and a part of the water were distilled off at a temperature of 50°C or less under reduced pressure, and the solid content concentration of the aqueous dispersion was measured, and the solid content concentration of the aqueous dispersion was adjusted to 20% by mass with deionized water to obtain a core resin dispersion. The volume median particle size (D 50 ) was 200 nm and the CV value was 24%.

[0147] <Preparation of Aqueous Dispersion of Shell Resin Particles> 600g of methyl ethyl ketone was put into a 5-liter container equipped with a stirrer, reflux condenser, dropping funnel, thermometer and nitrogen inlet tube, and 150g of resin AH1 was added at 60°C and dissolved. 5% by mass of sodium hydroxide aqueous solution was added to the obtained solution so that the degree of neutralization was 60 mol% with respect to the acid value of the resin, and the mixture was stirred for 30 minutes to obtain a mixture. Then, 675g of deionized water was added over 77 minutes. Next, while stirring at 250r / min, methyl ethyl ketone and a part of the water were distilled off at a temperature of 50°C or less under reduced pressure, and the solid content concentration of the aqueous dispersion was measured, and the solid content concentration of the aqueous dispersion was adjusted to 20% by mass with deionized water to obtain a shell resin dispersion. The volume median particle size (D 50 ) was 110 nm and the CV value was 20%.

[0148] <Preparation of Quaternary Ammonium Salt Compound Dispersion> In a 1-liter beaker, 100.0 g of a positively charged charge control agent "FCA-201-PS" (manufactured by Fujikura Chemical Industries, Ltd.), which is a styrene-based resin containing a quaternary ammonium salt, 133.3 g of an anionic surfactant "Neopelex (registered trademark) G-15" (manufactured by Kao Corporation, 15% by mass sodium dodecylbenzenesulfonate aqueous solution), and 268.5 g of deionized water were mixed, and dispersed at room temperature for 1 hour at a rotation speed of 8000 r / min of the stirring blade using a homogenizer "TKAGI HOMOMIXER 2M-03" (manufactured by Primix Corporation). Then, 12 passes were performed at a pressure of 150 MPa using a homogenizer "Microfluidizer M-110EH" (manufactured by Microfluidics Corporation). Then, the mixture was passed through a 200-mesh filter, and deionized water was added so that the solid concentration was 12% by mass, to obtain a quaternary ammonium salt compound dispersion. The volume median particle size (D 50 ) was 150 nm and the CV value was 30%.

[0149] <Preparation of Colorant Dispersion> In a 1-liter beaker, 116.2 g of copper phthalocyanine pigment "ECB-301" (Dainichi Seikagaku Chemical Industry Co., Ltd., phthalocyanine blue (PB15:3)), 154.9 g of anionic surfactant "Neopelex (registered trademark) G-15" (Kao Corporation, 15% by mass sodium dodecylbenzenesulfonate aqueous solution) and 340 g of deionized water were mixed and dispersed using a homogenizer at room temperature for 3 hours, and then deionized water was added so that the solids concentration became 24% by mass, thereby obtaining a colorant dispersion containing colorant particles. The volume median particle diameter (D 50 ) was 118 nm and the CV value was 27%.

[0150] <Preparation of release agent dispersion> 50 g of paraffin wax (manufactured by Nippon Seiro Co., Ltd., trade name: HNP090, melting point: 85° C.), 5 g of a cationic surfactant (manufactured by Kao Corporation, trade name: Sanisol B50) and 200 g of deionized water were heated to 95° C., and the paraffin wax was dispersed using a homogenizer, followed by a dispersion treatment using a pressure discharge homogenizer to obtain a release agent dispersion liquid containing release agent particles with a solid content concentration of 20 mass %. The volume median particle diameter (D 50 ) was 550 nm and the CV value was 26%.

[0151] <Preparation of Toner Particles> In a 3-liter four-neck flask equipped with a dehydration tube, a stirrer, and a thermocouple, 500 g of the core resin dispersion, 180 g of the quaternary ammonium salt compound dispersion, 63 g of the colorant dispersion, 49 g of the release agent dispersion, and 3.3 g of a 15% by mass aqueous solution of sodium dodecylbenzenesulfonate "Neopelex G-15" (manufactured by Kao Corporation, an anionic surfactant) were mixed at a temperature of 25° C. Next, while stirring the resulting mixture, a solution obtained by dissolving 40 g of ammonium sulfate in 570 g of deionized water and adding a 4.8% by mass aqueous solution of potassium hydroxide to adjust the pH to 8.2 was added dropwise over 10 minutes at 25° C., and the temperature was then raised to 62° C. over 2 hours to measure the volume median particle diameter (D 50 The temperature was maintained at 62° C. until the particle size reached 6.9 μm, thereby obtaining a dispersion of aggregated particles (I).

[0152] While maintaining the temperature of the obtained dispersion of aggregated particles (I) at 62° C., 215 g of the shell resin dispersion was added dropwise at a rate of 0.6 mL / min (0.6 g / min) to obtain a dispersion of aggregated particles (II). 50 ) was 7.0 μm.

