Aqueous ink composition for writing boards

The aqueous ink composition for writing boards, incorporating a neutralized isobutylene/maleic anhydride copolymer and starch saccharide, addresses the issues of scratch resistance and erasability on non-absorbing surfaces by maintaining color development and ease of removal under UV and high-temperature exposure.

JP2024168920AInactive Publication Date: 2024-12-05MITSUBISHI PENCIL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023085980
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional water-based ink compositions for writing instruments are not suitable for non-absorbing surfaces like window glass, as they lack sufficient scratch resistance and suffer from reduced color development and erasability due to exposure to ultraviolet rays and high temperatures.

Method used

An aqueous ink composition for writing boards containing a neutralized isobutylene/maleic anhydride copolymer, water-soluble resin, reduced starch saccharide, and optionally resin emulsion, along with hollow particles, to enhance scratch resistance and maintain color development and erasability under UV and high-temperature conditions.

Benefits of technology

The composition provides sufficient scratch resistance and excellent color development, with easy erasability even when exposed to UV rays or high temperatures, ensuring durable and clear markings on non-absorbing surfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168920000001
    Figure 2024168920000001
  • Figure 2024168920000002
    Figure 2024168920000002
  • Figure 2024168920000003
    Figure 2024168920000003
Patent Text Reader

Abstract

To provide an aqueous ink composition for writing boards that exhibits abrasion resistance even when applied to non-absorbent surfaces, while maintaining excellent coloration and erasability when exposed to environments with ultraviolet light or high temperatures.SOLUTION: An aqueous ink composition for writing boards contains at least a colorant, a neutralized product of an isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion, reduced starch hydrolysate, and water.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aqueous ink composition for writing boards, which can be used on non-absorbent surfaces such as glass surfaces, whiteboards, or blackboards, particularly on writing boards such as glass surfaces, and which has good color development of drawn lines even under ultraviolet light or high temperature environments, good erasability when wiped with water, and which is also abrasion resistance. [Background technology]

[0002] Conventional aqueous ink compositions for writing instruments and the like that have good erasability, water-resistant adhesion, etc. include, for example, [1] An ink composition for a marking pen containing water, a colorant, and a resin, characterized in that the resin is a water-soluble polyvinyl acetal resin (see, for example, Patent Document 1). [2] An aqueous pigment composition that aims to provide an aqueous pigment ink composition that, when used as a storefront sign or the like on a whiteboard or blackboard, the lines drawn on the non-absorbent surface can be easily erased by wiping with water despite having excellent water-resistant adhesion, and furthermore does not leave any residual image (see, for example, Patent Document 2). [3] A water-based marking pen ink composition for a writing board, which contains, as essential components in a solvent mainly composed of water, a pigment as a colorant, a resin, and a release agent, and the release agent is a phosphoric acid ester compound represented by the general formula 1 (see, for example, Patent Document 3). [4] A water-based ink composition for a writing board, comprising at least a pigment, a pigment dispersing resin, a masking agent, and modified polyvinyl alcohol or polyvinyl alcohol having a degree of saponification of 40 to 84% (see, for example, Patent Document 4). etc. are known.

[0003] However, with the aqueous ink compositions for writing instruments described in Patent Documents 1 to 4, when used as window glass paint for decorating storefront window glass surfaces and the like with an aqueous marking pen, as has been in demand in recent years, the abrasion resistance of lines drawn on glass surfaces is not sufficient, and furthermore, the color development and erasure properties of lines drawn on window glass surfaces when exposed to sunlight from outdoors, ultraviolet light, and a high-temperature environment are not excellent. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP-A-5-171092 (Claims, Examples, etc.) [Patent Document 2] JP 2015-48437 A (Claims, Examples, etc.) [Patent Document 3] JP 6-184486 A (claims, examples, etc.) [Patent Document 4] JP 2021-91815 A (Claims, Examples, etc.) Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, window glass paint has been used to decorate storefront window glass surfaces using water-based marking pens, but this has the problem that the lines are easily erased when touched or rubbed hard. Furthermore, window glass surfaces are easily exposed to sunlight from outside, and exposure to ultraviolet rays and high temperatures causes the lines to stick to the glass surface, reducing color development and erasability. The present invention has been made in consideration of the development process of the above-mentioned conventional technologies and the associated problems and current situation, and aims to solve these problems, and provides an aqueous ink composition for writing boards which has excellent abrasion resistance even when written on a non-absorbent surface, particularly a glass surface, and further which is resistant to deterioration in the color development of drawn lines even in ultraviolet or high temperature environments, and which can be easily erased. [Means for solving the problem]

[0006] In view of the above-mentioned problems in the prior art, the inventors have conducted intensive research and have found that the above-mentioned aqueous ink composition for writing boards can be obtained by containing at least a colorant, a neutralized product of isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion, reduced starch saccharification product, and water, thereby completing the present invention.

