Gas barrier laminate and packaging bag

The gas barrier laminate with a polyolefin heat-sealing layer having a controlled carboxyl group ratio addresses corrosion issues, maintaining water vapor barrier and light shielding properties by using an ammonium salt to neutralize the layer and prevent aluminum corrosion.

JP2024168988AInactive Publication Date: 2024-12-05TOPPAN HOLDINGS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023086146
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing gas barrier laminates using paper and aluminum vapor-deposited layers suffer from corrosion issues that lead to deterioration of water vapor barrier properties and light shielding properties due to the alkalinity of polyolefin-based heat-sealing layers.

Method used

A gas barrier laminate is designed with a polyolefin heat-sealing layer containing a carboxyl group, where the ratio of the peak area derived from the salt of the carboxyl group to the peak area derived from the carboxyl group in the IR spectrum is 0.1 or less, using an ammonium salt to maintain neutrality and prevent corrosion of the aluminum layer.

Benefits of technology

The laminate effectively suppresses deterioration of water vapor barrier properties and maintains light shielding properties by preventing corrosion of the aluminum layer, ensuring long-term performance in high humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168988000001_ABST
    Figure 2024168988000001_ABST
Patent Text Reader

Abstract

To provide a gas barrier laminate made from paper that prevents deterioration in water vapor barrier performance.SOLUTION: A gas barrier laminate has a paper substrate, an aluminum-evaporated layer, and a heat seal layer in this order. The heat seal layer contains a polyolefin with carboxy groups. In the IR spectrum of the heat seal layer, the ratio of the peak area derived from salts of carboxy groups to the peak area derived from the carboxy groups is 0.1 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas barrier laminate and a packaging bag. [Background technology]

[0002] In many fields, such as food, beverages, pharmaceuticals, and chemicals, packaging materials are used according to the contents. Packaging materials are required to have gas barrier properties that prevent the permeation of oxygen and water vapor, which can cause deterioration of the contents.

[0003] In recent years, the momentum for a plastic-free society has been growing due to growing environmental awareness triggered by the problem of marine plastic waste. From the viewpoint of reducing the amount of plastic materials used, the use of paper instead of plastic materials has been considered in various fields. For example, the following Patent Document 1 discloses a gas barrier laminate in which a barrier layer is laminated on paper. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-69783 A Summary of the Invention [Problem to be solved by the invention]

[0005] In order to realize high gas barrier properties and high light shielding properties in a paper packaging material, it is possible to use a laminate in which an aluminum vapor deposition layer is provided on a paper base material. In addition, a gas barrier laminate using paper may be provided with a heat seal layer so that a packaging bag can be formed by heat sealing. The heat seal layer is formed, for example, by applying a coating liquid in which a polyolefin is dispersed in water onto an aluminum vapor deposition layer and drying it. However, according to the study by the present inventors, it was found that a gas barrier laminate having the above-mentioned configuration is prone to aluminum corrosion and a decrease in water vapor barrier properties.

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a gas barrier laminate using paper, which is capable of suppressing a decrease in water vapor barrier property due to corrosion of aluminum, and a packaging bag including the same. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides the following gas barrier laminate and packaging bag. [1] A gas barrier laminate comprising, in this order, a paper base material, an aluminum vapor-deposited layer, and a heat seal layer, wherein the heat seal layer contains a polyolefin having a carboxy group, and in an IR spectrum of the heat seal layer, the ratio of the area of ​​a peak attributable to a salt of the carboxy group to the area of ​​a peak attributable to the carboxy group is 0.1 or less. [2] The gas barrier laminate according to the above-mentioned [1], wherein the polyolefin having a carboxy group is an ethylene-(meth)acrylic acid copolymer. [3] The gas barrier laminate according to [1] or [2] above, in which no peak derived from a salt of a carboxy group is detected in the IR spectrum of the heat seal layer. [4] The gas barrier laminate according to any one of the above [1] to [3], further comprising an anchor coat layer between the paper substrate and the aluminum vapor deposition layer. [5] The gas barrier laminate according to [4] above, wherein the anchor coat layer contains a polyolefin having a carboxy group, and in an IR spectrum of the anchor coat layer, the ratio of the area of ​​the peak attributable to the carboxy group to the area of ​​the peak attributable to the salt of the carboxy group is 0.1 or less. [6] The gas barrier laminate according to [4] or [5] above, in which no peak derived from a salt of a carboxy group is detected in the IR spectrum of the anchor coat layer. [7] A packaging bag comprising the gas barrier laminate according to any one of [1] to [6] above. Effect of the Invention