[0153] To the dispersion of the obtained aggregated particles (II), an aqueous solution of 20 g of sodium polyoxyethylene lauryl ether sulfate "EMAL E-27C" (Kao Corporation, anionic surfactant, effective concentration 27% by mass), 280 g of deionized water, and 40 g of 0.1 mol / L aqueous sulfuric acid solution was added. The temperature was then raised to 80°C over 1 hour, and the mixture was kept at 80°C for 30 minutes, after which 10 g of 0.1 mol / L aqueous sulfuric acid solution was added and the mixture was kept at 80°C for another 15 minutes. Thereafter, 15 g of 0.1 mol / L aqueous sulfuric acid solution was added again, and the mixture was kept at 80°C until the circularity reached 0.970, thereby obtaining a dispersion of fused particles (core-shell particles) in which the aggregated particles were fused.

[0154] The obtained core-shell particle dispersion was cooled to 30°C, and the dispersion was filtered under suction to separate the solid content, which was then washed with deionized water at 25°C and filtered under suction for 2 hours at 25°C. The solid content was then vacuum dried at 33°C for 24 hours using a vacuum constant temperature dryer "DRV622DA" (manufactured by ADVANTEC Corporation) to obtain toner particles. The particle size of the obtained toner particles was 7.0 μm and the circularity was 0.970. The composition ratio (mass ratio) of the binder resin of the obtained toner particles was resin AH1 / resin AL1 / resin C1=30 / 60 / 10.

[0155] 100 parts by mass of the obtained toner particles and 0.5 parts by mass of hydrophobic silica "TG820F" (manufactured by Cabot Corporation, hydrophobic treatment agent: HMDS and cyclic silazane, average particle diameter 8 nm) and 1.0 part by mass of hydrophobic silica "NA50Y" (manufactured by Nippon Aerosil Co., Ltd., hydrophobic treatment agent: silicone oil and aminosilane, average particle diameter 40 nm) as external additives were mixed in a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 3000 r / min (circumferential speed 32 m / sec) for 3 minutes to obtain a toner.

[0156] Test Example 1 [Charging Stability of Toner] Under high temperature and humidity conditions of 25°C and 50%, 0.6 g of toner and 19.4 g of silicone ferrite carrier (Kanto Denka Kogyo Co., Ltd., average particle size 90 μm) were placed in a 50 mL polyethylene container and mixed at 250 rpm using a ball mill. The charge amount of the toner was measured using a Q / M meter (EPPING) according to the following method.

[0157] After 60 or 600 seconds of mixing, a specified amount of toner and carrier mixture was put into a cell attached to the Q / M meter, and only the toner was sucked through a 32 μm mesh sieve (stainless steel, twill weave, wire diameter: 0.0035 mm) for 90 seconds. The voltage change on the carrier that occurred at that time was monitored, and the value of [total amount of electricity after 90 seconds (μC) / amount of sucked toner (g)] was taken as the charge amount (μC / g). The ratio of the charge amount after 60 seconds of mixing to the charge amount after 600 seconds of mixing (charge amount after 60 seconds of mixing / charge amount after 600 seconds of mixing) was calculated to evaluate the charge stability. The results are shown in Table 4. The higher the value, the better the charge stability.

[0158] Test Example 2 [Bending resistance] The toner was mounted on a copy machine "AR-505" (manufactured by Sharp Corporation) whose fixing unit was modified to enable fixing outside the machine, and a printout was obtained in an unfixed state (print area: 20 cm × 20 cm, adhesion amount: 0.5 mg / cm 2 Then, the image was fixed by adjusting the temperature of the fixing roll to 160°C using a fixing machine (fixing speed 300mm / sec) adjusted to a total fixing pressure of 40kgf. 2 The print was folded inward for 30 seconds at 100° C., reopened, and the damaged image was wiped off with a soft cloth. The maximum width of the image defect after this was used as an index of the folding resistance of the print. The results are shown in Table 4. The smaller the maximum width of the image defect, the better the folding resistance of the print. The fixing paper used was "CopyBond SF-70NA" (manufactured by Sharp Corporation, 75 g / m 2 ) was used.

[0159] [Table 4]

[0160] From the above results, it can be seen that the toners of Examples 1 to 19 have good charge stability and folding resistance of printed matter, compared to Comparative Examples 1 and 2 containing amorphous polyester resins or crystalline polyester resins with low ester group concentrations, and Comparative Example 3 containing a small amount of quaternary ammonium salt compound. In particular, a comparison between Example 1 and Example 12 shows that a higher effect can be obtained by including a polymer type quaternary ammonium salt compound. [Industrial Applicability]

[0161] The toner for developing electrostatic images of the present invention is suitably used for developing latent images formed in electrophotography, electrostatic recording, electrostatic printing and the like.

Claims

1. 1. A toner for developing electrostatic images, comprising a crystalline polyester resin C, an amorphous polyester resin A, and a quaternary ammonium salt compound X, wherein the crystalline polyester resin C has an ester group concentration of 6.5 mmol / g or more and 12.0 mmol / g or less, the amorphous polyester resin A has an ester group concentration of 7.5 mmol / g or more and 10.5 mmol / g or less, and the content of the quaternary ammonium salt compound X is 8 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the total of the crystalline polyester resin C and the amorphous polyester resin A.

2. 2. The toner for developing electrostatic images according to claim 1, wherein a mass ratio of the crystalline polyester resin C to the amorphous polyester resin A is 3 / 97 or more and 30 / 70 or less.

3. 3. The toner for developing electrostatic images according to claim 1, wherein the quaternary ammonium salt compound X is a quaternary ammonium salt-containing resin.

Citation Information

Patent Citations

  • Binder resin for toner

    JP2013024985A

  • Toner

    JP2015102842A

  • Positively-charged toner for electrophotography

    JP2016126156A

  • Magnetic toner

    JP2016197212A