Dry film, integrated type sealing sheet, light-emitting type electronic component, and method for manufacturing light-emitting type electronic component

The use of a layered dry film with specific elastic properties addresses the challenges of resin removal and brightness uniformity in mini LED and micro LED components, achieving efficient and cost-effective manufacturing without etching, ensuring consistent brightness and reduced production costs.

JP2024168732AActive Publication Date: 2024-12-05SHIN ETSU POLYMER CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023085636
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-12-05
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

Existing methods for manufacturing mini LED and micro LED electronic components face challenges such as time-consuming etching processes, difficulty in completely removing resin from light-emitting elements, and potential brightness loss due to residual adhesive layers, leading to uneven brightness and increased costs.

Method used

A dry film with a layered structure comprising a low-elastic black curable resin layer, a low-elastic transparent curable resin layer, and a high-elastic transparent curable resin layer is used, which is bonded to the substrate without etching, ensuring uniform adhesion and removal of the black adhesive layer, even with varying light-emitting element heights and tilts.

Benefits of technology

This approach eliminates the need for time-consuming etching, maintains consistent brightness, and reduces production costs while ensuring high brightness and uniformity across the display, without compromising energy efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168732000001_ABST
    Figure 2024168732000001_ABST
Patent Text Reader

Abstract

To provide a dry film which allows sufficiently filling light elements with a low elastic black curable resin layer, can be cured at a normal curing temperature in a normal curing time, and prevents poor appearance after curing and generation of a spot caused by partially lowering brightness, and an integrated type sealing sheet, a light-emitting type electronic component and a method for manufacturing a light-emitting type electronic component using the dry film.SOLUTION: A dry film includes a low elastic black curable resin layer 1, a low elastic transparent curable resin layer 2 and a high elastic transparent curable resin layer 3, wherein the total light transmittance of the low elastic black curable resin layer 1 is 0 to 30%, the total light transmittance of the sum of the low elastic transparent curable resin layer 2 and the high elastic transparent curable resin layer 3 is 70 to 99%, and the storage elastic modulus of the high elastic transparent curable resin layer 3 is larger than the storage elastic moduli of the low elastic black curable resin layer 1 and the low elastic transparent curable resin layer 2, at 100°C and 150°C.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dry film, an integrated encapsulating sheet, a light-emitting electronic component, and a method for manufacturing a light-emitting electronic component. [Background technology]

[0002] In recent years, display technologies that use extremely small light-emitting diodes, known as mini-LED and micro-LED, have been attracting attention. Mini LEDs and micro LEDs can be used in two ways. One is a technology that allows the brightness of a liquid crystal backlight to be controlled locally by configuring a large number of LEDs arranged on a substrate. The other system uses LEDs of the respective colors to emit the R (red), G (green), and B (blue) that make up a pixel, and the high-purity colors emitted by the LEDs of each color reach the eye as is.

[0003] Mini LEDs and micro LEDs use electronic components in which multiple light-emitting elements are arranged on a substrate. In such electronic components, a dry film is used to fill the spaces between the multiple light-emitting elements with a resin that prevents light diffusion (Patent Document 1). A dry film is a resin film obtained by applying and drying a curable resin composition onto a protective film, which is then pressed onto the surface of the substrate on which the light-emitting elements are arranged, filling the spaces between the light-emitting elements, and then cured.

[0004] In Patent Document 1, in order to prevent light diffusion between a plurality of light emitting elements, a resin having light diffusion preventing properties is used as a dry film. When a dry film made of a light-diffusion preventing resin is pressure-attached to the surface of the substrate on which the light-emitting elements are arranged, a light-diffusion preventing resin layer is inevitably formed not only between the light-emitting elements but also on the light-emitting elements.

[0005] If the resin layer having light diffusion prevention properties formed on the light emitting elements is left as it is, not only will light be diffused between the light emitting elements, but light that should be emitted toward the viewer will also be blocked. Therefore, Patent Document 1 describes that after the dry film is pressed, the resin on the light-emitting element is removed by etching such as plasma treatment, and the exposed light-emitting element is covered with a light-transmitting sealant.

[0006] Therefore, Patent Document 2 describes how by using a two-layer dry film consisting of a black adhesive layer that is lower than the height of the light-emitting element and a transparent adhesive layer that has a higher melting point than the black adhesive layer, the black adhesive layer on the light-emitting element can be washed away by the transparent adhesive layer that is melted later, and the transparent adhesive layer can be pressed against the bottom of the substrate between the light-emitting elements, so that no black adhesive layer remains on the light-emitting element. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent Publication No. 2022-22562 [Patent Document 2] China Patent Application Publication No. 115084320 Summary of the Invention [Problem to be solved by the invention]

[0008] However, when etching such as plasma treatment is performed as in Patent Document 1, it takes a lot of time, which is a factor in increasing manufacturing costs. In addition, it is difficult to completely remove the resin on the light-emitting element by etching, and there is a risk of partial reduction in brightness and unevenness. Furthermore, in order to provide a sealant layer on the outermost surface, an additional step of laminating a dry film of the sealant is required.

[0009] Furthermore, Patent Document 2 states that the black adhesive layer on the light-emitting elements can be washed away by the transparent adhesive layer and pressed against the bottom of the substrate between the light-emitting elements, so that the black adhesive layer does not remain on the light-emitting elements. However, when mounting the light-emitting elements with solder, differences in the inclination and height of the light-emitting elements occur, so the transparent adhesive layer cannot wash away the black adhesive layer evenly, and the black adhesive layer remains on some of the light-emitting elements, reducing brightness.

[0010] In view of the above circumstances, the present invention aims to provide a dry film that can omit a time-consuming etching process such as plasma treatment and that suppresses a decrease in brightness even if the inclination or height of each light-emitting element differs from one light-emitting element to another, an integrated encapsulating sheet using this dry film, a light-emitting electronic component, and a method for manufacturing a light-emitting electronic component. [Means for solving the problem]

[0011] In order to achieve the above object, the present invention employs the following configuration. [1] A dry film that is pressure-bonded to a surface of a substrate having a plurality of light-emitting elements arranged thereon, the surface having the plurality of light-emitting elements arranged thereon, The dry film includes a low-elasticity black curable resin layer, a low-elasticity transparent curable resin layer, and a high-elasticity transparent curable resin layer, which are laminated in this order from the side that will be in direct contact with the element-mounted substrate during the pressure bonding. [2] The dry film according to [1], wherein at 100°C, the storage modulus of the high elasticity transparent curable resin layer is greater than the storage modulus of the low elasticity transparent curable resin layer and the low elasticity black curable resin layer. [3] The dry film according to [1] or [2], wherein the storage modulus of the low elasticity transparent curable resin layer is greater than the storage modulus of the low elasticity black curable resin layer at 100°C. [4] The storage modulus of the highly elastic transparent curable resin layer at 100° C. is 1.0×10 7 The dry film according to any one of [1] to [3], wherein the viscosity is 0.01 Pa or less. [5] The storage modulus of the low elasticity black curable resin layer is 1.0 × 10 at 100 ° C. 5The dry film according to any one of [1] to [4], wherein the viscosity is 0.01 Pa or less. [6] The storage modulus of the low elasticity transparent curable resin layer is 1.0 × 10 at 100 °C. 5 The dry film according to any one of [1] to [5], wherein the viscosity is 0.01 Pa or less. [7] The storage modulus of the highly elastic transparent curable resin layer is 1.0 × 10 at 150 °C. 5 The dry film according to any one of [1] to [6], wherein the resistance of the dry film is 10 Pa or more. [8] The dry film according to any one of [1] to [7], wherein the low elasticity black curable resin layer has a total light transmittance of 0 to 30%. [9] The dry film according to any one of [1] to [8], wherein the low elasticity, transparent, curable resin layer has a total light transmittance of 50% or more.

[10] The dry film according to any one of [1] to [9], wherein the highly elastic, transparent, curable resin layer has a total light transmittance of 50% or more.

[11] The dry film according to any one of [1] to

[10] , wherein the highly elastic, transparent, curable resin layer contains a high molecular weight epoxy resin.

[12] The dry film according to

[11] , wherein the high molecular weight epoxy resin has a weight average molecular weight of 10,000 to 100,000.

[13] The dry film according to

[11] or

[12] , wherein the highly elastic transparent curable resin layer contains a phenoxy type epoxy resin as the high molecular weight epoxy resin.

[14] The dry film according to any one of

[11] to

[13] , wherein the amount of the high molecular weight epoxy resin is 30 to 80 mass % relative to 100 mass % of the total resin solid content of the highly elastic, transparent, curable resin layer.

[15] The dry film according to any one of [1] to

[14] , wherein the low elasticity black curable resin layer contains an elastomer.

[16] The dry film according to

[15] , wherein the elastomer is a modified elastomer.

[17] The dry film according to

[16] , wherein the modified elastomer is an acid-modified acrylonitrile butadiene rubber.

[18] The dry film according to any one of [1] to

[17] , wherein the low elasticity black curable resin layer contains carbon black.

[19] An integrated sealing sheet comprising the dry film according to any one of [1] to

[18] and a sealing film layer provided on the opposite side of the high elasticity, transparent curable resin layer to the low elasticity, transparent curable resin layer.

[20] The integral sealing sheet according to

[19] , wherein the sealing film layer comprises a support film layer and a hard coat layer provided on the side of the support film layer opposite the highly elastic transparent curable resin layer.

[21] A substrate having a plurality of light-emitting elements arranged on a substrate, and the dry film according to any one of [1] to

[18] , which is pressure-bonded to a surface of the substrate having the light-emitting elements arranged thereon; the low elasticity black cured resin layer, the low elasticity transparent cured resin layer, and a part of the high elasticity transparent cured resin layer are filled between the plurality of light emitting elements; The light-emitting electronic component, in which the low elasticity black curable resin layer, the low elasticity transparent curable resin layer, and the high elasticity transparent curable resin layer are cured.

[22] A substrate having a plurality of light-emitting elements arranged on a substrate, and the integrated encapsulating sheet according to

[19] or

[20] , which is pressure-bonded to a surface of the substrate having the light-emitting elements arranged thereon, the low elasticity black cured resin layer, and a part of the low elasticity transparent cured resin layer and the high elasticity transparent cured resin layer are filled between the plurality of light emitting elements; The light-emitting electronic component, in which the low elasticity black curable resin layer, the low elasticity transparent curable resin layer, and the high elasticity transparent curable resin layer are cured.

[23] A dry film according to any one of [1] to

[18] is placed on a surface of a substrate having a plurality of light-emitting elements arranged thereon, the surface being in contact with the low-elasticity black curable resin layer, and then thermally bonded to the surface by pressure bonding; The low elasticity black curable resin layer, the low elasticity transparent curable resin layer, and the high elasticity transparent curable resin layer are cured by heating.

[24] The method for producing a light-emitting electronic component according to

[23] , wherein the temperature during the thermocompression bonding is 80 to 120°C, and the curing is carried out by heating at 100 to 160°C.

[25] The integrated encapsulating sheet according to

[19] or

[20] is placed on a surface of a substrate on which a plurality of light-emitting elements are arranged, so that the low elasticity black curable resin layer is in contact with the surface, and then thermally bonded to the surface; The low elasticity black curable resin layer, the low elasticity transparent curable resin layer, and the high elasticity transparent curable resin layer are cured by heating.

[26] The method for producing a light-emitting electronic component according to

[25] , wherein the temperature during the thermocompression bonding is 80 to 120°C, and the curing is performed by heating at 100 to 160°C. Effect of the Invention

[0012] According to the dry film or integrated encapsulating sheet of the present invention, even if the inclination or height of each light-emitting element differs, the decrease in brightness can be suppressed without performing etching such as plasma treatment, which takes a lot of time. Furthermore, according to the light-emitting electronic component and the method for manufacturing the light-emitting electronic component of the present invention, a light-emitting electronic component having sufficient brightness and blackness can be obtained without increasing production costs or energy consumption. [Brief description of the drawings]

[0013] [Figure 1] 1 is a schematic cross-sectional view of a dry film according to a first embodiment of the present invention. [Diagram 2] 1A to 1C are schematic explanatory diagrams of a method for manufacturing a light-emitting electronic component according to a first embodiment of the present invention. [Diagram 3] 1A to 1C are schematic explanatory diagrams of a method for manufacturing a light-emitting electronic component according to a first embodiment of the present invention. [Figure 4] 1A to 1C are schematic explanatory diagrams of a method for manufacturing a light-emitting electronic component according to a first embodiment of the present invention. [Diagram 5] 1A to 1C are schematic explanatory diagrams of a method for manufacturing a light-emitting electronic component according to a first embodiment of the present invention. [Figure 6]1A to 1C are schematic explanatory diagrams of a method for manufacturing a light-emitting electronic component according to a first embodiment of the present invention. [Figure 7] FIG. 4 is a schematic cross-sectional view of an integrated encapsulating sheet according to a second embodiment of the present invention. [Figure 8] 5A to 5C are schematic explanatory diagrams of a method for producing a light-emitting electronic component according to a second embodiment of the present invention. [Figure 9] 5A to 5C are schematic explanatory diagrams of a method for producing a light-emitting electronic component according to a second embodiment of the present invention. [Figure 10] 5A to 5C are schematic explanatory diagrams of a method for producing a light-emitting electronic component according to a second embodiment of the present invention. [Figure 11] 5A to 5C are schematic explanatory diagrams of a method for producing a light-emitting electronic component according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] In this specification and claims, the term "main component" refers to a component that accounts for 50% by mass or more of the total solid content of the entire composition. A numerical range expressed by "to" refers to a numerical range with the numerical values ​​before and after "to" as the lower and upper limits.

[0015] First Embodiment <Dry film> A dry film 100 according to the first embodiment will be described with reference to Figures 1 and 2. As shown in Figure 1, the dry film 100 is basically constructed by laminating a low-elasticity black curable resin layer 1, a low-elasticity transparent curable resin layer 2, and a high-elasticity transparent curable resin layer 3. The dry film 100 of this embodiment may further have a protective film on one or both of the surfaces of the low-elasticity black curable resin layer 1 and the high-elasticity transparent curable resin layer 3 for ease of handling.

[0016] 1 shows an example in which protective films are provided on the surfaces of both the low-elasticity black curable resin layer 1 and the high-elasticity transparent curable resin layer 3. Specifically, the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, the high-elasticity transparent curable resin layer 3, and the second protective film 7 are laminated in this order on the first protective film 6.

[0017] 2, the dry film 100 is used to fill spaces between a plurality of light-emitting elements (light-emitting element 12, light-emitting element 13, light-emitting element 14) of an element-mounted substrate 10 in which a plurality of light-emitting elements are arranged on a substrate 11. The details of the element-mounted substrate 10 will be described later. The dry film 100 is used such that the low-elasticity black curable resin layer 1 is in direct contact with the element-mounted substrate 10 during pressure bonding, as shown in FIG. A specific method for obtaining a light-emitting electronic component by pressure-bonding the dry film 100 to the device-mounted substrate 10 will be described later.