[0008] Effects of the Invention According to the present invention, it is possible to provide a gas barrier laminate using paper, which is capable of suppressing a decrease in water vapor barrier property due to corrosion of aluminum, and a packaging bag including the gas barrier laminate. [Brief description of the drawings]

[0009] [Figure 1] 1 is a schematic cross-sectional view showing a gas barrier laminate according to one embodiment of the present invention. [Diagram 2] 1 is a perspective view showing a packaging bag according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings where necessary. However, the present invention is not limited to the following embodiments.

[0011] <Gas barrier laminate> The gas barrier laminate comprises a paper substrate, an aluminum vapor deposition layer, and a heat seal layer in this order, the heat seal layer contains a polyolefin having a carboxy group, and in the IR spectrum of the heat seal layer, the ratio of the area of ​​the peak derived from the carboxy group to the area of ​​the peak derived from the carboxy group salt is 0.1 or less. The carboxy group may be in an anhydride state (a carboxylic acid anhydride group).

[0012] The gas barrier laminate having the above-mentioned configuration can suppress the deterioration of the water vapor barrier property due to the corrosion of aluminum. The present inventors speculate as follows about the reason why such an effect is obtained. When forming a heat seal layer in a gas barrier laminate using a paper substrate, an aqueous coating liquid is almost always used from the viewpoint of odor and the like. A typical material for the heat seal layer is polyolefin, but since polyolefin is insoluble in water, an aqueous coating liquid is used in which acrylic acid or methacrylic acid is copolymerized with olefin to introduce a carboxyl group, and a metal salt of the carboxyl group is formed using sodium hydroxide, potassium hydroxide, or the like and dispersed in water. However, after extensive research, the present inventors found that if excess sodium hydroxide or potassium hydroxide remains in the heat seal layer, the heat seal layer exhibits alkalinity and tends to corrode the aluminum vapor deposition layer, which is an amphoteric compound. This causes defects such as holes in the aluminum vapor deposition layer, resulting in problems such as a decrease in water vapor barrier property and a decrease in light blocking property. In contrast, for example, if a water-based coating liquid is used in which ammonia is used to convert a carboxy group into an ammonium salt of the carboxy group and the ammonium salt is dispersed in water, the ammonia contained in the coating liquid in excess volatilizes during the drying process, and the heat seal layer becomes neutral. Furthermore, the ammonia released from the ammonium salt also volatilizes, resulting in a heat seal layer with many carboxy groups. In other words, the area (A COOH ) relative to the area of ​​the peak derived from the salt of the carboxyl group (A COOX ) ratio (A COOX / A COOH By making the above A ) 0.1 or less, the heat seal layer exhibits a neutral state, and corrosion of the aluminum deposition layer can be suppressed, and the deterioration of the water vapor barrier property and the light shielding property can be suppressed. COOX The above-mentioned A can be reduced by, for example, adjusting the material used to form the heat seal layer, the film formation conditions, etc., to suppress the salt of the carboxyl group from remaining in the heat seal layer. COOX By reducing the peak area ratio (A COOX / A COOH) can be lowered.

[0013] In the IR spectrum, the peak due to the carboxyl group is at 1700 cm -1 The peak due to the salt of the carboxyl group appears around 1490 to 1620 cm, depending on the type of salt. -1 For example, the peaks due to sodium salts of carboxyl groups and potassium salts of carboxyl groups appear between 1540 cm -1 The peak due to the ammonium salt of the carboxyl group appears around 1520 cm -1 By calculating the area of ​​such peaks, the area of ​​the peaks derived from the carboxyl group (A COOH ) and the area of ​​the peak due to the salt of the carboxyl group (A COOX ) can be obtained.

[0014] Fig. 1 is a schematic cross-sectional view showing a gas barrier laminate according to one embodiment. A gas barrier laminate 10 according to one embodiment includes, in this order, a paper base material 1, an anchor coat layer 2, an aluminum vapor deposition layer 3, and a heat seal layer 4. The gas barrier laminate does not necessarily need to include the anchor coat layer 2. Each layer will be described below.

