Polyethylene laminate film and medical container

A laminated film with specific polyethylene layer configurations and compositions addresses the challenges of transparency, heat resistance, and gas barrier properties in medical containers, achieving effective performance even in thin films.

JP2024168226APending Publication Date: 2024-12-05TOSOH CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023084715
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing laminated films used in medical containers face challenges in achieving high transparency, heat resistance, and gas barrier properties, especially when made thinner, with polypropylene films having cleanliness issues and polyethylene films lacking in heat resistance and gas barrier properties.

Method used

A laminated film structure with specific thickness ratios and compositions of polyethylene layers, including a three-layer configuration with A, B, and C layers, where each layer is composed of polyethylene, with controlled water vapor permeability and light transmittance, ensuring a total thickness of 200 μm or less.

Benefits of technology

The laminated film maintains excellent transparency, heat resistance, and gas barrier properties, even when thin, suitable for medical containers like infusion bags and blood bags, reducing resin usage and ensuring minimal evaporation of internal fluids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168226000001
    Figure 2024168226000001
  • Figure 2024168226000002
    Figure 2024168226000002
  • Figure 2024168226000003
    Figure 2024168226000003
Patent Text Reader

Abstract

To provide a polyethylene laminate film excellent in heat resistance and water vapor barrier properties even when thinned and capable of holding high transparency and a medical container obtained therefrom.SOLUTION: A polyethylene laminate film having a thickness of 200 μm or less which is characterized in that the laminate film having a C layer and a B layer arranged between thereof, having the water vapor transmission rate measured by a water vapor transmission meter conforming to JIS K7129-1 of 2.0 g / m2 / day or less, and the light transmittance measured at a wavelength of 450 nm in pure water of 70% or more, a ratio of a thickness of the B layer relative to the thickness of the C layer of 6 times or less, and the ratio of the thickness of the B layer relative to the thickness of the A layer of 6 times or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated film made of polyethylene. [Background technology]

[0002] Films used for medical containers filled with drug solutions, blood, etc., are required to have transparency to check for contamination by foreign matter or changes due to drug compounding, heat resistance to withstand sterilization, flexibility to facilitate the discharge of drug solutions, gas barrier properties to prevent deterioration of drug solutions and quality deterioration due to the infiltration of water vapor and oxygen into the container, and reduction of particulate elution from the container (low particulate). Films made of polypropylene resin and polyethylene such as high-pressure low-density polyethylene, linear low-density polyethylene, and high-density polyethylene are used for such films. However, polypropylene has repeated tertiary carbons and is inherently prone to oxidative deterioration, so the addition of antioxidants is essential, making it difficult to clean. In addition, polypropylene films generally have poor cold impact resistance, making it difficult to make them thin. On the other hand, polyethylene films have excellent cleanliness, but have problems such as reduced heat resistance and gas barrier properties when made thin, and films made of polyethylene with high density to meet heat resistance have problems such as reduced transparency and flexibility.

[0003] Therefore, a laminated film is used in which a film having high heat resistance and high water vapor barrier properties is laminated with a film having high transparency (see Patent Documents 1 and 2), but there are still problems in making the film thinner. Also, a laminated film having a specific inner layer thickness has been proposed, but no specific example is given of a laminated film having a thickness of 200 μm or less (see Patent Document 3). A film that has excellent transparency, heat resistance, and gas barrier properties even when made thin is desired. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-96190 A [Patent Document 2] JP 2015-74197 A [Patent Document 3] JP 2005-7888 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a laminate film which, even when made thin, has excellent gas barrier properties against the permeation of water vapor, oxygen, etc., and which maintains high transparency and heat resistance, and a medical container using this laminate film. [Means for solving the problem]

[0006] As a result of extensive research, the inventors discovered that the above problems could be solved by using a laminate film in which polyethylene is arranged at a specific thickness ratio as a medical container, and thus completed the present invention.

[0007] That is, the present invention resides in the following [1] to [3]. [1] A laminate of three or more layers having at least an A layer, a B layer, and a C layer in that order, with the A layer, the B layer, and the C layer being made of polyethylene, and having a water vapor transmission rate of 2.0 g / m2 measured using a water vapor transmission rate meter conforming to JIS K7129-1. 2 / day or less, and has a light transmittance of 70% or more when measured in pure water at a wavelength of 450 nm, the ratio of the thickness of layer B to the thickness of layer C is 6 times or less, the ratio of the thickness of layer B to the thickness of layer A is 6 times or less, and the thickness of the entire film is 200 μm or less. [2] The laminate film according to [1], wherein the layer C and / or the layer A comprises a polyethylene resin composition containing 20 to 50% by weight of a high-density polyethylene (A) satisfying the following properties (a) to (c), and 50 to 80% by weight of an ethylene polymer (B) satisfying the following properties (d) to (g) (the total of (A) and (B) being 100% by weight), and satisfying the following properties (h) to (i); and the layer B comprises a resin composition containing 10 to 40% by weight of a high-density polyethylene (A) satisfying the properties (a) to (c), and 0 to 10% by weight of an ethylene polymer (B) satisfying the following properties (d) to (g), and 60 to 90% by weight of a linear low-density polyethylene (C) satisfying the following properties (j) to (k), (the total of (A), (B) and (C) being 100% by weight). (a) Density is 945-970 kg / m 3 (b) The melt flow rate (hereinafter referred to as MFR) measured at 190° C. under a load of 21.18 N is 0.1 to 30 g / 10 min. (c) 13 The number of hexyl or higher branches (LCB) per 1,000 carbon atoms, as determined by C-NMR spectroscopy, is less than 0.5. (d) density is 945-954 kg / m 3 It is. (e) The MFR is 0.1 to 1.0 g / 10 min. (f) In molecular weight measurement by gel permeation chromatography, the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) (Mw / Mn) is in the range of 3.0 to 5.0. (g) 13 The number of hexyl or higher branches (LCB) per 1000 carbon atoms determined from C-NMR spectroscopy is 0.5 to 2.0. (h) density is 951-957 kg / m 3 It is. (i) The MFR is 0.1 to 1.5 g / 10 min. (j) density is 880-915 kg / m 3 It is. (k) The MFR is 0.1 to 15 g / 10 min. [3] A medical container having a storage section for storing a medicinal solution, wherein at least the storage section is made of the laminated film described in [1] or [2], and layer A is an inner layer. Effect of the Invention

