Release agent composition and release sheet
A solvent-free release agent composition with controlled reactivity and crosslinked structure addresses environmental and health concerns while achieving high peeling forces and stable performance, overcoming the limitations of existing solvent-based and high-reactivity compositions.
Patent Information
- Application Number
- JP2023085604
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Existing release agent compositions for heavy release applications are either harmful to the environment and human health due to solvent use, or they do not achieve sufficient heavy peeling effects without solvents, and they often form gels quickly due to high reactivity.
A solvent-free release agent composition comprising specific components: (A) alkenyl group-containing organopolysiloxane, (B) three-dimensional network organopolysiloxane, (C) olefin liquid, (D) organohydrogenpolysiloxane, and (E) platinum group metal catalyst, which form a crosslinked structure with controlled reactivity to achieve high peeling forces and prevent gel formation.
The composition provides a high peeling force of 3.0 N/25 mm or more with a stable pot life, ensuring effective and safe heavy release performance without solvent use.
Smart Images

Figure 2024168708000001 
Figure 2024168708000002 
Figure 2024168708000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an addition reaction curing type release agent composition that provides an excellent heavy release effect, and a release sheet using the same. More specifically, the present invention relates to a release agent composition that is not a solvent-based or emulsion-based release agent composition, and more preferably to a solventless type release agent composition. [Background technology]
[0002] Conventionally, in order to prevent adhesion or fixation between a substrate such as paper or plastic and an adhesive material, a cured film of an organopolysiloxane composition is formed on the substrate surface to impart release properties. As a method for forming a cured organopolysiloxane film on the substrate surface, a method for forming a release film by addition reaction is widely used because of its excellent curability.
[0003] Methods for forming peelable coatings through addition reactions include a type in which the organopolysiloxane composition is dissolved in an organic solvent, a type in which an emulsifier is used to disperse the organopolysiloxane composition in water to form an emulsion, and a solventless type consisting only of organopolysiloxane. However, since the solvent-based types have the disadvantage that they can be harmful to the human body and the environment, there is a shift from the solvent-based types to the solventless types for safety reasons.
[0004] In general, organopolysiloxane compositions for release paper are required to have various release strengths depending on the purpose. For applications requiring strong release, three-dimensional network organopolysiloxanes called MQ resins (M units are R'3SiO 1 / 2 Unit, Q unit is SiO 4 / 2 R' is a monovalent hydrocarbon group) is widely used.
[0005] However, alkenyl group-containing MQ resins are often resinous or highly viscous compounds, and when added in large quantities, they cannot be used without diluting with an organic solvent. Also, when added in small quantities, they can be used without a solvent, but in that case, the heavy release effect is insufficient.
[0006] Patent Document 1 discloses a release regulator comprising an organopolysiloxane resin-organopolysiloxane condensation product obtained by condensing (a1) 100 parts by mass of an MQ type resin having a molar ratio of M units to Q units of 0.6 to 1.0 and a hydroxyl or alkoxy group content in the range of 0.3 to 2.0 mass% and (a2) 20 to 150 parts by mass of a linear polydiorganosiloxane having a hydroxyl or alkoxy group and an average degree of polymerization of 100 to 1,000. In Patent Document 1, the release force in the examples increases only 1.4 to 2.2 times at a low speed (0.3 m / min) compared to the comparative example in which the condensation reaction product is not added, and a sufficient release strength effect is not obtained. This is presumably because the hydroxyl or alkoxy group content of (a1) used is low at a range of 0.3 to 2.0 mass%, there are few reaction sites with (a2), and there is no crosslinking structure due to sufficient condensation. Furthermore, since the condensation reaction between the components (a1) and (a2) is time-consuming, there is a demand for a high release composition that can be produced by a simpler and less expensive method.
[0007] In Patent Document 2, a pressure-sensitive adhesive is blended as a release regulator into a mixture of reactive siloxane polymer, siloxane crosslinker, and catalyst to achieve a high peel strength. However, since it is believed that the adhesive effect appears when the blending amount of the pressure-sensitive adhesive is increased, there is a limit to how high the peel strength can be achieved, and it cannot be said from the examples that a sufficient peel strength effect is obtained. In addition, pressure-sensitive adhesives have a high viscosity and are generally diluted in a solvent such as toluene, but in order to add them to the composition, it becomes necessary to replace the solvent with α-olefin, etc., due to the recent trend toward non-solvents.
[0008] Patent Document 3 is a mixture of an alkenyl group-containing MQ resin, an organofunctional siloxane having a low viscosity of 5 to 80 centipoise, and an organohydrogen polysiloxane, and because the organofunctional siloxane has high addition reactivity, it can easily form a crosslinked structure and achieve heavy peeling. However, when the inventors reproduced the above composition, they found that a silicone gel, which is thought to be an addition reaction product, was formed in the composition immediately after preparation due to its high reactivity. It is believed that immediately after adding the catalyst, the concentration distribution of the catalyst becomes uneven, and crosslinking proceeds at room temperature. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2010-37557 A [Patent Document 2] Special Publication No. 2007-523225 [Patent Document 3] Special Publication No. 2017-523258 Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a solvent-free release agent composition which is not too highly reactive and prevents the generation of gel after preparation, and which is capable of forming a crosslinked structure that can achieve excellent heavy release, and a release sheet on which a cured coating of the composition is formed. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention provides a release agent composition comprising the following components (A) to (E): (A) a linear or branched organopolysiloxane having at least three alkenyl groups bonded to silicon atoms in a side chain per molecule, a viscosity at 25°C of 100 mPa s or more, and a vinyl value of 0.05 to 0.3 mol / 100 g: 20 to 65 parts by mass per 100 parts by mass of the combined total of said component (A) and the following component (B), (B)R'3SiO 1 / 2 Units and SiO 4 / 2 Units and / or R'SiO 3 / 2 an organopolysiloxane having a three-dimensional network structure and having at least two alkenyl groups bonded to silicon atoms in each molecule (in each of the above formulas, R' is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 12 carbon atoms which may have an unsaturated bond): 35 to 80 parts by mass per 100 parts by mass of the combined total of the component (A) and the component (B); (C) an olefin that is liquid at 25°C: 0 to 20 parts by mass per 100 parts by mass of the total of the components (A) and (B), (D) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms per molecule: an amount such that the ratio of the number of hydrogen atoms bonded to silicon atoms in component (D) to the total number of alkenyl groups in components (A), (B), and (C) is 0.5 to 5; and (E) Platinum group metal catalyst: an effective amount
[0012] Such a release agent composition is a solvent-free type, does not have excessively high addition reactivity, prevents the generation of gel after preparation, and yet can form a crosslinked structure that can achieve excellent heavy release.
[0013] In the present invention, the component (A) is represented by the following average composition formula (1): (R 2 3SiO 1 / 2 ) a (R 1 R 2 2SiO 1 / 2 ) b (R 1 R 2 SiO) c (R 2 2SiO) d (R1 SiO 3 / 2 ) e (R 2 SiO 3 / 2 ) f (SiO 4 / 2 ) g (1) (In the formula, R 1 each independently represents an alkenyl group; R 2 are independently an unsubstituted or substituted monovalent hydrocarbon group not containing an alkenyl group, and a, b, c, d, e, f and g are each independently a number of 0 or more and are preferably represented by the following formula: 0≦a, 0≦b, 2≦a+b, 3≦c, 50≦d, 90≦c+d≦400, 0≦e≦8, 3≦b+c+e, 0≦f≦8, 0≦g≦8, 0≦f+g≦8).