[0015] (Paper base material) The paper base material 1 is not particularly limited and may be appropriately selected depending on the application of the packaging bag to which the gas barrier laminate 10 is applied. The paper base material 1 may be paper containing plant-derived pulp as a main component. Specific examples of the paper base material 1 include fine paper, special fine paper, coated paper, art paper, cast-coated paper, imitation paper, kraft paper, and glassine paper. The thickness (basis weight) of the paper base material 1 is, for example, 20 to 500 g / m 2 , 30~100g / m 2 It may be.

[0016] The paper base material 1 may have a coating layer at least on the side in contact with the anchor coat layer 2 described below. By providing the coating layer, it is possible to prevent the anchor coat layer from soaking into the paper, and it also plays a role of filling the unevenness of the paper, and the anchor coat layer can be formed uniformly without defects. For example, the coating layer may contain various copolymers such as styrene-butadiene, styrene-acrylic, and ethylene-vinyl acetate, polyvinyl alcohol resin, cellulose resin, paraffin (WAX), etc. as binder resin, and may contain clay, kaolin, calcium carbonate, talc, mica, etc. as filler.

[0017] The thickness of the coating layer is not particularly limited, but may be, for example, 1 to 10 μm, or 3 to 8 μm.

[0018] The mass of the paper is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, based on the mass of the entire gas barrier laminate. If the mass of the paper is 50% by mass or more based on the mass of the entire gas barrier laminate, the amount of plastic material used can be sufficiently reduced, the gas barrier laminate as a whole can be said to be made of paper, and recyclability is excellent.

[0019] (Anchor coat layer) The anchor coat layer 2 is provided on the surface of the paper base material 1 as necessary to improve adhesion between the paper base material 1 and the aluminum vapor deposition layer 3 (hereinafter simply referred to as "vapor deposition layer 3") described below, and to improve the gas barrier properties of the gas barrier laminate.

[0020] The anchor coat layer 2 may contain at least one resin selected from the group consisting of a polyolefin resin having a polar group, a polyvinyl alcohol resin, an acrylic resin, an epoxy resin, an acrylic urethane resin, a polyester polyurethane resin, and a polyether polyurethane resin. From the viewpoint of further suppressing the decrease in the water vapor barrier property, the anchor coat layer 2 may contain at least one resin selected from the group consisting of a polyolefin resin having a polar group, an epoxy resin, and an acrylic urethane resin.

[0021] When the anchor coat layer 2 contains a polyolefin having a polar group, the anchor coat layer 2 has excellent flexibility, and can suppress cracking of the deposition layer 3 described below after bending (folding), and can improve adhesion between the anchor coat layer 2 and the deposition layer 3. Furthermore, when the anchor coat layer 2 contains a polyolefin having a polar group, a dense film can be formed due to the crystallinity of the polyolefin, and water vapor barrier properties are expressed. The water vapor barrier properties are expressed due to the crystallinity of the polyolefin, and the presence of a polar group results in adhesion to the deposition layer 3.

[0022] The polyolefin having a polar group may have at least one group selected from a carboxy group, a salt of a carboxy group, a carboxylic anhydride group, and a carboxylic ester.

[0023] As the polyolefin having a polar group, a copolymer of ethylene or propylene with an unsaturated carboxylic acid (an unsaturated compound having a carboxy group, such as acrylic acid, methacrylic acid, or maleic anhydride) or an unsaturated carboxylic acid ester, or a salt obtained by neutralizing a carboxylic acid with a basic compound may be used. In addition, a copolymer of vinyl acetate, an epoxy compound, a chlorine compound, a urethane compound, a polyamide compound, or the like may also be used.

[0024] Specific examples of polyolefins having a polar group include ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, copolymers of acrylic acid esters and maleic anhydride, ethylene-vinyl acetate copolymers, and ethylene-glycidyl methacrylate copolymers.

[0025] The anchor coat layer 2 may contain components other than the above-mentioned resins. Examples of the other components include polyolefins other than the above-mentioned polyolefins having polar groups, silane coupling agents, organic titanates, polyesters, polycarbonates, polyureas, polyamides, polyimides, melamines, phenols, and the like.