[0007] In other words, the aqueous ink composition for writing boards of the present invention is characterized by containing at least a colorant, a neutralized product of isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion, a reduced starch saccharification product, and water. The water-based ink composition for a writing board preferably contains hollow particles. The aqueous ink composition for a writing board preferably has a viscosity measured at a temperature of 25° C. and a shear rate of 38.3 (S-1) using an ELD type rotational viscometer of 10 to 35 (mPa·s). Effect of the Invention

[0008] According to the present invention, there is provided an aqueous ink composition for writing boards which has sufficient abrasion resistance when drawn on a non-absorbent surface, particularly a glass surface, and further has excellent color development and erasability of drawn lines even when exposed to ultraviolet light or in a high-temperature environment. The objects and advantages of the invention will be realized and obtained by means of the elements and combinations particularly pointed out in the claims. Both the foregoing general description and the following detailed description are exemplary and explanatory but are not restrictive of the invention as claimed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The following describes in detail the embodiments of the present invention. However, please note that the technical scope of the present invention is not limited to the embodiments described in detail below, but extends to the inventions described in the claims and their equivalents. The present invention can be implemented based on the contents disclosed in this specification and common technical knowledge in the relevant field (including design matters and obvious matters).

[0010] <Water-based ink composition for writing board> The aqueous ink composition for writing boards of the present invention is characterized by containing at least a colorant, a neutralized product of isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion, a reduced starch saccharification product, and water.

[0011] <Coloring material> The coloring materials used in the present invention include all dyes that dissolve or disperse in water, conventionally known inorganic and organic pigments such as titanium oxide, resin particle pigments containing pigments, pseudopigments in which resin emulsions are colored with dyes, white plastic pigments, hollow resin pigments (particles), pigments in which the surface is multi-layer-coated with iron oxide or titanium oxide or the like on a substrate of silica or mica, glittering pigments such as aluminum pigments, thermochromic pigments (particles), photochromic pigments (particles), and composite pigments (particles) thereof. Commercially available aluminum pigments that can be used include, for example, the WXM series in which the aluminum surface is rust-proofed with a phosphorus compound, the WL series in which the aluminum surface is rust-proofed with a molybdenum compound, the EMR series in which the surface of aluminum flakes is coated with high-density silica (all manufactured by Toyo Aluminum Co., Ltd.), SW-120PM (all manufactured by Asahi Kasei Chemicals Co., Ltd.), and the like, which can be used alone or in a mixture of two or more kinds. In the case where titanium oxide is added, it is desirable to use, for example, titanium oxide that has been treated with alumina or silica, or with zirconia or zinc, and it is preferable to use rutile or anatase type titanium oxide. Examples of dyes include acid dyes such as eosin, fuoxin, water yellow #6-C, acid red, water blue #105, brilliant blue FCF, and nigrosine NB; direct dyes such as direct black 154, direct sky blue 5B, and violet BB; and basic dyes such as rhodamine and methyl violet.

[0012] Examples of inorganic pigments include azo lakes, insoluble azo pigments, chelate azo pigments, phthalocyanine pigments, perylene and perinone pigments, and nitroso pigments. More specifically, inorganic pigments such as carbon black, titanium black, zinc oxide, red iron oxide, aluminum, chromium oxide, iron black, cobalt blue, iron oxide yellow, viridian, zinc sulfide, lithopone, cadmium yellow, vermilion, cadmium red, yellow lead, molybdate orange, zinc chromate, strontium chromate, white carbon, clay, talc, ultramarine blue, precipitated barium sulfate, baryte powder, calcium carbonate, lead white, navy blue, Prussian blue, manganese violet, aluminum powder, and brass powder; CI Pigment Blue 17, CI Pigment Blue 15, CI Pigment Blue 17, CI Pigment Blue 27, CI Pigment Red 5, CI Pigment Red 22, CI Pigment Red 38, CI Pigment Red 48, CI Pigment Red 49, CI Pigment Red 53, CI Pigment Red 57, C I Pigment Red 81, CI Pigment Red 104, CI Pigment Red 146, CI Pigment Red 245, CI Pigment Yellow 1, CI Pigment Yellow 3, CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14, CI Pigment Yellow 17, CI Pigment Yellow 34, CI Pigment Yellow 55, CI Pigment Yellow 74, CI Pigment Yellow 95, CI Pigment Yellow 166, CI Pigment Yellow 167, CI Pigment Orange 5, CI Pigment Orange 13, CI Pigment Orange 16, CI Pigment Violet 1, CI Pigment Violet 3, CI Pigment Violet 19, CI Pigment Violet 23, CI Pigment Violet 50, CI Pigment Green 7, etc.