[0008] The laminated film of the present invention has excellent transparency, gas barrier properties and heat resistance even when made thin, and therefore can reduce the amount of resin used, making it suitable for use in medical containers such as infusion bags and blood bags. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in detail below.

[0010] The laminated film according to one embodiment of the present invention is a laminate of three or more layers, which has an A layer, a B layer, and a C layer in this order, and the A layer, the B layer, and the C layer are made of polyethylene. The laminated film has a water vapor permeability of 2.0 g / m2 as measured by a water vapor permeability meter conforming to JIS K7129-1. 2 / day or less, and the light transmittance measured in pure water at a wavelength of 450 nm is 70% or more, the ratio of the thickness of layer B to the thickness of layer C is 6 times or less, the ratio of the thickness of layer B to the thickness of layer A is 6 times or less, and the thickness of the entire film is 200 μm or less.

[0011] The laminated film is not particularly limited in terms of the other layer configurations, so long as it has an A layer, a B layer, and a C layer. The number of layers is most preferably three layers consisting of the A layer / B layer / C layer, but is not limited thereto. Alternatively, a layer configuration of A layer / B layer / center layer / B layer / C layer, in which a layer is further configured within the B layer in the A layer / B layer / C layer, or other layers can be appropriately provided between the B layer and the C layer or between the A layer and the B layer, as necessary. Examples of such other layers include an adhesive layer, a gas barrier layer, etc. For example, a five-layer structure such as A layer / adhesive layer / B layer / gas barrier layer / C layer can be used. Also, a new layer can be provided on the C side of the C layer. The symbol / between layers indicates that they are adjacent layers.

[0012] The thickness ratio of each layer is preferably 2 to 4 times the thickness of the B layer relative to the thickness of the C layer, and 2 to 4 times the thickness of the B layer relative to the thickness of the A layer, since the thickness ratio of the B layer relative to the thickness of the C layer is 6 times or less, and the thickness ratio of the B layer relative to the thickness of the A layer is 6 times or less, and a laminated film having better transparency and water vapor barrier properties can be obtained. Here, if the thickness ratio of the B layer relative to the thickness of the C layer exceeds 6 times, or if the thickness ratio of the B layer relative to the thickness of the A layer exceeds 6 times, the film will have poor water vapor barrier properties and heat resistance during moist heat sterilization. The thicknesses of the C layer and the A layer may be the same or different. A specific example of the thickness ratio of each layer is a laminated film having a C layer:B layer:A layer=1:4:1 (times).

[0013] The total thickness of the laminated film can be appropriately determined as needed so long as it is 200 μm or less, and is preferably 100 to 200 μm in terms of excellent transparency and water vapor barrier properties.

[0014] The upper laminate film has a light transmittance of 70% or more when measured in pure water at a wavelength of 450 nm. A light transmittance of 70% or more is preferable because when the laminate film is used as a medical container, the internal liquid has excellent visibility.

[0015] The above laminated film has a water vapor transmission rate of 2.0 g / m2, measured by gravimetric method in accordance with JIS K7219-1. 2 / day or less. Water vapor transmission rate is 2.0g / m 2 / day, this is preferable because it results in a laminated film with low evaporation of the internal liquid when used as a medical container.

[0016] The method for producing the laminated film is not particularly limited, but examples thereof include a method for producing a multilayer film or sheet by a water-cooled or air-cooled coextrusion multilayer inflation method, a coextrusion multilayer T-die method, a dry lamination method, an extrusion lamination method, etc. Among these, it is preferable to use a water-cooled coextrusion multilayer inflation method or a coextrusion multilayer T-die method. In particular, when a water-cooled coextrusion multilayer inflation method is used, it has many advantages in terms of transparency, hygiene, etc.

