Silicon nitride-sintered compact, mechanical component using the same, and bearing
A silicon nitride sintered body with controlled hardness, pore size, and crystallinity, combined with rare earth and aluminum elements, addresses processing challenges while maintaining mechanical properties for enhanced product life.
Patent Information
- Application Number
- JP2023084994
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Silicon nitride sintered bodies are difficult to process due to their high hardness, which increases processing time and cost, and lowering hardness to improve workability compromises wear resistance, potentially shortening product life.
A silicon nitride sintered body with Vickers hardness of 1220 Hv to 1400 Hv, maximum pore diameter of 30 μm or less in the surface layer, and crystallinity of 75% to 90%, containing rare earth and aluminum elements, which enhance workability while maintaining mechanical properties.
The solution achieves both improved workability and mechanical properties, ensuring a good product life for applications such as bearing members by controlling pore size and crystallinity.
Smart Images

Figure 2024168385000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a silicon nitride sintered body, and a machine part and a bearing each using the same. [Background technology]
[0002] Silicon nitride (Si3N4) sintered bodies have excellent mechanical properties, thermal conductivity, and electrical insulation, and therefore are being applied to bearing components, engine parts, tool materials, and heat dissipation substrate materials. It is known that silicon nitride sintered bodies are manufactured using silicon nitride powder as a starting material. Since silicon nitride powder is difficult to sinter, sintering aids are used together with silicon nitride powder to manufacture densified silicon nitride sintered bodies. Such sintering aids generally include oxides of rare earth elements, aluminum oxide, magnesium oxide, silicon oxide, and the like.
[0003] Since silicon nitride powder is expensive, when silicon nitride sintered bodies are manufactured using silicon nitride powder, the price of the silicon nitride sintered bodies also tends to rise. Therefore, a manufacturing method of manufacturing silicon nitride sintered bodies by using silicon powder (metal silicon powder), which is less expensive than silicon nitride powder, as a starting material and reactively sintering it has attracted attention (for example, Patent Documents 1 to 3). As such a manufacturing method, a method called PS-RBSN (Post-Sintering of Reaction Bonded Silicon-Nitride) method is known. The PS-RBSN method includes a first step of nitriding a compact formed from silicon powder by heat treatment, for example, at a temperature of about 1100°C to 1450°C in an environment containing nitrogen gas, and a second step of densifying the nitride obtained in the first step by heat treatment, for example, at a temperature of about 1600°C to 1950°C. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2004-149328 A [Patent Document 2] JP 2008-247716 A [Patent Document 3] JP 2013-49595 A [Patent Document 4] Patent Publication No. 2021-95317 Summary of the Invention [Problem to be solved by the invention]
[0005] Meanwhile, silicon nitride sintered bodies have excellent mechanical properties, but on the other hand, they are difficult to process because of their extremely high hardness (the Vickers hardness of typical silicon nitride sintered bodies is about 1400 to 1500 Hv). This increases the time required for processing, which may result in higher costs. On the other hand, lowering the hardness to improve processability also reduces the wear resistance (see Patent Document 4), so that the use of silicon nitride sintered bodies in bearing members and the like may lead to a shortened product life.
[0006] The present invention has been made in view of the above circumstances, and has an object to provide a silicon nitride sintered body that combines workability with good mechanical properties, and a machine part and a bearing that use the same. [Means for solving the problem]
[0007] The silicon nitride sintered body of the present invention is characterized in that it has a Vickers hardness of 1220Hv to 1400Hv and that the maximum diameter of pores in the surface layer, which is a region within 2 mm from the surface of the silicon nitride sintered body, is 30 μm or less. Note that the silicon nitride sintered body also includes a form in which there are no pores in the surface layer.
[0008] The silicon nitride sintered body is characterized in that the degree of crystallinity is 75% or more and 90% or less.
[0009] The silicon nitride sintered body contains a rare earth element and an aluminum element, and the content of the rare earth element is, in terms of oxide, 6 to 13% by weight, based on the total weight of the silicon nitride sintered body, and the content of the aluminum element is, in terms of oxide, 6 to 13% by weight, based on the total weight of the silicon nitride sintered body.
[0010] The total content of the rare earth element and the aluminum element is 15% by weight or more and 26% by weight or less, calculated as oxide, based on the total weight of the silicon nitride sintered body.
[0011] The rare earth element is characterized by including at least one element selected from the group consisting of Y, Ce, Nd, and Eu.