[0018] <Low elasticity black curable resin layer> The low-elasticity black curable resin layer 1 is a layer that prevents light diffusion between light-emitting elements and improves the contrast of the display. In addition, this layer is used to sufficiently fill the spaces between multiple light-emitting elements arranged on the element-mounted substrate 10 during the thermocompression bonding process, thereby preventing poor appearance due to expansion of unfilled gaps during the thermal curing process and damage to the light-emitting elements due to external factors in subsequent processes.

[0019] [Total light transmittance] The low elasticity black curable resin layer 1 has a low total light transmittance. The total light transmittance of the low elasticity black curable resin layer 1 is measured in a cured state. The low elasticity black curable resin layer 1 is prepared so that the total light transmittance in a cured state is 0 to 30%. The low elasticity black curable resin layer 1 is preferably prepared so that the total light transmittance in a cured state is 0 to 20%, and more preferably 0 to 10%. When the low elasticity black curable resin layer 1 has a total light transmittance in a cured state of not more than the upper limit, light diffusion between light emitting elements can be prevented.

[0020] The total light transmittance in this specification can be measured by a haze meter. The total light transmittance in the cured state can be adjusted mainly by the presence or absence of a pigment or dye such as carbon black or the amount of the pigment or dye added, as well as by the thickness of the resin layer and the type of resin.

[0021] [Storage modulus] The low elasticity black curable resin layer 1 is in an uncured or semi-cured state before being pressure-bonded to the element-mounted substrate 10 and cured. The storage modulus of the low elasticity black curable resin layer 1 before curing is smaller at 100° C. than the storage modulus of the high elasticity transparent curable resin layer 3 before curing. In addition, it is preferably smaller than the storage modulus of the low elasticity transparent curable resin layer 2 before curing at 100° C.

[0022] The storage modulus of the low elasticity black curable resin layer 1 before curing is 1.0×10 5 Pa or less, and 1.0×10 2 Pa or more, 1.0×10 5 Pa or less, and 1.0×10 3 Pa or higher, 5.0×10 4 It is more preferable that the pressure is 0.1 Pa or less.

[0023] Since the storage modulus at 100°C of the low-elasticity black curable resin layer 1 before curing is equal to or less than the preferred upper limit, sufficient fluidity is obtained when the layer is pressed against the element-mounted substrate 10, and the layer can conform to the unevenness of the element-mounted substrate 10 caused by the multiple light-emitting elements and sufficiently fill in the spaces between the multiple light-emitting elements. By making the storage modulus at 100°C of the low elasticity black curable resin layer 1 before curing equal to or greater than the preferred lower limit, it is possible to prevent uneven pressure during thermocompression bonding and maintain a uniform appearance. In addition, it is possible to prevent the resin from flowing out of the range and ensure the film thickness after compression bonding.

[0024] [Curable resin composition] The low elasticity black curable resin layer 1 is composed of a curable resin composition. The curable resin composition may be a thermosetting resin composition containing at least one resin selected from an epoxy resin, an acrylic resin, a polyester resin, and a polyurethane resin, and a curing agent.

[0025] Among these, an epoxy resin composition is preferred because it can be cured at low temperatures and has excellent heat resistance and reliability. In this specification, the epoxy resin composition refers to a composition containing an epoxy resin as a main component, or a composition containing an epoxy resin and a curing agent as main components.

[0026] (Epoxy resin) In this specification and claims, an epoxy resin is a compound having an epoxy group in the molecule. The epoxy resin used in the present invention is preferably one having two or more epoxy groups in one molecule. This is because a crosslinked structure is formed by reaction with a modified resin having a functional group capable of reacting with an epoxy group, and the cured product can exhibit high heat resistance. In addition, when an epoxy resin having two or more epoxy groups is used, the degree of crosslinking with a curing agent having a functional group capable of reacting with an epoxy group is sufficient, and sufficient heat resistance can be obtained in the cured product.

[0027] Examples of epoxy resins having two or more epoxy groups in one molecule include bifunctional epoxy resins having two epoxy groups in the molecule, polyfunctional epoxy resins having three or more epoxy groups in the molecule, and high molecular weight epoxy resins having a weight average molecular weight of 10,000 or more. Epoxy resins obtained by hydrogenating these may also be used.

[0028] In this specification and claims, high molecular weight epoxy resins are not classified as difunctional epoxy resins or polyfunctional epoxy resins, regardless of the number of epoxy groups in the molecule, but are classified as phenoxy-type epoxy resins. The weight average molecular weight of the epoxy resin is a polystyrene-equivalent molecular weight measured by gel permeation chromatography.

[0029] Examples of epoxy resins include bisphenol-based epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, or phenoxy type epoxy resins obtained by polymerizing these resins, and hydrogenated versions of these resins; novolac type epoxy resins such as phenol novolac epoxy resins, o-cresol novolac epoxy resins, bisphenol A novolac epoxy resins, xylene structure-containing novolac epoxy resins, and naphthol novolac type epoxy resins; glycidyl ester-based epoxy resins such as phthalic acid diglycidyl ester, isophthalic acid diglycidyl ester, terephthalic acid diglycidyl ester, p-hydroxybenzoic acid glycidyl ester, tetrahydrophthalic acid diglycidyl ester, succinic acid diglycidyl ester, adipic acid diglycidyl ester, sebacic acid diglycidyl ester, and trimellitic acid triglycidyl ester; ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycidyl ether-based epoxy resins such as tetraglycidyl diglycidyl ether, trimethylolpropane triglycidyl ether, pentaerythritol tetraglycidyl ether, tetraphenyl glycidyl ether ethane, triphenyl glycidyl ether ethane, polyglycidyl ether of sorbitol, and polyglycidyl ether of polyglycerol; glycidyl amine-based epoxy resins such as triglycidyl isocyanurate and tetraglycidyl diaminodiphenylmethane; linear aliphatic epoxy resins such as epoxidized polybutadiene and epoxidized soybean oil; and special skeleton epoxy resins such as brominated bisphenol A type epoxy resins, phosphorus-containing epoxy resins, fluorine-containing epoxy resins, dicyclopentadiene skeleton-containing epoxy resins, naphthalene skeleton-containing epoxy resins, anthracene type epoxy resins, tertiary butyl catechol type epoxy resins, triphenylmethane type epoxy resins, tetraphenylethane type epoxy resins, biphenyl type epoxy resins, and bisphenol S type epoxy resins. However, the epoxy resins are not limited to these.

[0030] As the high molecular weight epoxy resin, a phenoxy type epoxy resin, an epoxy modified polybutadiene, a copolymer of glycidyl methacrylate and methyl methacrylate, a modified polymer obtained by epoxy modifying other resins, and the like can be used. These epoxy resins may be used alone or in combination of two or more.

[0031] Among the above epoxy resins, the epoxy resin used in the low elasticity black curable resin layer 1 is preferably a multifunctional epoxy resin from the viewpoint of increasing the crosslink density after curing. Among the polyfunctional epoxy resins, novolac-type epoxy resins are particularly preferred because they are epoxy resins to which a moderately flexible skeleton can be introduced and whose flexibility and softening point can be adjusted, making the cured product less susceptible to brittle fracture, improving the stability of performance over long-term use of the cured product of the epoxy resin composition, increasing the crosslink density, and improving heat resistance.

[0032] Specific examples of novolac-type epoxy resins include "YX7700" manufactured by Mitsubishi Chemical Corporation, "NC7000L", "XD1000", and "EOCN-1020" manufactured by Nippon Kayaku Co., Ltd., "ESN485" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "N-690", "N-695", "HP-7200H", and "HP-7200L" manufactured by DIC Corporation.

[0033] The amount of the polyfunctional epoxy resin in the low elasticity black curable resin layer 1 is preferably 10 to 99% by mass, more preferably 40 to 95% by mass, and even more preferably 60 to 90% by mass, based on 100% by mass of the total resin solid content of the low elasticity black curable resin layer 1. When the amount is equal to or greater than the lower limit, the crosslinking density can be increased to provide chemical resistance and heat resistance. When the amount is equal to or less than the upper limit, the storage modulus during thermocompression bonding can be adjusted, and the fluidity of the low elasticity black curable resin layer 1 can be ensured.

[0034] It is preferable that the low elasticity black curable resin layer 1 does not contain a high molecular weight epoxy resin, or if it does contain one, it contains it in an amount less than that of the high elasticity transparent curable resin layer 3. This makes it easier to ensure sufficient fluidity during thermocompression bonding.

[0035] The amount of the high molecular weight epoxy resin in the low elasticity black curable resin layer 1 is preferably less than 50 mass%, more preferably less than 30 mass%, and even more preferably less than 10 mass%, relative to 100 mass% of the total resin solid content of the low elasticity black curable resin layer 1.

[0036] From the viewpoint of ensuring sufficient fluidity during thermocompression bonding, the low elasticity black curable resin layer 1 preferably contains an epoxy resin having a softening point or melting point of 100° C. or less. From the viewpoint of handleability and heat resistance of the cured product, it is more preferable that the low elasticity black curable resin layer 1 contains an epoxy resin having a softening point or melting point of 50 to 95° C. By containing an epoxy resin having a softening point or melting point within the above range, it becomes possible to control the storage modulus.

[0037] The total amount of epoxy resin in the low elasticity black curable resin layer 1 is preferably 10 to 100% by mass, more preferably 20 to 99% by mass, and even more preferably 35 to 95% by mass, relative to 100% by mass of the total resin solid content of the low elasticity black curable resin layer 1. Within the above range, the storage modulus can be controlled, and appropriate fluidity during thermocompression bonding can be ensured. Furthermore, if it is equal to or greater than the above lower limit, heat resistance after curing can be improved.

[0038] (Elastomer) The low elasticity black curable resin layer 1 preferably contains an elastomer in addition to a resin such as an epoxy resin, etc. By containing an elastomer, it becomes easier to control the storage modulus, that is, to control the fluidity.

[0039] As the elastomer, a thermosetting elastomer, generally called "rubber", is preferred because it provides excellent heat resistance. Examples of thermosetting elastomers include acrylonitrile butadiene rubber (NBR), which is a random copolymer of butadiene and acrylonitrile, acrylic rubber, styrene butadiene rubber, vinyl acetate resin, silicone resin, etc. Among them, NBR is preferred because it has good compatibility with epoxy resins, allows control of the fluidity of the low-elasticity black curable resin layer 1 at around 100°C, and has good adhesion to the low-elasticity transparent curable resin layer 2 and the element-mounted substrate 10.

[0040] The weight average molecular weight of the elastomer is preferably 100,000 to 1,000,000, more preferably 120,000 to 500,000, and even more preferably 150,000 to 300,000. When the weight average molecular weight of the elastomer is within the above range, the storage modulus of the low elasticity black curable resin layer 1 can be controlled, and the flowability during thermocompression bonding can be ensured. When the weight average molecular weight of the elastomer is equal to or less than the above upper limit, the compatibility with the epoxy resin is improved, and the flowability during thermal curing can be more effectively controlled.

[0041] In particular, when the low elasticity black curable resin layer 1 is composed of an epoxy resin composition, it is preferable to include a modified elastomer having a functional group capable of reacting with an epoxy group. If there is a modified elastomer having a functional group capable of reacting with an epoxy group, it also acts as a curing agent for the epoxy resin. In addition, since it can react and bond with the epoxy resin, the heat resistance and reliability against thermal shock are improved. Furthermore, the difference in polarity between the functional group capable of reacting with the epoxy resin and the resin skeleton has a favorable effect on dispersibility, and good dispersibility can be obtained when carbon black is contained in the low elasticity black curable resin layer 1.

[0042] Examples of functional groups capable of reacting with an epoxy group include acid groups such as a carboxy group, a sulfo group, a nitro group, and a phosphoric acid group, as well as their acid anhydride groups, a hydroxyl group, and an amino group. Among these, an acid group or an acid anhydride group is preferred, and a carboxy group or a carboxylic acid anhydride group is particularly preferred, since they can be cured at low temperatures and can ensure a long pot life.

[0043] That is, when the low elasticity black curable resin layer 1 is composed of an epoxy resin composition, it preferably contains an acid-modified elastomer having an acid group or an acid anhydride group, more preferably contains an acid-modified elastomer having a carboxy group, and particularly preferably contains an acid-modified acrylonitrile butadiene rubber (acid-modified NBR) having a carboxy group.

[0044] The acid-modified NBR having a carboxy group is preferably a carboxylated acrylonitrile rubber into which acrylic acid, methacrylic acid, maleic anhydride, etc. are introduced. Commercially available products of the carboxylated acrylonitrile rubber include Nipol (registered trademark) NX775 and Nipol 1072CGJ manufactured by Zeon Corporation. Two or more types of modified elastomers having a functional group capable of reacting with an epoxy group may be used in combination.

[0045] The amount of elastomer blended in the low elasticity black curable resin layer 1 is preferably greater than the amount of elastomer blended in the high elasticity transparent curable resin layer 3. This allows the storage modulus of the low elasticity black curable resin layer 1 during thermocompression bonding to be adjusted to an appropriate range lower than that of the high elasticity transparent curable resin layer 3, and flow during thermal curing to be suppressed, when the low elasticity black curable resin layer 1 contains a large amount of low molecular weight components such as polyfunctional epoxy. As a result, the low elasticity black curable resin layer 1 can have sufficient flowability during thermocompression bonding and can be prevented from flowing out during thermal curing.

[0046] The amount of the elastomer in the low elasticity black curable resin layer 1 is preferably 0.01 to 90% by mass, more preferably 1 to 80% by mass, and even more preferably 5 to 65% by mass, based on 100% by mass of the total resin solid content of the low elasticity black curable resin layer 1. Within the above range, the storage modulus can be controlled, and appropriate fluidity during thermocompression bonding can be ensured. Furthermore, when the amount is equal to or greater than the above lower limit, the dispersibility of carbon black is improved. Furthermore, the film-forming property is improved, and the film thickness distribution can be narrowed when the epoxy resin composition is applied to form a film.

[0047] (hardening agent) When the low elasticity black curable resin layer 1 is made of an epoxy resin composition, it may contain a curing agent for epoxy resin other than the modified elastomer having a functional group capable of reacting with an epoxy group. Examples of the other curing agent include known curing agents such as phenol-based curing agents, acid anhydride-based curing agents, and amine-based curing agents. Two or more of the other curing agents may be used in combination.

[0048] (curing catalyst) When the low elasticity black curable resin layer 1 is made of an epoxy resin composition, it may contain a curing catalyst that accelerates the curing reaction of the epoxy resin. Examples of the curing catalyst include imidazole-based, tertiary amine-based, phosphorus compound-based, etc. Among them, imidazole-based catalysts are preferred because they have good compatibility with epoxy resins and are less likely to cause yellowing. Among imidazole-based curing catalysts, those having a cyanoethyl group are particularly preferred because they are easily soluble in epoxy resins.