[0013] Examples of thermochromic pigments (particles) include thermochromic pigments produced by microencapsulating a thermochromic composition containing at least a leuco dye that functions as a color former, a color developer that is a component capable of causing the leuco dye to develop color, and a color change temperature regulator that can control the color change temperature in the color development of the leuco dye and the color developer, so as to have a predetermined average particle size (e.g., 0.1 to 10 μm). Examples of photochromic pigments (particles) include photochromic particles composed of at least one selected from photochromic dyes (compounds), fluorescent dyes, etc., and a resin such as a terpene phenol resin; and photochromic pigments (particles) produced by microencapsulating a photochromic composition containing at least one selected from photochromic dyes (compounds), fluorescent dyes, etc., an organic solvent, and additives such as an antioxidant, a light stabilizer, and a sensitizer, so as to have a predetermined average particle size (for example, 0.1 to 10 μm). In the present invention (including the examples), the "average particle size" is a value measured by laser diffraction or dynamic light scattering. The D50 value is calculated on a volume basis, and this measurement can be performed using, for example, a particle size distribution analyzer HRA9320-X100 manufactured by Nikkiso Co., Ltd. The average particle size measured using dynamic light scattering is, for example, the average particle size value calculated using a concentrated particle size analyzer FPAR-1000 (manufactured by Otsuka Electronics Co., Ltd.) as determined by cumulant method analysis in scattering intensity distribution.

[0014] These coloring materials can be used alone or in combination of two or more (hereinafter simply referred to as "at least one"). Furthermore, among these coloring materials, from the standpoint of line color development and erasability, it is desirable to use pigments, that is, colored resin pigments such as the above-mentioned inorganic pigments, organic pigments, resin particle pigments containing pigments, or pseudo-pigments obtained by coloring resin emulsions with dyes, white plastic pigments, hollow resin pigments (particles), pigments based on silica or mica and surface-coated with a multilayer of iron oxide or titanium oxide, photoluminescent pigments such as aluminum pigments, thermochromic pigments (particles), photochromic pigments (particles), etc., and composite pigments (particles) of these.

[0015] The (total) content of these coloring materials is preferably 0.5 to 50% by mass, more preferably 2 to 40% by mass, and particularly preferably 5 to 30% by mass, based on the total amount of the aqueous ink composition for writing boards (hereinafter simply referred to as the "total amount of ink composition"). By making the content of this coloring material 0.5% by mass or more, it is possible to realize the color development of drawn lines and the formation of more beautiful drawn lines even when exposed to ultraviolet light or a high-temperature environment, while by making the content 50% by mass or less, it is preferable in that the erasability is good, the increase in viscosity is suppressed, and the ink fluidity is good. Among the above-mentioned coloring materials, it is more preferable to use a pigment in the ink composition for writing boards of the present invention in terms of erasability and maintaining the color development of drawn lines under ultraviolet light or a high-temperature environment.

[0016] The neutralized product of isobutylene-maleic anhydride copolymer used in the present invention is a neutralized product of a copolymer of isobutylene and maleic anhydride, and in the present invention, when used in combination with the water-soluble resin (including the resin emulsion) described below, it becomes a component that exhibits the function of enhancing abrasion resistance and achieving a good balance with erasability. In the neutralized product of isobutylene-maleic anhydride copolymer used, the basic structure of the isobutylene-maleic anhydride copolymer is represented by the following formula (I), and the following formula (II) is an ammonia-neutralized product (modified product) of isobutylene-maleic anhydride copolymer that can be preferably used in the present invention.