[0017] The laminated film may be any film so long as the A layer, B layer and C layer are made of polyethylene. The polyethylene may be any polyethylene so long as it is called polyethylene, and examples of such polyethylene include ethylene homopolymers and ethylene-α-olefin polymers. Among these, since a laminate film having particularly excellent transparency and water vapor barrier properties can be obtained, it is preferred that layer C and / or layer A is a polyethylene resin composition containing 20 to 50% by weight of a high-density polyethylene (A) satisfying the following properties (a) to (c), and 50 to 80% by weight of an ethylene-based polymer (B) satisfying the following properties (d) to (g) (the total of (A) and (B) being 100% by weight), and satisfying the following properties (h) to (i), and layer B is a resin composition containing 10 to 40% by weight of a high-density polyethylene (A) satisfying the above properties (a) to (c), 0 to 10% by weight of an ethylene-based polymer (B) satisfying the above properties (d) to (g), and 60 to 90% by weight of a linear low-density polyethylene (C) satisfying the above properties (j) to (k), (the total of (A), (B) and (C) being 100% by weight). (a) Density is 945-970 kg / m 3 (b) The melt flow rate (hereinafter referred to as MFR) measured at 190° C. under a load of 21.18 N is 0.1 to 30 g / 10 min. (c) 13 The number of hexyl or higher branches (LCB) per 1,000 carbon atoms, as determined by C-NMR spectroscopy, is less than 0.5. (d) density is 945-954 kg / m 3 It is. (e) The MFR is 0.1 to 1.0 g / 10 min. (f) In molecular weight measurement by gel permeation chromatography, the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) (Mw / Mn) is in the range of 3.0 to 5.0. (g) 13 The number of hexyl or higher branches (LCB) per 1000 carbon atoms determined from C-NMR spectroscopy is 0.5 to 2.0. (h) density is 951-957 kg / m 3 It is. (i) The MFR is 0.1 to 1.5 g / 10 min. (j) density is 880-915 kg / m 3 It is. (k) The MFR is 0.1 to 15 g / 10 min.

[0018] The high-density polyethylene (A) is an ethylene homopolymer or a copolymer of ethylene and an α-olefin, such as an ethylene-hexene-1 copolymer, an ethylene-butene-1 copolymer, or an ethylene-octene-1 copolymer.

[0019] The high density polyethylene (A) is particularly excellent in transparency, and since a laminated film with little thickness unevenness can be obtained, it is preferable that the MFR measured at 190°C under a load of 21.18 N according to JIS K6922-1 is 0.1 to 30 g / 10 min. Also, since a polyethylene laminated film with excellent transparency and gas barrier properties can be obtained, the density according to JIS K6922-1 is 945 to 970 kg / m 3 is preferably 950 to 965 kg / m 3 In addition, a laminated film having excellent heat resistance can be obtained. 13The number of hexyl or more branches (LCB) per 1000 carbon atoms determined by C-NMR spectrum measurement is preferably less than 0.5. The high-density polyethylene (A) can be produced by, for example, a slurry method, a solution method, a gas phase method, or other production method, and generally, a Ziegler catalyst consisting of a solid catalyst component containing magnesium and titanium and an organoaluminum compound, a metallocene catalyst consisting of an organotransition metal compound containing a cyclopentadienyl derivative and a compound and / or an organometallic compound that reacts with the organoaluminum compound to form an ionic complex, a vanadium-based catalyst, or the like can be used, and the high-density polyethylene (A) can be produced by homopolymerizing ethylene or copolymerizing ethylene and an α-olefin using the catalyst, and can be obtained, for example, by the method described in Japanese Patent No. 3319051.

[0020] The high density polyethylene (A) may be a commercially available product, for example, Nipolon Hard 5700, 4030 (trade name) manufactured by Tosoh Corporation.

[0021] The ethylene polymer (B) preferably has an MFR of 0.1 to 1.0 g / 10 min as measured at 190° C. under a load of 21.18 N according to JIS K6922-1, since a laminated film having excellent transparency and formability can be obtained. Also, the ethylene polymer (B) preferably has a density of 945 to 954 kg / m as measured in accordance with JIS K6922-1, since a laminated film having excellent transparency and gas barrier properties can be obtained. 3 In order to obtain a laminated film having excellent transparency and capable of being stably produced, the ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) in molecular weight measurement by gel permeation chromatography (hereinafter referred to as GPC) is preferably in the range of 3.0 to 5.0, more preferably 3.5 to 4.5. In addition, in order to obtain a laminated film having excellent heat resistance, it is further 13 The number of hexyl or higher branches (LCB) per 1000 carbon atoms determined by C-NMR spectroscopy is preferably 0.5 to 2.

[0022] The ethylene polymer (B) is produced using a metallocene catalyst. The metallocene catalyst used has one metallocene complex, an activating cocatalyst, and, if necessary, an organoaluminum compound as constituent components, and it is preferable to carry out copolymerization of the macromonomer with ethylene, or of the macromonomer with ethylene and an olefin having 3 to 6 carbon atoms, simultaneously with the synthesis of the macromonomer. The macromonomer is an olefin polymer having a vinyl group at the end, and is an ethylene polymer having a vinyl group at the end obtained by homopolymerizing ethylene or copolymerizing ethylene with an olefin having 3 to 6 carbon atoms.

[0023] The activating cocatalyst used as a constituent component of the metallocene catalyst refers to a compound that plays a role in converting a metallocene complex or a reaction product of a metallocene complex and an organoaluminum compound into an active species capable of polymerizing an olefin, and is preferably a compound that produces a cationic compound from the metallocene complex.

[0024] When preparing the metallocene catalyst, an alkylaluminum such as triethylaluminum or triisobutylaluminum may be used as necessary for activating the metallocene complex or removing impurities in the solvent.

[0025] When producing the ethylene polymer (B), the polymerization temperature is preferably −100 to 120° C., and particularly in consideration of productivity, the polymerization temperature is preferably 20 to 120° C., and more preferably 60 to 120° C. The polymerization time is preferably in the range of 10 seconds to 20 hours, and the polymerization pressure is preferably in the range of normal pressure to 300 MPa.