[0026] The thickness of the anchor coat layer 2 may be, for example, 1 μm or more, 2 μm or more, 20 μm or less, 10 μm or less, or 5 μm or less. If the thickness of the anchor coat layer 2 is 1 μm or more, the unevenness of the paper base material described above can be efficiently filled, and the deposition layer described later can be laminated uniformly. Also, if the thickness of the anchor coat layer 2 is 20 μm or less, the deposition layer can be laminated uniformly while suppressing costs.

[0027] Examples of the solvent contained in the coating liquid of the anchor coat layer 2 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Furthermore, from the viewpoint of the environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.

[0028] When the anchor coat layer 2 contains a polyolefin having a carboxy group as a polar group, the area of ​​the peak derived from the carboxy group in the IR spectrum of the anchor coat layer 2 (A COOH ) relative to the area of ​​the peak derived from the salt of the carboxyl group (A COOX ) ratio (A COOX / A COOH The peak area ratio (A) may be 0.1 or less, may be 0.05 or less, or may be 0.03 or less. COOX / A COOH ) is not particularly limited, and may be, for example, 0.001 or more. In addition, a peak derived from a salt of a carboxy group may not be detected in the IR spectrum of the anchor coat layer 2. When the anchor coat layer 2 satisfies the above conditions, corrosion of the deposition layer 3 by the anchor coat layer 2 can be suppressed, and deterioration of the water vapor barrier property can be further suppressed.

[0029] The anchor coat layer 2 can be obtained by applying a coating liquid containing the above-mentioned resin and solvent onto a paper substrate and drying it. When a polyolefin having a carboxy group is used as the material for the anchor coat layer 2, it is preferable to use an aqueous dispersion of a polyolefin having an ammonium salt of a carboxy group as the coating liquid. When the aqueous dispersion is used, ammonia is likely to volatilize when the coating film dries, so the anchor coat layer 2 becomes neutral. Therefore, the anchor coat layer 2 can suppress corrosion of the deposition layer 3, and can further suppress deterioration of the water vapor barrier property.

[0030] The drying temperature of the coating liquid is preferably 105 to 160°C, more preferably 110 to 155°C, further preferably 120 to 150°C, and particularly preferably 125 to 145°C. By setting the drying temperature to the above lower limit or more, when a polyolefin having a carboxy group is used as the material of the anchor coat layer 2, alkaline ammonia is less likely to remain in the anchor coat layer 2. Therefore, the anchor coat layer 2 can prevent the deposition layer 3 from corroding, and the water vapor barrier property can be further prevented from decreasing. On the other hand, by setting the drying temperature to the above upper limit or less, the occurrence of poor appearance such as wrinkles due to sudden shrinkage of the paper can be prevented. The drying time of the coating film may be, for example, 0.1 to 5 minutes, or 1 to 3 minutes.

[0031] (Aluminum vapor deposition layer) The deposition layer 3 is obtained by depositing aluminum. The aluminum is aluminum oxide (AlO x ) may also be included.

[0032] The thickness of the deposited layer 3 may be appropriately set depending on the application, but is preferably 10 to 300 nm, and more preferably 30 to 100 nm. By setting the thickness of the deposited layer 3 to 10 nm or more, the continuity of the deposited layer 3 can be easily ensured, and by setting the thickness to 300 nm or less, the occurrence of curling or cracking can be sufficiently suppressed, and sufficient gas barrier performance and flexibility can be easily achieved.

[0033] From the viewpoint of oxygen gas barrier performance and film uniformity, it is preferable to form the deposition layer 3 by a vacuum deposition method. There are known deposition methods such as vacuum deposition, sputtering, and chemical vapor deposition (CVD), but vacuum deposition is preferred because of its fast deposition rate and high productivity. Among the vacuum deposition methods, deposition by electron beam heating is particularly effective because the deposition rate can be easily controlled by the irradiation area and electron beam current, and the temperature of the deposition material can be raised and lowered in a short time.

[0034] (Heat seal layer) The heat seal layer 4 is provided on the surface of the vapor-deposited layer 3 so as to be in contact with the vapor-deposited layer 3, and contains a polyolefin having a carboxy group.