[0017] [ka]

[0018] [ka]

[0019] In the present invention, in addition to the ammonia-neutralized product of the above formula (II), sodium hydroxide-neutralized product and amine-neutralized product may be used. The values ​​of n in the above formula (I), l and m in (II), and j and k in the following formula (III) vary depending on the weight-average molecular weight described below, and the preferred ranges are determined. In the present invention, the copolymer may be a neutralized product obtained by imidizing (imide-modifying) an isobutylene-maleic anhydride copolymer represented by the following formula (III) and neutralizing the copolymer with ammonia, sodium hydroxide, an amine, or the like. [ka]

[0020] The weight-average molecular weight of each neutralized product of the isobutylene-maleic anhydride copolymer of the above formula (II), formula (III) or the like is preferably 3,000 to 400,000, more preferably 5,000 to 200,000, particularly preferably 30,000 to 100,000, and most preferably 50,000 to 70,000. This weight-average molecular weight is a value calculated in terms of polystyrene by aqueous gel permeation chromatography (GPC) analysis. The above isobutylene-maleic anhydride copolymer and its neutralized product can be a commercially available product, for example, "ISOBAM" manufactured by Kuraray Co., Ltd., and examples thereof include neutralized products of ISOBAM-04, 06, 10, and 18, and ISOBAM-104 and 110, which are commercially available products of ammonia neutralization (modification) of the isobutylene-maleic anhydride copolymer in the above formula (II), and further examples include neutralized products of ISOBAM-304, 306, and 310. When preparing a neutralized product of the isobutylene-maleic anhydride copolymer [from the above formula (I) etc.] to be used, for example, when all the carboxyl groups of the isobutylene-maleic anhydride copolymer are neutralized, the degree of neutralization is set to 1, and each neutralized product can be obtained by calculating and preparing the necessary amounts of ammonia, sodium hydroxide, amine, etc. to be used for neutralization.

[0021] The content of the neutralized product of the isobutylene-maleic anhydride copolymer is preferably 0.01 to 4 mass %, more preferably 0.05 to 3 mass %, and particularly preferably 0.1 to 2 mass %, based on the total amount of the ink composition. If the content of the neutralized product of this isobutylene-maleic anhydride copolymer is less than 0.01% by mass, sufficient abrasion resistance cannot be obtained on non-absorbent surfaces such as glass surfaces. On the other hand, if it exceeds 4% by mass, the viscosity increases and the ink ejection properties decrease, adversely affecting the writing properties and leading to a decrease in erasability.

[0022] The water-soluble resin and resin emulsion used in the present invention function as a fixing agent, dispersant and stabilizer, and examples thereof include at least one type selected from water-soluble resins having a hydrophobic portion in the molecule, such as polyacrylic acid, acrylic resins, water-soluble styrene-acrylic resins, water-soluble styrene-maleic acid resins, polyvinyl alcohol, polyvinylpyrrolidone, water-soluble maleic acid resins, water-soluble styrene resins, water-soluble ester-acrylic resins, ethylene-maleic acid copolymers, polyethylene oxide and water-soluble urethane resins, and resin emulsions, such as acrylic emulsions, vinyl acetate emulsions, polyolefin emulsions, urethane emulsions, styrene-butadiene emulsions, styrene-acrylonitrile emulsions, silicone resin emulsions and silicone-acrylic copolymer emulsions. From the viewpoints of dispersibility of coloring materials, viscosity adjustment, and fixing power improvement, it is preferable to use the above-mentioned water-soluble resins and resin emulsions having a glass transition temperature (Tg) of 140° C. or less, and more preferable to use acrylic resins, water-soluble styrene-acrylic resins, styrene maleic acid, water-soluble resins such as urethane resins, or acrylic resin emulsions, each of which has a glass transition temperature (Tg) of 140° C. or less. The lower limit of the glass transition temperature (Tg) is preferably −50° C. or more from the viewpoints of line drawing quality such as low gloss and abrasion resistance. By adjusting the glass transition temperature (Tg) of the resin to 140° C. or lower, it is possible to improve the scratch resistance and erasability without deteriorating the quality of the lines drawn in the coating film, such as cracks. In the present invention, the "glass transition temperature" is Tg measured in accordance with JIS K7121, and can be measured using, for example, Rigaku thermo plus evo DSC8230 (manufactured by Rigaku Corporation).