[0012] The silicon nitride sintered body has a Vickers hardness of 1250 Hv or more and 1320 Hv or less, a crystallinity of 75% or more and 85% or less, contains rare earth elements and aluminum elements, and does not contain transition metal elements, the content of the rare earth elements is 7.5% or more and 13% or less by weight, calculated as an oxide, relative to the total weight of the silicon nitride sintered body, the content of the aluminum elements is 7.5% or more and 13% or less by weight, calculated as an oxide, relative to the total weight of the silicon nitride sintered body, the total content of the rare earth elements and the aluminum elements is 15% or more and 26% or less by weight, calculated as an oxide, relative to the total weight of the silicon nitride sintered body, and the rare earth element is Y or Ce.
[0013] A machine part of the present invention is characterized in that it uses the silicon nitride sintered body of the present invention. The machine part is characterized in that it is a rolling element.
[0014] The bearing of the present invention is characterized by using the above-mentioned rolling elements. Effect of the Invention
[0015] According to the present invention, by defining the maximum pore size (and further the degree of crystallinity) while maintaining a low Vickers hardness of the silicon nitride sintered body, it is possible to achieve both processability and good mechanical properties, and for example, when the silicon nitride sintered body is processed into products such as bearing members, a good product life can be achieved. [Brief description of the drawings]
[0016] [Figure 1] 1 is a vertical sectional view showing an example of a bearing of the present invention. [Diagram 2] FIG. 4 is a vertical sectional view showing another example of a bearing of the present invention. [Diagram 3] FIG. 4 is a vertical sectional view showing another example of a bearing of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described. (Silicon nitride sintered body) The silicon nitride sintered body of this embodiment is mainly composed of a crystalline phase of silicon nitride, and contains an appropriate amount of a glass phase (amorphous phase) made of a sintering aid, etc. The sintering aid, etc. will be described later.
[0018] The silicon nitride sintered body of this embodiment has a Vickers hardness of 1220 Hv or more and 1400 Hv or less. By setting the Vickers hardness to 1400 Hv or less, which is lower than that of normal silicon nitride sintered bodies, the processability is improved. In addition, by setting the Vickers hardness to 1220 Hv or more, mechanical properties such as wear resistance are ensured.
[0019] In the present invention, the Vickers hardness is preferably 1250Hv or more, and may be 1280Hv or more. From the viewpoint of processability, the Vickers hardness is preferably 1350Hv or less, and may be 1320Hv or less. The Vickers hardness is measured by the method described in the examples below.
[0020] In addition, the silicon nitride sintered body of this embodiment has a maximum diameter of pores in the surface layer, which is a region within 2 mm from the surface, of 30 μm or less. The maximum diameter of the pores may be 25 μm or less, and in this embodiment, the silicon nitride sintered body may not have pores. By having a maximum diameter of pores of 30 μm or less, it is possible to maintain mechanical properties while maintaining low hardness, and when the silicon nitride sintered body is processed into products such as rolling elements of bearings, a good product life can be obtained. The pores in the surface layer refer to those present in the surface layer, which is a region within 2 mm from the surface of the silicon nitride sintered body, and refer to those in which the entire pores exist in the surface layer. The maximum diameter of the pores in the surface layer refers to the diameter of the pores that have the largest diameter among the pores present in the surface layer. When producing a silicon nitride sintered body, the maximum diameter of the pores can be adjusted by adjusting the content of the base material (silicon nitride or silicon) used as a raw material and / or the amount of sintering aid added.
[0021] The maximum diameter of the pores is a value measured for pores that are entirely present in the surface layer portion in a cross section of a test piece prepared by the method described in the Examples below. The maximum diameter of the pores can be calculated by the method described in the Examples below.
[0022] The silicon nitride sintered body may have inclusions (I) in the surface layer, which is a region within 2 mm from the surface. The inclusions (I) contain components other than silicon nitride, and examples thereof include inclusions (It) containing transition metal elements and inclusions (Is) containing non-nitrided silicon elements. The inclusions (It) are derived from, for example, a sintering aid (usually an oxide of a transition metal element) containing a transition metal element used in the production of the silicon nitride sintered body, and are, for example, silicides of transition metal elements. The inclusions (Is) are, for example, aggregates of non-nitrided silicon elements, and it is preferable that the inclusions (Is) are not included or that the proportion of inclusions is small. The inclusions refer to those that are entirely present in the surface layer, which is a region within 2 mm from the surface of the silicon nitride sintered body.
[0023] It is preferable that the silicon nitride sintered body does not contain a transition metal element. In other words, in this case, the silicon nitride sintered body does not have inclusions (It). The transition metal element is an element included in Groups 3 to 11 of the IUPAC periodic table, such as Fe, Ti, Cr, and Mn.