[0035] Examples of polyolefins having a carboxy group include copolymers of ethylene or propylene with unsaturated carboxylic acids (unsaturated compounds having a carboxy group, such as acrylic acid and methacrylic acid) or unsaturated carboxylic acid esters, and salts of carboxylic acids neutralized with basic compounds. In addition, copolymers of ethylene or propylene with vinyl acetate, epoxy compounds, chlorine compounds, urethane compounds, polyamide compounds, and the like may also be used.

[0036] Specific examples of polyolefins having a carboxy group include ethylene-(meth)acrylic acid copolymers (ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers), ethylene-maleic anhydride copolymers, and the like.

[0037] Such a heat seal layer 4 has excellent flexibility, can suppress cracking of the deposition layer after bending (folding), and has excellent adhesion to the deposition layer. Furthermore, by containing the polyolefin having the above-mentioned carboxy group, a dense film can be formed due to the crystallinity of the polyolefin, and water vapor barrier properties are exhibited. Furthermore, by containing the carboxy group, which is a polar group, adhesion to the deposition layer is exhibited. Furthermore, by containing the polyolefin having the above-mentioned carboxy group, the heat seal layer 4 functions as a heat seal layer.

[0038] The heat seal layer 4 may contain other components in addition to the polyolefin having a carboxy group. Examples of the other components include polyolefins other than the polyolefin having a carboxy group, silane coupling agents, organic titanates, polyacrylics, polyesters, polyurethanes, polycarbonates, polyureas, polyamides, polyolefin-based emulsions, polyimides, melamines, and phenols.

[0039] The content of the polyolefin having a carboxy group in the heat seal layer 4 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.

[0040] The thickness of the heat seal layer 4 may be, for example, 0.05 μm or more, 0.5 μm or more, 1 μm or more, 20 μm or less, 10 μm or less, or 5 μm or less. If the thickness of the heat seal layer 4 is 0.05 μm or more, the heat seal layer 4 can fully fulfill the role of the heat seal layer described above. Also, if the thickness of the heat seal layer 4 is 20 μm or less, the heat seal layer 4 can fully fulfill the adhesiveness to the deposition layer and the barrier property while suppressing the cost.

[0041] Examples of the solvent contained in the coating liquid for the heat seal layer 4 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Furthermore, from the viewpoint of the environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.

[0042] In the IR spectrum of the heat seal layer 4, the area of ​​the peak derived from the carboxyl group (A COOH ) relative to the area of ​​the peak derived from the salt of the carboxyl group (A COOX ) ratio (A COOX / A COOH ) is 0.1 or less, may be 0.05 or less, or may be 0.03 or less. COOX / A COOH) is not particularly limited, and may be, for example, 0.001 or more. In addition, a peak derived from a salt of a carboxy group may not be detected in the IR spectrum of the heat seal layer 4. When the heat seal layer 4 satisfies the above conditions, corrosion of the deposition layer 3 by the heat seal layer 4 can be suppressed, and a decrease in the water vapor barrier property can be suppressed.

[0043] The heat seal layer 4 can be obtained by applying a coating liquid containing the above-mentioned polyolefin having a carboxy group and a solvent onto the deposition layer, and drying the coating liquid. As the coating liquid, it is preferable to use an aqueous dispersion of a polyolefin having an ammonium salt of a carboxy group. When the above-mentioned aqueous dispersion is used, ammonia is likely to volatilize when the coating film is dried, so that alkaline substances are unlikely to remain in the heat seal layer 4, and the heat seal layer 4 becomes neutral. Therefore, the heat seal layer 4 can suppress corrosion of the deposition layer 3, and the deterioration of the water vapor barrier property can be further suppressed.

[0044] The drying temperature of the coating liquid is preferably 105 to 160°C, more preferably 110 to 155°C, further preferably 120 to 150°C, and particularly preferably 125 to 145°C. By setting the drying temperature to the above lower limit or more, alkaline substances are less likely to remain in the heat seal layer 4. Therefore, the heat seal layer 4 can prevent the deposition layer 3 from corroding, and the water vapor barrier property can be further prevented from decreasing. On the other hand, by setting the drying temperature to the above upper limit or less, the occurrence of poor appearance such as wrinkles due to sudden shrinkage of the paper can be prevented. The drying time of the coating film may be, for example, 0.1 to 5 minutes, or 1 to 3 minutes.

[0045] When the anchor coat layer 2 contains a polyolefin having a carboxy group, the polyolefins having a carboxy group contained in the anchor coat layer 2 and the heat seal layer 4 may be the same or different, but may be the same if consideration is given to ease of production, etc.