[0014] With such component (A), it is possible to obtain more preferable viscosity of the release agent composition and more preferable release strength of the cured product.
[0015] In the present invention, the component (B) is preferably represented by the following average composition formula (2). (R 4 3SiO 1 / 2 ) h (R 3 R 4 2SiO 1 / 2 ) i (R 3 R 4 SiO) j (R 4 2SiO) k (R 3 SiO 3 / 2 ) l (R 4 SiO 3 / 2 ) m (SiO 4 / 2 ) n (2) (In the formula, R 3 are each independently an alkenyl group having 2 to 8 carbon atoms, and R 4 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms that is not an alkenyl group, provided that all R 4at least 80 mol % of the groups are methyl groups, and h, i, j, k, l, m, and n are each independently a number equal to or greater than 0, provided that i+j+l>0, l+m+n>0, and h+i+j+k+l+m+n=1.
[0016] Such component (B) can provide a more preferable strong release effect.
[0017] In the present invention, the component (C) is preferably a linear monoolefin having 10 to 18 carbon atoms, or a branched monoolefin having 10 or more carbon atoms.
[0018] Such a component (C) is preferable because it is possible to reduce the viscosity of the release agent composition and the crosslink density does not become too high.
[0019] In the present invention, the component (D) is represented by the following average composition formula (3): (R 6 3SiO 1 / 2 ) p (R 5 R 6 2SiO 1 / 2 ) q (R 5 R 6 SiO) r (R 6 2SiO) s (R 5 SiO 3 / 2 ) t (R 6 SiO 3 / 2 ) u (SiO 4 / 2 ) v (3) (In the formula, R 5 each independently represents a hydrogen atom; R 6are independently an unsubstituted or substituted monovalent hydrocarbon group other than a hydrogen atom, and p, q, r, s, t, u, and v are each independently a number equal to or greater than 0, and are preferably a linear or branched organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in side chains per molecule and having a viscosity at 25°C of 100 mPa s or greater, represented by the formula: 0≦p, 0≦q, 0≦p+q, 0≦r, 40≦s, 90≦r+s≦400, 0≦t≦8, 2≦q+r+t, 0≦u≦8, 0≦v≦8, 0≦u+v≦8).
[0020] If the component (D) is of this type, the release agent composition will have a more suitable viscosity, and the handling properties and coating accuracy will be more favorable.
[0021] In the present invention, it is preferable to contain 0 to 20 parts by mass of an organopolysiloxane (F) represented by the following formula, where 1≦p≦20 and X is a group selected from a methyl group, a methoxy group and a vinyl group, or an oxygen atom which gives a cyclic structure. [ka]
[0022] When such a component (F) is contained, a more suitable release agent composition can be obtained.
[0023] In the present invention, the viscosity of the stripping agent composition at 25° C. is preferably 50 to 1000 mPa·s.
[0024] Such a viscosity is preferable because it allows coating when forming a cured coating on a substrate and results in a uniform coating.
[0025] In the present invention, it is preferable that the stripping composition does not contain a solvent.
[0026] Such a stripping composition that does not contain a solvent is preferable because it is highly safe for the human body and the environment.
[0027] The present invention also provides a release sheet having a sheet-like substrate and a cured coating formed by curing the release agent composition on one or both surfaces of the substrate.
[0028] Such a release sheet is preferred because it provides an excellent release strength.
[0029] In the present invention, it is preferred that the release sheet has a peel strength of 3.0 N / 25 mm or more when a 25 mm wide polyester adhesive tape is attached to the cured coating at an angle of 180° and a peel speed of 0.3 m / min.
[0030] Such a release sheet is preferable because it reliably provides a high degree of release effect. Effect of the Invention
[0031] The release agent composition of the present invention can obtain a very high release strength compared to conventional high release compositions. In addition, it has an excellent pot life and the release strength does not decrease much over time after curing, so it is useful as a material for a release sheet with high release strength. And, an excellent release sheet is provided by using such a release agent composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] As described above, there has been a demand for the development of a solvent-free release agent composition that is not too highly reactive during addition, prevents the generation of gel after preparation, and yet is capable of forming a crosslinked structure that can achieve excellent heavy release, as well as a release sheet on which a cured coating of the composition is formed.
[0033] The present inventors have conducted intensive research into the above-mentioned problems and have discovered that a composition comprising (A) a linear or branched organopolysiloxane having at least three alkenyl groups bonded to silicon atoms in each molecule in its side chains and having a viscosity of 100 mPa s or more at 25°C and a vinyl value of 0.05 to 0.3 mol / 100 g, (B) a three-dimensional network organopolysiloxane resin having at least two alkenyl groups in each molecule, (C) an olefin that is liquid at 25°C, (D) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms in each molecule, and (E) a platinum group metal catalyst has an excellent heavy release effect, inhibits a decrease in release force over time after curing, and further has an excellent pot life, which has led to the completion of the present invention. In particular, by using a linear or branched organopolysiloxane that has at least three alkenyl groups bonded to silicon atoms in each molecule, has a viscosity of 100 mPa s or more at 25°C, and a vinyl value of 0.05 to 0.3 mol / 100 g, the composition of the present invention can provide a solvent-free release sheet that has extremely strong release properties while not exhibiting excessively high addition reactivity.
[0034] That is, the present invention is a release agent composition comprising the following components (A) to (E): (A) a linear or branched organopolysiloxane having at least three alkenyl groups bonded to silicon atoms in a side chain per molecule, a viscosity at 25°C of 100 mPa s or more, and a vinyl value of 0.05 to 0.3 mol / 100 g: 20 to 65 parts by mass per 100 parts by mass of the combined total of said component (A) and the following component (B), (B)R'3SiO 1 / 2 Units and SiO 4 / 2 Units and / or R'SiO 3 / 2 an organopolysiloxane having a three-dimensional network structure and having at least two alkenyl groups bonded to silicon atoms in each molecule (in each of the above formulas, R' is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 12 carbon atoms which may have an unsaturated bond): 35 to 80 parts by mass per 100 parts by mass of the combined total of the component (A) and the component (B); (C) an olefin that is liquid at 25°C: 0 to 20 parts by mass per 100 parts by mass of the total of the components (A) and (B), (D) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms per molecule: an amount such that the ratio of the number of hydrogen atoms bonded to silicon atoms in component (D) to the total number of alkenyl groups in components (A), (B), and (C) is 0.5 to 5; and (E) Platinum group metal catalyst: an effective amount
[0035] The present invention will be described in detail below, but the present invention is not limited thereto. In this specification, "Me" represents a methyl group, and "Vi" represents a vinyl group. [(A) Alkenyl-containing organopolysiloxane] Component (A) is a linear or branched organopolysiloxane which has at least three alkenyl groups bonded to silicon atoms in the side chains per molecule, has a viscosity of 100 mPa s or more at 25°C, and a vinyl value of 0.05 or more and 0.3 mol / 100 g or less.