[0024] The silicon nitride sintered body of this embodiment preferably has a crystallinity of 75% or more and 90% or less. Here, the crystallinity of the silicon nitride sintered body means the ratio of the crystalline phase to all the components constituting the silicon nitride sintered body, and is calculated from the following formula based on the XRD diffraction pattern of a mirror-polished cut surface of the silicon nitride sintered body. Crystallinity (%) = crystalline peak area / (crystalline peak area + amorphous peak area) x 100
[0025] Specifically, the crystallinity of the silicon nitride sintered body is the "peak area of crystalline silicon nitride and other crystalline components in the XRD diffraction pattern" divided by the "sum of the peak areas of all components constituting the sintered body in the XRD diffraction pattern." Here, the crystalline silicon nitride is crystalline silicon nitride having an α-type, β-type, or γ-type crystal structure. In addition, all components constituting the sintered body are, for example, silicon, silicon nitride, and components derived from sintering aids that promote sintering during heat treatment in producing silicon nitride.
[0026] When a silicon nitride sintered body is produced, for example, by the PS-RBSN method (two-stage sintering method) using silicon powder and a sintering aid, under certain conditions, the sintering aid becomes the main component of the amorphous phase in the sintered body. The PS-RBSN method refers to a two-stage sintering method including a silicon nitriding step and a subsequent sintering step. For example, when a compact made of silicon powder and a sintering aid is heat-treated in a nitrogen atmosphere by the PS-RBSN method, the silicon is completely nitrided, and all of the sintering aid is made amorphous, the crystallinity is "peak area of crystalline silicon nitride in the XRD diffraction pattern" / "sum of each peak area of all components constituting the sintered body in the XRD diffraction pattern". In addition, when silicon is completely nitrided and a part of the sintering aid is crystallized, the crystallinity is "peak area of crystalline silicon nitride and crystalline components derived from the sintering aid in the XRD diffraction pattern" / "sum of each peak area of all components constituting the sintered body in the XRD diffraction pattern".
[0027] As the raw material of the silicon nitride sintered body, only silicon nitride powder may be used, silicon powder may be used, or silicon powder and a sintering aid may be used. Note that, as the raw material and manufacturing method of the silicon nitride sintered body, any raw material may be used as long as the silicon nitride sintered body can be obtained, and the manufacturing method is not limited to the PS-RBSN method. In addition, the atmospheric gas used during the heat treatment may be nitrogen gas, or a mixture of nitrogen gas, hydrogen gas, or argon gas.
[0028] The crystallinity of the silicon nitride sintered body may be 78% or more, or 81% or more. The crystallinity may be 87% or less, or 85% or less. When the crystallinity of the silicon nitride sintered body is in the range of 75% to 90%, the mechanical properties are easily maintained while the hardness is low, and when the silicon nitride sintered body is processed into products such as rolling elements of bearings, the product tends to have a good life.
[0029] The silicon nitride sintered body of this embodiment may contain rare earth elements and / or aluminum elements. When the silicon nitride sintered body contains rare earth elements, the content of the rare earth elements is preferably 6% by weight or more and 13% by weight or less in terms of oxide, based on the total weight of the silicon nitride sintered body. When the silicon nitride sintered body contains aluminum elements, the content of the aluminum elements is preferably 6% by weight or more and 13% by weight or less in terms of oxide, based on the total weight of the silicon nitride sintered body.
[0030] Examples of rare earth elements include yttrium (Y), lanthanum (La), cerium (Ce), samarium (Sm), neodymium (Nd), dysprosium (Dy), europium (Eu), erbium (Er), etc. Among these, yttrium (Y), cerium (Ce), neodymium (Nd), and europium (Eu) are preferred.
[0031] The silicon nitride sintered body preferably contains a rare earth element in the amorphous phase, more preferably one or more selected from the group consisting of Y, Ce, Nd, and Eu. The silicon nitride sintered body may contain a rare earth element in the crystalline phase.
[0032] The content of the rare earth element is more preferably 6.5% by weight or more, may be 7.0% by weight or more, or may be 7.5% by weight or more, calculated as oxide, based on the total weight of the silicon nitride sintered body. The content of the rare earth element is more preferably 12.5% by weight or less, may be 11.5% by weight or less, or may be 10.5% by weight or less.
[0033] The content of the aluminum element is more preferably 6.5% by weight or more, may be 7.0% by weight or more, or may be 7.5% by weight or more, calculated as oxide, based on the total weight of the silicon nitride sintered body. The content of the aluminum element is more preferably 12.5% by weight or less, may be 11.5% by weight or less, or may be 10.5% by weight or less. When the silicon nitride sintered body contains a rare earth element and an aluminum element, the content of the aluminum element (in terms of oxide) may be within ±5% by weight, ±2% by weight, or ±1% by weight of the content of the rare earth element (in terms of oxide), or may be the same as the content of the rare earth element.