[0049] The amount of the curing catalyst is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the total resin solid content of the low elasticity black curable resin layer 1. When it is within the above range, curing can be sufficiently promoted and the usable life of the dry film 100 can be ensured. Two or more types of curing catalysts may be used in combination.

[0050] (Black pigment or black dye) The low elasticity black curable resin layer 1 is colored black. For coloring, it is preferable that the layer contains a black pigment or a black dye, more preferable that the layer contains a black pigment, and further preferable that the layer contains carbon black. By being colored black, the layer can prevent light diffusion between the multiple light emitting elements of the element-mounted substrate 10.

[0051] The particle size of the carbon black is preferably 10 to 500 nm, more preferably 10 to 300 nm, and particularly preferably 10 to 100 nm. The particle size refers to the average particle size, and can be determined by a measuring device using the dynamic light scattering method. An example of a measuring device using the dynamic light scattering method is NanotracWave II UT151 manufactured by Microtrack Bell.

[0052] The pH of carbon black based on ISO 787-9 is preferably 5 or less, more preferably 1 to 4.5, and even more preferably 2 to 4. When the pH of the carbon black is equal to or lower than the preferred upper limit, good dispersibility can be obtained and the blackness can be improved.When the pH of the carbon black is equal to or higher than the preferred lower limit, the dispersion stability in the coating liquid of the low elasticity black curable resin layer is improved, and the stability of sedimentation and blackness is improved.

[0053] As the carbon black, one or more of known carbon blacks such as gas black, channel black, furnace black, thermal black, lamp black, etc. may be used. Resin-coated carbon black may also be used. Furthermore, carbon nanofibers and carbon nanotubes may also be used.

[0054] Among these, gas black, which is an acidic carbon, is preferred because it has a large amount of surface functional groups, has high dispersibility, and exerts a sufficient light diffusion prevention function even when added in a small amount. In addition, when the low elasticity black curable resin layer 1 contains a modified elastomer having a functional group capable of reacting with an epoxy resin, the dispersibility is further increased due to the interaction between the surface functional group of the gas black and the functional group of the modified elastomer having a functional group capable of reacting with an epoxy resin, and good light diffusion prevention properties and coating liquid stability can be ensured.

[0055] The amount of carbon black is preferably 0.1 to 15 mass %, and more preferably 1.0 to 10 mass %, based on the total solid content of the low elasticity black curable resin layer 1. When the amount of carbon black is equal to or greater than the above lower limit, sufficient light blocking properties are obtained. When the amount of carbon black is greater than the above upper limit, the thixotropy of the low elasticity black curable resin layer 1 increases, the fluidity during thermocompression bonding decreases, and the gaps between the multiple light emitting elements of the element-mounted substrate 10 cannot be sufficiently filled.

[0056] (Other Ingredients) The low elasticity black curable resin layer 1 may contain an inorganic filler in order to improve flame retardancy and heat resistance and to adjust the refractive index. The low elasticity black curable resin layer 1 may further contain, as necessary, resins other than the epoxy resin and elastomer, thickeners, antifoaming agents and / or leveling agents, adhesion enhancers such as coupling agents, and flame retardants.

[0057] <Transparent curable resin layer> The dry film 100 of this embodiment includes two transparent curable resin layers, a low-elasticity transparent curable resin layer 2 and a high-elasticity transparent curable resin layer 3. These two layers have high total light transmittance. The total light transmittance of each of the low-elasticity transparent curable resin layer 2 and the high-elasticity transparent curable resin layer 3 is measured in a cured state.

[0058] <Low elasticity transparent curable resin layer 2> The low-elasticity transparent curable resin layer 2 is a layer that is filled at least partially between the multiple light-emitting elements while the low-elasticity black curable resin layer 1 is pressed between the multiple light-emitting elements arranged on the element-mounted substrate 10 during the thermocompression bonding process.

[0059] [Total light transmittance] The low elasticity transparent curable resin layer 2 is preferably prepared so that the total light transmittance in the cured state is 50% or more, more preferably 50 to 95%, and even more preferably 80 to 90%. Since the total light transmittance of the low-elasticity, transparent, cured resin layer 2 in a cured state is equal to or greater than the lower limit, even if the low-elasticity, transparent, cured resin layer 2 in a cured state remains on the light-emitting element, the light is not prevented from reaching the viewer.

[0060] [Storage modulus] The low elasticity, transparent, curable resin layer 2 is in an uncured or semi-cured state before being pressure-bonded to the element-mounted substrate 10 and cured. The storage modulus of the low elasticity, transparent, curable resin layer 2 before curing at 100° C. is smaller than that of the high elasticity, transparent, curable resin layer 3 before curing. In addition, it is preferably equal to or larger than the storage modulus of the low elasticity, black, curable resin layer 1 before curing at 100° C.

[0061] The storage modulus of the low elastic transparent curable resin layer 2 before curing is 1.0×10 5 Pa or less, and 1.0×10 3 ~1.0×10 5 Pa, preferably 5.0×10 3 ~1.0×10 5 Pa is more preferred.

[0062] Since the storage modulus at 100°C of the low-elasticity transparent curable resin layer 2 before curing is equal to or less than the preferred upper limit, sufficient fluidity is obtained when the layer is pressed against the element-mounted substrate 10, and the layer can conform to the unevenness of the element-mounted substrate 10 caused by the multiple light-emitting elements and sufficiently fill the spaces between the multiple light-emitting elements together with the low-elasticity black curable resin layer 1.

[0063] If the storage modulus at 100°C of the low-elasticity, transparent, curable resin layer 2 before curing exceeds the preferable upper limit, the fluidity of the low-elasticity, transparent, curable resin layer 2 will be insufficient, making it difficult to sufficiently fill the spaces between multiple light-emitting elements and difficult to sufficiently press the low-elasticity, black, curable resin layer 1 into the spaces between multiple light-emitting elements. The storage modulus of the low elasticity transparent curable resin layer 2 at 100° C. before curing is preferably 0.8 to 1000 times, more preferably 1 to 100 times, the storage modulus of the low elasticity black curable resin layer 1 before curing.

[0064] [Curable resin composition] The low elasticity transparent curable resin layer 2 is composed of a curable resin composition. As with the low elasticity black curable resin layer 1, the curable resin composition may be a thermosetting resin composition containing at least one resin selected from epoxy resin, acrylic resin, polyester resin, and polyurethane resin, and a curing agent. Among them, an epoxy resin composition is preferable because it can achieve curing at low temperature and has excellent heat resistance and reliability.

[0065] (Epoxy resin) Examples of epoxy resins used in the low elasticity transparent curable resin layer 2 include the same types as those used in the low elasticity black curable resin layer 1. Among the above epoxy resins, the epoxy resin used for the low elasticity transparent curable resin layer 2 is preferably a multifunctional epoxy resin, since it can increase the crosslink density after curing and has an appropriate molecular weight, making it easy to adjust the elastic modulus.

[0066] When the low elasticity, transparent, curable resin layer 2 contains a high molecular weight epoxy resin, the blending amount thereof is preferably 50 mass % or less, more preferably 35 mass % or less, and even more preferably 10 to 35 mass %, relative to 100 mass % of the total resin solid content of the low elasticity, transparent, curable resin layer 2. When the amount of the high molecular weight epoxy resin in the low elasticity transparent curable resin layer 2 is equal to or more than the above-mentioned preferable lower limit, it becomes easy to obtain a storage modulus that sufficiently presses the low elasticity black curable resin layer 1 into the gaps between the plurality of light emitting elements. When the amount is equal to or less than the preferable upper limit, the low elasticity transparent curable resin layer 2 easily fills the gaps between the plurality of light emitting elements.

[0067] The total amount of epoxy resin in the low elasticity, transparent, curable resin layer 2 is preferably 10 to 100 mass%, more preferably 20 to 99 mass%, and even more preferably 35 to 95 mass%, relative to 100 mass% of the total resin solid content of the low elasticity, transparent, curable resin layer 2. When the total amount of the epoxy resin in the low elasticity transparent curable resin layer 2 is within the above range, the storage modulus can be controlled and appropriate fluidity during thermocompression bonding can be ensured. Also, when the amount is equal to or greater than the lower limit, the heat resistance after curing can be improved.

[0068] (Elastomer) The low elastic transparent curable resin layer 2 preferably contains an elastomer in addition to a resin such as an epoxy resin, etc. By containing an elastomer, it becomes easier to control the storage modulus.

[0069] Examples of the elastomer include the same types as those of the low elasticity black curable resin layer 1. Among them, NBR is preferred because it has good compatibility with epoxy resins, can increase the storage modulus of the low elasticity transparent curable resin layer 2 at around 150° C., and has good adhesion to the low elasticity black curable resin layer 1. The preferred weight average molecular weight of the elastomer is also the same as that of the low elasticity black curable resin layer 1.

[0070] In particular, when the low elasticity transparent curable resin layer 2 is composed of an epoxy resin composition, it is preferable to include a modified elastomer having a functional group capable of reacting with an epoxy group. If there is a modified elastomer having a functional group capable of reacting with an epoxy group, it also acts as a curing agent for the epoxy resin. In addition, since it can react and bond with the epoxy resin, the heat resistance and reliability against thermal shock are improved.

[0071] Examples of functional groups capable of reacting with an epoxy group include the same types as those in the low elasticity black curable resin layer 1. Among them, an acid group or an acid anhydride group is preferred, and a carboxy group or a carboxylic acid anhydride group is particularly preferred, since they can be cured at low temperatures and can ensure a long pot life.

[0072] When the low-elasticity transparent curable resin layer 2 is composed of an epoxy resin composition, it particularly preferably contains acid-modified NBR having a carboxy group. As the acid-modified NBR having a carboxy group, the same types as those of the low elasticity black curable resin layer 1 can be mentioned. Two or more types of modified elastomers having a functional group capable of reacting with an epoxy group may be used in combination.

[0073] The amount of elastomer contained in the low elasticity, transparent, curable resin layer 2 is preferably 90 mass% or less, more preferably 1 to 80 mass%, and even more preferably 5 to 65 mass%, relative to 100 mass% of the total resin solid content of the low elasticity, transparent, curable resin layer 2. When the blending amount of the elastomer in the low-elasticity, transparent, curable resin layer 2 is equal to or more than the above-mentioned preferable lower limit, the film-formability is improved and the distribution of the film thickness during film formation can be narrowed. When the blending amount is equal to or less than the preferable upper limit, the low-elasticity, transparent, curable resin layer 2 is easily filled between a plurality of light-emitting elements.

[0074] (hardening agent) When the low elasticity transparent curable resin layer 2 is composed of an epoxy resin composition, it may contain a curing agent for epoxy resin other than the modified elastomer having a functional group capable of reacting with an epoxy group. Examples of the other curing agent include the same curing agents as those for the low elasticity black curable resin layer 1. Two or more types of the other curing agents may be used in combination.

[0075] (curing catalyst) When the low-elasticity transparent curable resin layer 2 is made of an epoxy resin composition, it may contain a curing catalyst that accelerates the curing reaction of the epoxy resin. As the curing catalyst, the same curing catalyst as that for the low elasticity black curable resin layer 1 can be mentioned, and the preferred embodiments are also the same.

[0076] The amount of the curing catalyst is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the total resin solid content of the low elasticity transparent curable resin layer 2. When it is within the above range, curing can be sufficiently promoted and the usable life of the dry film 100 can be ensured. Two or more types of curing catalysts may be used in combination.

[0077] (Other Ingredients) The low-elasticity transparent curable resin layer 2 may contain a black pigment or black dye in order to suppress uneven light emission and color unevenness.

[0078] From the viewpoint of increasing the total light transmittance, when the low elasticity transparent curable resin layer 2 contains carbon black, the blending amount thereof is preferably less than 5 parts by mass, more preferably 1 part by mass or less, and even more preferably 0.1 part by mass or less, per 100 parts by mass of the total resin solid content. The low elasticity transparent curable resin layer 2 may further contain, if necessary, resins other than epoxy resins and elastomers, thickeners, antifoaming agents and / or leveling agents, adhesion enhancers such as coupling agents, and flame retardants.

[0079] <Highly elastic transparent curable resin layer 3> The high-elasticity transparent curable resin layer 3 is a layer for removing the low-elasticity black curable resin layer 1 from above the light-emitting elements in the thermocompression bonding process by sufficiently pressing the low-elasticity black curable resin layer 1 and the low-elasticity transparent curable resin layer 2 between the multiple light-emitting elements arranged on the element-mounted substrate 10.

[0080] [Total light transmittance] The highly elastic, transparent, curable resin layer 3 is preferably prepared so that the total light transmittance in the cured state is 50% or more, more preferably 75 to 99.5%, and even more preferably 80 to 99.5%. When the highly elastic, transparent, curable resin layer 3 has a total light transmittance in a cured state of not less than the lower limit, light is not prevented from reaching the viewer's side.

[0081] [Storage modulus] The high elasticity, transparent, curable resin layer 3 is in an uncured or semi-cured state before being pressure-bonded to the element-mounted substrate 10 and cured. The storage modulus of the high elasticity, transparent, curable resin layer 3 before being cured is greater than the storage modulus of the low elasticity, black, curable resin layer 1 before being cured and the low elasticity, transparent, curable resin layer 2 before being cured at 100°C. The storage modulus of the high elasticity transparent curable resin layer 3 before curing is preferably greater than the storage modulus of the low elasticity black curable resin layer 1 before curing and the low elasticity transparent curable resin layer 2 before curing at 100°C to 150°C.

[0082] In addition, when the storage modulus of the high elasticity, transparent curable resin layer 3 before curing is greater than the storage modulus of the low elasticity, black curable resin layer 1 before curing and the low elasticity, transparent curable resin layer 2 before curing at 100°C and 150°C, the storage modulus of the high elasticity, transparent curable resin layer 3 before curing is usually greater than the storage modulus of the low elasticity, black curable resin layer 1 before curing and the low elasticity, transparent curable resin layer 2 before curing over the entire range of 100°C to 150°C.

[0083] The storage modulus of the highly elastic transparent curable resin layer 3 before curing is 1.0×10 7 Pa or less, and 1.0×10 4 Pa or more, 1.0×10 7 Pa or less, and 5.0×10 4 Pa or higher, 5.0×10 6 It is more preferable that the pressure is 0.1 Pa or less.

[0084] Since the storage modulus at 100°C of the high elasticity transparent curable resin layer 3 before curing is within a preferred range, stress can be transmitted to the low elasticity black curable resin layer 1 and the low elasticity transparent curable resin layer 2 when the layer is pressed against the element-mounted substrate 10, providing both the elasticity required to sufficiently remove the low elasticity black curable resin layer 1 from above the light-emitting elements and the flexibility required to deform in accordance with the unevenness of the multiple light-emitting elements, making it easier for the low elasticity black curable resin layer 1 and the low elasticity transparent curable resin layer 2 to sufficiently fill the spaces between the multiple light-emitting elements.