[0036] The component (A) is a component for adjusting the viscosity of the composition and the release strength of the cured product, and is specifically represented by the following average composition formula (1): (R 2 3SiO 1 / 2 ) a (R 1 R 2 2SiO 1 / 2 ) b (R 1 R 2 SiO) c (R 2 2SiO) d (R 1 SiO 3 / 2 ) e (R 2 SiO 3 / 2 ) f (SiO 4 / 2 ) g (1) (In the formula, R 1 each independently represents an alkenyl group; R 2are independently unsubstituted or substituted monovalent hydrocarbon groups not containing alkenyl groups, and a, b, c, d, e, f, and g are each independently a number equal to or greater than 0, and are represented by the following formula: 0≦a, 0≦b, 2≦a+b, 3≦c, 50≦d, 90≦c+d≦400, 0≦e≦8, 3≦b+c+e, 0≦f≦8, 0≦g≦8, 0≦f+g≦8, and component (A) is a linear organopolysiloxane having at least 3, preferably 3 to 50, and more preferably 3 to 30 alkenyl groups bonded to silicon atoms in the side chains per molecule. The organopolysiloxane has a viscosity at 25°C of 5,000 mPa·s or less, preferably 3,000 mPa·s or less, and more preferably 1,500 mPa·s or less. Organopolysiloxanes having a linear molecular structure in which the main chain is composed of repeating diorganosiloxane units and the molecular chain ends are blocked with triorganosiloxy groups are preferred. If the viscosity is within the above upper limit, the desired heavy release effect can be obtained without decreasing the crosslink density of the cured product, which is preferable. The lower limit is 100 mPa·s or more, preferably 200 mPa·s or more. If the viscosity is below the above lower limit, silicone gel may easily form in the composition, which is undesirable. Furthermore, even if no silicone gel is formed, there is a risk of the composition having a significantly high viscosity. In the present invention, the viscosity is measured as the absolute viscosity value measured with a B-type rotational viscometer at 25°C (the same applies hereinafter).
[0037] The vinyl value of component (A) is 0.05 or more and 0.3 mol / 100 g or less. If the vinyl value of component (A) is less than 0.05 mol / 100 g, the curability may decrease. On the other hand, if the vinyl value exceeds 0.3 mol / 100 g, the release property of the cured coating may decrease. The vinyl value is preferably 0.07 or more and 0.2 mol / 100 g or less.
[0038] In the above formula (1), a, b, c, d, e, f, and g are each independently a number of 0 or more, where 0 ≤ a, 0 ≤ b, 2 ≤ a + b, 3 ≤ c, 50 ≤ d, 90 ≤ c + d ≤ 400, 0 ≤ e ≤ 8, 3 < b + c + e, 0 ≤ f ≤ 8, 0 ≤ g ≤ 8, and 0 ≤ f + g ≤ 8. Preferably, 2 ≤ a ≤ 20, 2 ≤ b ≤ 20, 4 ≤ a + b ≤ 20, 3 ≤ c ≤ 40, 55 ≤ d ≤ 220, 95 ≤ c + d ≤ 250, 0 ≤ e ≤ 5, 5 ≤ b + c + e ≤ 60, 0 ≤ f ≤ 5, 0 ≤ g ≤ 5, and 0 ≤ f + g ≤ 5.
[0039] The alkenyl group bonded to the silicon atom preferably has 2 to 8 carbon atoms, more preferably 2 to 4 carbon atoms. For example, a vinyl group, an aryl group, a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, etc. can be mentioned, and a vinyl group is preferred. The alkenyl group bonded to the silicon atom may be present at the molecular chain end in addition to the molecular chain side chain in the molecule of the organopolysiloxane.
[0040] The organic group bonded to the silicon atom other than the alkenyl group is not particularly limited as long as it does not have an aliphatic unsaturated bond. For example, it can be an unsubstituted or substituted monovalent hydrocarbon group having usually 1 to 12 carbon atoms, preferably 1 to 10 carbon atoms. Examples of the unsubstituted or substituted monovalent hydrocarbon group include alkyl groups such as methyl group, ethyl group, propyl group, butyl group, pentyl group, hexyl group, and heptyl group; cycloalkyl groups such as cyclohexyl group; aryl groups such as phenyl group, tolyl group, xylyl group, and naphthyl group; aralkyl groups such as benzyl group and phenethyl group; and halogenated alkyl groups such as chloromethyl group, 3-chloropropyl group, and 3,3,3-trifluoropropyl group in which part or all of the hydrogen atoms of these groups are substituted with halogen atoms such as chlorine atom, fluorine atom, and bromine atom. An alkyl group is preferred, and a methyl group is more preferred.
[0041] The amount of the (A) component is 20 to 65 parts by mass, preferably 22 to 55 parts by mass, and more preferably 25 to 50 parts by mass, per 100 parts by mass of the total of the (A) component and the (B) component. If the content of the (A) component is less than the lower limit, the viscosity of the resulting composition becomes significantly high, and the handling property and the coating accuracy decrease. If the amount of the (A) component exceeds the upper limit, the crosslink density of the cured product decreases, making it difficult to obtain the desired high peel effect.
[0042] Examples of the linear organopolysiloxane (A) include those having the structure shown below: In the formula, R is a methyl group or a vinyl group, and the component (A) may be used alone or in combination of two or more types.
[0043] [ka]
[0044] [ka]
[0045] [ka]
[0046] [ka]
[0047] [ka]
[0048] [ka]
[0049] [(B) Three-dimensional network organopolysiloxane] Component (B) is R'3SiO 1 / 2 Units and SiO4 / 2 Units and / or R'SiO 3 / 2 The organopolysiloxane has a three-dimensional network structure, has at least two alkenyl groups bonded to silicon atoms in each molecule (in each of the above formulas, R' is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 12 carbon atoms which may have an unsaturated bond). The component (B) is a component for imparting a strong peeling effect, and specifically, is represented by the following average composition formula (2): (R 4 3SiO 1 / 2 ) h (R 3 R 4 2SiO 1 / 2 ) i (R 3 R 4 SiO) j (R 4 2SiO) k (R 3 SiO 3 / 2 ) l (R 4 SiO 3 / 2 ) m (SiO 4 / 2 ) n (2) (In the formula, R 3 are each independently an alkenyl group having 2 to 8 carbon atoms, and R 4 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms that is not an alkenyl group, provided that all R 4 are methyl groups, and h, i, j, k, l, m, and n are each independently a number equal to or greater than 0, with the proviso that i+j+l>0, l+m+n>0, and h+i+j+k+l+m+n=1. Component (B) is preferably waxy or solid at 25°C. Here, "waxy" means a gum-like (raw rubber-like) structure that exhibits almost no self-fluidity, with a viscosity of 10,000 Pa s or more, particularly 100,000 Pa s or more, at 25°C.
[0050] In the above formula (2), h, i, j, k, l, m, and n are each independently a number equal to or greater than 0, provided that i+j+l>0, l+m+n>0, and h+i+j+k+l+m+n=1. The character h is a number from 0 to 0.65, and is particularly preferably a number from 0.2 to 0.4. The letter i is a number from 0 to 0.12, and is particularly preferably a number from 0.03 to 0.07. j is a number from 0 to 0.2, and is particularly preferably a number from 0 to 0.1. k is a number from 0 to 0.2, and is particularly preferably a number from 0 to 0.1. The letter l is a number from 0 to 0.2, and is particularly preferably a number from 0 to 0.1. m is a number from 0 to 0.2, and is particularly preferably a number from 0 to 0.1. n is preferably a number from 0 to 0.6, and particularly preferably from 0.23 to 0.6. Furthermore, i+j+l is preferably 0 to 0.5, and particularly preferably 0 to 0.2, and l+m+n is preferably 0.1 to 0.8, and particularly preferably 0.2 to 0.6.