[0034] By having the rare earth element and aluminum element contents in the silicon nitride sintered body within the above ranges, when producing a silicon nitride sintered body by the PS-RBSN method, the nitriding reaction of the raw material silicon powder (metallic silicon powder) can be promoted, and the subsequent sintering can be promoted, making it easier to set the Vickers hardness, maximum pore diameter, and crystallinity of the silicon nitride sintered body to the desired range. The rare earth element and aluminum element contents can be adjusted by the amount of sintering aid containing a rare earth element (e.g., oxide of a rare earth element) and sintering aid containing an aluminum element (e.g., aluminum oxide) added to the raw material.
[0035] The total content of the rare earth element and the aluminum element is preferably 15% by weight or more and 26% by weight or less, calculated as oxide, based on the total weight of the silicon nitride sintered body.
[0036] The above contents of rare earth elements and aluminum elements may be determined using an X-ray fluorescence analyzer (XRF), an energy dispersive X-ray analyzer (EDX), or an inductively coupled plasma (ICP) emission analyzer. Specifically, the contents of rare earth elements and aluminum elements in the silicon nitride sintered body may be determined using the above analyzer, and converted into oxides of rare earth elements (RE) (RE2O3 or REO2) and aluminum oxide (Al2O3). The elements of other components constituting the silicon nitride sintered body may also be analyzed using the above analyzer, and the total weight of the silicon nitride sintered body may be calculated to determine the above contents of rare earth elements and aluminum elements. When silicon (metal silicon powder) is contained in the raw material powder used to manufacture the silicon nitride sintered body and the silicon is nitrided to become Si3N4, the weight of Si3N4 in the silicon nitride sintered body is 1.67 times the weight of silicon. Therefore, taking into account the weight change when silicon is nitrided, the contents of the oxides of rare earth elements and aluminum oxide can be calculated from the composition of the raw material powder.
[0037] A particularly preferred embodiment of the silicon nitride sintered body of this embodiment is a silicon nitride sintered body that contains rare earth elements and aluminum elements, but does not contain transition metal elements, has a Vickers hardness of 1250Hv or more and 1320Hv or less, has a maximum diameter of pores in the surface layer portion, which is a region within 2 mm from the surface of the silicon nitride sintered body, of 30 μm or less, has a crystallinity of 75% or more and 85% or less, contains one or more elements selected from the group consisting of Y, Ce, Nd, and Eu in the amorphous phase, and has a rare earth element content of 6% to 13% by weight in oxide equivalent relative to the total weight of the silicon nitride sintered body, and has an aluminum element content of 6% to 13% by weight in oxide equivalent relative to the total weight of the silicon nitride sintered body. Furthermore, it is preferable that the total content of the rare earth element and the aluminum element is 15% to 26% by weight in oxide equivalent relative to the total weight of the silicon nitride sintered body. In addition, the above-mentioned numerical ranges can be appropriately combined with the above-mentioned embodiment.
[0038] The shape of the silicon nitride sintered body of this embodiment is not particularly limited, and may be appropriately selected depending on the application from spherical, cylindrical, conical, truncated conical, rectangular, etc., but is preferably spherical. The size of the silicon nitride sintered body is also not particularly limited, and for example, if it is spherical, the diameter can be 0.5 cm to 10 cm, and if it is cylindrical, the bottom diameter can be 0.5 cm to 15 cm and the height can be 3 cm to 20 cm.
[0039] (Production of sintered silicon nitride) Generally, a method for producing a silicon nitride sintered body includes a mixing step of mixing raw material powder containing silicon nitride powder or silicon powder and a sintering aid, a molding step of molding the mixed raw material powder into a green compact, and a sintering step of sintering the green compact. After the sintering step, the silicon nitride sintered body may be polished as necessary. It is preferable that the silicon nitride sintered body in the present invention contains silicon powder as a raw material and uses the PS-RBSN method (two-stage sintering method) for the sintering step.
[0040] In the mixing step, for example, the raw material powder is mixed in a dry manner without using water and an organic solvent. In this case, it is preferable to mix without using a binder component. The particle size of the powder after mixing is not particularly limited, but it is preferable that D90 is 10 μm or more and 100 μm or less. It is also preferable that D50 is 2 μm or more and 10 μm or less. By having D90 and / or D50 within the above range, it is possible to obtain a dense silicon nitride sintered body while exhibiting good fluidity and moldability. Note that D50 and D90 are the cumulative 50% diameter and cumulative 90% diameter on a volume basis, respectively, and are obtained by laser diffraction scattering type particle size distribution measurement, etc.