[0023] The water-soluble resin and resin emulsion may be commercially available. For example, water-soluble resins such as Joncryl JDX6500 (Tg; 65°C), JDX6180 (Tg: 134°C), 52J (Tg; 56°C), 70J (Tg; 102°C), and PDX-6137A (Tg; 102°C) manufactured by BASF Corporation may be used. Resin emulsions such as Joncryl PDX352D (Tg; 52°C), PDX7199 (Tg; 88°C), and PDX7537 (Tg; -4°C) manufactured by BASF Corporation, or KE-1062 (96°C) and PE-1304 (Tg; 9°C) manufactured by Seiko PMC Corporation may be used.

[0024] The content (total: solid content) of these water-soluble resins and resin emulsions, apart from the neutralized product of the isobutylene-maleic anhydride copolymer, is preferably 0.1 to 20 mass % based on the total amount of the ink composition, more preferably 0.5 to 15 mass %, and particularly preferably 1 to 10 mass %. If the content of this water-soluble resin or resin emulsion is less than 0.1% by mass, the abrasion resistance decreases, while if it exceeds 20% by mass, the erasability decreases, the viscosity of the aqueous ink composition for a writing board increases, and the ink ejection properties decrease, resulting in a deterioration in the quality of the drawn lines.

[0025] The reduced starch saccharification product used in the present invention is used as an additive that acts as an erasing agent, and when incorporated into the aqueous ink composition for writing boards, it does not cause a decrease in the ink performance. The reduced starch saccharified product used is a type of sugar alcohol, a chain polyhydric alcohol obtained by reducing the carbonyl groups of starch. For example, starch is liquefied with α-amylase or acid, and then partially hydrolyzed with an enzyme such as β-amylase to produce a saccharified solution, which is itself produced by catalytic reduction under hydrogen pressure using a known method. Examples of the reduced starch saccharification product that can be used include those obtained by the above-mentioned production method, as well as those commercially available for food or general use under the name of reduced starch saccharification product, such as PO-10 (trade name), PO-20 (trade name), PO-30 (trade name), PO-40 (trade name), Amenko (manufactured by Sumika Green Co., Ltd.), Ecopita Liquid (manufactured by Kyoyu Agri Co., Ltd.), and H-PDX (manufactured by Matsutani Chemical Industry Co., Ltd.) as reduced maltodextrin.

[0026] The content of these reduced starch saccharification products is desirably 0.1 to 5%, and preferably 0.5 to 4%, in terms of solid content concentration relative to the total amount of the ink composition. If this content is less than 0.1%, the effect as an erasing agent will be low, which is not preferred. On the other hand, if it exceeds 5%, the viscosity of the aqueous ink composition for a writing board will become too high, the abrasion resistance will decrease, and problems will arise with the storage stability of the ink, which is also not preferred.

[0027] The ink composition for writing boards of the present invention preferably uses hollow particles in terms of erasability and color development of lines exposed to ultraviolet light or a high-temperature environment. When written lines are exposed to ultraviolet light or a high-temperature environment, the coating film sticks to the glass surface, reducing the erasability of the lines. Furthermore, the color development of the lines due to ultraviolet light is also likely to decrease. However, the inclusion of hollow particles makes it easier to maintain a uniform and flexible coating film over time, and as a result, good erasability can be obtained even for drawn lines exposed to ultraviolet light or in a high-temperature environment, and fading of the drawn lines is suppressed, resulting in drawn lines with good color development.

[0028] The hollow particles used in the present invention are hollow particles having an average particle diameter of 0.1 to 2.0 μm, for example, commercially available products such as Ropeake OP-62 (average particle diameter 450 nm, hollow ratio 33%), Ropeake OP-91, Ropeake HP-1055 (average particle diameter 1000 nm, hollow ratio 55%), Ropeake HP-91 (average particle diameter 1000 nm, hollow ratio 50%), Ropeake ULTRA (average particle diameter 380 nm, hollow ratio 45%), Ropeake ULTRA E (average particle diameter 380 nm, hollow ratio 45%), Ropeake ULTRA At least one of the following may be used: DUAL (average particle size 380 nm, hollow ratio 45%) (all manufactured by DOW), SX-863(A), SX-864(B), SX-866(A), SX-866(B) (average particle size 300 nm, hollow ratio 30%), SX-868 (average particle size 500 nm) (all manufactured by JSR), Nipol MH5055 (average particle size 500 nm), Nipol MH8101 (average particle size 1 μm) (all manufactured by Zeon Corporation). The content of these hollow particles is preferably 0.1 to 10%, more preferably 0.5 to 8%, in terms of solid content concentration, relative to the total amount of the aqueous ink composition for writing boards. If the content of these hollow particles is less than 1%, erasability and color development tend to decrease, while if it exceeds 10%, the ink storage stability tends to decrease and the desired color development is impaired, which is undesirable.