[0026] The polymerizable monomer is preferably ethylene and an α-olefin having 3 to 6 carbon atoms, and the supply ratio of ethylene and an α-olefin having 3 to 6 carbon atoms can be such that the α-olefin having 3 to 6 carbon atoms / ethylene (molar ratio) is 0 to 0.2, preferably 0 to 0.15. It is also possible to adjust the molecular weight by using hydrogen or the like during polymerization. In this case, the amount of hydrogen used can be such that the hydrogen / ethylene (molar ratio) is 0 to 0.002 (hydrogen concentration: 2,000 ppm), preferably 0 to 0.0005 (hydrogen concentration: 500 ppm).

[0027] The polymerization can be carried out by any of batch, semi-continuous, and continuous methods, and can also be carried out in two or more stages by changing the polymerization conditions. After the polymerization is completed, the ethylene-α-olefin copolymer can be separated and recovered from the polymerization solvent by a conventionally known method, and then dried to obtain the copolymer.

[0028] The polymerization can be carried out in a slurry state, a solution state, or a gas phase state, and in particular, when the polymerization is carried out in a slurry state, an ethylene-based polymer having a regular powder particle shape can be efficiently and stably produced. The ethylene-based polymer (B) can be obtained by a known method such as that described in JP2011-105934A.

[0029] The linear low density polyethylene (C) preferably has an MFR of 0.1 to 15 g / 10 min measured at 190° C. under a load of 2.16 kg according to JIS K6922-1, since a laminated film having excellent moldability can be obtained. Also, the linear low density polyethylene (C) preferably has a density of 890 to 915 kg / m according to JIS K6922-1, since a laminated film having excellent transparency and flexibility can be obtained. 3 It is preferable that:

[0030] The linear low-density polyethylene (C) can be produced by, for example, a high-pressure method, a solution method, a gas-phase method, etc. In general, a Ziegler catalyst consisting of a solid catalyst component containing magnesium and titanium and an organoaluminum compound, a metallocene catalyst consisting of an organotransition metal compound containing a cyclopentadienyl derivative and a compound and / or an organometallic compound that reacts with the organotransition metal compound to form an ionic complex, a vanadium catalyst, etc. can be used, and the polyethylene can be produced by copolymerizing ethylene and an α-olefin, and can be obtained by, for example, the methods described in JP-A-2009-275059, JP-A-2013-81494, etc.

[0031] The linear polyethylene (C) may be a commercially available product, for example, Niporon-Z HF210K, ZF220, FY12, etc. (trade name) manufactured by Tosoh Corporation.

[0032] The polyethylene resin composition can be obtained by mixing the above-mentioned high-density polyethylene (A) and / or the ethylene polymer (B) and / or the linear low-density polyethylene (C) by a conventionally known method, for example, by mixing with a Henschel mixer, a V-blender, a ribbon blender, a tumbler blender or the like, or by further melt-kneading the mixture obtained by such a method with a single-screw extruder, a twin-screw extruder, a kneader, a Banbury mixer or the like, and then granulating the mixture.

[0033] From the viewpoint of water vapor barrier property, the polyethylene resin composition constituting Layer C and / or Layer A preferably contains 20 to 50% by weight of the high density polyethylene (A) and 50 to 80% by weight of the ethylene polymer (B) (the total of (A) and (B) is 100% by weight), and more preferably contains 30 to 45% by weight of the high density polyethylene (A) and 55 to 70% by weight of the ethylene polymer (B). Note that (A) and (B) are contained in a ratio such that the total is 100% by weight.

[0034] The polyethylene resin composition used in the C layer and / or the A layer has a density of 951 to 957 kg / m from the viewpoint of heat resistance. 3It is preferable that:

[0035] The polyethylene resin composition used in the layer C and / or layer A preferably has an MFR of 0.1 to 1.5 g / 10 min, more preferably 0.6 to 1.2 g / 10 min, from the viewpoint of molding stability.

[0036] The polyethylene resin composition constituting layer B preferably contains 10 to 40% by weight of the high density polyethylene (A), 0 to 10% by weight of the ethylene polymer (B), and 60 to 90% by weight of the linear low density polyethylene (C), and more preferably contains 10 to 40% by weight of the high density polyethylene (A), 0 to 10% by weight of the ethylene polymer (B), and 60 to 90% by weight of the linear low density polyethylene (C). Note that (A), (B), and (C) are contained in such a ratio that the total weight is 100%.

[0037] To the polyethylene resin composition, commonly used known additives such as antioxidants, antistatic agents, lubricants, antiblocking agents, antifogging agents, organic or inorganic pigments, ultraviolet absorbers, dispersants, etc. may be appropriately blended as necessary within the scope of not significantly impairing the effects of the present invention. The method of blending the above-mentioned additives to the resin composition of the present invention is not particularly limited, but examples thereof include a method of directly adding the additives in the pelletizing step after polymerization, and a method of preparing a high-concentration master batch in advance and dry-blending this at the time of molding.

[0038] The polyethylene resin composition may also be blended with other thermoplastic resins such as polypropylene, ethylene-propylene copolymer rubber, poly-1-butene, etc., within the range that does not impair the effects of the present invention.

[0039] A medical container according to one embodiment of the present invention is a medical container having a storage section for storing a medicinal solution, and at least the storage section is preferably made of the laminate film, with Layer A being the inner layer.

[0040] The shape of the container that contains the liquid medicine can be, for example, a film bag or a bottle.