[0085] When the storage modulus at 100°C of the high elasticity transparent curable resin layer 3 before curing exceeds a preferred upper limit, the high elasticity transparent curable resin layer 3 has insufficient fluidity and is difficult to deform following the unevenness of the multiple light emitting elements, so that the low elasticity black curable resin layer 1 cannot be sufficiently removed only from the upper part of the low height light emitting element, and the luminance is likely to decrease, and it is difficult to sufficiently push the low elasticity black curable resin layer 1 between the multiple light emitting elements, which makes it easy to generate defects such as air bubbles due to the remaining voids. In addition, cracks are generated in the high elasticity transparent curable resin layer 3 during thermocompression bonding, making it easy to generate crack-like defects.

[0086] If the storage modulus at 100°C of the high elasticity transparent curable resin layer 3 before curing is below the preferred lower limit, it becomes difficult to sufficiently remove the low elasticity black curable resin layer 1 on the light emitting element. Also, the fluidity of the high elasticity transparent curable resin layer 3 is too high, and the surface of the high elasticity transparent curable resin layer 3 becomes uneven to match the light emitting element after thermocompression bonding, which is likely to result in poor appearance.

[0087] The storage modulus of the highly elastic transparent curable resin layer 3 before curing is 1.0×10 4 Pa or more, and 1.0×10 4 ~5.0×10 7 Pa is preferably 1.0×10 5 ~1.0×10 7 Pa is more preferred.

[0088] If the storage modulus at 150°C of the highly elastic, transparent, curable resin layer 3 before curing exceeds the preferred upper limit, cracks are likely to occur due to cure shrinkage during thermal curing. If the storage modulus at 150°C of the highly elastic, transparent, curable resin layer 3 before curing is equal to or greater than the preferred lower limit, flow during thermal curing can be suppressed, post-curing appearance defects such as repelling can be suppressed, and furthermore, problems are less likely to occur when etching is performed in a later step.

[0089] The storage modulus of the high elasticity transparent curable resin layer 3 at 100°C before curing is preferably 10 to 1000 times, and more preferably 30 to 500 times, the storage modulus of each of the low elasticity black curable resin layer 1 and the low elasticity transparent curable resin layer 2 before curing. The storage modulus of the high elasticity transparent curable resin layer 3 at 150°C before curing is preferably 5 to 10000 times, and more preferably 10 to 1000 times, the storage modulus of each of the low elasticity black curable resin layer 1 and the low elasticity transparent curable resin layer 2.

[0090] [Curable resin composition] The high elasticity transparent curable resin layer 3 is composed of a curable resin composition. As with the low elasticity black curable resin layer 1, the curable resin composition may be a thermosetting resin composition containing at least one resin selected from an epoxy resin, an acrylic resin, a polyester resin, and a polyurethane resin, and a curing agent. Among them, an epoxy resin composition is preferable because it can be cured at low temperature and has excellent heat resistance and reliability.

[0091] (Epoxy resin) Examples of epoxy resins used in the high-elasticity transparent curable resin layer 3 include the same types as those used in the low-elasticity black curable resin layer 1.

[0092] From the viewpoint of imparting an appropriate viscosity during compression to the highly elastic, transparent, curable resin layer 3, the highly elastic, transparent, curable resin layer 3 preferably contains a high molecular weight epoxy resin having a weight average molecular weight of 10,000 to 100,000. From the viewpoint of good compatibility with other resin components and dissolving without the need to mix with a high boiling point solvent that may remain in the dry film even after drying, the highly elastic, transparent, curable resin layer 3 more preferably contains a high molecular weight epoxy resin having a weight average molecular weight of 10,000 to 35,000.

[0093] By including a high molecular weight epoxy resin having a weight average molecular weight of 10,000 to 100,000 as the epoxy resin used in the highly elastic, transparent, curable resin layer 3, the highly elastic, transparent, curable resin layer 3 has an appropriate viscosity when heated, and therefore the storage modulus of the highly elastic, transparent, curable resin layer 3 in the range of 100°C to 150°C can be adjusted to a preferred range. The high molecular weight epoxy resin used in the highly elastic transparent curable resin layer 3 is preferably a phenoxy type epoxy resin because it has good compatibility with other epoxy resins.

[0094] Phenoxy type epoxy resin has a relatively large molecular weight among epoxy resins and has an appropriate viscosity when heated, so that the storage modulus of the highly elastic transparent curable resin layer 3 can be adjusted to a preferred range in the range of 100°C to 150°C. In addition, unlike other thermoplastic resins such as polyester, phenoxy type epoxy resin can be cured as an epoxy resin, so that the crosslink density can be increased and the heat resistance of the cured product and the reliability of performance for long-term use are not impaired.

[0095] From the viewpoint of ensuring a storage modulus sufficient to compress the low elasticity black curable resin layer 1 during thermocompression bonding, the glass transition temperature of the phenoxy type epoxy resin used in the high elasticity transparent curable resin layer 3 is preferably 100° C. or higher.

[0096] Specific examples of phenoxy type epoxy resins include "1256", "YX7200", "YX8100", and "YX7180" manufactured by Mitsubishi Chemical Corporation, "YP-50", "YP-50S", and "YP-70" manufactured by Nippon Steel Chemical & Material Co., Ltd., "N-690" manufactured by DIC Corporation, and "H-157" and "EXA-192" manufactured by DIC Corporation.

[0097] The amount of the high molecular weight epoxy resin in the highly elastic, transparent, curable resin layer 3 is preferably 30 to 80 mass%, more preferably 40 to 75 mass%, and even more preferably 45 to 70 mass%, relative to 100 mass% of the total resin solid content of the highly elastic, transparent, curable resin layer 3. The preferred blending amount of the phenoxy type epoxy resin in the highly elastic transparent curable resin layer 3 is also the same.

[0098] Within the above range, the storage modulus can be controlled, the storage modulus for pressing the low elasticity black curable resin layer 1 and the high elasticity transparent curable resin layer 3 during thermocompression bonding can be secured, and the low elasticity black curable resin layer 1 can be sufficiently removed from above the light emitting element. In addition, flow during thermal curing can be suppressed, and appearance defects after curing such as repelling can be suppressed, and further, problems are unlikely to occur when etching is performed in a later process. In addition, toughness is improved, and crack-like defects are unlikely to occur during thermocompression bonding. When the content is equal to or less than the above upper limit, the crosslink density of the highly elastic transparent curable resin layer 3 in a cured state can be increased, and the heat resistance and chemical resistance can be improved.

[0099] Furthermore, it is preferable that the epoxy resin used in the highly elastic, transparent, curable resin layer 3 contains a polyfunctional epoxy resin. The polyfunctional epoxy resin can increase the crosslink density, thereby further improving the stability of the performance of the cured product of the epoxy resin composition over long-term use, and also improving the heat resistance. In addition, since the viscosity in the range of 100°C to 150°C is lower than that of the phenoxy type epoxy resin, the storage modulus of the highly elastic, transparent, curable resin layer 3 can be adjusted by combining it with the phenoxy type epoxy resin.

[0100] Specific examples of polyfunctional epoxy resins include "YX7700", "157S70", and "1032S60" manufactured by Mitsubishi Chemical Corporation, "NC7000L", "XD1000", and "EOCN-1020" manufactured by Nippon Kayaku Co., Ltd., "ESN485" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "N-690", "N-695", and "HP-7200H" manufactured by DIC Corporation.

[0101] The amount of the polyfunctional epoxy resin in the highly elastic, transparent, curable resin layer 3 is preferably 90% by mass or less, more preferably 10 to 80% by mass, and even more preferably 20 to 70% by mass, relative to 100% by mass of the total resin solid content of the highly elastic, transparent, curable resin layer 3. Within the above range, the storage modulus of the highly elastic, transparent, curable resin layer 3 during thermocompression bonding can be controlled, and heat resistance and chemical resistance can be imparted in the cured state.

[0102] From the viewpoint of ensuring sufficient fluidity during thermocompression bonding, the highly elastic transparent curable resin layer 3 preferably contains an epoxy resin having a softening point or melting point of 120° C. or less. From the viewpoint of handleability and heat resistance of the cured product, it is more preferable that the highly elastic transparent curable resin layer 3 contains an epoxy resin having a softening point or melting point of 50 to 105° C. By containing an epoxy resin having a softening point or melting point within the above range, it becomes possible to control the storage modulus.

[0103] The total amount of epoxy resin in the high elasticity transparent curable resin layer 3 is preferably 10 to 100% by mass, more preferably 30 to 99% by mass, and even more preferably 50 to 95% by mass, based on 100% by mass of the total resin solid content of the high elasticity transparent curable resin layer 3. Within the above range, the storage modulus can be controlled, and the storage modulus for pressing the low elasticity black curable resin layer 1 during thermocompression bonding can be ensured. In addition, flow during thermal curing can be suppressed, and poor appearance after curing such as repelling can be suppressed, and further, problems are less likely to occur when etching is performed in a later process. In addition, when the amount is equal to or greater than the above lower limit, heat resistance in the cured state is improved.

[0104] (Elastomer) The highly elastic transparent curable resin layer 3 preferably contains an elastomer in addition to a resin such as an epoxy resin, etc. By containing an elastomer, it becomes easier to control the storage modulus.

[0105] Examples of the elastomer include the same types as those of the low elasticity black curable resin layer 1. Among them, NBR is preferred because it has good compatibility with epoxy resins, can increase the storage modulus of the high elasticity transparent curable resin layer 3 at around 150°C, and has good adhesion to the low elasticity transparent curable resin layer 2. The preferred weight average molecular weight of the elastomer is also the same as that of the low elasticity black curable resin layer 1.

[0106] In particular, when the highly elastic transparent curable resin layer 3 is composed of an epoxy resin composition, it is preferable to include a modified elastomer having a functional group capable of reacting with an epoxy group. A modified elastomer having a functional group capable of reacting with an epoxy group also acts as a curing agent for the epoxy resin. In addition, since it can react and bond with the epoxy resin, the heat resistance and reliability against thermal shock are improved. Furthermore, the difference in polarity between the functional group capable of reacting with the epoxy resin and the resin skeleton has a favorable effect on dispersibility, and good dispersibility can be obtained when carbon black is contained in the highly elastic transparent curable resin layer 3.

[0107] Examples of functional groups capable of reacting with an epoxy group include the same types as those in the low elasticity black curable resin layer 1. Among them, an acid group or an acid anhydride group is preferred, and a carboxy group or a carboxylic acid anhydride group is particularly preferred, since they can be cured at low temperatures and can ensure a long pot life.

[0108] When the highly elastic, transparent, curable resin layer 3 is made of an epoxy resin composition, it particularly preferably contains an acid-modified NBR having a carboxy group. As the acid-modified NBR having a carboxy group, the same types as those of the low elasticity black curable resin layer 1 can be mentioned. Two or more types of modified elastomers having a functional group capable of reacting with an epoxy group may be used in combination.

[0109] The amount of the elastomer in the high elasticity transparent curable resin layer 3 is preferably 0 to 50% by mass, more preferably 1 to 70% by mass, and even more preferably 5 to 50% by mass, based on 100% by mass of the total resin solid content of the high elasticity transparent curable resin layer 3. When the amount is within the above range, the storage modulus can be controlled. When the amount is equal to or less than the above upper limit, the storage modulus can be secured to press the low elasticity black curable resin layer during thermocompression bonding. In addition, flow during thermal curing can be suppressed, and poor appearance after curing such as repelling can be suppressed, and further, problems are less likely to occur when etching is performed in a later process. When the amount is equal to or more than the above lower limit, the dispersibility of carbon black is improved. Furthermore, the film-forming property is improved, and the distribution of film thickness can be narrowed when the epoxy resin composition is applied to form a film.

[0110] (hardening agent) When the high elasticity transparent curable resin layer 3 is composed of an epoxy resin composition, it may contain a curing agent for epoxy resin other than the modified elastomer having a functional group capable of reacting with an epoxy group. Examples of the other curing agent include the same curing agents as those used in the low elasticity black curable resin layer 1 and the low elasticity transparent curable resin layer 2. Two or more types of the other curing agents may be used in combination.

[0111] (curing catalyst) When the highly elastic, transparent, curable resin layer 3 is made of an epoxy resin composition, it may contain a curing catalyst that accelerates the curing reaction of the epoxy resin. As the curing catalyst, the same curing catalysts as those for the low elasticity black curable resin layer 1 and the low elasticity transparent curable resin layer 2 can be mentioned, and the preferred embodiments are also the same.

[0112] The amount of the curing catalyst is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the total resin solid content of the highly elastic, transparent, curable resin layer 3. When it is within the above range, curing can be sufficiently promoted and the usable life of the dry film 100 can be ensured. Two or more types of curing catalysts may be used in combination.

[0113] (Other Ingredients) The highly elastic transparent curable resin layer 3 may contain a black pigment or black dye in order to suppress uneven light emission and color unevenness. From the viewpoint of increasing the total light transmittance, when the highly elastic, transparent, curable resin layer 3 contains carbon black, the blending amount thereof is preferably less than 5 parts by mass, more preferably 1 part by mass or less, and even more preferably 0.1 part by mass or less, per 100 parts by mass of the total resin solid content. The highly elastic transparent curable resin layer 3 may further contain, as necessary, resins other than the epoxy resin and elastomer, thickeners, antifoaming agents and / or leveling agents, adhesion enhancers such as coupling agents, and flame retardants.

[0114] <Protective film> The first protective film 6 and the second protective film 7 (hereinafter, the first protective film 6 and the second protective film 7 may be collectively referred to simply as the "protective films") have the role of protecting the low elasticity black curable resin layer 1, the low elasticity transparent curable resin layer 2 and the high elasticity transparent curable resin layer 3, and can also be used as films onto which a coating liquid of a curable resin composition is applied when these curable resin layers are formed.

[0115] Examples of the protective film that can be used include polyester films such as polyethylene terephthalate and polyethylene naphthalate, films made of thermoplastic resins such as polyimide films, polyamideimide films, polyethylene films, polytetrafluoroethylene films, polypropylene films, and polystyrene films, as well as surface-treated paper.

[0116] Among these, polyester films can be preferably used from the viewpoints of heat resistance, mechanical strength, ease of handling, etc. The thickness of the protective film is not particularly limited, but is appropriately selected from the range of about 10 to 150 μm depending on the application. The surface of the protective film on which the resin layer is provided may be subjected to a release treatment.

[0117] <Method of manufacturing dry film> To obtain the dry film 100, first, a coating liquid of the curable resin composition for the high elasticity, transparent curable resin layer 3 is applied to the second protective film 7 and dried, and a coating liquid of the curable resin composition for the low elasticity, transparent curable resin layer 2 is applied to a release film and dried. These are stacked and laminated so that the high elasticity, transparent curable resin layer 3 and the low elasticity, transparent curable resin layer 2 are in contact with each other, and the release film is peeled off to obtain a laminate in which the low elasticity, transparent curable resin layer 2, the high elasticity, transparent curable resin layer 3, and the second protective film 7 are laminated in that order. Next, a coating liquid of the curable resin composition for the low elasticity black curable resin layer 1 is applied to the first protective film 6 and then dried to prepare the first protective film 6.