[0046] <Packaging bag> 2 is a perspective view showing a gusset bag 20 made of a gas barrier laminate 10. A packaging bag is produced by sealing the opening at the top of the gusset bag 20. The gusset bag 20 has portions where the gas barrier laminate 10 is folded (folded portions B1, B2). The folded portion B1 is a portion where the gas barrier laminate 10 is folded in a valley direction when viewed from the innermost layer side, while the folded portion B2 is a portion where the gas barrier laminate 10 is folded in a mountain direction when viewed from the innermost layer side.

[0047] The packaging bag may be formed into a bag shape by folding one gas barrier laminate in half so that the heat seal layers 4 face each other, and then folding and heat sealing the laminate into the desired shape, or may be formed into a bag shape by stacking two gas barrier laminates together so that the heat seal layers 4 face each other, and then heat sealing the laminate.

[0048] In the packaging bag according to the present embodiment, the heat seal strength may be 2 N or more, or 4 N or more. The upper limit of the heat seal strength is not particularly limited, but may be, for example, 10 N or less.

[0049] The packaging bag can accommodate contents such as food, medicine, etc. In particular, it is suitable for accommodating food such as sweets. The packaging bag according to the present embodiment can suppress a decrease in water vapor barrier property.

[0050] In this embodiment, a gusset bag is given as an example of a packaging bag, but the gas barrier laminate according to this embodiment may be used to produce, for example, a pillow bag, a three-side sealed bag, or a standing pouch. EXAMPLES

[0051] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0052] <Preparation of gas barrier laminate> Example 1 On the surface of a paper substrate (coated paper, basis weight 55 g / m 2 ), a water dispersion of a polyolefin having an ammonium salt of a carboxy group (manufactured by Sumitomo Seika Chemical Co., Ltd., trade name: ZEIKEN AC, particle size: less than 0.2 μm, solvent: water / IPA = 1 / 1 (mass ratio), solid content concentration: 20% by mass) was applied at a coating speed of 200 m / min so that the thickness after drying with a gravure coater would be 3 μm. Subsequently, the coating film was dried in an oven at 125°C for 3 minutes to form an anchor coat layer.

[0053] Subsequently, AL vapor deposition was performed on the anchor coat layer by a vacuum vapor deposition method to form an AL vapor deposition layer (aluminum vapor deposition layer) with a thickness of 50 nm. Then, on the AL vapor deposition layer, a water dispersion of a polyolefin having an ammonium salt of a carboxy group (manufactured by Sumitomo Seika Chemical Co., Ltd., trade name: ZEIKEN AC, particle size: less than 0.2 μm, solvent: water / IPA = 1 / 1 (mass ratio), solid content concentration: 20% by mass) was applied at a coating speed of 200 m / min so that the thickness after drying with a gravure coater would be 3 μm. Subsequently, the coating film was dried in an oven at 125°C for 3 minutes to form a heat seal layer. Thus, a gas barrier laminate having a laminated structure of paper substrate / anchor coat layer / AL vapor deposition layer / heat seal layer was obtained.

[0054] (Comparative Example 1) In the same manner as in Example 1, an anchor coat layer and an AL vapor deposition layer were formed on a paper substrate. Then, on the AL vapor deposition layer, a water dispersion of a polyolefin having a sodium salt of a carboxy group (manufactured by Mitsui Chemicals, Inc., trade name: CHEMIPEARL S100, particle size: less than 0.1 μm, solvent: water / IPA = 1 / 1 (mass ratio), solid content concentration: 20% by mass) was applied at a coating speed of 200 m / min so that the thickness after drying with a gravure coater would be 3 μm. Subsequently, the coating film was dried in an oven at 125°C for 3 minutes to form a heat seal layer. Thus, a gas barrier laminate having a laminated structure of paper substrate / anchor coat layer / AL vapor deposition layer / heat seal layer was obtained.