[0051] In the above formula (2), R 3 Examples of the alkenyl group represented by the formula (I) include the silicon-bonded alkenyl groups exemplified for component (A), and vinyl groups are particularly preferred. 4 Examples of the unsubstituted or substituted monovalent hydrocarbon group other than an alkenyl group, represented by the formula (I), include the organic groups other than the silicon-bonded alkenyl groups exemplified in the component (A). Among these, a methyl group is preferred, and when all R 4 At least 80 mol %, preferably 90 to 98 mol %, of the total R 4 When the content is 80 mol % or more, the compatibility with the above-mentioned component (A) is excellent, the stripping composition does not become cloudy and separate, and a uniform coating can be obtained.
[0052] In component (B), the content of alkenyl groups bonded to silicon atoms is preferably in the range of 0.01 to 1 mol, more preferably in the range of 0.05 to 0.2 mol, and even more preferably in the range of 0.06 to 0.1 mol, per 100 g of component (B). When the content of alkenyl groups is in the range of 0.01 to 1 mol, the crosslinking reaction proceeds sufficiently, and a cured product with higher hardness can be obtained.
[0053] The amount of the (B) component is 35 to 80 parts by mass, preferably 40 to 60 parts by mass, and more preferably 45 to 50 parts by mass, per 100 parts by mass of the total of the (A) and (B) components. If the content of the (B) component exceeds the upper limit, the viscosity of the resulting composition becomes significantly high, and the handling property and coating accuracy decrease. If the amount of the (B) component is less than the lower limit, the crosslink density of the cured product decreases, making it difficult to obtain the desired high peel strength effect.
[0054] Examples of the organopolysiloxane resin of component (B) include the following: (Me3SiO 1 / 2 ) h (ViMe2SiO 1 / 2 ) i (SiO 4 / 2 ) n (ViMe2SiO 1 / 2 ) i (SiO 4 / 2 ) n (ViMeSiO) j (Me2SiO) k (MeSiO 3 / 2 ) m (ViMe2SiO 1 / 2 ) i (Me2SiO) k (ViSiO 3 / 2 ) l (ViMe2SiO 1 / 2 ) i (Me2SiO) k (MeSiO 3 / 2 ) m (Me3SiO1 / 2 ) h (ViMe2SiO 1 / 2 ) i (Me2SiO) k (MeSiO 3 / 2 ) m (Me3SiO 1 / 2 ) h (ViMe2SiO 1 / 2 ) i (Me2SiO) k (ViMeSiO) j (MeSiO 3 / 2 ) m (In the formula, h, i, j, k, l, m, and n are as defined in the above average composition formula (2).)
[0055] In particular, Me3SiO 1 / 2 , ViMe2SiO 1 / 2 and SiO 4 / 2 It is more preferable to use an organopolysiloxane resin composed of units. By using such an organopolysiloxane resin, the crosslink density of the obtained cured product is sufficiently high, and it is possible to obtain the desired high release effect. The (B) component may be used alone or in combination of two or more kinds.
[0056] [(C) Liquid olefin] Component (C) is an olefin that is liquid at 25°C. The component (C) is a so-called viscosity reducer that can reduce the viscosity of the composition by adding a small amount. It is not particularly limited as long as it is an olefin that is liquid at 25°C, and may be appropriately selected from known olefins, but monoolefins are particularly preferred. For example, in the case of diolefins, the crosslinking density becomes too high, which may cause peeling noise during peeling. It is preferable to use linear monoolefins having 10 to 18 carbon atoms or branched monoolefins having 10 or more carbon atoms.
[0057] In the past, methods such as adding a solvent or adding a low-viscosity organopolysiloxane component were used to reduce the viscosity of organopolysiloxane compositions, but when a highly volatile solvent is used, it may be harmful to the human body or the environment, and the use of a solvent is not preferable from the perspective of safety.In addition, the viscosity can also be reduced by adding a low-viscosity organopolysiloxane component with low volatility, but the inventor has conducted extensive research and found that the viscosity reducing effect is lower than that of hydrocarbon-based compounds.Therefore, in order to reduce the viscosity by adding a low-viscosity organopolysiloxane component, it is necessary to add a large amount of the component, which makes it difficult to obtain the desired heavy release effect.
[0058] In contrast, olefins that are liquid at 25°C (particularly preferably linear monoolefins having 10 to 18 carbon atoms or branched monoolefins having 10 or more carbon atoms) have a high viscosity reducing effect on organopolysiloxane compositions, so that a small amount is sufficient to reduce the viscosity, and the strong release effect is not impaired. In addition, since they have reactive groups (particularly olefin moieties) with organopolysiloxane compositions (particularly SiH), they are incorporated into the cured coating and do not volatilize or migrate to the tape. Therefore, they are very useful in controlling the viscosity of the release agent composition.
[0059] In the present invention, the olefin may be either linear or branched, but is preferably a linear monoolefin having 10 to 18 carbon atoms or a branched monoolefin having 10 or more carbon atoms. The linear monoolefin preferably has 10 to 18 carbon atoms, more preferably 12 to 18 carbon atoms, and even more preferably 14 to 18 carbon atoms. If the number of carbon atoms of the monoolefin is within the above upper limit, it is preferable because it is liquid at 25°C. Furthermore, if the number of carbon atoms of the monoolefin is equal to or greater than the above lower limit, it is low in volatility, and therefore is highly safe for the human body and the environment. Examples of such linear monoolefins include 1-tetradecene, 1-hexadecene, and 1-octadecene. More specifically, commercially available products in the "Linearene" (manufactured by Idemitsu Kosan Co., Ltd.) series (for example, "Linearene 14", "Linearene 16", "Linearene 18", etc.) can be used.
[0060] From the viewpoint of volatility, the branched monoolefin preferably has 10 or more carbon atoms, more preferably 15 or more. The upper limit of the number of carbon atoms is not particularly limited, and it is sufficient that it is liquid at 25°C. It is preferably 50 or less, more preferably 40 or less. In addition, when the branched monoolefin is a mixture of two or more kinds, such as HS dimer A-20P exemplified below, a small amount of a branched monoolefin having more than 50 carbon atoms may be mixed. As such a branched monoolefin, for example, a commercially available product of the series of the product name "HS dimer" (manufactured by Toyokuni Oil Mills Co., Ltd.) represented by the following formula (for example, the product names "A-20", "A-20P", etc.) can be used. The component (C) may be used alone or in combination of two or more kinds.
[0061] HS Dimer A-20 [ka] HS Dimer A-20P [ka]
[0062] The amount of component (C) is 0 to 20 parts by mass, preferably 0.1 to 18 parts by mass, more preferably 1 to 15 parts by mass, and even more preferably 4 to 12 parts by mass, per 100 parts by mass of the total of components (A) and (B). If the amount of component (C) exceeds the upper limit, the viscosity of the resulting composition becomes too low, resulting in poor coatability. When component (C) is used, it is preferable that the amount of component (C) is equal to or greater than the lower limit, since this component is effective as a viscosity reducer.