[0118] Then, these are stacked and laminated so that the low elasticity transparent curable resin layer 2 and the low elasticity black curable resin layer 1 are in contact, thereby obtaining a laminate in which the low elasticity black curable resin layer 1, the low elasticity transparent curable resin layer 2, the high elasticity transparent curable resin layer 3, and the second protective film 7 are stacked in that order on the first protective film 6.

[0119] It is preferable that the coating liquid of the curable resin composition for the low elasticity black curable resin layer 1, the coating liquid of the curable resin composition for the low elasticity transparent curable resin layer 2, and the coating liquid of the curable resin composition for the high elasticity transparent curable resin layer 3 contain an organic solvent in an amount that gives a viscosity that allows for unhindered application. The organic solvent is not particularly limited, and examples thereof include ketones, aromatic hydrocarbons, glycol ethers, glycol ether acetates, esters, alcohols, aliphatic hydrocarbons, petroleum-based solvents, etc. Specific examples of the organic solvent include ketones such as methyl ethyl ketone, cyclohexanone, methyl butyl ketone, and methyl isobutyl ketone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ethyl acetate, butyl acetate, isobutyl acetate, ethylene glycol diethyl ether, and triethylene glycol monoethyl ether; Examples of the solvent include esters such as propylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, and propylene glycol butyl ether acetate; alcohols such as ethanol, propanol, 2-methoxypropanol, n-butanol, isobutyl alcohol, isopentyl alcohol, ethylene glycol, and propylene glycol; aliphatic hydrocarbons such as octane and decane; petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha, as well as N,N-dimethylformamide (DMF), tetrachloroethylene, and turpentine.

[0120] When carbon black is blended into the coating liquid, carbon black powder or a carbon black dispersion may be added.

[0121] Examples of a method for applying the coating liquid of the curable resin composition for the low elasticity black curable resin layer 1, the coating liquid of the curable resin composition for the low elasticity transparent curable resin layer 2, and the coating liquid of the curable resin composition for the high elasticity transparent curable resin layer 3 include various coaters such as a die coater, a gravure coater, a roll coater, a curtain flow coater, a spin coater, a bar coater, a reverse coater, a kiss coater, a fountain coater, a rod coater, an air doctor coater, a knife coater, a blade coater, a cast coater, and a screen coater. The drying temperature is preferably from 60 to 160°C, more preferably from 80 to 130°C, and further preferably from 90 to 120°C.

[0122] The temperature during lamination is preferably 20 to 120° C., more preferably 30 to 100° C., and even more preferably 40 to 80° C. By setting the temperature during lamination to a preferred lower limit or higher, it is possible to ensure sufficient adhesion between the low elasticity black curable resin layer 1 and the low elasticity transparent curable resin layer 2, which allows handling even in an uncured or semi-cured state. In addition, by setting the temperature during lamination to a preferred upper limit or lower, it is possible to prevent the formation of air bubbles and wrinkles. The lamination can be carried out using a roll laminator, a press, a vacuum press, or the like.

[0123] <Substrate with elements> As shown in Fig. 2, the element-mounted substrate 10 has a plurality of light-emitting elements arranged on a substrate 11. Fig. 2 and other figures show a schematic view of a portion where three light-emitting elements (light-emitting element 12, light-emitting element 13, and light-emitting element 14) are arranged.

[0124] There is no limitation on the material of the substrate 11, but a known printed circuit board can be suitably used. Examples of known printed circuit boards include a glass epoxy board, a fluororesin board, and a ceramic board. The light emitting element is typically a light emitting diode, and the present invention is particularly suitable for use in cases where the light emitting element is extremely small.

[0125] For example, a light emitting diode having a height of 1000 nm to 200 μm and a side length of 0.001 to 0.5 mm can be used. In the element-mounted substrate 10 for obtaining mini LEDs or micro LEDs, light-emitting diodes of three colors R, G, and B can be used as the light-emitting elements, or a blue light-emitting diode can be used as the light-emitting element.

[0126] <Method of manufacturing light-emitting electronic components> The method for manufacturing a light-emitting electronic component of the present invention is a method in which the dry film 100 of the present invention is placed on a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, so that the low-elasticity black curable resin layer 1 is in contact with the surface, and the dry film 100 is thermocompression-bonded to fill the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and a portion of the high-elasticity transparent curable resin layer 3 between the plurality of light-emitting elements, and the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and the high-elasticity transparent curable resin layer 3 are cured by heating. Hereinafter, a method for producing a light-emitting electronic component according to one embodiment of the present invention will be described with reference to FIGS.

[0127] In the manufacturing method of this embodiment, first, as shown in Figure 2, a dry film 100 from which the first protective film 6 has been peeled off to expose the low-elasticity black curable resin layer 1 is placed on the surface of the element-mounted substrate 10 on which the light-emitting elements 12, 13, and 14 are arranged, so that the low-elasticity black curable resin layer 1 is in contact with the dry film 100.

[0128] At this time, that is, before compression bonding, the thickness of the low elasticity black curable resin layer 1 is preferably 10 to 80% of the height of the light emitting element. The lower limit is more preferably 15% or more, and even more preferably 30% or more. The upper limit is more preferably 70% or less, even more preferably 65% ​​or less, and particularly preferably 55% or less.

[0129] When the thickness of the low elasticity black curable resin layer 1 is 10% or more of the height of the light emitting element, the function of preventing light diffusion between the light emitting elements is sufficient. When the thickness of the low elasticity black curable resin layer 1 is 15% or more of the height of the light emitting element, the resin can be sufficiently filled between the light emitting elements. When the thickness of the low elasticity black curable resin layer 1 is 30% or more of the height of the light emitting element, the rate of change in the film thickness of the low elasticity black curable resin layer 1 after curing is small, and a uniform blackness can be achieved throughout the light emitting electronic component.

[0130] If the thickness of the low-elasticity black curable resin layer 1 is 80% or less of the height of the light-emitting element, the decrease in brightness can be prevented even if there is a difference in the inclination or height of the light-emitting element, and the light from the light-emitting element is not prevented from reaching the viewer. If the thickness of the low-elasticity black curable resin layer 1 is 70% or less of the height of the light-emitting element, the low-elasticity black curable resin layer can be prevented from leaking out during thermocompression bonding. If the thickness of the low-elasticity black curable resin layer 1 is 55% or less of the height of the light-emitting element, the low-elasticity black curable resin layer 1 having a light diffusion prevention function can be appropriately filled between the light-emitting elements.

[0131] The thickness of the low elasticity transparent curable resin layer 2 before compression bonding is preferably 10 to 80% of the height of the light emitting element. The lower limit is more preferably 15% or more, and even more preferably 20% or more. The upper limit is more preferably 70% or less, and even more preferably 60% or less.

[0132] When the thickness of the low elasticity transparent curable resin layer 2 is 10% or more of the height of the light emitting element, the low elasticity transparent curable resin layer 2 can sufficiently press the low elasticity black curable resin layer 1 between a plurality of light emitting elements. When the thickness of the low elasticity transparent curable resin layer 2 is 15% or more of the height of the light emitting element, the low elasticity black curable resin layer 1 can be pressed uniformly during thermocompression bonding, and the occurrence of black shading due to fluctuations in the film thickness of the flowed low elasticity black curable resin layer 1 can be prevented. When the thickness of the low elasticity transparent curable resin layer 2 is 20% or more of the height of the light emitting element, the low elasticity black curable resin layer 1 can be made thinner, and the low elasticity black curable resin layer 1 is less likely to remain on the light emitting element.

[0133] When the thickness of the low-elasticity transparent curable resin layer 2 is 80% or less of the height of the light-emitting element, a decrease in brightness can be prevented even if there is a difference in the inclination or height of the light-emitting element. When the thickness of the low-elasticity transparent curable resin layer 2 is 70% or less of the height of the light-emitting element, leakage of the low-elasticity transparent curable resin layer 2 to the outside during thermocompression bonding can be prevented.

[0134] The thickness of the highly elastic transparent curable resin layer 3 before compression bonding is preferably 10 to 500% of the height of the light emitting device. The lower limit is more preferably 15% or more, and even more preferably 20% or more. The upper limit is more preferably 200% or less, and even more preferably 150% or less.

[0135] When the thickness of the high elasticity transparent curable resin layer 3 is 10% or more relative to the height of the light emitting element, the high elasticity transparent curable resin layer 3 can remove the low elasticity black curable resin layer 1 on the light emitting element, and the light from the light emitting element does not reach the viewer side by not leaving the shielding low elasticity black curable resin layer 1 on the light emitting element. When the thickness of the high elasticity transparent curable resin layer 3 is 15% or more relative to the height of the light emitting element, the low elasticity black curable resin layer 1 and the low elasticity transparent curable resin layer 2 can be uniformly pressed in during thermocompression bonding, and the occurrence of black shading due to the fluctuation in the film thickness of the flowed low elasticity black curable resin layer 1 can be prevented. When the thickness of the high elasticity transparent curable resin layer 3 is 20% or more relative to the height of the light emitting element, the low elasticity black curable resin layer 1 and the low elasticity transparent curable resin layer 2 are less susceptible to the effect of deformation during thermal curing, and appearance defects are less likely to occur.

[0136] When the thickness of the highly elastic transparent curable resin layer 3 is 500% or less of the height of the light emitting device, a uniform film without residual solvent concentration difference or thermal history unevenness in the thickness direction can be formed. When the thickness of the highly elastic transparent curable resin layer 3 is 200% or less of the height of the light emitting device, the fluidity of the highly elastic transparent curable resin layer 3 near the upper surface of the light emitting device during thermocompression bonding can be increased, and the low elastic black curable resin layer 1 can be more efficiently removed from above the light emitting device. When the thickness of the highly elastic transparent curable resin layer 3 is 150% or less of the height of the light emitting device, the total light transmittance of the highly elastic transparent curable resin layer 3 can be increased.

[0137] The total thickness of the low elasticity black curable resin layer 1, the low elasticity transparent curable resin layer 2 and the high elasticity transparent curable resin layer 3 before compression bonding is preferably 100 to 550%, more preferably 110 to 400%, and more preferably 120 to 300% of the height of the light emitting element.

[0138] When the total thickness of the low elasticity black curable resin layer 1, the low elasticity transparent curable resin layer 2 and the high elasticity transparent curable resin layer 3 is equal to or greater than the above-mentioned lower limit value with respect to the height of the light-emitting element, the curable resin can be sufficiently embedded between the light-emitting elements. When the total thickness of the low elasticity black curable resin layer 1, the low elasticity transparent curable resin layer 2 and the high elasticity transparent curable resin layer 3 is equal to or less than the upper limit value relative to the height of the light emitting element, thickness unevenness is unlikely to occur during compression bonding, and poor appearance is unlikely to occur on the surface.

[0139] The ratio of the thickness of the low elasticity black curable resin layer 1 before compression to the total thickness of the low elasticity black curable resin layer 1, the low elasticity transparent curable resin layer 2, and the high elasticity transparent curable resin layer 3 before compression is preferably 3 to 70%, more preferably 5 to 60%, and even more preferably 10 to 50%. If the ratio of the thickness of the low-elasticity black curable resin layer 1 before compression to the total thickness of the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and the high-elasticity transparent curable resin layer 3 is equal to or greater than the lower limit, the degree of blackness can be increased and the contrast of the display can be sufficiently improved. If it is equal to or less than the upper limit, the low-elasticity black curable resin layer 1 is unlikely to remain on the light-emitting element during compression, and the brightness can be sufficiently improved.

[0140] The ratio of the thickness of the low elasticity transparent curable resin layer 2 before compression to the total thickness of the low elasticity transparent curable resin layer 2 and the high elasticity transparent curable resin layer 3 before compression is preferably 3 to 70%, more preferably 5 to 60%, and even more preferably 10 to 50%. If the ratio of the thickness of the low-elasticity transparent curable resin layer 2 before compression to the total thickness of the low-elasticity transparent curable resin layer 2 and the high-elasticity transparent curable resin layer 3 before compression is equal to or greater than the above lower limit, the low-elasticity transparent curable resin layer 2 can sufficiently press the low-elasticity black curable resin layer 1 between the multiple light-emitting elements. If it is equal to or less than the above upper limit, a decrease in brightness can be prevented even if there is a difference in the inclination or height of the light-emitting elements.

[0141] 2, the low elasticity black curable resin layer 1, the low elasticity transparent curable resin layer 2 and a part of the high elasticity transparent curable resin layer 3 of the dry film 100 are embedded between the light emitting elements as shown in FIG. In this case, the low elasticity black curable resin layer 1 has a low storage modulus and ensures fluidity, so that it is easily filled between the light emitting elements, and is preferable because it is easily removed from above the light emitting elements by the high elasticity transparent curable resin layer 3 and the low elasticity transparent curable resin layer 2. In addition, the low elasticity transparent curable resin layer 2 also has a relatively low storage modulus and ensures fluidity, so that it is easily filled between the light emitting elements while uniformly pushing the low elasticity black curable resin layer 1 into the light emitting elements. Furthermore, since the high-elasticity transparent curable resin layer 3 has a relatively high storage modulus and is kept within a deformable range, the low-elasticity black curable resin layer 1 can be easily and satisfactorily removed from above the light-emitting element even if there is a difference in the inclination or height of the light-emitting element.

[0142] The temperature in the thermocompression bonding is preferably 80 to 120°C, and more preferably 90 to 110°C. By setting the temperature in the thermocompression bonding to 80°C or higher, it is easy to ensure the fluidity of the low elasticity black curable resin layer 1 and the low elasticity transparent curable resin layer 2, and the flexibility of the high elasticity transparent curable resin layer 3. Furthermore, by setting the temperature in the thermocompression bonding to 120°C or lower, the light emitting element is less likely to be damaged. By setting the temperature in the thermocompression bonding to 90 to 110°C, the fluidity can be controlled more precisely, and the occurrence of unevenness and crack-like defects can be suppressed.

[0143] The pressure in the thermocompression bonding is preferably 0.05 to 1.0 MPa, more preferably 0.1 to 0.5 MPa. By setting the pressure in the thermocompression bonding to the preferred lower limit or more, the low elasticity black curable resin layer 1 does not remain on the light emitting element, and light from the light emitting element is not prevented from reaching the viewer. By setting the pressure to the preferred upper limit or less, the light emitting element is less likely to be damaged.

[0144] The thermocompression bonding is preferably carried out using a vacuum press capable of molding in a vacuum state, which makes it easier to avoid defects caused by air being mixed into the obtained light-emitting electronic component.

[0145] After the bonding, the second protective film 7 is peeled off as shown in FIG. 4, and then the resulting mixture is thermally cured to form the low elasticity black curable resin layer 1 into the black cured material layer 21 (the low elasticity black curable resin layer 1 in a cured state), the low elasticity transparent curable resin layer 2 into the first transparent cured material layer 22 (the low elasticity transparent curable resin layer 2 in a cured state), and the high elasticity transparent curable resin layer 3 into the second transparent cured material layer 23 (the high elasticity transparent curable resin layer 3 in a cured state), as shown in FIG. 5. 6, the assembly is sealed with a sealant 25. In this way, a light-emitting electronic component 31 is obtained.