[0041] In addition, wet granulation may be performed in the mixing step to obtain granulated powder as a mixture. In this case, the raw material powder and the binder component are mixed with water and / or an organic solvent (e.g., ethanol) to form a slurry, which is then spray-dried and granulated to obtain granulated powder. An organic binder is used as the binder component, and is added in an amount of, for example, 1% by weight to 10% by weight based on the total raw material powder.
[0042] In the molding process, the mixture obtained in the mixing process is molded into a predetermined shape to obtain a green compact. For example, in the case of a spherical shape, a press molding such as cold isostatic pressing is performed to obtain a spherical green compact, which is then processed in a green processing device to obtain a green sphere.
[0043] The sintering step is, for example, a step of heating the obtained green compact in a nitrogen atmosphere from a temperature in the range of, for example, 800°C to 1200°C to the sintering temperature at a predetermined heating rate, and then maintaining the temperature for a predetermined time (for example, 5 hours to 8 hours) to perform heat treatment to sinter the green compact. By heating the green compact without maintaining the temperature at the predetermined temperature before sintering at the sintering temperature, it is possible to improve the manufacturing efficiency. The heating rate is, for example, 2.0°C / min or more and less than 10°C / min, preferably 2.0°C / min or more and less than 5.0°C / min, and may be 2.0°C / min or more and 4.0°C / min or less. The sintering temperature is, for example, 1600°C to 1950°C, preferably 1600°C to 1800°C, and more preferably 1650°C to 1750°C. By raising the temperature relatively slowly and controlling the nitriding rate of silicon, the sintered compact is easily densified, and the maximum diameter of pores present in the surface layer is easily reduced while reducing the hardness of the surface. In addition, the crystallinity can be easily adjusted to a desired range.
[0044] In the manufacture of the silicon nitride sintered body, the sintering aid used in the raw material powder may contain a rare earth element, an aluminum element, or a transition metal element. The sintering aid containing a rare earth element preferably contains any one of Y2O3, CeO2, Nd2O3, and Eu2O3. The sintering aid containing an aluminum element preferably contains Al2O3. In addition, the sintering aid containing a transition metal element may include Cr2O3, TiO2, MnO, Fe2O3, etc.
[0045] The raw material powder may contain silicon nitride powder and / or an organic binder in addition to silicon powder and a sintering aid, and may contain a sintering aid containing an element other than a rare earth element, an aluminum element, and a transition metal element.
[0046] The content of silicon powder in the raw material powder is preferably 65% by weight or more, more preferably 67% by weight or more, and even more preferably 69% by weight or more, and may be 71% by weight or more, preferably 80% by weight or less, 78% by weight or less, or 76% by weight or less, based on the total weight of silicon powder, silicon nitride powder, and sintering aid. The raw material powder may or may not contain silicon nitride powder.
[0047] The content of the sintering aid containing a rare earth element (for example, an oxide of a rare earth element) contained in the raw material powder is preferably 10% by weight or more, more preferably 11% by weight or more, even more preferably 12% by weight or more, and may be 13% by weight or more, based on the total weight. The content of the rare earth element may be 17.5% by weight or less, 16.5% by weight or less, or 15.5% by weight or less. The content of the sintering aid containing an aluminum element (for example, aluminum oxide) contained in the raw material powder is preferably 10% by weight or more, more preferably 11% by weight or more, even more preferably 12% by weight or more, and may be 13% by weight or more, based on the total weight. The content of the aluminum element may be 17.5% by weight or less, 16.5% by weight or less, or 15.5% by weight or less. If the content of the sintering aid contained in the raw material powder is low, it is difficult to obtain a dense silicon nitride sintered body, and if the content of the sintering aid is high, the mechanical properties of the silicon nitride sintered body tend to deteriorate.
[0048] The average particle size of the silicon powder contained in the raw material powder can be, for example, 5 μm or less. When silicon nitride is contained, the average particle size can be, for example, 0.5 μm or less. The average particle size of the sintering aid is preferably 10 μm or less, and may be 7 μm or less, 5 μm or less, 3 μm or less, 2 μm or less, 1 μm or less, or 0.4 μm or less, depending on the type of sintering aid. The average particle size is the cumulative 50% diameter based on volume, and is obtained by laser diffraction scattering type particle size distribution measurement or the like.