[0063] [(D) Organohydrogenpolysiloxane] Component (D) is an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms (hereinafter referred to as SiH groups) in each molecule. Any known organohydrogensiloxane used in addition reaction type silicone compositions can be used. For example, an organohydrogenpolysiloxane represented by the following average composition formula (3): (R 6 3SiO 1 / 2 ) p (R 5 R 6 2SiO 1 / 2 ) q (R 5 R 6 SiO) r (R 6 2SiO) s (R 5 SiO 3 / 2 ) t (R 6 SiO 3 / 2 ) u (SiO 4 / 2 ) v (3) (In the formula, R 5 each independently represents a hydrogen atom; R 6 are independently an unsubstituted or substituted monovalent hydrocarbon group other than a hydrogen atom, and p, q, r, s, t, u and v are independently numbers of 0 or more and are represented by the following expressions: 0≦p, 0≦q, 0≦p+q, 0≦r, 40≦s, 90≦r+s≦400, 0≦t≦8, 2≦q+r+t, 0≦u≦8, 0≦v≦8, 0≦u+v≦8).
[0064] The alkenyl groups contained in the (A), (B) and (C) components react with the SiH groups in the (D) component to form a crosslinked structure. That is, the (D) component functions as a crosslinking agent. The (D) component preferably has a viscosity of 1,000 mPa·s or less at 25°C, more preferably 100 to 500 mPa·s, and even more preferably 100 to 200 mPa·s. If the viscosity is within the above upper limit, the composition as a whole does not become highly viscous, and the handling and coating accuracy are good. The viscosity is the absolute viscosity value measured by a B-type rotational viscometer at 25°C. From the viewpoint of crosslinking balance, the amount of the (D) component is preferably an amount such that the ratio of the number of SiH groups in the (D) component to the number of all alkenyl groups in the (A), (B) and (C) components is 0.5 to 5.0, preferably 0.7 to 3.0. If the amount of the (D) component does not satisfy the above range, the crosslinking balance may be inappropriate.
[0065] In the component (D), the content of the SiH group is preferably in the range of 0.1 to 2 mol, and more preferably in the range of 0.2 to 1.7 mol, per 100 g of the component (D). 6 The unsubstituted or substituted monovalent hydrocarbon group other than a hydrogen atom, represented by the formula (I), is exemplified by the silicon-bonded organic groups other than the alkenyl group exemplified for component (A) above. A methyl group is preferred, and all R 6 It is preferable that at least 50 mol %, typically 60 to 100 mol %, of the total R be methyl groups. 6 When the content is 50 mol % or more, the compatibility with the (A) component and the (B) component is excellent, and the release agent composition does not become cloudy and does not undergo phase separation. In the above average composition formula (3), p, q, r, s, t, u, and v are each independently a number of 0 or more, and are 0≦p, 0≦q, 0≦p+q, 0≦r, 40≦s, 90≦r+s≦400, 0≦t≦8, 2≦q+r+t, 0≦u≦8, 0≦v≦8, and 0≦u+v≦8. Preferably, 0≦p≦20, 0≦q≦20, 0≦p+q≦20, 3≦r≦60, 50≦s≦200, 95≦r+s≦250, 0≦t≦5, 5≦q+r+t≦70, 0≦u≦5, 0≦v≦5, and 0≦u+v≦5.
[0066] The component (D) has at least two SiH groups in one molecule, usually 2 to 200, and preferably 3 to 100. The SiH groups may be located at either the terminal or intermediate portions of the molecular chain, or may be located at both. The molecular structure of the organohydrogenpolysiloxane may be linear, cyclic, branched, or a three-dimensional network structure, and the number of silicon atoms (or degree of polymerization) in one molecule is usually 100 to 300, and preferably about 100 to 200.
[0067] Examples of organohydrogenpolysiloxanes represented by the above average composition formula (3) include methylhydrogensiloxane-dimethylsiloxane cyclic copolymers, dimethylsiloxane-methylhydrogensiloxane copolymers capped at both ends with trimethylsiloxy groups, dimethylpolysiloxanes capped at both ends with dimethylhydrogensiloxane groups, dimethylsiloxane-methylhydrogensiloxane copolymers capped at both ends with dimethylhydrogensiloxy groups, and methylhydrogensiloxane-diphenylsiloxane copolymers capped at both ends with trimethylsiloxy groups. , methylhydrogensiloxane-diphenylsiloxane-dimethylsiloxane copolymers both ends blocked with trimethylsiloxy groups, methylhydrogensiloxane-methylphenylsiloxane-dimethylsiloxane copolymers both ends blocked with trimethylsiloxy groups, methylhydrogensiloxane-dimethylsiloxane-diphenylsiloxane copolymers both ends blocked with dimethylhydrogensiloxy groups, methylhydrogensiloxane-dimethylsiloxane-methylphenylsiloxane copolymers both ends blocked with dimethylhydrogensiloxy groups, etc. Component (D) may be used alone or in combination of two or more types.
[0068] Examples of the component (D) include cyclic siloxanes or linear siloxanes represented by the following formulas. [ka]
[0069] [ka]
[0070] [ka]
[0071] [ka]
[0072] [ka]
[0073] [(E) Platinum group metal catalyst] The platinum group metal catalyst of component (E) is a catalyst for promoting the addition reaction of component (A), component (B), and component (C) with component (D), and any catalyst known to those skilled in the art for promoting the so-called hydrosilylation reaction can be used. Such platinum group metal catalysts include, for example, platinum-based, palladium-based, rhodium-based, and ruthenium-based catalysts, and among these, platinum-based catalysts are particularly preferred. Examples of the platinum catalyst include chloroplatinic acid, alcoholic or aldehyde solutions of chloroplatinic acid, complexes of chloroplatinic acid with various olefins or vinylsiloxanes, and complexes of platinum with various olefins or vinylsiloxanes.
[0074] The amount of component (E) to be blended should be what is called an effective amount as a catalyst, for example, in order to obtain a good cured coating and from an economical standpoint, the amount should be in the range of 0.1 to 1000 ppm, more preferably 1 to 500 ppm, calculated as the mass of platinum group metal relative to the total mass of components (A), (B), (C) and (D).
[0075] [Other ingredients] The release agent composition of the present invention may contain any other components in addition to the above components (A) to (E). For example, the following components may be included. Each of these other components may be used alone or in combination of two or more.
[0076] Alkenyl-containing compounds other than components (A), (B) and (C) In addition to the components (A), (B) and (C), the composition of the present invention may appropriately contain an alkenyl-containing compound that undergoes an addition reaction with the component (D). Such an alkenyl-containing compound other than the components (A), (B) and (C) is preferably one that is involved in the formation of a cured product, and may be an organopolysiloxane other than the components (A), (B) and (C) that has at least one alkenyl group per molecule. The molecular structure may be, for example, linear, cyclic, branched, or three-dimensional network. In particular, it is preferable to contain 0 to 20 parts by mass of the component (F) having the following structure.
[0077] [ka] (1≦p≦20, X is a group selected from a methyl group, a methoxy group, and a vinyl group, or an oxygen atom that gives a cyclic structure) The term "oxygen atom gives a cyclic structure" means that when X is an oxygen atom, the Si on the left and right sides of the formula are linked to O via a siloxane bond to form a cyclic structure.