[0041] When the laminated film is formed into a film shape by a water-cooled or air-cooled coextrusion multilayer inflation method, a coextrusion multilayer T-die method, a dry lamination method, an extrusion lamination method, or the like, two sheets of the obtained film are stacked and the peripheral parts are heat-sealed to form a bag-shaped storage part. In addition, the obtained film can be formed into a recessed part to be the storage part by hot plate forming such as vacuum forming or pressure forming, and then the recessed parts are stacked so that they face each other and the peripheral parts are heat-sealed to form the storage part. In this case, the port part to be the inlet and outlet of the drug solution may be formed by heat sealing at the same time as the formation of the storage part, or the formation of the storage part and the formation of the port part can be performed in separate steps. The laminate can be formed into a bottle shape by a multilayer blow molding method, or the like to form the storage part. In addition, the port part can be formed by using a mold for integral molding with the storage part, a method of heat-sealing the port part to the storage part, a method of integrating the storage part with the storage part by insert blow molding, or the like.

[0042] The medical containers can be used in general medical applications, such as blood bags, platelet storage bags, infusion (medicinal fluid) bags, medical multi-chamber containers, and bags for artificial dialysis. EXAMPLES

[0043] The present invention will be described in more detail below by showing examples, but the present invention is not limited to these examples. A. Resin The properties of the resins used in the examples and comparative examples were evaluated by the following methods.

[0044] <density> The density was measured by a density gradient tube method in accordance with JIS K6922-1.

[0045] <mfr> The MFR (melt flow rate) was measured in accordance with JIS K6922-1.

[0046] <Molecular weight, molecular weight distribution> Weight average molecular weight (Mw), number average molecular weight (Mn), and the ratio of weight average molecular weight to number average molecular weight (Mw / Mn) were measured by GPC. A GPC device (Tosoh Corporation (trade name) HLC-8121GPC / HT) and a column (Tosoh Corporation (trade name) TSKgel GMHhr-H(20)HT) were used, the column temperature was set to 140°C, and 1,2,4-trichlorobenzene was used as the eluent. The measurement sample was prepared at a concentration of 1.0 mg / ml, and 0.3 ml was injected for measurement. The molecular weight calibration curve was calibrated using a polystyrene sample with a known molecular weight. Note that Mw and Mn were calculated as values ​​converted into linear polyethylene.

[0047] <Long chain branching> The number of long chain branches per 1000 carbon atoms was measured by carbon nuclear magnetic resonance ( 13 The carbon nuclear magnetic resonance (C-NMR) method was used to measure the carbon 13 The C-NMR spectrum was measured, and the number of long chain branches per 1000 carbon atoms in the polymer was calculated using the following calculation method. The measurement temperature was set at 130°C, and a mixed solution of 1,2-dichlorobenzene / 1,2-dichlorobenzene-d4 = 75 / 25 (volume ratio) was used as the solvent.

[0048] <How to calculate the number of long chain branches (LCB)> In the NMR spectrum with a Gaussian window function, the sum of the peak areas of all peaks having a peak top at 5 to 50 ppm was set to 1000, and the number of long chain branches (the number of branches having 7 or more carbon atoms) was calculated from the peak area of ​​the peak derived from the methine carbon bonded with a branch having 7 or more carbon atoms. Under these measurement conditions, the number of long chain branches (the number of branches having 7 or more carbon atoms) was calculated from the peak area of ​​the peak having a peak top near 38.22 to 38.27 ppm. The peak area of ​​the peak was taken as the area of ​​the signal in the range from the chemical shift of the valley with the adjacent peak on the high magnetic field side to the chemical shift of the valley with the adjacent peak on the low magnetic field side. In addition, under these measurement conditions, the peak top position of the peak derived from the methine carbon bonded with the hexyl branch was 38.21 ppm in the measurement of the ethylene-1-octene copolymer.

[0049] In the examples and comparative examples, resins produced by the following methods and commercially available products were used. (1) High-density polyethylene A-1: The following commercially available products were used.

[0050] Tosoh Corporation, (product name) Nipolon Hard 5700 (MFR = 0.9 g / 10 min, density = 954 kg / m 3 The results of the evaluation of the basic characteristics of A-1 are shown in Table 1.

[0051] A-2: The following commercially available products were used.

[0052] Tosoh Corporation, (product name) Nipolon Hard 4030 (MFR = 5.0 g / 10 min, density = 965 kg / m 3 The results of the evaluation of the basic characteristics of A-2 are shown in Table 1.

[0053] A-3: The following commercially available products were used.