[0029] When the aqueous ink composition for writing boards of the present invention has a viscosity measured at 25°C using an ELD type rotational viscometer at a shear rate of 38.3 (S-1) of 10 to 35 (mPa s), it becomes easier to form more uniform lines on the glass surface, which is more preferable in terms of the scratch resistance, color development, and erasability of the drawn lines. In the present invention, the viscosity is the measured value at a temperature of 25°C using an ELD type rotational viscometer with a shear rate of 38.3 (S-1), and can be measured using a Tokimec TV-20L viscometer (cone plate type) with a standard rotor (1°34' x R24).

[0030] The aqueous ink composition for writing boards of the present invention contains at least the neutralized product of the above-mentioned colorant and isobutylene-maleic anhydride copolymer, a water-soluble resin and / or resin emulsion, and reduced starch saccharification product, as well as water (tap water, purified water, distilled water, ion-exchanged water, pure water, etc.) as the solvent as the remainder, and may also contain appropriate amounts of dispersants, lubricants, pH adjusters, rust inhibitors, preservatives or antibacterial agents, thickeners, etc., within the scope of the invention that does not impair the effects of the present invention.

[0031] The dispersing agent that can be used includes nonionic and anionic surfactants and water-soluble resins other than the water-soluble resins mentioned above, and is preferably a water-soluble polymer. Examples of lubricants include nonionic lubricants such as fatty acid esters of polyhydric alcohols, higher fatty acid esters of sugars, polyoxyalkylene higher fatty acid esters, and alkyl phosphate esters, which are also used as surface treatment agents for pigments; anionic lubricants such as alkyl sulfonates and alkyl aryl sulfonates of higher fatty acid amides; derivatives of polyalkylene glycols, fluorine-based surfactants, acetylene-based activators, and polyether-modified silicones. Among these, from the viewpoint of the fixation of the drawn line coating film and the storage stability of the ink, it is preferable to use acetylene-based activators, and examples of commercially available products include the Surfynol series, such as Surfynol 104H (manufactured by Nissin Chemical Industry Co., Ltd.), and it is more preferable to contain 0.01 to 2% by mass of the aqueous ink composition for writing boards of the present invention based on the total amount of the composition.

[0032] Examples of pH adjusters include ammonia, urea, monoethanolamine, diethanolamine, triethanolamine, alkali metal salts of carbonates and phosphoric acids such as sodium tripolyphosphate and sodium carbonate, and hydrates of alkali metals such as sodium hydroxide. Examples of rust inhibitors include benzotriazole, tolyltriazole, dicyclohexylammonium nitrite, and saponins, while examples of preservatives or antibacterial agents include phenol, sodium omadine, sodium benzoate, and benzimidazole-based compounds. Examples of the thickener that can be used include cellulose derivatives, such as hydroxyalkyl celluloses such as hydroxyethyl cellulose, carboxymethyl cellulose (CMC) or a salt thereof, fermented cellulose, crystalline cellulose, polysaccharides, etc. Examples of polysaccharides that can be used include xanthan gum, guar gum, hydroxypropylated guar gum, casein, gum arabic, gelatin, amylose, agarose, agaropectin, arabinan, curdlan, callose, carboxymethyl starch, chitin, chitosan, quince seed, glucomannan, gellan gum, tamarind seed gum, dextran, nigeran, hyaluronic acid, pustulan, funoran, HM pectin, porphyran, laminaran, lichenan, carrageenan, alginic acid, tragacanth gum, alkaloid gum, succinoglycan, locust bean gum, tara gum, etc. Examples of synthetic polymers include polyacrylic acids, polyvinyl alcohol, polyethylene oxide, polyvinylpyrrolidone, polyvinyl methyl ether, bisacrylamide methyl ether, polyacrylamide, polyethyleneimine, polyethylene glycol, polydioxolane, polystyrene sulfonic acid, and polypropylene oxide. These may be used alone or in combination of two or more. If commercially available products of these are available, they may be used.