[0146] The curing temperature is preferably 100 to 160° C., and more preferably 120 to 150° C. By setting the curing temperature to 100° C. or higher, the low elasticity black curable resin layer 1, the low elasticity transparent curable resin layer 2, and the high elasticity transparent curable resin layer 3 can be cured. By setting the curing temperature to 120° C. or higher, the curing time of the low elasticity black curable resin layer 1, the low elasticity transparent curable resin layer 2, and the high elasticity transparent curable resin layer 3 can be shortened. In addition, by setting the curing temperature to the above upper limit temperature or lower, the light emitting element is less likely to be damaged.

[0147] The curing time varies depending on the curing temperature, but is preferably from 30 to 360 minutes, and more preferably from 45 to 180 minutes. At the curing temperature, the highly elastic transparent curable resin layer 3 has a relatively high storage modulus and its fluidity is suppressed, so that defects in appearance after curing are suppressed. As a result, a light-emitting electronic component 31 is obtained in which the dry film 100 is pressure-bonded to the surface of the element-mounted substrate 10, on which a plurality of light-emitting elements are arranged on the substrate 11, on which the light-emitting elements are arranged.

[0148] In the obtained light-emitting electronic component 31, the low-elasticity black cured resin layer 1, the low-elasticity transparent cured resin layer 2, and the high-elasticity transparent cured resin layer 3 are cured to form a black cured material layer 21, a first transparent cured material layer 22, and a second transparent cured material layer 23, respectively, and portions of the black cured material layer 21, the first transparent cured material layer 22, and the second transparent cured material layer 23 are filled between multiple light-emitting elements. In addition, FIG. 6 shows an example in which the black cured material layer 21 and the first transparent cured material layer 22 are all filled between multiple light-emitting elements, and a portion of the second transparent cured material layer 23 is filled between multiple light-emitting elements.

[0149] Second Embodiment <Integrated sealing sheet> The integrated encapsulating sheet 200 according to the second embodiment will be described below. In the description of the second embodiment, the same components as those in the first embodiment are denoted by the same reference numerals, and detailed description thereof will be omitted.

[0150] As shown in FIG. 7, the integrated encapsulating sheet 200 is basically configured by laminating a low elasticity black curable resin layer 1, a low elasticity transparent curable resin layer 2, a high elasticity transparent curable resin layer 3, and a encapsulating film layer 9,

[0151] The integrated encapsulating sheet 200 of the present embodiment may further have a protective film on one or both of the surfaces of the low-elasticity black curable resin layer 1 and the encapsulating film layer 9 for ease of handling. An example having protective films on both surfaces is shown in Fig. 7. Specifically, a low elasticity black curable resin layer 1, a low elasticity transparent curable resin layer 2, a high elasticity transparent curable resin layer 3, a sealing film layer 9, and a second protective film 7 are laminated in this order on a first protective film 6. If the surface hardness of the sealing film layer 9 is sufficient, the second protective film 7 can be omitted.

[0152] The integrated encapsulating sheet 200 is used such that the low elasticity black curable resin layer 1 is in direct contact with the element-mounted substrate 10 during pressure bonding, as shown in FIG. A specific method for obtaining a light-emitting electronic component by pressure-bonding the integrated encapsulating sheet 200 to the element-mounted substrate 10 will be described later. The element-mounted substrate 10 is similar to the element-mounted substrate 10 in the first embodiment.

[0153] <Curable resin layer> The low elasticity black curable resin layer 1, the low elasticity transparent curable resin layer 2, and the high elasticity transparent curable resin layer 3 in this embodiment are similar to those in the dry film 100 of the first embodiment, and the preferred aspects are also similar.

[0154] <Sealing film layer> The sealing film layer 9 is a layer for protecting the light emitting element from external physical impact, humidity, moisture, etc. The sealing film layer 9 of this embodiment is composed of a support film layer 4 and a hard coat layer 5 provided on the side of the support film layer 4 opposite to the highly elastic transparent curable resin layer 3.

[0155] [Total light transmittance] The sealing film layer 9 as a whole (in this embodiment, the combination of the support film layer 4 and the hard coat layer 5) preferably has a total light transmittance of 20 to 80%, more preferably 30 to 80%, and even more preferably 40 to 75%. When the total light transmittance of the sealing film layer 9 is equal to or greater than the lower limit, the light is not prevented from reaching the viewer side. When the total light transmittance of the sealing film layer 9 is equal to or less than the upper limit, the degree of blackness is more easily ensured. When the total light transmittance is within the above range, the contrast is further improved.

[0156] [Storage modulus] The storage modulus of the sealing film layer 9 as a whole (in this embodiment, the support film layer 4 and the hard coat layer 5 combined) at 100° C. is 1.0×10 8 Pa or more, 1.0×10 10 Pa or less, and 1.0×10 9 Pa or higher, 9.0×10 9 Pa or less, and 3.0×10 9 Pa or higher, 8.0×10 9 It is more preferable that the pressure is 0.1 Pa or less.

[0157] When the storage modulus of the sealing film layer 9 at 100°C is equal to or less than the preferred upper limit, appropriate flexibility is obtained that does not hinder the flow of the low elasticity black curable resin layer 1 and the like when pressure-bonded to the element-mounted substrate 10, improving workability and preventing cracks due to pressure.

[0158] Since the storage modulus of the sealing film layer 9 at 100°C is equal to or greater than the preferred lower limit, the sealing film layer 9 is less likely to deform when pressed against the element-mounted substrate 10, and pressure can be reliably transmitted to the low-elasticity black curable resin layer 1, etc., preventing defects such as cracks and deformation in the hard coat layer 5.

[0159] <Support film layer> The support film layer 4 in the sealing film layer 9 is a layer for protecting the light emitting element from external physical impact, humidity, moisture, and the like.

[0160] [Total light transmittance] The total light transmittance of the support film layer 4 alone is preferably from 30 to 99%, more preferably from 50 to 95%, and even more preferably from 70 to 95%. When the total light transmittance of the support film layer 4 alone is equal to or greater than the above lower limit, an inexpensive commercially available film can be used.

[0161] [resin] The support film layer 4 may be made of a thermoplastic resin or a thermosetting resin. Examples of the resin constituting the support film layer 4 include polyethylene terephthalate resin, polyethylene 2,6-naphthalate resin, polycarbonate resin, triacetyl cellulose resin, polymethylpentene resin, phenoxy resin, syndiotactic polystyrene resin, polyimide resin, etc., and it is preferable that the support film layer 4 contains at least one resin selected from polyethylene terephthalate resin, polyethylene 2,6-naphthalate resin, and polycarbonate resin in terms of heat resistance, weather resistance, availability, cost, etc. By including these resins, deformation during compression bonding can be prevented.

[0162] [Film thickness] The thickness of the support film layer 4 is preferably from 10 to 250 μm, more preferably from 20 to 200 μm, and further preferably from 25 to 150 μm. When the thickness of the support film layer 4 is equal to or greater than the preferred lower limit, the layer has sufficient strength to protect the element. When the thickness of the support film layer 4 is equal to or less than the preferred upper limit, the layer has improved visibility and costs can be reduced.

[0163] <Hard coat layer> [hardness] The hard coat layer 5 is a layer for protecting the light-emitting electronic component from scratches. The pencil hardness of the surface of the hard coat layer 5 is preferably H or higher, more preferably 2H or higher, and even more preferably 3H or higher.

[0164] [Surface roughness] The surface roughness Ra of the hard coat layer 5 is preferably from 0.1 to 1 μm, more preferably from 0.2 to 1 μm, and even more preferably from 0.3 to 1 μm. By setting the surface roughness of the hard coat layer 5 to the preferred lower limit or more, it is possible to reduce the reflectance of the surface of the hard coat layer 5. By setting the surface roughness of the hard coat layer 5 to the preferred upper limit or less, production becomes easy.

[0165] [Total light transmittance] The hard coat layer 5 is prepared so that the total light transmittance is preferably 30 to 99%, more preferably 50 to 99%, and even more preferably 60 to 99%. When the total light transmittance of the hard coat layer 5 is equal to or greater than the lower limit, light is not prevented from reaching the viewer's side.

[0166] [Curable resin composition] The hard coat layer 5 is composed of a curable resin composition. Examples of the curable resin composition constituting the hard coat layer 5 include a thermosetting resin composition, an ultraviolet curable resin composition, and an electron beam curable resin composition. Among them, an ultraviolet curable resin composition is preferred. Examples of the ultraviolet-curable resin composition include acrylic resin, urethane resin, silicone resin, and the like, and the composition may contain one or more of these. Examples of the thermosetting resin composition include acrylic resin, urethane resin, silicone resin, melamine resin, and the like, and the composition may contain one or more of these.

[0167] [Fine particles] The hard coat layer 5 preferably contains fine particles. As the fine particles, one or both of inorganic fine particles and organic fine particles can be used. Examples of inorganic fine particles include silica fine particles and titanium fine particles, and examples of organic fine particles include polymethyl methacrylate resin (PMMA resin) and urethane resin. Among these, silica fine particles are preferable. By including the fine particles, it is possible to adjust the surface roughness and improve the surface hardness.

[0168] [Film thickness] The thickness of the hard coat layer 5 is preferably from 0.5 to 20 μm, more preferably from 1 to 10 μm, and further preferably from 1.5 to 8 μm. When the thickness of the hard coat layer 5 is equal to or greater than the preferred lower limit, sufficient hardness can be ensured. When the thickness of the hard coat layer 5 is equal to or less than the preferred upper limit, defects such as curling do not occur. The hard coat layer 5 may contain a black pigment or black dye in order to suppress uneven light emission or color unevenness.

[0169] [Glossiness] The gloss level of the hard coat layer 5 measured by a gloss meter (JIS-Z-8741) is preferably 1-50, more preferably 3-30, and even more preferably 5-25. When the glossiness of the hard coat layer 5 side is equal to or higher than the lower limit, production is easy. When the glossiness of the hard coat layer 5 is equal to or lower than the preferred upper limit, the visibility of the display is improved.

[0170] <Semi-transparent resin layer> The sealing film layer 9 may have a semi-transparent resin layer provided on one or both surfaces of the support film layer 4. By providing a semi-transparent resin layer, the blackness of the display can be increased, and the contrast can be improved. Furthermore, when a semi-transparent resin layer is provided on the viewer side of the support film layer 4, diffuse reflection of external light from the support film layer 4 can be made less visible.

[0171] [Total light transmittance] The total light transmittance of the semi-transparent resin layer is preferably from 20 to 80%, more preferably from 30 to 80%, and further preferably from 40 to 75%. When the total light transmittance of the semitransparent resin layer is equal to or greater than the lower limit, light is not prevented from reaching the viewer side. When the total light transmittance of the semitransparent resin layer is equal to or less than the upper limit, the degree of blackness is increased, and the contrast improvement effect is further improved.

[0172] [Overall haze] The semi-transparent resin layer preferably has an overall haze based on JIS K 7136 of 7% or more, more preferably 10 to 70%, and even more preferably 15 to 65%. When the total haze of the semitransparent resin layer is equal to or greater than the preferred lower limit, the ability to conceal diffuse reflection of external light in the support film layer 4 is improved. When the total haze of the semitransparent resin layer is equal to or less than the preferred upper limit, the degree of blackness is increased. The total haze of the semitransparent resin layer can be adjusted by the compatibility of the carbon black, filler, and resin contained in the semitransparent resin composition.

[0173] [Storage modulus] The storage modulus of the semi-transparent resin layer at 100°C is 1.0×10 6 Pa or more, and 1.0×10 6 Pa or more, 1.0×10 10 Pa or less, and more preferably 1.0×10 7 Pa or higher, 5.0×10 9 More preferably, the surface tension is 1.0×10 Pa or less. 8 Pa or higher, 5.0×10 9 It is particularly preferable that the pressure is 0.1 Pa or less.

[0174] If the thickness of the semitransparent resin layer varies, the degree of blackness may become non-uniform in the surface direction, which may cause spots. By having the storage modulus at 100°C of the semitransparent resin layer be equal to or greater than the preferred lower limit, the semitransparent resin layer is less likely to deform when pressure-bonded to the element-mounted substrate 10, and the thickness is less likely to vary. Therefore, uneven light emission and color unevenness can be suppressed.

[0175] When the storage modulus at 100° C. of the semitransparent resin layer is equal to or less than the preferred upper limit, it is easy to prevent the occurrence of cracks during pressure bonding to the element-mounted substrate 10. In addition, it is easy to ensure adhesion between the semitransparent resin layer and the support film layer 4 or the hard coat layer 5.

[0176] [Translucent resin composition] The semitransparent resin layer can be composed of a coating film of a semitransparent resin composition containing carbon black, etc., or a cured product thereof. The semitransparent resin composition is a thermoplastic resin composition or a curable resin composition, and is preferably a curable resin composition from the viewpoint of being less likely to deform during durability tests under thermal shock or high humidity.

[0177] Examples of the resin contained in the translucent resin composition include epoxy resin, acrylic resin, polyester resin, polyurethane resin, polycarbonate resin, polyimide resin, acrylonitrile butadiene copolymer, styrene butadiene copolymer, vinyl acetate resin, and silicone resin. When the semitransparent resin composition is a curable resin composition, it is preferably a cured film from the viewpoints of being less prone to deformation and having stable coloration. In other words, it is preferably cured before being pressure-bonded to the element-mounted substrate 10.

[0178] <Protective film> As the first protective film 6 and the second protective film 7, the same protective films as those in the first embodiment can be used, and the preferred aspects are also the same.

[0179] <Manufacturing method of integrated encapsulating sheet> To obtain the integrated encapsulating sheet 200, a release sheet is prepared by coating and drying a coating liquid of the curable resin composition for the low elasticity transparent curable resin layer 2, and a sealing film layer 9 is prepared by coating and drying a coating liquid of the curable resin composition for the high elasticity transparent curable resin layer 3.

[0180] Thereafter, these are stacked and laminated so that the low elasticity, transparent curable resin layer 2 and the high elasticity, transparent curable resin layer 3 are in contact with each other, thereby obtaining a laminate (1) in which the high elasticity, transparent curable resin layer 3 and the low elasticity, transparent curable resin layer 2 are sequentially stacked on the sealing film layer 9. The second protective film 7 is laminated on the surface of this sealing film layer 9, if necessary.

[0181] In addition, a coating solution of a curable resin composition for the low elasticity black curable resin layer 1 is applied to a first protective film 6 and dried, and the release sheet of the laminate (1) from which the release sheet has been peeled off is layered on top of the laminate (1) so that the low elasticity black curable resin layer and the low elasticity transparent curable resin layer 2 are in contact with each other, and laminated to obtain an integrated encapsulating sheet 200.