[0054] Tosoh Corporation, (product name) Nipolon Hard 1000 (MFR = 20.0 g / 10 min, density = 964 kg / m 3 The results of the evaluation of the basic characteristics of A-3 are shown in Table 1. A-4: Produced by the following method. [Preparation of organically modified clay] In a 1-liter flask, 300 mL of industrial alcohol (product name: Enekin F-3, manufactured by Japan Alcohol Distributors) and 300 mL of distilled water were added, and 15.0 g of concentrated hydrochloric acid and dioleylmethylamine ((C 18 H 35 )2(CH3)N, and Lipomin MO6 (120mmol) manufactured by Lion Specialty Chemicals Co., Ltd. were added, and the mixture was heated to 45℃, after which 100g of synthetic hectorite (BYK, Labo-Nite RD) was dispersed in it, and the temperature was raised to 60℃ and stirred for 1 hour while maintaining the temperature. The slurry was filtered, washed twice with 600mL of water at 60℃, and dried in a dryer at 85℃ for 12 hours to obtain 130g of organically modified clay. The organically modified clay was then pulverized in a jet mill to a median diameter of 15μm. [Preparation of polymerization catalyst] After replacing the air in a 300mL flask equipped with a thermometer and reflux tube with nitrogen, 25.0g of the organically modified clay obtained in [Preparation of organically modified clay] and 108mL of hexane were added, followed by the addition of 0.392 (1mmol) of bis(indenyl)zirconium dichloride and 142mL of 20% triisobutylaluminum, and stirring for 3 hours at 60°C. After cooling to room temperature, the supernatant was removed and washed twice with 220mL of hexane, and then 220mL of hexane was added to obtain a catalyst suspension (solid weight content: 12.0wt%). [Production of A-4] In a 2L autoclave, 1.2L of hexane, 1.0mL of 20% triisobutylaluminum, and 200mg (equivalent to 24mg of solids) of the catalyst suspension obtained in [Preparation of polymerization catalyst] were added, and the temperature was raised to 85°C. Then, ethylene / hydrogen mixed gas was continuously fed so that the partial pressure was 0.90MPa (hydrogen concentration in ethylene / hydrogen mixed gas: 450ppm). After 90 minutes, the pressure was released, and the slurry was filtered and dried to obtain 205g of polymer. The MFR of this polymer was 1.0g / 10min, and the density was 952kg / m 3 The results of the evaluation of the basic characteristics of A-4 are shown in Table 1.

[0055] [Table 1]

[0056] (2) Ethylene-based polymers B-1: Produced by the following method. [Preparation of denatured clay] 300 mL of industrial alcohol (trade name: Ekinen F-3, manufactured by Japan Alcohol Sales Co., Ltd.) and 300 mL of distilled water were placed in a 1 L flask, 15.0 g of concentrated hydrochloric acid and 42.4 g (120 mmol) of dimethylbehenylamine (trade name: Armin DM22D, manufactured by Lion Corporation) were added, and the mixture was heated to 45 ° C. to disperse 100 g of synthetic hectorite (trade name: Laponite RDS, manufactured by Rockwood Additives Co., Ltd.), and then heated to 60 ° C. and stirred for 1 hour while maintaining the temperature. After filtering the slurry, it was washed twice with 600 mL of water at 60 ° C. and dried in a dryer at 85 ° C. for 12 hours to obtain 122 g of organically modified clay. This organically modified clay was spray-dried to a median diameter of 15 μm. [Preparation of polymerization catalyst] After replacing the air in a 300mL flask equipped with a thermometer and reflux condenser with nitrogen, 25.0g of the organically modified clay obtained in (1) and 108mL of hexane were added, followed by the addition of 0.4406g of dimethylsilylene(cyclopentadienyl)(2,4,7-trimethyl-1-indenyl)zirconium dichloride and 142mL of 20% triisobutylaluminum, and stirring for 3 hours at 60°C. After cooling to 45°C, the supernatant was removed and washed five times with 200mL of hexane, and 200mL of hexane was added to obtain a catalyst suspension (solid weight content: 12.0wt%). [Production of B-1] In a 2L autoclave, 1.2L of hexane, 1.0mL of 20% triisobutylaluminum, and 358mg (equivalent to 43mg of solids) of the catalyst suspension obtained in [Preparation of polymerization catalyst] were added, and after heating to 70°C, 1.2g of 1-butene was added, and ethylene / hydrogen mixed gas was continuously fed so that the partial pressure was 0.80MPa (hydrogen concentration in ethylene / hydrogen mixed gas: 765ppm). After 90 minutes, the pressure was released, and the slurry was filtered and dried to obtain 65g of polymer. The MFR of this polymer was 0.4g / 10min, and the density was 947kg / m 3 The number average molecular weight (Mn) was 3.2 × 10 4 , weight average molecular weight is 13.0 × 10 4 The Mw / Mn was 4.1, and the number of long chain branches contained in the polymer was 0.8 per 1000 carbon atoms in the main chain. The results of the evaluation of the basic properties of B-1 are shown in Table 2.

[0057] B-2: Produced by the following method. [Preparation of denatured clay] A modified clay compound was prepared in the same manner as in B-1. [Preparation of polymerization catalyst] A polymerization catalyst was prepared in the same manner as in B-1. [Production of B-2] In a 2L autoclave, 1.2L of hexane, 1.0mL of 20% triisobutylaluminum, and 358mg (equivalent to 43mg of solids) of the catalyst suspension obtained in [Preparation of polymerization catalyst] were added, and after heating to 70°C, 4.6g of 1-butene was added, and ethylene / hydrogen mixed gas was continuously fed so that the partial pressure was 0.80MPa (hydrogen concentration in ethylene / hydrogen mixed gas: 1600ppm). After 90 minutes, the pressure was released, and the slurry was filtered and dried to obtain 86g of polymer. The MFR of this polymer was 2.0g / 10min, and the density was 942kg / m 3 The number average molecular weight (Mn) was 2.0×10 4 , weight average molecular weight is 9.5 × 10 4 The Mw / Mn was 4.5, and the number of long chain branches contained in the polymer was 1.6 per 1000 carbon atoms in the main chain. The results of the evaluation of the basic properties of B-2 are shown in Table 2.