[0049] The method for producing the silicon nitride sintered body of this embodiment includes a mixing step of mixing a raw material powder containing silicon powder and a sintering aid, a molding step of molding the mixed raw material powder into a powder compact, and a sintering step of sintering the powder compact. The sintering step is a step of heating the sintered body in a nitrogen atmosphere at a predetermined heating rate to a sintering temperature, and then maintaining the sintering temperature for a predetermined time to perform a heat treatment. The heating rate is preferably 2.0°C / min or more and less than 5.0°C / min. The sintering temperature is more preferably 1600°C to 1800°C. The sintering aid contains a rare earth oxide and aluminum oxide, but does not contain a transition metal oxide, and the raw material powder contains the rare earth oxide in an amount of 9.5% by weight to 17% by weight based on the entire raw material powder, and the aluminum oxide in an amount of 9.5% by weight to 17% by weight based on the entire raw material powder. The above-mentioned numerical ranges can be appropriately combined with the above-mentioned method.
[0050] (Applications of sintered silicon nitride) The use of the silicon nitride sintered body of the present embodiment is not particularly limited, but since it has excellent mechanical properties, it is preferably used as a mechanical part. The mechanical part is used, for example, in a rolling part or a sliding part. The mechanical part of the present invention is a part using the silicon nitride sintered body of the present invention as a part or all of its configuration. Examples of the mechanical part include sliding members, bearing members, rolling roll materials, compressor vanes, engine parts such as gas turbine blades, cutting tools (chips), etc. Examples of the bearing member include raceways such as inner and outer rings, rolling elements for bearings, and retainers. The bearing of the present invention is a bearing that includes this mechanical part as a part or all of its bearing member, and examples of the bearing include rolling bearings, sliding bearings (spherical bushes, etc.), linear guide bearings, ball screws, linear bearings, etc. In particular, the bearing of the present invention is preferably a rolling bearing using the silicon nitride sintered body as a rolling element for bearings.
[0051] An example of the bearing of this embodiment will be described with reference to FIG. 1. FIG. 1 is a cross-sectional view of a deep groove ball bearing. In the rolling bearing 1, an inner ring 2 having an inner ring raceway surface 2a on its outer peripheral surface and an outer ring 3 having an outer ring raceway surface 3a on its inner peripheral surface are concentrically arranged, and a plurality of balls (rolling elements) 4 are arranged between the inner ring raceway surface 2a and the outer ring raceway surface 3a. These balls 4 are formed of the above-mentioned silicon nitride sintered body. The balls 4 are held by a cage 5. In addition, openings 8a, 8b at both axial ends of the inner and outer rings are sealed by a seal member 6, and a grease composition 7 is enclosed at least around the balls 4. The grease composition 7 is interposed between the raceway surface of the balls 4 to provide lubrication. The bearing type of the rolling bearing is not limited to a deep groove ball bearing, and may be an angular ball bearing, a thrust ball bearing, or the like.
[0052] Another example of the bearing of this embodiment will be described with reference to FIG. 2. FIG. 2 is a cross-sectional view showing a ball screw. As shown in FIG. 2, the ball screw has a screw groove 12 formed on the outer peripheral surface of a screw shaft 11, which is a guide member, and a screw groove 14 formed on the inner peripheral surface of a ball nut 13, with a plurality of balls 15 interposed between them. The rotational power of the screw shaft 11 (or the ball nut 13) is transmitted to the ball nut 13 (or the screw shaft 11) via the balls 15, and the ball nut 13 is moved in the axial direction. In FIG. 2, the balls 15 are formed of the above-mentioned silicon nitride sintered body, and the screw shaft 11 and the ball nut 13 are formed of steel (for example, bearing steel or low carbon steel). In addition, a grease composition is filled around the balls 15 between the screw shaft 11 and the ball nut 13, and is sealed by a seal member 16 for the ball screw.
[0053] In the ball screw shown in Fig. 2, the ball circulation system is not particularly limited, and any of the following circulation systems can be used: tube type, return tube (pipe) type, deflector type, end deflector type, end cap type, top type, etc. In any circulation system, the circulation path has a large effect on the smooth circulation of the balls.
[0054] Specifically, the ball screw is used to convert the rotational motion of a motor into linear motion, and can be suitably used in, for example, electric actuators, positioning devices, electric jacks, servo cylinders, electric servo presses, mechanical presses, electric brake devices, transmissions, electric power steering devices, electric injection molding machines, and the like.
[0055] Here, ball screws are required to have wear resistance, toughness, high load capacity, etc. In recent years, with the trend towards miniaturization, there is a growing demand for performance that can withstand high loads, as well as the need to suppress hydrogen embrittlement caused by hydrogen generated from lubricants due to slippage or high loads. In the example of Figure 2, the above-mentioned silicon nitride sintered body is used as the ball, which makes it easy to meet these requirements and also provides a long product life for the ball.