[0182] The sealing film layer 9 having the hard coat layer 5 formed on the support film layer 4 can be obtained by applying a coating agent for the hard coat layer to the surface of the support film layer 4, drying the coating agent, and then curing the coating agent. When the sealing film layer 9 is formed by sequentially forming a translucent resin layer and a hard coat layer 5 on a support film layer 4, the sealing film layer 9 can be obtained by applying and drying a coating liquid of a translucent resin composition for the translucent resin layer on the surface of the support film layer 4, applying and drying a coating agent for the hard coat layer, and then curing the coating agent.

[0183] In addition, when the sealing film layer 9 is formed by forming a translucent resin layer on one side of the support film layer 4 and a hard coat layer 5 on the other side, the sealing film layer 9 can be obtained by applying and drying a coating liquid of a translucent resin composition for the translucent resin layer on one side of the support film layer 4, applying and drying a coating agent for the hard coat layer on the other side, and then curing the coating agent. The coating agent for the hard coat layer may be applied after the semi-transparent resin composition is cured.

[0184] <Method of manufacturing light-emitting electronic components> The method for producing a light-emitting electronic component of the present invention is a method in which the integrated encapsulating sheet 200 of the present invention is placed on a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, so that the low-elasticity black curable resin layer 1 is in contact with the surface, and the sheet is thermocompression-bonded to fill the low-elasticity black curable resin layer 1, the low-elasticity transparent curable resin layer 2, and a portion of the high-elasticity transparent curable resin layer 3 between the plurality of light-emitting elements, and the sheet is heated to cure these curable resin layers. Hereinafter, a method for manufacturing a light-emitting electronic component according to one embodiment of the present invention will be described with reference to FIGS.

[0185] In the manufacturing method of this embodiment, first, as shown in FIG. 8, an integrated encapsulating sheet 200 in which the first protective film 6 has been peeled off to expose the low elasticity black curable resin layer 1 is placed on the surface of the element-mounted substrate 10 on which the light emitting elements 12, 13, and 14 are arranged, so that the low elasticity black curable resin layer 1 is in contact with the surface.

[0186] At this time, i.e., before bonding, preferred aspects such as the thickness of the low elasticity black curable resin layer 1, the total thickness of the low elasticity transparent curable resin layer 2 and the high elasticity transparent curable resin layer 3, the total thickness of the low elasticity black curable resin layer 1, the low elasticity transparent curable resin layer 2 and the high elasticity transparent curable resin layer 3, and the ratio of the thicknesses of each layer are the same as those described for the case where the dry film 100 of the first embodiment is used.

[0187] 8, the dry film 100 is thermocompressed to embed the low elasticity black curable resin layer 1, the low elasticity transparent curable resin layer 2, and a part of the high elasticity transparent curable resin layer 3 between the light emitting elements as shown in FIG. In this case, since the low elasticity black curable resin layer 1 has a relatively low storage modulus and ensures fluidity, it is easy to fill between the light emitting elements by conforming to the unevenness of the light emitting elements, and is also unlikely to remain on the light emitting elements, which is preferable. In addition, the low elasticity transparent curable resin layer 2 also has a relatively low storage modulus and ensures fluidity, so that it easily follows the unevenness of the light emitting elements and is easily filled between the light emitting elements together with the low elasticity black curable resin layer 1.

[0188] The preferred conditions for the thermocompression bonding, such as temperature and pressure, are similar to those described for the case where the dry film 100 of the first embodiment is used. As in the first embodiment, it is preferable to use a vacuum press machine capable of molding in a vacuum state.

[0189] After the pressure bonding, the second protective film 7 is peeled off as shown in Fig. 10, and then the resulting mixture is thermally cured to form the low elasticity black curable resin layer 1 into a black cured material layer 21 (low elasticity black curable resin layer 1 in a cured state), the low elasticity transparent curable resin layer 2 into a first transparent cured material layer 22 (low elasticity transparent curable resin layer 2 in a cured state), and the high elasticity transparent curable resin layer 3 into a second transparent cured material layer 23 (high elasticity transparent curable resin layer 3 in a cured state) as shown in Fig. 11. This results in a light-emitting electronic component 32.

[0190] In the obtained light-emitting electronic component 32, the low-elasticity black cured resin layer 1, the low-elasticity transparent cured resin layer 2, and the high-elasticity transparent cured resin layer 3 are cured to form a black cured material layer 21, a first transparent cured material layer 22, and a second transparent cured material layer 23, respectively, and portions of the black cured material layer 21, the first transparent cured material layer 22, and the second transparent cured material layer 23 are filled between multiple light-emitting elements. In addition, FIG. 11 shows an example in which the black cured material layer 21 and the first transparent cured material layer 22 are all filled between multiple light-emitting elements, and a portion of the second transparent cured material layer 23 is filled between multiple light-emitting elements.

[0191] <Action and Effect> According to the dry film or integrated encapsulating sheet of the present invention, the low-elasticity black curable resin layer and the low-elasticity transparent curable resin layer are soft and fluid when pressed, while the high-elasticity transparent curable resin layer is hard, so that the stress of pressing can be sufficiently transmitted to the low-elasticity black curable resin layer and the low-elasticity transparent curable resin layer, and the low-elasticity black curable resin layer and the low-elasticity transparent curable resin layer can be sufficiently filled between the optical elements. In addition, since the highly elastic transparent curable resin layer has sufficient hardness, the black curable resin layer on the light emitting element can be removed even in areas where the light emitting elements have different inclinations and heights and are low in height and are not easily subjected to stress. Therefore, even if the light emitting elements have different inclinations and heights, a decrease in brightness can be suppressed without performing etching such as plasma treatment, which takes a lot of time.

[0192] According to the light-emitting electronic component and the method for producing the light-emitting electronic component of the present invention, the highly elastic transparent curable resin layer on the surface side of the dry film is the hardest, so that the appearance defect after curing can be suppressed. Since the integrated encapsulating sheet has the encapsulating film layer laminated thereon, the encapsulating work can be completed with a single pressure bonding, and even if the height or inclination of the light-emitting element is different, the black curable resin layer on the light-emitting element can be removed. Therefore, a light-emitting electronic component having sufficient brightness and blackness can be obtained without increasing the production cost or energy consumption. EXAMPLES

[0193] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the description of these examples. Note that the blend amounts in the following description are all calculated on a solid content basis.

[0194] <Raw materials> Details of the raw materials used in each of the examples and comparative examples are as follows. [Epoxy resin] EOCN (registered trademark)-1020-55: Manufactured by Nippon Kayaku Co., Ltd., cresol novolac type multifunctional epoxy resin (solid), softening point 55.7°C, epoxy equivalent 195g / eq. EPICLON(registered trademark) HP-7200H: Manufactured by DIC Corporation, cyclopentadiene novolac type multifunctional epoxy resin (solid), softening point 82°C, epoxy equivalent 227g / eq. jER (registered trademark) YX7200B35: Manufactured by Mitsubishi Chemical Corporation, a phenoxy-type epoxy resin (MEK solution, solid content 35 mass%), an epoxy resin having a glass transition temperature of 150°C, an epoxy equivalent of 8750 g / eq., and a weight average molecular weight of 27,218. [Elastomer] · Nipol NX775: Manufactured by Zeon Corporation, carboxy-modified nitrile rubber, elastomer with a weight average molecular weight of 208,000.

[0195] [Curing catalyst] Curesol (registered trademark) 2PZ-CN: 1-cyanoethyl-2-phenylimidazole, manufactured by Shikoku Kasei Corporation. ·Curesol 2E4MZ: Shikoku Kasei Corporation, 2-ethyl-4-methylimidazole.

[0196] [Carbon black] Special Black 4: ORION ENGINEERED CARBONS, gas black, pH 3, average particle size 25 nm.

[0197] [solvent] MEK: Methyl ethyl ketone, manufactured by Junsei Chemical Co., Ltd. PGM: Propylene glycol monomethyl ether, manufactured by Junsei Chemical Co., Ltd.

[0198] [Support film layer] -Cosmoshine (registered trademark) A4300: Toyobo Co., Ltd., PET film, thickness 75 μm. [Removable PET] · 1-E: Made by Nippa, thickness 50μm. · 1-TRE: Made by Nippa, thickness 50μm.

[0199] [Resin for hard coat layer] ACRIT (registered trademark) 8KX-078: Manufactured by Taisei Fine Chemical Co., Ltd., solid content concentration 40 mass%, UV-curable acrylic polymer, weight average molecular weight 40,000.

[0200] [Fine particles] Chemisnow (registered trademark) MX-500L: manufactured by Soken Chemical & Engineering Co., Ltd., cross-linked acrylic monodisperse particles, average particle diameter 5 μm. [Photoradical polymerization initiator] Omnirad(R) TPO H: Manufactured by IGM Resins BV.

[0201] <Preparation of coating solution>

[0202] [Coating liquid for transparent curable resin layer] The raw materials having the composition shown in Table 1 were mixed in a solvent of MEK / PGM=80 / 20 (volume ratio) to prepare coating liquids for transparent curable resin layer (raw materials 3-1 to 3-3) having a solid content concentration of 35% by mass. That is, the total amount of the raw materials having the composition shown in Table 1 (converted into solid content) was 35% by mass with respect to the entire coating liquid obtained.

[0203] [Table 1]

[0204] [Coating liquid for low elasticity black curable resin layer] 70 parts by mass of epoxy resin EPICLON HP-7200H (manufactured by DIC Corporation), 30 parts by mass of elastomer Nipol NX775 (manufactured by Nippon Zeon Corporation), 3 parts by mass of curing catalyst Curesol 2PZ-CN (manufactured by Shikoku Kasei Corporation), and 4 parts by mass of carbon black Special Black 4 (manufactured by Orion Engineered Carbons) were mixed in a solvent of MEK / PGM = 80 / 20 (volume ratio) to prepare a low-elasticity black curable resin layer coating liquid (raw material 4) with a solids concentration of 35 mass%.

[0205] [Coating liquid of semi-transparent resin composition] 80 parts by mass of epoxy resin EOCN-1020-55 (manufactured by Nippon Kayaku Co., Ltd.), 20 parts by mass of elastomer Nipol NX775 (manufactured by Nippon Zeon Co., Ltd.), 3 parts by mass of curing catalyst Curesol 2E4MZ (manufactured by Shikoku Kasei Co., Ltd.), and 0.5 parts by mass of carbon black Special Black 4 (manufactured by Orion Engineered Carbons) were mixed in a solvent of MEK / PGM = 80 / 20 (volume ratio) to prepare a translucent resin composition (raw material 1) with a solid concentration of 25 mass%.

[0206] [Coating agent for hard coat layer] 100 parts by mass of hard coat layer resin 8KX-078 (manufactured by Taisei Fine Chemical Co., Ltd.), 4.5 parts by mass of fine particle Chemisnow MX-500L (manufactured by Soken Chemical & Engineering Co., Ltd.), and 0.6 parts by mass of photoradical polymerization initiator Omnirad TPO H (manufactured by IGM Resins BV) were mixed into a solvent of MEK / PGM = 80 / 20 (volume ratio) to prepare a coating agent (raw material 2) for the hard coat layer with a solid concentration of 25 mass%.

[0207] <Total light transmittance of each layer> The total light transmittance of Cosmoshine A4300 (manufactured by Toyobo Co., Ltd.) was measured in accordance with JIS K 7361 using a haze meter NDH5000 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0208] The coating liquid for the low elasticity, transparent curable resin layer and the coating liquid for the high elasticity, transparent curable resin layer were each applied to Cosmoshine A4300 (manufactured by Toyobo Co., Ltd.) using an applicator so that the dry film thickness was 25 μm (50 μm in Comparative Examples 1 and 2), and the coating liquid for the low elasticity, transparent curable resin layer or the coating liquid for the high elasticity, transparent curable resin layer was cured by heating in a hot air circulating oven at 150° C. for 1 hour, thereby obtaining a film with each cured transparent curable resin layer. The total light transmittance of the obtained cured film with a transparent curable resin layer was measured using a haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K 7361, with the transmitted light of Cosmoshine A4300 being taken as 100%. The measurement results of the total light transmittance of each transparent curable resin layer are shown in Tables 2 and 3.

[0209] The coating liquid for the low elasticity black curable resin layer was applied to Cosmoshine A4300 (manufactured by Toyobo Co., Ltd.) using an applicator so that the dry film thickness would be 30 μm, and the coating liquid for the low elasticity black curable resin layer was cured by heating in a hot air circulating oven at 150°C for 1 hour, thereby obtaining a film with a cured low elasticity black curable resin layer. The total light transmittance of the obtained film with the cured low elasticity black curable resin layer was measured using a haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K 7361, with the transmitted light of Cosmoshine A4300 being taken as 100%. The measurement results of the total light transmittance of the low elasticity black curable resin layer are shown in Tables 2 and 3.

[0210] <Storage modulus of each monolayer> Onto the release surface of release PET 1-E (manufactured by Nippa Corporation, 50 μm), an applicator was used to apply the coating liquid for the low elasticity transparent curable resin layer, the coating liquid for the high elasticity transparent curable resin layer, and the coating liquid for the low elasticity black curable resin layer so that the dry film thickness was 40 μm, and after drying for 5 minutes at 120° C., the release PET 1-E was peeled off to obtain single-layer sheets of each of the low elasticity transparent curable resin layer, the high elasticity transparent curable resin layer, and the low elasticity black curable resin layer.

[0211] The storage modulus of each of the obtained monolayer sheets at 100° C. was measured using a viscoelasticity measuring device (TA Instruments, RSA-G2) at a measurement frequency of 1 Hz and a heating rate of 5° C. / min according to JIS K7244. The results are shown in Tables 2 and 3.

[0212] The storage modulus of the obtained highly elastic transparent curable resin layer at 150° C. was measured using a viscoelasticity measuring device (RSA-G2 manufactured by TA Instruments) at a measurement frequency of 1 Hz and a heating rate of 5° C. / min according to JIS K7244. The results are shown in Table 2.

[0213] <Substrate with evaluation element> A substrate with LED light emitting elements for evaluation was prepared by arranging multiple LED light emitting elements, each of which was 0.1×0.2 mm and 65 μm high, on an epoxy glass substrate.

[0214] <Dry film> [Examples 1 and 2] Onto the release surface of release PET 1-TRE (Nippa Corporation, 50 μm), an applicator was used to apply the coating liquid for the highly elastic, transparent, curable resin layer shown in Table 2 (raw material 3-2 or raw material 3-3) to a dry film thickness of 25 μm, and the coating was dried at 120° C. for 5 minutes to obtain a first sheet in which the highly elastic, transparent, curable resin layer was supported by the release PET.

[0215] A coating liquid (raw material 3-1) for a low elasticity, transparent, curable resin layer was applied to the release surface of release PET 1-E (Nippa Corporation, 50 μm) using an applicator so that the dry film thickness was 25 μm, and then dried at 120°C for 5 minutes to obtain a second sheet in which the low elasticity, transparent, curable resin layer was supported by the release PET.