[0058] B-3: Produced by the following method. [Preparation of denatured clay] A modified clay compound was prepared in the same manner as in B-1. [Preparation of polymerization catalyst] A polymerization catalyst was prepared in the same manner as in B-1. [Production of B-3] In a 2L autoclave, 1.2L of hexane, 1.0mL of 20% triisobutylaluminum, and 358mg (equivalent to 43mg of solids) of the catalyst suspension obtained in [Preparation of polymerization catalyst] were added, and the temperature was raised to 70°C. Then, ethylene / hydrogen mixed gas was continuously fed so that the partial pressure was 0.80MPa (hydrogen concentration in ethylene / hydrogen mixed gas: 2000ppm). After 90 minutes, the pressure was released, and the slurry was filtered and dried to obtain 291g of polymer. The MFR of this polymer was 1.0g / 10min, and the density was 958kg / m 3 The number average molecular weight (Mn) was 2.0×10 4 , weight average molecular weight is 9.1 × 10 4 The Mw / Mn ratio was 4.0, and the number of long chain branches contained in the polymer was 1.3 per 1000 carbon atoms in the main chain.

[0059] The results of the basic characteristic evaluation of B-3 are shown in Table 2.

[0060] [Table 2]

[0061] (3) Linear low-density polyethylene C-1: Produced by the following method. [Preparation of denatured clay] 30 ml of 37% hydrochloric acid and 106 g of N,N-dimethyl-behenylamine were added to 1,500 ml of water to prepare an aqueous solution of N,N-dimethyl-behenylammonium hydrochloride. 300 g of montmorillonite with an average particle size of 7.8 μm (prepared by pulverizing Kunipia F, a product of Kunimine Industries, with a jet pulverizer) was added to the aqueous solution of hydrochloride and reacted for 6 hours. After the reaction was completed, the reaction solution was filtered and the resulting cake was dried under reduced pressure for 6 hours to obtain 370 g of a modified clay compound. [Preparation of polymerization catalyst] In a 20L stainless steel container under nitrogen atmosphere, 3.3L of heptane, 1.13mol (0.9L) of a heptane solution of triethylaluminum (20% by weight diluted product) per aluminum atom, and 50g of the modified clay compound obtained above were added and stirred for 1 hour. Diphenylmethylene (4-phenyl-indenyl) (2,7-di-t-butyl-9-fluorenyl) zirconium dichloride was added at 1.25mmol per zirconium atom and stirred for 12 hours. 5.8L of an aliphatic saturated hydrocarbon solvent (Idemitsu Petrochemicals, product name IP Solvent 2835) was added to the resulting suspension to prepare a catalyst. (Zirconium concentration 0.125mmol / L) [Production of C-1] Using a tank-type reactor equipped for high-temperature, high-pressure polymerization, ethylene and 1-hexene were continuously pumped into the reactor, and the total pressure was set to 90 MPa, the 1-hexene concentration to 18 mol%, and the hydrogen concentration to 5 mol%. The reactor was then stirred at 1,500 rpm, and the polymerization catalyst obtained above was continuously fed from the reactor's feed port, and the polymerization reaction was carried out while maintaining the average temperature at 200°C. The linear, low-density polymer obtained had an MFR of 2.0 g / 10 min and a density of 907 kg / m 3 The results of the basic characteristic evaluation of C-1 are shown in Table 3.

[0062] C-2: Produced by the following method. [Preparation of denatured clay] A modified clay compound was prepared in the same manner as in C-1. [Preparation of polymerization catalyst] A polymerization catalyst was prepared in the same manner as in C-1. [Production of C-2] Using a tank-type reactor equipped for high-temperature, high-pressure polymerization, ethylene and 1-hexene were continuously pumped into the reactor, and the total pressure was set to 90 MPa, the 1-hexene concentration to 23 mol%, and the hydrogen concentration to 1 mol%. The reactor was then stirred at 1,500 rpm, and the polymerization catalyst obtained above was continuously fed from the reactor's feed port, and the polymerization reaction was carried out while maintaining the average temperature at 200°C. The MFR of this polymer was 0.8 g / 10 min, and the density was 900 kg / m 3 The results of the basic characteristic evaluation of C-2 are shown in Table 3.

[0063] C-3: The following commercially available products were used.

[0064] Tosoh Corporation, product name Nipolon-Z ZF220 (MFR = 2.0 g / 10 min, density = 913 kg / m 3 The results of the evaluation of the basic characteristics of C-3 are shown in Table 3.

[0065] C-4: Produced by the following method. [Preparation of denatured clay] A modified clay compound was prepared in the same manner as in C-1. [Preparation of polymerization catalyst] A polymerization catalyst was prepared in the same manner as in C-1. [Production of C-4] Using a tank-type reactor equipped for high-temperature, high-pressure polymerization, ethylene and 1-hexene were continuously fed into the reactor, and the total pressure was set to 90 MPa, the 1-hexene concentration to 20 mol%, and the hydrogen concentration to 15 mol%. The reactor was stirred at 1,500 rpm, and the polymerization catalyst obtained above was continuously fed from the feed port of the reactor, and the polymerization reaction was carried out while maintaining the average temperature at 200°C. The MFR of this polymer was 12 g / 10 min, and the density was 907 kg / m 3 The results of the basic characteristic evaluation of C-4 are shown in Table 3.