[0056] Furthermore, in a ball screw, if there is a large misalignment due to an installation error or the like when installing the ball screw, there is a risk of twisting (i.e., a relative inclination between the screw shaft and the nut). If a moment due to twisting acts on the ball screw, the load balance in the nut is lost, and there are places where the contact surface pressure increases partially, which may shorten the lifespan. In response to this, by using the above-mentioned silicon nitride sintered body as the balls, the circulation performance of the balls can be improved, making it easier to suppress a decrease in lifespan.
[0057] Further, another example of the bearing of this embodiment will be described with reference to FIG. 3. FIG. 3 is a cross-sectional view showing an example of a spherical plain bearing. As shown in FIG. 3, the spherical plain bearing 21 is a combination of an inner ring 22 having a spherical outer peripheral surface 22b and a bearing hole 24 formed in an inner peripheral surface 22a through which a support shaft can be inserted, and an outer ring 23 having a concave surface 23a corresponding to the outer peripheral surface 22b. In the spherical plain bearing 21, at least one of the inner ring 22 and the outer ring 23 is formed of the above-mentioned silicon nitride sintered body. The material of the other member is not particularly limited, and can be, for example, made of a metal such as an aluminum alloy, stainless steel, or steel, a synthetic resin, or a ceramic other than the above-mentioned silicon nitride sintered body.
[0058] A spherical plain bearing is a self-aligning plain bearing with a spherical sliding surface that can withstand radial loads and axial loads in both directions. Spherical plain bearings are suitable for oscillating and aligning motions, and are used in the joints of industrial and construction machinery. Spherical plain bearings can be either oil-free (see Figure 3) or oil-lubricated; for example, in the case of an oil-lubricated type, oil holes and oil grooves are provided in the inner and outer rings. When installing a spherical plain bearing, grease may be applied to the sliding surfaces. EXAMPLES
[0059] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to these examples.
[0060] <Examples 1 to 7, Comparative Examples 1 to 2> Raw material powders were prepared in the compounding ratios shown in Table 1, and dry mixed for 48 hours in a ball mill at 200 rpm using silicon nitride balls as media. Note that the specific surface area of the metallic silicon used as the raw material may be adjusted in order to suppress melting of the metallic silicon and facilitate the progress of the nitriding reaction.
[0061] [Table 1]
[0062] The obtained mixed powder was molded into a spherical green compact with a diameter of 12 mm by the RIP (Rubber Isostatic Pressing) method. The shape of the rubber mold may be adjusted during molding to suppress cracking of the green compact due to springback of the rubber mold or air stagnation in the rubber mold. For example, a gap may be provided between the mating surfaces of the upper and lower rubber molds. The obtained green compact was heated from 800°C to 1750°C (sintering temperature) at a heating rate of 2.5°C / min in a nitrogen atmosphere (pressure: 0.9 MPa), and then held for 6 hours to obtain a silicon nitride sintered compact.
[0063] Regarding the composition ratios of each oxide in the obtained silicon nitride sintered body, the values calculated from the composition ratios of the raw material powders are shown in Table 2, assuming that all of the silicon (metallic silicon) contained in the raw material powders is nitrided and the weight of silicon nitride is 1.67 times the weight of silicon.
[0064] [Table 2]
[0065] The obtained spherical silicon nitride sintered body was subjected to ball polishing to G5 in accordance with JIS B 1563, to prepare spherical test pieces of 3 / 8 inch (diameter 9.525 mm).
[0066] <Calculation of processing rate> In the above polishing, a #200 diamond surface plate was used to polish the balls up to a diameter of 9.625 mm. During this process, the ball dimensions were measured every hour in accordance with JIS B 1501, and the processing rate μm / h was calculated. The results are shown in Table 3.
[0067] <Measurement of maximum hole diameter> The test pieces obtained in the examples and comparative examples were cut at a cross section passing through the center, and the cut surface was mirror-polished. The mirror-polished cut surface was photographed using "VHX5000" manufactured by Keyence Corporation, and the photographed image was analyzed using "WinRoof" manufactured by Mitani Shoji Co., Ltd., to measure the maximum diameter of pores present in the surface layer, which is a region corresponding to a range within 2 mm from the surface of the spherical test piece. The diameter of the pores was calculated as the square root of the envelope area of the pores (pore diameter = √ (envelope area of the pores)). The surface layer was evaluated as "A" when there were no pores with a diameter of more than 30 μm, and as "B" when there were pores. The pores were measured when the entire pores were present in the surface layer. The results are shown in Table 3.
[0068] <Vickers hardness measurement> The Vickers hardness of the mirror-polished test pieces was measured in accordance with JIS R 1610.