[0078] Addition reaction regulator In order to ensure pot life, an addition reaction inhibitor can be blended into the composition of the present invention. The addition reaction inhibitor is not particularly limited as long as it is a compound that has a curing inhibitory effect against the platinum group metal catalyst (E), and conventionally known ones can be preferably used. For example, phosphorus-containing compounds such as triphenylphosphine; nitrogen-containing compounds such as tributylamine, tetramethylethylenediamine, and benzotriazole; sulfur-containing compounds; acetylene-based compounds such as acetylene alcohols (e.g., 1-ethynylcyclohexanol, 3,5-dimethyl-1-hexyne-3-ol); compounds containing two or more alkenyl groups; hydroperoxy compounds; maleic acid derivatives, etc. are mentioned. The degree of the curing inhibitory effect of the addition reaction inhibitor varies depending on its chemical structure. Therefore, the amount of each addition reaction inhibitor used can be appropriately adjusted according to a conventionally known method. By adding an appropriate amount of the addition reaction inhibitor, the release agent composition has better long-term storage stability at room temperature and heat curing properties.
[0079] Other optional ingredients Furthermore, if necessary, known antioxidants, pigments, stabilizers, antistatic agents, defoamers, adhesion improvers, thickeners, or inorganic fillers such as silica may be blended in. The blending amounts may be appropriately selected according to conventional techniques.
[0080] [Removal agent composition] The composition of the present invention preferably has a viscosity at 25°C of 50 to 1000 mPa·s. More preferably, it is 80 to 500 mPa·s. If the viscosity is within the above range, it is preferable because it can be applied when forming a cured coating on a substrate, and a uniform coating can be obtained. Since the composition of the present invention does not require a solvent, it can be made into a solventless release agent composition.
[0081] [Method of manufacturing the composition for release sheet] The method for producing the release agent composition of the present invention is not particularly limited, but a method in which the above components (A) to (D) and any optional components are uniformly mixed in advance and then the catalyst (E) is added immediately before use is preferable in terms of pot life.
[0082] [Release sheet] The present invention further provides a release sheet having a sheet-like substrate and a cured coating formed by curing the release agent composition on one or both sides of the substrate surface. The coating method is not particularly limited, but for example, the composition of the present invention can be applied to one or both sides of a sheet-like substrate such as paper or film at an amount of 0.01 to 100 g / m using a coating method such as coating with a comma coater, lip coater, roll coater, die coater, knife coater, blade coater, rod coater, kiss coater, gravure coater, wire bar coater, screen coating, dip coating, or cast coating. 2 After coating, a cured coating can be formed on the substrate by heating for 1 to 120 seconds at a temperature in the range of 50 to 200° C. When forming release layers on both sides of the substrate, it is preferable to perform the operation of forming a cured coating on each side of the substrate at a time.
[0083] The sheet-like substrate includes paper and various known films. Examples of the substrate include polyethylene laminated paper, glassine paper, wood-free paper, craft paper, and various coated papers such as clay-coated paper, synthetic paper such as Yupo, polyethylene film, polypropylene film such as CPP and OPP, polyester film such as polyethylene terephthalate film, polyamide film, polyimide film, polylactic acid film, polyphenol film, and polycarbonate film. It may also be a process paper for manufacturing artificial leather, ceramic sheet, and double-sided separator. In order to improve the adhesion between these substrates and the release layer (cured film), the substrate surface may be corona-treated, etched, primer-treated, or plasma-treated.
[0084] In more detail, the method for producing the release sheet is, for example, to apply the release agent composition of the present invention to a polylaminated paper substrate in an amount of 1.0 to 1.5 g / m 2 After coating, the coating can be prepared by heating at 140° C. for 30 seconds. The release sheet preferably has a peel strength of 3.0 N / 25 mm or more when a 25 mm wide polyester adhesive tape is attached to the cured film and measured at an angle of 180° and a peel speed of 0.3 m / min. There is no particular upper limit, but if the peel strength is too high, cohesive failure may occur between the adhesive tape and the film, so it can be set to 20.0 N / 25 mm or less. EXAMPLES
[0085] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited thereto. The viscosities listed below are all values measured at 25°C using a B-type rotational viscometer. In the following, parts represent parts by mass. In the following, Me and Vi represent methyl and vinyl groups, respectively.
[0086] The components used in the examples and comparative examples are as follows. In the following, the vinyl value is the number of moles of vinyl groups per 100 g of each component, and the SiH group content is the number of moles of SiH groups per 100 g of each component. The viscosity is the value at 25°C. The bonding order of each siloxane unit shown in parentheses is not limited to the following. Component (A) (A1)(ViMe2SiO 1 / 2 )2(Me2SiO) 120 (ViMeSiO) 18 Vinyl value: 0.187 mol / 100 g, Viscosity: 300 mPa s (A2)(ViMe2SiO 1 / 2 )2(Me2SiO) 95 (ViMeSiO)3 Vinyl value: 0.068 mol / 100 g, Viscosity: 200 mPa s (A3)(ViMe2SiO 1 / 2 )2(Me2SiO) 210 (ViMeSiO) 10 Vinyl value: 0.071 mol / 100 g, Viscosity: 840 mPa s (a4)(ViMe2SiO 1 / 2 )2(Me2SiO)101 Vinyl value: 0.027 mol / 100 g, Viscosity: 190 mPa s (a5)(ViMe2SiO 1 / 2 )3(Me2SiO) 157 (MeSiO 3 / 2 ) Vinyl value: 0.026 mol / 100 g, Viscosity: 250 mPa s (a6)(ViMe2SiO 1 / 2 )2(Me2SiO) 10 Vinyl value: 0.211 mol / 100 g, Viscosity: 9.0 mPa s (a7)(ViMe2SiO 1 / 2 )2(Me2SiO) 60 Vinyl value: 0.039 mol / 100 g, Viscosity: 100 mPa s (B) Component (B1)(MeSiO 1 / 2 ) 0.38 (ViMe2SiO 1 / 2 ) 0.06 (SiO 4 / 2 ) 0.56 Vinyl number: 0.086 mol / 100 g, solid at 25°C (C) Component (C1) 1-Tetradecene (Linearene 14 manufactured by Idemitsu Kosan Co., Ltd.) Vinyl value: 0.51 mol / 100 g, Viscosity: 2.4 mPa s (D) Component (D1)(MeSiO 1 / 2 )2(MeHSiO) 30 (Me2SiO) 70 SiH group content: 1.098mol / 100g, viscosity: 119mPa·s (D2)(MeSiO 1 / 2 )2(MeHSiO) 50 (Me2SiO) 48 SiH group content: 0.791mol / 100g, viscosity: 118mPa·s (E) Component (E1) Catalyst: Platinum-vinylsiloxane complex Ingredient (F) (F1)(MeSiO 3 / 2 -ViMe2SiO 1 / 2 )n Vinyl value: 0.53 mol / 100 g, viscosity: 25 mPa s (G) Ingredients (other ingredients) (G1) Addition reaction inhibitor (pot life extender): 1-ethynylcyclohexanol
[0087] [Example 1] Above (A1) average formula: (ViMe2SiO 1 / 2 )2(Me2SiO) 120 (ViMeSiO 1 / 2 ) 18 and the linear dimethylpolysiloxane represented by the above average formula (B1) (Me3SiO 1 / 2 ) 0.38 (ViMe2SiO 1 / 2 ) 0.06 (SiO 4 / 2 ) 0.56 The xylene was removed from the mixture at 150° C. under reduced pressure of 20 mmHg or less, and the mixture was cooled. Then, 6.0 parts by mass of (C1) 1-tetradecene and (D1) an organosiloxane having the average formula: (Me3SiO 1 / 2 )2(MeHSiO) 30 (Me2SiO) 70 A transparent liquid was obtained by mixing 25.2 parts by mass of a methylhydrogenpolysiloxane represented by the formula: (a) (2.8 parts by mass of the above (F)) and 0.2 parts by mass of the above (G) 1-ethynylcyclohexanol. (The molar ratio of SiH groups in component (D1) to the total molar amount of alkenyl groups in components (A1), (B1) and (C1), i.e., H / Vi, was 1.8.) The catalyst (E) was added to the mixture obtained above in an amount of 100 ppm, calculated as platinum mass, relative to the total mass of the components (A1), (B1), (C1), and (D1), and the mixture was stirred and mixed to obtain a transparent composition having a viscosity of 223 mPa s.