[0216] The obtained first sheet and second sheet were stacked so that the low elasticity transparent curable resin layer and the high elasticity transparent curable resin layer were in contact with each other, and laminated with a roll laminator at 60°C. The release PET 1-E used in the second sheet was peeled off to obtain a third sheet.

[0217] In addition, the coating liquid (raw material 4) for the low elasticity black curable resin layer was applied to the release surface of release PET 1-E (manufactured by Nippa Corporation, 50 μm) using an applicator so that the dry film thickness was 30 μm, and then dried at 120° C. for 5 minutes to obtain a fourth sheet in which the low elasticity black curable resin layer was supported by the release PET.

[0218] The obtained third sheet and fourth sheet were overlapped so that the low elasticity transparent curable resin layer and the low elasticity black curable resin layer were in contact with each other, and laminated with a roll laminator at 60°C to obtain a dry film for each Example.

[0219] [Comparative Example 1]

[0220] A coating liquid (raw material 3-3) for a highly elastic, transparent, curable resin layer was applied to the release surface of release PET 1-TRE (Nippa Corporation, 50 μm) using an applicator so that the dry film thickness was 50 μm, and then dried at 120°C for 5 minutes to obtain a fifth sheet in which the highly elastic, transparent, curable resin layer was supported by the release PET.

[0221] In addition, the coating liquid (raw material 4) for the low elasticity black curable resin layer was applied to the release surface of release PET 1-E (manufactured by Nippa Corporation, 50 μm) using an applicator so that the dry film thickness was 30 μm, and then dried at 120° C. for 5 minutes to obtain a sixth sheet in which the low elasticity black curable resin layer was supported by the release PET.

[0222] The obtained fifth sheet and sixth sheet were overlapped so that the high elasticity transparent curable resin layer and the low elasticity black curable resin layer were in contact with each other, and laminated with a roll laminator at 60° C. to obtain a dry film of Comparative Example 1.

[0223] [Dry film mounting] The release PET 1-E on the low elasticity black curable resin layer side of the dry film of each example was peeled off, and the low elasticity black curable resin layer was placed in contact with the LED light emitting element of the evaluation element-mounted substrate. Then, using a vacuum press, dry film 1 was filled between the light-emitting elements under conditions of a vacuum of 100 hPa, 100°C, 0.36 MPa, and 3 minutes. The release PET 1-TRE in contact with the highly elastic transparent curable resin layer was peeled off, and the resulting product was then heated in an oven at 150°C for 1 hour to be thermally cured, thereby obtaining 10 light-emitting electronic components of each example.

[0224] [Brightness after mounting / Brightness before mounting] For ten light-emitting electronic components in each example, the luminance of the light-emitting electronic components was measured before and after mounting the dry film using a Konica Minolta CA-410 luminance meter, and the luminance after mounting was divided by the luminance before mounting to calculate the ratio of luminance after mounting to luminance before mounting. The average values ​​of the results for the ten light-emitting electronic components are shown in Table 2.

[0225] [Table 2]

[0226] As shown in Table 2, it was confirmed that the dry film according to the present invention can suppress the loss of the overall brightness.

[0227] <Sealing film layer> A coating solution of a translucent resin composition was applied to the first surface of a support film layer (Cosmoshine A4300: manufactured by Toyobo Co., Ltd.) using a bar coater so that the dry thickness was 7 μm, and the coating was dried at 120° C. for 5 minutes, and then heated in a hot air circulating oven at 80° C. for 72 hours to harden the translucent resin composition. Next, a corona treatment was performed on the surface of the translucent resin layer opposite the film layer, and a coating agent for a hard coat layer was applied using a bar coater so that the dry thickness was 3 μm. Then, after drying at 120° C. for 5 minutes, 400 mJ / cm 2 The coating agent for the hard coat layer was cured by irradiating it with ultraviolet light of 1000 nm to obtain a sealing film layer in which the semi-transparent resin layer and the hard coat layer were supported by the support film layer.

[0228] <Total light transmittance of sealing film layer> The total light transmittance of the obtained sealing film layer was measured using a haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K 7361. The results are shown in Table 3.

[0229] <Storage modulus of sealing film layer> The storage modulus of the obtained sealing film layer at 100° C. was measured using a viscoelasticity measuring device (RSA-G2 manufactured by TA Instruments) at a measurement frequency of 1 Hz and a temperature rise rate of 5° C. / min according to JIS K7244. The results are shown in Table 3.

[0230] <Integrated sealing sheet> [Examples 3 and 4] The coating liquid for the highly elastic transparent curable resin layer shown in Table 3 (raw material 3-2 or raw material 3-3) was applied to the second surface (the surface opposite to the first surface) of the support film layer in the sealing film layer using an applicator so that the dry film thickness was 25 μm, and then dried at 120° C. for 5 minutes to obtain a seventh sheet in which the seventh transparent curable resin layer was supported by the release PET.

[0231] The coating liquid (raw material 3-1) for the low elasticity transparent curable resin layer was applied to the release surface of release PET 1-E (Nippa Corporation, 50 μm) using an applicator so that the dry film thickness was 25 μm. Then, it was dried at 120 ° C for 5 minutes to obtain an eighth sheet in which the low elasticity transparent curable resin layer was supported by the release PET layer.

[0232] The obtained seventh sheet and eighth sheet were stacked so that the high elasticity transparent curable resin layer and the third low elasticity transparent curable resin layer were in contact, and laminated with a roll laminator at 60°C. The release PET used in the eighth sheet was peeled off to obtain a ninth sheet.

[0233] In addition, the coating liquid (raw material 4) for the low elasticity black curable resin layer was applied to the release surface of release PET 1-E (manufactured by Nippa Corporation, 50 μm) using an applicator so that the dry film thickness was 30 μm, and then dried at 120° C. for 5 minutes to obtain a 10th sheet in which the low elasticity black curable resin layer was supported by the release PET.

[0234] The obtained ninth sheet and tenth sheet were stacked so that the low elasticity transparent curable resin layer and the low elasticity black curable resin layer were in contact with each other, and laminated with a roll laminator at 60°C to obtain an integrated encapsulating sheet for each Example.

[0235] [Comparative Example 2] The coating liquid (raw material 3-3) for the high elasticity transparent curable resin layer was applied to the second surface (opposite surface to the first surface) of the support film layer in the sealing film layer using an applicator so that the dry film thickness was 50 μm. Then, it was dried at 120 ° C for 5 minutes to obtain an eleventh sheet in which the high elasticity transparent curable resin layer was supported by the sealing film layer.

[0236] In addition, the coating liquid (raw material 4) for the low elasticity black curable resin layer was applied to the release surface of release PET 1-E (manufactured by Nippa Corporation, 50 μm) using an applicator so that the dry film thickness was 30 μm, and then dried at 120° C. for 5 minutes to obtain a 12th sheet in which the low elasticity black curable resin layer was supported by the release PET.

[0237] The obtained 11th sheet and 12th sheet were stacked so that the high elasticity transparent curable resin layer and the low elasticity black curable resin layer were in contact with each other, and laminated with a roll laminator at 60°C to obtain an integrated encapsulating sheet of Comparative Example 2.

[0238] [Implementation of integrated encapsulating sheet] The release PET 1-E of the integrated encapsulating sheet of each example was peeled off, and the low elasticity black curable resin layer was placed in contact with the LED light emitting element of the evaluation element-mounted substrate. Then, using a vacuum press, a low-elasticity black curable resin layer and a low-elasticity transparent curable resin layer were filled between the light-emitting elements under conditions of a vacuum of 100 hPa, 100°C, 0.36 MPa, and 3 minutes, and the layers were then heated in an oven at 150°C for 1 hour to thermally cure, obtaining 10 light-emitting electronic components of each example.

[0239] [Lab] The Lab values ​​on the hard coat layer side of the 10 light-emitting electronic components obtained for each example were measured using a spectrophotometer CM-5 manufactured by Konica Minolta in accordance with JIS K 8722. The average Lab values ​​of the 10 light-emitting electronic components for each example are shown in Table 3.

[0240] [Brightness after mounting / Brightness before mounting] For ten light-emitting electronic components in each example, the luminance of the light-emitting electronic components before and after mounting the integrated encapsulant sheet was measured using a Konica Minolta CA-410 luminance meter, and the luminance after mounting was divided by the luminance before mounting to calculate the ratio of luminance after mounting / luminance before mounting. The average value of the results for the ten light-emitting electronic components is shown in Table 3.

[0241] [Table 3]

[0242] As shown in Table 3, it was confirmed that the dry film according to the present invention can suppress the loss of the overall brightness. [Explanation of symbols]

[0243] 1 Low elasticity black curable resin layer 2 Low elasticity transparent curable resin layer 3 Highly elastic transparent curable resin layer 4 Support film layer 5 Hard Coat Layer 6 First protective film 7 Second protective film 9. Sealing film layer 10 Substrate with element 11 Substrate 12 Light emitting element 13 Light emitting element 14 Light emitting element 21 Black cured material layer 22 First transparent cured material layer 23 Second transparent cured layer 25 Encapsulating materials 31 Light-emitting electronic components 32 Light-emitting electronic components 100 Dry Film 200 Integrated sealing sheet

Claims

1. A dry film is pressure-bonded to a surface of a substrate on which a plurality of light-emitting elements are arranged, the surface being provided with the plurality of light-emitting elements, The dry film includes a low-elasticity black curable resin layer, a low-elasticity transparent curable resin layer, and a high-elasticity transparent curable resin layer, which are laminated in this order from the side that will be in direct contact with the element-mounted substrate during the pressure bonding.

2. 2. The dry film according to claim 1, wherein the storage modulus of the high elasticity transparent curable resin layer at 100°C is greater than the storage modulus of the low elasticity transparent curable resin layer and the low elasticity black curable resin layer.

3. 3. The dry film according to claim 1, wherein the storage modulus of the low elasticity transparent curable resin layer at 100°C is greater than the storage modulus of the low elasticity black curable resin layer.

4. The storage modulus of the highly elastic transparent curable resin layer is 1.0×10 7 The dry film according to claim 1 or 2, wherein the viscosity is 0.1 Pa or less.

5. The storage modulus of the low elasticity black curable resin layer is 1.0×10 at 100° C. 5 The dry film according to claim 1 or 2, wherein the viscosity is 0.1 Pa or less.

6. The storage modulus of the low elasticity transparent curable resin layer is 1.0×10 at 100° C. 5 The dry film according to claim 1 or 2, wherein the viscosity is 0.1 Pa or less.

7. The storage modulus of the highly elastic transparent curable resin layer is 1.0×10 5 The dry film according to claim 1 or 2, having a modulus of elasticity of 1 Pa or more.

8. 3. The dry film according to claim 1, wherein the low elasticity black curable resin layer has a total light transmittance of 0 to 30%.

9. 3. The dry film according to claim 1, wherein the low-elasticity transparent curable resin layer has a total light transmittance of 50% or more.

10. 3. The dry film according to claim 1, wherein the highly elastic, transparent, curable resin layer has a total light transmittance of 50% or more.

11. The dry film according to claim 1 or 2, wherein the highly elastic transparent curable resin layer comprises a high molecular weight epoxy resin.

12. The dry film according to claim 11, wherein the high molecular weight epoxy resin has a weight average molecular weight of 10,000 to 100,000.

13. The dry film according to claim 11 , wherein the highly elastic transparent curable resin layer contains a phenoxy type epoxy resin as the high molecular weight epoxy resin.

14. The dry film according to claim 11, wherein the amount of the high molecular weight epoxy resin is 30 to 80% by mass relative to 100% by mass of the total resin solid content of the highly elastic transparent curable resin layer.

15. The dry film according to claim 1 , wherein the low elasticity black curable resin layer comprises an elastomer.

16. The dry film of claim 15 , wherein the elastomer is a modified elastomer.

17. The dry film according to claim 16, wherein the modified elastomer is an acid-modified acrylonitrile butadiene rubber.

18. The dry film according to claim 1 , wherein the low elasticity black curable resin layer contains carbon black.

19. 3. An integrated sealing sheet comprising: the dry film according to claim 1 or 2; and a sealing film layer provided on the opposite side of the high elasticity transparent curable resin layer to the low elasticity transparent curable resin layer.

20. 20. The integral encapsulating sheet according to claim 19, wherein the encapsulating film layer comprises a support film layer and a hard coat layer provided on the side of the support film layer opposite the highly elastic transparent curable resin layer.

21. A device-mounted substrate having a plurality of light-emitting elements arranged on a substrate, and the dry film according to claim 1 or 2, which is pressure-bonded to a surface of the device-mounted substrate on which the plurality of light-emitting elements are arranged, the low elasticity black cured resin layer, the low elasticity transparent cured resin layer, and a part of the high elasticity transparent cured resin layer are filled between the plurality of light emitting elements; The light-emitting electronic component, in which the low elasticity black curable resin layer, the low elasticity transparent curable resin layer, and the high elasticity transparent curable resin layer are cured.

22. A substrate having a plurality of light-emitting elements arranged on a substrate, and the integrated encapsulating sheet according to claim 19, which is pressure-bonded to a surface of the substrate having the light-emitting elements arranged thereon, the low elasticity black cured resin layer, and a part of the low elasticity transparent cured resin layer and the high elasticity transparent cured resin layer are filled between the plurality of light emitting elements; The light-emitting electronic component, in which the low elasticity black curable resin layer, the low elasticity transparent curable resin layer, and the high elasticity transparent curable resin layer are cured.

23. 3. A substrate having a plurality of light emitting elements arranged thereon, the dry film according to claim 1 or 2 is arranged on a surface on which the plurality of light emitting elements are arranged, so that the low elasticity black curable resin layer is in contact with the surface, and the dry film is thermally compressed; The low elasticity black curable resin layer, the low elasticity transparent curable resin layer, and the high elasticity transparent curable resin layer are cured by heating.

24. The method for producing a light-emitting electronic component according to claim 23, wherein the temperature during the thermocompression bonding is 80 to 120°C, and the curing is performed by heating at 100 to 160°C.

25. The integrated encapsulating sheet according to claim 19 is placed on a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, so that the low-elasticity black curable resin layer is in contact with the surface, and the sheet is thermally compressed. The low elasticity black curable resin layer, the low elasticity transparent curable resin layer, and the high elasticity transparent curable resin layer are cured by heating.

26. The method for producing a light-emitting electronic component according to claim 25, wherein the temperature during the thermocompression bonding is 80 to 120°C, and the curing is performed by heating at 100 to 160°C.

Citation Information

Patent Citations

  • LED packaging method, LED lamp and LED display

    CN115084320A

  • Sealing sheet, manufacturing method of sealing sheet, light emitting diode device, and manufacturing method of light emitting diode device

    JP2013077811A

  • Adhesive sheet and display body

    JP2020169262A

  • Optical laminate

    JP2021161263A

  • Thermosetting resin composition

    JP2023012051A