[0069] <Calculation of crystallinity> The crystallinity of the silicon nitride sintered body was calculated based on the XRD diffraction pattern of the mirror-polished cut surface described above, using the following formula. Crystallinity (%) = crystalline peak area / (crystalline peak area + amorphous peak area) x 100
[0070] <Rolling fatigue test> Using the test pieces obtained in the examples and comparative examples, and using NTN Corporation's "6206" as the bearing outer ring, bearing inner ring, and cage, rolling fatigue tests were performed at a rotation speed of 3000 rpm, a load of 1.5 GPa, and a test time of 168 hours to evaluate the product life. The lubricant used was JXTG Nippon Oil & Energy Corporation's additive-free turbine oil "VG56." Test pieces that did not peel off within the test time were rated "a," and those that peeled off were rated "b." The results are shown in Table 3.
[0071] [Table 3]
[0072] As shown in Table 3, Examples 1 to 7, which have a Vickers hardness of 1220 Hv to 1400 Hv and a maximum pore diameter of 30 μm or less, have a good processing rate (for example, 10 μm / h or more), and all of the rolling fatigue test results were "a", indicating excellent peeling resistance. The crystallinity of Examples 1 to 7 was within the range of 75% to 90% (specifically, 76% to 88%). The results of the Examples show that the silicon nitride sintered body of the present invention can maintain mechanical properties usable as a rolling element and have a good product life, while improving the processability compared to ordinary silicon nitride sintered bodies.
[0073] The embodiments and examples disclosed herein are illustrative in all respects and should not be considered as limiting. The scope of the present invention is defined by the claims rather than the above-described embodiments, and is intended to include the equivalent meaning of the claims and all modifications within the scope of the claims. [Industrial Applicability]
[0074] The silicon nitride sintered body of the present invention can be suitably used as a rolling element of bearings such as rolling bearings, linear guide bearings, ball screws, and linear bearings. [Explanation of symbols]
[0075] 1. Rolling bearings 2. Inner Circle 3 Outer ring 4 Rolling elements 5 Cage 6 Sealing material 7 Grease 8a, 8b opening 11 Screw shaft 12 Thread groove 13 Ball nut 14 Thread groove 15 Ball 16 Ball screw seal material 21 Spherical plain bearing 22 Inner Circle 23 Outer Ring 24 Bearing hole
Claims
1. A silicon nitride sintered body, A silicon nitride sintered body having a Vickers hardness of 1220 Hv or more and 1400 Hv or less, and a maximum diameter of pores in a surface layer portion, which is a region within 2 mm from the surface of the silicon nitride sintered body, of 30 μm or less.
2. 2. The silicon nitride sintered body according to claim 1, wherein the silicon nitride sintered body has a crystallinity of 75% or more and 90% or less.
3. The silicon nitride sintered body contains a rare earth element and an aluminum element, 3. The silicon nitride sintered body according to claim 1, wherein the content of the rare earth element is, in terms of oxide, 6 to 13 weight % of the total weight of the silicon nitride sintered body, and the content of the aluminum element is, in terms of oxide, 6 to 13 weight % of the total weight of the silicon nitride sintered body.
4. 4. The silicon nitride sintered body according to claim 3, characterized in that the total content of said rare earth element and said aluminum element is 15% by weight or more and 26% by weight or less, calculated as oxide, based on the total weight of said silicon nitride sintered body.
5. 4. The silicon nitride sintered body according to claim 3, wherein the rare earth element includes at least one element selected from the group consisting of Y, Ce, Nd, and Eu.
6. The silicon nitride sintered body has a Vickers hardness of 1250 Hv or more and 1320 Hv or less, a crystallinity of 75% or more and 85% or less, contains a rare earth element and an aluminum element, and does not contain a transition metal element; The silicon nitride sintered body according to claim 1, characterized in that the content of the rare earth element is 7.5% by weight or more and 13% by weight or less, calculated as an oxide, relative to the total weight of the silicon nitride sintered body, the content of the aluminum element is 7.5% by weight or more and 13% by weight or less, calculated as an oxide, relative to the total weight of the silicon nitride sintered body, the total content of the rare earth element and the aluminum element is 15% by weight or more and 26% by weight or less, calculated as an oxide, relative to the total weight of the silicon nitride sintered body, and the rare earth element is Y or Ce.
7. 3. A machine part using the silicon nitride sintered body according to claim 1 or 2.
8. 8. The mechanical part according to claim 7, wherein the mechanical part is a rolling element.
9. A bearing using the rolling element according to claim 8.
Citation Information
Patent Citations
Process for manufacturing silicon nitride sintered compact
JP2004149328A
Reaction sintering silicon nitride-based sintered body and its producing process
JP2008247716A
Method for producing silicon nitride sintered compact
JP2013049595A
Silicon nitride sintered compact and bearing using the same
JP2021095317A