[0088] [Examples 2 to 6, Comparative Examples 1 to 4] Using the same procedure as in Example 1, components (A) and (B) were mixed in the compositions shown in Tables 1 and 2 below, and then the xylene in component (B) was removed by distillation under reduced pressure. Components (C), (D), (F) and (G) were then mixed, and then a platinum catalyst (E) was added to obtain compositions of Examples 2 to 6 and Comparative Examples 1 to 4. The amounts of each component are shown in Tables 1 and 2 below. Using the obtained compositions, coated products (release sheets) were produced and evaluated by the methods described below.
[0089] [Peeling force] The obtained composition was applied to the surface of polyethylene laminated paper in an amount of 1.0 to 1.1 g / m 2 The resulting cured film was then subjected to separator aging at 25°C for 1 day, after which a 25mm wide polyester adhesive tape (NO. 31B 75 High, product name of Nitto Denko) was attached to the surface of the cured film and heated at 70°C with a load of 20gf / cm. 2 The tape was then aged for one day at 100° C. One end of the tape was then peeled off, and the end was pulled at an angle of 180° to the polyethylene laminated paper substrate at a peeling speed of 0.3 m / min to measure the peel strength (N / 25 mm) using a tensile tester. The tensile tester used was an AGS-50G model manufactured by Shimadzu Corporation. [Residual adhesion rate] A 25mm wide polyester adhesive tape (No. 31B75 High, product name of Nitto Denko) was attached to the surface of the cured film after separator aging, and the tape was subjected to a load of 20gf / cm at 70℃. 2The tape was peeled off from the cured film, and was laminated on a 25 μm PET film, and pressed once with a 2 kg tape roller, and then peeled off at an angle of 180° at 0.3 m / min using a tensile tester, and the force F (N / 25 mm) required for peeling was measured. For comparison, the polyester adhesive tape was laminated on a Teflon (registered trademark) plate instead of the cured film, and the force F0 (N / 25 mm) required for peeling was measured in the same manner as above. The percentage of adhesive strength remaining in the polyester adhesive tape after peeling from the release layer compared to the polyester adhesive tape peeled from the Teflon (registered trademark) plate (residual adhesive rate (%)) was calculated by the formula: F / F0×100. [Whether or not gel occurs in the treatment bath] After preparing the composition excluding component (E) shown in Tables 1 and 2 below, component (E) was added and stirred, and then it was checked whether any silicone gel matter was attached to or floating on the walls of the treatment bath container or in the treatment bath. If no silicone gel matter was found, it was marked with an ◯, and if a silicone gel matter was found, it was marked with an ×. The results are shown in Tables 1 and 2.
[0090] [Table 1]
[0091] [Table 2]
[0092] The results of Examples 1 to 6 show that the release agent composition of the present invention has a viscosity of 500 mPa·s or less at 25°C, which is suitable for a solvent-free heavy release agent composition. The release sheet obtained using the composition has a high release force of 3.0 N / 25 mm or more. In addition, the use of an organopolysiloxane having a high vinyl value while having side-chain alkenyl groups with reduced addition reactivity can suppress the generation of silicone gel immediately after the preparation of the composition. On the other hand, in the systems using organopolysiloxanes with no alkenyl groups in the side chains and low vinyl values (Comparative Examples 1, 2, and 4), the crosslinking density is low, resulting in a weak peeling force. In the system using a short-chain polyorganosiloxane containing alkenyl groups at both ends (Comparative Example 3), although a high peeling force is shown, the high reactivity of the system makes it easy for silicone gel to be generated after the treatment bath is prepared. From the above results, the compositions shown in Comparative Examples 1 to 4 are not suitable for the intended uses of the present invention.
[0093] The present specification includes the following aspects. [1]: A release agent composition comprising the following components (A) to (E): (A) a linear or branched organopolysiloxane having at least three alkenyl groups bonded to silicon atoms in a side chain per molecule, a viscosity at 25°C of 100 mPa s or more, and a vinyl value of 0.05 to 0.3 mol / 100 g: 20 to 65 parts by mass per 100 parts by mass of the combined total of said component (A) and the following component (B), (B)R'3SiO 1 / 2 Units and SiO 4 / 2 Units and / or R'SiO 3 / 2 an organopolysiloxane having a three-dimensional network structure and having at least two alkenyl groups bonded to silicon atoms in each molecule (in each of the above formulas, R' is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 12 carbon atoms which may have an unsaturated bond): 35 to 80 parts by mass per 100 parts by mass of the combined total of the component (A) and the component (B); (C) an olefin that is liquid at 25°C: 0 to 20 parts by mass per 100 parts by mass of the total of the components (A) and (B), (D) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms per molecule: an amount such that the ratio of the number of hydrogen atoms bonded to silicon atoms in component (D) to the total number of alkenyl groups in components (A), (B), and (C) is 0.5 to 5; and (E) Platinum group metal catalyst: an effective amount [2]: The component (A) is represented by the following average composition formula (1): (R 2 3SiO1 / 2 ) a (R 1 R 2 2SiO 1 / 2 ) b (R 1 R 2 SiO) c (R 2 2SiO) d (R 1 SiO 3 / 2 ) e (R 2 SiO 3 / 2 ) f (SiO 4 / 2 ) g (1) (In the formula, R 1 each independently represents an alkenyl group; R 2 are independently an unsubstituted or substituted monovalent hydrocarbon group not containing an alkenyl group, and a, b, c, d, e, f and g are each independently a number of 0 or more and are represented by the following expressions: 0≦a, 0≦b, 2≦a+b, 3≦c, 50≦d, 90≦c+d≦400, 0≦e≦8, 3≦b+c+e, 0≦f≦8, 0≦g≦8, 0≦f+g≦8. [3]: The stripping composition according to [1] or [2], wherein the component (B) is represented by the following average composition formula (2): (R 4 3SiO 1 / 2 ) h (R 3 R 4 2SiO 1 / 2 ) i (R 3 R 4 SiO) j (R 4 2SiO) k (R 3 SiO 3 / 2 ) l (R 4 SiO 3 / 2 ) m (SiO 4 / 2 ) n (2) (In the formula, R 3 are each independently an alkenyl group having 2 to 8 carbon atoms, and R 4are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms that is not an alkenyl group, provided that all R 4 at least 80 mol % of the groups are methyl groups, and h, i, j, k, l, m, and n are each independently a number equal to or greater than 0, provided that i+j+l>0, l+m+n>0, and h+i+j+k+l+m+n=1. [4]: The stripping composition according to any one of [1] to [3], wherein the component (C) is a linear monoolefin having 10 to 18 carbon atoms or a branched monoolefin having 10 or more carbon atoms. [5]: The component (D) is represented by the following average composition formula (3): (R 6 3SiO 1 / 2 ) p (R 5 R 6 2SiO 1 / 2 ) q (R 5 R 6 SiO) r (R 6 2SiO) s (R 5 SiO 3 / 2 ) t (R 6 SiO 3 / 2 ) u (SiO 4 / 2 ) v (3) (In the formula, R 5 each independently represents a hydrogen atom; R 6 are independently an unsubstituted or substituted monovalent hydrocarbon group other than a hydrogen atom, and p, q, r, s, t, u and v are each independently a number equal to or greater than 0, and are represented by the following expressions: 0≦p, 0≦q, 0≦p+q, 0≦r, 40≦s, 90≦r+s≦400, 0≦t≦8, 2≦q+r+t, 0≦u≦8, 0≦v≦8, 0≦u+v≦8), which is a linear or branched organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in side chains per molecule and having a viscosity at 25°C of 100 mPa s or greater. [6]: The release agent composition according to any one of [1] to [5], comprising 0 to 20 parts by mass of an organopolysiloxane (F) represented by the following formula, where 1≦p≦20, and X is a group selected from a methyl group, a methoxy group, and a vinyl group, or an oxygen atom that gives a cyclic structure. [ka] [7]: The stripping composition according to any one of [1] to [6], which has a viscosity at 25°C of 50 to 1000 mPa·s. [8]: The stripping composition according to any one of [1] to [7], which does not contain a solvent. [9]: A release sheet having a sheet-like substrate and a cured coating formed on one or both surfaces of the substrate by curing the release agent composition according to any one of [1] to [8].