[0055] (Measurement of IR Spectrum) The IR spectrum of the heat seal layer of the gas barrier laminate obtained in the examples and comparative examples was measured using a Fourier transform infrared spectrophotometer (manufactured by Perkin Elmer, product name: Frontier). -1 The carboxyl group peak appears around 1620-1770 cm -1 The area of ​​the peak between the two peaks was calculated as the area of ​​the peak derived from the carboxyl group (A COOH ) was calculated. On the other hand, 1520-1540 cm -1 The peak of the carboxyl group salt, which appears as a maximum around 1490-1620 cm -1 The area of ​​the peak between the two peaks was calculated as the area of ​​the peak derived from the salt of the carboxyl group (A COOX From these results, the ratio of the area of ​​the peak derived from the carboxyl group to the area of ​​the peak derived from the salt of the carboxyl group (A COOX / A COOH The results are shown in Table 1. The peak area ratios (A COOX / A COOH ) is the peak area ratio (A COOX / A COOH )

[0056] <Water vapor transmission rate (WVTR) measurement> The water vapor permeability (g / m) of the gas barrier laminate obtained in the examples and comparative examples under an atmosphere of 40°C and 90% RH 2 ·day) was measured using a water vapor permeability measuring device (manufactured by MOCON, product name: PERMATRAN 3 / 34G) in accordance with JIS K7129. The results are shown in Table 1 as the water vapor permeability of the initial gas barrier laminate.

[0057] <Measurement of Water Vapor Transmission Rate (WVTR) after Acceleration Test> An accelerated test was carried out by storing the gas barrier laminates obtained in the examples and comparative examples in an environment of 40°C and 90% RH. The water vapor permeability of the gas barrier laminates after storage for 7 days and 21 days was measured in the same manner as above. The water vapor permeability after storage for 7 days and 21 days was divided by the initial water vapor permeability to obtain the degree of deterioration of the water vapor barrier property. The smaller the degree of deterioration, the more the deterioration of the water vapor barrier property is suppressed. The results are shown in Table 1.

[0058] [Table 1]

[0059] As shown in Table 1, the peak area ratio (A COOX / A COOH ) was more than 0.1, whereas the peak area ratio (A COOX / A COOH ) was 0.1 or less, and it was confirmed that even when the gas barrier laminate was stored for a long period of time in a high humidity environment, the deterioration of the water vapor barrier property was suppressed. In Comparative Example 1, as peaks derived from the salts of the carboxyl groups, mainly peaks of the sodium salt of the carboxyl group (COONa) were detected, and A COOX In Comparative Example 1, sodium hydroxide did not volatilize from the coating film during drying when the heat seal layer was formed, and it is believed that a large amount of sodium salt of the carboxy group (COONa) remained. In contrast, in Example 1, ammonia volatilized from the coating film during drying when the heat seal layer was formed, and the ammonium salt of the carboxy group (COONH4) was converted to a carboxy group (COOH), so A COOX is thought to have become smaller. [Explanation of symbols]

[0060] Reference Signs List: 1...paper base material, 2...anchor coat layer, 3...aluminum vapor deposition layer, 4...heat seal layer, 10...gas barrier laminate, 20...gusset bag, B1, B2...folded portion.

Claims

1. A gas barrier laminate comprising a paper substrate, an aluminum vapor deposition layer, and a heat seal layer in this order, The heat seal layer comprises a polyolefin having a carboxy group, A gas barrier laminate, wherein in an IR spectrum of the heat seal layer, the ratio of the area of ​​a peak derived from a salt of a carboxy group to the area of ​​a peak derived from a carboxy group is 0.1 or less.

2. 2. The gas barrier laminate according to claim 1, wherein the polyolefin having a carboxy group is an ethylene-(meth)acrylic acid copolymer.

3. The gas barrier laminate according to claim 1 , wherein no peak derived from a salt of a carboxy group is detected in the IR spectrum of the heat seal layer.

4. The gas barrier laminate according to claim 1 , further comprising an anchor coat layer between the paper substrate and the aluminum vapor deposition layer.

5. The anchor coat layer contains a polyolefin having a carboxy group, 5. The gas barrier laminate according to claim 4, wherein in an IR spectrum of the anchor coat layer, the ratio of the area of ​​a peak derived from a salt of a carboxy group to the area of ​​a peak derived from a carboxy group is 0.1 or less.

6. The gas barrier laminate according to claim 4 , wherein no peak derived from a salt of a carboxy group is detected in the IR spectrum of the anchor coat layer.

7. A packaging bag comprising the gas barrier laminate according to any one of claims 1 to 6.