[0033] The aqueous ink composition for writing boards of the present invention is prepared by appropriately combining at least the above-mentioned colorant, neutralized product of isobutylene-maleic anhydride copolymer, water-soluble resin and / or resin emulsion, reduced starch saccharification product, water, and other components depending on the intended use of the ink for a writing instrument (for a ballpoint pen, a marking pen, etc.), stirring and mixing with a stirrer such as a homomixer, homogenizer, or disper, and further, if necessary, removing coarse particles from the ink composition by filtration or centrifugation, thereby obtaining an aqueous ink composition for writing boards with excellent color development. The pH (25°C) of the aqueous ink composition for writing boards of the present invention is preferably adjusted to 5 to 10 using a pH adjuster or the like from the viewpoints of usability, safety, the stability of the ink itself, and compatibility with the ink container, and is more preferably adjusted to 6 to 9.5.

[0034] The aqueous ink composition for writing boards of the present invention, which is configured in this manner, contains at least the above-mentioned colorant, neutralized product of isobutylene-maleic anhydride copolymer, water-soluble resin and / or resin emulsion, reduced starch saccharification product, and water. The colorant, water-soluble resin, resin emulsion, neutralized product of isobutylene-maleic anhydride copolymer, and reduced starch saccharification product make it possible to obtain an aqueous ink composition for writing boards which is scratch-resistant and does not easily stick to glass surfaces, even when lines are exposed to ultraviolet light or high temperature environments, and which can be easily erased.

[0035] Furthermore, the heating residue in the ink composition for writing boards of the present invention is preferably 2 to 60% by mass, more preferably 3 to 55% by mass, and even more preferably 5 to 50% by mass, in that good erasability can be obtained for lines exposed to a high-temperature environment. The heating residue in the present invention is a value measured in accordance with the method of JIS K 5601-1-2 (2008), and is a value measured for 2.0 g of an ink sample at a heating temperature of 150°C for a heating time of 60 minutes.

[0036] <Writing instruments> The writing instrument of the present invention is equipped with an aqueous ink composition for writing boards having the above-mentioned characteristics, and even when writing on a non-absorbent surface, particularly a glass surface, a writing instrument having excellent abrasion resistance, color development, erasability, etc. is obtained. As a writing instrument, for example, it is mounted on a ballpoint pen, a marking pen, etc., having a pen tip portion such as a ballpoint tip, a fiber tip, a felt tip, a plastic tip, a fiber core, or a porous core.

[0037] In the present invention, a "marking pen" refers to a pen having a mechanism for supplying ink stored in an ink reservoir to a resin writing part by capillary action, and includes pens referred to as "felt-tip pens." Additionally, a "ballpoint pen" refers to a pen having a mechanism for exuding ink stored in an ink reservoir by the rotation of a ball provided in the writing part. For a ballpoint pen, the aqueous ink composition for writing boards having the above composition is contained in a ballpoint pen ink container (refill) equipped with a ball having a diameter of 0.18 to 2.0 mm, and an ink follower is added. The ink follower is a liquid that is incompatible with the aqueous ink composition for writing boards having the above characteristics contained in the ink container and has a smaller specific gravity than the aqueous ink composition, such as polybutene, silicone oil, mineral oil, etc. The structure of the ballpoint pen, marking pen, etc. is not particularly limited, and may be, for example, a direct ink type ballpoint pen or marking pen having a collector structure (ink retention mechanism) in which the barrel itself serves as an ink container and is filled with the aqueous ink composition for writing boards having the above-mentioned configuration. In the aqueous ink composition for writing boards of the present invention, a direct ink marking pen having a fiber core is preferred, and a writing flow rate on the surface of a glass plate (15 cm long × 30 cm wide × 1 cm thick, ordinary plate glass) of 20 to 400 mg / m (straight line writing) is preferred, as this will provide better erasability and color development. EXAMPLES

[0038] Next, the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0039] [Examples 1 to 8 and Comparative Examples 1 to 5] Each aqueous ink composition for writing boards was prepared by a conventional method according to the formulation shown in Table 1. The pH of each aqueous ink composition for writing boards at room temperature (25°C) was measured with a pH meter (HORIBA Corporation) and was within the range of 7.9 to 8.2. Furthermore, the viscosity was measured by thoroughly stirring each aqueous ink composition for writing boards and then measuring the viscosity using a TV-20L viscometer (cone plate type) manufactured by Tokimec Co., Ltd. with a standard rotor (1°34′×R24) and a shear rate of 38.3 (S-1). For each of the aqueous ink compositions for writing boards obtained above, a writing instrument (marking pen) was prepared by the method described below, and the scratch resistance, color development, and erasability of drawn lines were evaluated by the evaluation methods described below. The glass plate used in the test was an ordinary plate glass measuring 15 cm in length, 30 cm in width, and 1 cm in thickness. The results are shown in Table 1 below.