[10] : The release sheet according to [9], which has a peel strength of 3.0 N / 25 mm or more when a 25 mm wide polyester adhesive tape is attached to the cured coating and measured at an angle of 180° and a peel speed of 0.3 m / min.
[0094] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.
Claims
1. A stripping agent composition comprising the following components (A) to (E): (A) a linear or branched organopolysiloxane having at least three alkenyl groups bonded to silicon atoms in a side chain per molecule, a viscosity at 25° C. of 100 mPa·s or more, and a vinyl value of 0.05 or more and 0.3 mol / 100 g or less: 20 to 65 parts by mass per 100 parts by mass of the total of said component (A) and the following component (B), (B) R' 3 SiO 1/2 Units and SiO 4/2 Units and / or R'SiO 3/2 an organopolysiloxane having a three-dimensional network structure and having an alkyl group, the alkyl group having an alkyl group bonded to a silicon atom in each molecule being at least two alkenyl groups bonded to silicon atoms (in each of the above formulae, R' is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 12 carbon atoms which may have an unsaturated bond): 35 to 80 parts by mass per 100 parts by mass of the total of the component (A) and the component (B); (C) an olefin that is liquid at 25° C.: 0 to 20 parts by mass per 100 parts by mass of the total of the components (A) and (B), (D) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms per molecule: an amount such that the ratio of the number of hydrogen atoms bonded to silicon atoms in component (D) to the total number of alkenyl groups in components (A), (B), and (C) is 0.5 to 5; and (E) Platinum group metal catalyst: effective amount
2. The component (A) has the following average composition formula (1): (R 2 3 SiO 1/2 ) a (R 1 R 2 2 SiO 1/2 ) b (R 1 R 2 SiO) c (R 2 2 SiO) d (R 1 SiO 3/2 ) e (R 2 SiO 3/2 ) f (SiO 4/2 ) g (1) (In the formula, R 1 each independently represents an alkenyl group; R 2 are independently an unsubstituted or substituted monovalent hydrocarbon group not containing an alkenyl group, and a, b, c, d, e, f and g are each independently a number of 0 or more and are represented by the following expressions: 0≦a, 0≦b, 2≦a+b, 3≦c, 50≦d, 90≦c+d≦400, 0≦e≦8, 3≦b+c+e, 0≦f≦8, 0≦g≦8, 0≦f+g≦8.
3. The stripping composition according to claim 1 , wherein the component (B) is represented by the following average composition formula (2): (R 4 3 SiO 1/2 ) h (R 3 R 4 2 SiO 1/2 ) i (R 3 R 4 SiO) j (R 4 2 SiO) k (R 3 SiO 3/2 ) l (R 4 SiO 3/2 ) m (SiO 4/2 ) n (2) (In the formula, R 3 are each independently an alkenyl group having 2 to 8 carbon atoms; R 4 are each independently a non-alkenyl, unsubstituted or substituted, monovalent hydrocarbon group having 1 to 12 carbon atoms, provided that all R 4 are methyl groups; and h, i, j, k, l, m, and n are each independently a number equal to or greater than 0, provided that i+j+l>0, l+m+n>0, and h+i+j+k+l+m+n=1.
4. 2. The stripping composition according to claim 1, wherein the component (C) is a linear monoolefin having 10 to 18 carbon atoms or a branched monoolefin having 10 or more carbon atoms.
5. The component (D) is represented by the following average composition formula (3): (R 6 3 SiO 1/2 ) p (R 5 R 6 2 SiO 1/2 ) q (R 5 R 6 SiO) r (R 6 2 SiO) s (R 5 SiO 3/2 ) t (R 6 SiO 3/2 ) u (SiO 4/2 ) v (3) (In the formula, R 5 each independently represents a hydrogen atom; R 6 are independently an unsubstituted or substituted monovalent hydrocarbon group other than a hydrogen atom, and p, q, r, s, t, u and v are each independently a number of 0 or more, and are a linear or branched organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in side chains per molecule and having a viscosity at 25° C. of 100 mPa·s or more, wherein 0≦p, 0≦q, 0≦p+q, 0≦r, 40≦s, 90≦r+s≦400, 0≦t≦8, 2≦q+r+t, 0≦u≦8, 0≦v≦8, 0≦u+v≦8.
6. The release agent composition according to claim 1, comprising 0 to 20 parts by mass of an organopolysiloxane (F) represented by the following formula: where 1≦p≦20, and X is a group selected from a methyl group, a methoxy group, and a vinyl group, or an oxygen atom that gives a cyclic structure. 【Chemistry 1】
7. The stripping composition according to claim 1, which has a viscosity at 25° C. of 50 to 1000 mPa·s.
8. The stripper composition of claim 1 which is solvent-free.
9. A release sheet comprising a sheet-like substrate and a cured coating formed on one or both surfaces of the substrate by curing the release agent composition according to any one of claims 1 to 8.
10. 10. The release sheet according to claim 9, which has a peel strength of 3.0 N / 25 mm or more when a 25 mm wide polyester adhesive tape is attached to the cured coating and measured at an angle of 180° and a peel speed of 0.3 m / min.
Citation Information
Patent Citations
Release modifier composition
JP2017523258A
Oil-in-water silicone emulsion composition for release film, release film, and method for producing the release film, method for adjusting coatability, and peelability in release film
JP2020139040A
Compositions for preparing release coatings, release coating compositions, and related methods
JP2023508494A
Release coatings, compositions for preparing release coating compositions, and related methods
JP2023508668A
Curable siloxane composition with modified surface properties
JP2007523225A
Cited By
Hair iron
JP2026060146A