[0066] [Table 3]

[0067] <Resin composition> The above-mentioned high density polyethylene (A), ethylene polymer (B) and linear low density polyethylene (C) were dry blended in the ratios described in the Examples and Comparative Examples. B. Laminates and sealed containers The laminated films and medical containers used in the examples and comparative examples were produced and evaluated by the following methods.

[0068] <Laminated film> Using a three-layer water-cooled inflation molding machine (Placo), a three-layer film with a film width of 135 mm and a film thickness of 100 to 250 μm was molded at a cylinder temperature of 180° C., a water bath temperature of 15° C., and a take-up speed of 6 m / min.

[0069] <Light transmittance> A test piece measuring 10 mm in width and 50 mm in length was cut out from the three-layer film, and the light transmittance at a wavelength of 450 nm was measured in pure water using an ultraviolet-visible spectrophotometer (Model V-730, manufactured by JASCO Corporation).

[0070] <Water vapor permeability> 10cm from the three-layer film 2 x10cm 2 A piece of film was cut out, and in accordance with JIS K7129-1, an aluminum mask was attached and the water vapor transmission rate was measured at a measurement diameter of 10 cm.

[0071] <Medical containers> From the three-layer film, an area of ​​420 cm 2 A rectangular piece of film was cut out, printed on the surface, and one end was heat-sealed to form a bag. 78.5 g of sodium chloride and 300 ml of pure water were then filled into the bag, and a head space of 50 ml was provided before heat-sealing to create a bag-shaped container, which was used as a medical container for evaluation.

[0072] <Legibility> The bag-shaped containers were sterilized for 20 minutes at 121°C using a steam sterilizer (manufactured by Hisaka Works, Ltd.). Containers with good readability were those that had no wrinkles on the surface and the letters printed on the film were legible.

[0073] <Dropped bag test> The bag-shaped container was dropped twice from a height of 1800 mm, and the container was checked for breakage and those that were not broken were considered to be good containers.

[0074] <Separation of contents> The bag-shaped containers were stored at a temperature of 25°C and a humidity of 65% for 40 days, and those in which no sodium chloride precipitated inside the container were considered to be good containers.

[0075] Examples 1 to 5, Comparative Examples 1 to 5 The resin composition shown in Table 4 was used to mold the film into a thickness of 100 to 250 μm using a water-cooled inflation molding machine, and the molding stability and the light transmittance and water vapor transmittance of the resulting three-layer film were evaluated. Next, a bag-shaped container was made from the resulting three-layer film, and the readability, bag drop, and precipitation of the contents were evaluated. The evaluation results are shown in Tables 4 and 5. In the tables, the outer layer corresponds to layer C, the middle layer corresponds to layer B, and the inner layer corresponds to layer A.

[0076] [Table 4]

[0077] [Table 5] < / mfr>

Claims

1. A laminate of three or more layers having at least an A layer, a B layer, and a C layer in this order, the A layer, the B layer, and the C layer being made of polyethylene, the water vapor transmission rate being 2.0 g / m as measured by a water vapor transmission rate meter conforming to JIS K7129-1. 2 / day or less, and has a light transmittance of 70% or more when measured in pure water at a wavelength of 450 nm, a ratio of the thickness of layer B to the thickness of layer C is 6 times or less, and a ratio of the thickness of layer B to the thickness of layer A is 6 times or less, and a total thickness of the film is 200 μm or less.

2. 2. The laminated film according to claim 1, wherein the C layer and / or the A layer comprises 20 to 50% by weight of a high-density polyethylene (A) satisfying the following properties (a) to (c), and 50 to 80% by weight of an ethylene-based polymer (B) satisfying the following properties (d) to (g) (the total of (A) and (B) is 100% by weight%), and is made of a polyethylene resin composition satisfying the following properties (h) to (i); and the B layer comprises a resin composition comprising 10 to 40% by weight of a high-density polyethylene (A) satisfying the properties (a) to (c), and 0 to 10% by weight of an ethylene-based polymer (B) satisfying the following properties (d) to (g), and 60 to 90% by weight of a linear low-density polyethylene (C) satisfying the following properties (j) to (k), (the total of (A), (B), and (C) is 100% by weight%). (a) Density is 945 to 970 kg / m 3 (b) The melt flow rate (hereinafter referred to as MFR) measured at 190° C. under a load of 21.18 N is 0.1 to 30 g / 10 min. (c) 13 The number of hexyl or higher branches (LCB) per 1,000 carbon atoms, as determined by C-NMR spectroscopy, is less than 0.

5. (d) density is 945 to 954 kg / m 3 It is. (e) The MFR is 0.1 to 1.0 g / 10 min. (f) In the molecular weight measurement by gel permeation chromatography, the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is in the range of 3.0 to 5.

0. (g) 13 The number of hexyl or higher branches (LCB) per 1,000 carbon atoms, as determined by C-NMR spectroscopy, is 0.5 to 2.

0. (h) density is 951 to 957 kg / m 3 It is. (i) The MFR is 0.1 to 1.5 g / 10 min. (j) density is 880 to 915 kg / m 3 It is. (k) The MFR is 0.1 to 15 g / 10 min.

3. 3. A medical container having a container section for containing a medical solution, wherein at least the container section is made of the laminate film according to claim 1 or 2, and layer A is an inner layer.

Citation Information

Patent Citations

  • Laminated body and container

    JP2005007888A

  • Laminate made of polyethylene and medical container comprising the same

    JP2015074197A

  • Polyethylene resin composition, laminate composed thereof, and medical container using laminate