[0040] (Making a marking pen) A marking pen was prepared using each of the ink compositions obtained above. Specifically, the barrel of a marking pen (manufactured by Mitsubishi Pencil Co., Ltd., product name: PXW-200-5M, barrel material: recycled PP resin, pen core: PET fiber) was used and each ink composition for writing board was loaded to prepare each direct ink marking pen. It was confirmed that the writing flow rate of each marking pen on the glass plate was within the range of 20 to 400 mg / m. Using the obtained marking pens of Examples 1 to 8 and Comparative Examples 1 to 5, various evaluations were carried out.

[0041] (Method of evaluating scratch resistance) Each pen was used to draw three spiral lines of circles about 2 cm in diameter on a glass plate, and the resulting lines were allowed to dry for 30 minutes. A waste paper (Kimwipe; made by Nippon Paper Crecia Co., Ltd.) was placed on the lines, a 500 g weight was placed on top, and the waste paper together with the weight was rubbed back and forth horizontally 20 times, after which the condition of the handwriting was evaluated according to the following criteria. Evaluation criteria: ○: No defects were observed in the writing △: There were one or two thin lines missing from the handwriting. ✕: There was a clear gap in the writing

[0042] (Method of evaluating color development) Each pen tip was used to draw three spiral lines of a circle with a diameter of approximately 2 cm on a glass plate. The resulting lines were then dried and exposed to light for 50 hours using a xenon fade meter X25F (FLR40SW / M / 36, manufactured by Suga Test Instruments Co., Ltd., with the black panel temperature set to 50±3°C during exposure). After this, the drawn lines were evaluated according to the following criteria: In the present invention, for white (or similar) or metallic color ink compositions for writing boards, if the lines drawn after the test using the Xenon Fedometer X25F showed a color change such as yellowing or browning compared to the initial hue, the ink compositions were judged to have inferior color development and were evaluated. Evaluation criteria: ◯: The drawn lines are the same as the initial ones. △: The color development of the drawn lines is slightly inferior to that of the above ○. ×: The color of the drawn lines is significantly inferior to that of the ○ above.

[0043] (Method of evaluating erasability) Each pen was used to draw three spiral lines of a circle with a diameter of approximately 2 cm on a glass plate. The resulting lines were then dried and exposed to light for 50 hours using a xenon fade meter X25F (FLR40SW / M / 36, manufactured by Suga Test Instruments Co., Ltd., with the black panel temperature during exposure set to 50±3°C). The lines were then erased with a tissue moistened with water and evaluated according to the following criteria. Evaluation criteria: ○: The drawn lines are erased cleanly. △: Compared to the above ○, there are some areas where the drawn lines remain slightly. ✕: Compared to the above ○, most of the lines remain.

[0044] [Table 1]

[0045] As is clear from the results in Table 1 above, the aqueous ink compositions for writing boards of Examples 1 to 8 of the present invention are superior in color development and erasability of drawn lines even when exposed to ultraviolet light or in a high-temperature environment, while being scratch-resistant when written on a non-absorbent surface, particularly a glass surface, compared to the aqueous ink compositions for writing boards of Comparative Examples 1 to 5, which are outside the scope of the present invention. [Industrial Applicability]

[0046] The ink can be suitably used in aqueous ink compositions for writing boards such as ballpoint pens and marking pens.

Claims

1. An aqueous ink composition for a writing board, comprising at least a coloring material, a neutralized product of an isobutylene-maleic anhydride copolymer, a water-soluble resin and / or a resin emulsion, a reduced starch saccharification product, and water.

2. 2. The water-based ink composition for writing boards according to claim 1, which contains hollow particles.

3. 3. The aqueous ink composition for writing boards according to claim 1 or 2, characterized in that the viscosity measured at a temperature of 25° C. and a shear rate of 38.3 (S-1) using an ELD type rotational viscometer is 10 to 35 (mPa·s).

Citation Information

Patent Citations

  • Ink composition for marking pen

    JP1993171092A

  • Aqueous marking pen ink composition for writing board

    JP1994184486A

  • Watercolor pigment ink composition